Gravure ink for cosmetic materials

The gravure ink for decorative materials addresses adhesion and VOC emission issues by using a urethane resin-based formulation with specific properties, ensuring effective adhesion and reduced environmental impact.

JP7552797B2Active Publication Date: 2024-09-18TOYO INK MFG CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023092035
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-06-07
Filing Date
2023-06-05
Publication Date
2024-09-18
Estimated Expiration
2043-06-05

Smart Images

  • Figure 0007552797000001
    Figure 0007552797000001
  • Figure 0007552797000002
    Figure 0007552797000002
  • Figure 0007552797000003
    Figure 0007552797000003
Patent Text Reader

Abstract

To provide rotogravure ink for a decorative material excellent in adhesion when used for printing on a paper substrate and having less environmental load.SOLUTION: A rotogravure ink for a decorative material is used for forming a printed layer of a decorative material including the printed layer on a paper substrate. The rotogravure ink contains a resin component including an urethane resin and an inorganic pigment. The urethane resin component has an amine value. The sum of the urethane bond concentration and urea bond concentration of the urethane resin is 0.5-3 mmol / g. The rupture ductility of the resin component is 100-400%, and the rupture strength of the resin component is 5 MPa or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gravure ink for a decorative material including a paper substrate, and more specifically to a gravure ink for a decorative material having good adhesion to a paper substrate. [Background technology]

[0002] Decorative materials used for furniture, cabinets, etc. include wood-based materials, inorganic materials, synthetic resin-based materials, and metal-based materials such as steel plates, and are laminated with decorative sheets on which patterns such as wood grain patterns are printed using ink. Such decorative sheets are required to have various properties during use, such as weather resistance, light resistance, heat resistance, water resistance, solvent resistance, surface hardness, abrasion resistance, scratch resistance, etc. In order to satisfy these requirements, a surface protective layer is applied to the surface of the substrate (Patent Document 1). Conventionally, as gravure inks for decorative materials including paper substrates, soluble cellulose-plasticizer-based inks containing soluble cellulose resin as a binder and a plasticizer, and soluble cellulose-alkyd-based inks containing soluble cellulose resin and alkyd resin as binders have been used. Of these, soluble cellulose-plasticizer-based printing inks lack flexibility of printed matter, and in addition, have poor adhesion to resin-impregnated reinforced paper between sheets. On the other hand, soluble cellulose-alkyd-based inks improve the flexibility of printed matter, but have poor adhesion to resin-impregnated reinforced paper between sheets, and adhesion when urethane resin or aminoalkyd resin is used in the top coat layer. In response to these issues, inks using urethane resin and soluble cellulose resin as binder resins have been developed, but the inks contain aromatic organic solvents, and there remain issues in terms of environmental impact (Patent Document 2).

[0003] On the other hand, from the viewpoint of protecting the global environment, the release of volatile organic compounds (VOCs) into the atmosphere during printing with inks that use organic solvents has become a problem. The impact is particularly large in gravure printing for mass-produced cosmetic materials, and reducing VOC emissions is one of the challenges. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-178329 A [Patent Document 2] JP 2001-115076 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide a gravure ink for decorative materials that has good adhesion and hiding power when printed on a paper substrate, can reduce VOCs, and has a lower environmental impact. [Means for solving the problem]

[0006] In view of the above problems, the present inventors conducted intensive research and found that the problems could be solved by using the gravure ink for decorative materials described below, thereby completing the present invention.

[0007] That is, the present invention provides a gravure ink for a decorative material for forming a printed layer of a decorative material including a printed layer on a paper base material, the gravure ink comprising: The gravure ink contains a resin component including a urethane resin and an inorganic pigment, The urethane resin component has an amine value, the sum of the urethane bond concentration and the urea bond concentration of the urethane resin is 0.5 to 3 mmol / g; The resin component has a breaking elongation of 100 to 400%, and The present invention relates to a gravure ink for decorative materials, wherein the resin component has a breaking strength of 5 MPa or more.

[0008] The present invention also relates to the gravure ink for decorative materials, wherein the inorganic pigment is a white pigment.

[0009] The present invention also relates to the gravure ink for decorative materials, wherein the urethane resin has a weight average molecular weight of 5,000 to 100,000.

[0010] The present invention also relates to the gravure ink for decorative materials, wherein the resin component further contains a soluble nitrocellulose resin, and the mass ratio of the urethane resin to the soluble nitrocellulose resin is 60 / 40 to 90 / 10.

[0011] The present invention also relates to the gravure ink for decorative materials, wherein the resin component further contains an isocyanate-based curing agent, and the mass ratio of the urethane resin to the isocyanate-based curing agent is 100 / 0 to 30 / 70.

[0012] The present invention also relates to the gravure ink for decorative materials, wherein the resin component has an acid value.

[0013] The present invention also relates to the gravure ink for decorative materials, which further contains a dispersant and / or a silane coupling agent.

[0014] The present invention also provides a printing layer formed by printing the above gravure ink for decorative materials on a paper substrate. The present invention relates to a printed matter for a cosmetic material having the above-mentioned properties.

