Laminated separator for power storage device, and power storage device

The laminated separator with polyolefin and inorganic particle layers addresses insulation and safety issues in lithium ion batteries by maintaining high insulation at elevated temperatures, ensuring safety and performance in electric vehicles.

JP7551328B2Active Publication Date: 2024-09-17ASAHI KASEI BATTERY SEPARATOR CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020081230
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-01
Publication Date
2024-09-17
Estimated Expiration
2040-05-01

AI Technical Summary

Technical Problem

Existing laminated separators for lithium ion secondary batteries used in electric vehicles have insufficient insulation properties at high temperatures, leading to potential safety issues due to heat generation, and they require complex manufacturing processes that reduce productivity.

Method used

A laminated separator composed of a porous layer A containing a polyolefin resin and a porous layer B with a high content of inorganic particles, specifically designed to maintain insulation properties at high temperatures and improve safety, with a membrane resistance value exceeding 200Ω·cm at 200°C, achieved through a coextrusion method and controlled stretching processes.

Benefits of technology

The laminated separator effectively maintains battery safety by increasing insulation properties and reducing the risk of fire, while also enhancing durability and output characteristics, thus improving the safety and performance of large batteries in electric vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551328000004
    Figure 0007551328000004
  • Figure 0007551328000003
    Figure 0007551328000003
  • Figure 0007551328000005
    Figure 0007551328000005
Patent Text Reader

Abstract

To provide a laminate separator for a power storage device which is superior in high-temperature insulating property, and a power storage device having such a separator.SOLUTION: A laminate separator for a power storage device comprises at least one porous layer A containing a polyolefin resin and at least one porous layer B containing inorganic particles. In the laminate separator, the content of the inorganic particles in the porous layer B is 60 mass% or more and less than 100 mass%; a 200°C-film resistance value is 200 Ω cm2 or more and over a 170°C-film resistance value; and the at least one porous layer A and the at least one porous layer B are laminated.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated separator for an electricity storage device, and an electricity storage device using the separator. [Background technology]

[0002] Energy storage devices are used in a wide range of applications, including power sources for consumer devices, in-vehicle power sources, stationary power sources, etc. Among energy storage devices, lithium-ion secondary batteries have excellent characteristics such as high energy density and high durability, and in recent years their use as power sources for electric vehicles has rapidly expanded.

[0003] In lithium ion secondary batteries, a polyolefin microporous membrane is generally used as a separator that is disposed between a positive electrode and a negative electrode and prevents electronic conduction due to direct contact or short circuit between the positive and negative electrodes, while allowing ionic conduction via an electrolyte solution held in the microporous membrane.

[0004] Large batteries are generally used as lithium-ion secondary batteries for electric vehicles. The use of large batteries increases the energy density when multiple batteries are connected to construct a storage module, and the productivity of the storage module is also improved because the number of connected batteries can be reduced compared to small batteries. However, large batteries have poor heat dissipation properties due to their size, and if the battery generates abnormal heat due to an internal short circuit, the temperature at the center of the battery can easily reach 400°C or more, which can easily lead to serious accidents such as fire.

[0005] In addition, batteries for electric vehicles are often densely packed in order to make effective use of the limited space inside the vehicle. Therefore, if one battery catches fire, it can easily affect other batteries. Therefore, it is necessary to maintain a high level of safety for all batteries installed in an electric vehicle.

[0006] Under such circumstances, the separator is required to have a property of maintaining sufficient electrical insulation even when the inside of the battery becomes hot, and maintaining the safety of the battery. In recent years, various attempts have been made to improve the insulation of the separator at high temperatures, but the most widely used method is to form an inorganic layer mainly made of inorganic particles on a substrate such as a polyolefin microporous film by coating. For example, in Patent Document 1, an inorganic layer mainly made of boehmite is formed on a polyolefin microporous film by coating, to produce a laminated separator consisting of a polyolefin layer and an inorganic layer.

[0007] On the other hand, techniques for forming an inorganic layer by methods other than coating have also been proposed. For example, in Patent Document 2, a laminated separator composed of two polyolefin layers and one inorganic layer, with the inorganic layer containing silica at a maximum of 98% by mass, is produced by a co-extrusion method. In addition, Patent Document 3 discloses a technique for producing a laminated separator composed of two polyolefin layers and one inorganic layer, with the inorganic layer containing barium sulfate at a maximum of 97% by mass, by a co-extrusion method. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2014 / 208454 [Patent Document 2] JP 2017-80977 A [Patent Document 3] International Publication No. 2019 / 235112 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the laminated separator described in Patent Document 1 has an insufficient property of maintaining insulation at high temperatures, because the film resistance value decreases as the temperature increases above the melting point of the polyolefin resin, as shown in Comparative Example 1 described later. In addition, this technology requires separate manufacturing steps for the polyolefin layer and the inorganic layer, which results in a large number of steps and low productivity.

[0010] Furthermore, as shown in Comparative Example 2 described later, the laminated separator described in Patent Document 2 has an insufficient density of the inorganic layer, and is not satisfactory in terms of maintaining insulating properties at high temperatures. Furthermore, there is room for improvement in terms of battery durability and output characteristics.

[0011] Furthermore, in the laminate separator described in Patent Document 3, as shown in Comparative Example 3 described later, the density of the inorganic layer is insufficient, and there is room for improvement in terms of the property of maintaining insulating properties at high temperatures.

[0012] In view of the above circumstances, an object of the present invention is to provide a laminate separator for an electricity storage device that has excellent insulating properties at high temperatures, and an electricity storage device including the separator. [Means for solving the problem]

[0013] As a result of intensive research aimed at achieving the above object, the present inventors have found that the above-mentioned problems can be solved by a laminate separator for an electricity storage device, which has a porous layer A containing a polyolefin resin and a porous layer B containing a large amount of inorganic particles and exhibits a specific resistance behavior at high temperatures, and have completed the present invention. One embodiment of the present invention is illustrated below. [1] The porous layer A contains a polyolefin resin, and the porous layer B contains inorganic particles, the content of the inorganic particles in the porous layer B is 60% by mass or more and less than 100% by mass, and the film resistance at 200°C is 200 Ω cm 2 and a membrane resistance value exceeding 170° C., and comprising at least one layer of the porous layer A and at least one layer of the porous layer B laminated together. [2] 2. The laminate separator for an electricity storage device according to item 1, wherein the porosity of the porous layer B is 30% or more and 70% or less. [3] 3. The laminate separator for an electricity storage device according to item 1 or 2, wherein at least two layers of the porous layer A and at least one layer of the porous layer B are laminated. [4] 3. The laminate separator for an electricity storage device according to item 1 or 2, wherein at least one layer of the porous layer A and at least two layers of the porous layer B are laminated. [5] 5. The laminate separator for an electricity storage device according to any one of items 1 to 4, wherein both surface layers are the porous layer A or the porous layer B. [6] 6. The laminate separator for an electricity storage device according to any one of items 1 to 5, wherein the inorganic particles are surface-treated inorganic particles. [7] 7. The laminate separator for an electricity storage device according to any one of items 1 to 6, wherein the inorganic particles have an average particle size of 31 nm or more and 1000 nm or less. [8] 8. The laminate separator for an electricity storage device according to any one of items 1 to 7, wherein the inorganic particles are one or more selected from the group consisting of boehmite, alumina, titania, magnesium oxide, zinc oxide, calcium sulfate, aluminum sulfate, barium sulfate, magnesium hydroxide, lithium phosphate, sodium phosphate, and magnesium phosphate. [9] 9. The laminate separator for an electricity storage device according to any one of items 1 to 8, wherein the porous layer A contains polyethylene having a viscosity average molecular weight of 500,000 or more and 5,000,000 or less.

[10] 10. The laminate separator for an electricity storage device according to any one of items 1 to 9, wherein the porous layer B contains a polyolefin having a viscosity average molecular weight of 200,000 or more and 10,000,000 or less.

[11] 11. The laminate separator for an electricity storage device according to any one of items 1 to 10, wherein the laminate separator for an electricity storage device has an air permeability of 30 sec / 100 ml or more and 150 sec / 100 ml or less.

[12] 12. An electricity storage device comprising: a positive electrode, a negative electrode, and the laminate separator for an electricity storage device according to any one of items 1 to 11. Effect of the Invention

[0014] According to the present invention, it is possible to provide a laminated separator for an electricity storage device that can maintain the safety of a large battery even when abnormal heat generation occurs in the battery, and an electricity storage device including the separator. [Brief description of the drawings]

[0015] [Figure 1A] FIG. 2 is a schematic diagram of a measuring device for film resistance value. [Figure 1B] 1B is a schematic diagram illustrating overlapping of a plurality of members in the measuring device of FIG. 1A. [Diagram 2] 1 is a graph showing the relationship between temperature and film resistance value. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment for carrying out the present invention (hereinafter, abbreviated as "present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be carried out in various modifications within the scope of the gist of the present invention.

[0017] 《Porous layer A》 The laminate separator for an electricity storage device according to this embodiment has a polyolefin resin-containing porous layer A. The laminate separator contains at least one porous layer A, and may contain two or more porous layers.

[0018] The thickness of each layer of the porous layer A is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 3 μm or more. When the thickness of each layer of the porous layer A is 1 μm or more, the mechanical strength and voltage resistance of the laminated separator are improved. Furthermore, the thickness of each layer of the porous layer A is preferably 17 μm or less, more preferably 15 μm or less, and even more preferably 13 μm or less. When the thickness of each layer of the porous layer A is 17 μm or less, the energy density of the electricity storage device can be increased.

