In-plane switching liquid crystal display element and method for manufacturing the in-plane switching liquid crystal cell
The horizontal electric field liquid crystal display element addresses transmittance and voltage holding issues by using a lower anchoring energy alignment film on the counter substrate, enhancing backlight transmittance and response speed while reducing burn-in.
Patent Information
- Application Number
- JP2021535362
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-29
- Filing Date
- 2020-07-28
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-07-28
AI Technical Summary
Existing liquid crystal display technologies face challenges such as reduced backlight light transmittance, non-uniform electric fields, and voltage holding ratio issues due to weak anchoring energy, leading to problems like disclination and image sticking, which affect battery consumption and image quality.
A horizontal electric field liquid crystal display element with a comb-teeth electrode substrate and a counter substrate, where the anchoring energy of the liquid crystal alignment film on the counter substrate is lower than that on the comb-teeth electrode substrate, using a weak anchoring treatment and radical polymerization of a liquid crystal alignment film on the counter substrate to stabilize the liquid crystal alignment.
The solution achieves high backlight light transmittance, fast response speed, and high voltage holding rate, reducing burn-in and improving image quality.
Smart Images

Figure 0007552597000029 
Figure 0007552597000030 
Figure 0007552597000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an in-plane switching liquid crystal display element that achieves both high-speed response and high backlight transmittance and has a high voltage holding ratio, and to a method for manufacturing an in-plane switching liquid crystal cell that can be used to manufacture the in-plane switching liquid crystal display element. [Background technology]
[0002] In recent years, liquid crystal display elements are widely used in displays for mobile phones, computers, and televisions. Liquid crystal display elements have characteristics such as thinness, light weight, and low power consumption, and are expected to be applied to further content in the future, such as VR (Virtual Reality) and ultra-high resolution displays. Various display modes have been proposed for liquid crystal displays, such as TN (Twisted Nematic), IPS (In-Plane Switching), and VA (Vertical Alignment), and all modes use a film (liquid crystal alignment film) that guides the liquid crystal into a desired alignment state.
[0003] In particular, for products equipped with touch panels such as tablet PCs, smartphones, and smart TVs, the IPS mode is preferred because it is less likely to distort the display when touched. In recent years, LCD display elements using FFS (Frindge Field Switching) and non-contact technology using optical alignment have come to be used to improve contrast and viewing angle characteristics.
[0004] In recent years, an IPS mode that utilizes something called weak anchoring has been proposed, and it has been reported that this method enables a significant improvement in transmittance and lower voltage driving compared to conventional IPS modes (see Patent Document 1). Specifically, this method uses a liquid crystal alignment film with strong anchoring energy on one of the substrates, and processes the other substrate equipped with the electrode that generates a lateral electric field so that it no longer has the ability to regulate the alignment of the liquid crystal, and uses these to create an IPS mode liquid crystal display element.
[0005] In recent years, a weak anchoring IPS mode technology has been proposed by creating a weak anchoring state using dense polymer brushes, etc. (Patent Documents 2 and 3). This technology has achieved a significant improvement in contrast ratio and a significant reduction in driving voltage. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 4053530 [Patent Document 2] JP 2013-231757 A [Patent Document 3] International Patent Application Publication No. 2019-004433 Brochure Summary of the Invention [Problem to be solved by the invention]
[0007] The above-mentioned technology using weak anchoring makes it possible to improve the transmittance in IPS mode, which is expected to resolve the problems of FFS mode such as Vcom shift and expensive substrate costs, but on the other hand, IPS mode has issues with miniaturizing the comb-tooth electrodes, and there are also problems such as difficulty in patterning quality control and poor yield. Therefore, it is thought that technology that can be applied to FFS is also required.
[0008] On the other hand, this technology has a problem that arises in principle, and in the FFS driving method, when the anchoring energy on the electrode substrate side is reduced, the transmittance of light from the backlight tends to deteriorate depending on the state of the liquid crystal at the interface of the weak anchoring film. Unlike IPS, FFS is known to have an uneven electric field application, and in particular, in cases where anchoring energy is generated even slightly in the polar angle direction under a weak anchoring state, the liquid crystal is not subjected to an orientation restriction force when in a weak anchoring state and can move with a weak force, so that the liquid crystal in the area close to the vertical electric field on the electrode substrate side, which normally does not move, moves, causing disclination, which is thought to result in a decrease in transmittance. Furthermore, when a polymerizable compound is added to liquid crystal to weaken the anchoring, it is considered that the additive may cause a decrease in the voltage holding ratio, image sticking, and the like. If these technical challenges can be resolved, it is likely that panel manufacturers will also benefit from reduced battery consumption and improved image quality.
[0009] The present invention has been made to solve the above-mentioned problems, and aims to provide a horizontal electric field liquid crystal display element that combines high-speed response with high backlight light transmittance, has a high voltage holding rate and is less susceptible to burn-in, and a horizontal electric field liquid crystal cell that can be used to manufacture such an electric field liquid crystal display element. [Means for solving the problem]
[0010] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved, and have completed the present invention having the following gist.
[0011] That is, the present invention includes the following. [1] A lateral electric field liquid crystal display element having a comb-tooth electrode substrate having a liquid crystal alignment film and an opposing substrate having a liquid crystal alignment film, with the two liquid crystal alignment films facing each other and liquid crystal filled between the liquid crystal alignment films, characterized in that the anchoring energy of the liquid crystal alignment film on the opposing substrate side is smaller than the anchoring energy of the liquid crystal alignment film on the comb-tooth electrode substrate side. [2] A horizontal electric field liquid crystal display element as described in [1], in which the liquid crystal alignment film on the comb-tooth electrode substrate side and the liquid crystal alignment film on the opposing substrate side are both liquid crystal alignment films that have been subjected to uniaxial alignment treatment, and only the liquid crystal alignment film on the opposing substrate side has been subjected to weak anchoring treatment. [3] The IPS liquid crystal display element according to [1] or [2], wherein the comb electrode substrate is an IPS substrate or an FFS substrate. [4] A horizontal electric field liquid crystal display element according to any one of [1] to [3], wherein the liquid crystal alignment film on the opposing substrate side is obtained by polymerizing the radical polymerizable compound in a state in which a liquid crystal composition containing the liquid crystal and a radical polymerizable compound is brought into contact with a radical generating film. [5] The in-plane switching liquid crystal display element according to [4], wherein the radical-generating film is a film having an organic group that induces radical polymerization fixed thereon. [6] The IPS LCD element according to [4] or [5], wherein the radical-generating film is made of a polymer containing an organic group that induces radical polymerization. [7] The horizontal electric field liquid crystal display element according to [6], wherein the polymer containing an organic group capable of inducing radical polymerization is at least one polymer selected from a polyimide precursor, a polyimide, a polyurea, and a polyamide obtained using a diamine component containing a diamine containing an organic group capable of inducing radical polymerization. [8] The lateral electric field liquid crystal display element according to [6] or [7], wherein the organic group capable of inducing radical polymerization is an organic group represented by the following structure [X-1] to [X-18], [W], [Y], or [Z]. [ka] (In formulas [X-1] to [X-18], * represents a bonding site, S1 and S2 each independently represent -O-, -NR-, or -S-, and R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms (among the alkyl groups having 1 to 10 carbon atoms, a portion of the -CH2- groups of the alkyl group having 2 to 10 carbon atoms may be replaced with an oxygen atom. However, in S2R or NR, when a portion of the -CH2- groups of the alkyl group are replaced with an oxygen atom, the oxygen atom is not directly bonded to S2 or N.) R 1 , and R 2 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms. [ka] (In the formulae [W], [Y], and [Z], * represents a bonding site, Ar represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, which may have an organic group and / or a halogen atom as a substituent, and R 9 and R 10 each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms; R 9 and R 10 When each of the alkyl groups is an alkyl group, they may be bonded to each other at the terminals to form a ring structure. Q represents any of the following structures. [ka] (In the formula, R 11 represents -CH2-, -NR-, -O-, or -S-, each R independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * indicates a bonding site. 3 represents a single bond, -O-, -NR- (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or -S-. R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms. [9] The IPS LCD element according to [7], wherein the diamine containing an organic group capable of inducing radical polymerization has a structure represented by the following general formula (6) or (7): [ka] (In formula (6), R 6 represents a single bond, -CH2-, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH3)-, -CON(CH3)-, or -N(CH3)CO-, R 7 represents a single bond, or an alkylene group having 1 to 20 carbon atoms which is unsubstituted or substituted by a fluorine atom, and one or more of any -CH2- or -CF2- in the alkylene group may be each independently replaced by a group selected from -CH=CH-, a divalent carbocycle, and a divalent heterocycle, and may further be replaced by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH-, or -NH-, provided that they are not adjacent to each other; R 8 represents a radical polymerization reactive group represented by a formula selected from the following formulas [X-1] to [X-18]. [ka] (In formulas [X-1] to [X-18], * represents a bonding site, S1 and S2 each independently represent -O-, -NR-, or -S-, and R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms (among the alkyl groups having 1 to 10 carbon atoms, a portion of the -CH2- groups of the alkyl group having 2 to 10 carbon atoms may be replaced with an oxygen atom. However, in S2R or NR, when a portion of the -CH2- groups of the alkyl group are replaced with an oxygen atom, the oxygen atom is not directly bonded to S2 or N.) R 1 , and R 2 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms. [ka] (In formula (7), T 1 and T 2each independently represents a single bond, -O-, -S-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH)-, -CON(CH)-, or -N(CH)CO-, S represents a single bond, or an alkylene group having 1 to 20 carbon atoms which is unsubstituted or substituted by a fluorine atom, and one or more of any -CH2- or -CF2- in the alkylene group may be each independently replaced by a group selected from -CH=CH-, a divalent carbocycle, and a divalent heterocycle, and may further be replaced by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH-, or -NH-, provided that these groups are not adjacent to each other; J is an organic group represented by a formula selected from the following formulae [W], [Y], and [Z]. [ka] (In the formulas [W], [Y], and [Z], * represents T 2 Ar represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, which may have an organic group and / or a halogen atom as a substituent; R 9 and R 10 each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, Q represents one of the following structures: [ka] (In the formula, R 11 represents -CH2-, -NR-, -O-, or -S-, each R independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * represents a bonding site; R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms. S 3 represents a single bond, -O-, -NR- (wherein R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or -S-.
[10] The horizontal electric field liquid crystal display element according to any one of [4] to [9], wherein at least one of the radical polymerizable compounds is a compound having one polymerizable reactive group in one molecule and is compatible with liquid crystal.
[11] The in-plane switching liquid crystal display element according to
[10] , wherein the polymerizable reactive group of the radical polymerizable compound is selected from the following structures: [ka] (In the formula, * indicates a binding site. R b represents a linear alkyl group having 2 to 8 carbon atoms, and E represents a bond selected from a single bond, -O-, -NRc-, -S-, an ester bond, and an amide bond. Rc represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[12] The horizontal electric field liquid crystal display element according to any one of [4] to
[11] , wherein the radical polymerizable compound is a radical polymerizable compound such that the Tg of the polymer obtained by polymerizing the radical polymerizable compound is 100°C or less.
[13] preparing a comb electrode substrate as a first substrate having a liquid crystal alignment film, and an opposing substrate as a second substrate having a radical generating film; creating a cell such that the radical generating film on the second substrate faces the first substrate; and A method for manufacturing an in-plane switching liquid crystal cell, comprising the step of filling a liquid crystal composition containing liquid crystal and a radical polymerizable compound between the first substrate and the second substrate.
[14] The method for manufacturing an in-plane switching liquid crystal cell according to
[13] , wherein the second substrate is a substrate coated with a liquid crystal alignment film having uniaxial alignment properties.
[15] The method for producing a lateral electric field liquid crystal cell according to
[14] , wherein the liquid crystal alignment film having uniaxial alignment is a liquid crystal alignment film for horizontal alignment.
