Electronic Components
By integrating a Cu segregated substance at the interface between the ceramic element body and glass insulating film, the adhesion issue in laminated coil components is resolved, leading to improved stability and durability.
Patent Information
- Application Number
- JP2022578103
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-01
- Filing Date
- 2021-12-07
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-12-07
AI Technical Summary
The adhesion between the element body and the insulating layer in laminated coil components is low, necessitating an improvement.
Incorporating a ceramic element body containing Cu element with a Cu segregated substance at the interface between the element body and an insulating film made of glass, enhancing adhesion through the anchor effect of Cu segregates at the grain boundaries.
The enhanced adhesion between the element body and insulating film results in improved stability and durability of the electronic component.
Smart Images

Figure 0007552739000008 
Figure 0007552739000007 
Figure 0007552739000009
Abstract
Description
[Technical field]
[0001] The present invention relates to electronic components. [Background technology]
[0002] 2. Description of the Related Art Multilayer coil components are known in which an insulating film containing glass is formed on the surface of an element body made of sintered ferrite.
[0003] Patent Document 1 discloses a laminated coil component including an element body made of a sintered ferrite body and a coil formed by electrically connecting a plurality of internal conductors arranged in parallel within the element body, the surface of the element body being covered with an insulating layer containing glass. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-204565 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the laminated coil component described in Patent Document 1, the adhesion between the element body and the insulating layer (insulating film) is low, and there is room for improvement in the adhesion.
[0006] The present invention has been made to solve the above problems, and has an object to provide an electronic component having high adhesion between the element body and the insulating film. [Means for solving the problem]
[0007] One embodiment of the electronic component of the present invention includes a ceramic body containing Cu, an insulating film containing glass covering at least a portion of a surface of the body, and Cu segregated material containing Cu, wherein the Cu segregated material is in contact with the element body and the insulating film at an interface between the element body and the insulating film. Effect of the Invention
[0008] According to the present invention, it is possible to provide an electronic component having high adhesion between the element body and the insulating film. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a perspective view that illustrates an example of an electronic component according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 3 is a perspective view that illustrates a schematic diagram of another example of an electronic component according to an embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. [Diagram 5] FIG. 5 is a cross-sectional view showing a schematic example of the state of the interface between the element body and the insulating film in one embodiment of the electronic component of the present invention. [Figure 6] FIG. 6 is a cross-sectional view showing a schematic diagram of another example of the state of the interface between the element body and the insulating film in an embodiment of the electronic component of the present invention. [Figure 7] FIG. 7 is a cross-sectional view showing a schematic diagram of yet another example of the state of the interface between the element body and the insulating film in an embodiment of the electronic component of the present invention. [Figure 8] FIG. 8 is an element mapping image of Cu at the interface between the element body and the insulating film of the electronic component according to Example 2. In FIG. [Figure 9] FIG. 9 is an element mapping image of Cu at the interface between the element body and the insulating film of the electronic component according to Example 2. In FIG. [Figure 10] FIG. 10 is an element mapping image of Cu at the interface between the element body and the insulating film of the electronic component according to Example 2. In FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The electronic component of the present invention will now be described. However, the present invention is not limited to the following configuration, and can be modified and applied as appropriate within the scope that does not deviate from the gist of the present invention.
[0011] The following embodiments are merely examples, and it goes without saying that partial replacement or combination of the configurations shown in the different embodiments is possible. From the second embodiment onwards, a description of the matters common to the first embodiment will be omitted, and only the differences will be described. In particular, similar effects due to similar configurations will not be mentioned in each embodiment.
[0012] The drawings shown below are schematic, and the dimensions and aspect ratios may differ from the actual products.
[0013] One embodiment of the electronic component of the present invention includes a ceramic body containing Cu, an insulating film containing glass covering at least a portion of a surface of the body, and Cu segregated material containing Cu, wherein the Cu segregated material is in contact with the element body and the insulating film at an interface between the element body and the insulating film.
[0014] FIG. 1 is a perspective view that illustrates an example of an electronic component according to an embodiment of the present invention. The electronic component 1 shown in FIG. 1 comprises an element body 10 and an insulating film 20 that covers part of the surface of the element body 10 . The element body 10 has a generally rectangular parallelepiped shape having a first end face 10a and a second end face 10b facing in the longitudinal direction L, a first side face 10c and a second side face 10d facing in a width direction W perpendicular to the longitudinal direction L, and a top face 10e and a bottom face 10f facing in a thickness direction T perpendicular to the longitudinal direction L and the width direction W. The insulating film 20 includes an insulating film 20a covering the entire second side surface 10d of the element body 10, and parts of the first end surface 10a, the second end surface 10b, the top surface 10e, and the bottom surface 10f, and an insulating film 20b covering the entire first side surface 10c of the element body 10, and parts of the first end surface 10a, the second end surface 10b, the top surface 10e, and the bottom surface 10f. On the top surface 10e and the bottom surface 10f of the element body 10, the insulating film 20a and the insulating film 20b are provided so as to partially overlap each other. The number of insulating films covering the surface of the element body may be one, or may be three or more. For example, the entire surface of the element body may be covered with one or more insulating films, except for a portion where a conductor layer, which will be described later, is exposed on the surface of the element body.
