Dielectric films for all-solid-state and semi-solid-state lithium batteries

A three-layer dielectric film with PVDF-HFP-based polymer layers and inorganic ceramics addresses issues of side reactions and connectivity in lithium batteries, enhancing conductivity and reducing short circuits for improved battery performance.

JP3249415UActive Publication Date: 2024-12-09SHENZHEN TXD TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2024003385U
Authority / Receiving Office
JP · JP
Patent Type
Utility models
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-09
Estimated Expiration
2034-10-11

AI Technical Summary

Technical Problem

Conventional solid and semi-solid electrolytes in lithium batteries face issues such as side reactions leading to dead lithium, low lithium ion capacity, lithium ion concentration on particle surfaces causing capacity decrease, poor connectivity resulting in short circuits, and high conduction energy levels reducing ionic conductivity.

Method used

A three-layer dielectric film structure comprising PVDF-HFP-based polymer layers with lithium salts and inorganic ceramics, specifically designed to enhance lithium ion conductivity and adhesion, reduce short circuits, and improve battery performance.

Benefits of technology

The three-layer dielectric film enhances battery performance by reducing short circuits, improving connectivity, and increasing ionic conductivity, thereby maintaining higher power storage capacity and reducing the risk of lithium crystal formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0003249415000001_ABST
    Figure 0003249415000001_ABST
Patent Text Reader

Abstract

Dielectric films for all-solid-state and semi-solid lithium batteries are provided. [Solution] A dielectric film 30 includes a first film layer 31 connected to the positive electrode of a lithium battery, a third film layer 33 connected to the negative electrode of the lithium battery, and a second film layer 32 connected between the first and third film layers. The first film layer includes a first polymer material 311 used in part as a plasticizer, and a first lithium salt 312 dispersed in the first polymer material. The second film layer includes a second polymer material 321 used in part as a plasticizer, a second lithium salt 322 dispersed in the second polymer material, and a second inorganic ceramic 323 dispersed in the second polymer material. The third film layer includes a third polymer material 331 used in part as a plasticizer, a third lithium salt 333, and a third inorganic ceramic 334.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to dielectric films for batteries, and more particularly to dielectric films for all-solid-state and semi-solid lithium batteries. [Background technology]

[0002] Prior art solid and semi-solid battery structures consist of an anode, a cathode, and a dielectric film located between the cathode and anode. The anode is filled with an anode slurry as a binder and a plurality of anode particles distributed within the anode slurry. The cathode is filled with a cathode slurry as a binder and a plurality of cathode particles distributed within the cathode slurry. The dielectric film is used to separate and join the anode and cathode. Summary of the Invention [Problem to be solved by the invention]

[0003] In the conventional solid or semi-solid electrolyte, the positive electrode slurry and the negative electrode slurry are used to guide the lithium ions. However, the positive electrode slurry and the negative electrode slurry are prone to side reactions with the lithium ions remaining in the positive electrode slurry and the negative electrode slurry, resulting in dead lithium and lithium depletion. This is due to irreversible chemical reactions, and the fewer the number of lithium ions in the battery, the lower the battery's charge storage capacity. In addition, because the lithium ion capacity of the multiple positive electrode particles and the negative electrode particles in the positive electrode slurry and the negative electrode slurry is low, the lithium ions in the positive electrode slurry and the negative electrode slurry are prone to concentrate on the surfaces of the positive electrode particles and the negative electrode particles, and these lithium ions cause side reactions with the molecules in the positive electrode slurry and the negative electrode slurry, which reduces the capacitance of the positive electrode and the negative electrode when used for a long time, and the number of lithium ions decreases due to the side reactions, resulting in a decrease in the charge storage capacity of the battery.

[0004] In addition, the conventional dielectric film has a single-layer structure, is biased toward a hard structure, and has a low lithium salt concentration, so when the dielectric film is bonded to the positive electrode, the lamination between them is not tight, which deteriorates the overall structure and bonding. In addition, the conventional dielectric film material cannot fill the cracks between the two, which makes it easy for short circuits to occur and reduces the yield.

