Combined hexagonal belt and its manufacturing method
The bonded hexagonal belt, connected by continuous fabrics with a crosslinked rubber composition, addresses manufacturing difficulties and enhances transmission performance in high-load environments by ensuring stable, high-capacity, and double-sided power transmission.
Patent Information
- Application Number
- JP2022118553
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-29
- Filing Date
- 2022-07-26
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2042-07-26
AI Technical Summary
Connecting multiple hexagonal belts in the width direction is difficult to manufacture and has not been practically implemented, leading to issues such as tension differences, overturning, and vibration in high-load environments.
A bonded hexagonal belt is manufactured using a fabric containing a crosslinked rubber composition, with adjacent hexagonal belt parts connected by continuous fabrics on both inner and outer circumferential surfaces, allowing for high-performance double-sided transmission and high-capacity transmission.
The solution enables stable, high-performance double-sided transmission and high-capacity transmission by integrating hexagonal belt portions through a continuous fabric connection, overcoming manufacturing challenges and improving durability.
Smart Images

Figure 0007554232000031 
Figure 0007554232000023 
Figure 0007554232000019
Abstract
Description
[Technical field]
[0001] The present invention relates to a combined hexagonal belt in which multiple V-belts capable of double-sided transmission are connected in the width direction, and a method for manufacturing the same. [Background technology]
[0002] Friction transmission belts such as V-belts, V-ribbed belts, and flat belts are known as power transmission belts. There are two types of V-belts: raw-edge type (raw-edge V-belts) in which the friction transmission surface is an exposed rubber layer, and wrapped type (wrapped V-belts) in which the friction transmission surface (V-shaped side) is covered with an outer covering fabric. These V-belts are widely and commonly used in general industrial and agricultural machinery.
[0003] A single V-belt is used in applications where a single V-belt is sufficient to transmit power. For example, in high-load operating environments that require enormous power transmission while repeatedly rotating forward and backward on multiple shafts, such as large agricultural machinery used on large farms in Europe and the United States, multiple V-belts must be used simultaneously. In other words, multiple V-belts must be wrapped around the pulleys of the belt transmission mechanism in parallel (multiple V-belts) to rotate and run.
[0004] However, when multiple V-belts are used, tension differences occur between the parallel V-belts, which may impair stable power transmission. Furthermore, contact between adjacent V-belts may cause the inner and outer circumferential sides of the belt to reverse, resulting in an inverted structure, which may result in overturning. In addition, the running layout of the belt transmission mechanism in large agricultural machines in Europe and the United States has a very long center distance between the pulleys around which the V-belt is wound, which makes the V-belt prone to vibrating significantly while running, and if the lengths of the multiple belts are not uniform, there is a risk of vibration.
[0005] Therefore, in an environment where multiple V-belts are run in parallel, a combined belt (combined V-belt) is used, which is configured by connecting multiple annular V-belt parts having a similar configuration to the V-belt or a configuration corresponding to the V-belt in the belt width direction. This combined belt is configured as a V-belt in which multiple belt parts are arranged in parallel and connected and connected with tie bands (connecting members such as fabric).
[0006] Regarding the joined V-belts, for example, a raw edge joined V-belt is disclosed in Figures 1 and 2 of JP 10-274290 A (Patent Document 1) and Figure 2 of JP 2001-241513 A (Patent Document 2), and a wrapped joined V-belt is disclosed in Figure 1 of JP 04-351350 A (Patent Document 3) and Figure 1 of JP 2020-3061 A (Patent Document 4). These joined V-belts can transmit large power by multiple V-shaped protrusions while solving the above-mentioned problems that may occur when multiple V-belts are hung on pulleys.
[0007] On the other hand, in a belt transmission mechanism requiring multi-axis transmission using such a coupled V-belt, power may be transmitted not only by the inner peripheral surface of the belt but also by the outer peripheral surface (back surface) of the belt. In such a transmission mechanism, in order to improve the transmission performance on the outer peripheral surface (back surface), it is preferable to have a V-belt portion having a V-shaped side surface that can contact a V-pulley on the outer peripheral surface as well. In other words, if the belt has V-shaped side surfaces that can contact a V-pulley on both the inner peripheral surface and the outer peripheral surface and is configured as an endless belt with a substantially hexagonal cross section, it becomes a coupled V-belt that can transmit power on both sides with high performance.
[0008] In addition, regarding a V-belt capable of double-sided transmission (commonly known as a hexagonal belt), a single belt (not connected in multiples) is disclosed in, for example, JP 2018-059626 A (Patent Document 5) and JP 2019-032078 A (Patent Document 6). This hexagonal belt has V-shaped side surfaces that can contact a V-pulley on both the inner and outer circumferential surfaces, and is configured as an endless V-belt having a hexagonal cross section. In addition, a core body is provided between the radially inner rubber layer portion and the radially outer rubber layer portion of the hexagonal belt. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 10-274290 [Patent Document 2] JP 2001-241513 A [Patent Document 3] Japanese Patent Application Publication No. 04-351350 [Patent Document 4] JP 2020-3061 A [Patent Document 5] JP 2018-059626 A [Patent Document 6] JP 2019-032078 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, connecting multiple hexagonal belts in the width direction is difficult in terms of manufacturing, and has not yet been put to practical use.
[0011] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a linked hexagonal belt capable of high performance double-sided transmission and high capacity transmission, and a manufacturing method thereof. [Means for solving the problem]
[0012] As a result of intensive research into achieving the above-mentioned object, the present inventors have found that in a joined hexagonal belt including a plurality of hexagonal belt portions having a hexagonal cross section aligned in the belt width direction, the inner and outer circumferential surfaces of the belt are each covered with a fabric which may contain a cross-linked rubber composition, and adjacent hexagonal belt portions are connected with a continuous piece of the fabric, thereby providing a connected-type hexagonal belt capable of high-performance double-sided transmission and high-capacity transmission, and have completed the present invention.
[0013] That is, the combined hexagonal belt according to the embodiment [1] of the present invention is as follows: A combined hexagonal belt in which a plurality of hexagonal belt portions each having a hexagonal cross section are arranged in the belt width direction, the hexagonal belt portion includes a core layer, an inner rubber layer laminated on the inner circumferential surface side of the core layer and having a trapezoidal cross section, an inner outer covering material covering the inner rubber layer and including an inner outer covering fabric, an outer rubber layer laminated on the outer circumferential surface side of the core layer and having a trapezoidal cross section, and an outer outer covering material covering the outer rubber layer and including an outer outer covering fabric, Adjacent hexagonal belt portions are connected to each other via connecting portions, and The adjacent inner cover fabric is formed from a continuous inner fabric, and the adjacent outer cover fabric is formed from a continuous outer fabric.
[0014] Aspect [2] of the present invention is an aspect of aspect [1], wherein the connecting portion includes an inner connecting material that forms the inner surface of the belt and an outer connecting material that forms the outer surface of the belt, the inner connecting material includes an inner connecting fabric, and the outer connecting material includes an outer connecting fabric, the inner fabric is a fabric in which the inner connecting fabric and the inner outer cover fabric are continuous, and the outer fabric is a fabric in which the outer connecting fabric and the outer outer cover fabric are continuous.
[0015] The embodiment [3] of the present invention is an embodiment in which, in the embodiment [2], the connecting portion further contains a cross-linked rubber composition.
[0016] Aspect [4] of the present invention is any of aspects [1] to [3] above, wherein an inner reinforcing material is interposed between the inner outer covering material and the inner rubber layer, and an outer reinforcing material is interposed between the outer outer covering material and the outer rubber layer.
[0017] Aspect [5] of the present invention is any of aspects [1] to [4] above, wherein the inner rubber layer includes a first inner rubber layer laminated on the core layer side, and a second inner rubber layer having a lower rubber hardness than the first inner rubber layer and laminated on the inner circumferential side of the belt.
[0018] The present invention also includes, as aspect [6], a method for producing a combined hexagonal belt according to any one of aspects [1] to [5], which includes a cross-linking molding step of heating and pressurizing a combined hexagonal belt precursor placed in a press mold to cross-link the combined hexagonal belt.
[0019] Aspect [7] of the present invention is an aspect in which, in the manufacturing method of aspect [6], the connecting portion contains a cross-linked rubber composition, and in the cross-linking molding step, the cross-linking molding of the hexagonal belt portion and the cross-linking molding of the connecting portion are carried out simultaneously.
[0020] The present invention relates to an embodiment [8] of the manufacturing method of the embodiment [7], wherein the press mold is a combination of an inner press mold having an inner groove portion corresponding to the inner shape of the combined hexagonal belt and an outer press mold having an outer groove portion corresponding to the outer shape of the combined hexagonal belt, The bonded hexagonal belt precursor includes an inner fabric precursor for forming an inner fabric, an outer fabric precursor for forming an outer fabric, and a hexagonal belt portion precursor including an uncrosslinked rubber composition, In the crosslinking molding process, the inner fabric precursor is arranged along the inner groove portion, the hexagonal belt portion precursor is laminated onto the inner fabric precursor, the outer fabric precursor is arranged along the hexagonal belt portion precursor, and then the outer groove portion is brought into contact with the outer fabric precursor, and the combined hexagonal belt precursor is sandwiched between the inner press mold and the outer press mold.
[0021] Aspect [9] of the present invention is an aspect in which the manufacturing method of aspect [8] is a manufacturing method of a bonded hexagonal belt including an inner reinforcement and an outer reinforcement, the hexagonal belt portion precursor is a combination of an inner hexagonal belt portion precursor and an outer hexagonal belt portion precursor, and in the crosslinking molding process, the inner hexagonal belt portion precursor is laminated to the inner fabric precursor, and then the outer hexagonal belt portion precursor is laminated.
[0022] Aspect
[10] of the present invention is the manufacturing method of aspect [9], further comprising a hexagonal belt portion precursor preparation step as a pre-step of the cross-linking molding step, The hexagonal belt portion precursor manufacturing step includes a step of manufacturing an inner hexagonal belt portion precursor and a step of manufacturing an outer hexagonal belt portion, a step of preparing the inner hexagonal belt portion precursor, comprising: laminating a core layer precursor for forming a core layer on a thin outer rubber layer precursor for forming a part of the outer rubber layer; laminating an inner rubber layer precursor for forming an inner rubber layer on the core layer precursor; and then cutting a side surface of the inner rubber layer precursor; In this embodiment, the step of producing the outer hexagonal belt portion precursor is a step of cutting a side surface of a thick outer rubber layer precursor for forming the remaining portion of the outer rubber layer. Effect of the Invention
[0023] In the present invention, in a combined hexagonal belt including a plurality of hexagonal belt portions arranged in the belt width direction, the inner and outer circumferential surfaces of the belt are each covered with a fabric that may contain a cross-linked rubber composition, and adjacent hexagonal belt portions are connected to each other by the continuous fabric, so that a combined hexagonal belt capable of high-performance double-sided transmission and high-capacity transmission can be provided. Furthermore, although it was difficult to manufacture a plurality of hexagonal belts in the width direction, the present invention has succeeded in easily manufacturing a combined hexagonal belt having the above characteristics by using a specific manufacturing method. [Brief description of the drawings]
[0024] [Figure 1]FIG. 1 is a schematic, partially cutaway perspective view showing an example of a coupled hexagonal belt according to the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view for explaining a hexagonal belt portion and a connecting portion in FIG. [Diagram 3] FIG. 3 is a schematic partial cross-sectional perspective view showing another example of a coupled hexagonal belt according to the present disclosure. [Figure 4] FIG. 4 is a schematic cross-sectional view showing an example of a coupled hexagonal belt according to the present disclosure, and an enlarged view of a connecting portion in the cross-sectional view. [Diagram 5] FIG. 5 is a cross-sectional view of a hexagonal belt portion of the combined hexagonal belt of FIG. [Figure 6] FIG. 6 is a cross-sectional view of the hexagonal belt portion of FIG. 5, in which the inner rubber layer and the outer rubber layer have a two-layer structure. [Figure 7] FIG. 7 is a cross-sectional view of a hexagonal belt portion of the combined hexagonal belt of FIG. [Figure 8] FIG. 8 is a cross-sectional view of the hexagonal belt portion of FIG. 7, in which the inner rubber layer and the outer rubber layer have a two-layer structure. [Figure 9] FIG. 9 is a schematic diagram showing a cutting step for cutting the hexagonal belt portion precursor into rings. [Figure 10] FIG. 10 is a schematic diagram showing a skiving process in which a cut hexagonal belt portion precursor is cut into a V shape. [Figure 11] FIG. 11 is a schematic diagram showing a cutting step for cutting the inner hexagonal belt portion precursor into rings. [Figure 12] FIG. 12 is a schematic diagram showing the steps of producing an inner hexagonal belt portion precursor having a reinforcing material. [Figure 13] FIG. 13 is a schematic diagram showing the steps of producing an outer hexagonal belt portion precursor having a reinforcing material. [Figure 14] FIG. 14 is a schematic overall view showing the steps of connecting and cross-linking the hexagonal belt portion precursor. [Figure 15] FIG. 15 is a cross-sectional view taken along line AB in FIG. [Figure 16]16 is a schematic perspective view of the protrusion of the inner press mold in FIG. 15 as viewed in the direction from C to D. FIG. [Figure 17] FIG. 17 is a schematic diagram showing a process of aligning an inner fabric precursor along an inner groove of an inner press mold and then fitting a part of a hexagonal belt portion precursor into the inner groove along which the inner fabric precursor has been aligned. [Figure 18] FIG. 18 is a cross-sectional view showing a state in which a hexagonal belt portion precursor is fitted into an inner groove of an inner press mold via an inner fabric precursor. [Figure 19] FIG. 19 is a cross-sectional view showing a state in which an outer fabric precursor is disposed along the hexagonal belt portion precursor of FIG. 18 using a jig. [Figure 20] FIG. 20 is a cross-sectional view showing a state in which the outer groove of the outer press mold is brought into contact with the outer fabric precursor of FIG. 19, and the combined hexagonal belt precursor is sandwiched between the inner press mold and the outer press mold. [Figure 21] FIG. 21 is a cross-sectional view showing a state in which a part of a hexagonal belt portion precursor is fitted into an inner groove of an inner press mold via an inner fabric precursor. [Figure 22] FIG. 22 is a cross-sectional view showing a state in which the remaining part of the hexagonal belt portion precursor is laminated on a part of the hexagonal belt portion precursor of FIG. [Figure 23] FIG. 23 is a cross-sectional view showing a state in which an outer fabric precursor is disposed along the hexagonal belt portion precursor of FIG. 22 using a jig. [Figure 24] FIG. 24 is a cross-sectional view showing a state in which the outer groove of the outer press mold is brought into contact with the outer fabric precursor of FIG. 23 and the combined hexagonal belt precursor is sandwiched between the inner press mold and the outer press mold. [Diagram 25] FIG. 25 is a cross-sectional view showing the state in which the cross-linked hexagonal belt precursor obtained after removing the press mold is cut. [Figure 26] FIG. 26 is a diagram showing a multi-axis layout which is an arrangement for a belt running test of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] <Combined hexagonal belt> The combined hexagonal belt of the present invention is a friction drive belt capable of transmitting power on both the outer and inner circumferential sides, and for example, a fabric covering the surface of a plurality of hexagonal belts (a plurality of hexagonal belt parts aligned in the belt width direction) aligned in parallel with their longitudinal directions is divided into an outer circumferential side and an inner circumferential side, and each of them is connected in the width direction while also serving as a tie band (connecting member). That is, the fabric has a function of covering the surface of the hexagonal belt parts and a function of connecting adjacent hexagonal belt parts, and by the fabric having such a structure, it has been possible to successfully provide a robust combined hexagonal belt, which can transmit power on both sides with high performance and can transmit power at a high capacity.