[0015] An external electrode 50 is provided on the surface of the element body 10 . The external electrode 50 is provided so as to cover the first end face 10a and the second end face 10b of the element body 10. A portion of the external electrode 50 covering the first end face 10a of the element body 10 is formed so as to wrap around parts of the first side face 10c, the second side face 10d, the top face 10e, and the bottom face 10f of the element body 10. A portion of the external electrode 50 covering the second end face 10b of the element body 10 is formed so as to wrap around parts of the first side face 10c, the second side face 10d, the top face 10e, and the bottom face 10f of the element body 10. Part of the surface of element body 10 is covered with insulating film 20 (20a, 20b), and the part of the surface of element body 10 not covered with insulating film 20 is covered with external electrode 50. Therefore, the surface of element body 10 is not exposed. However, part of the surface of the element body may be exposed and not covered by the insulating film and external electrode.
[0016] FIG. 2 is a cross-sectional view taken along line II-II in FIG. 2, the element body 10 has a conductor layer 40 therein. The conductor layer 40 is exposed at the first end face 10a and the second end face 10b of the element body 10, and is electrically connected to an external electrode 50. The conductor layers 40 as a whole form a coil. The coil axis of the coil formed by the conductor layers 40 is parallel to the longitudinal direction L.
[0017] FIG. 3 is a perspective view that illustrates a schematic diagram of another example of an electronic component according to an embodiment of the present invention. 3 includes an element body 11 and an insulating film 20 covering part of the surface of element body 11. The shape of element body 11 is a barbell shape having a columnar winding core 60 around which wire 43 is wound, and flanges 61 connected to both ends in the length direction L of winding core 60. Wire 43 is wound around winding core 60 of element body 11.
[0018] FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. 4, insulating film 20 covers the entire flange portion 61 and the entire winding core portion 60 of element body 11. Because the entire surface of element body 11 is covered with insulating film 20, winding 43 is not in contact with element body 11. Although not shown, an end of winding 43 is connected to external electrode 50. 3 and 4, the entire surface of element body 11 is covered with insulating film 20, and winding 43 is not in contact with element body 11. There is no particular limit to the number of insulating films covering the surface of the element body, and the surface of the element body may be covered with two or more insulating films.
[0019] [Base body] In one embodiment of the electronic component of the present invention, the body is a ceramic containing Cu element.
[0020] Examples of ceramics containing Cu include known ceramics such as ferrite, alumina, barium titanate, and Zn-based ceramics containing Cu. The ceramic containing Cu element may contain additives such as Mn3O4, Co3O4, SnO2, Bi2O3, and SiO2.
[0021] The content of Cu element in the element body is preferably 6 mol % or more and 10 mol % or less. The Cu element content in the element body does not take into consideration the Cu element constituting the Cu segregation products segregated on the surface of the element body. The Cu element content in the element can be measured by polishing the element to expose a cross section 10 μm or more inward from its surface, and measuring it with wavelength dispersive X-ray fluorescence (WD-XRF) with a spot diameter of φ1 μm or more to eliminate the effects of segregation. Note that WD-XRF measurement may be performed on about five samples to further reduce variation depending on the measurement location.
[0022] The content of Fe element in the element body is preferably 40 mol % or more and 49.5 mol % or less in terms of Fe2O3.
[0023] The Ni / Zn molar ratio in the element is not particularly limited, but is preferably 1.8 or more and 2.8 or less.
[0024] The shape of the element body is not particularly limited, but examples thereof include a cube shape, a rectangular parallelepiped shape, a barbell shape, an H shape, an I shape, and an annular shape. Although there are no particular limitations on the outer dimensions of the element body, the smaller the size, the smaller the contact area between the element body and the insulating film, making it more difficult to improve adhesion between the element body and the insulating film. For example, the outer dimensions of the element are preferably 5.7 mm or less in length × 5.0 mm or less in width × 5.0 mm or less in height, and particularly preferably 1.6 mm or less in length × 0.8 mm or less in width × 0.8 mm or less in height.
[0025] The element body may have a conductor layer therein. The conductor layers formed inside the element body may form passive elements such as coils, capacitors, resistors, thermistors, etc. A plurality of passive elements may be formed inside the element body. The orientation of the passive element formed in the element body is arbitrary. Therefore, the coil axis of the coil formed in the element body may be horizontal or vertical to the mounting surface of the electronic component. In addition, the number of coils formed in the element body may be one or more. An example of the electronic component of the present invention in which a coil is formed within the element body is a laminated coil component, but depending on the type of passive element formed by the conductor layers, the electronic component may be a laminated capacitor component, a laminated resistor component, a laminated thermistor component, or the like.
[0026] The element body does not need to have a conductive layer inside. In this case, the element body can also be used as a winding core by winding a winding around it. An example of the electronic component of the present invention in which a wire is wound around the element body is a wire-wound coil component. The number of coils formed by winding a wire around the element body may be one or more.
[0027] [Insulating film] In one embodiment of the electronic component of the present invention, the insulating film covers at least a part of the surface of the element body.
[0028] The insulating film includes glass. Examples of glass that can be used to form the insulating film include B-Si glass, Ba-B-Si glass, B-Si-Zn glass, B-Si-Zn-Ba glass, and B-Si-Zn-Ba-Ca-Al glass. In addition to these, alkali metal glasses such as Na-Si glass, K-Si glass, and Li-Si glass, alkaline earth metal glasses such as Mg-Si glass, Ca-Si glass, Ba-Si glass, and Sr-Si glass, Ti-Si glass, Zr-Si glass, and Al-Si glass can also be used. The glass may be a crystallizable glass.
[0029] The weight percentage of glass in the insulating film is not particularly limited, but is preferably 90% by weight or more.
[0030] The thickness of the insulating film is not particularly limited, but is preferably 0.005 μm or more and 10,000 μm or less, and more preferably 0.030 μm or more and 1,500 μm or less. By making the thickness of the insulating film 10 μm or less, the influence on the characteristics of the electronic components can be greatly reduced. The thickness of the insulating film can be measured by observing a cross section of the insulating film cut in the thickness direction with a scanning electron microscope (SEM).
