Water-based ink composition for writing implements and writing implements using the same
A water-based ink composition using polyamide resin and fatty acid amide stabilizes pigment dispersibility, addressing sedimentation and blurring issues, ensuring stable and clear handwriting in writing instruments.
Patent Information
- Application Number
- JP2020211015
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-25
- Filing Date
- 2020-12-21
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-12-21
AI Technical Summary
Existing water-based ink compositions for writing instruments face issues with pigment sedimentation, leading to shading and blurring of handwriting due to differences in specific gravity between pigments and solvents, which necessitate the use of metal agitators or result in unsuitable ink viscosity for low viscosity inks like marking pens and fountain pens.
A water-based ink composition comprising polyamide resin and fatty acid amide, with specific content ratios and solubility parameters, forms a three-dimensional network structure to stabilize pigment dispersibility and suppress sedimentation, enhancing color tone and preventing blurring.
The composition effectively stabilizes pigment dispersibility, preventing sedimentation and blurring, while maintaining suitable viscosity for smooth ink discharge, thereby improving handwriting quality and stability over time.
Smart Images

Figure 0007554661000002 
Figure 0007554661000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous ink composition for a writing instrument, and more specifically, to an aqueous ink composition for a writing instrument that inhibits sedimentation of colorants (pigments), resin particles, etc., produces excellent handwriting color tones, and inhibits handwriting smearing, and to a writing instrument using the same. [Background technology]
[0002] Conventionally, aqueous ink compositions for writing instruments using pigments have been well known. In the case of such aqueous ink compositions for ballpoint pens using pigments, unlike dye-based aqueous ink compositions, the use of pigments with a large difference in specific gravity from the ink causes aggregation of the pigments and the associated sedimentation, which causes problems such as uneven shading of handwriting during long-term storage and an effect on the color tone of handwriting when written. In particular, in inks using metallic pigments or pearlescent pigments, the specific gravity of the pigment is greater than that of the solvents generally used in ink compositions, so the pigment is prone to settling in the ink and the ink has poor stability over time.
[0003] In order to solve these problems, proposals have been made such as JP-A-63-152681 ("Water-Based Black Pigment Ink for Ballpoint Pens"), which uses a polymer dispersant as the pigment dispersant; JP-A-11-12524 ("Water-Based Glossy Ink Composition"), which uses a fatty acid ester of polyoxyethylene diglycerin borate; and JP-A-7-118592 ("Water-Based Metallic Glossy Color Ink for Ballpoint Pens"), which uses the seed polysaccharide guar gum, locust bean gum, as a gelling agent.
[0004] However, when the ink viscosity of the aqueous ink composition for writing instruments of Patent Documents 1 and 2 is set to a low value in order to set the ink viscosity suitable for marking pen ink, fountain pen ink, etc., or to improve the color tone (metallic luster) of handwriting by increasing the ink discharge amount, there is a problem that pigment sedimentation and the accompanying hard caking occur because the metallic pigment and pearl pigment have a large specific gravity. Therefore, as a countermeasure against pigment sedimentation and the accompanying hard caking, it is necessary to insert a metallic agitator into the ink storage tube and redisperse the pigment. Furthermore, in Patent Document 3, a gelling agent is used to increase the ink viscosity and the viscosity is set to 10,000 to 150,000 (mPa s). This makes it possible to suppress pigment sedimentation and does not require a metal stirrer. However, the ink viscosity is too high and is not suitable for low-viscosity inks such as marking pen inks and fountain pen inks. Furthermore, the ink ejection volume is small, so the color tone (metallic luster) of the handwriting is insufficient and the handwriting becomes smudged. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] "Unexamined Japanese Patent Publication No. 63-152681" [Patent Document 2] "Unexamined Japanese Patent Publication No. 11-12524" [Patent Document 3] "Unexamined Japanese Patent Publication No. 7-118592" Summary of the Invention [Problem to be solved by the invention]
[0006] In view of the above problems, the object of the present invention is to provide a water-based ink composition for a writing instrument, which suppresses settling of colorants (pigments), resin particles, etc., thereby eliminating the need to place a metal stirrer in the ink reservoir, and which also produces excellent color tones in handwriting and suppresses smearing of handwriting, and a writing instrument using the same. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention provides "1. A water-based ink composition for a writing instrument, comprising water, a colorant, a polyamide resin, and a fatty acid amide. 2. The water-based ink composition for writing instruments according to item 1, wherein the total content of the polyamide resin and the fatty acid amide is 0.01 to 5% by mass based on the total amount of the ink composition. 3. The water-based ink composition for a writing instrument according to item 1 or 2, wherein the colorant is a metallic pigment. 4. The aqueous ink composition for a writing instrument according to any one of items 1 to 3, characterized in that the aqueous ink composition for a writing instrument contains a solvent having a solubility parameter of 8 to 12. 5. The aqueous ink composition for a writing instrument according to any one of claims 1 to 4, characterized in that the pH value of the aqueous ink composition for a writing instrument is 6 to 10. 6. A writing instrument, characterized in that the aqueous ink composition for a writing instrument according to any one of items 1 to 5 is directly packed in an ink reservoir. Let us assume that. Effect of the Invention
[0008] The present invention has the effect of stabilizing the dispersibility of colorants (pigments) and resin particles in an aqueous ink composition for writing instruments, suppressing the settling of colorants (pigments), resin particles, etc., resulting in even handwriting, excellent color tones, and suppressing smudges in handwriting. BEST MODE FOR CARRYING OUT THEINVENTION
[0009] The feature of the present invention is that by providing an aqueous ink composition for a writing instrument comprising a polyamide resin and a fatty acid amide, the dispersibility of the colorant (pigment) and resin particles is stabilized, and sedimentation of the colorant (pigment), resin particles, etc. is suppressed, resulting in even handwriting, excellent color tone, and suppression of handwriting smearing.
[0010] The polyamide resin used in the present invention can stabilize the dispersion of colorants (pigments) and resin particles and suppress sedimentation by using it in combination with a fatty acid amide. This is because polyamide resins form a three-dimensional network structure by interaction with a solvent such as water, but by using fatty acid amide in combination, the polyamide resins are mutually entangled to form a denser three-dimensional network structure, and by forming a strong network structure, the colorant (pigment), resin particles, etc. are hooked to the formed three-dimensional network structure, suppressing the sedimentation of the colorant (pigment) and resin particles, and in particular, the dispersibility of pigments with a large specific gravity can be stabilized, and the sedimentation of pigments can be suppressed, even for metal pigments with a large specific gravity. In addition, by stabilizing the pigment dispersion, the sedimentation of pigments can be easily suppressed, handwriting is less likely to become shady, and the color tone (metallic luster) is more likely to be good. In particular, when a metal pigment containing metal powder is used, the orientation of the metal powder is easily stabilized, and the metallic luster of handwriting is easily obtained, which is preferable.
