Method for manufacturing copper alloy sheet material, and copper alloy sheet material
A controlled manufacturing process for copper alloy sheet materials with specific element compositions stabilizes resistivity by generating a short-range ordered arrangement, addressing fluctuations in high-temperature environments.
Patent Information
- Application Number
- JP2025174575
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-10-16
- Publication Date
- 2026-11-02
AI Technical Summary
The existing method for producing copper alloy sheet materials for resistors results in disordered element arrangements, leading to significant fluctuations in volume resistivity when exposed to high-temperature environments for extended periods.
A manufacturing process involving specific compositions of Mn, Ni, Al, Mg, and Cu, including melting, casting, hot rolling, cold rolling, and controlled annealing to generate a short-range ordered arrangement, followed by welding and stress-relieving annealing to stabilize resistivity.
The process effectively suppresses the rate of change in volume resistivity, maintaining stability even in high-temperature environments, with a rate of change within 0.02 to 0.24% after 2000 hours at 150°C.
Smart Images

Figure 2026175266000001_ABST
Abstract
Description
Technical Field
[0001] The disclosure described in the present specification relates to a method for producing a copper alloy sheet material, a method for producing a resistor, a copper alloy sheet material, and a resistor.
Background Art
[0002] Patent Document 1 discloses a copper alloy sheet material used for resistors. In Patent Document 1, the temperature coefficient of resistance of the copper alloy sheet material is reduced by adjusting the content of Mn and the like contained in the copper alloy sheet material, so that the resistance of the resistor remains stable even when the ambient temperature changes.
Prior Art Documents
Patent Documents
[0003]
Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0004] However, in the method for producing a copper alloy sheet material disclosed in Patent Document 1, there is a risk that the arrangement of different types of elements contained in the copper alloy sheet material will not be ordered and will remain disordered. For this reason, when the copper alloy sheet material is left in a high-temperature environment for a long time, there is a risk that the rate of change in volume resistivity of the copper alloy sheet material will fluctuate significantly.
[0005] An object of the present disclosure is to provide a method for producing a copper alloy sheet material, a method for producing a resistor, a copper alloy sheet material, and a resistor in which an increase in the rate of change in volume resistivity is suppressed even when left in a high-temperature environment for a long time.
Means for Solving the Problems
[0006] The method for producing a copper alloy sheet material according to the disclosed aspect is A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. Copper alloy material is melted and cast to produce an ingot. By hot rolling the ingot, a hot-formed body is produced. By performing cold rolling on a hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. The cold-formed body, from which residual strain has been removed, is held in a temperature range of 110°C to less than 200°C.
[0007] The method for manufacturing a copper alloy sheet material according to the disclosed embodiment is: A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. Copper alloy material is melted and cast to produce an ingot. By hot rolling the ingot, a hot-formed body is produced. By performing cold rolling on a hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. A short-range ordered arrangement is generated in a cold-formed body from which residual strain has been removed.
[0008] A method for manufacturing a resistor according to the disclosed embodiment is: A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. Copper alloy material is melted and cast to produce an ingot. By hot rolling the ingot, a hot-formed body is produced. By performing cold rolling on a hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. A cold-formed body from which residual strain has been removed is held in a temperature range of 110°C to less than 200°C to produce a copper alloy sheet material (300). A resistor (110) is manufactured by welding a copper alloy sheet to a metal busbar (200). By holding the resistor at a temperature of 200°C or higher, the distortion caused by welding in the copper alloy plate material is removed.
[0009] A method for manufacturing a resistor according to the disclosed embodiment is: A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. Copper alloy material is melted and cast to produce an ingot. By hot rolling the ingot, a hot-formed body is produced. By performing cold rolling on a hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. A copper alloy sheet material (300) is manufactured in which a short-distance ordered arrangement is generated in a cold-formed body from which residual strain has been removed. A resistor (110) is manufactured by welding a copper alloy sheet to a metal busbar (200). By holding the resistor at a temperature of 200°C or higher, the distortion caused by welding in the copper alloy plate material is removed.
[0010] A method for manufacturing a resistor according to the disclosed embodiment is: A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. Copper alloy material is melted and cast to produce an ingot. By hot rolling the ingot, a hot-formed body is produced. A cold-formed body is produced by subjecting a hot-formed body to cold rolling, The cold-formed body is held within a predetermined temperature range to produce a copper alloy sheet material (300) from which residual strain generated in the cold-formed body by cold rolling has been removed, The copper alloy sheet material is welded to a metal bus bar (200) to produce a resistor (110), The resistor is held at 200°C or higher to remove strain generated in the copper alloy sheet material by welding, The resistor is held within a temperature range of 110°C or higher and lower than 200°C.
[0011] The disclosed method for manufacturing a resistor according to the disclosed aspect is: Preparing a copper alloy material containing 10.0 to 14.0 mass% of Mn, 1.0 to 4.0 mass% of Ni, 0 to 0.10 mass% of Al, 0 to 0.10 mass% of Mg, with the balance consisting of Cu and unavoidable impurities, The copper alloy material is melted and cast to produce an ingot, The ingot is subjected to hot rolling to produce a hot-formed body, The hot-formed body is subjected to cold rolling to produce a cold-formed body, The cold-formed body is held within a predetermined temperature range to produce a copper alloy sheet material (300) from which residual strain generated in the cold-formed body by cold rolling has been removed, The copper alloy sheet material is welded to a metal bus bar (200) to produce a resistor (110), The resistor is held at 200°C or higher to remove strain generated in the copper alloy sheet material by welding, A short-range ordered arrangement is generated in the copper alloy sheet material.
[0012] The copper alloy sheet material according to the disclosed aspect is: Containing 10.0 to 14.0 mass% of Mn, 1.0 to 4.0 mass% of Ni, 0 to 0.10 mass% of Al, 0 to 0.10 mass% of Mg, with the balance consisting of Cu and unavoidable impurities, The absolute value of the change rate of the volume resistivity value when held at a constant temperature of 150°C for 2000 hours is 0.05 to 1.06%.
[0013] A resistor in the disclosed embodiment is A copper alloy plate material (300) containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities, It has a metal busbar (200) in which copper alloy plates are welded together, The absolute value of the rate of change in volume resistivity when maintained at a constant temperature of 150°C for 2000 hours is 0.02 to 0.24%.
[0014] According to this, even when exposed to high-temperature environments for extended periods, the rate of change in the volume resistivity of the copper alloy plate material is suppressed.