[0031] In addition to glass, the insulating film may contain pigments, silicone-based flame retardants, surface treatment agents such as silane coupling agents and titanate coupling agents, antistatic agents, and the like.
[0032] [Cu segregated product] In one embodiment of the electronic component of the present invention, the Cu segregation containing Cu element is in contact with the element body and the insulating film at the interface between the element body and the insulating film.
[0033] The presence of Cu segregation at the interface between the element body and the insulating film increases the adhesion between the element body and the insulating film. The Cu segregates may be present anywhere on the element body, but are preferably present on the grain boundaries of the ceramic of the element body. Since the grain boundaries of the ceramic of the element body are concave on the surface of the element body, the presence of the Cu segregates on the concave grain boundaries generates an anchor effect, which further improves the adhesion between the Cu segregates and the element body.
[0034] The composition of the Cu segregated matter is not particularly limited as long as it contains at least Cu element, and examples thereof include Cu, CuO, Cu2O, etc. Furthermore, the Cu segregated matter may contain glass.
[0035] A plurality of Cu segregated objects may be present at the interface between the element body and the insulating film. If a plurality of Cu segregated objects are present at the interface between the element body and the insulating film, the adhesion between the element body and the insulating film can be further improved.
[0036] Whether or not Cu segregation is present at the interface between the element body and the insulating film can be confirmed by observing the interface between the element body and the insulating film on a cut surface of the electronic component using a scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX). By checking the concentration distribution of Cu element from the element mapping image near the interface between the element body and the insulating film obtained by SEM-EDX, the shape of Cu segregation near the interface between the element body and the insulating film can be identified. When the element is ferrite, the element is mainly composed of Fe, the Cu segregates are mainly composed of Cu, and the insulating film is mainly composed of Si. Therefore, by comparing the concentrations of Fe, Cu, and Si in the element mapping image, the element, Cu segregates, and insulating film in the element mapping image can be distinguished. Furthermore, when the element body is a ceramic other than ferrite, the element body, Cu segregation, and insulating film in the element mapping image can be distinguished by comparing the concentrations of the main component elements of the ceramic with the Cu element and the Si element. For example, when the element body is alumina, the Al element can be taken as the main component of the ceramic; when the element body is barium titanate for a capacitor, the Ti element or Ba element can be taken as the main component of the ceramic; and when the element body is Zn-based ceramic for a thermistor, the Zn element can be taken as the main component of the ceramic.
[0037] The shape of the Cu segregates is not particularly limited, and may be granular, wedge-shaped, or lamellar. The shape of the Cu segregation can be determined by the aspect ratio and by judging whether the Cu segregation protrudes toward the element body. The aspect ratio of the Cu segregation is expressed as the ratio [La / Lb] (hereinafter also referred to as the aspect ratio) of the length La of the Cu segregation in the direction in which the interface between the element body and the insulating film extends, where La is the length of the Cu segregation in the direction perpendicular to the length La, and Lb is the length of the Cu segregation in the direction perpendicular to the length La. The length Lb corresponds to the distance between two lines, which are assumed to pass through the points closest to the element body and the point farthest from the element body, and are parallel to the direction in which the interface between the element body and the insulating film extends.
[0038] When the shape of the Cu segregation protrudes toward the element body, the shape is made wedge-shaped regardless of the aspect ratio of the Cu segregation. When the shape of the Cu segregation is not wedge-shaped, the shape with the aspect ratio of 3 or less is granular, and the shape with the aspect ratio of more than 3 is layer-shaped. When the shape of the segregated Cu is wedge-shaped, the shape of the segregated Cu except for the portion protruding towards the element body may be granular or lamellar. The layer-like Cu segregation exists only in a part of the interface between the element body and the insulating film, and does not cover the entire interface between the element body and the insulating film.
[0039] FIG. 5 is a cross-sectional view showing a schematic example of the state of the interface between the element body and the insulating film in one embodiment of the electronic component of the present invention. 5, Cu segregations 30 (31, 32) are present at the interface between the element body 10 and the insulating film 20 and are in contact with the element body 10 and the insulating film 20. The thickness of the insulating film 20 in a portion where no Cu segregations 30 are present (the thickness of the insulating film 20 directly above and in contact with the element body 10) is the length indicated by the double-headed arrow T0. Note that the thickness T0 of the insulating film 20 may vary from place to place. In FIG. 5, it can be said that a plurality of Cu segregations exist at the interface between one insulating film 20 and element body 10.
[0040] The length of the Cu segregation 31 in the direction in which the interface between the element body 10 and the insulating film 20 extends (hereinafter also referred to as the horizontal direction) is indicated by a double-headed arrow La1. The length of the Cu segregation 31 in the direction perpendicular to the horizontal direction (hereinafter also referred to as the vertical direction) is indicated by a double-headed arrow Lb1. The aspect ratio [La1 / Lb1] of the Cu segregation 31 is approximately 1.4. Therefore, the shape of the Cu segregation 31 is granular. The thickness of the Cu segregation 31 is the length indicated by the double-headed arrow Lb1, and the thickness of the insulating film 20 directly above and in contact with the Cu segregation 31 is the length indicated by the double-headed arrow T1. The Cu segregates 31 do not protrude toward the element body 10. In FIG. 5, the sum of the thickness Lb1 of the Cu segregates 31 and the thickness T1 of the insulating film 20 that is in contact with and directly above the Cu segregates 31 is equal to the thickness T0 of the insulating film 20. Furthermore, the thickness T0 of the insulating film 20 is thicker than the thickness T1 of the insulating film 20 directly above and in contact with the Cu segregation 31. When the thickness T0 of the insulating film 20 is thicker than the thickness T1 of the insulating film 20 directly above and in contact with the Cu segregation 31, the unevenness of the surface of the insulating film caused by the presence of the Cu segregation is reduced, and the smoothness of the surface of the insulating film is improved.
