Method for producing low-loss optical fiber - Patents.com
The use of non-carbon reducing agents and controlled alkali doping in the optical fiber manufacturing process addresses high attenuation and hydrogen aging issues, achieving low loss and stable transmission in the C-band and L-band.
Patent Information
- Application Number
- JP2024527342
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-29
- Filing Date
- 2022-11-16
- Publication Date
- 2024-12-03
AI Technical Summary
Existing methods for manufacturing optical fibers result in high attenuation and susceptibility to hydrogen aging, particularly in the C-band and L-band transmission regions, due to the formation of oxygen-rich hydrogen aging defects and absorption peaks.
A manufacturing process involving the use of non-carbon reducing agents like SiCl4 during the densification of cladding soot blanks to reduce oxygen-rich hydrogen aging defects and minimize absorption peaks, combined with controlled alkali metal oxide doping to achieve low attenuation and improved refractive index profiles.
The process results in optical fibers with reduced attenuation across the C-band and L-band, minimizing absorption peaks and hydrogen aging sensitivity, ensuring stable performance in communication applications.
Smart Images

Figure 2024544516000001_ABST
Abstract
Description
Priority
[0001] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 283,604, filed November 29, 2021, the contents of which are relied upon and incorporated by reference in their entirety into this specification. [Technical field]
[0002] The present disclosure relates to optical fibers, and more particularly to methods for manufacturing low-loss optical fibers having low water peaks and low attenuation for C-band and L-band transmission. [Background technology]
[0003] Optical fibers are used in a variety of communication applications. The manufacturing process for producing optical fibers typically involves drawing the optical fiber from a heated glass preform in a draw furnace, cooling the drawn optical fiber, and coating the optical fiber. Summary of the Invention
[0004] According to one aspect of the disclosure, there is provided a method of manufacturing an optical fiber preform, the optical fiber having a core region and a cladding region, the method including forming a porous clad soot blank by depositing silica soot onto a core cane. The core cane includes a core portion having a composition corresponding to at least a portion of the core region of the optical fiber, the concentration of alkali metal oxide in the core portion of the core cane being between 0.1% and 1.5% by weight. The method includes exposing the porous clad soot blank to a fluorine doping precursor in the presence of SiCl4, the fluorine doping precursor doping the porous clad soot blank with fluorine to form a fluorine doped porous clad soot blank. The exposing includes providing a flow of the fluorine doping precursor to the porous clad soot blank. The method includes densifying a fluorine-doped porous clad soot blank in the presence or absence of a fluorine-doping precursor to form a densified fluorine-doped clad cane, the densifying step including exposing the fluorine-doped porous clad soot blank to SiCl4.
[0005] According to another aspect of the disclosure, a method of manufacturing an optical fiber, the optical fiber having a core region and a cladding region, the method includes forming an alkali-doped core cane. The alkali-doped core cane includes a portion having a composition corresponding to at least a portion of the core region of the optical fiber. The method includes forming a porous cladding soot blank by depositing silica soot on the alkali-doped core cane, and exposing the porous cladding soot blank to a fluorine-doping precursor. The fluorine-doping precursor dopes the silica soot with fluorine to form the fluorine-doped porous cladding soot blank. The exposing includes providing a flow of the fluorine-doping precursor to the porous cladding soot blank. The method includes densifying the fluorine-doped porous cladding soot blank in the absence or presence of the flow of the fluorine-doping precursor to form a fluorine-doped cladding cane having a portion having a composition corresponding to the cladding region of the optical fiber. The exposing step includes exposing the porous clad soot blank to a fluorine doping precursor in the presence of SiCl4, or the densifying step includes exposing the fluorine doped porous clad soot blank to SiCl4.
[0006] According to another aspect of the present disclosure, an optical fiber includes a core region comprising silica glass doped with an alkali metal oxide. A cladding region surrounds and is immediately adjacent to the core region. The cladding region includes a depressed-index cladding region surrounding the core region. The depressed-index cladding region comprises silica glass doped with a first fluorine concentration. The depressed-index cladding region has a minimum relative refractive index Δ in the range of −0.80% to −0.30%. 3min The cladding region includes an outer cladding region surrounding the depressed-index cladding region and immediately adjacent the depressed-index cladding region. The outer cladding region includes silica glass doped with a second fluorine concentration less than the first fluorine concentration. The outer cladding region has a relative refractive index Δ3 having a refractive index of Δ4-Δ 3min>0.05%. The optical fiber has a time to peak (TTP) hydrogen aging value of less than 100 hours at 23°C upon exposure of said optical fiber to a gas atmosphere having a total pressure of 1 atm (101325 Pa) and including a H2 partial pressure of 0.01 atm (1013.25 Pa) and a N2 partial pressure of 0.99 atm (100311.8 Pa). The optical fiber exhibits an attenuation of less than 0.16 dB / km at 1583 nm, with the attenuation increasing monotonically from about 1570 nm to about 1600 nm. [Brief description of the drawings]
[0007] Below are descriptions of the figures in the accompanying drawings: These figures are not necessarily to scale, and certain features and certain perspectives of the figures may be shown exaggerated in scale or schematic diagram form for the sake of clarity and conciseness. [Figure 1] 1 is a schematic cross-sectional view of an optical fiber according to the present disclosure; [Diagram 2] 4 is an exemplary step index refractive index profile of an optical fiber having an alkali metal oxide concentration that varies with the radius of the optical fiber in accordance with the present disclosure. [Diagram 3] 1 is an exemplary K2O concentration profile for an optical fiber according to the present disclosure. [Figure 4] 1 is an exemplary relative refractive index profile of an optical fiber according to the present disclosure. [Diagram 5] 1 is an exemplary relative refractive index profile of an optical fiber according to the present disclosure. [Figure 6] 1 is an exemplary relative refractive index profile of an optical fiber according to the present disclosure. [Figure 7A] 1 is an exemplary relative refractive index profile of an optical fiber according to the present disclosure. [Figure 7B] 1 is an exemplary relative refractive index profile of an optical fiber according to the present disclosure. [Figure 8] FIG. 1 is a schematic diagram illustrating a process for depositing glass soot in accordance with the present disclosure. [Figure 9]FIG. 1 is a schematic diagram of a method for doping a glass tube with an alkali metal oxide according to the present disclosure. [Figure 10] FIG. 2 is a flow diagram of a method for manufacturing an alkali-metal doped optical fiber in accordance with the present disclosure. [Figure 11] FIG. 2 is a flow diagram of a method for manufacturing an alkali-doped optical fiber according to the present disclosure. [Figure 12] 1 is a graph comparing the attenuation of an optical fiber using carbon monoxide as the reducing agent with a non-carbon reducing agent according to the present disclosure; [Figure 13] 1 illustrates an exemplary alkali metal oxide diffusion in an optical fiber according to the present disclosure. [Figure 14] FIG. 1 is a schematic diagram of a process for redrawing a glass rod according to the present disclosure. [Figure 15] 1 is a schematic diagram of a process for drawing optical fiber from a preform in accordance with the present disclosure. [Figure 16] 1 is an exemplary refractive index profile of a core cane utilizing a non-carbon reducing agent in the manufacturing process according to the present disclosure. [Figure 17] 1 is an exemplary refractive index profile of an optical fiber utilizing a non-carbon reducing agent in the manufacturing process according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Additional features and advantages are set forth in the following detailed description, and will become apparent to those skilled in the art from the description, or may be learned by practicing the embodiments as described in the following description, taken in conjunction with the claims and the accompanying drawings.
[0009] As used herein, the term "and / or," when used in a list of two or more items, means that any one of the listed items can be used by itself, or any combination of two or more of the listed items can be used. For example, if a composition is described as containing components A, B, and / or C, the composition may contain only A, only B, only C, a combination of A and B, a combination of A and C, a combination of B and C, or a combination of A, B, and C.
[0010] In this document, relative terms such as first and second, upper and lower, etc. are used only to distinguish one entity or act from another, and do not necessarily require or imply any such actual relationship or order between such entities or acts.
[0011] Modifications of the disclosure will occur to those skilled in the art and to those who make or use the disclosure. Accordingly, it is understood that the above-described embodiments illustrated in the drawings are merely illustrative and are not intended to limit the scope of the disclosure, which is defined by the following claims, as interpreted in accordance with patent law principles, including the doctrine of equivalents.
[0012] For purposes of this disclosure, the term "coupled" (in all of its forms: coupled, bonded, coupled, etc.) generally means joining two components to one another directly or indirectly. Such joining may be fixed in nature or movable in nature. Such joining may be accomplished whereby the two components and any additional intermediate members are integrally formed with one another or with the two components as a single, unitary entity. Unless otherwise noted, such joining may be permanent in nature or removable or releasable in nature.
[0013] As used herein, the term "about" means that amounts, sizes, formulations, parameters, and other quantities and characteristics are not and need not be exact, but may be approximate and / or may be greater or smaller, as appropriate, reflecting tolerances, conversion rates, rounding, measurement errors, and the like, and other factors known to those skilled in the art. When the term "about" is used to describe a value or an end point of a range, the disclosure should be understood to include the specific value or end point referred to. Regardless of whether "about" is used for a numerical value or an end point of a range herein, the numerical value or end point of the range is intended to include two embodiments, i.e., one modified by "about" and one not modified by "about". Moreover, it will be understood that the end points of each range are significant both in relation to the other end point and independently of the other end point.
[0014] As used herein, the terms "substantial", "substantially", and variations thereof are intended to state that the described feature is equal or approximately equal to a value or description. For example, a "substantially flat" surface is intended to indicate a flat or approximately flat surface. Furthermore, "substantially" is intended to indicate that two values are equal or approximately equal. In some embodiments, "substantially" may refer to values within about 10% of each other, e.g., within about 5% of each other, or within about 2% of each other.
[0015] As used herein, the terms "the," "a," or "an" mean "at least one" and should not be limited to "only one" unless expressly indicated to the contrary. Thus, for example, reference to a "component" includes embodiments having two or more such components unless the context clearly indicates otherwise.
[0016] As used herein, directional terms, such as upward, downward, right, left, front, rear, top, bottom, are used only with reference to the drawings depicted and are not intended to imply absolute orientations.
[0017] "Radial position", "radial distance", or radial coordinate "r" refers to the radial position in an optical fiber relative to the centerline of the core (r=0). The length dimension "μm" may be referred to herein as μm or micrometers.
[0018] A "refractive index profile" is the relationship between refractive index or relative refractive index and radial distance r from the centerline of the core. For relative refractive index profiles shown herein as having step boundaries between adjacent cladding regions, normal variations in process conditions may prevent obtaining an abrupt step boundary at the interface of the adjacent regions. Although the boundaries of the refractive index profile may be shown herein as a step change in refractive index, it is understood that the actual boundaries may be rounded or may otherwise deviate from a perfect step function characteristic. Furthermore, it is understood that the value of the relative refractive index may vary with radial position within the core region and / or any cladding region.
