Light-absorbing anisotropic layer, laminate, optical film, image display device, backlight module
A light-absorbing anisotropic layer with a dichroic substance oriented perpendicularly to the film surface addresses the challenge of achieving high front transmittance and low oblique transmittance in liquid crystal displays, improving energy efficiency and color neutrality.
Patent Information
- Application Number
- JP2021567239
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-30
- Filing Date
- 2020-12-11
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-12-11
AI Technical Summary
Existing technologies face challenges in achieving high transmittance in the front direction and low transmittance in oblique directions for liquid crystal display devices, particularly in energy-saving organic EL displays, without compromising color neutrality.
A light-absorbing anisotropic layer containing a dichroic substance oriented perpendicularly to the film surface with a degree of orientation of 0.95 or more at 550 nm, combined with a laminate structure that includes a polarizer layer, to achieve high front transmittance and low oblique transmittance.
The solution provides a light-absorbing anisotropic layer with high transmittance when viewed from the front and low transmittance from oblique directions, enhancing energy efficiency and color neutrality in image display devices.
Smart Images

Figure 0007553474000053 
Figure 0007553474000014 
Figure 0007553474000048
Abstract
Description
[Technical field]
[0001] The present invention relates to an optically absorptive anisotropic layer, a laminate, an optical film, an image display device, and a backlight module. [Background technology]
[0002] A technique is known in which an anisotropic light absorbing layer having an absorption axis in the thickness direction is used to prevent people from looking into a liquid crystal display device and to control the viewing angle. For example, Patent Documents 1 and 2 propose a polarizing element related to a viewing angle control system using a film containing a dichroic material and having an absorption axis with an angle of 0 to 45° between the normal line of the film surface. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-145776 A [Patent Document 2] International Publication No. 2018 / 079854 Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, issues such as energy conservation and the lifespan of organic electroluminescence (EL) displays have led to an increasing demand for films with high transmittance in the front direction relative to the membrane surface.
[0005] An object of the present invention is to provide an optically absorptive anisotropic layer which contains a dichroic material and has high transmittance when viewed from the front direction and low transmittance when viewed from an oblique direction. Another object of the present invention is to provide a laminate, an optical film, an image display device, and a backlight module. [Means for solving the problem]
[0006] The inventors discovered that by setting the degree of orientation at a wavelength of 550 nm of an optically absorptive anisotropic layer in which a dichroic material is oriented perpendicular to the film surface to 0.95 or more, it is possible to achieve high front transmittance and low oblique transmittance, and thus arrived at the present invention.
[0007] That is, it has been found that the above problems can be solved by the following configuration.
[0008] (1) A liquid crystal compound and at least one dichroic substance, A light absorbing anisotropic layer in which a dichroic substance is oriented perpendicular to a film surface, An optically absorptive anisotropic layer having a degree of orientation of 0.95 or more at a wavelength of 550 nm. (2) The optically absorptive anisotropic layer according to (1), wherein the optically absorptive anisotropic layer has a degree of orientation of 0.93 or more at a wavelength of 420 nm. (3) An optically absorptive anisotropic layer having a region A containing a liquid crystal compound and at least one dichroic substance, and a region B having a higher oblique transmittance as viewed from a polar angle of 30° than that of the region A, The dichroic material is oriented perpendicular to the film surface. An optically absorptive anisotropic layer, in which the degree of orientation in region A at a wavelength of 550 nm is 0.95 or more. (4) The optically absorptive anisotropic layer according to (3), wherein the region A has an oblique transmittance as viewed from a polar angle of 30° of 10% or less, and the region B has an oblique transmittance as viewed from a polar angle of 30° of 80% or more. (5) A laminate comprising the optically absorptive anisotropic layer according to any one of (1) to (4) and a polarizer layer in which a dichroic material is oriented horizontally to the film surface. (6) A laminate comprising the light absorptive anisotropic layer according to any one of (1) to (4) and a polarizer layer in which a liquid crystalline compound and a dichroic substance are oriented horizontally to the film surface. (7) An optical film having the optically absorptive anisotropic layer according to any one of (1) to (4) or the laminate according to (5) or (6). (8) An image display device comprising the optically absorptive anisotropic layer according to any one of (1) to (4), the laminate according to (5) or (6), or the optical film according to (7). (9) The image display device according to (8), wherein the display portion has a curved surface. (10) An image display device having the optically absorptive anisotropic layer according to (3) or (4) above, and capable of switching the viewing angle. (11) An image display device having the optically absorptive anisotropic layer according to (1) or (2) above, and capable of switching the viewing angle. (12) A liquid crystal display device having a first light guide plate, an optical filter element, and a second light guide plate from a viewing side, The optical filter element is the optically absorptive anisotropic layer according to (1) or (2). A backlight module that allows you to switch the viewing angle. Effect of the Invention
[0009] According to the present invention, it is possible to provide an optically absorptive anisotropic layer which contains a dichroic material and has high transmittance when viewed from the front direction and low transmittance when viewed from an oblique direction. Furthermore, according to the present invention, it is possible to provide a laminate, an optical film, an image display device, and a backlight module. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram of a backlight module according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, parallel and perpendicular do not mean parallel and perpendicular in the strict sense, but mean a range of ±5° from parallel or perpendicular. In this specification, the dichroic material is defined as being oriented perpendicularly when the transmittance is measured by changing the tilt angle (polar angle) and tilt direction (azimuth angle) relative to the normal direction of the optically absorptive anisotropic layer, and the direction with the highest transmittance is defined as the transmittance central axis, and the angle between the transmittance central axis and the film surface (main surface of the optically absorptive anisotropic layer) of the optically absorptive anisotropic layer is almost perpendicular. The perpendicular orientation between the transmittance central axis and the film surface means an orientation within a range of 70 to 90°, preferably an orientation within a range of 80 to 90°, and more preferably an orientation within a range of 85 to 90°.
[0012] In this specification, the liquid crystal composition and liquid crystal compound conceptually include those that no longer exhibit liquid crystallinity due to curing or the like.
[0013] In the present specification, each component may be used alone or in combination of two or more substances corresponding to the component. When two or more substances are used in combination for each component, the content of the component refers to the total content of the substances used in combination, unless otherwise specified. In addition, in this specification, "(meth)acrylate" is a notation representing "acrylate" or "methacrylate", "(meth)acryl" is a notation representing "acryl" or "methacryl", and "(meth)acryloyl" is a notation representing "acryloyl" or "methacryloyl".
[0014] <First embodiment of the optically absorptive anisotropic layer> A first embodiment of the optically absorptive anisotropic layer of the present invention is an optically absorptive anisotropic layer comprising a liquid crystal compound and at least one dichroic substance, in which the dichroic substance is oriented perpendicular to the film surface (the main surface of the optically absorptive anisotropic layer), and the degree of orientation of the optically absorptive anisotropic layer at a wavelength of 550 nm is 0.95 or more. The degree of orientation of the optically absorptive anisotropic layer at a wavelength of 550 nm is preferably 0.96 or more, since the optically absorptive anisotropic layer has a higher transmittance when viewed from the front and a lower transmittance when viewed from an oblique direction (hereinafter, simply referred to as "the effect of the present invention is superior"). The upper limit is not particularly limited, but may be 1.00.
[0015] The degree of orientation at a wavelength of 550 nm is calculated by the following method. The transmittance of the optically absorptive anisotropic layer at a wavelength of 550 nm is measured using AxoScan OPMF-1 (manufactured by Optoscience). During the measurement, the polar angle, which is the angle with respect to the normal direction of the optically absorptive anisotropic layer, is changed in increments of 5° from 0 to 60°, and the transmittance at a wavelength of 550 nm at all azimuth angles at each polar angle is measured. Next, after removing the influence of surface reflection, the transmittance at the azimuth angle and polar angle with the highest transmittance is defined as Tm(0), and the transmittance at an angle tilted by 40° from the polar angle with the highest transmittance in the azimuth angle direction with the highest transmittance is defined as Tm(40). The absorbance is calculated from the obtained Tm(0) and Tm(40) using the following formula, and A(0) and A(40) are calculated. A = -log(Tm) Here, Tm represents the transmittance and A represents the absorbance. From the calculated A(0) and A(40), the degree of orientation S defined by the following formula is calculated. S=(4.6×A(40)-A(0)) / (4.6×A(40)+2×A(0))
[0016] The first embodiment of the optically absorptive anisotropic layer of the present invention can achieve high transmittance in the front direction and low transmittance in oblique directions. This is presumably due to the following reasons. The transmittance in the oblique direction can be reduced by increasing the thickness of the optically absorptive anisotropic layer, but at the same time, the transmittance in the front direction decreases. It is believed that by increasing the degree of orientation of the optically absorptive anisotropic layer to 0.95 or more at a wavelength of 550 nm, the frequency of the dichroic material whose absorption axis is shifted from the vertical direction decreases. This suppresses absorption by the dichroic material when the optically absorptive anisotropic layer is viewed from the front direction, which is presumably why the transmittance in the front direction can be increased.
[0017] In addition, the degree of orientation of the light absorption anisotropic layer at a wavelength of 420 nm is preferably 0.93 or more in order to make the color in the front direction neutral. In particular, the degree of orientation at a wavelength of 420 nm is preferably 0.94 or more in order to make the color in the front direction more neutral. There is no particular upper limit, but it is preferably 1.00. The color of the light-absorption anisotropic layer containing a dichroic material is usually controlled by adjusting the amount of the dichroic material added to the light-absorption anisotropic layer. However, it has been found that it is not possible to make the color neutral in both the front and oblique directions by simply adjusting the amount of the dichroic material added. It has been found that the reason why the color cannot be made neutral in both the front and oblique directions is that the degree of orientation at a wavelength of 420 nm is low, and it is possible to make the color neutral in both the front and oblique directions by increasing the degree of orientation at a wavelength of 420 nm.
[0018] The method for calculating the degree of orientation at a wavelength of 420 nm may be a method in which the measurement wavelength in the above-mentioned method for calculating the degree of orientation at a wavelength of 550 nm is changed from 550 nm to 420 nm.
[0019] [Liquid crystal compound] The light absorptive anisotropic layer contains a liquid crystalline compound, which can align the dichroic material with a high degree of orientation while preventing precipitation of the dichroic material. The liquid crystal compound is a liquid crystal compound that does not exhibit dichroism. As the liquid crystal compound, either a low molecular weight liquid crystal compound or a polymeric liquid crystal compound can be used, and it is also preferable to use both in combination. Here, the term "low molecular weight liquid crystal compound" refers to a liquid crystal compound that does not have a repeating unit in its chemical structure. Also, the term "polymeric liquid crystal compound" refers to a liquid crystal compound that has a repeating unit in its chemical structure.
[0020] Examples of the low molecular weight liquid crystal compound include the liquid crystal compounds described in JP 2013-228706 A. As the low molecular weight liquid crystal compound, a liquid crystal compound exhibiting a smectic phase can also be preferably used.
[0021] Examples of the polymeric liquid crystal compound include the thermotropic liquid crystal polymer described in JP-A-2011-237513. In addition, from the viewpoint of excellent strength (particularly bending resistance) of the light absorption anisotropic film, the polymeric liquid crystal compound preferably has a repeating unit having a crosslinkable group at the end. Examples of the crosslinkable group include the polymerizable groups described in paragraphs
[0040] to
[0050] of JP-A-2010-244038. Among these, from the viewpoint of improving reactivity and synthesis suitability, an acryloyl group, a methacryloyl group, an epoxy group, an oxetanyl group, or a styryl group is preferred, and an acryloyl group or a methacryloyl group is more preferred.
[0022] In the case where the light absorption anisotropic layer in the present invention contains a polymeric liquid crystal compound, the polymeric liquid crystal compound preferably forms a nematic liquid crystal phase. The temperature range in which the liquid crystal exhibits a nematic liquid crystal phase is preferably from room temperature (23° C.) to 450° C., and from the viewpoints of handling and manufacturing suitability, preferably from 50 to 400° C.
[0023] The content of the liquid crystal compound is preferably 25 to 2000 parts by mass, more preferably 100 to 1300 parts by mass, and even more preferably 200 to 900 parts by mass, relative to 100 parts by mass of the dichroic substance in the light absorption anisotropic layer. When the content of the liquid crystal compound is within the above range, the degree of orientation of the light absorption anisotropic layer is further improved. The liquid crystal compound may be contained alone or in combination with two or more kinds. When two or more kinds of liquid crystal compounds are contained, the content of the liquid crystal compounds means the total content of the liquid crystal compounds.
[0024] From the viewpoint of achieving a better degree of alignment, the liquid crystal compound is preferably a polymeric liquid crystal compound containing a repeating unit represented by the following formula (1L) (hereinafter also referred to as "repeating unit (1L)").
[0025] [ka]
[0026] In the above formula (1L), P1 represents the main chain of the repeating unit, L1 represents a single bond or a divalent linking group, SP1 represents a spacer group, M1 represents a mesogenic group, and T1 represents a terminal group.
[0027] Specific examples of the main chain of the repeating unit represented by P1 include groups represented by the following formulae (P1-A) to (P1-D). Among these, the group represented by the following formula (P1-A) is preferred from the viewpoints of the variety of monomers that serve as raw materials and ease of handling.
[0028] [ka]
[0029] In formulae (P1-A) to (P1-D), "*" represents the bonding position with L1 in formula (1L). 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms. The alkyl group may be a straight-chain or branched alkyl group, or an alkyl group having a cyclic structure (cycloalkyl group). The alkyl group preferably has 1 to 5 carbon atoms. The group represented by formula (P1-A) is preferably one unit of a partial structure of a poly(meth)acrylic acid ester obtained by polymerization of a (meth)acrylic acid ester. The group represented by formula (P1-B) is preferably an ethylene glycol unit formed by ring-opening polymerization of the epoxy group of a compound having an epoxy group. The group represented by the formula (P1-C) is preferably a propylene glycol unit formed by ring-opening polymerization of the oxetane group of a compound having an oxetane group. The group represented by formula (P1-D) is preferably a siloxane unit of a polysiloxane obtained by condensation polymerization of a compound having at least one of an alkoxysilyl group and a silanol group. Here, the compound having at least one of an alkoxysilyl group and a silanol group is preferably a compound represented by the formula SiR 4 (OR 5 )2-, wherein R 4 is R in formula (P1-D) 4 Synonymous with R 5 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.
[0030] L1 is a single bond or a divalent linking group. The divalent linking group represented by L1 is -C(O)O-, -OC(O)-, -O-, -S-, or -C(O)NR 3 -, -NR 3 C(O)-, -SO2-, and -NR 3 R 4 In the formula, R 3 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms which may have a substituent W (described later). When P1 is a group represented by formula (P1-A), L1 is preferably a group represented by -C(O)O- from the viewpoint of achieving a better degree of orientation. When P1 is a group represented by any of the formulae (P1-B) to (P1-D), L1 is preferably a single bond from the viewpoint of achieving a better degree of orientation.
[0031] From the viewpoints of ease of expressing liquid crystallinity and availability of raw materials, it is preferable that the spacer group represented by SP1 contains at least one structure selected from the group consisting of an oxyethylene structure, an oxypropylene structure, a polysiloxane structure, and an alkylene fluoride structure. Here, the oxyethylene structure represented by SP1 is *-(CH2-CH2O) n1A group represented by -* is preferred. In the formula, n1 represents an integer of 1 to 20, and * represents the bonding position with L1 or M1 in the above formula (1L). From the viewpoint of achieving a better degree of orientation, n1 is preferably an integer of 2 to 10, more preferably an integer of 2 to 4, and even more preferably 3. In addition, the oxypropylene structure represented by SP1 is *-(CH(CH3)-CH2O) from the viewpoint of a better degree of orientation. n2 A group represented by -* is preferred, in which n2 represents an integer of 1 to 3, and * represents the bonding position to L1 or M1. In addition, the polysiloxane structure represented by SP1 is *-(Si(CH3)2-O) from the viewpoint of a better degree of orientation. n3 A group represented by -* is preferred, in which n3 represents an integer of 6 to 10, and * represents the bonding position to L1 or M1. In addition, the fluorinated alkylene structure represented by SP1 is preferably *-(CF2-CF2) from the viewpoint of a better degree of orientation. n4 A group represented by -* is preferred, in which n4 represents an integer of 6 to 10, and * represents the bonding position to L1 or M1.
[0032] The mesogenic group represented by M1 is a group that represents the main skeleton of the liquid crystal molecule that contributes to the formation of liquid crystal. The liquid crystal molecule exhibits liquid crystallinity, which is an intermediate state (mesophase) between the crystalline state and the isotropic liquid state. There are no particular limitations on the mesogenic group, and reference can be made, for example, to the description in "Flussige Kristalle in Tabellen II" (VEB Deutsche Verlag fur Grundstoff Industrie, Leipzig, published in 1984), particularly pages 7 to 16, and the description in "Liquid Crystal Handbook" edited by the Liquid Crystal Handbook Editorial Committee (Maruzen, published in 2000), particularly chapter 3. As the mesogenic group, for example, at least one group having a cyclic structure selected from the group consisting of an aromatic hydrocarbon group, a heterocyclic group, and an alicyclic group is preferable. From the viewpoint of achieving a better degree of orientation, the mesogenic group preferably has an aromatic hydrocarbon group, more preferably has 2 to 4 aromatic hydrocarbon groups, and even more preferably has 3 aromatic hydrocarbon groups.
