Sputtering target and method for manufacturing sputtering target

The sputtering target with an Al-Cu-Mg alloy layer addresses bonding issues by enhancing adhesion, ensuring structural stability during thermal cycles.

JP7551893B2Active Publication Date: 2024-09-17JX NIPPON MINING & METALS CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023501674
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-11
Filing Date
2022-06-10
Publication Date
2024-09-17
Estimated Expiration
2042-06-10

AI Technical Summary

Technical Problem

The challenge in sputtering targets is the insufficient bonding strength between constituent members due to thermal expansion and contraction, leading to potential peeling at the bonding interface.

Method used

A sputtering target with an alloy layer containing Al, Cu, and a Mg-containing layer with at least 5.0% Mg is used to firmly join the first and second components, enhancing bonding strength through diffusion bonding.

Benefits of technology

The alloy layer with a Mg-containing layer effectively prevents peeling by ensuring strong adhesion between the components, maintaining structural integrity during sputtering processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551893000006
    Figure 0007551893000006
  • Figure 0007551893000007
    Figure 0007551893000007
  • Figure 0007551893000005
    Figure 0007551893000005
Patent Text Reader

Abstract

This sputtering target is formed from multiple structural members including a target and a substrate. The multiple structural members include a first structural member and a second structural member that are layered together. The first structural member contains Al and the second structural member contains Cu. At least one of the first structural member and the second structural member contains Mg. The sputtering target contains Al and Cu between the first structural member and the second structural member and has an alloy layer contacting the first structural member and the second structural member. At least a portion of the alloy layer further includes an Mg-containing layer in which Mg content is 5.0 at% or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This specification discloses techniques relating to sputtering targets and methods for producing sputtering targets. [Background technology]

[0002] In recent years, with the rapid progress of semiconductor-related technologies, there is a tendency for semiconductors to be highly integrated and for electronic devices equipped with semiconductor chips to be miniaturized. Under such circumstances, in the manufacture of electronic devices, a large number of thin films are formed by sputtering using various sputtering targets. Such thin films include, for example, titanium or titanium alloy films, titanium silicide films, titanium nitride films, and the like, and in sputtering, sputtering targets equipped with target materials made of materials such as titanium that correspond to the material of the thin films are used.

[0003] The formation of a thin film by sputtering is carried out, for example, as follows. First, in a vacuum, a high voltage is applied between the substrate and the sputtering target while introducing an inert gas such as Ar gas. Then, ionized Ar + Ions such as these are collided with the target material of the sputtering target. The collision energy causes atoms in the target material to be released and deposited on the substrate. This forms a thin film on the substrate. Sputtering targets come in various shapes, such as flat plate and cylindrical, but generally include a target material and a substrate that is superimposed and bonded to the target material.

[0004] Among these types of techniques, those related to target materials mainly containing titanium are described in, for example, Patent Documents 1 to 5. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] WO 01 / 38598 [Patent Document 2] U.S. Patent No. 6,755,948 [Patent Document 3] Special Publication No. 2001-509548 [Patent Document 4] U.S. Pat. No. 5,993,621 [Patent Document 5] JP 2010-235998 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in a sputtering target composed of multiple components including a target material and a substrate, the first and second components stacked on top of each other may not be bonded firmly enough. In this case, warping due to thermal expansion during sputtering and contraction during cooling may cause peeling at the bonded interface, which may affect the sputtering process.

[0007] This specification discloses a sputtering target capable of firmly bonding a first component member and a second component member stacked on top of each other in the sputtering target, and a method for manufacturing the sputtering target. [Means for solving the problem]

[0008] The sputtering target disclosed in this specification is a sputtering target composed of multiple components including a target material and a substrate, the multiple components including a first component and a second component stacked on top of each other, the first component containing Al and the second component containing Cu, and at least one of the first component and the second component containing Mg, the sputtering target has an alloy layer between the first component and the second component containing Al and Cu and in contact with the first component and the second component, and the alloy layer further includes a Mg-containing layer containing 5.0 at% or more Mg in at least a portion of the alloy layer.

