Ultraviolet-curable resin composition, method for manufacturing light-emitting device, and light-emitting device

A UV curable resin composition with a cationically polymerizable compound and catalyst addresses high viscosity and stability issues, enabling precise application and durable sealing in light-emitting devices with improved light transmission and heat resistance.

JP7554992B2Active Publication Date: 2024-09-24PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020099572
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-10
Filing Date
2020-06-08
Publication Date
2024-09-24
Estimated Expiration
2040-06-08

AI Technical Summary

Technical Problem

Existing ultraviolet curable resin compositions used for sealing light-emitting elements in devices face challenges with high viscosity, which affects their applicability and storage stability, leading to issues like increased volatility and the formation of defective droplets during application, compromising the precision and durability of the sealing material.

Method used

A UV curable resin composition containing a cationically polymerizable compound, such as an aromatic epoxy compound, and a cationic curing catalyst is used to create a low-viscosity, stable sealing material that can be applied using an inkjet method, ensuring precise alignment and improved storage stability while maintaining high reactivity and heat resistance.

Benefits of technology

The composition achieves low viscosity for easy application, enhances storage stability, reduces satellite droplet formation, and provides a sealing material with high light transmittance and heat resistance, ensuring efficient light transmission and durability in light-emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554992000031
    Figure 0007554992000031
  • Figure 0007554992000030
    Figure 0007554992000030
  • Figure 0007554992000029
    Figure 0007554992000029
Patent Text Reader

Abstract

To provide an ultraviolet curable resin composition that is used for preparing an optical component and has low viscosity and excellent storage stability.SOLUTION: An ultraviolet curable resin composition contains a cationic polymerizable compound (F) and a cation curing catalyst (G). The cationic polymerizable compound (F) contains an aromatic epoxy compound (f1) represented by formula (30) and a compound (f3) having an oxetane group, where X is at least one selected from the group consisting of H, halogen, an alkyl group, an aryl group and an alkylene glycol group, R is a single bond or an organic group, Y is H or an organic group, n is a number of 1 to 3.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ultraviolet-curable resin composition, a method for manufacturing a light-emitting device, and a light-emitting device, and more particularly, to an ultraviolet-curable resin composition containing a cationic polymerizable compound and a cationic curing catalyst, a method for manufacturing a light-emitting device using this ultraviolet-curable resin composition, and a light-emitting device including an encapsulant made of a cured product of the ultraviolet-curable resin composition. [Background technology]

[0002] Light-emitting devices equipped with light-emitting elements such as organic electroluminescence (EL) elements and micro-LEDs are used for lighting, display, and other purposes, and are expected to become more widespread in the future.

[0003] In order to prevent the light-emitting element in the light-emitting device from being deteriorated by moisture, the light-emitting element is covered with a sealant. In this case, light emitted by the light-emitting element passes through the sealant and is emitted to the outside. The sealant is made from a composition containing, for example, a cationic curable resin and a cationic polymerization initiator (see Patent Document 1). In this case, the sealant can be made by curing the composition by irradiation with ultraviolet light or the like, so that the sealant can be made without applying a thermal load to the light-emitting element. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5703429 Summary of the Invention [Problem to be solved by the invention]

[0005] According to the inventor's consideration, precise alignment of the material is required to prepare an encapsulant so as to cover a light-emitting element in a light-emitting device. If the composition, which is the material of the encapsulant, has good coatability, the composition can be easily applied to a desired position, and therefore precise alignment of the encapsulant is possible.

[0006] However, when the viscosity of the composition is reduced in order to improve the coatability of the composition, the volatility of the composition tends to increase, resulting in a deterioration in the storage stability of the composition.

[0007] An object of the present invention is to provide an ultraviolet-curable resin composition that can be used to produce an optical component that transmits light emitted by a light source and has low viscosity and good storage stability, a method for producing a light-emitting device, and a light-emitting device. [Means for solving the problem]

[0008] The ultraviolet-curable resin composition according to one embodiment of the present invention contains a cationic polymerizable compound (F) and a cationic curing catalyst (G). The cationic polymerizable compound (F) contains an aromatic epoxy compound (f1) represented by the following formula (30).

[0009] [ka]

[0010] In formula (30), X is at least one selected from the group consisting of halogen, H, a hydrocarbon group, and an alkylene glycol group, and when there are multiple X in one molecule, they may be the same or different. R is a single bond or a divalent organic group. Y is H or a monovalent organic group. n is any number from 1 to 3. The ultraviolet-curable resin composition is used to produce an optical component that transmits light emitted by a light source.

[0011] A method for producing a light-emitting device according to one aspect of the present invention is a method for producing a light-emitting device including a light source and an optical component that transmits light emitted by the light source, the method including discharging the ultraviolet-curable resin composition by an inkjet method at a position through which the light emitted by the light source passes to produce a coating film, and irradiating the coating film with ultraviolet light to produce the optical component.

[0012] A light emitting device according to one aspect of the present invention includes a light source and an optical component that transmits light emitted from the light source, the optical component being made of a cured product of the ultraviolet curable resin composition. Effect of the Invention

[0013] According to one aspect of the present invention, there are provided an ultraviolet-curable resin composition that can be used to produce optical components and has low viscosity and good storage stability, a method for producing a light-emitting device using the ultraviolet-curable resin composition, and a light-emitting device including an encapsulant made of a cured product of the ultraviolet-curable resin composition. [Brief description of the drawings]

[0014] [Figure 1] 1 is a schematic cross-sectional view showing a first example of a light emitting device according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view showing a second example of a light emitting device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, one embodiment of the present invention will be described.

[0016] The ultraviolet-curable resin composition according to this embodiment (hereinafter also referred to as composition (X)) is used to produce an optical component that transmits light emitted by a light source. The optical component is a component for transmitting light emitted by a light source such as a light-emitting element in a device having an optical system (e.g., a light-emitting device). The optical component is, for example, a sealant for a light-emitting element. The optical member is, for example, a thin film, and more specifically, for example, a film having a thickness of 2 μm to 50 μm, or 2 μm to 30 μm.

[0017] The composition (X) contains a cationic polymerizable compound (F) and a cationic curing catalyst (G). The cationic polymerizable compound (F) contains a compound (f1) represented by the following formula (30) (hereinafter, also referred to as aromatic epoxy compound (f1)).

[0018] [ka]

[0019] In formula (30), X is at least one selected from the group consisting of halogen, H, a hydrocarbon group, and an alkylene glycol group, and when there are multiple X in one molecule, they may be the same or different from each other. The hydrocarbon group is, for example, an alkyl group or an aryl group. When X is a hydrocarbon group, the carbon number of X is, for example, in the range of 1 to 10. R is a single bond or a divalent organic group. When R is a divalent organic group, the divalent organic group is, for example, an alkylene group, an oxyalkylene group, a carbonyloxyalkylene group (for example, -CO-O-CH2-), or a -C(Ph)2-O-CH2- group. It is particularly preferable that the divalent organic group is -CH2-, -O-CH2-, or -CO-O-CH2-. Y is H or a monovalent organic group. When Y is a monovalent organic group, the monovalent organic group is, for example, an alkyl group or an aryl group.

[0020] The cationically polymerizable compound (F) preferably further contains a compound (f3) having an oxetane group.

[0021] When the cationic polymerizable compound (F) contains an aromatic epoxy compound (f1), the aromatic epoxy compound (f1) has a low viscosity, so that the aromatic epoxy compound (f1) tends to lower the viscosity of the composition (X). In addition, the aromatic epoxy compound (f1) is not easily volatilized, so that even if the composition (X) is stored, the composition (X) is not easily changed in composition due to the volatilization of the aromatic epoxy compound (f1). Therefore, the aromatic epoxy compound (f1) tends to increase the storage stability of the composition (X). In addition, the aromatic epoxy compound (f1) has high reactivity, so that unreacted components are not easily left in the cured product, so that outgassing is not easily generated from the cured product. Furthermore, the aromatic epoxy compound (f1) tends to increase the glass transition temperature of the cured product, so that the heat resistance of the cured product is easily increased.

[0022] In addition, the aromatic epoxy compound (f1) is less likely to produce defective droplets called satellites when the composition (X) is discharged by an inkjet method. A satellite is a droplet that separates from the original droplet and adheres to a position on the coating target different from the original attachment position of the droplet when the droplet is discharged by an inkjet method. If a satellite is produced, the dimensional accuracy of a sealant or the like produced from the composition (X) will be deteriorated.

[0023] R in formula (30) is preferably a single bond or an alkylene group. When n in formula (30) is 2 or 3, at least one of the multiple R in formula (30) is preferably a single bond or an alkylene group. In these cases, the reactivity of the aromatic epoxy compound (f1) tends to be high, and therefore the curability of the composition (X) tends to be high when the composition (X) is irradiated with ultraviolet light.

[0024] In addition, the cationically polymerizable compound (F) contains the compound (f3) having an oxetane group, and thus can suppress the rapid progress of the reaction when the composition (X) is irradiated with ultraviolet light, making the cured product less likely to turn yellow or become cloudy, and can allow the reaction to proceed sufficiently to make it less likely to generate outgassing from the cured product.

[0025] The cured product obtained by irradiating the composition (X) with light and then heating it preferably has a glass transition temperature of 80°C or higher. In this case, the cured product can have good heat resistance. Therefore, for example, when the cured product is subjected to a treatment accompanied by an increase in temperature, the cured product is less likely to deteriorate. The glass transition temperature of the cured product is more preferably 90°C or higher, and even more preferably 100°C or higher.

[0026] The viscosity of composition (X) at 25°C is preferably 1 mPa·s or more and 40 mPa·s or less. In this case, composition (X) can be molded by applying it by a casting method at room temperature or discharging it by an inkjet method. It is more preferable that this viscosity is 35 mPa·s or less, even more preferable that it is 30 mPa·s or less, particularly preferable that it is 20 mPa·s or less, and most preferable that it is 15 mPa·s or less. It is also preferable that this viscosity is 5 mPa·s or more, and more preferable that it is 8 mPa·s or more. For example, it is preferable that this viscosity is 8 mPa·s or more and 35 mPa·s or less.

[0027] It is also preferable that the viscosity of the composition (X) at 40°C is 1 mPa·s or more and 40 mPa·s or less. In this case, no matter what the viscosity of the composition (X) at room temperature is, it is possible to lower the viscosity by slightly heating the composition (X). Therefore, by heating, the composition (X) can be easily molded by a method such as a casting method, and the composition (X) can also be ejected by an inkjet method. In addition, since the viscosity of the composition (X) can be lowered without significantly heating it, it is possible to prevent the composition of the composition (X) from changing due to the volatilization of the components in the composition (X). It is more preferable that the viscosity is 35 mPa·s or less, even more preferable that the viscosity is 30 mPa·s or less, particularly preferable that the viscosity is 20 mPa·s or less, and most preferable that the viscosity is 15 mPa·s or less. It is also preferable that the viscosity is 5 mPa·s or more, and more preferable that the viscosity is 8 mPa·s or more and 35 mPa·s or less. For example, it is preferable that the viscosity is 8 mPa·s or more and 35 mPa·s or less.

[0028] Such a low viscosity of composition (X) at 25° C. or 40° C. can be achieved by the composition of composition (X) described in detail below.

[0029] The total light transmittance of the cured product of composition (X) is preferably 90% or more when the thickness dimension is 10 μm. In this case, when the cured product is applied to an optical component such as the encapsulant 5 in the light emitting device 1, the extraction efficiency of the light that passes through the optical component and is emitted to the outside can be particularly improved. Such light transmittance of the cured product can also be achieved by the composition of composition (X) described in detail below.