[0011] (Polyamide resin, fatty acid amide) Polyamide-based resins are resins having amide bonds, and examples thereof include polyamides and modified polyamides. By neutralizing the polyamide resins with a neutralizing agent, they tend to form a stable structure with fatty acid amides in the ink, and therefore it is preferable to convert them into polyamide salts, and from further consideration, it is preferable to convert them into polyamide amine salts.
[0012] The fatty acid amide can be obtained by reacting a carboxylic acid having 2 to 22 carbon atoms with a diamine having 2 to 12 carbon atoms or a monoamine having 2 to 22 carbon atoms. Examples of monocarboxylic acids having 2 to 22 carbon atoms include acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, oleic acid, behenic acid, etc. These may be used alone or in combination of two or more. Examples of diamines having 2 to 12 carbon atoms include ethylenediamine, 1,4-diaminobutane, hexamethylenediamine, metaxylylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine, 1,12-dodecamethylenediamine, etc., and examples of monoamines having 2 to 22 carbon atoms include ethylamine, monoethanolamine, propylamine, butylamine, pentylamine, hexylamine, octylamine, decylamine, laurylamine, myristylamine, cetylamine, stearylamine, behenylamine, etc. These may be used alone or in combination of two or more.
[0013] Furthermore, if the total content of the polyamide resin and the fatty acid amide is less than 0.01% by mass relative to the total amount of the ink composition, the desired inhibition of sedimentation of the colorant (pigment) and resin particles and the desired color tone of the handwriting cannot be obtained, whereas if it exceeds 5% by mass, the ink dischargeability is likely to deteriorate and the color tone of the handwriting is likely to deteriorate. Therefore, the total content is preferably 0.01 to 5% by mass, and from further consideration, 0.1 to 3% by mass is more preferable, and from further consideration, 0.3 to 3% by mass is more preferable, and further 0.5 to 2% by mass is more preferable.
[0014] When a polyamide resin is used in combination with a fatty acid amide, the three-dimensional network structure is easily formed stably, and in consideration of improving dispersibility, it is preferable to mix the polyamide resin with a solvent in advance to form a mixture of the polyamide resin and the fatty acid amide, and from a more particular consideration, it is preferable to mix a solvent having a solubility parameter (value) of 8 to 12 as the solvent. The acid value of the mixture of the polyamide resin and the fatty acid amide is preferably 40 (mgKOH / g) or less. This is because it is easy to keep the three-dimensional network structure formed by the polyamide resin and the fatty acid amide dense, easy to form a stable structure that easily catches colorants (pigments) and resin particles, easy to suppress sedimentation, and easy to improve the color tone (metallic gloss) of handwriting. In consideration of suppressing the sedimentation of the pigment, it is preferable that the acid value is 30 (mgKOH / g) or less, and more preferably, it is 20 (mgKOH / g) or less, and more preferably, the acid value is 3 to 20 (mgKOH / g). The acid value of polyamide resins can be determined by known methods, for example, by dissolving the resin in a 1:1 solution of xylene and dimethylformamide, titrating it with a 0.1 mol / L potassium hydroxide-ethanol solution by potentiometric titration, and calculating the acid value from the amount of potassium hydroxide solution titrated to the end point. In detail, this can be done based on "JIS-K2501-2003 Petroleum products and lubricants - Neutralization number test method".
[0015] Specific examples of the mixture of the polyamide resin and fatty acid amide include Disparlon AQH-800 and Disparlon AQH-810 (both manufactured by Kusumoto Chemicals Co., Ltd.).
[0016] (Coloring agent) The colorant used in the present invention may be a pigment or a dye, and is not particularly limited. However, the aqueous ink composition for a writing instrument containing a polyamide resin and a fatty acid amide as in the present invention has the effect of stabilizing the pigment dispersion, and is therefore effective in pigment inks, and is therefore preferred. In particular, the composition is more effective when a metal pigment is used, since it can stabilize the dispersion of a pigment having a high specific gravity and inhibit the pigment from settling. Examples of pigments include inorganic, organic, and processed pigments, and more specifically, carbon black, aniline black, ultramarine, yellow lead, phthalocyanine, azo, quinacridone, quinophthalone, threne, triphenylmethane, perinone, perylene, dioxazine, microcapsules, metal pigments, fluorescent pigments, phosphorescent pigments, and complementary color pigments. Examples of dyes that can be used include direct dyes, acid dyes, basic dyes, metal-containing dyes, and various salt-forming dyes. These pigments and dyes may be used alone or in combination of two or more.
[0017] In the present invention, when a metal pigment is used as a colorant, examples of the metal pigment include metal powders of aluminum, brass, stainless steel, bronze, titanium oxide, iron oxide, aluminum oxide, zinc oxide, and the like, metal powders of alloys, and pigments containing at least these metals. Specifically, metal powders of aluminum powder, brass powder, stainless steel powder, bronze powder, titanium oxide, and the like may be used as metal pigments as they are, or metal pigments in which a colorant is adsorbed onto these metal pigments may be used. In addition, the metal powder pigments such as aluminum powder may be processed and dispersed in advance with a surfactant, resin, solvent, and the like to form a paste-like pigment dispersion or a liquid metal pigment dispersion, or the metal powder pigments such as aluminum powder may be processed or dispersed with wax, surfactant, resin, and the like to form a solid metal pigment that does not contain a solvent. Examples of metallic pigments include aluminum paste pigments, aluminum powder pigments, titanium oxide pigments, metal vapor deposition powder pigments (pigments in which a thin metal film is coated with a resin), glass flake pigments, and pearl pigments.
[0018] The metallic pigment is preferably a metallic pigment coated with a coating material such as silica, molybdenum, or a phosphoric acid compound such as phosphate, phosphonic acid, or phosphoric acid ester, etc. This is because the use of a metallic pigment coated with a coating material such as silica makes it easier for the metallic pigment to stably become entangled with the three-dimensional network structure formed by the polyamide resin and fatty acid amide, making the metallic pigment less likely to settle. Furthermore, metal pigments coated with a coating material such as silica are preferred because they have low reactivity with water and solvents and high stability, and therefore are less susceptible to bubble generation and deterioration of metallic luster over time, and among the above coatings, silica coating and phosphate compound coating are preferred because of their low reactivity with water and solvents and high stability. From further consideration, phosphate compound coating is more preferred.
[0019] In addition, the amount of the metal pigment coated with the silica or the like is preferably 0.001 to 0.5 times the total mass of the coating material such as the silica or the phosphate compound relative to the total mass of the metal powder in the total amount of the ink composition. This is because if it is less than 0.001 times, it is difficult to coat the entire surface of the metal powder, and it is difficult to obtain the above-mentioned effects such as the inhibition of metal pigment sedimentation, and if it exceeds 0.5 times, the coating material is likely to be surplus to the metal powder, and the surplus is likely to precipitate or generate metal salt precipitates. From a further consideration, it is preferable that the content ratio is 0.01 to 0.3 times by mass, and more preferably 0.01 to 0.1 times.