[0015] The present invention also provides a method for producing a decorative material, comprising the steps of: A step of gravure printing the above-mentioned gravure ink for decorative materials onto a paper substrate. The present invention relates to a method for producing a cosmetic material, comprising the steps of:

[0016] The present invention also provides a decorative material comprising a printed layer on a paper substrate, The printing layer contains a resin component including a urethane resin and an inorganic pigment, The urethane resin component has an amine value, the sum of the urethane bond concentration and the urea bond concentration of the urethane resin is 0.5 to 3 mmol / g; The resin component has a breaking elongation of 100 to 400%, and The decorative material relates to the resin component having a breaking strength of 5 MPa or more. Effect of the Invention

[0017] INDUSTRIAL APPLICABILITY The present invention makes it possible to provide a gravure ink for decorative materials which has good adhesion and hiding power when printed on a paper substrate, reduces VOCs, and has a lower environmental impact. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] A typical embodiment of the present invention is a gravure ink (hereinafter, simply referred to as "ink") that is printed on a paper substrate to form a printed layer, which becomes a printed matter for a decorative material. The printed matter for a decorative material can be used as it is as decorative paper or a decorative material, or can be laminated to another substrate as a decorative sheet to make a decorative material. The gravure ink for decorative materials of the present invention contains a resin component and a pigment, and the resin component contains a urethane resin having a urethane bond concentration of 0.5 to 3 mmol / g. The resin component also has a specific breaking elongation and breaking strength. In the present invention, unless otherwise specified, the urethane resin includes a urethane urea resin. If the breaking strength of the resin component is weak, the cohesive failure of the printing layer is likely to occur due to the weak cohesive force of the ink, and the adhesion is reduced. If the breaking elongation of the resin component is small, the stress applied to the printing layer when peeling off the cellophane tape, as in the case of evaluating the adhesion to the substrate, is difficult to disperse, and the printing layer is likely to be broken or torn, and the adhesion is reduced. In addition, the larger the breaking elongation, the higher the molecular weight tends to be, and the larger the amount of dilution solvent used during printing, so the breaking elongation is 400% or less from the viewpoint of reducing VOC emissions. That is, when the breaking elongation of the resin component is 100 to 400% and the breaking strength of the resin component is 5 MPa or more, the ink cohesive force and the adhesion between the paper substrate and the ink are balanced, and the ink adhesion to the substrate is good, and further, the environmental load can be reduced from the viewpoint of reducing VOC emissions.

[0019] <Breaking elongation, breaking strength> In the present invention, the breaking elongation of the resin component refers to the elongation percentage when a dry coating film of the resin component having dimensions of a thickness of 0.15 mm, a width of 5 mm, and a length of 30 mm is pulled by a tensile tester and the coating film breaks, and refers to a value measured at a pulling speed of 50 mm / min and a room temperature of 25°C using a tensile tester manufactured by Intesco in accordance with JIS K7127. When the breaking elongation is 100 to 400% based on the length before pulling, the ink has good adhesion to the substrate. The breaking elongation is preferably 150 to 380%, and more preferably 200 to 375%. The breaking strength refers to the stress when the dried coating film of the resin component is pulled under the above conditions and the coating film breaks. When the breaking strength is 5 to 100 MPa, the ink has good adhesion to the substrate in balance with the breaking elongation. The breaking elongation is preferably 7 to 70 MPa, and more preferably 7 to 50 MPa. In order to obtain the above breaking elongation and breaking strength, it is effective to use, for example, a urethane resin having an amine value. In addition, a method of selecting a nitrocellulose resin as a co-resin and using it with the urethane resin described below in a mass ratio (urethane resin / nitrocellulose resin) of 60 / 40 to 100 / 0, a method of adjusting the urethane bond concentration to 0.5 to 3 mmol / g or a urethane bond concentration described later, etc. can be taken. Among these, it is preferable to adjust the breaking elongation and breaking strength using a curing agent. The amount of the curing agent used is preferably the content ratio described later. In addition, it is possible to take a method of adjusting the weight average molecular weight of the urethane resin to 5000 to 100000 or a weight average molecular weight described later. Among these, it is preferable to combine the condition of the urethane bond concentration with the adjustment of the mass ratio of the urethane resin and the co-resin in order to adjust the breaking elongation and breaking strength, and it is more preferable to combine it with the adjustment of the amount of the curing agent used. However, the means are not limited to these.

[0020] <Resin component> The resin component is a so-called binder resin, and includes a resin and a curing agent for the resin used as necessary. The resin may be selected from urethane resin, nitrocellulose resin, acrylic resin, alkyd resin, vinyl chloride-vinyl acetate copolymer resin, and other known resins, and may be used alone or in combination of two or more kinds. From the viewpoint of adhesion to the substrate, at least a urethane resin is included. The mass ratio of the urethane resin to the resin other than the urethane resin is preferably 60 / 40 to 100 / 0, more preferably 70 / 30 to 100 / 0, and even more preferably 80 / 20 to 100 / 0. In addition, when the resin component has an acid value, the pigment dispersibility is improved and the amount of dilution solvent used during ink printing can be reduced, which is preferable from the perspective of reducing VOC emissions. Furthermore, the reduced amount of dilution solvent increases the amount of ink applied during ink printing, improving the hiding power of the printed matter. The acid value of the resin component is preferably from 0.01 to 10 mgKOH / g, more preferably from 0.1 to 8 mgKOH / g, further preferably from 0.5 to 5 mgKOH / g, and particularly preferably from 0.5 to 3 mgKOH / g.