[0019] When the relative refractive index varies with radial position in a particular region of the fiber (the core region and / or any cladding region), this may be expressed in terms of an actual or approximate functional dependence, or in terms of an average value applicable to the region. Unless otherwise specified, when the relative refractive index of a region (the core region and / or any cladding region) is expressed as a single value, it is understood that the relative refractive index within this region is constant or nearly constant and corresponds to this single value, or that this single value represents an average value of the non-constant relative refractive index that depends on the radial position in this region. Whether by design or as a result of normal manufacturing variations, the dependence of the relative refractive index on radial position may be sloped, curvilinear, or otherwise non-constant.
[0020] As used herein with respect to optical fibers and fiber cores of optical fibers, "relative refractive index" or "relative refractive index percent" is defined as follows:
[0021]
number
[0022] where n(r) is the refractive index at radial distance r from the centerline of the core at a wavelength of 1550 nm, unless otherwise specified, and n c is approximately 1.444, which is the refractive index of undoped silica glass at a wavelength of 1550 nm. As used herein, the relative refractive index is expressed as Δ (or "delta") or Δ% (or "delta %), and values are given in units of "%" unless otherwise stated. The relative refractive index is sometimes expressed as Δ(r) or Δ(r)%. When the refractive index of a region is compared to a reference refractive index n c If the refractive index of a region is less than the reference refractive index n, then the relative refractive index is negative and may be referred to as a depressed-index region, trench, or moat. c If it is greater than 0.1, then the relative refractive index is positive and the region can be said to have elevated or positive refractive index.
[0023] Furthermore, the term “α-profile”, also referred to as “alpha profile”, refers to a relative refractive index profile Δ(r) having the following functional form:
[0024]
number
[0025] In the formula, r o is the point where Δ(r) is maximum, r1 is the point where Δ(r) is zero, and r is the point where r i ≦r≦r f is in the range of r i is the initial point of the α-profile, and rf are the α-profile points, where α is a real number. In some embodiments, examples shown herein may have a core alpha where 1≦α≦100. In practice, even if the target profile is an alpha profile, some deviation from the ideal configuration may occur. Thus, the alpha parameter of an optical fiber may be obtained from a best fit of the measured refractive index profile, as known in the art.
[0026] The disclosure herein relates to optical fiber preforms (also referred to herein as "preforms") or elements used in their fabrication, such as canes, rods, soot blanks, or deposition tubes. A core cane or core rod is a densified glass body having a composition corresponding to at least a portion of the core or core region of an optical fiber drawn from the preform. An optical fiber preform is a densified glass article suitable for drawing into an optical fiber. An optical fiber preform includes a central core region surrounded by one or more cladding regions, the refractive indices of the core and cladding regions being configured such that an optical fiber drawn from the finished optical fiber preform functions as a waveguide for light having a wavelength of 1550 nm. Additionally, as used herein, "cane," "core region" or "core," "cladding region" or "cladding," and other similar terms refer to densified glass. In some embodiments, the densified glass is prepared by depositing soot (e.g., soot particles including silica or doped silica) to form a porous body (e.g., core soot to form a porous core soot blank, or clad soot to form a porous clad soot blank) and densifying the soot. In some embodiments, the porous body is formed on the densified glass (e.g., depositing clad soot on a core cane to form a porous clad soot blank).
[0027] As used herein, "ppm (10 -6"%" means parts per million by mass, or "ppm (10 -6 %)" or "ppm (10 -6 %), and mass percent (mass%) measurements are multiplied by 10,000 to convert them to ppm (10 -6 %) can be converted to
[0028] 1 and 2, an optical fiber 10 disclosed herein includes a core region or core 12 and a cladding region or cladding 14 surrounding the core 12. The core 12 refers to a portion of the optical fiber 10 that generally has an elevated refractive index relative to the cladding 14 such that the transmitted optical power of the guided light propagates primarily through the core 12. The core 12 generally has a non-negative relative refractive index relative to the cladding 14. The core 12 may include one or more regions. An individual core region may have a refractive index greater than, equal to, or less than pure silica. The cladding 14 may be an annular ring surrounding and immediately adjacent to the core 12. The core 12 may have a radius r of about 2 μm to about 8 μm, about 3 μm to about 6 μm, or about 3.5 μm to about 4.5 μm. The core 12 may include a single core region as shown, or alternatively may include multiple core regions within the core radius.
[0029] Dopants may be utilized to increase or decrease the relative refractive index of the core 12 and cladding 14. Updopants are used to refer to dopants that increase the relative refractive index compared to pure undoped silica. Non-limiting updopants include, for example, chlorine. Downdopants are used to refer to dopants that decrease the relative refractive index compared to pure undoped silica. Non-limiting examples of downdopants include, for example, fluorine and boron.
[0030] 2, the illustrated embodiment of optical fiber 10 includes a silica-based core 12 extending from about 0 μm to about 4 μm. The cladding is fluorine-doped silica, and a fluorine-doped silica cladding 14 surrounds the core 12. The core 12 includes an alkali metal oxide, as discussed further herein, having an average concentration of about 50 ppm by mass (about 50×10 -6 %) to about 500 ppm (about 500 x 10 -6 %). Core 12 may also include chlorine and / or fluorine. The average amount of chlorine and fluorine in core 12 may be greater than the amount of alkali metal oxide.
[0031] In the illustrated example, the core 12 includes a central core region 16 that is located along a centerline 18 of the core 12 and extends to about 1 μm. The central core region 16 contains a lower average concentration of chlorine than is contained in an outer core region 20 that extends from about 1 μm to about 4 μm of the core 12 around the central core region 16. The average concentration of chlorine present in the central core region 16 is about 100 ppm (about 100×10 -6 %) or less than about 50 ppm (about 50 x 10 -6 The average concentration of chlorine in the outer core region 20 may be less than about 500 ppm (about 500×10 -6 %) super, about 750ppm (about 750×10 -6 %) super, about 1000ppm (about 1000×10 -6 %) or about 1500 ppm (about 1500 x 10 -6 %). The peak concentration of chlorine in the core 12 is generally greater than about 500 ppm (about 500×10 -6 %) super, about 1000ppm (about 1000×10 -6 %) or about 1500 ppm (about 1500 x 10 -6 %).
[0032] The average concentration of fluorine present in the central core region 16 is generally about 500 ppm (about 500×10 -6 %) super, about 750ppm (about 750×10 -6 %) or about 1000 ppm (about 1000 x 10-6 %. The average concentration of fluorine in the outer core region 20 is also about 500 ppm (about 500×10 -6 %) super, about 750ppm (about 750×10 -6 %) or about 1000 ppm (about 1000 x 10 -6 %. The average concentration of fluorine throughout the core 12 is generally greater than about 500 ppm (about 500×10 -6 %) and approximately 4000 ppm (approximately 4000 x 10 -6 %). The concentration of fluorine in core 12 is typically about 0.15% to about 0.25% by weight. The level of fluorine in core 12 is low and core 12 has a slightly positive delta due to potassium in core 12.
[0033] The optical fiber 10 also includes an alkali metal oxide. The alkali metal oxide is typically an oxide of at least one of K, Na, Li, Cs, Rb, or a combination thereof. The alkali metal oxide may include at least one of KO, NaO, LiO, RbO, CsO, or a combination thereof. Typically, the concentration of the alkali metal oxide in the core region 12 is between 0.1% and 1.5% by weight. In certain embodiments, the alkali metal oxide may be formed from KI and O.
[0034] An exemplary concentration profile for the dopants is illustrated in FIG. 3. The optical fiber 10 includes a core 12 and a cladding 14 surrounding the core 12. In general, the concentration of the alkali metal varies as a function of radius r. The concentration of the alkali metal oxide may decrease as radius r increases from a centerline 18 of the optical fiber 10 along at least a portion of the optical fiber radius r. The relative refractive index profile of the core 12 may have a step, round, alpha, or triangular shape. The K2O profile of FIG. 3 shown was measured by ToF-SIMS.
[0035] In various examples, the optical fiber 10 formed by the disclosed process contains little or no germanium in the core 12. In such examples, the silica glass core 12 and cladding 14 of the optical fiber 10 contain sufficient concentrations of updopants and / or downdopants to produce a relative refractive index profile within the scope of the present disclosure. The relative refractive index of the cladding 14 is less than that of the core 12. As discussed herein, refractive index reducing dopants (downdopants) for use in the cladding 14 are typically fluorine.
[0036] The optical fiber 10 having the relative refractive index profile 22 as shown in FIG. 4 typically has a zero dispersion wavelength λ0 of about 1280 nm to about 1340 nm, a dispersion coefficient of about 0.07 ps / nm 2 The single mode optical fiber 10 has a dispersion slope at about 1550 nm of less than about 15 ps / nm / km, and a total dispersion at 1550 nm of about 15 ps / nm / km to about 20 ps / nm / km. However, other relative refractive index profiles 22 could be used to achieve these same or similar characteristics. The optical fiber 10 generally has a cutoff wavelength of about 1300 nm or less. The optical fiber 10 has a cutoff wavelength of about 70 μm at 1550 nm. 2 The optical fiber 10 may have an effective area of greater than about 3 μm, or between about 3 μm and 5 μm. Additionally, the optical fiber 10 may have a mode field diameter at 1550 nm of greater than about 9 μm, between about 9.5 μm and about 11 μm, or between about 10 μm and about 11 μm.
[0037] An exemplary relative refractive index profile 22 that may be produced by the processes disclosed herein is illustrated in Figure 4. Core 12 has a non-negative relative refractive index Δ1. Cladding region 14 has a negative relative refractive index. Cladding region 14 includes an inner cladding region 24 having a relative refractive index Δ2, a depressed-index cladding region or moat 26 having a relative refractive index Δ3, and an outer cladding region 28 having a relative refractive index Δ4. Moat 26 has a relative refractive index Δ3 and a minimum relative refractive index Δ 3minis less than -0.30%. In certain embodiments, moat 26 has a relative refractive index Δ3 and a minimum relative refractive index Δ 3min In various embodiments, outer cladding region 28 has a relative refractive index Δ4, where Δ4 and Δ 3min The difference between is more than 0.05% (e.g., Δ4-Δ 3min >0.05%), and Δ4 may be greater than, equal to, or less than zero. The preform 50 that is drawn into optical fiber 10 may also have refractive index values in the same or similar ranges.
[0038] A negative relative refractive index can be formed using a downdopant such as fluorine. In various examples, the moat 26 is silica glass doped with a first fluorine concentration and the outer cladding region 28 is silica glass doped with a second fluorine concentration. The second fluorine concentration is lower than the first fluorine concentration, resulting in a lower relative refractive index at the moat 26. In general, about 1 wt. % Cl doping increases Δ by about 0.1% and about 1 wt. % F decreases Δ by about 0.3%. When both Cl and F are present, the effects of each of Cl and F on Δ are independent and the concentrations net out to yield the Δ disclosed herein.
