Separator for aluminum electrolytic capacitor and aluminum electrolytic capacitor

A separator for aluminum electrolytic capacitors, composed of natural cellulose and beaten regenerated cellulose fibers, addresses short-circuit and impedance issues by optimizing fiber proportions and mesh configuration, enhancing tear strength and impedance.

JP7554590B2Active Publication Date: 2024-09-20NIPPON KODOSHI
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020114400
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-01
Publication Date
2024-09-20
Estimated Expiration
2040-07-01

AI Technical Summary

Technical Problem

Existing aluminum electrolytic capacitors face issues with short circuits due to separator damage from mechanical stress, electrical stress, and oxide film defects, and there is a need for alternative raw materials that maintain impedance characteristics and strength properties.

Method used

A separator for aluminum electrolytic capacitors made from a combination of natural cellulose fibers and beaten regenerated cellulose fibers, with controlled fiber proportions and mesh configuration to reduce parenchyma cells, ensuring high tear strength, short-circuit resistance, and impedance characteristics.

Benefits of technology

The proposed separator achieves excellent tear strength, reduced short-circuit rates, and improved impedance characteristics, using stably available raw materials like mallow pulp, lindenaceous pulp, and gramineous pulp, while maintaining capacitor performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554590000001
    Figure 0007554590000001
Patent Text Reader

Abstract

To provide a separator for an aluminum electrolytic capacitor, which is formed from a natural cellulose fiber and a beaten regenerated cellulose fiber, and which is superior in tear strength, short-resistance performance and impedance characteristic.SOLUTION: A separator for an aluminum electrolytic capacitor is to be interposed between positive and negative electrodes of an aluminum electrolytic capacitor. The separator comprises 50-90 mass% of a natural cellulose fiber and 50-10 mass% of a beaten regenerated cellulose fiber. The separator is 20-100 mNm2 / g in specific tear strength, and 10% or less in the rate of occurrence of short circuit when being subjected to application of 500 V in a separator dielectric breakdown test.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator for an aluminum electrolytic capacitor that is suitable for use in an aluminum electrolytic capacitor, and to an aluminum electrolytic capacitor using the separator for an aluminum electrolytic capacitor. [Background technology]

[0002] In general, aluminum electrolytic capacitors are made by creating a capacitor element by placing electrolytic paper between anode aluminum foil and cathode aluminum foil as a separator, impregnating this capacitor element with an electrolyte, inserting it into a case, and then sealing it.

[0003] In aluminum electrolytic capacitors, the main role of the separator is to separate the two electrodes and retain the electrolyte. To separate the two electrodes, the separator is required to have low resistance but high shielding properties. Furthermore, the separator material must be electrically insulating, and must be hydrophilic and oleophilic to retain various types of electrolytes. Therefore, separators made from cellulose, which has both of these properties, are used.

[0004] Various configurations have been proposed so far as separators for electrochemical elements, including aluminum electrolytic capacitors (see, for example, Patent Documents 1 to 6). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 53-142652 [Patent Document 2] Japanese Patent Application Publication No. 3-222315 [Patent Document 3] Japanese Patent Application Publication No. 5-315193 [Patent Document 4] Japanese Patent Application Publication No. 8-250376 [Patent Document 5] Japanese Patent Application Publication No. 5-267103 [Patent Document 6] International Patent Publication No. 2017 / 047699 Summary of the Invention [Problem to be solved by the invention]

[0006] Short circuits in aluminum electrolytic capacitors that are related to the separator include (1) compression or breakage of the separator due to the tab part, (2) penetration or breakage of the separator due to burrs on the edge of the electrode foil or burrs at the connection between the electrode foil and the lead wire, (3) breakage of the separator due to mechanical stress such as vibration or impact, (4) electrical stress such as spark discharge, (5) dielectric breakdown of the oxide film due to defects in the oxide film during aging during capacitor manufacturing, etc. The uniformity and strength characteristics of the separator affect resistance to these causes of short circuits, but improving short-circuit resistance is a perpetual challenge for separators.

[0007] Among aluminum electrolytic capacitors, separators using the technology described in Patent Documents 1 and 2, i.e., cylindrical mesh laminated separators made of Manila hemp pulp and Esparto pulp, are commonly used, particularly in the low voltage range of 100V or less. However, Manila hemp pulp is mainly produced in the Philippines, and Esparto pulp is mainly produced in Tunisia. Due to recent political instability and a decrease in the number of people working in the primary industry, it is becoming more difficult to obtain them year by year, and prices are also continuing to rise. Therefore, there is an urgent need to develop alternative products using raw materials that are stably available.

[0008] In aluminum electrolytic capacitors, the separator has a large effect on impedance characteristics, especially equivalent series resistance (ESR). It is known that the closer the cross-sectional shape of the pulp used in the separator is to a circle and the smaller the diameter, the lower the impedance characteristics become. Wood-derived pulp, such as softwood pulp and hardwood pulp, is produced in large quantities and can be obtained stably. However, wood pulp has a flat cross-sectional shape and is large in size, making it unsuitable as a raw material for low-voltage separators, which place importance on impedance characteristics.

[0009] Examples of non-wood pulps that are mass-produced industrially and are available at relatively low cost include mallow plant pulp, linden plant pulp, and grass plant pulp. As separators for aluminum electrolytic capacitors using pulp from grass family plants other than esparto, Patent Document 3 proposes a separator using straw fiber and Manila hemp pulp, and Patent Document 4 proposes a separator using bamboo pulp. However, both Patent Document 3 and Patent Document 4 aim to improve the sound quality of audio equipment. The main required characteristic of a separator for audio equipment is the sound quality sensed by humans, which is significantly different from the impedance characteristic required for a general low-voltage separator.