[0005] Furthermore, the lithium salt in the conventional single-layer dielectric film has only a specific single concentration, so the conduction energy level required for lithium ions is high, the ion conductivity is low, and the performance of the entire battery is reduced. When the single-layer dielectric film is bonded to the negative electrode, the ion conductivity is low, so that the deposition of dead lithium is likely to occur on the negative electrode, the generation of lithium crystals is increased, the risk of puncture is increased, and the storage capacity of the battery is reduced.

[0006] Therefore, the inventor believed that the above-mentioned shortcomings could be improved, and after extensive research, he came up with the present invention, which effectively improves the above-mentioned problems through rational design.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a dielectric film for all-solid-state and semi-solid lithium batteries. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention adopts the following means. According to one aspect of the present invention, there is provided a dielectric film for an all-solid-state and semi-solid lithium battery, the lithium battery includes an anode and a cathode, the dielectric film is disposed between the cathode and the anode, the anode is filled with an anode slurry as a binder and a plurality of anode particles, the cathode is filled with a cathode slurry as a binder and a plurality of anode particles, and the dielectric film is: a first film layer, a second film layer, and a third film layer, the first film layer being connected to the positive electrode, the third film layer being connected to the negative electrode, and the second film layer being connected between the first film layer and the third film layer; The first film layer is a first polymer material as a base material of the first film layer, the first polymer material being a mixture of PVDF-HFP (Polyvinylidene fluoride-hexafluoropropylene copolymer), ADN (Adiponitrile), GLN (Glutaronitrile), and SN (Succinonitrile), the ADN, GLN, and SN of the first polymer material being used as plasticizers dispersed in the PVDF-HFP, the functions of which are to reduce precipitation of crystalloids in the first polymer material and to aid in dissociation of lithium salts by dispersing the first polymer material as a whole, so that the first film layer can easily conduct lithium ions and can be easily plastically processed; a first lithium salt dispersed in the first polymeric material, the first lithium salt being a mixture of LiBOB (LiB(C2O4)2, Lithium bis(oxalate)borate), LiTFSI (LiN(CF3SO2)2, Lithium bis(trifluoromethanesulfonyl)imide), and LiFSI (F2LiNO4S2, Lithium bis(fluorosulfonyl)imide); The second film layer is a second polymer material as a base material for the second film layer, the second polymer material being a mixture of PVDF-HFP, PAN (Polyacrylonitrile) and SN, the PAN and the SN of the second polymer material being used as plasticizers dispersed in the PVDF-HFP, and the PAN and the SN being used to assist the dissociation of the lithium salt of the second film layer and to increase ionic conductivity; a second lithium salt dispersed in the second polymeric material, the second lithium salt comprising LiFSI and LiTSFI; A second inorganic ceramic is dispersed in the second polymeric material, the second inorganic ceramic being a plurality of first LLZO particles having an outer coating of a first dopamine layer, each of the first LLZO particles being lithium lanthanum zirconium oxide (Li7La3Zr2O 12 ) or a second inorganic ceramic composed of lithium lanthanum zirconium oxide doped with at least one metal element; The third film layer is a third polymer material as the base material of the third film layer, the third polymer material being a mixture of PEO (Poly(ethylene oxide)) and PAN, the PEO having high stability at the reduction potential of the negative electrode and moderate ionic conductivity, the PAN having good electronic and ionic conductivity, further improving the overall performance of PEO, the PAN of the third polymer material being used as a plasticizer and dispersed in the PEO; a third lithium salt dispersed in the third polymeric material, the third lithium salt being LiTFSI; A third inorganic ceramic is dispersed in the third polymeric material, the third inorganic ceramic being a plurality of second LLZO particles having an outer coating of a second dopamine layer, each of the second LLZO particles being lithium lanthanum zirconium oxide (Li7La3Zr2O 12 ) or lithium lanthanum zirconium oxide doped with at least one metal element, the third inorganic ceramic being used to increase ionic conductivity, wherein the concentration of the first lithium salt in the first film layer is greater than the concentration of the second lithium salt in the second film layer, the concentration of the second lithium salt in the second film layer is greater than the concentration of the third lithium salt in the third film layer, and the first film layer and the third film layer are used as interface adhesion layers. Effect of the Invention

[0009] The present invention adds a first film layer and a third film layer on both sides of the conventional single-layer dielectric film to form a three-layer dielectric film, which has a soft structure and can fill the gap between the positive and negative electrodes of a lithium battery, improving the gap when the positive and negative electrodes are attached, improving the performance of the battery, reducing the risk of short circuit, and improving the yield of the battery.