[0039] The relative concentrations of chlorine may also vary between the moat 26 and the outer cladding region 28. In various examples, the moat 26 has a first chlorine concentration and the outer cladding region 28 has a second chlorine concentration. The second chlorine concentration may be lower than the first chlorine concentration.
[0040] 5-7B, exemplary refractive index profiles 22 are illustrated. Cl and F are subtracted to form the disclosed refractive index profile 22. In FIG. 5, the maximum concentration of fluorine in the moat 26 is about 1 wt. % fluorine, and the maximum concentration of fluorine in the outer cladding region 28 is about 0.9 wt. % fluorine. In some examples, the concentration of chlorine in the moat 26 is greater than 200 ppm (200×10 -6In another example, the concentration of chlorine at moat 26 is greater than 500 ppm (500×10 -6 In an additional non-limiting example, the concentration of chlorine at moat 26 is greater than 1000 ppm (1000×10 -6 %. In various examples, the concentration of chlorine in the outer cladding region 28 is greater than 200 ppm (200×10 -6 %), and in other examples, the concentration of chlorine in the outer cladding region 28 is less than 100 ppm (100×10 -6 %).
[0041] 6, the maximum concentration of fluorine in the moat 26 is about 1.25 wt. % fluorine, and the maximum concentration of fluorine in the outer cladding region 28 is about 1 wt. % fluorine. In various examples, the concentration of chlorine in the moat 26 is about 200 ppm (200×10 -6 %) and in other examples, more than 500 ppm (500×10 -6 In an additional non-limiting example, the concentration of chlorine at moat 26 is greater than 1000 ppm (1000×10 -6 In some examples, the concentration of chlorine in the outer cladding region 28 is greater than 200 ppm (200×10 -6 %) or less than 100 ppm (100 x 10 -6 %).
[0042] 7A and 7B, additional exemplary refractive index profiles 22 are illustrated. The fluorine concentration is generally equal to -% delta refractive index / 0.3. The particular Δ disclosed in Figures 7A and 7B is generated from the difference between updoping with Cl and downdoping with F.
[0043] 8-11, an optical fiber 10 having an alkali doped core 12 and reduced attenuation is produced by a manufacturing method 40 that generally involves four stages 42, 44, 46, 48 to form a preform 50, followed by a final draw of the preform 50 into optical fiber 10. The first two stages 42, 44 involve forming the inner or central core region 16 (first stage 42) and the outer core region 20 (second stage 44). As described further herein, the first stage 42 includes steps 60-72 to form the central core region 16, and the second stage 46 includes steps 74-82 to form the outer core region 20. The next two stages 46, 48 form the cladding region 14, including the inner cladding region 24 (if present), the moat 26 (third stage 46), and the outer cladding 28 (fourth stage 48). A third phase 46 includes steps 84-92 for forming the inner cladding region 24 and / or the moat region 26, and a fourth phase includes steps 94-100 for forming the outer cladding region 28. After the four phases 42, 44, 46, and 48 of the method 40 are completed, a preform 50 is formed and ready for drawing into optical fiber 10 (step 102).
[0044] As described herein, various locations in optical fiber 10 are described as "regions," such as inner core region 16, outer core region 20, and cladding region 14 (including inner cladding region 24, moat region 26, and outer cladding region 28). Corresponding locations in preform 50 may be described as "portions," such as an inner core portion corresponding to inner core region 16, an outer core portion corresponding to outer core region 24, and cladding portion 14 corresponding to cladding region 14. Further, an inner cladding portion corresponds to inner cladding region 24, a moat portion or depressed-index cladding portion corresponds to moat region 26, and an outer cladding region corresponds to outer cladding region 28.
[0045] To form the preform 50, multiple layers of silica soot are deposited on a mandrel 114 via a soot burner 112 to form an initial or core silica soot tube 110 (step 60). The soot tube 110 defines a central passage 116 extending along the length of the soot tube 110. The resulting soot tube 110 is dried using a chlorine drying technique (e.g., exposure to Cl2) (step 62). The soot tube 110 is then treated with fluorine by exposing the porous soot tube 110 to a fluorine-containing atmosphere (e.g., fluorine sweep with a fluorine doping precursor such as SiF4) for a time and temperature sufficient to remove most or all of the chlorine remaining from the drying step (e.g., step 62) (step 64). The intent of the fluorine treatment of the soot tube 110 is to remove the chlorine so that interaction with the chlorine does not contribute to devitrification of the glass. Exposure to the fluorine-containing atmosphere may be accomplished at a temperature below 1100° C. to avoid doping the soot tube 110 with high levels of fluorine. However, the fluorine treatment may introduce low levels of fluorine into the soot tube 110. Small levels of fluorine may also help lower the fictive temperature of the glass without adversely affecting the concentration fluctuation contribution to Rayleigh scattering.
[0046] The fluorine doped soot tube 110 is then sintered and densified into a densified tube 118 (step 66). In various examples, the soot tube 110 contains about 0.1% to about 0.4% fluorine by weight after densification. In certain embodiments, the densified tube 118 can be drawn into a series of smaller densified tubes 118. The densified tubes 118 or the resulting smaller tubes 118 are each assembled with a handle 120 and transferred from the mandrel 114 to a rotating lathe located near a heat source 122. The rotating lathe can be a glass processing lathe or a modified chemical vapor deposition (MCVD) glass forming lathe. The handle 120 can be a glass handle 120 that becomes an integral part of the preform 50. The handle 120 provides a support structure for subsequent processing steps. The handle 120 is coupled to a lathe such that the handle 120 , and therefore the densification tube 118 , is rotated and moved relative to the soot burner 112 .
[0047] The densification tube 118 defines an annular reservoir 130 for containing an alkali metal doping material 132. The material is formed of oxygen (O2) and an alkali salt, which is introduced into the annular reservoir 130. The alkali metal source compound 132 includes at least one of K, Na, Li, Cs, Rb, Br, I, and F. The alkali metal source compound 132 can be at least one of KBr, KI, and KNO3. The alkali metal oxide diffused into the densification tube 118 can be KO, Na2O, LiO2, Rb2O, and Cs2O. The annular reservoir 130 is formed near one end of the densification tube 118 by forging two annular neck-like deformations in the wall of the densification tube 118 by flame processing or by welding the annular reservoir 130 to the densification tube 118. The densification tube 118 has a central passage 116 to allow diffusion along the length of the soot tube 110 .
[0048] An alkali metal source compound 132 is introduced into the central passage 116 of the densification tube 118 in a reservoir 130 and heated by a heat source 122 to form a vapor as the densification tube 118 rotates in a lathe (step 68). The alkali halide precursor vaporizes and flows through the densification tube 118 (e.g., a substrate tube). A carrier gas, such as oxygen (O2), flows through a rotating seal 136 into an inlet 134 of the densification tube 118. In FIG. 8, the handle 120 is considered to be located to the right (off page) at the opposite end of the densification tube 118 compared to the inlet 132. The gas travels from the inlet 134 toward the opposite end of the densification tube 118, referred to as the downstream portion 138. The downstream portion 138 of the densification tube 118 is heated to promote diffusion of the alkali metal oxide or alkali metal to the inner surface 140 of the densification tube 118.
[0049] In certain embodiments, the dopant can be KO. O can flow over the KI and form gas phase KO, which is carried downstream to dope the densification tube 118. More preferably, K is the dopant and K is deposited and diffused into the densification tube 118. This process can be faster than deposition of KO and therefore can be a preferred method for doping the densification tube 118 with a selected alkali weight percentage. The downstream portion 138 of the densification tube 118 should be heated to a temperature sufficient to promote rapid diffusion of the alkali metal oxide or alkali metal to the inner surface 140 and prevent devitrification of the densification tube 118. For example, the downstream portion 138 of the densification tube 118 can be heated to a temperature of about 1500° C. to about 2000° C.
[0050] A heat source 122 is traversed along the length of the densified tube 118 to form a mobile hot spot to diffuse alkali metal oxide into the densified tube 118. The alkali metal oxide may diffuse from the inner surface 140 to a depth of about 100 μm to 500 μm to form an alkali-doped densified tube 150. The concentration of the diffused alkali metal oxide dopant generally varies radially, with a higher concentration (wt%) in the inner half 152 and a lower concentration in the outer half 154. A vacuum is pulled on the alkali-doped densified tube 150 and heat is increased to relax or partially collapse the alkali-doped tube 150. The alkali-doped densified tube 150 may be cut into base material ingots 156 for further processing.
[0051] To prevent crystallization of alkali metals or alkali halides (e.g., KCl), it may be advantageous for the alkali-doped densified tube 150 and any additional soot deposited thereon to be substantially chlorine-free. Substantially chlorine-free generally means exhibiting a sufficiently low chlorine content so that optical losses due to alkali chlorine are generally avoided. For example, the chlorine content in the alkali-doped densified tube 150 may be about 500 ppm by mass (about 500×10 -6 %), about 100 ppm (about 100 x 10-6 %) or less than about 50 ppm (about 50 x 10 -6 %). The crystalline phase may be crystallobolite, which is a silica phase, and the alkali metal aids in crystal formation by reducing viscosity. However, other crystallizations may form without departing from the teachings herein.
[0052] It may be advantageous for the alkali-doped densified tube 150 and any additional soot deposited thereon to be substantially free of "water." As described herein, "water" refers to hydroxyl groups OH. Water is generally associated with a water peak (i.e., an absorption peak due to hydroxyl groups) centered at or near about 1383 nm. This absorption peak may extend into the operating wavelength region of the optical fiber 10 (e.g., 1310 nm or 1550 nm) and therefore may have a negative effect on the attenuation of the optical fiber 10. In general, it is advantageous to reduce the water peak by reducing the OH content of the glass. For example, the alkali-doped densified tube 150 may have a water content of about 100 ppm by mass (about 100×10 -6 %). To remove the "water" from the densified tube 150, a chlorine drying technique may be utilized.
[0053] The alkali-doped densified tube 150 may be etched with an etchant such as an aqueous HF solution (step 70). The etchant may remove a depth of silica from the interior surface of the alkali-doped densified tube 150 to remove or reduce impurities that may have diffused through the interior surface of the densified tube 150 during alkali doping and / or densification. It is also contemplated to use fluorine gases such as CF4, SF4, NF3, C2F6, or combinations thereof as the etchant. The depth of silica removal may depend on the processing conditions during the diffusion and collapse process. It may be advantageous to remove to a depth of about 5% of the total diffusion depth of the alkali metal oxide.