[0015] The reference numbers in parentheses above merely indicate the correspondence with the configurations described in the embodiments below, and do not limit the technical scope in any way. [Brief explanation of the drawing]
[0016] [Figure 1] This is a control module block. [Figure 2] This is a schematic diagram showing a current sensor. [Figure 3] This is a flowchart showing a method for manufacturing resistors. [Figure 4] This is a flowchart showing a method for manufacturing resistors. [Figure 5] This is a flowchart showing a method for manufacturing resistors. [Figure 6] This is a diagram showing the compositional materials of the test specimen. [Figure 7] This is a schematic diagram illustrating the apparatus and method for measuring the volume resistivity of a test specimen. [Figure 8] This is a chart showing the volume resistivity of the test specimen and its rate of change. [Figure 9] This graph shows the temperature during SRO annealing. [Figure 10] This chart shows the relationship between SRO annealing time and the rate of resistance change, as well as the relationship between SRO annealing temperature and the progress of SRO annealing. [Figure 11] This graph shows the progress of SRO annealing. [Figure 12] This is a magnified view of the area enclosed by the dashed line shown in Figure 11. [Figure 13] This chart shows the resistance value and resistance change rate of the test specimen during durability testing. [Figure 14] This graph shows the rate of resistance change during durability testing. [Figure 15] This graph shows the relationship between the resistance change rate due to durability testing and the resistance change rate due to SRO annealing. [Figure 16] This chart shows the resistance change rate of resistors that have undergone SRO annealing. [Figure 17] This graph shows the rate of change in resistance of resistors that have undergone SRO annealing. [Figure 18] This chart shows the rate of change in resistance of resistors that have undergone distortion-removing annealing. [Figure 19] This graph shows the rate of change in resistance of a resistor that has undergone distortion-relieving annealing. [Figure 20] This chart shows the percentage change in resistance of resistors that have undergone stress-relieving annealing and SRO annealing after welding. [Figure 21] This graph shows the percentage change in resistance of resistors that underwent stress-relieving annealing and SRO annealing after welding. [Figure 22] This chart shows the percentage change in resistance of resistors that underwent SRO annealing before welding and then distortion-relieving annealing after welding. [Figure 23] This chart shows the percentage change in resistance of resistors that underwent SRO annealing before welding and then distortion-relieving annealing after welding. [Modes for carrying out the invention]
[0017] The following describes several embodiments for implementing this disclosure with reference to the drawings. In later embodiments, parts corresponding to matters described in earlier embodiments may be given the same reference numerals, and redundant explanations may be omitted. If only a part of the configuration is described in each embodiment, the description of the earlier embodiment may be applied to the other parts of the configuration.
[0018] It is possible to combine parts that are explicitly shown to be combinable in each form. Furthermore, if there are no particular problems with the combination, it is also possible to partially combine multiple forms with each other, a form with a modified form, and multiple modified forms with each other, even if it is not explicitly shown that they can be combined.
[0019] <First Embodiment> <Control Module> As shown in Figure 1, the control module 10 includes a sensor device 20 and a control device 30.
[0020] The sensor device 20 detects a physical quantity. The sensor device 20 converts the physical quantity into an analog signal. In the drawing, the sensor device 20 is indicated as SD. SD stands for Sensor Device.
[0021] Examples of items that the sensor device 20 can detect include batteries, converters, inverters, motors, engines, drivetrains, and busbars. Examples of physical quantities that the sensor device 20 can detect include current, voltage, temperature, acceleration, angular velocity, flow rate, and pressure. The items and physical quantities that the sensor device 20 can detect are not particularly limited, even if not explicitly stated.
[0022] The control device 30 receives the physical quantity converted into an analog signal by the sensor device 20. The control device 30 converts this analog signal into a digital signal. In the drawing, the control device 30 is shown as CU. CU is an abbreviation for Control Unit.
[0023] The control module 10, which includes these sensor devices 20 and control device 30, can be appropriately adopted in vehicle systems for mobile vehicles such as electric vehicles, hybrid vehicles, gasoline vehicles, and trucks. The mobile vehicles to which the control module 10 is applied are not particularly limited, unless otherwise specified.
[0024] As described above, the physical quantity detected by the sensor device 20 is electric current. The current sensor 100 included in this sensor device 20 will be explained in detail below.
[0025] <Current Sensor> The current sensor 100 shown in Figure 2 performs the function of detecting the current flowing through the PN busbar connecting the battery pack mounted on the mobile device to the PCU. PCU stands for Power Control Unit. The PCU includes at least an inverter. The PCU may also include a converter. The PN busbar includes a P busbar connected to the positive terminal of the battery pack and an N busbar connected to the negative terminal of the battery pack.
[0026] The current sensor 100 includes a resistor 110, a wiring board 120, and a connector 130.
[0027] The resistor 110 has a metal busbar 200 and a shunt resistor 300. The metal busbar 200 and the shunt resistor 300 are welded together. The metal busbar 200 and the shunt resistor 300 are made of different types of metal materials.
[0028] The metal busbar 200 has a first metal busbar 210 and a second metal busbar 220. The first metal busbar 210 and the second metal busbar 220 are connected via a shunt resistor 300.
[0029] A first hole 210a is formed in the first metal busbar 210. A second hole 220a is formed in the second metal busbar 220. A bolt is passed through the first hole 210a to connect the metal busbar 200 and the PN busbar. A bolt is also passed through the second hole 220a to connect the metal busbar 200 and the PN busbar.
[0030] A detection pin 230 is connected to the metal busbar 200. The detection pin 230 has a first detection pin 231 and a second detection pin 232. The first detection pin 231 is connected to the first metal busbar 210. The second detection pin 232 is connected to the second metal busbar 220. The first detection pin 231 and the second detection pin 232 are aligned with the shunt resistor 300 in between, in the direction of the alignment of the first hole 210a and the second hole 220a.
[0031] The detection pin 230 is connected to the wiring board 120. A connector 130 is also connected to the wiring board 120. The connector 130 is connected to the control device 30 via a wire harness. This electrically connects the current sensor 100 to the control device 30.
[0032] With the configuration described above, the voltage across the shunt resistor 300 is input to the control device 30. The control device 30 stores the resistance value of the shunt resistor 300. The control device 30 calculates the current flowing through the shunt resistor 300 from the input voltage and the stored resistance value. As a result, the current flowing through the PN busbar is detected.
[0033] Incidentally, naturally, when current flows through the shunt resistor 300, the temperature of the shunt resistor 300 rises. If it is left in a harsh environment such as high temperature for a long period of time, the durability of the shunt resistor 300 may be impaired, and there is a risk that a discrepancy may occur between the actual resistance value of the shunt resistor 300 and the resistance value stored in the control device 30. As a result, there is a risk that the accuracy of current detection will decrease. The shunt resistor 300 will be explained in detail below.
[0034] <Composition materials for shunt resistors> The shunt resistor 300 is made of copper alloy sheet material. The copper alloy sheet material contains Mn, Ni, Mg, the remainder being Cu, and unavoidable impurities. Al may also be present in the copper alloy sheet material. The reasons for the inclusion of these elements in the copper alloy sheet material are as follows:
[0035] Mn dissolves in Cu and plays a role in reducing the temperature coefficient of resistance of a shunt resistance of 300. However, if the amount of Mn is excessive, the volume resistivity increases. Therefore, the amount of Mn is 10.0 to 14.0 mass%. The preferred amount of Mn is 11.0 to 13.0 mass%.
[0036] Ni dissolves in Cu and plays a role in lowering the temperature coefficient of resistance of a shunt resistance of 300. However, if the amount of Ni is excessive, the volume resistivity increases. Therefore, the amount of Ni is between 1.0 and 4.0 mass%. The preferred amount of Ni is between 2.00 and 3.00 mass%.
[0037] Mg contributes to improved workability during hot rolling, as described later. The preferred amount of Mg is 0.001 to 0.05 mass%.
[0038] If oxygen is introduced into the shunt resistor 300, there is a risk of Cu2O precipitation and hydrogen embrittlement. Therefore, Al is added to the shunt resistor 300. This forms Al2O3, which traps oxygen and suppresses the precipitation of Cu2O. The preferred amount of Al is 0.001 to 0.05 mass%.