[0041] The Cu segregation 32 has a protruding portion 32a that protrudes toward the element body 10. Therefore, the shape of the Cu segregation 32 can be said to be wedge-shaped, regardless of the aspect ratio. Whether or not the Cu segregation protrudes toward the element body is determined by estimating the shape of the element body surface in the case where no Cu segregation is present in a portion where Cu segregation is present, from the shape of the element body surface in the portion where no Cu segregation is present, and when the Cu segregation is located inside (toward the element body) the estimated element body surface, the Cu segregation is deemed to protrude toward the element body. The Cu segregation may protrude not to the element body side but to the insulating film side. However, if the Cu segregation protrudes only to the insulating film side but not to the element body side, it is judged whether the shape is granular or layered depending on the aspect ratio.
[0042] FIG. 6 is a cross-sectional view showing a schematic diagram of another example of the state of the interface between the element body and the insulating film in an embodiment of the electronic component of the present invention. The Cu segregation 33 has a horizontal length indicated by a double-headed arrow La3 and a vertical length indicated by a double-headed arrow Lb3. The aspect ratio [La3 / Lb3] is about 10. Therefore, the shape of the Cu segregation 33 is layered. The layer-like Cu segregation exists only in a part of the interface between the element body and the insulating film, and does not cover the entire interface between the element body and the insulating film. The thickness of the Cu segregation 33 is the length indicated by the double-headed arrow Lb3, and the thickness of the insulating film 20 directly above and in contact with the Cu segregation 33 is the length indicated by the double-headed arrow T3. The Cu segregates 33 do not protrude toward the element body 10. In FIG. 6, the sum of the thickness Lb3 of the Cu segregates 33 and the thickness T3 of the insulating film 20 that is in contact with and directly above the Cu segregates 33 is equal to the thickness T0 of the insulating film 20. Moreover, the thickness T0 of the insulating film 20 is thicker than the thickness T3 of the insulating film 20 directly above and in contact with the Cu segregation 33.
[0043] The shape of the Cu segregation is related to the thickness of the insulating film directly above and in contact with the Cu segregation. When the thickness of the insulating film directly above and in contact with the segregated Cu is less than 0.5 μm, the segregated Cu tends to have a granular or wedge-like shape. On the other hand, when the thickness of the insulating film directly on and in contact with the segregated Cu is 0.5 μm or more, the segregated Cu tends to have a layered shape. In addition, when identifying the shape of the Cu segregation, the portion where the Cu segregation is mixed with the glass that constitutes the insulating film is also considered to be part of the Cu segregation. Therefore, the shape is identified as one Cu segregation, including the portion where the Cu segregation is mixed with the glass that constitutes the insulating film. The boundary between the Cu segregation and the insulating film can be confirmed by performing elemental mapping of the Si element and the Cu element by SEM-EDX.
[0044] The shape and aspect ratio of the segregated Cu particles, and the thickness of the insulating film directly on and in contact with the segregated Cu particles can be measured by SEM-EDX. The shape and aspect ratio of the Cu segregation are determined for each individual Cu segregation. The thickness of the insulating film directly above the Cu segregation is the minimum value of the length from a point on the top surface of the Cu segregation to a point on the top surface of the insulating film directly above in the vertical direction for each individual Cu segregation, based on an SEM-EDX image taken so that the Cu segregation and the insulating film are within one field of view. The thickness of the insulating film in a portion where no Cu segregation is present is the average value of the lengths from the surface of the element body to the top surface of the insulating film measured at three points. The above three points are selected by visual inspection from the point where the length from the surface of the element body to the top surface of the insulating film is the longest, the point where the length is the shortest, and the point where the length is intermediate between these two.
[0045] The surface of the element body may be covered with multiple insulating films. The element body 10 shown in Figures 1 and 2 and the element body 11 shown in Figures 3 and 4 are both examples in which the surface is covered with multiple insulating films. The insulating films may have different compositions or may have the same composition.
[0046] When the surface of the element body is covered with multiple insulating films, Cu segregation may be present at the interface between each insulating film and the element body. Also, a part of the Cu segregation may not be covered by the insulating film. Such Cu segregation is exposed on the surface of the element body.
[0047] The insulating film may be scattered on the surface of the element body. An example in which insulating films are scattered on the surface of the element body will be described with reference to FIG. FIG. 7 is a cross-sectional view showing a schematic diagram of yet another example of the state of the interface between the element body and the insulating film in an embodiment of the electronic component of the present invention. Two insulating films 20a, 20b are provided on the surface of the element body 10 shown in Fig. 7. Cu segregations 34a, 34b are present at the interfaces between the insulating films 20a, 20b and the element body 10, respectively. The surface of element body 10 has portions that are not covered with insulating film 20, and these portions expose the surface of element body 10. Cu segregates 34c exist in portions of the surface of element body 10 that are not covered with insulating film 20. Therefore, Cu segregates 34c are exposed on the surface of element body 10.
[0048] The surface of the element constituting the electronic component of the present invention has Cu segregation, which makes plating growth likely to occur. By covering the Cu segregation with an insulating film, the promotion of plating growth by the Cu segregation is inhibited, and plating growth in unintended areas of the surface of the element can be suppressed. From the above viewpoint, it is preferable that an insulating film that covers the Cu segregation is formed around the external electrode to be plated. If an insulating film is formed around the external electrode to be plated, the formation of plating in the area where the insulating film is formed can be suppressed.