[0026] The combined hexagonal belt of the present invention will be described in detail below with reference to the accompanying drawings as necessary. In the following description, the same reference numerals may be used to designate elements (or members) that are the same or have the same functions.
[0027] An example of the combined hexagonal belt of the present invention is shown in Figures 1 and 2. As shown in Figures 1 and 2, this combined hexagonal belt 1 has two hexagonal belt parts arranged in parallel with their tops facing each other and spaced apart in the belt width direction, and the outer periphery (surface) of the two hexagonal belt parts is covered with an inner outer covering material 4 and an outer outer covering material 6. The inner outer covering material 4 and the outer outer covering material 6 are formed of a fabric containing a crosslinked rubber composition.
[0028] In the joined hexagonal belt 1, adjacent hexagonal belt parts are connected by a connecting part including an inner connecting member 7 and an outer connecting member 8. The inner connecting member 7 and the outer connecting member 8 are also formed of a fabric containing a crosslinked rubber composition. The fabric of the inner connecting member 7 is continuous with the fabric of the inner outer covering material 4, forming an inner fabric integrated with the inner circumferential surface of the belt. The fabric of the outer connecting member 8 is also continuous with the fabric of the outer outer covering material 6, forming an outer fabric integrated with the outer circumferential surface of the belt. Furthermore, in addition to the fabric, the inner connecting member 7 and the outer connecting member 8 contain a crosslinked rubber composition that has permeated the fabric in advance and a crosslinked rubber composition that has flowed in from the hexagonal belt part and crosslinked, and are integrated with the fabric together with the crosslinked rubber composition present between the inner connecting member 7 and the outer connecting member 8. Therefore, the connecting part is a strong composite in which the fabric and the crosslinked rubber composition are integrated.
[0029] The inside of the hexagonal belt portion covered with the inner outer covering material 4 and the outer outer covering material 6 has a structure in which, from the inner circumference side of the belt, an inner rubber layer 3, a core layer 2 including a core wire 2a, and an outer rubber layer 5 are laminated.
[0030] The combined hexagonal belt 10 shown in Fig. 3 is a combined hexagonal belt of the same embodiment as the combined hexagonal belt of Fig. 1, except that a reinforcing material is interposed between the inner and outer covering materials and the inner and outer rubber layers. That is, in this combined hexagonal belt, the surfaces of the inner rubber layer 13, the core layer 12 including the core wires 12a, and the outer rubber layer 15 are covered with a reinforcing material 11, and the inner and outer covering materials 14 and 16 are laminated on the reinforcing material 11, and the fabrics of the inner and outer covering materials 14 and 16 are continuous with the fabrics of the inner connecting material 17 and the outer connecting material 18, respectively. By interposing the reinforcing material 11, the combined hexagonal belt 10 reinforces the friction transmission surface, improving durability (wear resistance).
[0031] The structure and size of the combined hexagonal belt of the present disclosure will be described in more detail with reference to FIG. 4. The combined hexagonal belt 1 of FIG. 4 is a schematic cross-sectional view of a combined hexagonal belt without a reinforcing material, as in FIG. 1, but H in the figure indicates the thickness (height in the belt thickness direction) of the hexagonal belt part, W in the figure indicates the width of the hexagonal belt part, and P in the figure indicates the pitch (distance between the centers of adjacent hexagonal belt parts). Furthermore, in the enlarged view of the connecting part, d in the figure indicates the thickness (minimum thickness) of the connecting part, and e in the figure indicates the width (spacing between adjacent hexagonal belt parts) of the connecting part. Regarding these sizes, the dimensions of AA type, BB type, and CC type, which are representative examples of combined hexagonal belts, are shown in Table 1.
[0032] [Table 1]
[0033] In the combined hexagonal belt of the present invention, the thickness H (average thickness) of the hexagonal belt portion (combined hexagonal belt) is, for example, 5 to 30 mm, preferably 7 to 20 mm, and more preferably 10 to 18 mm.
[0034] The width W (average width) of the hexagonal belt portion is, for example, 7 to 40 mm, preferably 10 to 30 mm, and more preferably 12 to 25 mm.
[0035] The pitch P (average distance) of the hexagonal belt portion is, for example, 5 to 50 mm, preferably 8 to 40 mm, and more preferably 10 to 30 mm.
[0036] The combined hexagonal belt of the present invention may have a plurality of hexagonal belt parts aligned parallel to the width direction, and is not limited to an arrangement with intervals as shown in Figs. 1 to 4, but may be arranged without intervals. In an arrangement with hexagonal belt parts aligned without intervals, the boundaries between adjacent inner outer covering materials and the boundaries between adjacent outer covering materials become the connecting parts. Among these, from the viewpoint of productivity, it is preferable to arrange adjacent combined hexagonal belt parts with intervals.
[0037] The thickness d (average thickness) of the connecting portion is, for example, 0.5 to 5 mm, preferably 0.8 to 4 mm, and more preferably 1 to 3 mm. If the thickness d of the connecting portion is too thin, the durability may decrease, and conversely, if it is too thick, the power transmission may decrease.
[0038] When the hexagonal belt parts are arranged at intervals, the width e of the connecting part may be 0.5 mm or more, for example, 0.5 to 8 mm, preferably 1 to 5 mm, and more preferably 1.5 to 4 mm. If the width e of the connecting part is too small, there is a risk of a decrease in productivity.
[0039] In this example, a layer formed of a crosslinked rubber composition is present between the inner and outer connecting members forming the connecting portion. The inner and outer connecting members are not limited to fabrics containing a crosslinked rubber composition, i.e., fabrics in which the crosslinked rubber composition has permeated between the fibers inside, as shown in Figs. 1 and 2, and may be fabrics not containing a crosslinked rubber composition, but fabrics containing a crosslinked rubber composition are preferred in terms of improving the mechanical properties of the connecting members. As shown in Fig. 4, in the connecting portion, a layer formed of a crosslinked rubber composition is usually present between the inner and outer connecting members. The layer formed of the crosslinked rubber composition may be an integral structure as shown in Fig. 4, or may be a structure in which the inner and outer connecting members are separated by contact at the center of the connecting portion.
[0040] The number of hexagonal belt portions is not limited to 2-3 as shown in Figs. 1-4, but may be any number as long as it is plural, for example 2-10, preferably 2-8, and more preferably 2-6.
[0041] [Hexagonal belt part] The shape (external shape) of the hexagonal belt part may be the same as that of a conventional hexagonal belt, that is, it may be endless, and the cross-sectional shape perpendicular to the belt longitudinal direction may be substantially hexagonal. The structure (internal structure) of the hexagonal belt part may be the same as that of a conventional hexagonal belt, and may be the same as that of a conventional hexagonal belt, and may be the same as that of a wrapped V-belt part that includes a core layer (bonded rubber layer) including a core body, an outer rubber layer laminated on the outer periphery side of the core layer, and an inner rubber layer laminated on the inner periphery side of the core layer, and is covered with an outer covering cloth (cover cloth) over the entire belt surface including the friction transmission surface. In such a hexagonal belt part, both left and right side surfaces of the V-shaped cross section facing the core layer (both side surfaces of the cross-section trapezoidal shape) form the friction transmission surface. Examples of the structure of the hexagonal belt part include the structures shown in Figs. 5 to 8.
[0042] Fig. 5 is a cross-sectional view of the hexagonal belt portion of the combined hexagonal belt of Fig. 1. The hexagonal belt portion shown in Fig. 5 is formed of a core layer 2 formed of adhesive rubber 2b including a core (core wire) 2a, an inner rubber layer 3 laminated on the inner peripheral surface side of the core layer 2 and having a trapezoidal cross section, an inner outer covering material 4 covering the inner rubber layer 3 and including an inner outer covering fabric, an outer rubber layer 5 laminated on the outer peripheral surface side of the core layer 2 and having a trapezoidal cross section, and an outer outer covering material 6 covering the outer rubber layer 5 and including an outer outer covering fabric. That is, from the inner periphery of the belt, it is formed of an endless belt body in which an inner rubber layer 3, a core layer 2, and an outer rubber layer 5 are laminated in that order, and an inner outer covering material 4 and an outer outer covering material 6 which cover the periphery of this belt body over the entire circumferential length of the belt, with the core layer 2, inner rubber layer 3, and inner outer covering material 4 forming an inner hexagonal belt portion, and the outer rubber layer 5 and outer outer covering material forming an outer hexagonal belt portion.
[0043] Fig. 6 is a cross-sectional view of the hexagonal belt part of Fig. 5, in which the inner rubber layer and the outer rubber layer have a two-layer structure. That is, in the hexagonal belt part of Fig. 5, the inner rubber layer and the outer rubber layer have a single-layer structure, whereas in the hexagonal belt part of Fig. 6, the inner rubber layer has a two-layer structure of a first inner rubber layer 3a that is laminated on the inner peripheral surface side of the core layer 2 and has a trapezoidal cross section, and a second inner rubber layer 3b that is laminated on the inner rubber layer 3a and has a trapezoidal cross section, and the outer rubber layer has a two-layer structure of a first outer rubber layer 5a that is laminated on the outer peripheral surface side of the core layer 2 and has a trapezoidal cross section, and a second outer rubber layer 5b that is laminated on the outer rubber layer 5a and has a trapezoidal cross section. Except for this, the hexagonal belt part of Fig. 5 is the same as the hexagonal belt part of Fig. 5. By adjusting the inner rubber layer and the outer rubber layer to a two-layer structure with different rubber hardness, the lateral pressure resistance of the belt can be improved.
[0044] Fig. 7 is a cross-sectional view of the hexagonal belt part of the combined hexagonal belt of Fig. 3. The hexagonal belt part shown in Fig. 7 is formed of a core layer 12 formed of an adhesive rubber 12b including a core (core wire) 12a, a reinforcing material 11a covering the side surface of the core layer 12, an inner rubber layer 13 laminated on the inner peripheral surface side of the core layer 12 and having a trapezoidal cross section, an inner reinforcing material 11b covering the inner rubber layer 13, an inner outer covering material 14 covering the inner reinforcing material 11b and including an inner outer covering fabric, an outer rubber layer 15 laminated on the outer peripheral surface side of the core layer 12 and having a trapezoidal cross section, an outer reinforcing material 11c covering the outer rubber layer 15, and an outer outer covering material 16 covering the outer reinforcing material 11c and including an outer outer covering fabric. That is, from the inner circumferential side of the belt, the belt is formed of an endless belt body in which an inner rubber layer 13 covered with an inner reinforcing material 11b, a core layer 12 in which a core 12a is embedded in adhesive rubber 12b, and an outer rubber layer 15 covered with an outer reinforcing material 11c are laminated in this order, and an inner outer covering material 14 and an outer outer covering material 16 which cover the periphery of this belt body over the entire circumferential length of the belt.
[0045] Fig. 8 is a cross-sectional view of a hexagonal belt part in which the inner rubber layer and the outer rubber layer have a two-layer structure in the hexagonal belt part in Fig. 7. That is, while the inner rubber layer and the outer rubber layer have a single-layer structure in the hexagonal belt part in Fig. 7, the hexagonal belt part in Fig. 8 has a two-layer structure in which the inner rubber layer is laminated on the inner peripheral surface side of the core layer 12 and has a trapezoidal cross section, and the second inner rubber layer 13b is laminated on the inner rubber layer 13a and also has a trapezoidal cross section, and the outer rubber layer is laminated on the outer peripheral surface side of the core layer 12 and has a two-layer structure in which the first outer rubber layer 15a is laminated on the outer rubber layer 15a and also has a trapezoidal cross section, except that the hexagonal belt part in Fig. 7 has a two-layer structure in which the outer rubber layer is laminated on the outer peripheral surface side of the core layer 12 and has a trapezoidal cross section, and the second outer rubber layer 15b is laminated on the outer rubber layer 15a and also has a trapezoidal cross section.