[16] The method for producing a lateral electric field liquid crystal cell according to any one of
[13] to
[15] , wherein the comb electrode substrate is an IPS substrate or an FFS substrate. Effect of the Invention
[0012] The in-plane switching liquid crystal display element of the present invention is resistant to burn-in, and can achieve high backlight transmittance, fast response speed, and high voltage holding rate. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic cross-sectional view showing an example of a horizontal electric field liquid crystal display element of the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view showing another example of a horizontal electric field liquid crystal display element of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The in-plane electric field liquid crystal display element of the present invention is a in-plane electric field liquid crystal display element having a comb-tooth electrode substrate with a liquid crystal alignment film and an opposing substrate with a liquid crystal alignment film, with the two liquid crystal alignment films facing each other, and a liquid crystal composition filled between the two liquid crystal alignment films, characterized in that the anchoring energy of the liquid crystal alignment film on the opposing substrate side is smaller than the anchoring energy of the liquid crystal alignment film on the comb-tooth electrode substrate side. More preferably, the liquid crystal alignment film on the opposing substrate side is a weak anchoring film in a lateral electric field liquid crystal display element. In this specification, the anchoring energy refers to the anchoring energy in the in-plane direction of the liquid crystal alignment film, that is, the azimuthal anchoring energy. The azimuthal anchoring energy can be obtained, for example, by a method of estimating using the driving threshold voltage in the electro-optical response of the liquid crystal cell (Fredericks transition method), a method of estimating using the threshold voltage in the capacitance change (strong electric field method, capacitance method), a method of applying a strong magnetic field to the liquid crystal cell and evaluating the optical response of the liquid crystal, etc. (details are described in the Journal of the Japanese Liquid Crystal Society, Vol. 9. No. 4, 2005, Liquid Crystal Chemistry Experiment Course: Method of Measuring the Interfacial Anchoring Energy Coefficient). However, the above method has various prerequisites, and has only been studied with films having strong anchoring energy, and research is currently being conducted on how to accurately determine very weak anchoring energy.
[0015] FIG. 1 is a schematic cross-sectional view showing an example of a horizontal electric field liquid crystal display element of the present invention, which is an example of an IPS mode liquid crystal display element. In the in-plane electric field liquid crystal display element 1 illustrated in FIG. 1, liquid crystal 3 is sandwiched between a comb-tooth electrode substrate 2 having a liquid crystal alignment film 2c and a counter substrate 4 having a liquid crystal alignment film 4a. The comb-tooth electrode substrate 2 has a base material 2a, a plurality of linear electrodes 2b formed on the base material 2a and arranged in a comb-tooth shape, and a liquid crystal alignment film 2c formed on the base material 2a so as to cover the linear electrodes 2b. The counter substrate 4 has a base material 4b and a liquid crystal alignment film 4a formed on the base material 4b. In the in-plane electric field liquid crystal display element 1, the anchoring energy of the liquid crystal alignment film 4a on the counter substrate 4 side is smaller than the anchoring energy of the liquid crystal alignment film 2c on the comb-tooth electrode substrate 2 side. The liquid crystal alignment film 4a is, for example, a weak anchoring film obtained by chemically changing a radical-generating film. The liquid crystal alignment film on the counter substrate side is obtained, for example, by polymerizing the radical-polymerizing compound in a state in which a liquid crystal composition containing liquid crystal and a radical-polymerizing compound is contacted with the radical-generating film. In this IPS LCD element 1, when a voltage is applied to the linear electrodes 2b, an electric field is generated between the linear electrodes 2b as indicated by electric force lines L.
[0016] FIG. 2 is a schematic cross-sectional view showing another example of the in-plane switching liquid crystal display element of the present invention, which is an example of an FFS mode liquid crystal display element. In the lateral electric field liquid crystal display element 1 illustrated in FIG. 2, liquid crystal 3 is sandwiched between a comb-tooth electrode substrate 2 having a liquid crystal alignment film 2h and a counter substrate 4 having a liquid crystal alignment film 4a. The comb-tooth electrode substrate 2 has a base material 2d, a plane electrode 2e formed on the base material 2d, an insulating film 2f formed on the plane electrode 2e, a plurality of linear electrodes 2g formed on the insulating film 2f and arranged in a comb-tooth shape, and a liquid crystal alignment film 2h formed on the insulating film 2f so as to cover the linear electrodes 2g. The counter substrate 4 has a base material 4b and a liquid crystal alignment film 4a formed on the base material 4b. In the lateral electric field liquid crystal display element 1, the anchoring energy of the liquid crystal alignment film 4a on the counter substrate 4 side is smaller than the anchoring energy of the liquid crystal alignment film 2h on the comb-tooth electrode substrate 2 side. The liquid crystal alignment film 4a is, for example, a weak anchoring film obtained by chemically changing a radical generating film. The liquid crystal alignment film on the opposing substrate side can be obtained, for example, by bringing a liquid crystal composition containing liquid crystal and a radically polymerizable compound into contact with the radical-generating film and polymerizing the radically polymerizable compound. In this IPS LCD element 1, when a voltage is applied to the plane electrodes 2e and the linear electrodes 2g, an electric field is generated between the plane electrodes 2e and the linear electrodes 2g as indicated by electric field lines L.
[0017] A "weak anchoring film" is a film that has no orientation control force for liquid crystal molecules in the in-plane direction, or if there is any, it is weaker than the intermolecular force between liquid crystal molecules, and this film alone does not uniaxially align the liquid crystal molecules in any direction. In addition, this weak anchoring film is not limited to a solid film, but also includes a liquid film that covers a solid surface. Normally, a liquid crystal display element uses a film that controls the orientation of liquid crystal molecules, i.e., a liquid crystal alignment film, in pairs to align the liquid crystal, but the liquid crystal can also be aligned when this weak anchoring film and liquid crystal alignment film are used in pairs. This is because the orientation control force of the liquid crystal alignment film is transmitted in the thickness direction of the liquid crystal layer by the intermolecular force between the liquid crystal molecules, and as a result, the liquid crystal molecules close to the weak anchoring film are also aligned. Therefore, when a liquid crystal alignment film for horizontal alignment is used as the liquid crystal alignment film, a horizontal alignment state can be created throughout the entire liquid crystal cell. Horizontal alignment refers to a state in which the long axis of the liquid crystal molecules is aligned almost parallel to the liquid crystal alignment film surface, and an inclined alignment of several degrees is also included in the category of horizontal alignment.
[0018] The weak anchoring film can be obtained, for example, by polymerizing the polymerizable compound by UV or heat while contacting the liquid crystal containing a specific polymerizable compound with the radical-generating film. More specifically, the method for producing the weak anchoring film includes a step of preparing a cell having a liquid crystal composition containing liquid crystal and a radical-polymerizable compound between a first substrate having a liquid crystal alignment film and a second substrate having a radical-generating film, and a step of polymerizing the radical-polymerizable compound in the cell. Preferably, the method for producing a liquid crystal cell includes a step of preparing a first substrate having a liquid crystal alignment film and a second substrate having a radical-generating film, a step of preparing a cell so that the radical-generating film faces the first substrate, and a step of filling a liquid crystal composition containing liquid crystal and a radical-polymerizable compound between the first substrate and the second substrate. For example, the method for producing a low-voltage-driven in-plane switching liquid crystal display element includes a first substrate having no radical-generating film and a substrate having a liquid crystal alignment film that has been subjected to uniaxial alignment treatment, and a substrate having a comb-tooth electrode.
[0019] On the other hand, the weak anchoring state refers to a state in which there is a slight alignment control force, which is not strong enough to align the liquid crystal, but has optical anisotropy. The magnitude of the anchoring energy is about 10 -3 ~10 -6 (J / m 2 ) range. The weak anchoring state can be obtained, for example, by applying a method for producing a weak anchoring film to the second substrate having the radical generating film, which has been subjected to an alignment treatment. This alignment treatment may be performed by a rubbing method or photoalignment.
[0020] [Radical-generating film-forming composition] The radical-generating film-forming composition for forming the radical-generating film used in the present invention contains, for example, a polymer as a component and contains a group capable of generating radicals. In this case, the composition may contain a polymer to which a group capable of generating radicals is bonded, or may be a composition of a compound having a group capable of generating radicals and a polymer serving as a base resin. By applying and curing such a composition to form a film, a radical-generating film in which a group capable of generating radicals is fixed in the film can be obtained. The group capable of generating radicals is preferably an organic group that induces radical polymerization.
[0021] Examples of such organic groups that induce radical polymerization include organic groups represented by a formula selected from the above formulas [X-1] to [X-18], [W], [Y] and [Z]. Here, Ar in the formulae [W], [Y], and [Z] represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, and the aromatic hydrocarbon group may have an organic group and / or a halogen atom as a substituent. In R of the formulas [X-1] to [X-18], examples of the alkyl group having 2 to 10 carbon atoms in which some of the -CH2- groups may be replaced by oxygen atoms include alkoxy groups having 1 to 9 carbon atoms. However, R in S2R or NR is not an alkoxy group.
[0022] The polymer is preferably at least one polymer selected from the group consisting of, for example, a polyimide precursor, and polyimide, polyurea, polyamide, polyacrylate, polymethacrylate, and the like.
[0023] In order to obtain the radical generating film used in the present invention, when a polymer having an organic group that induces radical polymerization is used, in order to obtain a polymer having a group that can generate radicals, it is preferable to use, as a monomer component, a monomer having a photoreactive side chain containing at least one selected from a methacryl group, an acrylic group, a vinyl group, an allyl group, a coumarin group, a styryl group, and a cinnamoyl group, or a monomer having a site on the side chain that decomposes and generates radicals by ultraviolet irradiation. On the other hand, since the monomer that generates radicals may have problems such as spontaneously polymerizing itself and becoming an unstable compound, from the viewpoint of ease of synthesis, a polymer derived from a diamine having a radical generating site is preferable, and more preferably, a polyimide precursor such as polyamic acid or polyamic acid ester, polyimide, polyurea, polyamide, etc. are preferable.
[0024] Specific examples of such diamines containing a radical generating site include diamines having a side chain capable of generating radicals and polymerizing, such as the diamine represented by the above formula (6), but are not limited thereto.
[0025] The bonding positions of the two amino groups (-NH2) in formula (6) are not limited. Specifically, the bonding positions on the benzene ring relative to the bonding group of the side chain include the 2,3 position, the 2,4 position, the 2,5 position, the 2,6 position, the 3,4 position, and the 3,5 position. Among them, the 2,4 position, the 2,5 position, or the 3,5 position is preferable from the viewpoint of reactivity in synthesizing a polyamic acid. Taking into account the ease of synthesizing a diamine, the 2,4 position or the 3,5 position is more preferable.
[0026] Specific examples of diamines having a photoreactive group containing at least one selected from the group consisting of a methacryl group, an acrylic group, a vinyl group, an allyl group, a coumarin group, a styryl group, and a cinnamoyl group include, but are not limited to, the following compounds. [ka] (In the formula, J1 is a bonding group selected from a single bond, -O-, -COO-, -NHCO-, and -NH-; J 2 represents a single bond, or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms.
[0027] Diamines having a side chain having a moiety that decomposes upon irradiation with ultraviolet light to generate radicals include, but are not limited to, diamines represented by the above formula (7).
[0028] The bonding positions of the two amino groups (-NH2) in the above formula (7) are not limited. Specifically, the bonding positions on the benzene ring relative to the bonding group of the side chain include the 2,3 positions, the 2,4 positions, the 2,5 positions, the 2,6 positions, the 3,4 positions, and the 3,5 positions. Among them, the 2,4 positions, the 2,5 positions, and the 3,5 positions are preferred from the viewpoint of reactivity during synthesis of polyamic acid.
[0029] In particular, in view of ease of synthesis, versatility, properties, etc., structures represented by the following formulas are most preferable, but are not limited thereto. [ka] (In the formula, n is an integer of 2 to 8.)
[0030] The above diamines can be used alone or in combination of two or more depending on the properties such as liquid crystal alignment properties, sensitivity in the polymerization reaction, voltage retention properties, and stored charge when formed into a radical generating film.
[0031] The diamine having such a site where radical polymerization occurs is preferably used in an amount of 5 to 50 mol %, more preferably 10 to 40 mol %, and particularly preferably 15 to 30 mol %, of the total diamine components used in the synthesis of the polymer contained in the radical-generating film-forming composition.
