Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element using the same
A liquid crystal aligning agent with specific polymer and compound components addresses the issue of bright spots in liquid crystal display elements by enhancing alignment stability and reducing charge accumulation, ensuring high voltage retention.
Patent Information
- Application Number
- JP2021505114
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-12
- Filing Date
- 2020-03-11
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-03-11
AI Technical Summary
Existing liquid crystal display elements suffer from bright spots due to physical friction caused by spacers, which disrupt the alignment of liquid crystal molecules, leading to light leakage and reduced voltage holding rates.
A liquid crystal aligning agent containing specific components, including a polymer with certain repeating units and a compound with a molecular weight of 2000 or less and a basic site containing a nitrogen atom, is used to enhance the alignment stability and reduce friction-induced bright spots.
The solution maintains high voltage holding rates and minimizes bright spots in liquid crystal display elements, even under physical stress, by improving alignment and reducing accumulated charge.
Smart Images

Figure 0007552582000038 
Figure 0007552582000063 
Figure 0007552582000020
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal aligning agent, a liquid crystal alignment film, and a liquid crystal display element using the same. [Background technology]
[0002] Various driving methods have been developed for liquid crystal display elements, which differ in electrode structure, physical properties of the liquid crystal molecules used, manufacturing process, etc., and known liquid crystal display elements include the TN (twisted nematic) type, STN (super-twisted nematic) type, VA (vertical alignment) type, MVA (multi-domain vertical alignment) type, IPS (in-plane switching) type, FFS (fringe field switching) type, and PSA (polymer-sustained alignment) type. These liquid crystal display elements are provided with a liquid crystal alignment film to align the liquid crystal molecules. The material for the liquid crystal alignment film is generally a coating made of a polymer such as polyamic acid, polyimide, or polysiloxane, because these have various good properties such as heat resistance, mechanical strength, and affinity with liquid crystal.
[0003] In recent years, there has been an increasing demand for liquid crystal display elements with higher image quality. For example, liquid crystal display elements with less accumulated charge while maintaining a high voltage holding ratio are desired, and Patent Document 1 discloses a liquid crystal alignment agent containing a specific compound. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2008-052260 Summary of the Invention [Problem to be solved by the invention]
[0005] Furthermore, as so-called touch panel type liquid crystal display elements have become widespread, users often apply strong pressure to the display elements with their fingers. When this happens, the spacers present inside the liquid crystal display element move within the liquid crystal display element and rub against the liquid crystal alignment film. The liquid crystal alignment film stressed by the spacers is unable to regulate the alignment of the liquid crystals, and this causes a problem in that, even when the liquid crystal display element is displaying black, light escapes from the periphery of the spacers, resulting in bright spots.
[0006] The configurations of liquid crystal alignment agents proposed in the past could not necessarily achieve all of the above problems. The present invention has been made based on the above circumstances, and an object of the present invention is to provide a liquid crystal display element that maintains a high voltage holding ratio, has little accumulated charge, and can minimize bright spots even when physical friction occurs, such as rubbing with a spacer. Another object of the present invention is to provide a liquid crystal alignment film and a liquid crystal alignment agent suitable for such a liquid crystal display element. [Means for solving the problem]
[0007] The present inventors have conducted extensive research and found that the above problems can be solved by using a liquid crystal aligning agent containing a specific component, and have completed the present invention.
[0008] A liquid crystal aligning agent comprising the following components (A) and (B): Component (A): A polymer (A) having at least one repeating unit selected from the group consisting of a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2): Component (B): A compound (B) having a molecular weight of 2000 or less, which has a partial structure represented by the following formula (b) in the molecule and is equipped with a basic site containing a nitrogen atom. [ka] In formula (1), X1 is a tetravalent organic group, Y1 is a divalent organic group, R1 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, Z 11 , Z 12 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an alkenyl group having 2 to 10 carbon atoms which may have a substituent, an alkynyl group having 2 to 10 carbon atoms which may have a substituent, a tert-butoxycarbonyl group, or a 9-fluorenylmethoxycarbonyl group. [ka] * represents a bond, R1 represents an alkanediyl group having 1 to 4 carbon atoms, and m1 represents an integer of 1 or 2. Effect of the Invention
[0009] The liquid crystal aligning agent of the present invention provides a liquid crystal display element that maintains a high voltage retention rate while having little accumulated charge and that can minimize bright spots even when physical friction such as rubbing with a spacer occurs, and a liquid crystal alignment film that provides the liquid crystal display element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, each component contained in the liquid crystal aligning agent of the present disclosure and other components that are optionally blended as necessary will be described. <Polymer (A)> The liquid crystal aligning agent of the present invention contains a polymer (A) having at least one repeating unit selected from the group consisting of the repeating unit represented by the above formula (1) and the repeating unit represented by the above formula (2). Specific examples of the alkyl group having 1 to 5 carbon atoms for R1 in the above formula (2) include a methyl group, an ethyl group, a propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, an n-pentyl group, etc. From the viewpoint of ease of imidization by heating, R1 is preferably a hydrogen atom or a methyl group.
[0011] Z in the above formula (2) 11 , Z 12Specific examples of the alkyl group having 1 to 10 carbon atoms include, in addition to the specific examples of the alkyl group having 1 to 5 carbon atoms exemplified for R1 above, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, etc. 11 , Z 12 Specific examples of the alkenyl group having 2 to 10 carbon atoms include a vinyl group, a propenyl group, and a butynyl group, which may be linear or branched. 11 , Z 12 Specific examples of the alkynyl group having 2 to 10 carbon atoms include an ethynyl group, a 1-propynyl group, and a 2-propynyl group.
[0012] Above Z 11 , Z 12 may have a substituent, and examples of the substituent include a halogen atom (such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom), a hydroxyl group, a cyano group, and an alkoxy group.
[0013] In terms of reducing image retention, the above Z 11 , Z 12 It is preferable that each independently represents a hydrogen atom or a methyl group.
[0014] In the above formulas (1) and (2), X1 and Y1 are as defined above. X1 in formula (1) is a tetravalent organic group derived from at least one selected from the group consisting of tetracarboxylic dianhydrides, tetracarboxylic diesters, and tetracarboxylic diester dihalides (hereinafter, these are also collectively referred to as "tetracarboxylic acid derivatives"). Specific examples include tetravalent organic groups derived from aromatic tetracarboxylic dianhydrides, aliphatic tetracarboxylic dianhydrides, alicyclic tetracarboxylic dianhydrides, or tetracarboxylic diesters or tetracarboxylic diester dihalides thereof. Y1 in formula (1) is a divalent organic group derived from a diamine.
[0015] Here, the aromatic tetracarboxylic dianhydride is a compound having at least one carbon atom bonded to an aromatic ring. The acid free radicals obtained by intramolecular dehydration of four carboxyl groups, including the carboxyl group, It is a water. Aliphatic tetracarboxylic acid dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups bonded to a chain hydrocarbon structure. However, it is not necessary to be composed of only a chain hydrocarbon structure, and it may have an alicyclic structure or an aromatic ring structure as a part of it. Alicyclic tetracarboxylic acid dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups including at least one carboxyl group bonded to an alicyclic structure. However, none of these four carboxyl groups are bonded to an aromatic ring. It is not necessary to be composed of only an alicyclic structure, and it may have a chain hydrocarbon structure or an aromatic ring structure as a part of it.
[0016] From the viewpoint of obtaining a high voltage holding ratio and suppressing bright spots caused by physical friction, X1 is preferably a tetravalent organic group selected from the group consisting of the following formulae (4a) to (4n), (5a) and (6a): [ka] x and y are a single bond, an ether, a carbonyl, an ester, an alkanediyl group having 1 to 5 carbon atoms, 1,4-phenylene, a sulfonyl or an amide group. 1 ~Z 6 each independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a benzene ring. j and k are 0 or 1. m is an integer of 1 to 5. * represents a bond.
[0017] From the viewpoint of obtaining a high voltage holding ratio and suppressing bright spots caused by physical friction, preferred specific examples of the above formula (4a) include structures represented by the following formulas (4a-1) to (4a-4). [ka]
[0018] Examples of the alkanediyl group having 1 to 5 carbon atoms in the above formulas (5a) and (6a) include methylene, ethylene, 1,3-propanediyl, 1,4-butanediyl, and 1,5-pentanediyl.
[0019] From the viewpoint of obtaining a high voltage holding ratio and suppressing bright spots caused by physical friction, X1 in the above formula (1) may be a tetravalent organic group selected from the above formulas (4a) to (4h), (4j), (4l), and (4m) to (4n).
[0020] From the viewpoint of obtaining a high voltage holding ratio and suppressing bright spots caused by physical friction, the content of one or more repeating units selected from the group consisting of repeating units represented by formula (1) and repeating units represented by formula (2), in which X1 is a tetravalent organic group selected from the group consisting of formulas (4a) to (4n), (5a), and formula (6a), and Y1 is a divalent organic group (hereinafter also referred to as repeating units (t)), may be 5 mol % or more, 10 mol % or more, or 20 mol % or more in total, based on all repeating units of polymer (A).
[0021] Examples of Y1 in formula (1) include divalent organic groups derived from diamines, such as divalent organic groups derived from aliphatic diamines, alicyclic diamines, or aromatic diamines. Specific examples of aliphatic diamines include metaxylylenediamine, ethylenediamine, 1,3-propanediamine, tetramethylenediamine, and hexamethylenediamine; alicyclic diamines include 1,4-cyclohexanediamine and 4,4'-methylenebis(cyclohexylamine);
[0022] Examples of aromatic diamines include p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminobenzophenone, 4,4'-diaminodiphenyl ether, 4,4'-diaminoazobenzene, 1-(4-aminophenyl)-1,3,3-trimethyl-1H-indan-5-amine, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-inden-6-amine, nitrogen-containing heterocycles, diphenylamine structures, and triphenylamine structures. Diamines having at least one selected from the group consisting of diphenylamine structures and triphenylamine structures (hereinafter also referred to as "nitrogen-containing diamines"). 3,5-diaminobenzoic acid, 2,2'-dimethyl-4,4'-diaminobiphenyl, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]ether, 4,4'-bis(4- (aminophenoxy)biphenyl, 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, diamines represented by the following formula (H), diamines represented by the following formulas (H2) to (H3), diamines represented by the following formulas (V-1) to (V-3), diamines having a radical initiating function represented by the following formulas (R1) to (R5), 2-(2,4-diaminophenoxy)ethyl methacrylate, 2,4-diamino-N,N-diallylaniline, etc. Examples of the diamine having a photopolymerizable group at an end include the diamine having a photoalignment structure described in paragraph
[0053] of International Publication WO2014 / 080865, the diamine having a carbon-carbon unsaturated bond described in paragraph
[0057] , the diamine having an azobenzene skeleton described in paragraph
[0058] , and the diamine having photoreactivity described in paragraphs
[0069] to
[0072] of International Publication WO2012 / 086715. [ka] R 3 are -NRCO-, -COO-, -NRCONR-, -(CH2) n- (wherein n is an integer of 2 to 20), and any -CH2- may be replaced with -O-, -COO-, -ND-, -NRCO-, -NRCONR-, -NRCOO-, or -OCOO-. D represents a thermally detachable group, and R represents a hydrogen atom or a monovalent organic group. R 4 is a single bond or a benzene ring, and any hydrogen atom on the benzene ring may be replaced with a monovalent organic group. [ka] X1 is -CO-, -O-, -COO-, -L1-R-L2- (L1 and L2 are each independently a single bond, an oxygen atom, or -COO-, and R is -(CH2) n -(n is an integer of 1 to 12). ) or -NRCO-(R represents a hydrogen atom or a methyl group), and X2 represents a single bond, -NRCO-(R represents a hydrogen atom or a methyl group), or -COO-. n represents an integer of 1 to 2. Any hydrogen atom on the benzene ring may be replaced with a monovalent organic group. [ka] In the formula, each of the two Xs independently represents -O-, -COO-, -NHCO-, -C(=O)-, or -(CH2) n -(n is an integer of 1 to 12), L1 and L2 each independently represent a single bond, -O- or -COO-, and R represents -CH2- or -(CH2) n -(n is an integer of 2 to 12), or the above -(CH2) n - represents a group in which any CH2 in - is replaced with an oxygen atom. Any hydrogen atom on the benzene ring may be replaced with a monovalent organic group.
[0023] [ka] X is a single bond, -O-, -C(CH3)2-, -NH-, -CO-, -NHCO-, -COO-, -(CH2) m -, -SO2-, -O-(CH2) m -O-, -OC(CH3)2-, -CO-(CH2) m-, -NH-(CH2) m -, -SO2-(CH2) m -, -CONH-(CH2) m -, -CONH-(CH2) m -NHCO- or -COO-(CH2) m Represents -OCO-. X 1 and X 2 are each independently a single bond, -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -COO-, -OCO- or -((CH2) a1 -A1) m1 In this formula, each of the multiple a1's independently represents an integer of 1 to 15, each of the multiple A1's independently represents an oxygen atom or -COO-, and m1 is 1 to 2. X 3 represents a single bond, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -COO- or -OCO-. X 4 represents -CONH-, -NHCO-, -O-, -COO- or -OCO-. G1 and G2 each independently represent a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms, such as phenylene, biphenylene, and naphthalene, or a divalent alicyclic group having 3 to 8 carbon atoms, such as cyclopropylene and cyclohexylene. Any hydrogen atom on the cyclic group may be substituted with an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorine-containing alkyl group having 1 to 3 carbon atoms, a fluorine-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. k represents 0 or 1, m and n each independently represent an integer of 0 to 3, and the sum of m and n is 1 to 4. R 1 R represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms. 1 Any hydrogen in the formula may be replaced by fluorine. R 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms; R 2Any hydrogen atom in the group R may be replaced by fluorine. 3 represents a structure having a steroid skeleton.
[0024] [ka] n represents an integer of 2 to 10.