[0021] <Urethane resin> The urethane resin may be any resin having a urethane bond. It is preferably a urethane resin obtained by reacting a polyol with a polyisocyanate, and more preferably a resin obtained by reacting a polyol, a polyhydroxy acid, and a polyisocyanate to form a urethane prepolymer having an isocyanate group at its end, with a polyamine to extend the chain. For example, in this case, in the reaction of the polyol, the polyhydroxy acid, and the polyisocyanate (hereinafter referred to as the urethane-forming step), the functional group molar ratio (NCO / OH) of the polyisocyanate to the polyol and the hydroxy acid is preferably 1.0 to 3.0, and more preferably 1.1 to 2.8. In addition, the functional group molar ratio (amino group / NCO) of the isocyanate group of the urethane prepolymer to the amino group of the polyamine is preferably 0.7 to 1.3.

[0022] In the present invention, the urethane bond concentration of the urethane resin is preferably 0.5 to 3 mmol / g, and more preferably 1 to 2 mmol / g. When the urethane resin contains a urethane urea resin, the total concentration of the urethane bond and the urea bond is preferably 0.5 to 3 mmol / g, and more preferably 1 to 2 mmol / g. By setting the urethane bond concentration and the urea bond concentration within the corresponding range, the ink has good adhesion to the substrate.

[0023] The urethane bond concentration is a value represented by the following formula (1) when (number of moles of NCO / number of moles of OH)>1 in the urethanization step, and is a value represented by the following formula (2) when (number of moles of NCO / number of moles of OH)≦1. Equation (1): Urethane bond concentration (mmol / g) = total number of moles of hydroxyl groups (mmol) / total mass of solids (g) Equation (2): Urethane bond concentration (mmol / g) = total number of moles of isocyanate groups (mmol) / total mass of solids (g) In formulas (1) and (2), the total number of moles of hydroxyl groups represents the total number of moles of hydroxyl groups contained in the polyol, hydroxy acid, and the like used in the urethane-forming step, the total mass of solids represents the total mass of non-volatile components of the urethane resin, and the total number of moles of isocyanate groups represents the total number of moles of isocyanate groups contained in the polyisocyanate.

[0024] The urea bond concentration is a value applied to a urethanization reaction carried out under the condition of (NCO mole number / OH mole number)>1. In the urea formation step, the urea bond concentration is a value represented by the following formula (3) when (number of moles of amino groups / number of moles of NCO)>1, and is a value represented by the following formula (4) when (number of moles of amino groups / number of moles of NCO)≦1. Equation (3): Urea bond concentration (mmol / g) = [total number of moles of isocyanate groups (mmol) - total number of moles of hydroxyl groups (mmol)] / total mass of solids (g) Equation (4): Urea bond concentration (mmol / g) = total number of moles of amino groups (mmol) / total mass of solids (g) In formulas (3) and (4), the total number of moles of isocyanate groups represents the total number of moles of isocyanate groups contained in the polyisocyanate used in the urethanization step, the total number of moles of hydroxyl groups represents the total number of moles of hydroxyl groups contained in the polyol, polyhydroxy acid, etc. used in the urethanization step, the total number of moles of amino groups represents the total number of moles of primary and / or secondary amino groups contained in the polyamine used in the urethanization step, and the total mass of solids represents the total mass of non-volatile components of the urethane resin.

[0025] From the viewpoints of hiding power, adhesion to substrates, and reduction of VOC emissions, the acid value of the urethane resin is preferably 0.01 to 10 mgKOH / g, more preferably 0.1 to 8 mgKOH / g, further preferably 0.5 to 5 mgKOH / g, and particularly preferably 0.5 to 3 mgKOH / g. In order to obtain this acid value, if a polyhydroxy acid is used as the raw material for the urethane resin in the above, most of the acid remains unreacted even in the urethane synthesis reaction, and the urethane resin has an acid value derived from the polyhydroxy acid.

[0026] <Amine value> It was found that when the resin component contains a urethane resin having an amine value, the presence of amino groups improves adhesion. This was particularly noticeable when a curing agent, preferably an isocyanate curing agent, was used. As a result, both hiding power and adhesion could be achieved even in a situation where the pigment concentration was increased to improve hiding power. The amine value of the urethane resin is preferably 0.01 to 30 mgKOH / g, more preferably 0.1 to 20 mgKOH / g, even more preferably 0.5 to 15 mgKOH / g, and particularly preferably 0.5 to 10 mgKOH / g. When it is 0.01 mgKOH / g or more, the cohesive force of the resin can be expected, and when it is 30 mgKOH / g or less, the usable time during ink printing becomes good. The urethane resin having an amine value can be synthesized by using a compound having an amino group such as polyamine as a raw material. A specific synthesis method will be described later.

[0027] The weight-average molecular weight of the urethane resin is preferably 5000 to 100000, and more preferably 10000 to 60000. If the weight-average molecular weight is 5000 or more, the solvent resistance of the ink film after curing is good, and if the weight-average molecular weight is 100000 or less, the amount of dilution organic solvent used during ink printing is reduced, and less VOC is emitted during drying, which is preferable. In addition, if the weight-average molecular weight is small, the breaking elongation tends to be small, and if the molecular weight is large, the breaking elongation tends to be large, and the breaking elongation can be adjusted.