[0046] In these examples, the core is a cord (twisted cord) arranged at a predetermined interval in the belt width direction. The core layer is formed of a crosslinked rubber composition (bonded rubber layer) in which the core is embedded, but the core layer may be formed only of a core disposed at the interface between the inner rubber layer and the outer rubber layer. In the present application, when the core layer is formed only of a core, the core disposed at an interval in the belt body is referred to as the core layer, and such a core layer includes not only a form in which the core is disposed at the interface between the inner rubber layer and the outer rubber layer, but also a form in which a part or all of the core disposed at the interface between the inner rubber layer and the outer rubber layer is embedded in the inner rubber layer or the outer rubber layer during the manufacturing process.
[0047] (Inner and outer rubber layers) The inner rubber layer is a rubber layer disposed radially inward (inner periphery of the belt) of the core layer in the annular hexagonal belt portion, and the outer rubber layer is a rubber layer disposed radially outward (outer periphery of the belt) of the core layer. The inner rubber layer and the outer rubber layer each extend in the circumferential direction (have the same length as the hexagonal belt portion), and have a substantially trapezoidal cross section perpendicular to the belt longitudinal direction.
[0048] The outer rubber layer and the inner rubber layer constituting each hexagonal belt portion may be a single layer (one layer) as shown in Figs. 5 and 7, or may be a laminated structure including two types of rubber layers as shown in Figs. 6 and 8, in which the rubber hardness and strength of each layer are adjusted.
[0049] Among these, from the viewpoint of achieving both lateral pressure resistance and flexibility, the hexagonal belt portion is preferably configured such that the inner rubber layer has a laminated structure of two or more layers including a first inner rubber layer laminated on the core layer side and a second inner rubber layer laminated on the inner circumferential side of the belt, the rubber hardness of which is lower than that of the first inner rubber layer. Also, the hexagonal belt portion is preferably configured such that the outer rubber layer has a laminated structure of two or more layers including a first outer rubber layer laminated on the core layer side and a second outer rubber layer laminated on the outer circumferential side of the belt, the rubber hardness of which is lower than that of the first outer rubber layer. Note that, with regard to the laminated structure, the inner rubber layer and the outer rubber layer do not need to be configured in the same manner, and may be combined from these modes as necessary.
[0050] Considering the balance between lateral pressure resistance and productivity, it is particularly preferable that the inner rubber layer has a two-layer structure (first inner rubber layer and second inner rubber layer) and the outer rubber layer has a single-layer structure or a two-layer structure (first outer rubber layer and second outer rubber layer).
[0051] In the case of a single-layer structure, the rubber hardness Hs of each of the inner rubber layer and the outer rubber layer can be selected, for example, from the range of about 60 to 90°, and is preferably 72 to 80°, more preferably 73 to 78°, even more preferably 74 to 78°, and most preferably 75 to 77°. If the rubber hardness is too low, there is a risk of reduced lateral pressure resistance, and conversely, if it is too high, there is a risk of reduced flexibility.
[0052] In this application, the rubber hardness of each rubber layer indicates a value Hs (Type A) measured using a Type A durometer in accordance with the spring type durometer hardness test specified in JIS K6253 (2012) (Vulcanized rubber and thermoplastic rubber - Determination of hardness) and may be simply referred to as rubber hardness. In detail, it can be measured by the method described in the examples below.
[0053] The tensile strength of the inner rubber layer and the outer rubber layer in the belt width direction is, for example, 12 to 20 MPa, preferably 13 to 18 MPa, and more preferably 14 to 17 MPa. If the tensile strength is too small, the lateral pressure resistance may decrease, and conversely, if it is too large, the flexibility may decrease.
[0054] In the present application, the tensile strength of each rubber layer is measured by a method conforming to JIS K6251 (2017) and the value of the tensile strength T of each rubber layer is used as an index value of the tensile strength. In detail, the tensile strength can be measured by the method described in the examples described later.
[0055] In order to improve the lateral pressure resistance, when the two-layer structure is used, it is preferable that the first inner rubber layer and the first outer rubber layer arranged on the core layer side are high hardness rubber layers. The rubber hardness Hs of the first inner rubber layer and the first outer rubber layer can be selected from the range of about 80 to 100°, for example, and is preferably 85 to 95°, more preferably 87 to 94°, even more preferably 90 to 93°, and most preferably 92 to 93°. If the rubber hardness is too low, the lateral pressure resistance may decrease, and conversely, if it is too high, the fit with the pulley groove and the flexibility may decrease.
[0056] On the other hand, the rubber hardness Hs of the second inner rubber layer and the second outer rubber layer may be approximately the same as the rubber hardness Hs shown in the above-mentioned case of the single-layer structure.
[0057] Furthermore, the difference in rubber hardness Hs between the first inner rubber layer and the second inner rubber layer (rubber hardness of the first inner rubber layer - rubber hardness of the second inner rubber layer) may be, for example, 1° or more (particularly 5° or more), and is preferably 5 to 30° (e.g. 7 to 27°), more preferably 10 to 25° (e.g. 12 to 20°), even more preferably 14 to 20° (e.g. 15 to 19°), and most preferably 14 to 17° (particularly 15 to 17°). If the difference in rubber hardness between the second inner rubber layer and the first inner rubber layer is too small, there is a risk of reduced flexibility.
[0058] The difference in rubber hardness Hs between the first outer rubber layer and the second outer rubber layer can be selected from the same range as the difference in rubber hardness Hs between the first inner rubber layer and the second inner rubber layer, including the preferred range.
[0059] The tensile strength of the first inner rubber layer in the belt width direction is, for example, 25 to 50 MPa, preferably 25 to 40 MPa, more preferably 26 to 35 MPa, and most preferably 28 to 32 MPa. If the tensile strength is too small, the lateral pressure resistance may decrease, and conversely, if it is too large, the flexibility may decrease. The tensile strength of the second inner rubber layer may be approximately the same as the tensile strength shown in the case of the single layer structure described above.
[0060] The tensile strengths of the first outer rubber layer and the second outer rubber layer can be selected from the same ranges, including preferred ranges, as the tensile strengths of the first inner rubber layer and the second inner rubber layer, respectively.
[0061] The average thickness of the entire inner rubber layer and the average thickness of the entire outer rubber layer are, for example, 1 to 12 mm, preferably 2 to 10 mm, further preferably 2.5 to 9 mm, and further preferably 3 to 8 mm, respectively.
[0062] The average thickness of the first inner rubber layer can be selected from the range of about 95 to 30% of the average thickness of the entire inner rubber layer, and is preferably 90 to 50%, more preferably 85 to 55%, even more preferably 80 to 60%, and most preferably 75 to 70%. This ratio may be the ratio when the inner rubber layer is composed of only the first inner rubber layer and the second inner rubber layer (two-layer structure). If the thickness ratio of the first inner rubber layer is too small, there is a risk of reduced lateral pressure resistance, and conversely, if it is too large, there is a risk of reduced flexibility.
[0063] The ratio of the first outer rubber layer to the average thickness of the entire outer rubber layers can be selected from the same range as the ratio of the first inner rubber layer to the average thickness of the entire inner rubber layers, including the preferred range.
[0064] The inner rubber layer may further include other rubber layers having different rubber hardness in addition to the first inner rubber layer and the second inner rubber layer. The other rubber layers may be a single layer or multiple layers. The other rubber layers may be laminated on either the upper or lower surfaces of the first inner rubber layer or the lower surface of the second inner rubber layer. The average thickness of the other rubber layers may be, for example, 30% or less, preferably 10% or less, and more preferably 5% or less, of the average thickness of the entire inner rubber layer. That is, it is preferable that the inner rubber layer includes the first inner rubber layer and the second inner rubber layer as main layers, and the average thickness of the total of the first inner rubber layer and the second inner rubber layer may be, for example, 70% or more, preferably 90% or more, and more preferably 95% or more, of the average thickness of the entire inner rubber layer, and it is particularly preferable that the inner rubber layer is composed of only the first inner rubber layer and the second inner rubber layer.
[0065] The outer rubber layer may further include other rubber layers having different rubber hardness in addition to the first outer rubber layer and the second outer rubber layer. The other rubber layers may be a single layer or multiple layers. The other rubber layers may be laminated on either the upper or lower surfaces of the first outer rubber layer or the lower surface of the second outer rubber layer. The average thickness of the other rubber layers may be, for example, 30% or less, preferably 10% or less, and more preferably 5% or less, of the average thickness of the entire outer rubber layer. That is, it is preferable that the outer rubber layer includes the first outer rubber layer alone as a main layer, or includes a combination of the first outer rubber layer and the second outer rubber layer as a main layer, and the average thickness of the total of the first outer rubber layer and the second outer rubber layer may be, for example, 70% or more, preferably 90% or more, and more preferably 95% or more, of the average thickness of the entire outer rubber layer. It is particularly preferable that the outer rubber layer is composed of only the first outer rubber layer alone, or only the combination of the first inner rubber layer and the second inner rubber layer.
[0066] The inner rubber layer and the outer rubber layer may each be formed of a crosslinked rubber composition commonly used as a rubber composition for a hexagonal belt. The crosslinked rubber composition may be a crosslinked rubber composition containing a rubber component, and by appropriately adjusting the composition of the composition, it is possible to adjust the rubber hardness of each layer constituting the inner rubber layer and the outer rubber layer, particularly the rubber hardness of the first inner rubber layer and the second inner rubber layer, and the rubber hardness of the first outer rubber layer and the second outer rubber layer. The method of adjusting the rubber hardness, etc. is not particularly limited, and may be adjusted by changing the composition and / or type of the components constituting the composition, and from the viewpoint of simplicity, etc., it is preferable to adjust by changing the ratio and / or type of short fiber or filler.
[0067] (A) Rubber component The rubber component contained in the crosslinked rubber composition of the inner rubber layer and the outer rubber layer can be selected from known vulcanizable or crosslinkable rubbers and / or elastomers, such as diene rubbers [natural rubber, isoprene rubber, butadiene rubber, chloroprene rubber (CR), styrene butadiene rubber (SBR), vinylpyridine-styrene-butadiene copolymer rubber, acrylonitrile butadiene rubber (nitrile rubber); hydrogenated products of the diene rubbers such as hydrogenated nitrile rubber (including a mixed polymer of hydrogenated nitrile rubber and an unsaturated carboxylic acid metal salt)], olefin rubbers [e.g., ethylene-α-olefin rubbers (ethylene-α-olefin elastomers), polyoctenylene rubbers, ethylene-vinyl acetate copolymer rubbers, chlorosulfonated polyethylene rubbers, alkylated chlorosulfonated polyethylene rubbers], epichlorohydrin rubbers, acrylic rubbers, silicone rubbers, urethane rubbers, fluororubbers, etc. These rubber components can be used alone or in combination of two or more.
[0068] Among these, ethylene-α-olefin elastomers [ethylene-α-olefin rubbers such as ethylene-propylene copolymer (EPM) and ethylene-propylene-diene terpolymer (EPDM)] and chloroprene rubber are widely used because crosslinking agents and crosslinking accelerators are easily diffused, and chloroprene rubber and EPDM are preferred because they are excellent in balance of mechanical strength, weather resistance, heat resistance, cold resistance, oil resistance, adhesiveness, etc., particularly when used in a high-load environment. Furthermore, chloroprene rubber is particularly preferred because it is excellent in abrasion resistance in addition to the above characteristics. The chloroprene rubber may be a sulfur-modified type or a non-sulfur-modified type.
[0069] When the rubber component contains chloroprene rubber, the proportion of the chloroprene rubber in the rubber component may be, for example, 50 mass % or more (particularly about 80 to 100 mass %), and 100 mass % (only chloroprene rubber) is particularly preferred.
[0070] (B) Short Fiber The crosslinked rubber composition may further contain short fibers in addition to the rubber component. Examples of the short fibers include polyolefin fibers (e.g., polyethylene fibers, polypropylene fibers, etc.), polyamide fibers (e.g., polyamide 6 fibers, polyamide 66 fibers, polyamide 46 fibers, aramid fibers, etc.), polyalkylene arylate fibers [e.g., polyethylene terephthalate (PET) fibers, polytrimethylene terephthalate (PTT) fibers, polybutylene terephthalate (PBT) fibers, polyethylene naphthalate (PEN) fibers, etc.] 2-4 Alkylene C 8-14 Examples of the short fibers include synthetic fibers such as arylate fibers, vinylon fibers, polyvinyl alcohol fibers, and polyparaphenylene benzobisoxazole (PBO) fibers; natural fibers such as cotton, hemp, and wool; and inorganic fibers such as carbon fibers. These short fibers can be used alone or in combination of two or more.
[0071] Among these short fibers, synthetic and natural fibers, especially C fibers such as ethylene terephthalate and ethylene-2,6-naphthalate, 2-4 Alkylene C8-14 Synthetic fibers such as polyester fibers (polyalkylene arylate fibers) and polyamide fibers (aramid fibers, etc.) whose main constituent unit is arylate, and inorganic fibers such as carbon fibers are widely used, and among them, fibers that are rigid and have high strength and modulus, such as polyester fibers (particularly polyethylene terephthalate fibers and polyethylene naphthalate fibers) and polyamide fibers (particularly aramid fibers), are preferred. Aramid fibers also have high abrasion resistance. Therefore, the short fibers preferably contain at least fully aromatic polyamide fibers such as aramid fibers. The aramid fibers may be commercially available products such as those under the trade names "Conex", "Nomex", "Kevlar", "Technora", and "Twaron (registered trademark)".
[0072] The average fiber diameter of the short fibers is, for example, 2 μm or more, preferably 2 to 100 μm, more preferably 3 to 50 μm (e.g., 5 to 50 μm), more preferably 7 to 40 μm, and most preferably 10 to 30 μm. The average length of the short fibers is, for example, 1 to 20 mm, preferably 1.5 to 10 mm, more preferably 2 to 5 mm, and more preferably 2.5 to 4 mm.