[0010] At least the following points will become apparent from the following specification and drawings. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic diagram illustrating a dielectric film for solid-state and semi-solid lithium batteries according to an embodiment of the present invention; FIG. [Diagram 2] 1 is a schematic diagram showing a dielectric film for solid-state and semi-solid lithium batteries according to an embodiment of the present invention; FIG. [Diagram 3] FIG. 1 is a schematic diagram showing a first LLZO particle according to an embodiment of the present invention. [Figure 4] FIG. 2 is a schematic diagram showing a second LLZO particle according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The following describes in detail the embodiments of the present invention, but the present invention is not limited to these, and various modifications are possible within the scope of the description, and embodiments obtained by appropriately combining the technical means disclosed in the different embodiments are also included in the technical scope of the present invention.

[0013] First, referring to Figs. 1 to 4, an embodiment of a dielectric film 30 for all-solid and semi-solid lithium batteries according to the present invention will be described. The lithium battery includes an anode 10 and a cathode 20, and as shown in Fig. 2, the dielectric film 30 according to the present invention is located between the cathode 20 and the anode 10. The anode 10 is filled with an anode slurry 12 as a binder, and a plurality of anode particles 15 (e.g., SiC (silicon carbide) particles having a tin layer) distributed in the anode slurry 12. The outer surface of the anode particles 15 has a function of accommodating lithium ions and allowing the lithium ions of the anode to flow evenly. The anode particles 15 cause partial side reactions with the lithium ions, reducing the number of available lithium ions and reducing the overall capacitance of the battery in the long term. The cathode 20 is filled with a cathode slurry 22 as a binder, and a plurality of anode particles 26 distributed in the cathode slurry 22. The positive electrode slurry 22 and the positive electrode particles 26 undergo side reactions with the passing lithium ions, resulting in the depletion of available lithium ions.

[0014] In this case, as shown in Figures 1 and 2, the dielectric film 30 of the present invention is located between the negative electrode 10 and the positive electrode 20, and is used to separate and join the negative electrode 10 and the positive electrode 20. The dielectric film 30 includes a first film layer 31, a second film layer 32, and a third film layer 33. The first film layer 31 is connected to the positive electrode 20, the third film layer 33 is connected to the negative electrode 10, and the second film layer 32 is connected between the first film layer 31 and the third film layer 33.

[0015] The first film layer mainly comprises the following components, each of which will be described below.

[0016] First, a first polymer material 311 is used as a base material of the first film layer 31. The first polymer material is a mixture of PVDF-HFP (Polyvinylidene fluoride-hexafluoropropylene copolymer), ADN (Adiponitrile), GLN (Glutaronitrile), and SN (Succinonitrile), and the first polymer material 311 forms the base material of the first film layer 31. In the first polymer material 311, the ratio of the weight of the PVDF-HFP to the "total weight of the ADN, the GLN, and the SN" is in the range of 12:1 to 8:1.

[0017] The ADN, GLN, and SN of the first polymer material 311 are plasticizers dispersed in the PVDF-HFP to disperse the overall structure of the first polymer material 311, reduce the precipitation of crystalloids in the first polymer material, and aid in the dissociation of the lithium salt (i.e., the first lithium salt 312 described below). This allows the entire first film layer 31 to easily conduct lithium ions and facilitate plastic processing. The weight ratio of the ADN, GLN, and SN is in the range of 1:2:7 to 0.5:1:9.5.

