Method for producing aqueous pigment dispersion and aqueous ink, and method for designing aqueous pigment dispersion and aqueous ink

By optimizing pigment, dispersant, and medium composition using NMR and solubility parameters, the method addresses the challenge of achieving rapid and stable aqueous pigment dispersions, enhancing production efficiency and reducing costs.

JP7552065B2Active Publication Date: 2024-09-18DIC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020078664
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-27
Publication Date
2024-09-18
Estimated Expiration
2040-04-27

Smart Images

  • Figure 0007552065000023
    Figure 0007552065000023
  • Figure 0007552065000022
    Figure 0007552065000022
  • Figure 0007552065000006
    Figure 0007552065000006
Patent Text Reader

Abstract

To provide a method capable of manufacturing an aqueous pigment dispersion having high pigment dispersion stability in a short time.SOLUTION: A manufacturing method of an aqueous pigment dispersion comprises a step of preparing a plurality of evaluation dispersions having different composition ratios of a first pigment dispersing agent to a first pigment, a step of obtaining an index of hydrophilicity and a step of obtaining an index of total surface area of particles for each of the plurality of evaluation dispersions, a step of determining the range of a composition mass ratio (R / P) of the first pigment dispersing agent to the first pigment ±0.2 or smaller as a compositional mass ratio of a second pigment dispersing agent to a second pigment in the aqueous pigment dispersion, and a step of mixing the second pigment, the second pigment dispersing agent, and a second aqueous solvent in accordance with the determined composition mass ratio, in which a Hansen solubility parameter of the second pigment, the second pigment dispersing agent and the second aqueous medium are, relative to the first Hansen parameter, ±3(J / cm3)1 / 2 or smaller, ±10(J / cm3)1 / 2 or smaller, and ±3(J / cm3)1 / 2 or smaller, respectively.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an aqueous pigment dispersion and an aqueous ink, and a method for designing an aqueous pigment dispersion and an aqueous ink. [Background technology]

[0002] In recent years, water-based inks have been replacing organic solvent-based inks in a wide range of fields due to their safety and low environmental impact. In particular, water-based inks have almost no odor and are therefore in high demand as inks that can be used in closed spaces such as offices.

[0003] Water-based inks are applied to various printing methods such as offset printing, gravure printing, and inkjet recording. Among them, the inkjet recording method allows on-demand printing, and is currently being studied extensively as an alternative to the electrophotographic (toner) method used in offices, etc.

[0004] Aqueous inks are produced, for example, by supplying and mixing, as necessary, a binder resin, an aqueous medium, etc. to an aqueous pigment dispersion obtained by dispersing a pigment in an aqueous medium in advance using a pigment dispersant. Therefore, when using an aqueous ink in an inkjet recording method, in order to impart good ejection stability, it is important to use an aqueous pigment dispersion that can reduce the generation of coarse particles, for example, due to the pigment, which can cause clogging of aqueous ink ejection nozzles, and can prevent the pigment and the like from settling over time.

[0005] In order to control the aggregation and sedimentation of pigments in an aqueous pigment dispersion and obtain an aqueous pigment dispersion having high pigment dispersion stability, it is important to quantify the interactions between the pigment, the pigment dispersant, and the aqueous medium (in other words, the phenomena occurring near the pigment interface). However, these interactions are dynamic behaviors, and it is difficult to quantify them by direct observation. Therefore, currently, the phenomena occurring near the pigment interface can only be qualitatively explained by combining multiple analytical methods.

[0006] Under such circumstances, a method has been proposed to quantify the phenomena occurring near the pigment interface in an aqueous pigment dispersion by combining the results of small-angle X-ray scattering of ink using a large synchrotron radiation facility (SPring8) with the easily measurable physical properties of the aqueous pigment dispersion (viscosity, particle size, etc.) (see Non-Patent Document 1). This method is praised for successfully quantifying the interactions between the pigment, pigment dispersant, and aqueous medium, as well as the dispersion state of the pigment. However, since the method requires measurements at the large synchrotron radiation facility (SPring8), which is the only one in Japan, and is both extremely large and extremely expensive, it is difficult to use it every time in product development and when responding to problems.

[0007] On the other hand, a storage test is generally carried out as a simple method for evaluating the pigment dispersion stability of an aqueous pigment dispersion. However, even if the storage test is accelerated by applying a temperature load of, for example, 60°C, the evaluation of the pigment dispersion stability may usually require a period of one month or more. Therefore, the conventional storage test has been a factor in lengthening the product development period. [Prior art documents] [Non-patent literature]

[0008] [Non-Patent Document 1] J.Jpn.SOC.Colour Mater.,92 213(2019) Summary of the Invention [Problem to be solved by the invention]

[0009] Therefore, an object of the present invention is to provide a method for producing an aqueous pigment dispersion that does not require large-scale equipment and that can produce an aqueous pigment dispersion having high pigment dispersion stability in a short period of time, and a method for producing an aqueous ink using the aqueous pigment dispersion. Another object of the present invention is to provide a method for designing an aqueous pigment dispersion, which can design an aqueous pigment dispersion having high pigment dispersion stability in a short period of time without requiring large-scale equipment, and a method for designing an aqueous ink using the design method. [Means for solving the problem]

[0010] As a result of intensive research to solve the above-mentioned problems, the inventors have found that the above-mentioned problems can be solved by determining an index of hydrophilicity using pulse NMR measurement for a pigment dispersion for evaluation containing a pigment, a pigment dispersant, and an aqueous medium, and also determining an index of the total surface area of ​​the particles, and using these determined indices to determine the composition ratios of the pigment and pigment dispersant in an aqueous pigment dispersion containing a pigment, a pigment dispersant, and an aqueous medium having solubility parameters that are approximate to those of the pigment, pigment dispersant, and aqueous medium in the pigment dispersion for evaluation, respectively, thereby completing the present invention.

[0011] That is, the present invention includes the following aspects. [1] A method for producing an aqueous pigment dispersion containing a second pigment, a second pigment dispersant, and a second aqueous medium, comprising: preparing a plurality of evaluation dispersions each containing a first pigment, polyvinylpyrrolidone as a first pigment dispersant, and a first aqueous medium, the dispersions having different composition ratios of the first pigment dispersant to the first pigment; determining a T2 relaxation time for each of the plurality of evaluation dispersions by pulse NMR measurement, and obtaining an index of hydrophilicity based on the reciprocal of the T2 relaxation time; measuring the volume average particle size of the particles for each of the plurality of evaluation dispersions to obtain an index of the total surface area of ​​the particles; determining a composition mass ratio of the second pigment dispersant to the second pigment in the aqueous pigment dispersion within a range of ±0.2 or less of a composition mass ratio (R / P) of the first pigment dispersant to the first pigment when the index of the total surface area of ​​the particles takes a maximum value in a graph showing the relationship between the index of the hydrophilicity degree, the index of the total surface area of ​​the particles, and the composition ratio, with the index of the hydrophilicity degree being plotted on the horizontal axis and the index of the total surface area of ​​the particles being plotted on the vertical axis; mixing the second pigment, the second pigment dispersant, and the second aqueous medium in accordance with the determined composition mass ratio; Including, The Hansen solubility parameter of the second pigment is within ±3 (J / cm) of the Hansen solubility parameter of the first pigment. 3 ) 1 / 2 is as follows: The Hansen solubility parameter of the second pigment dispersant is within ±10 (J / cm) of the Hansen solubility parameter of the first pigment dispersant. 3 ) 1 / 2 is as follows: The Hansen solubility parameter of the second aqueous medium is within ±3 (J / cm) of the Hansen solubility parameter of the first aqueous medium. 3 ) 1 / 2 Below is the A method for producing an aqueous pigment dispersion comprising the steps of: [2] The step of obtaining an index of hydrophilicity includes determining a T2 relaxation time by the pulse NMR measurement for a blank solution having the same composition ratio of the first pigment dispersant and the first aqueous medium in one of the plurality of evaluation dispersions and not containing the first pigment, and calculating an index of hydrophilicity (R sp For each of the plurality of dispersions for evaluation, A method for producing the aqueous pigment dispersion described in [1] above.

number

number

number

[0012] According to the present invention, it is possible to provide a method for producing an aqueous pigment dispersion that does not require large-scale equipment and that can produce an aqueous pigment dispersion having high pigment dispersion stability in a short period of time, and a method for producing an aqueous ink using the aqueous pigment dispersion. Furthermore, according to the present invention, it is possible to provide a method for designing an aqueous pigment dispersion, which can design an aqueous pigment dispersion having high pigment dispersion stability in a short period of time without requiring large-scale equipment, and a method for designing an aqueous ink using the design method. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a plot of Rsp vs. TSA for evaluation dispersions with different ratios of pigment to pigment dispersant. [Diagram 2] FIG. 1 is a plot of Ka vs. TSA for evaluation dispersions with different ratios of pigment to pigment dispersant. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the methods for producing the aqueous pigment dispersion and aqueous ink of the present invention, and the methods for designing the aqueous pigment dispersion and aqueous ink will be described in detail. However, the explanation of the constituent elements described below is an example of one embodiment of the present invention, and the present invention is not limited to these contents.