[0025] Specific examples of the nitrogen-containing heterocycle include pyrrole, imidazole, pyridine, pyrimidine, pyridazine, pyrazine, carbazole, benzimidazole, piperidine, piperazine, pyrrolidine, and hexamethyleneimine. Examples of the diphenylamine structure include diphenylamine, N-methyldiphenylamine, and N-tert-butoxycarbonyldiphenylamine. Specific examples of the nitrogen-containing diamine include 2,6-diaminopyridine, 3,4-diaminopyridine, 3,5-diamino-N-(pyridin-3-ylmethyl)benzamide, 2,4-diaminopyrimidine, 3,6-diaminocarbazole, N-methyl-3,6-diaminocarbazole, bis(4-aminophenyl)amine, N,N-bis(4-aminophenyl)methylamine, N,N'-bis(4-aminophenyl)-benzidine, N,N'-bis(4-aminophenyl)-N,N'-dimethylbenzidine, 1,4-bis(4-aminophenyl)-piperazine, 4-(4-aminophenoxycarbonyl)-1-(4-aminophenyl)piperidine, 4,4'-[4,4'-propane-1,3-diylbis(piperidine-1,4-diyl)]dianiline, and diamines represented by the following formulas (z-1) to (z-19).
[0026] [ka] [ka] Boc represents a tert-butoxycarbonyl group.
[0027] In the above formulae (H), (H2) and (H3), the hydrogen atom on the benzene ring may be replaced by a monovalent organic group such as an alkyl group having 1 to 5 carbon atoms, such as a methyl group or an ethyl group, an alkoxy group having 1 to 5 carbon atoms, such as a methoxy group, a halogen atom, such as a fluorine atom, a halogenated alkyl group having 1 to 5 carbon atoms, such as a trifluoromethyl group, -NR1R2 (R1 and R2 respectively represent a hydrogen atom, a methyl group or a tert-butoxycarbonyl group), a cyano group or a hydroxy group.
[0028] From the viewpoint of enhancing the liquid crystal alignment property, among the diamines represented by the above formula (H), diamines represented by the following formulas (H-1) to (H-17) may be used. [ka] [ka] (R represents a hydrogen atom, a methyl group, or a tert-butoxycarbonyl group. Boc represents a tert-butoxycarbonyl group.)
[0029] From the viewpoint of enhancing the liquid crystal alignment property, diamines represented by the following formulas (H2-1) to (H2-17) may be used among the diamines represented by the above formula (H2). [ka] [ka] R represents a hydrogen atom, a methyl group, or a tert-butoxycarbonyl group. * represents a bond. Boc represents a tert-butoxycarbonyl group.
[0030] From the viewpoint of enhancing the liquid crystal alignment property, among the diamines represented by the above formula (H3), diamines represented by the following formulas (H3-1) to (H3-4) may be used. [ka]
[0031] From the viewpoint of enhancing the liquid crystal alignment property, diamines represented by the following formulae (V2-1) to (V2-13) may be used among the diamines (V-1) to (V-3). [ka] [ka] In the formula, X v1 ~X v4 , X p1 ~X p8 Each of is independently -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -CHOCO-, -COO-, or -OCO-; X v5 represents -O-, -CH2O-, -CH2OCO-, -COO-, or -OCO-; X V6 ~X V7 , X s1 ~X s4 Each independently represents -O-, -COO- or -OCO-. X a ~X f is a single bond, -O-, -NH-, or -O-(CH2) m -O-, R v1 ~R v4 , R 1a ~R 1h each independently represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms. m represents an integer of 1 to 8.
[0032] When applied as a liquid crystal aligning agent for TN-type, STN-type or vertical alignment-type liquid crystal display elements, from the viewpoint of enhancing liquid crystal alignment, the polymer (A) may contain one or more repeating units (hereinafter also referred to as repeating units (a)) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), in which X1 is a tetravalent organic group and Y1 is a divalent organic group derived from a diamine represented by the above formulas (V1) to (V3). From the viewpoint of enhancing liquid crystal alignment, the content of the repeating units (a) may be 1 mol % or more, 3 mol % or more, or 5 mol % or more in total, based on the total repeating units of the polymer (A).
[0033] When applied to a liquid crystal alignment agent for a PSA-type liquid crystal display element, from the viewpoint of enhancing liquid crystal alignment, the polymer (A) may contain one or more repeating units (hereinafter also referred to as repeating units (b)) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), in which X1 is a tetravalent organic group and Y1 is a divalent organic group derived from a diamine selected from the group consisting of the diamine having the above radical initiation function and the diamine having the above photopolymerizable group at its terminal. From the viewpoint of enhancing liquid crystal alignment, the content of the repeating units (b) may be 1 mol% or more, 3 mol% or more, or 5 mol% or more in total, based on the total repeating units of the polymer (A). In this case, the polymer (A) may use one or more repeating units (a) in combination. The upper limit of the content of the repeating units (a) and (b) may be 99 mol% or less, 97 mol% or less, or 95 mol% or less, based on the total repeating units of the polymer (A). In this case, repeating units other than the repeating units (a) and (b) may be contained depending on the purpose.
[0034] When applied as a liquid crystal aligning agent for IPS-type or FFS-type liquid crystal display elements, from the viewpoint of enhancing liquid crystal alignment properties, the polymer (A) may contain one or more repeating units (hereinafter also referred to as repeating units (c)) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), in which X1 is a tetravalent organic group and Y1 is a divalent organic group derived from a diamine selected from the group consisting of p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 4,4'-diaminoazobenzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]ether, 4,4'-bis(4-aminophenoxy)biphenyl, diamines represented by the above formula (H), and diamines represented by the above formulas (H2) to (H3). From the viewpoint of improving the liquid crystal alignment property, the content of the repeating unit (c) may be 5 mol % or more, or 10 mol % or more in total, based on all the repeating units of the polymer (A).
[0035] When the coating film formed by the liquid crystal alignment agent is given liquid crystal alignment ability by a photoalignment method, the polymer (A) may contain one or more repeating units (hereinafter also referred to as repeating units (d)) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), in which X1 is a tetravalent organic group and Y1 is a divalent organic group derived from a diamine selected from the group consisting of the diamine having the above photoalignment structure, the diamine having the above carbon-carbon unsaturated bond, the diamine having the above azobenzene skeleton, and the diamine having photoreactivity. From the viewpoint of giving liquid crystal alignment ability, the content of the repeating units (d) may be 20 mol% or more, or 30 mol% or more in total, based on the total repeating units of the polymer (A). From the viewpoint of imparting liquid crystal alignment ability by a photoalignment method and maintaining a high voltage holding ratio, the polymer (A) may contain one or more repeating units (hereinafter also referred to as repeating units (e)) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), in which X1 is the above formulas (4a) to (4c), (4f) to (4g), and Y1 is a divalent organic group. The content of the repeating units (e) may be 5 mol % or more, or 10 mol % or more in total, based on the total repeating units of the polymer (A).
[0036] From the viewpoint of low accumulated charge, the polymer (A) may contain one or more repeating units (hereinafter also referred to as repeating units (n)) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), in which X1 is a tetravalent organic group and Y1 is a divalent organic group derived from a nitrogen-containing diamine. The content of the repeating units (n) may be 5 mol % or more, or 10 mol % or more in total, based on the total repeating units of the polymer (A).
[0037] The liquid crystal aligning agent of the present invention may contain one type of polymer (A) or may contain two or more types of polymer (A). Specific examples of the case where the polymer (A) is two or more types include an embodiment in which at least one type of polymer having the repeating unit (t) and any one of the repeating units (a) to (e) is contained, from the viewpoint of low accumulated charge and suppression of bright spots caused by physical friction. Also, an embodiment in which at least one type of polymer having the repeating unit (n) is contained, from the viewpoint of low accumulated charge. When the polymer (A) is composed of two types, the blending ratio of the first polymer and the second polymer ((first polymer) / (second polymer)) may be 5 / 95 to 95 / 5, 10 / 90 to 90 / 10, or 20 / 80 to 80 / 20 in mass ratio, from the viewpoint of improving the liquid crystal alignment property, low accumulated charge, and suppression of bright spots caused by physical friction.
[0038] <Compound (B)> The liquid crystal alignment agent of the present invention contains the compound (B). The compound (B) has a basic site containing a nitrogen atom in the molecule, which increases the imidization rate of the polymer (A) during baking, and the resulting liquid crystal alignment film has a high voltage retention rate. In addition, since the compound (B) has a methylol group in the molecule, a crosslinking reaction occurs between the polymer (A) and the compound (B) or between the compounds (B), which increases the film strength of the resulting liquid crystal alignment film. Therefore, the liquid crystal display element having the liquid crystal alignment film of the present invention can minimize bright spots even when physical friction occurs, such as rubbing with a spacer. In addition, the compound (B) has an effect of increasing the crosslink density of the liquid crystal alignment film, and therefore has excellent ability to capture impurity components derived from the substrate, and therefore the resulting liquid crystal alignment film has a high voltage retention rate. In addition, since the compound (B) has a phenylene site in the molecule, charge transfer in the liquid crystal alignment film is promoted, and a liquid crystal alignment film with less accumulated charge can be obtained.
[0039] The basic site means a site where the pKa of the conjugate acid is -3 or more. This pKa is preferably within the range of -3 to 15, and more preferably within the range of 0 to 15. This pKa means a calculated value obtained by ACD / ChemSketch (ACD / Labs 8.00 Release Product Version: 8.08). The basic site includes, for example, a structure selected from the group consisting of a secondary amine, a group in which one or two hydrogen atoms have been removed from a tertiary amine, and a nitrogen-containing heterocyclic group. Examples of the secondary amine or tertiary amine include an aliphatic amine and an aromatic amine. Examples of aromatic amines include a structure in which at least one aromatic ring such as a benzene ring is bonded to a nitrogen atom. The hydrogen atom on the benzene ring may be unsubstituted or substituted with a monovalent organic group, and examples of the monovalent organic group include a halogen atom (fluorine atom, chlorine atom, bromine atom, iodine atom, etc.), an alkyl group having 1 to 5 carbon atoms such as a methyl group, an alkoxy group having 1 to 5 carbon atoms such as a methoxy group, a nitro group, a hydroxyl group, an amino group, a mercapto group, a nitroso group, an alkylsilyl group, an alkoxysilyl group, a silanol group, a sulfino group, a phosphino group, a carboxyl group, a cyano group, a sulfo group, an acyl group, and a "-R1-OH" group (R1 is an alkanediyl group having 1 to 4 carbon atoms).
[0040] The nitrogen-containing heterocycle may be monocyclic or polycyclic. Specific examples of the nitrogen-containing heterocycle include pyrrole, imidazole, pyrazole, triazole, pyridine, pyrimidine, pyridazine, pyrazine, indole, benzimidazole, purine, quinoline, isoquinoline, naphthyridine, quinoxaline, phthalazine, triazine, thiazole, isothiazole, benzothiazole, 5,6,7,8-tetrahydroquinoline, piperidine, piperazine, pyrrolidine, hexamethyleneimine, decahydroquinoline, imidazoline, and carbazole. In the partial structure represented by the above formula (b), examples of the alkanediyl group having 1 to 4 carbon atoms for R1 include a methylene group, an ethylene group, a propanediyl group, and a butanediyl group. Among these, a methylene group is preferred from the viewpoint of high crosslinking effect. m1 is preferably 2 from the viewpoint of high crosslinking effect. From the viewpoint of ease of synthesis, the compound (B) is preferably at least one compound selected from the group consisting of the following formulae (B1), (B2-1) to (B2-2), and (B3-1) to (B3-3). [ka]
[0041] R1 represents an alkanediyl group having 1 to 4 carbon atoms. L1 represents a divalent organic group selected from the following formulae (L1-1) to (L1-3). S 21a , S 21b are each independently represented by the following formula (2S-1) or the following formula (2S-2): 2a +2) or (m 2b +2)valent organic group. 22 , S 32 are each independently a single bond, -O-, -CO-, -CH2-, -CH(CH3)-, -C(CH3)2-, or -(CH2) n -(n represents an integer of 2 to 20), or the above -(CH2) n It represents a divalent organic group in which non-adjacent CH2s are replaced by -O-, -CO-, -CH(CH3)-, or -C(CH3)2-. S 31a is a single bond, -O-, -CH2-, -CH(CH3)-, -C(CH3)2-, -(CH2) n -(n is an integer of 2 to 18), -CO-, -C≡C-, -CH=CH-, a phenylene group, a divalent organic group selected from the above formulas (M-1) to (M-10), or the above -(CH2) n represents a divalent organic group in which any CH2 in - is replaced with -O-, -CH(CH3)-, -C(CH3)2-, -CO-, a phenylene group, or a divalent organic group selected from the above formulas (M-1) to (M-11). S31b is S 31a In addition to the divalent organic group defined above, a divalent organic group represented by the above formula (M-11), -C(R 32 ) 2-m3b (Q 3b ) m3b -(m 3b represents an integer between 1 and 2. 32 represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. R2, R 31 , R 33 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.