[0033] As the mesogenic group, from the viewpoints of expression of liquid crystallinity, adjustment of the liquid crystal phase transition temperature, availability of raw materials and suitability for synthesis, as well as from the viewpoint of a more excellent degree of orientation, a group represented by the following formula (M1-A) or the following formula (M1-B) is preferable, and a group represented by formula (M1-B) is more preferable.
[0034] [ka]
[0035] In formula (M1-A), A1 is a divalent group selected from the group consisting of aromatic hydrocarbon groups, heterocyclic groups, and alicyclic groups. These groups may be substituted with an alkyl group, a fluorinated alkyl group, an alkoxy group, or a substituent W. The divalent group represented by A1 is preferably a 4- to 6-membered ring. In addition, the divalent group represented by A1 may be a monocyclic ring or a condensed ring. * indicates the binding position to SP1 or T1.
[0036] Examples of the divalent aromatic hydrocarbon group represented by A1 include a phenylene group, a naphthylene group, a fluorene-diyl group, an anthracene-diyl group, and a tetracene-diyl group. From the viewpoints of the diversity of mesogenic skeleton designs and the availability of raw materials, a phenylene group or a naphthylene group is preferred, and a phenylene group is more preferred.
[0037] The divalent heterocyclic group represented by A1 may be either aromatic or non-aromatic, but is preferably a divalent aromatic heterocyclic group from the viewpoint of further improving the degree of orientation. The atoms other than carbon constituting the divalent aromatic heterocyclic group include a nitrogen atom, a sulfur atom, and an oxygen atom. When the aromatic heterocyclic group has a plurality of atoms other than carbon constituting the ring, these atoms may be the same or different. Specific examples of divalent aromatic heterocyclic groups include, for example, a pyridylene group (pyridine-diyl group), a pyridazine-diyl group, an imidazole-diyl group, a thienylene (thiophene-diyl group), a quinolylene group (quinoline-diyl group), an isoquinolylene group (isoquinoline-diyl group), an oxazole-diyl group, a thiazole-diyl group, an oxadiazole-diyl group, a benzothiazole-diyl group, a benzothiadiazole-diyl group, a phthalimido-diyl group, a thienothiazole-diyl group, a thiazolothiazole-diyl group, a thienothiophene-diyl group, and a thienoxazole-diyl group.
[0038] Specific examples of the divalent alicyclic group represented by A1 include a cyclopentylene group and a cyclohexylene group.
[0039] In formula (M1-A), a1 represents an integer of 1 to 10. When a1 is 2 or more, multiple A1 may be the same or different.
[0040] In formula (M1-B), A2 and A3 are each independently a divalent group selected from the group consisting of an aromatic hydrocarbon group, a heterocyclic group, and an alicyclic group. Specific examples and preferred embodiments of A2 and A3 are the same as those of A1 in formula (M1-A), and therefore the description thereof is omitted. In formula (M1-B), a2 represents an integer of 1 to 10, and when a2 is 2 or more, multiple A2 may be the same or different, multiple A3 may be the same or different, and multiple LA1 may be the same or different. From the viewpoint of a better degree of orientation, a2 is preferably an integer of 2 or more, and more preferably 2. In formula (M1-B), when a2 is 1, LA1 is a divalent linking group. When a2 is 2 or more, each of the multiple LA1 is independently a single bond or a divalent linking group, and at least one of the multiple LA1 is a divalent linking group. When a2 is 2, from the viewpoint of a better degree of orientation, it is preferable that one of the two LA1 is a divalent linking group and the other is a single bond.
[0041] In formula (M1-B), the divalent linking group represented by LA1 is -O-, -(CH2) g -, -(CF2) g -, -Si(CH3)2-, -(Si(CH3)2O) g -, -(OSi(CH3)2) g -(g represents an integer from 1 to 10.), -N(Z)-, -C(Z)=C(Z')-, -C(Z)=N-, -N=C(Z)-, -C(Z)2- C(Z')2-, -C(O)-, -OC(O)-, -C(O)O-, -OC(O)O-, -N(Z)C(O)-, -C(O)N(Z)-, -C(Z)=C(Z')-C(O)O-, -OC(O)-C(Z)=C(Z')-, -C(Z)=N-, -N=C(Z)-, -C(Z)= C(Z')-C(O)N(Z")-, -N(Z")-C(O)-C(Z)=C(Z')-, -C(Z)=C(Z')-C(O)-S-, -S Examples of such groups include C(O)-C(Z)=C(Z')-, -C(Z)=NN=C(Z')- (Z, Z', and Z" each independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group, an aryl group, a cyano group, or a halogen atom), -C≡C-, -N=N-, -S-, -S(O)-, -S(O)(O)-, -(O)S(O)O-, -O(O)S(O)O-, -SC(O)-, and -C(O)S-. Of these, -C(O)O- is preferred from the viewpoint of achieving a higher degree of orientation. LA1 may be a group formed by combining two or more of these groups.
[0042] Specific examples of M1 include the following structures: In the following specific examples, "Ac" represents an acetyl group.
[0043] [ka]
[0044] [ka]
[0045] Examples of the terminal group represented by T1 include a hydrogen atom, a halogen atom, a cyano group, a nitro group, a hydroxy group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkoxycarbonyloxy group having 1 to 10 carbon atoms, an alkoxycarbonyl group having 1 to 10 carbon atoms (ROC(O)-: R is an alkyl group), an acyloxy group having 1 to 10 carbon atoms, an acylamino group having 1 to 10 carbon atoms, an alkoxycarbonylamino group having 1 to 10 carbon atoms, a sulfonylamino group having 1 to 10 carbon atoms, a sulfamoyl group having 1 to 10 carbon atoms, a carbamoyl group having 1 to 10 carbon atoms, a sulfinyl group having 1 to 10 carbon atoms, a ureido group having 1 to 10 carbon atoms, and a (meth)acryloyloxy group-containing group. Examples of the (meth)acryloyloxy group-containing group include a group represented by -LA (L represents a single bond or a linking group. Specific examples of the linking group are the same as those of L1 and SP1 described above. A represents a (meth)acryloyloxy group). From the viewpoint of achieving a better degree of orientation, T1 is preferably an alkoxy group having 1 to 10 carbon atoms, more preferably an alkoxy group having 1 to 5 carbon atoms, and further preferably a methoxy group. These terminal groups may be further substituted with these groups or the above-mentioned crosslinkable groups. The number of atoms in the main chain of T1 is preferably 1 to 20, more preferably 1 to 15, even more preferably 1 to 10, and particularly preferably 1 to 7, from the viewpoint of a better degree of orientation. When the number of atoms in the main chain of T1 is 20 or less, the degree of orientation of the light absorption anisotropic layer is further improved. Here, the "main chain" in T1 means the longest molecular chain bonded to M1, and hydrogen atoms are not counted in the number of atoms in the main chain of T1. For example, when T1 is an n-butyl group, the number of atoms in the main chain is 4, and when T1 is a sec-butyl group, the number of atoms in the main chain is 3.
[0046] From the viewpoint of achieving a better degree of orientation, the content of the repeating unit (1L) is preferably 20 to 100% by mass relative to 100% by mass of all repeating units contained in the polymeric liquid crystal compound. In the present invention, the content of each repeating unit contained in the polymeric liquid crystal compound is calculated based on the charged amount (mass) of each monomer used to obtain each repeating unit. The repeating unit (1L) may be contained in the polymeric liquid crystal compound either alone or in combination of two or more kinds. In particular, from the viewpoint of achieving a more excellent degree of orientation, it is preferred that the polymeric liquid crystal compound contains two kinds of repeating units (1L).
[0047] When the polymeric liquid crystal compound contains two types of repeating units (1L), from the viewpoint of achieving a better degree of orientation, it is preferable that the terminal group represented by T1 in one (repeating unit A) is an alkoxy group, and the terminal group represented by T1 in the other (repeating unit B) is a group other than an alkoxy group. In terms of achieving a better degree of orientation, the terminal group represented by T1 in the repeating unit B is preferably an alkoxycarbonyl group, a cyano group, or a group containing a (meth)acryloyloxy group, and more preferably an alkoxycarbonyl group or a cyano group. From the viewpoint of achieving a better degree of orientation, the ratio (A / B) of the content of the repeating unit A in the polymeric liquid crystal compound to the content of the repeating unit B in the polymeric liquid crystal compound is preferably 50 / 50 to 95 / 5, more preferably 60 / 40 to 93 / 7, and even more preferably 70 / 30 to 90 / 10.
[0048] The polymeric liquid crystal compound may have a repeating unit having no mesogenic group in addition to the repeating unit (1L). An example of the repeating unit having no mesogenic group is a repeating unit in which M1 in formula (1L) is a single bond. When the polymer liquid crystal compound has a repeating unit that does not have a mesogenic group, from the viewpoint of achieving a better degree of orientation, the amount of the repeating unit is preferably more than 0% by mass and not more than 30% by mass, and more preferably more than 10% by mass and not more than 20% by mass, relative to 100% by mass of all repeating units contained in the polymer liquid crystal compound.
[0049] From the viewpoint of achieving a better degree of orientation, the weight average molecular weight (Mw) of the polymer liquid crystal compound is preferably from 1,000 to 500,000, and more preferably from 2,000 to 300,000. When the Mw of the polymer liquid crystal compound is within the above range, the polymer liquid crystal compound is easy to handle. In particular, from the viewpoint of suppressing cracks during application, the weight average molecular weight (Mw) of the polymeric liquid crystal compound is preferably 10,000 or more, and more preferably 10,000 to 300,000. From the viewpoint of the temperature latitude of the orientation degree, the polymer liquid crystal compound preferably has a weight average molecular weight (Mw) of less than 10,000, and more preferably from 2,000 to less than 10,000. Here, the weight average molecular weight and number average molecular weight in the present invention are values measured by gel permeation chromatography (GPC). Solvent (eluent): N-methylpyrrolidone ·Device name: TOSOH HLC-8220GPC Column: Three TOSOH TSKgel SuperAWM-H (6 mm x 15 cm) columns connected together Column temperature: 25℃ Sample concentration: 0.1% by mass ·Flow rate: 0.35mL / min Calibration curve: TOSOH TSK standard polystyrene Calibration curve using 7 samples with Mw = 2,800,000 to 1,050 (Mw / Mn = 1.03 to 1.06)
[0050] The substituent W in this specification will be explained. Examples of the substituent W include an alkyl group (preferably an alkyl group having 1 to 20 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms, and further preferably an alkyl group having 1 to 8 carbon atoms, such as a methyl group, an ethyl group, an isopropyl group, a tert-butyl group, an n-octyl group, an n-decyl group, an n-hexadecyl group, a cyclopropyl group, a cyclopentyl group, and a cyclohexyl group), an alkenyl group (preferably an alkenyl group having 2 to 20 carbon atoms, more preferably an alkenyl group having 2 to 12 carbon atoms, and further preferably an alkenyl group having 2 to 8 carbon atoms). Examples of the alkyl group include a vinyl group, an aryl group, a 2-butenyl group, and a 3-pentenyl group, etc.), an alkynyl group (preferably an alkynyl group having 2 to 20 carbon atoms, more preferably an alkynyl group having 2 to 12 carbon atoms, and even more preferably an alkynyl group having 2 to 8 carbon atoms, and examples of the alkyl group include a propargyl group and a 3-pentynyl group, etc.), an aryl group (preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and even more preferably an aryl group having 6 to 12 carbon atoms, and examples of the alkyl group include a phenyl group, a 2,6-diethylphenyl group, a 3, 5-ditrifluoromethylphenyl group, styryl group, naphthyl group, biphenyl group, etc.), substituted or unsubstituted amino group (preferably an amino group having 0 to 20 carbon atoms, more preferably an amino group having 0 to 10 carbon atoms, and further preferably an amino group having 0 to 6 carbon atoms, for example, an unsubstituted amino group, a methylamino group, a dimethylamino group, a diethylamino group, an anilino group, etc.), alkoxy group (preferably an alkoxy group having 1 to 20 carbon atoms, more preferably an amino group having 1 to 15 carbon atoms, for example, a methoxy group, an ethoxy group, , and butoxy group.), oxycarbonyl group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 15 carbon atoms, and even more preferably having 2 to 10 carbon atoms; examples of such groups include a methoxycarbonyl group, an ethoxycarbonyl group, and a phenoxycarbonyl group.), acyloxy group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and even more preferably having 2 to 6 carbon atoms; examples of such groups include an acetoxy group, a benzoyloxy group, an acryloyl group, and a methacryloyl group.), acylamino group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and even more preferably having 2 to 6 carbon atoms; examples of which include an acetylamino group and a benzoylamino group), alkoxycarbonylamino group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and even more preferably having 2 to 6 carbon atoms; examples of which include a methoxycarbonylamino group), aryloxycarbonylamino group (preferably having 7 to 20 carbon atoms, more preferably having 7 to 16 carbon atoms, and even more preferably having and 7 to 12 carbon atoms, for example, a phenyloxycarbonylamino group.), a sulfonylamino group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and even more preferably having 1 to 6 carbon atoms, for example, a methanesulfonylamino group and a benzenesulfonylamino group.), a sulfamoyl group (preferably having 0 to 20 carbon atoms, more preferably having 0 to 10 carbon atoms, and even more preferably having 0 to 6 carbon atoms, for example, a sulfamoyl group, a methylsulfamoyl group, a dimethylsulfamoyl group, and a phenoxy group. ylsulfamoyl group, etc.), carbamoyl group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and even more preferably having 1 to 6 carbon atoms, for example, an unsubstituted carbamoyl group, a methylcarbamoyl group, a diethylcarbamoyl group, and a phenylcarbamoyl group, etc.), alkylthio group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and even more preferably having 1 to 6 carbon atoms, for example, a methylthio group, and an ethylthio group, etc.), arylthio group (preferably has 6 to 20 carbon atoms, more preferably 6 to 16 carbon atoms, and even more preferably 6 to 12 carbon atoms, and examples thereof include a phenylthio group.), a sulfonyl group (preferably has 1 to 20 carbon atoms, more preferably 1 to 10 carbon atoms, and even more preferably has 1 to 6 carbon atoms, and examples thereof include a mesyl group and a tosyl group.), a sulfinyl group (preferably has 1 to 20 carbon atoms, more preferably has 1 to 10 carbon atoms, and even more preferably has 1 to 6 carbon atoms, and examples thereof include a methanesulfinyl group and a benzenesulfinyl group.), a ureido group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and even more preferably having 1 to 6 carbon atoms; examples of which include an unsubstituted ureido group, a methylureido group, and a phenylureido group), a phosphoramido group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and even more preferably having 1 to 6 carbon atoms; examples of which include a diethylphosphoramido group and a phenylphosphoramido group), a hydroxy group, a mercapto group, a halogen atom (for example, a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom), a cyano group, a nitro group, a hydroxamic acid group, a sulfino group, a hydrazino group, an imino group, an azo group, a heterocyclic group (preferably and the like. Examples of the heterocyclic group include a heterocyclic group having a heteroatom such as a nitrogen atom, an oxygen atom, or a sulfur atom, and examples thereof include an epoxy group, an oxetanyl group, an imidazolyl group, a pyridyl group, a quinolyl group, a furyl group, a piperidyl group, a morpholino group, a maleimide group, a benzoxazolyl group, a benzimidazolyl group, and a benzthiazolyl group.), a silyl group (preferably a silyl group having a carbon number of 3 to 40, more preferably a carbon number of 3 to 30, and even more preferably a carbon number of 3 to 24, and examples thereof include a trimethylsilyl group and a triphenylsilyl group.), a carboxy group, a sulfonic acid group, and a phosphate group.
[0051] [Dichroic substance] The dichroic substance used in the present invention is not particularly limited, and examples thereof include visible light absorbing substances (dichroic dyes, dichroic azo compounds), luminescent substances (fluorescent substances, phosphorescent substances), ultraviolet absorbing substances, infrared absorbing substances, nonlinear optical substances, carbon nanotubes, and inorganic substances (e.g., quantum rods), and any conventionally known dichroic substance (dichroic dye) can be used.
[0052] A dichroic substance that is particularly preferably used is a dichroic azo dye compound. The dichroic azo dye compound is not particularly limited, and any conventionally known dichroic azo dye can be used, but the compounds described below are preferably used.
[0053] In the present invention, the dichroic azo dye compound means a dye whose absorbance varies depending on the direction. The dichroic azo dye compound may or may not exhibit liquid crystallinity. When the dichroic azo dye compound exhibits liquid crystallinity, it may exhibit either nematic or smectic properties. The temperature range in which the liquid crystal phase is exhibited is preferably room temperature (about 20° C. to 28° C.) to 300° C., and more preferably 50 to 200° C. from the viewpoints of handling and manufacturing suitability.
[0054] In the present invention, from the viewpoint of adjusting color, it is preferable that the light absorption anisotropic layer contains at least one dye compound having a maximum absorption wavelength in the wavelength range of 560 to 700 nm (hereinafter also referred to as "first dichroic azo dye compound") and at least one dye compound having a maximum absorption wavelength in the wavelength range of 455 nm or more and less than 560 nm (hereinafter also referred to as "second dichroic azo dye compound"). Specifically, it is more preferable that the light absorption anisotropic layer contains at least a dichroic azo dye compound represented by formula (1) described below and a dichroic azo dye compound represented by formula (2) described below.