[0020] Among the phosphoric acid compound coatings, phosphonic acid coatings are preferred, and alkylphosphonic acid coatings are more preferred. This is a phosphonic acid compound having an alkyl group, and since both the phosphonic acid group and the alkyl group of the alkylphosphonic acid are easily adsorbed to the metal powder, the adsorption is stable for a long period of time, and the long-term stability over time is better than that of conventional metal pigments, and the above-mentioned effects are easily obtained over a long period of time. In particular, in consideration of the dispersibility of the metal pigment, it is preferable to use a metal pigment in which the metal powder has been surface-treated with an alkylphosphonic acid, and more preferably, it is preferable to use a metal pigment in which the metal powder has been surface-treated in advance with an alkylphosphonic acid.
[0021] Regarding the alkylphosphonic acid, the number of carbon atoms in the alkyl group is preferably 1 to 20 in consideration of improving the adsorption to the metal powder, suppressing the elution of metal ions, improving the inhibition of pigment sedimentation (dispersibility of metal pigment), and improving the ink stability over time by suppressing metal salt precipitation, and also considering the metallic luster of the handwriting. This is because the longer the alkyl group, the wider the adsorption area and the easier it is to be adsorbed to the metal powder. From further consideration, the number of carbon atoms in the alkyl group is preferably 1 to 12, and from further consideration, the number of carbon atoms in the alkyl group is 6 to 10, and most preferably the number of carbon atoms in the alkyl group is 8. Furthermore, the alkyl group is not limited to those having a straight chain structure or a branched chain structure, but an alkyl group having a straight chain structure is preferable because it has a wider adsorption area and is easier to be adsorbed to the metal powder, and is more preferable because it tends to improve the inhibition of metal pigment sedimentation (dispersibility of metal pigment).
[0022] Furthermore, in consideration of suppressing sedimentation of the metal pigment (metal pigment dispersibility) and improving the color tone of the handwriting (metallic luster), it is preferable to use an aluminum paste pigment or a metal vapor-deposited powder pigment, and from further consideration, it is preferable to use an aluminum paste pigment.
[0023] Among metal pigments, those using aluminum powder are preferred because the metallic luster of the handwriting is good, the specific gravity is relatively small among metals, and the metal powder is less likely to settle. Regarding the shape of the metal powder, if it is shaped like a scale, a corner, or a plate, it is likely to be caught in the three-dimensional network structure formed by the polyamide resin and the fatty acid amide, suppressing the sedimentation of the metal pigment, and further, such a shape is preferred because it is easy to diffuse light and makes the metallic luster clearer. There are also leafing and non-leafing types, and the leafing type is more preferred because the metal powder floats and is arranged on the surface layer of the ink film, making the metallic luster of the handwriting good.
[0024] The size of the metal pigment is preferably 1 to 50 μm in average particle diameter, because in the above range, the metal pigment is easily caught in the three-dimensional network structure formed by the polyamide resin and the fatty acid amide, the metal pigment is inhibited from settling, and a good color tone (metallic luster) is easily obtained, and furthermore, the metal pigment in the ink is less likely to clog the pen tip. In particular, in consideration of the inhibition of the settling of the metal pigment by making it easy to be caught in the three-dimensional network structure, the average particle diameter is preferably 3 to 20 μm, and most preferably 5 to 15 μm. Here, the average particle diameter can be determined by the laser diffraction method, specifically, the particle diameter at 50% cumulative volume (D50) of the particle size distribution measured based on the value calibrated using a standard sample or other measurement method using a laser diffraction type particle size distribution measuring instrument (product name "MicrotracHRA9320-X100", Nikkiso Co., Ltd.). Since the metal powder exerts the above-mentioned effects in a dispersed state in the ink composition, it is preferable to determine the particle size in the dispersed state.
[0025] In addition, in the total amount of the ink composition, the total mass ratio of the polyamide resin and the fatty acid amide to the total mass of the pigment (polyamide resin + fatty acid amide / pigment) is preferably 0.1 to 3 times. This is because if it is less than 0.1 times, it is difficult to obtain the above-mentioned effects such as suppression of pigment sedimentation and good color tone of handwriting, and if it exceeds 3 times, the ink viscosity is too high, the ink discharge amount is likely to be small, and the color tone of the handwriting is likely to be affected. From further consideration, the content ratio is preferably 0.2 to 2 times by mass, and more preferably 0.5 to 1.5 times.
[0026] Specific examples of metal pigments include aluminum paste pigments such as WXM0630, WB0230, 400SW, and FM4010WG (all manufactured by Toyo Aluminium Co., Ltd.), and colored aluminum pigments such as F503RG, F503BG, F500SI, F500RE, F500RE, and F500BL (all manufactured by Toyo Aluminium Co., Ltd.), the Chromal series, and solid RotosafeAqua250 042, 250 022, and 260 003 (all manufactured by ECKART Co., Ltd.). Examples of aluminum powder include AA12, AA8, No. 900, and No. 18000 (all manufactured by Fukuda Metal Foil and Powder Co., Ltd.). Metal-deposited powder pigments include LG Silver #500, #325, and #200 (all manufactured by Oike Kogyo Co., Ltd.), which are made by vacuum-depositing aluminum onto synthetic resin, protecting the metal layer with resin, and then pulverizing them into flakes.Furthermore, LG R.Gold #500, B.Gold #500, R.Gold #325, B.Gold #325, Red #325, Blue #325, Green #325, Violet #325, Black #325, Copper #325, R.Gold #200, B.Gold #200, Red #200, Blue #200, Green #200, Violet #200, Black #200, and Copper #200 (all manufactured by Oike Kogyo Co., Ltd.), which are made by coloring the resin layer, are also included. Examples of glass flake pigments include Metashine REFSX-2015PS, -2025PS, -2040PS, RCFSX-5030NS, -5030NB, -5030PS, -2015PS, and -5090GG (all manufactured by Nippon Sheet Glass Co., Ltd.), which are glass flakes coated with metal by electroless plating. Examples of pearl pigments include Iriodin 120 Luster Satin, 123 Bright Luster Satin, 201 Rutile Fine Gold, 211 Rutile Fine Red, 221 Rutile Fine Blue, 223 Rutile Fine Lilac, 231 Rutile Fine Green, 302 Gold Satin, 323 Royal Gold Satin, 520 Bronze Satin, 522 Red Brown Satin, and 524 Red Satin (all manufactured by Merck Japan Ltd.). Examples of titanium oxide pigments include Titone SR-1, Titone R-650, R-3L, A-110, A-150, R-5N, and R-7E (all manufactured by Sakai Chemical Industry Co., Ltd.), Typeake R-580, R-550, R-780, R-780-2, R-930, A-100, A-220, and Typeake CR-58 (all manufactured by Ishihara Sangyo Kaisha, Ltd.), Cronos KR-310, KR-380, KR-480, KA-10, KA-20, and KA-30 (all manufactured by Titanium Industries Co., Ltd.), Typeure R-900, R-931, R-960, and R-960VHG (all manufactured by DuPont Japan Limited). In addition, it is preferable to use a commercially available aqueous dispersion of titanium dioxide such as LIOFAST WHITE H201, EM WHITE H, EMWHITE FX9048 (all manufactured by Toyo Ink Co., Ltd.), Pollux White PC-CR (manufactured by Sumitomo Color Co., Ltd.), FUJISP WHITE 11, 1011, 1036, and 1051 (all manufactured by Fuji Color Co., Ltd.), since this allows the dispersion step to be omitted in production and ink can be easily produced.