[0019] The porosity of the porous layer A is preferably 30% or more, more preferably 35% or more, and even more preferably 40% or more from the viewpoint of increasing the ion permeability of the laminated separator, while it is preferably 75% or less, more preferably 70% or less, and even more preferably 65% ​​or less from the viewpoint of maintaining the structure of the laminated separator.

[0020] The thickness ratio of the porous layer A to the entire laminate separator is preferably 5% or more, more preferably 10% or more, and even more preferably 15% or more, taking into consideration the physical strength of the laminate separator. When the thickness ratio of the porous layer A is 5% or more, the laminate separator is given fuse characteristics and the insulating properties at high temperatures are improved, which is preferable. On the other hand, from the viewpoint of increasing the ion permeability of the laminate separator, the thickness ratio of the porous layer A is preferably 90% or less, more preferably 85% or less, and even more preferably 80% or less. When the thickness ratio of the porous layer A is 90% or less, the dimensional stability of the laminate separator at high temperatures is improved, and the insulating properties at high temperatures are improved, which is preferable.

[0021] The method for producing the porous layer A is not particularly limited, and various methods can be used, specifically, a stretching process such as uniaxial stretching or biaxial stretching, a process for removing a third component other than the polyolefin resin and the ionic compound by a method such as extraction, volatilization, decomposition, etc. As the third component, a plasticizer such as liquid paraffin or dioctyl phthalate, or a solvent such as acetone or water can be used alone or in combination.

[0022] From the viewpoint of reducing the manufacturing cost of the laminated separator and improving the quality such as the uniformity of the film thickness, the method for producing the porous layer A preferably has at least a stretching step, more preferably has a stretching step and a third component removal step, further preferably has a stretching step and a third component extraction step, and particularly preferably has a biaxial stretching step and a plasticizer extraction step. When the porous layer A is produced by these methods, not only can the porous layer A be formed uniformly, but also the physical properties such as the thickness and porosity of the entire laminated separator for an electricity storage device can be easily adjusted.

[0023] <Polyolefin resin> The laminated separator for an electricity storage device according to this embodiment has a porous layer A containing a polyolefin resin. The polyolefin resin used in this embodiment is a polyolefin resin used in normal extrusion, injection, inflation, and blow molding, and is a polymer containing an olefin hydrocarbon as a monomer component, such as a homopolymer, copolymer, or multistage polymer of ethylene, propylene, 1-butene, 2-butene, 4-methyl-1-pentene, 1-hexene, or 1-octene. Polyolefins selected from the group consisting of these homopolymers, copolymers, and multistage polymers can also be used alone or in combination.

[0024] Specifically, the polyolefin resin is low-density polyethylene (density 0.910 g / cm 3 More than 0.930g / cm 3 less than 0.910g / cm 3 More than 0.940g / cm 3 less than 0.930g / cm 3 More than 0.942g / cm 3 less than 0.942g / cm 3 or more), ultra-high molecular weight polyethylene (density 0.910g / cm 3 More than 0.970g / cm 3hereinafter), isotactic polypropylene, syndiotactic polypropylene, atactic polypropylene, polybutene, polymethylpentene, and ethylene propylene rubber.

[0025] The proportion of the polyolefin resin in the porous layer A is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. When the proportion of the polyolefin resin is 70% by mass or more, the porous layer A is easily formed, and physical strength and fuse characteristics can be imparted to the porous layer A. In addition, this proportion is preferably 100% by mass or less, and more preferably 100% by mass. When the proportion of the polyolefin resin is 100% by mass or less, the uniformity of the porous layer A tends to be improved.

[0026] The polyolefin resin preferably contains high-density polyethylene. The proportion of high-density polyethylene in the polyolefin resin is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and may be 100% by mass. When the proportion of high-density polyethylene in the polyolefin resin is 70% by mass or more, the mechanical strength of the laminated separator is increased due to entanglement of high-density polyethylene molecular chains.

[0027] The polyolefin resin preferably contains a high molecular weight polyethylene. The proportion of the high molecular weight polyethylene in the polyolefin resin is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and may be 100% by mass. The viscosity average molecular weight (Mv) of the high molecular weight polyethylene is preferably 500,000 or more and 5,000,000 or less, more preferably 600,000 or more and 4,000,000 or less, and even more preferably 700,000 or more and 3,000,000 or less. The viscosity average molecular weight can be obtained by measuring the intrinsic viscosity of decalin solvent at 135°C based on ASTM-D4020 and calculating from a calculation formula corresponding to the polyolefin resin. For polyethylene, Mv can be calculated using the following formula: [η]=6.77×10 -4 Mv 0.67 For polypropylene, Mv can be calculated using the following formula: [η]=1.10×10 -4 Mv 0.80

[0028] The use of a polyolefin resin having a viscosity average molecular weight of 500,000 or more is preferable from the viewpoint of maintaining high melt tension and ensuring good moldability when melt-kneading the polyolefin resin composition, and from the viewpoint of imparting sufficient entanglement to the molecular chains of the polyolefin resin and enhancing the mechanical strength of the laminated separator. On the other hand, adjusting the viscosity average molecular weight to 5,000,000 or less is preferable from the viewpoint of improving the stability of extrusion molding of the polyolefin resin.

[0029] The polyolefin resin preferably contains polypropylene from the viewpoint of improving the heat resistance of the laminated separator. The proportion of polypropylene in the polyolefin resin is preferably 1 mass% or more, more preferably 3 mass% or more, and even more preferably 5 mass% or more. The proportion of polypropylene in the polyolefin resin is preferably 30 mass% or less, more preferably 25 mass% or less, and even more preferably 20 mass% or less. Adjusting the proportion of polypropylene to 1 mass% or more is preferable from the viewpoint of improving the heat resistance of the laminated separator. On the other hand, from the viewpoint of increasing the uniformity of the laminated separator, the proportion of polypropylene is preferably 30 mass% or less.

[0030] The polyolefin resin used in this embodiment may be mixed with additives such as phenol-based, phosphorus-based, and sulfur-based antioxidants; metal soaps such as calcium stearate and lithium stearate; ultraviolet absorbers, light stabilizers, antistatic agents, antifogging agents, and coloring pigments, as necessary, within the scope of the advantages of the present invention.

[0031] 《Porous layer B》 The laminate separator for an electricity storage device according to this embodiment has a porous layer B containing a large amount of inorganic particles. The laminate separator includes at least one porous layer B, and may include two or more porous layers.

[0032] The thickness of each layer of the porous layer B is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 3 μm or more. When the thickness of each layer of the porous layer B is 1 μm or more, the insulating properties of the laminated separator at high temperatures are improved. Furthermore, the thickness of each layer of the porous layer B is preferably 17 μm or less, more preferably 15 μm or less, and even more preferably 13 μm or less. When the thickness of each layer of the porous layer B is 17 μm or less, the energy density of the electricity storage device can be increased.

[0033] From the viewpoint of increasing the ion permeability of the laminated separator, the porosity of the porous layer B is preferably 30% or more, more preferably 35% or more, even more preferably 40% or more, and particularly preferably 45% or more. On the other hand, from the viewpoint of maintaining the insulating properties of the laminated separator at high temperatures, the porosity of the porous layer B is preferably 70% or less, more preferably 68% or less, even more preferably 66% or less, and particularly preferably 64% or less.

[0034] The thickness ratio of the porous layer B to the entire laminate separator is preferably 5% or more, more preferably 10% or more, and even more preferably 15% or more, from the viewpoint of improving the insulating properties of the laminate separator at high temperatures. If the thickness ratio of the porous layer B is 5% or more, the insulating properties of the laminate separator at high temperatures are improved, which is preferable. On the other hand, from the viewpoint of facilitating the production of the laminate separator, the thickness ratio of the porous layer B is preferably 95% or more, more preferably 90%, and even more preferably 85% or less.

[0035] The method for producing the porous layer B is not particularly limited and various methods can be used, but specifically, a stretching process such as uniaxial stretching or biaxial stretching, a process for removing a third component other than the polyolefin resin and the ionic compound by a method such as extraction, volatilization, decomposition, etc. As the third component, a plasticizer such as liquid paraffin or dioctyl phthalate, or a solvent such as acetone or water can be used alone or in combination.

[0036] From the viewpoint of reducing the manufacturing cost of the laminated separator and improving the quality such as the uniformity of the film thickness, the method for producing the porous layer B preferably has at least a stretching step, more preferably has a stretching step and a third component removal step, further preferably has a stretching step and a third component extraction step, and particularly preferably has a biaxial stretching step and a plasticizer extraction step. When the porous layer B is produced by these methods, not only can the porous layer B be formed uniformly, but also the physical properties such as the thickness and porosity of the entire laminated separator for an electricity storage device can be easily adjusted.

[0037] The content of inorganic particles in the porous layer B is 60% by mass or more, preferably 65% ​​by mass or more, more preferably 70% by mass or more, and even more preferably 75% by mass or more. When the content of inorganic particles is 60% by mass or more, the insulating properties of the laminated separator at high temperatures tend to be improved. In addition, the content of inorganic particles is less than 100% by mass, preferably 99.5% by mass or less, more preferably 99% by mass or less, and even more preferably 98.5% by mass or less. When the content of inorganic particles is less than 100% by mass, the inorganic particles are prevented from falling off from the porous layer B, and the uniformity of the porous layer B can be improved.