[0055] In the present invention, three or more kinds of dichroic azo dye compounds may be used in combination. For example, from the viewpoint of making the light absorption anisotropic layer closer to black, it is preferable to use in combination a first dichroic azo dye compound, a second dichroic azo dye compound, and at least one dye compound having a maximum absorption wavelength in the wavelength range of 380 nm or more and less than 455 nm (hereinafter also referred to as a "third dichroic azo dye compound").
[0056] In the present invention, from the viewpoint of improving pressure resistance, it is preferable that the dichroic azo dye compound has a crosslinkable group. Specific examples of the crosslinkable group include a (meth)acryloyl group, an epoxy group, an oxetanyl group, and a styryl group, and among these, a (meth)acryloyl group is preferable.
[0057] (First dichroic azo dye compound) The first dichroic azo dye compound is preferably a compound having a chromophore core and a side chain bonded to an end of the chromophore. Specific examples of the chromophore include aromatic ring groups (e.g., aromatic hydrocarbon groups, aromatic heterocyclic groups) and azo groups. A structure having both an aromatic ring group and an azo group is preferred, and a bisazo structure having an aromatic heterocyclic group (preferably a thienothiazole group) and two azo groups is more preferred. The side chain is not particularly limited, and examples thereof include groups represented by R1, R2 and R3 in formula (1) described below.
[0058] The first dichroic azo dye compound is a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 560 nm or more and 700 nm or less. From the viewpoint of adjusting the color of the light absorption anisotropic layer, the first dichroic azo dye compound is preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 560 to 650 nm, and more preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 560 to 640 nm. The maximum absorption wavelength (nm) of the dichroic azo dye compound in this specification is determined from an ultraviolet-visible light spectrum in the wavelength range of 380 to 800 nm measured with a spectrophotometer using a solution in which the dichroic azo dye compound is dissolved in a good solvent.
[0059] In the present invention, from the viewpoint of further improving the degree of orientation of the light absorptive anisotropic layer to be formed, the first dichroic azo dye compound is preferably a compound represented by the following formula (1).
[0060] [ka]
[0061] In formula (1), Ar1 and Ar2 each independently represent a phenylene group which may have a substituent or a naphthylene group which may have a substituent, and a phenylene group is preferable.
[0062] In formula (1), R1 represents a hydrogen atom, a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxy group, an alkylthio group, an alkylsulfonyl group, an alkylcarbonyl group, an alkyloxycarbonyl group, an acyloxy group, an alkylcarbonate group, an alkylamino group, an acylamino group, an alkylcarbonylamino group, an alkoxycarbonylamino group, an alkylsulfonylamino group, an alkylsulfamoyl group, an alkylcarbamoyl group, an alkylsulfinyl group, an alkylureido group, an alkylphosphoric acid amide group, an alkylimino group, or an alkylsilyl group. The -CH2- constituting the alkyl group may be substituted by -O-, -CO-, -C(O)-O-, -OC(O)-, -Si(CH3)2-O-Si(CH3)2-, -N(R1')-, -N(R1')-CO-, -CO-N(R1')-, -N(R1')-C(O)-O-, -OC(O)-N(R1')-, -N(R1')-C(O)-N(R1')-, -CH=CH-, -C≡C-, -N=N-, -C(R1')=CH-C(O)- or -OC(O)-O-. When R1 is a group other than a hydrogen atom, the hydrogen atom of each group may be replaced by a halogen atom, a nitro group, a cyano group, -N(R1')2, an amino group, -C(R1')=C(R1')-NO2, -C(R1')=C(R1')-CN, or -C(R1')=C(CN)2. R1' represents a hydrogen atom or a linear or branched alkyl group having a carbon number of 1 to 6. When there are a plurality of R1' in each group, they may be the same or different.
[0063] In formula (1), R2 and R3 each independently represent a hydrogen atom, a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, an alkoxy group, an acyl group, an alkyloxycarbonyl group, an alkylamide group, an alkylsulfonyl group, an aryl group, an arylcarbonyl group, an arylsulfonyl group, an aryloxycarbonyl group, or an arylamide group. The -CH2- constituting the alkyl group may be substituted by -O-, -S-, -C(O)-, -C(O)-O-, -OC(O)-, -C(O)-S-, -SC(O)-, -Si(CH3)2-O-Si(CH3)2-, -NR2'-, -NR2'-CO-, -CO-NR2'-, -NR2'-C(O)-O-, -OC(O)-NR2'-, -NR2'-C(O)-NR2'-, -CH=CH-, -C≡C-, -N=N-, -C(R2')=CH-C(O)- or -OC(O)-O-. When R2 and R3 are groups other than hydrogen atoms, the hydrogen atoms of each group may be replaced by halogen atoms, nitro groups, cyano groups, -OH groups, -N(R2')2, amino groups, -C(R2')=C(R2')-NO2, -C(R2')=C(R2')-CN, or -C(R2')=C(CN)2. R2' represents a hydrogen atom or a linear or branched alkyl group having a carbon number of 1 to 6. When there are a plurality of R2' in each group, they may be the same or different. R2 and R3 may be bonded to each other to form a ring, or R2 or R3 may be bonded to Ar2 to form a ring.
[0064] From the viewpoint of light resistance, R1 is preferably an electron-withdrawing group, and R2 and R3 are preferably groups having low electron-donating properties. Specific examples of such groups include alkylsulfonyl groups, alkylcarbonyl groups, alkyloxycarbonyl groups, acyloxy groups, alkylsulfonylamino groups, alkylsulfamoyl groups, alkylsulfinyl groups, and alkylureido groups for R1, and groups of the following structure for R2 and R3, which are shown in the above formula (1) including the nitrogen atom to which R2 and R3 are bonded.
[0065] [ka]
[0066] Specific examples of the first dichroic azo dye compound are shown below, but the invention is not limited thereto.
[0067] [ka] JPEG0007553474000009.jpg161127 JPEG0007553474000010.jpg1295
[0068] (Second dichroic azo dye compound) The second dichroic azo dye compound is a compound different from the first dichroic azo dye compound, specifically, the chemical structure thereof is different. The second dichroic azo dye compound is preferably a compound having a chromophore which is the core of the dichroic azo dye compound, and a side chain bonded to an end of the chromophore. Specific examples of the chromophore include aromatic ring groups (e.g., aromatic hydrocarbon groups, aromatic heterocyclic groups) and azo groups. A structure having both an aromatic hydrocarbon group and an azo group is preferred, and a bisazo or trisazo structure having an aromatic hydrocarbon group and two or three azo groups is more preferred. The side chain is not particularly limited, and examples thereof include groups represented by R4, R5, or R6 in formula (2) described below.
[0069] The second dichroic azo dye compound is a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 455 nm or more and less than 560 nm. From the viewpoint of adjusting the color of the light absorption anisotropic layer, the second dichroic azo dye compound is preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 455 to 555 nm, and more preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 455 to 550 nm. In particular, by using a first dichroic azo dye compound having a maximum absorption wavelength in the range of 560 to 700 nm and a second dichroic azo dye compound having a maximum absorption wavelength in the range of 455 nm or more and less than 560 nm, it becomes easier to adjust the color of the light absorption anisotropic layer.
[0070] The second dichroic azo dye compound is preferably a compound represented by formula (2) in that the degree of orientation of the light absorptive anisotropic layer is further improved.
[0071] [ka]
[0072] In formula (2), n represents 1 or 2. In formula (2), Ar3, Ar4 and Ar5 each independently represent a phenylene group which may have a substituent, a naphthylene group which may have a substituent, or a heterocyclic group which may have a substituent. The heterocyclic group may be either aromatic or non-aromatic. Examples of the atoms other than carbon that constitute the aromatic heterocyclic group include a nitrogen atom, a sulfur atom, and an oxygen atom. When the aromatic heterocyclic group has a plurality of atoms that constitute the ring other than carbon, these atoms may be the same or different. Specific examples of aromatic heterocyclic groups include, for example, a pyridylene group (pyridine-diyl group), a pyridazine-diyl group, an imidazole-diyl group, a thienylene (thiophene-diyl group), a quinolylene group (quinoline-diyl group), an isoquinolylene group (isoquinoline-diyl group), an oxazole-diyl group, a thiazole-diyl group, an oxadiazole-diyl group, a benzothiazole-diyl group, a benzothiadiazole-diyl group, a phthalimido-diyl group, a thienothiazole-diyl group, a thiazolothiazole-diyl group, a thienothiophene-diyl group, and a thienoxazole-diyl group.
[0073] In formula (2), the definition of R4 is the same as that of R1 in formula (1). In formula (2), R5 and R6 are defined the same as R2 and R3 in formula (1), respectively.
[0074] From the viewpoint of light resistance, R4 is preferably an electron-withdrawing group, and R5 and R6 are preferably groups having low electron-donating properties. Among such groups, specific examples when R4 is an electron-withdrawing group are the same as the specific examples when R1 is an electron-withdrawing group, and specific examples when R5 and R6 are groups with low electron-donating property are the same as the specific examples when R2 and R3 are groups with low electron-donating property.
[0075] Specific examples of the second dichroic azo dye compound are shown below, but the invention is not limited thereto.
[0076] [ka]
[0077] [ka]
[0078] [ka]
[0079] [ka]
[0080] (difference in logP values) The logP value is an index expressing the hydrophilic and hydrophobic properties of a chemical structure. The absolute value of the difference between the logP value of the side chain of the first dichroic azo dye compound and the logP value of the side chain of the second dichroic azo dye compound (hereinafter also referred to as "logP difference") is preferably 2.30 or less, more preferably 2.0 or less, even more preferably 1.5 or less, and particularly preferably 1.0 or less. If the logP difference is 2.30 or less, the affinity between the first dichroic azo dye compound and the second dichroic azo dye compound is increased, making it easier to form an ordered structure, and therefore the degree of orientation of the light absorption anisotropic layer is further improved. When the first dichroic azo dye compound or the second dichroic azo dye compound has a plurality of side chains, it is preferable that at least one of the logP differences satisfies the above value. Here, the side chains of the first dichroic azo dye compound and the second dichroic azo dye compound refer to groups bonded to the ends of the above-mentioned chromophores. For example, when the first dichroic azo dye compound is a compound represented by formula (1), R1, R2, and R3 in formula (1) are side chains, and when the second dichroic azo dye compound is a compound represented by formula (2), R4, R5, and R6 in formula (2) are side chains. In particular, when the first dichroic azo dye compound is a compound represented by formula (1) and the second dichroic azo dye compound is a compound represented by formula (2), it is preferable that at least one of the logP differences between R1 and R4, the logP difference between R1 and R5, the logP difference between R2 and R4, and the logP difference between R2 and R5 satisfies the above value.
[0081] Here, the logP value is an index expressing the hydrophilic and hydrophobic properties of a chemical structure, and is sometimes called the hydrophilic-hydrophobic parameter. The logP value can be calculated using software such as ChemBioDraw Ultra or HSPiP (Ver. 4.1.07). It can also be experimentally determined by the method of OECD Guidelines for the Testing of Chemicals, Section 1, Test No. 117, etc. In the present invention, unless otherwise specified, the value calculated by inputting the structural formula of a compound into HSPiP (Ver. 4.1.07) is adopted as the logP value.
[0082] (Third dichroic azo dye compound) The third dichroic azo dye compound is a dichroic azo dye compound other than the first dichroic azo dye compound and the second dichroic azo dye compound, and specifically, has a chemical structure different from that of the first dichroic azo dye compound and the second dichroic azo dye compound. When the light absorption anisotropic layer contains the third dichroic azo dye compound, there is an advantage that the color of the light absorption anisotropic layer can be easily adjusted. The maximum absorption wavelength of the third dichroic azo dye compound is 380 nm or more and less than 455 nm, and preferably 385 to 454 nm.
[0083] The third dichroic azo dye compound is preferably a dichroic azo dye represented by the following formula (6).
[0084] [ka]
[0085] In formula (6), A and B each independently represent a crosslinkable group. In formula (6), a and b each independently represent 0 or 1. From the viewpoint of achieving an excellent degree of orientation at a wavelength of 420 nm, it is preferable that a and b are both 0. In formula (6), L1 represents a monovalent substituent when a = 0, and L1 represents a single bond or a divalent linking group when a = 1. Furthermore, L2 represents a monovalent substituent when b = 0, and L2 represents a single bond or a divalent linking group when b = 1. In formula (6), Ar1 represents an (n1+2)-valent aromatic hydrocarbon group or heterocyclic group, Ar2 represents an (n2+2)-valent aromatic hydrocarbon group or heterocyclic group, and Ar3 represents an (n3+2)-valent aromatic hydrocarbon group or heterocyclic group. In formula (6), R1, R2, and R3 each independently represent a monovalent substituent. When n1≧2, multiple R1s may be the same or different from each other, when n2≧2, multiple R2s may be the same or different from each other, and when n3≧2, multiple R3s may be the same or different from each other. In formula (6), k represents an integer of 1 to 4. When k≧2, multiple Ar2's may be the same or different, and multiple R2's may be the same or different. In formula (6), n1, n2, and n3 each independently represent an integer of 0 to 4, provided that when k=1, n1+n2+n3≧0, and when k≧2, n1+n2+n3≧1.
[0086] In formula (6), examples of the crosslinkable groups represented by A and B include the polymerizable groups described in paragraphs
[0040] to
[0050] of JP 2010-244038 A. Among these, from the viewpoint of improving reactivity and synthesis suitability, an acryloyl group, a methacryloyl group, an epoxy group, an oxetanyl group, or a styryl group is preferred, and from the viewpoint of further improving solubility, an acryloyl group or a methacryloyl group is more preferred.
[0087] In formula (6), L1 represents a monovalent substituent when a = 0, and L1 represents a single bond or a divalent linking group when a = 1. Furthermore, L2 represents a monovalent substituent when b = 0, and L2 represents a single bond or a divalent linking group when b = 1.
[0088] The monovalent substituents represented by L1 and L2 are preferably groups introduced to increase the solubility of the dichroic substance, or groups having electron-donating or electron-withdrawing properties introduced to adjust the color tone as a dye. For example, the substituents are an alkyl group (preferably an alkyl group having 1 to 20 carbon atoms, more preferably 1 to 12 carbon atoms, and further preferably 1 to 8 carbon atoms, such as a methyl group, an ethyl group, an isopropyl group, a tert-butyl group, an n-octyl group, an n-decyl group, an n-hexadecyl group, a cyclopropyl group, a cyclopentyl group, or a cyclohexyl group); alkenyl groups (preferably alkenyl groups having 2 to 20 carbon atoms, more preferably 2 to 12 carbon atoms, and even more preferably 2 to 8 carbon atoms, examples of which include a vinyl group, an allyl group, a 2-butenyl group, and a 3-pentenyl group); an alkynyl group (preferably an alkynyl group having 2 to 20 carbon atoms, more preferably 2 to 12 carbon atoms, and further preferably 2 to 8 carbon atoms, examples of which include a propargyl group and a 3-pentynyl group); an aryl group (preferably an aryl group having 6 to 30 carbon atoms, more preferably 6 to 20 carbon atoms, and even more preferably 6 to 12 carbon atoms, examples of which include a phenyl group, a 2,6-diethylphenyl group, a 3,5-ditrifluoromethylphenyl group, a naphthyl group, and a biphenyl group); a substituted or unsubstituted amino group (preferably an amino group having 0 to 20 carbon atoms, more preferably 0 to 10 carbon atoms, and further preferably 0 to 6 carbon atoms; examples of such an amino group include an unsubstituted amino group, a methylamino group, a dimethylamino group, a diethylamino group, and an anilino group); an alkoxy group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 15 carbon atoms, and examples thereof include a methoxy group, an ethoxy group, and a butoxy group); an oxycarbonyl group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 15 carbon atoms, and further preferably having 2 to 10 carbon atoms; examples of such a group include a methoxycarbonyl group, an ethoxycarbonyl group, and a phenoxycarbonyl group); acyloxy groups (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and even more preferably having 2 to 6 carbon atoms; examples of such groups include an acetoxy group and a benzoyloxy group); acylamino groups (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and further preferably having 2 to 6 carbon atoms; examples of such groups include an acetylamino group and a benzoylamino group), an alkoxycarbonylamino group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and further preferably having 2 to 6 carbon atoms; for example, a methoxycarbonylamino group is included); an aryloxycarbonylamino group (preferably having 7 to 20 carbon atoms, more preferably having 7 to 16 carbon atoms, and further preferably having 7 to 12 carbon atoms; for example, a phenyloxycarbonylamino group is mentioned); sulfonylamino groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and further preferably having 1 to 6 carbon atoms; examples thereof include a methanesulfonylamino group and a benzenesulfonylamino group), Sulfamoyl groups (preferably having 0 to 20 carbon atoms, more preferably having 0 to 10 carbon atoms, and further preferably having 0 to 6 carbon atoms; examples of such groups include a sulfamoyl group, a methylsulfamoyl group, a dimethylsulfamoyl group, and a phenylsulfamoyl group), a carbamoyl group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and still more preferably having 1 to 6 carbon atoms; examples of such a group include an unsubstituted carbamoyl group, a methylcarbamoyl group, a diethylcarbamoyl group, and a phenylcarbamoyl group); an alkylthio group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and further preferably having 1 to 6 carbon atoms; examples of such groups include a methylthio group and an ethylthio group); An arylthio group (preferably having 6 to 20 carbon atoms, more preferably having 6 to 16 carbon atoms, and further preferably having 6 to 12 carbon atoms; for example, there can be mentioned a phenylthio group), A sulfonyl group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and further preferably having 1 to 6 carbon atoms; examples of such a group include a mesyl group and a tosyl group), a sulfinyl group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and further preferably having 1 to 6 carbon atoms; examples of such a group include a methanesulfinyl group and a benzenesulfinyl group), a ureido group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and further preferably having 1 to 6 carbon atoms; examples of such a group include an unsubstituted ureido group, a methylureido group, and a phenylureido group), a phosphoric acid amide group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and further preferably having 1 to 6 carbon atoms; examples of such a group include a diethyl phosphoric acid amide group and a phenyl phosphoric acid amide group); heterocyclic group (preferably a heterocyclic group having 1 to 30 carbon atoms, more preferably 1 to 12 carbon atoms, for example, a heterocyclic group having a heteroatom such as a nitrogen atom, an oxygen atom, or a sulfur atom, and examples thereof include an imidazolyl group, a pyridyl group, a quinolyl group, a furyl group, a piperidyl group, a morpholino group, a benzoxazolyl group, a benzimidazolyl group, and a benzthiazolyl group), a silyl group (preferably a silyl group having 3 to 40 carbon atoms, more preferably 3 to 30 carbon atoms, and even more preferably 3 to 24 carbon atoms, examples of which include a trimethylsilyl group and a triphenylsilyl group); Halogen atoms (for example, fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, etc.), Hydroxy groups, mercapto groups, cyano groups, nitro groups, hydroxamic acid groups, sulfino groups, hydrazino groups, imino groups, and azo groups can be used. These substituents may be further substituted with other substituents. When there are two or more substituents, they may be the same or different. If possible, they may be bonded to each other to form a ring. Examples of the group in which the above-mentioned substituent is further substituted with the above-mentioned substituent include an alkoxy group substituted with an alkyl group, R B -(OR A ) na -group, where R A represents an alkylene group having 1 to 5 carbon atoms, R B represents an alkyl group having 1 to 5 carbon atoms, and na represents an integer of 1 to 10 (preferably 1 to 5, more preferably 1 to 3). Among these, examples of the monovalent substituent represented by L1 and L2 include an alkyl group, an alkenyl group, an alkoxy group, and a group in which these groups are further substituted with these groups (for example, the above-mentioned R B -(OR A ) na -group), and alkyl groups, alkoxy groups, and groups in which these groups are further substituted with these groups (for example, the above-mentioned R B -(OR A )na -group) is more preferred.