[0049] [External electrode] One embodiment of the electronic component of the present invention has external electrodes, but the form thereof is not particularly limited. Examples of the external electrode include a combination of a base electrode layer and a coating layer formed on the surface of the base electrode layer, a metal plate, a lead terminal, etc. The base electrode layer may be an electrode formed by applying a glass paste containing glass and a conductor to the surface of the element body and baking it, or an electrode formed directly on the surface of the element body by sputtering or plating.
[0050] As the glass contained in the base electrode layer, the same glass as that constituting the insulating film can be suitably used. The base electrode layer preferably has a conductor portion containing a conductor and a glass portion containing glass. The conductor portion preferably contains at least one metal element selected from the group consisting of Ni, Sn, Pd, Au, Ag, Pt, Bi, Cu, and Zn as a conductor, and preferably contains conductive particles containing these elements. The conductor portion preferably contains Ag as a conductor. Ag has high electrical conductivity. Furthermore, a base electrode layer containing Ag as a conductor is easy to form.
[0051] The average particle size of the conductive particles is not particularly limited, but is preferably 0.5 μm or more and 10 μm or less.
[0052] The weight ratio of the conductive particles in the base electrode layer is not particularly limited, but is preferably 71% by weight or more and 98% by weight or less.
[0053] The weight percentage of glass in the base electrode layer is preferably 2% by weight or more and 15% by weight or less. When the weight ratio of glass in the base electrode layer is 15% by weight or less, the resistance value of the base electrode layer does not become too large. Also, when the weight ratio of glass in the base electrode layer is 2% by weight or more, the density of the base electrode layer can be increased, and the plating solution and moisture can be prevented from penetrating into the inside of the base electrode layer and from penetrating into the element through the base electrode layer.
[0054] The covering layer is preferably, for example, a plating layer provided on the surface of the base electrode layer. The plating layer preferably contains at least one metal selected from the group consisting of Cu, Ni, Sn, Pd, Au, Ag, Pt, Bi, and Zn. The plating layer may be a single layer or may be two or more layers. It is more preferable that the plating layer is a layer having a Ni plating layer and a Sn plating layer provided on the base electrode layer. The Ni plating layer prevents water from penetrating into the element body, and the Sn plating layer improves the mountability of the electronic component.
[0055] Cu segregation may be present at the interface between the element body and the base electrode layer (preferably at the interface between the element body and the glass portion). The presence of Cu segregation at the interface between the element body and the base electrode layer enhances adhesion between the element body and the base electrode layer.
[0056] The electronic component of this embodiment has excellent adhesion between the element body and the insulating film. The electronic component of this embodiment is not limited to a laminated coil component or a wound coil component, and may be any component that uses a ceramic containing Cu as the element body.
[0057] [Electronic component manufacturing method] First embodiment A first embodiment of a method for manufacturing an electronic component of the present invention includes a ceramic sheet preparation step of preparing a ceramic sheet by forming a ceramic raw material containing Cu into a sheet shape; a conductor pattern formation step of forming a conductor pattern that becomes a via hole and a coil pattern in the ceramic sheet; a laminate preparation step of obtaining a laminate by stacking the ceramic sheets; a firing step of firing the laminate to obtain a ceramic body; and an insulating film formation step of forming an insulating film containing glass on the surface of the body.
[0058] [Ceramic sheet preparation process] In the ceramic sheet preparation step, a ceramic raw material containing Cu element is formed into a sheet shape. When a ferrite raw material is used as the ceramic raw material, a powdered ferrite raw material can be obtained, for example, by weighing out Fe2O3, ZnO, CuO, and NiO to a predetermined ratio, wet mixing the mixture, and then pulverizing, drying, and pre-firing the mixture.
[0059] Next, the ceramic raw material, an organic binder such as a polyvinyl butyral resin, an organic solvent such as ethanol or toluene, etc. are mixed and pulverized to produce a ceramic slurry. Next, the ceramic slurry is formed into a sheet of a predetermined thickness by a doctor blade method or the like, and then punched out into a predetermined shape to produce a ceramic sheet.
[0060] The content of Cu element in the ceramic raw material is preferably 6 mol % or more and 10 mol % or less. The higher the Cu content in the ceramic raw material, the more likely Cu segregation is to occur on the surface of the element body.
[0061] The content of the organic binder in the ceramic sheet is preferably 25% by weight or more and 35% by weight or less. The organic binder contained in the ceramic sheet contains carbon, which combines with oxygen in the atmosphere during firing to reduce the oxygen concentration. Therefore, the higher the organic binder content, the more likely it is that the oxygen concentration will be lower during the firing process, and as a result, Cu segregation will be more likely to occur on the surface of the element.
[0062] The thickness of the ceramic sheet is not particularly limited, but is preferably 15 μm or more and 50 μm or less.
[0063] [Conductor pattern formation process] In the conductor pattern formation process, a conductive paste such as Ag paste is applied to each ceramic sheet by screen printing, etc. to form a conductor pattern. When forming the conductor pattern that will become the via conductor, via holes are formed in advance by irradiating a laser onto predetermined locations on the ceramic sheet, and the via holes are filled with the conductive paste.
[0064] [Laminate preparation process] After stacking the ceramic sheets, they are pressed together by a warm isostatic press (WIP) process or the like to produce a laminate. The number of laminated ceramic sheets is not particularly limited, but is preferably 30 layers or more and 100 layers or less.
