NCM cathode particles coated with LLZO and glass phase
Coating NCM particles with a glass phase and LLZO, combined with carbon nanotubes and amorphous carbon, addresses interface side reactions and enhances conductivity, improving battery performance and stability.
Patent Information
- Application Number
- JP2024002748U
- Authority / Receiving Office
- JP · JP
- Patent Type
- Utility models
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2034-08-16
AI Technical Summary
Conventional positive electrode particles in batteries, particularly those made of NCM materials, suffer from side reactions at their interfaces, leading to low electron conductivity and reduced battery effectiveness.
Coating NCM particles with a glass phase and LLZO fine particles, and incorporating carbon nanotubes and nanoscale amorphous carbon to create a stable electron and lithium ion conduction path, reducing interfacial resistance and enhancing conductivity.
The coating and composite structure improve charge and discharge performance, increase mechanical stability, and extend battery life by providing suitable paths for lithium ions and electrons, while reducing cobalt usage and manufacturing costs.
Smart Images

Figure 0003248737000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to positive electrode particles, and more particularly to NCM positive electrode particles coated with LLZO and glass phases. [Background technology]
[0002] A battery is mainly composed of a positive electrode and a negative electrode disposed in an electrolyte. The positive electrode is formed by mixing and stirring many positive electrode conductive units (positive electrode materials such as lithium cobalt oxide) and dispersing them in a slurry. In general, the positive electrode conductive units are first mixed and stirred with the conductive slurry, then applied to an electrode sheet, and assembled into a battery. Therefore, since each of the positive electrode conductive units is connected via the conductive slurry, the conductive slurry has conductive auxiliary properties or conductivity, which allows free electrons to migrate in different positive electrode conductive units, and eliminates the need to consume excessive energy due to internal resistance, thereby achieving the purpose of effective conduction. Therefore, in order to adjust the conductivity of the slurry, it is necessary to manufacture the slurry using a specific conductive material. Summary of the Invention [Problem to be solved by the invention]
[0003] In order to improve the electrical conductivity, a plurality of positive electrode particles are filled in the positive electrode slurry, the material of the positive electrode particles being selected from lithium nickel manganese cobalt oxide (NCM), lithium manganese iron phosphate (LMFP), or a mixture thereof, and the positive electrode particles are distributed in the positive electrode slurry. However, the positive electrode particles in the prior art are prone to side reactions at their interfaces, shortening the service life of the positive electrode and lowering the overall efficiency of the battery due to low electronic conductivity.
[0004] The present invention has been made to solve the above problems of the prior art. That is, the object of the present invention is to provide an NCM positive electrode particle that is coated with LLZO and a glass phase. [Means for solving the problem]
[0005] In order to solve the above problems, the present invention provides an NCM positive electrode particle coated with LLZO and a glass phase in one embodiment, in which the outer surface of the NCM large particle is coated with a glass phase, and the glass phase can prevent the NCM large particle from directly contacting the electrolyte, suppressing side reactions at the interface, and at the same time reducing the interface resistance when lithium ions enter and exit the NCM large particle, improving the multiplying charge and discharge performance, accommodating the volume change caused by charge and discharge, improving the mechanical properties of the powder, and reducing crushing. The present invention coats the NCM large particle with a number of LLZO fine particles, and the LLZO fine particles have the ability to accommodate and uniformly guide lithium ions. When lithium ions pass through the positive electrode, they are guided by the LLZO fine particles and disperse the lithium ion passages, so the present invention provides a more suitable passage for lithium ions. In the present invention, the outer surface of the NCM large particle that covers the LLZO fine particles is further coated with a number of carbon nanotubes and nano-scale amorphous carbon, allowing electrons to be conducted on the composite NCM particle, and the nano-scale amorphous carbon is filled between the carbon nanotubes to form a complete electron conduction path, thereby providing stability to the entire cathode structure and reducing the amount of cobalt used.
[0006] At least the following points will become apparent from the following specification and drawings. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a schematic diagram showing a positive electrode particle according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic diagram of a positive electrode according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing a composite NCM particle according to an embodiment of the present invention. [Figure 4] It is a configuration diagram showing composite NCM particles and short-chain carbon nanotubes according to an embodiment of the present invention. [Diagram 5] It is a configuration diagram showing a positive electrode particle coated with a carbon nanotube according to an embodiment of the present invention.
Mode for Carrying Out the Invention
[0008] Hereinafter, the present invention will be described through embodiments of the invention. However, the following embodiments do not limit the invention according to the claims. Also, not all combinations of features described in the embodiments are essential for the solution means of the invention.