[0027] In addition, when a metal pigment is used, it is preferable to include a black colorant, since the black colorant improves the visibility of handwriting on white paper and thus the color tone is easily improved. The content of the black colorant is preferably 0.001 to 1 mass %, and more preferably 0.01 to 0.5 mass %, based on the total amount of the ink composition, taking the color tone into consideration.
[0028] Furthermore, if the content of the colorant is less than 1% by mass relative to the total amount of the ink composition, the desired color tone (metallic gloss) of the written lines cannot be obtained, and if it is 20% by mass or more, the pigment may settle and the ink stability over time may be affected. Therefore, the content is preferably 1 to 20% by mass, more preferably 1 to 15% by mass, and most preferably 2 to 10% by mass.
[0029] (solvent) In the present invention, it is preferable to use a solvent in consideration of the solubility of the ink components, dispersion stability, prevention of water evaporation and drying, etc. When using a polyamide resin or fatty acid amide as in the present invention, taking into consideration the effect of inhibiting pigment sedimentation by facilitating the stable formation of a three-dimensional network structure in the ink, it is preferable to use a solvent with a solubility parameter (SP value) of 8 to 12, and more preferably a solvent with a solubility parameter (SP value) of 8.5 to 10.5. Specifically, propylene glycol monomethyl ether (SP value 10.2), propylene glycol monopropyl ether (SP value 9.4), propylene glycol monobutyl ether (SP value 9.0), dipropylene glycol monomethyl ether (SP value 9.1), triethylene glycol monomethyl ether (SP value 11.2), tripropylene glycol monomethyl ether (SP value 9.1), ethylene glycol-2-ethylhexyl ether (SP value 9.0), diethylene glycol-2-ethylhexyl ether (SP value 9.2), ethylene glycol isopropyl ether (SP value 9.2), diethylene glycol monobutyl ether (SP value 9.5), 2-ethylhexanol (S Examples of suitable terpolymers include propylene glycol monomethyl ether (SP value 10.2), propylene glycol monobutyl ether (SP value 9.0), and propylene glycol monomethyl ether (SP value 9.5), 3-methoxy-3-methylbutanol (SP value 9.3), hexylene glycol (SP value 10.5), diethylene glycol monomethyl ether (SP value 10.7), triethylene glycol monomethyl ether (SP value 11.2), phenyl glycol (SP value 11.5), tetraethylene glycol dimethyl ether (SP value 9.4), diethylene glycol ethyl methyl ether (SP value 8.9), and triethylene glycol monobutyl methyl ether (SP value 8.9). Considering the stability with polyamide resins, it is preferable to use propylene glycol monomethyl ether (SP value 10.2) and propylene glycol monobutyl ether (SP value 9.0).
[0030] In addition, as the solvent, it is preferable to use the following water-soluble solvents in consideration of prevention of water evaporation and drying, metal pigment dispersion stability, etc. Specifically, polyhydric alcohol solvents such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, polyethylene glycol, and glycerin, and alcohol-based solvents such as methanol, ethanol, 1-propanol, 2-propanol, isopropanol, isobutanol, t-butanol, propargyl alcohol, allyl alcohol, 3-methyl-1-butyn-3-ol, ethylene glycol monomethyl ether acetate, and other higher alcohols are listed. Among them, polyhydric alcohols are preferable in consideration of the fact that they are easy to suppress pigment sedimentation as a pigment dispersion aid, and that when the pen tip dries, the pigments (aluminum powder, stainless steel powder, titanium oxide powder) in the ink are hard particles, which easily affect the writing performance during drying up, and therefore the polyhydric alcohol is easy to improve. In particular, it is preferable to contain at least a polyhydric alcohol having a divalent or trivalent hydroxyl group. A polyhydric alcohol solvent is a compound in which two or more hydroxyl groups are bonded to different carbon atoms of an aliphatic or alicyclic compound. These may be used alone or in combination of two or more kinds.
[0031] The content of the solvent is preferably 1 to 40% by mass, more preferably 3 to 30% by mass, and more preferably 5 to 25% by mass, based on the total amount of the ink composition, taking into consideration the solubility of the polyamide resin, fatty acid amide, and metal pigment, drying-up property, bleeding, and the like.
[0032] (water) The water is not particularly limited, and for example, tap water, ion-exchanged water, ultrafiltered water, distilled water, or the like can be used.
[0033] (Resin particles) In the present invention, the inclusion of resin particles is preferable because, in the case of a ballpoint pen, it is easy to suppress ink leakage by causing physical obstacles in the gap between the ball and the inner wall of the tip end. Furthermore, since organic resin particles have a lower hardness than inorganic particles, the particles are partially deformed and adhere to each other to form a structure formed by weak aggregation, and a structure with high resistance to ink leakage when left still is formed in the ink, which is easy to suppress ink leakage, and is preferable. In the present invention, the use of polyamide resin and fatty acid amide is effective because it is easy to hook resin particles to the formed three-dimensional network structure, which stabilizes the dispersion of resin particles and easily suppresses sedimentation.
[0034] Examples of resin particles include olefin resin particles such as polyethylene resin and polypropylene resin, nitrogen-containing resin particles containing nitrogen atoms in the chemical structure such as melamine-formaldehyde resin, benzoguanamine-formaldehyde resin, benzoguanamine-melamine-formaldehyde resin, urea-formaldehyde resin, nylon resin, acrylic resin particles, styrene resin particles, epoxy resin particles, urethane resin particles, cellulose resin particles, etc. These organic resin particles may be used alone or in combination of two or more kinds.
[0035] The pH value of the aqueous ink composition for writing instruments of the present invention is preferably 6.0 to 10.0, taking into consideration the dispersibility of polyamide resin, colorant (pigment) by fatty acid amide, and resin particles. This is because if the pH value approaches the acidic side of less than 6 or the strong alkaline side of more than 10, it will affect the dispersibility of metal pigments, and the metal pigments will be easily corroded and will be easily affected by the metallic gloss. In particular, when aluminum powder is used, the pH value is more preferably 7.0 to 9.0, taking into consideration the corrosion of aluminum. The pH value is shown as a value measured at 20°C using a pH meter HM-30R manufactured by DKK-TOA Corporation.