[0018] Next, a first lithium salt 312 is dispersed in the first polymer material 311, the first lithium salt 312 including a mixture of LiBOB (LiB(C2O4)2, Lithium bis(oxalate)borate), LiTFSI (LiN(CF3SO2)2, Lithium bis(trifluoromethanesulfonyl)imide), and LiFSI (F2LiNO4S2, Lithium bis(fluorosulfonyl)imide). The weight ratio of the total weight of the first lithium salt 312 to the total weight of the first polymer material 311 is in the range of 1:2.5 to 1:5, the LiTFSI and the LiFSI are used to increase lithium ion conductivity, the LiBOB is used to prevent the LiTFSI and the LiFSI from being corroded by water, and is used to prevent the performance of the entire battery from being reduced by the attack of HF (hydrofluoric acid) generated by the reaction of water and LiTFSI, and allows the first lithium salt 312 to withstand a high voltage difference. In this way, the first polymer material 311 is stable even under the high pressure of the positive electrode 20. The LiBOB increases the stability of the first polymer material 311. In the first film layer 31, the ratio of "the total weight of the LiTFSI and the LiFSI" to the weight of the LiBOB is 2:3 (weight ratio). The weight ratio of the LiFSI to the LiTFSI is 2:1.

[0019] Next, the second film layer 32 has a second polymer material 321 as a base material of the second film layer 32, the second polymer material 321 including a mixture of PVDF-HFP, PAN (Polyacrylonitrile), and SN as a base material. In the second polymer material 321, the weight ratio of the weight of the PVDF-HFP, the weight of the PAN, and the weight of the SN is in the range of 8:1.2:1 to 8:1:1.6.

[0020] The PAN and SN of the second polymer material 321 are plasticizers dispersed in the PVDF-HFP, and their functions are to disperse the overall structure of the second polymer material 321 and reduce the precipitation of crystalloids in the second polymer material 321. The PAN and SN are used to assist the dissociation of the lithium salt (i.e., the second lithium salt 322 described below) in the second film layer 32 and to increase the ionic conductivity.

[0021] Next, the second lithium salt 322 is dispersed in the second polymer material 321 and includes LiFSI and LiTSFI. In the second film layer 32, the weight ratio of the LiFSI weight to the LiTSFI weight is 1:2. The second lithium salt 322 is used to lower the energy level and increase the stability and improve the conductivity when conducting lithium ions in each of the polymer materials. The weight ratio of the total weight of the second lithium salt 322 to the total weight of the second polymer material 321 is in the range of between 1:3 and 1:9.

[0022] Next, a second inorganic ceramic 323 is dispersed in the second polymer material 321, the second inorganic ceramic 323 being a plurality of first LLZO particles 326 outer-coated with a first dopamine layer 324 (see FIG. 3). In the second film layer 32, the overall radial length of each of the first LLZO particles 326 is less than 100 nm. The second inorganic ceramic 323 is used to increase the ionic conductivity and mechanical strength of the entire second film layer 32. The weight percentage of the second inorganic ceramic 323 in the second polymer material 321 ranges between 8%wt and 20%wt of the total weight.

[0023] The first LLZO particles 326 are lithium lanthanum zirconium oxide (Li7La3Zr2O 12) or lithium lanthanum zirconium oxide doped with at least one metal element. The first LLZO particles 326 are preferably made of Cu-LLZO (copper doped lithium lanthanum zirconium oxide).

[0024] The PVDF-HFP of the second polymer material 321 easily reacts with the first LLZO particles 326, so that the entire particle is unlikely to become a film. Therefore, the outer surface of the first LLZO particles 326 is covered with the first dopamine layer 324 to protect the first LLZO particles 326. In addition, the first LLZO particles 326 easily generate alkaline by-products when wet, and cause a lithium fluoridation reaction with PVDF-HFP. Since dopamine is hydrophobic, the outer surface of the first LLZO particles 326 is covered with the first dopamine layer 324 to prevent moisture from entering the first LLZO particles 326, and the functional group of dopamine is compatible with the PAN of the second polymer material 321. In each of the first LLZO particles 326, the weight percentage of the weight of the first dopamine layer 324 in the first LLZO particles 326 is less than 5% wt. The thickness of the first dopamine layer 324 is less than 3 nm.

[0025] Next, the third film layer 33 includes a third polymer material 331 that serves as a base material for the third film layer 33. The third polymer material 331 includes: It contains a mixture of PEO (Poly(ethylene oxide), polyethylene oxide, polyethylene oxide) and PAN. The weight ratio of the PEO to the PAN is in the range of 5:1 to 8:1, and the PEO has high stability at the reduction potential of the negative electrode 10 and moderate ionic conductivity. Since the PAN has good electronic and ionic conductivity, the performance of the entire PEO is further improved by mixing with the PAN.

