Ultraviolet-curable resin composition, optical component, method for manufacturing optical component, light-emitting device, and method for manufacturing light-emitting device

A polyfunctional acrylic compound with a nitrogen atom and a photopolymerization initiator in the ultraviolet curable resin composition addresses the issues of adhesion and curability, ensuring effective curing and reduced outgassing for optical components and light emitting devices.

JP7555047B2Active Publication Date: 2024-09-24PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020020121
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-07
Publication Date
2024-09-24
Estimated Expiration
2040-02-07

AI Technical Summary

Technical Problem

Existing ultraviolet curable resin compositions containing cyclic amide monomers like acryloylmorpholine face challenges in increasing ultraviolet curability and adhesion to inorganic materials, leading to outgassing and insufficient curing, especially under atmospheric conditions.

Method used

The composition incorporates a polyfunctional acrylic compound with a nitrogen atom and a photopolymerization initiator, optimized for low dissolved oxygen content and low viscosity, allowing for improved adhesion and curability under atmospheric conditions using an inkjet method.

Benefits of technology

The solution enhances adhesion to inorganic materials, reduces outgassing, and ensures effective curing even in the presence of oxygen, maintaining high reactivity and stability, suitable for producing optical components and light emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555047000016
    Figure 0007555047000016
  • Figure 0007555047000005
    Figure 0007555047000005
  • Figure 0007555047000011
    Figure 0007555047000011
Patent Text Reader

Abstract

To provide a UV-curable resin composition that readily improves adhesion between a cured product and inorganic material, and readily possesses excellent ultraviolet curability.SOLUTION: A UV-curable resin composition has a polyfunctional acryl compound having a nitrogen atom (Y) and a photopolymerization initiator (B).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ultraviolet-curable resin composition, an optical component, a method for manufacturing an optical component, a light-emitting device, and a method for manufacturing a light-emitting device, and more particularly to an ultraviolet-curable resin composition that can be molded by an inkjet method, an optical component made from the ultraviolet-curable resin composition, a method for manufacturing an optical component using the ultraviolet-curable resin composition, a light-emitting device including the optical component, and a method for manufacturing a light-emitting device using the ultraviolet-curable resin composition. [Background technology]

[0002] Patent Document 1 discloses that when a barrier layer (functional layer) of an inorganic compound is deposited on a substrate to protect the light-emitting element from water vapor and an organic layer is provided to protect the barrier layer, the organic layer is made from a photocurable composition containing a cyclic amide monomer such as acryloylmorpholine, a polyfunctional (meth)acrylate compound, and a photopolymerization initiator, thereby improving the adhesion between the functional layer and the organic layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-127597 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the inventor's research, it is difficult to improve the UV curability of a composition containing a cyclic amide monomer such as acryloylmorpholine, and therefore outgassing is likely to occur from the cured product of the composition. In particular, it is very difficult to sufficiently cure the composition in an air atmosphere.

[0005] An object of the present invention is to provide an ultraviolet-curable resin composition that is likely to improve adhesion between the cured product and an inorganic material and that is likely to have good ultraviolet curability, an optical component made from the ultraviolet-curable resin composition, a method for manufacturing an optical component using the ultraviolet-curable resin composition, a light-emitting device including the optical component, and a method for manufacturing a light-emitting device using the ultraviolet-curable resin composition. [Means for solving the problem]

[0006] An ultraviolet-curable resin composition according to one embodiment of the present invention contains a polyfunctional acrylic compound (Y1) having a nitrogen atom and a photopolymerization initiator (B).

[0007] An optical component according to one aspect of the present invention includes a cured product of the ultraviolet-curable resin composition.

[0008] A method for producing an optical component according to one aspect of the present invention includes molding the ultraviolet-curable resin composition by an inkjet method, and then irradiating the ultraviolet-curable resin composition with ultraviolet light to cure it.

[0009] A light emitting device according to one aspect of the present invention includes a light source and an optical component that transmits light emitted from the light source. The optical component includes a cured product of the ultraviolet curable resin composition.

[0010] A method for manufacturing a light emitting device according to one aspect of the present invention is a method for manufacturing a light emitting device including a light source and an optical component that transmits light emitted by the light source, the method including manufacturing the optical component by the method for manufacturing the optical component. Effect of the Invention

[0011] According to one aspect of the present invention, there are provided an ultraviolet-curable resin composition that is likely to improve adhesion between the cured product and an inorganic material and that is likely to have good ultraviolet curability, a method for producing the ultraviolet-curable resin composition, an optical component made from the ultraviolet-curable resin composition, a method for producing an optical component using the ultraviolet-curable resin composition, a light-emitting device including the optical component, and a method for producing a light-emitting device using the ultraviolet-curable resin composition. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic cross-sectional view showing a first example of a light emitting device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, one embodiment of the present invention will be described.

[0014] The ultraviolet-curable resin composition according to this embodiment (hereinafter also referred to as composition (X)) contains a nitrogen-atom-containing polyfunctional acrylic compound (Y1) and a photopolymerization initiator (B).

[0015] According to this embodiment, the nitrogen atom-containing polyfunctional acrylic compound (Y1) easily improves the adhesion between the cured product of the composition (X) and inorganic materials. In addition, the nitrogen atom-containing polyfunctional acrylic compound (Y1) is polyfunctional, so it easily increases the reactivity of the composition (X), and therefore the composition (X) is likely to have good ultraviolet curability.

[0016] The composition (X) preferably has ultraviolet curability in the air. The ultraviolet curability in the air can be achieved by increasing the reactivity of the composition (X). The ultraviolet curability in the air means that the pencil hardness of the cured product obtained by curing the composition (X) in the air is 4B or more, preferably 2B or more. The test conditions for confirming the ultraviolet curability in the air will be described in detail in the Examples section below.

[0017] In this embodiment, the proportion of dissolved oxygen in the composition (X) is preferably 50 mg / L or less relative to the composition (X). In this case, when an optical component is produced from the composition (X), oxygen derived from the optical component is unlikely to reach the light source in a light-emitting device equipped with the optical component. Therefore, even if the composition (X) is applied to produce an optical component in a light-emitting device, deterioration of the light source due to oxygen is unlikely to occur. In addition, since the proportion of dissolved oxygen is 50 mg / L or less, oxygen inhibition is unlikely to occur when the composition (X) is photocured. Therefore, the ultraviolet curability of the composition (X) in the air atmosphere is more easily realized.

[0018] It is preferable that the dissolved oxygen content is 70 mg / L or less, and more preferable that the dissolved oxygen content is 50 mg / L. The lower the dissolved oxygen content, the more preferable, and ideally 0 mg / L. The dissolved oxygen content is substantially 5 mg / L or more, and it is very difficult to reduce the dissolved oxygen content below this level. The method for measuring the dissolved oxygen content will be described in detail in the Examples section below.

[0019] As described above, the composition (X) can be used to manufacture optical components, and a light-emitting device equipped with the optical components can also be manufactured. The use of the composition (X) is not limited to the manufacture of optical components, and the composition (X) can be used in various applications that utilize the properties of the composition (X).

[0020] The composition (X) is preferably molded by an inkjet method. In this case, it is easy to prepare a cured product of the composition (X) with good positional accuracy. In addition, when the composition (X) is molded by an inkjet method, foreign matter is less likely to be mixed into the composition (X) and its cured product, compared with the case where the composition (X) is molded by a printing method involving contact such as a screen printing method, and therefore the yield in manufacturing optical parts is less likely to deteriorate.

[0021] The viscosity of composition (X) at 25°C is preferably 30 mPa·s or less. In this case, composition (X) can be easily molded at room temperature, particularly by the inkjet method. It is more preferable that this viscosity is 25 mPa·s or less, even more preferable that it is 20 mPa·s or less, and particularly preferable that it is 15 mPa·s or less. It is also preferable that this viscosity is 1 mPa·s or more, and it is also preferable that it is 5 mPa·s or more.