[0015] (Method of producing aqueous pigment dispersion and method of designing aqueous pigment dispersion) The method for producing an aqueous pigment dispersion of the present invention includes a step of preparing a plurality of dispersions for evaluation, a step of obtaining an index of the degree of hydrophilicity, a step of obtaining an index of the total surface area of ​​the particles, a determining step, and a mixing step, and further includes other steps as necessary. The method for producing an aqueous pigment dispersion is a method for producing an aqueous pigment dispersion containing a second pigment, a second pigment dispersant, and a second aqueous medium. The second pigment, the second pigment dispersant, and the second aqueous medium will be described in detail below. The method for designing an aqueous pigment dispersion of the present invention includes a step of preparing a plurality of dispersions for evaluation, a step of obtaining an index of the degree of hydrophilicity, a step of obtaining an index of the total surface area of ​​the particles, a first determining step, and a second determining step, and may further include other steps as necessary.

[0016] The present inventors have conducted extensive research with the aim of providing a method for producing an aqueous pigment dispersion that does not require large-scale equipment and that can produce an aqueous pigment dispersion having high pigment dispersion stability in a short period of time, and a method for producing an aqueous ink using the aqueous pigment dispersion. The present inventors also conducted intensive research with the aim of providing a method for designing an aqueous pigment dispersion, which can produce an aqueous pigment dispersion having high pigment dispersion stability in a short period of time without requiring large-scale equipment, and a method for designing an aqueous ink using the design method. Using an index of hydrophilicity obtained by pulse NMR measurement of the aqueous pigment dispersion and an index of the total surface area of ​​the particles, we were able to find a ratio of pigment to pigment dispersant that is effective for pigment dispersion stability in the aqueous pigment dispersion. We also found that this ratio can be applied to pigments, pigment dispersants, and aqueous media that have Hansen solubility parameters similar to those of the pigments, pigment dispersants, and aqueous media used in the measurement. As a result, the inventors found that the problems of the present invention can be solved by determining an index of the degree of hydrophilicity using pulse NMR measurement for a pigment dispersion for evaluation containing a pigment, a pigment dispersant, and an aqueous medium, and also determining an index of the total surface area of ​​the particles, and using these determined indices to determine the composition ratios of the pigment and pigment dispersant in an aqueous pigment dispersion containing a pigment, pigment dispersant, and an aqueous medium having solubility parameters approximate to those of the pigment, pigment dispersant, and aqueous medium in the dispersion for evaluation, respectively, thereby completing the present invention. Specifically, the inventors have found that when the composition ratio of the pigment dispersant to the pigment is plotted on a graph with the hydrophilicity index determined for the evaluation dispersion on the horizontal axis and the total surface area index of the particles on the vertical axis, the composition ratio that gives the maximum value is the composition ratio that provides excellent pigment dispersion stability.

[0017] <Step of Preparing Multiple Dispersions for Evaluation> The step of preparing a plurality of dispersions for evaluation is not particularly limited as long as it is a step of preparing a plurality of dispersions for evaluation containing a first pigment, polyvinylpyrrolidone as a first pigment dispersant, and a first aqueous medium, and having different composition ratios of the first pigment dispersant to the first pigment. The dispersion for evaluation is usually obtained by mixing the first pigment, the first pigment dispersant, and the first aqueous medium.

[0018] The first pigment dispersant is preferably polyvinylpyrrolidone, since it has a simple composition, is a standard pigment dispersant, and has high affinity for a wide range of pigments, although other pigment dispersants may be used as the first pigment dispersant. The molecular weight of polyvinylpyrrolidone is not particularly limited, but a weight average molecular weight of 80,000 to 120,000 is preferred in view of the standard molecular weight for a pigment dispersant. The first pigment, the other first pigment dispersants, and the first aqueous medium will be described in detail below.

[0019] The concentration (content) of the first pigment in the dispersion for evaluation is not particularly limited, but may be, for example, 1 to 40 mass %, 5 to 30 mass %, or 10 to 25 mass %. The content of the first aqueous medium in the dispersion for evaluation is not particularly limited, but may be, for example, 50 to 99 mass %, 60 to 95 mass %, or 75 to 90 mass %. The composition mass ratio of the first pigment dispersant to the first pigment in the multiple evaluation dispersions is not particularly limited, but may be, for example, 0.01 to 0.99, 0.05 to 0.80, or 0.10 to 0.70. However, the first pigment, the first pigment dispersant, and the first aqueous medium in the dispersion for evaluation The total content does not exceed 100% by mass.

[0020] When preparing multiple dispersions for evaluation, the difference in the composition mass ratio of the first pigment dispersant to the first pigment is not particularly limited, but may be, for example, changed in increments of 0.05 or in increments of 0.1.

[0021] The dispersion for evaluation can be produced, for example, by the following method. (1) A method of preparing a dispersion for evaluation by adding a first pigment to a mixture containing a first pigment dispersant and a first aqueous medium, and then dispersing the first pigment in the mixture using a stirring and dispersing device. (2) A method in which a first pigment and a first pigment dispersant are kneaded using a kneading machine such as a two-roll mill or a mixer, the resulting kneaded mixture is added to a first aqueous medium, and a dispersion for evaluation is prepared using a stirring and dispersing device. (3) A method in which a first pigment is added to a solution obtained by dissolving a first pigment dispersant in an organic solvent that is compatible with water, such as methyl ethyl ketone, tetrahydrofuran, etc., and then the first pigment is dispersed in the organic solution using a stirring and dispersing device. Next, phase inversion emulsification is performed using an aqueous medium, and then the organic solvent is distilled off to prepare a dispersion for evaluation.

[0022] The kneading machine is not particularly limited, and examples thereof include a Henschel mixer, a pressure kneader, a Banbury mixer, an intensive mixer, a planetary mixer, and a butterfly mixer.

[0023] As the stirring and dispersing device, for example, an ultrasonic homogenizer, a high-pressure homogenizer, a paint shaker, a ball mill, a roll mill, a sand mill, a sand grinder, a Dyno Mill, a Dispermat, an SC Mill, a Nanomizer, etc. can be used alone or in combination of two or more kinds.

[0024] <Step of Obtaining an Index of Hydrophilicity> The process for obtaining an index of the degree of hydrophilicity is not particularly limited, so long as it is a process for determining the T2 relaxation time for each of a plurality of dispersions for evaluation by pulse NMR measurement, and obtaining an index of the degree of hydrophilicity based on the reciprocal of the T2 relaxation time.

[0025] Pulsed NMR (Nuclear Magnetic Resonance) is a technique specialized in obtaining the relaxation time (spin-lattice relaxation time: T1 relaxation time) and spin-spin relaxation time (T2 relaxation time) of 1H nuclei, which are indicators of molecular mobility. Pulsed NMR measurement has the following features: -Highly sensitive to sample conditions (hardness of solid materials, molecular motion of liquid samples, etc.) No pretreatment such as drying or degassing is required The upper limit of concentration is fundamentally unlimited, and the lower limit of concentration is 1% to 2%. Measurement time is only about 5 minutes from start to finish -Good reproducibility

[0026] In general, the movement of liquid molecules adsorbed on particle surfaces is restricted, whereas liquid molecules in bulk liquids can move freely. As a result, the NMR relaxation time (T2 relaxation time) of liquid molecules adsorbed on particle surfaces is shorter than the T2 relaxation time of molecules in bulk liquids, and can differ by several orders of magnitude. The inverse of the T2 relaxation time is related to the degree of hydrophilicity of particles in particle dispersions.

[0027] Pulsed NMR measurements can be performed, for example, under the following conditions. Measurement equipment: Acron Area (manufactured by XiGo Nanotools) Pulse sequence: CPMG method ·Resonance frequency: 13MHz ·Measurement temperature: 30℃ Measurement sample: 1.0 cm 3

[0028] The index of hydrophilicity is preferably calculated from the reciprocal of the T2 relaxation time of the dispersion for evaluation and the reciprocal of the T2 relaxation time of the blank solution. That is, the step of obtaining an index of the hydrophilicity preferably includes a process of determining the T2 relaxation time by pulse NMR measurement for a blank solution that has the same composition ratio of the first pigment dispersant and the first aqueous medium in one of the multiple evaluation dispersions and does not contain the first pigment, and obtaining an index of the hydrophilicity (Rsp), which is an index of the hydrophilicity, from the reciprocal of the T2 relaxation time of one of the evaluation aqueous dispersions and the reciprocal of the T2 relaxation time of the blank solution according to the following formula (1), for each of the multiple evaluation dispersions.

number

[0029] <Step for obtaining an index of total surface area of ​​particles> The step of obtaining an index of the total surface area of ​​the particles is not particularly limited as long as it is a step of measuring the volume average particle size of the particles for each of a plurality of dispersions for evaluation and obtaining an index of the total surface area of ​​the particles.