[0026] The third polymeric material 331, PAN, is used as a plasticizer and is dispersed in the PEO.

[0027] The additive 332 is FEC (Fluoroethylene carbonate), which is dispersed in the third polymer material 331 and is used to help the negative electrode 10 form a good artificial solid electrolyte interphase (ASEI). The weight percentage of the additive 332 in the third polymer material 331 is less than 10% wt.

[0028] Next, a third lithium salt 333 is dispersed in the third polymer material 331, and the third lithium salt 333 is LiTFSI. During the formation or charge / discharge process, fluorine (F) of the LiTFSI and liberated lithium (Li) ions are deposited on the surface of the negative electrode 10 to form LiF (lithium fluoride), which has the effect of protecting the negative electrode 10 and helps the formation of the ASEI. The third lithium salt 333 is used to lower the energy level and increase the conductivity when conducting lithium ions in each of the polymer materials. The weight ratio of the total weight of the third lithium salt 333 to the third polymer material 331 is in the range of 1:3 to 1:9.

[0029] Finally, a third inorganic ceramic 334 is dispersed in the third polymer material 331, the third inorganic ceramic 334 being a plurality of second LLZO particles 336 outer-coated with a second dopamine layer 335 (see FIG. 4). In the third film layer 33, the overall radial size of each of the second LLZO particles 336 ranges between 200 nm and 300 nm, and the third inorganic ceramic 334 is used to enhance ionic conductivity. In this way, the negative electrode 10 has good ionic conductivity, and also reduces the deposition of dead lithium, suppresses the formation of lithium crystallites, reduces the risk of puncture, enhances mechanical performance, suppresses partial negative electrode expansion, and provides a stress source. The weight percentage of the total weight of the third inorganic ceramic 334 in the third polymer material 331 ranges between 10% wt and 20% wt. In each of the second LLZO particles 336, the weight percentage of the weight of the second dopamine layer 335 in the second LLZO particle 336 is less than 5% wt. The thickness of the second dopamine layer 335 is less than 3 nm.

[0030] The second LLZO particles 336 are lithium lanthanum zirconium oxide (Li7La3Zr2O 12 ) or lithium lanthanum zirconium oxide doped with at least one metal element. Preferably, the second LLZO particles 336 are made of Cu-LLZO (copper doped lithium lanthanum zirconium oxide).

[0031] The first film layer 31 does not have ceramic particles and is a soft material, so it has high adhesion to the positive electrode. The first polymer material 311 of the first film layer 31 is a soft material and can fill the gap between the dielectric film 30 and the positive electrode 20. In addition, the lithium salt selected for the first film layer 31 can reduce the energy level difference and increase the conductivity of lithium ions.

[0032] The concentration of the first lithium salt 312 in the first film layer 31 is higher than the concentrations of the lithium salts in the second film layer 32 and the third film layer 33 (i.e., the second lithium salt 322 and the third lithium salt 333), primarily for the purpose of lowering the boundary energy level that lithium ions must overcome in the respective polymer materials of the film layers, thereby increasing conductivity.

[0033] The lithium salt concentration of each of the film layers of the present invention gradually decreases from the first film layer 31 to the third film layer 33. That is, the concentration of the first lithium salt 312 in the first film layer 31 is higher than the concentration of the second lithium salt 322 in the second film layer 32, and the concentration of the second lithium salt 322 in the second film layer 32 is higher than the concentration of the third lithium salt 333 in the third film layer 33. This reduces the energy level and increases the conductivity when conducting lithium ions.

[0034] If the concentration of each of the polymer materials is too high, crystal precipitation is likely to occur, and the polymer cannot be effectively chain-bonded to form a film. However, the plasticizer of the polymer material can prevent the crystal precipitation of each of the polymer materials, and the plasticizer supports each of the polymer material structures, thereby improving the overall structure of the polymer material. The plasticizer is a highly polar plasticizer, and the highly polar nature of the plasticizer makes each of the lithium salts more easily dissociated, increasing the amount of free lithium ions, thereby further improving the lithium ion conductivity. In addition, inorganic ceramic materials may be added to the second film layer 32 and the third film layer 33 to improve the conductivity and mechanical properties of lithium ions.