[0038] The porous layer B may contain a polyolefin resin. When the porous layer B contains a polyolefin resin, the inorganic particles are bonded to each other, and the inorganic particles can be prevented from falling off from the porous layer B. Examples of the polyolefin resin include homopolymers, copolymers, and multi-stage polymers of ethylene, propylene, 1-butene, 2-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene, and from the viewpoint of improving moldability, polyethylene and polypropylene are preferable. The polyolefin resin may be used alone or in combination of two or more kinds.

[0039] The polyolefin resin in the porous layer B preferably has a specific molecular weight from the viewpoint of ensuring the moldability and physical strength of the porous layer B. The viscosity average molecular weight (Mv) of the polyolefin resin in the porous layer B is preferably 200,000 or more and 10,000,000 or less, more preferably 300,000 or more and 8,000,000 or less, and even more preferably 400,000 or more and 6,000,000 or less.

[0040] By using a polyolefin resin having a viscosity average molecular weight of 200,000 or more, it is possible to maintain high melt tension and ensure good moldability when melt-kneading the composition constituting the porous layer B. Furthermore, since sufficient entanglement is imparted to the polyolefin molecular chains, it becomes possible to stretch the porous layer B uniformly when stretching it. On the other hand, by using a polyolefin resin having a viscosity average molecular weight of 10,000,000 or less, it is possible to increase the dimensional stability of the porous layer B at high temperatures, thereby improving the insulating properties of the laminated separator at high temperatures.

[0041] The content of the polyolefin resin in the porous layer B is preferably more than 0% by mass, more preferably 0.1% by mass or more, even more preferably 0.5% by mass or more, and particularly preferably 1% by mass or more. When the content of the polyolefin resin exceeds 0% by mass, the uniformity of the porous layer B is increased, and the dropping of inorganic particles from the porous layer B tends to be suppressed. In addition, the content of this polyolefin resin is preferably 40% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less. When the content of the polyolefin resin is 40% by mass or less, the dimensional stability of the porous layer B at high temperatures can be improved.

[0042] 《Inorganic particles》 The laminated separator for an electricity storage device according to this embodiment has a porous layer B containing inorganic particles. The inorganic particles used in this embodiment are particulate substances mainly composed of elements other than carbon. It is desirable for the inorganic particles to have no electronic conductivity, a decomposition temperature or melting point of 500°C or higher, and be chemically stable in the special environment inside the electricity storage device. By using inorganic particles having these properties, the safety of the electricity storage device can be maintained even if the inside of the electricity storage device becomes hot due to abnormal heat generation or the like.

[0043] The inorganic particles are particulate substances mainly composed of elements other than carbon, have no electronic conductivity, have a decomposition temperature or melting point of 500°C or higher, and are not particularly limited as long as they are chemically stable inside the electricity storage device. Examples of the inorganic particles include metal oxides such as silica, boehmite, alumina, titania, magnesium oxide, and zinc oxide; silicate minerals such as mica, clay, and kaolin; sulfates such as sodium sulfate, magnesium sulfate, calcium sulfate, barium sulfate, and aluminum sulfate; nitrates such as sodium nitrate, magnesium nitrate, and potassium nitrate; phosphates such as lithium phosphate, sodium phosphate, and magnesium phosphate; halides such as lithium fluoride, sodium chloride, and sodium bromide; carbonates such as lithium carbonate, sodium carbonate, and sodium bicarbonate; and hydroxides such as magnesium hydroxide and aluminum hydroxide.

[0044] Considering both the stability inside the electricity storage device and the cost, the inorganic particles are preferably boehmite, alumina, titania, magnesium oxide, zinc oxide, calcium sulfate, aluminum sulfate, barium sulfate, magnesium hydroxide, lithium phosphate, sodium phosphate, and magnesium phosphate, more preferably boehmite, alumina, titania, zinc oxide, barium sulfate, magnesium hydroxide, lithium phosphate, and sodium phosphate, further preferably boehmite, alumina, titania, and barium sulfate, and particularly preferably barium sulfate. One type of inorganic particle may be used alone, or two or more types may be used in combination.

[0045] Examples of the shape of the inorganic particles include plate-like, scaly, needle-like, columnar, spherical, polyhedral, and block-like, and a combination of a plurality of inorganic particles having the above shapes may be used. The shape of the inorganic particles is not particularly limited, but from the viewpoint of suppressing the rupture of the separator, columnar, spherical, or polyhedral particles are preferred, and spherical particles are more preferred.

[0046] The average particle size of the inorganic particles is preferably 31 nm or more, more preferably 40 nm or more, and even more preferably 50 nm or more. By having an average particle size of 31 nm or more, the aggregation of inorganic particles is suppressed, and the separator film breakage can be suppressed. On the other hand, the average particle size is preferably 1000 nm or less, more preferably 900 nm or less, and even more preferably 800 nm or less. By having an average particle size of 1000 nm or less, the formation of pores due to interfacial peeling during stretching of the porous layer B is suppressed, and the density of the porous layer B can be increased. The average particle size refers to the average value of the particle sizes of 30 randomly selected inorganic particles that can be confirmed in the field of view when the porous layer B is observed at 30,000 times magnification with a scanning electron microscope. When calculating the average particle size, the particle size when each particle exists alone is used, and when the particles are aggregated, the particle size of the primary particles that constitute the aggregate is used.

[0047] Carbonates such as calcium carbonate have long been used as fillers for various polymers, and their performance as fillers has been demonstrated in a variety of applications. However, in the special environment inside an electricity storage device, carbonates are likely to decompose and generate carbon dioxide, which is undesirable.

[0048] In addition, depending on the conditions of use of the electricity storage device, silica and silicate minerals may react with hydrogen fluoride produced as a by-product inside the electricity storage device to generate silicon tetrafluoride gas, which may result in the electricity storage device expanding and impairing the safety and durability of the electricity storage device, which is undesirable.

[0049] The inorganic particles may be surface-treated with a surface treatment agent. Specifically, the surface treatment agent may be a saturated fatty acid such as stearic acid and its salt, an unsaturated fatty acid such as oleic acid and its salt, polysiloxane, or a silane coupling agent. From the viewpoint of improving compatibility with polyolefin resins, the surface treatment agent for inorganic particles is preferably a saturated fatty acid and its salt, an unsaturated fatty acid and its salt, or a silane coupling agent, more preferably a saturated fatty acid having 8 or more carbon atoms and its salt, or an unsaturated fatty acid having 8 or more carbon atoms and its salt, or even more preferably a saturated fatty acid having 12 or more carbon atoms and its salt, or an unsaturated fatty acid having 12 or more carbon atoms and its salt. The surface treatment agent may be used alone or in combination.

[0050] <Laminated separator for power storage device> The laminate separator for an electricity storage device according to the present embodiment has a high film resistance at high temperatures exceeding the melting point of the polyolefin resin, and has excellent insulating properties. Therefore, an electricity storage device using the laminate separator can maintain safety even if it becomes hot due to some factor.

[0051] Film resistance of laminated separator for power storage device (Ω cm 2) is measured by the method described below. Figure 1A shows a schematic diagram of the measurement device. 1 is a separator, 2A and 2B are a positive electrode and a negative electrode prepared by the method described in the Examples. 3 is a separator with an area of ​​2 cm 2 1 is an aramid film with a circular hole, which defines the effective electrode area. 4 is a silicone rubber sheet, which serves to reduce the variation in the surface pressure applied to the members 1 to 3. 5 is a ceramic plate with a thermocouple embedded in it. 6 is a heater, which heats the separator. 7 is a hydraulic press, which applies surface pressure to the members 1 to 4. 8 is an AC electrical resistance measuring device, which is connected to the current collector parts 2A and 2B, and measures the resistance between 2A and 2B. 9 is a thermometer, which is connected to the thermocouple of 5, and measures the temperature. 10 is a data collector, which is connected to the AC electrical resistance measuring device 8 and the thermometer 9, and records the resistance and temperature.

[0052] To explain in more detail, first, the separator 1, the positive electrode 2A, and the negative electrode 2B are sufficiently impregnated with an electrolyte (lithium fluoroborate / propylene carbonate / ethylene carbonate / γ-butyrolactone / trioctyl phosphate = weight ratio 7.2 / 23.3 / 25.7 / 43.3 / 0.5) on the portions coated with the electrode active materials. Then, the separator 1, the positive electrode 2A, the negative electrode 2B, the aramid film 3, and the silicone rubber 4 are stacked as shown in FIG. 1B and placed on a ceramic plate 5.

[0053] Next, while applying a surface pressure of 4 MPa to members 1 to 4 with a hydraulic press 7, the heater 6 is heated and the temperature and resistance value are continuously measured. The temperature is raised from room temperature 23°C to 200°C at a rate of 10°C / min, and the resistance value is measured with an AC of 1V and 1kHz. The obtained resistance value (Ω) is multiplied by the effective electrode area of ​​2 cm. 2 Multiplying this by 1 gives the membrane resistance (Ω cm 2 ) is calculated. 2 ) refer to the film resistance values ​​when the temperatures measured by a thermocouple embedded in the ceramic plate 5 are 170° C. and 200° C., respectively.