[0030] The volume average particle size of the particles can be measured, for example, under the following conditions. Measurement device: Microtrac MT3000II (Microtrac Bell) Measurement solvent: Water Solvent refractive index: 1.333 Presence ratio: Volume basis ·Particle permeability: Transmission ·Particle shape: non-spherical Particle refractive index: 1.81 Analysis mode: Rosin-Rammler distribution (±2σ) (Software included with the device: DMS ver.11.0.0-246V)

[0031] The index of the total surface area of ​​the particles is preferably a value that is directly proportional to the reciprocal of the volume average particle size of the particles. Furthermore, the step of obtaining an index of the total surface area of ​​the particles preferably includes a process of obtaining a total surface area value (TSA) of the particles, which is an index of the total surface area of ​​the particles, from the volume average particle size of the particles using the following formula (2), for each of the multiple evaluation dispersions.

number

number

[0032] <Determining (first) step> The step of determining the composition mass ratios in the manufacturing method of an aqueous pigment dispersion, and the first step of determining the composition mass ratios in the design method of an aqueous pigment dispersion are not particularly limited as long as they are steps of determining, as the composition mass ratio of the second pigment dispersant to the second pigment in the aqueous pigment dispersion, a range of not more than ±0.2 of the composition mass ratio (R / P) of the first pigment dispersant to the first pigment when the index of the total surface area of ​​the particles takes a maximum value in a graph showing the relationship between the index of the hydrophilicity degree, the index of the total surface area of ​​the particles, and the composition ratios, with the index of the hydrophilicity degree on the horizontal axis and the index of the total surface area of ​​the particles on the vertical axis. The pigment dispersion stability of the dispersion for evaluation is most stable at the maximum value in the graph. If the index of the total surface area of ​​the particles is within ±0.2 of the composition mass ratio (R / P) when the index is at the maximum value in the graph, the pigment dispersion stability is superior to other ranges. The reason why the local maximum value was adopted instead of the maximum value is as follows. The pigment surface has a wide distribution in terms of interface chemistry, and even if a pigment dispersion is uniform when viewed macroscopically, it is expected that the pigment surface is likely to have non-uniform adsorption of the solvent or resin when viewed microscopically. Furthermore, the interface chemistry distribution may also have multiple peaks depending on the pigment type. For this reason, if the maximum value instead of the local maximum value is adopted in the graph, there is a concern that the optimal value will be overlooked.

[0033] The range of the composition mass ratio (R / P) within ±0.2 is further defined as within ±10% of the TSA at the maximum value and within the R sp It is preferable that the composition mass ratio (R / P) is within ±5% of the above.

[0034] <Mixing process> The mixing step is not particularly limited as long as it is a step of mixing the second pigment, the second pigment dispersant, and the second aqueous medium in accordance with the determined composition mass ratio. Here, when the second pigment, the second pigment dispersant, and the second aqueous medium are mixed according to the determined composition mass ratio, the composition mass ratio may be exactly the same as the determined composition mass ratio, or the composition mass ratio may be slightly changed within a range that does not impair the pigment dispersion stability. For example, the concentration of the second pigment in the aqueous pigment dispersion to be produced may differ by ±2 mass% from the concentration of the second pigment in the aqueous pigment dispersion at the determined composition mass ratio. For example, the concentration of the second pigment dispersant in the aqueous pigment dispersion to be produced may differ by ±2 mass% from the concentration of the second pigment dispersant in the aqueous pigment dispersion at the determined composition mass ratio. For example, the concentration of the second aqueous medium in the aqueous pigment dispersion to be produced may differ by ±2 mass% from the concentration of the second aqueous medium in the aqueous pigment dispersion at the determined composition mass ratio.

[0035] The mixing method may be, for example, the following method. (1) A method for preparing an aqueous pigment dispersion by adding a second pigment to a mixture containing a second pigment dispersant and a second aqueous medium, and then dispersing the second pigment in the mixture using a stirring and dispersing device. (2) A method in which a second pigment and a second pigment dispersant are kneaded using a kneading machine such as a two-roll mill or a mixer, the resulting kneaded mixture is added to a second aqueous medium, and an aqueous pigment dispersion is prepared using a stirring and dispersing device. (3) A method in which a second pigment is added to a solution obtained by dissolving a second pigment dispersant in an organic solvent compatible with water, such as methyl ethyl ketone or tetrahydrofuran, and the like, and then the second pigment is dispersed in the organic solution using a stirring and dispersing device, and then phase inversion emulsification is performed using an aqueous medium, and the organic solvent is then distilled off to prepare an aqueous pigment dispersion.

[0036] Examples of the kneader and stirring / dispersing device include the kneader and stirring / dispersing device mentioned in the above-mentioned method for producing the dispersion for evaluation.

[0037] <The second step of deciding> The second determining step in the method for designing an aqueous pigment dispersion is not particularly limited, so long as it is a step of determining the compositional ratio of the second pigment, the second pigment dispersant, and the second aqueous medium in the aqueous pigment dispersion in accordance with the determined compositional mass ratio. Here, when determining the composition ratio of the second pigment, the second pigment dispersant, and the second aqueous medium according to the determined composition mass ratio, the composition ratio may be exactly the same as the determined composition mass ratio, or may be slightly changed within a range that does not impair the pigment dispersion stability. For example, the concentration of the second pigment in the designed aqueous pigment dispersion may differ by ±2 mass% from the concentration of the second pigment in the aqueous pigment dispersion at the determined composition mass ratio. For example, the concentration of the second pigment dispersant in the designed aqueous pigment dispersion may differ by ±2 mass% from the concentration of the second pigment dispersant in the aqueous pigment dispersion at the determined composition mass ratio. For example, the concentration of the second aqueous medium in the designed aqueous pigment dispersion may differ by ±2 mass% from the concentration of the second aqueous medium in the aqueous pigment dispersion at the determined composition mass ratio.

[0038] The Hansen solubility parameter of the second pigment is within ±3 (J / cm) of the Hansen solubility parameter of the first pigment. 3 ) 1 / 2 The following is the result. The Hansen solubility parameter of the second pigment dispersant is within ±10 (J / cm) of the Hansen solubility parameter of the first pigment dispersant. 3 ) 1 / 2 The following is the result. The Hansen solubility parameter of the second aqueous medium is within ±3 (J / cm) of the Hansen solubility parameter of the first aqueous medium. 3 ) 1 / 2 The following is the result. Hansen solubility parameter (HSP) is a value used to predict the solubility of a substance. HSP is based on the idea that two substances with similar intermolecular interactions are likely to dissolve in each other. HSP (unit: J / cm 3 ) 1 / 2 ] is composed of the following three parameters: δd: Energy due to dispersion forces between molecules δp: Energy due to dipole interactions between molecules δh: Energy due to hydrogen bonds between molecules These three parameters can be considered as coordinates in a three-dimensional space (Hansen space). When the HSPs of two substances are placed in Hansen space, the closer the distance between the two points, the easier it is for them to dissolve in each other. In other words, the difference in the Hansen solubility parameters of two substances indicates that the hydrophilic and hydrophobic states of the two substances are similar.

[0039] The Hansen solubility parameter of the second pigment is within ±3 (J / cm) of the Hansen solubility parameter of the first pigment. 3 ) 1 / 2 If the above is the case, the two pigments can be said to have similar hydrophilic and hydrophobic states in terms of pigment dispersion stability. The Hansen solubility parameter of the second pigment dispersant is within ±10 (J / cm) of the Hansen solubility parameter of the first pigment dispersant. 3 )1 / 2 If the above conditions are met, the two pigment dispersants can be said to have similar hydrophilic and hydrophobic states in terms of pigment dispersion stability. The Hansen solubility parameter of the second aqueous medium is within ±3 (J / cm) of the Hansen solubility parameter of the first aqueous medium. 3 ) 1 / 2 If the above conditions are met, the two aqueous media can be said to have similar hydrophilic and hydrophobic states in terms of pigment dispersion stability. Therefore, within these ranges, even if the composition ratio of the pigment to the pigment dispersant with excellent pigment dispersion stability obtained in the evaluation dispersion is applied to the composition ratio of the pigment to the pigment dispersant in the aqueous pigment dispersion, an aqueous pigment dispersion with excellent pigment dispersion stability can be obtained. The first pigment and the second pigment may be the same. The first pigment dispersant and the second pigment dispersant may be the same. The first aqueous medium and the second aqueous medium may be the same.

[0040] The Hansen solubility parameter of the second pigment is within ±2.5 (J / cm) of the Hansen solubility parameter of the first pigment. 3 ) 1 / 2 It is preferable that the temperature is within ±2 (J / cm 3 ) 1 / 2 More preferably, it is ±1.5 (J / cm 3 ) 1 / 2 It is even more preferable that: The Hansen solubility parameter of the second pigment dispersant is within ±8 (J / cm) of the Hansen solubility parameter of the first pigment dispersant. 3 ) 1 / 2 It is preferable that the temperature is within ±5 (J / cm 3 ) 1 / 2 More preferably, it is ±3 (J / cm 3 ) 1 / 2 It is even more preferable that: The Hansen solubility parameter of the second aqueous medium is within ±2.5 (J / cm) of the Hansen solubility parameter of the first aqueous medium. 3 ) 1 / 2 It is preferable that the temperature is within ±2 (J / cm 3 )1 / 2 More preferably, it is ±1.5 (J / cm 3 ) 1 / 2 It is even more preferable that:

[0041] The Hansen solubility parameter of a pigment can be determined, for example, by the following method. Transparent screw cap bottle (screw cap bottle, capacity: 20cm 3 ) is charged with 10 mg (0.01 g) of the pigment to be measured and 9.99 g of organic solvent (pigment concentration: 0.1% by mass), shaken and mixed for 30 minutes using a high-speed shaker (Cute Mixer), and then centrifuged at 4000 rpm for 30 minutes (25°C) using a LUMiSizer, a multi-sample particle size distribution measurement device for evaluating dispersibility. If the amount of light transmitted is less than 20%, the pigment dispersibility is deemed good and the organic solvent is judged to be a "good solvent," and if the amount of light transmitted is 20% or more, the organic solvent is judged to be a "poor solvent." The organic solvent and its corresponding judgment result of "good solvent" or "poor solvent" are input into computer software Hansen Solubility Parameters in Practice 4th Edition 4.1.07 (HSPiP) to calculate the Hansen solubility parameter of the pigment to be measured. For the Hansen solubility parameters of the organic solvents used, the values ​​recorded in the above-mentioned computer software Hansen Solubility Parameters in Practice 4th Edition 4.1.07 (HSPiP) can be used as is.