[0054] Once the etching process is complete, the alkali-doped densified tube 150 is further heated to completely collapse the alkali-doped densified tube 150 downstream of the alkali metal source compound 132, closing the central passage 116 and forming a cylinder of glass referred to herein as a core rod 160 (step 72). The core rod 160 is a solid alkali-doped glass body that is separate from the portion of the alkali-doped densified tube 150 that contains the annular reservoir 130. The core rod 160 at least partially forms the central core portion of the preform 50, which corresponds to the central core region 16 in the resulting optical fiber 10 obtained after drawing the preform 50. The core rod 160 may be resized by redrawing. Additionally, the core rod 160 may be etched to remove some or all of the hydrated glass or hydroxyl groups that may have been formed by the heat source (e.g., a torch) during the collapse process. However, if a dry heat source, such as an induction or resistance heater, a plasma torch, or a dry heat source using a non-hydrogen containing fuel (e.g., CO), is used for the collapse process, additional etching may not be necessary. The dry heat source can minimize rewetting (e.g., OH resorption and / or diffusion) of the densified tube 150 without supplying or generating H, OH, or HO, thereby reducing decay.
[0055] The core rod 160 is generally the final product of the first stage 42 of the manufacturing method 40. The core rod 160 is then utilized as the initial product of the second stage 44, which forms the outer core portion of the preform 50, corresponding to the outer core region 20. Using the soot burner 112, multiple layers of porous silica soot are deposited onto the core rod 160 to form a porous core soot blank 162 (step 74). The soot may be deposited onto the core rod 160 using an outside vapor deposition (OVD) method. Generally, a flame is emitted from the soot burner 112. A silica precursor gas-vapor mixture is oxidized or combusted within the flame to form a silica-containing soot flow toward the core rod 160.
[0056] The core rod 160 is moved multiple times relative to the soot burner 112 to cause a layer build-up of silica soot-containing layers to form a soot coating, thereby forming a porous core soot blank 162. The translational motion is generally accomplished by moving the soot burner 112 relative to the core rod 160, although the core rod 160 may be moved relative to the soot burner 112 without departing from the teachings herein. Alternatively, both the soot burner 112 and the core rod 160 may be moved. The soot coating forms at least a portion of the core 12 (e.g., the outer radial portion of the inner core region 16 or the outer core region 20), may also include a portion of the cladding 14 (e.g., the inner cladding region 24) of the optical fiber 10 drawn from the preform 50, and may be formed substantially of pure silica.
[0057] The porous core soot blank 162 is dried using chlorine drying techniques and heat (step 76). The porous core soot blank 162 is then treated with fluorine by exposing the porous core soot blank 162 to a fluorine-containing atmosphere for a time and at a temperature sufficient to remove most or all of the chlorine remaining from the drying step (e.g., step 76) (step 78). The fluorine-containing atmosphere may include a fluorine doping precursor, such as SiF4 or CF4, which may introduce low levels of fluorine as a dopant into the porous regions of the porous core soot blank 162.
[0058] The fluorine-treated soot blank 162 is then sintered and densified by heating to form a core cane 164 (step 80). This process generally forms the core portion of the preform 50, which forms the core 12 having both the central core region 16 and the outer core region 20 of the optical fiber 10 drawn from the preform 50. The core cane 164 is redrawn (heated and sized to a smaller diameter) and cut as necessary to form a core cane 166 (step 82) for processing in the third stage 46. Additional core layers can be added to produce a core cane 164 / 166 having three or more core regions, with the core cane 164 / 166 including at least one core region and at least one cladding region, without departing from the teachings herein.
[0059] The third stage 46 of the method 40 forms the moat portion of the preform 50 that forms the trench or moat 26 of the cladding region 14, and may optionally produce the inner cladding region 24 of the cladding region 14 of the optical fiber drawn from the preform 50. The core cane 166 produced in the second stage 44 of the method 40 is utilized as the initial product of the third stage 46 of the method 40. The core cane 166 is further processed to add additional glass layers, thereby ultimately forming the depressed-index cladding region or moat 26 (step 84). A soot burner 112 is utilized to deposit multiple layers of soot onto the core cane 166 to form a subsequent porous clad soot blank 170. The resulting porous clad soot blank 170 is dried using a chlorine drying technique (step 86). The porous clad soot blank 170 is doped with a downdopant for moat reduction (step 88), preferably in a clad doping atmosphere containing a fluorine doping precursor such as SiF4 or CF4. In various examples, the porous clad soot blank 170 is exposed to the fluorine doping precursor at about 1225° C. for about 60 minutes to 120 minutes. In certain embodiments, the clad doping atmosphere also includes SiCl4, which can be advantageous for reducing attenuation of the resulting optical fiber 10, as discussed further herein.
[0060] The fluorine doped porous clad soot blank 170 is then sintered and densified by passing it downstream through a high temperature zone at about 1450° C. to about 1500° C. at about 7-10 mm / min to form a clad cane 172 (step 90). Densification may be performed in the presence of a non-carbon reducing agent, such as SiCl4. In various examples, the reducing agent SiCl4 is present throughout the densification process when the preform 50 becomes fully porous. Alternatively, the SiCl4 may be present in a range of temperatures up to about 100° C. to about 1500° C. to form a clad cane 172. 3 , 1.7g / cm 3 , 1.8g / cm 3 , or 1.9 g / cm 3) after which the presence of SiCl4 may be optional. Densification of the clad cane 172 is generally performed in the absence, or at a minimal level, of the fluorine doping precursor used to form the moat 26 in the clad region 14.
[0061] In certain embodiments, the fluorine doping precursor may be actively pumped out of the environment. Alternatively, the supply of the fluorine doping precursor may be stopped. The fluorine doping precursor is reduced to minimal or trace levels during densification of the clad cane 172.
[0062] The reducing agent may be utilized at one or two steps during the manufacturing process, including when exposing the porous clad soot blank 170 to a fluorine doping precursor (step 88), when densifying the porous clad soot blank 170 into a clad cane 172 (step 90), or both steps. The porous clad soot blank 170 and / or the clad cane 172 are exposed to a non-carbon reducing agent (e.g., SiCl4) to control the oxidation state. The SiCl4 is included in a reducing gas environment having a predetermined concentration of the non-carbon reducing agent. In various examples, the concentration of the non-carbon reducing agent ranges from about 0.1% to about 15% by volume of the total reducing gas environment during these processes. In additional examples, the concentration of the non-carbon reducing agent ranges from about 0.5% to about 10% by volume of the gas environment. The SiCl4 may be introduced into the gas environment during the fluorine doping process (step 88), during the sintering process (step 90), or during both the fluorine doping and sintering processes (steps 88, 90). In certain embodiments, if preform 50 becomes fully porous, treatment with SiCl4 may be more effective during sintering process 90. Clad cane 172 is preferably redrawn to a predetermined diameter into clad cane 174 (step 92) for use in overclad and fourth stage 48 of manufacturing method 40, as discussed further herein.
[0063] The use of the reducing agent SiCl4 in the third stage 46 helps control the oxidation state of the glass forming the moat 26. However, the use of SiCl4 during moat formation can be counterproductive to downdoping with fluorine because, when incorporated as a dopant, Cl acts as an updopant and counters the index reducing effect of F. The conditions under which SiCl4 is used in the third stage 46 are controlled such that SiCl4 controls the oxidation state (by acting as a reducing agent) without substantially introducing Cl as a dopant and thus affecting the relative refractive index profile of the resulting optical fiber 10. In certain embodiments, the concentration of SiCl4 in the gas environment during the sintering process (step 90) is between about 0.25 mol % and about 6 mol %. In additional examples, the concentration of SiCl4 in the gas environment during the sintering process (step 90) is between about 0.25 mol % and about 4 mol %. In further examples, the concentration of SiCl4 in the gas environment during the sintering process (step 90) is between about 1 mol % and about 3 mol %.
[0064] 5 and 6, and with further reference to FIG. 9, moat formation in the third stage 46 of the manufacturing process may introduce defects that alter various properties of the resulting optical fiber 10. Under certain operating conditions, the intensity distribution of the guided optical signal extends to the moat 26, and defects at the moat 26 may interact with the optical signal, increasing the attenuation of the guided optical signal. The presence of defects at the moat 26 may also interact with components present in the optical fiber's deployment environment (e.g., surrounding coatings or cables, or the external atmosphere) over time, resulting in time changes in the attenuation of the optical signal (referred to herein as "aging").
[0065] A common constituent known to be present in optical fiber deployment environments is hydrogen. Optical fibers 10 having alkali-doped cores are utilized in terrestrial and submarine networks due to their inherently low attenuation of optical signals. However, over time during use in the field, such optical fibers 10 may become susceptible to hydrogen aging if oxygen-rich hydrogen aging defects are formed during fiber processing. Hydrogen aging occurs when hydrogen interacts with oxygen-rich hydrogen aging defects to form defects (e.g., hydroxyl radicals) that cause certain wavelengths of light to be absorbed, thus increasing the attenuation of the optical fiber 10 at those wavelengths. Typically, known oxygen-rich hydrogen aging defects have the properties of a hydro-I response, i.e., the concentration of oxygen-rich hydrogen aging defects continues to grow with time with a scaling factor of log(time). It would be advantageous to change the oxidation state of the optical fiber 10 to significantly reduce the concentration of oxygen-rich hydrogen aging defects in the optical fiber 10, thereby reducing the prevalence of oxygen-rich hydrogen aging defects and the hydrogen aging sensitivity of the optical fiber 10, or to create hydrogen aging insensitivity of the optical fiber 10.
[0066] The optical fiber 10 is periodically tested for hydrogen aging. In the hydrogen aging test used herein, the optical fiber 10 is exposed to a gas atmosphere containing H2 at 23°C for a predetermined period of time. The gas atmosphere includes H2 in the presence of an inert gas. For the purpose of testing hydrogen aging in this disclosure, the H2-containing gas atmosphere is at a total pressure of 1.0 atm (101325 Pa) and includes a hydrogen (H2) gas partial pressure of 0.01 atm (1013.25 Pa) and a nitrogen (N2) gas partial pressure of 0.99 atm (100311.8 Pa). During the hydrogen aging test, light of various wavelengths is introduced into the optical fiber 10 and the change in attenuation as a function of exposure time to the H2-containing gas atmosphere is monitored relative to the initial attenuation of the optical fiber 10 before exposure to the H2-containing gas atmosphere.
[0067] For example, one wavelength of interest for communications applications is 1383 nm. This wavelength is monitored in the hydrogen aging test disclosed herein. The time elapsed from exposure of the optical fiber 10 to an H2-containing gas to the time when the onset of an increase in absorption at 1383 nm occurs is referred to herein as the 1383 nm "Time to Peak" (or "Time-to-Peak") value (which may be abbreviated herein as TTP). The significance of this measurement is that, as described herein, when exposed to H2 for an extended period of time, such as one week, reactive oxygen centers of oxygen-rich hydrogen aging defects in the optical fiber 10 react with hydrogen to form -OH species (e.g., silanol groups) that absorb light at typical communications wavelengths and have an absorbance maximum at about 1383 nm. The formation of absorbing -OH species upon exposure of the fiber to hydrogen gas over time is a process referred to herein as hydrogen aging.
