Resin composition for active energy ray-curable adhesive and adhesive sheet
Patent Information
- Application Number
- JP2019189238
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-10-16
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-10-16
AI Technical Summary
【0008】 本発明により、比較的低分子量で糊残りの無い良好な粘着性を持つ活性エネルギー線硬化性粘着剤用樹脂組成物を得ることができる。
Smart Images

Figure 0007552009000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition for pressure-sensitive adhesive which is cured by active energy rays to form a film, and to a pressure-sensitive adhesive sheet. [Background technology]
[0002] Active energy ray curing technology has advantages such as energy saving, space saving, short-time curing, etc., and its scope of use has expanded in recent years. In particular, solvent-free active energy ray curable resin compositions containing polymerizable monomers have attracted attention. Solvent-free active energy ray curable resin compositions are composed of polymerizable oligomers, polymerizable monomers, polymerization initiators (not required for electron beam curing), other additives, etc.
[0003] As the polymerizable oligomer, unsaturated polyester, urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, etc. are used, and among them, urethane (meth)acrylate resin is often used in woodwork coating because it is fast curing and has a large degree of freedom in resin design. For example, a curable resin composition containing urethane (meth)acrylate resin is disclosed in Patent Document 1 and Patent Document 2. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2000-281935 A [Patent Document 2] JP 2001-2744 A Summary of the Invention [Problem to be solved by the invention]
[0005] For pressure-sensitive adhesives, which have so far been mainly thermosetting or two-component curing, active energy ray curing has been actively investigated for the purpose of saving energy and shortening the process. However, unlike urethanes, which react linearly with functional groups in a one-to-one relationship, radical polymerization-based active energy ray-curable resins form films through three-dimensional crosslinking by acryloyl groups, which means that the coating film tends to harden and is disadvantageous in terms of flexibility required for mitigating external stress in adhesives. This can be solved by increasing the molecular weight of the resin and decreasing the concentration of acryloyl groups, but on the other hand, the viscosity increases with increasing molecular weight, and deterioration of handleability is unavoidable. An object of the present invention is to provide an active energy ray-curable resin composition for adhesives which has a relatively low molecular weight and provides good adhesive properties. [Means for solving the problem]
[0006] As a result of extensive investigation into the above-mentioned techniques, the inventors have discovered that by replacing the hydroxyl-containing acrylate, which is a constituent material of typical polyol-based urethane acrylates, with an alcohol, sufficient adhesive strength can be achieved even with a relatively low molecular weight composition. The present invention relates to [1] a resin composition for active energy ray-curable adhesives, comprising as its constituent a urethane (meth)acrylate resin obtained by reacting a polyisocyanate compound (a) having two or more isocyanate groups per molecule, at least one polyol (b) selected from polyester polyols, polycaprolactone polyols, polyether polyols, and polycarbonate polyols, a hydroxyl group-containing (meth)acrylate (c), and an aliphatic alcohol (d) having 4 to 12 carbon atoms, such that the sum of the isocyanate groups of the isocyanate compound (a) and the hydroxyl groups of the polyol (b), the hydroxyl group-containing (meth)acrylate (c), and the aliphatic alcohol (d) is equal, and the molar ratio of the hydroxyl group-containing (meth)acrylate (c) to the aliphatic alcohol (d) is 1 / 9 to 2 / 8.
[0007] The present invention also relates to [2] the active energy ray-curable resin composition for adhesives according to [1], wherein the polyol (b) has a molecular weight of 1,000 to 3,000. The present invention also relates to [3] the active energy ray-curable resin composition for adhesives according to [1] or [2], wherein the hydroxyl group-containing (meth)acrylate (c) is 2-hydroxyethyl acrylate. The present invention also relates to [4] a pressure-sensitive adhesive sheet obtained by coating a paper or film substrate with the active energy ray-curable resin composition for pressure-sensitive adhesives according to any one of [1] to [3] above. Effect of the Invention
[0008] According to the present invention, it is possible to obtain a resin composition for an active energy ray-curable adhesive which has a relatively low molecular weight and good adhesiveness without leaving any adhesive residue. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Representative compounds include an isocyanate compound (a), a polyol (b), a hydroxyl group-containing (meth)acrylate (c), and an aliphatic alcohol (d). In the present invention, the polyisocyanate compound (a) may be a diisocyanate compound such as tolylene diisocyanate, hydrogenated tolylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, lysine diisocyanate, naphthalene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, or hydrogenated xylylene diisocyanate.