[0028] The polyol preferably has a number average molecular weight of 500 to 10,000 and preferably contains structural units derived from polyether polyol and / or polyester polyol. The total content thereof is preferably 5 to 80 mass%, more preferably 10 to 60 mass%, and even more preferably 10 to 50 mass%, relative to 100 mass% of the urethane resin solid content. The number average molecular weight is calculated from the hydroxyl value assuming that the terminals are hydroxyl groups, and is determined by formula (5). Equation (5) Number average molecular weight of polyol = 1000 × 56.1 × hydroxyl value / hydroxyl value

[0029] Examples of polyols include polyester polyols, polyether polyols, polylactone polyols, polycarbonate polyols, polyolefin polyols, castor oil polyols, hydrogenated castor oil polyols, dimer diols, hydrogenated dimer diols, etc. Polyether polyols and / or polyester polyols are preferred, and polyester polyols are particularly preferred.

[0030] The polyester polyol preferably contains a polyester-derived structural unit composed of a diol and a dibasic acid, including an aliphatic dibasic acid having 5 to 11 carbon atoms, and the aliphatic dibasic acid more preferably has 6 to 10 carbon atoms, which provides good adhesion to the substrate.

[0031] Examples of polyether polyols include polypropylene glycol, polyethylene glycol, polytetramethylene glycol, polytrimethylene glycol, and polyether polyols which are copolymers selected from these.

[0032] Examples of the polyisocyanate include various known aromatic diisocyanates, aliphatic diisocyanates, alicyclic diisocyanates, etc., which are generally used in the production of urethane resins. These may be trimers having an isocyanurate ring structure. Examples of aromatic diisocyanates include 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, and tolylene diisocyanate. Examples of the aliphatic diisocyanate include butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate. Examples of alicyclic diisocyanates include cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, norbornane diisocyanate, m-tetramethylxylylene diisocyanate, hydrogenated 4,4-diphenylmethane diisocyanate, and dimer diisocyanate in which the carboxyl group of a dimer acid is converted into an isocyanate group. Among them, at least one selected from tolylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, bis(isocyanatomethyl)cyclohexane, hexamethylene diisocyanate, and a trimer of hexamethylene diisocyanate is preferred. These polyisocyanates can be used alone or in combination of two or more.

[0033] When it is desired to introduce a carboxyl group into the urethane resin, it is possible to use dimethylolalkanoic acids such as dimethylolpropionic acid, dimethylolbutanoic acid, 2,2-dimethylolacetic acid, 2,2-dimethylolbutyric acid, 2,2-dimethylolpentanoic acid, dihydroxypropionic acid, etc., and polyhydroxy acids such as dihydroxysuccinic acid, dihydroxybenzoic acid, etc. In particular, it is preferable to use dimethylolpropionic acid, dimethylolbutanoic acid, and 2,2-dimethylolbutyric acid in terms of reactivity and solubility.

[0034] (Polyamine) In the present invention, it is also preferable that the urethane resin is chain-extended with a polyamine to have a urea bond derived from the polyamine. Examples of the polyamine include ethylenediamine, propylenediamine, hexamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, and further diamines such as dimer diamines in which the carboxyl groups of dimer acid are converted to amino groups, and ethylenediaminehexamethylenediamine and isophoronediamine are preferred. When the urethane resin contains a structural unit derived from a polyamine, the cohesive force of the resin increases, and therefore the adhesion of the ink to the substrate is improved.

[0035] Of the above urethane resin raw materials, the mass ratio of the total mass of polyol (hereinafter also referred to as soft segment) to the total mass of polyisocyanate and polyamine (hereinafter also referred to as hard segment) is preferably soft segment / hard segment=50 / 50 to 95 / 5, more preferably 60 / 40 to 90 / 10, and even more preferably 70 / 30 to 85 / 15. In the present invention, the soft segment is a soft and elastic part in the urethane resin structure. On the other hand, the hard segment is a hard and tough part in the urethane resin structure, and when the soft segment / hard segment mass ratio is within the above range, the ink has good adhesion to the substrate.

[0036] <Nitrified cotton resin> In the present invention, it is possible to use soluble nitrocellulose resin together with the urethane resin. By using soluble nitrocellulose resin, the heat resistance of the ink film after curing is improved. The mass ratio of the urethane resin to the soluble nitrocellulose resin is preferably 60 / 40 to 100 / 0, more preferably 70 / 30 to 100 / 0, and even more preferably 80 / 20 to 90 / 10. When the ratio of the urethane resin is 60% by mass or more, the adhesion to the substrate is improved.

[0037] <Pigments> The pigment used in the present invention is not particularly limited as long as it is a colorant used in gravure ink, but inorganic pigments are preferred. Examples of inorganic pigments include titanium oxide, iron hydroxide, iron oxide, zinc sulfide, and silica. White pigments are preferred as the pigment used in the present invention. The mass ratio (non-volatile content) of the pigment to the resin component is more preferably 60 / 40 to 95 / 5, and even more preferably 75 / 25 to 93 / 7.

[0038] <White pigment> The white pigment used in the present invention may contain an extender pigment, and examples thereof include titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, and silica. Among them, titanium oxide is preferred from the viewpoints of coloring power, hiding power, chemical resistance, and weather resistance. Moreover, titanium oxide that has been treated with silica and / or alumina is more preferred from the viewpoint of printing performance.

[0039] These pigments can be used alone or in combination of two or more kinds. The pigment is preferably contained in an amount of 0.05 to 60 mass %, more preferably 3 to 50 mass %, based on the total mass of the ink.