[0042] Q 2a , Q 2b , Q 3a , Q 3b Each independently represents a monovalent organic group selected from the following formulas (Q-1) to (Q-17). 22 , S 32 If each is a single bond, Q 2a , Q 3a represents a monovalent organic group selected from (Q-1), (Q-3), (Q-7) to (Q-13) or (Q-17). l2 and l3 each independently represent an integer of 1 to 2. m1 represents an integer of 1 to 2, and multiple m1 may be the same or different. 2a , m 2b each independently represents an integer of 1 to 2. [ka] M represents a divalent organic group selected from the following formulae (M-1) to (M-11). R1 and R2 each independently represent a hydrogen atom or a methyl group. T1 and T2 each independently represent a single bond, -O-, -NR- (R represents a hydrogen atom or a methyl group), -CONR- (R represents a hydrogen atom or a methyl group), -NRCONR- (R represents a hydrogen atom or a methyl group), a phenylene group, -CH2-, -CH(CH3)-, -C(CH3)2-, -(CH2) n -(n is an integer of 2 to 20), or the above -(CH2) nAny CH2 in - represents a divalent organic group replaced with -CH(CH3)-, -C(CH3)2-, -O-, -NR- (R represents a hydrogen atom or a methyl group), -CONR- (R represents a hydrogen atom or a methyl group), -NRCONR- (R represents a hydrogen atom or a methyl group), or a phenylene group. Any hydrogen atom on the phenylene group may be replaced with a monovalent organic group. T3 is -CH2-, -CH(CH3)-, -C(CH3)2-, -(CH2) n -(n is an integer of 2 to 18), a phenylene group, or the above-(CH2) n represents a divalent organic group in which any CH2 in - is replaced by -O-, -CH(CH3)-, -C(CH3)2-, -CONR- (R represents a hydrogen atom or a methyl group), -NRCONR- (R represents a hydrogen atom or a methyl group), or a phenylene group. n1 represents an integer of 1 to 3. n3 represents an integer of 0 to 1. [ka] R1, R2, R3, and R4 each independently represent a hydrogen atom or a methyl group. *1 represents a bond, and *2 represents a bond bonded to a carbon atom. [ka]
[0043] *1 is a nitrogen atom or (Q 2b ) and *2 represents a bond bonded to the benzene ring. n represents an integer of 1 to 2. L11 , A L12 are each independently a single bond, -O-, -CH2-, -CH(CH3)-, -C(CH3)2-, or -(CH2) n -(n represents an integer of 2 to 20), -COO-, -OCO-, -CONR- (R represents a hydrogen atom or a methyl group), or the above-(CH2) n represents a divalent organic group in which any CH2 in - is replaced by -O-, -CH(CH3)-, -C(CH3)2-, -COO-, -OCO-, or -CONR- (R represents a hydrogen atom or a methyl group). L12If there are multiple A's, multiple A's L12 may be the same or different. A S11 , A S21 are each independently a single bond, -O-, -CO-, -CH2-, -CH(CH3)-, -C(CH3)2-, or -(CH2) n -(n represents an integer of 2 to 20), a phenylene group, or the above-(CH2) n R represents a divalent organic group in which any CH2 in R is replaced by -CH(CH3)-, -C(CH3)2-, -O-, -CO-, or a phenylene group. L represents a hydrogen atom, a hydroxyl group or a methyl group, and p represents an integer of 1 or 2. [ka]
[0044] R1, R3, R7, and R8 each represent a hydrogen atom or a methyl group. 16 , R 17 represents a phenyl group. *1 represents a bond, and *2 represents a bond bonded to a carbon atom. The hydrogen atom on the phenylene group in L1 may be replaced by a monovalent organic group such as an alkyl group having 1 to 5 carbon atoms, such as a methyl group or an ethyl group, an alkoxy group having 1 to 5 carbon atoms, such as a methoxy group, a halogen atom, such as a fluorine atom, a halogenated alkyl group having 1 to 5 carbon atoms, such as a trifluoromethyl group, -NR1R2 (R1 and R2 represent a hydrogen atom, a methyl group, or a tert-butoxycarbonyl group, respectively), a cyano group, or a hydroxy group.
[0045] In the divalent organic groups represented by the above formulas (M-1) to (M-11) and the monovalent organic groups represented by the above formulas (Q-1) to (Q-17), any hydrogen atom on the benzene ring or heterocycle may be replaced with a monovalent organic group, and specific examples of such monovalent organic groups include the structures exemplified as the monovalent organic groups replacing the hydrogen atoms on the phenylene group in the above L1. In the above formula (B1), from the viewpoint of ease of synthesis, L1 may be any of the following formulae (L1-a-1) to (L1-a-12), (L1-b-1) to (L1-b-3), or (L1-c-1) to (L1-c-3). [ka] [ka]
[0046] Above A L11 , A L12 From the viewpoint of ease of synthesis, single bonds, -O-, -CH2-, -(CH2) n -(n represents an integer of 2 to 20), -COO-, -OCO-, -CONR- (R represents a hydrogen atom or a methyl group), or the above-(CH2) n A divalent organic group in which any CH2 of - is replaced by -O- or -CONR- (R represents a hydrogen atom or a methyl group) is preferred. Above S 21a From the viewpoint of ease of synthesis, the compound represented by the following formula (S 21a -1-1)~(S 21a -1-5) or (S 21a -2-1) may also be used. [ka]
[0047] *1 represents the bond bonded to the nitrogen atom, and *2 represents the bond bonded to the benzene ring. Above S 21b From the viewpoint of ease of synthesis, the above-mentioned formula (S 21a -1-1)~(S 21a -1-5), (S 21a -2-1), the following formula (S 21b -1-1) may be used. However, the above formula (S 21a -1-1)~(S 21a -1-5), (S 21a In -2-1), *1 is (Q 2b) and *2 represents the bond bonding to the benzene ring. [ka]
[0048] *1 is a nitrogen atom or (Q 2b ) and *2 represents the bond bonding to the benzene ring. Above S 31a From the viewpoint of ease of synthesis, the following formula (S 31a -1)~(S 31a -5) may also be used. [ka] *1 represents a bond bonded to a nitrogen atom, *2 represents a bond bonded to a benzene ring, and M represents a group selected from the above formulas (M-1) to (M-10). Above S 31b In view of ease of synthesis, a single bond, -O-, the above formula (S 31a -1)~(S 31a -5), the following formula (S 31b -1)~(S 31b -5) may be used. However, the above formula (S 31a -1)~(S 31a -5), *1 is (Q 3b ) and *2 represents the bond bonding to the benzene ring. [ka]
[0049] *1 is Q 3b represents a bond bonded to the benzene ring, and M represents a group selected from the above formulas (M-1) to (M-10). Q 3b has the same meaning as the above formula (B3-2). Above R 33 From the viewpoint of ease of synthesis, may be a hydrogen atom, a methyl group, or an ethyl group. Preferred specific examples of compound (B) include compounds represented by the following formulas (B1-1-1) to (B1-1-4), (B1-2-1) to (B1-2-2), (B1-3-1) to (B1-3-26), (B2-1-1) to (B2-1-2), (B2-2-1) to (B2-2-18), (B3-1-1) to (B3-1-7), (B3-2-1) to (B3-2-11), and (B3-3-1). [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[0050] The content of the compound (B) is preferably 0.1 to 40 parts by mass, more preferably 0.5 to 35 parts by mass, and even more preferably 0.5 to 30 parts by mass, per 100 parts by mass of the component (A).
[0051] <Method of producing polyamic acid> The polymer (A) in the present invention can be obtained, for example, by reacting a tetracarboxylic acid derivative having the above-mentioned structure of X1 with a diamine having the above-mentioned structure of Y1 by a known method such as that described in International Publication WO2013 / 157586.
[0052] [Terminal Modifier] In synthesizing the polymer (A) in the present invention, a terminal-modified polymer may be synthesized by using a suitable terminal-capping agent together with the above-mentioned tetracarboxylic acid derivative and diamine.
[0053] Examples of the terminal modifier include acid monoanhydrides such as maleic anhydride, nadic anhydride, phthalic anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride, 3-hydroxyphthalic anhydride, trimellitic anhydride, compounds represented by the following formulas (m-1) to (m-6), 3-(3-trimethoxysilyl)propyl)-3,4-dihydrofuran-2,5-dione, 4,5,6,7-tetrafluoroisobenzofuran-1,3-dione, and 4-ethynylphthalic anhydride; [ka] Examples of the dicarbonate diester compounds include di-tert-butyl dicarbonate and diallyl dicarbonate; chlorocarbonyl compounds include acryloyl chloride, methacryloyl chloride and nicotinic acid chloride; monoamine compounds include aniline, 2-aminophenol, 3-aminophenol, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, cyclohexylamine, n-butylamine, n-pentylamine, n-hexylamine, n-heptylamine and n-octylamine; and monoisocyanate compounds include ethyl isocyanate, phenyl isocyanate and naphthyl isocyanate.
[0054] The proportion of the terminal modifier used is preferably 20 parts by mol or less, and more preferably 10 parts by mol or less, based on 100 parts by mol of the total of the diamines used.
[0055] <Liquid crystal alignment agent> The liquid crystal alignment agent of the present invention may contain other polymers in addition to the polymer (A). Examples of the other polymers include polyester, polyamide, polyurea, polyorganosiloxane, cellulose derivatives, polyacetal, polystyrene or its derivatives, poly(styrene-phenylmaleimide) derivatives, and poly(meth)acrylates. In addition, the polyorganosiloxane preferably has at least one of an oxetanyl group and an oxiranyl group from the viewpoint of easy synthesis.
[0056] The liquid crystal aligning agent is used to prepare a liquid crystal alignment film, and takes the form of a coating liquid from the viewpoint of forming a uniform thin film. The liquid crystal aligning agent of the present invention is also preferably a coating liquid containing the above-mentioned polymer component and an organic solvent. In this case, the concentration of the polymer in the liquid crystal aligning agent can be appropriately changed depending on the thickness of the coating film to be formed. From the viewpoint of forming a uniform and defect-free coating film, it is preferably 1% by mass or more, and from the viewpoint of storage stability of the solution, it is preferably 10% by mass or less. A particularly preferable concentration of the polymer is 2 to 8% by mass.
[0057] The organic solvent contained in the liquid crystal alignment agent is not particularly limited as long as the polymer component is dissolved uniformly. Specific examples thereof include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethylsulfoxide, γ-butyrolactone, γ-valerolactone, 1,3-dimethyl-2-imidazolidinone, methyl ethyl ketone, cyclohexanone, cyclopentanone, N,N-dimethyllactamide, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide (collectively referred to as "good solvent"). From the viewpoint of good printability, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-dimethyllactamide, or γ-butyrolactone may be used. From the viewpoint of good printability, the good solvent in the liquid crystal aligning agent of the present invention may be 20 to 99 mass %, or 20 to 90 mass %, or 30 to 80 mass % of the total solvent contained in the liquid crystal aligning agent.
[0058] In addition, the organic solvent contained in the liquid crystal alignment agent is preferably a mixed solvent containing the above-mentioned solvent and a solvent (also called a poor solvent) that improves the coating property and the surface smoothness of the coating film when the liquid crystal alignment agent is applied. Specific examples of the organic solvent to be used in combination are listed below, but are not limited to these examples. For example, diisopropyl ether, diisobutyl ether, diisobutyl carbinol (2,6-dimethyl-4-heptanol), ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, 1,2-butoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, 4-hydroxy-4-methyl-2-pentanone, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, 3-ethoxybutyl acetate, 1-methylpentyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, ethylene glycol monoacetate, ethylene glycol diacetate, propylene carbonate, ethylene carbonate, ethylene glycol monobutyl ether, ethylene glycol monoisoamyl ether, ethylene glycol monohexyl ether, propylene glycol monobutyl ether, 1-(2-butoxyethoxy)-2-propanol, 2-(2-butoxy)-2-propanol, Examples of the ethoxy)-1-propanol, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, ethylene glycol monobutyl ether acetate, ethylene glycol monoacetate, ethylene glycol diacetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, 2-(2-ethoxyethoxy)ethyl acetate, diethylene glycol acetate, propylene glycol diacetate, n-butyl acetate, propylene glycol monoethyl ether acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, propyl 3-methoxypropionate, butyl 3-methoxypropionate, n-butyl lactate, isoamyl lactate, diethylene glycol monoethyl ether, diisobutyl ketone (2,6-dimethyl-4-heptanone), and the like.
[0059] Among these, from the viewpoint of good printability, the poor solvent may be diisobutyl carbinol, propylene glycol monobutyl ether, propylene glycol diacetate, diethylene glycol diethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, or diisobutyl ketone.
[0060] From the viewpoint of good printability, the combinations of good and poor solvents are as follows: N-methyl-2-pyrrolidone and ethylene glycol monobutyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, and ethylene glycol monobutyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, and propylene glycol monobutyl ether, N-ethyl-2-pyrrolidone and propylene glycol monobutyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone, and diethylene glycol diethyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether, and 2,6- Examples of the combinations include dimethyl-4-heptanone, N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether, and diisopropyl ether, N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether, and 2,6-dimethyl-4-heptanol, N-methyl-2-pyrrolidone, γ-butyrolactone, and dipropylene glycol dimethyl ether, N-methyl-2-pyrrolidone, propylene glycol monobutyl ether, and dipropylene glycol dimethyl ether, and N-ethyl-2-pyrrolidone, propylene glycol monobutyl ether, and dipropylene glycol dimethyl ether. These poor solvents may be 1 to 80% by mass, 10 to 80% by mass, or 20 to 70% by mass of the entire solvent contained in the liquid crystal alignment agent. The type and content of such a solvent are appropriately selected depending on the coating device, coating conditions, and coating environment of the liquid crystal alignment agent.
[0061] The liquid crystal alignment agent of the present invention may additionally contain components other than the polymer component, the component (B) and the organic solvent. Such additional components include an adhesion assistant for increasing the adhesion between the liquid crystal alignment film and the substrate or between the liquid crystal alignment film and the sealant, a compound for increasing the strength of the liquid crystal alignment film (hereinafter also referred to as a crosslinking compound), a dielectric or conductive substance for adjusting the dielectric constant or electrical resistance of the liquid crystal alignment film, etc.
[0062] As the crosslinkable compound, from the viewpoints of reducing the generation of residual images and achieving a high effect of improving film strength, a compound having at least one group selected from the group consisting of an oxiranyl group, an oxetanyl group, a protected isocyanate group, a protected isothiocyanate group, a group containing an oxazoline ring structure, a group containing a Meldrum's acid structure, a cyclocarbonate group, and a group represented by the following formula (d), or a compound selected from the compounds represented by the following formulas (e-1) to (e-8) (hereinafter these are also collectively referred to as compound (C)). [ka] In the formula, R1 is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or "*-CH2-OH", and R2 and R3 are each independently a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or "*-CH2-OH". * indicates a bond. [ka]
[0063] Specific examples of compounds having an oxiranyl group include compounds having two or more oxiranyl groups, such as the compounds described in paragraph
[0037] of JP-A-10-338880 and compounds having a triazine ring skeleton described in International Publication WO2017 / 170483. Among these, from the viewpoint of high crosslinking effect, compounds containing nitrogen atoms such as N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-p-phenylenediamine, and compounds represented by the following formulas (r-1) to (r-3) may be used. [ka]
[0064] Specific examples of the compound having an oxetanyl group include compounds having two or more oxetanyl groups described in paragraphs
[0170] to
[0175] of WO 2011 / 132751.