[0022] It is also preferable that the viscosity of the composition (X) at 40°C is 30 mPa·s or less. In this case, no matter what the viscosity of the composition (X) is at room temperature, it is possible to lower the viscosity by slightly heating the composition (X). Therefore, the composition (X) can be easily molded by heating, particularly by the inkjet method. In addition, since the viscosity of the composition (X) can be lowered without significantly heating it, it is possible to prevent the composition of the composition (X) from changing due to the volatilization of the components in the composition (X). It is more preferable that the viscosity is 25 mPa·s or less, even more preferable that the viscosity is 20 mPa·s or less, and particularly preferable that the viscosity is 15 mPa·s or less. It is also preferable that the viscosity is 1 mPa·s or more, and it is also preferable that the viscosity is 5 mPa·s or more.

[0023] Such a low viscosity of composition (X) at 25° C. or 40° C. can be achieved by the composition of composition (X) described in detail below. The method and conditions for measuring the viscosity of composition (X) at 25° C. and 40° C. will be described in detail in the Examples section below.

[0024] When the proportion of dissolved oxygen is 50 mg / L or less, molding defects are unlikely to occur when the composition (X) is produced by the inkjet method. This is presumably because, when the proportion of dissolved oxygen in the composition (X) is 50 mg / L or less, bubbles are unlikely to occur in the droplets of the composition (X) discharged by the inkjet method, and therefore defective droplets such as satellites and mist are unlikely to occur. Note that satellites are droplets that separate from the original droplets when droplets are discharged by the inkjet method. Mists are multiple small droplets that separate from the original droplets. Satellites and mist tend to adhere to positions on the coating target that are different from the positions where the original droplets were attached, and therefore the dimensional accuracy of the cured product produced from the composition (X) tends to deteriorate.

[0025] It is preferable that the rate of outgassing generated when the cured product of the composition (X) is heated at 80°C for 30 minutes is 60 ppm or less. In this case, outgassing is unlikely to occur from the cured product. Therefore, for example, it is possible to make it difficult for voids due to outgassing to occur in a light-emitting device equipped with an optical component made of the cured product. Therefore, it is difficult for water and oxygen to reach the light-emitting element through the voids, and the light-emitting element is unlikely to deteriorate due to water and oxygen. The method and conditions for measuring the rate of outgassing will be explained in detail in the Examples section below.

[0026] In addition, when a test is conducted in which composition (X) is left to stand for two months at a temperature of 60°C under a nitrogen atmosphere, it is preferable that the viscosity change rate Rμ calculated from the viscosity μ0 of composition (X) before the test and the viscosity μ1 of composition (X) after the test by the following formula (M1) is less than 20%. Rμ={(μ1-μ0) / μ0}×100(%) …(M1) In this case, the composition (X) can have particularly good storage stability. It is more preferable that the viscosity change rate Rμ is 10% or less. The lower the viscosity change rate Rμ, the more preferable, and ideally it is 0%.

[0027] It is preferable that the composition (X) does not contain a solvent or the content of the solvent is 1% by mass or less. In this case, outgassing derived from the solvent is unlikely to occur from the composition (X) and the cured product of the composition (X). In addition, a drying step for removing the solvent from the composition (X) and the cured product during the production of the optical component and the light emitting device can be eliminated. A drying step for removing the solvent from at least one of the composition (X) and the cured product may be performed. In this case, at least one of the heating temperature and the heating time in the drying step can be reduced. Therefore, outgassing can be unlikely to occur from the optical component without reducing the production efficiency of the optical component and the light emitting device. Furthermore, when the composition (X) is molded, in particular by the inkjet method, the thickness is unlikely to decrease due to the evaporation of the solvent from the composition (X) after molding, and therefore the thickness of the optical component is unlikely to decrease. Therefore, the thickness of the optical component can be secured as large as possible while molding by the inkjet method. The content of the solvent is more preferably 0.5% by mass or less, even more preferably 0.3% by mass or less, and particularly preferably 0.1% by mass or less. It is particularly preferred that the composition (X) does not contain a solvent or contains only an unavoidably mixed solvent.

[0028] The glass transition temperature of the cured product of the composition (X) is preferably 80° C. or higher. That is, the composition (X) preferably has a property of curing to become a cured product having a glass transition temperature of 80° C. or higher. In this case, the cured product can have good heat resistance. Therefore, for example, when the cured product is subjected to a treatment accompanied by a temperature increase, the cured product is not easily deteriorated. Therefore, for example, when an inorganic material layer (e.g., passivation layer 6) that overlaps an optical component is produced by a deposition method such as a plasma CVD method, the optical component is not easily deteriorated even if the optical component is heated. In addition, by increasing the heat resistance, the optical component can be adapted to an in-vehicle application that has strict requirements for heat resistance. The glass transition temperature of the cured product is more preferably 90° C. or higher, and even more preferably 100° C. or higher. This glass transition temperature of the cured product can be achieved by the composition of the composition (X) described in detail below.

[0029] The volatility of 20 mg of composition (X) is preferably 40% or less when heated at 100°C for 30 minutes using a thermogravimetric analyzer. The volatility of composition (X) is defined as the percentage of the weight loss of composition (X) after treatment (the difference between the weight of composition (X) before treatment and the weight of composition (X) after treatment) relative to the weight of composition (X) before treatment. In this case, the low volatility of composition (X) can enhance the storage stability of composition (X). In addition, outgassing is less likely to occur from the cured product of composition (X) and optical components. Therefore, voids due to outgassing are further less likely to occur in the light-emitting device. The volatility of composition (X) can be determined by heating 20 mg of composition (X) at 100°C for 30 minutes using a thermogravimetric analyzer and calculating the weight loss of the weight after treatment relative to the weight before treatment. When 20 mg of composition (X) is heated at 100° C. for 30 minutes using a thermogravimetric analyzer, the volatility is more preferably 30% or less, and even more preferably 20% or less. The lower limit of the volatility of composition (X) is not particularly limited, but may be, for example, 0.1% or more.

[0030] The components contained in the composition (X) will be described in more detail below.

[0031] The composition (X) contains an acrylic compound (Y) having at least one (meth)acrylic group in one molecule. The acrylic compound (Y) contains at least one component selected from the group consisting of, for example, a monomer, an oligomer, and a prepolymer.

[0032] The viscosity of the entire acrylic compound (Y) at 25°C is preferably 50 mPa·s or less. In this case, the acrylic compound (Y) can particularly reduce the viscosity of the composition (X). The viscosity of the entire acrylic compound (Y) is more preferably 30 mPa·s or less, and particularly preferably 20 mPa·s or less. The viscosity of the entire acrylic compound (Y) is, for example, 3 mPa·s or more.

[0033] It is also preferable that the viscosity of the entire acrylic compound (Y) at 40°C is 50 mPa·s or less. In this case, the acrylic compound (Y) can particularly reduce the viscosity of the composition (X) when heated. It is more preferable that the viscosity of the entire acrylic compound (Y) is 30 mPa·s or less, and particularly preferable that the viscosity is 20 mPa·s or less. Moreover, the viscosity of the entire acrylic compound (Y) is, for example, 3 mPa·s or more.

[0034] The percentage of the component having a boiling point of 270° C. or more in the acrylic compound (Y) is preferably 80% by mass or more. In this case, the storage stability of the composition (X) is particularly unlikely to be impaired, and outgassing from the cured product is particularly unlikely to occur. It is more preferable that the percentage of the component having a boiling point of 280° C. or more in the acrylic compound (Y) is 80% by mass or more.

[0035] The acrylic compound (Y) preferably contains a component having a viscosity of 20 mPa·s or less at 25° C. In this case, the viscosity of the composition (X) can be reduced.

[0036] The proportion of the component having a viscosity of 20 mPa·s or less at 25°C relative to the total amount of the acrylic compound (Y) is preferably 50% by mass or more and 100% by mass or less. In this case, the viscosity of the composition (X) can be particularly reduced, making the composition (X) particularly easy to apply by the inkjet method. This proportion is more preferably 60% by mass or more, and even more preferably 70% by mass or more. In addition, this proportion is more preferably 95% by mass or less, and even more preferably 90% by mass or less.

[0037] The component having a viscosity of 20 mPa·s or less at 25°C preferably contains a compound having a glass transition temperature of 80°C or more. In this case, the glass transition temperature of the cured product can be increased while lowering the viscosity of composition (X). It is more preferable that this component contains a compound having a glass transition temperature of 90°C or more, and even more preferable that it contains a compound having a glass transition temperature of 100°C or more. There is no upper limit to the glass transition temperature of the compound contained in this component, but it is, for example, 150°C or less.