[0068] In one test example, four single mode optical fibers having a diameter of 125 μm were produced by forming and drawing each fiber from a different preform to test hydrogen aging. Each preform was formed by forming a core cane, forming cladding soot on the core cane, and densifying the cladding soot. The densification of the cladding soot included an isothermal first stage in which the cladding soot was exposed to a first process gas containing Cl2 at a temperature of about 1150° C. for about 240 minutes to dry the cladding soot, and a second stage in which the cladding soot was exposed to a second process gas at a temperature of about 1150° C. to about 1500° C. for about 6 hours. The four preforms from which the four fibers were drawn were produced in substantially the same manner, except that the process gases for the first and second stages for each of the four preforms contained different concentrations of Cl2 and CO (the remaining gases included helium) as shown in Table 1 below. Each of the fibers in Table 1 includes a germania-doped core, a silica inner cladding, a fluorine-doped trench, and a chlorine-doped outer cladding. In comparison, each layer of the optical fiber 10 of the present disclosure is doped with fluorine except for about the inner 30% of the core 12, and the fiber 10 is alkali doped. The fibers in Table 1 are similar in structure but different in composition from the present fiber 10.
[0069] [Table 1]
[0070] Each of the four fibers was exposed to a gas atmosphere at 23° C. with a total pressure of 1 atm (101325 Pa) containing a partial pressure of H2 of 0.01 atm (1013.25 Pa) and a partial pressure of N2 of 0.99 atm (100311.8 Pa). The time for hydrogen to diffuse through the fiber cladding to the fiber core under these conditions was measured in terms of the TTP for each fiber. The TTP was measured based on the time dependence of the attenuation of an optical signal having a wavelength of 1383 nm and corresponds to the time after the fiber was exposed to the H2-containing gas at which a sharp increase in attenuation was observed. For exposure times below the TTP, essentially no change in attenuation was observed at 1383 nm. For exposure times equal to the TTP, the onset of an increase in attenuation was observed at 1383 nm. For exposure times above the TTP, a significant increase in attenuation was observed at 1383 nm. The fiber drawn from preform #1 had an average TTP at 1383 nm of about 105 hours. The fiber drawn from preform #2 had an average TTP at 1383 nm of about 76 hours. The fiber drawn from preform #3 had an average TTP at 1383 nm of about 58 hours. The fiber drawn from preform #4 had an average TTP at 1383 nm of about 40 hours. This test method can be used to determine the TTP of fibers, including fiber 10 disclosed herein, using a non-carbon reducing agent such as SiCl4.
[0071] A low TTP value (short TTP time) means a low concentration of oxygen-rich hydrogen aging defects in the cladding region of the optical fiber. Hydrogen from the gas atmosphere contacts the optical fiber at the outer surface and diffuses radially inward through the cladding to the core. If hydrogen encounters an oxygen-rich defect in the cladding as it diffuses, it reacts with the defect to form a hydroxyl group and diffusion stops. The oxygen-rich hydrogen aging defects closest to the outer surface of the optical fiber are converted to hydroxyl groups at the initial exposure time. Upon formation of the hydroxyl group, the oxygen-rich hydrogen aging defect is neutralized, and subsequent exposure of the optical fiber to the H2-containing gas atmosphere allows hydrogen to diffuse to the oxygen-rich hydrogen aging defects located further away from the surface and closer to the core. As the exposure time increases, the hydroxyl groups form even closer to the core. At short exposure times, the hydroxyl groups are too far away from the core to interact with the optical signal, and no increase in attenuation is observed. At a sufficiently long exposure time, OH groups form close enough to the core region (e.g., in the core region itself or in a portion of the cladding region close enough to the core region) to interact with the optical signal (e.g., by absorption) and cause attenuation of the optical signal. The TTP indicates the exposure time at which the forming OH groups are close enough to the core to begin to interact with the optical signal. A low TTP suggests that the OH groups have a short time to form close enough to the core to interact with the optical signal, which is consistent with a low concentration of oxygen-rich defects in the core region.
[0072] To prevent such aging and absorption, which results in a decrease in the transmission signal strength, the optical fiber can be treated with a reducing agent to reduce aging and absorption. One conventional approach is to treat the optical fiber with deuterium gas to form -OD species from reactive oxygen centers, such as oxygen-rich hydrogen aging defects, present in the fiber. Unlike -OH, -OD does not absorb at 1383 nm. When using deuterium gas, oxygen leakage is also tightly controlled during the drawing process of the resulting fiber. D2 treatment is performed on the fiber after the drawing process is completed, and not during the drawing itself. However, deuterium gas is expensive, and it is desirable to identify other methods to improve hydrogen aging.
[0073] A second conventional method for reducing oxygen-rich hydrogen aging defects involves exposing the optical fiber preform to carbon monoxide (CO) as a reducing agent during densification (or doping), as illustrated in the previous example associated with Table 1. Carbon monoxide, however, results in an absorption peak in the L-band portion of the communications spectrum, generally at or near 1583 nm, and to a lesser extent, in the C-band portion of the communications spectrum, generally at or near 1547 nm. Absorption wavelengths in the C-band and L-band spectra adversely affect the performance of the optical fiber 10, particularly in the L-band spectrum. When CO is used as the reducing agent, CO2 may form in the fiber and affect attenuation. The absorption peak at 1583 nm occurs when CO is used as the reducing agent and may result from CO or from other structural effects in the silica caused by carbon or CO. The absorption peak at 1583 nm affects the overall performance of the resulting fiber.
[0074] The method 40 disclosed herein utilizes a non-carbon based reducing agent during moat formation in the manufacturing process to reduce oxygen-rich hydrogen aging defects in the optical fiber 10. The non-carbon based reducing agent is SiCl4. Use of the non-carbon based reducing agent reduces (1) the water peak, typically at a wavelength of about 1383 nm, (2) the attenuation in the C-band spectrum, typically at a wavelength of about 1547 nm, and (3) the attenuation in the L-band spectrum, typically at a wavelength of about 1583 nm. Use of the non-carbon based reducing agent reduces or avoids oxygen-rich hydrogen aging defects without forming carbon dioxide CO2, thereby reducing or eliminating undesirable absorption peaks in the L-band and / or C-band. Additionally, the optical fiber 10 produced via the method 40 herein has a TTP at 1383 nm of less than 100 hours at 23° C. upon exposure to an H2-containing gas atmosphere having a total pressure of 1 atm (101325 Pa) and including an H2 partial pressure of 0.01 atm (1013.25 Pa) and an N2 partial pressure of 0.99 atm (100311.8 Pa). The TTP is determined using the method described herein in connection with Table 1. As previously stated, a low TTP value means that the optical fiber has a low concentration of oxygen-rich hydrogen aging defects in the cladding region.
[0075] As previously mentioned, the third stage 46 of the manufacturing process involves doping the porous clad soot blank 170 with fluorine to form the trench inner cladding region (e.g., moat 26) of the profile of the optical fiber 10 (e.g., step 136). Generally, the moat index is lower than the index of the core 12. There is sufficient power in the trench region or moat 26 that defects in the moat 26 generally contribute to the aging behavior of the optical fiber 10. When the optical fiber 10 is exposed to hydrogen, absorption peaks at or near 1383 nm and 1550 nm are formed if no reducing agent is used. Conventional methods using CO to reduce oxygen-rich hydrogen aging defects can result in CO2 formation or other contaminating or structural effects in the optical fiber 10, causing absorption peaks at or near about 1583 nm in the L-band and to a lesser extent about 1547 nm in the C-band, as illustrated in FIG. 9.
[0076] In the process disclosed herein, SiCl4 interacts with the porous cladding soot blank 170 to reduce or eliminate oxygen-rich hydrogen aging defects in the optical fiber 10 without forming carbon dioxide CO2 or other residual contaminating or structural effects associated with CO. As a result, the absorption peak at or near 1583 nm is avoided, resulting in reduced attenuation in the L-band transmission spectrum. SiCl4 renders the optical fiber 10 insensitive to hydrogen aging, or at least reduces its sensitivity, while simultaneously reducing or eliminating the absorption peaks in the C-band and L-band that are known to arise when CO is used as the reducing agent.
[0077] When SiCl4 is used as a reducing agent rather than a carbon-based reducing agent, no absorption peaks are formed in the C-band and L-band. Additionally, SiCl4 also assists in the reduction of water, i.e., SiOH, within the optical fiber 10. The use of SiCl4 eliminates the absorption peaks at or near about 1583 nm and 1547 nm, and reduces the water peak at or near about 1383 nm.
[0078] The use of SiCl4 during processing produces optical fiber 10 with low attenuation at or near 1383 nm, 1547 nm, and 1583 nm, respectively. Due to exposure to SiCl4 during formation of moat 26, optical fiber 10 exhibits less than 0.16 dB / km attenuation at 1583 nm and less than 0.0005 dB / km incremental peak or attenuation above a baseline at 1583 nm. In certain embodiments, optical fiber 10 may exhibit less than 0.0005 dB / km incremental attenuation above a baseline at 1583 nm due to CO2 absorption. The baseline is a best fit attenuation across the C-band and L-band excluding the wavelength range centered around 1583 nm. The best fit attenuation is a function of wavelength from about 1530 nm (e.g., the lower limit of the C-band) to about 1625 nm (e.g., the upper limit of the L-band), excluding the range from about 1570 nm to about 1590 nm. The baseline considers no absorption at 1583 nm, producing a smooth curve over wavelengths from 1550 nm to 1625 nm, in accordance with standard spectroscopic measurements.
[0079] Additionally, the attenuation may be monotonically increasing from about 1570 nm to about 1600 nm, or may be monotonically increasing from about 1570 nm to about 1590 nm. Monotonically increasing attenuation is a property of the SiCl4-treated optical fiber 10 that is not present in the comparative CO-treated optical fiber. Additionally or alternatively, the optical fiber 10 may exhibit less than 0.16 dB / km attenuation at 1583 nm and less than 0.0003 dB / km incremental attenuation above the baseline at 1583 nm. Additionally, the optical fiber 10 exhibits less than 0.5 dB / km attenuation at 1383 nm.
[0080] The third stage 46 of the manufacturing process, forming the moats, affects the overall performance of the resulting optical fiber 10. Exposure to a non-carbon reducing agent reduces the attenuation of the optical fiber 10, improving the performance of the optical fiber 10. The use of SiCl4 reduces attenuation in both the C-band and L-band spectra, thereby improving the optical transmission and overall performance through each of these regions.