[0073] From the viewpoint of dispersibility and adhesiveness of the short fibers in the crosslinked rubber composition, the short fibers may be subjected to an adhesion treatment (or surface treatment) by a conventional method. Examples of the surface treatment method include a method of treating with a treatment liquid containing a conventional surface treatment agent. Examples of the surface treatment agent include an RFL liquid containing resorcin (R), formaldehyde (F), and rubber or latex (L) [for example, an RFL liquid in which resorcin (R) and formaldehyde (F) form a condensate (RF condensate), and the rubber or latex contains, for example, vinylpyridine-styrene-butadiene copolymer rubber], an epoxy compound, a polyisocyanate compound, a silane coupling agent, a crosslinked rubber composition (for example, a crosslinked rubber composition containing wet-process white carbon containing hydrated silica as a main component, which contains surface silanol groups and is advantageous for increasing the chemical bonding strength with rubber, etc.). These surface treatment agents may be used alone or in combination of two or more types, and the short fibers may be treated multiple times with the same or different surface treatment agents.
[0074] The short fibers may be embedded in the inner rubber layer and the outer rubber layer while being oriented in the width direction of the belt in order to suppress compressive deformation of the belt due to pressure from the pulleys.
[0075] The proportion of the short fibers can be selected from a range of about 50 parts by mass or less per 100 parts by mass of the rubber component, for example, 30 parts by mass or less, and preferably 10 to 30 parts by mass. If the proportion of the short fibers is too low, the rubber hardness of the inner rubber layer and the outer rubber layer may decrease, whereas if the proportion is too high, the rubber hardness may be too high, resulting in reduced flexibility.
[0076] When the outer rubber layer and the inner rubber layer have a two-layer structure, the proportion of the short fibers in the first inner rubber layer and the first outer rubber layer is, for example, 5 to 50 parts by mass, preferably 10 to 30 parts by mass, more preferably 15 to 25 parts by mass, and more preferably 18 to 22 parts by mass, per 100 parts by mass of the rubber component (first rubber component).The proportion of the short fibers in the second inner rubber layer and the second outer rubber layer is, for example, 30 parts by mass or less, preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the rubber component (second rubber component).
[0077] (C) Filler The crosslinked rubber composition may further contain a filler in addition to the rubber component. Examples of the filler include carbon black, silica, clay, calcium carbonate, talc, and mica. The filler often contains a reinforcing filler, and such a reinforcing filler may be carbon black, reinforcing silica, or the like. Note that the reinforcing property of silica is usually smaller than that of carbon black. These fillers may be used alone or in combination of two or more kinds. In the present disclosure, in order to improve lateral pressure resistance, it is preferable to contain a reinforcing filler, and it is particularly preferable to contain carbon black.
[0078] The average particle size (number average primary particle size) of carbon black is, for example, 5 to 200 nm, preferably 10 to 150 nm, and more preferably 15 to 100 nm. In terms of high reinforcing effect, the carbon black may be small in particle size, for example, 5 to 38 nm, preferably 10 to 35 nm, and more preferably 15 to 30 nm. Examples of small particle size carbon black include SAF, ISAF-HM, ISAF-LM, HAF-LS, HAF, and HAF-HS. These carbon blacks can be used alone or in combination of two or more.
[0079] The proportion of the filler (particularly carbon black) relative to 100 parts by mass of the rubber component is, for example, 10 to 100 parts by mass, preferably 12 to 80 parts by mass, further preferably 15 to 70 parts by mass, and further preferably 20 to 60 parts by mass.
[0080] When the outer rubber layer and the inner rubber layer have a two-layer structure, the ratio of the filler (particularly, carbon black) in the first inner rubber layer and the first outer rubber layer is, for example, 10 to 100 parts by mass, preferably 20 to 80 parts by mass, more preferably 30 to 70 parts by mass, and more preferably 40 to 60 parts by mass, per 100 parts by mass of the rubber component (first rubber component).The ratio of the filler (particularly, carbon black) in the second inner rubber layer and the second outer rubber layer is, for example, 5 to 80 parts by mass, preferably 10 to 60 parts by mass, more preferably 15 to 50 parts by mass, and more preferably 20 to 40 parts by mass, per 100 parts by mass of the rubber component (second rubber component).
[0081] The proportion of carbon black relative to the total filler may be, for example, 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, or may be 100% by mass. If the proportion of carbon black relative to the total filler is too low, the rubber hardness of the inner rubber layer and the outer rubber layer may decrease.
[0082] (D) Other Additives The crosslinked rubber composition may contain, as necessary, a crosslinking agent (or vulcanizing agent), a co-crosslinking agent (crosslinking assistant), a crosslinking accelerator, a crosslinking retarder, a metal oxide (calcium oxide, barium oxide, iron oxide, copper oxide, titanium oxide, aluminum oxide, etc.), a softener (oils such as paraffin oil and naphthenic oil), a processing agent or processing assistant (for example, fatty acid such as stearic acid, fatty acid metal salt such as stearate metal salt, fatty acid amide such as stearic acid amide, wax, paraffin, etc.), an adhesion improver [for example, resorcinol-formaldehyde cocondensate (RF condensate), amino resin (condensate of nitrogen-containing cyclic compound and formaldehyde, for example, melamine such as hexamethylol melamine, hexaalkoxymethyl melamine (hexamethoxymethyl melamine, hexabutoxymethyl melamine, etc.)], Resins, urea resins such as methylol urea, benzoguanamine resins such as methylol benzoguanamine resins, co-condensates thereof (resorcin-melamine-formaldehyde co-condensates, etc.), antioxidants (antioxidants, heat aging inhibitors, flex crack inhibitors, ozone degradation inhibitors, etc.), plasticizers [aliphatic carboxylic acid ester plasticizers (adipic acid ester plasticizers, sebacic acid ester plasticizers, etc.), aromatic carboxylic acid ester plasticizers (phthalic acid ester plasticizers, trimellitic acid ester plasticizers, etc.), oxycarboxylic acid ester plasticizers, phosphate ester plasticizers, ether plasticizers, ether ester plasticizers, etc.], colorants, tackifiers, lubricants, coupling agents (silane coupling agents, etc.), stabilizers (ultraviolet ray absorbers, heat stabilizers, etc.), flame retardants, antistatic agents, etc. may be included. The metal oxide may act as a crosslinking agent. In the adhesion improver, the resorcinol-formaldehyde cocondensate and the amino resin may be an initial condensate (prepolymer) of resorcinol and / or a nitrogen-containing cyclic compound (such as melamine) with formaldehyde.
[0083] As the crosslinking agent, a conventional component can be used depending on the type of rubber component, and examples thereof include metal oxides (magnesium oxide, zinc oxide, lead oxide, etc.), organic peroxides (diacyl peroxide, peroxy ester, dialkyl peroxide, etc.), and sulfur-based crosslinking agents. Examples of sulfur-based crosslinking agents include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, and sulfur chlorides (sulfur monochloride, sulfur dichloride, etc.). These crosslinking agents can be used alone or in combination of two or more. When the rubber component is chloroprene rubber, metal oxides (magnesium oxide, zinc oxide, etc.) may be used as the crosslinking agent. The metal oxides may be used in combination with other crosslinking agents (sulfur-based crosslinking agents, etc.), and the metal oxides and / or sulfur-based crosslinking agents may be used alone or in combination with a crosslinking accelerator.
[0084] The ratio of the crosslinking agent can be selected from the range of, for example, about 1 to 20 parts by mass relative to 100 parts by mass of the rubber component, calculated as solid content, depending on the type of crosslinking agent and rubber component. For example, the ratio of the metal oxide as the crosslinking agent is, for example, 1 to 20 parts by mass, preferably 3 to 17 parts by mass, more preferably 5 to 15 parts by mass, and more preferably 7 to 13 parts by mass, relative to 100 parts by mass of the rubber component. When the metal oxide as the crosslinking agent is combined with a sulfur-based crosslinking agent, the ratio of the sulfur-based crosslinking agent is, for example, 0.1 to 50 parts by mass, preferably 1 to 30 parts by mass, and more preferably about 3 to 10 parts by mass, relative to 100 parts by mass of the metal oxide. The ratio of the organic peroxide is, for example, 1 to 8 parts by mass, preferably 1.5 to 5 parts by mass, and more preferably 2 to 4.5 parts by mass, relative to 100 parts by mass of the rubber component.
[0085] Examples of the co-crosslinking agent (crosslinking aid or co-vulcanizing agent) include known crosslinking aids, such as polyfunctional (iso)cyanurates [e.g., triallyl isocyanurate (TAIC), triallyl cyanurate (TAC), etc.], polydiene (e.g., 1,2-polybutadiene, etc.), metal salts of unsaturated carboxylic acids [e.g., (meth)acrylic acid polyvalent metal salts such as zinc (meth)acrylate and magnesium (meth)acrylate], oximes (e.g., quinone dioxime, etc.), guanidines (e.g., diphenyl guanidine, etc.), polyfunctional (meth)acrylates [e.g., alkanediol di(meth)acrylate such as ethylene glycol di(meth)acrylate and butanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetraacetate, etc., alkane polyol poly(meth)acrylates such as cyclohexyl (meth)acrylate, bismaleimides (aliphatic bismaleimides such as alkylene bismaleimides such as N,N'-1,2-ethylene dimaleimide, N,N'-hexamethylene bismaleimide, 1,6'-bismaleimide-(2,2,4-trimethyl)cyclohexane; arene bismaleimides or aromatic bismaleimides such as N,N'-m-phenylene dimaleimide, 4-methyl-1,3-phenylene dimaleimide, 4,4'-diphenylmethane dimaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, 4,4'-diphenylether dimaleimide, 4,4'-diphenylsulfone dimaleimide, 1,3-bis(3-maleimidophenoxy)benzene, etc.). These crosslinking aids can be used alone or in combination of two or more. Among these crosslinking aids, polyfunctional (iso)cyanurates, polyfunctional (meth)acrylates, and bismaleimides (arene bismaleimides such as N,N'-m-phenylenedimaleimide or aromatic bismaleimides) are preferred, and bismaleimides are often used. The addition of a crosslinking aid (e.g., bismaleimides) can increase the degree of crosslinking and prevent adhesion wear and the like.
[0086] The proportion of the co-crosslinking agent (crosslinking assistant) such as bismaleimides, calculated as solid content, relative to 100 parts by mass of the rubber component is, for example, 0.1 to 10 parts by mass, preferably 0.5 to 8 parts by mass, more preferably 1 to 5 parts by mass, and even more preferably 2 to 4 parts by mass.
[0087] Examples of crosslinking accelerators (vulcanization accelerators) include thiuram accelerators [e.g., tetramethylthiuram monosulfide (TMTM), tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), tetrabutylthiuram disulfide (TBTD), dipentamethylenethiuram tetrasulfide (DPTT), N,N'-dimethyl-N,N'-diphenylthiuram disulfide, etc.], thiazole accelerators [e.g., 2-mercaptobenzothiazole, submersible 2-mercaptobenzothiazole, etc.], Lead salts, 2-mercaptothiazoline, dibenzothiazyl disulfide, 2-(4'-morpholinodithio)benzothiazole, etc., sulfenamide accelerators [e.g., N-cyclohexyl-2-benzothiazylsulfenamide (CBS), N,N'-dicyclohexyl-2-benzothiazylsulfenamide, etc.], guanidines (diphenylguanidine, di-o-tolylguanidine, etc.), urea or thiourea accelerators (e.g., ethylenethiourea, etc.), dithiocarbamates, xanthogenates, etc. These crosslinking accelerators can be used alone or in combination. Among these crosslinking accelerators, TMTD, DPTT, CBS, etc. are commonly used.
[0088] The proportion of the crosslinking accelerator, calculated as solid content, may be 15 parts by mass or less (e.g., 0 to 15 parts by mass) relative to 100 parts by mass of the rubber component, and is, for example, 0.1 to 10 parts by mass, preferably 0.2 to 5 parts by mass, further preferably 0.3 to 3 parts by mass, and further preferably 0.5 to 1.5 parts by mass.
[0089] The proportion of the softener (oils such as naphthenic oils) may be 30 parts by mass or less (e.g., 0 to 30 parts by mass) per 100 parts by mass of the rubber component, calculated as solid content, and is, for example, 1 to 30 parts by mass, preferably 3 to 20 parts by mass, and more preferably 3 to 10 parts by mass.
[0090] When the outer rubber layer and the inner rubber layer have a two-layer structure, the ratio of the softener in the first inner rubber layer and the first outer rubber layer is, for example, 1 to 30 parts by mass, preferably 3 to 20 parts by mass, and more preferably 3 to 10 parts by mass, per 100 parts by mass of the rubber component (first rubber component).The ratio of the softener in the second inner rubber layer and the second outer rubber layer is, for example, 20 parts by mass or less, preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, per 100 parts by mass of the rubber component (second rubber component).
[0091] The proportion of the processing agent or processing aid (such as stearic acid) may be 10 parts by mass or less (e.g., 0 to 10 parts by mass) per 100 parts by mass of the rubber component, calculated as solid content, and is, for example, 0.1 to 5 parts by mass, preferably 0.5 to 3 parts by mass, and more preferably 1 to 3 parts by mass.
[0092] The proportion of the antioxidant, calculated as solid content, relative to 100 parts by mass of the rubber component is, for example, 0.5 to 15 parts by mass, preferably 1 to 10 parts by mass, further preferably 2.5 to 7.5 parts by mass, and further preferably 3 to 7 parts by mass.
[0093] The proportion of the plasticizer, calculated as solid content, may be 30 parts by mass or less (e.g., 0 to 30 parts by mass) per 100 parts by mass of the rubber component, for example, 0.5 to 20 parts by mass, preferably 1 to 10 parts by mass, and more preferably 3 to 7 parts by mass.