[0010] Malvaceae pulp, linden pulp, and grass pulp contain many plant-derived parenchyma cells, which are very wide and short compared to pulp. If many parenchyma cells are present in a separator, problems such as a deterioration in impedance characteristics, as well as a decrease in tensile strength and tear strength occur. In addition, mallow pulp, linden pulp, and grass pulp have a short average fiber length of the main fiber compared to coniferous pulp, Manila hemp pulp, and the like, and are inferior in strength characteristics such as tensile strength and tear strength. Therefore, it has been difficult to achieve the short circuit resistance and impedance performance required for general low-voltage separators with a separator mainly made of mallow pulp, linden pulp, and grass pulp.

[0011] Beatable regenerated cellulose fibers have the characteristic that when beaten to a high degree, fibrils with high rigidity and small fiber diameters are generated, and it is known that separators with excellent short-circuit resistance and impedance characteristics can be produced. For this reason, many separators using beatable regenerated cellulose fibers have been proposed in recent years. In addition, since beatable regenerated cellulose fibers are industrial products, they can be steadily obtained.

[0012] Patent Document 5 proposes a method of using beatable regenerated cellulose fibers to increase the density of the separator and improve the impedance characteristics. A separator using beaten regenerated cellulose fibers has a highly dense and microporous paper quality, and an aluminum electrolytic capacitor made using this separator has a reduced short-circuit defect rate and improved impedance characteristics.

[0013] However, when a separator made of 100% by mass of beatable regenerated cellulose fibers is used as in Patent Document 5, the separator may break during the manufacturing process of the aluminum electrolytic capacitor due to its low tensile strength and tear strength. In addition, due to its low strength, it has low resistance to parts that are subject to stress, such as the tabs and foil burrs of the aluminum electrolytic capacitor, and the separator may break and cause a short circuit.

[0014] Patent Document 5 also proposes blending Manila hemp pulp, sisal hemp pulp, etc. with beatable regenerated cellulose fibers. Although blending Manila hemp pulp or sisal hemp pulp with beatable regenerated cellulose fibers improves tensile strength and tear strength, there is a problem that the formation of the separator is poor because the Manila hemp pulp or sisal hemp pulp with a high CSF value that has hardly been beaten has a long fiber length. The longer the fiber length, the more difficult it is to uniformly disperse the fibers in water, and the more difficult it is to form a uniform paper layer during papermaking. In order to improve the formation, it is necessary to shorten the fiber length by further beating the Manila hemp pulp or sisal hemp pulp, but beating Manila hemp pulp or sisal hemp pulp greatly deteriorates the impedance characteristics, so beating has rarely been performed.

[0015] Patent Document 6 proposes a separator made of natural cellulose fiber A, natural cellulose fiber B, and beaten regenerated cellulose fiber, which has improved tensile strength and short-circuit resistance while maintaining the same density and impedance characteristics as a separator made of highly beaten regenerated cellulose. The separator in Patent Document 6 uses natural cellulose fiber with a short average fiber length, which is highly beaten, in order to make a separator with good texture using a Fourdrinier papermaking machine. Therefore, the separator in Patent Document 6 has a relatively short average fiber length, and the tear strength could not be improved compared to a separator made of 100% beatable regenerated cellulose fiber. In the manufacturing process of an aluminum electrolytic capacitor, when tension is applied to the separator, if the separator is twisted, the separator with low tear strength may break.

[0016] An object of the present invention is to provide a separator for an aluminum electrolytic capacitor which is made of natural cellulose fibers and beaten regenerated cellulose fibers and has excellent tear strength, short-circuit resistance and impedance characteristics. Another object of the present invention is to provide an aluminum electrolytic capacitor that includes this separator for an aluminum electrolytic capacitor and has excellent short-circuit resistance and impedance characteristics. [Means for solving the problem]

[0017] The separator for an aluminum electrolytic capacitor of the present invention is an aluminum electrolytic capacitor separator interposed between an anode and a cathode of the aluminum electrolytic capacitor, and comprises natural cellulose fibers and beaten regenerated cellulose fibers, Tear strength is 20 to 100 mN m 2 / g and density is 0.25 to 0.70 g / cm 3 And, The short circuit rate when 500V is applied in the separator insulation breakdown test is 10% or less. The natural cellulose fiber is made of one or more materials selected from the group consisting of Malvaceae plant pulp, Tilia family plant pulp, and Gramineae plant pulp, and the surface to back ratio of the parenchyma cells present on the surface of the separator for aluminum electrolytic capacitor is 5 or less. It is something.

[0018] The aluminum electrolytic capacitor of the present invention comprises an anode, a cathode, and a separator interposed between the anode and the cathode, and the separator is the above-mentioned aluminum electrolytic capacitor separator of the present invention. Effect of the Invention

[0019] According to the present invention described above, it is possible to provide a separator for an aluminum electrolytic capacitor having excellent tear strength, short-circuit resistance and impedance characteristics, and an aluminum electrolytic capacitor using said separator.

[0020] Furthermore, according to the present invention, the short-circuit rate when 500 V is applied in a separator dielectric breakdown test is 10% or less, which makes it possible to construct a separator using inexpensive fibers such as mallow plant pulp, tilia plant pulp, and grass plant pulp. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] An embodiment of the present invention will be described in detail below.

[0022] The separator for an aluminum electrolytic capacitor of the present invention is an aluminum electrolytic capacitor separator interposed between an anode and a cathode of the aluminum electrolytic capacitor, and has a configuration in which the short-circuit rate when 500 V is applied in a separator dielectric breakdown test is 10% or less.

[0023] The aluminum electrolytic capacitor of the present invention comprises an anode, a cathode, and a separator interposed between the anode and the cathode, and the separator is the aluminum electrolytic capacitor separator of the present invention.

[0024] In the separator for aluminum electrolytic capacitor of the present invention, the separator is preferably made of 50 to 90 mass % of one or more kinds of natural cellulose fibers selected from the group consisting of mallow plant pulp, tilia plant pulp, and grass plant pulp, and 50 to 10 mass % of beaten regenerated cellulose fibers, which allows the separator to be made using stably available raw materials.