[0030] It is also preferable that the surface tension of the composition (X) is 20 mN / cm or more and 40 mN / cm or less. In this case, when the composition (X) is discharged by the inkjet method, the discharge stability is good, and it is possible to prevent the generation of defective droplets called satellites. It is more preferable that the surface tension is 30 mN / cm or more and 40 mN / cm or less, and even more preferable that the surface tension is 31 mN / cm or more and 38 mN / cm or less.

[0031] This embodiment will be described in further detail below.

[0032] 1. Structure of the light-emitting device First, the structure of the light emitting device 1 will be described when the device having an optical system is the light emitting device 1 and the optical component is a sealant 5 that seals the light emitting element 4 in the light emitting device 1. The light emitting device 1 includes a light emitting element 4 and a sealant 5 that covers the light emitting element 4. The sealant 5 may cover the light emitting element 4 in a state of direct contact with the light emitting element 4, or may cover the light emitting element 4 with some layer interposed between the sealant 5 and the light emitting element 4. The light emitting device 1 may be, for example, a lighting device or a display device.

[0033] The light-emitting element 4 includes, for example, a light-emitting diode. The light-emitting diode includes, for example, at least one of an organic EL element (organic light-emitting diode) and a micro light-emitting diode. When the light-emitting element 4 includes an organic light-emitting diode, the light-emitting device 1 including the light-emitting element 4 is, for example, an organic EL display. When the light-emitting element 4 includes a micro light-emitting diode, the light-emitting device 1 including the light-emitting element 4 is, for example, a micro LED display. Note that EL stands for electroluminescence, and LED stands for light-emitting diode.

[0034] A first example of the structure of the light emitting device 1 will be described with reference to Fig. 1. This light emitting device 1 is a top emission type. The light emitting device 1 includes a support substrate 2, a transparent substrate 3 that faces the support substrate 2 with a gap therebetween, a light emitting element 4 on the surface of the support substrate 2 that faces the transparent substrate 3, and a sealant 5 that is filled between the support substrate 2 and the transparent substrate 3. In addition, in the first example, the light emitting device 1 includes a passivation layer 6 that covers the surface of the support substrate 2 that faces the transparent substrate 3 and the light emitting element 4. That is, the passivation layer 6 is interposed between the light emitting element 4 and the sealant 5 that covers the light emitting element 4.

[0035] The support substrate 2 is made of, for example, a resin material, but is not limited thereto. The transparent substrate 3 is made of a material having light-transmitting properties. The transparent substrate 3 is, for example, a glass substrate or a transparent resin substrate. When the light-emitting element 4 includes an organic EL element, the organic EL element includes, for example, a pair of electrodes and an organic light-emitting layer between the electrodes. The organic light-emitting layer includes, for example, a hole injection layer, a hole transport layer, an organic light-emitting layer, and an electron transport layer, and these layers are laminated in the above order. Although only one light-emitting element 4 is shown in FIG. 1, the light-emitting device 1 may include a plurality of light-emitting elements 4, and the plurality of light-emitting elements 4 may form an array on the support substrate 2. The passivation layer 6 is preferably made of silicon nitride or silicon oxide.

[0036] A second example of the structure of the light emitting device 1 will be described with reference to Fig. 2. Elements in Fig. 2 that are common to the first example shown in Fig. 1 are given the same reference numerals as in Fig. 1, and detailed descriptions thereof will be omitted as appropriate. The light emitting device 1 shown in Fig. 2 is also of a top emission type. The light emitting device 1 includes a support substrate 2, a transparent substrate 3 that faces the support substrate 2 with a gap therebetween, a light emitting element 4 on the surface of the support substrate 2 that faces the transparent substrate 3, and a sealant 5 that covers the light emitting element 4.

[0037] When the light-emitting element 4 includes an organic EL element, the organic EL element, like the first example, includes, for example, a pair of electrodes 41, 43 and an organic light-emitting layer 42 between the electrodes 41, 43. The organic light-emitting layer 42 includes, for example, a hole injection layer 421, a hole transport layer 422, an organic light-emitting layer 423, and an electron transport layer 424, which are laminated in the above order.

[0038] The light emitting device 1 includes a plurality of light emitting elements 4, which form an array 9 (hereinafter referred to as element array 9) on a support substrate 2. The element array 9 also includes a partition 7. The partition 7 is located on the support substrate 2 and separates two adjacent light emitting elements 4. The partition 7 is produced, for example, by forming a photosensitive resin material using a photolithography method. The element array 9 also includes connection wiring 8 that electrically connects the electrodes 43 and the electron transport layers 424 of adjacent light emitting elements 4 to each other. The connection wiring 8 is provided on the partition 7.

[0039] The light emitting device 1 also includes a passivation layer 6 covering the light emitting element 4. The passivation layer 6 is preferably made of silicon nitride or silicon oxide. The passivation layer 6 includes a first passivation layer 61 and a second passivation layer 62. The first passivation layer 61 covers the element array 9 in a state where the first passivation layer 61 is in direct contact with the element array 9, thereby covering the light emitting element 4. The second passivation layer 62 is disposed on the opposite side of the element array 9 with respect to the first passivation layer 61, and a gap is provided between the second passivation layer 62 and the first passivation layer 61. The sealant 5 is filled between the first passivation layer 61 and the second passivation layer 62. That is, the first passivation layer 61 is interposed between the light emitting element 4 and the sealant 5 covering the light emitting element 4.

[0040] Furthermore, a second sealing material 52 is filled between the second passivation layer 62 and the transparent substrate 3. The second sealing material 52 is made of, for example, a transparent resin material. The material of the second sealing material 52 is not particularly limited. The material of the second sealing material 52 may be the same as or different from the sealing material 5.

[0041] The encapsulant 5 in the light-emitting device 1 having the above-exemplified structure can be produced from the composition (X). That is, the composition (X) is used to produce the encapsulant 5 for the light-emitting element 4. In other words, the composition (X) is preferably a composition for producing an encapsulant, a composition for sealing a light-emitting element, or a composition for producing a light-emitting device.

[0042] 2. Ultraviolet curable resin composition The composition (X) contains a curable component having ultraviolet curability. The curable component contains a cationic polymerizable compound (F) and a cationic curing catalyst (photocationic curing catalyst) (G). The cationic polymerizable compound (F) contains, for example, at least one of a polyfunctional cationic polymerizable compound (F1) and a monofunctional cationic polymerizable compound (F2).

[0043] The polyfunctional cationically polymerizable compound (F1) may contain either one or both of a polyfunctional cationically polymerizable compound (F11) having no siloxane skeleton and a polyfunctional cationically polymerizable compound (F12) having a siloxane skeleton.

[0044] The polyfunctional cationically polymerizable compound (F11) does not have a siloxane skeleton and has two or more cationically polymerizable functional groups per molecule. The number of cationically polymerizable functional groups per molecule of the polyfunctional cationically polymerizable compound (F11) is preferably 2 to 4, and more preferably 2 to 3.

[0045] The cationically polymerizable functional group is, for example, at least one group selected from the group consisting of an epoxy group, an oxetane group, and a vinyl ether group.

[0046] The polyfunctional cationically polymerizable compound (F11) contains at least one compound selected from the group consisting of, for example, polyfunctional alicyclic epoxy compounds, polyfunctional heterocyclic epoxy compounds, polyfunctional oxetane compounds, alkylene glycol diglycidyl ethers, and alkylene glycol monovinyl monoglycidyl ethers.

[0047] The polyfunctional alicyclic epoxy compound contains, for example, either one or both of a compound represented by the following formula (1) and a compound represented by the following formula (20).

[0048] [ka]

[0049] In formula (1), R 1 ~R 18 are each independently a hydrogen atom, a halogen atom, or a hydrocarbon group. The number of carbon atoms in the hydrocarbon group is preferably within the range of 1 to 20. Examples of the hydrocarbon group include alkyl groups having 1 to 20 carbon atoms, such as methyl groups, ethyl groups, and propyl groups; alkenyl groups having 2 to 20 carbon atoms, such as vinyl groups and allyl groups; and alkylidene groups having 2 to 20 carbon atoms, such as ethylidene groups and propylidene groups. The hydrocarbon group may contain an oxygen atom or a halogen atom. 1 ~R 18 Each of the is independently preferably a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, more preferably a hydrogen atom or a methyl group, and most preferably a hydrogen atom.

[0050] In formula (1), X is a single bond or a divalent organic group, and the organic group is, for example, -CO-O-CH2-.

[0051] Examples of the compound represented by formula (1) include a compound represented by the following formula (1a) and a compound represented by the following formula (1b).

[0052] [ka]

[0053] [ka]

[0054] [ka]

[0055] In formula (20), R 1 ~R 12 are each independently a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 20 carbon atoms. The halogen atom is, for example, a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom. The hydrocarbon group having 1 to 20 carbon atoms is, for example, an alkyl group having 1 to 20 carbon atoms such as a methyl group, an ethyl group, or a propyl group; an alkenyl group having 2 to 20 carbon atoms such as a vinyl group or an allyl group; or an alkylidene group having 2 to 20 carbon atoms such as an ethylidene group or a propylidene group. The hydrocarbon group having 1 to 20 carbon atoms may contain an oxygen atom or a halogen atom.

[0056] R 1 ~R 12 Each of the is independently preferably a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, more preferably a hydrogen atom or a methyl group, and most preferably a hydrogen atom.

[0057] An example of the compound represented by formula (20) includes the tetrahydroindene diepoxide represented by formula (20a) below.

[0058] [ka]

[0059] The polyfunctional heterocyclic epoxy compound contains, for example, a trifunctional epoxy compound as shown in the following formula (2).

[0060] [ka]

[0061] The polyfunctional oxetane compound contains, for example, a bifunctional oxetane compound as shown in the following formula (3).

[0062] [ka]

[0063] The alkylene glycol diglycidyl ether contains at least one compound selected from the group consisting of compounds represented by the following formulas (4) to (7).

[0064] [ka]

[0065] [ka]

[0066] [ka]

[0067] [ka]

[0068] The alkylene glycol monovinyl monoglycidyl ether contains, for example, a compound represented by the following formula (8).

[0069] [ka]

[0070] More specifically, the polyfunctional cationically polymerizable compound (F11) may contain at least one component selected from the group consisting of, for example, CELLOXIDE 2021P and CELLOXIDE 8010 manufactured by Daicel, TEPIC-VL manufactured by Nissan Chemical, OXT-221 manufactured by Toagosei, and 1,3-PD-DEP, 1,4-BG-DEP, 1,6-HD-DEP, NPG-DEP, and butylene glycol monovinyl monoglycidyl ether manufactured by Yokkaichi Chemical.

[0071] It is also preferred that the polyfunctional cationically polymerizable compound (F11) contains a polyfunctional alicyclic epoxy compound, in which case the composition (X) can have particularly high cationic polymerization reactivity.

[0072] The polyfunctional alicyclic epoxy compound preferably contains either one or both of the compound represented by formula (1) and the compound represented by formula (20). In this case, the composition (X) can have higher cationic polymerization reactivity.

[0073] When the polyfunctional alicyclic epoxy compound contains a compound represented by formula (1), the compound represented by formula (1) preferably contains a compound represented by formula (1a). In this case, the composition (X) can have a higher cationic polymerization reactivity and a particularly low viscosity.