[0094] When the outer rubber layer and the inner rubber layer have a two-layer structure, the ratio of the plasticizer in the first inner rubber layer and the first outer rubber layer is, for example, 20 parts by mass or less, preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, per 100 parts by mass of the rubber component (first rubber component).The ratio of the plasticizer in the second inner rubber layer and the second outer rubber layer is, for example, 1 to 30 parts by mass, preferably 3 to 20 parts by mass, and more preferably 3 to 10 parts by mass, per 100 parts by mass of the rubber component (second rubber component).
[0095] (Core layer) The core layer may contain a core, and may be a core layer formed only of a core as described above, but is preferably a core layer (adhesive rubber layer) formed of a crosslinked rubber composition in which a core is embedded, from the viewpoint of suppressing interlayer peeling and improving belt durability. A core layer formed of a crosslinked rubber composition in which a core is embedded is usually called an adhesive rubber layer, and an adhesive rubber layer in which a core may be embedded in a layer formed of a crosslinked rubber composition containing a rubber component is preferably interposed between the inner rubber layer and the outer rubber layer to bond the inner rubber layer and the outer rubber layer, and the core is preferably embedded in the adhesive rubber layer.
[0096] The average thickness of the core layer (particularly the adhesive rubber layer) is, for example, 0.2 to 5 mm, preferably 0.3 to 4 mm, further preferably 0.5 to 3.5 mm, further preferably 0.8 to 3 mm, and most preferably 1 to 2.5 mm.
[0097] (A) Crosslinked Rubber Composition The rubber hardness Hs of the crosslinked rubber composition forming the core layer (particularly the adhesive rubber layer) is, for example, 72 to 80°, preferably 73 to 78°, and more preferably 75 to 77°. If the rubber hardness is too low, there is a risk that the resistance to lateral pressure will decrease, whereas if the rubber hardness is too high, the crosslinked rubber composition around the core will become rigid, making it difficult for the core to bend, and this will cause heat deterioration (cracks) of the core layer, bending fatigue of the core, and the like, which may result in the core peeling off.
[0098] The tensile strength of the crosslinked rubber composition forming the core layer (particularly the adhesive rubber layer) in the belt width direction is, for example, 12 to 20 MPa, preferably 13 to 18 MPa, and more preferably 14 to 17 MPa. If the tensile strength is too small, the lateral pressure resistance may decrease, whereas if it is too large, the flexibility may decrease.
[0099] As the rubber component (A1) constituting the crosslinked rubber composition forming the core layer, the rubber components exemplified as the rubber component (A) of the inner rubber layer and the outer rubber layer can be used, and preferred embodiments can be selected from the preferred embodiments of the rubber component (A).
[0100] The crosslinked rubber composition of the core layer may further contain a filler (A2) in addition to the rubber component (A1). As the filler (A2), the fillers exemplified as the filler (C) of the inner rubber layer and the outer rubber layer can be used. Among the above fillers, carbon black and reinforcing silica are preferred, and a combination of carbon black and reinforcing silica is particularly preferred.
[0101] In the core layer, the proportion of the filler (A2) is, for example, 1 to 100 parts by mass, preferably 10 to 80 parts by mass, more preferably 30 to 70 parts by mass, and more preferably 40 to 60 parts by mass, relative to 100 parts by mass of the rubber component (A1). When carbon black and reinforcing silica are combined, the proportion of the reinforcing silica is, for example, 10 to 200 parts by mass, preferably 30 to 100 parts by mass, and more preferably 50 to 80 parts by mass, relative to 100 parts by mass of the carbon black.
[0102] The crosslinked rubber composition of the core layer may further contain other additives (A3) in addition to the rubber component (A1). The other additives (A3) may be the additives exemplified as the other additives (D) of the inner rubber layer and the outer rubber layer, and crosslinking agents, crosslinking accelerators, processing agents or processing aids, plasticizers, antiaging agents, etc. are preferably used. The proportion of the other additives (A3) may be selected from the same range as the additives (D) of the inner rubber layer and the outer rubber layer, including the preferred range.
[0103] (B) Core body The cores contained in the core layer are not particularly limited, but are usually core wires (twisted cords) arranged at a predetermined interval in the belt width direction. The core wires are arranged extending in the longitudinal direction of the belt, and may be arranged extending in parallel with the longitudinal direction of the belt at a predetermined pitch. However, from the viewpoint of productivity, they are usually arranged in a spiral shape extending in parallel with the longitudinal direction of the belt at a predetermined pitch. When arranged in a spiral shape, the angle of the core wire with respect to the longitudinal direction of the belt may be, for example, 5° or less, and from the viewpoint of belt running properties, the closer to 0° the better. In addition, the pitch or interval (particularly the spinning pitch of the core wire), which is the distance between the centers of adjacent cores, is preferably set in the range of 1.0 to 3.6 mm, more preferably set in the range of 1.2 to 3 mm, and even more preferably set in the range of 1.4 to 2.4 mm.
[0104] When the core is embedded in the adhesive rubber constituting the core layer, it is sufficient that a part of the core is embedded in the adhesive rubber, and from the viewpoint of improving durability, a form in which the core is not exposed on the surface of the core layer (a form in which the entire core is completely embedded in the adhesive rubber) is preferred.
[0105] Examples of fibers constituting the core wire include polyolefin fibers (polyethylene fibers, polypropylene fibers, etc.), polyamide fibers [aliphatic polyamide fibers (nylon fibers) such as polyamide 6 fibers, polyamide 66 fibers, and polyamide 46 fibers, and aramid fibers, etc.], polyester fibers (polyalkylene arylate fibers) [polyethylene terephthalate (PET) fibers, polyethylene naphthalate (PEN) fibers, and other poly-C fibers], 2-4 Alkylene-C 8-14 Commonly used fibers include synthetic fibers such as arylate fibers, vinylon fibers, polyvinyl alcohol fibers, and polyparaphenylene benzobisoxazole (PBO) fibers; natural fibers such as cotton, hemp, and wool; and inorganic fibers such as carbon fibers. These fibers can be used alone or in combination of two or more.
[0106] Among these fibers, ethylene terephthalate, ethylene-2,6-naphthalate, and other C fibers are preferred due to their high modulus. 2-4 Alkylene-C 8-14 Synthetic fibers such as polyester fibers (polyalkylene arylate fibers) having arylate as the main structural unit, polyamide fibers (aramid fibers, etc.), and inorganic fibers such as carbon fibers are commonly used, with polyester fibers (particularly polyethylene terephthalate fibers and polyethylene naphthalate fibers) and polyamide fibers (particularly aramid fibers) being preferred.
[0107] The fiber may be in the form of a multifilament yarn. The fineness of the multifilament yarn may be, for example, 2000 to 10000 denier (particularly, 4000 to 8000 denier). The multifilament yarn may contain, for example, about 100 to 5000 filaments, preferably 500 to 4000 filaments, and more preferably 1000 to 3000 filaments.
[0108] The core wire may generally be a twisted cord (e.g., multiple twist, single twist, Lang twist, etc.) using multifilament yarn. The average diameter of the core wire (fiber diameter of the twisted cord) may be, for example, 0.5 to 3 mm, preferably 0.6 to 2.5 mm, more preferably 0.7 to 2 mm, and even more preferably 1.1 to 2 mm.
[0109] When the core wire is embedded in the adhesive rubber, the core wire may be surface-treated to improve adhesion to the crosslinked rubber composition that forms the adhesive rubber. Examples of the surface treatment agent include those exemplified as the surface treatment agents for the short fibers (B) of the inner rubber layer and the outer rubber layer. The surface treatment agents may be used alone or in combination of two or more, and the core wire may be treated successively a plurality of times with the same or different surface treatment agents. It is preferable to perform the adhesion treatment on the core wire with at least an RFL liquid.
[0110] (Inner and outer covering materials) The inner and outer covering materials include an inner and outer covering fabric, respectively. The inner and outer covering fabrics (cover fabrics) are each formed of a conventional fabric (A). Examples of the fabric (A) include woven fabrics, knitted fabrics (weft knitted fabrics, warp knitted fabrics), nonwoven fabrics, and other fabric materials. Among these, woven fabrics woven in the form of plain weave, twill weave, satin weave, and other forms, woven fabrics woven at a wide angle of more than 90° and less than 120° between the warp and weft, knitted fabrics, and other fabrics are preferred, and woven fabrics commonly used as cover fabrics for transmission belts for general industry and agricultural machinery [plain weave fabrics in which the warp and weft cross at a right angle, and plain weave fabrics (wide-angle canvas) in which the warp and weft cross at a wide angle of more than 90° and less than 120°] are particularly preferred. Furthermore, in applications requiring durability, wide-angle canvas may be used.
[0111] Examples of fibers constituting the fabric (A) include synthetic fibers such as polyolefin fibers (polyethylene fibers, polypropylene fibers, etc.), polyamide fibers (polyamide 6 fibers, polyamide 66 fibers, polyamide 46 fibers, aramid fibers, etc.), polyester fibers (polyalkylene arylate fibers, etc.), vinyl alcohol fibers (polyvinyl alcohol fibers, ethylene-vinyl alcohol copolymer fibers, vinylon fibers, etc.), and polyparaphenylene benzobisoxazole (PBO) fibers; natural fibers such as cellulose fibers (cellulose fibers, cellulose derivative fibers, etc.), and wool; and inorganic fibers such as carbon fibers. These fibers may be used alone as a single yarn, or may be used as a blended yarn in which two or more types are combined.
[0112] Among these fibers, a blended yarn of polyester-based fibers and cellulosic fibers is preferred from the viewpoints of excellent mechanical properties and economic efficiency.
[0113] The polyester fiber may be a polyalkylene arylate fiber. Examples of the polyalkylene arylate fiber include poly(C) fibers such as polyethylene terephthalate (PET) fibers and polyethylene naphthalate (PEN) fibers. 2-4 Alkylene-C 8-14 Examples include arylate fibers.
[0114] The cellulose-based fibers include cellulose fibers (cellulose fibers derived from plants, animals, bacteria, etc.) and fibers of cellulose derivatives. Examples of cellulose fibers include cellulose fibers (pulp fibers) derived from natural plants such as wood pulp (coniferous and broadleaf pulp, etc.), bamboo fibers, sugarcane fibers, seed hair fibers (cotton fibers (cotton linters), kapok, etc.), ginseng bark fibers (hemp, paper mulberry, Mitsumata, etc.), and leaf fibers (Manila hemp, New Zealand hemp, etc.); cellulose fibers derived from animals such as sea squirt cellulose; bacterial cellulose fibers; algae cellulose, etc. Examples of fibers of cellulose derivatives include cellulose ester fibers; regenerated cellulose fibers (rayon, cupra, lyocell, etc.); and the like.
[0115] The mass ratio of the polyester fibers to the cellulosic fibers is, for example, the former / the latter=90 / 10 to 10 / 90, preferably 80 / 20 to 20 / 80, more preferably 70 / 30 to 30 / 70, and even more preferably 60 / 40 to 40 / 60.
[0116] The average fineness of the fibers constituting the fabric (A) is, for example, 5 to 30 count, preferably 10 to 25 count, and more preferably 10 to 20 count.
[0117] The basis weight of the fabric (raw fabric) (A) is, for example, 100 to 500 g / m 2 , preferably 200 to 400 g / m 2 , and more preferably 250 to 350 g / m 2 It is.
[0118] When the fabric (raw fabric) (A) is a woven fabric, the thread density (density of warp and weft threads) of the fabric is, for example, 60 to 100 threads / 50 mm, preferably 70 to 90 threads / 50 mm, and more preferably 75 to 85 threads / 50 mm.
[0119] The inner and outer covering fabrics may each be a single layer or multiple layers (e.g., 2 to 5 layers, preferably 2 to 4 layers, and more preferably 2 to 3 layers), but from the standpoint of productivity, a single layer (1 ply) or two layers (2 plies) is preferred.
[0120] In order to improve adhesion to the belt body (inner rubber layer and outer rubber layer) or the reinforcing material described later, the inner and outer covering materials may further contain a crosslinked rubber composition as a rubber component in addition to the inner and outer covering fabrics, respectively. The rubber component may permeate the inner and outer covering materials, may permeate near the surface, or may be attached to the surface. Examples of a method for manufacturing the inner and outer covering materials containing a crosslinked rubber composition include a method of soaking (immersing) the inner and outer covering fabrics in a rubber paste in which the rubber composition is dissolved in a solvent, and a method of rubbing (rubbing) a solid rubber composition into the inner and outer covering fabrics. The rubber component may be attached to at least one surface of the inner and outer covering fabrics, and is preferably attached to at least the surface that contacts the belt body.
[0121] As the rubber component (a) constituting the cross-linked rubber composition contained in each of the inner and outer covering materials (hereinafter referred to as the "cross-linked rubber composition of the covering material"), the rubber components exemplified as the rubber component (A) of the inner rubber layer and the outer rubber layer can be used, and preferred embodiments can be selected from the preferred embodiments of the rubber component (A).
[0122] The crosslinked rubber composition of the covering material may further contain a filler (b) in addition to the rubber component (a). As the filler (b), the fillers exemplified as the filler (C) of the inner rubber layer and the outer rubber layer can be used, and the preferred embodiment and the proportion of carbon black in the filler can be selected from the embodiment and proportion of the filler (C).
[0123] In the crosslinked rubber composition of the covering material, the proportion of the filler (b) (particularly, carbon black) is, for example, 5 to 80 parts by mass, preferably 10 to 75 parts by mass, more preferably 30 to 70 parts by mass, and even more preferably 40 to 60 parts by mass, per 100 parts by mass of the rubber component (a).
[0124] The crosslinked rubber composition of the outer covering material may further contain a plasticizer (c) in addition to the rubber component (a). As the plasticizer (c), the plasticizers exemplified as the plasticizers for the inner rubber layer and the outer rubber layer can be used. Among the plasticizers, ether ester plasticizers are preferred. The proportion of the plasticizer (c) is, for example, 3 to 50 parts by mass, preferably 5 to 40 parts by mass, more preferably 10 to 30 parts by mass, and even more preferably 15 to 25 parts by mass, relative to 100 parts by mass of the rubber component (a).