[0054] 170℃ membrane resistance (Ω cm) of laminated separator for power storage device 2 ) is 140 Ω cm from the viewpoint of improving the insulation properties of the laminated separator at high temperatures. 2 More than 160 Ω cm is preferable. 2 More preferably, 180 Ω cm or more. 2 On the other hand, from the viewpoint of increasing the productivity of the laminated separator, the 170°C membrane resistance is preferably 10,000 Ω cm. 2 Less than 9000 Ω cm is preferable. 2 Less than 8000 Ω cm is preferable. 2 The following is even more preferred:

[0055] 200℃ film resistance (Ω cm) of laminated separator for power storage device 2 ) is 200 Ω cm from the viewpoint of improving the insulation properties of the laminated separator at high temperatures. 2 More than 250 Ω cm 2 More than 300 Ω cm is preferable. 2 More preferably, 350 Ω cm or higher. 2 On the other hand, from the viewpoint of increasing the productivity of the laminate separator, the film resistance at 200°C is more preferably 20,000 Ω cm. 2 Less than 18000 Ω cm is preferable. 2 Less than 16000 Ω cm is preferable. 2 The following is even more preferred:

[0056] The rate of increase in membrane resistance (Ω cm) of laminated separators for power storage devices in the temperature range from 170°C to 200°C 2 / ℃) is 0 Ω cm 2 / °C, preferably above 1 Ω cm 2 / ℃ or more, and more preferably 2 Ω cm 2 / ℃ or more, and more preferably 3 Ω cm 2 / ℃ or more. The rate of increase in film resistance in the temperature range from 170℃ to 200℃ is the 200℃ film resistance (Ω cm 2 ) to 170℃ film resistance (Ω cm 2) and divide by a temperature difference of 30°C to calculate the average increase in film resistance per 1°C in the temperature range from 170°C to 200°C. A high rate of increase in film resistance means that the insulating properties of the separator become stronger as the temperature rises, and the use of a separator with a high rate of increase in film resistance improves the safety of the electricity storage device.

[0057] The thickness of the laminate separator for an electricity storage device is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 50 μm or less, and further preferably 3 μm or more and 25 μm or less. From the viewpoint of ensuring mechanical strength, a thickness of 1 μm or more is preferable, and from the viewpoint of increasing the energy density of the electricity storage device, a thickness of 100 μm or less is preferable. The thickness can be adjusted by controlling the die lip distance, the stretching ratio in the stretching step, etc.

[0058] From the viewpoint of achieving both ion conductivity and voltage resistance, the average pore size of the laminated separator for an electricity storage device is preferably 10 nm to 100 nm, more preferably 20 nm to 90 nm, and even more preferably 30 nm to 80 nm. The average pore size can be adjusted by controlling the composition ratio, the cooling rate of the extruded sheet, the stretching temperature, the stretching ratio, the heat setting temperature, the stretching ratio during heat setting, and the relaxation rate during heat setting, or by combining these.

[0059] The porosity of the laminated separator for an electricity storage device is preferably 25% to 95%, more preferably 30% to 90%, even more preferably 35% to 85%, and particularly preferably 40% to 80%. In order to improve ion conductivity, a porosity of 25% or more is preferable, and in order to ensure voltage resistance, a porosity of 95% or less is preferable. The porosity of the separator can be adjusted by controlling the composition of the porous layer A and the porous layer B, the stretching temperature, the stretching ratio, the heat setting temperature, the stretching ratio during heat setting, and the relaxation ratio during heat setting, or by combining these.

[0060] The air permeability of the laminated separator for an electricity storage device is preferably 30 seconds / 100 ml or more, more preferably 40 seconds / 100 ml or more, and even more preferably 50 seconds / 100 ml or more. If the air permeability is 30 seconds / 100 ml or more, self-discharge tends to be suppressed when used as a separator for an electricity storage device. On the other hand, the air permeability is preferably 150 seconds / 100 ml or less, more preferably 140 seconds / 100 ml or less, and even more preferably 130 seconds / 100 ml or less. If the air permeability is 150 seconds / 100 ml or less, good input / output characteristics tend to be obtained when used as a separator for an electricity storage device, which is preferable.

[0061] The reason why the laminated separator for a power storage device of this embodiment has high insulation at high temperatures is not necessarily clear, and is not limited to the action or principle described below, but it is believed that the separator of this embodiment has a good interface between the porous layer A mainly made of polyolefin resin and the porous layer B mainly made of inorganic particles. When the inorganic layer is formed by coating, components such as binders and dispersants may segregate at the interface between the substrate and the inorganic layer when the medium is volatilized by drying. In that case, the interaction between the substrate and the inorganic layer is weakened, and under severe conditions such as high temperature conditions, the molten substrate and the inorganic layer may separate, the insulation may not be maintained, and the membrane resistance value may decrease. In the laminated separator for a power storage device of this embodiment, since the porous layer A and the porous layer B are laminated by a co-extrusion method, it is believed that no components segregate at the interface between the porous layer A and the porous layer B, and the porous layer A and the porous layer B do not separate even at high temperatures.

[0062] One of the features of the laminated separator for an electricity storage device of this embodiment is that, at high temperatures where the polyolefin resin melts, the membrane resistance value increases as the temperature rises. In the separator of this embodiment, the inorganic particles contained in the porous layer B are subjected to a specific surface treatment, which increases the affinity between the inorganic particles and the polyolefin resin contained in the porous layer A, and the porous layer B and the porous layer A are further combined at high temperatures, which may increase the membrane resistance value.

[0063] Furthermore, the laminate separator for an electricity storage device of this embodiment has a lower porosity of the porous layer B, i.e., a higher density of the porous layer B, compared to a laminate separator produced by a conventional co-extrusion method. Generally, the process of producing a separator includes a process of stretching to an areal ratio of 50 times or more. After such a process, the porous layer B containing a large amount of inorganic particles is likely to break, and even if it can be stretched, the porosity of the porous layer B is likely to be higher than necessary. Since the density of the porous layer B is increased in the laminate separator for an electricity storage device of this embodiment, it is estimated that the insulating properties are easily maintained at high temperatures and the membrane resistance value is high.

[0064] <<Method for manufacturing laminated separator for power storage device>> An example of a method for producing a laminated separator for an electric storage device according to the present invention will be described below, but the method is not necessarily limited to this example. The method for producing a separator may, for example, include the following steps: (1) A step of melt-kneading a polyolefin resin and a plasticizer to obtain a molten material for forming the porous layer A; (2) A step of melt-kneading inorganic particles, a polyolefin resin, and a plasticizer to obtain a molten material for forming the porous layer B; (3) A step of forming a sheet-like melt having the porous layer A and the porous layer B laminated thereon; (4) cooling and solidifying the sheet-like melt; (5) stretching the sheet-like molded product at least uniaxially at an areal magnification of 20 times or more but less than 200 times; (6) extracting the plasticizer from the sheet-like molding; may also include

[0065] In the step (1), the polyolefin resin and the plasticizer are melt-kneaded. The melt-kneading method may, for example, be a method in which the polyolefin resin, the plasticizer, and other additives as necessary are fed into a resin kneading device such as an extruder, a kneader, a lab plastomill, a kneading roll, or a Banbury mixer, and the plasticizer is introduced at an arbitrary ratio while the resin components are heated and melted, and kneaded.

[0066] The plasticizer is not particularly limited, but it is preferable to use a non-volatile solvent that can form a homogeneous solution at or above the melting point of the polyolefin resin. Specific examples of such non-volatile solvents include, for example, hydrocarbons such as liquid paraffin and paraffin wax; esters such as dioctyl phthalate and dibutyl phthalate; and higher alcohols such as oleyl alcohol and stearyl alcohol. These plasticizers may be recovered and reused by distillation or other operations after extraction.

[0067] In addition, it is preferable to pre-mix the polyolefin resin and, if necessary, other additives in a predetermined ratio using a Henschel mixer or the like before feeding them into the resin kneading device. In the pre-kneading, it is preferable not to feed a plasticizer, and even if a plasticizer is fed, it is preferable to feed only a part of it, and to knead the remaining plasticizer while appropriately heating it and side-feeding it into the resin kneading device. By using such a kneading method, the dispersibility of the plasticizer is increased, and when the sheet-shaped molded product is stretched in the subsequent process, it tends to be possible to stretch it at a high ratio without film breakage.

[0068] Among the plasticizers, liquid paraffin is preferred because, when the polyolefin resin is polyethylene or polypropylene, it has high compatibility with these, and even when the molten mixture is stretched, interfacial peeling between the resin and the plasticizer is unlikely to occur, making it easier to perform uniform stretching.

[0069] The ratio of the polyolefin resin and the plasticizer is not particularly limited as long as they can be uniformly melted and kneaded to form into a sheet. For example, the mass fraction of the plasticizer in the composition consisting of the polyolefin resin and the plasticizer is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more and 80% by mass or less. When the mass fraction of the plasticizer is 90% by mass or less, the melt tension during melt molding tends to be sufficient to improve moldability. On the other hand, when the mass fraction of the plasticizer is 10% by mass or more, even when the mixture of the polyolefin resin composition and the plasticizer is stretched at a high ratio, the polyolefin molecular chain does not break, and a uniform and fine pore structure tends to be formed.

[0070] In the step (2), inorganic particles, polyolefin resin, and plasticizer are melt-kneaded. Examples of the melt-kneading method include a method in which inorganic particles, polyolefin resin, plasticizer, and other additives as necessary are fed into a resin kneading device such as an extruder, kneader, lab plastomill, kneading roll, or Banbury mixer, and the plasticizer is introduced at an arbitrary ratio while the resin components are heated and melted, and kneaded.