[0010] Furthermore, biuret-type polyisocyanate compounds obtained by reacting the various diisocyanate compounds described above with water, adduct-type polyisocyanate compounds obtained by reacting the various diisocyanate compounds described above with a polyhydric alcohol such as trimethylolpropane, or polymers obtained by isocyanurating the various diisocyanate compounds described above can be used.
[0011] In the present invention, the polyester polyol of the component (b) is obtained by subjecting a polyvalent carboxylic acid and a polyhydric alcohol to an esterification reaction. Examples of polyvalent carboxylic acids include known and commonly used polyvalent carboxylic acids such as adipic acid, azelaic acid, sebacic acid, succinic acid, dimer acid, phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, tetrahydrophthalic anhydride, fumaric acid, maleic acid, maleic anhydride, itaconic acid, trimellitic acid, trimellitic anhydride, pyromellitic acid, and pyromellitic anhydride.
[0012] Examples of polyhydric alcohols include well-known and commonly used ones such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, neopentyl glycol, 1,4-butanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, an ethylene oxide or propylene oxide adduct of bisphenol A, glycerin, trimethylolpropane, trimethylolethane, pentaerythritol, dimethylolpropionic acid, and dimethylolbutanoic acid.
[0013] In the present invention, examples of the polycaprolactone polyol of the component (b) include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, neopentyl glycol, 1,4-butanediol, 1,6-hexanediol, an ethylene oxide or propylene oxide adduct of bisphenol A, glycerin, trimethylolpropane, trimethylolethane, pentaerythritol, and other commonly known and commonly used polyhydric alcohols such as ε-caprolactone adducts.
[0014] In the present invention, the polyether polyol of the component (b) may be any of the known and commonly used polyether polyols obtained by cationic polymerization of ethylene oxide, propylene oxide, and tetrahydrofuran.
[0015] In the present invention, examples of the polycarbonate polyol of component (b) include known and commonly used polycarbonate polyols obtained by, for example, reacting glycols such as 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and diethylene glycol with dimethyl carbonate, diethyl carbonate, ethylene carbonate, diphenyl carbonate, and phosgene.
[0016] In the present invention, the molecular weight of the polyol (b) is preferably within the range of 1000 to 4000. If it is smaller than this, good adhesion cannot be obtained, whereas if it is larger, the viscosity becomes high and handling properties are significantly deteriorated.
[0017] In the present invention, the hydroxyl group-containing (meth)acrylate of the component (c) may be any of the known and commonly used ones such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, butanediol mono(meth)acrylate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, glycidol di(meth)acrylate, pentaerythritol tri(meth)acrylate, etc. Here, (meth)acrylate refers to acrylate and / or methacrylate.
[0018] Examples of the aliphatic alcohol having 4 to 12 carbon atoms include known and commonly used alcohols such as butyl alcohol, hexyl alcohol, octyl alcohol, decyl alcohol, lauryl alcohol, and isomers thereof. Commercially available products can be used, and examples of linear saturated aliphatic alcohols include Conol 10WS, Conol 1098, Conol 1275 (trade names, manufactured by New Japan Chemical Co., Ltd.), Kalcol 0898, Kalcol 0880, Kalcol 1098, and Kalcol 2098 (trade names, manufactured by Kao Corporation).