[0081] Referring again to FIGS. 5 and 6 and FIG. 10, when the clad cane 174 is incorporated into the preform 50, the heating that occurs during the drawing process of the preform 50 causes the alkali metal oxide concentration to diffuse deeper into the clad cane 174. The diffusion of the alkali metal oxide is at least partially dependent on the temperature of the doped glass. The diffusion of the alkali metal oxide can be controlled by the drawing process. By varying the drawing conditions (e.g., the temperature used to draw the optical fiber 10 from the preform 50), the concentration of the alkali metal oxide can be distributed within the preform 50 with a predetermined concentration profile. In various examples, the relationship between the radius r and the alkali metal concentration is generally linear. Thus, the amount of time the preform 50 remains at a selected temperature is a factor in the diffusion of the alkali metal oxide and the concentration profile of the alkali metal oxide in the core and cladding regions of the optical fiber 10. The time and temperature to which the clad cane 174 drawn from the final preform 50 and the resulting optical fiber 10 are exposed during the draw process are controlled by varying the draw process by controlling the draw speed and temperature of the draw furnace. For example, increasing the draw speed reduces the time of a particular portion of the optical fiber 10 in the draw furnace 180 (FIG. 11), which in turn reduces the distance that the alkali metal oxide dopant diffuses within the core and / or cladding regions of the preform 50. This may result in less alkali metal oxide diffusing into the cladding 14, and therefore a higher concentration of alkali metal oxide in the core 12 of the optical fiber 10 formed by drawing the preform 50.
[0082] Conversely, decreasing the draw speed may increase this time, thereby allowing the alkali metal oxide to diffuse further into the cladding 14 of the optical fiber 10, thereby decreasing the concentration of alkali metal oxide in the core 12 of the optical fiber 10. Additionally, increasing the temperature of the draw furnace may increase the diffusion rate, decreasing the concentration of alkali metal oxide in the core 12 and increasing the concentration of alkali metal oxide in the cladding.
[0083] 5 and 6, after the depressed-index cladding region 26 is formed in the third stage 46 of fabrication, the outer cladding region 28 is formed in the fourth stage 48. A soot layer is laid down on the clad cane 174 utilizing a soot burner 112 to form a porous overclad soot blank 190 (step 94). The resulting porous overclad soot blank 190 is dried using a chlorine drying technique (step 96). The porous overclad soot blank 190 is doped with a fluorine doping precursor such as SiF4 (step 98) to include a depressed-index cladding region. The use of SiCl4 is generally counterproductive to downdoping with fluorine, so the porous overclad soot blank 190 is exposed to the fluorine doping precursor in the absence or at a minimal level of the reducing agent SiCl4.
[0084] The outer cladding region 28 generally has a lower refractive index than the core 12 and a higher refractive index than the moat 26. In various examples, the doping of the outer cladding region 28 is sufficient to achieve a relative refractive index delta % between the maximum of the core 12 and the minimum of the cladding 14, for example, from about 0.3% to about 0.4%. In the outermost cladding layer (e.g., the outer cladding region 28), the weight % of fluorine may be slightly less, from about 0.1% to about 0.5% by weight, to achieve a relative refractive index within a preferred range and minimize the effects of stresses that arise when drawing optical fiber from the preform 50. The fluorine-doped porous overclad soot blank 190 is then sintered and densified to form the preform 50 (step 100).
[0085] The preform 50 created by the various steps 42, 44, 46, 48 is drawn 102 into an optical fiber 10 having selected dimensions and properties. The method 40 described herein produces an alkali-doped silica optical fiber 10 having an attenuation at 1583 nm of less than 0.16 dB / km and an incremental attenuation at 1583 nm of less than 0.0005 dB / km above a baseline, and an attenuation at 1547 nm of less than 0.16 dB / km and an incremental attenuation at 1547 nm of less than 0.0003 dB / km above a baseline, after exposure to an H2-containing atmosphere containing 1% H2 by volume and 99% N2 by volume at 23° C. for one week. Additionally, the optical fiber 10 resulting from drawing the preform 50 produced from the method 40 exhibits an attenuation at 1383 nm of less than 0.5 dB / km.
[0086] With further reference to FIG. 5, and FIGS. 11 and 12, the redraw process described herein may be performed by a draw system 200. The handle 120 is attached to the cane 164, 172 by steps described herein. Depending on the stage of the manufacturing process, the core cane 164 or clad cane 172 is attached to a movable downfeed support above a draw furnace 180. The furnace 180 generally includes a heating element 202 and a muffle 204 that is heated to a selected temperature. A sacrificial glass rod 206 may be coupled to the end of the cane 164, 172 and may be pulled by a motor-driven tractor 208 to draw the cane 164, 172 at a selected rate. The draw speed or draw rate may be adjusted based on a sensor 210 that measures the diameter d of the cane 164, 172. The cane 164, 172 is drawn to a smaller diameter d until the cane 164, 172 is at the selected diameter.
[0087] The final drawing process (step 102) of drawing the preform 50 into the optical fiber 10 is performed in a similar manner (FIG. 12). The preform 50 is positioned approximately vertically in the drawing furnace 180. The muffle 204 is heated to a temperature range of about 1700° C. to about 2100° C. The optical fiber 10 is drawn from the heated preform 50 in the form of a bare optical fiber 10 (e.g., not coated with a polymer-based material). After leaving the muffle 204, the optical fiber 10 may encounter a sensor 214 for monitoring the diameter d. The sensor 214 may provide feedback to the controller 212 for a feedback control loop to adjust the speed of the puller 208 to keep the diameter d of the optical fiber 10 substantially constant. It is also contemplated that the optical fiber 10 may be drawn by a tension monitoring device 216 to monitor the tension of the optical fiber 10. The tension monitoring device 216 may also be in communication with the controller 212 to adjust the drawing tension of the optical fiber 10.
[0088] The draw system 200 may include a cooling system 218. Once the optical fiber 10 is drawn from the preform 50, the optical fiber 10 may be cooled in a cooling tube or another device. The cooling system 218 may be coupled to an outlet of the furnace 180, or alternatively, may be remote therefrom. The optical fiber 10 may then be coated by a coating system 220, which may apply a polymer-based coating material to an outer surface of the optical fiber 10. It is also contemplated that the coated optical fiber 10 may pass through a coating curing device within the coating system 220. The coated optical fiber 10 may be wound onto a reel or spool 222.
[0089] The line drawing system 200 is illustrated as having a controller 212, which may have a microprocessor or processor 224, memory 226, and other control circuitry. The memory 226 may store instructions 228 executable by the processor 224. It is contemplated that any digital and / or analog processing circuitry and memory storage medium may be used.
[0090] The controller 212 can modify the manufacturing process, such as by adjusting the draw speed of the draw system 200, modifying the temperature of the furnace 180, and / or modifying the draw tension applied to the optical fiber 10. The draw system 200 can utilize various drawing mechanisms and / or pulleys to provide a selected draw tension to the optical fiber 10 as it is drawn by the draw system 200.
[0091] 13 and 14, the method 40 disclosed herein can be used to create cores 12 that are ultimately drawn into different alkali-doped optical fibers 10 with different properties. The refractive index profile 240 as illustrated in FIG. 13 is a first cane profile before final drawing, and the refractive index profile 242 as illustrated in FIG. 14 is a second cane profile measured before final drawing. Furthermore, the refractive index profile 242 in FIG. 14 is in fiber space where the outer radius of the fiber 10 is about 62.5 μm. The profile 242 in normalized (e.g., normalized to the maximum outer radius) radius space is generally similar in the preform 50 and fiber space, with some variation due to alkali diffusion and stress optical effects. The method 40 disclosed herein can be used to form both preforms 50 and optical fibers 10, which are different products with different properties.
[0092] 1-14, a method 40 disclosed herein produces an optical fiber 10 having selected characteristics, such as reduced attenuation at various wavelengths, a selected TTP, and a selected relative refractive index. The optical fiber 10 includes a core 12 doped with an alkali metal oxide. The core 12 has an alkali metal oxide concentration between 0.5% and 1.5% by weight. The cladding 14 surrounds the core 12 and includes a moat 26 and an outer cladding region 28. The moat 26 has a first fluorine concentration and may have a first chlorine concentration. The moat 26 has a relative refractive index Δ3 and a minimum relative refractive index Δ 3min is in the range of about -0.80% to about -0.30%. Due to this concentration difference, generally, moat 26 has a lower relative refractive index than outer cladding 28. Outer cladding region 28 has a second fluorine concentration, which is generally lower than the first fluorine concentration. Outer cladding region 28 may have a second chlorine concentration, which may be lower than the first chlorine concentration. Outer cladding region 28 has a Δ4-Δ 3min >0.05%. The lower chlorine concentration in the outer cladding 28 typically results from the use of SiCl4 during the moat formation process, but the outer cladding region 28 is not exposed to SiCl4.
[0093] Additionally, optical fiber 10 has a TTP hydrogen aging value of less than 100 hours upon exposure at 23° C. to an H2-containing gas atmosphere having a total pressure of 1 atm (101325 Pa) and including an H2 partial pressure of 0.01 atm (1013.25 Pa) and an N2 partial pressure of 0.99 atm (100311.8 Pa). Additionally, due to exposure to SiCl4 during formation of moat 26, optical fiber 10 exhibits an attenuation of less than 0.16 dB / km at 1583 nm and an incremental attenuation of less than 0.0005 dB / km above a baseline at 1583 nm. Additionally or alternatively, optical fiber 10 may exhibit an attenuation of less than 0.16 dB / km at 1547 nm and an incremental attenuation of less than 0.0003 dB / km above a baseline at 1547 nm. For example, optical fiber 10 exhibits less than 0.16 dB / km attenuation at 1547 nm and less than 0.0003 dB / km incremental attenuation above a baseline at 1547 nm. Additionally, optical fiber 10 may exhibit less than 0.5 dB / km attenuation at 1383 nm. It is contemplated that a cathodoluminescence or 240 nm absorption measurement process may be utilized to determine whether preform 50 was made by method 40.
[0094] Currently, optical fiber 10 can transmit at wavelengths of about 1550 nm and / or about 1580 nm. Communications techniques may use wavelength division multiplexing, allowing multiple wavelength channels to be located on the same optical fiber 10. In such configurations, both the C-band and L-band transmission spectra can be utilized. Removal of absorption peaks from the L-band spectrum reduces attenuation in the L-band, resulting in improved performance of the optical fiber 10. The method 40 disclosed herein reduces attenuation while mitigating absorption peaks at or near 1547 nm and 1583 nm, as well as the water peak at or near 1383 nm.
