Fiber-reinforced composite frame
The fiber-reinforced composite frame addresses delamination and buckling by using high-toughness materials at corners and low-toughness materials elsewhere, with a tapered design to enhance bending strength and reduce costs.
Patent Information
- Application Number
- JP2021045403
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-19
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2041-03-19
AI Technical Summary
Fiber-reinforced composite frames experience delamination and buckling at corners due to compressive stress, leading to reduced bending strength and increased manufacturing costs when high-toughness materials are used to prevent these issues.
A fiber-reinforced composite frame design with high-toughness material at corner regions and low-toughness material elsewhere, combined with a tapered shape to manage stress concentration and delamination, reduces manufacturing costs while enhancing bending strength.
The frame effectively suppresses delamination and buckling, improving bending strength while minimizing costs by strategically using high-toughness materials only where needed.
Smart Images

Figure 0007551544000006 
Figure 0007551544000008 
Figure 0007551544000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a fiber-reinforced composite frame. [Background technology]
[0002] 2. Description of the Related Art Conventionally, for frames constituting the body of a vehicle, etc., a fiber-reinforced composite frame manufactured from a lightweight and highly rigid fiber-reinforced composite material has been used.
[0003] For example, the fiber-reinforced composite frame described in Patent Document 1 has a quasi-isotropic structure that allows it to withstand input loads from all directions, and specifically, has a structure formed by stacking multiple fiber orientation layers in which the reinforcing fibers are oriented in different directions.
[0004] Furthermore, in this frame, in order to improve the rigidity of the corners of the frame, the lamination of the fiber orientation layers at the corners of the frame cross section is increased to locally increase the thickness of the corners. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-193362 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, even in a structure in which the number of fiber-oriented layers is increased at the corners, as in the frame described above, it is difficult to prevent a problem unique to fiber-reinforced composite frames, namely buckling caused by delamination at the corners.
[0007] That is, when a bending load is applied to a fiber-reinforced composite frame, delamination occurs between the fiber-oriented layers at the corners of the frame cross section, and cracks occur starting from the delaminated corners in the fiber-oriented layers of the frame on the surface where compressive stress acts (i.e., the inner curved surface of the bent frame) and on the adjacent surfaces, causing buckling of the frame. If buckling of the frame occurs, the bending strength will be significantly reduced. Therefore, the frame described in the above Patent Document 1 cannot prevent the occurrence of such a phenomenon.
[0008] Therefore, in order to suppress the occurrence of buckling of the frame, it is conceivable to construct the entire frame from a high-toughness fiber-reinforced composite material with high toughness values between fiber orientation layers (resin layers). However, in this case, the problem of increased manufacturing costs for the frame arises.
[0009] The present invention has been made in consideration of the above circumstances, and has an object to provide a fiber-reinforced composite frame that suppresses the occurrence of buckling and improves bending strength while reducing manufacturing costs. [Means for solving the problem]
[0010] A fiber-reinforced composite frame according to claim 1 of the present invention is a fiber-reinforced composite frame extending in a predetermined direction so as to form a closed cross-section having a plurality of corners, and manufactured from a fiber-reinforced composite material in which a plurality of resin layers are laminated, the frame comprising: a compression surface portion in which a compressive stress is generated along the longitudinal direction when a bending load that bends the frame in a lateral direction perpendicular to the longitudinal direction of the frame is input to the frame; a side portion extending in the lateral direction from the corner adjacent to the compression surface portion; and a tensile surface portion extending in the longitudinal direction at a position spaced from the compression surface portion, the tensile stress being generated along the longitudinal direction when the bending load is input to the frame; and a region of the corner adjacent to the compression surface portion comprises a high-toughness fiber-reinforced composite material having a higher toughness value in the shear direction between resin layers than the fiber-reinforced composite material constituting the region of the tensile surface portion.
[0011] According to this configuration, when a bending load is input to the frame constituting a closed cross section in a direction perpendicular to the longitudinal direction of the frame, a compressive stress is generated in the compression surface portion along the longitudinal direction of the frame. The corner region adjacent to the compression surface portion is provided with a high-toughness fiber-reinforced composite material having a higher toughness value in the shear direction between the resin layers than the fiber-reinforced composite material constituting the tensile surface portion. In this configuration, since the corner region adjacent to the compression surface portion is provided with a high-toughness fiber-reinforced composite material, it is possible to delay the occurrence of delamination at the corner portion and to reduce the speed of progression of delamination. On the other hand, since the tensile surface portion separated from the compression surface portion does not contribute to bending strength, it is possible to use a low-toughness, inexpensive fiber-reinforced composite material and reduce the manufacturing cost of the frame. As a result, it is possible to suppress the progression of delamination to the compression surface portion and the side portion, suppress the occurrence of buckling of the frame, and improve the bending strength of the frame while reducing the manufacturing cost of the frame.
[0012] In the above-mentioned fiber-reinforced composite frame, it is preferable that the portions in the corner regions that are located on the same plane as the side portions are formed from the high-toughness fiber-reinforced composite material.
[0013] According to this configuration, the corner regions located on the same plane as the side portions are made of high toughness fiber reinforced composite material, so that it is possible to prevent delamination at the corners from progressing toward the side portions when the frame is bent, thereby further suppressing buckling of the frame and further improving the bending strength of the frame.
[0014] A fiber-reinforced composite frame according to claim 3 of the present invention is a fiber-reinforced composite frame extending in a predetermined direction so as to form a closed cross-section having a plurality of corners, and manufactured from a fiber-reinforced composite material in which a plurality of resin layers are laminated, wherein the frame comprises: a compression surface portion in which a compressive stress is generated along the longitudinal direction when a bending load that bends the frame in a lateral direction perpendicular to the longitudinal direction of the frame is input to the frame; a side portion extending in the lateral direction from the corner adjacent to the compression surface portion; and a tensile surface portion extending in the longitudinal direction at a position spaced from the compression surface portion, and in which a tensile stress is generated along the longitudinal direction when the bending load is input to the frame; and the side portion comprises a high-toughness fiber-reinforced composite material having a higher toughness value in the shear direction between resin layers than the fiber-reinforced composite material constituting the region of the tensile surface portion.