[0038] Compounds that the acrylic compound (Y) may contain will be described below.

[0039] In this embodiment, the acrylic compound (Y) contains a polyfunctional acrylic compound (Y1) having a nitrogen atom. That is, as described above, the composition (X) contains a polyfunctional acrylic compound (Y1). The polyfunctional acrylic compound (Y1) has at least one nitrogen atom in the molecular skeleton and has two or more (meth)acryloyl groups in one molecule. Since the polyfunctional acrylic compound (Y1) has a nitrogen atom, it is easy to increase the adhesion between the cured product of the composition (X) and an inorganic material. Furthermore, since the polyfunctional acrylic compound (Y1) has two or more (meth)acryloyl groups in one molecule, it has good reactivity and therefore is easy to increase the ultraviolet curing property of the composition (X).

[0040] The polyfunctional acrylic compound (Y1) preferably has a nitrogen atom by having at least one amide group in one molecule. In this case, it is particularly easy to increase the adhesion between the cured product and the inorganic material. The acrylic compound (Y1) may have multiple amide groups in one molecule. In that case, it is particularly easy to increase the adhesion between the cured product and the inorganic material. The amide group may include at least one of a secondary amide group and a tertiary amide group. The polyfunctional acrylic compound (Y1) contains, for example, at least one of a compound having two amide groups in one molecule, a compound having three amide groups in one molecule, and a compound having four amide groups in one molecule. The polyfunctional acrylic compound (Y1) may contain a compound having five or more amide groups in one molecule.

[0041] The polyfunctional acrylic compound (Y1) preferably contains a polyfunctional acrylamide compound (Y11) having two or more (meth)acrylamide groups in one molecule, i.e., a N-CO-CR=CH2 group (R is H or CH3). In this case, it is particularly easy to increase the adhesion between the cured product and the inorganic material, and particularly easy to increase the reactivity of the composition (X). The polyfunctional acrylamide compound (Y11) contains at least one of the group consisting of, for example, a bifunctional compound having two (meth)acrylamide groups in one molecule, a trifunctional compound having three (meth)acrylamide groups in one molecule, and a tetrafunctional compound having four (meth)acrylamide groups in one molecule.

[0042] The bifunctional compound includes, for example, a compound represented by the following formula (51).

[0043] [ka]

[0044] The trifunctional compound includes, for example, a compound represented by the following formula (52).

[0045] [ka]

[0046] The tetrafunctional compound contains, for example, at least one of a compound represented by the following formula (53) and a compound represented by the following formula (54).

[0047] [ka]

[0048] [ka]

[0049] The compounds that the polyfunctional acrylamide compound (Y11) may contain are not limited to those mentioned above. The polyfunctional acrylamide compound (Y11) may also contain a pentafunctional or higher compound.

[0050] The ratio of the polyfunctional acrylic compound (Y1) to the total acrylic compound (Y) is preferably 3% by mass or more and 40% by mass or less. When the ratio of the polyfunctional acrylic compound (Y1) is 3% by mass or more, the adhesion between the cured product and the inorganic material and the reactivity of the composition (X) are particularly likely to be increased. Furthermore, when the ratio of the polyfunctional acrylic compound (Y1) is 40% by mass or less, precipitation does not occur and storage stability is improved. This ratio is more preferably 35% by mass or less, even more preferably 30% by mass or less, and even more preferably 25% by mass or less. Furthermore, this ratio is more preferably 5% by mass or more, and even more preferably 10% by mass or more.

[0051] The acrylic compound (Y) may further contain an acrylic compound (Y2) other than the polyfunctional acrylic compound (Y1).

[0052] The acrylic compound (Y2) preferably contains a polyfunctional acrylic compound (Y21) having two or more radically polymerizable functional groups including a (meth)acryloyl group in one molecule. In this case, the polyfunctional acrylic compound (Y21) can increase the glass transition temperature of the cured product, and therefore can increase the heat resistance of the cured product. The total ratio of the polyfunctional acrylamide compound (Y1) and the polyfunctional acrylic compound (Y21) is preferably 50% by mass or more and 100% by mass or less based on the total acrylic compound (Y). The acrylic compound (Y) may contain only the polyfunctional acrylic compound (Y1), or may contain only the polyfunctional acrylic compound (Y1) and the polyfunctional acrylic compound (Y21).

[0053] Examples of the polyfunctional acrylic compound (Y21) include 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol oligoacrylate, diethylene glycol diacrylate, 1,6-hexanediol oligoacrylate, neopentyl glycol diacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, dipropylene glycol diacrylate, cyclohexane dimethanol diacrylate, tricyclodecane dimethanol diacrylate, bisphenol A polyethoxy diacrylate, bisphenol F polyethoxy diacrylate, pentatriestrol tetraacrylate, propoxylated (2) neopentyl glycol diacrylate, trimethylolpropane triacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, pentaerythritol triacrylate, ethoxylated (3) trimethylol propane triacrylate, propoxylated (3) glyceryl triacrylate, pentaerythritol tetraacrylate, ditrimethylolpropane tetraacrylate, ethoxylated (4) pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, 2-(2-ethoxyethoxy)ethyl acrylate, hexadiol diacrylate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, tripropylene glycol triacrylate, bispentaerythritol hexaacrylate, ethylene glycol diacrylate, 1,6-hexanediol diacrylate, ethoxylated 1,6-hexanediol diacrylate, polypropylene glycol diacrylate, 1,4-butanediol diacrylate, 1,9-nonanediol diacrylate, tetraethylene glycol diacrylate, 2-n-butyl-2-ethyl-1,3-Propanediol diacrylate, hydroxypivalic acid neopentyl glycol diacrylate, hydroxypivalic acid trimethylolpropane triacrylate, ethoxylated phosphoric acid triacrylate, ethoxylated tripropylene glycol diacrylate, neopentyl glycol modified trimethylolpropane diacrylate, stearic acid modified pentaerythritol diacrylate, tetramethylolpropane triacrylate, tetramethylolmethane triacrylate, caprolactone modified trimethylolpropane triacrylate, propoxylated glyceryl triacrylate, tetramethylolmethane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, dipentaerythritol diacrylate, The composition contains at least one compound selected from the group consisting of erythritol hexaacrylate, caprolactone-modified dipentaerythritol hexaacrylate, dipentaerythritol hydroxypentaacrylate, neopentyl glycol oligoacrylate, trimethylolpropane oligoacrylate, pentaerythritol oligoacrylate, ethoxylated neopentyl glycol di(meth)acrylate, propoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, and 2-(2-vinyloxyethoxy)ethyl acrylate.

[0054] The acrylic equivalent of the polyfunctional acrylic compound (Y21) is preferably 150 g / eq or less, more preferably 90 g / eq or more and 150 g / eq or less. The weight average molecular weight of the polyfunctional acrylic compound (Y21) is, for example, 100 or more and 1000 or less, more preferably 200 or more and 800 or less.

[0055] The polyfunctional acrylic compound (Y21) preferably contains a compound (Y211) having a structure represented by the following formula (200).

[0056] CH2=CR 1 -COO-(R 3 -O)n -CO-CR 2 =CH2…(200) In formula (200), R 1 and R 2 Each of the groups is a hydrogen atom or a methyl group, n is an integer of 1 or more, R 3 is an alkylene group having 1 or more carbon atoms, and when n is 2 or more, multiple R 3 may be the same or different from each other.

[0057] Compound (Y211) has the structure shown in formula (200), particularly R 3 Since the carbon number of R is 3 or more, it is difficult to increase the affinity of the cured product with water. 3 The number of carbon atoms in is, for example, 1 or more and 15 or less, preferably 3 or more and 15 or less. In addition, the compound (Y211) can increase the glass transition temperature of the cured product by having the structure shown in formula (200), particularly by having two (meth)acryloyl groups in one molecule, and therefore can increase the heat resistance of the cured product. In addition, n in formula (200) is, for example, an integer of 1 or more and 12 or less.