[0039] Unavoidable impurities are trace elements that are unintentionally mixed into the copper alloy material from the furnace wall or other parts of the casting furnace during the melting and casting process described later, and whose content is within a range that does not adversely affect the electrical properties of the shunt resistance 300. Examples of unavoidable impurities include C, P, S, Mo, Si, Cr, O, and N. The content of these elements is preferably limited as shown below, and the lower the better. C ≤ 0.03 mass%, preferably C ≤ 0.01 mass%. P ≤ 0.03 mass%, preferably P ≤ 0.01 mass%. S ≤ 0.03 mass%, preferably S ≤ 0.01 mass%. Mo ≤ 0.03 mass%, preferably Mo ≤ 0.01 mass%. Si ≤ 0.05 mass%, preferably Si ≤ 0.03 mass%. Cr ≤ 0.05 mass%, preferably Cr ≤ 0.03 mass%. O ≤ 0.03 mass%, preferably O ≤ 0.01 mass%. N ≤ 0.03 mass%, preferably N ≤ 0.01 mass%. Furthermore, in order to suppress the deterioration of the electrical characteristics of the shunt resistance 300, the total content of impurity elements, including the above-mentioned C, P, S, Mo, Si, Cr, O, and N, is preferably 0.30 mass% or less. This total content is even more preferably 0.10 mass% or less.
[0040] <Method of manufacturing a resistor> The shunt resistor 300 and the resistor 110 containing it in this embodiment undergo the manufacturing process shown in Figure 3, thereby suppressing fluctuations in their volume resistivity even when placed in harsh environments.
[0041] First, in step S10, a copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities.
[0042] In step S20, an ingot is produced by melting and casting the copper alloy material. The method and conditions of melting and casting are not particularly limited.
[0043] If the ingot is left as is, elements are prone to segregation, and there is a risk that homogeneous properties cannot be obtained. Therefore, in step S30, the ingot is subjected to homogenization heat treatment to remove elemental segregation. A heat-treated body with a homogenized internal structure is obtained.
[0044] In step S40, the heat-treated body is subjected to hot rolling. This produces a hot-formed body. Hot rolling is performed to homogenize the structure of the heat-treated body and to process it into a rough shape. The method and conditions of hot rolling are not particularly limited, as long as the desired homogenization of the structure and processing into a rough shape can be achieved.
[0045] In step S50, the hot-formed body is cold-rolled. This produces a cold-formed body. Normally, high thickness accuracy cannot be obtained by hot-rolling alone. Cold-rolling is performed to process the body to the final thickness. The method and conditions of cold-rolling are not particularly limited, as long as the desired dimensional accuracy can be obtained. Note that the oxidized areas on the surface of the hot-formed body may be removed before cold-rolling.
[0046] In step S60, the cold-formed body is held within a predetermined temperature range and annealed. This recrystallizes the cold-formed body and removes the residual strain generated in the cold-formed body during cold rolling. For example, a temperature range of 500°C to 850°C can be used for the annealing process.
[0047] If residual strain is not sufficiently removed by annealing, the strain will gradually ease under the operating environment, and the rate of change in the volume resistivity of the shunt resistor 300 will increase.
[0048] If the annealing temperature is too low or the annealing time is too short, strain removal and recrystallization will be insufficient. The lower limit of the annealing temperature is 500°C or higher, more preferably 600°C or higher. The lower limit of the annealing time is preferably 30 seconds or higher.
[0049] If the annealing temperature is too high or the annealing time is too long, the crystal grains may grow rapidly, which can reduce the material's strength. The upper limit for annealing temperature is 850°C or lower, more preferably 800°C or lower. The upper limit for annealing time is preferably 3 hours or less.
[0050] In step S70, the cold-formed body, from which residual strain has been removed, is held in a temperature range of 110°C to less than 200°C to perform SRO annealing. This generates a short-range ordered arrangement in the cold-formed body. SRO stands for Short Range Order.
[0051] In addition, short-range order patterns may be formed in the hot-formed body during the cooling process of the hot-rolling treatment in step S40. However, these short-range order patterns are destroyed by the cold-rolling in step S50. Furthermore, short-range order patterns may be formed in the cold-formed body during the cooling process after annealing in step S60. However, if the cooling process is too rapid, the short-range order patterns may not be sufficiently formed. Therefore, in step S70, a heat treatment is performed on the cold-formed body with the aim of creating short-range order patterns.
[0052] If the SRO annealing temperature is too low or the SRO annealing time is too short, the generation of short-range ordered sequences will be insufficient. If the SRO annealing temperature is too high, the generation of short-range ordered sequences may also be insufficient. Furthermore, from the perspective of generating short-range ordered sequences, even if the SRO annealing time is too long, it is unlikely to be a major problem. However, from the perspective of manufacturing costs, if a sufficient amount of short-range ordered sequences are generated, further SRO annealing is unnecessary. Therefore, an SRO annealing time of less than 24 hours is preferable. The temperature and time to address this will be discussed later.
[0053] The copper alloy plate material for the shunt resistor 300 is manufactured by going through the manufacturing process described above in steps S10 to S70. The manufacturing method for the shunt resistor 300 is a process that precedes the welding process in step S80, which will be described next. A dashed line is added to Figure 3 and to Figures 4 and 5 described later to indicate this.
[0054] Next, in step S80, the shunt resistor 300 and the metal busbar 200 are laser-welded together.
[0055] Finally, in step S90, the welded metal busbar 200 of the shunt resistor 300 is held within a predetermined temperature range and subjected to stress-relieving annealing to remove the stress caused in the shunt resistor 300 and the metal busbar 200 by laser welding. The resistor 110 is manufactured through these processes.
[0056] The temperature for strain-relieving annealing and the temperature for SRO annealing may overlap to some extent. However, generally, the temperature for strain-relieving annealing is 200°C or higher. This is the temperature at which oxygen-free copper recrystallizes. The annealing temperature for removing strain from this material is described, for example, in Japanese Patent Publication No. 7158053, No. 7167385, No. 6961861, and No. 6762438.
[0057] As will be explained later, 200°C is not necessarily the most suitable temperature for short-distance regular arrangement of shunt resistors 300. Therefore, when actually manufacturing shunt resistors 300 and resistors 110, the temperature range for strain relief annealing and the temperature range for SRO annealing should be clearly distinguished. These temperature ranges should be clearly differentiated. The temperature range for strain relief annealing will be higher than the temperature range for SRO annealing. For example, a temperature range of 200°C to 400°C can be used for strain relief annealing. The temperature for SRO annealing will be below 200°C.
[0058] Up to this point, we have shown an example in which SRO annealing is performed immediately after step S60. We have shown an example in which copper alloy sheet material for shunt resistor 300 is manufactured by performing SRO annealing. However, copper alloy sheet material for shunt resistor 300 may be manufactured without performing SRO annealing. For example, as shown in Figures 4 and 5, SRO annealing may be performed on the shunt resistor 300 welded to the metal busbar 200 after the welding process in step S80. Alternatively, copper alloy sheet material for shunt resistor 300 may be manufactured without performing SRO annealing, welded to the metal busbar 200, and then SRO annealing may be performed.
[0059] In the manufacturing method shown in Figure 4, after the welding process in step S80, SRO annealing in step S70 is performed, followed by strain relief annealing in step S90. In this manufacturing method, once the temperature range for SRO annealing is reached from room temperature, the temperature is maintained in that range, or the heating rate is slowed down in that range. Thus, SRO annealing may be performed during the heating process from room temperature to the temperature range for strain relief annealing. Alternatively, after performing SRO annealing, the temperature may be lowered once, and then the temperature may be raised again to perform strain relief annealing.
[0060] In the manufacturing method shown in Figure 5, the welding process in step S80 is followed by the stress relief annealing in step S90, and then the SRO annealing in step S70. In this manufacturing method, first, the temperature is raised from room temperature to the temperature at which stress relief annealing is performed, and then the stress relief annealing is carried out. After that, during the cooling down process to room temperature, if the temperature range for SRO annealing is reached, the temperature is maintained in that range, or the cooling speed is slowed in that range. In this way, SRO annealing may be carried out during the cooling process from the temperature range for stress relief annealing to room temperature. Alternatively, after performing stress relief annealing, the temperature may be lowered once, and then the temperature may be raised and SRO annealing may be carried out.
