Water-based ballpoint pen

The use of a tungsten carbide and cobalt-nickel mixture in the writing ball of water-based ballpoint pens stabilizes resin particles, enhancing initial writing performance by preventing ink dispersibility issues.

JP7554336B2Active Publication Date: 2024-09-19MITSUBISHI PENCIL CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023190220
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-11-07
Publication Date
2024-09-19
Estimated Expiration
2039-05-14

AI Technical Summary

Technical Problem

Water-based ballpoint pens with relatively large resin particles face issues with ink stability and dispersibility when exposed to air, leading to difficulties in initial writing performance.

Method used

Aqueous ballpoint pens incorporating a writing ball made of a mixture containing tungsten carbide as a hard phase and cobalt and nickel as binder components, along with resin particles of 0.3 μm or more, to maintain ink stability and dispersibility.

Benefits of technology

Improves initial writing performance by maintaining ink stability and dispersibility even after exposure to air, ensuring clear lines without blurring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554336000004
    Figure 0007554336000004
  • Figure 0007554336000002
    Figure 0007554336000002
  • Figure 0007554336000003
    Figure 0007554336000003
Patent Text Reader

Abstract

To provide an aqueous ball-point pen using an ink composition containing resin particles of a relatively large average particle size of 0.3 μm or more, improved in initial writing property after leaving a ball-point pen tip exposed in ambient air, without changing the ink composition.SOLUTION: An aqueous ball-point pen 10 stores an aqueous ink composition blended with resin particles of an average particle size of 0.3 μm or more, and has a ball-point pen tip 20 having a writing ball 30 formed of a mixture containing tungsten carbide as a hard phase element, cobalt and nickel as a binder phase element, and chromium.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous ballpoint pen having a writing ball having a hard phase component and a binder phase component. [Background technology]

[0002] As materials for constructing ballpoint pen balls, cemented carbide and ceramics are widely known, as described in the following Patent Documents 1 to 3. Improvements in the ink adhesion and writing feel of such cemented carbide balls are discussed in the following Patent Documents 4 and 5.

[0003] Furthermore, the inclusion of colored resin particles in water-based ballpoint pen ink is disclosed in the following Patent Document 6, and in particular the use of a microsphere colorant is disclosed in the following Patent Document 7.

[0004] Furthermore, the improvement of writing performance by using an ink that uses a thermally modified pigment and a ball that contains cobalt and nickel is disclosed in the following Patent Document 8. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Utility Model Application Publication No. 52-106235 [Patent Document 2] JP 2002-19366 A [Patent Document 3] JP 2015-51571 A [Patent Document 4] Special Publication No. 50-31049 [Patent Document 5] JP 2002-19366 A [Patent Document 6] JP 2003-155435 A [Patent Document 7] JP 2017-214540 A [Patent Document 8] JP 2006-142511 A [Patent Document 9] JP 2016-132749 A Summary of the Invention [Problem to be solved by the invention]

[0006] When an aqueous ballpoint pen using an ink composition containing resin particles with a relatively large average particle size of 0.3 μm or more is left exposed to the outside air, the ink often becomes sloppy when the pen tip is first written. This is presumably because the water contained in the ink attached to the tip of the ballpoint pen evaporates, causing the resin particles to lose stable dispersion in the ink and form loose aggregates. This phenomenon is likely to occur when the average particle size of the resin particles in the ink is relatively large or when the amount of resin particles mixed is large.

[0007] Attempts have already been made to solve such problems related to initial writing performance by adjusting the composition of the ink, as described in the above-mentioned Patent Document 9. However, no attempt has been made to improve the initial writing performance without changing the composition of the ink.