[0089] Examples of the divalent linking group represented by L1 and L2 include -O-, -S-, -CO-, -COO-, -OCO-, -O-CO-O-, and -CO-NR N -, -O-CO-NR N -, -NR N -CO-NR N Examples of such groups include -, -SO2-, -SO-, an alkylene group, a cycloalkylene group, and an alkenylene group, as well as groups formed by combining two or more of these groups. Among these, preferred are groups each comprising an alkylene group in combination with one or more groups selected from the group consisting of -O-, -COO-, -OCO- and -O-CO-O-. Here, R N represents a hydrogen atom or an alkyl group. N If there are multiple R N may be the same or different from each other.
[0090] From the viewpoint of further improving the solubility of the dichroic substance, the number of atoms in the main chain of at least one of L1 and L2 is preferably 3 or more, more preferably 5 or more, further preferably 7 or more, and particularly preferably 10 or more. The upper limit of the number of atoms in the main chain is preferably 20 or less, and more preferably 12 or less. On the other hand, from the viewpoint of further improving the degree of orientation of the optically absorptive anisotropic layer, the number of atoms in the main chain of at least one of L1 and L2 is preferably 1 to 5. Here, when A in formula (6) is present, the "main chain" in L1 refers to a portion necessary for directly connecting the "O" atom connected to L1 and "A", and the "number of atoms in the main chain" refers to the number of atoms constituting the above portion. Similarly, when B in formula (6) is present, the "main chain" in L2 refers to a portion necessary for directly connecting the "O" atom connected to L2 and "B", and the "number of atoms in the main chain" refers to the number of atoms constituting the above portion. Note that the "number of atoms in the main chain" does not include the number of atoms in the branched chain described below. In addition, when A is not present, the "number of atoms in the main chain" in L1 refers to the number of atoms in L1 that does not include branched chains. When B is not present, the "number of atoms in the main chain" in L2 refers to the number of atoms in L2 that does not include branched chains. Specifically, in the following formula (D1), the number of atoms in the main chain of L1 is 5 (the number of atoms in the dotted frame on the left side of the following formula (D1)), and the number of atoms in the main chain of L2 is 5 (the number of atoms in the dotted frame on the right side of the following formula (D1)). In addition, in the following formula (D10), the number of atoms in the main chain of L1 is 7 (the number of atoms in the dotted frame on the left side of the following formula (D10)), and the number of atoms in the main chain of L2 is 5 (the number of atoms in the dotted frame on the right side of the following formula (D10)).
[0091] [ka]
[0092] L1 and L2 may have a branched chain. Here, when A is present in formula (6), the "branched chain" in L1 refers to a portion other than the portion necessary for directly linking the "O" atom linked to L1 in formula (6) to "A". Similarly, when B is present in formula (6), the "branched chain" in L2 refers to a portion other than the portion necessary for directly linking the "O" atom linked to L2 in formula (6) to "B". In addition, when A is not present in formula (6), the "branched chain" in L1 refers to a portion other than the longest atomic chain (i.e., the main chain) extending from the "O" atom connecting to L1 in formula (6). Similarly, when B is not present in formula (6), the "branched chain" in L2 refers to a portion other than the longest atomic chain (i.e., the main chain) extending from the "O" atom connecting to L2 in formula (6). The number of atoms in the branched chain is preferably 3 or less. The number of atoms in the branched chain is preferably 3 or less, which has the advantage of further improving the degree of orientation of the light absorption anisotropic layer. Note that the number of atoms in the branched chain does not include the number of hydrogen atoms.
[0093] In formula (6), Ar1 represents an (n1+2)-valent (e.g., trivalent when n1 is 1), Ar2 represents an (n2+2)-valent (e.g., trivalent when n2 is 1), and Ar3 represents an (n3+2)-valent (e.g., trivalent when n3 is 1) aromatic hydrocarbon group or heterocyclic group. Here, Ar1 to Ar3 can be said to be divalent aromatic hydrocarbon groups or divalent heterocyclic groups substituted with n1 to n3 substituents (R1 to R3 described below), respectively. The divalent aromatic hydrocarbon group represented by Ar1 to Ar3 may be a single ring or may have a condensed ring structure of two or more rings. From the viewpoint of further improving the solubility, the number of rings in the divalent aromatic hydrocarbon group is preferably 1 to 4, more preferably 1 or 2, and even more preferably 1 (i.e., a phenylene group). Specific examples of the divalent aromatic hydrocarbon group include a phenylene group, an azulene-diyl group, a naphthylene group, a fluorene-diyl group, an anthracene-diyl group, and a tetracene-diyl group. From the viewpoint of further improving solubility, a phenylene group or a naphthylene group is preferable, and a phenylene group is more preferable. Specific examples of the third dichroic dye compound are shown below, but the present invention is not limited thereto. In the following specific examples, n represents an integer of 1 to 10.
[0094] [ka]
[0095] [ka]
[0096] In terms of achieving an excellent degree of alignment at 420 nm, it is preferable that the third dichroic azo dye compound does not have a radical polymerizable group. For example, the following structure can be mentioned.
[0097] [ka] JPEG0007553474000021.jpg12119
[0098] The third dichroic azo dye compound is more preferably a dichroic substance having a structure represented by the following formula (1-1), in that it has a particularly excellent degree of alignment at 420 nm.
[0099] [ka]
[0100] In formula (1-1), R1, R3, R4, R5, n1, n3, L1 and L2 are defined the same as R1, R3, R4, R5, n1, n3, L1 and L2 in formula (1), respectively. In formula (1-1), R 21 and R 22 Each of the above is independently defined as R2 in formula (1). In formula (1-1), n21 and n22 each independently have the same definition as n2 in formula (1). n1+n21+n22+n3≧1, and n1+n21+n22+n3 is preferably an integer of 1 to 9, and more preferably an integer of 1 to 5.
[0101] Specific examples of the dichroic material are shown below, but the present invention is not limited to these.
[0102] [ka]
[0103] [ka]
[0104] [ka]
[0105] The content of the dichroic substance is preferably 10 to 30% by mass, more preferably 15 to 30% by mass, further preferably 18 to 28% by mass, and particularly preferably 20 to 26% by mass, based on the total mass of the light absorption anisotropic layer. If the content of the dichroic substance is within the above range, a light absorption anisotropic layer with a high degree of orientation can be obtained even when the light absorption anisotropic layer is made into a thin film. Therefore, a light absorption anisotropic layer with excellent flexibility can be easily obtained. The content of the first dichroic azo dye compound is preferably from 40 to 90 parts by mass, and more preferably from 45 to 75 parts by mass, relative to 100 parts by mass of the total content of the dichroic substances in the light absorption anisotropic layer. The content of the second dichroic azo dye compound is preferably from 6 to 50 parts by mass, and more preferably from 8 to 35 parts by mass, based on 100 parts by mass of the total content of the dichroic substances in the light absorption anisotropic layer. The content of the third dichroic azo dye compound is preferably from 3 to 35 parts by mass, and more preferably from 5 to 35 parts by mass, based on 100 parts by mass of the dichroic azo dye compound in the light absorption anisotropic layer. The content ratio of the first dichroic azo dye compound, the second dichroic azo dye compound, and the third dichroic azo dye compound used as necessary can be set arbitrarily in order to adjust the color of the light absorption anisotropic layer. However, the content ratio of the second dichroic azo dye compound to the first dichroic azo dye compound (second dichroic azo dye compound / first dichroic azo dye compound) is preferably 0.1 to 10, more preferably 0.1 to 2, and even more preferably 0.1 to 0.5, in molar terms. If the content ratio of the second dichroic azo dye compound to the first dichroic azo dye compound is within the above range, the degree of orientation can be increased.
[0106] The optically absorptive anisotropic layer in the invention can be prepared, for example, by using a composition for forming an optically absorptive anisotropic layer, which contains the above-mentioned liquid crystal compound and a dichroic substance. The composition for forming the optically absorptive anisotropic layer may contain components other than the liquid crystal compound and the dichroic substance, such as a solvent, a vertical alignment agent, an interface improver, a polymerizable component, and a polymerization initiator (e.g., a radical polymerization initiator), etc. In this case, the optically absorptive anisotropic layer in the present invention contains a solid component other than the liquid component (solvent, etc.).
[0107] As the interface improver, the interface improvers described in the Examples section below can be used. When the composition for forming an optically absorptive anisotropic layer contains an interfacial improving agent, the content of the interfacial improving agent is preferably 0.001 to 5 parts by mass per 100 parts by mass of the total of the dichroic substance and the liquid crystal compound in the composition for forming an optically absorptive anisotropic layer.
[0108] The polymerizable component may be a compound containing an acrylate (for example, an acrylate monomer). In this case, the light absorption anisotropic layer in the present invention contains a polyacrylate obtained by polymerizing the compound containing the acrylate. Examples of the polymerizable component include the compounds described in paragraph
[0058] of JP2017-122776A. When the composition for forming an optically absorptive anisotropic layer contains a polymerizable component, the content of the polymerizable component is preferably 3 to 20 parts by mass per 100 parts by mass of the total of the dichroic substance and the liquid crystal compound in the composition for forming an optically absorptive anisotropic layer.
[0109] When a liquid crystal compound is used, for example, the technology of a guest-host type liquid crystal cell can be used to make the molecules of the dichroic material have the desired orientation as described above in association with the orientation of the host liquid crystal. Specifically, the light absorption anisotropic layer of the present invention can be produced by mixing a dichroic material as a guest with a liquid crystal compound as a host liquid crystal, orienting the host liquid crystal, orienting the molecules of the dichroic material along the orientation of the liquid crystal molecules, and fixing the orientation state.
[0110] In order to prevent the light absorption characteristics of the light absorption anisotropic layer of the present invention from varying depending on the use environment, it is preferable to fix the alignment of the dichroic material by forming a chemical bond. For example, the alignment can be fixed by promoting polymerization of the host liquid crystal, the dichroic material, or a polymerizable component added as required.
[0111] In addition, a guest-host type liquid crystal cell having a liquid crystal layer containing at least a dichroic material and a liquid crystal compound (host liquid crystal) between a pair of substrates may itself be used as the light absorption anisotropic layer in the present invention. The orientation of the host liquid crystal (and the accompanying orientation of the dichroic material) can be controlled by an orientation film formed on the inner surface of the substrate, and the orientation state is maintained unless an external stimulus such as an electric field is applied, making it possible to keep the light absorption characteristics of the light absorption anisotropic layer in the present invention constant.
[0112] [Vertical alignment agent] The vertical alignment agent includes a boronic acid compound and an onium salt.
[0113] The boronic acid compound is preferably a compound represented by formula (30).
[0114] Formula (30) [ka]
[0115] In formula (30), R 1 and R 2each independently represents a hydrogen atom, a substituted or unsubstituted aliphatic hydrocarbon group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heterocyclic group. R 3 represents a substituent containing a (meth)acrylic group. Specific examples of the boronic acid compound include boronic acid compounds represented by general formula (I) described in paragraphs
[0023] to
[0032] of JP-A-2008-225281. As the boronic acid compound, the compounds exemplified below are also preferred.
[0116] [ka]
[0117] The onium salt is preferably a compound represented by the formula (31).
[0118] Formula (31) [ka]
[0119] In formula (31), ring A represents a quaternary ammonium ion consisting of a nitrogen-containing heterocycle. - represents an anion. 1 represents a divalent linking group. 2 represents a single bond or a divalent linking group. 1 represents a divalent linking group having a 5- or 6-membered ring as a partial structure. Z represents a divalent linking group having 2 to 20 alkylene groups as a partial structure. P 1 and P 2 each independently represents a monovalent substituent having a polymerizable ethylenically unsaturated bond. Specific examples of the onium salt include the onium salts described in JP-A-2012-208397, paragraphs
[0052] to
[0058] , the onium salts described in JP-A-2008-026730, paragraphs
[0024] to
[0055] , and the onium salts described in JP-A-2002-037777.
[0120] The content of the vertical alignment agent in the optically absorptive anisotropic layer-forming composition (optically absorptive anisotropic layer) is preferably from 0.1 to 400% by mass, more preferably from 0.5 to 350% by mass, based on the total mass of the liquid crystal compound. The vertical alignment agent may be used alone or in combination of two or more kinds. When two or more kinds of vertical alignment agents are used, the total amount thereof is preferably within the above range.
[0121] [Leveling agent suitable for vertical alignment] The composition for forming an optically absorptive anisotropic layer (optically absorptive anisotropic layer) preferably contains the following leveling agent. When the composition for forming an optically absorptive anisotropic layer (optically absorptive anisotropic layer) contains a leveling agent, surface roughness caused by dry air on the surface of the optically absorptive anisotropic layer is suppressed, and the dichroic material is more uniformly oriented. The leveling agent is not particularly limited, and is preferably a leveling agent containing a fluorine atom (fluorine-based leveling agent) or a leveling agent containing a silicon atom (silicon-based leveling agent), and more preferably a fluorine-based leveling agent.
[0122] Examples of fluorine-based leveling agents include fatty acid esters of polyvalent carboxylic acids in which a part of the fatty acid is substituted with a fluoroalkyl group, and polyacrylates having a fluoro substituent. In particular, when rod-shaped compounds are used as the dichroic material and the liquid crystal compound, a leveling agent containing a repeating unit derived from the compound represented by formula (40) is preferred from the viewpoint of promoting the vertical alignment of the dichroic material and the liquid crystal compound.
[0123] Formula (40)
[0124] [ka]
[0125] R 0 represents a hydrogen atom, a halogen atom, or a methyl group. L represents a divalent linking group. L is preferably an alkylene group having 2 to 16 carbon atoms, and any non-adjacent -CH2- in the alkylene group may be substituted with -O-, -COO-, -CO-, or -CONH-. n represents an integer of 1 to 18.
[0126] The leveling agent having a repeating unit derived from the compound represented by formula (40) may further contain other repeating units. The other repeating units include a repeating unit derived from a compound represented by formula (41).
[0127] Formula (41)
[0128] [ka]
[0129] R 11 represents a hydrogen atom, a halogen atom, or a methyl group. X is an oxygen atom, a sulfur atom, or -N(R 13 )-. R 13 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. R 12 represents a hydrogen atom, an alkyl group which may have a substituent, or an aromatic group which may have a substituent. The number of carbon atoms in the alkyl group is preferably 1 to 20. The alkyl group may be linear, branched, or cyclic. Examples of the substituent that the alkyl group may have include a poly(alkyleneoxy) group and a polymerizable group. The polymerizable group is defined as above.