[0025] Beaten regenerated cellulose fibers have superior short-circuit resistance and impedance characteristics compared to one or more types of natural cellulose fibers selected from the group consisting of mallow plant pulp, linden plant pulp, and grass plant pulp. In addition, by controlling the degree of beating and the average fiber length, it is possible to improve the tensile strength and tear strength compared to a separator consisting of only one or more types of natural cellulose fibers selected from the group consisting of mallow plant pulp, linden plant pulp, and grass plant pulp. Therefore, it is possible to improve the tensile strength and tear strength of a separator consisting of only one or more types of natural cellulose fibers selected from the group consisting of mallow plant pulp, linden plant pulp, and grass plant pulp, particularly at 0.45 g / cm 3 When producing the low-density separator described below, the degree of beating of the natural cellulose fibers to improve the tensile strength can be reduced, and the impedance characteristics of the separator can be improved. If the ratio of the beaten regenerated cellulose fibers is less than 10% by mass, it becomes difficult to obtain the effects of improving short-circuit resistance and strength characteristics, and the effects of reducing impedance.

[0026] It is preferable to use a cylinder-type multi-layer papermaking machine for making the separator of the present invention. The cylinder-type papermaking machine rotates a cylinder covered with a mesh (hereinafter abbreviated as "cylinder") in a tank containing a pulp suspension, and forms a paper layer on the mesh when water flows into the cylinder through the mesh due to the difference in water level. When forming the paper layer, pulp accumulates on the mesh in the early stage, but the mesh gradually becomes clogged in the later stage, so that the fine pulp and parenchyma cells that flow out with the water in the early stage become contained in the paper layer in the middle and later stages. Therefore, paper made by a cylinder-type papermaking machine generally has a different ratio of parenchyma cells present on the front and back sides.

[0027] Malvaceae pulp, linden pulp, and grass pulp contain a large amount of parenchyma cells. The materials constituting the separator can be classified into fibrous pulp and parenchyma cells based on their shape. Compared to pulp, parenchyma cells are very wide and short, which adversely affects the impedance characteristics and tensile strength of the separator. Malvaceae pulp, linden pulp, and grass pulp have a shorter average fiber length than Manila hemp pulp, making it easier to make the paper texture uniform and easier to manufacture separators with excellent density. However, because the average fiber length is short, strength properties such as tensile strength and tear strength tend to be inferior. By reducing the number of parenchyma cells in the separator, the average fiber length can be increased, and strength properties can be improved.

[0028] In the present invention, it is preferable to use multiple circular meshes in order to reduce the number of parenchyma cells remaining in the separator. In other words, a single separator is formed by stacking multiple paper layers made of materials only in the initial stage of paper layer formation, i.e., paper layers with a low parenchyma cell content, and this allows the number of parenchyma cells in the separator to be significantly reduced. By controlling the number of parenchyma cells in the separator, even a separator containing a large amount of mallow plant pulp, linden plant pulp, and grass plant pulp can achieve short-circuit resistance and impedance characteristics that are usable as a separator for an aluminum electrolytic capacitor.

[0029] Beaten regenerated cellulose fibers have fibrils with small fiber diameters, and therefore form a dense paper layer. However, if the proportion of beaten regenerated cellulose fibers in the separator of the present invention is high, the yield of parenchyma cells of natural fibers is improved, and therefore the impedance characteristics are unlikely to decrease even if the blending ratio is increased. Therefore, the proportion of beaten regenerated cellulose fibers in the separator of the present invention must be 50 mass% or less.

[0030] When making paper from the same raw materials, a cylinder papermaking machine can control the weight per unit area of ​​the paper (hereinafter abbreviated as "basis weight") by changing the pulp suspension concentration and the cylinder rotation speed. Therefore, when producing paper of the same basis weight at the same speed, for example, by changing from one cylinder to two cylinders, the pulp suspension concentration can be roughly halved. The thinner the concentration of the pulp suspension, the more the parenchyma cells in the separator can be reduced. It is preferable that the concentration of the pulp suspension be 0.3% or less.

[0031] In the present invention, the size of the mesh openings is also important. The size of typical parenchyma cells is about (20 to several tens of μm) × (20 to 150 μm), and in order to promote the outflow of parenchyma cells, the mesh openings are preferably 0.1 mm or more × 0.1 mm or more.

[0032] By significantly reducing the number of parenchyma cells in the separator, the impedance characteristics of the separator are improved, and even when using mallow plant pulp, linden plant pulp, and grass plant pulp, it is possible to achieve impedance characteristics at the same level as those of cylindrical mesh multi-layer separators made of Manila hemp pulp, esparto pulp, etc.

[0033] As an index of the number of parenchyma cells contained in the separator, it is preferable that the front / back ratio (anti-circular mesh contact surface / circular mesh contact surface) of the number of parenchyma cells present on the separator surface is 5 or less. It is difficult to make the front / back ratio less than 1 because the number of parenchyma cells is small on the surface in contact with the mesh and large on the surface not in contact with the mesh. On the other hand, if the front / back ratio is greater than 5, the outflow of parenchyma cells becomes insufficient, and the impedance characteristics and tensile strength of the separator are likely to deteriorate. In addition, when a separator with a front / back ratio exceeding 5 is used in an aluminum electrolytic capacitor, the short circuit rate is likely to deteriorate due to a decrease in tensile strength, etc. In addition, if it is difficult to distinguish between the rete contact surface and the anti-rete contact surface, the ratio of surfaces with a high number of parenchyma cells to surfaces with a low number of parenchyma cells may be set to 5 or less.

[0034] The pulp of a mallow plant, a linden plant, and a grass plant used in the present invention is not particularly limited, and any fiber can be used. For example, kenaf pulp, jute pulp, rice straw pulp, wheat straw pulp, bamboo pulp, bagasse pulp, reed pulp, sabai grass pulp, tsuga grass pulp, and lalang grass pulp are preferably used. One of these materials may be used, or two or more of them may be mixed and used. In addition, these pulps may be bleached, or may be refined like dissolving pulp, or mercerized pulp.