[0042] The Hansen solubility parameter of a pigment dispersant can be determined, for example, by the following method. Transparent screw cap bottle (screw cap bottle, capacity: 20cm 3 ) was charged with 50 mg (0.05 g) of the pigment dispersant to be measured and 9.95 g of organic solvent (pigment dispersant concentration: 0.5% by mass), shaken and mixed for 30 minutes using a high-speed shaker (cute mixer), and then allowed to stand for 24 hours in an environment at 25°C. If it is confirmed by visual observation after leaving the organic solvent to stand for 24 hours that the entire amount of the pigment dispersant has been dissolved, the organic solvent is judged to be a "good solvent." If it is not confirmed that the entire amount of the pigment dispersant has been dissolved, for example because some of the pigment dispersant remains dissolved, the organic solvent is judged to be a "poor solvent." The organic solvent and its corresponding judgment result of "good solvent" or "poor solvent" are input into computer software Hansen Solubility Parameters in Practice 4th Edition 4.1.07 (HSPiP) to calculate the Hansen solubility parameters of the pigment dispersant to be measured. For the Hansen solubility parameters of the organic solvents used, the values ​​recorded in the above-mentioned computer software Hansen Solubility Parameters in Practice 4th Edition 4.1.07 (HSPiP) can be used as is.

[0043] The Hansen solubility parameters of the aqueous medium can be the values ​​listed in the above Hansen Solubility Parameters in Practice 4th Edition 4.1.07 (HSPiP). Also, the Hansen solubility parameters of the aqueous medium can be known values. The Hansen solubility parameters of an example of an aqueous medium are known as follows:

[0044] [Table 1]

[0045] <Pigments> The first pigment and the second pigment (hereinafter, sometimes simply referred to as "pigments") are not particularly limited, and for example, organic pigments or inorganic pigments that are typically used in conventional screen printing or aqueous inkjet recording inks can be used.

[0046] The pigment may be either a non-acid-treated pigment or an acid-treated pigment, and may be in either a dry powder or wet cake form.

[0047] As the inorganic pigment, for example, iron oxide and carbon black produced by a contact method, a furnace method, a thermal method, or the like can be used.

[0048] Examples of organic pigments that can be used include azo pigments (including azo lakes, insoluble azo pigments, condensed azo pigments, chelate azo pigments, etc.), polycyclic pigments (such as phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments, etc.), lake pigments (such as basic dye-type chelates, acid dye-type chelates, etc.), nitro pigments, nitroso pigments, aniline black, and the like.

[0049] Specific examples of pigments used in black inks include Mitsubishi Chemical's No. 2300, No. 2200B, No. 900, No. 980, No. 960, No. 33, No. 40, No. 45, No. 45L, No. 52, HCF88, MCF88, MA7, MA8, MA100, etc.; Columbia's Raven 5750, Raven 5250, Raven 5000, Raven 3500, Raven 1255, Raven 700, etc.; Cabot's Regal 400R, Regal 330R, Regal 660R, Mogul L, Mogul 700, Monarch 800, Monarch 880, Monarch 900, Monarch 1000, Monarch 1100, Monarch 1300, Monarch 1400, etc.; and Degussa's Color Black. Carbon blacks such as FW1, FW2, FW2V, FW18, FW200, S150, S160, S170, Printex 35, U, V, 1400U, Special Black 6, 5, 4, 4A, NIPEX150, NIPEX160, NIPEX170, and NIPEX180 can be used.

[0050] Specific examples of pigments used in yellow inks include CI Pigment Yellow 1, 2, 12, 13, 14, 16, 17, 73, 74, 75, 83, 93, 95, 97, 98, 109, 110, 114, 120, 128, 129, 138, 150, 151, 154, 155, 174, 180, and 185.

[0051] Specific examples of pigments used in the magenta ink include CI Pigment Violet 19, CI Pigment Red 5, 7, 12, 48(Ca), 48(Mn), 57(Ca), 57:1, 112, 122, 123, 146, 168, 176, 184, 185, 202, 209, and mixtures or solid solutions of at least two or more pigments selected from these pigments.

[0052] Specific examples of pigments used in cyan inks include CI Pigment Blue 1, 2, 3, 15, 15:3, 15:4, 15:6, 16, 22, 60, 63, 66, and the like.

[0053] Specific examples of pigments used in the red ink include one or more pigments selected from the group consisting of CI Pigment Red 17, 49:2, 112, 149, 150, 177, 178, 179, 188, 254, 255, and 264.

[0054] Specific examples of pigments used in orange inks include CI Pigment Orange 1, 2, 5, 7, 13, 14, 15, 16, 24, 34, 36, 38, 40, 43, 63, 64, 71, 73, and 81.

[0055] Specific examples of pigments used in green inks include CI Pigment Green 7, 10, 36, 58, 59, and the like.

[0056] Specific examples of pigments used in the violet ink include CI Pigment Violet 19, 23, 32, 33, 36, 38, 43, 50, and the like.

[0057] Specific examples of pigments that can be used in the white ink include alkaline earth metal sulfates, carbonates, finely powdered silicic acid, synthetic silicates, and other silicates, calcium silicate, alumina, alumina hydrate, titanium oxide, zinc oxide, talc, clay, etc. These may be surface-treated.

[0058] As the pigment, the above-mentioned pigments can be used alone or in combination of two or more kinds.

[0059] <Pigment dispersant> Examples of the first pigment dispersant and the second pigment dispersant (hereinafter, sometimes simply referred to as "pigment dispersant") include polyvinyl alcohols; polyvinylpyrrolidones; acrylic resins such as acrylic acid-acrylic acid ester copolymers; styrene-acrylic resins such as styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-methacrylic acid-acrylic acid ester copolymers, styrene-α-methylstyrene-acrylic acid copolymers, and styrene-α-methylstyrene-acrylic acid-acrylic acid ester copolymers; aqueous resins such as styrene-maleic acid copolymers, styrene-maleic anhydride copolymers, and vinylnaphthalene-acrylic acid copolymers, and salts of aqueous resins. Examples of pigment dispersants that can be used include the Ajisper PB series from Ajinomoto Fine-Techno Co., Ltd., the Disperbyk series from BYK Japan Co., Ltd., the EFKA series and JONCRYL series from BASF, the SOLSPERSE series from Lubrizol Japan Co., Ltd., and the TEGO series from Evonik.

[0060] As a pigment dispersant, it is preferable to use the polymer (G) described below, which can significantly reduce coarse particles and, as a result, impart the good ejection stability required when the ink is ejected by an inkjet method.

[0061] As the polymer (G), a polymer having an anionic group can be used. In particular, it is preferable to use a polymer having a number average molecular weight in the range of 500 to 30,000, which has a solubility in water of 0.1 g / 100 mL or less and is capable of forming fine particles in water when the neutralization rate of the anionic group with a basic compound is 100%.

[0062] As the anionic group, for example, a carboxyl group, a carboxylate group, a sulfonic acid group, a sulfonate group, etc. can be used. Among them, it is preferable to use a carboxylate group or a sulfonate group in which a part or all of the carboxyl group or the sulfonic acid group is neutralized with a basic compound or the like in order to impart good water dispersion stability.

[0063] Such a polymer having an anionic group may be produced by a known method or may be a commercially available product, such as Acrydic WML-542 (manufactured by DIC Corporation) or Unidic EMG-1015 (manufactured by DIC Corporation).

[0064] The solubility of polymer (G) in water was defined as follows. That is, 0.5 g of polymer (E) whose particle size was adjusted to the range of 250 μm to 90 μm using sieves with 250 μm and 90 μm openings was sealed in a bag made of 400 mesh wire netting, immersed in 50 mL of water, and left to stand for 24 hours with gentle stirring at a temperature of 25°C. After immersion for 24 hours, the 400 mesh wire netting containing polymer (E) was dried for 2 hours in a dryer set at 110°C. The change in weight of the 400 mesh wire netting containing polymer (E) before and after immersion in water was measured, and the solubility was calculated by the following formula.

[0065]

number

[0066] In the present invention, whether or not fine particles are formed in water when the neutralization rate of the anionic group with the basic compound is 100% is judged as follows. (1) The acid value of polymer (G) is measured in advance by an acid value measurement method based on JIS test method K 0070-1992. Specifically, 0.5 g of polymer (G) is dissolved in tetrahydrofuran, and the acid value is determined by titration with 0.1 M potassium hydroxide alcohol solution using phenolphthalein as an indicator. (2) 1 g of polymer (G) is added to 50 mL of water, and then a 0.1 mol / L aqueous potassium hydroxide solution sufficient to neutralize the resulting acid value 100% is added to neutralize the acid value 100%. (3) The 100% neutralized liquid is exposed to ultrasonic waves in an ultrasonic cleaner (SND Corporation ultrasonic cleaner US-102, 38 kHz self-oscillation) at a temperature of 25°C for 2 hours, and then left at room temperature for 24 hours.