[0065] [Firing process] In the firing step, the laminate is fired to obtain an element body. The firing conditions are set so that Cu segregation occurs on the surface of the body. Whether or not Cu segregation occurs on the surface of the element body is influenced not only by the composition of the ceramic raw materials, but also by the amount of carbon contained in the laminate, the firing temperature (maximum temperature), the rate of temperature rise, the firing atmosphere, the material of the firing furnace, etc. When these conditions are appropriately selected, Cu segregation will precipitate on the surface of the element body. In other words, if the firing conditions are not appropriate, Cu segregation will not precipitate on the surface of the body even if the composition of the ceramic raw materials is the same.
[0066] The firing temperature (maximum temperature) in the firing step is preferably 1000°C or higher and 1300°C or lower. If the firing temperature (maximum temperature) in the firing step is 1000° C. or higher, Cu segregation is likely to occur on the surface of the element body.
[0067] The oxygen concentration in the firing step is preferably 15% by volume or less, and more preferably 5% by volume or less. If the oxygen content in the firing atmosphere is 15% by volume or less, Cu segregation is likely to occur on the surface of the body. The balance gas in the firing step is preferably nitrogen or argon.
[0068] The temperature rise rate in the firing step is preferably 10° C. / min or less. The shorter the time required to reach the sintering temperature, the more likely Cu segregation is to occur on the surface of the element body.
[0069] The furnace material constituting the firing furnace in which the laminate is fired in the firing step is preferably made of a high-density material such as a mixture of alumina and silicon. If the furnace materials that make up the firing furnace are made of high-density materials, Cu segregation is likely to occur.
[0070] [Insulating film formation process] In the insulating film forming step, an insulating film containing glass is formed on the surface of the element obtained in the firing step.
[0071] The insulating film can be formed by applying a paste containing glass (hereinafter referred to as glass paste) to the surface of the element body and baking (firing) it. The glass paste may contain a resin and a dispersion medium in addition to glass.
[0072] As the glass, B-Si glass, Ba-B-Si glass, B-Si-Zn glass, B-Si-Zn-Ba glass, B-Si-Zn-Ba-Ca-Al glass, etc. can be used. In addition to these, alkali metal glass such as Na-Si glass, K-Si glass, Li-Si glass, alkaline earth metal glass such as Mg-Si glass, Ca-Si glass, Ba-Si glass, Sr-Si glass, Ti-Si glass, Zr-Si glass, Al-Si glass, etc. can also be used. The glass may be a crystallizable glass.
[0073] The average particle size of the glass constituting the glass paste is not particularly limited, but is preferably 0.01 μm or more and 4.00 μm or less.
[0074] The larger the average particle size of the glass constituting the glass paste, the lower the fluidity of the glass paste during firing, and the thicker the insulating film becomes, which makes it easier for layered Cu segregation to form. On the other hand, the smaller the average particle size of the glass constituting the glass paste, the higher the fluidity of the glass paste during firing, and the thinner the insulating film becomes, which makes it easier for granular or wedge-shaped Cu segregation to form.
[0075] The glass paste applied to the surface of the element is dried. There are no particular limitations on the drying conditions, but it is sufficient to heat the element at 150°C for about 30 minutes. When the glass paste is applied to the surface of the element body multiple times, it is preferable to repeat the application and drying of the glass paste. In addition to the application and drying of the glass paste, the insulating film can also be formed by repeating one or more sets of baking, which will be described later, in addition to the application and drying of the glass paste.
[0076] The temperature (baking temperature) when forming the insulating film is not particularly limited, but is preferably 750°C or higher and 900°C or lower. If the baking temperature is 750° C. or higher and 900° C. or lower, Cu segregation is more likely to occur on the surface of the element body. In addition, the Cu segregation and the glass contained in the insulating film are more likely to form a mixture, which can improve the adhesion between the element body and the insulating film. The baking is preferably carried out in a non-oxidizing atmosphere. By performing the baking in a non-oxidizing atmosphere at 825°C or higher, it is possible to promote segregation of Cu on the surface of the element body, which in turn improves the adhesion between the element body and the insulating film.
[0077] The method for forming an insulating film on the surface of an element body is not limited to the above-mentioned method of applying and firing a glass paste, and examples thereof include sputtering, electron beam deposition, thermal CVD, plasma CVD, spraying, dipping, dip spin coating, and sol-gel methods, and two or more of these may be combined.
[0078] The method for manufacturing the element may be a method other than the sheet lamination method described above. Examples of methods other than the sheet lamination method include a print lamination method (build-up method). In addition to the above-mentioned methods, a method using photolithography can also be used to form wiring and vias on the sheet surface. Following the above steps, an external electrode forming step may be carried out to form external electrodes on the surface of the element body.
[0079] [External electrode formation process] In the external electrode forming step, external electrodes are formed on the surface of the element body. The external electrode formation step may be, for example, a method in which Ni plating and Sn plating are carried out in this order on the surface of the element body to form a Ni / Sn plating layer.
[0080] In the external electrode formation process, prior to the process of forming the plating layer, a glass paste containing glass and conductive particles may be applied to the surface of the element body and fired (coated) to form a base electrode layer, and a Ni / Sn plating layer serving as a coating layer may be formed on the surface of this layer.
[0081] By the above steps, an electronic component having a conductor layer inside an element body, for example as shown in FIG. 1 and FIG. 2, can be manufactured.
[0082] Second Embodiment A second embodiment of the method for manufacturing an electronic component of the present invention includes a body preparation step of preparing a ceramic body by shaping a ceramic raw material containing Cu element, an insulating film formation step of forming an insulating film on the surface of the body, and a coil formation step of winding a wire that will become a coil around the surface of the body.