[0009] Furthermore, the method for manufacturing a sputtering target disclosed in this specification is a method for manufacturing a sputtering target composed of multiple components including a target material and a substrate, the multiple components including a first component and a second component stacked on top of each other, the first component containing Al and the second component containing Cu, and at least one of the first component and the second component containing Mg, the method including a preparation step of preparing the multiple components including the first component and the second component, and a joining step of pressing and joining the multiple components including the first component and the second component in a stacked state. Effect of the Invention

[0010] According to the above-described sputtering target and method for producing a sputtering target, the first component member and the second component member stacked on each other in the sputtering target can be firmly bonded to each other. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a plan view of a sputtering target showing the positions at which samples were taken when measuring the bonding strength between an insert material and a substrate. [Diagram 2]1 is an SEM image of a cross section in the thickness direction of the sputtering target of Example 1. [Diagram 3] 1 is an SEM image of a cross section in the thickness direction of the sputtering target of Example 2. [Figure 4] 1 is an SEM image of a cross section in the thickness direction of the sputtering target of Comparative Example 1. [Diagram 5] 1 is an SEM image of a cross section in the thickness direction of the sputtering target of Comparative Example 2. [Figure 6] 1 shows an SEM image showing the scan range by EDX LineScan for a cross section in the thickness direction of the sputtering target of Example 1, and a graph showing the variation in the content of each element. [Figure 7] 1 is an SEM image showing the scan range by LineScan of EDX for a cross section in the thickness direction of the sputtering target of Example 2, and a graph showing the variation in the content of each element. [Figure 8] 1 shows an SEM image showing the scan range by LineScan of EDX for a cross section in the thickness direction of the sputtering target of Example 3, and a graph showing the variation in the content of each element. [Figure 9] 1 shows an SEM image showing the scan range by LineScan of EDX for a cross section in the thickness direction of the sputtering target of Comparative Example 1, and a graph showing the fluctuation in the content of each element. [Figure 10] 1 is an SEM image showing the scan range by LineScan of EDX for a cross section in the thickness direction of the sputtering target of Comparative Example 2, and a graph showing the fluctuation in the content of each element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the above-mentioned sputtering target and method for producing the sputtering target will be described in detail. The sputtering target of one embodiment is composed of a plurality of components including a target material and a substrate. The plurality of components include a first component and a second component stacked on each other, the first component containing Al, the second component containing Cu, and at least one of the first component and the second component containing Mg. The sputtering target has an alloy layer between the first component and the second component containing Al and Cu and in contact with the first component and the second component. The alloy layer further includes a Mg-containing layer containing 5.0 at% or more of Mg in at least a part of the alloy layer. In the following, for convenience of explanation, one of the components of the sputtering target stacked on each other and containing Al is referred to as the first component, and the other component containing Cu is referred to as the second component.

[0013] In a sputtering target in which a target material and a substrate are laminated, either the target material or the substrate may be a first component containing Al, and the other may be a second component containing Cu. In a sputtering target in which a target material, an insert material, and a substrate are laminated in this order, the target material may be a first component containing Al and the insert material may be a second component containing Cu, or the insert material may be a first component containing Al and the substrate may be a second component containing Cu.

[0014] It was found that the bonding strength of such a first component containing Al and a second component containing Cu would be low if they were directly laminated and bonded together. This is believed to be because Cu and Al form brittle intermetallic compounds (CuAl, CuAl2, etc.) due to mutual diffusion at the interface between the first and second components. If the bonding strength between the first and second components is low, there is a risk that the first and second components will peel off at the bonding interface due to thermal expansion during sputtering and contraction during cooling.

[0015] In contrast, in this embodiment, an alloy layer containing Al and Cu between the first and second components is provided, and the alloy layer includes an Mg-containing layer containing 5.0 at% or more of Mg in addition to Al and Cu in at least a part of the alloy layer. This allows the first and second components to be firmly joined. It is presumed that the Mg-containing layer in at least a part of the alloy layer thus contains Mg in addition to Cu and Al, suppressing the formation of an intermetallic compound between Cu and Al, and forming a stronger Al, Cu, and Mg alloy. However, the present invention is not limited to such a theory, and it is sufficient that at least a part of the alloy layer containing Al and Cu between the first and second components contains an Mg-containing layer containing Al, Cu, and Mg and having a portion with a Mg content of 5.0 at% or more.