[0061] <Manufacturing of test specimens> Using a vacuum induction furnace, ingots of copper alloy material having the composition shown in Figure 6 were prepared. The units of these compositional materials are mass percent. After homogenization heat treatment of the prepared ingots, a hot-rolled plate-shaped hot-formed body with a thickness of 5 mm was formed. After removing the oxidized region from the surface of the hot-formed body by surface grinding, it was cold-rolled to form a plate-shaped cold-formed body with a thickness of 2.8 mm. Multiple test pieces with a thickness of 2.8 mm, a width of 2 mm, and a length of 130 mm were taken from the obtained cold-formed body. Annealing was performed on multiple test pieces. In addition, SRO annealing was performed on some of these test pieces. SRO annealing was performed at 110°C, 130°C, 150°C, 170°C, 190°C, and 210°C for 12 hours.
[0062] <Measurement of volume resistance> Next, as shown in Figure 7, the test specimen was placed in a constant temperature bath 400. Both ends of the test specimen were held with first alligator clips 410 and connected to the constant current source 421 of the resistance meter 420. Two platinum wires 430 were connected 40 mm apart at the center of the test specimen, and second alligator clips 440 were connected to them. The spacing between the two platinum wires 430 is a length expected to ensure a sufficiently stable current distribution. Then, the two second alligator clips 440 were connected to the voltmeter 422 of the resistance meter 420. Current was passed between the two first alligator clips 410, and the voltage was measured at the two second alligator clips 440. In this way, the volume resistivity of the test specimen was measured. Of course, the volume resistivity of the test specimen can also be calculated from this measured volume resistivity.
[0063] For the resistance meter 420, a HIOKI R3543 was used. As described above, the four-terminal method was adopted for measurement. The resistance measurement range was 10 mΩ, and the display had 7 digits. The display resolution was 0.01 μΩ, and the measurement accuracy was ±0.060%rdg. ±0.001%fs.
[0064] The ambient temperature of the constant temperature chamber was maintained at 25±3°C. Then, the temperature of the constant temperature chamber 400 was set to 150°C and maintained for 2000 hours to conduct a durability test of the test specimen. The volume resistivity of the test specimen was measured during this durability test.
[0065] Figure 8 shows the volume resistivity of the test specimen and its rate of change. In accordance with JIS-C2525, the volume resistivity of the test specimen was measured at 20°C during the initial 0 hours before the start of the test. The volume resistivity of the test specimen was measured at 150°C after 2000 hours at the end of the test. The rate of change (resistivity change rate) was calculated to determine how much the volume resistivity of the test specimen changed when it was exposed to a high temperature of 150°C for 2000 hours compared to its volume resistivity at 20°C.
[0066] The resistance values of the test specimens that were not SRO annealed and those that were SRO annealed at 110°C are approximately 2.5 mΩ. In contrast, the resistance value of the test specimens that were SRO annealed at 130°C to 210°C is approximately 5.9 mΩ. The difference between the two is due to the difference in the connection points of the two platinum wires 430 during the measurement of volume resistance. Although there is a difference in volume resistance values due to these slight differences in measurement conditions, this does not pose a problem when verifying the rate of change of volume resistance.
[0067] As shown in Figure 8, the rate of change in volume resistivity decreases when SRO annealing is performed. The rate of change in volume resistivity decreases as the SRO annealing temperature increases.
[0068] The rate of change in volume resistivity of test specimens subjected to 110°C SRO annealing was 0.22% lower than the rate of change in volume resistivity of test specimens not subjected to SRO annealing, after being left at a high temperature of 150°C for 2000 hours.
[0069] As will be described later, the maximum measurement variation in the rate of change of volume resistance of resistor 110, which has more components than shunt resistor 300, is less than 0.2%. Therefore, it is expected that the maximum measurement variation of shunt resistor 300 alone will also be less than 0.2%. The difference of 0.22% in the rate of change of volume resistance between test specimens that underwent 110°C SRO annealing and test specimens that did not undergo SRO annealing is greater than the maximum measurement variation of 0.2%. Therefore, this experiment shows that 110°C SRO annealing is also effective in generating short-range ordered arrangements.
[0070] As shown above, an effective temperature for SRO annealing is 110°C to 210°C, and a duration of 12 hours is sufficient. Assuming a measurement variability of 0.2%, the absolute value of the rate of change in volume resistivity is 0.02 to 1.06% when the SRO annealing temperature is 110°C to 210°C. When the SRO annealing temperature is 110°C to 190°C, the absolute value of the rate of change in volume resistivity is 0.05 to 1.06%. When the SRO annealing temperature is 150°C to 190°C, the absolute value of the rate of change in volume resistivity is 0.05 to 0.48%.
[0071] <SROアニール> Next, we will explain SRO annealing in more detail.
[0072] Six target temperatures were set for performing SRO annealing: 110°C, 130°C, 150°C, 170°C, 190°C, and 210°C. As shown in Figure 9, the test specimens were heated starting from 50°C and gradually increased to these target temperatures.
[0073] It took approximately 0.2 hours to reach the target temperatures of 110°C and 130°C. It took approximately 0.3 hours to reach the target temperature of 150°C. In the process of reaching the target temperatures of 170°C, 190°C, and 210°C, as described later, it took approximately 0.2 hours to reach 150°C, where short-range ordered sequences begin to be effectively generated. It took approximately 0.4 hours to reach the target temperatures of 170°C, 190°C, and 210°C.
[0074] Once these target temperatures were reached, the test specimens were maintained at the target temperature for 12 hours, including the heating process, and SRO annealing was performed. Volume resistivity was measured at 0 hours, 0.25 hours, 0.5 hours, 0.75 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, and 12 hours after the start of SRO annealing. The rate of change from the volume resistivity at the start of SRO annealing was then calculated as the resistance change rate. The calculation results are shown in Figure 10.
[0075] Furthermore, for specimens subjected to 12 hours of SRO annealing, it was assumed that a sufficient short-range ordered arrangement had been generated, and the volume resistivity of these specimens was normalized to 1. The ratio of this volume resistivity to the volume resistivity of specimens subjected to other treatment times was considered to represent the degree of SRO annealing. The experimental results are shown in Figure 10. These experimental results were also plotted in a graph, which is shown in Figure 11.
[0076] As shown in Figure 11, the rate of change in the annealing progress increases rapidly from the start of heating, and then gradually slows down after reaching the target temperature. The SRO annealing progress increases from 0% to about 70%, and then gradually increases to 80% and 90%. When the annealing progress reaches 80%, it is considered that a short-range ordered arrangement has been generated in most areas of the specimen.
[0077] As shown in the enlarged view in Figure 12, when the SRO annealing temperature is 110°C, it takes approximately 5.6 hours to reach 80% annealing progress after raising the temperature from 50°C. After raising the temperature from 50°C to 110°C and maintaining it at 110°C, it takes approximately 5.4 hours to reach 80% annealing progress.
[0078] When the SRO annealing temperature is 130°C, it takes approximately 4.7 hours to reach 80% annealing progress after raising the temperature from 50°C. After raising the temperature from 50°C to 130°C and maintaining it at 130°C, it takes approximately 4.5 hours to reach 80% annealing progress.
[0079] When the SRO annealing temperature is 150°C, it takes approximately 3.0 hours to reach 80% annealing progress after raising the temperature from 50°C. After raising the temperature from 50°C to 150°C and maintaining that temperature, it takes approximately 2.7 hours to reach 80% annealing progress.