[0035] The mallow plant pulp, linden plant pulp, and grass plant pulp used in the present invention are preferably beaten, although the beating treatment may not be necessary depending on the density of the separator to be produced.

[0036] Examples of regenerated cellulose fibers used in the present invention include solvent-spun rayon, such as Lyocell, and polynosic rayon, but are not limited to these examples, and any regenerated cellulose fiber that can be beaten can be used.

[0037] Any fiber diameter can be used for the regenerated cellulose fiber before beating, but if the fiber diameter before beating is too large, the fluidity during beating is poor and problems such as clogging are likely to occur. If the fiber diameter before beating is too small, the amount of fibrils generated by beating is reduced, making it difficult to ensure denseness. For this reason, the fiber diameter before beating is preferably 3 to 18 μm.

[0038] The degree of beating of the regenerated cellulose fibers is preferably 200 ml or less in terms of CSF value. If the CSF value is higher than 200 ml, the density of the separator becomes insufficient.

[0039] If the average fiber length is too short, the tear strength will be weak, so the average fiber length of the regenerated cellulose fiber is preferably 1.0 mm or more. If the average fiber length is too long, it will be difficult to uniformly disperse the fiber in water during papermaking, which will cause the separator to have a poor texture and poor short circuit resistance. For this reason, the average fiber length of the regenerated cellulose fiber is preferably 3.5 mm or less.

[0040] For the beating treatment of natural cellulose fibers and regenerated cellulose fibers, any beating machine used for preparing raw materials for papermaking, such as a disc refiner, a conical refiner, a high-pressure homogenizer, a beater, etc., can be used without any particular limitation. The beating treatment of natural cellulose fibers and regenerated cellulose fibers may be carried out separately or in combination.

[0041] When producing the separator, additives such as dispersants, defoamers, and paper strength agents may be used as necessary as long as they do not impair the function of the separator for a capacitor. In addition, the paper strength enhancing processing may be performed by coating a water-soluble polymer after producing the separator.

[0042] When making paper using a cylinder-type multi-layer papermaking machine, the raw materials used for each layer may be the same, or the degree of beating or the type of raw material may be changed. When the same raw materials are used, the process can be simplified.

[0043] As described above, the separator of the present invention is configured such that the short-circuit rate when 500 V is applied in the separator dielectric breakdown test is 10% or less. If the short-circuit rate exceeds 10% when 500V is applied in the separator dielectric breakdown test, short circuits are more likely to occur in the aging test of the aluminum electrolytic capacitor.

[0044] In the separator according to the present invention, the tensile strength of the separator is preferably 9.8 N / 15 mm or more. If the tensile strength is less than 9.8 N / 15 mm, the separator is likely to break during the production of an aluminum electrolytic capacitor element.

[0045] The thickness of the separator is preferably 20 to 120 μm. Since the cross-sectional fiber diameter of mallow plant pulp, linden plant pulp, and grass plant pulp is about 10 to 15 μm, when there are multiple layers formed on a cylinder papermaking machine, if the thickness is made less than 20 μm, it is difficult to maintain the strength required for the separator. If the separator is thicker than 120 μm, it is disadvantageous for miniaturizing the aluminum electrolytic capacitor.

[0046] The density of the separator is 0.25 to 0.70 g / cm 3 is preferred. Density 0.25g / cm 3 If it is lowered, the strength of the separator decreases significantly. Density 0.70g / cm 3 If you try to make it higher, the impedance characteristics of the capacitor will deteriorate significantly.

[0047] The specific tear strength of the separator of the present invention is 20 to 100 mN·m 2 / g, and the separator basis weight is 8 g / m 2 The above is preferred. The separator's specific tear strength is 20mN·m 2 If the tear strength per unit basis weight is less than 1 / g, the separator has a low tear strength and is prone to tearing and breaking in the width direction when the separator is twisted during the manufacturing process of the aluminum electrolytic capacitor. On the other hand, the separator's tear strength is 100 mN m 2If the fiber length exceeds 1 / g, it means that the fiber length of the separator is long. If the fiber length is long, the sheet may lack uniformity and may include areas where the separator density is locally reduced.

[0048] Basis weight 8g / m 2 If the basis weight is less than 8 g / m, the number of fibers constituting the separator is small, and there is a risk of an increase in short-circuit defects in the aluminum electrolytic capacitor, as described above. 2 If the separator has a basis weight of less than 8 g / m, the tear strength is weak even if the specific tear strength is high, and the productivity of aluminum electrolytic capacitors may not be significantly improved. 2 The above is preferred.

[0049] It has been found that the above separator structure makes it possible to obtain a separator for an aluminum electrolytic capacitor which is made of natural cellulose fibers and beaten regenerated cellulose fibers and has excellent tear strength, short-circuit resistance and impedance characteristics.

[0050] The aluminum electrolytic capacitor of the present invention can be produced by using the above-mentioned separator for an aluminum electrolytic capacitor of the present invention. For example, an aluminum electrolytic capacitor can be produced by forming an element by winding an anode aluminum foil and a cathode aluminum foil with a separator interposed between them, impregnating the element with an electrolyte, inserting the element into a case, and then sealing the case. EXAMPLES

[0051] Hereinafter, various specific examples and comparative examples of the separator for an aluminum electrolytic capacitor according to the present invention and an aluminum electrolytic capacitor including the separator for an aluminum electrolytic capacitor will be described in detail.

[0052] [Method of measuring the characteristics of separators and aluminum electrolytic capacitors] Specific measurements of the characteristics of the separator and aluminum electrolytic capacitor of the present embodiment were performed under the following conditions and by the following method.

[0053] [CSF value] The CSF value is a value measured in accordance with JIS P8121-2 "Pulps-Determination of drainability-Part 2: "Canadian Standard" freeness method" (ISO5267-2 "Pulps-Determination of drainability-Part 2: "Canadian Standard" freeness method").