[0016] Here, we will mainly explain in detail an example of a sputtering target in which a target material, an insert material, and a substrate are laminated in this order, in which the first component is the insert material and the second component is the substrate, or an example in which the first component is the substrate and the second component is the insert material. Although detailed explanation is omitted, either one of the first component and the second component may be the target material and the other may be the insert material. Furthermore, sputtering targets that do not include an insert material may also be targeted. For example, it is possible to use the first component as the target material and the second component as the substrate, or to use the first component as the substrate and the second component as the target material.

[0017] (Target material) The target material has a sputtering surface to be used for sputtering, and generally has a shape such as a disk or other flat plate, or a cylindrical shape. The material of the target material is appropriately determined according to the material of the thin film to be formed on the substrate by sputtering. If the insert material contains Al, the target material may be a material that can be bonded to the insert material containing Al, such as Ti, Ta, Cu, Cu alloy, W, WSi, Co, Al, etc.

[0018] Among them, the target material typically contains Ti. In this case, the target material can be made of pure Ti that mainly contains Ti. The target material made of pure Ti typically has a Ti content of 99.995% by mass or more, but may also have a Ti content of 99.999% by mass or more, or even 99.9995% by mass or more. The target material made of pure Ti may contain at least one impurity selected from the group consisting of Al, Fe, Ni, and Cu.

[0019] Alternatively, the target material may be made of a Ti alloy containing Ti and Al. In the case of such a target material made of a Ti alloy, the Al content is, for example, 30 at% to 70 at%, and as an example, may be about 50 at%.

[0020] (base material) The substrate has a shape such as a flat plate or a cylindrical shape corresponding to the target material, and is disposed on the back side of the target material opposite to the sputtering surface, and may also be called a backing plate or a backing tube. In this embodiment, the substrate is disposed with an insert material (to be described later) sandwiched between the substrate and the target material. In other words, the sputtering target of this embodiment is a laminate of the target material, the insert material, and the substrate in this order.

[0021] When the insert material described later is a first component containing Al, the substrate is a second component containing Cu. Alternatively, when the insert material is a second component containing Cu, the substrate is a first component containing Al. Typically, the insert material is a first component containing Al, and the substrate is a second component containing Cu.

[0022] More specifically, when the substrate is the second component, it may be made of pure Cu containing mainly Cu, or when the substrate is the first component, it may be made of pure Al containing mainly Al.

[0023] Alternatively, when the substrate is the second component, it can be made of a Cu alloy containing Cu and Mg. Alternatively, when the substrate is the first component, it can be made of an Al alloy containing Al and Mg. The Al alloy may contain Si, Mn, Cr, Zn, etc. in addition to Mg. In a specific embodiment, the substrate does not contain Mg, and the insert material further contains Mg. However, both the substrate and the insert material may contain Mg.

[0024] In particular, the substrate is preferably made of a Cu alloy or an Al alloy containing Mg. In this case, the Mg content in the substrate is preferably 1.0 mass% to 10.0 mass%, more preferably 3.4 mass% or more. If the Mg content in the substrate is too low, it is difficult to form an alloy layer including a Mg-containing layer containing Al, Cu, and Mg between the substrate and the insert material, and there is a concern that the required bonding strength between the substrate and the insert material is not ensured. If the Mg content in the substrate is too high, there is a possibility that the properties inherently required for the substrate containing Mg are impaired.

[0025] (insert material) An insert material may be interposed between the target material and the substrate. The insert material may be provided for the purpose of performing intermetallic diffusion bonding to improve the bonding strength between the target material and the substrate. The insert material also has functions such as mitigating warping of the sputtering target and absorbing distortion during sputtering.

[0026] As mentioned above, when the substrate is the second component and contains Cu, the insert material is the first component and contains Al, and when the substrate is the first component and contains Al, the insert material is the second component and contains Cu.

[0027] More specifically, when the insert material is the first component, it may be made of pure Al containing mainly Al, or when the insert material is the second component, it may be made of pure Cu containing mainly Cu.

[0028] Alternatively, when the insert material is the first component, it may be made of an Al alloy containing Al and Mg. The Al alloy may contain Si, Mn, Cr, Zn, etc. in addition to Mg. Alternatively, when the insert material is the second component, it may be made of a Cu alloy containing Cu and Mg.