[0009] First, an example of a specific embodiment of NCM positive electrode particles coated with LLZO and a glass phase of the present invention will be described with reference to FIGS. 1 to 5.
[0010] NCM positive electrode particles coated with LLZO and a glass phase according to an embodiment of the present invention are such that NCM positive electrode particles coated with LLZO and a glass phase are mainly used for a positive electrode 100 of general solid or solid batteries (see FIG. 2). The positive electrode 100 includes a positive electrode substrate 10 and a positive electrode slurry layer 12 applied to the positive electrode substrate 10. The positive electrode slurry layer 12 includes a positive electrode slurry 14 having a binder and a plurality of positive electrode particles 200 distributed in the positive electrode slurry 14. The total weight of the plurality of positive electrode particles 200 accounts for 80 wt% to 98 wt% of the weight of the positive electrode slurry layer 12.
[0011] The NCM positive electrode particles coated with LLZO and a glass phase according to the present invention are each of the positive electrode particles 200 and mainly have the following configuration.
[0012] <NCM (lithium nickel manganese cobalt oxide) large particles 22> The size of the NCM large particles 22 ranges between 3 μm and 5 μm and has a single crystal structure. As shown in Figure 1, the NCM large particles 22 have an irregular cubic shape. NCM is a ternary oxide.
[0013] The outer surface of the NCM large particle 22 is covered with a glass phase 25, and the glass phase 25 covers a part or the whole (preferably the whole) of the outer surface of the NCM large particle. As shown in FIG. 3, an NCM particle 250 having a glass phase as a whole is formed. The glass phase 25 has a lithium ion conductivity of 10 -5 The glass phase 25 is composed of an amorphous oxide or non-oxide solid electrolyte having a crystallinity higher than 10 ... x where R is at least one element selected from boron (B), aluminum (Al), silicon (Si), germanium (Ge), phosphorus (P), and arsenic (As), and x=1 to 3; lithium halides or lithium halogen-oxides (e.g., Li-MO, where M is at least one element selected from the halogen elements fluorine (F), chlorine (Cl), bromine (Br), and iodine (I)); lithium sulfides (e.g., Li2S-P2S5); amorphous oxide-based solid electrolytes (e.g., amorphous perovskite-based solid electrolytes (Li-La-Ti-O, LLTO)); garnet-based solid electrolytes (Li-La-Zr-O, LLZO); or lithium phosphorus oxynitride (LiPON).
[0014] The thickness of the glass phase 25 ranges between 5 nm and 100 nm.
[0015] The glass phase 25 can prevent the NCM large particles 22 from directly contacting the electrolyte, suppressing side reactions at the interface, and at the same time reducing the interface resistance when lithium ions enter and exit the NCM large particles 22, improving the charge / discharge performance. The glass phase 25 can accommodate the volume that changes with charge and discharge, improving the mechanical properties of the powder and reducing crushing.
[0016] A plurality of LLZO particles 24 are distributed in the glass phase 25 or on the surface of the glass phase 25, and a composite NCM particle 20 is formed by the NCM large particle 22, the glass phase 25, and the plurality of LLZO particles 24. The size of the NCM large particle 22 is larger than the size of each of the LLZO particles 24. Each of the LLZO particles 24 is lithium lanthanum zirconium oxide (Li7La3Zr2O 12 , LLZO) or lithium lanthanum zirconium oxide doped with at least one metal element (e.g., Li 6.2 Ga 0.8 La3Zr2O 12 , gallium (Ga)-doped lithium lanthanum zirconium oxide, or aluminum (Al)-doped or barium (Ba)-doped lithium lanthanum zirconium oxide). The lateral size of each of the LLZO particles 24 (i.e., the size along the direction of the sphere of the corresponding NCM large particle 22) ranges between 50 nm and 300 nm. The multiple LLZO particles 24 are distributed in the glass phase 25 by sintering, and each of the LLZO particles 24 becomes shorter in its longitudinal size (i.e., the size perpendicular to the lateral direction) and wider in its lateral size after sintering, but the total volume does not change. In the composite NCM particle 20, the total weight of the multiple LLZO particles 24 and the weight ratio of the NCM particle 250 having the glass phase ranges between 0.2% and 2%.
[0017] In the present invention, a plurality of LLZO particles 24 are attached to the inside and outside of the glass phase 25 on the outer surface of the NCM large particles 22, and the ion guiding ability of the LLZO particles 24 for lithium ions is much higher than that of the NCM large particles 22, and no side reactions occur with the lithium ions, so that when the lithium ions pass through the positive electrode 100, the dispersed plurality of LLZO particles 24 can guide and disperse the paths of the lithium ions. In this way, the present invention allows the lithium ions to have more suitable paths, greatly improving the overall efficiency of the battery, and preventing side reactions, thereby extending the service life of the entire battery.