[0080] When the SRO annealing temperature is 170°C, it takes approximately 1.4 hours to reach 80% annealing progress after raising the temperature from 50°C. After raising the temperature from 50°C to 150°C, it takes approximately 1.2 hours to reach 80% annealing progress. After raising the temperature from 50°C to 170°C and maintaining that temperature, it takes approximately 1.0 hour to reach 80% annealing progress.
[0081] When the SRO annealing temperature is 190°C, it takes approximately 1.4 hours to reach 80% annealing progress after raising the temperature from 50°C. After raising the temperature from 50°C to 150°C, it takes approximately 1.2 hours to reach 80% annealing progress. After raising the temperature from 50°C to 190°C and maintaining that temperature, it takes approximately 1.0 hour to reach 80% annealing progress.
[0082] When the SRO annealing temperature is 210°C, it takes approximately 2.9 hours to reach 80% annealing progress after raising the temperature from 50°C. After raising the temperature from 50°C to 150°C, it takes approximately 2.7 hours to reach 80% annealing progress. After raising the temperature from 50°C to 210°C and maintaining it at 210°C, it takes approximately 2.5 hours to reach 80% annealing progress.
[0083] Thus, as the SRO annealing temperature increases from 110°C to 150°C, the annealing progresses more rapidly, reaching its fastest point at 170°C. At an even higher SRO annealing temperature of 190°C, the annealing progress slows down slightly. From these results, it appears that the generation of short-range ordered sequences proceeds effectively in the temperature range above 150°C and below 190°C.
[0084] Based on the experimental results above, when performing SRO annealing in the temperature range of 170°C to 210°C, it takes 1.0 to 2.5 hours to reach 80% annealing progress. More specifically, when performing SRO annealing in the temperature range of 200°C, it is estimated that it takes 1.0 to 2.5 hours to reach 80% annealing progress.
[0085] When the SRO annealing temperature is 170°C, it takes approximately 1.2 hours from the time the temperature reaches 150°C, when SRO annealing begins to work effectively, until the annealing progress reaches 80%.
[0086] When the SRO annealing temperature is 190°C, it takes approximately 1.2 hours from the time the temperature reaches 150°C, when SRO annealing begins to work effectively, until the annealing progress reaches 80%.
[0087] When the SRO annealing temperature is 210°C, it takes approximately 2.7 hours from the time the temperature reaches 150°C, when SRO annealing begins to work effectively, until the annealing progress reaches 80%.
[0088] Furthermore, it takes approximately 1.0 to 5.4 hours for the annealing progress to reach 80% after maintaining the SRO annealing temperature at 110°C to 210°C. As mentioned above, when performing SRO annealing in the temperature range of 170°C to 200°C, it is estimated that it will take 1.0 to 2.5 hours for the annealing progress to reach 80% after maintaining the SRO annealing temperature at 170°C to 200°C. Therefore, it takes approximately 1.0 to 5.4 hours for the annealing progress to reach 80% after maintaining the SRO annealing temperature at 110°C to 200°C.
[0089] After maintaining the SRO annealing temperature at 150°C to 190°C, where it is most effective, it takes approximately 1.0 to 2.7 hours for the annealing progress to reach 80%. Similarly, after maintaining the SRO annealing temperature at 150°C to 200°C, it is estimated that it takes approximately 1.0 to 2.7 hours for the annealing progress to reach 80%.
[0090] Furthermore, experimental results at 170°C and 190°C, where SRO annealing is more effective, show that it only takes about 10, 20, and 30 minutes to achieve 50%, 60%, and 70% annealing progress, respectively.
[0091] <Volume Resistivity> Next, we will explain volume resistivity in more detail.
[0092] Two test specimens were prepared: one that had not undergone SRO annealing and another that had undergone SRO annealing at the target temperature described above. These specimens were left at a high temperature of 150°C for an extended period of time to conduct durability tests. Durability was evaluated by volume resistivity. Volume resistivity was measured at 0 hours, 250 hours, 500 hours, 750 hours, 1000 hours, 1500 hours, and 2000 hours. The measurement results are shown in Figure 13.
[0093] The rate of change from the initial volumetric resistance value was considered as the resistance change rate. The experimental results are shown in Figure 13. These experimental results were also graphed, and this graph is shown in Figure 14.
[0094] As shown in Figure 14, the resistance change rate of the test specimens increases with increasing exposure time at a high temperature of 150°C. However, the magnitude of the resistance change rate differs between test specimens that have not undergone SRO annealing and those that have undergone SRO annealing.
[0095] In test specimens that have not undergone SRO annealing, the absolute value of the resistance change rate exceeds 1.0% when left at a high temperature of 150°C for 2000 hours. In contrast, in test specimens that have undergone SRO annealing, the absolute value of the resistance change rate is kept below 1.0%.
[0096] As shown in Figure 15, the absolute value of the resistance change rate of the test specimen decreases as the SRO annealing temperature increases from 110°C to 210°C. The absolute value of the resistance change rate of test specimens subjected to SRO annealing at temperatures between 150°C and 210°C is kept below 0.3% even when left at a high temperature of 150°C for 2000 hours. The vertical axis in Figure 15 shows the percentage change in volume resistivity from the volume resistivity before SRO annealing to the volume resistivity after 12 hours of SRO annealing. This is the resistance change rate value when SRO annealing is performed for 12 hours, as shown in Figure 10.
[0097] <Volume resistance of a resistor> Next, we will explain the volume resistance of resistor 110.
[0098] As the first group, seven resistors 110 were manufactured by performing SRO annealing at 175°C for 24 hours using the manufacturing method described in Figure 3, without performing the strain-relieving annealing in step S90.
[0099] In the second group, seven resistors 110 were manufactured using the manufacturing method shown in Figure 3, but without performing the SRO annealing in step S70, by performing a strain-relieving annealing at 220°C for 2 hours.
[0100] As the third group, eight resistors 110 were manufactured using the manufacturing method shown in Figure 5, by performing strain-relieving annealing at 220°C for 2 hours and SRO annealing at 175°C for 24 hours.
[0101] As the fourth group, seven resistors 110 were manufactured by performing SRO annealing at 175°C for 24 hours and strain-relieving annealing at 220°C for 2 hours, using the manufacturing method described in Figure 3.
[0102] The resistors 110 from groups 1 through 4 were placed in a constant temperature bath 400 and left at a high temperature of 150°C for 2000 hours. The volume resistance of the shunt resistor 300 was measured at 0 hours, 250 hours, 500 hours, 1000 hours, 1500 hours, and 2000 hours.
[0103] The rate of change from the initial volume resistance was considered as the resistance change rate. The experimental results are shown in Figures 16, 18, 20, and 22. The Ave value in these figures represents the average of the resistance change rates of multiple resistors 110. 3σ indicates the measurement variability. These experimental results were also graphed, and are shown in Figures 17, 19, 21, and 23. In these graphs, the average resistance change rate of multiple resistors 110 is shown by a solid line.
[0104] Figures 16 and 17 show the resistance change rate of the shunt resistor 300 included in the first group of resistors 110. In the first group, the shunt resistor 300 is recrystallized by welding, causing a portion of the short-range ordered arrangement to be destroyed. In addition, the distortion caused by welding has not been removed.
[0105] Therefore, although the resistance change rate is smaller than that of the shunt resistor 300 that has not undergone annealing, the resistance change rate is larger than that of the test specimens when SRO annealing was performed at 170°C and 210°C, as shown in Figure 14. The resistance change rate after 2000 hours is -0.70%, and the measurement variability is 0.15%. The absolute value of the resistance change rate of the shunt resistor 300 of resistor 110 that underwent only SRO annealing is 0.55 to 0.85%.