[0065] Specific examples of compounds having a protected isocyanate group include compounds having two or more protected isocyanate groups described in paragraphs
[0046] to
[0047] of JP 2014-224978 A, compounds having three or more protected isocyanate groups described in paragraphs
[0119] to
[0120] of WO 2015 / 141598 A, etc. Among these, compounds represented by the following formulae (bi-1) to (bi-3) may be used in view of their high crosslinking effect. [ka]
[0066] Specific examples of compounds having a protected isothiocyanate group include compounds having two or more protected isothiocyanate groups described in JP2016-200798A.
[0067] Specific examples of the compound having a group containing an oxazoline ring structure include compounds containing two or more oxazoline structures described in paragraph
[0115] of JP-A-2007-286597.
[0068] Specific examples of the compound having a group containing a Meldrum's acid structure include compounds having two or more Meldrum's acid structures described in International Publication WO2012 / 091088.
[0069] Specific examples of the compound having a cyclocarbonate group include the compounds described in International Publication WO2011 / 155577.
[0070] Examples of the alkyl group having 1 to 3 carbon atoms for R1, R2, and R3 in the group represented by the above formula (d) include a methyl group, an ethyl group, and a propyl group.
[0071] Specific examples of the compound having a group represented by the above formula (d) include compounds having two or more groups represented by the above formula (d) described in International Publication WO2015 / 072554 and paragraph
[0058] of JP2016-118753A, compounds described in JP2016-200798A, etc. Among these, compounds represented by the following formulas (hd-1) to (hd-8) may be used in view of their high crosslinking effect. [ka]
[0072] The above compounds are examples of crosslinkable compounds, and are not limited thereto. For example, components other than those described above disclosed on pages 53
[0105] to 55
[0116] of International Publication No. 2015 / 060357 can be mentioned. In addition, the crosslinkable compound contained in the liquid crystal aligning agent of the present invention may be one type, or two or more types may be combined. The content of the crosslinkable compound in the liquid crystal aligning agent of the present invention may be 0.5 to 20 parts by mass, or 1 to 15 parts by mass, relative to 100 parts by mass of the polymer component contained in the liquid crystal aligning agent, from the viewpoint of proceeding with the crosslinking reaction to exhibit the intended effect and enhancing the liquid crystal alignment property.
[0073] Examples of the adhesion aid include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyldiethoxymethylsilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, N-ethoxycarbonyl-3-aminopropyltriethoxysilane, N-triethoxysilylpropyltriethylenetriamine, N-trimethoxy ... triethylenetriamine, 10-trimethoxysilyl-1,4,7-triazadecane, 10-triethoxysilyl-1,4,7-triazadecane, 9-trimethoxysilyl-3,6-diazanonyl acetate, 9-triethoxysilyl-3,6-diazanonyl acetate, N-benzyl-3-aminopropyltrimethoxysilane, N-benzyl-3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, N-bis(oxyethylene)-3-aminopropyltrimethoxysilane, N-bis(oxyethylene)-3-aminopropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,Examples of silane coupling agents include 4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane. When using these silane coupling agents, the amount may be 0.1 to 30 parts by mass, or 0.1 to 20 parts by mass, per 100 parts by mass of the polymer component contained in the liquid crystal alignment agent, from the viewpoint of improving the liquid crystal alignment property.
[0074] <Liquid crystal alignment film / Liquid crystal display element> A liquid crystal alignment film can be manufactured by using the liquid crystal alignment agent. The liquid crystal display element according to the present invention includes a liquid crystal alignment film formed by using the liquid crystal alignment agent. The operation mode of the liquid crystal display element according to the present invention is not particularly limited, and it can be applied to various operation modes such as TN (Twisted Nematic) type, STN type, vertical alignment type (including VA-MVA type, VA-PVA type, etc.), in-plane switching type (IPS type), FFS (Fringe Field Switching) type, and optical compensation bend type (OCB type).
[0075] The liquid crystal display element according to the present invention can be manufactured, for example, by the following steps (1-1) to (1-3). In step (1-1), different substrates are used depending on the desired operation mode. Steps (1-2) and (1-3) are common to each operation mode.
[0076] [Step (1-1): Formation of coating film] First, the liquid crystal aligning agent of the present invention is applied onto a substrate, and then the applied surface is heated to form a coating film on the substrate.
[0077] (1-1A) For example, when manufacturing a TN-type, STN-type or VA-type liquid crystal display element, first, two substrates each having a patterned transparent conductive film are used as a pair, and the liquid crystal alignment agent prepared above is applied to the transparent conductive film-formed surface of each substrate, preferably by offset printing, spin coating, roll coating or inkjet printing. As the substrate, for example, a transparent substrate made of glass such as float glass or soda glass; or a plastic such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate or poly(alicyclic olefin) can be used. As the transparent conductive film provided on one side of the substrate, a NESA film (registered trademark of PPG, USA) made of tin oxide (SnO2), an ITO film made of indium oxide-tin oxide (In2O3-SnO2), or the like can be used. To obtain a patterned transparent conductive film, for example, a method of forming a pattern by photo-etching after forming a patternless transparent conductive film; a method of using a mask having a desired pattern when forming a transparent conductive film; or the like can be used. When applying the liquid crystal alignment agent, in order to further improve the adhesion between the substrate surface and the transparent conductive film and the coating film, the surface of the substrate on which the coating film is to be formed may be pretreated by applying a functional silane compound, a functional titanium compound, or the like.
[0078] After the liquid crystal alignment agent is applied, preheating (prebaking) is preferably performed for the purpose of preventing dripping of the applied liquid crystal alignment agent. The prebaking temperature is preferably 30 to 200°C, more preferably 40 to 150°C, and particularly preferably 40 to 100°C. The prebaking time is preferably 0.25 to 10 minutes, more preferably 0.5 to 5 minutes. Thereafter, the solvent is completely removed, and a baking (postbaking) step is performed for the purpose of thermally imidizing the amic acid structure present in the polymer as necessary. The baking temperature (postbaking temperature) at this time is preferably 80 to 300°C, more preferably 120 to 250°C. The postbaking time is preferably 5 to 200 minutes, more preferably 10 to 100 minutes. The film thickness of the film thus formed is preferably 0.001 to 1 μm, more preferably 0.005 to 0.5 μm.
[0079] (1-1B) When manufacturing an IPS or FFS type liquid crystal display element, a liquid crystal alignment agent is applied to the electrode forming surface of a substrate having an electrode made of a transparent conductive film or a metal film patterned into a comb-tooth shape and to one surface of an opposing substrate having no electrode, and then each applied surface is heated to form a coating film. The materials of the substrate and transparent conductive film used in this case, the coating method, the heating conditions after coating, the patterning method of the transparent conductive film or the metal film, the pretreatment of the substrate, and the preferred thickness of the coating film to be formed are the same as those in (1-1A) above. As the metal film, for example, a film made of a metal such as chromium can be used.
[0080] In both of the above (1-1A) and (1-1B), a liquid crystal alignment film or a coating film to be a liquid crystal alignment film is formed by applying the liquid crystal alignment agent onto a substrate and then removing the organic solvent. At this time, the coating film may be further heated after the coating film is formed to advance the dehydration ring-closing reaction of the polyamic acid, polyamic acid ester, and polyimide blended in the liquid crystal alignment agent according to the present invention, to form a more imidized coating film.
[0081] [Step (1-2): Treatment for imparting alignment ability] When manufacturing a TN-type, STN-type, IPS-type or FFS-type liquid crystal display element, a treatment is carried out to impart liquid crystal alignment ability to the coating film formed in the above step (1-1). This imparts the alignment ability of liquid crystal molecules to the coating film, forming a liquid crystal alignment film. Examples of the alignment ability imparting treatment include a rubbing treatment in which the coating film is rubbed in a certain direction with a roll wrapped with a cloth made of fibers such as nylon, rayon or cotton, and a photoalignment treatment in which the coating film is irradiated with polarized or non-polarized radiation. On the other hand, when manufacturing a VA-type liquid crystal display element, the coating film formed in the above step (1-1) can be used as it is as a liquid crystal alignment film, but the coating film may also be subjected to an alignment ability imparting treatment.
[0082] When the coating film is provided with liquid crystal alignment ability by photoalignment treatment, the radiation to be irradiated to the coating film is, for example, For example, ultraviolet light and visible light including light having a wavelength of 150 to 800 nm can be used. When the radiation is polarized, it may be linearly polarized or partially polarized. When the radiation used is linearly polarized or partially polarized, the radiation may be irradiated from a direction perpendicular to the substrate surface, from an oblique direction, or a combination of these. When irradiating with non-polarized radiation, the irradiation direction is an oblique direction.
[0083] Examples of light sources that can be used include low-pressure mercury lamps, high-pressure mercury lamps, deuterium lamps, metal halide lamps, argon resonance lamps, xenon lamps, and excimer lasers. Ultraviolet rays in a preferred wavelength range can be obtained by using a light source in combination with, for example, a filter, a diffraction grating, and the like. The radiation dose is preferably 10 to 5,000 mJ / cm. 2 and more preferably 30 to 2,000 mJ / cm 2 It is. The coating film may be irradiated with light while being heated in order to enhance reactivity. The temperature during heating is usually 30 to 250°C, preferably 40 to 200°C, and more preferably 50 to 150°C.
[0084] When ultraviolet light containing light having a wavelength of 150 to 800 nm is used, the light-irradiated film obtained in the above process can be used as a liquid crystal alignment film as it is, but the light-irradiated film may be baked, washed with water or an organic solvent, or a combination of these. The baking temperature is preferably 80 to 300°C, more preferably 80 to 250°C. The baking time is preferably 5 to 200 minutes, more preferably 10 to 100 minutes. The baking may be performed once or twice or more. The photo-alignment treatment here corresponds to a treatment of light irradiation in a state where the film is not in contact with the liquid crystal layer.
[0085] The organic solvent used for the washing is not particularly limited, but specific examples include water, methanol, ethanol, 2-propanol, acetone, methyl ethyl ketone, 1-methoxy-2-propanol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, methyl lactate, diacetone alcohol, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, propyl acetate, butyl acetate, and cyclohexyl acetate.
[0086] The liquid crystal alignment film after the rubbing treatment may be further subjected to a treatment to change the pretilt angle of a part of the liquid crystal alignment film by irradiating a part of the liquid crystal alignment film with ultraviolet light, or a treatment to form a resist film on a part of the surface of the liquid crystal alignment film and then perform a rubbing treatment in a direction different from that of the previous rubbing treatment, followed by removing the resist film, so that the liquid crystal alignment film has different liquid crystal alignment capabilities for each region. In this case, it is possible to improve the visibility characteristics of the resulting liquid crystal display element. The liquid crystal alignment film suitable for VA type liquid crystal display elements can also be suitably used for PSA (polymer sustained alignment) type liquid crystal display elements.
[0087] [Step (1-3): Construction of liquid crystal cell] (1-3A) Two substrates on which a liquid crystal alignment film is formed are prepared as described above, and a liquid crystal is disposed between the two substrates arranged opposite to each other to manufacture a liquid crystal cell. There are, for example, two methods for manufacturing a liquid crystal cell. The first method is a conventionally known method. First, two substrates are arranged opposite to each other with a gap (cell gap) between them so that the liquid crystal alignment films face each other, the peripheries of the two substrates are bonded together with a sealant, and liquid crystal is injected and filled into the substrate surfaces and the cell gap partitioned by the sealant, and then the injection hole is sealed to manufacture a liquid crystal cell. The second method is a technique called the ODF (One Drop Fill) method. For example, an ultraviolet light curable sealant is applied to a predetermined location on one of the two substrates on which a liquid crystal alignment film is formed, and liquid crystal is further dropped at several predetermined locations on the liquid crystal alignment film surface, and then the other substrate is bonded so that the liquid crystal alignment film faces each other, and the liquid crystal is spread over the entire surface of the substrate, and then ultraviolet light is irradiated over the entire surface of the substrate to cure the sealant, thereby manufacturing a liquid crystal cell. Regardless of which method is used, it is desirable to further heat the liquid crystal cell produced as described above to a temperature at which the liquid crystal used assumes an isotropic phase, and then slowly cool it to room temperature to remove the flow orientation that occurs during liquid crystal filling.
[0088] As the sealing agent, for example, an epoxy resin containing a hardener and aluminum oxide spheres as spacers can be used.
[0089] Examples of liquid crystals include nematic liquid crystals and smectic liquid crystals, among which nematic liquid crystals are preferred. For example, Schiff base liquid crystals, azoxy liquid crystals, biphenyl liquid crystals, phenylcyclohexane liquid crystals, ester liquid crystals, terphenyl liquid crystals, biphenylcyclohexane liquid crystals, pyrimidine liquid crystals, dioxane liquid crystals, bicyclooctane liquid crystals, cubane liquid crystals, etc. can be used. In addition, these liquid crystals may be used by adding cholesteric liquid crystals such as cholestyl chloride, cholesteryl nonaate, and cholesteryl carbonate; chiral agents such as those sold under the trade names "C-15" and "CB-15" (manufactured by Merck); and ferroelectric liquid crystals such as p-decyloxybenzylidene-p-amino-2-methylbutylcinnamate. The liquid crystal may also contain an anisotropic dye. The term "dye" may refer to a material capable of intensively absorbing or transforming light in at least a part or the entire visible light range, for example, a wavelength range of 400 nm to 700 nm, and the term "anisotropic dye" may refer to a material capable of anisotropically absorbing light in at least a part or the entire visible light range. The color of the liquid crystal cell can be adjusted by using such dyes. The type of anisotropic dye is not particularly limited, and for example, a black dye or a color dye can be used. The ratio of the anisotropic dye to the liquid crystal is appropriately selected within a range that does not impair the desired physical properties, and for example, the anisotropic dye can be included in a ratio of 0.01 to 5 parts by weight with respect to 100 parts by weight of the liquid crystal compound, but the above ratio can be changed to an appropriate range as necessary.