[0019] The aliphatic alcohol used in the present invention preferably has a carbon number of 4 to 12. If the carbon number is less than 4, the viscosity becomes high, and if the carbon number is more than 12, the adhesive strength is lost due to the crystallinity of the material.
[0020] In the present invention, the molar ratio of the hydroxyl group-containing (meth)acrylate (c) to the aliphatic alcohol (d) is preferably within the range of 1 / 9 to 2 / 8. If the ratio of the aliphatic alcohol (d) is greater than this range, adhesive residue will occur on the substrate, and conversely, if it is smaller, the coating film after curing will be too hard and will not exhibit good adhesion.
[0021] In the present invention, it is preferable to adjust the isocyanate group of the isocyanate compound (a) to be equal to the sum of the hydroxyl groups of the polyol (b), the hydroxyl group-containing (meth)acrylate (c), and the aliphatic alcohol (d). If there is too much isocyanate compound (a), the remaining isocyanate group reacts with moisture to form a urea bond, which causes high viscosity and cloudiness, and conversely, if there is too little, the aliphatic alcohol remains unreacted, which causes glue residue.
[0022] Examples of active energy rays in the present invention include electron beams, α rays, β rays, γ rays, infrared rays, visible light, ultraviolet rays, etc. Among them, electron beams and ultraviolet rays have been relatively well researched, and ultraviolet rays in particular have the advantage that irradiation equipment therefor is inexpensive.
[0023] When the active energy ray-curable pressure-sensitive adhesive resin composition of the present invention is cured with active energy rays, if the above-mentioned electron beam is used, it is not necessary to mix a photopolymerization initiator. When the active energy ray-curable pressure-sensitive adhesive resin composition is cured with ultraviolet rays, it is necessary to mix a photopolymerization initiator with the active energy ray-curable pressure-sensitive adhesive resin composition. Examples of photopolymerization initiators include 2,2-dimethoxy-1,2-diphenylethan-1-one, benzophenone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, oxy-phenyl-acetic acid 2-[2-oxo-2-phenyl-acetoxy-ethoxy]ethyl ester, oxy-phenyl-acetic acid 2-[2-hydroxy-ethoxy]ethyl ester, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-dimethylamino-2-(4-methylbenzyl)-(4-1-morpholin-4-yl-phenyl)-butan-1-one, bis(2,4,6-trimethylbenzoyl) Bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, 1,2-octanedione, 1-[4-(phenylthio)-, 2-(o-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime), 2-chlorothioxanthone, 2,4-diethylthioxanthone, benzophenone, [4-(methylphenylthio)phenyl]phenylmethanone, ethylanthraquinone, etc., may be used alone or in a mixture of two or more kinds. The amount of the photopolymerization initiator to be used may be 1 to 5% by mass based on the resin solid content of the resin composition for active energy ray-curable adhesives, from the standpoint of adhesion, curability, cost, etc.
[0024] In order to enhance the effect of the photopolymerization initiator, an initiator aid such as p-dimethylaminobenzoic acid isoamyl ester, p-dimethylamino-benzoic acid ethyl ester, N-methyldiethanolamine, bisethylaminobenzophenone, ethyl-4-dimethylaminobenzoate, or 2-ethylhexyl-4-dimethylaminobenzoate can also be used.
[0025] The active energy ray-curable resin composition for adhesives of the present invention can be applied (coated) to a substrate, and then irradiated with active energy rays to cure the composition to form a coating film (adhesive layer), which can be used as an adhesive sheet. When applied to a substrate, it is preferable to adjust the thickness of the coating to 5 to 50 μm based on the resin solid content.
[0026] Specific examples of substrates for pressure-sensitive adhesive sheets include film substrates such as polyethylene film, polypropylene film, polyethylene terephthalate film, and polyethylene naphthalate film, as well as paper substrates such as fine paper, medium quality paper, art paper, cast coated paper, and coated paper. EXAMPLES
[0027] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the examples and comparative examples, "parts" and "%" refer to parts by mass and % by mass unless otherwise specified. The performance evaluation of the pressure-sensitive adhesive tape was performed according to the following method.