[0029] In particular, the insert material is preferably made of an Al alloy or Cu alloy containing Mg. In this case, the Mg content in the insert material is preferably 1.0 mass% to 10.0 mass%, more preferably 3.4 mass% or more. If the Mg content in the insert material is too low, it is difficult to form an alloy layer including a Mg-containing layer containing Al, Cu and Mg between the insert material and the substrate, and there is a concern that the required bonding strength between the substrate and the insert material is not ensured. If the Mg content in the insert material is too high, there is a possibility that the properties inherently required of the insert material containing Mg are impaired.

[0030] (alloy layer) Between the first component such as an insert material and the second component such as a substrate, there is an alloy layer containing at least Al and Cu, and at least a part of the alloy layer includes a Mg-containing layer containing the three elements Al, Cu, and Mg. The Mg-containing layer contains 5.0 at% or more of Mg. This Mg-containing layer firmly bonds the first component and the second component. The alloy layer may include a layer that does not contain Mg but contains Al and Cu in addition to the Mg-containing layer. Even if there is a layer that does not contain Mg in the alloy layer, if there is an Mg-containing layer, a strong alloy of the three elements is formed there, and the bonding strength between the first component and the second component can be improved. However, if there is a part that contains both Al and Cu, there is a possibility that an intermetallic compound of Al and Cu is formed in that part, so it is preferable that the Mg-containing layer is formed in a relatively wide range in the alloy layer.

[0031] By performing SEM-EDX (energy dispersive X-ray analysis) on a cross section in the thickness direction perpendicular to the sputtering surface of the target material of the sputtering target, the alloy layer and the Mg-containing layer can be confirmed and the contents of each of the three elements can be measured.

[0032] The alloy layer means a portion between the first component and the second component where the content of each of Al and Cu is 5.0 at% or more in element ratio on the line when SEM-EDX line scan is performed on a cross section along the thickness direction of the sputtering target. The alloy layer is between the position on the first component side where both Al and Cu are 5.0 at% or more and the position on the second component side where both Al and Cu are 5.0 at% or more. When the content of Al or Cu is confirmed from the alloy layer toward the first component or the second component near the boundary between the alloy layer and the first component or the second component, if the content of Al or Cu does not decrease to less than 5.0 at%, the position where the content converges to a constant value is taken as the boundary between the alloy layer and the first component or the second component.

[0033] The Mg-containing layer is a portion of the above-mentioned alloy layer that contains the three elements Al, Cu, and Mg, and has a Mg content of 5.0 at% or more. The presence or absence of the Mg-containing layer can also be confirmed by performing a LineScan of SEM-EDX along the thickness direction of a cross section of the sputtering target along the thickness direction. Even if there is a portion in the alloy layer that contains the three elements Al, Cu, and Mg, if the Mg content is less than 5.0 at% in any portion of the portion, the portion is not considered to be a Mg-containing layer. The conditions for LineScan of SEM-EDX are a magnification of 1000 to 2000 times, a distance between the objective lens and the sample (WD, Working distance): 10 mm, and a scan distance: 30 μm to 50 μm.

[0034] The thickness of the alloy layer is preferably 5 μm to 20 μm, more preferably 10 μm to 15 μm. If the thickness of the alloy layer is too thin, the effect of improving the bonding strength by the Mg-containing layer is not sufficiently obtained, and there is a concern that the bonding strength will decrease. On the other hand, if the thickness of the alloy layer is too thick, the bonding strength by the intermetallic compound layer of Cu and Al will be dominant, and the bonding strength may decrease. The above-mentioned thickness of the alloy layer means the distance in the thickness direction between the position where the content of both Al and Cu is 5.0 at% or more on the first component side and the position where the content of both Al and Cu is 5.0 at% or more on the second component side when a line scan of SEM-EDX is performed on a cross section along the thickness direction passing through the center in the radial direction of the sputtering target.

[0035] When a line scan of an SEM-EDX is performed along the thickness direction of the sputtering target, the thickness of the Mg-containing layer is preferably 20% or more of the thickness of the alloy layer, which can greatly improve the bonding strength.