[0036] Examples of the pH adjuster include alkanolamines such as monoethanolamine, diethanolamine, triethanolamine, dimethylethanolamine, N-methylethanolamine, N-methyldiethanolamine, and diisopropanolamine, ammonia, alkaline inorganic salts such as sodium carbonate, potassium carbonate, sodium acetate, potassium acetate, sodium phosphate, potassium phosphate, sodium hydrogen phosphate, and potassium hydrogen phosphate, and organic acids such as lactic acid, acetic acid, and citric acid. Among these, in consideration of the ink stability over time, it is preferable to use alkanolamines which are more weakly basic.
[0037] In addition, the content of the pH adjuster is preferably 0.1 to 10 mass %, more preferably 0.3 to 5 mass %, based on the total amount of the ink composition, taking into consideration the ink stability over time.
[0038] When a metallic pigment is used as the colorant, it is preferable for the composition to contain a chelating agent, since this makes it easier to prevent the precipitation of metal salts and the like by sequestering the metal present in the aqueous ink composition for writing instruments. Furthermore, the water-based ink composition for writing instruments may be contained in a glass ink reservoir such as a glass bottle. Glass bottles are easy to mold, inexpensive and readily available, and can easily provide a desired strength. However, when inexpensive and versatile soda-lime glass is used, there is a high possibility that an alkali component in the glass will elute into the water-based ink composition for writing instruments if the ink composition is stored therein for a long period of time, and this eluted alkali component may react with a component of the water-based ink composition for writing instruments to form a precipitate. For this reason, it is effective to further use a chelating agent in the aqueous ink composition for a writing instrument of the present invention, and even when the composition is contained in a glass ink reservoir, the chelating agent can supplement the eluted alkaline components and prevent the alkaline components from reacting with the components in the aqueous ink composition for a writing instrument to produce water-insoluble precipitates, thereby preventing the ink flow path from being blocked by the produced precipitates, causing handwriting to fade or making it impossible to write.
[0039] Examples of the chelating agent include aminocarboxylic acids such as ethylenediaminetetraacetic acid (EDTA), hydroxyethylenediaminetriacetic acid (HEDTA), glycol ether diaminetetraacetic acid (GEDTA), nitrilotriacetic acid (NTA), hydroxyethyliminodiacetic acid (HIDA), dihydroxyethylglycine (DHEG), diethylenetriaminepentaacetic acid (DTPA), triethylenetetraminehexaacetic acid (TTHA), and alkali metal salts, ammonium salts, or amine salts thereof. Considering that the alkaline components can be sufficiently supplemented and that the physical properties of the aqueous ink composition for writing instruments before and after the incorporation of the chelating agent are not likely to be significantly affected, it is preferable to use aminocarboxylic acids among the above chelating agents, and in particular, it is preferable to use ethylenediaminetetraacetic acid (EDTA) and its salts.
[0040] The content of the chelating agent is preferably 0.01 to 1% by mass based on the total amount of the ink composition. If it is 1% by mass or less, it will not adversely affect the performance and physical properties of the ink composition, such as discoloration of the ink. If it is 0.01% by mass or more, it can supplement the alkaline components eluted from a glass ink container such as a glass bottle, and suppress the occurrence of precipitation. Furthermore, the addition of an appropriate amount of the chelating agent tends to further improve the resistance to leakage from the pen tip. Therefore, in consideration of suppressing the occurrence of precipitates and further improving the resistance to leakage from the pen tip, the amount is more preferably 0.01 to 0.5% by mass.
[0041] Furthermore, when a metallic pigment is used as the colorant, it is preferable that the ink composition contains a phosphate ester surfactant, because when a metallic pigment is used, the ink composition contains a phosphate ester surfactant, which sequesters the metal present in the ink composition, making it easier to suppress precipitation of metal salts and the like. Furthermore, when used in a ballpoint pen, the phosphate group adsorbs to metal, thereby improving lubricity, suppressing wear of the ball seat, and tending to improve the writing feel. Furthermore, taking lubricity into consideration, it is preferable to use a phosphate ester surfactant, and it is preferable to use a phosphate ester surfactant having an alkyl group. Examples of the types of phosphate ester surfactants having an alkyl group include styrenated phenols, nonylphenols, lauryl alcohols, tridecyl alcohols, octylphenols, octyl alcohols, etc. Among these, it is preferable to use phosphate ester surfactants that do not have a phenyl skeleton, since the phenyl skeleton tends to affect lubricity due to steric hindrance, and further tends to affect the ink stability over time due to compatibility with the metal pigment.
[0042] Examples of the phosphate surfactant include polyoxyethylene alkyl ether or polyoxyethylene alkylaryl ether phosphate monoesters, polyoxyethylene alkyl ether or polyoxyethylene alkylaryl ether phosphate diesters, polyoxyethylene alkyl ether or polyoxyethylene alkylaryl ether phosphate triesters, alkyl phosphate esters, alkyl ether phosphate esters, and derivatives thereof. These phosphate surfactants may be used alone or in combination of two or more kinds.
[0043] The content of the phosphate ester surfactant is preferably 0.1 to 5% by mass based on the total amount of the ink composition, because if it exceeds 5% by mass, the ink stability over time tends to be affected, and from further consideration, a content of 0.1 to 3% by mass is more preferable.
[0044] In addition, when a pigment is used as a colorant, since the pigment (aluminum powder, stainless steel powder, titanium oxide powder) in the ink is a hard particle when the pen tip dries, it is preferable to use a moisturizing agent because it is likely to affect the writing performance when the ink dries up.Specific examples include urea, sorbitol, N,N,N-trialkylamino acids such as trimethylglycine, triethylglycine, and tripropylglycine, but urea is preferable because it is easy to obtain a moisture absorption effect.In addition, if the ink is left for a long period of time, the pH value tends to become acidic due to carbon dioxide in the air, but by containing urea as in the present invention, the pH value is prevented from becoming less than 7 even after a long period of time, so that it can be used more effectively when setting the pH value.
[0045] In addition, when a metal pigment is used as in the present invention, it is preferable to contain a black colorant since the black colorant improves the visibility of handwriting on white paper and thus the color tone is easily improved. The content of the black colorant is preferably 0.001 to 1 mass %, and more preferably 0.01 to 0.5 mass %, based on the total amount of the ink composition, taking the color tone into consideration.
[0046] Furthermore, a preservative may be used. Examples of the rust inhibitor include benzotriazole and its derivatives, tolyltriazole, dicyclohexylammonium nitrite, diisopropylammonium nitrite, sodium thiosulfate, saponin, and dialkylthiourea.
[0047] Preservatives may also be used, and examples of the preservatives include phenol, sodium benzoate, sodium dehydroacetate, potassium sorbate, propyl paraoxybenzoate, 2,3,5,6-tetrachloro-4-(methylsulfonyl)pyridine, 2-pyridinethiol-1-oxide sodium, 1,2-benzisothiazolin-3-one, 2-methyl-4-isothiazolin-3-one, and 2-n-octyl-4-isothiazolin-3-one.