[0071] The plasticizer is not particularly limited, but it is preferable to use the same plasticizer as that used in the step (1). In addition, before being put into the resin kneading device, it is preferable to pre-knead the inorganic particles, polyolefin resin, and other additives as necessary in a predetermined ratio using a Henschel mixer or the like. In the pre-kneading, it is preferable not to add a plasticizer, and even if a plasticizer is added, it is preferable to add only a part of it, and knead the remaining plasticizer while appropriately heating it and side-feeding it into the resin kneading device. Furthermore, it is preferable to thoroughly disintegrate the pre-kneaded mixture using a roller mill, jet mill, hammer mill, pin mill, planetary mill, vibration mill, bead mill, or the like. By using such a kneading method, the uniformity of the composition is increased, and when the sheet-shaped molded product is stretched in the subsequent step, it tends to be possible to stretch it at a high ratio without film breakage.

[0072] The ratio of inorganic particles, polyolefin resin, and plasticizer is not particularly limited as long as they can be uniformly melted and kneaded to form a sheet. For example, the mass fraction of the plasticizer in the composition consisting of inorganic particles, polyolefin resin, and plasticizer is preferably 1% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 45% by mass or less, and even more preferably 10% by mass or more and 40% by mass or less. When the mass fraction of the plasticizer is 50% by mass or less, the melt tension during melt molding tends to be sufficient to improve moldability. On the other hand, when the mass fraction of the plasticizer is 1% by mass or more, flexibility is imparted to the melt kneaded product, and even when the kneaded product is stretched at a high ratio, a uniform and fine pore structure tends to be formed.

[0073] In the step (3), a sheet-like molten material is prepared in which the porous layer A and the porous layer B are laminated. Methods for forming the laminated sheet-like molten material include a method in which the layers are combined in a die and extruded into a sheet (in-die bonding method), and a method in which the layers are extruded into a sheet from a plurality of dies and bonded outside the die (out-of-die bonding method). From the viewpoint of increasing the adhesive strength of the porous layer A and the porous layer B, the in-die bonding method is preferred.

[0074] As an extrusion method for forming the laminated sheet-like melt, for example, a flat die method and an inflation method can be used. In either method, when bonding in the die, either a method in which the melts of the porous layer A and the porous layer B are supplied to separate manifolds of the lamination die and bonded in layers at the die lip inlet (multiple manifold method), or a method in which each melt is combined in layers in advance and supplied to the die (feed block method) can be used. The lip interval of the flat die is preferably 200 μm or more and 3,000 μm or less, and more preferably 500 μm or more and 2,500 μm or less. When the die lip interval is 200 μm or more, it is difficult for scum, streaks, defects, etc. to occur, and the quality of the separator is improved. On the other hand, when the die lip interval is 3,000 μm or less, the cooling speed of the laminated sheet-like melt is increased, and uneven cooling can be prevented, and the thickness stability of the sheet can be maintained.

[0075] In step (4), the sheet-shaped molten material is cooled and solidified to produce a sheet-shaped molded product. Examples of methods for cooling and solidifying the sheet-shaped molten material include a method in which the sheet-shaped molten material is brought into contact with a thermal conductor and cooled and solidified to a temperature sufficiently lower than the crystallization temperature of the resin component. Examples of thermal conductors used for cooling and solidifying include metal, water, air, and plasticizers. Among these, it is preferable to use a metal roll because of its high thermal conduction efficiency. In addition, it is more preferable to sandwich the extruded kneaded material between the metal rolls when bringing the kneaded material into contact with them, because this further increases the thermal conduction efficiency, orients the sheet to increase the film strength, and also tends to improve the surface smoothness of the sheet.

[0076] The sheet-shaped molded product may also be rolled. The rolling can be performed, for example, by a pressing method using a double belt press machine or the like. By performing rolling, the orientation of the surface layer portion in particular can be increased. The rolling area ratio is preferably more than 1 time and not more than 3 times, and more preferably more than 1 time and not more than 2 times. When the rolling ratio exceeds 1 time, the surface orientation increases, and the membrane strength of the finally obtained separator tends to increase. On the other hand, when the rolling ratio is 3 times or less, the difference in orientation between the surface layer portion and the central interior is small, and a uniform porous structure tends to be formed in the thickness direction of the membrane.

[0077] In the step (5), the sheet-form molded product is stretched. The stretching may be performed after the plasticizer is extracted from the sheet-form molded product. Furthermore, the stretching may be performed both before and after the plasticizer is extracted from the sheet-form molded product.

[0078] As the stretching process, either uniaxial stretching or biaxial stretching can be suitably used, but biaxial stretching is preferred from the viewpoint of improving the strength of the separator obtained. When the sheet-like molded product is stretched in the biaxial direction at a high ratio, the molecules are oriented in the plane direction, and the finally obtained separator becomes less likely to tear and has high puncture strength. Examples of the stretching method include simultaneous biaxial stretching, sequential biaxial stretching, multi-stage stretching, and multiple stretching. Simultaneous biaxial stretching is preferred from the viewpoint of improving puncture strength, uniformity of stretching, and fuse characteristics. Furthermore, sequential biaxial stretching is preferred from the viewpoint of easy control of plane orientation.

[0079] Simultaneous biaxial stretching refers to a stretching method in which stretching in MD (machine direction of separator continuous molding) and stretching in TD (direction crossing the separator MD at an angle of 90°) are performed simultaneously, and the stretching ratio in each direction may be different. Sequential biaxial stretching refers to a stretching method in which stretching in MD and TD is performed independently, and when stretching is performed in MD or TD, the other direction is in an unconstrained state or fixed at a fixed length.

[0080] The stretching ratio is preferably in the range of 20 to 200 times in area ratio, and more preferably in the range of 25 to 150 times. The stretching ratio in each axial direction is preferably in the range of 4 to 15 times in MD and 4 to 15 times in TD, and more preferably in the range of 5 to 12 times in MD and 5 to 12 times in TD. If the total area ratio is 25 times or more, sufficient strength tends to be imparted to the obtained separator, while if the total area ratio is 200 times or less, breakage of the separator during the stretching process tends to be prevented, and high productivity tends to be obtained.

[0081] In step (6), the plasticizer is removed from the sheet-like molded product to form a separator. For example, the plasticizer can be removed by immersing the sheet-like molded product in an extraction solvent to extract the plasticizer, followed by thorough drying. The method for extracting the plasticizer may be either a batch method or a continuous method. In order to suppress the shrinkage of the separator, it is preferable to restrain the ends of the sheet-like molded product during the series of immersion and drying steps. In addition, it is preferable to adjust the amount of plasticizer remaining in the separator to less than 1 mass% of the total mass of the separator.

[0082] The extraction solvent used for extracting the plasticizer is preferably a poor solvent for the polyolefin resin and a good solvent for the plasticizer, and has a boiling point lower than the melting point of the polyolefin resin. Examples of such extraction solvents include hydrocarbons such as n-hexane and cyclohexane; halogenated hydrocarbons such as methylene chloride and 1,1,1-trichloroethane; non-chlorine halogenated solvents such as hydrofluoroethers and hydrofluorocarbons; alcohols such as ethanol and isopropanol; ethers such as diethyl ether and tetrahydrofuran; and ketones such as acetone and methyl ethyl ketone. These extraction solvents may be recovered and reused by operations such as distillation.

[0083] In order to suppress the shrinkage of the separator, a heat treatment for heat setting may be performed after the stretching step or after the formation of the separator. The separator may also be subjected to post-treatment such as hydrophilization treatment with a surfactant or crosslinking treatment with ionizing radiation.

[0084] The separator is preferably subjected to a heat treatment for the purpose of heat setting in order to suppress shrinkage. Examples of the heat treatment method include a stretching operation performed in a predetermined temperature atmosphere and at a predetermined stretching ratio for the purpose of adjusting physical properties, and / or a relaxation operation performed in a predetermined temperature atmosphere and at a predetermined relaxation ratio for the purpose of reducing stretching stress. The relaxation operation may be performed after the stretching operation. These heat treatments can be performed using a tenter or roll stretching machine.

[0085] The stretching operation is preferably performed in the MD and / or TD of the membrane by 1.1 times or more, more preferably 1.2 times or more, from the viewpoint of obtaining a separator with higher strength and higher porosity. The relaxation operation is a reduction operation in the MD and / or TD of the membrane. The relaxation rate is a value obtained by dividing the dimension of the membrane after the relaxation operation by the dimension of the membrane before the relaxation operation. In addition, when both MD and TD are relaxed, the relaxation rate is a value obtained by multiplying the relaxation rate of MD and the relaxation rate of TD. The relaxation rate is preferably 1.0 or less, more preferably 0.97 or less, and even more preferably 0.95 or less. The relaxation rate is preferably 0.5 or more from the viewpoint of improving the quality of the separator. The relaxation operation may be performed in both MD and TD, or may be performed in only one of MD and TD.

[0086] The stretching and relaxation operation after the extraction of the plasticizer is preferably performed in TD. The temperature of the stretching and relaxation operation is preferably Tm-20°C or more and Tm+20°C or less, more preferably Tm-10°C or more and Tm+10°C or less, compared to the melting point (hereinafter also referred to as "Tm") of the polyolefin resin. The above-mentioned range of temperature for the stretching and relaxation operation is preferable from the viewpoint of the balance between the reduction of the heat shrinkage rate and the porosity.