[0032] When the polymer used in the radical generating film of the present invention is obtained from a diamine, other diamines than the diamine having the radical generating site can be used as the diamine component as long as the effect of the present invention is not impaired. Specifically, p-phenylenediamine, 2,3,5,6-tetramethyl-p-phenylenediamine, 2,5-dimethyl-p-phenylenediamine, m-phenylenediamine, 2,4-dimethyl-m-phenylenediamine, 2,5-diaminotoluene, 2,6-diaminotoluene, 2,5-diaminophenol, 2,4-diaminophenol, 3,5-diaminophenol, 3,5-diaminobenzyl alcohol, 2,4-diaminobenzyl alcohol, 4,6-diaminoresorcinol, 4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dihydroxy-4,4'-diaminobiphenyl, 3,3'-dicarboxy-4,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-diaminobiphenyl, 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 2,2'-diaminobiphenyl Phenyl, 2,3'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 2,2'-diaminodiphenylmethane, 2,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylether, 3,3'-diaminodiphenylether, 3,4'-diaminodiphenylether, 2,2'-diaminodiphenylether, 2,3'-diaminodiphenylether, 4,4'-sulfonyldianiline , 3,3'-sulfonyldianiline, bis(4-aminophenyl)silane, bis(3-aminophenyl)silane, dimethyl-bis(4-aminophenyl)silane, dimethyl-bis(3-aminophenyl)silane, 4,4'-thiodianiline, 3,3'-thiodianiline, 4,4'-diaminodiphenylamine, 3,3'-diaminodiphenylamine, 3,4'-diaminodiphenylamine, 2,2'-diaminodiphenylamine, 2,3'-diaminodiphenylamine, N-methyl(4,4'-diaminodiphenyl)amine, N-methyl(3,3'-diaminodiphenyl)amine, N-methyl(3,4'-diaminodiphenyl)amine, N-methyl(2,2'-diaminodiphenyl)amine, N-methyl(2,3'-diaminodiphenyl)amine, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 2,2'-diaminobenzophenone, 2,3'-diaminobenzophenone, 1,4-diaminonaphthalene, 1,5-diaminonaphthalene, 1,6-diaminonaphthalene, 1,7-diaminonaphthalene, 1,8-diaminonaphthalene, 2,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,7-diaminonaphthalene, 1,2-bis(4-aminophenyl)ethane, 1,2-bis(3-aminophenyl)ethane, 1,3-bis(4-aminophenyl)propane, 1,3-bis(3-aminophenyl)propane, 1,4-bis(4-aminophenyl)butane, 1,4-bis(3-aminophenyl)butane, bis(3,5-diethyl-4-aminophenyl)methane, 1,4-bis(4-aminophenoxy)benzene Zene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(4-aminobenzyl)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-[1,4-phenylenebis(methylene)]dianiline, 4,4'-[1,3-phenylenebis(methylene)]dianiline, 3,4'-[1,4-phenylenebis(methylene)]dianiline, 3,4'-[1,3-phenylenebis(methylene)]dianiline, 3,3'-[1,4 -phenylenebis(methylene)]dianiline, 3,3'-[1,3-phenylenebis(methylene)]dianiline, 1,4-phenylenebis[(4-aminophenyl)methanone], 1,4-phenylenebis[(3-aminophenyl)methanone], 1,3-phenylenebis[(4-aminophenyl)methanone], 1,3-phenylenebis[(3-aminophenyl)methanone], 1,4-phenylenebis(4-aminobenzoate), 1,4-phenylenebis(3-aminobenzoate), 1,3-phenylenebis(4-aminobenzoate), 1,3-phenylenebis(3-aminobenzoate), bis(4-aminophenyl)terephthalate, bis(3-aminophenyl)terephthalate, bis(4-aminophenyl)isophthalate, bis(3-aminophenyl)isophthalate, N,N'-(1,4-phenylene)bis(4-aminobenzamide), N,N'-(1,3-phenylene)bis(4-aminobenzamide), N,N'-(1,4-phenylene)bis(3-aminobenzamide), N,N'-(1,3-phenylene)bis(3-aminobenzamide), N,N'-bis(4-amino N,N'-bis(3-aminophenyl)terephthalamide, N,N'-bis(4-aminophenyl)isophthalamide, N,N'-bis(3-aminophenyl)isophthalamide, 9,10-bis(4-aminophenyl)anthracene, 4,4'-bis(4-aminophenoxy)diphenylsulfone, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 2,2'-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis(4-aminophenyl)hexafluoropropane propane, 2,2'-bis(3-aminophenyl)hexafluoropropane, 2,2'-bis(3-amino-4-methylphenyl)hexafluoropropane, 2,2'-bis(4-aminophenyl)propane, 2,2'-bis(3-aminophenyl)propane, 2,2'-bis(3-amino-4-methylphenyl)propane, trans-1,4-bis(4-aminophenyl)cyclohexane, 3,5-diaminobenzoic acid, 2,5-diaminobenzoic acid, bis(4-aminophenoxy)methane, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis (4-aminophenoxy)propane, 1,3-bis(3-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,4-bis(3-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,5-bis(3-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 1,6-bis(3-aminophenoxy)hexane, 1,7-bis(4-aminophenoxy)heptane, 1,7-bis(3-aminophenoxy)heptane, 1,8-bis(4-aminophenoxy)octane, 1,Aromatic diamines such as 8-bis(3-aminophenoxy)octane, 1,9-bis(4-aminophenoxy)nonane, 1,9-bis(3-aminophenoxy)nonane, 1,10-bis(4-aminophenoxy)decane, 1,10-bis(3-aminophenoxy)decane, 1,11-bis(4-aminophenoxy)undecane, 1,11-bis(3-aminophenoxy)undecane, 1,12-bis(4-aminophenoxy)dodecane, and 1,12-bis(3-aminophenoxy)dodecane; alicyclic diamines such as bis(4-aminocyclohexyl)methane and bis(4-amino-3-methylcyclohexyl)methane; 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, and 1,7-diaminoheptane. aliphatic diamines such as 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, and 1,12-diaminododecane; diamines having a urea structure such as 1,3-bis[2-(p-aminophenyl)ethyl]urea and 1,3-bis[2-(p-aminophenyl)ethyl]-1-tert-butoxycarbonylurea; diamines having a nitrogen-containing unsaturated heterocyclic structure such as Np-aminophenyl-4-p-aminophenyl(tert-butoxycarbonyl)aminomethylpiperidine; and diamines having an N-Boc group (Boc represents a tert-butoxycarbonyl group) such as N-tert-butoxycarbonyl-N-(2-(4-aminophenyl)ethyl)-N-(4-aminobenzyl)amine.
[0033] The above other diamines can be used alone or in combination of two or more depending on the properties such as liquid crystal alignment properties, sensitivity in the polymerization reaction, voltage retention properties, and stored charge when formed into a radical generating film.
[0034] In the synthesis of a polymer in the form of a polyamic acid, the tetracarboxylic dianhydride to be reacted with the diamine component is not particularly limited. Specific examples of the tetracarboxylic dianhydride include pyromellitic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 1,2,5,6-naphthalenetetracarboxylic acid, 1,4,5,8-naphthalenetetracarboxylic acid, 2,3,6,7-anthracenetetracarboxylic acid, 1,2,5,6-anthracenetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, bis(3,4-dicarboxyphenyl)ether, 3,3',4,4'-benzophenonetetracarboxylic acid, bis(3,4-dicarboxyphenyl)ether, bis(3,4-dicarboxy ... 2,2-bis(3,4-dicarboxyphenyl)sulfone, bis(3,4-dicarboxyphenyl)methane, 2,2-bis(3,4-dicarboxyphenyl)propane, 1,1,1,3,3,3-hexafluoro-2,2-bis(3,4-dicarboxyphenyl)propane, bis(3,4-dicarboxyphenyl)dimethylsilane, bis(3,4-dicarboxyphenyl)diphenylsilane, 2,3,4,5-pyridinetetracarboxylic acid, 2,6-bis(3,4-dicarboxyphenyl)pyridine, 3,3',4,4'-diphenylsulfonetetracarbo tetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, 1,3-diphenyl-1,2,3,4-cyclobutanetetracarboxylic acid, oxydiphthaltetracarboxylic acid, 1,2,3,4-cyclobutanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic acid, 1,2-dimethyl-1,2,3,4-cyclobutanetetracarboxylic acid, 1,3-dimethyl-1,2,3,4-cyclo 1,2,3,4-cycloheptanetetracarboxylic acid, 2,3,4,5-tetrahydrofurantetracarboxylic acid, 3,4-dicarboxy-1-cyclohexylsuccinic acid, 2,3,5-tricarboxycyclopentylacetic acid, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalenesuccinic acid, bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic acid, bicyclo[4,3,0]nonane-2,4,7,9-tetracarboxylic acid, bicyclo[4,4,0]decane-2,4,7,9-tetracarboxylic acid, bicyclo[4,4,0]decane-2,4,8,10-tetracarboxylic acid, tricyclo[6.3.0.0<2,6>]undecane-3,5,9,11-tetracarboxylic acid, 1,2,3,4-butanetetracarboxylic acid, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydrinaphthalene-1,2-dicarboxylic acid, bicyclo[2,2,2]oct-7-ene-2, Examples of the dianhydrides include tetracarboxylic acids such as 3,5,6-tetracarboxylic acid, 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexane-1,2-dicarboxylic acid, tetracyclo[6,2,1,1,0<2,7>]dodeca-4,5,9,10-tetracarboxylic acid, 3,5,6-tricarboxynorbornane-2:3,5:6 dicarboxylic acid, and 1,2,4,5-cyclohexanetetracarboxylic acid.
[0035] Of course, one or more kinds of tetracarboxylic dianhydrides may be used in combination depending on the properties such as liquid crystal alignment properties, sensitivity in polymerization reaction, voltage retention properties, and accumulated charge when used as a radical generating film.
[0036] In the synthesis of a polyamic acid ester polymer, the structure of the tetracarboxylic acid dialkyl ester reacted with the above diamine component is not particularly limited, but specific examples are given below. Specific examples of the aliphatic tetracarboxylic acid diester include 1,2,3,4-cyclobutane tetracarboxylic acid dialkyl ester, 1,2-dimethyl-1,2,3,4-cyclobutane tetracarboxylic acid dialkyl ester, 1,3-dimethyl-1,2,3,4-cyclobutane tetracarboxylic acid dialkyl ester, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic acid dialkyl ester, 1,2,3,4-cyclopentane tetracarboxylic acid dialkyl ester, 2,3,4,5-tetrahydrofuran tetracarboxylic acid dialkyl ester, 1,2,4,5-cyclohexane tetracarboxylic acid dialkyl ester, 3,4-dicarboxy-1-cyclohexyl succinic acid dialkyl ester, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic acid dialkyl ester, 1,2,3,4-butane tetracarboxylic acid dialkyl ester, esters, bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic acid dialkyl esters, 3,3',4,4'-dicyclohexyl tetracarboxylic acid dialkyl esters, 2,3,5-tricarboxycyclopentyl acetate dialkyl esters, cis-3,7-dibutylcycloocta-1,5-diene-1,2,5,6-tetracarboxylic acid dialkyl esters, tricyclo[4.2.1.0<2,5>]nonane-3,4 ,7,8-tetracarboxylic acid-3,4:7,8-dialkyl ester, hexacyclo[6.6.0.1<2,7>.0<3,6>.1<9,14>.0<10,13>]hexadecane-4,5,11,12-tetracarboxylic acid-4,5:11,12-dialkyl ester, and 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarbon dialkyl ester.
[0037] Examples of aromatic tetracarboxylic acid dialkyl esters include pyromellitic acid dialkyl esters, 3,3',4,4'-biphenyl tetracarboxylic acid dialkyl esters, 2,2',3,3'-biphenyl tetracarboxylic acid dialkyl esters, 2,3,3',4-biphenyl tetracarboxylic acid dialkyl esters, 3,3',4,4'-benzophenone tetracarboxylic acid dialkyl esters, 2,3,3',4'-benzophenone tetracarboxylic acid dialkyl esters, bis(3,4-dicarboxyphenyl)ether dialkyl esters, bis(3,4-dicarboxyphenyl)sulfone dialkyl esters, 1,2,5,6-naphthalene tetracarboxylic acid dialkyl esters, and 2,3,6,7-naphthalene tetracarboxylic acid dialkyl esters.