[0015] As described above, when a bending load is applied to the frame constituting a closed cross section in a direction perpendicular to the longitudinal direction of the frame, a compressive stress is generated in the compression surface portion along the longitudinal direction of the frame. In this configuration, the side portion extending in the short direction from the corner adjacent to the compression surface portion is provided with a high-toughness fiber-reinforced composite material having a higher toughness value in the shear direction between the resin layers than the fiber-reinforced composite material constituting the region of the tensile surface portion, so that the corner portion can be reinforced by the side portion provided with the high-toughness fiber-reinforced composite material. This makes it possible to delay the timing of occurrence of delamination at the corner portion and to reduce the speed of progression of delamination. On the other hand, since the tensile surface portion separated from the compression surface portion does not contribute to bending strength, it is possible to use a low-toughness, inexpensive fiber-reinforced composite material and reduce the manufacturing cost of the frame. As a result, it is possible to suppress the progression of delamination to the compression surface portion and the side portion, suppress the occurrence of buckling of the frame, and improve the bending strength of the frame while reducing the manufacturing cost of the frame.
[0016] In the fiber-reinforced composite frame according to claim 1, it is preferable that an area of the side portion is provided with the high toughness fiber-reinforced composite material.
[0017] With this configuration, even if delamination occurs at a corner adjacent to a compression surface portion during bending deformation of the frame, the delamination is guided to progress to the compression surface portion made of a low toughness fiber reinforced composite material without progressing to the side surface portion made of a high toughness fiber reinforced composite material, which makes it possible to further suppress crack progression to the side surface portion, further suppress buckling of the frame, and further improve the bending strength of the frame.
[0018] In the above-mentioned fiber-reinforced composite frame, it is preferable that the compression surface area is composed of a low-toughness fiber-reinforced composite material having a lower toughness value in the shear direction between resin layers than the high-toughness fiber-reinforced composite material.
[0019] With this configuration, the occurrence of buckling of the frame is suppressed by the high-toughness fiber-reinforced composite material provided at the corners adjacent to the compression surface portion, and the manufacturing cost of the frame can be further reduced by constructing the compression surface portion from an inexpensive low-toughness fiber-reinforced composite material.
[0020] In the above-mentioned fiber-reinforced composite frame, the high toughness fiber-reinforced composite is preferably disposed on the center side in the thickness direction of the corner portion.
[0021] When a bending load is applied to the frame, delamination tends to occur more easily at corners closer to the center in the thickness direction. Therefore, by disposing the high toughness fiber reinforced composite material on the center side in the thickness direction of the corners as in the above configuration, it is possible to delay the timing of delamination and slow down the speed at which delamination progresses even with a small amount of high toughness fiber reinforced composite material. As a result, it is possible to suppress the occurrence of buckling in the frame and improve the bending strength of the frame while further reducing the manufacturing cost of the frame.
[0022] In the fiber-reinforced composite frame according to claim 1 above, it is preferable that the end portion of the high-toughness fiber-reinforced composite material on the compression surface side and / or the side surface side has a tapered shape in which the thickness of the end portion gradually changes.
[0023] When a bending load is applied to the frame, delamination tends to occur easily at the interface between a high-toughness fiber-reinforced composite material and another fiber-reinforced composite material having lower toughness. In the above-mentioned configuration, the end portion on the compression surface side and / or the side surface side of the high-toughness fiber-reinforced composite material has a tapered shape in which the thickness of the end portion gradually changes, thereby mitigating the sudden change in toughness near the end portion of the high-toughness fiber-reinforced composite material. This makes it possible to mitigate stress concentration near the end portion and suppress delamination. As a result, it is possible to further suppress buckling of the frame and further improve the bending strength of the frame.
[0024] In the above-mentioned fiber-reinforced composite frame, it is preferable that the frame is applied to at least one selected from the group consisting of a center pillar, a bumper beam, a side sill, a hinge pillar, a front pillar, and a cross member that constitute the body of a vehicle.
[0025] According to this configuration, by applying the above frame to at least one of the center pillar, bumper beam, side sill, hinge pillar, front pillar, and cross member that constitute the body of the vehicle, when a bending load is input to the frames that constitute each of the above parts of the body during a vehicle collision, buckling of the entire frame is prevented and the frame can withstand the bending load, thereby improving the rigidity of the vehicle body. Effect of the Invention
[0026] According to the fiber-reinforced composite frame of the present invention, it is possible to reduce the manufacturing costs of the frame while suppressing the occurrence of buckling of the frame and improving the bending strength. [Brief description of the drawings]
[0027] [Figure 1] 1 is a schematic perspective view showing the overall configuration of a fiber-reinforced composite frame according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a front view showing an end face of the fiber-reinforced composite frame of FIG. [Diagram 3] FIG. 3 is an exploded perspective view partially showing the layered structure of the fiber-reinforced composite frame of FIG. 2. [Figure 4] FIG. 1 is an explanatory diagram of toughness values, where (a) is a diagram for explaining the toughness value (GIC) in the peel direction between layers of a fiber-reinforced composite material, and (b) is a diagram for explaining the toughness value (GIIC) in the shear direction between layers of a fiber-reinforced composite material. [Diagram 5] FIG. 3 is a cross-sectional explanatory view showing the cross-sectional structure of the fiber-reinforced composite frame of FIG. 2. [Figure 6] FIG. 13 is an explanatory diagram showing the cross-sectional structure of each frame and the load distribution when a bending load is input to each frame: I: a frame of this embodiment; II: a frame of variant example 1 of the present invention; III: a frame made only of a high-toughness fiber-reinforced composite material as comparative example 1; and IV: a frame made only of a low-toughness fiber-reinforced composite material as comparative example 2. [Figure 7] FIG. 5 is an explanatory diagram showing the cross-sectional structure of each frame and the load distribution when a bending load is input to each frame, in V: a frame according to variant example 2 of the present invention, in which only the side portions are made of a high-toughness fiber-reinforced composite material, and III to IV: frames of comparative examples 1 and 2. [Figure 8] FIG. 6 is an explanatory diagram showing the cross-sectional structure of each frame and the load distribution when a bending load is input to each frame in Comparative Example 4 (frame VI), in which only the compression surface portion is made of a high-toughness fiber-reinforced composite material, and Comparative Examples 1 and 2 (frames III to IV). [Figure 9] FIG. 7 is an explanatory diagram showing the cross-sectional structure of each frame and the load distribution when a bending load is input to each frame in Comparative Example 5 (frame VII), in which only the tensile surface portion is made of a high-toughness fiber-reinforced composite material, and Comparative Examples 1 and 2 (frames III to IV). [Figure 10]VIII(1): An explanatory diagram showing the cross-sectional structure of each frame and the load distribution when a bending load is input to each frame in a frame in which a high-toughness fiber-reinforced composite material is arranged in the range from the surface layer of the corner to a small depth, which is the first stage of variant example 3 of the present invention, and in frames III to IV: comparative examples 1 and 2. [Figure 11] VIII(2): A frame in which a high-toughness fiber-reinforced composite material is arranged in the range from the surface layer of the corner to a medium depth, which is the second stage of variant 3 of the present invention, and III to IV: frames of comparative examples 1 and 2. An explanatory diagram showing the cross-sectional structure of the frame of variant 3 and the load distribution when a bending load is input to each frame. [Figure 12] VIII(3): A frame in which a high-toughness fiber-reinforced composite material is arranged in a range from the surface layer of the corner to a depth of about 100 mm, which is the third stage of the modified example 3 of the present invention, and III to IV: frames of comparative examples 1 and 2. An explanatory diagram showing the cross-sectional structure of the frame of the modified example 3 and the load distribution when a bending load is input to each frame. [Figure 13] 10A to 10C are cross-sectional explanatory views showing the cross-sectional structures of frames when the material arrangement and lamination configuration within the cross section of the high toughness fiber reinforced composite material in the frame are changed, as various modified examples of the present invention. [Figure 14] This is a cross-sectional explanatory diagram of a structure, as another variation of the present invention, in which high-toughness fiber-reinforced composite material is placed inside the corners and side portions of the frame, and the end portion of the high-toughness fiber-reinforced composite material on the compression surface portion side has a tapered convex portion. [Figure 15] FIG. 11 is a cross-sectional explanatory diagram of a structure, as yet another variation of the present invention, in which a high-toughness fiber-reinforced composite is placed inside a corner of a frame, and the end of the high-toughness fiber-reinforced composite on the compression surface side has a tapered convex portion, and the end on the side surface side has a tapered concave portion. [Figure 16] FIG. 2 is an explanatory perspective view showing an example in which the fiber-reinforced composite frame of FIG. 1 is applied to components of various parts of a vehicle body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the accompanying drawings.