[0090] (1-3B) When producing a PSA type liquid crystal display element, a liquid crystal cell is constructed in the same manner as in (1-3A) above, except that a photopolymerizable compound such as any of the following formulae (w-1) to (w-5) is injected or dropped together with the liquid crystal. [ka] Thereafter, the liquid crystal cell is irradiated with light while a voltage is applied between the conductive films of the pair of substrates. The voltage applied here can be, for example, 5 to 50 V DC or AC. The light to be irradiated can be, for example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm, but ultraviolet light containing light with a wavelength of 300 to 400 nm is preferred. The light source for the irradiated light can be, for example, a low pressure mercury lamp, a high pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, or the like. The ultraviolet light in the above-mentioned preferred wavelength range can be obtained by using the light source in combination with, for example, a filter diffraction grating. The light irradiation dose is preferably 100 mJ / cm. 2 More than 30,000mJ / cm 2 More preferably, it is 100 to 20,000 mJ / cm 2 It is.
[0091] (1-3C) When a coating film is formed on a substrate using a liquid crystal alignment agent containing a compound (polymer or additive) having a photopolymerizable group, a liquid crystal cell may be constructed in the same manner as in (1-3A) above, and then a liquid crystal display element may be manufactured by a process of irradiating the liquid crystal cell with light while applying a voltage between the conductive films of a pair of substrates. According to this method, the merits of the PSA mode can be realized with a small amount of light irradiation. Examples of additives having a photopolymerizable group include the structures exemplified by the above formulas (w-1) to (w-5), and the blending amount may be 1 to 30 mass % with respect to the total solid content of the polymer contained in the liquid crystal alignment agent, or 1 to 20 mass %, or 1 to 15 mass %. The light irradiation to the liquid crystal cell may be performed in a state where the liquid crystal is driven by applying a voltage, or may be performed in a state where a low voltage that does not drive the liquid crystal is applied. The voltage to be applied may be, for example, 0.1 to 30 V of direct current or alternating current. The conditions of the light to be irradiated can be the same as those described in (1-3B) above. The light irradiation treatment here corresponds to the light irradiation treatment in a state of contact with the liquid crystal layer.
[0092] The liquid crystal display element according to the present invention can be obtained by attaching a polarizing plate to the outer surface of the liquid crystal cell. Examples of the polarizing plate to be attached to the outer surface of the liquid crystal cell include a polarizing film called an "H film" made by absorbing iodine while stretching and aligning polyvinyl alcohol, sandwiched between cellulose acetate protective films, and a polarizing plate made of the H film itself. The liquid crystal display element according to the present invention can be effectively applied to various devices, and can be used in various display devices such as watches, portable games, word processors, notebook computers, car navigation systems, camcorders, PDAs, digital cameras, mobile phones, smartphones, various monitors, liquid crystal televisions, and information displays. As described above, by using the liquid crystal aligning agent of the present invention, it is possible to obtain a liquid crystal alignment film which generates little residual images and can minimize bright spots even when physical friction occurs, such as rubbing with a spacer, and a liquid crystal display element having the same. In addition, the obtained liquid crystal display element has high reliability. EXAMPLES
[0093] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. The abbreviations of the compounds and the measurement methods of the respective properties are as follows. Compound (c-2) was synthesized according to the method described in Synthesis Example 3 of JP-A-2008-052260. (Diamine) DA-1 to DA-27: Compounds represented by the following formulas (DA-1) to (DA-27) (Tetracarboxylic acid dianhydride) CA-1 to CA-8: Compounds represented by the following formulas (CA-1) to (CA-8) (Tetracarboxylic acid diester dihalide) CE-1: A compound represented by the following formula (CE-1): (Monocarboxylic acid chloride) E-1: Acryloyl chloride (Additives) b-1 to b-9: Compounds represented by the following formulas (b-1) to (b-9) (Other additives) c-1: A compound represented by the following formula (c-1): c-2: A compound represented by the following formula (c-2): F-1: N-α-(9-fluorenylmethyloxycarbonyl)-N-τ-t-butoxycarbonyl-L-histidine (compound represented by the following formula (F-1)) s-1: 3-glycidoxypropyltriethoxysilane (compound represented by the following formula (s-1)) s-2: 3-glycidoxypropylmethyldiethoxysilane (compound represented by the following formula (s-2)) M-1: 3-picolylamine (Organic solvent) NMP: N-methyl-2-pyrrolidone, GBL: γ-butyrolactone, BCS: butyl cellosolve, DIBK: diisobutyl ketone, NEP: N-ethyl-2-pyrrolidone, DAA: diacetone alcohol PC: propylene carbonate, DME: dipropylene glycol dimethyl ether, DPM: Dipropylene glycol monomethyl ether; PB: propylene glycol monobutyl ether; PGDAC: propylene glycol diacetate; DEDE: diethylene glycol diethyl ether; GVL: γ-valerolactone, DML: N,N-dimethyllactamide EEP: Ethyl 3-ethoxypropionate [ka] [ka] Boc represents a tert-butoxycarbonyl group.
[0094] [ka] [ka] [ka]
[0095] [ka]
[0096] [ka] [ka]
[0097] Boc represents a tert-butoxycarbonyl group. Fmoc represents a 9-fluorenylmethyloxycarbonyl group. [viscosity] The viscosity of the solution was measured using an E-type viscometer TVE-22H (manufactured by Toki Sangyo Co., Ltd.) with a sample volume of 1.1 mL, a cone rotor TE-1 (1°34′, R24), and a temperature of 25°C. [Molecular weight] The molecular weight was measured by a GPC (room temperature gel permeation chromatography) device, and the number average molecular weight (Mn) and weight average molecular weight (Mw) were calculated as polyethylene glycol and polyethylene oxide equivalent values. GPC apparatus: Shodex (GPC-101), column: Shodex (KD803, KD805 in series), column temperature: 50°C, eluent: N,N-dimethylformamide (additives: lithium bromide monohydrate (LiBr·H2O) 30 mmol / L, phosphoric acid·anhydrous crystal (o-phosphoric acid) 30 mmol / L, tetrahydrofuran (THF) 10 mL / L), flow rate: 1.0 mL / min Standard samples for creating a calibration curve: TSK standard polyethylene oxide manufactured by Tosoh Corporation (weight average molecular weight (Mw) approximately 900,000, 150,000, 100,000, 30,000), and polyethylene glycol manufactured by Polymer Laboratory Co., Ltd. (peak top molecular weight (Mp) approximately 12,000, 4,000, 1,000). In order to avoid overlapping peaks, measurements were performed separately on two samples: a sample made by mixing four types of 900,000, 100,000, 12,000, and 1,000, and a sample made by mixing three types of 150,000, 30,000, and 4,000.
[0098] <Measurement of imidization rate> 20 mg of polyimide powder was placed in an NMR sample tube (NMR sampling tube standard, φ5 (Kusano Scientific Co., Ltd.)), deuterated dimethyl sulfoxide (DMSO-d6, 0.05% TMS (tetramethylsilane) mixture) (0.53 mL) was added, and the mixture was completely dissolved by ultrasonication. This solution was measured by 500 MHz proton NMR using an NMR measurement device (JNW-ECA500) (JEOL Datum Co., Ltd.). The imidization rate was calculated by the following formula using the proton peak integrated value of this proton and the proton peak integrated value of the proton peak derived from the NH group of the amic acid that appears around 9.5 ppm to 10.0 ppm. Imidization rate (%) = (1-α·x / y) × 100 In the above formula, x is the integrated value of the proton peak derived from the NH group of the amic acid, y is the integrated value of the peak of the reference proton, and α is the ratio of the number of reference protons to one NH group proton of the amic acid in the case of polyamic acid (imidization rate 0%).
[0099] [Synthesis of compound (B)] <Synthesis example (b-1)> Compound (b-1) was synthesized according to the route shown below. [ka] 2,5-pyridinedicarboxylic acid (3.00 g, 18.0 mmol), 4-aminophenol (4.11 g, 37.7 mmol) and N,N-dimethylformamide (DMF) (100 g) were added to a recovery flask, and the mixture was stirred at room temperature. Next, N-ethylmorpholine (4.34 g, 37.7 mmol) and 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride (DMT-MM) (10.43 g, 37.7 mmol) were added, and the mixture was stirred at room temperature overnight. Water (600 g) was added to the reaction solution to precipitate a solid, and the obtained solid was washed with methanol. Next, the solvent was distilled off under reduced pressure to obtain 4.23 g of compound (b-1-1). Compound (b-1-1) (2.00 g, 5.72 mmol), 24% aqueous sodium hydroxide solution (3.81 g, 22.8 mmol) and pure water (1.16 g) were added to a four-neck flask, and 37% aqueous formaldehyde solution (4.68 g, 57.2 mmol) was added dropwise under stirring at room temperature to cause a reaction. The reaction solution was heated to 35-40°C and stirred, and then a portion of the reaction solution was taken out and measured by LC / MS. The end point of the reaction was confirmed by the disappearance of the peak of the raw material. After the reaction was completed, the obtained reaction mixture was neutralized with acetic acid, and then stirred for 2 hours, and the precipitated crystals were filtered. The solvent was distilled off under reduced pressure to obtain 2.41 g of compound (b-1).
[0100] <Synthesis example (b-2)> Compound (b-2) was obtained by synthesizing in the same manner as in Scheme 1, except that 4-aminophenol was changed to tyramine. [ka]
[0101] <Synthesis example (b-3)> Compound (b-3) was synthesized according to the route shown below. [ka] 4,4'-Dimethoxydiphenylamine (3.00g, 13.1mmol), potassium carbonate (5.43g, 39.3mmol) and N,N-dimethylformamide (DMF) (18.6g) were added to a recovery flask, and the mixture was stirred at room temperature. Next, iodomethane (7.43g, 52.3mmol) was added, and the temperature was raised to 40-50°C and stirred, and then a portion of the reaction solution was taken out and measured by LC / MS. The end point of the reaction was confirmed by the disappearance of the peak of the raw material. Tetrahydrofuran (THF) (50g), toluene (10g) and water (50g) were added to the reaction solution, and the organic layer was separated. The organic layer was washed with 10% saline, and then the solvent was distilled off under reduced pressure, and methanol was added to the concentrate to obtain compound (b-3-1). Compound (b-3-1) (2.00 g, 8.22 mmol) and dichloromethane (12.7 g) were added to a recovery flask, the mixture was stirred, and cooled to -5°C under a nitrogen atmosphere. Next, a 17% dichloromethane solution of boron tribromide (22.69 g, 15.4 mmol) was added dropwise, and after the addition was completed, the mixture was allowed to react at room temperature for 2 hours. After ice water was added to the reaction solution, ethyl acetate was added, and the organic layer was extracted. The solvent was removed under reduced pressure to obtain compound (b-3-2). Compound (b-3-2) (1.68 g, 7.84 mmol), 24% aqueous sodium hydroxide solution (5.20 g, 31.4 mmol) and pure water (4.32 g) were added to a four-neck flask, and 37% aqueous formaldehyde solution (6.35 g, 78.4 mmol) was added dropwise under stirring at room temperature to cause a reaction. The reaction solution was heated to 30-40°C and stirred, and then a portion of the reaction solution was taken out and measured by LC / MS. The end point of the reaction was confirmed by the disappearance of the peak of the raw material. After the reaction was completed, the obtained reaction mixture was neutralized with acetic acid, and then stirred for 2 hours, and the precipitated crystals were filtered. The solvent was distilled off under reduced pressure to obtain compound (b-3).
[0102] <Synthesis example (b-4)> Compound (b-4) was synthesized according to the route shown below. [ka] 5-(3-pyridinyl)-1,3-benzenedicarboxylic acid (CAS No. 1262962-06-0) (4.38 g, 18.0 mmol), tyramine (5.17 g, 37.7 mmol) and N,N-dimethylformamide (DMF) (100 g) were added to a recovery flask, and the mixture was stirred at room temperature. Next, N-ethylmorpholine (4.34 g, 37.7 mmol) and 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride (DMT-MM) (10.43 g, 37.7 mmol) were added, and the mixture was stirred at room temperature overnight. Water (600 g) was added to the reaction solution to precipitate a solid, and the obtained solid was washed with methanol. Next, the solvent was distilled off under reduced pressure to obtain compound (b-4-1). Next, compound (b-4) was obtained by synthesizing in the same manner as in Scheme 2, except that compound (b-3-2) was changed to compound (b-4-1).
[0103] <Synthesis example (b-5)> Compound (b-5) was obtained by synthesizing in the same manner as in Scheme 2, except that compound (b-3-2) was changed to 4,4'-(2-pyridinylmethylene)bisphenol (CAS No. 603-41-8). [ka]
[0104] <Synthesis example (b-6)> Compound (b-6) was obtained by synthesizing in the same manner as in Scheme 2, except that compound (b-3-2) was changed to 4-[[4-(2-pyridinyl)-1-piperazinyl]methyl]phenol (CAS No. 414887-31-3). [ka]
[0105] <Synthesis example (b-7)> Compound (b-7) was synthesized according to the route shown below. [ka] 2,6-Bis(hydroxymethyl)-4-aminophenol was prepared according to a procedure similar to that described by Mameri, Samir et al., European Journal of Inorganic Chemistry (2014) 26:4326-4334. Compound (b-7-1) (CAS No. 22100-88-5) (5.00 g, 18.9 mmol) and N,N-dimethylformamide (DMF) (45 g) were added to a four-neck flask, and the mixture was stirred at room temperature. Next, 2,6-bis(hydroxymethyl)-4-aminophenol (6.40 g, 37.8 mmol) was added, and the mixture was stirred at room temperature. Dioxane was added to precipitate a solid, and the solvent was distilled off from the resulting solid under reduced pressure to obtain compound (b-7).