[0048] A pigment dispersant may be used to improve the dispersibility of the pigment, suppress pigment precipitation or aggregation, and improve the fixability of handwriting. Examples of pigment dispersants include acidic resins, basic resins, nonionic surfactants, and anionic surfactants, but considering long-term pigment dispersion stability, it is preferable to use acidic resins. Examples of acidic resins include acidic resins having a carboxyl group, a phenyl group, or a sulfonic acid group, and specific examples include acrylic resins, styrene-acrylic resins, styrene-maleic acid resins, phenolic resins, and polyvinyl-sulfonic acid resins. Among the above acidic resins, acidic resins having a carboxyl group are preferred.
[0049] The content of the pigment dispersant in the ink composition is preferably 0.1 to 5.0% by mass, more preferably 1.0 to 4.0% by mass, since if the content is less than 0.1% by mass, it is difficult to obtain the desired pigment dispersion effect and fixation of handwriting, and if the content is 5.0% by mass or more, the ink stability over time is likely to deteriorate.
[0050] In addition, when a metal pigment is used, the shape of the metal powder in the metal pigment may be scaly, angular, or plate-like, and since air bubbles entrapped during ink production tend to be difficult to remove, it is preferable to use an air bubble absorber. Examples of air bubble absorbers include hydroxylamines, ascorbic acids, erythorbic acids, and polyphenols. These air bubble absorbers are compounds that exhibit reducing properties, and absorb oxygen in the ink to achieve air bubble absorption. Examples of hydroxylamines, ascorbic acids, erythorbic acids, and polyphenols include hydroxylamines, hydroxylamine derivatives, polyphenols, polyphenol derivatives, ascorbic acid, ascorbic acid derivatives, erythorbic acid, erythorbic acid derivatives, and salts thereof.
[0051] As for the air bubble absorbent, some ascorbic acids are highly acidic (pH value = 2), and react with the components in the ink, affecting the ink stability over time and likely affecting the dispersibility of the metal powder used in the present invention, and since ascorbic acids and polyphenols tend to affect the color tone, it is preferable to use hydroxylamines and erythorbic acids. Furthermore, since hydroxylamines may produce an amine odor, it is preferable to use erythorbic acids.
[0052] The content of the bubble absorber is preferably 0.01 to 5% by mass based on the total amount of the ink composition. This is because if it is 0.01% by mass or less, it is difficult to sufficiently absorb oxygen in the ink, and if it exceeds 5% by mass, it is likely to affect the ink stability over time. From further consideration, it is preferably 0.1 to 3% by mass, and most preferably 0.1 to 1% by mass.
[0053] In addition, when the ink composition is used for a ballpoint pen, a shear thinning agent may be used in consideration of improving the pigment dispersibility. Examples of shear thinning agents include polyacrylic acid, xanthan gum, welan gum, succinoglycan, guar gum, locust bean gum, λ-carrageenan, cellulose derivatives, oxidized cellulose, diutan gum, etc., and by including these, a three-dimensional network structure is formed in the ink, which makes it easier to stabilize the dispersion of the metal pigment. These shear thinning agents may be used alone or in combination of two or more.
[0054] The ink viscosity is measured at a shear rate of 1.92 (sec -1) (at rest), the ink viscosity is preferably 1000 (mPa·s) or less. This is because maintaining a large ink discharge volume improves the color tone (metallic luster) of the handwriting, and also prevents good writing performance, color tone (metallic luster) of the handwriting, and blurring of the handwriting, so 600 (mPa·s) or less is preferable, and from a more specific perspective, 400 (mPa·s) or less is more preferable. Furthermore, from the perspective of preventing settling of colorants (pigments), resin particles, etc., a viscosity of 50 (mPa·s) or more is preferable, with 100 (mPa·s) or more being more preferable, and 150 (mPa·s) or more being even more preferable. In addition, at 20°C, the shear rate was 38.4 (sec -1 ), and the ink viscosity is preferably 100 (mPa·s) or less. This is because by maintaining a large ink discharge amount, the color tone (metallic gloss) of the handwriting can be improved and furthermore, blurring of the handwriting can be suppressed, so 70 (mPa·s) or less is preferable, and more preferably 55 (mPa·s) or less is preferable. If blurring of the handwriting is suppressed and good writing properties and color tone (metallic gloss) of the handwriting can be obtained, 45 (mPa·s) or less is preferable, and 35 (mPa·s) or less is preferable. Also, if it is necessary to suppress the settling of colorants (pigments), resin particles, etc., 5 (mPa·s) or more is preferable, 10 (mPa·s) or more is preferable, and 15 (mPa·s) or more is more preferable. As described above, when the ink viscosity is low, the pigment is likely to settle, so it is preferable to use polyamide resins and fatty acid amides as in the present invention, since a remarkable effect is easily obtained. Furthermore, in order to suppress blurring of handwriting and improve writing properties, the shear rate is 384 (sec -1 ) (at the time of writing), the ink viscosity is preferably 15 (mPa·s) or less, and more preferably 10 (mPa·s) or less. Furthermore, in order to maintain the ink ejection volume, improve the color tone (metallic luster) of the handwriting, and suppress blurring of the handwriting while also suppressing sedimentation of the metal pigment, it is preferable that the viscosity gradient during flow of the ink composition be at least a certain level, in other words, the viscosity ratio of the ink composition at high shear (when writing) to low shear (when stationary) be at least a certain level. Therefore, the viscosity ratio of the ink composition at high shear (when writing) and low shear (when stationary) (shear rate 1.92 sec -1 Viscosity at shear rate of 384sec -1 The viscosity ratio (at a shear rate of 1.92 sec) is preferably 10 or more, more preferably 20 or more, and even more preferably 25 or more. -1 Viscosity (at rest) / shear rate 384sec -1 The viscosity at the time of writing is 50 or less, and more preferably 40 or less.
[0055] (writing implements) The aqueous ink composition for writing instruments of the present invention can be used in writing instruments such as marking pens and ballpoint pens with pen cores such as fiber tips, felt tips, and plastic tips, or ballpoint pen tips, and fountain pens with metal pen tips. Even if the ink viscosity is low as in the present invention, pigment sedimentation can be suppressed, so that the aqueous ink composition for writing instruments of the present invention is effective for use as an ink composition for marking pens or fountain pens, and is particularly effective for use as an ink composition for fountain pens.
[0056] Furthermore, the ink composition for a writing instrument of the present invention can be used in a configuration in which the ink composition is directly filled, or in a configuration in which an ink reservoir capable of being filled with the ink composition is provided.