[0008] In view of the above problems, an object of the present invention is to improve the initial writing performance of an aqueous ballpoint pen using an ink composition containing resin particles with a relatively large average particle size of 0.3 μm or more, even after the ballpoint pen tip is left exposed to the outside air, without changing the ink composition. [Means for solving the problem]

[0009] In order to solve the above problems, a first aspect of the present invention is an aqueous ballpoint pen containing an aqueous ink composition containing resin particles having an average particle size of 0.3 μm or more, Tungsten carbide as a hard phase component; Cobalt and nickel as binder phase components; Chrome and The present invention is characterized in that it comprises a ballpoint pen tip having a writing ball made of a mixture containing

[0010] Although there is no particular upper limit to the average particle size of the resin particles, it is desirable that the average particle size be less than 5 μm so as not to impair the fluidity of the ink or the dispersibility of the resin particles.

[0011] Furthermore, an aqueous ballpoint pen according to a second aspect of the present invention is characterized in that, in addition to the characteristics of the above-mentioned first aspect, the aqueous ink composition contains 5 to 30 mass % of the resin particles.

[0012] Furthermore, the water-based ballpoint pen according to a third aspect of the present invention is characterized in that, in addition to the features of the first or second aspect, the resin particles contain a colorant. Effect of the Invention

[0013] As configured as described above, in the present invention, in an aqueous ballpoint pen using an ink composition containing resin particles with a relatively large average particle size of 0.3 μm or more, the initial writing performance is improved after the ballpoint pen tip is left exposed to the outside air without changing the ink composition. [Brief description of the drawings]

[0014] [Figure 1] 1 is a side view of a water-based ballpoint pen according to an embodiment of the present invention. [Diagram 2] A refill used in the water-based ballpoint pen of FIG. 1 is shown in cross section. [Diagram 3] 3 is an enlarged cross-sectional view showing the tip of the ballpoint pen tip used in the refill of FIG. 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, each embodiment of the present invention will be described with reference to the drawings. Among the reference numerals shown in each drawing, those common to a plurality of drawings have the same technical meaning even if not described in the following description of each drawing. In addition, in each drawing, the upper side of the drawing is the front end side, and the lower side of the drawing is the rear end side.

[0016] (1) Appearance 1 is a side view of an aqueous ballpoint pen 10 according to a first embodiment. The aqueous ballpoint pen 10 has an external appearance in which a cap 13 with a clip 14 is attached to the tip of a barrel 11, the rear end of which is fitted with a tail plug 12.

[0017] 2 is a cross-sectional view of the refill 15 mounted inside the barrel 11 of the water-based ballpoint pen 10 of FIG. 1. The refill 15 has a structure in which a ballpoint pen tip 20 is mounted via a joint 17 to the tip of an ink reservoir tube 16 in the shape of a long axis cylinder that contains an aqueous ink composition 40. The ballpoint pen tip 20 has a structure in which a writing ball 30 is mounted at the very end of a holder 21 that is tapered at its tip. A grease-like follower 41 is injected into the rear end of the water-based ink composition 40 to prevent the water-based ink composition 40 from flowing out from the rear end of the refill 15. This follower 41 follows the tip as the water-based ink composition 40 is consumed by writing.

[0018] 3 shows an enlarged cross-sectional view of the vicinity of the tip of the ballpoint pen tip 20. The ballpoint pen tip 20 is composed of a holder 21 having a tapered portion 27 formed so that the tip of the cylindrical body tapers to a narrower diameter, and a spherical writing ball 30 held inside the holder 21. The holder 21 is composed of a back hole 28 drilled from the rear end of the ballpoint pen tip 20, a ball house 22 formed by cutting and expanding the inner circumference near the tip of the holder 21, an ink guide hole 26 penetrating the ball house 22 and the back hole 28, and a crimped portion 23 that is sandwiched between the tip of the inner periphery of the ball house 22 and the tip of the tapered portion 27 and is crimped by plastic deformation toward the center of the writing ball 30. The ballpoint pen tip 20 further has a ball seat 24 provided at the bottom of the ball house 22 and formed around the ink guide hole 26, and ink grooves 25 arranged at equal intervals at four positions around the ink guide hole 26 so as to connect the ball seat 24 and the ink guide hole 26. The width and number of the ink grooves 25 may be changed depending on the viscosity of the aqueous ink composition 40, etc.