[0038] In the synthesis of a polyurea polymer, the diisocyanate to be reacted with the diamine component is not particularly limited, and can be used depending on availability, etc. Specific structures of diisocyanates are shown below. [ka] R in the formula 22 , and R 23 represents an aliphatic hydrocarbon group having 1 to 10 carbon atoms.
[0039] Aliphatic diisocyanates shown in K-1 to K-5 have the advantage of being inferior in reactivity but improving solvent solubility, while aromatic diisocyanates shown in K-6 to K-13 have high reactivity and the effect of improving heat resistance, but have the disadvantage of reducing solvent solubility. In terms of versatility and properties, K-1, K-7, K-8, K-9, and K-10 are preferred, while K-12 is preferred from the viewpoint of electrical properties, and K-13 is preferred from the viewpoint of liquid crystal alignment. Two or more diisocyanates can be used in combination, and it is preferable to apply them in various ways depending on the properties to be obtained. In addition, a part of the diisocyanate may be replaced with the above-described tetracarboxylic dianhydride, and the polyimide may be used in the form of a copolymer of polyamic acid and polyurea, or may be used in the form of a copolymer of polyimide and polyurea by chemical imidization.
[0040] In the synthesis of a polyamide polymer, the structure of the dicarboxylic acid to be reacted is not particularly limited, but specific examples are as follows: Aliphatic dicarboxylic acids include dicarboxylic acids such as malonic acid, oxalic acid, dimethylmalonic acid, succinic acid, fumaric acid, glutaric acid, adipic acid, muconic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, 2,2-dimethylglutaric acid, 3,3-diethylsuccinic acid, azelaic acid, sebacic acid, and suberic acid.
[0041] Examples of alicyclic dicarboxylic acids include 1,1-cyclopropanedicarboxylic acid, 1,2-cyclopropanedicarboxylic acid, 1,1-cyclobutanedicarboxylic acid, 1,2-cyclobutanedicarboxylic acid, 1,3-cyclobutanedicarboxylic acid, 3,4-diphenyl-1,2-cyclobutanedicarboxylic acid, 2,4-diphenyl-1,3-cyclobutanedicarboxylic acid, 1-cyclobutene-1,2-dicarboxylic acid, 1-cyclobutene-3,4-dicarboxylic acid, 1,1-cyclopentanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,1-cyclohexane ...3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid Examples of the dicarboxylic acid include cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,4-(2-norbornene)dicarboxylic acid, norbornene-2,3-dicarboxylic acid, bicyclo[2.2.2]octane-1,4-dicarboxylic acid, bicyclo[2.2.2]octane-2,3-dicarboxylic acid, 2,5-dioxo-1,4-bicyclo[2.2.2]octanedicarboxylic acid, 1,3-adamantanedicarboxylic acid, 4,8-dioxo-1,3-adamantanedicarboxylic acid, 2,6-spiro[3.3]heptanedicarboxylic acid, 1,3-adamantanediacetic acid, and camphoric acid.
[0042] Aromatic dicarboxylic acids include o-phthalic acid, isophthalic acid, terephthalic acid, 5-methylisophthalic acid, 5-tert-butylisophthalic acid, 5-aminoisophthalic acid, 5-hydroxyisophthalic acid, 2,5-dimethylterephthalic acid, tetramethylterephthalic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-anthracenedicarboxylic acid, 1,4-anthraquinonedicarboxylic acid, 2,5-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 1,5-biphenylenedicarboxylic acid, 4,4' '-Terphenyldicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylethanedicarboxylic acid, 4,4'-diphenylpropanedicarboxylic acid, 4,4'-diphenylhexafluoropropanedicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-bibenzyldicarboxylic acid, 4,4'-stilbenedicarboxylic acid, 4,4'-trans dicarboxylic acid, 4,4'-carbonyldibenzoic acid, 4,4'-sulfonyldibenzoic acid, 4,4'-dithiodibenzoic acid, p Examples of dicarboxylic acids include 4-carboxycinnamic acid, p-phenylenediacrylic acid, 3,3'-[4,4'-(methylenedi-p-phenylene)]dipropionic acid, 4,4'-[4,4'-(oxydi-p-phenylene)]dipropionic acid, 4,4'-[4,4'-(oxydi-p-phenylene)]dibutyric acid, (isopropylidenedi-p-phenylenedioxy)dibutyric acid, and bis(p-carboxyphenyl)dimethylsilane.
[0043] Examples of dicarboxylic acids containing a heterocycle include 1,5-(9-oxofluorene)dicarboxylic acid, 3,4-furandicarboxylic acid, 4,5-thiazoledicarboxylic acid, 2-phenyl-4,5-thiazoledicarboxylic acid, 1,2,5-thiadiazole-3,4-dicarboxylic acid, 1,2,5-oxadiazole-3,4-dicarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 2,5-pyridinedicarboxylic acid, 2,6-pyridinedicarboxylic acid, 3,4-pyridinedicarboxylic acid, and 3,5-pyridinedicarboxylic acid.
[0044] The above-mentioned various dicarboxylic acids may have an acid dihalide or anhydrous structure. These dicarboxylic acids are preferably dicarboxylic acids capable of giving a polyamide having a linear structure, in order to maintain the alignment of liquid crystal molecules. Among these, terephthalic acid, isoterephthalic acid, 1,4-cyclohexanedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylethanedicarboxylic acid, 4,4'-diphenylpropanedicarboxylic acid, 4,4'-diphenylhexafluoropropanedicarboxylic acid, 2,2-bis(phenyl)propanedicarboxylic acid, 4,4-terphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,5-pyridinedicarboxylic acid, or acid dihalides thereof are preferably used. Some of these compounds have isomers, and mixtures containing them may be used. Two or more compounds may be used in combination. The dicarboxylic acids used in the present invention are not limited to the above-mentioned exemplary compounds.
[0045] A known synthesis method can be used to obtain polyamic acid, polyamic acid ester, polyurea, or polyamide by reacting a diamine (also referred to as a "diamine component") as a raw material with a component selected from a tetracarboxylic dianhydride (also referred to as a "tetracarboxylic dianhydride component"), a tetracarboxylic diester, a diisocyanate, and a dicarboxylic acid as raw materials. Generally, the method involves reacting a diamine component with one or more components selected from a tetracarboxylic dianhydride component, a tetracarboxylic diester, a diisocyanate, and a dicarboxylic acid in an organic solvent.
[0046] The reaction between the diamine component and the tetracarboxylic dianhydride component is advantageous in that it proceeds relatively easily in an organic solvent and does not produce by-products.
[0047] The organic solvent used in the reaction is not particularly limited as long as the polymer produced is soluble in the organic solvent. Furthermore, even if the polymer is not soluble in the organic solvent, it may be mixed with the above-mentioned solvent to the extent that the polymer produced does not precipitate. Note that, since the moisture in the organic solvent inhibits the polymerization reaction and further causes the polymer produced to be hydrolyzed, it is preferable to use the organic solvent that has been dehydrated and dried.
[0048] Examples of the organic solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, N-methylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, N-methylcaprolactam, dimethylsulfoxide, tetramethylurea, pyridine, dimethylsulfone, hexamethylsulfoxide, γ-butyrolactone, isopropyl alcohol, methoxymethylpentanol, dipentaerythritol, methylsulfonyl ether ... ethyl amyl ketone, methyl nonyl ketone, methyl ethyl ketone, methyl isoamyl ketone, methyl isopropyl ketone, methyl cellosolve, ethyl cellosolve, methyl cellosolve acetate, butyl cellosolve acetate, ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol monobutyl ether, propylene glycol tert-butyl ether, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methylcyclohexene, propyl ether, dihexyl ether, dioxane, n-hexane, n-pentane, n-octane,Examples of the organic solvent include diethyl ether, cyclohexanone, ethylene carbonate, propylene carbonate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol monoethyl ether acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, diglyme, 4-hydroxy-4-methyl-2-pentanone, and 2-ethyl-1-hexanol. These organic solvents may be used alone or in combination.
[0049] When the diamine component and the tetracarboxylic dianhydride component are reacted in an organic solvent, any of the following methods may be used: a solution in which the diamine component is dispersed or dissolved in an organic solvent is stirred, and the tetracarboxylic dianhydride component is added as is or after being dispersed or dissolved in an organic solvent; a method in which the diamine component is added to a solution in which the tetracarboxylic dianhydride component is dispersed or dissolved in an organic solvent; a method in which the tetracarboxylic dianhydride component and the diamine component are added alternately; etc. In addition, when the diamine component or the tetracarboxylic dianhydride component is composed of a plurality of kinds of compounds, they may be reacted in a premixed state, or may be reacted individually in sequence, and low molecular weight compounds that have been reacted individually may be mixed and reacted to form a high molecular weight compound.
[0050] The temperature at which the diamine component and the tetracarboxylic dianhydride component are reacted can be selected arbitrarily, for example, within the range of −20 to 100° C., and preferably −5 to 80° C. The reaction can be carried out at an arbitrary concentration, and for example, the total amount of the diamine component and the tetracarboxylic dianhydride component relative to the reaction liquid is 1 to 50% by mass, and preferably 5 to 30% by mass.
[0051] In the above polymerization reaction, the ratio of the total number of moles of the tetracarboxylic dianhydride components to the total number of moles of the diamine components can be selected at any value depending on the molecular weight of the polyamic acid to be obtained. As in the case of a normal polycondensation reaction, the closer this molar ratio is to 1.0, the larger the molecular weight of the polyamic acid to be produced. The preferred range is 0.8 to 1.2.
[0052] The method for synthesizing the polymer used in the present invention is not limited to the above-mentioned method. When synthesizing a polyamic acid, a tetracarboxylic acid derivative such as a tetracarboxylic acid or a tetracarboxylic acid dihalide having a corresponding structure can be used instead of the above-mentioned tetracarboxylic acid dianhydride in the same manner as in the general polyamic acid synthesis method, and the corresponding polyamic acid can be obtained by reacting them by a known method. In addition, when synthesizing a polyurea, a diamine can be reacted with a diisocyanate. When producing a polyamic acid ester or polyamide, a diamine and a component selected from a tetracarboxylic acid diester and a dicarboxylic acid can be reacted with a diamine in the presence of a known condensing agent or after being derived into an acid halide by a known method.
[0053] The method of imidizing the above-mentioned polyamic acid to obtain a polyimide includes thermal imidization in which a solution of polyamic acid is heated as is, and catalytic imidization in which a catalyst is added to a solution of polyamic acid. The imidization rate from polyamic acid to polyimide is preferably 30% or more because it can increase the voltage holding rate, while it is preferably 80% or less from the viewpoint of whitening characteristics, i.e., suppressing precipitation of the polymer in the varnish.
[0054] The temperature when thermally imidizing the polyamic acid in a solution is usually 100 to 400° C., preferably 120 to 250° C., and it is preferable to carry out the imidization while removing water generated by the imidization reaction from the system.
[0055] The catalytic imidization of polyamic acid can be carried out by adding a basic catalyst and an acid anhydride to a solution of polyamic acid and stirring the mixture at -20 to 250°C, preferably 0 to 180°C. The amount of the basic catalyst is usually 0.5 to 30 times by mole, preferably 2 to 20 times by mole, the amount of the acid anhydride is usually 1 to 50 times by mole, preferably 3 to 3 .... Examples of the basic catalyst include pyridine, triethylamine, trimethylamine, tributylamine, trioctylamine, etc., and among these, pyridine is preferred because it has a suitable basicity for promoting the reaction. Examples of the acid anhydride include acetic anhydride, trimellitic anhydride, pyromellitic anhydride, etc., and among these, acetic anhydride is preferred because it facilitates purification after the reaction. The imidization rate by catalytic imidization can be controlled by adjusting the amount of the catalyst, the reaction temperature, the reaction time, etc.