[0074] In addition, since the compound represented by formula (20) has a low viscosity, the composition (X) can have good UV curing properties and a particularly low viscosity when the composition (X) contains the compound represented by formula (20). Furthermore, the compound represented by formula (20) has a low viscosity but is not easily volatilized. Therefore, even if the composition (X) contains the compound represented by formula (20), the composition (X) is not easily changed in composition due to the volatilization of the compound represented by formula (20). Therefore, the composition (X) can have a low viscosity without impairing storage stability by containing the compound represented by formula (20).

[0075] The compound represented by formula (20) can be synthesized, for example, by oxidizing a cyclic olefin compound having a tetrahydroindene skeleton with an oxidizing agent.

[0076] The compound represented by formula (20) may contain four stereoisomers based on the stereoconfiguration of the two epoxy rings. The compound represented by formula (20) may contain any of the four stereoisomers. That is, the compound represented by formula (20) may contain at least one component selected from the group consisting of the four stereoisomers. In the compound represented by formula (20), the total amount of the exo-endo isomer and the endo-endo isomer among the four stereoisomers is preferably 10% by mass or less, more preferably 5% by mass or less, based on the total epoxy compound (A1). In this case, the heat resistance of the cured product can be improved. The ratio of a specific stereoisomer in the compound represented by formula (20) can be determined based on the peak area ratio appearing in a chromatogram obtained by gas chromatography.

[0077] In order to reduce the amount of exo-endo isomer and endo-endo isomer in the compound represented by formula (20), an appropriate method can be applied, such as a method of subjecting the compound represented by formula (20) to precision distillation or a method of applying column chromatography using silica gel or the like as a packing material.

[0078] When the composition (X) contains a polyfunctional cationic polymerizable compound (F11), the ratio of the polyfunctional cationic polymerizable compound (F11) to the total amount of the resin components is preferably within the range of 5 to 95% by mass. The resin components refer to compounds having cationic polymerizability in the composition (X), and include the polyfunctional cationic polymerizable compound (F1) and the monofunctional cationic polymerizable compound (F2). When the ratio of the polyfunctional cationic polymerizable compound (F11) is 5% by mass or more, the composition (X) can have particularly excellent reactivity during the photocationic polymerization reaction, and the cured product can have high strength (hardness). When the ratio of the polyfunctional cationic polymerizable compound (F11) is 95% by mass or less, when the composition (X) contains a moisture absorbent (C), the moisture absorbent (C) can be particularly easily dispersed uniformly in the composition (X). The proportion of this polyfunctional cationic polymerizable compound (F11) is more preferably 12% by mass or more, even more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass or more. The proportion of this polyfunctional cationic polymerizable compound (F11) is more preferably 85% by mass or less, even more preferably 60% by mass or less. For example, the proportion of the polyfunctional cationic polymerizable compound (F11) is preferably within the range of 20 to 60% by mass.

[0079] When the polyfunctional cationic polymerizable compound (F11) contains a polyfunctional alicyclic epoxy compound, the polyfunctional alicyclic epoxy compound may be a part or the whole of the polyfunctional cationic polymerizable compound (F11). The ratio of the polyfunctional alicyclic epoxy compound to the polyfunctional cationic polymerizable compound (F11) is preferably within the range of 15 to 100 mass%. When this ratio is 15 mass% or more, the polyfunctional alicyclic epoxy compound can particularly contribute to improving the ultraviolet curing property of the composition (X).

[0080] The polyfunctional cationic polymerizable compound (F12) has a siloxane skeleton and two or more cationic polymerizable functional groups per molecule. The number of cationic polymerizable functional groups per molecule of the polyfunctional cationic polymerizable compound (F12) is preferably 2 to 6, more preferably 2 to 4. The polyfunctional cationic polymerizable compound (F12) can contribute to improving the cationic polymerization reactivity of the composition (X) and can also contribute to improving the heat discoloration resistance of the cured product and optical components. The polyfunctional cationic polymerizable compound (F12) can also contribute to lowering the elastic modulus of the cured product and optical components. When the composition (X) contains a moisture absorbent, the polyfunctional cationic polymerizable compound (F12) can also contribute to improving the dispersibility of the moisture absorbent in the composition (X) and the cured product.

[0081] The polyfunctional cationically polymerizable compound (F12) is preferably a liquid at 25° C. In particular, the viscosity of the polyfunctional cationically polymerizable compound (F12) at 25° C. is preferably within the range of 10 to 300 mPa s. In this case, an increase in the viscosity of the composition (X) can be suppressed.

[0082] The cationically polymerizable functional group contained in the polyfunctional cationically polymerizable compound (F12) is, for example, at least one group selected from the group consisting of an epoxy group, an oxetane group, and a vinyl ether group.

[0083] The siloxane skeleton of the polyfunctional cationic polymerizable compound (F12) may be linear, branched, or cyclic. The number of Si atoms in the siloxane skeleton is preferably within the range of 2 to 14. In this case, the composition (X) can have a particularly low viscosity. The number of Si atoms is more preferably within the range of 2 to 10, even more preferably within the range of 2 to 7, and particularly preferably within the range of 3 to 6.

[0084] The polyfunctional cationically polymerizable compound (F12) contains, for example, at least one of a compound represented by formula (10) and a compound represented by formula (11).

[0085] [ka]

[0086] [ka]

[0087] In each of formulas (10) and (11), R is a single bond or a divalent organic group, and is preferably an alkylene group. Y is a siloxane skeleton, which may be linear, branched, or cyclic, and the number of Si atoms is preferably within a range of 2 to 14, more preferably within a range of 2 to 10, even more preferably within a range of 2 to 7, and particularly preferably within a range of 3 to 6. n is an integer of 2 or more, and is preferably within a range of 2 to 4.

[0088] More specifically, for example, the polyfunctional cationically polymerizable compound (F12) contains a compound represented by the following formula (10a).

[0089] [ka]

[0090] R in formula (10a) is a single bond or a divalent organic group, and is preferably an alkylene group having 1 to 4 carbon atoms. n in formula (10a) is an integer of 0 or more. n is preferably within the range of 0 to 12, more preferably within the range of 0 to 8, even more preferably within the range of 0 to 5, and particularly preferably within the range of 1 to 4.

[0091] More specifically, the polyfunctional cationically polymerizable compound (F12) preferably contains at least one component selected from the group consisting of product numbers X-40-2669, X-40-2670, X-40-2715, X-40-2732, X-22-169AS, X-22-169B, X-22-2046, X-22-343, X-22-163, and X-22-163B manufactured by Shin-Etsu Chemical Co., Ltd.

[0092] The polyfunctional cationic polymerizable compound (F12) preferably has an alicyclic epoxy structure, and it is particularly preferred that the polyfunctional cationic polymerizable compound (F12) contains a compound represented by formula (10a). The compound represented by formula (10a) can particularly contribute to improving the cationic polymerization reactivity and lowering the viscosity of the composition (X), and can also particularly contribute to improving the heat discoloration resistance and lowering the elastic modulus of the cured product and optical parts. When the composition (X) contains a moisture absorbent (C), it can also particularly contribute to improving the dispersibility of the moisture absorbent (C) in the composition (X).

[0093] When the composition (X) contains a polyfunctional cationic polymerizable compound (F12), the ratio of the polyfunctional cationic polymerizable compound (F12) to the total amount of the resin components is preferably within the range of 5 to 95% by mass. In this case, when the composition (X) contains a moisture absorbent (C), the dispersibility of the moisture absorbent (C) in the composition (X) and in the cured product is particularly improved, and the composition (X) can have a particularly high photocationic polymerization reactivity.

[0094] The monofunctional cationically polymerizable compound (F2) has only one cationically polymerizable functional group per molecule, which is, for example, at least one group selected from the group consisting of an epoxy group, an oxetane group, and a vinyl ether group.

[0095] The viscosity of the monofunctional cationic polymerizable compound (F2) at 25°C is preferably 8 mPa·s or less. In this case, even if the composition (X) does not contain a solvent, the monofunctional cationic polymerizable compound (F2) can reduce the viscosity of the composition (X). In particular, the viscosity of the monofunctional cationic polymerizable compound (F2) at 25°C is preferably within the range of 0.1 to 8 mPa·s.

[0096] The monofunctional cationically polymerizable compound (F2) may contain, for example, at least one compound selected from the group consisting of the compounds represented by the following formulas (12) to (17) and limonene oxide.

[0097] [ka]

[0098]

change

[0099]

change

[0100]

change

[0101]

change

[0102]

change

[0103] The ratio of the monofunctional cationic polymerizable compound (F2) to the total amount of the resin components is preferably within the range of 5 to 50% by mass. If the ratio of the monofunctional cationic polymerizable compound (F2) is 5% by mass or more, the viscosity of the composition (X) can be particularly reduced. If the ratio of the monofunctional cationic polymerizable compound (F2) is 50% by mass or less, the composition (X) can have particularly excellent reactivity during the photocationic polymerization reaction, and the cured product can have high strength (hardness). The ratio of this monofunctional cationic polymerizable compound (F2) is more preferably 10% by mass or more, and even more preferably 15% by mass or more. The ratio of this monofunctional cationic polymerizable compound (F2) is more preferably 40% by mass or less, even more preferably 35% by mass or less, and particularly preferably 30% by mass or less. If the proportion of the monofunctional cationic polymerizable compound (F2) is particularly 35% by mass or less, the amount of volatilization of the components in the composition (X) during storage of the composition (X) can be effectively reduced, and therefore the properties of the composition (X) are less likely to be impaired even if the composition (X) is stored for a long period of time. Furthermore, the occurrence of tack in the cured product can be particularly suppressed. For example, it is preferable that the proportion of the monofunctional cationic polymerizable compound (F2) is within the range of 10 to 35% by mass.

[0104] The cationic polymerizable compound (F) may not contain the monofunctional cationic polymerizable compound (F2). In this embodiment, even if the cationic polymerizable compound (F) does not contain the monofunctional cationic polymerizable compound (F2), the transparency of the optical component is not easily decreased even if the curability of the composition (X) is increased, and the composition (X) is easily realized to have low viscosity and high storage stability.

[0105] In particular, when the composition (X) contains a polyfunctional cationic polymerizable compound (F11) and a polyfunctional cationic polymerizable compound (F12), the ratio of the polyfunctional cationic polymerizable compound (F11) is preferably within the range of 30-60 mass%, the ratio of the polyfunctional cationic polymerizable compound (F12) is preferably within the range of 15-30 mass%, and the ratio of the monofunctional cationic polymerizable compound (F2) is preferably within the range of 15-40 mass% based on the total amount of the resin components. In this case, the composition (X) can achieve a good balance of good storage stability, low viscosity, and good cationic polymerization reactivity, and further achieve a good balance of excellent transparency, excellent hygroscopicity, and high refractive index of the cured product.

[0106] When the cationically polymerizable compound (F) contains the compound represented by formula (3) and the compound represented by formula (16), by adjusting the ratio of the two, it is possible to appropriately adjust the ease of progress of the curing reaction when preparing a photocured product from the composition (X), while achieving a low viscosity and improved storage stability of the composition (X).

[0107] The amount of the compound represented by formula (16) is appropriately adjusted so that the composition (X) has the above-mentioned properties. For example, the amount of the compound represented by formula (16) is preferably 10 mass% or more and 40 mass% or less based on the total amount of the resin components.

[0108] As described above, when the cationic polymerizable compound (F) contains the aromatic epoxy compound (f1), the aromatic epoxy compound (f1) tends to lower the viscosity of the composition (X) and tends to improve the storage stability of the composition (X). In addition, the aromatic epoxy compound (f1) is less likely to generate outgassing from the cured product, tends to improve the heat resistance of the cured product, and tends to prevent satellites from being generated when the composition (X) is discharged by an inkjet method.