[0036] The Mg-containing layer is preferably formed over a relatively large area between the first and second components. When observing a cross section along the thickness direction passing through the center of the plan view of the sputtering target (when the sputtering target is a disk type, the plan view of the sputtering target from the sputtering surface side is circular, so the center in the radial direction of the circle), the Mg-containing layer is preferably formed at a ratio of 50% or more of the entire width of the first and second components along a direction perpendicular to the thickness direction of the cross section. The width of the first and second components here means the length along the direction perpendicular to the thickness direction of the region where the first and second components overlap in the cross section along the thickness direction. When the Mg-containing layer is present at such a relatively large ratio in the direction perpendicular to the thickness direction, further improvement in the bonding strength can be realized. There may be a part where the Mg-containing layer does not exist in a part of the region where the first and second components overlap.

[0037] The alloy layer and the Mg-containing layer are preferably formed by diffusion bonding between the first and second components. In such a case, the Al content of the alloy layer may be lower in the portion in contact with the second component than in the portion in contact with the first component. Also, the Cu content of the alloy layer may be lower in the portion in contact with the first component than in the portion in contact with the second component.

[0038] (Joining strength) The bond strength between the insert material (first component) and the base material (second component) is 5kgf / mm 2 More than 10kgf / mm 2 If the bonding strength between the insert material and the substrate is too low, there is a concern that the insert material will expand thermally during sputtering and shrink during cooling, resulting in peeling at the bonding interface via the alloy layer. There is no particular problem with a bonding strength that is too high, but it is preferable that the bonding strength is less than 15 kgf / mm. 2 The following may occur:

[0039] The bonding strength between the insert material and the substrate is measured as follows. First, samples including the target material, the insert material, and the substrate are taken in the thickness direction from a sputtering target having the target material, the insert material, and the substrate. In a sputtering target 1 having a circular shape in plan view as shown in Fig. 1, a total of seven sample taking points Ps are taken: one point at the center in plan view, three points at equal intervals in the circumferential direction on the outer periphery, and three points at the center in the radial direction between the central point and the point on the outer periphery. Then, each sample is subjected to a uniaxial tensile test along the thickness direction using a tensile tester. The strength at which the part of the sample corresponding to the insert material and the part corresponding to the substrate peel off is measured. The average value of the strengths for each sample is taken as the bonding strength.

[0040] (Manufacturing method) The above-mentioned sputtering target can be manufactured, for example, as described below.

[0041] First, in a preparation step, a plurality of components including a first component and a second component are prepared. The first component contains Al, the second component contains Cu, and at least one of the first component and the second component is made of an alloy containing Mg.

[0042] When manufacturing a sputtering target in which a target material, an insert material, and a substrate are laminated in this order, the above-mentioned target material, insert material, and substrate are each prepared. In this embodiment, either the insert material or the substrate is the above-mentioned first component member, and the other is the above-mentioned second component member.

[0043] As described above, typically, the insert material is a first component containing Al, and the substrate is a second component containing Cu. Typically, the substrate does not contain Mg, and the insert material further contains Mg. In a specific embodiment, the insert material is an Al alloy containing Mg. The target material may contain, for example, Ti.

[0044] Then, a bonding process is performed in which a plurality of components including the first component and the second component are laminated and pressed to bond them. In this embodiment, the target material, the insert material, and the base material are laminated in this order, and in this laminated state, they are pressed in the thickness direction to bond them. At this time, as described above, Mg diffuses from the first component and / or the second component containing Mg to the interface between the first component and the second component, and Al and Cu contained in the first component and the second component also diffuse at the interface. As a result, an alloy layer containing at least Al and Cu is formed at the interface between the insert material and the base material, and an Mg-containing layer containing 5.0 at% or more of Mg is further formed in the alloy layer. Since the Mg-containing layer containing the three elements Al, Cu, and Mg in the alloy layer has high strength, the first component and the second component are firmly bonded by the formation of the Mg-containing layer at the interface between the first component and the second component. Here, the insert material, which is either the first component member or the second component member, and the base material, which is the other, are firmly joined together.

[0045] The bonding process can be carried out by various methods such as hot isostatic pressing (HIP), hot pressing, cold isostatic pressing (CIP), and others. Among these, hot isostatic pressing is preferred because it applies isostatic pressure (hydrostatic pressure) while heating at a relatively high temperature, making it easier to effectively diffuse bond the entire interface.

[0046] After the bonding step, a sputtering target is obtained in which the target material, the insert material, and the substrate are laminated in this order. Since the alloy layer including the Mg-containing layer containing Al, Cu, and Mg is formed at least partially between the insert material and the substrate, the insert material and the substrate are bonded with a required strength. EXAMPLES

[0047] Next, a sputtering target as described above was prototyped and its effects were confirmed, which will be described below. However, the description here is merely for illustrative purposes and is not intended to be limiting.