[0125] The crosslinked rubber composition of the outer covering material may further contain other additives (d) in addition to the rubber component (a). As the other additives (d), the additives exemplified as the other additives (D) of the inner rubber layer and the outer rubber layer can be used, and crosslinking agents, crosslinking accelerators, processing agents or processing aids, antiaging agents, etc. can be preferably used. The proportion of the other additives (d) can be selected from the same range as that of the additives (D) of the inner rubber layer and the outer rubber layer, including the preferred range.
[0126] In the inner covering material, the proportion of the crosslinked rubber composition is, for example, 10 to 200 parts by mass, preferably 50 to 100 parts by mass, and more preferably 70 to 90 parts by mass, per 100 parts by mass of the inner covering fabric. The proportion of the crosslinked rubber composition in the outer covering material, including the preferred range, can be selected from the proportion in the inner covering material.
[0127] The average thickness of the inner and outer covering materials (the average thickness of each layer in the case of a multi-layer structure) is, for example, 0.4 to 2 mm, preferably 0.5 to 1.4 mm, and more preferably 0.6 to 1.2 mm. If the thickness of the covering fabric is too thin, the abrasion resistance may decrease, and if it is too thick, the flex resistance of the belt may decrease.
[0128] (Inner and outer stiffeners) The inner reinforcing material and the outer reinforcing material each include an inner reinforcing fabric and an outer reinforcing fabric. The inner reinforcing fabric and the outer reinforcing fabric are each formed of a conventional fabric (A1). As the fabric (A1), the fabrics exemplified as the fabric (A) of the inner outer covering material and the outer outer covering material can be used, and can be selected from the same aspects as the fabric (A), including preferred aspects.
[0129] The inner reinforcement material may further contain a cross-linked rubber composition in addition to the inner reinforcing fabric in order to improve adhesion between the inner rubber layer and the inner outer covering material, and the outer reinforcement material may further contain a cross-linked rubber composition in order to improve adhesion between the outer rubber layer and the outer covering material.
[0130] The crosslinked rubber composition contained in each of the inner reinforcing material and the outer reinforcing material can be the same as the crosslinked rubber composition of the outer covering material, and preferred embodiments can be selected from the preferred embodiments of the crosslinked rubber composition of the outer covering material.
[0131] The average thickness of the inner reinforcing material and the outer reinforcing material (the average thickness of each layer in the case of multiple layers) is, for example, 0.4 to 2 mm, preferably 0.5 to 1.4 mm, and more preferably 0.6 to 1.2 mm. If the thickness of the reinforcing fabric is too thin, the reinforcing effect of the friction transmission surface may decrease, and if it is too thick, the bending resistance of the belt may decrease.
[0132] One of the inner reinforcement material and the outer reinforcement material may cover the side surface of the core layer, and it is preferable that the inner reinforcement material covers the side surface of the core layer.
[0133] [Connection part] The connecting portion connects adjacent hexagonal belt portions. In an embodiment in which the hexagonal belt portions are arranged without any gaps, the connecting portion is a boundary between adjacent inner outer covering materials and a boundary between adjacent outer covering materials. On the other hand, in an embodiment in which the hexagonal belt portions are arranged with gaps, the connecting portion includes an inner connecting member that forms the inner circumferential surface of the belt and an outer connecting member that forms the outer circumferential surface of the belt.
[0134] The inner connecting material and the outer connecting material include an inner connecting fabric and an outer connecting fabric, respectively. The inner connecting fabric and the outer connecting fabric are each formed of a conventional fabric (A2). As the fabric (A2), the fabrics exemplified as the fabric (A) of the inner outer covering material and the outer outer covering material can be used, and can be selected from the embodiments of the fabric (A), including preferred embodiments.
[0135] The inner connecting material and the outer connecting material may further contain a crosslinked rubber composition in addition to the inner connecting fabric and the outer connecting fabric, respectively, in order to improve adhesion with the crosslinked rubber composition. The crosslinked rubber composition of the outer covering material can be used as the crosslinked rubber composition contained in the inner connecting material and the outer connecting material, respectively, and preferred embodiments can be selected from the preferred embodiments of the crosslinked rubber composition of the outer covering material.
[0136] The average thickness of the inner connecting material and the outer connecting material (the average thickness of each layer in the case of multiple layers) is, for example, 0.4 to 2 mm, preferably 0.5 to 1.4 mm, and more preferably 0.6 to 1.2 mm. If the thickness of the connecting material is too thin, the connecting effect may decrease, and if it is too thick, the flex resistance of the belt may decrease.
[0137] The connecting portion may include a rubber layer formed of a crosslinked rubber composition between the inner connecting material and the outer connecting material. The crosslinked rubber composition forming the rubber layer may be a crosslinked rubber composition into which a part of the rubber composition for forming the inner rubber layer, the core layer, and the outer rubber layer (particularly the rubber composition of the core layer) has flowed out. Therefore, the crosslinked rubber composition of the rubber layer may be the same as the crosslinked rubber composition of the core layer.
[0138] Manufacturing method of joined hexagonal belt The combined hexagonal belt of the present disclosure is obtained by a manufacturing method including a crosslinking molding step of heating and pressurizing a combined hexagonal belt precursor disposed in a press mold to crosslink it. In the manufacturing method of the present disclosure, a combined hexagonal belt can be manufactured through the crosslinking molding step, and there is no need to connect each hexagonal belt after crosslinking in advance. Therefore, in the manufacturing method of the present disclosure, a combined hexagonal belt, which is difficult to manufacture, can be easily manufactured with high production efficiency. In detail, in the manufacturing method of the present disclosure, a combined hexagonal belt precursor disposed in a press mold is heated and pressurized, so that a crosslinking reaction of an uncrosslinked rubber component contained in the combined hexagonal belt precursor progresses, and the constituent materials of the combined hexagonal belt precursor are integrated (bonded) and molded into a desired shape at the same time. In particular, when the connecting portion contains a crosslinked rubber composition, in the crosslinking molding step, the crosslinking molding of the hexagonal belt portion and the crosslinking molding of the connecting portion can be performed simultaneously. That is, in the manufacturing method of the present disclosure, the following three steps 1 to 3 are performed simultaneously in the crosslinking molding step, so that the crosslinking molding of each hexagonal belt portion and the connection of a plurality of hexagonal belt portions can be completed in one step.
[0139] Step 1 for crosslinking the uncrosslinked rubber component contained in the bonded hexagonal belt precursor Step 2: bonding and integrating each material constituting the bonded hexagonal belt precursor (by a crosslinking reaction of the uncrosslinked rubber components contained in each material) Step 3: forming the outer appearance of the joined hexagonal belt into a predetermined shape (including forming the predetermined joint structure).
[0140] The press mold is preferably a press mold combining an inner press mold having an inner groove portion corresponding to the inner shape of the combined hexagonal belt and an outer press mold having an outer groove portion corresponding to the outer shape of the combined hexagonal belt.
[0141] The bonded hexagonal belt precursor preferably includes an inner fabric precursor for forming the inner fabric, an outer fabric precursor for forming the outer fabric, and a hexagonal belt portion precursor containing an uncrosslinked rubber composition.
[0142] In the method for producing a combined hexagonal belt of the present disclosure, when the combined hexagonal belt precursor includes the hexagonal belt portion precursor, the method may further include a hexagonal belt portion precursor preparation step as a step preceding the crosslinking molding step.
[0143] [Hexagonal belt part precursor manufacturing process] In the hexagonal belt portion precursor preparation step, the hexagonal belt portion precursor (uncrosslinked hexagonal belt portion) may be prepared by a method conforming to a conventional method used in the manufacture of wrapped V-belts, etc. Examples of the method for preparing the hexagonal belt portion precursor include a method conforming to the method for producing a V-belt described in WO2015 / 104778.
[0144] In particular, in the manufacturing method of the present disclosure, the method for producing the hexagonal belt portion may be a method for producing a precursor of the entire hexagonal belt portion, which is a laminate of an inner rubber layer precursor (inner rubber layer sheet) for forming the inner rubber layer, a core layer precursor for forming the core layer, and an outer rubber layer precursor (outer rubber layer sheet) for forming the outer rubber layer (integrated manufacturing method), or a method for producing a precursor in which the hexagonal belt portion is divided (split type manufacturing method), that is, a method for separately producing an inner hexagonal belt portion precursor and an outer hexagonal belt portion precursor. Of these, in the embodiment not including a reinforcing material, the integrated type manufacturing method is preferred from the viewpoint of simplicity, and in the embodiment including a reinforcing material, the split type manufacturing method is preferred from the viewpoint of easily forming a strong connection portion.
[0145] (No reinforcement material included) In an embodiment that does not include a reinforcing material, the method (preparation process) for producing a precursor of the entire hexagonal belt portion may be a method (process) of laminating a core layer precursor for forming a core layer on an outer rubber layer precursor for forming an outer rubber layer, laminating an inner rubber layer precursor for forming an inner rubber layer on the core layer precursor, and then cutting the sides of the inner rubber layer precursor and the outer rubber layer precursor.
[0146] A specific manufacturing process will be described with reference to the drawings. In the embodiment not including a reinforcing material, as shown in Fig. 9, the uncrosslinked outer rubber layer sheet 25 obtained by rolling is set on a mantle, and the uncrosslinked adhesive rubber layer sheet 22b is wound around the outer periphery of the outer rubber layer sheet 25, and then the core body 22a is wound around the outer periphery of the wound adhesive rubber layer sheet 22b, and the uncrosslinked adhesive rubber layer sheet 22b and the inner rubber layer sheet 23 are wound around the outer periphery of the wound core body 22a in order in a winding process, a cutting process in which the obtained annular laminate (uncrosslinked sleeve) 20 is cut (sliced) in a state in which it is arranged around the outer periphery of the mantle, and a skiving process in which the cut annular laminate 20a is hung on a pair of pulleys and cut into a V shape while rotating as shown in Fig. 10 (a process of removing the excess part 23a of the inner rubber layer sheet 23 and the excess part 25a of the outer rubber layer sheet) to obtain a hexagonal belt part precursor (uncrosslinked hexagonal belt part).
[0147] (embodiment including reinforcing material) In an embodiment including a reinforcing material, the method (production process) for producing the inner hexagonal belt portion precursor may be a method (process) for laminating a core layer precursor for forming a core layer on a thin outer rubber layer precursor for forming a part of the outer rubber layer, laminating an inner rubber layer precursor for forming an inner rubber layer on the core layer precursor, and then cutting the side of the inner rubber layer precursor.
[0148] The method for producing the outer hexagonal belt portion precursor (production step) may be a step of cutting the side surface of a thick outer rubber layer precursor for forming the remaining portion of the outer rubber layer.
[0149] A specific manufacturing process will be described with reference to the drawings. In an embodiment that does not include a reinforcing material, as shown in Fig. 11, a release sheet (such as a nylon film) 36a is set on the mantle, and an uncrosslinked thin outer rubber layer sheet (a thin sheet that forms a part of the outer rubber layer) 35a and an uncrosslinked adhesive rubber layer sheet 32b are wound around the outer periphery of the release sheet 36a, and then a core body 32a is wound around the outer periphery of the wound adhesive rubber layer sheet 32b, and an uncrosslinked adhesive rubber layer sheet 32b and an inner rubber layer sheet 33 are wound around the outer periphery of the wound core body 32a in a winding process, and the obtained annular laminate (uncrosslinked sleeve) 30 is cut (sliced) in a state of being placed on the outer periphery of the mantle, to obtain an annular laminate 30a.
[0150] As shown in Fig. 12, the cut annular laminate 30a is placed over a pair of pulleys and cut into a V shape while rotating in a skiving process (a process for removing excess portions 33a) to obtain a skived annular laminate. At this point, the obtained annular laminate includes a release sheet 36a.
[0151] Next, the skived annular laminate is covered with the reinforcing material precursor 31a so as to cover the entire surface over the entire length. As a method for covering the reinforcing material precursor 31a, a known method described in JP-A-10-323915, JP-A-2016-87885, etc. can be used. The number of reinforcing material precursors to be covered can be selected as necessary.
[0152] Furthermore, the reinforcing material precursor on the back side of the precursor is peeled off (removed) from the annular laminate covered with the reinforcing material precursor 31a. Although there is no limitation to this method, from the viewpoint of productivity, a method is preferred in which a trim cut (reverse skive) is performed on both ends on the back side (ends 37a are removed to remove the release sheet), and the laminate 37b of the reinforcing material precursor and the release sheet is peeled off (upper reinforcing material peeling), thereby peeling off the reinforcing material precursor together with the release sheet. By this process, an inner hexagonal belt portion precursor (uncrosslinked inner hexagonal belt portion) is obtained.
[0153] As shown in FIG. 13, the outer hexagonal belt portion precursor (uncrosslinked outer hexagonal belt portion) can be obtained through a winding process in which a release sheet (such as a nylon film) 36b and an uncrosslinked thick outer rubber layer sheet 35b are wound around a mantle in this order, a cutting process in which the obtained annular laminate is cut (sliced into rings) on the mantle, a skiving process in which the cut annular laminate is placed over a pair of pulleys and cut into a V shape while rotating (a process for removing excess parts 35c), a covering process in which a reinforcing material precursor 31b is applied to the skived annular laminate so as to cover the entire surface over the entire length, a reverse skiving process in which a trim cut (reverse skiving) is performed on both ends on the back side (a process for removing excess parts 38a), and a peeling process in which the laminate 38b of the reinforcing material precursor and the release sheet is peeled off (upper reinforcing material peeling), thereby peeling off the reinforcing material precursor together with the release sheet.
[0154] In an embodiment including a reinforcing material, by using a split-type manufacturing method for producing the hexagonal belt portion, in the cross-linking molding process described below, a portion of the rubber composition for forming the inner rubber layer, core layer, and outer rubber layer (particularly the rubber composition of the core layer) flows out into the connecting portion from the gap between the reinforcing material precursor (inner reinforcing material precursor) 31a and the reinforcing material precursor (outer reinforcing material precursor) 31b, whereby the connecting fabric and the rubber composition are integrated at the connecting portion to form a strong connecting portion.