[0106] Figures 18 and 19 show the resistance change rate of the shunt resistor 300 included in the second group of resistors 110. In the second group, welding-induced distortion is removed, but a short-range ordered arrangement is not generated in the shunt resistor 300.
[0107] Therefore, the longer the test time, the larger the rate of resistance change. The long-term stability of the volume resistance value is compromised. After 2000 hours, the rate of resistance change is -0.40%, and the measurement variability is 0.12%. The absolute value of the rate of resistance change of the shunt resistor 300 of resistor 110, which underwent only strain-relieving annealing, is 0.28 to 0.52%.
[0108] Figures 20 and 21 show the resistance change rate of the shunt resistors 300 included in the third group of resistors 110. In the third group, the shunt resistors 300 are arranged in a short-distance regular pattern, eliminating the distortion caused by welding.
[0109] Therefore, the resistance change is the smallest compared to the other groups. The resistance change rate after 2000 hours is -0.11%, and the measurement variability is 0.09%. The absolute value of the resistance change rate of the shunt resistor 300 of resistor 110, which underwent SRO annealing and strain-relieving annealing after welding, is 0.02 to 0.20%.
[0110] Figures 22 and 23 show the resistance change rate of the shunt resistor 300 included in the fourth group of resistors 110. In the fourth group, the shunt resistor 300 is recrystallized by welding, causing a portion of the short-range ordered arrangement to be destroyed.
[0111] Therefore, the resistance change rate is slightly larger than that of the third group, which underwent SRO annealing after welding. The resistance change rate after 2000 hours was -0.18%, and the measurement variability was 0.06%. The absolute value of the resistance change rate of the shunt resistor 300 of resistor 110, which underwent SRO annealing before welding and distortion-relieving annealing after welding, was 0.12 to 0.24%.
[0112] As shown above, in the case of resistor 110 that has undergone both SRO annealing and strain-relieving annealing, the absolute value of the resistance change rate of the shunt resistor 300 is suppressed to 0.02-0.24%. This resistance change rate is smaller than the absolute value of the resistance change rate of the shunt resistor 300, which is 0.28-0.52%, in the case of resistor 110 that has undergone only strain-relieving annealing. This comparison shows that SRO annealing is effective.
[0113] <Effects and Effects> As explained above, performing SRO annealing in a temperature range of 110°C to 210°C generates a short-range ordered arrangement in the shunt resistor 300. However, considering the distinction from strain-relieving annealing performed at temperatures above 200°C, the temperature range for SRO annealing is 110°C to less than 200°C. The effects within this temperature range will be explained below.
[0114] When SRO annealing is performed in a temperature range of 110°C to less than 200°C, a short-range ordered arrangement is generated in the shunt resistor 300. This suppresses the large rate of change in the volume resistivity of the shunt resistor 300, even when it is left in a high-temperature environment for a long period of time.
[0115] SRO annealing is performed by maintaining a temperature range of 110°C to less than 200°C for 1.0 to 5.4 hours. This process promotes the generation of short-range ordered sequences in the shunt resistance 300 by more than 80%.
[0116] SRO annealing is performed in a temperature range of 150°C to less than 190°C. This efficiently generates a short-range ordered arrangement on the shunt resistor 300.
[0117] SRO annealing is performed by maintaining a temperature range of 150°C to less than 190°C for 1.0 to 2.7 hours. This process promotes the generation of short-range ordered sequences in the shunt resistance 300 by more than 80%.
[0118] A resistor 110, comprising a shunt resistor 300 and a metal busbar 200, is subjected to SRO annealing in a temperature range of 110°C to less than 200°C. Simultaneously, the resistor 110 is subjected to strain-relieving annealing at a temperature of 200°C or higher. This suppresses the rate of change in the volume resistivity of the shunt resistor 300 of the resistor 110, even when exposed to high-temperature environments for extended periods. Specifically, it is expected that the absolute value of the rate of change in the volume resistivity of the shunt resistor 300 after being kept at a constant temperature of 150°C for 2000 hours will be 0.02 to 0.24%.
[0119] After welding the shunt resistor 300 to the metal busbar 200, SRO annealing is performed on the resistor 110. This suppresses the destruction of the short-range ordered arrangement formed on the shunt resistor 300 by welding. In this case, it is expected that the absolute value of the rate of change in the volume resistivity of the shunt resistor 300 after constant temperature holding at 150°C for 2000 hours will be 0.02 to 0.20%.
[0120] <Variation> The disclosure in this specification is not limited to the exemplary embodiments. The disclosure encompasses the exemplary embodiments and variations thereof by those skilled in the art. For example, the disclosure is not limited to the combinations of parts and elements shown in the embodiments, but can be implemented in various variations. The disclosure can be implemented in a variety of combinations. The disclosure may have additional parts that can be added to the embodiments. The disclosure encompasses embodiments in which parts and elements have been omitted. The disclosure encompasses substitutions or combinations of parts and elements between one embodiment and another. The scope of the disclosed technical field is not limited to the descriptions of the embodiments. The scope of the disclosed technical field is indicated by the claims and should be understood to include all modifications within the meaning and scope equivalent to the claims.
[0121] <Disclosure of Technical Ideas> This specification discloses several technical concepts, as listed in the following paragraphs. Some paragraphs are written in a multiple dependent form, where subsequent paragraphs optionally refer to preceding paragraphs. Furthermore, some paragraphs are written in a multiple dependent form, referring to other multiple dependent forms. These paragraphs written in multiple dependent forms define several technical concepts.
[0122] <Technical philosophy 1> A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. A method for manufacturing a copper alloy sheet, comprising holding the cold-formed body from which residual strain has been removed in a temperature range of 110°C or more and less than 200°C.
[0123] <Technical philosophy 2> A method for manufacturing a copper alloy sheet material according to Technical Concept 1, comprising holding the cold-formed body from which the residual strain has been removed at a temperature range of 110°C to less than 200°C for 1.0 to 5.4 hours.
[0124] <Technical philosophy 3> A method for manufacturing a copper alloy sheet material according to technical concept 1, wherein the cold-formed body from which the residual strain has been removed is held in a temperature range of 150°C or more and less than 200°C.
[0125] <Technical philosophy 4> A method for manufacturing a copper alloy sheet material according to technical concept 3, comprising holding the cold-formed body from which the residual strain has been removed at a temperature range of 150°C or more and less than 200°C for 1.0 to 2.7 hours.
[0126] <Technical philosophy 5> A method for manufacturing a copper alloy sheet material according to technical concept 1, wherein the cold-formed body from which the residual strain has been removed is held in a temperature range of 150°C or more and less than 190°C.
[0127] <Technical philosophy 6> A method for manufacturing a copper alloy sheet material according to technical concept 5, comprising holding the cold-formed body from which residual strain has been removed at a temperature range of 150°C to less than 190°C for 1.0 to 2.7 hours.
[0128] <Technical philosophy 7> A method for manufacturing a copper alloy sheet material according to any one of technical ideas 1 to 6, comprising generating a short-range regular arrangement in the cold-formed body from which residual strain has been removed.
[0129] <Technical philosophy 8> A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. A method for manufacturing a copper alloy sheet, comprising generating a short-distance regular arrangement in the cold-formed body from which residual strain has been removed.
[0130] <Technical philosophy 9> A method for manufacturing a copper alloy sheet material according to any one of technical ideas 1 to 8, wherein the internal structure of the ingot is made uniform by performing a homogenization heat treatment on the ingot.