[0040] <Organic solvent> The gravure ink of the present invention may contain an organic solvent. The organic solvents used in the present invention include, but are not limited to, ester-based solvents, ketone-based solvents, alcohol-based solvents, glycol ether-based organic solvents, glycol monoalkyl ether-based organic solvents, and the like, which may be used alone or in combination of two or more kinds. Examples of the ester-based organic solvent include ethyl acetate, propyl acetate, n-butyl acetate, and isobutyl acetate. Examples of the ketone organic solvent include methyl ethyl ketone and methyl isobutyl ketone. Examples of the alcohol-based organic solvent include ethanol, 1-propanol, 2-propanol, 1-butanol, 2-methyl-1-propanol, 2-butanol, t-butanol, and 2-methyl-2-propanol. Examples of the glycol organic solvent include ethylene glycol, propylene glycol, butylene glycol and other alkylene glycols, dipropylene glycol, diethylene glycol and other dialkylene glycols, tripropylene glycol, triethylene glycol and other trialkylene glycols, and the like. Examples of the glycol monoalkyl ether organic solvent include propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, other propylene glycol monoalkyl ethers, dipropylene glycol monoethyl ether, dipropylene glycol monomethyl ether, other dipropylene monoalkyl ethers, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, other tripropylene glycol monoalkyl ethers, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, other diethylene glycol monoalkyl ethers, and propylene glycol monomethyl ether acetate.

[0041] <Isocyanate-based hardener> The gravure ink for decorative materials of the present invention preferably contains an isocyanate-based curing agent as a resin component. The mass ratio (non-volatile content) of the urethane resin to the isocyanate-based curing agent is preferably 100 / 0 to 30 / 70, more preferably 90 / 10 to 35 / 65, and even more preferably 80 / 20 to 45 / 55. By being in this range, the adhesion to the substrate and the hiding power are good, and furthermore, the usable time after the hardener is added is good.

[0042] As the isocyanate-based curing agent, it is preferable to use the polyisocyanates described above, and among them, isocyanurate-based polyisocyanates, adduct-based polyisocyanates, biuret-based polyisocyanates, allophanate-based polyisocyanates, etc. are preferably used. In the present invention, it is more preferable to use isocyanurate-based polyisocyanates and / or adduct-based polyisocyanates from the viewpoint of substrate adhesion, weather resistance, and wet heat resistance. The isocyanurate-based polyisocyanates refer to polyisocyanates having a structure in which diisocyanates are cyclized as trimers. The adduct-based polyisocyanates refer to polyisocyanates having a structure in which diisocyanates are added to the hydroxyl groups of compounds having hydroxyl groups, such as ethylene glycol, glycerin, and trimethylolpropane. The polyisocyanate reacts with reactive groups in the ink and / or the substrate to improve adhesion to the substrate layer, weather resistance, and moist heat resistance. Among them, it is preferable to use at least one selected from isocyanurate-based polyisocyanates of hexamethylene diisocyanate, isophorone diisocyanate, and adduct-based polyisocyanates consisting of adduct compounds of hexamethylene diisocyanate, isophorone diisocyanate, and xylylene diisocyanate and trimethylolpropane. As the isocyanate-based curing agent, the same compounds as the polyisocyanates are also preferably used. For example, trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, dodecamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, and the like. Socyanate (isophorone diisocyanate), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), 1,3-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane Aliphatic diisocyanates such as cyclohexane, 1,3-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, 2,4,6-triisocyanate toluene, 1,3,5-triisocyanate benzyl Examples of the aromatic diisocyanates include aromatic diisocyanates such as benzene, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, 4,4',4"-triphenylmethane triisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, ω,ω'-diisocyanate-1,4-diethylbenzene, 1,4-tetramethylxylylene diisocyanate, and 1,3-tetramethylxylylene diisocyanate.

[0043] <Additives> The gravure ink of the present invention may further contain additives. Examples of additives that may be used include dispersants, silane coupling agents, antiblocking agents, thickeners, rheology modifiers, defoamers, leveling agents, preservatives, surface tension modifiers, pH modifiers, waxes, etc. In particular, the combined use of dispersants and / or silane coupling agents is preferred.

[0044] <Dispersant> A dispersant can be used to improve the dispersibility of the pigment. As the dispersant, known dispersants such as anionic, nonionic, cationic, and amphoteric surfactants and high molecular weight compounds can be appropriately used. From the viewpoint of storage stability of the ink, the dispersant is preferably contained in the ink in an amount of 0.01 to 10% by mass relative to the total mass of the ink (100% by mass). More preferably, the dispersant is contained in the ink in an amount of 0.05 to 5% by mass. Even more preferably, the dispersant is contained in the ink in an amount of 0.1 to 3% by mass.

[0045] <Silane coupling agent> In the present invention, a silane coupling agent can be used. By using a silane coupling agent, not only the bonding strength between the resin and the pigment is increased, but also the bonding between the resin and the substrate is strengthened, improving the substrate adhesion. As the silane coupling agent, a known agent having various functional groups such as a vinyl group, an epoxy group, a styryl group, a methacryl group, an acrylic group, an amino group, or an isocyanurate group can be appropriately used. Among them, it is preferable to use a silane coupling agent having a methacryl group, an acrylic group, an amino group, or an isocyanurate group, and it is more preferable to use a silane coupling agent having an amino group. The content of the silane coupling agent is more preferably 10% by mass or less, and even more preferably 5% by mass or less, of the total mass of the gravure ink for decorative materials. By being in this range, not only the substrate adhesion but also the storage stability and the usable time when a curing agent is mixed are good.