[0019] When assembling the holder 21, the writing ball 30 is inserted into the ball house 22 from its tip end. Then, the upper part of the writing ball 30 is pressed toward the rear end, so that the ball seat 24 is deformed to conform to the outer shape of the writing ball 30. Thereafter, the tip of the tapered portion 27 is crimped using a tapered roller to provide the crimped portion 23, thereby forming the holder 21.

[0020] The holder 21 is made of stainless steel having a Vickers hardness of about 200 to 420. The holder 21 can also be made of other metals such as nickel silver, brass, or brass, or resin, but the Vickers hardness (Hv) is preferably 170 to 450.

[0021] Furthermore, in this embodiment, holder 21 is formed by cutting a solid wire material, but the method is not limited to cutting a wire material, and for example, it may be formed by plastic processing a hollow pipe material.

[0022] (2) Writing ball The writing ball 30 of this embodiment is made of a mixture containing tungsten carbide (WC) as a hard phase component, cobalt (Co) and nickel (Ni) as binder phase components, and chromium (Cr). The metal elements mentioned here may be either simple elements or compounds. The mixture may contain other metal elements, such as molybdenum (Mo).

[0023] The proportion of the hard phase components in the entire writing ball 30 is desirably 80 mass % or more.

[0024] The material powders of the hard phase components, binder phase components, and chromium, as well as any other components, are pulverized and mixed to form a roughly spherical mixture, which is then sintered to form a sphere. The resulting sphere is then rolled with diamond powder between two grindstones held at a fixed distance, and the ball surface 31 is mirror-finished to form the writing ball 30. The Vickers hardness (Hv) of the ball surface 31 is 1,600 to 2,000.

[0025] (3) Water-based ink composition 40 The aqueous ink composition 40 of this embodiment contains resin particles having an average particle diameter of 0.3 μm or more. The resin particles may be microspheres (microcapsules) containing a dye or pigment as a colorant. Furthermore, hollow resin may be used as the resin particles. The content of the resin particles is preferably 5 to 30 mass % of the total ink composition. The upper limit of the average particle diameter of the resin particles is not particularly limited as long as it does not impair the fluidity of the ink or the dispersibility of the resin particles, but it is preferable that the upper limit is less than 5 μm. EXAMPLES

[0026] (1) Writing ball Five writing balls were manufactured according to the following compositions:

[0027] (1-1) Ball 1 A writing ball was produced from the mixture having the following composition by the method described above and designated as Ball 1. WC (hard phase component): 91% by mass Co (bond phase component): 5% by mass Ni (bond phase component): 2% by mass Cr 3 C 2 :2 mass%

[0028] (1-2) Ball 2 A writing ball, designated as Ball 2, was produced from a mixture of the following composition by the method described above. WC (hard phase component): 89% by mass Co (bonded phase component): 3% by mass Ni (bond phase component): 5% by mass Cr 3 C 2 :3% by mass

[0029] (1-3) Ball 3 A writing ball, designated as Ball 3, was produced from a mixture of the following composition by the method described above. WC (hard phase component): 86% by mass Co (bond phase component): 10% by mass Ni (bond phase component): 1% by mass Cr 3 C 2 :3% by mass

[0030] (1-4) Ball 4 A writing ball, designated Ball 4, was produced from the mixture having the following composition by the method described above. WC (hard phase component): 85% by mass Co (bond phase component): 10% by mass Cr 3 C 2 :5% by mass

[0031] (1-5) Ball 5 A writing ball, designated as Ball 5, was produced from the mixture having the following composition by the method described above. WC (hard phase component): 91% by mass Ni (bond phase component): 6% by mass Cr3 C 2 :3% by mass

[0032] (2) Ink Inks 1 to 3 were prepared as follows.

[0033] (2-1) Ink 1 (2-1-1) Oil phase solution 12.5 parts by mass of ethyl acetate as an organic solvent was heated to 60° C., and 3.5 parts by mass of an oil-soluble black dye (Oil Black 860, Orient Chemical Industries) as a water-insoluble dye was added thereto and thoroughly dissolved. Next, 8 parts by mass of an isocyanurate-modified product of hexamethylene diisocyanate (TLA-100, Asahi Kasei Chemicals) as a prepolymer was added thereto to prepare an oil phase solution.