[0131] <Technical Thought 10> A method for manufacturing a copper alloy sheet material according to any one of technical ideas 1 to 9, wherein the cold-formed body is held in a temperature range of 500°C to 850°C to remove residual strain generated in the cold-formed body by cold rolling.
[0132] <Technical Thought 11> A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. The cold-formed body from which the residual strain has been removed is held in a temperature range of 110°C to less than 200°C to produce a copper alloy sheet material (300). A resistor (110) is manufactured by welding the copper alloy plate material to a metal busbar (200). A method for manufacturing a resistor, comprising holding the resistor at a temperature of 200°C or higher to remove the distortion caused in the copper alloy plate material by welding.
[0133] <Technical Thought 12> A method for manufacturing a resistor according to technical concept 11, wherein the cold-formed body from which residual strain has been removed is held at a temperature range of 110°C or more and less than 200°C for 1.0 to 5.4 hours to produce the copper alloy plate material.
[0134] <Technical Thought 13> A method for manufacturing a resistor according to technical concept 11, wherein the cold-formed body from which residual strain has been removed is held in a temperature range of 150°C or more and less than 200°C to produce the copper alloy plate material.
[0135] <Technical Thought 14> A method for manufacturing a resistor according to technical concept 13, wherein the cold-formed body from which residual strain has been removed is held at a temperature range of 150°C or more and less than 200°C for 1.0 to 2.7 hours to produce the copper alloy plate material.
[0136] <Technical Thought 15> A method for manufacturing a resistor according to technical concept 11, wherein the cold-formed body from which residual strain has been removed is held in a temperature range of 150°C or more and less than 190°C to manufacture the copper alloy plate material.
[0137] <Technical Thought 16> A method for manufacturing a resistor according to technical concept 15, wherein the cold-formed body from which residual strain has been removed is held at a temperature range of 150°C or more and less than 190°C for 1.0 to 2.7 hours to produce the copper alloy sheet material.
[0138] <Technical Thought 17> A method for manufacturing a resistor according to any one of technical ideas 11 to 16, comprising generating a short-distance regular arrangement in the cold-formed body from which residual strain has been removed.
[0139] <Technical Thought 18> A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. A copper alloy sheet material (300) is manufactured in which a short-distance regular arrangement is generated in the cold-formed body from which the residual strain has been removed. A resistor (110) is manufactured by welding the copper alloy plate material to a metal busbar (200). A method for manufacturing a resistor, comprising holding the resistor at a temperature of 200°C or higher to remove the distortion caused in the copper alloy plate material by welding.
[0140] <Technical Thought 19> A method for manufacturing a resistor according to any one of the technical ideas 11 to 18, wherein the internal structure of the ingot is made uniform by performing a homogenization heat treatment on the ingot.
[0141] <Technical Thought 20> A method for manufacturing a resistor according to any one of the technical concepts 11 to 19, wherein the cold-formed body is held in a temperature range of 500°C to 850°C to remove residual strain generated in the cold-formed body by cold rolling.
[0142] <Technical Thought 21> A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, a copper alloy sheet material (300) is produced from which residual strain generated in the cold-formed body by cold rolling has been removed. A resistor (110) is manufactured by welding the copper alloy plate material to a metal busbar (200). By holding the resistor at a temperature of 200°C or higher, the distortion caused in the copper alloy plate material by welding is removed. A method for manufacturing a resistor, comprising maintaining the resistor in a temperature range of 110°C or more and less than 200°C.
[0143] <Technical Thought 22> A method for manufacturing a resistor according to technical concept 21, comprising holding the resistor in a temperature range of 110°C or higher and less than 200°C for 1.0 to 5.4 hours.
[0144] <Technical Thought 23> A method for manufacturing a resistor according to technical concept 21, wherein the resistor is maintained in a temperature range of 150°C or more and less than 200°C.
[0145] <Technical Thought 24> A method for manufacturing a resistor according to technical concept 23, comprising holding the resistor in a temperature range of 150°C or more and less than 200°C for 1.0 to 2.7 hours.
[0146] <Technical Thought 25> A method for manufacturing a resistor according to technical concept 21, wherein the resistor is maintained in a temperature range of 150°C or more and less than 190°C.
[0147] <Technical Thought 26> A method for manufacturing a resistor according to technical concept 25, comprising holding the resistor in a temperature range of 150°C or higher and less than 190°C for 1.0 to 2.7 hours.
[0148] <Technical Thought 27> A method for manufacturing a resistor according to any one of technical ideas 21 to 26, comprising generating a short-range regular arrangement on the copper alloy plate material to which the metal busbars are welded.
[0149] <Technical Thought 28> A copper alloy material is prepared containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, a copper alloy sheet material (300) is produced from which residual strain generated in the cold-formed body by cold rolling has been removed. A resistor (110) is manufactured by welding the copper alloy plate material to a metal busbar (200). By holding the resistor at a temperature of 200°C or higher, the distortion caused in the copper alloy plate material by welding is removed. A method for manufacturing a resistor, comprising generating a short-distance ordered arrangement on the aforementioned copper alloy plate material.
[0150] <Technical Thought 29> A method for manufacturing a resistor according to any one of the technical ideas 21 to 28, wherein the internal structure of the ingot is made uniform by performing a homogenization heat treatment on the ingot.
[0151] <Technical Thought 30> A method for manufacturing a resistor according to any one of the technical concepts 21 to 29, wherein the cold-formed body is held in a temperature range of 500°C to 850°C to remove residual strain generated in the cold-formed body by cold rolling.
[0152] <Technical Thought 31> It contains 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. A copper alloy plate material in which the absolute value of the rate of change in volume resistivity is 0.05 to 1.06% when kept at a constant temperature of 150°C for 2000 hours.
[0153] <Technical Thought 32> A copper alloy plate material as described in Technical Idea 31, wherein the absolute value of the rate of change in volume resistivity when maintained at a constant temperature of 150°C for 2000 hours is 0.05 to 0.48%.
[0154] <Technical Thought 33> A copper alloy plate material (300) containing 10.0-14.0 mass% Mn, 1.0-4.0 mass% Ni, 0-0.10 mass% Al, and 0-0.10 mass% Mg, with the remainder being Cu and unavoidable impurities, The copper alloy plate material is welded together to form a metal busbar (200), A resistor whose absolute value of the rate of change in volume resistivity is 0.02 to 0.24% when kept at a constant temperature of 150°C for 2000 hours. [Explanation of Symbols]
[0155] 10...Control module, 20...Sensor device, 30...Control device, 100...Current sensor, 200...Metal busbar, 300...Shunt resistor
Claims
1. A copper alloy material is prepared containing 10.0 to 14.0 mass% Mn, 1.0 to 4.0 mass% Ni, 0 to 0.10 mass% Al, and 0 to 0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. A method for manufacturing a copper alloy sheet, comprising holding the cold-formed body from which residual strain has been removed in a temperature range of 110°C or more and less than 200°C.
2. A method for manufacturing a copper alloy sheet material according to claim 1, wherein the cold-formed body from which the residual strain has been removed is held at a temperature range of 110°C or more and less than 200°C for 1.0 to 5.4 hours.
3. A method for manufacturing a copper alloy sheet material according to claim 1, wherein the cold-formed body from which the residual strain has been removed is held in a temperature range of 150°C or more and less than 200°C.
4. The method for manufacturing a copper alloy sheet material according to claim 3, wherein the cold-formed body from which the residual strain has been removed is held at a temperature range of 150°C or more and less than 200°C for 1.0 to 2.7 hours.
5. A method for manufacturing a copper alloy sheet material according to claim 1, wherein the cold-formed body from which the residual strain has been removed is held in a temperature range of 150°C or more and less than 190°C.