[0056] When recovering the polymer generated from the reaction solution of the polymer, the reaction solution may be poured into a poor solvent to cause precipitation. Examples of poor solvents used for precipitation include methanol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, benzene, and water. The polymer precipitated by pouring into the poor solvent can be recovered by filtration, and then dried at room temperature or by heating under normal or reduced pressure. In addition, the polymer precipitated and recovered can be redissolved in an organic solvent and the reprecipitation and recovery operation can be repeated 2 to 10 times to reduce impurities in the polymer. Examples of poor solvents in this case include alcohols, ketones, and hydrocarbons, and it is preferable to use three or more poor solvents selected from these because the efficiency of purification is further improved.
[0057] In addition, when the radical-generating film is made of a polymer containing an organic group that induces radical polymerization, the radical-generating film-forming composition used in the present invention may contain a polymer other than the polymer containing an organic group that induces radical polymerization. In this case, the content of the other polymer in the total polymer components is preferably 5 to 95 mass %, more preferably 30 to 70 mass %.
[0058] The molecular weight of the polymer in the radical-generating film-forming composition is preferably 5,000 to 1,000,000, and more preferably 10,000 to 150,000, in terms of weight-average molecular weight measured by GPC (Gel Permeation Chromatography), taking into consideration the strength of the radical-generating film obtained by applying the radical-generating film, the workability during film formation, the uniformity of the film, and the like.
[0059] When the radical-generating film used in the present invention is obtained by applying a composition of a compound having a radical-generating group and a polymer, curing the composition to form a film and fixing the polymer in the film, the polymer may be at least one polymer selected from the group consisting of a polyimide precursor produced according to the above-mentioned production method, and polyimide, polyurea, polyamide, polyacrylate, polymethacrylate, etc., and the diamine having a site where radical polymerization occurs is 0 mol% of the total diamine components used to synthesize the polymer to be contained in the radical-generating film-forming composition. Examples of the compound having a radical-generating group to be added at this time include the following.
[0060] The compound that generates radicals when heated is a compound that generates radicals when heated to a temperature equal to or higher than its decomposition temperature. Examples of such radical thermal polymerization initiators include ketone peroxides (methyl ethyl ketone peroxide, cyclohexanone peroxide, etc.), diacyl peroxides (acetyl peroxide, benzoyl peroxide, etc.), hydroperoxides (hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, etc.), dialkyl peroxides (di-tert-butyl peroxide, dicumyl peroxide, dilauroyl peroxide, etc.), peroxyketals (dibutylperoxycyclohexane, etc.), alkyl peresters (peroxyneodecanoic acid-tert-butyl ester, peroxypivalic acid-tert-butyl ester, peroxy2-ethylcyclohexanoic acid-tert-amyl ester, etc.), persulfates (potassium persulfate, sodium persulfate, ammonium persulfate, etc.), and azo compounds (azobisisobutyronitrile, 2,2'-di(2-hydroxyethyl)azobisisobutyronitrile, etc.). Such radical thermal polymerization initiators can be used alone or in combination of two or more.
[0061] The compound that generates radicals by light is not particularly limited as long as it is a compound that initiates radical polymerization by light irradiation. Examples of such radical photopolymerization initiators include benzophenone, Michler's ketone, 4,4'-bis(diethylamino)benzophenone, xanthone, thioxanthone, isopropylxanthone, 2,4-diethylthioxanthone, 2-ethylanthraquinone, acetophenone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-2-methyl-4'-isopropylpropiophenone, 1-hydroxycyclohexylphenyl ketone, isopropyl benzoin ether, and isobutyl benzoin ether. , 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, camphorquinone, benzanthrone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 4-dimethylaminobenzoic acid ethyl, 4-dimethylaminobenzoic acid isoamyl, 4,4'-di(t-butylperoxycarbonyl)benzophenone, 3,4,4'-tri(t-butylperoxycarbonyl)benzophenone nyl)benzophenone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2-(4'-methoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(3',4'-dimethoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2',4'-dimethoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2'-methoxystyryl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4'-pentyloxystyryl) p-dimethylaminostyryl)-4,6-bis(trichloromethyl)-s-triazine, 4-[pN,N-di(ethoxycarbonylmethyl)]-2,6-di(trichloromethyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(2'-chlorophenyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(4'-methoxyphenyl)-s-triazine, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzthiazole, 2-mercaptobenzothiazole, 3,3'-Carbonylbis(7-diethylaminocoumarin), 2-(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetrakis(4-ethoxycarbonylphenyl)-1,2'-biimidazole, 2,2'-bis(2,4-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2, 4-dibromophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 3-(2-methyl-2-dimethylaminopropionyl)carbazole, 3,6-bis(2-methyl-2-morpholinopropionyl)-9-n-dodecylcarbazole, 1-hydroxycyclohexyl phenyl ketone, bis( 5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 3,3',4,4'-tetra(t-hexylperoxycarbonyl)benzophenone, 3,3'-di(methoxycarbonyl)-4,4'-di(t-butylperoxycarbonyl)benzophenone, 3,4'-di(meth Examples of the compound include 4,4'-di(methoxycarbonyl)-3,3'-di(t-butylperoxycarbonyl)benzophenone, 2-(3-methyl-3H-benzothiazol-2-ylidene)-1-naphthalen-2-yl-ethanone, and 2-(3-methyl-1,3-benzothiazol-2(3H)-ylidene)-1-(2-benzoyl)ethanone. These compounds may be used alone or in combination of two or more.
[0062] Even when the radical-generating film is made of a polymer containing an organic group that induces radical polymerization, it may contain a compound having a group that generates the above-mentioned radicals for the purpose of promoting radical polymerization when energy is applied.
[0063] The radical-generating film-forming composition may contain an organic solvent that dissolves or disperses the polymer component, and if necessary, the radical generator and other components. There is no particular limitation on such organic solvent, and examples thereof include the organic solvents exemplified in the synthesis of the polyamic acid described above. Among them, N-methyl-2-pyrrolidone, γ-butyrolactone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, etc. are preferred from the viewpoint of solubility. In particular, N-methyl-2-pyrrolidone or N-ethyl-2-pyrrolidone is preferred, but a mixed solvent of two or more kinds may be used.
[0064] In addition, it is preferable to use a solvent that improves the uniformity and smoothness of the coating film by mixing it with an organic solvent in which the components contained in the radical-generating film-forming composition are highly soluble.
[0065] Examples of solvents that improve the uniformity and smoothness of the coating film include isopropyl alcohol, methoxymethyl pentanol, methyl cellosolve, ethyl cellosolve, butyl cellosolve, methyl cellosolve acetate, butyl cellosolve acetate, ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethyl carbitol acetate, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol monobutyl ether, propylene glycol-tert-butyl ether, dipropylene glycol monomethyl ether, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and dipropylene glycol monoethyl ether. , dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methylcyclohexene, propyl ether, dihexyl ether, n-hexane, n-pentane n-octane, diethyl ether, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol monoethyl ether acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, 1-butoxy-2-propanol,Examples of the solvent include 1-phenoxy-2-propanol, propylene glycol monoacetate, propylene glycol diacetate, propylene glycol-1-monomethyl ether-2-acetate, propylene glycol-1-monoethyl ether-2-acetate, dipropylene glycol, 2-(2-ethoxypropoxy)propanol, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isoamyl lactate, and 2-ethyl-1-hexanol. A plurality of these solvents may be mixed. When using these solvents, the amount is preferably 5 to 80% by mass, more preferably 20 to 60% by mass, of the total solvent contained in the liquid crystal alignment agent.
[0066] The radical-generating film-forming composition may contain components other than those mentioned above. Examples of such components include compounds that improve the film thickness uniformity and surface smoothness when the radical-generating film-forming composition is applied, compounds that improve the adhesion between the radical-generating film-forming composition and a substrate, and compounds that further improve the film strength of the radical-generating film-forming composition.
[0067] Compounds that improve the uniformity of the film thickness and the surface smoothness include fluorine-based surfactants, silicone-based surfactants, and nonionic surfactants. More specifically, for example, EFTOP EF301, EF303, and EF352 (manufactured by Mitsubishi Materials Electronics Co., Ltd.), Megafac F171, F173, and R-30 (manufactured by DIC Corporation), Fluorad FC430 and FC431 (manufactured by 3M), Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (manufactured by AGC Corporation) can be mentioned. When using these surfactants, the proportion of the surfactant used is preferably 0.01 to 2 parts by mass, more preferably 0.01 to 1 part by mass, based on 100 parts by mass of the total amount of the polymer contained in the radical-generating film-forming composition.
[0068] Specific examples of compounds that improve the adhesion between the radical-generating film-forming composition and the substrate include functional silane-containing compounds and epoxy group-containing compounds.For example, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, N-ethoxycarbonyl-3-aminopropyltriethoxysilane silane, N-triethoxysilylpropyltriethylenetriamine, N-trimethoxysilylpropyltriethylenetriamine, 10-trimethoxysilyl-1,4,7-triazadecane, 10-triethoxysilyl-1,4,7-triazadecane, 9-trimethoxysilyl-3,6-diazanonyl acetate, 9-triethoxysilyl-3,6-diazanonyl acetate, N-benzyl-3-aminopropyltrimethoxysilane, N-benzyl-3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N- Phenyl-3-aminopropyltriethoxysilane, N-bis(oxyethylene)-3-aminopropyltrimethoxysilane, N-bis(oxyethylene)-3-aminopropyltriethoxysilane, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, Examples of suitable glycidyl ethers include serine diglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, 1,3,5,6-tetraglycidyl-2,4-hexanediol, N,N,N',N'-tetraglycidyl-m-xylylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, 3-(N-allyl-N-glycidyl)aminopropyltrimethoxysilane, and 3-(N,N-diglycidyl)aminopropyltrimethoxysilane.
[0069] In order to further increase the film strength of the radical-generating film, a phenol compound such as 2,2'-bis(4-hydroxy-3,5-dihydroxymethylphenyl)propane, tetra(methoxymethyl)bisphenol, etc. may be added. When using these compounds, the amount is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, per 100 parts by mass of the total amount of the polymer contained in the radical-generating film-forming composition.
[0070] Furthermore, in addition to the above, the radical-generating film-forming composition may contain a dielectric or conductive substance for the purpose of changing the electrical properties, such as the dielectric constant and conductivity, of the radical-generating film, as long as the effects of the present invention are not impaired.
[0071] [Radical generating film and liquid crystal alignment film] The radical-generating film of the present embodiment can be obtained, for example, by using the radical-generating film-forming composition. For example, the radical-generating film-forming composition used in the present invention can be applied to a substrate, and then dried and baked to obtain a cured film, which can be used as is as a radical-generating film. In addition, this cured film can be subjected to an alignment treatment by rubbing, irradiation with polarized light or light of a specific wavelength, or the like, or treatment with an ion beam, or the like, and it is also possible to irradiate a liquid crystal display element filled with liquid crystal with UV light to use it as an alignment film for PSA.
[0072] Examples of methods for applying the radical-generating film-forming composition include spin coating, printing, inkjet, spraying, and roll coating. From the viewpoint of productivity, the transfer printing method is widely used industrially and is also preferably used in the present invention.
[0073] The drying step after coating the radical-generating film-forming composition is not necessarily required, but when the time from coating to baking is not constant for each substrate, or baking is not performed immediately after coating, it is preferable to include a drying step. This drying is sufficient as long as the solvent is removed to an extent that the coating film shape is not deformed by transportation of the substrate, and the drying method is not particularly limited. For example, a method of drying on a hot plate at a temperature of 40 to 150°C, preferably 60 to 100°C, for 0.5 to 30 minutes, preferably 1 to 5 minutes, can be mentioned.
[0074] The coating film formed by applying the radical-generating film-forming composition by the above method can be baked to form a cured film. The baking temperature can be any temperature between 100 and 350°C, preferably between 140 and 300°C, more preferably between 150 and 230°C, and even more preferably between 160 and 220°C. The baking time can be any time between 5 and 240 minutes, preferably between 10 and 90 minutes, and more preferably between 20 and 90 minutes. Heating can be performed by a commonly known method, such as a hot plate, a hot air circulation oven, an IR (infrared) oven, or a belt furnace.