[0029] As shown in FIGS. 1 and 2, a fiber-reinforced composite frame 1 (hereinafter referred to as frame 1) is oriented in a predetermined direction (the longitudinal direction D in FIG. 1) so as to form a closed cross section 1b having a plurality of corners 5. L ) and is a high-strength member manufactured from a fiber-reinforced composite material in which a plurality of fiber orientation layers (resin layers) 11-14 (see FIG. 3) are laminated. The frame 1 is used as a member constituting each part of a vehicle body 121 (see FIG. 16) of a vehicle to be described later.
[0030] Specifically, the frame 1 has a basic structure in which the longitudinal direction D of the frame 1 is L The material has four surfaces extending in a axial direction, namely, a compression surface portion 2, a pair of side surface portions 3 spaced apart on both sides of the compression surface portion 2 in the width direction, and a tensile surface portion 4 spaced apart from but facing the compression surface portion 2.
[0031] The compression surface portion 2, the pair of side surface portions 3, and the tension surface portion 4 form a rectangular closed cross section 1b having four corners 5. The corners 5 may be chamfered in a straight line as shown in Fig. 2, or may be chamfered in an arc as shown in Fig. 5.
[0032] The compression surface portion 2 is in the longitudinal direction D of the frame 1. L (i.e., the longitudinal direction D L (inclined 90 degrees to the short side) D S A bending load F that bends frame 1 toward B When input to frame 1, the longitudinal direction D L In other words, the compressed surface portion 2 is the inner curved surface of the bent frame 1.
[0033] Here, the bending load F B is the longitudinal direction D of frame 1 L Short direction D perpendicular to SFor example, when a vehicle body 121 (see FIG. 16) of a vehicle collides with an external obstacle (such as an automobile or a roadside object), as shown in FIG. 1, the frame 1 is supported at both ends (for example, in the simplified model of FIG. 1, the frame 1 is supported at both ends by a pair of fulcrums S), and the compression surface portion 2 is subjected to a compression load (collision load) F. P in the short direction D S (i.e., the normal direction of the compression surface portion 2 in FIG. 1). In this case, the bending load F P is received by the compression surface portion 2 of the frame 1.
[0034] Or, bending load F B is the longitudinal direction D of frame 1 L From the end 1a in the longitudinal direction D L Bending loads that occur when a compressive load (collision load) is applied toward the cross member 126 are also assumed (for example, bending load of the cross member 126 when an obstacle collides with the side of the vehicle body 121 in FIG. 16). In this case, the compressive load is applied to the end 1a of the frame 1.
[0035] Each of the pair of side portions 3 is formed in a width direction D from a pair of corner portions 5 adjacent to the compression surface portion 2. S (specifically, the bending load F B or compressive load F P The side surface 3 is a portion that constitutes the frame 1 when the frame 1 is subjected to a bending load F B When subjected to a force, compressive stress is generated in an area closer to the compression surface portion 2 than the neutral axis N in Fig. 1, and tensile stress is generated in an area closer to the tensile surface portion 4 than the neutral axis N. Corners 5 are formed by each of the pair of side portions 3 and the compression surface portion 2.
[0036] The tensile surface portion 4 is spaced apart from the compression surface portion 2 in the longitudinal direction D L and bending load F B When input to frame 1, the longitudinal direction D LThe tensile stress σ2 occurs along the tensile surface 4. That is, the tensile surface portion 4 becomes the outer curved surface of the bent frame 1. The tensile surface portion 4 and each of the pair of side surface portions 3 form corner portions 5.
[0037] The compression surface portion 2, the pair of side portions 3, and the tensile surface portion 4 are each formed by a laminate formed by stacking a plurality of fiber orientation layers, for example, a longitudinal orientation layer 11, a transverse orientation layer 12, a +45 degree orientation layer 13, and a -45 degree orientation layer 14 as shown in Figure 3.
[0038] Specifically, the compression surface portion 2, the pair of side surface portions 3, and the tension surface portion 4 each have the same laminated structure so as to have quasi-isotropy, for example, as shown in Fig. 3. That is, each of the surface portions 2 to 4 is formed by a laminate formed by laminating a longitudinal orientation layer 11, a lateral orientation layer 12, a +45 degree orientation layer 13, and a -45 degree orientation layer 14 as a plurality of fiber orientation layers (resin layers) in approximately equal proportions so as to have quasi-isotropy.
[0039] Specifically, as shown in FIG. 3, the longitudinal orientation layer 11 is formed by a substrate 11b and a frame 1 in the longitudinal direction D. L Same direction as D 1 (i.e., in the longitudinal direction D L The reinforcing fibers 11a are oriented at an inclination angle of 0 degrees with respect to the surface.