[0034] (2-1-2) Aqueous phase solution 200 parts by mass of distilled water was heated to 60° C., and 15 parts by mass of polyvinyl alcohol (PVA-205, Kuraray) serving as a dispersant was dissolved therein to prepare an aqueous phase solution.

[0035] (2-1-3) Emulsion polymerization The oil phase solution was added to the aqueous phase solution heated to 60°C, and the mixture was emulsified and mixed with a homogenizer to complete the polymerization. The resulting dispersion was centrifuged to recover microspheres containing the colorant. The average particle size was 1.5 μm. The average particle size was measured using a particle size distribution analyzer (HRA9320-X100, Nikkiso) with a refractive index of 1.81 and a D calculated on a volume basis. 50 The values ​​were adopted (the same applies to inks 2 and 3 described below).

[0036] The ink composition having the following composition was designated as Ink 1. Microspheres: 15 parts by weight Xanthan gum (thickener, KESLAN S, Sankyo): 0.18 parts by weight Phosphate ester (Plysurf A219B, Daiichi Kogyo Seiyaku): 0.5 parts by mass Preservative (Bioden 421, Yamato Chemical Industry): 0.2 parts by weight Benzotriazole (rust inhibitor): 0.3 parts by weight Aminomethylpropanol (pH adjuster): 0.1 parts by mass, Propylene glycol (solvent): 15 parts by weight, Ion-exchanged water: 68.72 parts by weight

[0037] (2-2) Ink 2 (2-2-1) Thermochromic microcapsule pigment A homogeneous composition was obtained by heating and melting 1 part by mass of ETAC (Yamada Chemical Co., Ltd.) as a leuco dye, 2 parts by mass of bisphenol A as a color developer, and 24 parts by mass of myristyl myristate as a color-changing temperature regulator at 100°C.

[0038] 10 parts by mass of isocyanate and 10 parts by mass of polyol were added as capsule membrane agents to 27 parts by mass of the composition obtained above at 100°C, and the mixture was stirred and mixed. Next, 60 parts by mass of 12% aqueous polyvinyl alcohol solution was added as a protective colloid, and emulsified at 25°C to prepare a dispersion. Next, 5 parts by mass of 5% polyamine was added, and the mixture was treated at 85°C for 45 minutes to obtain core-shell type microcapsules containing a colorant. The average particle size was 2.1 μm.

[0039] The ink composition having the following formulation was designated as Ink 2. Thermochromic microcapsule pigment: 15 parts by weight Xanthan gum (thickener, KESLAN S, Sankyo): 0.3 parts by weight Phosphate ester (Plysurf A219B, Daiichi Kogyo Seiyaku): 0.3 parts by mass Preservative (Bioden 421, Yamato Chemical Industry): 0.2 parts by weight Benzotriazole (rust inhibitor): 0.3 parts by weight Triethanolamine (pH adjuster): 0.1 parts by weight Glycerin (solvent): 10 parts by weight Ion-exchanged water: 73.8 parts by weight

[0040] (2-3) Ink 3 The ink composition having the following composition was designated as Ink 3. Pigment (FUJI RED 2510, Fuji Pigment): 8 parts by weight Pigment dispersant (Joncryl 60, BASF JAPAN): 6 parts by weight Hollow resin particles (Ropeake OP-84J, Dow Chemical, solid content 42.5%, average particle size 0.55 μm): 10 parts by mass Xanthan gum (thickener, KESLAN S, Sankyo): 0.3 parts by weight Phosphate ester (Plysurf A219B, Daiichi Kogyo Seiyaku): 0.3 parts by mass Preservative (Bioden 421, Yamato Chemical Industry): 0.2 parts by weight Benzotriazole (rust inhibitor): 0.3 parts by weight Triethanolamine (pH adjuster): 0.5 parts by weight Glycerin (solvent): 10 parts by weight Ion-exchanged water: 64.4 parts by weight

[0041] (3) Examples and Comparative Examples Using the above-mentioned balls 1 to 5 and inks 1 to 3, the water-based ballpoint pens shown in the above embodiment were prepared.