[0109] The aromatic epoxy compound (f1) preferably contains at least one compound selected from the group consisting of the compounds represented by the following formulas (301) to (318).

[0110] [ka]

[0111] In particular, it is preferred that the aromatic epoxy compound (f1) contains at least one component selected from the group consisting of the compounds represented by the formulas (301) to (305), (312), (314), and (318). These compounds tend to have high reactivity because at least one epoxy group (oxirane) in the compound is bonded to a benzene ring via a single bond or an alkylene group, and therefore tend to enhance the curability of the composition (X).

[0112] The ratio of the aromatic epoxy compound (f1) to the entire cationic polymerizable compound (F) is preferably 5% by mass or more. In this case, the above-mentioned effect of the aromatic epoxy compound (f1) is particularly easily obtained. This ratio is also preferably 95% by mass or less. In this case, the storage stability of the composition (X) is easily improved. This ratio is more preferably 10% by mass or more and 90% by mass or less, and even more preferably 20% by mass or more and 85% by mass or less.

[0113] It is also preferred that the cationically polymerizable compound (F) contains a compound (f2) having an oxyalkylene skeleton. The oxyalkylene skeleton is a linear skeleton consisting of one or more linear oxyalkylene units.

[0114] When the cationic polymerizable compound (F) contains the compound (f2), the compound (f2) has a low viscosity, and therefore the compound (f2) tends to lower the viscosity of the composition (X). In addition, the compound (f2) is not easily volatilized, and therefore, even if the composition (X) is stored, the composition (X) is not easily changed in composition due to the volatilization of the aromatic epoxy compound (f1). Therefore, the compound (f2) tends to increase the storage stability of the composition (X).

[0115] In addition, the compound (f2) is less likely to produce defective droplets called satellites when the composition (X) is discharged by the inkjet method. Furthermore, the compound (f2) can make it difficult for satellites to be produced even if the speed of the droplets discharged by the inkjet method is increased. Therefore, although it depends on the inkjet conditions, it is possible to make the discharge speed of the droplets by the inkjet method 4 m / s or more without producing satellites, for example. If the droplet speed can be increased, the trajectory of the droplets is less susceptible to disturbances, so that the dimensional accuracy of the optical components produced from the composition (X) can be improved. Furthermore, the compound (f2) can increase the storage stability of the composition (X) as described above, so that the characteristic of the composition (X) of being less likely to produce satellites is easily maintained even if the composition (X) is stored for a long period of time.

[0116] It is particularly preferable that the oxyalkylene skeleton contains a structure of "-CCO-", that is, an oxymethylene unit. In this case, satellites are particularly unlikely to be generated, and even if the driving frequency is changed when discharging the composition (X) by an inkjet method, satellites are unlikely to be generated. In addition, the compound (f2) is less likely to volatilize and is more likely to have a lower viscosity, and further, the affinity (wettability) of the composition (X) to inorganic materials is likely to be increased.

[0117] The number of oxyalkylene units in the oxyalkylene skeleton of compound (f2) is preferably 1 to 8. In this case, compound (f2) tends to have a lower viscosity, so that satellites are particularly unlikely to be generated, and the crosslink density of the cured product tends to be high, so that the glass transition temperature of the cured product tends to be particularly high. The number of oxyalkylene units is more preferably 1 to 6, and even more preferably 1 to 4.

[0118] In addition, the oxyalkylene unit in the oxyalkylene skeleton of the compound (f2) may have a substituent other than hydrogen. For example, the oxymethylene unit contained in the oxyalkylene skeleton may have a structure of "-CH(CH3)-CH2-O-".

[0119] The ratio of the compound (f2) is preferably 10% by mass or more relative to the cationically polymerizable compound (F). In this case, the inkjet property is good, and the wettability to the substrate is improved. It is also preferable that this ratio is 70% by mass or less. In this case, the glass transition temperature can be sufficiently increased. This ratio is more preferably 15% by mass or more and 60% by mass or less, and even more preferably 20% by mass or more and 50% by mass or less.

[0120] The compound (f2) contains, for example, at least one compound selected from a compound (f21) having an oxyalkylene skeleton and an epoxy group, and a compound (f22) having an oxyalkylene group and an oxetane group.

[0121] Compound (f21) contains at least one compound selected from the group consisting of, for example, the compound represented by the above formula (1b), the compound represented by formula (4), the compound represented by formula (5), the compound represented by formula (6), the compound represented by formula (7), the compound represented by formula (8), the compound represented by formula (13), the compound represented by formula (14), etc. Note that the components that compound (f21) can contain are not limited to the above.

[0122] Compound (f22) contains at least one compound selected from the group consisting of compounds represented by the above formula (3), compounds represented by formula (12), compounds represented by formula (16), and compounds represented by formula (17). Note that the components that compound (f22) can contain are not limited to the above.

[0123] It is also preferable that the cationic polymerizable compound (F) contains an epoxy compound and the above-mentioned compound (f22). The epoxy compound contains at least one compound among the compounds having an epoxy group among the compounds that can be contained in the above-mentioned cationic polymerizable compound (F). When the cationic polymerizable compound (F) contains an epoxy compound and a compound (f22), the curability of the composition (X) is easily increased when the composition (X) is irradiated with ultraviolet light, and the composition (X) is not likely to be cured too rapidly at this time, so that the cured product is not likely to have a deterioration in transparency due to white turbidity or the like. The mechanism that causes this effect is presumed to be as follows. Since the reactivity of the compound (f22) is lower than that of the epoxy compound, when the composition (X) is irradiated with ultraviolet light, the epoxy compound reacts first. This reaction of the epoxy compound makes it easier to increase the curability of the composition (X). Subsequently, the compound (f22) reacts, making it difficult to cause a situation in which the epoxy compound and the compound (f22) react at the same time. It is considered that this makes it difficult to cause an excessively rapid reaction. In this case, the ratio of the compound (f22) to the cationic polymerizable compound (F) is preferably 20% by mass or more. In this case, the compound (f22) particularly easily reduces the viscosity of the composition (X) and particularly easily increases the storage stability of the composition (X). Furthermore, the compound (f22) particularly easily increases the curability of the composition (X). The ratio of the compound (f22) is also preferably 90% by mass or less. In this case, the curability of the cured product can be sufficiently increased. The ratio of the compound (f22) is more preferably 10% by mass or more and 90% by mass or less, and even more preferably 20% by mass or more and 80% by mass or less. In addition, the ratio of the epoxy compound in this case is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more and 80% by mass or less, and even more preferably 25% by mass or more and 75% by mass or less, based on the total amount of the cationic polymerizable compound (F). In these cases, the unreacted groups in the cured product can be sufficiently reduced, and the curability of the cured product can be sufficiently increased.

[0124] The epoxy compound preferably contains a compound having at least one oxirane ring that does not constitute a glycidyl ether group. In this case, the epoxy compound is particularly likely to enhance the curability of the composition (X). It is more preferable that the epoxy compound contains a compound having two or more oxirane rings that do not constitute a glycidyl ether group. It is also preferable that the epoxy compound contains a compound that does not have a glycidyl ether group. It is particularly preferable that the epoxy compound contains a compound that has two or more oxirane rings that do not constitute a glycidyl ether group and does not have a glycidyl ether group.

[0125] It is particularly preferred that the cationic polymerizable compound (F) contains the compound (f2) and an epoxy compound, and that the epoxy compound further contains the aromatic epoxy compound (f1) described above. In this case, the composition (X) is particularly likely to have excellent storage stability, and when the composition (X) is discharged by an inkjet method, defective droplets called satellites are particularly unlikely to be generated. Furthermore, even if the speed of the droplets discharged by the inkjet method is increased, satellites are particularly unlikely to be generated. Furthermore, even if the composition (X) is stored for a long period of time, the characteristic of the composition (X) that satellites are not likely to be generated is particularly likely to be maintained. In this case, it is particularly preferred that the compound (f2) contains the compound (f22).

[0126] The total ratio of the aromatic epoxy compound (f1) and the compound (f22) to the cationic polymerizable compound (F) is preferably 55% by mass or more. In this case, the effect of the combination of the aromatic epoxy compound (f1) and the compound (f22) is particularly remarkable. This ratio is more preferably 60% by mass or more, and even more preferably 70% by mass or more. It is particularly preferable that the cationic polymerizable compound (F) contains only the aromatic epoxy compound (f1) and the compound (f22).

[0127] The compound (f3) having an oxetane group may contain at least one selected from the group consisting of compounds having at least one oxetane group among the above compounds. For example, the compound (f3) may contain a compound (f22) having an oxyalkylene group and an oxetane group. The compound (f3) may also contain a compound having an oxetane group but not an oxyalkylene group.

[0128] The ratio of compound (f3) to cationic polymerizable compound (F) is preferably 10% by mass or more and 90% by mass or less. If this ratio is 10% by mass or more, the cured product is particularly unlikely to be colored due to yellowing or white turbidity. If this ratio is 90% by mass or less, there is an advantage that the reaction rate when irradiating composition (X) with ultraviolet light can be easily increased to a practically sufficient level. This ratio is more preferably 20% by mass or more. Also, this ratio is more preferably 80% by mass or less.

[0129] The cationic curing catalyst (G) is not particularly limited as long as it is a catalyst that generates a protonic acid or a Lewis acid upon irradiation with light. The cationic curing catalyst (G) may contain at least one of an ionic photoacid generator and a nonionic photoacid generator.

[0130] The ionic photoacid generator may contain at least one of onium salts and organometallic complexes. Examples of onium salts include aromatic diazonium salts, aromatic halonium salts, and aromatic sulfonium salts. Examples of organometallic complexes include iron-arene complexes, titanocene complexes, and arylsilanol-aluminum complexes. The ionic photoacid generator may contain at least one of these components.

[0131] The non-ionic photoacid generator can contain, for example, at least one component selected from the group consisting of nitrobenzyl esters, sulfonic acid derivatives, phosphate esters, phenolsulfonic acid esters, diazonaphthoquinones, and N-hydroxyimide phosphonates.