[0040] The base material 11b (12b, 13b, 14b) refers to a sheet-like base material made of reinforcing fibers 11a (12a, 13a, 14a) and resin used in autoclave molding or press molding, or a base material with reinforcing fibers 11a temporarily attached used in RTM molding. The base material 11b is made of, for example, a resin material having excellent heat resistance, strength, and processability, such as a resin such as epoxy resin. The reinforcing fibers 11a are made of a lightweight and high-strength fiber material, such as carbon fiber, glass fiber, aramid fiber, cellulose fiber, steel fiber, or the like. In particular, carbon fiber is preferable because it is both lightweight and strong.
[0041] Specifically, as shown in FIG. 3, the transverse direction orientation layer 12 is formed by a substrate 12b and a frame 1 in the transverse direction D. S , i.e., the longitudinal direction D L and the direction perpendicular to D 2 (at an inclination angle of 90 degrees). The base material 12b and the reinforcing fibers 12a of the short-side orientation layer 12 are made of the same material as the base material 11b and the reinforcing fibers 11a of the long-side orientation layer 11, but other materials may also be used.
[0042] The +45 degree orientation layer 13 has reinforcing fibers 13a arranged in the longitudinal direction D L The -45 degree orientation layer 14 is a layer in which the reinforcing fibers 14a are oriented in a direction rotated 45 degrees counterclockwise in the in-plane direction of the orientation layer 13 based on the longitudinal direction D. L It is a layer oriented in a direction rotated 45 degrees clockwise (−45 degrees if the counterclockwise direction is the positive direction) in the in-plane direction of the orientation layer 14 with respect to the reference direction.
[0043] Specifically, the +45-degree orientation layer 13 is, as shown in FIG. L Direction D is inclined +45 degrees to 3 Similarly, the −45° orientation layer 14 is specifically composed of a base material 14b and a reinforcing fiber 13a oriented in the longitudinal direction D, as shown in FIG. LD is inclined at -45 degrees to 4 The base materials 13b, 14b and the reinforcing fibers 13a, 14a are also made of the same materials as the base material 11b and the reinforcing fibers 11a of the longitudinal orientation layer 11, but other materials may also be used.
[0044] As described above, each of the compression surface portion 2, side surface portion 3, and tensile surface portion 4 that constitute the frame 1 of this embodiment is made of a fiber-reinforced composite material molded by stacking fiber orientation layers (resin layers) 11 to 14.
[0045] Here, it is believed that if a fiber-reinforced composite material having a high toughness value (degree of difficulty in peeling) between the above-mentioned fiber orientation layers (resin layers) 11 to 14 is used, interlayer peeling will be less likely to occur.
[0046] There are two types of toughness values between the resin layers. Specifically, as shown in Figs. 4(a) and (b), the toughness values in the peeling direction (thickness direction D) between the two resin layers A1 and A2 bonded to each other are T The toughness value (GIC) in the shear direction D between the resin layers A1 and A2 U There is a toughness value for this material (GIIC).
[0047] The inventors focused on the grain size integral coefficient of shear (GIIC), which has a significant effect on delamination of the resin layer, and created frame 1 of this embodiment, which makes it possible to suppress the progression of delamination while suppressing an increase in the manufacturing cost of frame 1, by partially arranging a fiber-reinforced composite material with a high grain size integral coefficient of shear (GIIC) (high-toughness fiber-reinforced composite material 21 in Figure 5) in the corner 5 adjacent to the compression surface 2, which is the starting point of delamination in frame 1.
[0048] That is, in the frame 1 of this embodiment, as shown in Figure 5, the region of the corner 5 adjacent to the compression surface portion 2 is provided with a high-toughness fiber-reinforced composite 21 having a higher toughness value (GIIC) in the shear direction between each fiber orientation layer (resin layer) 11 to 14 than the fiber-reinforced composite material (low-toughness fiber-reinforced composite material 22 in Figure 5) that constitutes the region of the tensile surface portion 4.
[0049] 5, the corners 5 adjacent to the compression surface portions 2 are made of the high toughness fiber reinforced composite material 21, while the portions other than the corners 5, i.e., the compression surface portion 2 and a portion connected to the pair of side surface portions 3 and the tensile surface portion 4, are made of the low toughness fiber reinforced composite material 22. The high toughness fiber reinforced composite material 21 has a property that the toughness value (GIIC) in the shear direction between the resin layers is higher than that of the low toughness fiber reinforced composite material 22.
[0050] In this embodiment, the high toughness fiber reinforced composite 21 has a toughness value (GIC) in the peel direction equivalent to that of the low toughness fiber reinforced composite 22, while the toughness value (GIIC) in the shear direction is greater than that of the low toughness fiber reinforced composite 22 (for example, about 0.65 greater).
[0051] In the frame 1 shown in FIG. 5, the region of the compression surface portion 2 is constituted by a low toughness fiber reinforced composite material 22 having a lower toughness value in the shear direction between the resin layers than the high toughness fiber reinforced composite material 21.
[0052] 5, the corner 5 has an arc-shaped portion (R portion) 5a that is chamfered into an arc shape, and a rounded portion 5b that is an end of the arc-shaped portion 5a and is located on the same plane as the side portion 3. The arc-shaped portion 5a and the rounded portion 5b are formed of a high-toughness fiber-reinforced composite material 21.
[0053] The frame 1 of this embodiment configured as described above is applied to various members constituting a vehicle body 121 that require high bending strength during a vehicle collision, for example, at least one selected from the group consisting of a center pillar 120, a bumper beam 122, a side sill 123, a hinge pillar 124, a front pillar 125, and a cross member 126, as shown in FIG. 16.
[0054] Of these groups, when the frame of the above embodiment is applied to the center pillar 120, the bumper beam 122, the side sill 123, the hinge pillar 124, and the front pillar 125, the compressed surface portion 2 (i.e., the surface to which the collision load is input) may be arranged on the surface facing the outside of the vehicle body 121. In this case, the corner portion 5 (made of the high-toughness fiber reinforced composite material 21) adjacent to the compressed surface portion 2 is located on the outside of the vehicle body 121, similar to the compressed surface portion 2.
[0055] Moreover, the cross member 126 may have the compressed surface portion 2 disposed on a surface facing upward or downward. In this case, the corner portion 5 (a component of the high toughness fiber reinforced composite material 21) adjacent to the compressed surface portion 2 is located on the upper or lower side of the cross member 126, similar to the compressed surface portion 2.