[0048] A target material, an insert material, and a substrate, all made of pure Ti, were prepared. In Example 1, a Cu-Ni-Si alloy containing 1.8-3.0 mass% Ni, 0.4-0.8 mass% Si, and Cu as the balance was prepared as the base material, and an Mg-based Al alloy containing about 4.0-4.9 mass% Mg, about 0.05-0.25 mass% Cr, about 0.4-1.0 mass% Mn, and Al as the balance was prepared as the insert material. Then, the target material, the insert material, and the base material were laminated in this order, and hot isostatic pressing (HIP) was performed. In this way, a sputtering target was manufactured.

[0049] In Example 2, a sputtering target was manufactured in the same manner as in Example 1, except that the insert material used was an Mg-based Al alloy containing approximately 2.2 to 2.8 mass% Mg, 0.15 to 0.35 mass% Cr, and the remainder Al.

[0050] In Example 3, a sputtering target was produced in the same manner as in Example 1, except that the HIP temperature and time were increased.

[0051] In Comparative Example 1, a sputtering target was produced in the same manner as in Example 1, except that an insert material made of pure Al, mainly consisting of Al, was used.

[0052] In Comparative Example 2, a sputtering target was manufactured in the same manner as in Example 1, except that the insert material used was a Cu-based Al alloy containing approximately 3.5 to 4.5 mass% Cu, approximately 0.4 to 0.8 mass% Mg, approximately 0.2 to 0.8 mass% Si, 0.4 to 0.8 mass% Mn, and the remainder being Al.

[0053] A cross section in the thickness direction of each of the sputtering targets of Examples 1 and 2 and Comparative Examples 1 and 2 was observed by SEM-EDX. The images are shown in Figures 2 to 5. From Figures 2 and 3, it is considered that an alloy layer containing Al and Cu is formed at the interface between the target material and the substrate.

[0054] Furthermore, a LineScan was performed by EDX on the cross section in the thickness direction of each of the sputtering targets of Examples 1 to 3 and Comparative Examples 1 and 2. This LineScan was performed on a sample taken from a position of 1 / 2R (a position half the radius R, the center position of the radius) on the cross section along the thickness direction passing through the radial center of the sputtering target. The results are shown in Figures 6 to 10. In the graphs shown in Figures 6 to 10, the horizontal axis represents the number of measurement points and the vertical axis represents the element ratio (at%).

[0055] From Figs. 6 to 8, it can be seen that in the sputtering targets of Examples 1 to 3, the alloy layer contains Al, Cu, and Mg, and at least a part of the Mg-containing layer has a Mg content of 5.0 at% or more. In Example 1 shown in Fig. 6, the thickness of the alloy layer was about 10 µm, and the thickness of the Mg-containing layer was about 4 µm. In Example 2 shown in Fig. 7, the thickness of the alloy layer was about 7.63 µm, and the thickness of the Mg-containing layer was about 1.55 µm. In Example 3, the thickness of the alloy layer was about 15 µm, and the thickness of the Mg-containing layer was about 7 µm. In all of Examples 1 to 3, the thickness of the Mg-containing layer was 20% or more of the thickness of the alloy layer. In Example 2 (Fig. 7), the Al content in the alloy layer on the substrate side did not decrease to less than 5.0 at%, but the Al content converged to a constant value (about 10 at%), and the position where the convergence begins is recognized as the boundary position between the alloy layer and the substrate.

[0056] In contrast, in the sputtering targets of Comparative Examples 1 and 2, as shown in FIGS. 9 and 10, even though Mg is contained in the alloy layer, the Mg content is less than 5.0 at %, which means that no Mg-containing layer is present.

[0057] In addition, for each of the sputtering targets of the above-mentioned Examples 1 to 3 and Comparative Examples 1 and 2, the bonding strength was measured using a tensile testing device (precision universal testing machine (autograph) AG-100kNX plus manufactured by Shimadzu Corporation) based on the above-mentioned method. The results are shown in Table 1.