[0087] The laminate separator for an electricity storage device of this embodiment functions sufficiently as a separator for an electricity storage device by itself, but may be coated with an inorganic material and / or an organic material as necessary.

[0088] <Electricity storage device> The electric storage device of the present embodiment includes a positive electrode, a negative electrode, and the laminated separator for an electric storage device according to the present embodiment. Specific examples of the electric storage device include lithium secondary batteries, lithium ion secondary batteries, sodium secondary batteries, sodium ion secondary batteries, potassium secondary batteries, potassium ion secondary batteries, magnesium secondary batteries, magnesium ion secondary batteries, calcium secondary batteries, calcium ion secondary batteries, aluminum secondary batteries, aluminum ion secondary batteries, nickel hydrogen batteries, nickel cadmium batteries, electric double layer capacitors, lithium ion capacitors, redox flow batteries, lithium sulfur batteries, lithium air batteries, and zinc air batteries. Among the above, from the viewpoint of practicality, lithium secondary batteries, lithium ion secondary batteries, potassium ion secondary batteries, nickel hydrogen batteries, or lithium ion capacitors are preferred, and lithium ion secondary batteries or potassium ion secondary batteries are more preferred.

[0089] The electricity storage device of this embodiment can be produced, for example, by stacking the above-mentioned positive electrode and negative electrode with a separator interposed therebetween and winding them as necessary to form a laminated electrode body or a wound electrode body, which is then loaded into an outer casing, connecting the positive and negative electrodes to the positive and negative electrode terminals of the outer casing via a lead body or the like, and further injecting a nonaqueous electrolyte solution containing a nonaqueous solvent such as a chain or cyclic carbonate and an electrolyte such as a lithium salt into the outer casing and then sealing the outer casing.

[0090] The exterior body of the electricity storage device is not particularly limited, but a metal can container, a laminate container made of a metal foil laminate film, etc. can be suitably used. The shape of the electricity storage device is not particularly limited, and examples thereof include a cylindrical shape, a square shape, a coin shape, a flat shape, a sheet shape, etc.

[0091] 《Positive electrode》 The positive electrode is prepared by adding an appropriate amount of a conductive assistant such as acetylene black and a binder such as polyvinylidene fluoride to a positive electrode active material to prepare a positive electrode mixture, which is then applied to a current collecting material such as aluminum foil, dried, and then pressed to fix a positive electrode mixture layer onto the current collecting material. However, the method for preparing the positive electrode is not limited to the above-mentioned example method.

[0092] The positive electrode active material is not particularly limited, but from the viewpoint of increasing the energy density and durability of the power storage device, it is preferable to use a positive electrode active material represented by the general formula LiNi x Co y Ma 1-x-y A layered oxide positive electrode active material represented by the general formula LiMnO2 {wherein Ma represents one or more selected from the group consisting of Mn and Al, 0≦x≦1, 0≦y≦1, and x+y≦1.} 2-x Mb x a spinel-type oxide positive electrode active material represented by the formula Li2McO3 and LiMdO2 {wherein Mc and Md each independently represent one or more metals selected from the group consisting of transition metals, and 0.2≦x≦0.7.}; a composite oxide represented by the general formula zLi2McO3-(1-z)LiMdO2 {wherein Mc and Md each independently represent one or more metals selected from the group consisting of transition metals, and 0.05≦z≦0.95.}; a Li-rich layered oxide positive electrode active material represented by the formula LiMe 1-x Fe x olivine-type positive electrode active material represented by the formula: Li2MfPO4 {wherein Me represents one or more selected from the group consisting of Mn and Co, and 0≦x≦1.}; and Li2MfPO4F {wherein Mf represents one or more selected from the group consisting of transition metals.}.

[0093] General formula LiNi x Co y Ma 1-x-y In view of structural stability, the layered oxide positive electrode active material represented by the formula: LiNiO2 {wherein Ma represents one or more selected from the group consisting of Mn and Al, 0≦x≦1, 0≦y≦1, and x+y≦1.} isx Co y Mn 1-x-y O2 {wherein 0≦x≦1, 0≦y≦1, and x+y≦1.} or LiNi x Co y Al 1-x-y It is preferable that the composition is represented by the formula: LiCoO2 {wherein 0.7≦x≦1, 0≦y≦0.3, and x+y≦1.} More preferable compositions are LiCoO2, LiNi x Co y Mn 1-x-y O2 {wherein 0.3≦x≦1, 0≦y≦0.4, and x+y≦1.}, and LiNi 0.85 Co 0.1 Al 0.05 One example is O2.

[0094] 《Negative electrode》 The negative electrode can be produced by adding an appropriate amount of a thickener such as carboxymethyl cellulose and a binder such as styrene butadiene rubber to the negative electrode active material to prepare a negative electrode mixture, which is then applied to a current collecting material such as copper foil, dried, and then pressed to fix the negative electrode mixture layer onto the current collecting material. However, the method for producing the negative electrode is not limited to the above-mentioned example method.

[0095] In this embodiment, the negative electrode active material that can be used for the negative electrode is not particularly limited, but for example, alloy compounds such as Al, Si, Sn, metal oxides such as CuO, CoO, lithium-containing compounds such as lithium titanate, and carbon materials can be used. From the viewpoint of improving the energy density of the power storage device, carbon materials that can absorb and release lithium ions at a relatively low potential are preferable. Examples of such carbon materials include, but are not limited to, hard carbon, soft carbon, artificial graphite, natural graphite, pyrolytic carbon, coke, glassy carbon, fired bodies of organic polymer compounds, fired bodies of organic natural products, carbon fibers, mesocarbon microbeads, and carbon black.

[0096] When a carbon material is used as the negative electrode active material, the interlayer distance d of the (002) plane of the carbon material 002is preferably 0.37 nm or less, more preferably 0.35 nm or less, and further preferably 0.34 nm or less. 002 The lower limit is not particularly limited, but is theoretically about 0.335 nm. The size of the crystallites in the c-axis direction of the carbon material is preferably 3 nm or more, more preferably 8 nm or more, and even more preferably 25 nm or more. The upper limit of the crystallite size is not particularly limited, but is usually about 200 nm. The average particle size of the carbon material is preferably 3 μm or more and 15 μm or less, and more preferably 5 μm or more and 13 μm or less. The purity of the carbon material is preferably 99.9% or more.

[0097] The power storage device according to this embodiment is highly safe and has excellent productivity, and therefore can be widely used not only as a battery for electric vehicles but also as a power source for various devices, including batteries for consumer devices such as smartphones. EXAMPLES

[0098] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. The analytical and evaluation methods used in the examples and comparative examples are as follows.

[0099] (1) Film thickness (μm) The film thickness of the sample was measured at room temperature of 23° C. using a micro thickness gauge (Type KBM, Toyo Seiki Seisakusho Co., Ltd.). The thickness of each layer of the sample was measured by observing the cross section of the sample with a scanning electron microscope.

[0100] (2) Porosity (%) A 10cm x 10cm square sample was cut from the separator and its volume (cm 3 ) and mass (g), and compare them with the film density (g / cm 3 ) the porosity was calculated using the following equation. Porosity (%) = (volume-mass / film density) / volume x 100 The film density was calculated from the respective densities and the mixing ratio of the polyolefin resin and inorganic particles used.

[0101] (3) Air permeability (sec / 100ml) The air permeability of the samples was measured using a Gurley air permeability meter (Toyo Seiki Seisakusho, Ltd.) conforming to JIS P-8117.

[0102] (4)Piercing strength (gf) Using a handy compression tester "KES-G5" (Kato Tech Co., Ltd.), the separator was fixed in a sample holder with an opening diameter of 11.3 mm. A puncture test was performed on the center of the fixed separator at room temperature of 23°C under conditions of a needle tip curvature radius of 0.5 mm and a puncture speed of 2 mm / sec, to measure the puncture strength (gf) as the maximum puncture load.

[0103] (5) Film resistance (Ω cm 2 ) A 40 mm × 30 mm square sample was cut from the separator to prepare sample 1. A 55 mm × 20 mm square positive electrode and negative electrode were cut from the positive electrode and negative electrode fabricated by the method described below to prepare positive electrode 2A and negative electrode 2B. Of the 55 mm length of 2A and 2B, 10 mm was not coated with the electrode active material, and the current collector was exposed.

[0104] Thereafter, the portions of sample 1, positive electrode 2A and negative electrode 2B on which the electrode active material was applied were sufficiently impregnated with an electrolyte (lithium borofluoride / propylene carbonate / ethylene carbonate / γ-butyrolactone / trioctyl phosphate=weight ratio 7.2 / 23.3 / 25.7 / 43.3 / 0.5).

[0105] Then, a measuring device was prepared as shown in FIG. 1A, and a sample 1, a positive electrode 2A, a negative electrode 2B, and a 2 cm 2 An aramid film 3 (thickness 9 μm) with a circular hole and a silicone rubber 4 (thickness 4 mm) were overlapped as shown in FIG. 1B and placed on a ceramic plate 5 with an embedded thermocouple.

[0106] Next, while applying a surface pressure of 4 MPa to members 1 to 4 with a hydraulic press 7, the heater 6 was heated, and the temperature and resistance value were continuously measured using a thermometer 9 connected to the thermocouple 5 and an AC electrical resistance measuring device 8 "AG-4311" (Ando Electric Co., Ltd.) connected to the current collectors of the positive electrode 2A and the negative electrode 2B. The temperature was raised from room temperature 23°C to 200°C at a rate of 10°C / min, and the resistance value was measured with an AC of 1V and 1kHz.