[0046] <Gravure ink manufacturing method> The gravure ink of the present invention is produced by mixing predetermined amounts of binder resin, white pigment and solvent, and then dispersing (pigment dispersion) using a bead mill or the like. The gravure ink can be produced by blending the obtained dispersion with an antifoaming agent, solvent, etc. as necessary. As a dispersing machine used for the pigment dispersion, a commonly used machine such as a roller mill, ball mill, pebble mill, attritor, sand mill, etc. can be used. Dispersion using a sand mill, gamma mill, or other bead mill is preferred.

[0047] <Printed materials for cosmetic materials> The gravure ink for decorative materials of the present invention is gravure printed on a paper substrate to form a printed layer, which becomes a printed matter for decorative materials (hereinafter, also simply referred to as a printed matter). After printing with the gravure ink of the present invention, the printed matter can be obtained by sufficiently drying the printed matter to remove volatile components such as organic solvents. Examples of the configuration of the printed matter include, but are not limited to, the following configurations. (1)Paper base material / printing layer (2) Paper base material / printing layer / topcoat layer (3) Paper base material / printing layer / primer layer / topcoat layer (4) Paper base material / sealer layer / printing layer / topcoat layer

[0048] <Gravure printing> (gravure version) In gravure printing, the gravure plate is a cylindrical metal plate, and recesses are made in each color by engraving, etching, or laser. There are no restrictions on the use of engraving and laser, and they can be set arbitrarily according to the pattern. Lines per page are appropriately set at 75 to 250 lines, and the higher the line count, the finer the printing. The thickness of the printing layer is preferably 0.1 μm to 100 μm.

[0049] From the viewpoint of achieving the effects of the present invention, the viscosity of the gravure ink of the present invention is preferably 10 to 1000 mPa·s, more preferably 30 to 800 mPa·s, and even more preferably 50 to 600 mPa·s. When the viscosity is within this range, the storage stability is good. During gravure printing, the viscosity is preferably 10 to 300 mPa·s, more preferably 20 to 280 mPa·s, and even more preferably 30 to 250 mPa·s. When the viscosity is within this range, the printability is good. The viscosity is a value obtained by the method described in JIS Z8803:2011, and is preferably a value measured at 25°C using a B-type viscometer.

[0050] <Printing machine> In a gravure printing press, one printing unit is equipped with the gravure plate and doctor blade. There are many printing units, and printing units corresponding to organic solvent-based printing inks and picture inks can be set, and each unit has an oven drying unit. Printing is performed by rotary printing, and a roll-to-roll printing method is used. The type of plate and the type of doctor blade are selected appropriately according to the specifications.

[0051] <Decorative materials> The printed matter obtained by the above method is attached to a wood substrate such as particle board or MDF (medium density fiberboard) via an adhesive or the like depending on the application to become a decorative material. The configuration of the decorative material can be exemplified by, but is not limited to, the following configurations. (1) Particleboard / printed matter (2)MDF / Printed material (3)Resin plate / printed matter (4)Wood / printed matter

[0052] <Paper base material> Examples of the paper substrate that can be used include thin paper, reinforced paper, kraft paper, wood-free paper, linter paper, baryta paper, parchment paper, and Japanese paper. Reinforced paper is preferred because it has high inter-paper strength and good resistance to scratches, abrasion, and other factors. The basis weight of the paper substrate is 20 g / m 2 ~150g / m 2It is preferable that the thickness is 25 g / m 2 ~100g / m 2 It is preferable that the thickness is 30 g / m 2 ~80g / m 2 The thickness of the paper base material is preferably 20 to 200 μm, more preferably 25 to 100 μm, and even more preferably 30 to 60 μm. EXAMPLES

[0053] More specific embodiments of the present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the examples and comparative examples, "parts" and "%" respectively mean "parts by mass" and "% by mass" unless otherwise specified.

[0054] <Weight average molecular weight> The weight average molecular weight is a value calculated as polystyrene by GPC (gel permeation chromatography). The dried aqueous urethane resin (A) was dissolved in tetrahydrofuran to prepare a 0.5% solution, and the weight average molecular weight was measured using Shodex GPC-104 (column number LF-404, molecular weight measurement range: about 3 million to about 2 million).

[0055] <Amine value> The amine value is the amount of potassium hydroxide in mg equivalent to the amount of hydrochloric acid required to neutralize the amino groups contained in 1 g of sample, and was measured in accordance with JIS K 0070. That is, 0.5 to 2 g of sample was precisely weighed out (sample solid content: Sg). 50 mL of a mixed solution of methanol / methyl ethyl ketone = 60 / 40 (mass ratio) was added to the precisely weighed sample to dissolve it. Bromophenol blue was added to the obtained solution as an indicator, and the obtained solution was titrated with a 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changed from green to yellow was set as the end point, and the titration amount (AmL) at this time was used to calculate the amine value according to the following formula.

[0056] <Acid value> The acid value is the number of milligrams of potassium hydroxide required to neutralize the free fatty acids, resin acids, etc. contained in 1 g of a sample, and was measured by the method described in JIS K 0070.