[0106] <Synthesis example (b-8)> Compound (b-8) was obtained by synthesizing in the same manner as in Scheme 4, except that compound (b-7-1) was changed to 3,5-diisocyanatopyridine (CAS No. 1620557-50-7). [ka]
[0107] <Synthesis example (b-9)> Compound (b-9) was synthesized according to the route shown below. [ka] 4-Hydroxyphenylboronic acid pinacol (7.10 g, 32.3 mmol), 4,6-dibromopyrimidine (2.57 g, 10.8 mmol), potassium carbonate (4.45 g, 32.3 mmol), water (82 g) and 1,4-dioxane (250 mL) were added to a four-neck flask, the mixture was stirred, and the reaction system was replaced with nitrogen. Next, tetrakis(triphenylphosphine)palladium (0.64 g) was added, and the mixture was heated and stirred at 100°C overnight. Chloroform was added to the reaction solution, and the chloroform layer was removed, and the solvent was distilled off under reduced pressure. Methanol and water were added to the resulting concentrate to obtain compound (b-9-1). (b-9-1) (1.00g, 3.78mmol), 24% aqueous sodium hydroxide solution (2.51g, 15.1mmol) and pure water (2.16g) were added to a four-neck flask, and 37% aqueous formaldehyde solution (3.06g, 37.8mmol) was added dropwise under stirring at room temperature to cause a reaction. The reaction solution was heated to 30-40°C and stirred, and then a portion of the reaction solution was taken out and measured by LC / MS. The end point of the reaction was confirmed by the disappearance of the peak of the raw material. After the reaction was completed, the obtained reaction mixture was neutralized with acetic acid, and then stirred for 2 hours, and the precipitated crystals were filtered. The solvent was distilled off under reduced pressure to obtain compound (b-9).
[0108] [Synthesis of polymer (A)] <Synthesis Example 1> In a four-neck flask equipped with a stirrer and a nitrogen inlet tube, CA-2 (2.25 g, 8.99 mmol), DA-6 (2.97 g, 8.99 mmol), and DA-7 (3.43 g, 9.01 mmol) were added and dissolved in NMP (34.6 g), and the mixture was reacted at 60° C. for 4 hours. Then, CA-3 (1.75 g, 8.92 mmol) and NMP (6.99 g) were added, and the mixture was reacted at 40° C. for 4 hours to obtain a polyamic acid solution. This polyamic acid solution (40 g) was diluted to 6.5% by mass with NMP, and then acetic anhydride (7.06 g) and pyridine (2.19 g) were added as imidization catalysts and reacted at 80° C. for 4 hours. This reaction solution was poured into methanol (463 g), and the resulting precipitate was filtered off. This precipitate was washed with methanol and dried under reduced pressure at 100° C. to obtain polyimide powder. The imidization rate of this polyimide was 74%, the number average molecular weight was 12,500, and the weight average molecular weight was 38,500. NMP (18.0 g) was added to the obtained polyimide powder (2.0 g), and M-1 was added so that the amount was 1 mass % based on the polyimide solid content. The mixture was dissolved by stirring at 70°C for 12 hours to obtain a solution of polyimide (PI-V-1) with a solid content concentration of 10%.
[0109] <Synthesis Example 2> In a four-neck flask equipped with a stirrer and a nitrogen inlet tube, CA-2 (1.20 g, 4.80 mmol), DA-8 (1.46 g, 9.59 mmol), DA-9 (1.74 g, 7.18 mmol), and DA-7 (2.74 g, 7.20 mmol) were added and dissolved in NMP (28.58 g), and reacted at 60 ° C for 2 hours. Then, CA-5 (1.05 g, 4.81 mmol) and NMP (4.19 g) were added and reacted at room temperature for 4 hours, and CA-3 (2.78 g, 14.18 mmol) and NMP (11.1 g) were added and reacted at room temperature for 4 hours to obtain a polyamic acid solution. This polyamic acid solution (40 g) was diluted to 6.5% by mass with NMP, and then acetic anhydride (8.90 g) and pyridine (2.76 g) were added as imidization catalysts and reacted at 80° C. for 4 hours. This reaction solution was poured into methanol (472 g), and the resulting precipitate was filtered off. This precipitate was washed with methanol and dried under reduced pressure at 100° C. to obtain polyimide powder. The imidization rate of this polyimide was 74%, the number average molecular weight was 13,000, and the weight average molecular weight was 39,000. NMP was added to the obtained polyimide powder so that the solid concentration was 10 mass %, and M-1 was added so that the concentration was 1 mass % relative to the polyimide solid content, and the mixture was dissolved by stirring at 70°C for 12 hours to obtain a solution of polyimide (PI-V-2).
[0110] <Synthesis Example 3> In a four-neck flask equipped with a stirrer and a nitrogen inlet tube, 5.86g (24.0mmol) of DA-2, 5.46g (16.0mmol) of DA-10, 1.73g (16.0mmol) of DA-4, 7.69g (24.0mmol) of DA-1, and 194g of NMP were added and dissolved while feeding nitrogen. While stirring this diamine solution, 17.1g (76.4mmol) of CA-1 was added, and NMP was further added so that the solid concentration became 12% by mass. The mixture was stirred at 40°C for 24 hours to obtain a polyamic acid solution (viscosity: 549mPa·s). The molecular weight of the polyamic acid was 12,400 in number average molecular weight and 33,000 in weight average molecular weight. The polyamic acid solution (225 g) was diluted to 9.0% by mass with NMP, and then acetic anhydride (17.1 g) and pyridine (3.54 g) were added as imidization catalysts and reacted at 55° C. for 3 hours. The reaction solution was poured into methanol (1111 g), and the resulting precipitate was filtered off. The precipitate was washed with methanol and dried at 60° C. for 12 hours to obtain a polyimide powder. The imidization rate of the polyimide powder was 66%, the number average molecular weight was 11,000, and the weight average molecular weight was 28,000. NMP was added to the obtained polyimide powder so that the solid content concentration became 15% by mass, and the mixture was stirred at 70° C. for 24 hours to dissolve the mixture, thereby obtaining a solution of polyimide (PI-I-3).
[0111] <Synthesis Example 4> 5.73g (20.0mmol) of DA-5 was weighed out into a 5L four-neck flask equipped with a stirrer and a nitrogen inlet tube, 115g of NMP was added, and the mixture was stirred and dissolved while feeding nitrogen. While stirring this diamine solution under water cooling, 2.94g (15.0mmol) of CA-3 was added, 19.1g of NMP was added, and the mixture was stirred at 23°C under a nitrogen atmosphere for 1 hour. Then, 11.9g (40.0mmol) of DA-3 and 6.01g (40.0mmol) of DA-11 were weighed out, 172g of NMP was added, and the mixture was stirred and dissolved while feeding nitrogen. While stirring this diamine solution under water cooling, 15.9 g (81.0 mmol) of CA-3 was added, NMP was added so that the solid concentration became 15 mass%, s-1 was added so that the solid concentration became 1 mass% based on the polyamic acid solid content, and the mixture was stirred for 6 hours at 23°C under a nitrogen atmosphere to obtain a solution of polyamic acid (PAA-I-4). The molecular weight of the polyamic acid was a number average molecular weight of 12,000 and a weight average molecular weight of 30,000.
[0112] <Synthesis Example 5> A 500mL four-neck flask equipped with a stirrer was placed in a nitrogen atmosphere, and 2.80g (25.9mmol) of DA-4, 1.54g (6.47mmol) of DA12, 111g of NMP, and 6.18g (78.1mmol) of pyridine as a base were added and stirred to dissolve. Next, 9.89g (30.4mmol) of CE-1 was added while stirring this diamine solution, and reacted at 15°C overnight. After stirring overnight, 0.38g (4.21mmol) of E-1 was added and reacted at 15°C for 4 hours. The obtained polyamic acid ester solution was poured into 1230g of water while stirring, and the precipitated white precipitate was collected by filtration, followed by washing five times with 1230g of isopropyl alcohol (IPA) and drying to obtain 10.2g of white polyamic acid ester resin powder. The yield was 83.0%. The molecular weight of this polyamic acid ester was 20,786 in number average molecular weight and 40,973 in weight average molecular weight. GBL was added to the obtained polyamic acid ester so that the solid content concentration became 10 mass %, and the mixture was stirred at room temperature for 24 hours to dissolve, thereby obtaining a solution of polyamic acid ester (PAE-I-5).
[0113] <Synthesis Example 6> In a four-neck flask equipped with a stirrer and a nitrogen inlet tube, 0.46g (3.00mmol) of DA-8, 3.00g (15.0mmol) of DA-13, 2.56g (12.0mmol) of DA-14, 11.0g of NMP, and 8.10g of GBL were added and dissolved by stirring while feeding nitrogen. While stirring this diamine solution, 4.76g (24.0mmol) of CA-6 was added, and 10.9g of GBL was added, and the mixture was stirred at room temperature for 2 hours. Next, 10.8g of GBL was added and stirred, after which 1.31g (6.01mmol) of CA-5 was added, and 14.3g of GBL was added, and the mixture was stirred at room temperature for 24 hours. The viscosity of the obtained polyamic acid solution at 25°C was 2,041mPa·s. The molecular weight of the polyamic acid was a number average molecular weight of 14,200 and a weight average molecular weight of 30,110. Then, s-2 was added to the polyamic acid solid content to be 1 mass %. NMP and GBL were added so that the mixing ratio of NMP and GBL became NMP:GBL=20:80 by mass and the solid content concentration became 15 mass %, thereby obtaining a solution of polyamic acid (PAA-I-6).
[0114] <Synthesis Examples 7-11, 14-19> The diamines, tetracarboxylic acid derivatives, and organic solvents shown in Table 1 below were used, and the same procedures as those in the above synthesis examples were carried out to obtain solutions of polyimides (PI-V-8) to (PI-V-9), (PI-I-11), and (PI-V-19), polyamic acids (PAA-I-7), (PAA-I-10), (PAA-V-14) to (PAA-V-16), and (PAA-I-17) to (PAA-I-18) shown in Table 1 below. In Table 1, the numbers in parentheses represent the blending ratio (molar parts) of each compound relative to 100 mol parts of the total amount of tetracarboxylic acid derivatives used in the synthesis for the tetracarboxylic acid component, and the blending ratio (molar parts) of each compound relative to 100 mol parts of the total amount of diamines used in the synthesis for the diamine component. The terminal modifier represents the blending ratio (molar parts) relative to 100 mol parts of the total amount of diamines used in the synthesis. The organic solvents are expressed as the blending ratio (parts by mass) of each organic solvent relative to 100 parts by mass of the total amount of the organic solvents used in the synthesis.
[0115] [Table 1]
[0116] [Synthesis of other polymers] <Synthesis Example 12> According to the method described in paragraph
[0091] of JP 2018-054761 A, a reactive polyorganosiloxane polymer was obtained using 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (ECETS). Next, according to the method described in paragraph
[0093] of JP 2018-054761 A, a polyorganosiloxane polymer represented by the following formula (P-S1) was obtained. The numerical values indicate the proportion of each compound used relative to the total of each silane compound used in the synthesis. [ka]
[0117] <Synthesis Example 13> According to the method described in paragraph
[0091] of JP 2018-54761 A, a reactive polyorganosiloxane polymer was obtained using 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (ECETS). Next, according to the method described in paragraph
[0093] of JP 2018-54761 A, a polyorganosiloxane polymer represented by the following formula (P-S2) was obtained. The numerical values indicate the proportion of each compound used relative to the total of each silane compound used in the synthesis. [ka]
[0118] <Example 1> [Preparation of liquid crystal alignment agent] The solution of polyimide (PI-V-1) obtained in Synthesis Example 1 and the solution of polyimide (PI-V-2) obtained in Synthesis Example 2 were diluted with NMP and BCS, and further compound (b-1) was added so that the amount was 10 parts by mass relative to 100 parts by mass of all polymers, and stirred at room temperature. Next, the obtained solution was filtered through a filter with a pore size of 0.5 μm to obtain a liquid crystal alignment agent (V1) having a polymer component ratio of (PI-V-1):(PI-V-2)=30:70 (solid content equivalent mass ratio), a solvent composition ratio of NMP:BCS=60:40 (mass ratio), a polymer solid content concentration of 4.5%, and a compounding ratio of compound (b-1) of 10 parts by mass relative to a total of 100 parts by mass of polymer components (Table 2 below). It was confirmed that this liquid crystal alignment agent was a uniform solution without any abnormalities such as turbidity or precipitation.
[0119] <Examples 2 to 50 and Comparative Examples 1 to 5> Except for using the polymers and additives in Tables 2 to 6 below, the same procedure as in Example 1 was carried out to obtain liquid crystal alignment agents (V2) to (V11), (I12-P) to (I29-P), (I30-U) to (I37-U), (V38) to (V43), (I44-P) to (I47-P), (V48-P) to (V49-P), (I50-U), (R-V1) to (R-V2), (R-I3-P), (R-I4-U), and (R-V5). In Table 2, the numbers in parentheses indicate the blending ratio (parts by mass) of each polymer component or additive relative to the total of 100 parts by mass of the polymer components used in the preparation of the liquid crystal alignment agent, respectively, for the polymers and additives. For the organic solvents, the blending ratio (parts by mass) of each organic solvent relative to the total of 100 parts by mass of the organic solvents used in the preparation of the liquid crystal alignment agent is indicated.
[0120] [Table 2]
[0121] [Table 3]
[0122] [Table 4]
[0123] [Table 5]
[0124] [Table 6]
[0125] [Fabrication and evaluation of liquid crystal display elements] 1-1. Fabrication of vertically aligned liquid crystal display element Two 40mm x 30mm glass substrates with ITO electrodes (length: 40mm, width: 30mm, thickness: 1.1mm) were prepared and washed with pure water and isopropyl alcohol. Next, liquid crystal alignment agents (V1) to (V11), (V38) to (V43), (R-V1) to (R-V2), and (R-V5) filtered through a filter with a pore size of 1.0 μm were spin-coated on each ITO surface, and the substrates were heated at 70°C for 90 seconds on a hot plate and at 230°C for 30 minutes in a heat circulation type clean oven to obtain ITO substrates with a film having a thickness of 100 nm. Next, the periphery was coated with a sealant (Mitsui Chemicals, Inc., XN-1500T). Next, the other substrate was attached to the previous substrate with the side on which the liquid crystal alignment film was formed facing inward, and the sealant was cured to prepare an empty cell. Liquid crystal MLC-3023 (Merck, Inc.) was injected by the reduced pressure injection method into the empty cells using the liquid crystal alignment agents (V1)-(V2), (V5)-(V11), (V38)-(V43), and (R-V1) to prepare a liquid crystal cell. After that, a DC voltage of 15 V was applied to the obtained liquid crystal cell, and in the state where all pixel areas were driven, ultraviolet rays having a wavelength of 365 nm and passed through a band-pass filter were irradiated at 10 J / cm using an ultraviolet irradiation device using a high-pressure mercury lamp as a light source. 2 The amount of ultraviolet light irradiation was measured using a UV-M03A manufactured by ORC Corporation, connected to a UV-35 receiver. Liquid crystal MLC-6608 (Merck) was injected into the empty cells using the liquid crystal alignment agents (V3)-(V4), (R-V2) and (R-V5) by the reduced pressure injection method to obtain liquid crystal display elements for evaluation. When the obtained liquid crystal display elements were observed with a polarizing microscope, it was confirmed that the liquid crystal was uniformly aligned in all cases.