[0107] The obtained resistance value (Ω) is multiplied by the effective electrode area of ​​2 cm 2 Multiplying this by 1 gives the membrane resistance (Ω cm 2 ) was calculated. The film resistances at 170°C and 200°C were calculated as the film resistances at 170°C and 200°C (Ω cm 2 ) and the rate of increase in film resistance (Ω cm 2 / ℃) is the 200℃ film resistance value (Ω cm 2 ) to 170℃ film resistance (Ω cm 2 ) and divided by the temperature difference of 30°C.

[0108] (6) Tests using lithium-ion secondary batteries <<Preparation of positive electrode sheet>> LiNi as the positive electrode active material 1 / 3 Mn 1 / 3 Co 1 / 3 O2 (Nippon Chemical Industry Co., Ltd.), acetylene black powder (Denka Co., Ltd.) as a conductive assistant, and polyvinylidene fluoride solution (Kureha Co., Ltd.) as a binder were mixed in a solid content mass ratio of 90:6:4, and N-methyl-2-pyrrolidone was added as a dispersion solvent so that the solid content was 40 mass%, and further mixed to prepare a slurry solution. This slurry solution was applied to both sides of an aluminum foil as a current collector material with a thickness of 20 μm, the solvent was dried and removed, and then the applied aluminum foil was rolled with a roll press to obtain a positive electrode sheet in which the porosity of the positive electrode mixture portion was adjusted to 38%.

[0109] <<Preparation of negative electrode sheet>> Artificial graphite (Hitachi Chemical Co., Ltd.) was mixed as the negative electrode active material, and styrene butadiene rubber and carboxymethyl cellulose aqueous solution as the binder in a solid content mass ratio of 100:1.5:1.8, and water was added as a dispersion solvent so that the solid content was 45 mass%, and further mixed to prepare a slurry solution. This slurry solution was applied to both sides of a copper foil as a current collector material with a thickness of 18 μm, the solvent was dried and removed, and then the applied copper foil was rolled with a roll press to obtain a negative electrode sheet in which the porosity of the negative electrode mixture portion was adjusted to 40%.

[0110] <Preparation of non-aqueous electrolyte> A solution containing 1 mol / L of LiPF6 in a mixed solvent of ethylene carbonate and ethyl methyl carbonate in a volume ratio of 1:2 as a non-aqueous solvent was prepared.

[0111] <<Preparation of lithium-ion secondary battery>> The positive electrode sheet and the negative electrode sheet prepared as described above were laminated on both sides of the separator obtained in the examples and comparative examples described below to obtain a laminate. The obtained laminate was inserted into a bag (exterior body) made of an aluminum laminate film in which both sides of an aluminum foil (thickness 40 μm) were covered with a resin layer, with the positive and negative terminals protruding. Thereafter, the nonaqueous electrolyte prepared as described above was injected into the bag, and the bag was vacuum sealed to produce a pouch-type lithium ion secondary battery.

[0112] <<First charge / discharge of a lithium-ion secondary battery>> The pouch-type lithium-ion secondary battery was placed in a thermostatic chamber "PLM-73S" (Futaba Scientific Co., Ltd.) set at 25°C and connected to a charge / discharge device "ACD-01" (Asuka Electronics Co., Ltd.). The secondary battery was then charged at a constant current of 0.1C until it reached a voltage of 4.2V, charged at a constant voltage of 4.2V for one hour, and then discharged at a constant current of 0.1C until it reached 3.0V. This charge / discharge cycle was repeated three times. The battery was then charged at a constant current of 0.1C until it reached a voltage of 4.2V, bringing the lithium-ion secondary battery into a fully charged state. Note that 1C represents the current value when the full capacity of the battery is discharged in one hour, and 0.1C represents 1 / 10 of that current value.

[0113] <20C discharge test of lithium-ion secondary battery> The pouch-type lithium-ion secondary battery after the initial charge and discharge was charged at a constant current of 1 / 3 C until it reached a voltage of 4.2 V, then charged at a constant voltage of 4.2 V for 1 hour, and discharged at a constant current of 1 C to 3.0 V. The battery was then charged at a constant current of 1 / 3 C until it reached a voltage of 4.2 V, then charged at a constant voltage of 4.2 V for 1 hour, and discharged at a constant current of 20 C to 3.0 V. From the results of the above series of charge and discharge, the 20 C capacity retention rate (%) was calculated using the following formula. 20C capacity retention rate (%) = 20C discharge capacity / 1C discharge capacity x 100

[0114] <Lithium-ion secondary battery cycle test> The pouch-type lithium-ion secondary battery after the 20C discharge test was placed in a thermostatic chamber "PLM-73S" (Futaba Scientific Co., Ltd.) set at 50°C, and connected to a charge / discharge device "ACD-01" (Asuka Electronics Co., Ltd.). The secondary battery was then charged at a constant current of 1C until it reached a voltage of 4.2V, then charged at a constant voltage of 4.2V for 1 hour, and discharged at a constant current of 1C until it reached 3.0V. The above series of charge / discharge cycles was counted as one cycle, and this cycle was repeated for 500 cycles, and the capacity retention rate (%) after 500 cycles was measured. The capacity retention rate (%) after 500 cycles was calculated using the following formula: Capacity retention rate after 500 cycles (%) = Discharge capacity at 500th cycle / Discharge capacity at 1st cycle x 100

[0115] <Safety testing of lithium-ion secondary batteries> A pouch-type lithium-ion secondary battery in a fully charged state after the first charge and discharge was placed on a pedestal installed in an explosion-proof booth whose temperature was controlled at 60°C. A nail (diameter 3 mm, made of SUS304) was then inserted into the battery at an angle of 90° to the flat surface of the battery, at a speed of 30 mm / sec, into the center of the battery until the nail penetrated the battery. The behavior of the battery after the nail was inserted was observed and a hazard level (HL) was assigned to it. The lower the HL number, the better the safety of the battery was maintained. HL0: No change HL1: Protection mechanism activated HL2: Corrupted HL3:Leakage HL4: Eruption HL5: Ignition HL6:Rupture HL7: Explosion

[0116] [Example 1] Composition A, the raw material for porous layer A, was prepared by mixing 47 parts by mass of high-density polyethylene (melting point 135°C) having a viscosity average molecular weight of 700,000, 46 parts by mass of high-density polyethylene (melting point 137°C) having a viscosity average molecular weight of 250,000, 7 parts by mass of polypropylene (melting point 163°C) having a viscosity average molecular weight of 400,000, and 0.3 parts by mass of tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane as an antioxidant using a tumbler blender.

[0117] Next, 98 parts by mass of surface-treated barium sulfate with an average particle size of 300 nm (1 part by mass of sodium stearate was used for surface treatment for 100 parts by mass of barium sulfate), 2 parts by mass of ultra-high molecular weight polyethylene (melting point 134°C) with a viscosity average molecular weight of 2 million, and 0.012 parts by mass of tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane as an antioxidant were mixed in a Henschel mixer to prepare composition B, which is the raw material for porous layer B, and composition B was finely pulverized using a jet mill.

[0118] Composition A was supplied to a twin-screw extruder, and liquid paraffin having a kinetic viscosity of 70.6 cSt at 40°C was side-fed into the twin-screw extruder cylinder so that the proportion of composition A in the melt-kneaded product was 35 mass% and the extrusion rate was 13 kg / h. The composition was melt-kneaded while being heated to 180°C in the twin-screw extruder.

[0119] Composition B was supplied to a twin-screw extruder, and liquid paraffin having a kinetic viscosity of 70.6 cSt at 40°C was side-fed into the twin-screw extruder cylinder so that the proportion of composition B in the molten mixture was 82 mass% and the extrusion rate was 16 kg / h. The mixture was melt-kneaded while being heated to 180°C in the twin-screw extruder.

[0120] The two obtained molten kneaded products were laminated in a T-die capable of co-extrusion of two types of three layers, so that the two outer layers were composition A and the middle layer was composition B, and extruded onto a cooling roll whose surface temperature was controlled at 90°C. The extrudate was brought into contact with the cooling roll, molded, and cooled to solidify, thereby obtaining a sheet-like molded product.

[0121] This sheet-like molded product was introduced into a simultaneous biaxial stretching machine and subjected to simultaneous biaxial stretching at a temperature of 122°C and a ratio of 7x7. Next, the sheet-like stretched product was introduced into an extraction tank and immersed in methylene chloride to extract and remove the liquid paraffin, and the methylene chloride was dried. Thereafter, the obtained porous film was introduced into a uniaxial stretching machine and stretched 1.7 times in the width direction at a temperature of 134°C, and then relaxed by about 20% in the width direction to obtain a laminated separator. The evaluation results of the obtained laminated separator are shown in Table 1 and FIG. 2.

[0122] [Example 2] A laminate separator was produced in the same manner as in Example 1, except that instead of the lamination method in Example 1, both surface layers were laminated with composition B and the intermediate layer was laminated with composition A. The evaluation results of the obtained laminate separator are shown in Table 1 and FIG.