[0132] More specific examples of compounds that can contain the cationic curing catalyst (G) include Midori Chemical's DPI series (105, 106, 109, 201, etc.), BI-105, MPI series (103, 105, 106, 109, etc.), BBI series (101, 102, 103, 105, 106, 109, 110, 200, 210, 300, 301, etc.), and TSP series. (102, 103, 105, 106, 109, 200, 300, 1000, etc.), HDS-109, MDS series (103, 105, 109, 203, 205, 209, etc.), BDS-109, MNPS-109, DTS series (102, 103, 105, 200, etc.), NDS series (103, 105, 155, 165, etc.), DAM series (10 1, 102, 103, 105, 201, etc.), SI series (105, 106, etc.), PI-106, NDI series (105, 106, 109, 1001, 1004, etc.), PAI series (01, 101, 106, 1001, 1002, 1003, 1004, etc.), MBZ-101, PYR-100, NB series (101, 201, etc.), NAI series series (100, 1002, 1003, 1004, 101, 105, 106, 109, etc.), TAZ series (100, 101, 102, 103, 104, 107, 108, 109, 110, 113, 114, 118, 122, 123, 203, 204, etc.), NBC-101, ANC-101, TPS-Acetate, DTS-Acetate, Di-Boc Bisphinol A, tert-Butyl lithocholate, tert-Butyl deoxycholate, tert-Butyl cholate, BX, BC-2, MPI-103, BDS-105, TPS-103, NAT-103, BMS-105, and TMS-105; Cyracure UVI-6970, Cyracure UVI-6974, Cyracure UVI-6990, and Cyracure UVI-950 manufactured by Union Carbide Corporation, USA; Irgacure 250, Irgacure 261 and Irgacure 264 from BASF; Ciba-Geigy CG-24-61; ADEKA OPTOMER SP-150, ADEKA OPTOMER SP-151, ADEKA OPTOMER SP-170 and ADEKA OPTOMER SP-171 manufactured by ADEKA Corporation; DAICAT II manufactured by Daicel Corporation; UVAC1590 and UVAC1591 manufactured by Daicel-Cytec Co., Ltd.; CI-2064, CI-2639, CI-2624, CI-2481, CI-2734, CI-2855, CI-2823, CI-2758, and CIT-1682 manufactured by Nippon Soda Co., Ltd.; PI-2074, tetrakis(pentafluorophenyl)borate toluylcumyl iodonium salt, from Rhodia; 3M FFC509; CD-1010, CD-1011 and CD-1012 manufactured by Sartomer, USA; CPI-100P, CPI-101A, CPI-110P, CPI-110A and CPI-210S manufactured by San-Apro Ltd.; and UVI-6992 and UVI-6976 manufactured by The Dow Chemical Company. The cationic curing catalyst (G) may contain at least one compound selected from the group consisting of these compounds.

[0133] The cationic curing catalyst (G) preferably contains a plurality of ionic photoacid generators having different conjugate acid strengths of anion species. In this case, among the plurality of ionic photoacid generators, the ionic photoacid generator having a higher conjugate acid strength can increase the reactivity of the composition (X), and therefore the efficiency of producing an optical component from the composition (X) can be increased. In addition, when the composition (X) contains the above-mentioned plurality of ionic photoacid generators, the composition (X) is less likely to gel during storage of the composition (X), that is, the storage stability of the composition (X) is less likely to decrease. This is presumably because, even if an anion species having a high conjugate acid strength is released from the ionic photoacid generator during storage of the composition (X), an anion species having a low conjugate acid strength is easily released due to an acid exchange reaction involving another ionic photoacid generator, and therefore the concentration of the anion species having a high conjugate acid strength in the composition (X) is less likely to increase. Furthermore, even when composition (X) is irradiated with ultraviolet light, composition (X) is unlikely to cure too rapidly, and therefore the cured product is unlikely to suffer from deterioration in transparency due to turbidity, etc. This is presumably because, even if an anion species having a high conjugate acid strength is released from the ionic photoacid generator by irradiation with ultraviolet light, an anion species having a low conjugate acid strength is likely to be released by the same mechanism as in the above case, and therefore an excessively rapid reaction caused by an anion species having a high conjugate acid strength is suppressed.

[0134] The cationic curing catalyst (G) preferably contains a first agent (g1) containing an ionic photoacid generator having an anion species whose conjugate acid strength is higher, and a second agent (g2) containing an ionic photoacid generator having an anion species whose conjugate acid strength is lower.

[0135] The first agent (g1) preferably contains an ionic photoacid generator having an anion species whose conjugate acid strength is equal to or greater than that of HSbF6. The second agent (g2) preferably contains an ionic photoacid generator having an anion species whose conjugate acid strength is lower than that of HSbF6, and more preferably contains an ionic photoacid generator having an anion species whose conjugate acid strength is equal to or less than that of HPF6.

[0136] The first agent (g1) is, for example, (Rf)n PF 6-n - (Rx) an ionic photoacid generator having n BX 4-n - and (Rx) n GaX 4-n - The second agent (g2) contains at least one ionic photoacid generator selected from the group consisting of ionic photoacid generators having the formula: - Ionic photoacid generator having BF4 - have Ionic photoacid generator, (Rf)SO3 - The photoacid generator contains at least one ionic photoacid generator selected from the group consisting of ionic photoacid generators having a sulfite ion, and ionic photoacid generators having a sulfite ion.

[0137] In addition, (Rf) n PF 6-n - and (Rf)SO3 - In the formula, Rf is a perfluoroalkyl group, (Rf) n PF 6-n - In this formula, n is a number between 1 and 5. (Rf) n PF 6-n - In the formula, the number of carbon atoms in Rf is, for example, 1 or more and 3 or less, and when there are multiple Rfs, the Rfs may be the same or different. (Rf)SO3 - In the formula, Rf has 1 or more and 8 or less carbon atoms.

[0138] (Rx) n BX 4-n - and (Rx) n GaX 4-n - In each of the above, Rx is a phenyl group in which some of the hydrogen atoms are substituted with halogen atoms or electron-withdrawing substituents. The halogen atoms are fluorine atoms, chlorine atoms, bromine atoms, etc. The electron-withdrawing substituents are, for example, trifluoromethyl groups, nitro groups, cyano groups, etc. (Rx) n BX4-n - and (Rx) n GaX 4-n - In each of the above, X is a halogen atom, and preferably a fluorine atom. (Rx) n BX 4-n - and (Rx) n GaX 4-n - In each of the formulas, n is any number from 1 to 4. When there are multiple Rx, Rx may be the same or different. Rx is, for example, C6F5, (CF3)2C6H3, CF3C6H4, or C6H3F2. (Rx) n BX 4-n - For example, (C6F5)4B - , ((CF3)2C6H3)4B - , (CF3C6H4)4B - , (C6F5)2BF2 - , C6F5BF3 - or (C6H3F2)4B - etc.

[0139] Cationic curing catalyst (G) is PF6 - When an ionic photoacid generator having the above formula is used, the PF6 relative to the total amount of cationic curing catalyst (G) is - The amount of the ionic photoacid generator having PF6 is preferably less than 50% by weight. - PF6 may generate a small amount of hydrofluoric acid, which may attack inorganic materials such as silicon nitride and silicon oxide, which are used in the passivation layer. - When the amount of the ionic photoacid generator having the formula PF6 is 50 mass % or less as described above, the risk of hydrofluoric acid corroding inorganic materials can be reduced. - It is more preferable that the amount of the ionic photoacid generator having the formula be 25% by mass or less.

[0140] The cationic curing catalyst (G) is (Rf) n PF 6-n -When an ionic photoacid generator having the formula (Rf) is contained, the total amount of the cationic curing catalyst (G) is n PF 6-n - The amount of the ionic photoacid generator having the formula (Rf) is preferably 75% by mass or less. n PF 6-n - PF6 - Although not as strong as fluorine, it may generate a small amount of hydrofluoric acid. n PF 6-n - When the amount of the ionic photoacid generator having the formula (I) is 75 mass % or less as described above, the risk of hydrofluoric acid attacking inorganic materials can be reduced.

[0141] In addition, the cationic curing catalyst (G) is PF6 - and an ionic photoacid generator having (Rf) n PF 6-n - When both an ionic photoacid generator having the same structure and a cationic curing catalyst (G) are used, the PF6 - It is preferable that the amount of the ionic photoacid generator having PF6 is 25% by mass or less. - and an ionic photoacid generator having (Rf) n PF 6-n - It is particularly preferable that the total amount of the ionic photoacid generator having the formula (I) is 80 mass % or less based on the total amount of the cationic curing catalyst (G).

[0142] On the other hand, (Rx) n BX 4-n - and (Rx) n GaX 4-n - The ionic photoacid generator having the above structure is unlikely to generate hydrofluoric acid. is preferable.

[0143] The cationic species in the ionic photoacid generator contained in the first agent (g1) and the cationic species in the ionic photoacid generator contained in the second agent (g2) are not particularly limited, and may be, for example, at least one selected from the group consisting of various aromatic oniums, more specifically, various aromatic diazoniums, aromatic haloniums, aromatic sulfoniums, and the like.

[0144] When the cationic curing catalyst (G) contains the first agent (g1) and the second agent (g2), the composition (X) has good curability, the cured product of the composition (X) is particularly unlikely to become cloudy, and the storage stability of the composition (X) is particularly likely to be high.

[0145] The ratio of the first agent to the total amount of the first agent (g1) and the second agent (g2) is preferably 50% by mass or more. In this case, the composition (X) can have good curability. In addition, this ratio is preferably 90% by mass or less. In this case, the cured product is particularly unlikely to become cloudy, and the storage stability of the composition (X) is particularly likely to be high. This ratio is more preferably 60% by mass or more and 90% by mass or less, and even more preferably 70% by mass or more and 85% by mass or less.

[0146] In this embodiment, the strengths of the conjugate acids of the compounds contained in the cationic curing catalyst (G) may all be the same, that is, for example, the cationic curing catalyst (G) may contain only one type of compound.

[0147] The proportion of the cationic curing catalyst (G) relative to the total amount of the resin components is preferably 1% by mass or more and 4% by mass or less. When this proportion is 1% by mass or more, the composition (X) can have particularly good cationic polymerization reactivity. Also, when this proportion is 4% by mass or less, the composition (X) can have good storage stability, and since it does not contain an excessive amount of the cationic curing catalyst (G), it is possible to reduce the production cost.

[0148] The composition (X) may contain a sensitizer (H). The sensitizer (H) contains, for example, either one or both of 9,10-dibutoxyanthracene and 9,10-diethoxyanthracene. The ratio of the sensitizer (H) to the total amount of the resin components is preferably in the range of more than 0 mass% and not more than 1 mass%. In this case, the sensitizer (H) is unlikely to inhibit the transparency of the cured product, and therefore the cured product can have good transparency. It is more preferable that the amount of the sensitizer (H) is more than 0 mass% and not more than 0.8 mass% to the total amount of the resin components.

[0149] The composition (X) may further contain a moisture absorbent (C). When the composition (X) contains the moisture absorbent (C), the cured product can have excellent moisture absorption. The average particle size of the moisture absorbent (C) is preferably 200 nm or less. In this case, the cured product can have high transparency despite containing the moisture absorbent (C). In addition, particularly when the composition (X) is discharged by an inkjet method, if the average particle size of the moisture absorbent (C) is 200 nm or less, there is an advantage that the composition (X) is less likely to clog the nozzle. Furthermore, if the average particle size of the moisture absorbent (C) is 200 nm or less, the moisture absorbent (C) is less likely to impair the smoothness of the surface of the optical component made from the composition (X). Therefore, the surface of the optical component can have good smoothness.

[0150] As described above, the moisture absorbent (C) allows the cured product to have high moisture absorption. The moisture absorption rate of the cured product is preferably 0.5% by mass or more, more preferably 1% by mass or more, and most preferably 2% by mass or more. The moisture absorption rate is determined by the following method. In an argon atmosphere, the composition (X) is applied and then irradiated with ultraviolet light to produce a film with a thickness of 10 μm. The ultraviolet light irradiation conditions are, for example, a peak wavelength of 365 nm and an ultraviolet light intensity of 3000 mW / cm. 2 The UV exposure time is 10 seconds. For example, the film is vacuum dried using a vacuum dryer at a heating temperature of 120°C for a heating time of 3 hours. The mass of the film after drying is measured. This measurement result is called the initial mass (M0). Next, the film is allowed to fully absorb moisture. To do this, for example, the film is exposed to conditions of 85°C and 85% RH for 24 hours. The mass of the film after moisture absorption is measured. This measurement result is called the mass after moisture absorption (M). The moisture absorption rate can be calculated from the initial mass (M0) and the mass after moisture absorption (M) using the formula (M-M0) / M0 x 100 (mass%).