[0126] 1-2. Evaluation of liquid crystal display elements (i) Evaluation of accumulated charge The liquid crystal display element prepared in 1-1 above was subjected to a 30Hz, 7.8V DC power supply with 2V DC superimposed. p-pA square wave of 10 ... (ii) Voltage holding ratio evaluation The liquid crystal display element prepared in 1-1 above was left in an 80°C oven under the irradiation of an LED lamp for 200 hours, then left at room temperature to cool naturally to room temperature. After that, a voltage of 1V was applied at 60°C for 60 microseconds over a span of 1667 milliseconds, and the voltage retention rate was measured 1,000 milliseconds after the application was removed. A measuring device manufactured by Toyo Corporation was used. (iii) Scratch resistance evaluation A liquid crystal alignment film was prepared on a pair of glass substrates (length: 40 mm, width: 30 mm, thickness: 1.1 mm) using the same procedure as in 1-1 above. A scratch test was performed on each liquid crystal alignment film surface using UMT-2 (manufactured by Bruker AXS). The FVL was selected as the sensor for UMT-2, and a 1.6 mm sapphire ball was attached to the tip of the scratch section. With the tip of the scratched area in contact with the surface of the liquid crystal alignment film under a load of 40 mN, a scratch was made over an area of 0.5 mm wide and 2.0 mm long. The tip of the scratched area was moved back and forth horizontally at a speed of 5.0 mm / sec. The scratched area was moved vertically by moving the substrate with the liquid crystal alignment film vertically at a speed of 20 μm / sec. After the scratch test, liquid crystal (MLC-3019) was dropped onto the surface of the liquid crystal alignment film that had been subjected to the scratch test. Another substrate with a liquid crystal alignment film and 4 μm spacers were then placed on top of it so that the liquid crystal alignment film surfaces faced each other, and the dropped liquid crystal was sandwiched between them. The scratched area was observed under a polarizing microscope (ECLIPSE E600WPOL) (Nikon Corporation) with the polarization axes of the upper and lower polarizing plates at 90° (crossed Nicols) to observe whether light was transmitted. The scratched area was rated as "good" when no bright spots or light leakage were observed, and "poor" when the entire scratched area was light leakage, as shown in Tables 7 to 9.
[0127] 2-1. Fabrication of FFS-type liquid crystal display elements by photoalignment First, a substrate with electrodes was prepared. The substrate was a glass substrate with a size of 30 mm x 50 mm and a thickness of 0.7 mm. An ITO electrode with a solid pattern was formed on the substrate as the first layer, which constituted the counter electrode. A SiN (silicon nitride) film formed by a CVD method was formed on the first layer of the counter electrode as the second layer. The thickness of the second layer of the SiN film was 500 nm, and it functions as an interlayer insulating film. A comb-shaped pixel electrode formed by patterning the ITO film as the third layer was arranged on the second layer of the SiN film, forming two pixels, a first pixel and a second pixel. The size of each pixel was 10 mm in length and about 5 mm in width. At this time, the first layer of the counter electrode and the third layer of the pixel electrode were electrically insulated by the action of the second layer of the SiN film.
[0128] The pixel electrode of the third layer has a comb-like shape composed of multiple V-shaped electrode elements arranged with the center part bent at an internal angle of 160°. The width of each electrode element in the short direction is 3 μm, and the distance between the electrode elements is 6 μm. Since the pixel electrode forming each pixel is composed of multiple V-shaped electrode elements arranged with the center part bent, the shape of each pixel is not rectangular, but has a bold V-shaped shape that is bent in the center like the electrode elements. Each pixel is divided into upper and lower parts with the central bend as a boundary, and has a first region above the bent part and a second region below the bent part.
[0129] Next, the liquid crystal alignment agents (I12-P) to (I29-P), (I44-P) to (I47-P) and (R-I3-P) were filtered through a filter with a pore size of 1.0 μm, and then applied by spin coating to the above-mentioned electrode-attached substrate and a glass substrate having a 4 μm-high columnar spacer with an ITO film formed on the back surface. The coating films obtained from the liquid crystal alignment agents (I12-P) to (I29-P) and (R-I3-P) were dried on a hot plate at 80°C for 5 minutes and then baked in a hot air circulating oven at 230°C for 20 minutes to obtain a polyimide film with a thickness of 100 nm. Then, the coating surface was irradiated with 500 mJ / cm2 of linearly polarized ultraviolet light with an extinction ratio of 26:1 through a polarizer. 2 The coating was then irradiated and then baked in a hot air circulating oven at 230° C. for 30 minutes to obtain a substrate with a liquid crystal alignment film having a thickness of 100 nm. The coating films obtained from the liquid crystal alignment agents (I44-P) to (I47-P) were dried on a hot plate at 80°C for 5 minutes, and then the coating film was irradiated with 500 mJ / cm2 of linearly polarized ultraviolet light with an extinction ratio of 26:1 and a wavelength of 254 nm through a polarizer. 2 The coating was then irradiated and then baked in a hot air circulating oven at 230° C. for 30 minutes to obtain a substrate with a liquid crystal alignment film having a thickness of 100 nm. Next, a sealant was printed on one of the pair of glass substrates with liquid crystal alignment film, and the other substrate was attached so that the liquid crystal alignment film faces each other. The sealant was cured to prepare an empty cell. Liquid crystal MLC-3019 (Merck) was injected into this empty cell by the reduced pressure injection method, and the injection port was sealed to obtain an FFS-driven liquid crystal display element. The obtained liquid crystal cell was then heated at 120°C for 1 hour and left overnight before evaluation of the afterimage characteristics. When the obtained liquid crystal display elements were observed under a polarizing microscope, it was confirmed that the liquid crystal was uniformly oriented in all cases.
[0130] 2-2. Evaluation of liquid crystal display elements (i) Evaluation of accumulated charge The liquid crystal cell prepared in 2-1 above was used and placed between two polarizing plates arranged so that the polarization axes were perpendicular to each other. The pixel electrode and the counter electrode were short-circuited to have the same potential, and the LED backlight was irradiated from below the two polarizing plates. The angle of the liquid crystal cell was adjusted so that the brightness of the LED backlight transmitted light measured on the two polarizing plates was minimized. Next, while applying a square wave with a frequency of 30 Hz to this liquid crystal cell, the VT characteristics (voltage-transmittance characteristics) were measured at a temperature of 23°C, and the AC voltage at which the relative transmittance was 23% was calculated. Next, an AC voltage at which the relative transmittance was 23% at a temperature of 23°C and a square wave with a frequency of 30 Hz were applied for 5 minutes, and then a DC voltage of +1.0 V was superimposed and driven for 30 minutes. Then, the DC voltage was turned off, and again an AC voltage at which the relative transmittance was 23% and only a square wave with a frequency of 30 Hz was applied for 30 minutes. The evaluation was performed by defining the relative transmittance after 30 minutes of DC voltage superposition as "excellent" if it decreased to less than 27%, "good" if it decreased to 27% or more but less than 29%, and "poor" if the relative transmittance was 29% or more. (ii) Voltage holding ratio evaluation Two 40mm x 30mm glass substrates with ITO electrodes (length: 40mm, width: 30mm, thickness: 1.1mm) were prepared, and a liquid crystal alignment film with a thickness of 100nm was fabricated on the ITO surface using the same procedure as in 2-1 above. Bead spacers with a diameter of 4μm (manufactured by JGC Catalysts and Chemicals, Shinshikyu, SW-D1) were applied to the liquid crystal alignment film surface of one of the substrates. Next, the periphery was coated with a sealant (Mitsui Chemicals, Inc., XN-1500T). Next, the other substrate was laminated with the surface on which the liquid crystal alignment film was formed facing inward, and the sealant was cured to prepare an empty cell. Liquid crystal MLC-3019 (Merck, Inc., trade name) was injected into this empty cell by a reduced pressure injection method to prepare a liquid crystal display element. Next, this liquid crystal display element was left to stand for 200 hours in an 80°C oven under the irradiation of an LED lamp, and then left to stand at room temperature and naturally cooled to room temperature. Thereafter, evaluation was performed in the same manner as in 1-2 (ii). (iii) Scratch resistance evaluation The same procedure as in (iii) of 1-2 above was followed, except that the same liquid crystal alignment film as in 2-1 above was used and the liquid crystal was changed to MLC-3019.
[0131] 3-1. Fabrication of FFS-type liquid crystal display devices using rubbing alignment First, the liquid crystal alignment agents (I30-U) to (I37-U), (I50-U), and (R-I4-U) filtered through a filter with a pore size of 1.0 μm were applied to each surface of a pair of glass substrates similar to those in 2-1 above using an inkjet coating device (HIS-200, manufactured by Hitachi Plant Technologies, Ltd.). The coating was performed under the conditions of a coating area of 70 × 70 mm, a nozzle pitch of 0.423 mm, a scan pitch of 0.5 mm, a coating speed of 40 mm / sec, and a 60-second delay from coating to drying. Next, the substrate was dried on a hot plate at 80 ° C for 5 minutes, and then baked in a hot air circulation oven at 230 ° C for 20 minutes to obtain a polyimide film with a thickness of 100 nm. This polyimide film was rubbed with a rayon cloth (roller diameter: 120 mm, roller rotation speed: 500 rpm, moving speed: 30 mm / sec, pressing length: 0.3 mm, rubbing direction: inclined at 10° to the third layer IZO comb electrode), and then ultrasonically washed in pure water for 1 minute to remove water droplets. Then, it was dried at 80°C for 15 minutes to obtain a substrate with a liquid crystal alignment film. These two substrates with liquid crystal alignment film were combined into a set, and a sealant was printed on the substrate with a liquid crystal injection port remaining, and another substrate was attached so that the liquid crystal alignment film surfaces faced each other and the rubbing directions were antiparallel. Then, the sealant was cured to prepare an empty cell with a cell gap of 4 μm. Liquid crystal MLC-7026-100 (manufactured by Merck) was injected into this empty cell by a reduced pressure injection method, and the injection port was sealed to obtain an FFS type liquid crystal display element. The resulting liquid crystal display elements were then heated at 120° C. for 1 hour and left overnight at 23° C. before being used for evaluation of image retention. When the resulting liquid crystal display elements were observed under a polarizing microscope, it was confirmed that the liquid crystals were uniformly aligned in all cases.
[0132] 3-2. Evaluation of liquid crystal display elements (i) Evaluation of accumulated charge The liquid crystal display device prepared in the above 3-1 was used and evaluated in the same manner as in the above 2-2(i), except that the liquid crystal was changed to MLC-7026-100. (ii) Voltage holding ratio evaluation The same liquid crystal alignment film as in 3-1 above was used, and evaluation was carried out in the same manner as in (ii) of 2-2 above, except that the liquid crystal was MLC-7026-100. (iii) Scratch resistance evaluation The same liquid crystal alignment film as in 3-1 above was used, and evaluation was carried out in the same manner as in (iii) of 2-2 above, except that the liquid crystal was MLC-7026-100.
[0133] 4-1. Fabrication of VA-type liquid crystal display elements using photoalignment Two glass substrates similar to those in 1-1 above were prepared, and liquid crystal alignment agent (V48-P) or (V49-P) was spin-coated onto each substrate. The substrates were then heated at 80°C for 90 seconds on a hot plate and at 200°C for 40 minutes in a heat-circulating clean oven to obtain an ITO substrate with a liquid crystal alignment film having a thickness of 100 nm. The substrate is then exposed to linearly polarized UV light at an incidence angle of 40° relative to the normal to the substrate surface. The applied exposure dose is 20 mJ / cm 2 After exposure, a cell having two substrates was assembled so that the exposed alignment layer faced the inside of the cell, and the substrates were adjusted so that the alignment directions were parallel to each other. Next, liquid crystal MLC-7067 (Merck) was injected. After that, it was annealed at about 90°C for 10 minutes, cooled to room temperature, and then used for evaluation of image retention. When the obtained liquid crystal display element was observed with a polarizing microscope, it was confirmed that the liquid crystal was uniformly aligned in all cases.
[0134] 4-2. Evaluation of liquid crystal display elements (i) Evaluation of accumulated charge The liquid crystal display device prepared in the above 4-1 was evaluated in the same manner as in the above 1-2(i). The evaluation results are shown in Tables 7 to 9. (ii) Voltage holding ratio evaluation The same liquid crystal alignment film as in 4-1 above was used, and evaluation was carried out in the same manner as in 1-2(ii) above, except that the liquid crystal was MLC-7067. The evaluation results are shown in Tables 7 to 9. (iii) Scratch resistance evaluation The same liquid crystal alignment film as in 4-1 above was used, and evaluation was carried out in the same manner as in 1-2(iii) above, except that the liquid crystal was changed to MLC-7067. The evaluation results are shown in Tables 7 to 9.
[0135] [Table 7]
[0136] [Table 8]
[0137] [Table 9] [Industrial Applicability]
[0138] The liquid crystal aligning agent of the present invention is useful for forming liquid crystal alignment films in various liquid crystal display elements such as vertical alignment type and FFS driving type. The entire contents of the specification, claims and abstract of Japanese Patent Application No. 2019-044856, filed on March 12, 2019, are hereby incorporated by reference as the disclosure of the specification of the present invention.