[0130] When the leveling agent contains a repeating unit derived from the compound represented by formula (40) and a repeating unit derived from the compound represented by formula (41), the content of the repeating unit derived from the compound represented by formula (40) is preferably 10 to 90 mol %, and more preferably 15 to 95 mol %, based on the total repeating units contained in the leveling agent. When the leveling agent contains a repeating unit derived from the compound represented by formula (40) and a repeating unit derived from the compound represented by formula (41), the content of the repeating unit derived from the compound represented by formula (41) is preferably 10 to 90 mol %, and more preferably 5 to 85 mol %, based on the total repeating units contained in the leveling agent.
[0131] Further, the leveling agent may also include a leveling agent containing a repeating unit derived from a compound represented by formula (42) instead of the repeating unit derived from the compound represented by formula (40) described above.
[0132] Formula (42)
[0133] [ka]
[0134] R 2 represents a hydrogen atom, a halogen atom, or a methyl group. L 2 represents a divalent linking group. n represents an integer of 1 to 18.
[0135] Specific examples of the leveling agent include the compounds exemplified in paragraphs
[0046] to
[0052] of JP-A-2004-331812 and the compounds described in paragraphs
[0038] to
[0052] of JP-A-2008-257205.
[0136] The content of the leveling agent in the composition for forming an optically absorptive anisotropic layer (optically absorptive anisotropic layer) is preferably from 0.001 to 10% by mass, and more preferably from 0.01 to 5% by mass, based on the total mass of the liquid crystal compound. The leveling agent may be used alone or in combination of two or more kinds. When two or more kinds of leveling agents are used, the total amount thereof is preferably within the above range.
[0137] [Polymerization initiator] The composition for forming the optically absorptive anisotropic layer preferably contains a polymerization initiator. The polymerization initiator is not particularly limited, but is preferably a compound having photosensitivity, that is, a photopolymerization initiator. As the photopolymerization initiator, various compounds can be used without any particular limitation. Examples of the photopolymerization initiator include α-carbonyl compounds (U.S. Pat. Nos. 2,367,661 and 2,367,670), acyloin ethers (U.S. Pat. No. 2,448,828), α-hydrocarbon-substituted aromatic acyloin compounds (U.S. Pat. No. 2,722,512), polynuclear quinone compounds (U.S. Pat. Nos. 3,046,127 and 2,951,758), combinations of triaryl imidazole dimers and p-aminophenyl ketones (U.S. Pat. No. 3,549,367), Examples of the compound include acridine and phenazine compounds (JP 60-105667 A and U.S. Pat. No. 4,239,850 A), oxadiazole compounds (U.S. Pat. No. 4,212,970 A), o-acyloxime compounds (JP 2016-027384 A, paragraph
[0065] ), and acylphosphine oxide compounds (JP 63-40799 A, JP 5-029234 B, JP 10-095788 A, and JP 10-029997 A). As such a photopolymerization initiator, commercially available products can be used, such as Irgacure-184, Irgacure-907, Irgacure-369, Irgacure-651, Irgacure-819, Irgacure-OXE-01, and Irgacure-OXE-02 manufactured by BASF.
[0138] When the composition for forming an optically absorptive anisotropic layer contains a polymerization initiator, the content of the polymerization initiator is preferably 0.01 to 30 parts by mass, more preferably 0.1 to 15 parts by mass, relative to 100 parts by mass of the total of the dichroic substance and the liquid crystal compound in the composition for forming an optically absorptive anisotropic layer. When the content of the polymerization initiator is 0.01 part by mass or more, the durability of the optically absorptive anisotropic film becomes good, and when it is 30 parts by mass or less, the degree of orientation of the optically absorptive anisotropic film becomes better. The polymerization initiator may be used alone or in combination of two or more. When two or more polymerization initiators are used, the total amount thereof is preferably within the above range.
[0139] [solvent] From the viewpoint of workability and the like, the composition for forming the optically absorptive anisotropic layer preferably contains a solvent. Examples of the solvent include ketones (e.g., acetone, 2-butanone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone), ethers (e.g., dioxane, tetrahydrofuran, 2-methyltetrahydrofuran, cyclopentyl methyl ether, tetrahydropyran, and dioxolane), aliphatic hydrocarbons (e.g., hexane), alicyclic hydrocarbons (e.g., cyclohexane), aromatic hydrocarbons (e.g., benzene, toluene, xylene, and trimethylbenzene), halogenated carbons (e.g., dichloromethane, trichloromethane, dichloroethane, dichlorobenzene, and chlorotoluene), esters (e.g., acetic acid, Examples of the organic solvent include organic solvents such as methyl, ethyl acetate, butyl acetate, and ethyl lactate, alcohols (e.g., ethanol, isopropanol, butanol, cyclohexanol, isopentyl alcohol, neopentyl alcohol, diacetone alcohol, and benzyl alcohol), cellosolves (e.g., methyl cellosolve, ethyl cellosolve, and 1,2-dimethoxyethane), cellosolve acetates, sulfoxides (e.g., dimethyl sulfoxide), amides (e.g., dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and N-ethylpyrrolidone), and heterocyclic compounds (e.g., pyridine), as well as water. These solvents may be used alone or in combination of two or more. Of these solvents, ketones (particularly cyclopentanone and cyclohexanone), ethers (particularly tetrahydrofuran, cyclopentyl methyl ether, tetrahydropyran and dioxolane), and amides (particularly dimethylformamide, dimethylacetamide, N-methylpyrrolidone and N-ethylpyrrolidone) are preferred. When the composition for forming an optically absorptive anisotropic layer contains a solvent, the content of the solvent is preferably 80 to 99 mass %, more preferably 83 to 98 mass %, and even more preferably 85 to 96 mass %, based on the total mass of the composition for forming an optically absorptive anisotropic layer. When two or more solvents are contained, the content of the solvents means the total content of the solvents.
[0140] <Method of forming optically absorptive anisotropic layer> The method for forming the optically absorptive anisotropic layer is not particularly limited, and examples thereof include a method including, in this order, a step of forming a coating film by applying the above-mentioned composition for forming an optically absorptive anisotropic layer (hereinafter also referred to as a "coating film forming step") and a step of orienting the liquid crystalline component contained in the coating film (hereinafter also referred to as an "orientation step"). The liquid crystal component is a component including not only the above-mentioned liquid crystal compound but also a dichroic substance having liquid crystallinity when the above-mentioned dichroic substance has liquid crystallinity. The optically absorptive anisotropic layer is preferably a layer obtained by using a composition for forming an optically absorptive anisotropic layer, and more preferably a layer (cured layer) obtained by subjecting a coating film obtained by using the composition for forming an optically absorptive anisotropic layer to a curing treatment.
[0141] [Coating film formation process] The coating film forming step is a step of forming a coating film by applying a composition for forming an optically absorptive anisotropic layer. By using a composition for forming an optically absorptive anisotropic layer that contains the above-mentioned solvent, or by using a composition for forming an optically absorptive anisotropic layer that has been made into a liquid such as a molten liquid by heating or the like, it becomes easy to apply the composition for forming an optically absorptive anisotropic layer. The contents of the various components contained in the composition for forming an optically absorptive anisotropic layer are preferably adjusted to the contents of the respective components in the optically absorptive anisotropic layer described above. Specific examples of the method for applying the composition for forming the optically absorptive anisotropic layer include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spraying, and inkjet methods.
[0142] [Orientation process] The alignment step is a step for aligning the liquid crystal component contained in the coating film, thereby obtaining a light absorptive anisotropic layer. The orientation step may include a drying treatment. By the drying treatment, components such as a solvent can be removed from the coating film. The drying treatment may be performed by leaving the coating film at room temperature for a predetermined time (for example, natural drying), or may be performed by heating and / or blowing air. Here, the liquid crystal component contained in the composition for forming an optically absorptive anisotropic layer may be aligned by the above-mentioned coating film forming process or drying treatment. For example, in an embodiment in which the composition for forming an optically absorptive anisotropic layer is prepared as a coating liquid containing a solvent, the coating film is dried to remove the solvent from the coating film, thereby obtaining a coating film having optical absorption anisotropy (i.e., an optically absorptive anisotropic film). When the drying treatment is carried out at a temperature equal to or higher than the transition temperature of the liquid crystal component contained in the coating film to a liquid crystal phase, the heating treatment described below does not need to be carried out.
[0143] The transition temperature of the liquid crystal component contained in the coating film to the liquid crystal phase is preferably 10 to 250°C, more preferably 25 to 190°C, from the viewpoint of manufacturability. If the transition temperature is 10°C or higher, cooling treatment or the like is not required to lower the temperature to the temperature range in which the liquid crystal phase is exhibited, which is preferable. In addition, if the transition temperature is 250°C or lower, a high temperature is not required even when the film is once in an isotropic liquid state at a temperature higher than the temperature range in which the liquid crystal phase is exhibited, which is preferable, as it is possible to reduce waste of thermal energy and deformation and deterioration of the substrate.
[0144] The alignment step preferably includes a heat treatment, which allows the liquid crystal component contained in the coating film to be aligned, so that the coating film after the heat treatment can be suitably used as an optically absorptive anisotropic film. From the viewpoint of manufacturability, the heat treatment temperature is preferably from 10 to 250° C., more preferably from 25 to 190° C. The heating time is preferably from 1 to 300 seconds, more preferably from 1 to 60 seconds.
[0145] The alignment step may include a cooling treatment carried out after the heating treatment. The cooling treatment is a treatment for cooling the coated film after heating to about room temperature (20 to 25°C). This makes it possible to fix the alignment of the liquid crystal component contained in the coated film. The cooling means is not particularly limited and can be carried out by a known method. By the above steps, an optically absorptive anisotropic film can be obtained. In this embodiment, the method for aligning the liquid crystal component contained in the coating film includes drying treatment and heating treatment, but is not limited thereto and can be carried out by any known alignment treatment.
[0146] [Other processes] The method for forming the optically absorptive anisotropic layer may include a step of curing the optically absorptive anisotropic layer (hereinafter also referred to as a "curing step") after the above-mentioned alignment step. The curing step is carried out by heating and / or light irradiation (exposure) when the light absorption anisotropic layer has a crosslinkable group (polymerizable group), for example. Among these, the curing step is preferably carried out by light irradiation. The light source used for curing can be various light sources such as infrared light, visible light, and ultraviolet light, but ultraviolet light is preferable. In addition, ultraviolet light may be irradiated while heating during curing, or ultraviolet light may be irradiated through a filter that transmits only specific wavelengths. When the exposure is performed with heating, the heating temperature during exposure is preferably 25 to 140° C., although it depends on the transition temperature to a liquid crystal phase of the liquid crystal component contained in the liquid crystal film. The exposure may be carried out under a nitrogen atmosphere. When the curing of the liquid crystal film proceeds by radical polymerization, it is preferable to carry out the exposure under a nitrogen atmosphere, since this reduces the inhibition of polymerization caused by oxygen.
[0147] The thickness of the optically absorptive anisotropic layer is not particularly limited, but from the viewpoint of flexibility when the laminate of the present invention described below is used in a polarizing element, it is preferably 100 to 8000 nm, and more preferably 300 to 5000 nm.
[0148] <Second embodiment of the optically absorptive anisotropic layer> A second embodiment of the optically absorptive anisotropic layer of the present invention is an optically absorptive anisotropic layer having a region A containing a liquid crystal compound and at least one dichroic substance, and a region B having a higher oblique transmittance when viewed from a polar angle of 30° than that of region A, in which the dichroic substance is oriented perpendicular to the film surface (the main surface of the optically absorptive anisotropic layer), and the degree of orientation of region A at a wavelength of 550 nm is 0.95 or more. The second embodiment of the optically absorptive anisotropic layer has two regions, Region A and Region B, in the in-plane direction. Region A has the same configuration as the first embodiment of the optically absorptive anisotropic layer described above. That is, Region A contains the above-mentioned liquid crystal compound and dichroic material. In Region A, the dichroic material is aligned perpendicular to the film surface, and Region A exhibits a predetermined degree of alignment. Region B has a higher oblique transmittance when viewed from a polar angle of 30° than region A. In other words, when comparing the oblique transmittance when viewed from a polar angle of 30° of region A with the oblique transmittance when viewed from a polar angle of 30° of region B, the oblique transmittance when viewed from a polar angle of 30° of region B is higher. The oblique transmittance refers to the transmittance at a wavelength of 550 nm. Region B may be empty, or may be a region containing a liquid crystal compound like region A. Region B may contain a dichroic substance, and as described above, the content of the dichroic substance is adjusted so that region A and region B satisfy a predetermined transmittance relationship. The content of the dichroic substance in region B is preferably 3 mass % or less, more preferably 1 mass % or less, and even more preferably 0 mass %, based on the total mass of region B.
[0149] The oblique transmittance of region A as viewed from a polar angle of 30° is preferably 10% or less, and the oblique transmittance of region B as viewed from a polar angle of 30° is preferably 80% or more.
[0150] In the second embodiment of the light absorption anisotropic layer, it is possible to strengthen or weaken the viewing angle dependency (of the polarized light) in a part of the region. This makes it possible to display highly confidential information only in the region where the viewing angle dependency is strengthened. In addition, by freely controlling the viewing angle dependency as a display device, it is possible to design an excellent design. In order to prevent light leakage from the light emitting part to the surrounding area in a display device such as a micro LED (light emitting diode), it is also possible to increase the contrast between light and dark in the screen by patterning the region other than the light emitting part as the above region B and the light emitting part as the above region A.
[0151] The positions of the regions A and B in the optically absorptive anisotropic layer are not particularly limited, and they may be appropriately arranged depending on the purpose of use. For example, the regions A and B may be arranged alternately in a stripe pattern, or a part of the optically absorptive anisotropic layer may be the region B, and the rest of the layer may be the region A.
[0152] The method for forming the second embodiment of the light absorbing anisotropic layer is not particularly limited, and various known methods such as those described in WO2019 / 176918 can be used. Examples include a method for controlling the thickness of the light absorbing anisotropic layer in-plane, a method for unevenly distributing a dichroic dye compound in the light absorbing anisotropic layer, and a method for post-processing an optically uniform light absorbing anisotropic layer. Methods for controlling the in-plane thickness of an optically absorptive anisotropic layer include a method using lithography, a method using imprinting, and a method of forming an optically absorptive anisotropic layer on a substrate having a concave-convex structure. As a method for unevenly distributing the dichroic dye compound in the light absorption anisotropic layer, there is a method of extracting the dichroic dye by immersion in a solvent (bleaching). Furthermore, as a method for post-processing an optically uniform light-absorptive anisotropic layer, there is a method in which a part of a flat light-absorptive anisotropic layer is cut by laser processing or the like.
[0153] <Laminate> The laminate of the present invention is a laminate in which the above-mentioned light absorbing anisotropic layer (first and second embodiments) and a polarizer layer in which a dichroic material is horizontally oriented are laminated together. This makes it possible to reduce the transmittance of oblique light, and by narrowing the viewing angle, it can be used for applications such as privacy films. The polarizer layer in which the dichroic material is horizontally aligned is not particularly limited. It may be a polarizer in which the dichroic material is dyed in polyvinyl alcohol or other polymer resin and stretched to horizontally align the material, or a polarizer in which the dichroic material is horizontally aligned by utilizing the orientation of a liquid crystal compound as in the light absorption anisotropic layer of the present invention. However, a polarizer in which the dichroic material is aligned by utilizing the orientation of liquid crystal without stretching is preferred. Polarizers in which a dichroic material is oriented by utilizing the orientation properties of liquid crystals have many advantages, including the ability to make them extremely thin, with thicknesses of approximately 0.1 to 5 μm; the fact that they are less likely to crack when bent and have little thermal deformation, as described in JP 2019-194685 A; and the fact that they have excellent durability even in polarizing plates with high transmittance of over 50%, as described in JP 6483486 A. Taking advantage of these advantages, it can be used in applications that require high brightness, small size and light weight, fine optical applications, molding into curved surfaces, and flexible applications.
[0154] [Barrier layer] The laminate of the present invention preferably has a barrier layer in addition to the optically absorptive anisotropic layer. Here, the barrier layer is also called a gas barrier layer (oxygen barrier layer), and has the function of protecting the light absorption anisotropic layer of the present invention from gases such as oxygen in the atmosphere, moisture, or compounds contained in adjacent layers. For the barrier layer, reference can be made to the descriptions in, for example, paragraphs
[0014] to
[0054] of JP 2014-159124 A, paragraphs
[0042] to
[0075] of JP 2017-121721 A, paragraphs
[0045] to
[0054] of JP 2017-115076 A, paragraphs
[0010] to
[0061] of JP 2012-213938 A, and paragraphs
[0021] to
[0031] of JP 2005-169994 A.
[0155] [Refractive index adjustment layer] The laminate of the present invention may have a problem of internal reflection due to the high refractive index of the light-absorptive anisotropic layer. In that case, it is preferable that a refractive index adjustment layer is present. The refractive index adjustment layer is a layer disposed so as to be in contact with the light-absorptive anisotropic layer, and has an in-plane average refractive index of 1.55 to 1.70 at a wavelength of 550 nm. It is preferable that the refractive index adjustment layer is used for so-called index matching.