[0057] [Synthesis Example 1] (Synthesis of urethane resin PU001) A four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube was charged with 16 parts of a polyester polyol having a number average molecular weight of 2,000 obtained by condensation polymerization of adipic acid and neopentyl glycol (hereinafter also referred to as NPG / AdA), 7 parts of a polypropylene glycol having a number average molecular weight of 1,000 (hereinafter also referred to as PPG1000), 5 parts of toluene diisocyanate (hereinafter also referred to as TDI), and 20 parts of ethyl acetate, and the mixture was reacted at 120°C for 6 hours under a nitrogen stream to obtain a solution of a terminal isocyanate prepolymer. Next, the obtained solution of terminal isocyanate prepolymer was gradually added at room temperature to 2.4 parts of isophorone diamine (hereinafter also abbreviated as IPDA), 0.03 parts of N-(2-aminoethyl)ethanolamine (hereinafter also abbreviated as AEA), 0.15 parts of 2-aminoethanol (hereinafter also abbreviated as MEA), and mixed solvent 1 (a mixture of 70 parts of ethyl acetate and 30 parts of isopropyl alcohol (hereinafter also abbreviated as IPA)), and then reacted at 50°C for 1 hour.The amine value was then adjusted with the diisocyanate used in the reaction, and the solid content was adjusted to 30% with ethyl acetate, thereby obtaining a urethane resin PU001 solution with a weight average molecular weight of 19,000, a urethane bond concentration of 1.0, a urea bond concentration of 0.8, and a soft segment / hard cement=75 / 25.

[0058] [Synthesis Examples 2 to 12] (Synthesis of urethane resins PU002 to PU012) Urethane resins PU002 to PU012 were obtained in the same manner as in Synthesis Example 1, except that the raw material compounds shown in Table 1 were used instead. The abbreviations in Table 1 are as follows. MPD / AdA: Polyester polyol, a condensation product of 3-methyl-1.5-pentanediol and adipic acid, number average molecular weight 5000 NPG / AdA: Polyester polyol, a condensation product of neopentyl glycol and adipic acid, number average molecular weight 2000 ·MPD / SeA: Polyester polyol, a condensation product of 3-methyl-1.5-pentanediol and sebacic acid, number average molecular weight 2000 PPG1000: Polypropylene glycol, number average molecular weight 1000 NPG: Neopentyl glycol DMBA: Dimethylolbutanoic acid 1,4BD: 1,4-butanediol 1,3BD: 1,3-butanediol IPDI: Isophorone diisocyanate ·TDI: Toluene diisocyanate IPDA: Isophoronediamine AEA: N-(2-aminoethyl)ethanolamine ·MEA: 2-aminoethanol DBA: Dibutylamine

[0059] [Example 1] (Production of Ink S1) 50 parts of titanium oxide (product name: DuPont Ti-Pure R960), 23 parts of urethane resin PU001 (Mw19000), 25 parts of mixed solvent 2 (ethyl acetate / isopropyl alcohol = 50 / 50), and 2 parts of dispersant (BASF BYK220S) as an additive were mixed and stirred, and then the pigment was dispersed and adjusted using a sand mill to obtain ink S1. Five parts of an isocyanate-based hardener (Toyo Ink UR100B Varnish 80) were added to 100 parts of this ink to prepare the ink for evaluation.

[0060] [Examples 2 to 21, Comparative Examples 1 to 6] (Production of Inks S2 to S21 and Inks R1 to R6) Inks S2 to S21 and Inks R1 to R6 were obtained in the same manner as in the production of Ink S1, except that the raw materials and blending ratios shown in Tables 2 and 3 were used. The abbreviations in the table are as follows. Nitrocellulose resin: Nitrocellulose resin (solid content 30%) obtained by heating and mixing 46 parts of industrial nitrocellulose TR 1 / 16 manufactured by Taiwan Glass Co., Ltd. and 54 parts of ethyl acetate. Acrylic resin: Acrylic resin AP1 (solid content 40%) described in Synthesis Example 1 of JP2021-80308A

[0061] [Breaking strength, breaking elongation] A mixture (the non-volatile components of the mixture correspond to the "resin components") was prepared by mixing the resins and isocyanate-based curing agents shown in Tables 2 and 3 in the mixing ratios shown in the tables, and a dried coating film with dimensions of 0.15 mm thickness, 5 mm width, and 30 mm length was obtained. Using this dried coating film, a stress / strain curve was obtained from the tensile distance and load obtained at a tensile speed of 50 mm / min and room temperature of 25°C using an Intesco tensile tester with reference to JIS K7127. The elongation at which the coating film broke was taken as the breaking elongation, and the stress at this time was taken as the breaking strength.

[0062] [Example 1] (Printing with ink S1) The gravure ink S1 was adjusted to 16 seconds (viscosity 200 mPa s) using a Zahn cup #3 and printed on a gravure printing machine equipped with a gravure plate (conventional plate depth 60 μm, 100 lines / inch) using reinforced paper "HPN-29UB" (Tenma Paper Co., Ltd., basis weight 30 g / m 2 A printed matter for decorative materials was obtained by printing on a substrate (40 μm thick) at a printing speed of 40 m / min and a drying temperature of 80° C.

[0063] [Examples 2 to 21, Comparative Examples 1 to 6] (Printing with Inks S2 to S21 and R1 to R6) Gravure printing was carried out in the same manner as for printing with ink S1, except that inks S2 to S21 and inks R1 to R6 were used instead of ink S1, to obtain printed matter.

[0064] <Performance evaluation> The following evaluations were carried out using the inks and printed matter obtained in the above Examples and Comparative Examples.