[0054] [Thickness, basis weight and density] The thickness of the separator was measured using a micrometer as specified in "JIS C 2300-2 'Cellulose paper for electrical use - Part 2: Test methods' 5.1 Thickness" in "5.1.1 Measuring instruments and measurement methods a) When using an outside micrometer" and the method of folding the paper into 10 sheets as specified in "5.1.3 When measuring thickness by folding the paper". The basis weight of the separator was measured in an absolute dry state according to the method specified in "JIS C 2300-2 'Cellulose paper for electrical use - Part 2: Test method' 6 Basis weight". The density of the separator was measured in an absolute dry state according to the method specified in "JIS C 2300-2 'Cellulose paper for electrical use - Part 2: Test methods' 7.0A Density Method B".

[0055] [Tensile strength] The maximum tensile load in the longitudinal direction (manufacturing direction) of the separator was measured with a test width of 15 mm using the method specified in "JIS P 8113 'Paper and board-Determination of tensile properties-Part 2: Constant rate of elongation method'" (ISO1924-2 'Paper and board-Determination of tensile properties-Part 2: Constant rate of elongation method'), and this was taken as the tensile strength.

[0056] [Average fiber length] The average fiber length is the length-weighted average fiber length of the contour length (center line fiber length) measured using Kajaani Fiberlab Ver.4 (manufactured by Metso Automation) in accordance with JIS P 8226-2 "Pulps-Determination of fiber length by automated optical analysis-Part 2: Unpolarized light method" (ISO16065-2 "Pulps-Determination of fiber length by automated optical analysis-Part 2: Unpolarized light method").

[0057] [Specific tear strength] The separator's transverse (width) tear strength was measured using the method specified in "JIS P 8116 'Paper - Determination of tearing resistance - Elmendorf method'" (ISO1974 'Paper - Determination of tearing resistance - Elmendorf method'). The tear strength value obtained was then divided by the separator's basis weight to calculate the separator's specific tear strength.

[0058] [Short circuit rate when 500V is applied in separator insulation breakdown test] The separator's dielectric breakdown voltage was measured at a total of 100 locations using the method specified in "JIS C 2300-2 'Cellulose paper for electrical use - Part 2: Test methods' 24. Dielectric breakdown strength 24.2.2 In the case of direct current Method B 24.1.2.1 Method 2," and the percentage of short circuits at voltages of less than 500V was taken as the short circuit rate when 500V was applied in the separator dielectric breakdown test (hereinafter referred to as "short circuit rate when 500V was applied").

[0059] [Ratio of the number of parenchyma cells present on the separator surface to the front and back] Using a scanning electron microscope (hereinafter abbreviated as "SEM"), the number of parenchyma cells present on the front and back surfaces of a separator measuring 1000 μm (vertical) × 5000 μm (horizontal) was measured at a magnification of 200 times. The number of parenchyma cells on the anti-rete side was divided by the number of parenchyma cells on the rete side to obtain the front / back ratio of parenchyma cells present on the separator surface (hereinafter abbreviated as "front / back ratio of parenchyma cells").

[0060] [Preparation of aluminum electrolytic capacitor using separator] A method for producing an aluminum electrolytic capacitor using the separator of this embodiment will be described below. Using the separator having the above configuration, an element was formed by winding an anode aluminum foil and a cathode aluminum foil with the separator interposed between them, and then impregnated with an electrolytic solution, inserted into a case, and sealed to produce an aluminum electrolytic capacitor.

[0061] [Impedance] The impedance of the fabricated aluminum electrolytic capacitor was measured at 20° C. and a frequency of 100 kHz using an LCR meter.

[0062] Example 1 The raw material was a mixture of 60% by mass of kenaf pulp, which is a mallow plant pulp with a CSF value of 550 ml, and 40% by mass of lyocell fiber, which is a beaten regenerated cellulose fiber with a CSF value of 30 ml and an average fiber length of 1.75 mm. The raw material was beaten to a CSF value of 150 ml using a double disc refiner (hereinafter abbreviated as "DDR"), and then produced into a paper with a thickness of 50 μm and a basis weight of 22.5 g / m using a cylinder net three-layer papermaking machine. 2 , density 0.45g / cm 3 The tensile strength of this separator was 24.5N / 15mm and the tear strength was 47.9mN m. 2 / g, the short circuit rate when 500 V was applied was 0.2%, and the front / back ratio of parenchyma cells was 2.5. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.18 Ω.

[0063] Example 2 The raw material was a mixture of 80% by mass of kenaf pulp, which is a mallow plant pulp with a CSF value of 700 ml, and 20% by mass of beaten regenerated cellulose fiber, which has a CSF value of 200 ml and an average fiber length of 3.50 mm. The mixture was beaten to a CSF value of 400 ml using a DDR and made into paper using a cylinder three-layer papermaking machine. The paper was then impregnated with a water-soluble polymer paper strength agent and coated to a thickness of 60 μm and a basis weight of 15.0 g / m. 2 , density 0.25g / cm 3 The tensile strength of this separator was 16.7N / 15mm and the tear strength was 98.0mN m. 2 / g, the short circuit rate when 500 V was applied was 5.8%, and the front / back ratio of parenchyma cells was 1.7. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.15 Ω.

[0064] Example 3 The raw material was a mixture of 50% by mass of jute pulp, which is a linden plant pulp with a CSF value of 100 ml, and 50% by mass of lyocell fiber, which is a beaten regenerated cellulose fiber with a CSF value of 0 ml and an average fiber length of 1.05 mm. The raw material was beaten to a CSF value of 20 ml using a DDR, and then spun into a paper with a thickness of 20 μm and a basis weight of 9.0 g / m using a cylinder-net double-layer papermaking machine. 2 , density 0.45g / cm 3 The tensile strength of this separator was 10.0N / 15mm, and the tear strength was 38.1mN m. 2 / g, the short circuit rate when 500 V was applied was 9.6%, and the front / back ratio of parenchyma cells was 3.7. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.15 Ω.