[0018] Preferably, each of the LLZO particles 24 is composed of at least one element selected from Ga-LLZO (Ga-doped LLZO, gallium-doped lithium lanthanum zirconium oxide), Cu-LLZO (Cu-doped LLZO, copper-doped lithium lanthanum zirconium oxide), Ta-LLZO (Ta-doped LLZO, tantalum-doped lithium lanthanum zirconium oxide), Sr-LLZO (Sr-doped LLZO, strontium-doped lithium lanthanum zirconium oxide), and Al-LLZO (Al-doped LLZO, aluminum-doped lithium lanthanum zirconium oxide).
[0019] Preferably, each of the LLZO particles 24 is Cu. a ,X b -LLZO, a ,X b-LLZO is a lithium lanthanum zirconium oxide doped with copper and an element X, where X is selected from gallium (Ga), tantalum (Ta), strontium (Sr), barium (Ba), and aluminum (Al), and a>0 and b>0. Preferably, a+b=0.25-0.8, and a>0.1. Although the technique of doping LLZO with copper is very difficult, it further stabilizes the entire structure, makes the lithium ion channel smoother, and increases the sintering speed and manufacturing cost. In addition, when the LLZO particles 24 are exposed to air, the formation of lithium carbonate (Li2CO3) is reduced, and the surface stability of the entire material is improved during sintering.
[0020] Since both the LLZO fine particles 24 and the NCM large particles 22 have a crystalline structure, they have good overall stability and are not easily released or dissociated, thereby increasing the voltage of the entire battery.
[0021] 4 and 5, the present invention further includes a plurality of carbon nanotubes (CNTs) 30 covering the outer periphery of the composite NCM particle 20. The carbon nanotubes 30 and the composite NCM particle 20 form a positive electrode particle 300 covering the carbon nanotubes (see FIG. 5).
[0022] The carbon nanotubes 30 according to the present invention include a plurality of short carbon nanotubes 32 and a plurality of long carbon nanotubes 34, each of the short carbon nanotubes 32 having a length ranging from 0.5 μm to 1 μm, and each of the long carbon nanotubes 34 having a length ranging from 3 μm to 8 μm. The total weight of the carbon nanotubes 30 and the weight ratio of the composite NCM particles 20 ranges from 0.1% to 2%.
[0023] As shown in Figure 1, a number of the short-chain carbon nanotubes 32 are used to bridge the LLZO particulates 24 and the NCM large particles 22 (see Figure 4). A number of the long-chain carbon nanotubes 34 are used to coat the composite NCM particle 20 (see Figure 1), so that the entire composite NCM particle 20 has good electrical conductivity. Carbon nanotubes are very good conductive materials and help conduct electrons throughout the cathode 100. Meanwhile, the LLZO particulates 24 help conduct lithium ions.
[0024] The carbon nanotubes 30 are used to increase the electronic conductivity, i.e., conductive bridges are formed between the different LLZO particles 24, allowing electrons to be conducted on the composite NCM particles 20. Carbon nanotubes have extremely high electrical conductivity, allowing electrons to be conducted between the different LLZO particles 24 and the NCM large particles 22 through the carbon nanotubes 30, thereby increasing the overall electrical conductivity of the positive electrode 100. The carbon nanotubes 30 can form bridges with different numbers of layers on the LLZO particles 24 and the NCM large particles 22. The more carbon nanotubes 30 are added, the higher the overall electrical conductivity of the positive electrode 100.
[0025] The advantage of using carbon nanotubes in the present invention is that lithium ions are more easily stabilized between the carbon nanotubes, and the cathode slurry of the present invention has a large number of solid lithium ions, which increases the overall conductivity of lithium ions. Also, electrons are more easily fixed between the short-chain carbon nanotubes 32 and the long-chain carbon nanotubes 34, which increases the overall conductivity of lithium ions. In addition, the extremely high ion conductivity contributes to the high-speed charging and discharging of the entire battery, and further reduces the amount of cobalt used, which reduces the overall manufacturing cost.