[0083] [Body preparation process] As the ceramic raw material used in the element preparation step, the same ceramic raw material as that used in the first embodiment of the method for producing an electronic component of the present invention can be suitably used.
[0084] The ceramic raw material can be molded into a desired shape by a conventional powder molding method. In this case, resin, binder, etc. may be added to the ceramic raw material as necessary. The ceramic raw material is molded into a molded body, which is then fired to form an element body. In this case, the molded body is fired under conditions that cause Cu segregation on the surface of the element body. The element obtained by the above method does not contain any conductive layer inside.
[0085] [Insulating film formation process] In the insulating film forming step, an insulating film is formed on the surface of the element body obtained in the firing step. The insulating film forming step in the second embodiment of the method for producing an electronic component of the present invention is similar to the insulating film forming step in the first embodiment of the electronic component of the present invention.
[0086] [Coil forming process] In the coil formation process, a wire that will become the coil is wound around the surface of the element body. The number of turns of the winding and the diameter of the winding may be appropriately changed according to the characteristics required for the electronic component.
[0087] Through the above steps, the electronic component according to the embodiment of the present invention is manufactured. In the second embodiment of the method for producing an electronic component of the present invention, an external electrode forming step of forming external electrodes on the surface of the element body may be performed. The external electrode forming step in the second embodiment of the method for producing an electronic component of the present invention is similar to the external electrode forming step in the first embodiment of the method for producing an electronic component of the present invention. In this case, the external electrode forming step is performed before the coil forming step, and both ends of the wire that will become the coil may be connected to the external electrodes in the coil forming step. The method for connecting the windings that form the coil to the external electrodes is not particularly limited, but may be, for example, a method of joining them by thermocompression bonding.
[0088] By the above steps, it is possible to manufacture an electronic component in which a winding that forms a coil is wound around an element body, as shown in, for example, FIGS. EXAMPLES
[0089] Hereinafter, examples will be given that more specifically disclose an embodiment of the electronic component of the present invention, but the present invention is not limited to these examples.
[0090] Example 1 [Body preparation process] A ferrite raw material was prepared so that the Fe content was constant, the Ni / Zn molar ratio was 2.3, and the Cu content was 8 mol%, and was formed into a barbell shape having a winding portion and a flange portion to obtain a compact.
[0091] The green body was fired at 1100°C for 1 hour to obtain a ceramic body. The firing atmosphere was normal pressure with an oxygen partial pressure of 10% by volume. As shown in Figures 1 and 2, the shape of the obtained element was a substantially rectangular parallelepiped having a first end face and a second end face facing each other in the longitudinal direction, a first side face and a second side face facing each other in the width direction, and a top face and a bottom face facing each other in the thickness direction.
[0092] [Insulating film formation process] A glass paste was prepared by mixing glass frit (borosilicate glass) and a solvent (terpineol). The element body was immersed in the glass paste with the first side surface facing downward to a position halfway in the width direction of the element body, and then dried at 150°C for 30 minutes. The element body was then turned upside down, and the element body was immersed in the glass paste with the second side surface facing downward to a position halfway in the width direction of the element body, and then dried at 150°C for 30 minutes. Finally, baking was performed at 650°C for 10 minutes to form an insulating film, and the electronic component according to Example 1 was manufactured. Note that the higher the baking temperature, the more likely the segregation of Cu segregation is to occur, so 750°C or higher is preferable, and by setting the baking temperature to 850°C or higher, the fluidity of the Cu segregation itself is improved. As shown in FIG. 1 , an insulating film was formed on the surface of the body constituting the electronic component of Example 1, covering the entire first side surface of the body as well as parts of the first end surface, second end surface, top surface and bottom surface of the body, and an insulating film was formed on the surface of the body constituting the electronic component of Example 1, covering the entire second side surface of the body as well as parts of the first end surface, second end surface, top surface and bottom surface of the body.
[0093] (Example 2, Comparative Examples 1 to 3) Except for changing the Cu content to 6 mol%, 4 mol%, 1 mol%, and 0 mol% without changing the Fe amount and Ni / Zn molar ratio in the ferrite raw material, electronic components according to Example 2 and Comparative Examples 1 to 3 were manufactured in the same manner as in Example 1. The sintered density of the bodies of each Example and Comparative Example was approximately the same as that of Example 1.
[0094] Comparative Example 4 Except for changing the firing temperature (maximum temperature) of the compact to 950° C. or less without changing the composition of the ferrite raw material, an electronic device according to Comparative Example 4 was manufactured in the same manner as in Example 1. The sintered density of the body of Comparative Example 4 was approximately the same as that of Example 1.
[0095] [Measurement of Cu content in element body] When the Cu element content of the element bodies was measured by the above-mentioned WD-XRF, it was found to be the same as the Cu element content in the ferrite raw material.
[0096] [Observation by SEM-EDX] For the electronic device according to Example 2, the vicinity of the interface between the element body and the insulating film was observed at three points by SEM-EDX, and Cu element mapping was performed. The results are shown in FIGS. In addition, for the electronic components according to Example 1 and Comparative Examples 1 to 4, the vicinity of the interface between the element body and the insulating film was observed by SEM-EDX. As a result, in the electronic component according to Example 1, Cu segregation was confirmed at the interface between the element body and the insulating film, but in all of the electronic components according to Comparative Examples 1 to 4, no Cu segregation was confirmed.