[0151] The moisture absorbent (C) is preferably an inorganic particle having moisture absorbing properties, and preferably contains at least one component selected from the group consisting of, for example, zeolite particles, silica gel particles, calcium chloride particles, and titanium oxide nanotube particles. It is particularly preferable that the moisture absorbent (C) contains zeolite particles.

[0152] Zeolite particles having an average particle size of 200 nm or less can be produced, for example, by crushing general industrial zeolite. When producing zeolite particles, the zeolite may be crushed and then crystallized by hydrothermal synthesis or the like, in which case the zeolite particles can have particularly high hygroscopicity. As a method for producing such nano-sized zeolite particles, for example, the methods disclosed in JP 2016-69266 A and JP 2013-049602 A can be used.

[0153] The zeolite particles are preferably produced from a zeolite containing sodium ions as a raw material, and more preferably from at least one selected from the group consisting of A-type zeolite, X-type zeolite, and Y-type zeolite among the zeolites containing sodium ions as a raw material. It is particularly preferable that the zeolite particles are produced from 4A-type zeolite among the A-type zeolites as a raw material. In these cases, the zeolite particles have a crystal structure suitable for adsorbing moisture.

[0154] Here is a specific example of a method for producing zeolite particles with an average particle size of 200 nm or less. First, zeolite powder is prepared as a raw material, and the zeolite powder is physically pulverized. For example, the zeolite powder is mixed with water to prepare a slurry, and the slurry is put into a bead mill to physically pulverize the zeolite powder.

[0155] Next, the zeolite powder is crystallized by hydrothermal synthesis. For example, the slurry containing the zeolite powder after physical crushing is heated in an autoclave to perform hydrothermal synthesis. The conditions for hydrothermal synthesis are, for example, a heating temperature in the range of 150 to 200°C and a heating time in the range of 15 to 24 hours.

[0156] The zeolite powder is then dried. The drying temperature is, for example, within a range of 150 to 200° C., and the drying time is, for example, within a range of 2 to 3 hours. If necessary, the dried zeolite powder is crushed using a mortar or the like, and then sieved to adjust the particle size.

[0157] Subsequently, if necessary, the zeolite powder is subjected to an ion exchange treatment. In particular, when the zeolite powder is a sodium-containing zeolite such as LTA, it is preferable to perform an ion exchange treatment in which sodium in the zeolite powder is exchanged with magnesium.

[0158] The ion exchange treatment is carried out, for example, by dispersing zeolite powder in an aqueous solution containing magnesium ions to prepare a mixture, and heating the mixture. More specifically, the ion exchange treatment is carried out, for example, as follows. First, zeolite powder is mixed with magnesium chloride and water, and the resulting mixture is stirred while being heated. During this treatment, it is preferable to temporarily stop stirring, discard the supernatant of the mixture, and then replenish the mixture with water before restarting stirring, and repeat this operation several times at appropriate intervals. The heating temperature in this treatment is preferably within the range of 40 to 80°C, and the treatment time is within the range of 6 to 8 hours.

[0159] When the ion exchange treatment is performed, the zeolite powder is then dried. The drying temperature is, for example, within the range of 150 to 200°C, and the drying time is, for example, within the range of 2 to 3 hours. Then, if necessary, the dried zeolite powder is crushed using a mortar or the like and then sieved to adjust the particle size. This allows zeolite particles with an average particle size of 200 nm or less to be obtained.

[0160] The crystallization of the zeolite powder can also be carried out in the presence of silicate and alkali metal oxide. In that case, a specific example of a method for producing zeolite particles with an average particle size of 200 nm or less will be described. First, zeolite powder is prepared. The zeolite powder preferably has a composition of aM12O·bSiO2·Al2O3·cMe. M1 is an alkali metal, a proton, or an ammonium ion (NH4 + ), Me is an alkaline earth metal, a is a number within the range of 0.01 to 1, b is a number within the range of 20 to 80, and c is a number within the range of 0 to 1. The zeolite powder preferably contains a zeolite containing sodium ions, and more preferably contains at least one material selected from the group consisting of A-type zeolite, X-type zeolite, and Y-type zeolite among the zeolites containing sodium ions. It is particularly preferable that the zeolite powder contains 4A-type zeolite among the A-type zeolites. This zeolite powder is physically pulverized. For example, the zeolite powder can be physically pulverized by putting the zeolite powder into a bead mill pulverizer.

[0161] The physically pulverized zeolite powder is dispersed in a solution containing M22O, SiO2, and H2O to prepare a slurry. M2 is an alkali metal, preferably K or Na. The molar ratio of M22O / H2O is, for example, within a range of 0.003 to 0.01, and the molar ratio of SiO2 / H2O is, for example, within a range of 0.006 to 0.025. The amount of zeolite powder is, for example, 0.5 to 10 g per 100 ml of solution.

[0162] The slurry is heated in an autoclave to crystallize the zeolite powder. The conditions are, for example, a heating temperature in the range of 100 to 230°C and a heating time in the range of 1 to 24 hours. The zeolite powder is then washed and dried. This allows zeolite particles with an average particle size of 200 nm or less to be obtained.

[0163] The pH of the zeolite particles is preferably 7 or more and 10 or less. When the pH of the zeolite particles is 7 or more, the crystals of the zeolite particles are less likely to be destroyed, and therefore an optical component made from the composition (X) containing the zeolite particles can have particularly high hygroscopicity. In addition, when the pH of the zeolite particles is 10 or less, the zeolite particles are less likely to inhibit the curing of the composition (X).

[0164] The pH of the zeolite particles is a value obtained by heating the resulting dispersion of 0.05 g of zeolite particles in 99.95 g of ion-exchanged water at 90° C. for 24 hours, and then measuring the pH of the supernatant of the dispersion with a pH meter. The pH meter can be, for example, a compact pH meter manufactured by Horiba, Ltd. <laquatwin>B-711 can be used.

[0165] In order for the zeolite particles to have a pH of 7 or more and 10 or less, the zeolite particles are preferably made of FAU Y-type zeolite having protons as counter cations.

[0166] In the process of producing zeolite particles, when hydrothermal synthesis of zeolite is performed, a treatment for adjusting pH may be performed. The treatment for adjusting pH is performed, for example, before heating a slurry containing zeolite powder prepared for hydrothermal synthesis, during heating of the slurry, or after heating of the slurry. The pH is adjusted, for example, by adding an acid to the slurry. The acid contains at least one component selected from the group consisting of inorganic acids such as hydrochloric acid, sulfuric acid, and nitric acid, and organic acids such as formic acid, acetic acid, and oxalic acid.

[0167] The average particle size of the moisture absorbent (C) is preferably 10 nm or more and 200 nm or less. If the average particle size is 200 nm or less, the cured product can have particularly high transparency. If the average particle size is 10 nm or more, the moisture absorbent (C) can maintain good moisture absorption. Note that this average particle size is the median diameter calculated from the measurement results by dynamic light scattering method, that is, the cumulative 50% diameter (D50). Note that the Nanotrac Wave series from Microtrack Bell Co., Ltd. can be used as a measuring device.

[0168] The average particle size of the moisture absorbent (C) is preferably 150 nm or less, more preferably 100 nm or less, and particularly preferably 70 nm or less. The average particle size of the moisture absorbent (C) is preferably 20 nm or more, and more preferably 50 nm or more. In this case, the cured product can have particularly good transparency and moisture absorption.

[0169] It is also preferable that the cumulative 90% diameter (D90) of the moisture absorbent (C) is 100 nm or less. In this case, the cured product can have particularly high transparency.

[0170] The proportion of the moisture absorbent (C) relative to the total amount of the composition (X) is preferably 1% by mass or more and 20% by mass or less. If the proportion of the moisture absorbent (C) is 1% by mass or more, the cured product can have particularly high moisture absorption. If the proportion of the moisture absorbent (C) is 20% by mass or less, the viscosity of the composition (X) can be particularly reduced, and the composition (X) can have a sufficiently low viscosity to be ejected by an inkjet method. The proportion of the moisture absorbent (C) is more preferably 3% by mass or more, and particularly preferably 5% by mass or more. The proportion of the moisture absorbent (C) is more preferably 15% by mass or less, and particularly preferably 13% by mass or less.

[0171] The composition (X) may further contain an inorganic filler other than the moisture absorbent (C). In particular, the composition (X) preferably contains nano-sized high refractive index particles. Examples of high refractive index particles include zirconia particles. When the composition (X) contains high refractive index particles, the refractive index of the cured product can be increased while maintaining good transparency of the cured product. Therefore, when the cured product is applied to an optical component such as the sealing material 5 in the light emitting device 1, the extraction efficiency of the light that passes through the optical component and is emitted to the outside can be improved. The average particle size of the high refractive index particles is preferably within a range of 5 to 30 nm, and more preferably within a range of 10 to 20 nm.

[0172] The proportion of high refractive index particles in the composition (X) is appropriately designed so that the cured product has a desired refractive index. In particular, the high refractive index particles are preferably contained in the composition (X) so that the refractive index of the cured product is in the range of 1.45 or more and less than 1.55. In this case, the light extraction efficiency of the light emitting device 1 is particularly improved.

[0173] When the composition (X) contains the moisture absorbent (C), the composition (X) may further contain a dispersant (D). The dispersant (D) is a surfactant that can be adsorbed to the moisture absorbent (C). The dispersant (D) has, for example, an adsorption group (also called an anchor) that can be adsorbed to particles of the moisture absorbent (C), and a tail that is a chain-like or comb-like molecular skeleton that adheres to the particles of the moisture absorbent (C) by adsorbing the adsorption group to the particles. The dispersant (D) contains at least one component selected from the group consisting of an acrylic dispersant whose tail is an acrylic molecular chain, a urethane dispersant whose tail is a urethane molecular chain, and a polyester dispersant whose tail is a polyester molecular chain.

[0174] When the composition (X) contains a dispersant (D), the moisture absorbent (C) can be well dispersed in the composition (X) and the cured product. Therefore, even though the cured product and the optical component contain the moisture absorbent (C), the transparency of the cured product and the optical component is not easily reduced by the moisture absorbent (C). In addition, the dispersant (D) can effectively suppress the aggregation of the moisture absorbent (C) during storage of the composition (X). Therefore, the storage stability of the composition (X) is not easily reduced by the moisture absorbent (C).

[0175] Furthermore, the adhesion between the cured product and silicon nitride and silicon oxide is not easily reduced by the dispersant (D). This is believed to be because the dispersant (D) is easily adsorbed to the moisture absorbent (C) as described above, and therefore the dispersant (D) is less likely to affect the interface between the cured product and silicon nitride and silicon oxide. Therefore, the optical component can have high adhesion to the glass substrate. Furthermore, silicon nitride and silicon oxide are sometimes used as materials for the passivation layer 6 in the light-emitting device 1. Therefore, when the passivation layer 6 is made of silicon nitride or silicon oxide, the optical component can have high adhesion to the passivation layer 6.

[0176] The boiling point of the dispersant (D) is preferably not less than 200° C. In this case, the dispersant (D) is less likely to volatilize from the composition (X), and therefore the storage stability of the composition (X) is further improved.

[0177] The dispersant (D) preferably has either or both of a basic polar functional group and an acidic polar functional group as an adsorption group. In this case, the moisture absorbent (C) can be particularly well dispersed in the composition (X) and in the cured product. This is thought to be because the dispersant (D) has either or both of a basic polar functional group and an acidic polar functional group, so that it is easy to adsorb to the moisture absorbent (C), and therefore the effect of dispersing the moisture absorbent (C) is significantly expressed.