[0056] Here, the center pillar 120 is a member extending in the vertical direction between the front door and the rear door at the side end of the vehicle body 121. The bumper beam 122 is a member extending in the width direction of the vehicle body 121 at the front end of the vehicle body 121 and constituting a bumper. The side sill 123 is a member extending in the front-rear direction of the vehicle body 121 at the lower side end of the vehicle body 121. The hinge pillar 124 is a member extending in the vertical direction at the front side of the side end of the vehicle body 121 and to which the front door of the vehicle body 121 is hinged. The front pillar 125 is a member extending in a substantially arc shape upward and backward (diagonally backward) on both sides of the windshield at the front side of the vehicle body 121. The cross member 126 is a member extending in the width direction of the vehicle body 121 at the floor part of the vehicle body 121.
[0057] (Features of this embodiment) (1) As shown in Figs. 1 and 2, the frame 1 of this embodiment is extended in a predetermined direction so as to form a closed cross section 1b having a plurality of corners 5, and is manufactured from a fiber-reinforced composite material in which a plurality of resin layers are laminated. L Short direction D perpendicular to S A bending load F that bends frame 1 toward B When input to frame 1, the longitudinal direction D L The compression surface 2 along which the compressive stress σ1 occurs and the corner 5 adjacent to the compression surface 2 in the short direction D S and a side surface portion 3 extending in the longitudinal direction D at a position spaced apart from the compression surface portion 2. L and bending load F B When input to frame 1, the longitudinal direction D L and a tensile surface portion 4 along which a tensile stress σ2 occurs.
[0058] As shown in Figure 5, the area of the corner 5 adjacent to the compression surface portion 2 is provided with a high toughness fiber reinforced composite 21 having a higher toughness value in the shear direction between the resin layers than the low toughness fiber reinforced composite 22 that constitutes the area of the tensile surface portion 4.
[0059] According to this configuration, the frame 1 constituting the closed cross section 1b is in the longitudinal direction D of the frame 1. L Bending load F perpendicular to B When the input is made, the compression surface portion 2 is in the longitudinal direction D of the frame 1. LA compressive stress σ1 occurs along the tensile surface 4. The corner 5 region adjacent to the compression surface 2 is provided with a high-toughness fiber-reinforced composite material 21 having a higher toughness value in the shear direction between the resin layers than the fiber-reinforced composite material constituting the tensile surface 4 region. In this configuration, since the corner 5 region adjacent to the compression surface 2 is provided with the high-toughness fiber-reinforced composite material 21, it is possible to delay the timing of delamination at the corner 5 and to reduce the speed of delamination. On the other hand, the tensile surface 4 separated from the compression surface 2 does not contribute to bending strength, so that a low-toughness, inexpensive fiber-reinforced composite material can be used, thereby reducing the manufacturing cost of the frame 1. As a result, it is possible to reduce the manufacturing cost of the frame 1 while suppressing the development of delamination to the compression surface 2 and the side surface 3, suppressing the occurrence of buckling of the frame 1, and improving the bending strength of the frame 1.
[0060] (2) In the frame 1 of this embodiment, as shown in FIG. 5, the R-end portion 5b located on the same plane as the side portion 3 in the corner 5 area is formed from high-toughness fiber-reinforced composite material 21, similar to the arc-shaped portion (R portion) 5a.
[0061] According to this configuration, the rounded portion 5b located on the same plane as the side portion 3 in the area of the corner 5 is formed of the high toughness fiber reinforced composite material 21, so that it is possible to prevent delamination at the corner 5 from progressing toward the side portion 3 when the frame 1 is bent and deformed. This makes it possible to further prevent buckling of the frame 1 and further improve the bending strength of the frame 1.
[0062] (3) In the frame 1 of this embodiment, the region of the compression surface portion 2 is made of a low toughness fiber reinforced composite material 22 that has a lower toughness value in the shear direction between the resin layers than the high toughness fiber reinforced composite material 21. With this configuration, the occurrence of buckling of the frame 1 is suppressed by the high toughness fiber reinforced composite material 21 provided at the corner portion 5 adjacent to the compression surface portion 2, and by forming the compression surface portion 2 from the inexpensive low toughness fiber reinforced composite material 22, it is possible to further reduce the manufacturing cost of the frame 1.
[0063] (4) In the frame 1 of this embodiment, as shown in FIG. 16, the frame 1 is applied to at least one selected from the group consisting of a center pillar 120, a bumper beam 122, a side sill 123, a hinge pillar 124, a front pillar 125, and a cross member 126 that constitute the body of a vehicle.
[0064] According to this configuration, the frame 1 is applied to at least one of the center pillar 120, the bumper beam 122, the side sill 123, the hinge pillar 124, the front pillar 125, and the cross member 126 that constitute the body of the vehicle, so that in the event of a vehicle collision, a bending load F is applied to the frame 1 that constitutes each of the above-mentioned parts of the body. B When the input is made, the buckling of the entire frame 1 is avoided and the frame 1 is supported by the bending load F B This makes it possible to improve the rigidity of the vehicle body.
[0065] Example 1 Next, the bending strength of the frame 1 of this embodiment shown in FIG. 5 will be described in comparison with Modification 1 of the present invention and a comparative example.
[0066] The frame 1 of this embodiment has a square cross section with sides of 50 mm, and has arc-shaped chamfered portions with a radius of 10 mm at the corners 5. The thickness of each face of the frame 1 is 3.42 mm.
[0067] When examining the bending strength, the frame 1 is supported at both ends by two supports S (300 mm apart) as shown in Figure 1 based on the procedure of a general bending test. L The indenter was placed on the midpoint C of the frame 1 and displaced downward, bending the frame 1. As a result, the relationship between the downward displacement X of the indenter and the bending load P of the frame 1 (i.e., the reaction force that the indenter receives from the frame 1) was investigated, as shown by curve I in the graph of Figure 6.
[0068] In the frame 1 of this embodiment shown in Figures 5 and 6, the corner portions 5 adjacent to the compression surface portion 2 are made of a high toughness fiber reinforced composite material 21, and the compression surface portion 2 other than the corner portions 5, the pair of side portions 3 and the tensile surface portion 4 are made of a low toughness fiber reinforced composite material 22.
[0069] 5-6 in that both the corner portions 5 adjacent to the compression surface portion 2 and the pair of side portions 3 are made of high toughness fiber reinforced composite material 21, but the other configurations are the same. That is, in the frame 31 of modification 1 shown in FIG. 6, the corner portions 5 adjacent to the compression surface portion 2 and the pair of side portions 3 are made of high toughness fiber reinforced composite material 21, and the compression surface portion 2 and the tensile surface portion 4 are made of low toughness fiber reinforced composite material 22.