[0058] The percentage of the compound (Y211) relative to the acrylic compound (Y) is preferably 50% by mass or more. In this case, the storage stability of the composition (X) is effectively improved, the generation of outgassing from the cured product is effectively reduced, and the affinity of the cured product for water is particularly difficult to increase. The percentage of the compound (Y211) relative to the acrylic compound (Y) is, for example, 70% by mass or less, or 60% by mass or less, preferably 50% by mass or less.

[0059] The compound (Y211) preferably contains a component having a boiling point of 270° C. or higher. That is, the acrylic compound (Y) preferably contains a component having a structure shown in formula (200) and a boiling point of 270° C. or higher. In this case, the acrylic compound (Y) is unlikely to volatilize from the composition (X) during storage of the composition (X) and when the composition (X) is heated. Therefore, the storage stability of the composition (X) is unlikely to be impaired. In addition, even if the compound (Y211) remains unreacted in the cured product of the composition (X), outgassing due to the compound (Y211) is unlikely to occur from the cured product. Therefore, voids due to outgassing are unlikely to occur in the light-emitting device 1. If there are voids in the light-emitting device 1, moisture may penetrate into the light-emitting element 4 through the voids, but if voids are unlikely to occur, moisture is unlikely to penetrate into the light-emitting element 4. The boiling point is a boiling point under normal pressure obtained by converting the boiling point under reduced pressure, and is determined by the method shown in, for example, Science of Petroleum, Vol. II, p. 1281 (1938). It is more preferable that the compound (Y211) contains a component having a boiling point of 280° C. or higher.

[0060] The viscosity of the compound (Y211) at 25°C is preferably 25 mPa·s or less. In this case, the compound (Y211) can reduce the viscosity of the composition (X). The viscosity of the compound (Y211) at 25°C is more preferably 25 mPa·s or less, even more preferably 20 mPa·s or less, and particularly preferably 15 mPa·s or less. The viscosity of the compound (Y211) at 25°C is, for example, 1 mPa·s or more, preferably 3 mPa·s or more, and even more preferably 5 mPa·s or more.

[0061] The compound (Y211) contains, for example, at least one compound selected from the group consisting of alkylene glycol di(meth)acrylate, polyalkylene glycol di(meth)acrylate, and alkylene oxide-modified alkylene glycol di(meth)acrylate.

[0062] Alkylene glycol di(meth)acrylate is a compound of formula (200) where n is 1. In this case, R 3 The number of carbon atoms in R is preferably 4 to 12. 3 may be linear or branched. In particular, the alkylene glycol di(meth)acrylate preferably contains at least one compound selected from the group consisting of 1,4-butanediol diacrylate, 1,3-butylene glycol diacrylate, neopentyl glycol diacrylate, 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, 1,10-decanediol diacrylate, 1,4-butanediol dimethacrylate, 1,3-butylene glycol dimethacrylate, neopentyl glycol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol dimethacrylate, and 1,12-dodecanediol dimethacrylate. In addition, alkylene glycol di(meth)acrylate is Sartomer's product number SR213, Osaka Organic Chemical Industry's product number V195, Sartomer's product number SR212, Sartomer's product number SR247, Kyoei Chemical Industry's product name Light Acrylate NP-A, Sartomer's product number SR238NS, Osaka Organic Chemical Industry's product number V230, Daicel's product number HDDA, Kyoei Chemical Industry's product number 1,6HX-A, Osaka Organic Chemical Industry's product number V260, Kyoei Chemical Industry's product number 1,9-ND-A, Shin-Nakamura Chemical Industry's product number A-NOD-A, Sartomer's product number CD595, Sartomer's product number S It is preferable that the composition contains at least one compound selected from the group consisting of R214NS, product number BD made by Shin-Nakamura Chemical Co., Ltd., product number SR297 made by Sartomer, product number SR248 made by Sartomer, product number Light Ester NP made by Kyoei Chemical Co., Ltd., product number SR239NS made by Sartomer, product name Light Ester 1,6HX made by Kyoei Chemical Co., Ltd., product number HD-N made by Shin-Nakamura Chemical Co., Ltd., product name Light Ester 1,9ND made by Kyoei Chemical Co., Ltd., product number NOD-N made by Shin-Nakamura Chemical Co., Ltd., product name Light Ester 1,10DC made by Kyoei Chemical Co., Ltd., product number DOD-N made by Shin-Nakamura Chemical Co., Ltd., and product number SR262 made by Sartomer.

[0063] Polyalkylene glycol di(meth)acrylate is, for example, a compound represented by formula (200) in which n is 2 or more. n is, for example, 2 to 10, preferably 2 to 7, more preferably 2 to 6, and even more preferably 2 to 3. R 3 The number of carbon atoms is, for example, 2 to 7, and preferably 2 to 5. The larger the number of carbon atoms, the higher the hydrophobicity of the cured product, and the less moisture permeable the cured product becomes. The polyalkylene glycol di(meth)acrylate preferably contains at least one compound selected from the group consisting of diethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, hexaethylene glycol dimethacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, tripropylene glycol dimethacrylate, tritetramethylene glycol diacrylate, polyethylene glycol 200 dimethacrylate, and polyethylene glycol 200 diacrylate. In addition, the polyalkylene glycol di(meth)acrylate preferably contains at least one compound selected from the group consisting of Sartomer Corporation product number SR230, Sartomer Corporation product number SR508NS, Daicel Corporation product number DPGDA, Sartomer Corporation product number SR306NS, Daicel Corporation product number TPGDA, Osaka Organic Chemical Industry Co., Ltd. product number V310HP, Shin-Nakamura Chemical Co., Ltd. product number APG200, Kyoei Chemical Industry Co., Ltd. product name Light Acrylate PTMGA-250, Sartomer Corporation product number SR231NS, Kyoei Chemical Industry Co., Ltd. product name Light Ester 2EG, Sartomer Corporation product number SR205NS, Kyoei Chemical Industry Co., Ltd. product name Light Ester 3EG, Sartomer Corporation product number SR210NS, Kyoei Chemical Industry Co., Ltd. product name Light Ester 4EG, Mitsubishi Chemical Corporation product name Acrylate HX, and Shin-Nakamura Chemical Co., Ltd. product number 3PG.

[0064] The alkylene oxide modified alkylene glycol di(meth)acrylate includes, for example, propylene oxide modified neopentyl glycol. The alkylene oxide modified alkylene glycol di(meth)acrylate includes, for example, EBECRYL145 manufactured by Daicel Corporation.

[0065] When the acrylic compound (Y) contains a compound (Y211) having a structure represented by formula (200), it is preferable that the compound (Y211) does not contain a compound in which the value of n in formula (200) is 5 or more. (R 3 -O) n is a polyethylene glycol skeleton, it is particularly preferred that the compound (Y211) does not contain a compound having an n value of greater than 5 in formula (200). Even when the compound (Y211) contains a compound having an n value of greater than 5 in formula (200), the percentage of the compound having an n value of greater than 5 in formula (200) relative to the acrylic compound (Y) is preferably 20 mass% or less. Even when the compound (Y211) contains a compound having an n value of greater than 5 in formula (200), it is preferable that the compound (Y211) does not contain a compound having an n value of greater than 9, and more preferably does not contain a compound having an n value of greater than 7. In these cases, the viscosity increase of the composition (X) is particularly unlikely to occur.

[0066] It is particularly preferred that the polyfunctional acrylic compound (Y21) contains a polyalkylene glycol di(meth)acrylate, which has low viscosity and is not easily volatile, and therefore can contribute to lowering the viscosity of the composition (X), improving the storage stability of the composition (X), and reducing outgassing from the cured product.

[0067] When the polyfunctional acrylic compound (Y21) contains polyalkylene glycol di(meth)acrylate, the ratio of polyalkylene glycol di(meth)acrylate to the acrylic compound (Y) is preferably 40% by mass or more and 80% by mass or less. When the ratio of polyalkylene glycol di(meth)acrylate is 40% by mass or more, the viscosity of the composition (X) can be effectively reduced. When the ratio of polyalkylene glycol di(meth)acrylate is 80% by mass or less, the ratio of the compound having three or more (meth)acryloyl groups in the molecule increases, and the reactivity of the composition (X) and the glass transition temperature of the cured product can be increased. This ratio is more preferably 42% by mass or more and 75% by mass or less, and even more preferably 45% by mass or more and 70% by mass or less.