[0178] The dispersant (D) may contain a polymer. The weight average molecular weight of the polymer is, for example, 1000 or more. The polymer contains, for example, at least one component selected from the group consisting of hydroxyl group-containing carboxylic acid ester, salt of long-chain polyaminoamide and high molecular weight acid ester, salt of high molecular weight polycarboxylic acid, salt of long-chain polyaminoamide and polar acid ester, high molecular weight unsaturated acid ester, modified polyurethane, modified polyacrylate, polyether ester type anionic surfactant, salt of naphthalene sulfonic acid formalin condensate, polyoxyethylene alkyl phosphate ester, polyoxyethylene nonylphenyl ether, polyester polyamine, and stearylamine acetate. When the dispersant (D) contains a polymer, the steric hindrance effect generated when the polymer is adsorbed to the particles of the moisture absorbent (C) is improved, and the dispersibility of the moisture absorbent (C) can be improved.

[0179] The dispersant (D) can contain, for example, either or both of a dispersant (F1) having a basic polar functional group and a dispersant (F2) having an acidic polar functional group.

[0180] The basic polar functional group in the dispersant (F1) having a basic polar functional group includes at least one group selected from the group consisting of, for example, an amino group, an imino group, an amide group, an imide group, and a nitrogen-containing heterocyclic group. When the dispersant (F1) has a basic polar functional group, the dispersant (F1) is easily adsorbed to the moisture absorbent (C), so that the dispersibility of the moisture absorbent (C) can be improved. The basic polar functional group preferably includes an amino group, because it can particularly increase the adsorption ability of the dispersant (F1) to the moisture absorbent (C), can particularly improve the dispersibility of the moisture absorbent (C), and can particularly reduce the viscosity of the composition (X).

[0181] Examples of the dispersant (F1) having a basic polar functional group include Solsperse series manufactured by Nippon Louvre Resol Co., Ltd., such as Solsperse 24000 (amine value: 41.6 mg KOH / g), Solsperse 32000 (amine value: 31.2 mg KOH / g), Solsperse 39000 (amine value: 25.7 mg KOH / g), Solsperse J100, and Solsperse J200; H / g), DISPERBYK series manufactured by BYK Japan Co., Ltd., such as DISPERBYK-2050 (amine value: 30.7 mg KOH / g), DISPERBYK-2150 (amine value: 56.7 mg KOH / g); BYKJET series manufactured by BYK Japan Co., Ltd., such as BYKJET-9151 (amine value: 17.2 mg KOH / g), BYKJET-9152 (amine value: 27.3 mg KOH / g); and AJISPER series manufactured by Ajinomoto Fine-Techno Co., Ltd., such as AJISPER PB821 (amine value: 11.2 mg KOH / g), AJISPER PB822 (amine value: 18.2 mg KOH / g), AJISPER PB881 (amine value: 17.4 mg KOH / g).

[0182] The amine value of the dispersant (F1) is preferably 10 mgKOH / g or more, more preferably 10 mgKOH / g or more and 30 mgKOH / g or less, and even more preferably 15 mgKOH / g or more and 30 mgKOH / g or less. In addition, the dispersant (F1) preferably does not have a phosphate group. When the dispersant (F1) has a phosphate group, the acid value derived from the phosphate group is preferably equal to or less than the amine value. In this case, the dispersant (F1) can disperse the moisture absorbent (C) particularly well, can particularly increase the storage stability of the composition (X), can particularly increase the transparency of the cured product, and can further particularly increase the adhesion between the cured product and silicon nitride and silicon oxide. Among the components that can be contained in the dispersant (F1), an example of a dispersant having an amino group but not a phosphate group includes DISPERBYK-108 manufactured by BYK-Chemie. Examples of dispersants having an amino group and a phosphate group and an acid value derived from the phosphate group that is equal to or less than the amine value include DISPERBYK-2013 manufactured by BYK-Chemie and DISPERBYK-180 manufactured by BYK-Chemie.

[0183] The acidic polar functional group in the dispersant (F2) having an acidic polar functional group is, for example, a carboxyl group. The dispersant (F2) contains, for example, DISPERBYK-P105 manufactured by BYK-Chemie.

[0184] The amount of dispersant (D) per 100 parts by mass of moisture absorbent (C) is preferably 5 parts by mass or more and 60 parts by mass or less. When the amount of dispersant (D) is 5 parts by mass or more, the advantages of dispersant (D) can be particularly exhibited. When the amount of dispersant (D) is 60 parts by mass or less, the adhesion between the cured product and silicon nitride and silicon oxide can be further improved. The amount of dispersant (D) is more preferably 15 parts by mass or more. The amount of dispersant (D) is more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less, and particularly preferably 30 parts by mass or less.

[0185] It is preferable that the composition (X) does not contain a solvent or contains 1% by mass or less of the solvent. In this case, when preparing a cured product from the composition (X), it is not necessary to dry the composition (X) to volatilize the solvent. In addition, the storage stability of the composition (X) is further improved. The content of the solvent is more preferably 0.5% by mass or less, even more preferably 0.3% by mass or less, and particularly preferably 0.1% by mass or less. It is particularly preferable that the composition (X) does not contain a solvent or contains only a solvent that is inevitably mixed in.

[0186] Composition (X) can be prepared by mixing the above-mentioned components. Composition (X) is preferably liquid at 25°C.

[0187] 3. Method for producing sealing material and method for producing light-emitting device A method for producing the encapsulant 5 using the composition (X) and a method for producing the light emitting device 1 will be described.

[0188] In this embodiment, it is preferable to form a coating film on an object by discharging the composition (X) by an inkjet method, irradiate the composition (X) on the coating film, and then heat the composition (X) to produce the encapsulant 5. In this embodiment, it is possible to form a coating film by discharging the composition (X) from an inkjet head and applying it onto an object. More specifically, the composition (X) can be discharged by an inkjet method at a position through which light emitted by an organic EL element or the like, which is the light-emitting element 4, passes, to form a coating film.

[0189] When composition (X) is discharged by an inkjet method and applied onto an object, if composition (X) has a sufficiently low viscosity at room temperature, for example, a viscosity at 25°C of 30 mPa s or less, particularly 15 mPa s or less, composition (X) can be discharged by an inkjet method and applied onto an object without heating.

[0190] When composition (X) has the property of being reduced in viscosity by heating, composition (X) may be heated and then discharged by an inkjet method to apply onto an object. When composition (X) has a viscosity of 30 mPa·s or less, particularly 15 mPa·s or less at 40°C, composition (X) can be reduced in viscosity by simply heating it slightly, and this reduced-viscosity composition (X) can be discharged by an inkjet method. The heating temperature for composition (X) is, for example, 20°C or higher and 50°C or lower.

[0191] When the coating film obtained by molding the composition (X) is irradiated with light to cure, the light irradiated to the coating film is, for example, ultraviolet light. The ultraviolet light means light having a wavelength in the range of 200 nm to 410 nm. The wavelength of the light irradiated to the coating film is preferably in the range of 350 nm to 410 nm, more preferably 385 nm to 405 nm. A representative example of the light irradiated to the coating film is light having a wavelength of 395 nm. The wavelength of the light irradiated to the coating film is not limited to the above description, as long as it can cure the coating film.

[0192] The irradiation intensity of the light irradiated on the coating is 20mW / m 2 More than 20W / cm 2 It is preferable that the irradiation intensity of the light is not limited to the above description, so long as the coating film can be cured.

[0193] When the coating film is irradiated with light, the shape of the portion to which the light is irradiated may be an area type having a certain area, or a line type. In the case of a line type, the entire coating film can be irradiated with light by moving the coating film relative to the light source, or by moving the light source relative to the coating film. In this case, it is easy to adjust the time during which the coating film is irradiated with light, and by adjusting this time, it is easy to adjust the integrated light amount.

[0194] When the cured coating film is further heated, the heating temperature is preferably 90° C. or higher. In this case, the curing of the coating film is further advanced, and the linear expansion coefficient of the encapsulant 5 is easily reduced, and thus the linear expansion coefficient of the encapsulant 5 is easily achieved to be 100 ppm / ° C. or higher and 130 ppm / ° C. or lower. The heating temperature is preferably 150° C. or lower. In this case, the organic EL element or the like serving as the light-emitting element 4 can be made less susceptible to deterioration due to heat.

[0195] More specifically, for example, first, a support substrate 2 is prepared. A partition wall is formed on one surface of the support substrate 2 by, for example, photolithography using a photosensitive resin material. Then, a plurality of light-emitting elements 4, such as organic EL elements, are provided on one surface of the support substrate 2. The light-emitting elements 4, such as organic EL elements, can be produced by an appropriate method such as a vapor deposition method or a coating method. In particular, the light-emitting elements 4, such as organic EL elements, are preferably produced by a coating method such as an inkjet method, similar to the composition (X). In this way, an element array 9 is produced on the support substrate 2.

[0196] Next, a first passivation layer 61 is provided on the element array 9. The first passivation layer 61 can be formed by a deposition method such as a plasma CVD method.

[0197] Next, the composition (X) is discharged onto the first passivation layer 61 by, for example, an inkjet method to prepare a coating film. By applying the inkjet method to both the formation of the organic EL elements or the like that are the light-emitting elements 4 and the application of the composition (X), the manufacturing efficiency of the light-emitting device 1 can be particularly improved. Next, the coating film is cured by irradiating it with ultraviolet light to prepare the sealing material 5. The thickness of the sealing material 5 is, for example, 2 μm or more and 50 μm or less.

[0198] The thickness of the encapsulant 5 is preferably 2 μm or more and 30 μm or less, and more preferably 2 μm or more and 15 μm or less. As described above, in this embodiment, since small droplets of the composition (X) can be easily formed at high density by the inkjet method, it is easy to realize a thin encapsulant 5 having a thickness of 2 μm or more and 15 μm or less. By thinning the encapsulant 5 in this way, tensile stress and compressive stress are less likely to occur in the encapsulant 5 within the light emitting device 1. Therefore, it is easy to realize a flexible light emitting device 1.

[0199] Next, a second passivation layer 62 is provided on the sealing material 5. The second passivation layer 62 can be formed by a deposition method such as a plasma CVD method.

[0200] Next, an ultraviolet-curable resin material is provided on one surface of the support substrate 2 so as to cover the second passivation layer 62, and then the transparent substrate 3 is placed on the resin material. The transparent substrate 3 is, for example, a glass substrate or a transparent resin substrate.

[0201] Next, ultraviolet light is irradiated from the outside toward the transparent substrate 3. The ultraviolet light passes through the transparent substrate 3 and reaches the ultraviolet-curable resin material. As a result, the ultraviolet-curable resin material is cured, and the second sealing material 52 is produced.

[0202] As described above, the encapsulant 5 made of the cured product of the composition (X) can have good heat resistance. Therefore, when the passivation layer 6 (second passivation layer 62) is formed on the encapsulant 5 by a deposition method such as a plasma CVD method, the encapsulant 5 is unlikely to deteriorate even if the temperature of the encapsulant 5 rises. Furthermore, even if the temperature of the light emitting device 1 rises during use of the light emitting device 1, the encapsulant 5 is unlikely to deteriorate. Note that the light emitting element 4 is, for example, an organic EL element as described above, but the light emitting element 4 may be a micro light emitting diode or the like.