[0065] Example 4 A raw material consisting of 90% by mass of bamboo pulp, which is a grass plant pulp with a CSF value of 300 ml, and 10% by mass of beaten regenerated cellulose fiber, which is a Lyocell fiber with a CSF value of 10 ml and an average fiber length of 1.35 mm, was mixed and beaten to a CSF value of 200 ml using a DDR. The mixture was then spun into a paper with a thickness of 35 μm and a basis weight of 21.0 g / m using a cylinder-net double-layer papermaking machine. 2 , density 0.60g / cm 3 The tensile strength of this separator was 32.3N / 15mm and the tear strength was 35.0mN m. 2 / g, the short circuit rate when 500 V was applied was 1.6%, and the front / back ratio of parenchyma cells was 2.8. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.18 Ω.

[0066] Example 5 A raw material consisting of 50% by mass of wheat straw pulp, which is a grass plant pulp with a CSF value of 400 ml, and 50% by mass of beaten regenerated cellulose fiber, which is a Lyocell fiber with a CSF value of 100 ml and an average fiber length of 2.55 mm, was beaten to a CSF value of 160 ml using a DDR, and then spun into a paper with a thickness of 40 μm and a basis weight of 20.0 g / m using a cylinder-net double-layer papermaking machine. 2 , density 0.50g / cm 3 The tensile strength of this separator was 16.7N / 15mm, and the tear strength was 27.0mN m. 2 / g, the short circuit rate when 500 V was applied was 0.8%, and the front / back ratio of parenchyma cells was 4.8. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.22 Ω.

[0067] Example 6 A raw material consisting of 70% by mass of longhorn grass pulp, which is a grass plant pulp with a CSF value of 650 ml, and 30% by mass of beaten regenerated cellulose fiber, which is a polynosic rayon fiber with a CSF value of 70 ml and an average fiber length of 2.20 mm, was beaten to a CSF value of 380 ml using a DDR, and then spun into a paper with a thickness of 50 μm and a basis weight of 25.0 g / m using a cylinder net double-layer papermaking machine. 2 , density 0.50g / cm 3 The tensile strength of this separator was 29.4N / 15mm and the tear strength was 37.2mN m. 2 / g, the short circuit rate when 500 V was applied was 0.0%, and the front / back ratio of parenchyma cells was 4.1. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.20 Ω.

[0068] Comparative Example 1 The raw material was a mixture of 80% by mass of kenaf pulp, which is a mallow plant pulp with a CSF value of 700 ml, and 20% by mass of beaten regenerated cellulose fiber, which has a CSF value of 230 ml and an average fiber length of 3.70 mm. The mixture was beaten to a CSF value of 460 ml using a DDR and made into paper using a cylinder-net three-layer papermaking machine. The paper was then impregnated with a water-soluble polymer paper strength agent and finished to a thickness of 65 μm and a basis weight of 15.0 g / m. 2 , density 0.23g / cm 3 The tensile strength of this separator was 10.8N / 15mm, and the tear strength was 104.9mN m. 2 / g, the short circuit rate when 500 V was applied was 16.4%, and the front / back ratio of parenchyma cells was 1.5. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to create an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, and a diameter of 12.5 mm and a length of 20 mm. This aluminum electrolytic capacitor shorted out during the aging test, but the impedance of the capacitor that did not short out was 0.16 Ω.

[0069] Comparative Example 2 Using the same raw materials as in Example 3, a cylinder-type two-layer papermaking machine was used to produce a paper with a thickness of 18 μm and a basis weight of 7.7 g / m 2 , density 0.43g / cm 3 The tensile strength of this separator was 9.0N / 15mm and the tear strength was 38.0mN m. 2 / g, the short circuit rate when 500 V was applied was 23.0%, and the front / back ratio of parenchyma cells was 3.3. 500 capacitor elements were made using this separator, impregnated with an EG-based electrolyte, and then inserted into a case and sealed to create an aluminum electrolytic capacitor with a rated voltage of 100V, a capacity of 100μF, and a diameter of 12.5mm x length of 20mm. When making the capacitor elements, the separator broke during element production due to its weak tensile strength. This aluminum electrolytic capacitor shorted out during an aging test, but the impedance of the capacitor that did not short out was 0.13Ω.

[0070] Comparative Example 3 A raw material consisting of 95% by mass of bamboo pulp (grass plant pulp) with a CSF value of 300 ml and 5% by mass of beaten regenerated cellulose fiber (CSF value of 10 ml and average fiber length of 1.35 mm) was mixed and beaten to a CSF value of 270 ml using a DDR. The mixture was then spun into a paper with a thickness of 35 μm and a basis weight of 21.0 g / m using a cylinder-net double-layer papermaking machine. 2 , density 0.60g / cm 3 The tensile strength of this separator was 23.5N / 15mm and the tear strength was 23.3mN m. 2 / g, the short circuit rate when 500 V was applied was 2.6%, and the front / back ratio of parenchyma cells was 2.5. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.20 Ω.

[0071] Comparative Example 4 Bamboo pulp, which is a grass plant pulp, was beaten to a CSF value of 300 ml using a DDR, and then spun into paper with a thickness of 35 μm and a basis weight of 21.0 g / m using a cylinder-net two-layer papermaking machine. 2 , density 0.60g / cm 3 The tensile strength of this separator was 23.5N / 15mm and the tear strength was 22.4mN m 2 / g, the short circuit rate when 500 V was applied was 2.8%, and the front / back ratio of parenchyma cells was 2.4. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.20 Ω.