[0068] The polyfunctional acrylic compound (Y21) may contain a compound having three or more radical polymerizable functional groups, including a (meth)acryloyl group, in one molecule. In this case, the polyfunctional acrylic compound (Y21) may contain at least one selected from the group consisting of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, and pentaerythritol tetra(meth)acrylate. In this case, the glass transition temperature of the cured product can be particularly increased, and therefore the heat resistance of the cured product can be particularly increased.

[0069] The polyfunctional acrylic compound (Y21) preferably contains pentaerythritol tetra(meth)acrylate. In this case, the glass transition temperature of the cured product can be particularly increased, and the reactivity of the composition (X) can be improved. When the reactivity of the composition (X) is improved, the composition (X) can be easily cured even in an oxygen-containing environment such as the air atmosphere.

[0070] When the polyfunctional acrylic compound (Y21) contains pentaerythritol tetra(meth)acrylate, the ratio of pentaerythritol tetra(meth)acrylate to the acrylic compound (Y) is preferably 0.5% by mass or more and 10% by mass or less. In this case, the composition (X) can achieve both high reactivity and low viscosity. This ratio is more preferably 1% by mass or more and 9% by mass or less, and even more preferably 2% by mass or more and 8% by mass or less.

[0071] The polyfunctional acrylic compound (Y21) may have at least one of a benzene ring, an alicyclic ring, and a polar group. The polar group is, for example, an OH group. In this case, the shrinkage during curing of the composition (X) can be particularly reduced. Furthermore, the adhesion between the cured product and inorganic compounds such as silicon nitride and silicon oxide can be increased. The polyfunctional acrylic compound (Y21) preferably contains at least one compound selected from the group consisting of tricyclodecane dimethanol diacrylate, bisphenol A polyethoxy diacrylate, bisphenol F polyethoxy diacrylate, trimethylolpropane triacrylate, and pentaerythritol triacrylate. These compounds can particularly reduce the shrinkage during curing of the composition (X). Furthermore, these compounds can also increase the adhesion between the cured product and inorganic compounds such as silicon nitride and silicon oxide.

[0072] If the adhesion between the cured product and the inorganic material is increased, when the optical component is overlaid with a film made of an inorganic material (inorganic film) such as a SiN film, high adhesion is likely to be obtained between the optical component and the inorganic film.

[0073] It is particularly preferred that the polyfunctional acrylic compound (Y21) contains polyalkylene glycol di(meth)acrylate and pentaerythritol tetra(meth)acrylate. In this case, the composition (X) has low viscosity and excellent reactivity. Therefore, the composition (X) can be easily cured even in an oxygen-containing environment such as the air atmosphere.

[0074] The acrylic compound (Y2) preferably contains a monofunctional acrylic compound (Y22) having only one (meth)acryloyl group as a radical polymerizable functional group in one molecule. The monofunctional acrylic compound (Y22) can suppress shrinkage of the composition (X) during curing.

[0075] When the acrylic compound (Y2) contains a monofunctional acrylic compound (Y22), the amount of the monofunctional acrylic compound (Y22) relative to the total amount of the acrylic compound (Y) is preferably more than 0% by mass and not more than 50% by mass. If the amount of the monofunctional acrylic compound (Y22) is more than 0% by mass, the shrinkage during curing of the composition (X) can be suppressed. In addition, if the amount of the monofunctional acrylic compound (Y22) is 50% by mass or less, the total amount of the polyfunctional acrylic compound (Y1) and the polyfunctional acrylic compound (Y21) can be 50% by mass or more, and the heat resistance of the cured product can be particularly improved. It is more preferable that the amount of the monofunctional acrylic compound (Y22) is 5% by mass or more, more preferably 30% by mass or less, and particularly preferably 20% by mass or less.

[0076] Examples of the monofunctional acrylic compound (Y22) include tetrahydrofurfuryl acrylate, isobornyl acrylate, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, isobutyl acrylate, t-butyl acrylate, isooctyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 2-ethoxyethyl acrylate, 3-methoxybutyl acrylate, ethoxyethyl acrylate, butoxyethyl acrylate, ethoxydiethylene glycol acrylate, Methoxydixylethyl acrylate, ethyl diglycol acrylate, cyclic trimethylolpropane formal monoacrylate, imide acrylate, isoamyl acrylate, ethoxylated succinic acid acrylate, trifluoroethyl acrylate, ω-carboxypolycaprolactone monoacrylate, cyclohexyl acrylate, 2-(2-ethoxyethoxy)ethyl acrylate, stearyl acrylate, diethylene glycol monobutyl ether acrylate, lauryl acrylate, isodecyl acrylate, 3,3,5-trimethylcyclohexanol acrylate, isooctyl acrylate, octyl / decyl acrylate, tridecyl acrylate, caprolactone acrylate, ethoxylated (4)nylphenol acrylate, methoxypolyethylene glycol (350) monoacrylate, methoxypolyethylene glycol (550) monoacrylate, phenoxyethyl acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl acrylate, methylphenoxyethyl acrylate, 4-t-butylcyclohexyl acrylate, caprolactone-modified tetrahydrofurfuryl acrylate, tribromo The composition contains at least one compound selected from the group consisting of morphophenyl acrylate, ethoxylated tribromophenyl acrylate, 2-phenoxyethyl acrylate, an ethylene oxide adduct of 2-phenoxyethyl acrylate, a propylene oxide adduct of 2-phenoxyethyl acrylate, acryloyl morpholine, morpholine 4-yl acrylate, dicyclopentanyl acrylate, phenoxydiethylene glycol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 1,4-cyclohexanedimethanol monoacrylate, 3-methacryloyloxymethylcyclohexene oxide, and 3-acryloyloxymethylcyclohexene oxide.

[0077] The monofunctional acrylic compound (Y22) may contain at least one compound selected from the group consisting of compounds having an alicyclic structure and compounds having a cyclic ether structure.

[0078] The compound having an alicyclic structure contains at least one compound selected from the group consisting of, for example, phenoxyethyl acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl acrylate, methylphenoxyethyl acrylate, 4-t-butylcyclohexyl acrylate, caprolactone-modified tetrahydrofurfuryl acrylate, tribromophenyl acrylate, ethoxylated tribromophenyl acrylate, 2-phenoxyethyl acrylate, an ethylene oxide adduct of 2-phenoxyethyl acrylate, a propylene oxide adduct of 2-phenoxyethyl acrylate, acryloyl morpholine, morpholine 4-yl acrylate, isobornyl acrylate, dicyclopentanyl acrylate, phenoxydiethylene glycol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, and 1,4-cyclohexanedimethanol monoacrylate.

[0079] The number of ring members in the cyclic ether structure in the compound having a cyclic ether structure is preferably 3 or more, more preferably 3 to 4. The number of carbon atoms contained in the cyclic ether structure is preferably 2 to 9, more preferably 2 to 6. The compound having a cyclic ether structure contains, for example, at least one compound selected from the group consisting of 3-methacryloyloxymethylcyclohexene oxide and 3-acryloyloxymethylcyclohexene oxide.

[0080] The acrylic compound (Y2) may contain a compound having silicon in the molecular skeleton. In this case, the adhesion between the cured product and the inorganic material is improved. The compound having silicon in the molecular skeleton contains at least one compound selected from the group consisting of, for example, 3-(trimethoxysilyl)propyl acrylate (e.g., product number KBM5103 manufactured by Shin-Etsu Chemical Co., Ltd.) and (meth)acrylic group-containing alkoxysilane oligomer (e.g., product number KR-513 manufactured by Shin-Etsu Chemical Co., Ltd.).

[0081] The acrylic compound (Y2) may contain a compound having phosphorus in the molecular skeleton. In this case, the adhesion between the cured product and the inorganic material is improved. The compound having phosphorus in the molecular skeleton includes, for example, acid phosphoxy (meth)acrylate, such as acid phosphoxy polyoxypropylene glycol monomethacrylate.