[0203] The optical component is not limited to the sealing material 5 for the light-emitting element 4. The composition (X) can be used to manufacture various optical components. For example, the optical component may be a color resist. In this case, for example, a phosphor is contained in the composition (X), and a color resist in a color filter is manufactured from this composition (X). In this case, it is easy to manufacture the color resist in the color filter with high density and high accuracy. This color filter can be provided in a display device such as an organic EL display or a micro LED display. EXAMPLES

[0204] Specific examples of the present invention are presented below, but the present invention is not limited to the following examples.

[0205] 1. Preparation of the Composition The compositions of the examples and comparative examples were prepared by mixing the components shown in the table below. did.

[0206] The details of the components shown in the table are as follows. The viscosity of the following components was measured using a rheometer (Anton Paar Japan, model number DHR-2) at a temperature of 25°C and a shear rate of 1000 s -1 The values ​​were measured under the following conditions.

[0207] (1) Cationic polymerizable compound Phenylmethyloxirane: boiling point 235°C, viscosity at 25°C 6mPs·s. ·4-Fluorophenyloxirane: Boiling point 220°C, viscosity at 25°C 8 mPs·s. Styrene oxide: boiling point 200°C, viscosity at 25°C 4 mPa·s. ·BATG: Showa Denko, polyfunctional aromatic epoxy compound, product number BATG, boiling point over 300°C, viscosity at 25°C 10,000 mPa·s. · 2-Glycidyl-phenyloxirane: Boiling point above 300°C, viscosity at 25°C 17 mPa·s. ·OXT-221: Manufactured by Toagosei, product number OXT-221, compound shown by formula (3), boiling point 275℃, viscosity 11mPa·s. ·OXT-212: Manufactured by Toagosei, product number OXT-212, compound shown by formula (12), boiling point 277℃, surface tension 35mN / cm, viscosity 4mPa·s. AL-EOX: Yokkaichi Chemical Co., Ltd., product number AL-EOX, compound shown in formula (16), boiling point 200°C, surface tension 27 mN / cm, viscosity 2 mPa s. OXT-101: Manufactured by Toa Gosei, product number OXT-101, compound shown in the formula below, boiling point 247°C, surface tension 36mN / cm, viscosity 18mPa s.

[0208] [ka] Celloxide 8010: Manufactured by Daicel, product name Celloxide 8010, compound shown in formula (1a), boiling point 265°C, viscosity at 25°C 60 mPa s. Celloxide 8010 (heat-treated): The above Celloxide 8010 is heat-treated at 100°C for 30 minutes in an air atmosphere, with a boiling point of 265°C and a viscosity of 60 mPa s at 25°C. 1,2,7,8-Octane diepoxide: boiling point 230°C, viscosity at 25°C 3 mPa·s.

[0209] (2) Cationic curing catalyst CPI-310B: San-Apro Co., Ltd., triarylsulfonium salt type photoacid generator, anion species B(C6F5)4 - , part number CPI-310B. CPI-210S: San-Apro triarylsulfonium salt type photoacid generator, anion species (Rf) n PF 6-n - , part number CPI-310B. IK-1: San-Apro Co., Ltd., diaryliodonium salt type photoacid generator, anion species (Rf) n PF 6-n , product number IK-1. CPI-110P: San-Apro Co., Ltd., triarylsulfonium salt type photoacid generator, anion species PF6 - , part number CPI-110P. IRGACURE250: BASF, diaryliodonium salt type photoacid generator, anion species PF6 - , part number IRGACURE250.

[0210] (3) Sensitizer UVS1331: 9,10-Dibutoxyanthracene, manufactured by Kawasaki Kasei Co., Ltd., product number UVS1331. DETX-s: 2,4-diethylthioxanthen-9-one, manufactured by Nippon Kayaku Co., Ltd., product number DETX-s.

[0211] (4) Additives · BYK333: Leveling agent, manufactured by BYK Chemical, active ingredient is polyether modified polydimethylsiloxane.

[0212] 2.Evaluation Test The following evaluation tests were carried out on the examples and comparative examples, and the results are shown in the table below.

[0213] 2.1. Curability The composition was applied to a slide glass and then irradiated with an LED-UV irradiator manufactured by CCS Inc. at a peak wavelength of 395 nm and an output of 1 W / cm. 2 Under the condition of 1.5 J / cm 2 The film was photocured by irradiating it with a light intensity of 1000 nm. The atmosphere was dry air containing oxygen. This produced a film with a thickness of 10 μm. A tester touched the surface of this film with their finger to judge whether it had tack or not. The results were rated as "A" when the tester did not feel any tack, "B" when they felt tack but no adhesion to the finger, and "C" when they felt tack and part of the film adhered to the finger.

[0214] 2.2.Transmittance The composition was applied onto a flat and smooth surface, and then irradiated in dry air with an LED-UV irradiator manufactured by CCS Inc. at a peak wavelength of 395 nm and an output of 1 W / cm. 2 , Accumulated light intensity 1.5J / cm 2 The film was photocured by irradiating it with light under the above conditions. As a result, a film having a thickness of 15 μm was produced. The transmittance of this film at a wavelength of 430 nm was measured. For the measurement, a spectrophotometer (U-4100 manufactured by Hitachi, Ltd.) was used.

[0215] 2.3.Viscosity The viscosity of the composition was measured using a rheometer (Anton Paar Japan, model number DHR-2) at a temperature of 25°C and a shear rate of 1000 s -1 The measurements were performed under the following conditions.

[0216] 2.4.Surface tension The surface tension of the composition was measured by the Wilhelmy method using a surface tensiometer (manufactured by Kyowa Interface Science, model: CBVP-Z) with a platinum plate at a measurement temperature of 25°C.

[0217] 2.5.Storage stability The composition was left to stand for 2 weeks at a temperature of 60° C. The viscosity of the composition before and after this test was measured with a rheometer, and a rating of "A" was given if the viscosity change rate was less than 10%, a rating of "B" was given if the viscosity change rate was 10% or more and no gelation of the composition was observed after the test, and a rating of "C" was given if gelation of the composition was observed after the test.

[0218] 2.6. Inkjet properties 2.6.1. Presence or absence of satellites The resin composition was placed in the cartridge of an inkjet printer (manufactured by Ricoh Co., Ltd., "MH2420"), and after confirming that the resin composition in the cartridge could be discharged from the nozzle of the inkjet printer, the resin composition was discharged from the nozzle to continuously print a test pattern. The appearance of the droplets being discharged from the nozzle was photographed with a high-speed camera, and it was confirmed whether the droplets separated and satellites were generated. As a result, the case where the droplets did not separate was evaluated as "A", the case where the satellites separated from the original droplets and then merged with the original droplets to become one droplet again was evaluated as "B", and the case where the satellites separated from the original droplets and did not merge with each other was evaluated as "C".

[0219] 2.6.2.Inkjet speed (initial) In the above test of "2.4. Inkjet properties," the droplet ejection speed was changed to confirm the maximum ejection speed in the case where the droplets did not separate, or where the satellite separated from the original droplet and then merged with the original droplet to form a single droplet again.

[0220] 2.6.3. Inkjet speed (after storage) The composition was stored for 2 weeks at a temperature of 60° C. Then, the same test as in “2.4.2. Inkjet speed (initial)” above was carried out.

[0221] 2.6.4. Retention rate The percentage of the result of "2.6.3. Inkjet speed (after storage)" above to the result of "2.6.2. Inkjet speed (initial)" was calculated as the maintenance rate.

[0222] 2.7. Barrier Membrane Compatibility A 500 nm thick SiN film was prepared on a glass slide, and a 10 μm thick film was prepared on this SiN film under the same conditions as in "2.1. Curability". The film was stored in a thermo-hygrostat at 85°C and 85% RH for 168 hours, and then the surface of the film was observed with an SEM. As a result, the film was rated as "A" if no change was observed, "B" if the film had blisters or surface roughness but no cracks, and "C" if the film had cracks.

[0223] 2.8.Glass transition temperature The composition was applied to prepare a coating film, which was then irradiated with an LED-UV irradiator manufactured by CCS Inc. at a peak wavelength of 395 nm and an output of 1 W / cm. 2 Under the conditions of 5 J on each side for a total of 10 J / cm 2 A film having a thickness of 200 μm was produced by photocuring with an amount of light of 1000 μm. The glass transition temperature of a sample cut out from this film was measured using a viscoelasticity measuring device (manufactured by Hitachi High-Tech Science Corporation, model number DMA7100).

[0224] 2.9.Outgassing evaluation The amount of outgassing when the cured product of the composition was heated was measured by the following method: 100 mg of the composition was placed in a headspace vial, and the composition was irradiated with an LED-UV irradiator manufactured by CCS Inc. at a peak wavelength of 395 nm and approximately 100 mW / cm. 2 After the composition was cured by irradiating light under the conditions, the vial was sealed and heated at 100°C for 30 minutes, and then the gas phase in the vial was introduced into a gas chromatograph for analysis. From the results, the mass ratio of the generated gas to the composition was determined. In order to say that outgassing is unlikely to occur, this result is preferably 200 ppm or less, more preferably 100 ppm or less, even more preferably 50 ppm or less, and particularly preferably 25 ppm or less.

[0225] [Table 1]

[0226]

Table 2

[0227]

Table 3

Claims

1. A cationically polymerizable compound (F), A cationic curing catalyst (G), The cationic polymerizable compound (F) contains an aromatic epoxy compound (f1) represented by the following formula (30) and a compound (f3) having an oxetane group: [Formula 1] In formula (30), X is at least one selected from the group consisting of halogen, H, a hydrocarbon group, and an alkylene glycol group, and when there are multiple X in one molecule, they may be the same or different from each other, R is a single bond, -CH 2 --, --O-CH 2 -or-CO-O-CH 2 - and Y is H or a monovalent organic group; n is any number from 1 to 3 (excluding the cases where the aromatic epoxy compound (f1) is a polyphenyl compound or a condensed polycyclic aromatic compound), the proportion of the aromatic epoxy compound (f1) relative to the total amount of the cationic polymerizable compound (F) is 30 mass% or more; the ratio of the compound (f3) having an oxetane group to the cationic polymerizable compound (F) is 20% by mass or more and 90% by mass or less; The total light transmittance of the cured product when the thickness dimension is 10 μm is 90% or more. To produce an optical component that transmits light emitted by a light source, UV curable resin composition.

2. The composition does not contain a solvent or the solvent content is 1% by mass or less. The ultraviolet-curable resin composition according to claim 1 .

3. The viscosity at 25°C is 8 mPa·s or more and 40 mPa·s or less. The ultraviolet-curable resin composition according to claim 1 or 2.

4. The viscosity at 40°C is 8 mPa·s or more and 40 mPa·s or less. The ultraviolet-curable resin composition according to claim 1 .

5. A liquid that can be ejected by an inkjet method. The ultraviolet-curable resin composition according to claim 1 .

6. A method for manufacturing a light emitting device comprising a light source and an optical component that transmits light emitted by the light source, comprising the steps of: The ultraviolet-curable resin composition according to any one of claims 1 to 5 is ejected by an inkjet method at a position through which light emitted by the light source passes to prepare a coating film; and producing the optical component by irradiating the coating with ultraviolet light. A method for manufacturing a light emitting device.

7. A light source and an optical component that transmits light emitted by the light source, the optical component being made of a cured product of the ultraviolet-curable resin composition according to any one of claims 1 to 5. Light emitting device.

Citation Information

Patent Citations

  • Semiconductor circuit

    JP1982003429A

  • Epoxy resin composition

    JP2010163566A

  • Sealing agent for optical device

    JP2012017368A

  • Ultraviolet-curing composition

    WO2005085317A1

  • Ultraviolet-curable resin composition and laminated body

    WO2018051868A1