[0075] The thickness of the cured film can be selected as necessary, but is preferably 5 nm or more, more preferably 10 nm or more, since the reliability of the liquid crystal display element is easily obtained. Also, the thickness of the cured film is preferably 300 nm or less, more preferably 150 nm or less, since the power consumption of the liquid crystal display element is not extremely large.
[0076] A substrate having a radical generating film can be obtained in the manner described above, and the radical generating film can be subjected to a uniaxial alignment treatment. Methods for carrying out the uniaxial alignment treatment include photoalignment, oblique deposition, rubbing, and uniaxial alignment treatment using a magnetic field.
[0077] When performing alignment treatment by unidirectional rubbing, for example, a rubbing roller wrapped with a rubbing cloth is rotated while the substrate is moved so that the rubbing cloth comes into contact with the film. When using a photoalignment method, alignment treatment can be performed by irradiating the entire film with polarized UV of a specific wavelength and heating it as necessary.
[0078] The liquid crystal alignment film of the present embodiment can be obtained by the same method as for the radical-generating film, except that a liquid crystal alignment agent is used instead of the radical-generating film-forming composition.
[0079] The substrate to which the radical-generating film-forming composition is applied is not particularly limited as long as it is a highly transparent substrate. Specific examples include glass plates and plastic plates such as polycarbonate, poly(meth)acrylate, polyethersulfone, polyarylate, polyurethane, polysulfone, polyether, polyetherketone, trimethylpentene, polyolefin, polyethylene terephthalate, (meth)acrylonitrile, triacetyl cellulose, diacetyl cellulose, and acetate butyrate cellulose.
[0080] The substrate on which the liquid crystal alignment film is applied is preferably the above-mentioned substrate on which a transparent electrode for driving the liquid crystal is formed. Substrates that can be used for IPS-type liquid crystal display elements can also have electrode patterns such as standard IPS comb electrodes and PSA fishbone electrodes, or protrusion patterns such as MVA. Moreover, in highly functional elements such as TFT type elements, elements such as transistors are formed between electrodes for driving liquid crystal and a substrate.
[0081] When a transmissive liquid crystal display element is intended, the above-mentioned substrates are generally used, but when a reflective liquid crystal display element is intended, an opaque substrate such as a silicon wafer can be used for only one of the substrates. In that case, a material such as aluminum that reflects light can be used for the electrodes formed on the substrate.
[0082] When rubbing a liquid crystal alignment film on a substrate on which comb-tooth electrodes are formed, the rubbing direction is selected depending on the electrical properties of the liquid crystal. When using a liquid crystal having positive dielectric anisotropy, it is preferable that the rubbing direction be approximately the same as the direction in which the comb-tooth electrodes extend.
[0083] <Liquid crystal cell> The liquid crystal cell of the present invention can be obtained, for example, by arranging a substrate (second substrate) on which a radical generating film is formed by the above method and a substrate (first substrate) with an electrode having a liquid crystal alignment film so that the radical generating film and the liquid crystal alignment film face each other, sandwiching a spacer, fixing them with a sealant, injecting a liquid crystal composition containing liquid crystal and a radical polymerizable compound, and sealing it. In this case, the size of the spacer used is usually 1 to 30 μm, but preferably 2 to 10 μm. In addition, by arranging the rubbing direction of the first substrate and the rubbing direction of the second substrate parallel to each other, it can be used in IPS mode or FFS mode, and by arranging them so that the rubbing directions are perpendicular to each other, it can be used in twisted nematic mode. An IPS substrate, which is a comb-tooth electrode substrate used in IPS (In-Plane Switching) mode, has a base material, a plurality of linear electrodes formed on the base material and arranged in a comb-tooth shape, and a liquid crystal alignment film formed on the base material so as to cover the linear electrodes. The FFS substrate, which is a comb electrode substrate used in the FFS (Frindge Field Switching) mode, has a base material, a surface electrode formed on the base material, an insulating film formed on the surface electrode, a plurality of linear electrodes formed on the insulating film and arranged in a comb shape, and a liquid crystal alignment film formed on the insulating film to cover the linear electrodes.
[0084] The method for injecting the liquid crystal composition containing the liquid crystal and the radical polymerizable compound is not particularly limited, and examples thereof include a vacuum method in which the pressure inside the prepared liquid crystal cell is reduced and then a mixture containing the liquid crystal and the polymerizable compound is injected, and a dropping method in which a mixture containing the liquid crystal and the polymerizable compound is dropped and then sealed.
[0085] <Liquid crystal composition containing liquid crystal and radically polymerizable compound> In the preparation of the liquid crystal display element of the present invention, the polymerizable compound used together with the liquid crystal is not particularly limited as long as it is a radically polymerizable compound, and is, for example, a compound having one or more polymerizable reactive groups in one molecule. A compound having one polymerizable reactive group in one molecule is preferable (hereinafter, sometimes referred to as a "compound having a monofunctional radically polymerizable group"). The polymerizable reactive group is preferably a radically polymerizable reactive group, for example, a vinyl group.
[0086] At least one of the radically polymerizable compounds is preferably a compound having compatibility with liquid crystal and one polymerizable reactive group in one molecule, that is, a compound having a monofunctional radically polymerizable group.
[0087] The polymerizable group of the radically polymerizable compound is preferably a polymerizable group selected from the following structures. [ka] (In the formula, * indicates a binding site. R b represents a linear alkyl group having 2 to 8 carbon atoms, and E represents a bond selected from a single bond, -O-, -NRc-, -S-, an ester bond, and an amide bond. Rc represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0088] In addition, in a liquid crystal composition containing liquid crystal and a radically polymerizable compound, it is preferable to contain a radically polymerizable compound that can polymerize the polymer to have a Tg of 100° C. or less.
[0089] The compound having a monofunctional radically polymerizable group has a reactive group capable of undergoing radical polymerization in the presence of an organic radical, and examples of the compound include methacrylate monomers such as t-butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, lauryl methacrylate, and n-octyl methacrylate; acrylate monomers such as t-butyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, benzyl acrylate, lauryl acrylate, and n-octyl acrylate; styrene and styrene derivatives (e.g., o-, m-, and p-methoxystyrene, o-, m-, and pt-butoxystyrene, o-, m-, and p-chloromethyl styrene); Examples of the vinyl monomer include, but are not limited to, vinyl monomers such as vinyl esters (e.g., vinyl acetate, vinyl propionate, vinyl benzoate, vinyl acetate, etc.), vinyl ketones (e.g., vinyl methyl ketone, vinyl hexyl ketone, methyl isopropenyl ketone, etc.), N-vinyl compounds (e.g., N-vinyl pyrrolidone, N-vinyl pyrrole, N-vinyl carbazole, N-vinyl indole, etc.), (meth)acrylic acid derivatives (e.g., acrylonitrile, methacrylonitrile, acrylamide, isopropyl acrylamide, methacrylamide, etc.), and vinyl halides (e.g., vinyl chloride, vinylidene chloride, tetrachloroethylene, hexachloroprene, vinyl fluoride, etc.). These various radical polymerizable monomers may be used alone or in combination of two or more. In addition, it is preferable that these have compatibility with the liquid crystal.
[0090] Furthermore, the radically polymerizable compound is preferably a compound represented by the following formula (1). [ka] In formula (1), R a and R b each independently represents a linear alkyl group having 2 to 8 carbon atoms, and E represents a bonding group selected from a single bond, -O-, -NRc-, -S-, an ester bond, and an amide bond. In the description, Rc represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0091] As the radical polymerizable compound represented by formula (1), one in which E is an ester bond (a bond represented by -C(=O)-O- or -OC(=O)-) is preferred from the viewpoints of ease of synthesis, compatibility with liquid crystal, and polymerization reactivity. Specifically, a compound having the following structure is preferred, but there is no particular limitation thereon. [ka] In formulas (1-1) and (1-2), Ra and Rb each independently represent a linear alkyl group having 2 to 8 carbon atoms.
[0092] The content of the radically polymerizable compound in the liquid crystal composition is preferably 3 mass % or more, more preferably 5 mass % or more, and preferably 50 mass % or less, more preferably 20 mass % or less, relative to the total mass of the liquid crystal and the radically polymerizable compound.
[0093] The polymer obtained by polymerizing the radically polymerizable compound preferably has a Tg of 100° C. or lower.
[0094] Liquid crystal generally refers to a substance that exhibits both solid and liquid properties, and representative liquid crystal phases include nematic liquid crystal and smectic liquid crystal, but the liquid crystal that can be used in the present invention is not particularly limited. One example is 4-pentyl-4'-cyanobiphenyl.
[0095] Next, a liquid crystal cell containing the mixture (liquid crystal composition) containing the liquid crystal and the radical polymerizable compound is given sufficient energy to polymerize the radical polymerizable compound. This can be done, for example, by applying heat or irradiating with UV light, and the radical polymerizable compound is polymerized in situ to develop the desired characteristics. Among these, UV irradiation is preferred because it allows patterning of the alignment and also allows the polymerization reaction to occur in a short time. When using the liquid crystal composition in a twisted nematic mode, a chiral dopant may be introduced into the liquid crystal cell as necessary in addition to the liquid crystal composition.
[0096] The heating temperature during UV irradiation is preferably within a temperature range in which the introduced liquid crystal exhibits liquid crystallinity, and is usually 40° C. or higher, and is preferably below the temperature at which the liquid crystal changes to an isotropic phase.
[0097] In this case, the wavelength of UV irradiation in the case of UV irradiation is preferably selected so as to provide the best reaction quantum yield of the polymerizable compound to be reacted, and the UV irradiation dose is usually 0.01 to 30 J / cm. 2 However, preferably, 10 J / cm 2 A lower amount of UV irradiation is preferable because it can prevent deterioration in reliability due to damage to the components that make up the liquid crystal display, and also because it can improve the manufacturing takt time by reducing the UV irradiation time.
[0098] When polymerization is carried out by heating alone, rather than by UV irradiation, the heating is preferably carried out at a temperature within a range where the polymerizable compound reacts and is lower than the decomposition temperature of the liquid crystal, specifically, 100 to 150°C.
[0099] When applying sufficient energy to cause a polymerization reaction of the radical polymerizable compound, it is preferable that no voltage is applied and that the device is in an electric field-free state.
[0100] <Liquid crystal display element> A liquid crystal display device can be produced using the liquid crystal cell thus obtained. For example, this liquid crystal cell can be made into a reflective liquid crystal display element by providing a reflective electrode, a transparent electrode, a λ / 4 plate, a polarizing film, a color filter layer, etc., in accordance with a conventional method, as necessary. Furthermore, if necessary, a backlight, a polarizing plate, a λ / 4 plate, a transparent electrode, a polarizing film, a color filter layer, etc. may be provided in the liquid crystal cell in a conventional manner to form a transmission type liquid crystal display element. EXAMPLES
[0101] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The abbreviations of the compounds used in the polymerization of the polymer and the preparation of the film-forming composition, and the methods of evaluating the properties are as follows. [ka] NMP: N-methyl-2-pyrrolidone, GBL: gamma-butyrolactone; BCS: Butyl cellosolve
[0102] <Viscosity measurement> The viscosity of the polyamic acid solution at 25° C. was measured using an E-type viscometer TVE-22H (manufactured by Toki Sangyo Co., Ltd.) with a sample amount of 1.1 mL and a cone rotor TE-1 (1°34′, R24).
[0103] <Molecular weight measurement> The molecular weight was measured using a room temperature gel permeation chromatography (GPC) apparatus (GPC-101) (manufactured by Showa Denko KK) and columns (KD-803, KD-805) (manufactured by Showa Denko KK) as follows. Column temperature: 50℃ Eluent: N,N-dimethylformamide (additives: lithium bromide monohydrate (LiBr·H2O) 30 mmol / L, phosphoric acid anhydrous crystal (o-phosphoric acid) 30 mmol / L, tetrahydrofuran (THF) 10 mL / L) Flow rate: 1.0mL / min Standard samples for preparing a calibration curve: TSK standard polyethylene oxide (molecular weight: approximately 900,000, 150,000, 100,000, and 30,000) (manufactured by Tosoh Corporation) and polyethylene glycol (molecular weight: approximately 12,000, 4,000, and 1,000) (manufactured by Polymer Laboratory Co., Ltd.).