6. The method for manufacturing a copper alloy sheet material according to claim 5, wherein the cold-formed body from which the residual strain has been removed is held at a temperature range of 150°C or more and less than 190°C for 1.0 to 2.7 hours.
7. A method for manufacturing a copper alloy sheet material according to any one of claims 1 to 6, comprising generating a short-distance regular arrangement in the cold-formed body from which residual strain has been removed.
8. A copper alloy material is prepared containing 10.0 to 14.0 mass% Mn, 1.0 to 4.0 mass% Ni, 0 to 0.10 mass% Al, and 0 to 0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. A method for manufacturing a copper alloy sheet, comprising generating a short-distance regular arrangement in the cold-formed body from which residual strain has been removed.
9. A method for manufacturing a copper alloy plate according to claim 1 or claim 8, wherein the internal structure of the ingot is made uniform by performing a homogenization heat treatment on the ingot.
10. A method for manufacturing a copper alloy sheet material according to claim 1 or claim 8, wherein the cold-formed body is held in a temperature range of 500°C to 850°C to remove residual strain generated in the cold-formed body by cold rolling.
11. A copper alloy material is prepared containing 10.0 to 14.0 mass% Mn, 1.0 to 4.0 mass% Ni, 0 to 0.10 mass% Al, and 0 to 0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. The cold-formed body from which the residual strain has been removed is held in a temperature range of 110°C to less than 200°C to produce a copper alloy sheet material (300). A resistor (110) is manufactured by welding the copper alloy plate material to a metal busbar (200). A method for manufacturing a resistor, comprising holding the resistor at a temperature of 200°C or higher to remove the distortion caused in the copper alloy plate material by welding.
12. The method for manufacturing a resistor according to claim 11, wherein the cold-formed body from which residual strain has been removed is held at a temperature range of 110°C or more and less than 200°C for 1.0 to 5.4 hours to produce the copper alloy plate material.
13. The method for manufacturing a resistor according to claim 11, wherein the cold-formed body from which the residual strain has been removed is held in a temperature range of 150°C or more and less than 200°C to manufacture the copper alloy plate material.
14. The method for manufacturing a resistor according to claim 13, wherein the cold-formed body from which residual strain has been removed is held at a temperature range of 150°C or more and less than 200°C for 1.0 to 2.7 hours to produce the copper alloy plate material.
15. The method for manufacturing a resistor according to claim 11, wherein the cold-formed body from which the residual strain has been removed is held in a temperature range of 150°C or more and less than 190°C to manufacture the copper alloy plate material.
16. The method for manufacturing a resistor according to claim 15, wherein the cold-formed body from which residual strain has been removed is held at a temperature range of 150°C or more and less than 190°C for 1.0 to 2.7 hours to produce the copper alloy plate material.
17. A method for manufacturing a resistor according to any one of claims 11 to 16, comprising generating a short-distance regular arrangement in the cold-formed body from which residual strain has been removed.
18. A copper alloy material is prepared containing 10.0 to 14.0 mass% Mn, 1.0 to 4.0 mass% Ni, 0 to 0.10 mass% Al, and 0 to 0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, residual strain generated in the cold-formed body due to cold rolling is removed. A copper alloy sheet material (300) is manufactured in which a short-distance regular arrangement is generated in the cold-formed body from which the residual strain has been removed. A resistor (110) is manufactured by welding the copper alloy plate material to a metal busbar (200). A method for manufacturing a resistor, comprising holding the resistor at a temperature of 200°C or higher to remove the distortion caused in the copper alloy plate material by welding.
19. A method for manufacturing a resistor according to claim 11 or claim 18, wherein the internal structure of the ingot is made uniform by performing a homogenization heat treatment on the ingot.
20. A method for manufacturing a resistor according to claim 11 or claim 18, wherein the cold-formed body is held in a temperature range of 500°C to 850°C to remove residual strain generated in the cold-formed body by cold rolling.
21. A copper alloy material is prepared containing 10.0 to 14.0 mass% Mn, 1.0 to 4.0 mass% Ni, 0 to 0.10 mass% Al, and 0 to 0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, a copper alloy sheet material (300) is produced from which residual strain generated in the cold-formed body by cold rolling has been removed. A resistor (110) is manufactured by welding the copper alloy plate material to a metal busbar (200). By holding the resistor at 200°C or higher, the distortion caused in the copper alloy plate material by welding is removed. A method for manufacturing a resistor, comprising maintaining the resistor in a temperature range of 110°C or more and less than 200°C.
22. The method for manufacturing a resistor according to claim 21, wherein the resistor is held in a temperature range of 110°C or more and less than 200°C for 1.0 to 5.4 hours.
23. The method for manufacturing a resistor according to claim 21, wherein the resistor is maintained in a temperature range of 150°C or more and less than 200°C.
24. The method for manufacturing a resistor according to claim 23, wherein the resistor is held in a temperature range of 150°C or more and less than 200°C for 1.0 to 2.7 hours.
25. The method for manufacturing a resistor according to claim 21, wherein the resistor is maintained in a temperature range of 150°C or more and less than 190°C.
26. A method for manufacturing a resistor according to claim 25, wherein the resistor is held in a temperature range of 150°C or more and less than 190°C for 1.0 to 2.7 hours.
27. A method for manufacturing a resistor according to any one of claims 21 to 26, wherein a short-distance regular arrangement is generated on the copper alloy plate material to which the metal busbar is welded.
28. A copper alloy material is prepared containing 10.0 to 14.0 mass% Mn, 1.0 to 4.0 mass% Ni, 0 to 0.10 mass% Al, and 0 to 0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. The copper alloy material is melted and cast to produce an ingot. A hot-formed body is produced by hot-rolling the aforementioned ingot. By performing cold rolling on the aforementioned hot-formed body, a cold-formed body is produced. By holding the cold-formed body within a predetermined temperature range, a copper alloy sheet material (300) is produced from which residual strain generated in the cold-formed body by cold rolling has been removed. A resistor (110) is manufactured by welding the copper alloy plate material to a metal busbar (200). By holding the resistor at 200°C or higher, the distortion caused in the copper alloy plate material by welding is removed. A method for manufacturing a resistor, comprising generating a short-distance ordered arrangement on the aforementioned copper alloy plate material.
29. A method for manufacturing a resistor according to claim 21 or claim 28, wherein the internal structure of the ingot is made uniform by performing a homogenization heat treatment on the ingot.
30. A method for manufacturing a resistor according to claim 21 or 28, wherein the cold-formed body is held in a temperature range of 500°C to 850°C to remove residual strain generated in the cold-formed body by cold rolling.
31. It contains 10.0 to 14.0 mass% Mn, 1.0 to 4.0 mass% Ni, 0 to 0.10 mass% Al, and 0 to 0.10 mass% Mg, with the remainder being Cu and unavoidable impurities. A copper alloy plate material in which the absolute value of the rate of change in volume resistivity is 0.05 to 1.06% when kept at a constant temperature of 150°C for 2000 hours.
32. The copper alloy plate material according to claim 31, wherein the absolute value of the rate of change of the volume resistivity when the material is kept at a constant temperature of 150°C for 2000 hours is 0.05 to 0.48%.
33. A copper alloy plate material (300) containing 10.0 to 14.0 mass% Mn, 1.0 to 4.0 mass% Ni, 0 to 0.10 mass% Al, and 0 to 0.10 mass% Mg, with the remainder being Cu and unavoidable impurities, The copper alloy plate material is welded to a metal busbar (200), A resistor whose absolute value of the rate of change in volume resistivity is 0.02 to 0.24% when kept at a constant temperature of 150°C for 2000 hours.
Citation Information
Patent Citations