[0082] The monofunctional acrylic compound (Y22) may contain a monofunctional acrylic compound (Y222) having a nitrogen atom. That is, the composition (X) may contain a monofunctional acrylic compound (Y222) having a nitrogen atom. In this case, the monofunctional acrylic compound (Y222) may improve the adhesion between the cured product and the inorganic material, similar to the polyfunctional acrylic compound (Y1). In addition, the improved adhesion makes it easier for the composition (X) to follow the unevenness of the substrate, and the flatness of the film made from the composition (X) can be sufficiently improved. Furthermore, the viscosity of the composition (X) can be sufficiently reduced, and the inkjet property can be improved. The monofunctional acrylic compound (Y222) includes at least one compound selected from the group consisting of compounds having a morpholine skeleton, such as acryloylmorpholine and 4-yl morpholine acrylate, diethylacrylamide, dimethylaminopropylacrylamide, and pentamethylpiperidyl methacrylate.

[0083] The ratio of the monofunctional acrylic compound (Y222) to the entire acrylic compound (Y) is preferably 5% by mass or more and 60% by mass or less. If this ratio is 5% by mass or more, the composition (X) is easily cured in the air. If this ratio is 50% by mass or less, outgassing is reduced, and the reliability of devices such as light-emitting devices manufactured using the composition (X) is improved. This ratio is more preferably 10% by mass or more and 55% by mass or less, and more preferably 20% by mass or more and 50% by mass or less.

[0084] In addition, the ratio of the compound having a nitrogen atom in the acrylic compound (Y) to the entire acrylic compound (Y) is preferably 5% by mass or more and 80% by mass or less. When this ratio is 5% by mass or more, the adhesion between the cured product and the inorganic material is particularly likely to be improved. When this ratio is 80% by mass or less, the compound having nitrogen in the molecular skeleton is less likely to inhibit the storage stability of the composition (X) and is less likely to generate satellites when the composition (X) is sprayed by the inkjet method. Therefore, the inkjet properties of the composition (X) are less likely to be inhibited. Furthermore, outgassing due to the compound having nitrogen in the molecular skeleton can be suppressed. This ratio is more preferably 10% by mass or more and 70% by mass or less, even more preferably 20% by mass or more and 60% by mass or less, and particularly preferably 25% by mass or more and 50% by mass or less. The compound having a nitrogen atom includes a polyfunctional acrylic compound (Y1). When the acrylic compound (Y) contains a monofunctional acrylic compound (Y222), the compound having a nitrogen atom also includes the monofunctional acrylic compound (Y222).

[0085] The acrylic compound (Y2) may contain a compound having an isobornyl skeleton. The compound having an isobornyl skeleton may contain, for example, one or more compounds selected from the group consisting of isobornyl acrylate and isobornyl methacrylate.

[0086] The acrylic compound (Y2) may contain a component consisting of a compound having at least one skeleton selected from the group consisting of a dicyclopentadiene skeleton, a dicyclopentanyl skeleton, a dicyclopentenyl skeleton, and a bisphenol skeleton. Specifically, the acrylic compound (Y) may contain at least one compound selected from the group consisting of, for example, tricyclodecane dimethanol diacrylate, bisphenol A polyethoxy diacrylate, and bisphenol F polyethoxy diacrylate. In this case, the adhesion between the cured product and the inorganic material can be increased.

[0087] The acrylic compound (Y2) may contain a compound represented by the following formula (100). In this case, the reactivity of the composition (X) can be increased, and the adhesion between the cured product and the inorganic material can be improved.

[0088] [ka]

[0089] In formula (100), R 0 is H or a methyl group. X is a single bond or a divalent hydrocarbon group. R 1 From R 11 Each of is H, an alkyl group or -R 12 -OH, R 12 is an alkylene group and R 1 From R 11 At least one of the groups is an alkyl group or -R 12 -OH. 1 From R 11 are not chemically bonded to each other.

[0090] Specifically, for example, the acrylic compound (Y2) may contain at least one compound selected from the group consisting of a compound represented by the following formula (110), a compound represented by the following formula (120), and a compound represented by the following formula (130).

[0091] [ka]

[0092] The composition (X) may further contain a radical polymerizable compound (Z) other than the acrylic compound (Y). The amount of the radical polymerizable compound (Z) relative to the total amount of the acrylic compound (Y) and the radical polymerizable compound (Z) is, for example, 10 mass% or less. The radical polymerizable compound (Z) may contain either one or both of a polyfunctional radical polymerizable compound (Z1) having two or more radical polymerizable functional groups in one molecule and a monofunctional radical polymerizable compound (Z2) having only one radical polymerizable functional group in one molecule. The polyfunctional radical polymerizable compound (Z1) may contain at least one compound selected from the group consisting of an aromatic urethane oligomer, an aliphatic urethane oligomer, an epoxy acrylate oligomer, a polyester acrylate oligomer, and other special oligomers having two or more ethylenic double bonds in one molecule. Note that the components that the polyfunctional radical polymerizable compound (Z1) may contain are not limited to those mentioned above. The monofunctional radical polymerizable compound (Z2) contains at least one compound selected from the group consisting of, for example, N-vinylformamide, vinylcaprolactam, vinylpyrrolidone, phenylglycidyl ether, p-tert-butylphenylglycidyl ether, butylglycidyl ether, 2-ethylhexylglycidyl ether, allylglycidyl ether, 1,2-butylene oxide, 1,3-butadiene monoxide, 1,2-epoxydodecane, epichlorohydrin, 1,2-epoxydecane, styrene oxide, cyclohexene oxide, 3-vinylcyclohexene oxide, 4-vinylcyclohexene oxide, N-vinylpyrrolidone and N-vinylcaprolactam. Note that the components that the monofunctional radical polymerizable compound (Z2) can contain are not limited to the above.

[0093] When the composition (X) contains a radical polymerizable compound (Z), the radical polymerizable compound (Z) may contain a compound having nitrogen in its molecular skeleton. The compound having nitrogen in its molecular skeleton includes at least one compound selected from the group consisting of N-vinylformamide, N-vinylpyrrolidone, and N-vinylcaprolactam. In this case, the adhesion between the cured product and the inorganic material is improved.

[0094] The total ratio of the compound having nitrogen in the molecular skeleton in the acrylic compound (Y) and the compound having nitrogen in the molecular skeleton in the radical polymerizable compound (Z) to the total of the acrylic compound (Y) and the radical polymerizable compound (Z) is preferably 5% by mass or more and 80% by mass or less. When this ratio is 5% by mass or more, the adhesion between the cured product and the inorganic material is particularly likely to be improved. When this ratio is 80% by mass or less, the compound having nitrogen in the molecular skeleton is less likely to inhibit the storage stability of the composition (X) and is less likely to generate satellites when the composition (X) is sprayed by the inkjet method. Therefore, the inkjet properties of the composition (X) are less likely to be inhibited. Furthermore, outgassing caused by the compound having nitrogen in the molecular skeleton can be less likely to occur. This ratio is more preferably 10% by mass or more and 70% by mass or less, even more preferably 20% by mass or more and 60% by mass or less, and particularly preferably 25% by mass or more and 50% by mass or less.

[0095] The ratio of the total of monofunctional compounds in the radical polymerizable compound (Z) (i.e., the total of the monofunctional acrylic compound (Y22) and the monofunctional radical polymerizable compound (Z2)) to the radical polymerizable compound (Z) is preferably 70% by mass or less. In this case, outgassing caused by the monofunctional compounds is less likely to occur. This ratio is more preferably 60% by mass or less, and even more preferably 50% by mass or less. The photopolymerization initiator (B) preferably contains a photoradical polymerization initiator (B1). The photoradical polymerization initiator is not particularly limited as long as it is a compound that generates radical species when irradiated with ultraviolet light. The photoradical polymerization initiator (B1) contains at least one compound selected from the group consisting of, for example, aromatic ketones, acylphosphine oxide compounds, aromatic onium salt compounds, organic peroxides, thio compounds (thioxanthone compounds, thiophenyl group-containing compounds, etc.), hexaarylbiimidazole compounds, oxime ester compounds, borate compounds, azinium compounds, metallocene compounds, active ester compounds, compounds having a carbon-halogen bond, and alkylamine compounds.

[0096] The ratio of the photoradical polymerization initiator (B1) to the acrylic compound (Y) (when the composition (X) contains a radically polymerizable compound (Z), the total of the acrylic compound (Y) and the radically polymerizable compound (Z)) is preferably 6% by mass or more. In this case, the composition (X) can have good ultraviolet curing properties, and can also have good ultraviolet curing properties in the air. This ratio is more preferably 7% by mass or more, and even more preferably 8% by mass or more. This ratio is, for example, 30% by mass or less, preferably 20% by mass or less, and even more preferably 18% by mass or less.