[0026] A plurality of nanoscale amorphous carbons 35 cover the outside of the positive electrode particles 300 covering the carbon nanotubes, and the nanoscale amorphous carbons 35 and the positive electrode particles 300 covering the carbon nanotubes form a positive electrode particle 350 covering a carbon material. Each of the nanoscale amorphous carbons 35 is mainly located in a gap formed by the intersection of the carbon nanotubes 30. Preferably, the nanoscale amorphous carbon 35 is amorphous carbon of a super P conductive additive. The size of the nanoscale amorphous carbon 35 is in the range of 20 nm to 100 nm. The total weight of the nanoscale amorphous carbon 35 and the weight ratio of the composite NCM particles 20 are in the range of 0.1% to 2%. The nanoscale amorphous carbon 35 and the carbon nanotubes 30 are both conductive additives. Since the nanoscale amorphous carbon 35 is in particle form and the carbon nanotubes 30 are elongated, gaps are formed between the carbon nanotubes 30 that cross vertically and horizontally, and electric current cannot be conducted through these gaps. Therefore, in the present invention, the nanoscale amorphous carbon 35 is placed in the gaps, so that electric charges can be conducted between different carbon nanotubes 30 by bridging the nanoscale amorphous carbon 35, further improving the electric current conduction efficiency.
[0027] The weight ratio of the total weight of the carbon nanotubes 30 and the nanoscale amorphous carbons 35 to the weight of the composite NCM particles 20 is (0.09-3):100.
[0028] The weight ratio of the plurality of carbon nanotubes 30, the plurality of nanoscale amorphous carbons 35, and the composite NCM particles 20 is 0.5:1:100.
[0029] By applying the above-mentioned structure, the positive electrode 100 can receive more lithium ions, which allows the positive electrode 100 to receive a higher voltage. For example, if a battery originally has a voltage of 4.3V, the voltage can be increased from 4.3V to 4.5V by applying the design of the present invention.
[0030] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means devised in different embodiments are also included in the technical scope of the present invention. [Explanation of symbols]
[0031] 10 Positive substrate 12 Positive electrode slurry layer 14 Positive electrode slurry 20 Composite NCM particles 22 NCM large particles 24 LLZO fine particles 25 Glass phase 30 Carbon Nanotubes 32 Short-Chain Carbon Nanotubes 34 Long-chain carbon nanotubes 35 Nanoscale amorphous carbon 100 positive electrode 200 Positive Particles 250 NCM particles with glass phase 300 Positive electrode particles coated with carbon nanotubes 350 Positive electrode particles that cover carbon materials
Claims
1. A NCM positive electrode particle having a LLZO and glass phase coating, the positive electrode particle being present in a positive electrode slurry layer of a positive electrode of a solid or solid-state battery, the NCM positive electrode particle having a LLZO and glass phase coating comprising: The present invention relates to a method for producing a lithium nickel manganese cobalt oxide (NCM) large particle having an irregular cubic shape, the NCM large particle having a glass phase on its exterior, the glass phase covering a part or all of the exterior surface of the NCM large particle to form an NCM particle having a glass phase as a whole, the glass phase being used to prevent the NCM large particle from directly contacting an electrolyte and suppressing side reactions at the interface, and at the same time reducing the interface resistance when lithium ions enter and exit the NCM large particle; A plurality of LLZO particles, each of which is distributed within the glass phase or on the surface of the glass phase, the NCM large particles, the glass phase, and the plurality of LLZO particles form a composite NCM particle, the size of the NCM large particles being larger than the size of each of the LLZO particles, and each of the LLZO particles being lithium lanthanum zirconium oxide (Li 7 La 3 Zr 2 O 12 and a plurality of LLZO particles formed of lithium lanthanum zirconium oxide (LLZO) or lithium lanthanum zirconium oxide doped with at least one metal element, The NCM positive electrode particles are coated with LLZO and a glass phase, characterized in that the multiple LLZO fine particles have a higher ion-guiding ability for lithium ions than the NCM large particles, do not cause side reactions with lithium ions, and when lithium ions pass through the positive electrode, they are guided by the multiple dispersed LLZO fine particles, thereby providing dispersed paths for lithium ions.
2. The NCM positive electrode particles coated with LLZO and glass phase as described in claim 1, characterized in that the size of the NCM large particles is in the range of between 3 μm and 5 μm, has a single crystal structure, and the thickness of the glass phase is in the range of between 5 nm and 100 nm.
3. The glass phase has a lithium ion conductivity of 10 -5 2. The NCM positive electrode particle covering the LLZO and glass phase according to claim 1, characterized in that the NCM positive electrode particle is composed of an amorphous oxide or non-oxide solid electrolyte having a conductivity of higher than 1.0 S / cm, and the amorphous oxide or non-oxide solid electrolyte is one element selected from the group consisting of lithium halides, lithium halogen-oxides, oxides of lithium and group IIIA, IVA, and VA elements, amorphous oxide-based solid electrolytes, amorphous perovskite-based solid electrolytes, garnet-based solid electrolytes, lithium phosphorus oxygen-nitrides, and lithium sulfides.