Claims
1. A liquid crystal aligning agent comprising the following components (A) and (B): Component (A): A polymer (A) having at least one repeating unit selected from the group consisting of a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2): Component (B): A compound (B) having a molecular weight of 2000 or less, which has a partial structure represented by the following formula (b) in the molecule and is equipped with a basic site containing a nitrogen atom. [Formula 1] In formula (1), X 1 is a tetravalent organic group selected from the group consisting of the following formulae (4a) to (4n), (5a), and (6a): 1 is a divalent organic group. 1 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; Z 11 , Z 12 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an alkenyl group having 2 to 10 carbon atoms which may have a substituent, an alkynyl group having 2 to 10 carbon atoms which may have a substituent, a tert-butoxycarbonyl group, or a 9-fluorenylmethoxycarbonyl group. [chemical 2] * represents a bond, R 1 represents an alkanediyl group having 1 to 4 carbon atoms. 1 represents an integer of 1 to 2. [C3] x and y are single bonds, ethers, carbonyls, esters, alkanediyl groups having 1 to 5 carbon atoms, 1,4-phenylene, sulfonyl or amide groups. Z 1 to Z 6 each independently represent a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a benzene ring. j and k are 0 or 1. m is an integer of 1 to 5. * represents a bond.
2. A liquid crystal aligning agent comprising the following components (A) and (B): Component (A): A polymer (A) having at least one repeating unit selected from the group consisting of a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2): Component (B): A compound (B) having a molecular weight of 2000 or less, which has a partial structure represented by the following formula (b) in the molecule and is equipped with a basic site containing a nitrogen atom, The aforementioned compound, wherein the basic site has a structure selected from the group consisting of a secondary amine, a group in which one or two hydrogen atoms have been removed from a tertiary amine, and a nitrogen-containing heterocyclic group. [C4] In formula (1), X 1 is a tetravalent organic group, Y 1 is a divalent organic group. 1 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; Z 11 , Z 12 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an alkenyl group having 2 to 10 carbon atoms which may have a substituent, an alkynyl group having 2 to 10 carbon atoms which may have a substituent, a tert-butoxycarbonyl group, or a 9-fluorenylmethoxycarbonyl group. [C5] * represents a bond, R 1 represents an alkanediyl group having 1 to 4 carbon atoms. 1 represents an integer of 1 to 2.
3. Above X 1 The liquid crystal aligning agent according to claim 2, wherein is a tetravalent organic group selected from the group consisting of the following formulas (4a) to (4n), the following formula (5a), and the following formula (6a): [C6] x and y are a single bond, an ether, a carbonyl, an ester, an alkanediyl group having 1 to 5 carbon atoms, 1,4-phenylene, a sulfonyl or an amide group. 1 ~Z 6 each independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom, or a benzene ring. j and k are 0 or 1. m is an integer of 1 to 5. * represents a bond.
4. The polymer (A) is 1 is a tetravalent organic group selected from the group consisting of the above formulas (4a) to (4n), (5a) and (6a), and Y 1 The liquid crystal aligning agent according to claim 3, comprising one or more repeating units (repeating units (t)) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), in which R represents a divalent organic group, and the content of the repeating units (t) is 5 mol% or more in total based on all repeating units of the polymer (A).
5. The polymer (A) is X 1 is a tetravalent organic group, Y 1 The liquid crystal aligning agent according to any one of claims 1 to 4, comprising one or more repeating units selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), wherein R is a divalent organic group derived from a diamine having at least one selected from the group consisting of a nitrogen-containing heterocycle, a diphenylamine structure, and a triphenylamine structure, and the content of the one or more repeating units is 5 mol% or more in total with respect to all repeating units of the polymer (A).
6. The polymer (A) is Y 1 The liquid crystal aligning agent according to any one of claims 1 to 5, comprising one or more repeating units selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), wherein R is a divalent organic group derived from a diamine having at least one selected from the group consisting of a nitrogen-containing heterocycle, a diphenylamine structure, and a triphenylamine structure, and the content of the one or more repeating units is 5 mol% or more in total with respect to all repeating units of the polymer (A).
7. The polymer (A) is X 1 is a tetravalent organic group, Y 1The liquid crystal aligning agent according to any one of claims 1 to 6, comprising at least one repeating unit (a) selected from the group consisting of a repeating unit represented by the above formula (1) and a repeating unit represented by the above formula (2), wherein the repeating unit (a) is a divalent organic group derived from a diamine represented by the following formulas (V1) to (V3), and the content of the repeating unit (a) is 1 mol% or more in total with respect to all repeating units of the polymer (A). [C7] X is a single bond, —O—, —C(CH 3 ) 2 -, -NH-, -CO-, -NHCO-, -COO-, -(CH 2 ) m -, -SO 2 -, -O-(CH 2 ) m -O-, -OC(CH 3 ) 2 --, --CO--(CH 2 ) m -, -NH-(CH 2 ) m -, -SO 2 - (CH 2 ) m -, -CONH-(CH 2 ) m -, -CONH-(CH 2 ) m -NHCO- or -COO-(CH 2 ) m It represents —OCO—. X 1 and X 2 are each independently a single bond, -(CH 2 ) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -COO-, -OCO- or -((CH 2 ) a1 -A 1 ) m1 In this case, each of the multiple a1's is independently an integer of 1 to 15, and the multiple A's are each independently an integer of 1 to 15. 1 each independently represents an oxygen atom or -COO-; m 1 is 1 to 2. 3is a single bond, -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -CH 2 represents -O-, -COO- or -OCO-; 4 represents -CONH-, -NHCO-, -O-, -COO- or -OCO-. G 1 and G 2 each independently represents a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms or a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted with an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorine-containing alkyl group having 1 to 3 carbon atoms, a fluorine-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. k represents 0 or 1, m and n each independently represent an integer of 0 to 3, and the sum of m and n is 1 to 4. R 1 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms. 1 Any hydrogen in the formula may be replaced by fluorine. R 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms; R 2 Any hydrogen atom in the group R may be replaced by fluorine. 3 represents a structure having a steroid skeleton.
8. The polymer (A) is Y 1 The liquid crystal aligning agent according to any one of claims 1 to 7, comprising at least one repeating unit (a) selected from the group consisting of a repeating unit represented by the above formula (1) and a repeating unit represented by the above formula (2), wherein the repeating unit (a) is a divalent organic group derived from a diamine represented by the following formulas (V1) to (V3), and the content of the repeating unit (a) is 1 mol% or more in total with respect to all repeating units of the polymer (A). [C8] X is a single bond, —O—, —C(CH 3 ) 2 -, -NH-, -CO-, -NHCO-, -COO-, -(CH 2 ) m -, -SO 2 -, -O-(CH 2 ) m -O-, -OC(CH 3 ) 2 --, --CO--(CH 2 ) m -, -NH-(CH 2 ) m -, -SO 2 - (CH 2 ) m -, -CONH-(CH 2 ) m -, -CONH-(CH 2 ) m -NHCO- or -COO-(CH 2 ) m It represents —OCO—. X 1 and X 2 are each independently a single bond, -(CH 2 ) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -COO-, -OCO- or -((CH 2 ) a1 -A 1 ) m1 In this case, each of the multiple a1's is independently an integer of 1 to 15, and the multiple A's are each independently an integer of 1 to 15. 1 each independently represents an oxygen atom or -COO-; m 1 is 1 to 2. 3 is a single bond, -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -CH 2 represents -O-, -COO- or -OCO-; 4 represents -CONH-, -NHCO-, -O-, -COO- or -OCO-. G 1 and G 2each independently represents a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms or a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted with an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorine-containing alkyl group having 1 to 3 carbon atoms, a fluorine-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. k represents 0 or 1, m and n each independently represent an integer of 0 to 3, and the sum of m and n is 1 to 4. R 1 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms. 1 Any hydrogen in the formula may be replaced by fluorine. R 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms; R 2 Any hydrogen atom in the group R may be replaced by fluorine. 3 represents a structure having a steroid skeleton.
9. The polymer (A) is X 1 is a tetravalent organic group, Y 1 The liquid crystal aligning agent according to any one of claims 1 to 8, which contains one or more repeating units (repeating units (c)) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), which are divalent organic groups derived from diamines selected from the group consisting of p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylether, 4,4'-diaminoazobenzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]ether, 4,4'-bis(4-aminophenoxy)biphenyl, diamines represented by the following formula (H), and diamines represented by the following formulas (H2) to (H3), and the content of the repeating units (c) is 5 mol% or more in total, based on the total repeating units of the polymer (A). [C9] R 3 is -NRCO-, -COO-, -NRCONR-, or -(CH 2 ) n - (where n is an integer from 2 to 20), and any -CH 2 - may be replaced by -O-, -COO-, -ND-, -NRCO-, -NRCONR-, -NRCOO-, or -OCOO-. D represents a thermally detachable group, and R represents a hydrogen atom or a monovalent organic group. R 4 is a single bond or a benzene ring, and any hydrogen atom on the benzene ring may be replaced with a monovalent organic group. [C10] X 1 is -CO-, -O-, -COO-, -L 1 -R-L 2 - (L 1 , L 2 are each independently a single bond, an oxygen atom, or -COO-, and R is -(CH 2 ) n - (n is an integer from 1 to 12), or -NRCO- (R is a hydrogen atom or a methyl group), 2 represents a single bond, -NRCO- (R represents a hydrogen atom or a methyl group), or -COO-. n represents an integer of 1 or 2. Any hydrogen atom on the benzene ring may be replaced with a monovalent organic group. [C11] In the formula, two X's each independently represent -O-, -COO-, -NHCO-, -C(=O)-, or -(CH 2 ) n - (n is an integer from 1 to 12), L 1 , L 2 are each independently a single bond, -O-, or -COO-, and R is -CH 2 - or -(CH 2 ) n -(n is an integer from 2 to 12), or the above-(CH 2 ) n Any CH of - 2 represents a group in which an oxygen atom is substituted. Any hydrogen atom on the benzene ring may be replaced with a monovalent organic group.
10. The polymer (A) is Y 1 The liquid crystal aligning agent according to any one of claims 1 to 9, wherein the repeating unit (c) is selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), which are divalent organic groups derived from diamines selected from the group consisting of p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylether, 4,4'-diaminoazobenzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]ether, 4,4'-bis(4-aminophenoxy)biphenyl, diamines represented by the following formula (H), and diamines represented by the following formulas (H2) to (H3), and the content of the repeating unit (c) is 5 mol% or more in total, based on the total repeating units of the polymer (A). [C12] R 3 is -NRCO-, -COO-, -NRCONR-, or -(CH 2 ) n - (where n is an integer from 2 to 20), and any -CH 2 - may be replaced by -O-, -COO-, -ND-, -NRCO-, -NRCONR-, -NRCOO-, or -OCOO-. D represents a thermally detachable group, and R represents a hydrogen atom or a monovalent organic group. R 4 is a single bond or a benzene ring, and any hydrogen atom on the benzene ring may be replaced with a monovalent organic group. [C13] X 1 is -CO-, -O-, -COO-, -L 1 -R-L 2 - (L 1 , L 2 are each independently a single bond, an oxygen atom, or -COO-, and R is -(CH 2 ) n- (n is an integer from 1 to 12), or -NRCO- (R is a hydrogen atom or a methyl group), 2 represents a single bond, -NRCO- (R represents a hydrogen atom or a methyl group), or -COO-. n represents an integer of 1 or 2. Any hydrogen atom on the benzene ring may be replaced with a monovalent organic group. [C14] In the formula, two X's each independently represent -O-, -COO-, -NHCO-, -C(=O)-, or -(CH 2 ) n - (n is an integer from 1 to 12), L 1 , L 2 are each independently a single bond, -O-, or -COO-, and R is -CH 2 - or -(CH 2 ) n -(n is an integer from 2 to 12), or the above-(CH 2 ) n Any CH of - 2 represents a group in which an oxygen atom is substituted. Any hydrogen atom on the benzene ring may be replaced with a monovalent organic group.
11. The polymer (A) is X 1 is a tetravalent organic group, Y 1 The liquid crystal aligning agent according to any one of claims 1 to 10, comprising at least one repeating unit (b) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), wherein the repeating unit (b) is a divalent organic group derived from a diamine selected from the group consisting of diamines having a radical initiation function and diamines having a photopolymerizable group at their ends, and the content of the repeating unit (b) is 1 mol% or more in total with respect to the total repeating units of the polymer (A).
12. The polymer (A) comprises the repeating unit (a) defined in claim 7 and the repeating unit (b) defined in claim 11, and the upper limit of the content of the repeating unit (a) and the repeating unit (b) is 99 mol% or less, based on the total repeating units of the polymer (A). The liquid crystal aligning agent according to claim 11.
13. The polymer (A) is Y 1 The liquid crystal aligning agent according to any one of claims 1 to 12, comprising at least one repeating unit (b) selected from the group consisting of repeating units represented by the above formula (1) and repeating units represented by the above formula (2), wherein the repeating unit (b) is a divalent organic group derived from a diamine selected from the group consisting of diamines having a radical initiation function and diamines having a terminal photopolymerizable group, and the content of the repeating unit (b) is 1 mol% or more in total relative to the total repeating units of the polymer (A).
14. The liquid crystal alignment agent according to any one of claims 1 to 13, wherein the liquid crystal alignment agent further comprises polyorganosiloxane, and the polyorganosiloxane has at least one of an oxetanyl group and an oxiranyl group.
15. The liquid crystal aligning agent according to any one of claims 1 to 14, wherein the component (A) comprises two or more kinds of polymers (A).
16. The liquid crystal aligning agent according to any one of claims 1 to 15, wherein the content of the compound (B) is 0.1 to 40 parts by mass per 100 parts by mass of the component (A).
17. A liquid crystal alignment film obtained from the liquid crystal aligning agent according to any one of claims 1 to 16.
18. A liquid crystal display device comprising the liquid crystal alignment film according to claim 17.
Citation Information
Patent Citations
Azo compound, composition for optical alignment film, optical alignment film, and liquid crystal display element
JP2007138138A
Liquid crystal aligning agent, liquid crystal alignment layer, and liquid crystal display element
JP2008052260A
Composition for photo-alignment film and optically anisotropic material
JP2008076839A
Azo compound, composition for optical alignment film using same, and method for producing optical alignment film
WO2006003893A1
Composition for photo-alignment film, optically anisotropic material and method for producing same
WO2007055316A1