[0035] The sum of the thicknesses of the first film layer 31, the second film layer 32, and the third film layer 33 is in the range of 12 μm to 24 μm. The thickness of the second film layer 32 is in the range of 10 μm to 18 μm. The thicknesses of the first film layer 31 and the third film layer 33 are each in the range of 1 μm to 3 μm.

[0036] The first film layer 31 and the third film layer 33 may be interface adhesive layers, bonding the first film layer 31 to the positive electrode 20 and bonding the third film layer 33 to the negative electrode 10 .

[0037] The above description is for the purpose of explaining the present invention, and should not be interpreted as limiting the invention described in the scope of the utility model registration claims or restricting the scope. In addition, the configuration of each part of the present invention is not limited to the above embodiment, and various modifications are possible within the technical scope described in the scope of the utility model registration claims. [Explanation of symbols]

[0038] 10 negative electrode 12 Anode slurry 15 Negative electrode particles 20 positive electrode 22 Positive electrode slurry 24 Positive electrode particles 30 Dielectric Film 31 First film layer 32 2nd film layer 33 3rd film layer 311 First polymer material 312 First Lithium Salt 321 Second polymer material 322 Secondary Lithium Salt 323 Secondary Inorganic Ceramics 324 First dopamine layer 326 First LLZO particle 331 Third Polymer Material 332 Additives 333 tertiary lithium salts 334 Third Inorganic Ceramics 335 Second Dopamine Layer 336 2nd LLZO particle

Claims

1. A dielectric film for an all-solid-state and semi-solid lithium battery, the lithium battery comprising an anode and a cathode, the dielectric film being located between the cathode and the anode, the anode being filled with an anode slurry as a binder and a plurality of anode particles, the cathode being filled with a cathode slurry as a binder and a plurality of cathode particles, the dielectric film being: a first film layer, a second film layer, and a third film layer, the first film layer being connected to the positive electrode, the third film layer being connected to the negative electrode, and the second film layer being connected between the first film layer and the third film layer; The first film layer is a first polymer material as a base material of the first film layer, the first polymer material being a mixture of PVDF-HFP (Polyvinylidene fluoride-hexafluoropropylene copolymer), ADN (Adiponitrile), GLN (Glutaronitrile), and SN (Succinonitrile), the ADN, GLN, and SN of the first polymer material being used as plasticizers dispersed in the PVDF-HFP, the functions of which are to reduce precipitation of crystalloids in the first polymer material and to aid in dissociation of lithium salts by dispersing the first polymer material as a whole, so that the first film layer can easily conduct lithium ions and can be easily plastically processed; A first lithium salt dispersed in the first polymeric material, the first lithium salt being LiBOB(LiB(C 2 O 4 ) 2 , Lithium bis(oxalate)borate, LiTFSI (LiN(CF 3 SO 2 ) 2 , Lithium bis(trifluoromethanesulfonyl)imide, and LiFSI (F 2 LiNO 4 S 2 a first lithium salt which is a mixture of lithium bis(fluorosulfonyl)imide; The second film layer is a second polymer material as a base material for the second film layer, the second polymer material being a mixture of PVDF-HFP, PAN (Polyacrylonitrile) and SN, the PAN and the SN of the second polymer material being used as plasticizers dispersed in the PVDF-HFP, and the PAN and the SN being used to assist the dissociation of the lithium salt of the second film layer and to increase ionic conductivity; a second lithium salt dispersed in the second polymeric material, the second lithium salt comprising LiFSI and LiTSFI; A second inorganic ceramic is dispersed in the second polymeric material, the second inorganic ceramic being a plurality of first LLZO particles having a first dopamine layer thereon, each of the first LLZO particles being lithium lanthanum zirconium oxide (Li 7 La 3 Zr 2 O 12 a second inorganic ceramic material composed of lithium lanthanum zirconium oxide doped with at least one metal element; The third film layer is a third polymer material as the base material of the third film layer, the third polymer material being a mixture of PEO (Poly(ethylene oxide)) and PAN, the PEO having high stability at the reduction potential of the negative electrode and moderate ionic conductivity, the PAN having good electronic and ionic conductivity, further improving the overall performance of PEO, the PAN of the third polymer material being used as a plasticizer and dispersed in the PEO; a third lithium salt dispersed in the third polymeric material, the third lithium salt being LiTFSI; A third inorganic ceramic is dispersed in the third polymeric material, the third inorganic ceramic being a plurality of second LLZO particles having an outer coating of a second dopamine layer, each of the second LLZO particles being lithium lanthanum zirconium oxide (Li 7 La 3 Zr 2 O 12 ) or lithium lanthanum zirconium oxide doped with at least one metal element, the third inorganic ceramic being used to increase ionic conductivity; A dielectric film for all-solid-state and semi-solid lithium batteries, characterized in that the concentration of the first lithium salt in the first film layer is greater than the concentration of the second lithium salt in the second film layer, the concentration of the second lithium salt in the second film layer is greater than the concentration of the third lithium salt in the third film layer, and the first and third film layers are used as interface adhesion layers.