[0028] 1) Preparation of adhesive sheet: 3% of 2,2-dimethoxy-1,2-diphenylethan-1-one was mixed with the resin composition prepared in the examples and comparative examples, and the mixture was applied to untreated PET (polyethylene terephthalate material whose surface had not been subjected to plasma treatment, etc.) to a thickness of 25 μm. The sheet was then irradiated with ultraviolet light from a high-pressure mercury lamp to obtain an accumulated light quantity of 500 mJ / cm. 2 The coating was cured and formed. 2) Adhesive strength: The adhesive sheet thus prepared was pressed against a stainless steel plate with a 2 kg roller in one reciprocating motion, cut into a width of 25 mm, and measured by pulling the sheet at 180° at a speed of 200 mm / min at room temperature (23°C). 3) Adhesive residue: The stainless steel plate used in the measurement in 2) was visually inspected and touched to confirm whether any adhesive remained.
[0029] [Example 1] In a flask equipped with a stirrer, a thermometer, a reflux condenser and a nitrogen inlet tube, 336 parts of HDI (manufactured by Tosoh Corporation, trade name hexamethylene diisocyanate) as an isocyanate compound (a) and 1000 parts of Exenol 1020 (manufactured by AGC Corporation, trade name polypropylene glycol with a molecular weight of 1000) as a polyol (b) were charged, and the temperature was raised to 90 ° C. and the reaction was allowed to proceed for 8 hours while keeping the temperature. After confirming that the NCO% was saturated, 23.2 parts of BHEA (manufactured by Nippon Shokubai Co., Ltd., trade name 2-hydroxyethyl acrylate) as a hydroxyl group-containing (meth)acrylate (c) and 66.6 parts of butyl alcohol as an aliphatic alcohol (d) were charged, and the reaction was allowed to proceed for 7 hours while keeping the temperature, and the IR was measured to confirm that the isocyanate group had disappeared, thereby obtaining an active energy ray-curable resin composition. The molar ratio of the hydroxyl group-containing (meth)acrylate to the aliphatic alcohol (d) was 1 / 9, and the number of carbon atoms of the aliphatic alcohol was 4.
[0030] [Example 2] In a flask similar to that of Example 1, 500 parts of MDI (manufactured by Tosoh Corporation, trade name diphenylmethane diisocyanate) as the isocyanate compound (a) and 2000 parts of Exenol 2020 (manufactured by AGC Corporation, trade name polypropylene glycol with a molecular weight of 2000) as the polyol (b) were charged, and the temperature was raised to 90 ° C. and the reaction was allowed to proceed for 8 hours. After confirming that the NCO% was saturated, 46.4 parts of BHEA (manufactured by Nippon Shokubai Co., Ltd., trade name 2-hydroxyethyl acrylate) as the hydroxyl group-containing (meth)acrylate (c) and 297.6 parts of Conol 1275 (manufactured by New Japan Chemical Co., Ltd., trade name lauryl alcohol) as the aliphatic alcohol (d) were charged, and the reaction was allowed to proceed for 7 hours by keeping the temperature constant. The IR was measured, and it was confirmed that the isocyanate group had disappeared, to obtain an active energy ray-curable resin composition. The molar ratio of the hydroxyl group-containing (meth)acrylate to the aliphatic alcohol (d) was 2 / 8, and the aliphatic alcohol had 12 carbon atoms.