[0095] Use of the disclosed process provides various advantages. For example, the non-carbon reducing agent reduces water (OH) formation and contaminant or structural defects associated with carbon-containing reducing agents in the optical fiber 10. Additionally, the non-carbon reducing agent can be SiCl4, which reduces the formation of SiOH in the optical fiber 10, thereby lowering the water peak. Additionally, the use of SiCl4 reduces or avoids absorption peaks in the C-band at or near about 1547 nm and the L-band at or near about 1583 nm. Additionally, the use of SiCl4 reduces attenuation, which positively impacts the performance of the optical fiber 10. Additionally, the non-carbon reducing agent reduces or eliminates oxygen-rich hydrogen aging defects in the optical fiber 10, thereby lowering attenuation. Additional benefits or advantages may be realized and / or achieved.
[0096] The devices and methods disclosed herein are further summarized in the following paragraphs and may be further characterized by any and all combinations of the various aspects described herein.
[0097] According to a first aspect, there is provided a method of manufacturing an optical fiber preform, the optical fiber having a core region and a cladding region, the method including forming a porous cladding soot blank by depositing silica soot onto a core cane. The core cane includes a core portion having a composition corresponding to at least a portion of the core region of the optical fiber, and a concentration of alkali metal oxide in the core portion of the core cane is between 0.1% and 1.5% by weight. The method includes exposing the porous cladding soot blank to a fluorine doping precursor in the presence of SiCl4, the fluorine doping precursor doping the porous cladding soot blank with fluorine to form a fluorine doped porous cladding soot blank. The exposing includes supplying a flow of the fluorine doping precursor to the porous cladding soot blank. The method includes densifying a fluorine-doped porous clad soot blank in the presence or absence of a fluorine doping precursor to form a densified fluorine-doped clad cane, the densifying step including exposing the fluorine-doped porous clad soot blank to SiCl4. The composition of the core portion of the core cane includes silica doped with an alkali metal oxide.
[0098] According to a second aspect, a method includes applying a fluorine-doped silica glass outer cladding layer to a densified fluorine-doped clad cane to form an optical fiber preform.
[0099] According to a third embodiment, SiCl is added at a concentration of about 1.6 g / cm3 in the densifying step. 3 There exists a minimum density of
[0100] According to a fourth aspect, a method includes forming a porous overclad soot blank by depositing silica soot on a densified fluorine-doped clad cane, exposing the porous overclad soot blank to a fluorine-doping precursor in the absence of SiCl4, and densifying the porous overclad soot blank to form a preform including a cladding portion having a composition corresponding to a cladding region of an optical fiber.
[0101] According to a fifth aspect, the cladding portion includes a depressed-index cladding portion surrounding the core portion and an outer cladding portion surrounding the depressed-index cladding portion, the depressed-index cladding portion having a first fluorine concentration and the outer cladding portion having a second fluorine concentration, the second fluorine concentration being lower than the first fluorine concentration.
[0102] According to the sixth aspect, the depressed-index cladding portion has a minimum relative refractive index Δ in the range of −0.80% to −0.30%. 3min and the outer cladding portion has a relative refractive index Δ3 having a refractive index Δ4-Δ 3min It has a relative refractive index Δ4 such that >0.05%.
[0103] According to a seventh aspect, the depressed-index cladding portion includes a first chlorine concentration and the outer cladding portion includes a second chlorine concentration, the second chlorine concentration being lower than the first chlorine concentration.
[0104] According to an eighth aspect, there is provided a method of manufacturing an optical fiber, the optical fiber having a core region and a cladding region, the method including forming an alkali-doped core cane. The alkali-doped core cane includes a portion having a composition corresponding to at least a portion of the core region of the optical fiber. The method includes forming a porous cladding soot blank by depositing silica soot on the alkali-doped core cane, and exposing the porous cladding soot blank to a fluorine-doping precursor. The fluorine-doping precursor dopes the silica soot with fluorine to form the fluorine-doped porous cladding soot blank. The exposing includes providing a flow of the fluorine-doping precursor to the porous cladding soot blank. The method includes densifying the fluorine-doped porous cladding soot blank in the absence or presence of the flow of the fluorine-doping precursor to form a fluorine-doped cladding cane having a portion having a composition corresponding to the cladding region of the optical fiber. The exposing step includes exposing the porous clad soot blank to a fluorine doping precursor in the presence of SiCl4, or the densifying step includes exposing the fluorine doped porous clad soot blank to SiCl4.
[0105] According to a ninth aspect, the exposing step includes exposing the porous clad soot blank to a fluorine doping precursor in the presence of SiCl4, and the densifying step includes exposing the fluorine doped porous clad soot blank to SiCl4.
[0106] According to a tenth aspect, a method includes drawing an optical fiber from a preform including a fluorine-doped clad cane, the optical fiber exhibiting an attenuation of less than 0.16 dB / km at 1583 nm, the attenuation increasing monotonically from about 1570 nm to about 1590 nm.
[0107] According to an eleventh aspect, forming an alkali-doped core cane includes vaporizing an alkali halide precursor and flowing it through a substrate tube, passing a heating burner over the exterior of the substrate tube with the alkali halide vapor flowing through the tube and diffusing through the tube wall to allow alkali doping inside the substrate tube, and collapsing the substrate tube to form a portion of the core cane, the portion of the core cane having a composition having an alkali concentration of 0.1% to 1.5% by weight.
[0108] According to a twelfth aspect, a portion having a composition corresponding to the cladding region of the optical fiber has a minimum relative refractive index Δ of less than −0.30%. 3min It has a relative refractive index Δ3 having
[0109] According to a thirteenth aspect, a method includes forming an outer cladding region by depositing silica soot on a fluorine-doped clad cane to form a porous overclad soot blank. The outer cladding region has a diameter of Δ4-Δ 3min >0.05%. The method includes densifying the porous overclad soot blank to form a preform and drawing an optical fiber from the preform. The optical fiber exhibits an attenuation of less than 0.16 dB / km at 1583 nm and an incremental attenuation above a baseline of less than 0.0005 dB / km at 1583 nm.
[0110] According to a fourteenth aspect, densifying the porous overclad soot blank includes exposing the porous overclad soot blank to a fluorine doping precursor in the absence of SiCl 4 .
[0111] According to a fifteenth aspect, if present in the exposing step or the densifying step, SiCl4 is provided to the gas atmosphere, and the concentration of SiCl4 in the gas atmosphere is between 0.1% and 15% by volume.
[0112] According to a sixteenth aspect, an optical fiber includes a core region comprising silica glass doped with an alkali metal oxide. A cladding region surrounds and is immediately adjacent to the core region. The cladding region includes a depressed-index cladding region surrounding the core region. The depressed-index cladding region comprises silica glass doped with a first fluorine concentration. The depressed-index cladding region has a minimum relative refractive index Δ in the range of −0.80% to −0.30%. 3min The cladding region includes an outer cladding region surrounding the depressed-index cladding region and immediately adjacent the depressed-index cladding region. The outer cladding region includes silica glass doped with a second fluorine concentration less than the first fluorine concentration. The outer cladding region has a relative refractive index Δ3 having a refractive index of Δ4-Δ 3min >0.05%. The optical fiber has a time to peak (TTP) hydrogen aging value of less than 100 hours at 23°C upon exposure of the optical fiber to a gas atmosphere having a total pressure of 1 atm (101325 Pa) and containing a H2 partial pressure of 0.01 atm (1013.25 Pa) and a N2 partial pressure of 0.99 atm (100311.8 Pa). The optical fiber exhibits an attenuation of less than 0.16 dB / km at 1583 nm, with the attenuation increasing monotonically from about 1570 nm to about 1600 nm.
[0113] According to the seventeenth aspect, the core region has an alkali metal oxide concentration of 0.5% by mass to 1.5% by mass.
[0114] According to an eighteenth embodiment, the alkali metal oxide comprises at least one of K2O, Na2O, LiO2, Rb2O and Cs2O.
[0115] According to a nineteenth aspect, the optical fiber exhibits an attenuation of less than 0.16 dB / km at 1547 nm and an incremental attenuation above a baseline of less than 0.0003 dB / km at 1547 nm.
[0116] According to a twentieth aspect, the optical fiber exhibits an attenuation of less than 0.5 dB / km at 1383 nm.
[0117] According to a twenty-first aspect, the preform is configured to be drawn into an optical fiber according to any one of the sixteenth to twentieth aspects.
[0118] While exemplary embodiments and examples have been described for illustrative purposes, the foregoing description is in no way intended to limit the scope of the disclosure and the appended claims. Thus, variations and modifications may be made to the above-described embodiments and examples without substantially departing from the spirit and various principles of the present disclosure. All such modifications and variations are intended to be included herein within the scope of this disclosure and protected by the following claims.
[0119] Preferred embodiments of the present invention will be described below in detail.
[0120] EMBODIMENT 1 1. A method of manufacturing an optical fiber preform, the optical fiber having a core region and a cladding region, the method comprising: forming a porous clad soot blank by depositing silica soot onto a core cane, the core cane including a core portion having a composition corresponding to at least a portion of the core region of the optical fiber, the core cane having an alkali metal oxide concentration of 0.1% to 1.5% by weight; exposing the porous clad soot blank to a fluorine doping precursor in the presence of SiCl4, the fluorine doping precursor doping the porous clad soot blank with fluorine to form a fluorine doped porous clad soot blank, the exposing step comprising supplying a flow of the fluorine doping precursor to the porous clad soot blank; densifying the fluorine-doped porous clad soot blank in the presence or absence of a fluorine-doping precursor to form a densified fluorine-doped clad cane, the densifying step comprising exposing the fluorine-doped porous clad soot blank to SiCl4; A method comprising:
[0121] EMBODIMENT 2 2. The method of embodiment 1, further comprising applying a fluorine-doped silica glass outer cladding layer to the densified fluorine-doped clad cane to form an optical fiber preform.
[0122] EMBODIMENT 3 The SiCl4 is about 1.6 g / cm3 in the densifying step. 3 3. The method of embodiment 1 or 2, wherein the cellular components are present to a minimum density of 0.1 to 0.5 μg / cm.
[0123] EMBODIMENT 4 forming a porous overclad soot blank by depositing silica soot on the densified fluorine-doped clad cane; exposing the porous overclad soot blank to the fluorine doping precursor in the absence of SiCl4; densifying the porous overclad soot blank to form the preform including a cladding portion having a composition corresponding to the cladding region of the optical fiber; 4. The method of any one of embodiments 1 to 3, further comprising:
[0124] EMBODIMENT 5 5. The method of embodiment 4, wherein the cladding portion includes a depressed-index cladding portion surrounding the core portion and an outer cladding portion surrounding the depressed-index cladding portion, the depressed-index cladding portion having a first fluorine concentration and the outer cladding portion having a second fluorine concentration, the second fluorine concentration being lower than the first fluorine concentration.
[0125] EMBODIMENT 6 The depressed-index cladding portion has a minimum relative refractive index Δ in the range of −0.80% to −0.30%. 3min and the outer cladding portion has a relative refractive index Δ3 having a refractive index Δ4-Δ 3min 6. The method of embodiment 5, having a relative refractive index Δ4 of >0.05%.