[0097] FIG. 8 is an element mapping image of Cu at the interface between the element body and the insulating film of the electronic component according to Example 2. In FIG. From the result in FIG. 8, it was confirmed that in the electronic component according to Example 2, a region with a high concentration of Cu element (Cu segregates 31) was present at the interface between the element body 10 and the insulating film 20. The aspect ratio of the Cu segregates 31 was 2.0. Therefore, it was confirmed that granular Cu segregates 31 were present in the SEM-EDX element mapping image shown in FIG. 8. The thickness of the insulating film 20 directly above and in contact with the Cu segregates 31 was 0.03 μm.
[0098] Fig. 9 is an element mapping image of Cu at the interface between the element body and the insulating film of the electronic component according to Example 2. The position where SEM-EDX is measured in Fig. 9 is different from the position where SEM-EDX is measured in Fig. 8. From the result in Fig. 9, it was confirmed that in the electronic component according to Example 2, a region with a high concentration of Cu element (Cu segregates 32) was present at the interface between the element body 10 and the insulating film 20. The Cu segregates 32 protruded toward the element body 10. Therefore, it was confirmed that the wedge-shaped Cu segregates 32 were present in the SEM-EDX element mapping image shown in Fig. 9. The thickness of the insulating film 20 directly above and in contact with the Cu segregates 32 was 0.13 µm.
[0099] Fig. 10 is an element mapping image of Cu at the interface between the element body and the insulating film of the electronic component according to Example 2. The position where SEM-EDX is measured in Fig. 10 is different from the position where SEM-EDX is measured in Fig. 8 and the position where SEM-EDX is measured in Fig. 9. 10, it was confirmed that in the electronic component according to Example 2, layer-like Cu segregation 33 was present at the interface between element body 10 and insulating film 20. The thickness of insulating film 20 directly above and in contact with Cu segregation 33 was 0.5 μm. In addition, from the results of FIGS. 8, 9, and 10, it was confirmed that a plurality of Cu segregated particles with different shapes existed at the interface between the insulating film and the element body in the same electronic component.
[0100] [Measurement of load capacity (scratch test)] Using an ultra-thin film scratch tester (CSR5000, manufactured by Rhesca Corporation), a diamond indenter (tip R: 5 μm) was pressed against the insulating film of each element with a specified load and moved 150 μm to check for peeling of the insulating film. The load was increased in 5 mN increments from 5 mN to 60 mN. The highest load at which peeling did not occur is shown in Table 1 as the withstand load. It should be noted that if the withstand load is 40 mN or more, it can be determined that the adhesion between the element and the insulating film is sufficiently high.
[0101] [Table 1]
[0102] From the results in Table 1, it was confirmed that the electronic component according to the embodiment of the present invention has high adhesion between the element body and the insulating film. [Industrial Applicability]
[0103] The electronic component according to the embodiment of the present invention can be suitably used as an inductor, an antenna, a noise filter, a radio wave absorber, an LC filter combined with a capacitor, a winding core, or the like. [Explanation of symbols]
[0104] 1, 2 Electronic components 10, 11 Base body 10a: First end surface of element 10b: second end surface of element 10c First side of the body 10d Second side of the body 10e Top surface of the body 10f Bottom of the body 20, 20a, 20b Insulating film 30, 31, 32, 33, 34a, 34b, 34c Cu segregated 32a Cu segregation protruding toward the element 40 Conductor Layer 43 Windings 50 external electrode 60 Winding core 61 Flange L Length direction The lateral length of La1, La3Cu segregates Lb1, Lb3: Longitudinal length of Cu segregates T thickness direction T0 Insulation Thickness T1, T3: Thickness of the insulating film directly on top of the Cu segregation W Width direction
Claims
1. A ceramic body containing Cu, an insulating film containing glass covering at least a part of a surface of the body, and Cu segregated matter containing Cu, the Cu segregation is in contact with the element body and the insulating film at an interface between the element body and the insulating film.
2. 2. The electronic component according to claim 1, wherein the shape of the segregated Cu is a wedge shape with a part of the segregated Cu protruding toward the element body.
3. 2. The electronic component according to claim 1, wherein, when a length of the Cu segregation in a direction in which an interface between the element body and the insulating film extends is La and a length in a direction perpendicular to the length La is Lb, the shape of the Cu segregation is granular such that a ratio [La / Lb] of the length La to the length Lb is 3 or less.
4. 4. The electronic component according to claim 2, wherein the insulating film directly above and in contact with the Cu segregation has a thickness of less than 0.5 [mu]m.
5. 2. The electronic component according to claim 1, wherein, when a length of the Cu segregation in a direction in which an interface between the element body and the insulating film extends is La and a length in a direction perpendicular to the length La is Lb, the shape of the Cu segregation is a layer such that a ratio [La / Lb] of the length La to the length Lb exceeds 3.
6. 6. The electronic component according to claim 5, wherein the insulating film directly above and in contact with the Cu segregation has a thickness of 0.5 [mu]m or more.
7. 7. The electronic component according to claim 1, wherein a plurality of said Cu segregated particles are present at the interface between said element body and said insulating film.
8. 8. The electronic component according to claim 1, wherein the insulating film directly above and in contact with the element body has a thickness greater than a thickness of the insulating film directly above and in contact with the Cu segregation.
9. 9. The electronic component according to claim 1, wherein a surface of said element body is covered with a plurality of said insulating films.
Citation Information
Patent Citations
Composite electronic apparatus and method for manufacturing same
JP2005317748A
Ceramic electronic component and method for manufacturing ceramic electronic component
JP2009302129A
Method of manufacturing ceramic electronic component
JP2014036056A
Laminated coil component
JP2017204565A
Ceramic electronic component and manufacturing method thereof
JP2018098372A