[0070] The bending strength of frame 31 of modified example 1 shown in FIG. 6 was also examined in the same manner as for frame 1, and the results are shown as curve II in the graph of FIG.
[0071] On the other hand, as comparative examples 1 and 2, frames 41 and 51 shown in FIG.
[0072] Frame 41 of Comparative Example 1 is generally made of high toughness fiber reinforced composite material 21, and has the same cross-sectional shape as frame 1. Frame 41 of Comparative Example 1 shown in Fig. 6 was also examined for bending strength in the same manner as frame 1, and the results are shown as curve III in the graph of Fig. 6.
[0073] Moreover, frame 51 of Comparative Example 2 is generally made of low toughness fiber reinforced composite material 22, and has the same cross-sectional shape as frame 1. For frame 51 of Comparative Example 2 shown in Fig. 6, the bending strength was examined in the same manner as for frame 1, and the results are shown as curve IV in the graph of Fig. 6.
[0074] In the graph of FIG. 6, first, curve III showing the bending load P of the frame 41 of Comparative Example 1, which is entirely made of the high toughness fiber reinforced composite material 21, shows a high bending load at all displacements X. On the other hand, curve IV showing the bending load P of the frame 51 of Comparative Example 2, which is entirely made of the low toughness fiber reinforced composite material 22, shows a low bending load at all displacements X. In view of this, it can be seen that if the frame is made of the high toughness fiber reinforced composite material 21, it is possible to suppress the progress of delamination and the occurrence of buckling of the frame 1, thereby improving the bending strength of the frame 1. However, if the entire frame is made of the high toughness fiber reinforced composite material 21, as in the case of the frame 41 of Comparative Example 1, there is a concern that the manufacturing cost will increase.
[0075] On the other hand, curve II showing the bending load P of the frame 31 of variant example 1 of the present invention, in which the corner portion 5 adjacent to the compression surface portion 2 and the pair of side portions 3 are made of high toughness fiber reinforced composite material 21, shows a high bending load at almost all displacements X, next to the above curve III.
[0076] Next, curve I, which shows the bending load P of the frame 1 of this embodiment in which only the corner 5 adjacent to the compression surface portion 2 is made of the high toughness fiber reinforced composite material 21, also shows a high bending load at almost all displacements X, next to the above curve II.
[0077] 6, it can be seen that even if only the corners 5 adjacent to the compression surface portions 2 are made of high toughness fiber reinforced composite material 21 as in the frame 1 of this embodiment, it is possible to sufficiently obtain the effect of suppressing the progression of delamination and suppressing the occurrence of buckling of the frame 1, thereby improving the bending strength of the frame 1. Moreover, because only the corners 5 adjacent to the compression surface portions 2 are made of high toughness fiber reinforced composite material 21, it is possible to suppress the occurrence of buckling of the frame 1 and improve the bending strength while reducing the manufacturing cost of the frame 1.
[0078] Furthermore, by looking at curve II of the graph in Figure 6, it can be seen that by constructing the corner portions 5 adjacent to the compression surface portion 2 and the pair of side portions 3 from high toughness fiber reinforced composite material 21, as in frame 31 of variant example 1 of the present invention, the manufacturing cost of frame 31 can be reduced while further suppressing the progression of interlayer delamination and suppressing the occurrence of buckling of frame 1 more than frame 1 of embodiment 1 described above, thereby further improving the bending strength of frame 1.
[0079] That is, in the frame 31 of the first modified example of the present invention, not only the corners 5 adjacent to the compression surface portions 2 but also the regions of the side surface portions 3 are provided with the high toughness fiber reinforced composite material 21. With this configuration, even if delamination occurs at the corners 5 adjacent to the compression surface portions 2 during bending deformation of the frame 1, the delamination is guided to progress to the compression surface portions 2 composed of the low toughness fiber reinforced composite material 22 without progressing to the side surface portions 3 composed of the high toughness fiber reinforced composite material 21. This makes it possible to further suppress crack progression to the side surface portions 3, further suppress buckling of the frame 1, and further improve the bending strength of the frame 1.
[0080] Next, Figures 7 to 9 show, as variant example 2 and three further comparative examples, frame 61 of variant example 2 of the present invention and comparative example 3 (only the side portion 3 is made of high toughness fiber reinforced composite material 21), frame 71 of comparative example 4 (only the compression surface portion 2 is made of high toughness fiber reinforced composite material 21), and frame 81 of comparative example 5 (only the tensile surface portion 4 is made of high toughness fiber reinforced composite material 21), with curves V to VII showing the bending strengths of these frames 61 to 81, respectively.
[0081] As shown in FIG. 7, when only the side portion 3 is made of the high toughness fiber reinforced composite material 21 as in the frame 61 of the modified example 2 of the present invention, the bending strength is lower than that of the curve III in the case of the frame 41 of the comparative example 1 (all made of the high toughness fiber reinforced composite material 21), but higher than that of the curve IV in the case of the frame 51 of the comparative example 2 (all made of the low toughness fiber reinforced composite material 22), as shown in the curve V. Therefore, it can be seen from the graph in FIG. 7 that the high toughness fiber reinforced composite material 21 constituting the side portion 3 of the frame 61 of the modified example 2 of the present invention contributes to improving the bending strength to some extent. That is, in the configuration in which only the side portion 3 adjacent to the corner portion 5 is provided with the high toughness fiber reinforced composite material 21 as in the modified example 2 of the present invention, it is possible to reinforce the corner portion 5 by the side portion 3 provided with the high toughness fiber reinforced composite material 21. This makes it possible to delay the timing of delamination at the corner portion 5 and to slow down the speed at which delamination progresses. On the other hand, since the tensile surface portions 4 separated from the compression surface portions 2 do not contribute to bending strength, it is possible to use an inexpensive fiber-reinforced composite material with low toughness, thereby reducing the manufacturing costs of the frame 61. As a result, it is possible to reduce the manufacturing costs of the frame 61 while suppressing the progression of delamination to the compression surface portions 2 and the side surface portions 3, thereby suppressing the occurrence of buckling of the frame 61, and improving the bending strength of the frame 1.
[0082] However, when only the compression surface portion 2 is made of the high toughness fiber reinforced composite material 21, as in the case of frame 71 of comparative example 4 shown in Figure 8, as shown by curve VI, the bending strength obtained is only slightly higher than that of curve IV in the case of frame 51 of comparative example 2 (all made of low toughness fiber reinforced composite material 22), and it can be seen that the high toughness fiber reinforced composite material 21 constituting the compression surface portion 2 makes little contribution to improving the bending strength.