[0067] After leaving it for 24 hours, the liquid at a depth of 2 centimeters from the liquid surface is sampled and the presence of fine particles is confirmed by determining whether light scattering information due to fine particle formation can be obtained using a dynamic light scattering particle size distribution analyzer (Nikkiso Co., Ltd., dynamic light scattering particle size analyzer "Microtrac Particle Size Distribution Analyzer UPA-ST150").

[0068] In order to further improve the stability of the fine particles formed by the polymer (G) in water, the particle diameter of the fine particles is preferably in the range of 5 nm to 1000 nm, more preferably in the range of 7 nm to 700 nm, and most preferably in the range of 10 nm to 500 nm. Although the narrower the particle size distribution of the fine particles, the better the dispersion stability, it is possible to obtain an ink with better dispersion stability than before, even if the particle size distribution is broad. The particle diameter and particle size distribution were measured using a dynamic light scattering particle size distribution measuring device (dynamic light scattering particle size measuring device "Microtrac Particle Size Distribution Meter UPA-ST150" manufactured by Nikkiso Co., Ltd.) in the same manner as in the measurement method for the fine particles.

[0069] The number average molecular weight of the polymer (G) is preferably in the range of 500 to 30,000, more preferably 1,000 to 6,000, even more preferably 1,300 to 5,000, and particularly preferably 1,500 to 4,500, which can effectively suppress aggregation of the pigment in the aqueous medium (C) and is therefore particularly preferred in terms of obtaining an ink with good pigment dispersion stability.

[0070] The number average molecular weight is a value calculated as polystyrene by GPC (gel permeation chromatography), specifically, a value measured under the following conditions.

[0071] (Method of measuring number average molecular weight (Mn)) Measurements were performed by gel permeation chromatography (GPC) under the following conditions. Measurement equipment: High-speed GPC equipment (Tosoh Corporation "HLC-8220GPC") Column: The following columns manufactured by Tosoh Corporation were used, connected in series.

[0072] "TSKgel G5000" (7.8mm I.D. x 30cm) x 1 "TSKgel G4000" (7.8mm I.D. x 30cm) x 1 "TSKgel G3000" (7.8mm I.D. x 30cm) x 1 "TSKgel G2000" (7.8mmI.D. x 30cm) x 1 Detector: RI (differential refractometer) Column temperature: 40℃ Eluent: Tetrahydrofuran Flow rate: 1.0mL / min Injection volume: 100 μL (sample concentration 0.4% by mass in tetrahydrofuran solution) Standard sample: A calibration curve was prepared using the following standard polystyrene. (Standard polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation

[0073] The surface tension of the ink containing the polymer (G) is preferably 30 dyn / cm or more, more preferably 40 dyn / cm or more, and particularly preferably 65 dyn / cm to 75 dyn / cm, which is close to the surface tension of water. The surface tension is a value measured for a 100% neutralized polymer solution by adding 1 g of the polymer (G) to water and then adding a 0.1 mol / L potassium hydroxide aqueous solution sufficient to neutralize the resulting acid value 100%.

[0074] The neutralization rate of the polymer (G) was determined by the following formula.

[0075]

number

[0076] The acid value of the polymer (G) was measured based on JIS test method K 0070-1992. Specifically, 0.5 g of a sample was dissolved in tetrahydrofuran, and titrated with a 0.1 M alcoholic solution of potassium hydroxide using phenolphthalein as an indicator. The method for measuring the acid value of other polymers in this specification also complies with JIS test method K 0070-1992.

[0077] The acid value of the polymer (G) is preferably in the range of 20 mgKOH / g to 400 mgKOH / g, more preferably 30 mgKOH / g to 300 mgKOH / g, and even more preferably 40 mgKOH / g to 190 mgKOH / g, which can effectively suppress aggregation of the pigment in the aqueous medium (C) and provide an ink with good dispersion stability of the pigment.

[0078] As the polymer (G), a polymer that is insoluble or poorly soluble in water when unneutralized and forms fine particles when 100% neutralized can be used, and is not particularly limited as long as it is a polymer that has a hydrophobic group in one molecule in addition to an anionic group, which is a hydrophilic group.

[0079] Such a polymer may be a block polymer having a polymer block having a hydrophobic group and a polymer block having an anionic group. In the polymer (G), the number of anionic groups and the solubility in water are not necessarily determined by the acid value or the number of anionic groups at the time of polymer design. For example, even if the polymer has the same acid value, the polymer with a low molecular weight tends to have a high solubility in water, and the polymer with a high molecular weight tends to have a low solubility in water.

[0080] The polymer (G) may be a homopolymer, but is preferably a copolymer, and may be a random polymer, a block polymer, or an alternating polymer, but is preferably a block polymer. The polymer may be a branched polymer, but is preferably a linear polymer.

[0081] In addition, the polymer (G) is preferably a vinyl polymer from the viewpoint of freedom in design, and as a method for producing a vinyl polymer having the desired molecular weight and solubility characteristics in the present invention, it is preferable to produce it by using "living polymerization" such as living radical polymerization, living cationic polymerization, or living anionic polymerization.

[0082] Among these, the polymer (G) is preferably a vinyl polymer produced using a (meth)acrylate monomer as one of the raw materials, and as a method for producing such a vinyl polymer, living radical polymerization and living anionic polymerization are preferred, and living anionic polymerization is further preferred from the viewpoint of enabling more precise design of the molecular weight of the block polymer and each segment.

[0083] <Aqueous medium> As the first aqueous medium and the second aqueous medium (hereinafter sometimes simply referred to as the "aqueous medium" or the "aqueous medium (C)"), water alone or a mixed solvent of water and an organic solvent (F) described below can be used.

[0084] As the water, specifically, pure water or ultrapure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, distilled water, etc. can be used.

[0085] Examples of the organic solvent (F) include ketones such as acetone, methyl ethyl ketone, methyl butyl ketone, and methyl isobutyl ketone; alcohols such as methanol, ethanol, 2-propanol, 2-methyl-1-propanol, 1-butanol, and 2-methoxyethanol; ethers such as tetrahydrofuran, 1,4-dioxane, and 1,2-dimethoxyethane; glycols such as dimethylformamide, N-methylpyrrolidone, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, polyethylene glycol, and polypropylene glycol; diols such as butanediol, pentanediol, hexanediol, and diols of the same group as these; and lauric acid proton. Glycol esters such as propylene glycol; glycol ethers such as cellosolves including diethylene glycol monoethyl, diethylene glycol monobutyl ether, diethylene glycol monohexyl ether, propylene glycol ether, dipropylene glycol ether, and triethylene glycol ether; alcohols such as methanol, ethanol, isopropyl alcohol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, and other butyl alcohols, pentyl alcohol, and alcohols of the same family; sulfolane; lactones such as γ-butyrolactone; and lactams such as N-(2-hydroxyethyl)pyrrolidone, which can be used alone or in combination of two or more kinds.

[0086] In addition to the organic solvents mentioned above, it is preferable to use, as the organic solvent (F), a water-soluble organic solvent (f1) having a boiling point of 100°C or more and 200°C or less and a vapor pressure of 0.5 hPa or more at 20°C, in order to obtain a quick-drying effect in which the ejected droplets quickly dry on the recording medium after landing on the surface of the recording medium.

[0087] Examples of the water-soluble organic solvent (f1) include 3-methoxy-1-butanol, 3-methyl-3-methoxy-1-butanol, 3-methoxy-3-methyl-1-butyl acetate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, ethylene glycol-t-butyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, dipropylene glycol dimethyl ether, 4-methoxy-4-methyl-2-pentanone, and ethyl lactate. Two or more of these may be used in combination.

[0088] Among these, it is preferable to use, as the water-soluble organic solvent (f1), a water-soluble organic solvent having a hydrogen bond term ΔH of HSP (Hansen Solubility Parameter) in the range of 6 to 20 in order to maintain good dispersion stability of the ink and to suppress deterioration of, for example, the ink ejection nozzle of an inkjet device due to the influence of the solvent contained in the ink.

[0089] Specific examples of water-soluble organic solvents having a hydrogen bond term of HSP within the above range include 3-methoxy-1-butanol, 3-methyl-3-methoxy-1-butanol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, ethylene glycol-t-butyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monopropyl ether, and more preferably 3-methoxy-1-butanol and 3-methyl-3-methoxy-1-butanol.

[0090] As an organic solvent that can be used in combination with the aqueous medium (C), in addition to the water-soluble organic solvent (f1) described above, or together with the water-soluble organic solvent (f1), a combination of propylene glycol (f2) and one or more organic solvents (f3) selected from the group consisting of glycerin, glycerin derivatives, diglycerin and diglycerin derivatives is preferably used, in order to achieve both the effect of quick-drying the ink on the recording medium and the effect of preventing the ink from drying or solidifying at the ink ejection orifice.

[0091] As the organic solvent (f3), for example, glycerin, diglycerin, polyglycerin, diglycerin fatty acid ester, polyoxypropylene (n) polyglyceryl ether represented by the following general formula (1), polyoxyethylene (n) polyglyceryl ether represented by the following general formula (2), etc. can be used alone or in combination of two or more kinds.

[0092] Among these, it is particularly preferable to use glycerin and polyoxypropylene (n) polyglyceryl ether (n=8 to 15) as the organic solvent (f3), as these have excellent setting properties for printed matter and are effective in preventing drying and solidification of the ink at the ink ejection orifices.