[0156] <Optical film> The optical film of the present invention has the above-mentioned light absorptive anisotropic layer or the above-mentioned laminate. The optical film may have other members in addition to the light absorptive anisotropic layer and the laminate.
[0157] [Transparent substrate film] The optical film of the present invention may have a transparent substrate film. The transparent substrate film may be a known transparent resin film, a transparent resin plate, a transparent resin sheet, etc., and is not particularly limited. Examples of the transparent resin film include a cellulose acylate film (e.g., a cellulose triacetate film (refractive index 1.48), a cellulose diacetate film, a cellulose acetate butyrate film, and a cellulose acetate propionate film), a polyethylene terephthalate film, a polyethersulfone film, a cycloolefin-based film, a polyacrylic resin film, a polyurethane resin film, a polyester film, a polycarbonate film, a polysulfone film, a polyether film, a polymethylpentene film, a polyether ketone film, and a (meth)acrylonitrile film.
[0158] Among these, a cellulose acylate film, which has high transparency, low optical birefringence, and is easy to produce, and is generally used as a protective film for a polarizing plate, is preferred, and a cellulose triacetate film is more preferred. The transparent substrate film usually has a thickness of 20 to 100 μm. In the present invention, it is preferable that the transparent substrate film is a cellulose ester film and has a thickness of 20 to 70 μm. In addition, by using a polyacrylic film or a high-hardness film provided with a hard coat layer as the transparent substrate, the light absorption anisotropic layer of the present invention can be prevented from being damaged during the process of bonding it to other components (such as a linear polarizing plate) or during the process of incorporating it into an image display device. Furthermore, by using a film with low moisture permeability and low oxygen permeability, such as a polyethylene terephthalate film or a cycloolefin film, as the transparent substrate, the high temperature and humidity resistance and light resistance of the light absorption anisotropic layer can be improved.
[0159] [Alignment film] The optical film of the present invention may have an alignment layer between the transparent substrate film and the light absorptive anisotropic layer. The alignment film may be any layer as long as it can cause the dichroic material to be aligned in a desired state on the alignment film. For example, a film formed from a polyfunctional acrylate compound or polyvinyl alcohol may be used, with polyvinyl alcohol being particularly preferred.
[0160] The light absorptive anisotropic layer, laminate and optical film of the present invention can also be used in combination with an optically anisotropic film or an optical rotator in order to control the angle dependency of the viewing angle.
[0161] <Method of manufacturing optical film> An example of a method for producing the optical film of the present invention includes a method comprising, in this order, a step of applying the optically absorptive anisotropic layer-forming composition onto the transparent substrate film to form a coating film, a step of orienting a liquid crystalline component contained in the coating film to obtain the optically absorptive anisotropic layer, and a step of forming a protective layer adjacent to the optically absorptive anisotropic layer. Each step can be carried out according to a known method, and is not particularly limited. The liquid crystal component is a component including not only the above-mentioned liquid crystal compound but also a dichroic substance having liquid crystallinity when the above-mentioned dichroic substance has liquid crystallinity.
[0162] [Adhesive layer] The laminate and the optical film of the present invention may have an adhesive layer. The adhesive layer is preferably a transparent, optically isotropic adhesive similar to those used in ordinary liquid crystal displays, and a pressure-sensitive adhesive is usually used.
[0163] In addition to the base material (adhesive), conductive particles, and thermally expandable particles used as needed, the adhesive layer may contain appropriate additives such as crosslinkers (e.g., isocyanate-based crosslinkers, epoxy-based crosslinkers, etc.), tackifiers (e.g., rosin derivative resins, polyterpene resins, petroleum resins, oil-soluble phenolic resins, etc.), plasticizers, fillers, antioxidants, surfactants, UV absorbers, light stabilizers, and antioxidants.
[0164] The thickness of the adhesive layer is not particularly limited, and is preferably 20 to 500 μm, and more preferably 20 to 250 μm. When the thickness of the adhesive layer is 20 μm or more, the required adhesive strength and rework suitability are easily obtained, and when the thickness of the adhesive layer is 500 μm or less, the adhesive can be further prevented from protruding or seeping out from the peripheral edge of the image display device.
[0165] Methods for forming the adhesive layer include, for example, a method in which a coating liquid containing a base material, conductive particles, and, if necessary, heat-expandable particles, additives, and a solvent, is directly applied to the article to be coated and then pressure-bonded via a release liner, and a method in which the coating liquid is applied to a suitable release liner (such as release paper) to form a heat-expandable adhesive layer, which is then pressure-transferred (adhered) onto the article to be coated.
[0166] [Adhesive layer] The laminate and the optical film of the present invention may have an adhesive layer. The adhesive contained in the adhesive layer exhibits adhesiveness by drying or reaction after lamination. For example, a polyvinyl alcohol adhesive (PVA adhesive) develops adhesive properties when dried, making it possible to bond materials together. Specific examples of curable adhesives that develop adhesiveness through a reaction include active energy ray curable adhesives such as (meth)acrylate adhesives and cationic polymerization curable adhesives. Incidentally, (meth)acrylate means acrylate and / or methacrylate. Examples of the curable components in (meth)acrylate adhesives include compounds having a (meth)acryloyl group and compounds having a vinyl group. In addition, compounds having an epoxy group or an oxetanyl group can also be used as cationic polymerization curable adhesives. The compound having an epoxy group is not particularly limited as long as it has at least two epoxy groups in the molecule, and various commonly known curable epoxy compounds can be used. Examples of preferred epoxy compounds include compounds having at least two epoxy groups and at least one aromatic ring in the molecule (aromatic epoxy compounds), and compounds having at least two epoxy groups in the molecule, at least one of which is formed between two adjacent carbon atoms constituting an alicyclic ring (alicyclic epoxy compounds). Among these, from the viewpoint of resistance to thermal deformation, an ultraviolet-curing adhesive that is cured by irradiation with ultraviolet light is preferably used.
[0167] Each of the adhesive layer and the pressure-sensitive adhesive layer may be provided with ultraviolet absorbing ability by treating it with an ultraviolet absorber such as a salicylic acid ester compound, a benzophenol compound, a benzotriazole compound, a cyanoacrylate compound, or a nickel complex salt compound.
[0168] The adhesive layer or the bonding layer can be applied to the film by a suitable method. For example, a method of preparing an adhesive solution of about 10 to 40% by weight by dissolving or dispersing a base polymer or its composition in a solvent consisting of a single or mixture of suitable solvents such as toluene or ethyl acetate, and directly applying the solution to the film by a suitable spreading method such as a casting method or a coating method, or a method of forming an adhesive layer on a separator and transferring the adhesive layer, etc., can be mentioned.
[0169] The adhesive layer and the bonding layer can be provided on one or both sides of the film as a superposed layer of layers having different compositions or types, etc. When provided on both sides, the adhesive layers on the front and back of the film can have different compositions, types, thicknesses, etc.
[0170] In addition, before applying the adhesive or pressure-sensitive adhesive, the object on which the adhesive or pressure-sensitive adhesive is to be applied may be subjected to a surface modification treatment in order to improve adhesion, etc. Specific examples of such treatments include corona treatment, plasma treatment, primer treatment, and saponification treatment.
[0171] <Image display device> The image display device of the present invention has the above-mentioned light absorption anisotropic layer of the present invention, the above-mentioned laminate of the present invention, or the above-mentioned optical film of the present invention. The optical film of the present invention has a high front transmittance and a low oblique transmittance compared to conventionally known viewing angle control films using dichroic materials, and is therefore highly useful for realizing a narrow viewing angle. As a viewing angle control film, the light control film manufactured by 3M is also well known, but it has problems such as being thick and prone to moire due to a periodic structure, so by replacing it with the optical film of the present invention, it can contribute to improving the image quality, making it thinner, making it smaller, and improving the design of image display devices. The display element used in the image display device of the present invention is not particularly limited, and examples thereof include a liquid crystal cell, an organic electroluminescence (hereinafter abbreviated as "EL") display panel, and a plasma display panel. Among these, a liquid crystal cell or an organic EL display panel is preferred, and a liquid crystal cell is more preferred. That is, the image display device of the present invention is preferably a liquid crystal display device using a liquid crystal cell as a display element, or an organic EL display device using an organic EL display panel as a display element, and more preferably a liquid crystal display device.
[0172] [Liquid crystal display device] A preferred embodiment of the liquid crystal display device, which is one example of the image display device of the present invention, is one having the above-mentioned light absorption anisotropic layer of the present invention and a liquid crystal cell. More preferred is a liquid crystal display device having the above-mentioned laminate of the present invention (not including a λ / 4 plate) and a liquid crystal cell. In the present invention, of the polarizing elements provided on both sides of the liquid crystal cell, it is preferable to use the laminate of the present invention as the front side polarizing element, and it is more preferable to use the laminate of the present invention as both the front side and the rear side polarizing elements. The liquid crystal cell constituting the liquid crystal display device will be described in detail below.
[0173] (Liquid crystal cell) The liquid crystal cell used in the liquid crystal display device is preferably in VA (Vertical Alignment) mode, OCB (Optically Compensated Bend) mode, IPS (In-Plane-Switching) mode, or TN (Twisted Nematic) mode, but is not limited to these. In a TN mode liquid crystal cell, rod-shaped liquid crystal molecules are aligned substantially horizontally when no voltage is applied, and further aligned in a twisted manner at an angle of 60 to 120°. TN mode liquid crystal cells are most commonly used as color TFT (Thin Film Transistor) liquid crystal display devices, and are described in many publications. In a VA mode liquid crystal cell, rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied. VA mode liquid crystal cells include (1) a narrow-sense VA mode liquid crystal cell (described in JP-A-2-176625) in which rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied and substantially horizontally when voltage is applied, (2) a VA mode multi-domain (MVA mode) liquid crystal cell (described in SID97, Digest of tech. Papers (Proceedings) 28 (1997) 845) in order to expand the viewing angle, (3) a mode (n-ASM mode) liquid crystal cell in which rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied and are aligned in a twisted multi-domain when voltage is applied (described in Proceedings of the Japan Liquid Crystal Discussion Society 58-59 (1998)), and (4) a SURVIVAL mode liquid crystal cell (announced at LCD International 98). The liquid crystal display may be of any of a PVA (Patterned Vertical Alignment) type, an optical alignment type, and a PSA (Polymer-Sustained Alignment) type. Details of these modes are described in Japanese Patent Application Laid-Open No. 2006-215326 and Japanese Patent Application Laid-Open No. 2008-538819. In the IPS mode liquid crystal cell, rod-shaped liquid crystal molecules are aligned substantially parallel to the substrate, and the liquid crystal molecules respond in a planar manner when an electric field parallel to the substrate surface is applied. In the IPS mode, the black display is achieved when no electric field is applied, and the absorption axes of the pair of upper and lower polarizing plates are perpendicular to each other. Methods of reducing light leakage during black display in an oblique direction and improving the viewing angle using an optical compensation sheet are disclosed in JP-A-10-54982, JP-A-11-202323, JP-A-9-292522, JP-A-11-133408, JP-A-11-305217, and JP-A-10-307291.
[0174] [Organic EL display device] A preferred embodiment of an organic EL display device, which is one example of the image display device of the present invention, has, from the viewing side, the above-mentioned light absorption anisotropic layer of the present invention, a horizontally aligned polarizer, a λ / 4 plate, and an organic EL display panel, in this order. The organic EL display panel is a display panel configured using an organic EL element having an organic light-emitting layer (organic electroluminescence layer) sandwiched between electrodes (cathode and anode). The configuration of the organic EL display panel is not particularly limited, and a known configuration may be adopted.
[0175] [Curved image display device] Examples of the curved image display device of the present invention are disclosed in JP-A-2017-181821, JP-A-2017-181819, JP-A-2017-102456, JP-A-2014-095901, and the like. A curved image display device has a curved surface in a display portion. Since the optically absorptive anisotropic layer of the present invention has low rigidity, it can be deformed to fit the curved surface of the display portion. In other words, the optically absorptive anisotropic layer of the present invention can be deformed to have a curved surface itself. In addition, since the laminate and optical film of the present invention also have low rigidity, the shape can be deformed to fit the curved surface of the display part. In other words, the laminate and optical film of the present invention can be deformed to have a curved surface itself.
[0176] [Image display device capable of switching viewing angles (Image display device capable of switching viewing angles)] The light emitting angle can be narrowed by using the light absorbing anisotropic layer, laminate, and optical film of the present invention. Various types of image display devices capable of switching the viewing angle are known, and the light absorbing anisotropic layer, laminate, and optical film of the present invention can be used to generate light with a narrow emission angle. For example, after generating light with a narrow exit angle using the optically absorptive anisotropic layer, laminate, and optical film of the present invention, the light can be passed through an element that controls whether or not the light is diffused, as described in JP-A-9-105907, thereby switching between a narrow viewing angle and a wide viewing angle. Alternatively, as described in JP 2017-098246 A, in a narrow viewing angle / wide viewing angle switching backlight system consisting of, from the viewing side, an inverted prism sheet, a first light guide plate that makes light incident on the inverted prism sheet at a relatively large angle of incidence (light emerging from the inverted prism sheet has a narrow viewing angle), an optical filter element that absorbs light incident from an oblique angle and makes light with a narrow exit angle incident on the inverted prism sheet at a relatively small angle of incidence, and a second light guide plate (light emerging from the inverted prism sheet has a narrow viewing angle), the optical filter element can be the light absorptive anisotropic layer, laminate, or optical film of the present invention. In addition, a retardation modulation element such as a liquid crystal cell can be disposed between the light absorption anisotropic layer of the present invention and the horizontally aligned polarizer to switch between a narrow viewing angle and a light viewing angle. For example, when a VA mode or ECB mode liquid crystal cell is used as the retardation modulation cell, the viewing angle becomes narrow when the liquid crystal in the liquid crystal cell is vertically aligned, and becomes wide viewing angle mode when the liquid crystal in the liquid crystal cell is tilted aligned, and the narrow viewing angle / wide viewing angle can be controlled by applying or not applying a voltage to the cell. It is also possible to use an IPS mode liquid crystal cell as a phase difference modulation cell. The alignment direction of the liquid crystal cell when no voltage is applied and the absorption axis direction of the horizontally aligned polarizer are set to be parallel or perpendicular, and the viewing angle can be switched from a narrow viewing angle to a wide viewing angle by changing the alignment direction of the liquid crystal cell by applying a voltage. Furthermore, as in Example 7 described later, by patterning the regions A and B described in claims 3 and 4 of the present invention for each light-emitting pixel and controlling the lighting of each light-emitting pixel, it is possible to switch between a narrow viewing angle and a wide viewing angle. EXAMPLES
[0177] The present invention will be specifically described below based on examples. The materials, reagents, amounts and ratios of substances, and operations shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the present invention is not limited to the following examples.
[0178] <Example 1> An optically absorbing anisotropic layer in which the dye was oriented in the vertical direction was prepared as follows.
[0179] [Preparation of transparent support 1] The surface of cellulose acylate film 1 (TAC substrate having a thickness of 40 μm; TG40, Fujifilm Corporation) was saponified with an alkaline solution, and the coating solution for forming an alignment layer 1 was applied thereon with a wire bar. The support on which the coating film was formed was dried with hot air at 60° C. for 60 seconds and then with hot air at 100° C. for 120 seconds to form an alignment layer, thereby obtaining a TAC film with an alignment layer. The thickness of the alignment layer was 1 μm.
[0180] ------------------------------------------------------------------ (Alignment layer forming coating solution 1) ------------------------------------------------------------------ 3.80 parts by weight of the following modified polyvinyl alcohol Initiator Irg2959 0.20 parts by weight ·Water 70 parts by mass Methanol 30 parts by weight ----------------------------------------------------------------------------------
[0181] Modified Polyvinyl Alcohol [ka]
[0182] [Formation of Optically Absorbing Anisotropic Layer P1] On the obtained alignment layer PA1, the following composition for forming an optically absorptive anisotropic layer P1 was continuously applied with a wire bar to form a coating layer P1. Next, the coating layer P1 was heated at 140° C. for 30 seconds, and then cooled to room temperature (23° C.). Next, the coating layer P1 was heated at 80° C. for 60 seconds and then cooled again to room temperature. Thereafter, the coating layer P1 was irradiated with an LED lamp (center wavelength 365 nm) at an illuminance of 200 mW / cm 2An optically absorptive anisotropic layer P1 was formed on the alignment layer 1 by irradiating the layer with light under the irradiation conditions for 2 seconds. The coating layer P1 had a thickness of 3 μm, and the degree of orientation of the optically absorptive anisotropic layer P1 at a wavelength of 550 nm was 0.96. This was designated as Light Absorption Anisotropic Film 1.