4. The glass phase has a lithium ion conductivity of 10 -5 2. The NCM positive electrode particle coated with LLZO and a glass phase according to claim 1, characterized in that the positive electrode particle is composed of an amorphous oxide or non-oxide solid electrolyte having a viscosity higher than 10000000000 S / cm, and the glass phase is composed of at least one of the following items (A), (B), (C), (D), (E) and (F). (A) Li-MO (wherein M is at least one element selected from the group consisting of fluorine (F), chlorine (Cl), bromine (Br), and iodine (I) halogen elements); (B) Li 2 O-RO x (where R is at least one element selected from boron (B), aluminum (Al), silicon (Si), germanium (Ge), phosphorus (P), and arsenic (As), and x=1 to 3). (C) LLTO (Li-La-Ti-O), (D) LLZO (Li-La-Zr-O), (E) LiPON (lithium phosphorus oxynitride), (F)Li 2 SP 2 WITH 5
5. The NCM positive electrode particles coated with LLZO and glass phases as described in claim 1, characterized in that the lateral size of the LLZO fine particles is in the range of 50 nm to 300 nm, and the lateral size is the size along the spherical direction of the corresponding NCM large particle.
6. The NCM positive electrode particle coated with LLZO and a glass phase as described in claim 1, characterized in that in the composite NCM particle, the total weight of the multiple LLZO microparticles and the weight ratio of the NCM particles having the glass phase are in the range of between 0.2% and 2%.
7. The NCM positive electrode particle covering LLZO and a glass phase as described in claim 1, further comprising a plurality of carbon nanotubes (CNTs) covering the outer periphery of the composite NCM particle, and a positive electrode particle covering the carbon nanotubes is formed by the plurality of carbon nanotubes and the composite NCM particles.
8. The NCM positive electrode particle coating LLZO and a glass phase as described in claim 7, characterized in that the plurality of carbon nanotubes include a plurality of short-chain carbon nanotubes and a plurality of long-chain carbon nanotubes, each of the short-chain carbon nanotubes having a length in the range of between 0.5 μm and 1 μm, each of the long-chain carbon nanotubes having a length in the range of between 3 μm and 8 μm, the plurality of short-chain carbon nanotubes being used to bridge the LLZO fine particles and the NCM large particles, and the plurality of long-chain carbon nanotubes being used to coat the composite NCM particles so that the entire composite NCM particle has suitable electrical conductivity.
9. The NCM positive electrode particles coated with LLZO and glass phases as described in claim 7, characterized in that the total weight ratio of the plurality of carbon nanotubes and the composite NCM particles is in the range between 0.1% and 2%.
10. The NCM positive electrode particle covering the LLZO and glass phase according to claim 7, further comprising a plurality of nanoscale amorphous carbons covering the outside of the positive electrode particles covering the carbon nanotubes, wherein the plurality of nanoscale amorphous carbons and the positive electrode particles covering the carbon nanotubes form positive electrode particles covering a carbon material, and each of the nanoscale amorphous carbons is located in a gap formed by the intersection of the plurality of carbon nanotubes.
11. The NCM positive electrode particles coating the LLZO and glass phase as described in claim 10, characterized in that the size of each of the nanoscale amorphous carbons ranges between 20 nm and 100 nm.
12. The NCM positive electrode particles coated with LLZO and glass phases as described in claim 10, characterized in that the total weight of the nano-scale amorphous carbon and the weight ratio of the composite NCM particles are in the range of between 0.1% and 2%, and the nano-scale amorphous carbon serves as a conductive auxiliary.
13. The NCM positive electrode particle coated with LLZO and a glass phase as described in claim 10, characterized in that the weight ratio of the total weight of the plurality of carbon nanotubes and the plurality of nanoscale amorphous carbons to the weight of the composite NCM particles is (0.09-3):
100.
14. The NCM positive electrode particle covering the LLZO and glass phase as described in claim 10, characterized in that the weight ratio of the plurality of carbon nanotubes, the plurality of nanoscale amorphous carbons, and the composite NCM particles is 0.5:1:100.
Citation Information
Cited By
Lithium ion battery positive electrode material with high interface conductivity and preparation method thereof
CN121439765A
Carbon-coated fast ion conductor modified cathode material and preparation method therefor
JP2026054456A
Positive electrode active material for secondary battery
JP2026079812A