[0155] The average thickness of the thin outer rubber layer sheet is, for example, 10 to 50%, preferably 20 to 40%, and more preferably 25 to 35% of the average thickness of the entire outer rubber layer sheet (the total thickness of the first outer rubber layer sheet and the second outer rubber layer sheet).
[0156] When the inner rubber layer or the outer rubber layer has a laminated structure of two or more layers, the above-mentioned uncrosslinked outer rubber layer sheet or inner rubber layer sheet may be arranged by laminating multiple types of sheets as necessary.
[0157] [Crosslinking molding process] The combined hexagonal belt precursor including the obtained hexagonal belt portion precursor is placed in a press mold and subjected to a crosslinking molding process. In the crosslinking molding process, when the press mold is a combination of an inner press mold and an outer press mold, the inner fabric precursor may be placed along the inner groove, the hexagonal belt portion precursor may be laminated on the inner fabric precursor, the outer fabric precursor may be placed along the hexagonal belt portion precursor, the outer groove may be brought into contact with the outer precursor, and the combined hexagonal belt precursor may be sandwiched between the inner press mold and the outer press mold. The crosslinking molding process will be described below with reference to the drawings.
[0158] 14 shows an overall view of a combined hexagonal belt precursor being crosslinked and molded using a crosslinking molding device 40. A plurality of uncrosslinked annular bodies (inner fabric precursor, hexagonal belt portion precursor, and outer fabric precursor) 41 held in a wound state around a pair of pulleys 44a, 44b are sandwiched between the pair of pulleys 44a, 44b by two press molds.
[0159] As shown in Figs. 15 and 16, the two press molds each have a structure corresponding to the shape of the connecting hexagonal belt. The first press mold is a combination of an inner press mold 42a having an inner groove with a trapezoidal cross section and an outer press mold 42b having an outer groove with a trapezoidal cross section, and the second press mold is a combination of an inner press mold 43a having an inner groove with a trapezoidal cross section and an outer press mold 43b having an outer groove with a trapezoidal cross section. When the inner press molds 42a, 43a and the outer press molds 42b, 43b are combined, a hollow portion with a hexagonal cross section corresponding to the shape of the hexagonal belt is formed inside the press mold. A heating plate 45 is disposed between the inner press mold 42a of the first press mold and the inner press mold 43a of the second press mold, and both press molds can be heated. Therefore, by disposing (fitting) a combined hexagonal belt precursor in the hollow portion and heating it, a part of the annular body 41 can be molded into the shape of a combined hexagonal belt and crosslinked. Then, by rotating the pair of pulleys 44a, 44b, the annular body 41 can be moved in a circumferential direction in sequence, and when the entire circumference of the annular body 41 is crosslinked in sequence, the combined hexagonal belt is completed.
[0160] The cross-linking molding process using this device will be described in detail below. First, as shown in Fig. 17, an inner fabric precursor 41a is fitted into a plurality of grooves having an inverted trapezoidal cross section formed in an inner press mold 42a using a jig 46a having a shape corresponding to the grooves. The inner fabric precursor 41a may contain an uncross-linked rubber composition.
[0161] Next, in an embodiment not including a reinforcing material, as shown in Fig. 18, the hexagonal belt portion precursor 47 is fitted into each groove into which the inner fabric precursor 41a is fitted, and then, in a state in which the hexagonal belt portion precursor is arranged in each groove arranged in the width direction, the outer fabric precursor 41b is placed on top of it (on the outer periphery side), and the outer fabric precursor 41b is aligned to the contour of the hexagonal belt portion precursor by a jig 46b, as shown in Fig. 19. The outer fabric precursor 41b may also contain an uncrosslinked rubber composition.
[0162] As shown in FIG. 20, an outer press mold 42b is disposed on the outer peripheral surface of the combined hexagonal belt precursor set in the inner press mold 42a, and the combined hexagonal belt precursor is subjected to a cross-linking molding process in which it is heated and pressurized while being sandwiched between the inner press mold 42a and the outer press mold 42b.
[0163] On the other hand, in an embodiment including a reinforcing material, as shown in FIG. 21, the inner hexagonal belt portion precursor 48 is fitted into each groove portion into which the inner fabric precursor 41a is fitted, and then, as shown in FIG. 22, the outer hexagonal belt portion precursor 49 is laminated on top (outer peripheral surface) of the inner hexagonal belt portion precursor 48 to form a hexagonal belt portion precursor.
[0164] 23, in a state where the hexagonal belt portion precursors are arranged in the grooves aligned in the width direction, the outer fabric precursor 41b is placed on top of them (on the outer periphery), and the outer fabric precursor 41b is aligned to the contour of the hexagonal belt portion precursor by a jig 46b. The outer fabric precursor 41b may also contain an uncrosslinked rubber composition.
[0165] As shown in FIG. 24, an outer press mold 42b is disposed on top (outer surface) of the combined hexagonal belt precursor set in the inner press mold 42a, and the combined hexagonal belt precursor is subjected to a cross-linking molding process in which it is heated and pressurized while being sandwiched between the inner press mold 42a and the outer press mold 42b.
[0166] In this crosslinking molding process, when the precursors are bonded and integrally crosslinked by the crosslinking reaction of the rubber components in a state molded into the form shape of the press mold, a crosslinked sleeve is formed in which multiple hexagonal belt parts are connected and bonded in the width direction. In this process, the connecting part is formed by integrally crosslinking the inner connecting material, which is a part of the inner fabric, the outer connecting material, which is a part of the outer fabric, and the rubber composition that has flowed out from the rubber layer of the hexagonal belt part precursor between the inner connecting material and the outer connecting material. In other words, the connecting part is formed as a complex composed of three components: the inner connecting material, the crosslinked rubber composition, and the outer connecting material.
[0167] In addition, the inner fabric precursor and the outer fabric precursor for forming the outer covering material and the connecting material can be treated (adhesive treatment) with an uncrosslinked rubber composition, so that the adhesive component attached to the inner fabric precursor and the outer fabric precursor can firmly bond to each hexagonal belt portion precursor (uncrosslinked hexagonal belt portion). For example, when a woven fabric (woven fabric with rubber) that has been treated by friction (rubbing) a solid rubber composition is used as the inner fabric precursor and the outer fabric precursor, they are bonded to each other by the crosslinking reaction of the friction rubber composition. That is, the process of setting the inner fabric precursor and the outer fabric precursor to the hexagonal belt portion precursor includes an uncrosslinked belt bonding process of bonding a plurality of hexagonal belt portion precursors to each other via the inner fabric precursor and the outer fabric precursor.
[0168] In the crosslinking molding step, the heating temperature can be selected depending on the type of rubber component and is, for example, 120 to 200°C, preferably 150 to 180°C. The pressure can be selected depending on the type of rubber component and is, for example, 0.1 to 10 MPa, preferably 0.5 to 3 MPa, and more preferably 0.9 to 1.5 MPa. In the present application, the pressure is a value converted into a press surface pressure. In addition, each rubber layer sheet containing short fibers can be rolled with a calender roll or the like to align (orient) the short fibers in the rolling direction.
[0169] The bridging sleeve thus formed is cut to a predetermined width as shown in Fig. 25 to form a combined hexagonal belt having a predetermined number of hexagonal belt portions (six in Fig. 25). Note that Fig. 25 is an example of a combined hexagonal belt in an embodiment that does not include a reinforcing material. EXAMPLES
[0170] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, the raw materials used in the rubber composition, the method for preparing the rubber composition, the fiber materials used, and the measurement or evaluation methods for each physical property are shown.
[0171] [Raw materials for rubber composition] Chloroprene rubber: DENKA Corporation "PM-40" Magnesium oxide: Kyowa Mag 30 manufactured by Kyowa Chemical Industry Co., Ltd. Stearic acid: NOF Corp. "Camellia Stearate" Anti-aging agent: "Nonflex OD-3" manufactured by Seiko Chemical Co., Ltd. Carbon black: "Seast 3" manufactured by Tokai Carbon Co., Ltd. Silica: Evonik Japan Co., Ltd., "ULTRASIL (registered trademark) VN3", BET specific surface area 175 m 2 / g Plasticizer: ADEKA Cizer RS-700 manufactured by ADEKA Corporation Crosslinking accelerator: "Noccela TT" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Zinc oxide: "Zinc oxide type 3" manufactured by Seido Chemical Industry Co., Ltd. Naphthenic oil: "NS-900" manufactured by Idemitsu Kosan Co., Ltd. N,N'-m-Phenylenedimaleimide: "Valnoc PM" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Aramid short fiber: Teijin Limited's "Conex short fiber" (average fiber length 3 mm, average fiber diameter 14 μm) is bonded with RFL liquid (2.6 parts by mass of resorcinol, 1.4 parts by mass of 37% formalin, 17.2 parts by mass of vinylpyridine-styrene-butadiene copolymer latex (manufactured by Zeon Corporation), 78.8 parts by mass of water) to produce short fibers with a solid adhesion rate of 6% by mass.
[0172] [Core] Twisted aramid fiber cord, average wire diameter 1.190mm.
[0173] [Rubber composition for adhesive rubber layer and friction rubber] Rubber composition A having the composition shown in Table 2 was kneaded in a Banbury mixer, and the kneaded rubber was passed through a calendar roll to form a rolled rubber sheet of a predetermined thickness to prepare an uncrosslinked rubber sheet for an adhesive rubber layer. Rubber composition B shown in Table 2 was kneaded in a Banbury mixer to prepare a lump-shaped uncrosslinked rubber composition for friction. Furthermore, the hardness and tensile strength of the crosslinked product (crosslinked rubber) of each rubber composition were measured, and the results are also shown in Table 2.
[0174] [Table 2]
[0175] [Rubber Composition for Inner Rubber Layer and Outer Rubber Layer] Rubber compositions C to D having the formulations shown in Table 3 were kneaded in a Banbury mixer, and the kneaded rubber was passed through a calendar roll to form a rolled rubber sheet of a predetermined thickness, thereby producing an uncrosslinked rubber sheet for an inner rubber layer and an uncrosslinked rubber sheet for an outer rubber layer. Furthermore, the hardness and tensile strength of the crosslinked product (crosslinked rubber) of each rubber composition were measured, and the results are also shown in Table 3.
[0176] [Table 3]
[0177] [Rubber hardness Hs of cross-linked rubber] Each uncrosslinked rubber sheet for rubber layer was press-heated at 160°C for 30 minutes to prepare a crosslinked rubber sheet (100mm x 100mm x 2mm thick). A laminate of three crosslinked rubber sheets was used as a sample, and the hardness of the crosslinked rubber sheet was measured using a type A durometer in accordance with the spring durometer hardness test specified in JIS K6253 (2012). For the lump uncrosslinked rubber composition B for friction, a test specimen was sampled from the lump rubber and passed through a calendar roll to prepare an uncrosslinked rolled rubber sheet of a predetermined thickness.
[0178] [Tensile strength of cross-linked rubber] The cross-linked rubber sheet prepared for measuring the rubber hardness Hs of cross-linked rubber was used as a sample, and a dumbbell-shaped (5-type) test specimen was prepared according to JIS K6251 (2017). For samples containing short fibers, dumbbell-shaped test specimens were taken so that the short fiber arrangement direction (parallel to the grain direction) was the tensile direction. Then, both ends of the test specimen were held with a chuck (gripping tool), and the test specimen was pulled at a speed of 500 mm / min until it broke. The maximum tensile force recorded when the test specimen was divided by the initial cross-sectional area of the test specimen (tensile strength T) was defined as the tensile strength.
[0179] [Sheathing, connecting and reinforcing materials] Woven fabric of polyester fiber and cotton blend yarn (polyester fiber / cotton = 50 / 50 mass ratio) (120° wide angle weave, 20-count warp thread and 20-count weft thread, warp and weft thread density 75 threads / 50mm, basis weight 280g / m 2 ) was used, and rubber composition B in Table 2 was used. Rubber composition B and the woven fabric were simultaneously passed between calendar rolls having different surface speeds, and a friction treatment was performed (once on each side of the woven fabric) in a manner that rubber composition B was rubbed into the weave of the woven fabric, to prepare a reinforcing material precursor (woven fabric with rubber), and inner and outer fabric precursors (woven fabric with rubber) for forming an outer covering material and a connecting material.
[0180] [Preparation of bonded hexagonal belt] Example 1 (Inner rubber layer / outer rubber layer are single layers, covered with reinforcing material) The rubber composition D in Table 3 was used for the outer rubber layer sheet and the inner rubber layer sheet. A release sheet (nylon film), an outer rubber layer sheet (thickness 0.5 mm), and an adhesive rubber layer sheet were wound in this order around the outer circumferential surface of the mantle, a core wire was spun in a spiral shape around the outer circumferential surface, and an adhesive rubber layer sheet and an inner rubber layer sheet were further wound in this order to form an uncrosslinked annular laminate (uncrosslinked sleeve). The obtained annular laminate was cut (sliced) in the circumferential direction at a predetermined width while being disposed around the outer periphery of the mantle, to form a plurality of annular laminates.
[0181] Next, the cut annular laminate was removed from the mantle, and while rotating it around a pair of pulleys, both sides of the annular laminate were cut (skived) at a predetermined angle, forming a V-shaped cross section of the annular laminate. Next, the skived annular laminate was covered with a reinforcing material precursor (woven fabric with rubber) over its entire periphery (covering), and then a trim cut (reverse skive) was performed on both ends of the back side, and the reinforcing material precursor was peeled off and removed together with the release sheet, forming an inner hexagonal belt portion precursor.