[0183] ------------------------------------------------------------------ Composition of optically absorptive anisotropic layer forming composition P1 ------------------------------------------------------------------ 0.40 parts by weight of the following dichroic substance D-1 0.15 parts by weight of the following dichroic substance D-2 0.63 parts by weight of the following dichroic substance D-3 3.65 parts by weight of the following polymer liquid crystal compound P-1 Polymerization initiator IRGACUREOXE-02 (BASF) 0.040 parts by mass 0.060 parts by weight of the following compound E-1 0.060 parts by weight of the following compound E-2 0.010 parts by weight of the following surfactant F-1 0.015 parts by weight of the following surfactant F-2 Cyclopentanone 47.00 parts by mass Tetrahydrofuran 47.00 parts by mass Benzyl alcohol 1.00 parts by weight ------------------------------------------------------------------
[0184] Dichroic substance D-1
[0185] [ka]
[0186] Dichroic substance D-2
[0187] [ka]
[0188] Dichroic substance D-3
[0189] [ka]
[0190] Polymer liquid crystal compound P-1
[0191] [ka]
[0192] Compound E-1
[0193] [ka]
[0194] Compound E-2
[0195] [ka]
[0196] Surfactant F-1
[0197] [ka]
[0198] Surfactant F-2
[0199] [ka]
[0200] [Preparation of laminate A1] Polarizing plate 1 having a polarizer with a thickness of 8 μm and one surface of the polarizer exposed was produced in the same manner as in polarizing plate 02 with a one-side protective film described in WO 2015 / 166991. The surface of the polarizer of the polarizing plate 1 on which the polarizer was exposed and the surface of the optically absorptive anisotropic layer of the optically absorptive anisotropic film 1 prepared above were subjected to a corona treatment, and then bonded together using the PVA adhesive 1 described below to prepare a laminate A1.
[0201] (Preparation of PVA adhesive 1) 100 parts by mass of a polyvinyl alcohol resin containing acetoacetyl groups (average degree of polymerization: 1200, degree of saponification: 98.5 mol%, degree of acetoacetylation: 5 mol%) was dissolved in pure water at a temperature of 30°C to prepare an aqueous solution with a solid content of 3.7% by mass.
[0202] [Fabrication of image display device A1] An iPad Air (registered trademark) Wi-Fi model 16GB (manufactured by APPLE), which is an IPS mode liquid crystal display device, was disassembled and the liquid crystal cell was taken out. The viewer-side polarizing plate was peeled off from the liquid crystal cell, and the laminate A1 prepared above was attached to the surface from which the viewer-side polarizing plate was peeled off, using the following adhesive sheet 1, with the polarizing plate 1 side facing the liquid crystal cell side. At this time, the polarizing plate 1 was attached so that the absorption axis direction was the same as the absorption axis of the viewer-side polarizing plate attached to the product. After lamination, the product was reassembled to prepare an image display device A1.
[0203] (Preparation of adhesive sheet 1) The acrylate-based polymer was prepared according to the following procedure. In a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer, 95 parts by weight of butyl acrylate and 5 parts by weight of acrylic acid were polymerized by solution polymerization to obtain an acrylate polymer A1 having an average molecular weight of 2,000,000 and a molecular weight distribution (Mw / Mn) of 3.0.
[0204] Next, in addition to the obtained acrylate-based polymer A1 (100 parts by mass), Coronate L (a 75% by mass ethyl acetate solution of trimethylolpropane adduct of tolylene diisocyanate, number of isocyanate groups in one molecule: 3, manufactured by Nippon Polyurethane Industry Co., Ltd.) (1.0 part by mass), and a silane coupling agent KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd.) (0.2 parts by mass) were mixed, and finally ethyl acetate was added so that the total solid concentration was 10% by mass to prepare a composition for forming an adhesive. This composition was applied to a separate film surface-treated with a silicone-based release agent using a die coater and dried for 1 minute in an environment of 90 ° C. to obtain an acrylate-based adhesive sheet (adhesive sheet 1). The thickness of the adhesive sheet 1 was 25 μm, and the storage modulus of the adhesive sheet 1 was 0.1 MPa.
[0205] <Example 2> An image display device A2 of Example 2 was produced in the same manner as in Example 1, except that the optically absorptive anisotropic layer-forming composition P1 was changed to the optically absorptive anisotropic layer-forming composition P2.
[0206] ------------------------------------------------------------------ Composition of the optically absorptive anisotropic layer forming composition P2 ------------------------------------------------------------------ 0.40 parts by weight of the following dichroic substance D-4 0.15 parts by weight of the above dichroic substance D-2 0.63 parts by weight of the above dichroic substance D-3 3.65 parts by weight of the polymer liquid crystal compound P-1 Polymerization initiator IRGACUREOXE-02 (BASF) 0.040 parts by mass 0.060 parts by weight of the above compound E-1 0.060 parts by weight of the above compound E-2 0.010 parts by weight of the above surfactant F-1 0.015 parts by weight of the above surfactant F-2 Cyclopentanone 47.00 parts by mass Tetrahydrofuran 47.00 parts by mass Benzyl alcohol 1.00 parts by weight ------------------------------------------------------------------
[0207] Dichroic substance D-4
[0208] [ka]
[0209] <Example 3> An image display device A3 of Example 3 was produced in the same manner as in Example 1, except that the optically absorptive anisotropic layer-forming composition P1 was changed to the optically absorptive anisotropic layer-forming composition P3.
[0210] ------------------------------------------------------------------ Composition of the optically absorptive anisotropic layer forming composition P3 ------------------------------------------------------------------ 0.40 parts by weight of the above dichroic substance D-1 0.15 parts by weight of the above dichroic substance D-2 0.63 parts by weight of the above dichroic substance D-3 3.20 parts by weight of the following polymer liquid crystal compound P-2 0.45 parts by weight of the following low molecular weight liquid crystal compound M-1 Polymerization initiator IRGACUREOXE-02 (BASF) 0.040 parts by mass 0.060 parts by weight of the following compound E-1 0.060 parts by weight of the following compound E-2 0.010 parts by weight of the following surfactant F-1 0.015 parts by weight of the following surfactant F-2 Cyclopentanone 47.00 parts by mass Tetrahydrofuran 47.00 parts by mass Benzyl alcohol 1.00 parts by weight ------------------------------------------------------------------
[0211] Polymer liquid crystal compound P-2
[0212] [ka]
[0213] Low molecular liquid crystal compound M-1
[0214] [ka]
[0215] <Example 4> An image display device A4 of Example 4 was produced in the same manner as in Example 1, except that the optically absorptive anisotropic layer-forming composition P1 was changed to the optically absorptive anisotropic layer-forming composition P4.
[0216] ------------------------------------------------------------------ Composition of optically absorptive anisotropic layer forming composition P4 ------------------------------------------------------------------ 0.40 parts by weight of the following dichroic substance D-5 0.15 parts by weight of the above dichroic substance D-2 0.63 parts by weight of the above dichroic substance D-3 3.65 parts by weight of the polymer liquid crystal compound P-1 Polymerization initiator IRGACUREOXE-02 (BASF) 0.040 parts by mass 0.060 parts by weight of the above compound E-1 0.060 parts by weight of the above compound E-2 0.010 parts by weight of the above surfactant F-1 0.015 parts by weight of the above surfactant F-2 Cyclopentanone 47.00 parts by mass Tetrahydrofuran 47.00 parts by mass Benzyl alcohol 1.00 parts by weight ------------------------------------------------------------------
[0217] Dichroic substance D-5
[0218] [ka]
[0219] <Example 5> [Preparation of Cellulose Acylate Film 1] (Preparation of Core Layer Cellulose Acylate Dope) The following composition was charged into a mixing tank and stirred to dissolve each component, thereby preparing a cellulose acetate solution to be used as a cellulose acylate dope for the core layer. ------------------------------------------------------------------ Core layer: Cellulose acylate dope ------------------------------------------------------------------ Cellulose acetate with an acetyl substitution degree of 2.88: 100 parts by weight In the embodiment of JP 2015-227955 A 12 parts by weight of the polyester compound B 2 parts by weight of the following compound F Methylene chloride (first solvent) 430 parts by weight Methanol (second solvent) 64 parts by weight ------------------------------------------------------------------
[0220] Compound F
[0221] [ka]
[0222] (Preparation of outer layer cellulose acylate dope) To 90 parts by weight of the above-mentioned cellulose acylate dope for the core layer, 10 parts by weight of the following matting agent solution was added to prepare a cellulose acetate solution to be used as the cellulose acylate dope for the outer layer.
[0223] ------------------------------------------------------------------ Matting agent solution ------------------------------------------------------------------ Silica particles with an average particle size of 20 nm (AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd.) 2 parts by weight Methylene chloride (first solvent) 76 parts by weight Methanol (second solvent) 11 parts by weight 1 part by weight of the above-mentioned cellulose acylate dope for the core layer ------------------------------------------------------------------
[0224] (Preparation of Cellulose Acylate Film 2) The above core layer cellulose acylate dope and the above outer layer cellulose acylate dope were filtered through a filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm, and then the above core layer cellulose acylate dope and the outer layer cellulose acylate dope on both sides were simultaneously cast onto a drum at 20°C from a casting nozzle (band casting machine). Next, the film with a solvent content of approximately 20% by mass was peeled off from the drum, both ends in the width direction of the film were fixed with tenter clips, and the film was stretched in the transverse direction at a stretch ratio of 1.1 times while being dried. Thereafter, the film was further dried by conveying it between rolls of a heat treatment device to prepare an optical film having a thickness of 20 μm, which was used as cellulose acylate film 2. The in-plane retardation of the obtained cellulose acylate film 2 was 0 nm.
[0225] [Preparation of transparent support 2] The coating solution PA1 for forming a photo-alignment layer, which will be described later, was continuously applied onto the cellulose acylate film 2 using a wire bar. The support on which the coating film was formed was dried with hot air at 140° C. for 120 seconds, and then the coating film was irradiated with polarized ultraviolet light (10 mJ / cm 2 ). 2 A photo-alignment layer PA1 was formed by irradiating the TAC film with the photo-alignment layer (using an ultra-high pressure mercury lamp). The film thickness of the photo-alignment layer PA1 was 0.3 μm.
[0226] ------------------------------------------------------------------ (Coating liquid PA1 for photo alignment layer formation) ------------------------------------------------------------------ Polymer PA-1 shown below: 100.00 parts by weight Acid generator PAG-1 (listed below) 5.00 parts by weight 0.005 parts by weight of the acid generator CPI-110TF Isopropyl alcohol 16.50 parts by weight Butyl acetate 1072.00 parts by mass Methyl ethyl ketone 268.00 parts by mass ------------------------------------------------------------------
[0227] Polymer PA-1
[0228] [ka]
[0229] Acid generator PAG-1
[0230] [ka]
[0231] Acid generator CPI-110F
[0232] [ka]
[0233] [Formation of Polarizer Layer 1] On the obtained photoalignment layer PA1, the following composition 1 for forming a polarizer layer was continuously applied with a wire bar to form a coating layer 1. Next, the coating layer 1 was heated at 140° C. for 30 seconds, and then the coating layer 1 was cooled to room temperature (23° C.). Next, the obtained coating layer 1 was heated at 80° C. for 60 seconds and then cooled again to room temperature. After that, an LED lamp (center wavelength 365 nm) was used to illuminate the sample at an intensity of 200 mW / cm 2 The polarizer layer 1 was formed on the photo-alignment layer PA1 by irradiating the polarizer layer 1 for 2 seconds under the irradiation conditions above. The film thickness of the polarizer layer 1 was 1.6 μm.
[0234] ------------------------------------------------------------------ Composition of polarizer layer forming composition 1 ------------------------------------------------------------------ 0.25 parts by weight of the above dichroic substance D-1 0.36 parts by weight of the dichroic substance D-2 0.59 parts by weight of the above dichroic substance D-3 2.21 parts by mass of the polymer liquid crystal compound P-2 1.36 parts by mass of the low molecular weight liquid crystal compound M-1 Polymerization initiator IRGACUREOXE-02 (BASF) 0.200 parts by mass 0.026 parts by weight of the following surfactant F-3 Cyclopentanone 46.00 parts by mass Tetrahydrofuran 46.00 parts by weight Benzyl alcohol 3.00 parts by weight ------------------------------------------------------------------
[0235] Surfactant F-3
[0236] [ka]
[0237] [Formation of alignment layer 1] After the surface of the polarizer layer 1 was subjected to a corona treatment, the above-mentioned coating solution 1 for forming an alignment layer was continuously applied with a wire bar. Then, the coating solution was dried with hot air at 100° C. for 2 minutes, thereby forming a polyvinyl alcohol (PVA) alignment layer 1 having a thickness of 1.0 μm on the polarizer layer 1.
[0238] [Formation of Optically Absorbing Anisotropic Layer P1] On the obtained alignment layer 1, the above-mentioned composition for forming an optically absorptive anisotropic layer P1 was continuously applied with a wire bar to form a coating layer P1. Next, the coating layer P1 was heated at 140° C. for 30 seconds, and then cooled to room temperature (23° C.). The resulting coating layer P1 was then heated at 80° C. for 60 seconds and cooled again to room temperature. After that, an LED lamp (center wavelength 365 nm) was used to illuminate the sample at an intensity of 200 mW / cm 2 An optically absorptive anisotropic layer P1 was formed on the alignment layer 1 for 2 seconds under the irradiation conditions described above, to prepare a laminate A5. The coating layer P1 had a thickness of 3 μm, and the degree of alignment of the optically absorptive anisotropic layer P1 at a wavelength of 550 nm was 0.96.
[0239] [Preparation of image display device A5] An iPad Air (registered trademark) Wi-Fi model 16GB (manufactured by APPLE), which is an IPS mode liquid crystal display device, was disassembled and a liquid crystal cell was taken out. The viewer-side polarizing plate was peeled off from the liquid crystal cell, and the laminate A5 prepared above was attached to the surface from which the viewer-side polarizing plate was peeled off, using the pressure-sensitive adhesive sheet 1, with the cellulose acylate film 2 side facing the liquid crystal cell side. At this time, the polarizer layer 1 was attached so that the absorption axis direction was the same as the absorption axis of the viewer-side polarizing plate attached to the product. After lamination, the product was reassembled to prepare an image display device A5.
[0240] <Comparative Example 1> An image display device B1 was produced in the same manner as in Example 1, except that the optically absorptive anisotropic layer-forming composition P1 was changed to the optically absorptive anisotropic layer-forming composition P5.
[0241] ------------------------------------------------------------------ Composition of optically absorptive anisotropic layer forming composition P5 ------------------------------------------------------------------ 8.71 parts by weight of the above dichroic substance D-5 10.59 parts by weight of the following dichroic substance D-6 44.13 parts by weight of the following polymer liquid crystal compound P-3 Polymerization initiator IRGACUREOXE-02 (BASF) 0.040 parts by mass 0.800 parts by weight of the above compound E-1 0.800 parts by weight of the above compound E-2 0.960 parts by weight of the above surfactant F-2 Cyclopentanone 793.90 parts by mass Tetrahydrofuran 140.10 parts by mass ------------------------------------------------------------------
[0242] Dichroic substance D-6
[0243] [ka]
[0244] Polymer liquid crystal compound P-3
[0245] [ka]
[0246] <Comparative Example 2> An image display device B2 was produced in the same manner as in Comparative Example 1, except that the thickness of the optically absorptive anisotropic layer was changed from 3 μm to 4.5 μm.
[0247] <Performance evaluation> (1) Evaluation of the degree of orientation The degree of orientation of the obtained anisotropic light absorbing layer at a wavelength of 550 nm was calculated by the following method. Using AxoScan OPMF-1 (manufactured by Optoscience), the transmittance was measured at all azimuth angles at a wavelength of 550 nm while changing the polar angle, which is the angle with respect to the normal direction of the light absorption anisotropic layer, from 0 to 90 degrees in 5 degree increments. Next, after removing the influence of surface reflection, the transmittance at the azimuth angle and polar angle with the highest transmittance was defined as Tm(0), and the transmittance at an angle tilted by 40 degrees from the polar angle with the highest transmittance in the azimuth angle direction with the highest transmittance was defined as Tm(40). The absorbance was calculated from the obtained Tm(0) and Tm(40) using the following formula, and A(0) and A(40) were calculated. A = -log(Tm) Here, Tm represents the transmittance and A represents the absorbance. From the calculated A(0) and A(40), the degree of orientation S at a wavelength of 550 nm, defined by the following formula, was calculated. S=(4.6×A(40)-A(0)) / (4.6×A(40)+2×A(0)) The wavelength was changed from 550 nm to 420 nm, and the degree of orientation S at a wavelength of 420 nm was calculated.
[0248] (2) Evaluation of transmittance and color The image display device A1 produced above was measured using a measuring device (EZ-Contrast XL88, manufactured by ELDIM) to measure the luminance Y(0)A1 at a polar angle of 0° (front direction) of the white display screen, the luminance Y(30)A1 at a polar angle of 30° (diagonal direction), and the color tone a at a polar angle of 0°. * (0) A1, color b * (0) A1, color tone at polar angle 30° a * (30) A1, color b * (30)A1 was measured. In addition, in the preparation of the image display device A1, an image display device C was prepared in the same manner as in Example 1, except that a polarizing plate without a light absorbing anisotropic layer was attached to the liquid crystal cell, and the luminance Y(0)C at a polar angle of 0° (front direction) and the luminance Y(30)C at a polar angle of 30° (oblique direction) of the white display screen were measured in the same manner as described above. The front transmittance T0 (T(0)) and the oblique transmittance T30 (T(30)) were obtained by comparing with the luminance of the image display device C that does not include a light absorbing anisotropic layer. Specifically, the transmittance was calculated using the following formula, and evaluated according to the following criteria. T(0) = {Y(0)A1 / Y(0)C} × 100 T(30)={Y(30)A1 / Y(30)C}×100 A: Polar angle 0° (front) transmittance is 80% or more, In addition, the transmittance at a polar angle of 30° (diagonal) is less than 10%. B: Polar angle 0° (front) transmittance is lower than 80%. In addition, the transmittance at a polar angle of 30° (diagonal) is less than 10%. Or, polar angle 0° (front) transmittance is 80% or more, In addition, the transmittance at a polar angle of 30° (oblique) is higher than 10%. Or, the polar angle 0° (front) transmittance is lower than 80%, In addition, the transmittance at a polar angle of 30° (oblique) is higher than 10%.