[0072] Comparative Example 5 A raw material consisting of 40% by mass of wheat straw pulp (grass plant pulp) with a CSF value of 400 ml and 60% by mass of beaten regenerated cellulose fiber (lyocell fiber) with a CSF value of 100 ml and an average fiber length of 2.55 mm was mixed and beaten to a CSF value of 140 ml using a DDR. The mixture was then spun into a paper with a thickness of 40 μm and a basis weight of 20.0 g / m using a cylinder-net two-layer papermaking machine. 2 , density 0.50g / cm 3 The tensile strength of this separator was 18.6N / 15mm, and the tear strength was 28.4mN m. 2 / g, the short circuit rate when 500 V was applied was 0.4%, and the front / back ratio of parenchyma cells was 5.3. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.27 Ω.

[0073] Comparative Example 6 A raw material consisting of 50% by mass of wheat straw pulp, which is a grass family plant pulp with a CSF value of 200 ml, and 50% by mass of beaten regenerated cellulose fiber, which is a Lyocell fiber with a CSF value of 0 ml and an average fiber length of 0.95 mm, was beaten to a CSF value of 40 ml using a DDR, and then spun into a paper with a thickness of 30 μm and a basis weight of 15.0 g / m using a cylinder net three-layer papermaking machine. 2 , density 0.50g / cm 3 The tensile strength of this separator was 14.7N / 15mm, and the tear strength was 18.3mN m. 2 / g, the short circuit rate when 500 V was applied was 0.4%, and the front / back ratio of parenchyma cells was 4.6. 500 capacitor elements were made using this separator, impregnated with an EG-based electrolyte, and then inserted into a case and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100V, a capacity of 100μF, and a diameter of 12.5mm x length of 20mm. Due to the low tear strength and specific tear strength, the separator broke during the production of the capacitor element. This aluminum electrolytic capacitor did not short circuit in the aging test, and had an impedance of 0.21Ω.

[0074] Comparative Example 7 The same raw material as in Example 6 was used to make a cylinder-type paper machine into a paper having a thickness of 50 μm and a basis weight of 25.0 g / m. 2 , density 0.50g / cm 3 The tensile strength of this separator was 28.4N / 15mm, and the tear strength was 36.8mN m. 2 / g, the short circuit rate when 500 V was applied was 2.4%, and the front / back ratio of parenchyma cells was 6.8. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.26 Ω.

[0075] [Conventional Example 1] Manila hemp pulp, which is a Musaceae plant pulp, and esparto pulp, which is a Gramineae plant pulp, were mixed in half and beaten using a DDR to a CSF value of 550 ml. The paper was then made into a paper with a thickness of 50 μm and a basis weight of 25.0 g / m using a cylinder-net two-layer papermaking machine. 2 , density 0.50g / cm 3 The tensile strength of this separator was 29.4N / 15mm and the tear strength was 32.9mN m. 2 / g, the short circuit rate when 500 V was applied was 4.0%, and the front / back ratio of parenchyma cells was 1.9. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.20 Ω.

[0076] [Conventional Example 2] Manila hemp pulp, which is a Musaceae plant pulp, and wheat straw pulp, which is a Gramineae plant pulp, were mixed in half and beaten using a DDR to a CSF value of 600 ml. The paper was then made into a paper with a thickness of 60 μm and a basis weight of 30.0 g / m using a cylinder three-layer papermaking machine. 2 , density 0.50g / cm 3 The tensile strength of this separator was 34.3N / 15mm and the tear strength was 24.2mN m. 2 / g, the short circuit rate when 500 V was applied was 3.7%, and the front / back ratio of parenchyma cells was 5.5. Using this separator, 500 capacitor elements were made, which were then impregnated with an EG-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 100 V, a capacity of 100 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit in an aging test, and had an impedance of 0.31 Ω.

[0077] Table 1 shows the evaluation results of impedance of the separators and capacitors with a rated voltage of 100 V of Examples 1 to 6, Comparative Examples 1 to 7, Conventional Examples 1 and 2.

[0078] [Table 1]

[0079] The separator of Example 2 used Lyocell fiber with a CSF value of 200 ml and an average fiber length of 3.50 mm, while the separator of Comparative Example 1 used Lyocell fiber with a CSF value of 230 ml and an average fiber length of 3.70 mm. The separator of Comparative Example 1 had a poor formation due to the longer average fiber length of the raw material, and the density was 0.25 g / cm. 3 As a result, the short-circuit rate at 500 V application worsened to 16.4%. In addition, the separator of Comparative Example 1 had a specific tear strength of 100 mN m 2 / g, exceeding 104.9 mN m 2 / g. Specific tear strength is 100mN·m 2 If the density exceeds 0.25 g / cm3, the average fiber length of the raw material becomes too long, which leads to poor formation and reduced short-circuit resistance of the separator. 3 Below this, the tensile strength decreases significantly.

[0080] The separators of Example 3 and Comparative Example 2 were made using the same raw materials on a cylinder-net double-layer papermaking machine, but the separator of Example 3 had a thickness of 20 μm and a basis weight of 9.0 g / m 2 The separator of Comparative Example 2 had a thickness of 18 μm and a basis weight of 7.7 g / m 2The separator of Comparative Example 2 was made using a multi-layer cylinder paper machine, but because the thickness was less than 20 μm, the tensile strength was significantly reduced to 9.0 N / 15 mm due to an insufficient number of overlapping fibers, and the separator broke during the production of the capacitor element. In addition, as a result of the reduced short-circuit resistance, the short-circuit rate when 500 V was applied was 23.0%, and aging shorts occurred. There is a relationship between the short-circuit rate when 500 V is applied and shorts in the aging test of the aluminum electrolytic capacitor, and in order to suppress shorts in the aging test of the aluminum electrolytic capacitor, it is necessary to make the short-circuit rate of the separator 10% or less when 500 V is applied. In addition, the separator of the present invention has a thickness of 20 μm or more and a basis weight of 8.0 g / m 2 More preferably, it is equal to or greater than this.