[0097] The photoradical polymerization initiator (B1) preferably contains a component having photobleachability. In this case, the cured product of the composition (X) is likely to have good light transmittance. The ratio of the component having photobleachability to the radical polymerizable compound (A1) is preferably 6% by mass or more. This ratio is more preferably 7% by mass or more, and even more preferably 8% by mass or more. This ratio is, for example, 30% by mass or less, preferably 20% by mass or less, and even more preferably 18% by mass or less.

[0098] The component having photobleachability contains, for example, at least one of an acylphosphine oxide-based photoinitiator and a compound having photobleachability among oxime ester-based photoinitiators.

[0099] It is also preferable that the photoradical polymerization initiator (B1) contains a component having a sensitizer skeleton in the molecule. The sensitizer skeleton contains, for example, at least one of a 9H-thioxanthen-9-one skeleton and an anthracene skeleton. That is, it is preferable that the photoradical polymerization initiator (B1) contains a component having at least one of a 9H-thioxanthen-9-one skeleton and an anthracene skeleton.

[0100] The photoradical polymerization initiator (B1) preferably contains an oxime ester photoinitiator, regardless of whether it has photobleachability. The oxime ester photoinitiator can improve the curability of the composition (X). Therefore, the composition (X) can be easily cured even in an oxygen-containing environment such as the air atmosphere, and the cured product can be made less likely to produce outgassing.

[0101] In order to prevent contamination of composition (X) and a production apparatus due to generation of decomposition products from composition (X) and to further prevent generation of outgas from the cured product, the oxime ester photoinitiator preferably contains a compound having an aromatic ring, more preferably contains a compound having a condensed ring containing an aromatic ring, and further preferably contains a compound having a condensed ring containing a benzene ring and a heterocycle.

[0102] Oxime ester photoinitiators include, for example, 1,2-octadione-1-[4-(phenylthio)-, 2-(o-benzoyloxime)], and ethanone, 1-[9-ethyl-6- (2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime), and at least one compound selected from the group consisting of oxime ester photoinitiators described in JP-A Nos. 2000-80068, 2001-233842, 2010-527339, 2010-527338, 2013-041153, and 2015-93842, etc. The oxime ester photoinitiator may contain at least one compound selected from the group consisting of commercially available products Irgacure OXE-02 (manufactured by BASF), Adeka Arcles NCI-831, N-1919 (manufactured by ADEKA Corporation), and TR-PBG-304 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), Irgacure OXE-01, Adeka Arcles NCI-930 (manufactured by ADEKA Corporation), TR-PBG-345, and TR-PBG-3057 (all manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), and TR-PBG-365 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) and SPI-04 (manufactured by Sanyang Co., Ltd.) having a fluorene skeleton. In particular, it is preferable that the oxime ester photoinitiator contains a compound having a diphenyl sulfide skeleton or a fluorene skeleton, since the cured product is less likely to be colored by photobleaching. It is also preferable that the oxime ester photoinitiator contains a compound having a carbazole skeleton, since the exposure sensitivity is likely to be increased.

[0103] It is also preferred that the oxime ester photoinitiator contains two or more compounds. In this case, for example, by containing two or more compounds having different exposure sensitivity, the amount of the photoradical polymerization initiator (B) can be reduced while maintaining good exposure sensitivity, so that outgassing from the cured product can be further suppressed.

[0104] The oxime ester compound having photobleachability contains, for example, at least one of the compound represented by the following formula (401) and the compound represented by the following formula (402). Among these, the compound represented by formula (402) has particularly high sensitivity, and therefore is particularly likely to enhance the photocurability of composition (X), and therefore is likely to realize ultraviolet curability of composition (X) in the air.

[0105] [ka]

[0106] [ka]

[0107] The acylphosphine oxide compound contains, for example, at least one selected from the group consisting of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)diphenylphosphine oxide.

[0108] The photoradical polymerization initiator (B1) may contain a sensitizer as a part of the photoradical polymerization initiator (B1). The sensitizer can promote the radical generation reaction of the photoradical polymerization initiator (B1) to improve the reactivity of the radical polymerization and improve the crosslink density. The sensitizer may contain at least one compound selected from the group consisting of, for example, 9,10-dibutoxyanthracene, 9-hydroxymethylanthracene, thioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxanthone, anthraquinone, 1,2-dihydroxyanthraquinone, 2-ethylanthraquinone, 1,4-diethoxynaphthalene, p-dimethylaminoacetophenone, p-diethylaminoacetophenone, p-dimethylaminobenzophenone, p-diethylaminobenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, p-dimethylaminobenzaldehyde, and p-diethylaminobenzaldehyde. Note that the components that the sensitizer may contain are not limited to those mentioned above.

[0109] The content of the sensitizer in the composition (X) is, for example, 0.1 to 5 parts by mass, preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the solid content of the composition (X). When the content of the sensitizer is within such a range, the composition (X) can be cured in air, and it is not necessary to cure the composition (X) in an inert atmosphere such as a nitrogen atmosphere.

[0110] The composition (X) may contain a polymerization accelerator in addition to the photoradical polymerization initiator (B1). The polymerization accelerator contains, for example, an amine compound such as ethyl p-dimethylaminobenzoate, 2-ethylhexyl p-dimethylaminobenzoate, methyl p-dimethylaminobenzoate, 2-dimethylaminoethyl benzoate, or butoxyethyl p-dimethylaminobenzoate. Note that the components that the polymerization accelerator can contain are not limited to those mentioned above.

[0111] The composition (X) may further contain a cationically polymerizable compound (W). In this case, the composition (X) may further contain a photocationic polymerization initiator (B2).

[0112] The composition (X) may further contain a moisture absorbent (C). When the composition (X) contains the moisture absorbent (C), the cured product of the composition (X) and the encapsulant 5 can have moisture absorption properties. Therefore, the encapsulant 5 can further prevent moisture from penetrating into the light emitting element 4 in the light emitting device 1. The average particle size of the moisture absorbent (C) is preferably 200 nm or less. In this case, the cured product can have high transparency.

[0113] The moisture absorbent (C) is preferably an inorganic particle having moisture absorbing properties, and preferably contains at least one component selected from the group consisting of, for example, zeolite particles, silica gel particles, calcium chloride particles, and titanium oxide nanotube particles. It is particularly preferable that the moisture absorbent (C) contains zeolite particles.

[0114] Zeolite particles having an average particle size of 200 nm or less can be produced, for example, by pulverizing general industrial zeolite. In producing the zeolite particles, the zeolite may be pulverized and then crystallized by hydrothermal synthesis or the like, in which case the zeolite particles can have particularly high hygroscopicity. Examples of the method for producing such zeolite particles are disclosed in JP 2016-69266 A, JP 2013-049602 A, and the like.

[0115] The zeolite particles preferably contain sodium ions. Therefore, the zeolite particles are preferably made of at least one selected from the group consisting of A-type zeolite, X-type zeolite, and Y-type zeolite. It is particularly preferable that the zeolite particles are made of 4A-type zeolite among A-type zeolites. In these cases, the zeolite particles have a crystal structure suitable for adsorbing moisture.

[0116] The pH of the zeolite particles is preferably 7 or more and 10 or less. When the pH of the zeolite particles is 7 or more, the crystals of the zeolite particles are less likely to be destroyed, and therefore a sealing material made from the composition (X) containing the zeolite particles can have particularly high moisture absorption. When the pH of the zeolite particles is 10 or less, the zeolite particles are less likely to hinder the curing of the composition (X) when it is cured. The pH of the zeolite particles is a value obtained by heating a dispersion obtained by adding 0.05 g of zeolite particles to 99.95 g of ion-exchanged water at 90° C. for 24 hours, and then measuring the pH of the supernatant of the dispersion with a pH meter. Examples of pH meter include a compact pH meter manufactured by Horiba, Ltd. <laquatwin>B-711 can be used.