[0065] [Adhesion] The adhesion of the ink to the substrate was evaluated by the following method: A 12 mm wide cellophane tape manufactured by Nichiban Co., Ltd. was applied to the ink film of the printed matter, and the state of ink removal when peeled off was visually evaluated on a 5-point scale. 5: Only the tape comes off, or the cellophane tape is stuck to the surface. The entire surface is peeled off between the layers of paper. 4: Half to less than the entire surface of the cellophane tape is peeled off between the layers of paper 3: Part to less than half of the cellophane tape surface is peeled off between the paper layers 2: Peeling occurs between the ink layers (cohesive failure of the ink film) 1: Ink / paper peeling (poor ink adhesion to substrate) A rating of 3 to 5 is considered practical.

[0066] [VOCs] The ink to be evaluated was diluted with a mixed solvent of ethyl acetate / isopropyl alcohol = 50 / 50 parts by mass to a Zahn cup #3 viscosity of 16 seconds (corresponding to a viscosity of 200 mPa s), and the diluted ink solid content was evaluated on a 5-point scale (the higher the solid content of the diluted ink, the less VOC is emitted when it dries, which is preferable). That is, the diluted ink (approximately 1 g) was dried at 150°C for 30 minutes, and the mass after drying was calculated using the following formula (6). Formula (6) Diluted ink solids content (%) = (mass after drying / mass of diluted ink) x 100 5: 50% or more 4: 45% or more, less than 50% 3: 40% or more, less than 45% 2: 35% or more, less than 40% 1: Less than 35% A rating of 3 to 5 is practically preferable.

[0067] [Concealment] The opacity was evaluated by the following method. The transmission density (OD value) of the printed matter was measured using a Macbeth TD931 and rated on a 5-point scale. A higher value indicates higher opacity, and a lower value indicates lower opacity. 6:0.83 or better 5: 0.80 or more, less than 0.83 4: 0.75 or more, less than 0.80 3: 0.70 or more, less than 0.75 2: 0.65 or more, less than 0.70 Less than 1:0.65 A rating of 3 to 6 is considered practically usable.

[0068] [Table 1]

[0069] [Table 2]

[0070] [Table 3]

[0071] By adjusting the amount of hardener used according to the urethane bond concentration, urea bond concentration, and amine value of the urethane resin, the resin's breaking elongation and breaking strength could be adjusted. In contrast, Comparative Examples 1 and 2, in which the breaking elongation was outside the range of 100 to 400%, and Comparative Example 3, in which the breaking strength was less than 5 MPa, did not meet the standards in any of the evaluation items. Comparative Example 4 did not contain an inorganic pigment, so the hiding power did not meet the standards, and Comparative Examples 5 and 6 used a urethane resin without an amine value, so the breaking strength did not meet the standards, and as a result, the adhesion did not meet the standards. From the above results, it is possible to provide a gravure ink for decorative materials of the present invention that has good adhesion when printed on a paper substrate and has a lower environmental impact.

Claims

1. A gravure ink for a decorative material for forming a printed layer on a paper base material, the gravure ink comprising: The gravure ink contains a resin component including a urethane resin and an inorganic pigment, The urethane resin component has an amine value, the sum of the urethane bond concentration and the urea bond concentration of the urethane resin is 0.5 to 3 mmol / g; The resin component has a breaking elongation of 100 to 400%, and A gravure ink for decorative materials, wherein the resin component has a breaking strength of 5 MPa or more.

2. 2. The gravure ink for decorative materials according to claim 1, wherein the inorganic pigment is a white pigment.

3. 3. The gravure ink for decorative materials according to claim 1, wherein the weight average molecular weight of the urethane resin is 5,000 to 100,000.

4. 3. The gravure ink for decorative materials according to claim 1, wherein the resin component further contains a soluble nitrocellulose resin, and the mass ratio of the urethane resin to the soluble nitrocellulose resin is 60 / 40 to 90 / 10.

5. The gravure ink for decorative materials according to claim 1 or 2, wherein the resin component further contains an isocyanate-based curing agent, and the mass ratio of the urethane resin to the isocyanate-based curing agent is 100 / 0 to 30 / 70 (excluding the case where it is 100 / 0).

6. 3. The gravure ink for decorative materials according to claim 1, wherein the resin component has an acid value.

7. The gravure ink for decorative materials according to claim 1 or 2, further comprising a dispersant and / or a silane coupling agent.

8. 3. A printed matter for decorative materials, comprising a printed layer formed by printing the gravure ink for decorative materials according to claim 1 or 2 on a paper base material.

9. A method for producing a decorative material, comprising the steps of: A method for producing a decorative material, comprising a step of gravure printing the gravure ink for decorative materials according to claim 1 or 2 onto a paper substrate.

10. A decorative material including a printed layer on a paper substrate, The printing layer contains a resin component including a urethane resin and an inorganic pigment, The urethane resin component has an amine value, the sum of the urethane bond concentration and the urea bond concentration of the urethane resin is 0.5 to 3 mmol / g; The resin component has a breaking elongation of 100 to 400%, and A decorative material, wherein the resin component has a breaking strength of 5 MPa or more.

Citation Information

Patent Citations

  • Printing ink composition for decorative paper and use thereof

    JP1997255909A

  • Printing ink composition for decorating paper and decorating paper prepared by using the same and decorating material

    JP2001115076A

  • Decorative material

    JP2005178329A