[0083] Furthermore, when only the tensile surface portion 4 is made of high toughness fiber reinforced composite material 21, as in the case of frame 81 of Comparative Example 5 shown in Figure 9, as shown by curve VII, the bending strength obtained is approximately the same as that of curve IV for frame 51 of Comparative Example 2 (all made of low toughness fiber reinforced composite material 22), and it can be seen that the high toughness fiber reinforced composite material 21 constituting the tensile surface portion 4 does not contribute to improving the bending strength.
[0084] 6 to 9, it can be seen that when the corners 5 adjacent to the compression surface portion 2 are made of high toughness fiber reinforced composite material 21, as in the case of frame 1 of this embodiment and frame 31 of modified example 1 in Fig. 6, the bending strength is greatly improved by the effect of suppressing the progress of delamination at the corners 5. Furthermore, it can be seen that when the side surface portion 3 is made of high toughness fiber reinforced composite material 21, next to the corners 5 adjacent to the compression surface portion 2, this also contributes greatly to improving the bending strength.
[0085] 6 to 9, it can be seen that even if the compression surface portion 2 and the tensile surface portion 4 are made of the high toughness fiber reinforced composite material 21, the contribution to improving the bending strength is low. This leads to the conclusion that it is preferable to use an inexpensive low toughness fiber reinforced composite material for the compression surface portion 2 and the tensile surface portion 4 in order to reduce the manufacturing cost of the frame.
[0086] Example 2 As shown in Figure 5, in the frame 1 of the above embodiment, the corner 5 adjacent to the compression surface 2 is made of high toughness fiber reinforced composite material 21 throughout the entire thickness direction. However, as in the frame 91 of variant example 3 of the present invention shown in Figures 10 to 12, the high toughness fiber reinforced composite material 21 may be arranged within a certain depth range from the surface layer of the corner 5, and a low toughness fiber reinforced composite material 22 may be arranged on the central side of the corner 5.
[0087] The frame 91 of the above-mentioned variant example 3 has a structure in which, in each of Figures 10 to 12, high toughness fiber reinforced composites 21 are arranged in small, medium and large ranges from the surface portion of the corner 5, and low toughness fiber reinforced composites 22 are arranged at the thickness-wise center of the corner 5.
[0088] When the high toughness fiber reinforced composite material 21 is arranged in a small range from the surface layer of the corner 5, as in the frame 91 of the modified example 3 shown in Fig. 10, the bending strength obtained is only slightly higher than that of the curve IV in the case of the frame 51 of the comparative example 2 (all made of the low toughness fiber reinforced composite material 22), as shown in the curve VIII(1), and the contribution to the improvement of the bending strength is low. However, from the curve VIII(2) in the case where the high toughness fiber reinforced composite material 21 is arranged in a medium range from the surface layer of the corner 5 shown in Fig. 11 and the curve VIII(3) in the case where the high toughness fiber reinforced composite material 21 is arranged in a large range shown in Fig. 12, it can be seen that the bending strength improves slightly as the high toughness fiber reinforced composite material 21 at the corner 5 becomes thicker.
[0089] However, it can be seen that the improvement in bending strength is smaller than that in the case of the frame 1 of the above embodiment, in which the corner 5 is made of the high toughness fiber reinforced composite material 21 over the entire thickness direction (curve I in FIG. 6). Considering this point, it can be deduced that if the high toughness fiber reinforced composite material 21 is disposed on the center side of the corner 5 of the frame 1 in the thickness direction, the improvement in bending strength will be greater.
[0090] Considering further, a bending load F B When the input (see FIG. 1) is made, delamination tends to occur more easily in the vicinity of the center position in the thickness direction of the corner 5. Therefore, as in frames 201-203 in FIGS. 13-14 described later, it is preferable that the high toughness fiber reinforced composite material 21 is disposed on the center side in the thickness direction of the corner 5. By disposing the high toughness fiber reinforced composite material 21 on the center side in the thickness direction of the corner 5 in this manner, it is possible to delay the occurrence of delamination and reduce the speed of progression of delamination even with a small amount of high toughness fiber reinforced composite material 21. As a result, it is possible to suppress the occurrence of buckling of the frame 1 and improve the bending strength of the frame 1 while further reducing the manufacturing cost of the frame 1.
[0091] Example 3 Taking the above embodiment and Examples 1 and 2 into consideration, the optimal arrangement of the high toughness fiber reinforced composite material 21 in the frame can be classified as shown in the table of FIG.
[0092] In the table of FIG. 13, first, the row (horizontal line) of "material arrangement in cross section" shows three cross-sectional structures in which the high toughness fiber reinforced composite material 21 is arranged in the cross section, that is, the high toughness fiber reinforced composite material 21 is arranged over at least the entire cross section of the corner portion 5. Specifically, as a first cross-sectional structure, a frame 101 in which the compression surface portion 2, a pair of corner portions 5, and a pair of side portions 3 are integrally formed with the high toughness fiber reinforced composite material 21 is shown as a material arrangement in the cross section when bending strength is given the highest priority. As a second cross-sectional structure, a frame 102 in which the pair of corner portions 5 and a pair of side portions 3 are integrally formed with the high toughness fiber reinforced composite material 21 is shown as a material arrangement in the cross section when bending strength and the amount of high toughness material input are balanced. As a third cross-sectional structure, a frame 103 in which only the pair of corner portions 5 are integrally formed with the high toughness fiber reinforced composite material 21 is shown as a material arrangement in the cross section when the amount of high toughness material input is minimized.
[0093] Also, in the row of "Lamination structure" in the table of FIG. 13, three cross-sectional structures are shown in which the high toughness fiber reinforced composite material 21 is laminated, that is, the high toughness fiber reinforced composite material 21 is arranged at least at the center side in the thickness direction of the corner portion 5, and the low toughness fiber reinforced composite material 22 is arranged on the surface layer side of the corner portion 5. Specifically, as a first cross-sectional structure, a frame 201 in which the high toughness fiber reinforced composite material 21 is arranged at the center side in the thickness direction of the compression surface portion 2, the pair of corner portions 5, and the pair of side portions 3 is shown as a laminate structure in which bending strength is given the highest priority. As a second cross-sectional structure, a frame 202 in which the high toughness fiber reinforced composite material 21 is arranged at the center side in the thickness direction of the pair of corner portions 5 and the pair of side portions 3 is shown as a laminate structure in which bending strength and the amount of high toughness material input are balanced. As a third cross-sectional structure, a frame 203 in which the high toughness fiber reinforced composite material 21 is arranged only at the center side in the thickness direction of the pair of corner portions 5 is shown as a laminate structure in which the amount of high toughness material input is minimized.