[0104] <Measurement of imidization rate> 20 mg of polyimide powder was placed in an NMR sample tube (Kusano Scientific NMR Sampling Tube Standard φ5), 0.53 mL of deuterated dimethyl sulfoxide (DMSO-d6, 0.05 mass% TMS (tetramethylsilane) mixture) was added, and the mixture was sonicated to completely dissolve. The 500 MHz proton NMR of this solution was measured using a measuring device (JNW-ECA500, manufactured by JEOL Datum Co., Ltd.). The imidization rate was determined by determining a proton derived from a structure that does not change before and after imidization as a reference proton, and using the peak integrated value of this proton and the peak integrated value of a proton derived from the NH of an amide group appearing in the vicinity of 9.5 to 10.0 ppm, according to the following formula. Imidization rate (%) = (1-α·x / y) × 100 In the formula, x is the integrated value of the proton peak derived from the NH of the amide group, y is the integrated value of the peak of the reference proton, and α is the ratio of the number of reference protons to one NH proton of the amide group in the case of polyamic acid (imidization rate 0%).
[0105] <Polymerization of polymer and preparation of radical-generating film-forming composition> Synthesis Example 1 Polymerization of TC-1, TC-2(50) / DA-1(50), DA-2(50) polyimides 1.62g (15.0mmol) of DA-1 and 4.96g (15.0mmol) of DA-2 were weighed out into a 100mL four-neck flask equipped with a nitrogen inlet tube, an air cooling tube, and a mechanical stirrer, and 51.9g of NMP was added and stirred under a nitrogen atmosphere to completely dissolve. After confirming dissolution, 3.75g (15.0mmol) of TC-2 was added and reacted for 3 hours at 60°C under a nitrogen atmosphere. The mixture was returned to room temperature, and 2.64g (13.5mmol) of TC-1 was added and reacted for 12 hours at 40°C under a nitrogen atmosphere. The polymerization viscosity was confirmed, and further TC-1 was added so that the polymerization viscosity was approximately 1000mPa·s, to obtain a polymerization liquid with a polyamic acid concentration of 20% by mass. 60 g of the polyamic acid solution obtained above was weighed out into a 200 mL Erlenmeyer flask equipped with a magnetic stirrer, 111.4 g of NMP was added to prepare a solution with a concentration of 7% by mass, and 8.38 g (81.4 mmol) of acetic anhydride and 3.62 g (45.8 mmol) of pyridine were added while stirring, and the mixture was stirred at room temperature for 30 minutes, and then stirred at 55 ° C for 3 hours to react. After the reaction was completed, the solution was returned to room temperature, and the reaction solution was poured into 500 mL of methanol while stirring, to precipitate a solid. The solid was collected by filtration, and the solid was further poured into 300 mL of methanol and stirred and washed for 30 minutes twice in total. The solid was collected by filtration, air-dried, and then dried at 60 ° C using a vacuum oven to obtain a polyimide powder (PI-1) with a number average molecular weight (Mn) of 16,200, a weight average molecular weight (Mw) of 35,200, and an imidization rate of 59%.
[0106] Synthesis Example 2 Polymerization of TC-1, TC-2(50) / DA-2(100) polyimides 9.91g (30.0mmol) of DA-2 was weighed out into a 100mL four-neck flask equipped with a nitrogen inlet tube, an air cooling tube, and a mechanical stirrer, and 65.95g of NMP was added and stirred under a nitrogen atmosphere to completely dissolve. After confirming dissolution, 3.75g (15.0mmol) of TC-2 was added and reacted for 3 hours at 60°C under a nitrogen atmosphere. The mixture was returned to room temperature, and 2.82g (14.4mmol) of TC-1 was added and reacted for 12 hours at 40°C under a nitrogen atmosphere. The polymerization viscosity was confirmed, and further TC-1 was added so that the polymerization viscosity was approximately 1000mPa·s, to obtain a polymerization liquid with a polyamic acid concentration of 20% by mass. 70 g of the polyamic acid solution obtained above was weighed out into a 200 mL Erlenmeyer flask equipped with a magnetic stirrer, 130.0 g of NMP was added to prepare a solution with a concentration of 7% by mass, and 6.90 g (67.5 mmol) of acetic anhydride and 2.96 g (37.4 mmol) of pyridine were added while stirring, and the mixture was stirred at room temperature for 30 minutes, and then stirred at 55 ° C for 3 hours to react. After the reaction was completed, the solution was returned to room temperature, and the reaction solution was poured into 500 mL of methanol while stirring, to precipitate a solid. The solid was collected by filtration, and then the solid was poured into 300 mL of methanol and stirred and washed for 30 minutes twice in total. The solid was collected by filtration, air-dried, and then dried at 60 ° C in a vacuum oven to obtain a polyimide powder (PI-2) with Mn of 18,300, Mw of 38,900, and imidization rate of 62%.
[0107] Preparation of radical-generating film-forming composition AL-1 2.0 g of the polyimide powder (PI-1) obtained in Synthesis Example 1 was weighed out into a 50 mL Erlenmeyer flask equipped with a magnetic stirrer, 18.0 g of NMP was added, and the mixture was stirred at 50° C. to completely dissolve it. Further, 6.7 g of NMP and 6.7 g of BCS were added, and the mixture was stirred for 3 hours to obtain a radical-generating film-forming composition according to the present invention: AL-1 (solid content: 6.0 mass%, NMP: 74 mass%, BCS: 20 mass%).
[0108] Preparation of radical-generating film-forming composition AL-2 2.0 g of the polyimide powder (PI-2) obtained in Synthesis Example 2 was weighed out into a 50 mL Erlenmeyer flask equipped with a magnetic stirrer, 18.0 g of NMP was added, and the mixture was stirred at 50° C. to completely dissolve it. Further, 6.7 g of NMP and 6.7 g of BCS were added, and the mixture was stirred for 3 hours to obtain a radical-generating film-forming composition according to the present invention: AL-2 (solid content: 6.0 mass%, NMP: 74 mass%, BCS: 20 mass%).
[0109] A method for preparing a liquid crystal cell for evaluating the liquid crystal alignment property will be described below. First, a substrate with electrodes was prepared. The substrate was a glass substrate with dimensions of 30 mm x 35 mm and a thickness of 0.7 mm. An IZO electrode with a solid pattern was formed on the substrate as the first layer, which constituted the counter electrode. A SiN (silicon nitride) film formed by CVD (chemical vapor deposition) was formed as the second layer on the first layer of the counter electrode. The thickness of the second layer of SiN film was 500 nm, and it functions as an interlayer insulating film. A comb-shaped pixel electrode formed by patterning the IZO film as the third layer was placed on the second layer of SiN film, forming two pixels, the first pixel and the second pixel. The size of each pixel was 10 mm long and approximately 5 mm wide. At this time, the first layer of the counter electrode and the third layer of the pixel electrode were electrically insulated by the action of the second layer of SiN film. The pixel electrode in the third layer has a comb-like shape in which multiple electrode elements, each 3 μm wide and bent at an interior angle of 160° in the center, are arranged in parallel at 6 μm intervals, as shown in Figure 3 of JP 2014-77845 (Japanese Unexamined Patent Publication), and each pixel has a first region and a second region separated by a line connecting the bent portions of the multiple electrode elements. Comparing the first and second regions of each pixel, the electrode elements of the pixel electrodes that compose them are formed in different directions. That is, based on the rubbing direction of the liquid crystal alignment film described later, the electrode elements of the pixel electrodes in the first region of the pixel are formed to form an angle of +10° (clockwise), and the electrode elements of the pixel electrodes in the second region of the pixel are formed to form an angle of -10° (counterclockwise). That is, in the first and second regions of each pixel, the liquid crystal is induced by the application of a voltage between the pixel electrode and the counter electrode, and the directions of the rotational movement (in-plane switching) within the substrate plane are opposite to each other. Hereinafter, this will be referred to as the FFS substrate (first substrate). In addition, a glass substrate (hereinafter referred to as the second substrate) having an ITO film formed on the rear surface and having columnar spacers with a height of 3.3 μm was prepared as an opposing substrate. Next, the radical-generating film-forming composition obtained by the above-mentioned method or a liquid crystal alignment material Sunever SE-6414 manufactured by Nissan Chemical Industries, Ltd. was filtered through a filter with a pore size of 1.0 μm, and then coated and formed on the above-prepared first substrate and second substrate by spin coating. Then, it was dried on a hot plate at 80° C. for 80 minutes, and then baked at 220° C. for 20 minutes to obtain a coating film with a thickness of 100 nm. The polyimide film on the first substrate side was rubbed in the direction along the direction of the comb teeth, and the polyimide film on the second substrate side was rubbed in the direction perpendicular to the direction of the comb teeth of the comb electrode of the first substrate when the second substrate and the first substrate were placed opposite each other. The cloth used for the rubbing treatment was rayon cloth: YA-20R manufactured by Yoshikawa Kako Co., Ltd., and rubbing was performed (roll diameter 120 mm). Regardless of the substrate, the substrate coated with SE-6414 was rubbing-treated at a rotation speed of 700 rpm, a moving speed of 30 mm / sec, and a push-in depth of 0.4 mm, while the substrate coated with the radical-generating film-forming composition was rubbing-treated at a rotation speed of 500 rpm, a moving speed of 30 mm / sec, and a push-in depth of 0.2 mm. After the rubbing treatment, the substrate was irradiated with ultrasonic waves in pure water for 1 minute, and dried at 80°C for 10 minutes. Then, the above two types of substrates were used, and the display element of the embodiment was combined with SE-6414 on the first substrate side and a radical generating film on the second substrate side. On the other hand, the display element of the comparison object was combined with SE-6414 on both substrates, or with a radical generating film on the first substrate side and SE-6414 on the second substrate side. Then, in each combination, the first substrate and the second substrate were combined so that the rubbing directions were antiparallel, and the periphery was sealed except for the liquid crystal injection port, to prepare an empty cell with a cell gap of about 3.3 μm. Liquid crystal (2% by mass of additive IDHex added to MLC-3019 manufactured by Merck) was injected into this empty cell under vacuum at room temperature, and the injection port was sealed to obtain an antiparallel aligned liquid crystal cell. The obtained liquid crystal cell constitutes an FFS mode liquid crystal display element. The obtained liquid crystal cell was then heat-treated at 120°C for 10 minutes, and then irradiated with UV (UV lamp: FLR40SUV32 / A-1) for 30 minutes using a UV-FL irradiation device manufactured by Toshiba Lighting & Technology Corporation without applying voltage to obtain a liquid crystal display element.
[0110] <Measurement of V-T Curve, Driving Threshold Voltage, and Maximum Luminance Voltage Evaluation> The white LED backlight and the luminance meter were set so that their optical axes were aligned. Between them, a liquid crystal cell (liquid crystal display element) with a polarizing plate attached so that the luminance was minimized was set. A voltage was applied up to 8V at 1V intervals, and the V-T curve was measured by measuring the luminance at each voltage. The driving threshold voltage and the voltage at which the luminance was maximized were estimated from the obtained V-T curve. Also, with the liquid crystal cell without voltage applied, the transmission luminance at parallel Nicol was set to 100%, and the maximum transmission rate was estimated by comparing the maximum transmission luminance in the V-T curve.
[0111] <Measurement of Response Time (Ton, Toff)> In addition to the above measurements, the response times Ton and Toff were measured by using an oscilloscope to measure the time change in luminance when a voltage at which the luminance was maximized was applied and the time change in luminance when the voltage was returned to 0V.
[0112] <Evaluation of Voltage Holding Ratio (VHR)> An AC pulse voltage with an offset voltage of 0V, an amplitude of 2Vp-p, a frequency of 0.6Hz, and a voltage application time of 60μs was applied to the liquid crystal cell in a hot air circulation oven at 60°C. The voltage immediately after the voltage application was released and the voltage (both positive and negative) 1667ms later were measured, and the voltage holding ratio (VHR) was measured by calculating the ratio of the voltages before and after the application. As the measuring device, VHR-1 manufactured by Toyo Technica Co., Ltd. was used. A higher VHR was considered better.