[0093] [ka]

[0094] In the general formula (1) and the general formula (2), m, n, o and p each independently represent an integer of 1 to 10.

[0095] The organic solvent (F) is preferably used in the range of 0.5% by mass to 30% by mass relative to the total amount of the aqueous pigment dispersion, and it is particularly preferable to use it in the range of 5% by mass to 20% by mass, since this prevents the aqueous ink obtained from the aqueous pigment dispersion from becoming insufficient in image density and also prevents a decrease in the dispersion stability of the pigment.

[0096] (Method of manufacturing water-based ink and method of designing water-based ink) The method for producing an aqueous ink of the present invention includes a step of producing an aqueous pigment dispersion and a mixing step, and further includes other steps as necessary. The method for designing an aqueous ink of the present invention includes a step of designing an aqueous pigment dispersion and a step of determining the composition ratio, and further includes other steps as necessary. The step of producing an aqueous pigment dispersion is a step of producing an aqueous pigment dispersion by the method for producing an aqueous pigment dispersion of the present invention. The step of designing an aqueous pigment dispersion is a step of designing an aqueous pigment dispersion by the method of designing an aqueous pigment dispersion of the present invention.

[0097] <Mixing process> The mixing step is not particularly limited as long as it is a step of mixing an aqueous pigment dispersion, a binder resin, and a third aqueous medium, and a mixing method typically used in producing aqueous inks can be used.

[0098] <Step of determining composition ratio> The step of determining the composition ratio is not particularly limited, so long as it is a step of determining the composition ratio of the designed aqueous pigment dispersion, binder resin, and third aqueous medium.

[0099] <Water-based ink> The aqueous ink produced in the present invention contains the aqueous pigment dispersion produced by the method for producing an aqueous pigment dispersion of the present invention, a binder resin, and a third aqueous medium. The water-based ink may further contain additives.

[0100] <<Binder resin>> The binder resin (A) is, for example, for fixing the pigment onto the recording medium.

[0101] Examples of the binder resin (A) include urethane resins, polyvinyl alcohols, polyvinylpyrrolidones, polyacrylic acids; acrylic acid-acrylonitrile copolymers, potassium acrylate-acrylonitrile copolymers, vinyl acetate-acrylic acid ester copolymers, acrylic acid-acrylic acid alkyl ester copolymers, and other acrylic copolymers; styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-methacrylic acid-acrylic acid alkyl ester copolymers, styrene-α-methylstyrene-acrylic acid copolymers, styrene-α-methylstyrene-acrylic acid-acrylic acid alkyl ester copolymers, and other styrene-acrylic acid resins; styrene-maleic acid; styrene-maleic anhydride; vinyl naphthalene-acrylic acid copolymers; vinyl naphthalene-maleic acid copolymers; vinyl acetate-ethylene copolymers, vinyl acetate-fatty acid vinyl ethylene copolymers, vinyl acetate-maleic acid ester copolymers, vinyl acetate-crotonic acid copolymers, vinyl acetate-acrylic acid copolymers, and other vinyl acetate-based copolymers and salts thereof can be used.

[0102] Among these, it is preferable to use a urethane resin or an acrylic resin as the binder resin, since these are easily available and improve the abrasion resistance of the printed matter.

[0103] Examples of the urethane resin include urethane resins obtained by reacting one or more polyols selected from the group consisting of polyether polyols, polyester polyols, and polycarbonate polyols, a polyol having a hydrophilic group that is an anionic group, a cationic group, a polyoxyethylene group, or a polyoxyethylene-polyoxypropylene group, and a polyisocyanate.

[0104] The weight average molecular weight of the urethane resin is not particularly limited, but in order to further improve the abrasion resistance of the printed matter, it is preferable to use one having a weight average molecular weight of 5,000 to 200,000, and more preferably 20,000 to 150,000.

[0105] A crosslinking agent can be used in the ink for the purpose of further improving the abrasion resistance. When a crosslinking agent is used, it is preferable to use a urethane resin having a functional group capable of undergoing a crosslinking reaction with the functional group of the crosslinking agent.

[0106] Examples of the functional group include a carboxyl group, a carboxylate group, etc. that can be used as a hydrophilic group. The carboxyl group etc. contributes to the aqueous dispersion stability of the urethane resin in an aqueous medium, and when they undergo a crosslinking reaction, they also act as a functional group and can partially crosslink with the crosslinking agent.

[0107] Examples of the crosslinking agent that can be used include polyisocyanate crosslinking agents, epoxy crosslinking agents, and melamine crosslinking agents. These crosslinking agents may be used alone or in combination of two or more. Among these, it is preferable to use a polyisocyanate crosslinking agent, since it reacts with the hydroxyl group of the urethane resin to form a three-dimensional crosslink, thereby obtaining good mechanical strength, step-following ability, substrate adhesion, sheet retention, and stain resistance.

[0108] The amount of crosslinking agent used is preferably in the range of 0.01 to 20 parts by mass, more preferably 0.05 to 15 parts by mass, and even more preferably 0.1 to 10 parts by mass, per 100 parts by mass of urethane resin (solid content), in order to achieve high levels of conformability to unevenness, adhesion to substrate, and sheet retention.

[0109] The urethane resin can be produced, for example, by reacting a polyol with a polyisocyanate and, if necessary, with a chain extender.

[0110] As the chain extender, polyamines and other compounds containing active hydrogen atoms can be used.

[0111] The chain extender is preferably used in an amount such that the equivalent of the amino group and active hydrogen atom-containing group in the chain extender is 1.9 or less (equivalent ratio) relative to the equivalent of the isocyanate group in the urethane prepolymer obtained by reacting a polyol with a polyisocyanate, more preferably in the range of 0.0 to 1.0 (equivalent ratio), and even more preferably at 0.5 mass%.

[0112] The chain extender can be used during or after the reaction of the polyol with the polyisocyanate, or when the resulting urethane resin is dispersed in an aqueous medium to make it aqueous.

[0113] The acrylic resin usable for the binder resin (A) is not particularly limited, and examples thereof include a homopolymer or copolymer of (meth)acrylate, and a resin copolymerized with a vinyl monomer copolymerizable with (meth)acrylate. In the present invention, "(meth)acrylic acid" refers to methacrylic acid or acrylic acid, "(meth)acrylate" refers to methacrylate or acrylate, and "(meth)acryloyl" refers to methacryloyl or acryloyl.

[0114] Examples of (meth)acrylates and vinyl monomers copolymerizable with (meth)acrylates include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, isopropyl (meth)acrylate, and isobutyl (meth)acrylate; aromatic (meth)acrylates such as benzyl (meth)acrylate; and hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate. Monomers; alkyl polyalkylene glycol mono(meth)acrylates such as methoxy polyethylene glycol mono(meth)acrylate and methoxy polypropylene glycol mono(meth)acrylate; fluorine-based (meth)acrylates such as perfluoroalkylethyl (meth)acrylate; styrene, styrene derivatives (p-dimethylsilylstyrene, (p-vinylphenyl)methylsulfide, p-hexynylstyrene, p-methoxystyrene, p-tert-butyldimethylsiloxystyrene, o-methylstyrene, p-methylstyrene, p-tert-butyldimethylsiloxystyrene, t-butylstyrene, α-methylstyrene, etc.), aromatic vinyl compounds such as vinyl naphthalene, vinyl anthracene, 1,1-diphenylethylene; glycidyl (meth)acrylate, epoxy (meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylene glycol tetra(meth)acrylate, 2-hydroxy-1,3-diacryloxypropane, 2,2-bis[4-(acryloxymethoxy)phenyl]propane, 2,2-bi (Meth)acrylate compounds such as tris[4-(acryloxyethoxy)phenyl]propane, dicyclopentenyl (meth)acrylate, tricyclodecanyl (meth)acrylate, tris(acryloxyethyl)isocyanurate, and urethane (meth)acrylate; (meth)acrylates having an alkylamino group such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminopropyl (meth)acrylate; vinylpyridine compounds such as 2-vinylpyridine, 4-vinylpyridine, and naphthylvinylpyridine;Conjugated dienes such as 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, and 1,3-cyclohexadiene can be used. These monomers can be used alone or in combination of two or more.

[0115] It is preferable to use an acrylic resin obtained by copolymerizing a monomer having a specific functional group in addition to the above-mentioned monomers in order to improve the texture of the printed matter, etc. Examples of the monomer having such a functional group include a monomer having a carboxyl group, a monomer having an epoxy group, a monomer having a hydrolyzable silyl group, and a monomer having an amide group.

[0116] Examples of monomers having a carboxyl group that can be used include (meth)acrylic acid, itaconic acid, crotonic acid, fumaric acid, maleic anhydride, and citraconic acid.

[0117] Examples of monomers having a hydrolyzable silyl group include vinyl silane compounds such as vinyl methyl dimethoxy silane, vinyl trimethoxy silane, vinyl triethoxy silane, and vinyl tris (2-methoxy ethoxy) silane; and (meth) acryloyloxy alkyl silane compounds such as 3- (meth) acryloyloxy propyl trimethoxy silane, 3- (meth) acryloyloxy propyl methyl dimethoxy silane, 3- (meth) acryloyloxy propyl triethoxy silane, and 3- (meth) acryloyloxy propyl methyl diethoxy silane. These monomers can be used alone or in combination of two or more.

[0118] Examples of the monomer having an amide group that can be used include acrylamide compounds such as (meth)acrylamide, N,N-dimethylacrylamide, isopropylacrylamide, and diacetoneacrylamide.