[0126] EMBODIMENT 7 7. The method of embodiment 5 or 6, wherein the depressed-index cladding portion comprises a first chlorine concentration and the outer cladding portion comprises a second chlorine concentration, the second chlorine concentration being less than the first chlorine concentration.
[0127] EMBODIMENT 8 1. A method of manufacturing an optical fiber, the optical fiber having a core region and a cladding region, the method comprising: forming an alkali-doped core cane including a portion having a composition corresponding to at least a portion of the core region of the optical fiber; forming a porous clad soot blank by depositing silica soot on the alkali doped core cane; exposing the porous clad soot blank to a fluorine doping precursor, the fluorine doping precursor doping the silica soot with fluorine to form a fluorine doped porous clad soot blank, the exposing step comprising supplying a flow of the fluorine doping precursor to the porous clad soot blank; densifying the fluorine-doped porous clad soot blank in the absence or presence of the flow of the fluorine-doping precursor to form a fluorine-doped clad cane having a portion having a composition corresponding to the cladding region of the optical fiber; Including, the exposing step comprises exposing the porous clad soot blank to the fluorine doping precursor in the presence of SiCl4, or the densifying step comprises exposing the fluorine doped porous clad soot blank to SiCl4; method.
[0128] EMBODIMENT 9 The method of embodiment 8, wherein the exposing step comprises exposing the porous clad soot blank to the fluorine doping precursor in the presence of SiCl4, and the densifying step comprises exposing the fluorine doped porous clad soot blank to SiCl4.
[0129] EMBODIMENT 10 10. The method of claim 8 or 9, further comprising drawing the optical fiber from a preform including the fluorine-doped clad cane, wherein the optical fiber exhibits an attenuation of less than 0.16 dB / km at 1583 nm, and the attenuation increases monotonically from about 1570 nm to about 1590 nm.
[0130] EMBODIMENT 11 forming the alkali doped core cane, vaporizing an alkali halide precursor and flowing it through a substrate tube; traversing a heating burner on the exterior of the substrate tube with alkali halide vapor flowing through the tube and diffusing through the tube wall, allowing alkali doping inside the substrate tube; collapsing the substrate tube to form a portion of the core cane; Including, The core cane portion has a composition having an alkali concentration of 0.1% by mass to 1.5% by mass. The method of any one of embodiments 8 to 10.
[0131] EMBODIMENT 12 The portion of the optical fiber having a composition corresponding to the cladding region has a minimum relative refractive index Δ of less than −0.30% 3min 12. The method of any one of embodiments 8 to 11, wherein the crystalline crystalline zirconia has a relative refractive index Δ3 having a refractive index of
[0132] EMBODIMENT 13 By depositing silica soot on the fluorine-doped clad cane, 3min forming an outer cladding region having a relative refractive index Δ4 >0.05% to form a porous overclad soot blank; densifying the porous overclad soot blank to form a preform; drawing the optical fiber from the preform, the optical fiber exhibiting an attenuation at 1583 nm of less than 0.16 dB / km and an incremental attenuation above a baseline at 1583 nm of less than 0.0005 dB / km; 13. The method of any one of embodiments 8 to 12, further comprising:
[0133] EMBODIMENT 14 14. The method of embodiment 13, wherein densifying the porous overclad soot blank comprises exposing the porous overclad soot blank to the fluorine doping precursor in the absence of SiCl.
[0134] EMBODIMENT 15 15. The method of any one of claims 8 to 14, wherein, if present in the exposing step or the densifying step, the SiCl4 is provided to a gas atmosphere, and the concentration of the SiCl4 in the gas atmosphere is 0.1 vol.% to 15 vol.%.
[0135] EMBODIMENT 16 An optical fiber, a core region comprising silica glass doped with an alkali metal oxide; a cladding region surrounding and immediately adjacent to said core region; Including, The cladding region is a depressed-index cladding region surrounding the core region, the depressed-index cladding region comprising silica glass doped with a first fluorine concentration and having a minimum relative refractive index Δ in the range of −0.80% to −0.30%; 3min a depressed-index cladding region having a relative refractive index Δ3 having an outer cladding region surrounding and immediately adjacent to the depressed-index cladding region, the outer cladding region comprising silica glass doped with a second fluorine concentration less than the first fluorine concentration; 3min an outer cladding region having a relative refractive index Δ4 >0.05%; Including, the optical fiber has a time to peak (TTP) hydrogen aging value of less than 100 hours at 23° C. upon exposure of the optical fiber to a gas atmosphere having a total pressure of 1 atm (101325 Pa) and including an H partial pressure of 0.01 atm (1013.25 Pa) and an N partial pressure of 0.99 atm (100311.8 Pa); the optical fiber exhibits an attenuation of less than 0.16 dB / km at 1583 nm, the attenuation increasing monotonically from about 1570 nm to about 1600 nm; Optical fiber.
[0136] EMBODIMENT 17 17. The optical fiber according to embodiment 16, wherein the core region has an alkali metal oxide concentration of 0.5% to 1.5% by mass.
[0137] EMBODIMENT 18 18. The optical fiber of embodiment 16 or 17, wherein the optical fiber exhibits an attenuation at 1547 nm of less than 0.16 dB / km and an incremental attenuation above a baseline at 1547 nm of less than 0.0003 dB / km.
[0138] EMBODIMENT 19 19. The optical fiber of any one of embodiments 16 to 18, wherein the optical fiber exhibits an attenuation of less than 0.5 dB / km at 1383 nm.
[0139] EMBODIMENT 20 20. A preform configured to be drawn into the optical fiber of any one of embodiments 16 to 19.
Claims
1. 1. A method of manufacturing an optical fiber preform, the optical fiber having a core region and a cladding region, the method comprising: forming a porous clad soot blank by depositing silica soot onto a core cane, the core cane including a core portion having a composition corresponding to at least a portion of the core region of the optical fiber, the concentration of alkali metal oxide in the core portion of the core cane being between 0.1% and 1.5% by weight; The porous clad soot blank was then subjected to a SiCl 4 exposing to a fluorine doping precursor in the presence of a fluorine doping precursor that dopes the porous clad soot blank with fluorine to form a fluorine doped porous clad soot blank, the exposing step comprising supplying a flow of the fluorine doping precursor to the porous clad soot blank; densifying the fluorine-doped porous clad soot blank in the presence or absence of a fluorine doping precursor to form a densified fluorine-doped clad cane, the densifying step comprising: densifying the fluorine-doped porous clad soot blank with SiCl 4 densifying, comprising exposing the A method comprising:
2. The method of claim 1 , further comprising the step of applying a fluorine-doped silica glass outer cladding layer to the densified fluorine-doped clad cane to form an optical fiber preform.
3. forming a porous overclad soot blank by depositing silica soot on the densified fluorine-doped clad cane; The porous overclad soot blank was then subjected to a SiCl 4 to said fluorine doping precursor in the absence of densifying the porous overclad soot blank to form the preform including a cladding portion having a composition corresponding to the cladding region of the optical fiber; The method of claim 1 or 2, further comprising:
4. 4. The method of claim 3, wherein the cladding portion comprises a depressed-index cladding portion surrounding the core portion and an outer cladding portion surrounding the depressed-index cladding portion, the depressed-index cladding portion having a first fluorine concentration and the outer cladding portion having a second fluorine concentration, the second fluorine concentration being less than the first fluorine concentration.
5. The method of claim 4 , wherein the depressed-index cladding portion comprises a first chlorine concentration and the outer cladding portion comprises a second chlorine concentration, the second chlorine concentration being less than the first chlorine concentration.
6. 1. A method of manufacturing an optical fiber, the optical fiber having a core region and a cladding region, the method comprising: forming an alkali-doped core cane including a portion having a composition corresponding to at least a portion of the core region of the optical fiber; forming a porous clad soot blank by depositing silica soot on the alkali doped core cane; exposing the porous clad soot blank to a fluorine doping precursor, the fluorine doping precursor doping the silica soot with fluorine to form a fluorine doped porous clad soot blank, the exposing step comprising supplying a flow of the fluorine doping precursor to the porous clad soot blank; densifying the fluorine-doped porous clad soot blank in the absence or presence of the flow of the fluorine-doping precursor to form a fluorine-doped clad cane having a portion having a composition corresponding to the cladding region of the optical fiber; Including, The exposing step comprises exposing the porous clad soot blank to SiCl 4 or the densifying step comprises exposing the fluorine doped porous clad soot blank to a fluorine doping precursor in the presence of SiCl 4 comprising exposing said method.
7. The exposing step comprises exposing the porous clad soot blank to SiCl 4 and the densifying step comprises exposing the fluorine doped porous clad soot blank to a fluorine doping precursor in the presence of SiCl. 4 The method of claim 6, comprising exposing the
8. By depositing silica soot on the fluorine doped clad cane, Δ 4 -Δ 3min Relative refractive index Δ 4 forming an outer cladding region having a porous overclad soot blank; densifying the porous overclad soot blank to form a preform; drawing the optical fiber from the preform, the optical fiber exhibiting an attenuation at 1583 nm of less than 0.16 dB / km and an incremental attenuation above a baseline at 1583 nm of less than 0.0005 dB / km; The method of claim 6 or 7, further comprising:
9. An optical fiber, a core region comprising silica glass doped with an alkali metal oxide; a cladding region surrounding and immediately adjacent to said core region; Including, The cladding region is a depressed-index cladding region surrounding the core region, the depressed-index cladding region comprising silica glass doped with a first fluorine concentration and having a minimum relative refractive index Δ in the range of −0.80% to −0.30%; 3min Relative refractive index Δ 3 a depressed-index cladding region having an outer cladding region surrounding and immediately adjacent to the depressed-index cladding region, the outer cladding region comprising silica glass doped with a second fluorine concentration lower than the first fluorine concentration; 4 -Δ 3min Relative refractive index Δ 4 an outer cladding region having Including, The optical fiber has a total pressure of 1 atm (101325 Pa) and a H 2 Partial pressure and 0.99 atm (100311.8 Pa) N 2 has a time to peak (TTP) hydrogen aging value of less than 100 hours at 23° C. upon exposure of the optical fiber to a gas atmosphere containing a hydrogen partial pressure; the optical fiber exhibits an attenuation of less than 0.16 dB / km at 1583 nm, the attenuation increasing monotonically from about 1570 nm to about 1600 nm; Optical fiber.
10. The optical fiber of claim 9, wherein the optical fiber exhibits an attenuation of less than 0.5 dB / km at 1383 nm.
11. A preform adapted to be drawn into the optical fiber of claim 9 or 10.
Citation Information
Patent Citations
Method of making halogen co-doped cores for optical fibers and optical fibers
WO2020033219A1
Cited By
Low-loss multimode optical fiber and preparation method thereof
CN122239217A