[0094] Here, in a configuration in which the high toughness fiber reinforced composite 21 is arranged at the center of the thickness direction of the corner 5, as in the frames 202, 203 in Figure 6, when a bending load is input to these frames 202, 203, interlayer delamination tends to occur easily at the interface between the high toughness fiber reinforced composite 21 and the low toughness fiber reinforced composite 22, which has lower toughness.
[0095] Therefore, in order to suppress such delamination, it is preferable that the ends 21a, 21b on the compression surface 2 side and / or the side surface portion 3 side of the high-toughness fiber-reinforced composite material 21 have a tapered shape in which the thickness of the ends 21a, 21b gradually changes, as shown in Figures 14 to 15.
[0096] Specifically, as shown in Figures 14 and 15, the end 21a on the compression surface portion 2 side of the high toughness fiber reinforced composite material 21 may have a tapered convex portion. Also, as shown in Figure 15, the end 21b on the side of the side surface portion 3 of the high toughness fiber reinforced composite material 21 may have a tapered concave portion (reverse tapered portion).
[0097] The method of forming the tapered end 21a and the inverse tapered end 21b composed of the high toughness fiber reinforced composite 21 is not particularly limited in the present invention, but for example, it is possible to form the tapered end 21a and the inverse tapered end 21b by arranging the fiber orientation layers (resin layers) 11-14 (see Figure 3) that respectively constitute the high toughness fiber reinforced composite 21 and the adjacent low toughness fiber reinforced composite 22 in a shifted direction along a surface such as the compression surface portion 2.
[0098] 14 and 15, the ends 21a, 21b of the high toughness fiber reinforced composite material 21 on the compression surface portion 2 side and / or the side surface portion 3 side have a tapered shape in which the thickness of the ends 21a, 21b gradually changes, making it possible to alleviate a sudden change in toughness near the ends 21a, 21b of the high toughness fiber reinforced composite material 21. This makes it possible to alleviate stress concentration near the ends 21a, 21b and suppress delamination. As a result, it is possible to further suppress buckling of the frame 1 and further improve the bending strength of the frame 1. [Explanation of symbols]
[0099] 1 Fiber-reinforced composite frame 2 Compression surface 3 Side part 4 Tensile surface 5 Corner 5b R stop part 11 Longitudinal orientation layer (resin layer) 12 Short-side orientation layer (resin layer) 13 +45 degree orientation layer (resin layer) 14 -45 degree orientation layer (resin layer) 11a~14a Reinforced Fiber 21 High toughness fiber reinforced composite material 22 Low toughness fiber reinforced composites 120 Center pillar 121 Body 122 Bumper beam 123 Side sill 124 Hinge pillar 125 Front pillar 126 Cross member
Claims
1. A fiber-reinforced composite frame is manufactured from a fiber-reinforced composite material having a plurality of resin layers laminated thereon, the fiber-reinforced composite frame being extended in a predetermined direction so as to form a closed cross section having a plurality of corners, The frame is a compression surface portion in which a compressive stress is generated along a short side direction perpendicular to a long side direction of the frame when a bending load that bends the frame in the short side direction perpendicular to the long side direction of the frame is input to the frame; a side surface portion extending in the short direction from the corner portion adjacent to the compression surface portion; a tension surface portion extending in the longitudinal direction at a position spaced apart from the compression surface portion, and in which a tensile stress is generated along the longitudinal direction when the bending load is input to the frame; Equipped with The corner region adjacent to the compression surface portion is provided with a high-toughness fiber-reinforced composite material having a higher toughness value in a shear direction between resin layers than the fiber-reinforced composite material constituting the tensile surface portion region. A fiber-reinforced composite frame.
2. 2. The fiber-reinforced composite frame according to claim 1, A portion of the corner region that is flush with the side surface portion is formed of the high toughness fiber reinforced composite material. A fiber-reinforced composite frame.
3. A fiber-reinforced composite frame is manufactured from a fiber-reinforced composite material having a plurality of resin layers laminated thereon, the fiber-reinforced composite frame being extended in a predetermined direction so as to form a closed cross section having a plurality of corners, The frame is a compression surface portion in which a compressive stress is generated along a short side direction perpendicular to a long side direction of the frame when a bending load that bends the frame in the short side direction perpendicular to the long side direction of the frame is input to the frame; a side surface portion extending in the short direction from the corner portion adjacent to the compression surface portion; a tension surface portion extending in the longitudinal direction at a position spaced apart from the compression surface portion, and in which a tensile stress is generated along the longitudinal direction when the bending load is input to the frame; Equipped with The side surface portion includes a high-toughness fiber-reinforced composite material having a higher toughness value in a shear direction between resin layers than the fiber-reinforced composite material constituting the region of the tensile surface portion. A fiber-reinforced composite frame.
4. 3. The fiber-reinforced composite frame according to claim 1, The side surface region is provided with the high toughness fiber reinforced composite material. A fiber-reinforced composite frame.
5. The fiber-reinforced composite frame according to any one of claims 1 to 4, The region of the compression surface portion is composed of a low-toughness fiber-reinforced composite material having a lower toughness value in a shear direction between resin layers than the high-toughness fiber-reinforced composite material. A fiber-reinforced composite frame.
6. The fiber-reinforced composite frame according to any one of claims 1 to 5, The high toughness fiber reinforced composite material is disposed on a center side in a thickness direction of the corner portion. A fiber-reinforced composite frame.
7. A fiber-reinforced composite frame according to claim 1, 2 or 4, The end portion of the high toughness fiber reinforced composite material on the compression surface portion side and / or the side surface portion side has a tapered shape in which the thickness of the end portion gradually changes. A fiber-reinforced composite frame.
8. The fiber-reinforced composite frame according to any one of claims 1 to 7, The frame is applied to at least one selected from the group consisting of a center pillar, a bumper beam, a side sill, a hinge pillar, a front pillar, and a cross member that constitute a body of a vehicle. A fiber-reinforced composite frame.
Citation Information
Patent Citations
Structure component for use in e.g. motor car, has channel broken by force applied by carriage in longitudinal direction of channel, where carriage is displaceable in direction of force application and force is larger than expansive force
DE102012014375A1
Board-shaped body and production thereof
JP1997254295A
Shock absorbing member
JP2006200702A
Fiber-reinforced composite material and method of producing fiber-reinforced composite material
JP2014004735A
Vehicle body structure of vehicle
JP2015193362A