2. In the first film layer, the weight ratio of said ADN, said GLN, and said SN ranges between 1:2:7 and 0.5:1:9.5; the ratio of the weight of the PVDF-HFP to the "total weight of the ADN, the GLN, and the SN" is in the range of between 12:1 and 8:1; a weight ratio of a total weight of the first lithium salt to a total weight of the first polymeric material ranges between 1:2.5 and 1:5; The dielectric film for all-solid-state and semi-solid lithium batteries according to claim 1, characterized in that the ratio of "the total weight of the LiTFSI and the LiFSI" to the weight of the LiBOB is 2:3, and the weight ratio of the LiFSI to the LiTFSI is 2:

1.

3. In the second film layer, the weight ratio of the second polymeric material to the weight of the PVDF-HFP, the weight of the PAN, and the weight of the SN ranges between 8:1.2:1 to 8:1:1.6; The weight ratio of the LiFSI to the LiTSFI is 1:2; a weight ratio of a total weight of the second lithium salt to a total weight of the second polymeric material ranges between 1:3 and 1:9; The dielectric film for all-solid-state and semi-solid lithium batteries according to claim 1, characterized in that the weight percentage of the total weight of the second inorganic ceramic in the second polymer material ranges between 8%wt and 20%wt.

4. each said first LLZO particle has an overall radial size of less than 100 nm; The dielectric film for all-solid-state and semi-solid lithium batteries as described in claim 1, characterized in that in each of the first LLZO particles, the weight percentage of the weight of the first dopamine layer in the first LLZO particle is less than 5% wt, and the thickness of the first dopamine layer is less than 3 nm.

5. In the third film layer, the weight ratio of the PEO to the PAN ranges between 5:1 and 8:1; The dielectric film for all-solid-state and semi-solid lithium batteries according to claim 1, characterized in that the weight ratio of the total weight of the third lithium salt to the weight of the third polymeric material ranges between 1:3 and 1:

9.

6. 2. The dielectric film for all-solid-state and semi-solid lithium batteries according to claim 1, wherein the third film layer further comprises an additive, the additive being fluoroethylene carbonate (FEC) dispersed in the third polymer material, for helping the anode form a good artificial solid electrolyte interphase (ASEI).

7. The dielectric film for all-solid-state and semi-solid lithium batteries according to claim 6, characterized in that the weight percentage of said additive in said third polymeric material is less than 10% wt.

8. The dielectric film for all-solid-state and semi-solid lithium batteries as described in claim 1, characterized in that the first LLZO particles and the second LLZO particles are composed of Cu-LLZO, and the Cu-LLZO is a lithium lanthanum zirconium oxide doped with copper.

9. the total radial size of each of said second LLZO particles is in the range between 200 nm and 300 nm; The dielectric film for all-solid-state and semi-solid lithium batteries according to claim 1, characterized in that the weight percentage of the total weight of the third inorganic ceramic in the third polymer material ranges between 10%wt and 20%wt.

10. The dielectric film for all-solid-state and semi-solid lithium batteries according to claim 1, characterized in that the sum of the thicknesses of the first film layer, the second film layer, and the third film layer is in the range of 12 μm to 24 μm, the thickness of the second film layer is in the range of 10 μm to 18 μm, and the thicknesses of the first film layer and the third film layer are in the range of 1 μm to 3 μm, respectively.

Citation Information

Cited By

  • Electrolyte composite comprising oxide-based solid electrolyte and method for manufacturing same