[0119] The dispersion form of the acrylic resin in water is not particularly limited, and examples thereof include emulsions forcibly emulsified with an emulsifier, and dispersions having nonionic groups or neutralized ionic groups in the resin. In particular, the above-mentioned acrylic resin is preferably a dispersion obtained by neutralizing an acrylic resin having a carboxyl group with a basic compound. The basic compound can be the same as the basic compound exemplified as one that can be used for neutralizing the carboxyl group of the urethane resin.

[0120] <<Aqueous medium>> The third aqueous medium may be the aqueous medium mentioned in the description of the aqueous pigment dispersion.

[0121] The third aqueous medium is preferably used in the range of 1% by mass to 50% by mass relative to the total amount of the ink, and is particularly preferably used in the range of 10% by mass to 30% by mass in order to obtain an ink that has the high ejection stability required when ejected by an inkjet method and can produce clear printed matter.

[0122] The organic solvent (F) is preferably used in the range of 1% by mass to 30% by mass based on the total amount of the ink, and it is particularly preferable to use it in the range of 5% by mass to 25% by mass, in order to achieve excellent setting properties of the printed matter and to prevent drying and solidification of the ink at the ink ejection orifices.

[0123] The water-soluble organic solvent (f1), propylene glycol (f2) and organic solvent (f3) are preferably used in such a manner that the mass ratio thereof [water-soluble solvent (f1) / propylene glycol (f2)] is in the range of 1 / 25 to 1 / 1, and it is particularly preferable to use them in the range of 1 / 20 to 1 / 1 in order to provide excellent setting properties for printed matter and to prevent drying and solidification of the ink at the ink ejection orifices.

[0124] The water-soluble organic solvent (f1), propylene glycol (f2), and organic solvent (f3) are preferably used in such a manner that the mass ratio thereof [propylene glycol (f2) / organic solvent (f3)] is in the range of 1 / 4 to 8 / 1, and it is particularly preferable to use them in the range of 1 / 2 to 5 / 1 in order to provide excellent setting properties for printed matter and to prevent drying and solidification of the ink at the ink ejection orifices.

[0125] <<Additives>> Examples of the additives include surfactants (E), sugars, preservatives, viscosity adjusters, pH adjusters, chelating agents, antioxidants, and ultraviolet absorbers.

[0126] The surfactant (E) can be used to improve the leveling properties of the ink by reducing the surface tension of the ink, etc. Furthermore, the surfactant (E) can prevent the occurrence of streaks in printed matter by allowing the ink discharged from the discharge port of the inkjet head to smoothly wet and spread on the surface after landing on a recording medium.

[0127] As the surfactant (E), various anionic surfactants, nonionic surfactants, cationic surfactants, amphoteric surfactants, etc. can be used, and it is preferable to use an anionic surfactant or a nonionic surfactant.

[0128] As the surfactant (E), it is preferable to use one having an HLB value in the range of 4 to 20 in order to stably maintain the state in which the surfactant (E) is dissolved in the ink containing water as the main solvent.

[0129] The surfactant (E) is preferably used in the range of 0.001% by mass to 2% by mass, more preferably in the range of 0.001% by mass to 1.5% by mass, and even more preferably in the range of 0.5% by mass to 1.5% by mass, based on the total amount of the ink. An ink-jet ink containing the surfactant (E) in the above range has good wettability of the discharged droplets on the surface of a recording medium, has sufficient wet spread on the recording medium, and is preferable in terms of preventing the occurrence of streaks in printed matter. Furthermore, an ink containing the surfactant (E) in the above range has the effect of improving wettability and leveling properties on a recording medium.

[0130] The pH of the aqueous ink is preferably 7.0 or more, more preferably 7.5 or more, and even more preferably 8.0 or more, in order to improve the storage stability and ejection stability of the ink, and to improve the wet spread, print density, and waterfastness when printed on a fabric that is easily or poorly ink-absorbent. The upper limit of the pH of the ink is preferably 11.0 or less, more preferably 10.0 or less, and even more preferably 9.5 or less, in order to suppress deterioration of the members (e.g., ink ejection port, ink flow path, etc.) constituting the ink application or ejection device and to reduce the effects of the ink adhering to the skin. EXAMPLES

[0131] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0132] (Preparation of Pigment Dispersion for Evaluation) The following raw materials were used to prepare pigment dispersions for evaluation:

[0133] <Ingredients> Pigment: Mitsubishi Carbon Black "#960" (product name, Mitsubishi Chemical Corporation) Pigment dispersant: Polyvinylpyrrolidone (PVP) "K-30" (product name, manufactured by Nippon Shokubai Co., Ltd.) Aqueous medium: "Ion-exchanged water"

[0134] The above pigment, pigment dispersant, and aqueous medium were mixed in the formulation shown in Table 2 below, and then dispersed to obtain a pigment dispersion for evaluation. Specifically, a 50 mL polyethylene sealed container was charged with a given amount of pigment, pigment dispersant, and aqueous medium according to the blending composition (g) in Table 2, and then 10 g of 0.5 mm diameter Zr beads YTZ-0.5 (product name, manufactured by Nikkato Corporation) was added and dispersed using a paint conditioner. The dispersion time was uniformly set to 2 hours. The numerical values ​​for the blend composition (g) in Table 2 are the actual amounts (g) charged. The total amount of materials for No.1-1 to No.1-9 (pigment concentration 10% by mass) is 10.00g. The total amount of materials for No.2-1 to No.2-9 (pigment concentration 15% by mass) is 6.67g. The total amount of materials for No.3-1 to No.3-9 (pigment concentration 20% by mass) is 5.00g.

[0135] (Measurement of volume average particle size) The volume average particle size of the obtained pigment dispersion for evaluation was measured by the following method, and the results are shown in Table 2. Measurement device: Microtrac MT3000II (Microtrac Bell) Measurement solvent: Water Solvent refractive index: 1.333 Presence ratio: Volume basis ·Particle permeability: Transmission ·Particle shape: non-spherical Particle refractive index: 1.81 Analysis mode: Rosin-Rammler distribution (±2σ) (Software included with the device: DMS ver.11.0.0-246V)

[0136] <Calculation of total surface area (TSA) of particles> Using the volume average particle diameter thus obtained, the total surface area (TSA) of the particles was calculated according to the following formula (2). The results are shown in Table 2.

number

number

[0137] Pulsed NMR measurements and R sp Calculation of > The obtained pigment dispersion for evaluation was subjected to pulse NMR measurement under the following conditions. sp The results are shown in Table 2.

[0138] <<Pulse NMR measurement conditions>> Measurement equipment: Acron Area (manufactured by XiGo Nanotools) Pulse sequence: CPMG method ·Resonance frequency: 13MHz ·Measurement temperature: 30℃ Measurement sample: 1.0 cm 3

[0139]

number

[0140] In addition, the dispersibility index K, which is an index of the thickness of the hydration layer, is calculated by the following formula: a The results are shown in Table 2.

number

[0141] [Table 2]

[0142] For each pigment concentration, R sp A graph was created with the horizontal axis representing β and the vertical axis representing TSA, and is shown in Figure 1. From the results in Table 2 and Figure 1, at a pigment concentration of 10% by mass, TSA showed a maximum value when the composition mass ratio (R / P) was 0.3. At a pigment concentration of 15% by mass, TSA showed a maximum value when the composition mass ratio (R / P) was 0.3. At a pigment concentration of 20% by mass, TSA showed a maximum value when the composition mass ratio (R / P) was 0.4.

[0143] On the other hand, for each pigment concentration, K a A graph was created with the horizontal axis representing β and the vertical axis representing TSA, and is shown in Figure 2. In Figure 2, no mountain-shaped curve was obtained as in Figure 1. This confirmed that it is appropriate to use the index of hydrophilicity and the index of the total surface area of ​​the particles when determining the composition mass ratio.

[0144] <Evaluation of pigment dispersion stability> The pigment dispersion stability of the evaluation dispersion was evaluated by the following evaluation method, and the results are shown in Table 3. The test sample was sealed in a polyethylene container and stored in an atmosphere at 60°C for 30 days, and the average particle size (D50) before and after storage was measured according to the following average particle size measurement method. Similarly, the viscosity of the evaluation dispersion before and after storage was measured according to the following viscosity measurement method.

[0145] The viscosity was measured (sample temperature 25° C.) using a Viscometer TV-20 (manufactured by Toki Sangyo Co., Ltd.). Measurements were performed (sample temperature 25° C.) using a dynamic light scattering Nanotrac particle size analyzer UPA-150EX (manufactured by Nikkiso Co., Ltd.) The particle size values ​​used were the volume average particle size (Mv) and the 50% particle size (D50).

[0146] The change in viscosity was calculated using the following formula: Ratio of change before and after storage (= (measured value after storage) / (measured value before storage) x 100(%))

[0147] The evaluation was performed according to the following criteria, and the results are shown in Table 3. <<Evaluation criteria>> ·Good: The change in average particle size (D50) and viscosity before and after storage is less than 20% ×: At least one of the average particle size (D50) and viscosity before and after storage changed by 20% or more.