[0031] [Comparative Example 1] In a flask similar to that of Example 1, 444 parts of Desmodur I (manufactured by Sumika Covestro Urethane Co., Ltd., trade name isophorone diisocyanate) as an isocyanate compound (a) and 1000 parts of Exenol 1020 (manufactured by AGC Corporation, trade name polypropylene glycol with a molecular weight of 1000) as a polyol (b) were charged, and the temperature was raised to 90 ° C., and the reaction was carried out by keeping the temperature for 8 hours. After confirming that the NCO% was saturated, 232 parts of BHEA (manufactured by Nippon Shokubai Co., Ltd., trade name 2-hydroxyethyl acrylate) as a hydroxyl group-containing (meth)acrylate (c) were charged, and the reaction was carried out by keeping the temperature for 7 hours, and the IR was measured, and it was confirmed that the isocyanate group had disappeared, and an active energy ray-curable resin composition was obtained. The molar ratio of the hydroxyl group-containing (meth)acrylate and the aliphatic alcohol (d) was 10 / 0.
[0032] [Comparative Example 2] In a flask similar to that of Example 1, 336 parts of HDI (manufactured by Tosoh Corporation, trade name hexamethylene diisocyanate) as the isocyanate compound (a) and 1000 parts of Exenol 1020 (manufactured by AGC Corporation, trade name polypropylene glycol with a molecular weight of 1000) as the polyol (b) were charged, and the temperature was raised to 90 ° C. and the reaction was carried out by keeping the temperature for 8 hours. After confirming that the NCO% was saturated, 46.4 parts of hydroxyl group-containing (meth)acrylate (c) manufactured by BHEA Corporation, trade name 2-hydroxyethyl acrylate) and 432 parts of Conol 30SS (manufactured by New Japan Chemical Co., Ltd., trade name stearyl alcohol) were charged as the aliphatic alcohol (d), and the reaction was carried out by keeping the temperature for 7 hours, and IR was measured to confirm that the isocyanate group had disappeared, to obtain an active energy ray-curable resin composition. The molar ratio of the hydroxyl group-containing (meth)acrylate to the aliphatic alcohol (d) was 2 / 8, and the aliphatic alcohol had 18 carbon atoms.
[0033] The evaluation results of Examples 1 and 2 and Comparative Examples 1 and 2 are shown in Table 1.
[0034] [Table 1]
[0035] From Table 1, it can be seen that good adhesive strength can be obtained by reacting a common urethane acrylate, which does not exhibit adhesive strength, with an aliphatic alcohol having 4 to 12 carbon atoms in an adjusted ratio of (c) / (d) = 1 / 9 to 2 / 8.
Claims
1. The resin composition for active energy ray-curable pressure-sensitive adhesives comprises as its constituent a urethane (meth)acrylate resin obtained by reacting a polyisocyanate compound (a) having two or more isocyanate groups per molecule, at least one polyol (b) selected from polyester polyols, polycaprolactone polyols, polyether polyols, and polycarbonate polyols, a hydroxyl group-containing (meth)acrylate (c), and an aliphatic alcohol (d) which is butyl alcohol, such that the sum of the isocyanate groups of the isocyanate compound (a) and the hydroxyl groups of the polyol (b), the hydroxyl group-containing (meth)acrylate (c), and the aliphatic alcohol (d) is equal, and the molar ratio of the hydroxyl group-containing (meth)acrylate (c) to the aliphatic alcohol (d) is 1 / 9 to 2 / 8.
2. 2. The active energy ray-curable resin composition for adhesives according to claim 1, wherein the polyol (b) has a molecular weight of 1,000 to 3,000.
3. 3. The active energy ray-curable resin composition for adhesives according to claim 1, wherein the hydroxyl group-containing (meth)acrylate (c) is 2-hydroxyethyl acrylate.
4. 4. An adhesive sheet comprising a paper or film substrate coated with the active energy ray-curable resin composition for adhesives according to claim 1.
Citation Information
Patent Citations
Method for synthesizing low-hardness polyurethane acrylate
CN101935385A
Curable composition
JP1989121381A
Urethane prepolymer, its production and pressure-sensitive adhesive containing the same as component
JP1998330453A
Ultraviolet curable coating resin composition
JP2000281935A
Ultraviolet-curable composition and surface-functional material
JP2001002744A