[0058] [Table 1]

[0059] From the test results of the bonding strength shown in Table 1, it can be seen that high bonding strength was exhibited between the insert material and the substrate in the sputtering targets of Examples 1 to 3. On the other hand, the bonding strength was lower in the sputtering targets of Comparative Examples 1 and 2 than in the sputtering targets of Examples 1 to 3. Moreover, when Examples 1 to 3 are compared, it is understood that the joint strength increases by increasing the Mg content of the insert material.

[0060] From the above, it has been found that the first component and the second component can be firmly joined by forming an Mg-containing layer containing Al, Cu and Mg and containing 5.0 at% or more of Mg in at least a part of the alloy layer between the first component, such as an insert material or a substrate, and the second component. [Explanation of symbols]

[0061] 1. Sputtering target Ps Sample collection location

Claims

1. A sputtering target composed of a plurality of components including a target material and a substrate, The plurality of components include a first component and a second component stacked on each other, the first component contains Al and the second component contains Cu; At least one of the first component and the second component contains Mg, the sputtering target has an alloy layer between the first component and the second component, the alloy layer containing Al and Cu and in contact with the first component and the second component; The sputtering target includes an Mg-containing layer, at least a portion of the alloy layer further containing 5.0 at % or more of Mg.

2. The sputtering target further includes an insert material, and the target material, the insert material, and the base material are laminated in this order; 2. The sputtering target according to claim 1, wherein the first component member is one of the insert material and the substrate, and the second component member is the other of the insert material and the substrate.

3. The sputtering target according to claim 2 , wherein the first component member is the insert material, and the second component member is the substrate.

4. The bonding strength between the first component and the second component is 5 kgf / mm 2 The sputtering target according to any one of claims 1 to 3.

5. The sputtering target according to any one of claims 1 to 3, wherein the target material contains Ti.

6. The sputtering target according to any one of claims 1 to 3, wherein the alloy layer and the Mg-containing layer are formed by diffusion bonding a first component member and a second component member.

7. 4. The sputtering target according to claim 1, wherein the Al content in the alloy layer is lower in a portion in contact with the second component than in a portion in contact with the first component.

8. 4. The sputtering target according to claim 1, wherein the alloy layer has a lower Cu content in a portion in contact with the first component member than in a portion in contact with the second component member.

9. The sputtering target according to any one of claims 1 to 3, wherein when a line scan of an SEM-EDX is performed along a thickness direction of the sputtering target, a thickness of the Mg-containing layer is 20% or more of a thickness of the alloy layer.

10. The sputtering target according to any one of claims 1 to 3, wherein, when a cross section passing through a center of the sputtering target in a plan view and along a thickness direction is observed, the Mg-containing layer is formed along a direction perpendicular to the thickness direction at a ratio of 50% or more of an entire width of the first component and the second component.

11. A method for producing the sputtering target according to any one of claims 1 to 3, comprising the steps of: a preparation step of preparing the plurality of components including the first component and the second component; a joining step of pressing and joining a plurality of components including the first component and the second component in a stacked state; A method for producing a sputtering target, comprising:

12. The method for producing a sputtering target according to claim 11, wherein the bonding step is performed by hot isostatic pressing.

13. The sputtering target further includes an insert material, and the target material, the insert material, and the base material are laminated in this order; 12. The method for manufacturing a sputtering target according to claim 11, wherein in the preparation step, a target material, an insert material, and a substrate are prepared, the first component member being one of the insert material and the substrate, and the second component member being the other of the insert material and the substrate.

14. The method for producing a sputtering target according to claim 13 , wherein the first component member prepared in the preparation step is the insert material, and the second component member is the substrate.

15. The method for producing a sputtering target according to claim 11 , wherein the target material contains Ti.

16. The method for producing a sputtering target according to claim 11 , wherein in the joining step, the first component member and the second component member are joined by diffusion bonding.

Citation Information

Patent Citations

  • Diffusion bonded sputtering target assembled body and its production

    JP1994172993A

  • Insert material for joining ti-al series intermetallic compound and ti base alloy and joining method therefor and joined body

    JP1999077365A

  • Backing plate for sputtering target and sputtering target / backing plate assembly

    JP1999236665A

  • Titanium sputtering target and manufacturing method thereof

    JP2001509548A

  • Diffusedly joined target assemblage of high purity cobalt target with backing plate made of copper alloy, and its production method

    JP2002105635A