[0182] The outer hexagonal belt portion precursor was formed by processing in the same manner as the inner hexagonal belt portion precursor, except for the process of wrapping a release sheet (nylon film) and an uncrosslinked outer rubber layer sheet, in that order, around the outer peripheral surface of the mantle to form an uncrosslinked annular laminate (uncrosslinked sleeve).
[0183] Then, in the manner described in the embodiment, the inner fabric precursor (woven fabric with rubber), the six inner hexagonal belt portion precursors and the outer hexagonal belt portion precursor, and the outer fabric precursor (woven fabric with rubber) were set in a press mold, pressurized to 1.2 MPa, and heated at a temperature of 160°C to obtain a crosslinked sleeve in which six hexagonal belt portions (ARPM AA type, cross-sectional dimensions: width 13 mm x thickness 8.5 to 10.2 mm, belt length 122 inches) were connected and bonded. The crosslinked sleeve obtained was cut to form a bonded hexagonal belt having two hexagonal belt portions (hexagonal belt portions having the structure shown in Figure 7).
[0184] Example 2 (two inner rubber layers, one outer rubber layer, covered with reinforcing material) Rubber composition D in Table 3 was used for the outer rubber layer sheet and the second inner rubber layer sheet, and rubber composition C having high hardness was used for the first inner rubber layer sheet.
[0185] In the manufacturing process of the inner hexagonal belt portion precursor, in the step of forming an uncrosslinked annular laminate (uncrosslinked sleeve), the core wire was spun into a spiral shape, and then the adhesive rubber layer sheet, the first inner rubber layer sheet, and the second inner rubber layer sheet were wound in this order, except that a combined hexagonal belt having two hexagonal belt portions was formed in the same manner as in Example 1. Note that the first inner rubber layer sheet containing short fibers had the short fibers aligned in the belt width direction.
[0186] Example 3 (Inner rubber layer / outer rubber layer each have two layers, and are covered with reinforcing fabric) For the second outer rubber layer sheet and the second inner rubber layer sheet, rubber composition D in Table 3 was used, and for the first outer rubber layer sheet and the first inner rubber layer sheet, rubber composition C with high hardness was used.
[0187] In the manufacturing process of the inner hexagonal belt portion precursor, a first outer rubber layer sheet was used as an outer rubber layer sheet having a thickness of 0.5 mm in the step of forming an uncrosslinked annular laminate (uncrosslinked sleeve), and in the manufacturing process of the outer hexagonal belt portion precursor, a release sheet (nylon film), a first outer rubber layer sheet, and a second outer rubber layer sheet were wound in this order around the outer peripheral surface of the mantle in the step of forming an uncrosslinked annular laminate (uncrosslinked sleeve). Except for this, a combined hexagonal belt having two hexagonal belt portions (hexagonal belt portions having the structure shown in FIG. 8) was formed in the same manner as in Example 2. The first outer rubber layer sheet and the first inner rubber layer sheet, which contained short fibers, had short fibers arranged in the belt width direction.
[0188] Example 4 (two inner rubber layers, one outer rubber layer, not covered with reinforcing material) Rubber composition D in Table 3 was used for the outer rubber layer sheet and the second inner rubber layer sheet, and rubber composition C having high hardness was used for the first inner rubber layer sheet.
[0189] A joined hexagonal belt having two hexagonal belt portions was formed by the manufacturing method not including a reinforcing material as described in the embodiment.
[0190] Comparative Example 1 A wrapped coupled V-belt according to Example 5 of JP 2020-3061 A (Patent Document 4) was formed.
[0191] [Belt running test (durability performance)] Using the combined hexagonal belt obtained in the embodiment and the wrapped combined V-belt obtained in the comparative example, the pulleys in the layout consisting of the driving pulley (Dr1), driven pulleys (Dn2 and Dn3), tension pulley (Ten4), and idler pulley (ID5) shown in Table 4 were arranged in the order of driving pulley (Dr1) 51, tension pulley (Ten4) 54, driven pulley (Dn3) 53, driven pulley (Dn2) 52, and idler pulley (ID5) 55 as shown in Figure 26. The belt was run under the conditions shown in Table 5, and the time until the belt broke was evaluated according to the following criteria. Note that, as for the load during running, as shown in Table 6, the test was performed under a load of 9.5 kW on the driven pulley (back driven pulley) Dn2 and 23.0 kW on the driven pulley Dn3, for a total of 32.5 kW. In the examples, V pulleys were used for Dr1, Dn2, and Dn3, and flat pulleys were used for Ten4 and ID5. In the comparative examples, V pulleys were used for Dr1 and Dn3, and flat pulleys were used for Dn2, Ten4, and ID5.
[0192] (Judgment criteria) ◎: 240 hours completed, no cracks, peeling or other abnormalities were observed 〇: 240 hours completed, slight cracks and peeling observed (no impact on performance) ×: Abnormalities (cracks or peeling) occurred that impair performance.
[0193] [Table 4]
[0194] [Table 5]
[0195] [Table 6]
[0196] [Belt running test (transmission performance)] Whether or not high-performance double-sided transmission is possible can be judged from the perspective of how much the transmission performance on the outer belt side (back side) has improved compared to a wrapped coupled V-belt (Comparative Example 1) in which the outer belt surface (back side) is formed flat. The transmission performance on the outer belt side (back side) is measured using the slip ratio value between the friction transmission surface on the outer belt side and the back driven pulley Dn2 as an index, and it was determined that the smaller the slip ratio value, the better the transmission performance on the outer belt side (back side) and the more highly efficient double-sided transmission is possible.
[0197] Specifically, for Examples 1 to 4 and Comparative Example 1, a test machine with a multi-axis layout similar to that used in the durability performance test was used to run the belt under the loads shown in Table 6 (9.5 kW on driven pulley Dn2, 23.0 kW on driven pulley Dn3, a total of 32.5 kW) before and after the run to evaluate the durability performance (conditions in Table 5), and the rotation speed (rpm) of the driven pulley (back driven pulley) Dn2 was measured to calculate the slip ratio according to the following formula. The rotation speeds of the drive pulley Dr1 and driven pulley Dn2 under no load and the rotation speed of the drive pulley Dr1 under load in this measurement are shown in Table 7.
[0198] If the slip rate (%) after driving (after completing 240 hours) is less than 1%, it is evaluated as having excellent transmission performance on the outer circumference (back side) of the belt and capable of high-performance double-sided transmission, and is rated as A. If the slip rate (%) after driving (after completing 240 hours) was 1% or more, the transmission performance on the outer circumference of the belt (back side) was evaluated as being inferior, and high-performance double-sided transmission was not possible, and the belt was given a rating of b. From the viewpoint of suitability for practical use in this application, belts rated A were considered to be at the pass level.
[0199] Slip rate (%) = [(K2-K1) / K1] x 100 [In the formula, K1=R1 / N1, K2=R2 / N2, R1 is the rotation speed (rpm) of the drive pulley when operating without load, N1 is the rotation speed (rpm) of the driven pulley when operating without load, R2 is the rotation speed (rpm) of the drive pulley when operating with load, and N2 is the rotation speed (rpm) of the driven pulley when operating with load]
[0200] [Table 7]
[0201] The results of the running evaluation of the resulting joined hexagonal belt are shown in Table 8.
[0202] [Table 8]
[0203] From the results in Table 8, each of the joined hexagonal belts of the examples did not show any significant abnormalities until the 240-hour cutoff time, and completed the run. As in Examples 2 to 4, it can be seen that the provision of a high-hardness rubber layer on the core layer side of the inner (outer) rubber layer has an effect on durability.
[0204] On the other hand, the wrapped combined V-belt of Comparative Example 1 also completed the test without any significant abnormality until the 240-hour cutoff time. The transmission performance (slip rate) was 1.00% (grade b) before the endurance test and 1.30% (grade b) after the endurance test.
[0205] In contrast, the transmission performance (slip rate) of the combined hexagonal belts of Examples 1 to 4 was 0.70% (a-judgment) before the endurance run and 0.90% (a-judgment) after the endurance run in all cases. In other words, the combined hexagonal belt has a suppressed slip rate on the outer belt side (back side) compared to the wrapped combined V-belt, and the transmission performance is improved. Therefore, it was confirmed that the combined hexagonal belt, which has a V-shaped side (friction transmission surface) that can contact the V-pulley on the outer peripheral side in addition to the inner peripheral side, is capable of high-performance double-sided transmission. [Industrial Applicability]
[0206] The combined hexagonal belt of the present disclosure can be used as various friction transmission belts that require double-sided driving, for example, in general industrial machines such as compressors, generators, pumps, etc.; textile machines such as spinning machines, spinning machines, looms, knitting machines, dyeing and finishing machines, etc.; agricultural machines such as tillers, rice planters, vegetable transplanters, transplanters, binders, combines, bean cutters, corn crushers, potato harvesters, beet harvesters, vegetable harvesters, grass cutters, threshers, rice hullers, rice polishers, etc. In particular, it is suitable for large, high-load agricultural machines used in Europe and the United States, for example, tillers, binders, combines, vegetable harvesters, threshers, bean cutters, corn crushers, potato harvesters, beet harvesters, etc. [Explanation of symbols]
[0207] 1…Connected hexagonal belt 2...Core layer 2a…core wire 3…Inner rubber layer 4…Inner outer covering material 5…Outer rubber layer 6…Outer jacket material 7…Inner connector 8…Outer connecting material
Claims
1. A combined hexagonal belt in which a plurality of hexagonal belt portions each having a hexagonal cross section are arranged in the belt width direction, the hexagonal belt portion includes a core layer, an inner rubber layer laminated on the inner circumferential surface side of the core layer and having a trapezoidal cross section, an inner outer covering material covering the inner rubber layer and including an inner outer covering fabric, an outer rubber layer laminated on the outer circumferential surface side of the core layer and having a trapezoidal cross section, and an outer outer covering material covering the outer rubber layer and including an outer outer covering fabric, Adjacent hexagonal belt portions are connected to each other via connecting portions, and A bonded hexagonal belt in which adjacent inner outer cover fabrics are formed from a continuous inner fabric and adjacent outer outer cover fabrics are formed from a continuous outer fabric.
2. The connecting portion includes an inner connecting member that forms an inner circumferential surface of the belt and an outer connecting member that forms an outer circumferential surface of the belt, The inner connecting material includes an inner connecting fabric, and the outer connecting material includes an outer connecting fabric, 2. The joined hexagonal belt according to claim 1, wherein the inner fabric is a fabric in which the inner connecting fabric and the inner outer cover fabric are continuous, and the outer fabric is a fabric in which the outer connecting fabric and the outer outer cover fabric are continuous.
3. The bonded hexagonal belt of claim 2 , wherein the joint further comprises a crosslinked rubber composition.
4. The bonded hexagonal belt according to any one of claims 1 to 3, wherein an inner reinforcing material is interposed between the inner outer covering material and the inner rubber layer, and an outer reinforcing material is interposed between the outer outer covering material and the outer rubber layer.
5. The combined hexagonal belt according to any one of claims 1 to 3, wherein the inner rubber layer includes a first inner rubber layer laminated on the core layer side, and a second inner rubber layer having a lower rubber hardness than the first inner rubber layer and laminated on the inner peripheral side of the belt.
6. The method for producing the combined hexagonal belt according to any one of claims 1 to 3, further comprising a crosslinking molding step of crosslinking and molding a combined hexagonal belt precursor placed in a press mold by heating and pressurizing the combined hexagonal belt precursor.
7. 7. The method according to claim 6, wherein the connecting portion contains a crosslinked rubber composition, and in the crosslinking molding step, crosslinking molding of the hexagonal belt portion and crosslinking molding of the connecting portion are carried out simultaneously.
8. The press mold is a combination of an inner press mold having an inner groove portion corresponding to the inner shape of the combined hexagonal belt and an outer press mold having an outer groove portion corresponding to the outer shape of the combined hexagonal belt, The bonded hexagonal belt precursor includes an inner fabric precursor for forming an inner fabric, an outer fabric precursor for forming an outer fabric, and a hexagonal belt portion precursor including an uncrosslinked rubber composition, 8. The manufacturing method according to claim 7, wherein in the crosslinking molding process, the inner fabric precursor is arranged along the inner groove portion, the hexagonal belt portion precursor is laminated onto the inner fabric precursor, the outer fabric precursor is arranged along the hexagonal belt portion precursor, and then the outer groove portion is brought into contact with the outer fabric precursor, and the combined hexagonal belt precursor is sandwiched between the inner press mold and the outer press mold.
9. 9. A method for manufacturing a combined hexagonal belt including an inner reinforcement and an outer reinforcement, wherein the hexagonal belt portion precursor is a combination of an inner hexagonal belt portion precursor and an outer hexagonal belt portion precursor, and in the crosslinking molding step, the inner hexagonal belt portion precursor is laminated on the inner fabric precursor, and then the outer hexagonal belt portion precursor is laminated on the inner hexagonal belt portion precursor.
10. The method further includes a hexagonal belt portion precursor preparation step as a step prior to the crosslinking molding step, The hexagonal belt portion precursor manufacturing step includes a step of manufacturing an inner hexagonal belt portion precursor and a step of manufacturing an outer hexagonal belt portion, a step of preparing the inner hexagonal belt portion precursor, comprising: laminating a core layer precursor for forming a core layer on a thin outer rubber layer precursor for forming a part of the outer rubber layer; laminating an inner rubber layer precursor for forming an inner rubber layer on the core layer precursor; and then cutting a side surface of the inner rubber layer precursor; 10. The method according to claim 9, wherein the step of preparing the outer hexagonal belt portion precursor comprises cutting a side surface of a thick outer rubber layer precursor for forming the remaining portion of the outer rubber layer.
Citation Information
Patent Citations
Transmission belt and manufacture thereof
JP1991033536A
Coupling v-belt for power transmission and its manufacture
JP1992351350A
Belt for power transmission
JP1998274290A
Transmission-bonding v belt
JP2001241513A
Double v-ribbed belt
JP2009250263A