[0081] The separators of Example 4, Comparative Example 3, and Comparative Example 4 are of the same thickness and density, but were made by changing the compounding ratio of bamboo pulp and lyocell fiber. The proportion of regenerated cellulose fiber in the separator of Example 4 is 10% by mass, while that of Comparative Example 3 is 5% by mass, and that of Comparative Example 4 is 0% by mass. The separator of Example 4 is superior to the separator of Comparative Example 4 in tensile strength, tear strength ratio, and short circuit rate when 500 V is applied. On the other hand, the separator of Comparative Example 3 had almost the same values ​​as the separator of Comparative Example 4 in terms of tensile strength, tear strength ratio, and short circuit rate when 500 V was applied. In order to obtain the effects of improving short-circuit resistance and strength properties, reducing impedance, etc. by adding beaten regenerated cellulose fibers, the proportion of beaten regenerated cellulose fibers must be 10 mass% or more.

[0082] The separators of Example 5 and Comparative Example 5 are separators of the same thickness and density, which are produced by changing the blending ratio of wheat straw pulp and Lyocell fiber. Generally, beaten regenerated cellulose fibers have superior impedance characteristics compared to natural cellulose fibers, so the impedance of the separator decreases as the blending ratio increases. However, the impedance of the capacitor using the separator of Comparative Example 5, which has a higher ratio of Lyocell fiber, is higher than that of the capacitor using the separator of Example 5, which has a lower ratio of Lyocell fiber. This is because the beaten regenerated cellulose fibers have many fibrils with small fiber diameters, which improves the density of the separator and captures the parenchyma cells in the natural cellulose fibers that would have flowed out into the white water during papermaking using a cylinder papermaking machine, thereby improving the ratio of parenchyma cells in the separator. When making paper by mixing natural cellulose fibers containing a large amount of parenchyma cells, particularly pulp from mallow plants, tilia plants, or grass plants, with beaten regenerated cellulose fibers, the proportion of beaten regenerated cellulose fibers must be 50 mass% or less.

[0083] The separators of Example 6 and Comparative Example 7 were made using the same raw materials and using a cylinder wire double layer paper machine or a cylinder wire single layer paper machine. The separator of Comparative Example 7 made using a cylinder wire single layer paper machine had a higher proportion of soft cells in the separator than the separator of Example 6 made using a cylinder wire double layer paper machine, so the tensile strength and tear strength ratio were slightly lower and the impedance of the capacitor was significantly worse. It is preferable to use a cylinder wire multilayer paper machine for making the separator of the present invention.

[0084] Example 7 A raw material consisting of 50% by mass of bagasse pulp, which is a grass plant pulp with a CSF value of 650 ml, and 50% by mass of beaten regenerated cellulose fiber, which is a Lyocell fiber with a CSF value of 200 ml and an average fiber length of 3.50 mm, was beaten to a CSF value of 300 ml using a DDR, and then produced using a cylinder-net three-layer papermaking machine with a thickness of 120 μm and a basis weight of 81.6 g / m 2 , density 0.68g / cm 3The tensile strength of this separator was 73.5N / 15mm and the tear strength was 30.0mN m. 2 / g, the short circuit rate when 500 V was applied was 0.0%, and the front / back ratio of the parenchyma cells was 4.8. Using this separator, 500 capacitor elements were produced, which were then impregnated with a GBL-based electrolyte, inserted into a case, and sealed to produce an aluminum electrolytic capacitor with a rated voltage of 400 V, a capacity of 10 μF, a diameter of 12.5 mm, and a length of 20 mm. This aluminum electrolytic capacitor did not short circuit during an aging test. Thus, it was confirmed that the separator of the present invention can also be applied to so-called medium- and high-voltage GBL-type aluminum electrolytic capacitors.

[0085] As described above, according to the present embodiment, it is possible to provide a separator for an aluminum electrolytic capacitor that is made using Malvaceae plant pulp, Tiliaceae plant pulp, and Gramineae plant pulp, which are stably available over the medium to long term, and beaten regenerated cellulose fibers, and that has excellent tear strength, short circuit resistance, and impedance characteristics, and an aluminum electrolytic capacitor that uses the separator.

[0086] An example in which the separator of this embodiment is used in an aluminum electrolytic capacitor has been described above. Although the details of other configurations and manufacturing methods of the aluminum electrolytic capacitor are omitted, the electrode materials and electrolyte materials in the aluminum electrolytic capacitor of the present invention do not need to be particularly limited, and various materials can be used. In addition, as long as the outer diameter of the element allows, it is also possible to use a plurality of separators of the present invention, or to use one or more separators of the present invention and stack them together with other separators.

Claims

1. A separator for an aluminum electrolytic capacitor, which is interposed between an anode and a cathode of the aluminum electrolytic capacitor, The separator for the aluminum electrolytic capacitor comprises 50 to 90% by mass of natural cellulose fibers and 50 to 10% by mass of beaten regenerated cellulose fibers, Tear strength is 20 to 100 mN / m 2 / g, The density is 0.25 to 0.70 g / cm 3 , In the separator dielectric breakdown test, the short circuit rate when 500 V is applied is 10% or less. The natural cellulose fibers are made of one or more materials selected from the group consisting of mallow plant pulp, linden plant pulp, and grass plant pulp, The ratio of the surface to the back of the soft cells present on the surface of the separator for an aluminum electrolytic capacitor is 5 or less.

1. A separator for an aluminum electrolytic capacitor comprising:

2. 2. The separator for an aluminum electrolytic capacitor according to claim 1, wherein the separator for an aluminum electrolytic capacitor has a thickness of 20 to 120 μm.

3. An anode, a cathode, and a separator interposed between the anode and the cathode, The separator for an aluminum electrolytic capacitor according to claim 1 or 2 is used.

1. An aluminum electrolytic capacitor comprising:

Citation Information

Patent Citations

  • Paper for electrolytic capacitor

    JP1978142652A

  • Electrolytic paper for electrolytic capacitor

    JP1991222315A

  • Electrolytic capacitor

    JP1993267103A

  • Electrolytic capacitor

    JP1993315193A

  • Aluminum electrolytic capacitor

    JP1996250376A