[0057] The aqueous ink composition for writing instruments of the present invention can be suitably used in writing instruments equipped with an ink reservoir (ink cartridge) that can be freely attached and detached to the main body of the writing instrument, or an ink reservoir (ink inhaler) that has the function of directly sucking ink into the ink reservoir from an ink container such as an ink bottle. Since the ink reservoir as described above may be provided inside the barrel of a writing instrument, the inner diameter of the ink reservoir is likely to be restricted. Therefore, the ink composition is unlikely to flow inside the ink reservoir, and special consideration must be given to the ink mobility inside the ink reservoir. The ink composition of the present invention can suppress the decrease in wettability of the ink reservoir when the ink moves, and has excellent ink mobility inside the ink reservoir, so it can be suitably used in a writing instrument equipped with the ink reservoir as described above. In particular, when the material of the ink reservoir is made of a resin material, the ink reservoir tends to have poor wettability with the ink composition, and it is necessary to take into consideration the ink mobility within the ink reservoir in particular. The ink composition of the present invention can suppress the decrease in wettability when the ink moves with respect to the resin material, and therefore can be suitably used in a writing instrument having a resin ink reservoir.
[0058] In addition, it is desirable for the ink reservoir to be made of a semi-transparent or transparent material that allows the remaining amount of ink to be seen. Examples of such materials include thermoplastic resins such as polyethylene, polypropylene, polymethylpentene, polyethylene terephthalate, polycyclohexane terephthalate, polycarbonate, and nylon. In addition, since the ink reservoir stores the ink composition for a long period of time, it is preferable to use a crystalline resin that has excellent chemical resistance, and therefore it is more preferable to use a crystalline olefin resin such as polyethylene, polypropylene, or polymethylpentene.
[0059] Furthermore, writing instruments in which the aqueous ink composition for writing instruments of the present invention can be used may be of a cap type having a cap that covers the writing tip, or may be of a retractable type in which the writing tip can be stored within the barrel, such as a knock type, a rotating type, or a sliding type.
[0060] The ink supply mechanism of a writing instrument in which the aqueous ink composition for a writing instrument of the present invention can be used is not particularly limited, and examples thereof include (mechanism 1) a mechanism having an ink guide core made of a fiber bundle or the like as an ink flow regulator, which supplies the ink composition to the pen tip through the ink guide core, (mechanism 2) a mechanism having a comb-shaped ink retaining member as an ink flow regulator, which supplies the ink composition to the pen tip, (mechanism 3) a mechanism having an ink flow regulator using a valve mechanism, which supplies the ink composition to the writing tip, and (mechanism 4) a mechanism that supplies the ink composition directly to the pen tip without an ink flow regulator.
[0061] In the case of a ballpoint pen, the ball material is not particularly limited, but examples thereof include a cemented carbide ball mainly composed of tungsten carbide, silicon carbide, alumina, zirconia, silicon nitride, etc. Considering the lack of metal corrosion and the writing feel, it is preferable to use a silicon carbide ball. The size of the ball is determined by the purpose of the writing instrument and the width of the drawn line required when writing, and is generally selected from the range of 0.1 to 2.0 mm.
[0062] The amount of movement of the ball of the ballpoint pen tip in the vertical axis direction is preferably 15 to 50 μm, because the color tone (metallic gloss) of the handwriting can be improved by maintaining a large ink discharge amount, and if it is less than 15 μm, the ink consumption is likely to be small and the metallic gloss of the handwriting is likely to be poor, and if it exceeds 50 μm, the drying speed of the handwriting and the suppression of ink leakage are likely to be poor. In consideration of the color tone (metallic gloss) of the handwriting, it is preferable to set it to 30 to 50 μm.
[0063] <Water-based ink products> The water-based ink product according to the present invention may contain the water-based ink composition for a writing instrument according to the present invention in an ink reservoir made of glass. In particular, when the water-based ink composition for a writing instrument contains a chelating agent, even when the composition is contained in a glass ink reservoir, the chelating agent supplements the eluted alkaline components, prevents the alkaline components from reacting with the components in the water-based ink composition for a writing instrument to form water-insoluble precipitates, and is effective and preferred because it is easy to prevent the ink flow path from being blocked by the precipitates, causing handwriting to fade or making writing impossible. In particular, when the water-based ink composition for a writing instrument is combined with a glass ink reservoir using soda-lime glass, a particularly high effect is easily exhibited, which is preferred.
[0064] The glass ink reservoir that contains the ink composition for a writing instrument can be a single glass product such as a glass bottle, or an ink reservoir with an exterior (decoration) made of resin, wood, lacquer, or the like.
[0065] (Method for producing water-based ink composition) The water-based ink composition for writing instruments of the present invention can be produced by any conventionally known method. Specifically, the ink components are mixed in the required amounts and mixed with various stirrers such as a propeller stirrer, a homodisper, or a homomixer, or various dispersers such as a bead mill, to produce the composition.
[0066] The present invention will now be described with reference to examples. (Water-based ink composition for writing instruments) Example 1 Metal pigment (containing 65% aluminum powder, 3% octylphosphonic acid, leafing type, mass ratio of alkylphosphonic acid to metal powder: 0.05 (alkylphosphonic acid / metal powder)) 2.0 parts by mass Dye (Direct Black 154) 0.01 parts by weight Water 80.5 parts by mass Polyhydric alcohol (diethylene glycol) 7.0 parts by mass Mixture of polyamide resin and fatty acid amide (active ingredient 10%, contains propylene glycol monomethyl ether (SP value 10.2), acid value: 7.5 (mgKOH / g), neutralized with alkanolamine) 8.0 parts by mass pH adjuster (triethanolamine) 1.0 parts by mass Aminocarboxylic acid (ethylenediaminetetraacetic acid) 0.5 parts by mass Phosphate ester surfactant 1.0 parts by weight
[0067] First, for the metal pigment, the metal powder was surface-treated with alkylphosphonic acid (octylphosphonic acid) and mixed with imidazoline and propylene glycol monomethyl ether (SP value 10.2) to create a paste-like metal pigment. Also, a polyamide resin, fatty acid amide, propylene glycol monomethyl ether (SP value 10.2), and water were mixed to create a paste-like mixture of polyamide resin and fatty acid amide. Thereafter, the dye, water, polyhydric alcohol, a mixture of polyamide resin and fatty acid amide, pH adjuster, aminocarboxylic acid, and phosphate ester surfactant were heated and stirred to prepare a base ink, and the previously prepared metallic pigment and the base ink were mixed, heated and stirred to prepare an aqueous ink composition for writing instruments.