[0123] [Example 3] Instead of composition B in Example 1, a laminate separator was produced in the same manner as in Example 1, except that composition B was used, which was prepared by mixing 95 parts by mass of surface-treated barium sulfate having an average particle size of 300 nm (1 part by mass of sodium stearate was used for surface treatment for 100 parts by mass of barium sulfate), 5 parts by mass of ultra-high molecular weight polyethylene having a viscosity average molecular weight of 2 million (melting point 134°C), and 0.03 parts by mass of tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane as an antioxidant with a Henschel mixer. The evaluation results of the obtained laminate separator are shown in Table 1.

[0124] [Example 4] A laminate separator was produced in the same manner as in Example 3, except that instead of the lamination method of Example 3, both surface layers were laminated with composition B and the intermediate layer was laminated with composition A. The evaluation results of the obtained laminate separator are shown in Table 1.

[0125] [Example 5] Instead of composition B in Example 1, 70 parts by mass of surface-treated barium sulfate with an average particle size of 300 nm (1 part by mass of sodium stearate was used for surface treatment for 100 parts by mass of barium sulfate), 30 parts by mass of high-density polyethylene (melting point 135°C) with a viscosity average molecular weight of 700,000, and 0.18 parts by mass of tetrakis [methylene-3- (3',5'-di-t-butyl-4'-hydroxyphenyl) propionate] methane as an antioxidant were mixed in a Henschel mixer to prepare composition B, and a laminate separator was produced in the same manner as in Example 1, except that the extrusion rate was set to 22 kg / h when composition B was supplied to an extruder and melt-kneaded. The evaluation results of the obtained laminate separator are shown in Table 1.

[0126] [Example 6] A laminate separator was produced in the same manner as in Example 5, except that instead of the lamination method in Example 5, both surface layers were laminated with composition B and the intermediate layer was laminated with composition A. The evaluation results of the obtained laminate separator are shown in Table 1.

[0127] [Example 7] A laminated separator was produced in the same manner as in Example 1, except that composition B was prepared using surface-treated boehmite having an average particle size of 300 nm (1 part by mass of sodium stearate was used for surface treatment per 100 parts by mass of boehmite) instead of the surface-treated barium sulfate having an average particle size of 300 nm in Example 1. The evaluation results of the obtained laminated separator are shown in Table 1.

[0128] [Example 8] A laminate separator was produced in the same manner as in Example 7, except that, instead of the lamination method in Example 7, both surface layers were laminated with composition B and the intermediate layer was laminated with composition A. The evaluation results of the obtained laminate separator are shown in Table 2.

[0129] [Example 9] A laminate separator was produced in the same manner as in Example 1, except that composition B was prepared using surface-treated titania having an average particle size of 300 nm (1 part by mass of sodium stearate was used for surface treatment per 100 parts by mass of titania) instead of the surface-treated barium sulfate having an average particle size of 300 nm in Example 1. The evaluation results of the obtained laminate separator are shown in Table 2.

[0130] [Example 10] A laminate separator was produced in the same manner as in Example 9, except that instead of the lamination method of Example 9, both surface layers were laminated with composition B and the intermediate layer was laminated with composition A. The evaluation results of the obtained laminate separator are shown in Table 2.

[0131] [Example 11] A laminated separator was produced in the same manner as in Example 1, except that composition B was prepared using surface-treated barium sulfate having an average particle size of 50 nm (3 parts by mass of sodium stearate was used for the surface treatment per 100 parts by mass of barium sulfate) instead of the surface-treated barium sulfate having an average particle size of 300 nm in Example 1. The evaluation results of the obtained laminated separator are shown in Table 2.

[0132] [Example 12] A laminated separator was produced in the same manner as in Example 1, except that composition B was prepared using surface-treated barium sulfate having an average particle size of 600 nm (0.5 parts by mass of sodium stearate was used for the surface treatment relative to 100 parts by mass of barium sulfate) instead of the surface-treated barium sulfate having an average particle size of 300 nm in Example 1. The evaluation results of the obtained laminated separator are shown in Table 2.

[0133] [Comparative Example 1] A laminated separator was produced according to the method described in Example 1 of Patent Document 1. The evaluation results of the obtained laminated separator are shown in Table 2 and Figure 2. In the measurement of the membrane resistance value and various evaluations using a lithium ion secondary battery, the laminated separator was arranged so that the inorganic coating layer faced the positive electrode.

[0134] [Comparative Example 2] A laminated separator was produced according to the method described in Example 5 of Patent Document 2. The evaluation results of the obtained laminated separator are shown in Table 2 and FIG.

[0135] [Comparative Example 3] A laminated separator was produced according to the method described in Example 5 of Patent Document 3. The evaluation results of the obtained laminated separator are shown in Table 2 and FIG.

[0136] [Comparative Example 4] An attempt was made to produce a laminated separator in the same manner as in Example 1, except that fine pulverization with a jet mill was not performed when preparing composition B of Example 1. However, breakage frequently occurred during the production of the laminated separator, and the separator could not be produced stably.

[0137] [Table 1]

[0138] [Table 2]

[0139] As seen from Tables 1 and 2, in comparison with Comparative Example 1 in which a laminated separator is produced by forming an inorganic layer on a polyolefin substrate by coating, Examples 1 to 12 have an excellent property of maintaining insulation at high temperatures, with the film resistance increasing as the temperature rises at temperatures above the melting point of the polyolefin resin. In a battery safety test, when the laminated separators of Examples 1 to 12 are used, the safety of the battery is maintained better than that of Comparative Example 1. Furthermore, Examples 1 to 12 are superior to Comparative Example 1 in terms of battery output characteristics.

[0140] Next, in comparison with Comparative Example 2 in which a laminated separator was produced by a co-extrusion method using silica as the inorganic particles, Examples 1 to 12 have a porous layer B containing inorganic particles with a high density, and are excellent in terms of the property of maintaining insulating properties at high temperatures. In addition, the battery has excellent cycle characteristics and output characteristics, and is also excellent in safety.

[0141] In addition, in Examples 1 to 12, the density of the porous layer B containing inorganic particles is high and the property of maintaining insulating properties at high temperatures is excellent compared to Comparative Example 3 in which the laminated separator is produced by co-extrusion using barium sulfate as the inorganic particles. As a result, in the battery safety test, when the laminated separators of Examples 1 to 12 are used, the safety of the battery is maintained better than that of Comparative Example 3.

[0142] From the above, it has become clear that a laminated separator for an electricity storage device, which has a porous layer A containing a polyolefin resin and a porous layer B containing a large amount of inorganic particles and exhibits specific resistance behavior at high temperatures, not only functions well as a separator, but also contributes to improving the safety of the electricity storage device at high temperatures, and further contributes to improving the durability and output characteristics of the electricity storage device. [Explanation of symbols]

[0143] 1 Separator 2A, 2B positive electrode, negative electrode 3 Area 2cm 2 Aramid film with circular holes 4 Silicone rubber sheet 5. Ceramic plate with embedded thermocouple 6. Heater 7. Hydraulic press 8. AC Electrical Resistance Measuring Device 9 Thermometer 10. Data Collector

Claims

1. The porous layer A contains a polyolefin resin, and the porous layer B contains inorganic particles that have been surface-treated with one or more selected from saturated fatty acids and their salts, unsaturated fatty acids and their salts, polysiloxanes, and silane coupling agents, the content of the inorganic particles in the porous layer B being 60% by mass or more and less than 100% by mass, the porosity of the porous layer B being 30% by mass or more and 70% by mass or less, and the film resistance at 200° C. being 200 Ω cm 2 and a membrane resistance value exceeding 170° C., and comprising at least one porous layer A and at least one porous layer B laminated together.

2. 2 . The laminate separator for an electricity storage device according to claim 1 , wherein at least two of the porous layers A and at least one of the porous layers B are laminated.

3. 2 . The laminate separator for an electricity storage device according to claim 1 , wherein at least one of the porous layers A and at least two of the porous layers B are laminated.

4. 4. The laminate separator for an electricity storage device according to claim 1, wherein both surface layers are the porous layer A or the porous layer B.

5. 5. The laminate separator for an electricity storage device according to claim 1, wherein the inorganic particles have an average particle size of 31 nm or more and 1000 nm or less.

6. The laminate separator for an electricity storage device according to any one of claims 1 to 5, wherein the inorganic particles are one or more selected from the group consisting of boehmite, alumina, titania, magnesium oxide, zinc oxide, calcium sulfate, aluminum sulfate, barium sulfate, magnesium hydroxide, lithium phosphate, sodium phosphate, and magnesium phosphate.

7. 7. The laminate separator for an electricity storage device according to claim 1, wherein the porous layer A contains polyethylene having a viscosity average molecular weight of 500,000 or more and 5,000,000 or less.

8. 8. The laminate separator for an electricity storage device according to claim 1, wherein the porous layer B contains a polyolefin having a viscosity average molecular weight of 200,000 or more and 10,000,000 or less.

9. 9. The laminate separator for an electricity storage device according to claim 1, wherein the laminate separator for an electricity storage device has an air permeability of 30 sec / 100 ml or more and 150 sec / 100 ml or less.

10. An electricity storage device comprising a positive electrode, a negative electrode, and the laminate separator for an electricity storage device according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • High-melting-point microporous lithium-ion rechargeable battery separator, manufacturing method, and usage method.

    JP2013535792A

  • Separator for electrochemical element

    JP2014086142A

  • Laminated porous film and non-aqueous electrolyte secondary battery

    JP2015171814A

  • Laminated microporous film and method for producing the same and cell separator

    JP2016060061A

  • Multilayer microporous membrane and separator for electricity storage device

    JP2017080977A