[0042] (3-1) Example 1 In the water-based ballpoint pen of Example 1, Ball 1 was used as the writing ball. Three types of refills containing Inks 1 to 3 were prepared.

[0043] (3-2) Example 2 In the water-based ballpoint pen of Example 2, Ball 2 was used as the writing ball. Three types of refills containing Inks 1 to 3 were prepared.

[0044] (3-3) Example 3 In the water-based ballpoint pen of Example 3, ball 3 was used as the writing ball. Three types of refills containing inks 1 to 3 were prepared.

[0045] (3-4) Comparative Example 1 Ball 4 was used as the writing ball for the water-based ballpoint pen of Comparative Example 1. Three types of refills containing inks 1 to 3 were prepared.

[0046] (3-5) Comparative Example 2 Ball 5 was used as the writing ball for the water-based ballpoint pen of Comparative Example 1. Three types of refills, each containing Inks 1 to 3, were prepared.

[0047] (4) Evaluation method and results The water-based ballpoint pens of Examples 1 to 3 and Comparative Examples 1 and 2 described above were left uncapped for 60 minutes in an environment of 25°C temperature and 50% humidity, after which a straight line was written on a PPC paper and the initial writing performance was evaluated according to the following evaluation criteria. A: No smudges in the lines are observed from the beginning. B: The lines are fading from the beginning The results based on this evaluation criteria are shown in Table 1 below.

[0048] [Table 1]

[0049] In the water-based ballpoint pens of Examples 1 to 3, which use writing balls 1 to 3 respectively, no smearing of the drawn lines occurs at the beginning of writing regardless of whether inks 1 to 3 are used, making these water-based ballpoint pens excellent in initial writing performance.

[0050] On the other hand, for the aqueous ballpoint pen of Comparative Example 1 using Ball 4, which does not contain nickel, smudged lines were observed at the beginning of writing regardless of whether any of Inks 1 to 3 was used. Similarly, for the aqueous ballpoint pen of Comparative Example 2 using Ball 5, which does not contain cobalt, smudged lines were observed at the beginning of writing regardless of whether any of Inks 1 to 3 was used.

[0051] From the above, it was found that by blending both cobalt and nickel in addition to tungsten carbide and chromium into the composition of the writing ball, the initial writing performance can be improved regardless of the type of resin particles. [Industrial Applicability]

[0052] The present invention can be used in a ballpoint pen that contains a water-based ink containing resin particles. [Explanation of symbols]

[0053] 10 Water-based ballpoint pen 11 Body 12 End cap 13 Cap 14 Clip 15 refill 16 ink reservoir tube 17 joint 20 Ballpoint pen tip 21 Holder 22 Ball house 23 Crimping part 24 Ball seat 25 Ink groove 26 Ink guide hole 27 Tapered portion 28 Back hole 30 Writing ball 31 Ball surface 40 Water-based ink composition 41 Followers

Claims

1. An aqueous ballpoint pen containing an aqueous ink composition containing resin particles having an average particle diameter of 0.3 μm or more, 80% by mass or more of tungsten carbide as a hard phase component; Cobalt and nickel as binder phase components are 11% by mass or less in total, Chromium carbide is 3% by mass or less, A water-based ballpoint pen comprising a ballpoint pen tip having a writing ball made of a mixture comprising:

2. 2. The water-based ballpoint pen according to claim 1, wherein the water-based ink composition contains 5 to 30% by mass of the resin particles.

3. 3. The water-based ballpoint pen according to claim 1, wherein the resin particles contain a colorant.

Citation Information

Patent Citations

  • JP1975031049A

  • JP1977106235U

  • Water-based ball-point ink

    JP1993339534A

  • Ball for ball point pen made of cemented carbide and manufacturing method therefor

    JP2002019366A

  • Ink composition for water-based ballpoint pen

    JP2003155435A