[0249] The color was evaluated using the following formula and the color was evaluated according to the following criteria. |a * b * |= √(a * (0)A1 2 +b * (0)A1 2 ) +√(a * (30)A1 2 +b * (30)A1 2 ) AA:|a * b * | is less than 12 A:|a * b * | is 12 or more and less than 15 B:|a* b * 15 or more |
[0250] Instead of the image display device A1, the image display devices A2 to A5 and B1 to B2 were used, and the transmittance and color tone were evaluated according to the same procedures as above.
[0251] In the optically absorptive anisotropic layers obtained in Examples 1 to 5, the dichroic material was oriented perpendicular to the film surface. The definition of "perpendicular orientation" is as described above.
[0252] In Table 1, "550 nm orientation degree" represents the orientation degree of the optically absorptive anisotropic layer at a wavelength of 550 nm, and "420 nm orientation degree" represents the orientation degree of the optically absorptive anisotropic layer at a wavelength of 420 nm. In the "Transmittance" column, the "Front" column indicates the front transmittance, and the "30°" column indicates the transmittance at a polar angle of 30° (oblique).
[0253] [Table 1]
[0254] [Confirmation of suitability for curved surface processing] The laminate A1 produced in Example 1 was attached to the display screen of a smartphone (Galaxy Note9, manufactured by Samsung) having a curved surface, with the polarizing plate 1 side attached to the side to be bonded, using a commercially available adhesive SK2057 (manufactured by Soken Chemical & Engineering Co., Ltd.) The laminate A1 had a thickness of 100 μm or less and low rigidity, so that it could be neatly attached to the curved surface of the display screen without any air bubbles. Next, we will discuss a louver-type optical film (3M) that has the same performance as the optical film of the present invention and is widely used on the market. TM A security / privacy filter (PF12 H2 series) was attached to the display screen of the smartphone using a commercially available adhesive SK2057 (manufactured by Soken Chemical & Technology Co., Ltd.) The louver-type optical film is 500μm thick and highly rigid, so air bubbles formed in the curved parts of the display screen, making it impossible to attach it neatly.
[0255] <Example 6> [Formation of optically absorptive anisotropic layer] An optically absorptive anisotropic layer having a pattern of region A and region B was prepared as follows. The optically absorptive anisotropic layer-forming composition P1 was continuously applied onto the alignment layer PA1 of Example 1 with a wire bar to form a coating layer P1. Next, the coating layer P1 was heated at 140° C. for 30 seconds, and then cooled to room temperature (23° C.). The resulting coating layer P1 was then heated at 80° C. for 60 seconds and cooled again to room temperature. Then, light emitted from a high-pressure mercury lamp was passed through a mask at an illuminance of 28 mW / cm 2 By irradiating for 60 seconds under the irradiation condition, a light absorbing anisotropic layer having a cured region and an uncured region of the liquid crystal compound in the plane was produced on the alignment film PA. The mask had a mask pattern having a rectangular light transmitting region of 10 mm length x 50 mm width as region A, a light shielding region (region B) and a light transmitting region. The film having an optically absorptive anisotropic layer having cured regions (region A) and uncured regions (region B) of the liquid crystalline compound within its plane was immersed in ethanol for 3 minutes to wash away the unpolymerized liquid crystalline compound, thereby forming optically absorptive anisotropic film 6 having a patterned optically absorptive anisotropic layer having regions A and B with different degrees of polarization within its plane. In the region A, the dichroic material was oriented perpendicular to the film surface. The definition of "perpendicular orientation" is as described above. In addition, the degree of orientation in region A at a wavelength of 550 nm was 0.96, and the degree of orientation at a wavelength of 420 nm was 0.94. Furthermore, in region A, the transmittance at a polar angle of 30° was 10% or less, and the front transmittance was 80% or more. In region B, both the transmittance at a polar angle of 30° and the front transmittance were 80% or more.
[0256] [Preparation of laminate A6] Polarizing plate 1 having a polarizer with a thickness of 8 μm and one surface of the polarizer exposed was produced in the same manner as in polarizing plate 02 with a one-side protective film described in WO 2015 / 166991. The surface of the polarizing plate 1 on which the polarizer was exposed was attached to the surface of the optically absorptive anisotropic layer of the optically absorptive anisotropic film 6 prepared above using the pressure-sensitive adhesive sheet 1 to prepare a laminate A6.
[0257] [Preparation of image display device A6] Image display device A6 was produced in the same manner as in the above image display device A1, except that laminate A1 was replaced with laminate A6. Only the area A had a narrow viewing angle and was clearly visible only from the front.
[0258] <Example 7> [Formation of optically absorptive anisotropic layer] An optically absorptive anisotropic layer having a pattern of region A and region B was prepared as follows. The optically absorptive anisotropic layer-forming composition P1 was continuously applied onto the alignment layer PA1 of Example 1 with a wire bar to form a coating layer P1. Next, the coating layer P1 was heated at 140° C. for 30 seconds, and then cooled to room temperature (23° C.). The resulting coating layer P1 was then heated at 80° C. for 60 seconds and cooled again to room temperature. Then, light emitted from a high-pressure mercury lamp was passed through a mask at an illuminance of 28 mW / cm 2 By irradiating the liquid crystal compound on the alignment film for 60 seconds under the irradiation condition, a light absorbing anisotropic layer having a cured region and an uncured region of the liquid crystal compound in the plane was produced. The mask used had a rectangular light transmitting portion of 85 μm length × 50 mm width as region A, and a rectangular light blocking portion of 85 μm length × 50 mm width as region B, and the mask pattern had a length of 50 mm in the vertical direction, in which the regions A and B were alternately arranged. The film having an optically absorptive anisotropic layer having a cured region (region A) and an uncured region (region B) of the liquid crystalline compound within its plane was immersed in ethanol for 3 minutes to wash away the unpolymerized liquid crystalline compound, thereby forming optically absorptive anisotropic film 7 having an optically absorptive anisotropic layer having region A and region B with different degrees of polarization within its plane. In the region A, the dichroic material was oriented perpendicular to the film surface. The definition of "perpendicular orientation" is as described above. In addition, the degree of orientation in region A at a wavelength of 550 nm was 0.96, and the degree of orientation at a wavelength of 420 nm was 0.94. Furthermore, in region A, the transmittance at a polar angle of 30° was 10% or less, and the front transmittance was 80% or more. In region B, both the transmittance at a polar angle of 30° and the front transmittance were 80% or more.
[0259] [Preparation of laminate A7] Polarizing plate 1 having a polarizer with a thickness of 8 μm and one surface of the polarizer exposed was produced in the same manner as in polarizing plate 02 with a one-side protective film described in WO 2015 / 166991. The surface of the polarizer of the polarizing plate 1 where the polarizer was exposed was attached to the surface of the optically absorptive anisotropic layer of the prepared optically absorptive anisotropic film 7 using a pressure sensitive adhesive SK2057 (manufactured by Soken Chemical & Engineering Co., Ltd.) to prepare a laminate A7.
[0260] [Preparation of image display device A7] A Samsung smartphone Galaxy S4 was disassembled, and the polarizing plate attached to the EL substrate was peeled off. Pure Ace WR W142 (Teijin) and the above-described laminate A7 were attached to the EL substrate from which the polarizing plate had been peeled off, using adhesive SK2057 (Soken Chemical Industries, Ltd.) so that Pure Ace WR W142 was on the EL substrate side and the light absorption anisotropic film 7 side of the laminate A7 was on the viewing side. At this time, the laminate A7 was attached so that region A and region B were aligned with the pixels of the EL substrate.
[0261] For the manufactured image display device A7, image α, which displays an image only in pixels overlapping region A, and image β, which displays an image only in pixels overlapping region B, were prepared. When image α was displayed, the image became dark and could not be recognized when viewed from a direction at a polar angle of 30° with respect to the absorption axis of the film attached to the image display device A7. When image β was displayed, the image was only slightly changed in brightness and could be recognized when viewed from a direction at a polar angle of 30° with respect to the absorption axis of the film attached to the image display device A7. Therefore, it was confirmed that an image display device capable of switching the viewing angle can be manufactured by using patterned light-absorbing anisotropic film 7.
[0262] <Example 8> With reference to the examples in JP2017-098246A, a backlight module capable of switching the viewing angle was produced using the light absorptive anisotropic film 1 produced in Example 1 as the optical filter element 140. FIG. 1 is a schematic diagram of a backlight module according to an embodiment of the present invention. Referring to FIG. 1, a backlight module 100 of this embodiment includes a first surface light source assembly 110, a second surface light source assembly 120, a first optical sheet 130 and a light filter element 140. As shown in FIG. The first surface light source assembly 110 includes a first light emitting unit 111 and a first light guide plate 112. The first light guide plate 112 has a first light emitting surface 114 and a first bottom surface 115 facing each other, and a first light incident surface 113 located between the first light emitting surface 114 and the first bottom surface 115. The first light emitting unit 111 is located near the first light incident surface 113 of the first light guide plate 112. The second surface light source assembly 120 is located above the first surface light source assembly 110, and includes a second light emitting unit 121 and a second light guide plate 122, the second light guide plate 122 having a second light emitting surface 124 and a second bottom surface 125 facing each other, and a second light incident surface 123 located between the second light emitting surface 124 and the second bottom surface 125, and the second light emitting unit 121 is located near the second light incident surface 123 of the second light guide plate 122. The first optical sheet 130 is located above the second surface light source assembly 120 and includes a plurality of prism pillars 131 arranged in a first direction (e.g., the X-axis direction), with the ends 132 of the prism pillars 131 facing the second surface light source assembly 120. In this embodiment, the axial extension direction of the prism pillars 131 extends in a second direction (e.g., the Z-axis direction), and the first direction is perpendicular to the second direction. The optical filter element 140 is located between the first surface light source assembly 110 and the second surface light source assembly 120, and the optical filter element 140 transmits incident light within a predetermined incident angle range. The first light-emitting unit 111 provides light rays that enter the first light guide plate 112 through a first light incident surface 113, and the first light guide plate 112 converts the light rays into a first surface light source that exits from a first light exit surface 114 of the first light guide plate 112. The second light-emitting unit 121 provides light rays that enter the second light guide plate 122 through a second light incident surface 123, and the second light guide plate 122 converts the light rays into a second surface light source that exits from a second light exit surface 124 of the second light guide plate 122. The first light-emitting unit 111 and the second light-emitting unit 121 each include, for example, but are not limited to, a substrate (not shown) and a plurality of light-emitting elements (not shown) disposed on the substrate, such as light-emitting diodes. The present invention does not limit the types of the first light-emitting unit 111 and the second light-emitting unit 121. In addition, the first bottom surface 115 of the first light guide plate 112 and the second bottom surface 125 of the second light guide plate 122 may be provided with a microstructure (not shown) for adjusting the type of light when the light is emitted from the first light-emitting surface 114 and the second light-emitting surface 124. The microstructure may be, but is not limited to, a halftone dot, a groove, etc. The first optical sheet 130 is, for example, an inverted prism sheet or a composite optical sheet having an inverted prism sheet structure, and light rays with different incident angles can be made to have different exit angles when they are emitted from the first optical sheet 130. Taking the light rays incident on the first surface 133 of the prism pillar 131 as an example, when the incident angle is relatively large, the light rays are refracted to the second surface 134 and are reflected by the second surface 134, and then are emitted from the light exit side 135 of the first optical sheet 130 at a relatively small exit angle. When the incident angle is relatively small, the light rays are refracted and then are emitted from the light exit side 135 of the first optical sheet 130 at a relatively large exit angle. In addition, the axial extension direction of each prism pillar 131 is, for example, parallel to the Z-axis direction. The tip 132 of each prism pillar 131 may be chamfered, for example, rounded. Specifically, when the first light-emitting unit 111 is turned on, the light ray L1 is mainly incident on the first surface 133 and the second surface 134 of the prism pillar 131 of the first optical sheet 130 at a relatively small incident angle, and is therefore emitted from the light-emitting side 135 of the first optical sheet 130 at a relatively large exit angle. When the second light-emitting unit 121 is turned on, the light ray L2 is mainly incident on the first surface 133 and the second surface 134 of the prism pillar 131 of the first optical sheet 130 of FIG. 1 at a relatively large incident angle, and is therefore emitted from the light-emitting side 135 of the first optical sheet 130 at a relatively small exit angle. When the first light-emitting unit 111 and the second light-emitting unit 121 are both turned on, the light ray L1 with a relatively large exit angle and the light ray L2 with a relatively small exit angle are emitted from the light-emitting side 135 of the first optical sheet 130, and after being overlapped, a wide viewing angle surface light source can be formed. Therefore, when the first light-emitting unit 111 and the second light-emitting unit 121 are both on, it can be defined as a wide viewing angle mode. On the other hand, when the first light-emitting unit 111 is off and the second light-emitting unit 121 is on, a narrow viewing angle surface light source is formed after the light ray L2 with a relatively small emission angle is emitted from the light-emitting side 135 of the first optical sheet 130. Therefore, when the second light-emitting unit 121 is on and the first light-emitting unit 111 is off, it can be defined as a narrow viewing angle mode. That is, the backlight module shown in FIG. 1 corresponds to a backlight module capable of switching the viewing angle. From the above, it was confirmed that by using the light absorptive anisotropic film 1 of the present invention as the optical filter element 140, a backlight module with high front luminance and switchable viewing angle can be obtained. [Explanation of symbols]
[0263] 100 Backlight Module 110 First surface source assembly 111 First light emitting unit 112 First light guide plate 113 First entrance plane 114 First exit surface 115 First bottom surface 120 Second surface source assembly 121 Second light emitting unit 122 Second light guide plate 123 Second entrance plane 124 Second exit surface 125 Second bottom surface 130 First Optical Sheet 131 Prism Pillar 132 Tip 133 First surface 134 Second surface 135 Seconded party 140 Optical filter element (light absorbing anisotropic film) 151, 153 Diffusion sheet 152 Prism sheet
Claims
1. Contains a liquid crystal compound and at least one dichroic substance, A light absorbing anisotropic layer in which the dichroic material is oriented perpendicular to a main surface, The optically absorptive anisotropic layer has a degree of orientation of 0.95 or more at a wavelength of 550 nm.
2. 2. The optically absorptive anisotropic layer according to claim 1, wherein the optically absorptive anisotropic layer has a degree of orientation of 0.93 or more at a wavelength of 420 nm.
3. A light absorption anisotropic layer having a region A containing a liquid crystalline compound and at least one dichroic substance, and a region B having a higher oblique transmittance as viewed from a polar angle of 30° than the region A, the dichroic material is oriented perpendicular to the main surface, An optically absorptive anisotropic layer, wherein the degree of orientation in the region A at a wavelength of 550 nm is 0.95 or more.
4. 4. The optically absorptive anisotropic layer according to claim 3, wherein the region A has an oblique transmittance as viewed from a polar angle of 30° of 10% or less, and the region B has an oblique transmittance as viewed from a polar angle of 30° of 80% or more.
5. An optically absorptive anisotropic layer described in any one of claims 1 to 4, further comprising a vertical alignment agent.
6. The optically absorbing anisotropic layer of claim 5, wherein the vertical alignment agent comprises a boronic acid compound.
7. The optically absorptive anisotropic layer of claim 5, wherein the vertical alignment agent comprises an onium salt.
8. 8. A laminate comprising the light absorptive anisotropic layer according to claim 1 and a polarizer layer in which a dichroic material is oriented horizontally to the film surface.
9. 8. A laminate comprising the light absorptive anisotropic layer according to claim 1 and a polarizer layer in which a liquid crystalline compound and a dichroic substance are oriented horizontally to the film surface.
10. 10. An optical film comprising the optically absorptive anisotropic layer according to any one of claims 1 to 7, or the laminate according to claim 8 or 9.
11. An image display device comprising the optically absorptive anisotropic layer according to any one of claims 1 to 7, the laminate according to claim 8 or 9, or the optical film according to claim 7.
12. The image display device according to claim 11, wherein the display portion has a curved surface.
13. 5. An image display device having the optically absorptive anisotropic layer according to claim 3, which is capable of switching the viewing angle.
14. 3. An image display device having the optically absorptive anisotropic layer according to claim 1, which is capable of switching the viewing angle.
15. An image display device capable of switching the viewing angle, comprising the light absorption anisotropic layer according to any one of claims 1 to 7 and a liquid crystal cell.
16. A first light guide plate, a light filter element, and a second light guide plate are arranged in this order from the viewing side. The optical filter element is the optically absorptive anisotropic layer according to claim 1 or 2. A backlight module that allows you to switch the viewing angle.
Citation Information
Patent Citations
Viewing angle control system and image display device
JP2009145776A
Optical film and liquid crystal display device
WO2018079854A1
Display device
WO2019235355A1