[0068] The ink viscosity of Examples 1, 2, 12 to 14, and Comparative Example 1 was measured using a TA Instruments rheometer AR-G2 viscometer (cone plate 40 mm, angle 2°) at a shear rate of 1.92 sec at 20°C. -1 (Rotation speed 0.5 rpm), shear speed 38.4 sec -1 (Rotation speed 10 rpm), shear rate 384 sec -1 The ink viscosity was measured at a rotation speed of 100 rpm. At 20℃, shear rate is 1.92sec -1 The ink viscosity was measured at a rotation speed of 0.5 rpm, and the results were Example 1: 315 (mPa·s), Example 2: 514 (mPa·s), Example 12: 80 (mPa·s), Example 13: 150 (mPa·s), Example 14: 172 (mPa·s), and Comparative Example 1: 3.2 (mPa·s). At 20℃, shear rate is 38.4sec -1The ink viscosity was measured at a rotation speed of 10 rpm, and the results were Example 1: 32 (mPa·s), Example 2: 51 (mPa·s), Example 12: 7 (mPa·s), Example 13: 14 (mPa·s), Example 14: 17 (mPa·s), and Comparative Example 1: 3.0 (mPa·s). In addition, at a shear rate of 384 sec -1 The ink viscosity was measured at a rotation speed of 100 rpm, and the results were Example 1: 9.5 (mPa·s), Example 2: 14 (mPa·s), Example 12: 4.1 (mPa·s), Example 13: 6.1 (mPa·s), Example 14: 6.7 (mPa·s), and Comparative Example 1: 2.4 (mPa·s). Viscosity ratio of the ink composition (shear rate 1.92 sec -1 Viscosity at shear rate of 384sec -1 The viscosity at 100° C. was 33.2 in Example 1, 36.7 in Example 2, 19.5 in Example 12, 24.6 in Example 13, 25.7 in Example 14, and 1.3 in Comparative Example 1. The pH values of Examples 1 and 2 were measured at 20° C. using a pH meter HM-30R manufactured by DKK-TOA Corporation, and were found to be 8.2 for Example 1 and 8.1 for Example 2.
[0069] Examples 2 to 15 Except for changing the ink formulation as shown in the table, the aqueous ink compositions for writing instruments of Examples 2 to 15 were obtained in the same manner as in Example 1. The ink formulations and evaluation results are shown in the table.
[0070] Comparative Examples 1 to 3 Except for changing the ink formulation as shown in the table, the water-based ink compositions for writing instruments of Comparative Examples 1 to 3 were obtained in the same manner as in Example 1. The ink formulations and evaluation results are shown in the table. [Table 1] [Table 2]
[0071] <Preparation of test writing implements> The aqueous ink compositions for writing implements of Examples 1 to 15 and Comparative Examples 1 to 3 were poured into an ink inhaler made of crystalline olefin resin (polymethylpentene) (an ink inhaler with a resin movable body movable in the forward and backward directions arranged therein) with the ink inhaler opening facing upward, and the movable body was completely immersed in the ink composition. The ink inhaler was attached to a retractable knock-type writing implement (Pilot Corporation, fountain pen, FCN-1MR-BM) with a fountain pen-shaped nib and a comb-shaped ink retaining member arranged as an ink flow rate regulator, and the following tests and evaluations were performed using the writing implement, and the color tone test and writing property test were performed using JIS P3201 writing paper A as the writing test paper.
[0072] Sedimentation test (sedimentation test of pigment and resin particles): Each water-based ink composition for writing instruments was placed in a 15 mm diameter tightly retractable glass test tube and allowed to stand at room temperature for 7 days, after which the sedimentation of pigment and resin particles was visually observed. There is almost no supernatant liquid (settling of pigment and resin particles) and it is in good condition. Although some supernatant liquid (sedimentation of pigment and resin particles) was observed, it was at a level that would not cause any problems in practical use. Sedimentation of pigments, etc. (sedimentation of pigments and resin particles) is so severe that it is problematic. ×
[0073] Color tone test: The color tone after handwriting was visually observed. The color tone (metallic luster) of the writing is very good and there is no shading. Good color tone (metallic luster) of handwriting...○ The color tone (metallic luster) of the writing is slightly inferior. The color tone (metallic luster) of the writing is poor and it is of little practical use. ×
[0074] Writability test: The handwritten mark was visually observed. No smudges in the writing...◎ Some handwriting is slightly smudged. The handwriting is smudged and not of practical use... ×
[0075] From the results in the table, good or problem-free performance was obtained in the color tone test, sedimentation test (sedimentation test of pigment and resin particles), and writing test in Examples 1 to 15. As in Examples 1 to 15, the water-based ink composition for writing instruments containing a chelating agent was stored in a glass ink storage unit (water-based ink product: glass bottle) using soda-lime glass, and the ink was observed under a microscope after 3 months at room temperature, and good performance was obtained with no practical problems.
[0076] As can be seen from the results in the table, in Comparative Examples 1 to 3, since no polyamide resin or fatty acid amide was used, sedimentation of the pigment (metal pigment) was severe, resulting in poor writing and smudged handwriting. [Industrial Applicability]
[0077] The aqueous ink composition for writing instruments of the present invention can be used as an aqueous ink composition for various writing instruments such as a fountain pen, a ballpoint pen, a brush pen, a calligraphy pen, a marking pen, a plate pen, etc. More specifically, the aqueous ink composition for writing instruments can be widely used as a writing instrument filled with the aqueous ink composition for writing instruments, such as a cap type or a retractable type.
Claims
1. A water-based ink composition for a writing instrument, comprising water, a pigment using aluminum powder, a polyamide resin, and a fatty acid amide, the total mass ratio of the polyamide resin and the fatty acid amide (polyamide resin + fatty acid amide / pigment) is 0.1 to 3 times the total mass of the pigment, The ink viscosity of the aqueous ink composition for a writing instrument is, in an environment of 20° C., 100 (mPa·s) or more and 600 (mPa·s) or less at a shear rate of 1.92 (sec −1 ), and 15 (mPa·s) or less at a shear rate of 384 (sec −1 ); and the ink viscosity ratio (viscosity at a shear rate of 1.92 sec -1 / viscosity at a shear rate of 384 sec -1 ) is 20 or more and 50 or less (excluding the erasable ink composition for writing boards).
2. The aqueous ink composition for writing instruments as described in claim 1 (excluding the erasable ink composition for writing boards), characterized in that the ink viscosity of the aqueous ink composition for writing instruments is 10 (mPa·s) or more and 70 (mPa·s) or less at a shear rate of 38.4 (sec -1 ) in an environment of 20°C.
3. An aqueous ink composition for a writing instrument as described in claim 1 or 2 (excluding an erasable ink composition for a writing board), characterized in that the aqueous ink composition for a writing instrument further contains a black colorant.
4. The aqueous ink composition for writing instruments (excluding the erasable ink composition for writing boards) according to any one of claims 1 to 3, characterized in that the total content of the polyamide resin and the fatty acid amide is 0.01 to 5 mass% based on the total amount of the ink composition.
5. The aqueous ink composition for a writing instrument according to any one of claims 1 to 4, characterized in that the aqueous ink composition for a writing instrument (excluding an erasable ink composition for a writing board) contains a solvent having a solubility parameter of 8 to 12.
6. A writing instrument, comprising an ink reservoir tube directly filled with the water-based ink composition for a writing instrument (excluding an erasable ink composition for a writing board) according to any one of claims 1 to 5.
Citation Information
Patent Citations
Water-based black pigment ink for ball-point pen
JP1988152681A
Water-base ballpoint ink with metallic luster
JP1995118592A
Oil-based ink composition for ball point pen
JP1995196972A
Aqueous gloss ink composition
JP1999012524A
Aqueous ink composition
JP2002194261A