[0113] <Burning-in Evaluation> A rectangular wave voltage (60Hz) at which the luminance was maximized was applied to the first pixel region of each liquid crystal cell, and a state where no voltage was applied to the other second pixel region was created, and the aging was performed by driving at 60°C for 168 hours. The burning-in was evaluated by comparing the luminances of the first pixel region and the second pixel region after aging. When the luminance ratio was 1.10 or less, it was defined as "good", and when it was greater than 1.10, it was defined as "bad".
[0114]
Table 1
[0115] <Drive threshold voltage, maximum luminance voltage, maximum transmittance, response time>
[0116]
Table 2
[0117] <VHR, burn-in evaluation>
[0118]
Table 3
[0119] Comparative Example 1 shows the characteristics of a conventional FFS display element using a strongly anchoring alignment film. Comparative Examples 2 and 3 show the characteristics of FFS display elements using a weakly anchoring film on the first substrate side. Examples 1 and 2 show the characteristics of FFS display elements according to the present invention using a weakly anchoring film on the second substrate side. That is, in Examples 1 and 2, the anchoring energy of the liquid crystal alignment film (weakly anchoring film) on the counter substrate (second substrate) side is smaller than the anchoring energy of the liquid crystal alignment film on the comb electrode substrate (first substrate) side. In Comparative Examples 2 and 3 (when using a weakly anchoring film on the first substrate side), which are configurations reported so far, the threshold voltage and the maximum luminance voltage shift to a lower voltage, and accordingly the transmittance also improves, but on the other hand, the response time tends to deteriorate. This is considered to be the result of the decrease in the anchoring energy on the first substrate side. It can be seen that the anchoring energy of Comparative Example 3 is lower than that of Comparative Example 2, and accordingly the transmittance improves, but the response time tends to deteriorate. On the other hand, when using a weakly anchoring film on the second substrate side according to the present invention, the threshold voltage and the maximum luminance voltage do not change, but it has been found that the transmittance increases and the response time is almost equivalent to that of the conventional FFS display element of Comparative Example 1. The response time of the horizontal electric field mode is (drive voltage V - drive threshold voltage V Th) is inversely proportional to the driving threshold voltage V Th Maximum brightness voltage V max Since the configuration of the present invention is not different from that of the conventional configuration, it is presumed that the configuration of the present invention does not have a large effect on the response time. In addition, in the conventional weak anchoring FFS display element configurations of Comparative Examples 2 and 3, the VHR deteriorates and the burn-in characteristics are worse than those of the conventional strong anchoring FFS display element, but it was found that by using the weak anchoring configuration of the present invention, the VHR improves and burn-in characteristics also improve accordingly. [Industrial Applicability]
[0120] According to the present invention, it is possible to provide an in-plane switching liquid crystal display element that can realize high burn-in characteristics (VHR, burn-in characteristics), high backlight transmittance, and fast response speed. Furthermore, the liquid crystal display element obtained by the method of the present invention is useful as an in-plane switching liquid crystal display element. [Explanation of symbols]
[0121] 1 In-plane switching liquid crystal display element 2. Interdigital electrode substrate 2a Base material 2b Linear electrode 2c Liquid crystal alignment film 2d base material 2e surface electrode 2f Insulating film 2g linear electrode 2h Liquid crystal alignment film 3 Liquid crystal 4 Opposing substrate 4a Liquid crystal alignment film 4b Base material L Electric field lines
Claims
1. An in-plane switching liquid crystal display element of an FFS driving method, comprising: a comb-tooth electrode substrate which is an FFS substrate and has a liquid crystal alignment film; and an opposing substrate which has a liquid crystal alignment film, the two liquid crystal alignment films facing each other, and liquid crystal is filled between the liquid crystal alignment films, wherein the anchoring energy of the liquid crystal alignment film on the opposing substrate side is smaller than the anchoring energy of the liquid crystal alignment film on the comb-tooth electrode substrate side, A horizontal electric field liquid crystal display element of an FFS driving type, in which, of the liquid crystal alignment film on the opposing substrate side and the liquid crystal alignment film on the comb-tooth electrode substrate side, only the liquid crystal alignment film on the opposing substrate side is obtained by polymerizing the radical polymerizable compound while contacting a liquid crystal composition containing the liquid crystal and a radical polymerizable compound with a radical generating film.
2. An FFS driving type horizontal electric field liquid crystal display element as described in claim 1, wherein the liquid crystal alignment film on the comb-tooth electrode substrate side and the liquid crystal alignment film on the opposing substrate side are both liquid crystal alignment films that have been subjected to uniaxial alignment treatment, and only the liquid crystal alignment film on the opposing substrate side has been subjected to weak anchoring treatment.
3. A horizontal electric field liquid crystal display element of an FFS drive type as described in claim 1 or 2, wherein the comb-tooth electrode substrate has a base material, a surface electrode formed on the base material, an insulating film formed on the surface electrode, and a plurality of linear electrodes formed on the insulating film and arranged in a comb-tooth shape.
4. 4. The in-plane switching liquid crystal display element of the FFS driving method according to claim 1, wherein the radical generating film is a film having an organic group that induces radical polymerization fixed thereon.
5. 5. The in-plane switching liquid crystal display element of the FFS driving method according to claim 1, wherein the radical generating film is made of a polymer containing an organic group that induces radical polymerization.
6. The in-plane switching liquid crystal display element of claim 5, wherein the polymer containing an organic group that induces radical polymerization is at least one polymer selected from a polyimide precursor, a polyimide, a polyurea, and a polyamide obtained using a diamine component containing a diamine containing an organic group that induces radical polymerization.
7. The organic group that induces radical polymerization is an organic group represented by the following structure [X-1] to [X-18], [W], [Y], or [Z]. A horizontal electric field liquid crystal display element of the FFS driving method according to claim 5 or 6. 【Chemistry 1】 (In formulas [X-1] to [X-18], * indicates a bonding site, and S 1 , and S 2 each independently represents -O-, -NR-, or -S-, and R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms (among the alkyl groups having 1 to 10 carbon atoms, -CH of an alkyl group having 2 to 10 carbon atoms is 2 A part of the - group may be replaced by an oxygen atom. 2 In R or NR, the alkyl group is —CH 2 When a part of the - group is replaced by an oxygen atom, the oxygen atom is S 2 Or, it is not directly bonded to N. 1 , and R 2 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms. 【Chemistry 2】 (In the formulae [W], [Y], and [Z], * represents a bonding site, Ar represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, which may have an organic group and / or a halogen atom as a substituent, and R 9 and R 10 each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms; R 9 and R 10 When represents an alkyl group, they may be bonded to each other at the terminals to form a ring structure. Q represents any one of the following structures: 【Chemistry 3】 (In the formula, R 11 Ha-CH 2 Each R independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * indicates a bonding site. 3 represents a single bond, -O-, -NR- (wherein R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or -S-. 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms.
8. 7. The in-plane switching liquid crystal display element of FFS driving mode according to claim 6, wherein the diamine containing an organic group capable of inducing radical polymerization is a diamine having a structure represented by the following general formula (6) or the following general formula (7): 【Chemistry 4】 (In formula (6), R 6 is a single bond, -CH 2 -, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH 2 O-, -N(CH 3 )-,-CON(CH 3 )- or -N(CH 3 ) CO-, R 7 represents a single bond, or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms, 2 -or-CF 2 One or more - may be independently replaced by a group selected from -CH=CH-, a divalent carbocyclic ring, and a divalent heterocyclic ring, and may further be replaced by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH-, or -NH-, provided that they are not adjacent to each other; R 8 represents a radical polymerization reactive group represented by a formula selected from the following formulas [X-1] to [X-18]. 【Chemistry 5】 (In formulas [X-1] to [X-18], * indicates a bonding site, and S 1 , and S 2 each independently represents -O-, -NR-, or -S-, and R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms (among the alkyl groups having 1 to 10 carbon atoms, -CH of an alkyl group having 2 to 10 carbon atoms is 2 A part of the - group may be replaced by an oxygen atom. 2 In R or NR, the alkyl group is —CH 2 When a part of the - group is replaced by an oxygen atom, the oxygen atom is S 2 Or, it is not directly bonded to N. 1 , and R 2 each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms. 【Chemistry 6】 (In formula (7), T 1 and T 2 each independently represents a single bond, —O—, —S—, —COO—, —OCO—, —NHCO—, —CONH—, —NH—, or —CH 2 O-, -N(CH 3 )-,-CON(CH 3 )- or -N(CH 3 ) CO-, S represents a single bond or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms, and any —CH 2 -or-CF 2 one or more - may be independently replaced by a group selected from -CH=CH-, a divalent carbocyclic ring, and a divalent heterocyclic ring, and may be further replaced by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH-, or -NH-, provided that these groups are not adjacent to each other: J is an organic group represented by a formula selected from the following formulae [W], [Y], and [Z]. 【Chemistry 7】 (In the formulas [W], [Y], and [Z], * represents T 2 Ar represents an aromatic hydrocarbon group selected from the group consisting of phenylene, naphthylene, and biphenylylene, which may have an organic group and / or a halogen atom as a substituent; R 9 and R 10 each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, Q represents any one of the following structures: 【Chemistry 8】 (In the formula, R 11 Ha-CH 2 Each R independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * indicates a bonding site. R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms. S 3 represents a single bond, -O-, -NR- (wherein R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms), or -S-.
9. 9. An in-plane switching liquid crystal display element of an FFS driving method according to claim 1, wherein at least one of the radical polymerizable compounds is a compound having one polymerizable reactive group in one molecule and is compatible with liquid crystal.
10. 10. The in-plane switching liquid crystal display element of FFS driving mode according to claim 9, wherein the polymerizable reactive group of the radical polymerizable compound is selected from the following structures: 【Chemistry 9】 (In the formula, * indicates a binding site. R b represents a linear alkyl group having 2 to 8 carbon atoms, and E represents a bond selected from a single bond, -O-, -NRc-, -S-, an ester bond, and an amide bond. Rc represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
11. The horizontal electric field liquid crystal display element of any one of claims 1 to 10, wherein the radical polymerizable compound is a radical polymerizable compound that allows the Tg of a polymer obtained by polymerizing the radical polymerizable compound to be 100°C or less.
12. preparing a comb electrode substrate which is a first substrate having a liquid crystal alignment film which is not a radical-generating film and which is an FFS substrate, and a counter substrate which is a second substrate having a radical-generating film; creating a cell such that the radical generating film on the second substrate faces the first substrate; and A method for manufacturing an in-plane switching liquid crystal cell of an FFS driving mode, comprising the step of filling a liquid crystal composition containing liquid crystal and a radical polymerizable compound between the first substrate and the second substrate.
13. 13. The method for manufacturing an in-plane switching liquid crystal cell of FFS driving mode according to claim 12, wherein the second substrate is a substrate coated with a liquid crystal alignment film having uniaxial alignment.
14. 14. The method for producing an in-plane switching liquid crystal cell of the FFS driving mode according to claim 13, wherein the liquid crystal alignment film having uniaxial alignment is a liquid crystal alignment film for horizontal alignment.
15. A method for manufacturing a horizontal electric field liquid crystal cell of an FFS driving type described in any of claims 12 to 14, wherein the comb-tooth electrode substrate has a base material, a surface electrode formed on the base material, an insulating film formed on the surface electrode, and a plurality of linear electrodes formed on the insulating film and arranged in a comb-tooth shape.
Citation Information
Patent Citations
Method of aligning liquid crystal having no anchoring in plane and non-contact liquid crystal aligning method using the same, and liquid crystal display device
JP2013231757A
Liquid crystal display element and manufacturing method for the same
JP2016170389A
Curable composition, cured product and liquid crystal display element
JP2018197856A
Zero plane anchoring liquid crystal alignment method and its liquid crystal device
JP4053530B2
Liquid crystal display device and method for manufacturing same
WO2014045923A1