[0148] [Table 3]

[0149] (Hansen solubility parameters) The Hansen solubility parameters of the following materials were determined using the method described herein, and the results are shown in Table 4. <Material> Pigment: Mitsubishi Carbon Black "#960" (product name, Mitsubishi Chemical Corporation) Pigment: Mitsubishi Carbon Black R (product name, Mitsubishi Chemical Corporation) Pigment dispersant: Polyvinylpyrrolidone (PVP) "K-30" (product name, manufactured by Nippon Shokubai Co., Ltd.) Pigment dispersant: Acrydic WML542 (product name, DIC Corporation, styrene acrylic resin, acid value = 170 mg KOH / g) Pigment dispersant: ARFON UH-2170 (product name, Toagosei Co., Ltd.)

[0150] [Table 4]

[0151] (Preparation of aqueous pigment dispersion 1) An aqueous pigment dispersion was prepared using the following raw materials:

[0152] <Ingredients> Pigment: Mitsubishi Carbon Black "#960" (product name, Mitsubishi Chemical Corporation) Pigment dispersant: Acrydic WML542 (product name, DIC Corporation, styrene acrylic resin, acid value = 170 mgKOH / g) theoretical value 100% neutralized (neutralizing agent: potassium hydroxide) Aqueous medium: "Ion-exchanged water"

[0153] The above pigment, pigment dispersant, and aqueous medium were mixed in the formulation shown in Table 5 below, and then dispersed to obtain an aqueous pigment dispersion. Specifically, a 50 mL polyethylene sealed container was charged with a given amount of pigment, pigment dispersant, and aqueous medium according to the blending composition (g) in Table 5, and then 10 g of Zr beads YTZ-0.5 (product name, manufactured by Nikkato Corporation) with a diameter of 0.5 mm was further added and dispersed using a paint conditioner. The dispersion time was uniformly set to 2 hours.

[0154] The volume average particle size and pigment dispersion stability of the resulting aqueous pigment dispersion were evaluated by the methods described above. The results are shown in Table 5.

[0155] [Table 5]

[0156] From Tables 2, 3, and Fig. 1, when the pigment concentration is 20.0 mass%, the optimum range of the mass ratio (R / P) is 0.4. Therefore, the preferable range of the mass ratio (R / P) in the aqueous pigment dispersion prepared above is 0.2 to 0.6. The results in Table 5 correspond to these results.

[0157] (Preparation of aqueous pigment dispersion 2) An attempt was made to prepare an aqueous pigment dispersion using the following raw materials in the same manner as in Preparation 1 of aqueous pigment dispersion, but no dispersion was obtained due to poor dispersion.

[0158] <Ingredients> Pigment: Mitsubishi Carbon Black R (product name, Mitsubishi Chemical Corporation) Pigment dispersant: ARFON UH-2170 (product name, Toagosei Co., Ltd.) Aqueous medium: "Ion-exchanged water"

Claims

1. A method for producing an aqueous pigment dispersion containing a second pigment, a second pigment dispersant, and a second aqueous medium, comprising the steps of: preparing a plurality of evaluation dispersions each containing a first pigment, polyvinylpyrrolidone as a first pigment dispersant, and a first aqueous medium, the dispersions having different composition ratios of the first pigment dispersant to the first pigment; determining a T2 relaxation time for each of the plurality of evaluation dispersions by pulse NMR measurement, and obtaining an index of hydrophilicity based on the reciprocal of the T2 relaxation time; measuring the volume average particle size of the particles for each of the plurality of evaluation dispersions to obtain an index of the total surface area of ​​the particles; determining, as a composition mass ratio of the second pigment dispersant to the second pigment in the aqueous pigment dispersion, a range of ±0.2 or less of a composition mass ratio (R / P) of the first pigment dispersant to the first pigment when the index of the total surface area of ​​the particles takes a maximum value in a graph showing the relationship between the index of the hydrophilicity degree, the index of the total surface area of ​​the particles, and the composition ratio, with the index of the hydrophilicity degree being plotted on the horizontal axis and the index of the total surface area of ​​the particles being plotted on the vertical axis; mixing the second pigment, the second pigment dispersant, and the second aqueous medium in accordance with the determined composition mass ratio; Including, The Hansen solubility parameter of the second pigment is within ±3 (J / cm) of the Hansen solubility parameter of the first pigment. 3 ) 1/2 is as follows: The Hansen solubility parameter of the second pigment dispersant is within ±5 (J / cm) of the Hansen solubility parameter of the first pigment dispersant. 3 ) 1/2 is as follows: The Hansen solubility parameter of the second aqueous medium is within ±3 (J / cm) of the Hansen solubility parameter of the first aqueous medium. 3 ) 1/2 is as follows: the second pigment dispersant is different from the first pigment dispersant, The second aqueous medium and the first aqueous medium are the same; A method for producing an aqueous pigment dispersion comprising the steps of:

2. The step of obtaining an index of hydrophilicity includes determining a T2 relaxation time by the pulse NMR measurement for a blank solution having the same composition ratio of the first pigment dispersant and the first aqueous medium in one of the plurality of evaluation dispersions and not containing the first pigment, and calculating an index of hydrophilicity (R sp ) for each of the plurality of dispersions for evaluation, A method for producing the aqueous pigment dispersion according to claim 1. [0010] In the formula (1), R av represents the reciprocal of the T2 relaxation time of the one aqueous dispersion for evaluation, R b represents the inverse of the T2 relaxation time of the blank solution.

3. 3. The method for producing an aqueous pigment dispersion according to claim 1, wherein the index of the total surface area of ​​the particles is a value that is directly proportional to the reciprocal of the volume average particle size of the particles.

4. the step of obtaining an index of the total surface area of ​​the particles includes a process of obtaining a total particle surface area value (TSA), which is an index of the total surface area of ​​the particles, from the volume average particle size of the particles by the following formula (2), for each of the plurality of evaluation dispersions; A method for producing the aqueous pigment dispersion according to any one of claims 1 to 3. [0025] In the formula (2), M v represents the volume average particle size of the particles. In the formula (2), Ψ p means a particle volume ratio and is expressed by the following formula (3). [0030] In the formula (2) and the formula (3), ρ p represents the density of the first pigment. In the formula (3), C p represents the concentration of the first pigment in the evaluation dispersion. In the above formula (3), ρ w represents the density of the first aqueous medium.

5. A step of producing an aqueous pigment dispersion by the method for producing an aqueous pigment dispersion according to any one of claims 1 to 4; mixing the aqueous pigment dispersion, a binder resin, and a third aqueous medium; A method for producing an aqueous ink, comprising:

6. A method for designing an aqueous pigment dispersion, the method comprising determining a composition ratio of a second pigment, a second pigment dispersant, and a second aqueous medium in an aqueous pigment dispersion containing the second pigment, the second pigment dispersant, and the second aqueous medium, the method comprising the steps of: preparing a plurality of evaluation dispersions each containing a first pigment, polyvinylpyrrolidone as a first pigment dispersant, and a first aqueous medium, the dispersions having different composition ratios of the first pigment dispersant to the first pigment; determining a T2 relaxation time for each of the plurality of evaluation dispersions by pulse NMR measurement, and obtaining an index of hydrophilicity based on the reciprocal of the T2 relaxation time; measuring the volume average particle size of the particles for each of the plurality of evaluation dispersions to obtain an index of the total surface area of ​​the particles; a first step of determining, as a composition mass ratio of the second pigment dispersant to the second pigment in the aqueous pigment dispersion, a range of ±0.2 or less of a composition mass ratio (R / P) of the first pigment dispersant to the first pigment when the index of the total surface area of ​​the particles takes a maximum value in a graph showing the relationship between the index of the hydrophilicity degree, the index of the total surface area of ​​the particles, and the composition ratio, with the index of the hydrophilicity degree being plotted on the horizontal axis and the index of the total surface area of ​​the particles being plotted on the vertical axis; a second step of determining a composition ratio of the second pigment, the second pigment dispersant, and the second aqueous medium in the aqueous pigment dispersion according to the determined composition mass ratio; Including, The Hansen solubility parameter of the second pigment is within ±3 (J / cm) of the Hansen solubility parameter of the first pigment. 3 ) 1/2 is as follows: The Hansen solubility parameter of the second pigment dispersant is within ±5 (J / cm) of the Hansen solubility parameter of the first pigment dispersant. 3 ) 1/2 is as follows: The Hansen solubility parameter of the second aqueous medium is within ±3 (J / cm) of the Hansen solubility parameter of the first aqueous medium. 3 ) 1/2 is as follows: the second pigment dispersant is different from the first pigment dispersant, The second aqueous medium and the first aqueous medium are the same; A method for designing an aqueous pigment dispersion comprising the steps of:

7. A step of designing an aqueous pigment dispersion containing the second pigment, the second pigment dispersant, and the second aqueous medium by using the method for designing an aqueous pigment dispersion according to claim 6; determining a composition ratio of the designed aqueous pigment dispersion, a binder resin, and a third aqueous medium; A method for designing an aqueous ink, comprising:

Citation Information

Patent Citations

  • Hydrophilic coloring cellulose microparticles

    EP3608670A1

  • Method for estimating optimum amount of additive according to zeta potential

    JP2001303887A

  • Method for producing pigment dispersion, inkjet-recording ink, method of inkjet-recording, ink cartridge and inkjet-recording device

    JP2006328119A

  • Hydrophilic carbon black aqueous dispersion, hydrophilic carbon black aqueous dispersion and manufacturing method of hydrophilic carbon black aqueous dispersion

    JP2017141315A

  • Aqueous pigment dispersion and inkjet ink

    JP2017226760A