[0117] The average particle size of the moisture absorbent (C) is preferably 10 nm or more and 200 nm or less. If the average particle size is 200 nm or less, the cured product can have particularly high transparency. If the average particle size is 10 nm or more, the moisture absorbent (C) can maintain good moisture absorption. Note that this average particle size is the median diameter calculated from the measurement results by dynamic light scattering method, that is, the cumulative 50% diameter (D50). Note that the Nanotrac Wave series from Microtrack Bell Co., Ltd. can be used as a measuring device.

[0118] The average particle size of the moisture absorbent (C) is preferably 150 nm or less, more preferably 100 nm or less, and particularly preferably 70 nm or less. The average particle size of the moisture absorbent (C) is preferably 20 nm or more, and more preferably 50 nm or more. In this case, the cured product can have particularly good transparency and moisture absorption.

[0119] It is also preferable that the cumulative 90% diameter (D90) of the moisture absorbent (C) is 100 nm or less. In this case, the cured product can have particularly high transparency.

[0120] When the composition (X) contains the moisture absorbent (C), the ratio of the moisture absorbent (C) to the total amount of the composition (X) is preferably 1% by mass or more and 20% by mass or less. If the ratio of the moisture absorbent (C) is 1% by mass or more, the cured product can have particularly high moisture absorption. If the ratio of the moisture absorbent (C) is 20% by mass or less, the viscosity of the composition (X) can be particularly reduced, and the composition (X) can have a sufficiently low viscosity to be applicable by the inkjet method. The ratio of the moisture absorbent (C) is more preferably 3% by mass or more, and particularly preferably 5% by mass or more. The ratio of the moisture absorbent (C) is more preferably 15% by mass or less, and particularly preferably 13% by mass or less.

[0121] The composition (X) may further contain an inorganic filler other than the moisture absorbent (C). In particular, the composition (X) preferably contains nano-sized high refractive index particles. Examples of high refractive index particles include zirconia particles. When the composition (X) contains high refractive index particles, the refractive index of the cured product can be increased while maintaining good transparency of the cured product. Therefore, when the cured product is applied to the encapsulant 5 in the light emitting device 1, the extraction efficiency of the light that passes through the encapsulant 5 and is emitted to the outside can be improved. The average particle size of the high refractive index particles is preferably within a range of 5 to 30 nm, and more preferably within a range of 10 to 20 nm.

[0122] The proportion of high refractive index particles in the composition (X) is appropriately set so that the cured product has the desired refractive index. In particular, it is preferable that the high refractive index particles are contained in the composition (X) so that the refractive index of the cured product falls within the range of 1.45 or more and less than 1.55. In this case, the light extraction efficiency of the light emitting device 1 is particularly improved.

[0123] When the composition (X) contains the moisture absorbent (C), the composition (X) preferably further contains a dispersant (D). In this case, the dispersant (D) can improve the dispersibility of the moisture absorbent (C) in the composition (X). Therefore, the composition (X) is less likely to suffer from the increase in viscosity and the decrease in storage stability caused by the moisture absorbent (C).

[0124] The dispersant (D) is a surfactant that can be adsorbed to particles. The dispersant (D) has an adsorption group (generally called an anchor) that can be adsorbed to particles, and a molecular skeleton (generally called a tail) that adheres to the particles by the adsorption of the adsorption group to the particles. The dispersant (D) contains at least one component selected from the group consisting of, for example, an acrylic dispersant whose tail is an acrylic molecular chain, a urethane dispersant whose tail is a urethane molecular chain, and a polyester dispersant whose tail is a polyester molecular chain. The adsorption group includes at least one of, for example, a basic polar functional group and an acidic polar functional group. The basic polar functional group includes at least one group selected from the group consisting of, for example, an amino group, an imino group, an amide group, an imide group, and a nitrogen-containing heterocyclic group. The acidic polar functional group includes at least one group selected from the group consisting of, for example, a carboxyl group and a phosphate group. The dispersant (D) may contain at least one compound selected from the group consisting of, for example, the Solsperse series manufactured by Nippon Louvre Resol Co., Ltd., the DISPERBYK series manufactured by BYK-Chemie Japan Co., Ltd., and the AJISPER series manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0125] When the composition (X) contains a moisture absorbent (C), the amount of the dispersant (D) relative to the moisture absorbent (C) is preferably 5 parts by mass or more and 60 parts by mass or less. When the amount of the dispersant (D) is 5 parts by mass or more, the function of the dispersant (D) can be effectively expressed, and when the amount is 60 parts by mass or less, free molecules of the dispersant (D) in the sealant 5 can be suppressed from impairing the adhesion between the sealant 5 and the member made of an inorganic material. In addition, the amount of the dispersant (D) is more preferably 15 parts by mass or more, more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less, and particularly preferably 30 parts by mass or less.

[0126] The method for producing the composition (X) will be described.

[0127] First, a mixture (X1) is prepared. The mixture (X1) contains at least the acrylic compound (Y) and the photopolymerization initiator (B) among the components of the composition (X). The mixture (X1) may contain only the acrylic compound (Y) and the photopolymerization initiator (B). The mixture (X1) may contain a part or all of the remaining components of the composition (X) in addition to the acrylic compound (Y) and the photopolymerization initiator (B). That is, the mixture (X1) may have the same composition as the composition (X) except that the mixture (X1) is not subjected to the deoxidation treatment described below.

[0128] It is preferable to subject the mixture (X1) to a deoxidizing treatment. This makes it easier to achieve a ratio of the composition (X) of 50 mg / L or less. The deoxidizing treatment is a treatment for removing oxygen from the mixture (X1) to reduce the oxygen content in the mixture (X1).

[0129] There is no particular restriction on the specific content of the deoxidation treatment. For example, the mixture (X1) can be deoxidized by exposing it to an atmosphere with an oxygen concentration lower than the air (hereinafter, low-oxygen atmosphere). In this case, the volume concentration of oxygen in the low-oxygen atmosphere is preferably 100 ppm or less. That is, it is preferable to expose the mixture (X1) to an atmosphere with a volume concentration of oxygen of 100 ppm or less. In this case, the proportion of dissolved oxygen in the composition (X) can be efficiently reduced. The volume concentration of oxygen in the low-oxygen atmosphere is more preferably 1% or less, and even more preferably 0.1% or less. The lower the volume concentration of oxygen in the low-oxygen atmosphere, the more preferable, and ideally 0 ppm. In the deoxidation treatment, the time for exposing the mixture (X1) to the low-oxygen atmosphere is preferably 1 hour or more. In this case, it is particularly easy to reduce the proportion of dissolved oxygen in the composition (X). This time is, for example, 1 hour or more and 72 hours or less.

[0130] The proportion of dissolved oxygen in composition (X) can also be reduced by reducing the dissolved gas in mixture (X1) using a vacuum degassing apparatus. Oxygen can also be removed from mixture (X1) by exposing mixture (X1) to a stream of inert gas such as nitrogen gas. Oxygen can also be removed from mixture (X1) by blowing inert gas into mixture (X1) to replace the oxygen in the mixture with the inert gas.

[0131] After the mixture (X1) is deoxidized, the remaining components of the composition (X) can be added to the mixture (X1) as necessary to prepare the composition (X). When the mixture (X1) contains all the components of the composition (X), the mixture (X1) is deoxidized to prepare the composition (X). The composition (X) is preferably placed in a sealed container to prevent the composition (X) from absorbing oxygen during the period from when the composition (X) is prepared until when it is used.

[0132] The structure of the light emitting device 1 will be described. The light emitting device 1 includes a light source and an optical component that transmits the light emitted by the light source. For example, the light emitting device 1 includes a light emitting element 4, and a sealant 5 and a passivation layer 6 that cover the light emitting element 4. In this case, the light emitting element 4 is the light source, the sealant 5 is the optical component, and the passivation layer 6 is an inorganic layer. The sealant 5 and the passivation layer 6 overlap each other.

[0133] The light-emitting element 4 includes, for example, a light-emitting diode. The light-emitting diode includes, for example, at least one of an organic EL element (organic light-emitting diode) and a micro light-emitting diode. When the light-emitting element 4 includes an organic light-emitting diode, the light-emitting device 1 including the light-emitting element 4 is, for example, an organic EL display. When the light-emitting element 4 includes a micro light-emitting diode, the light-emitting device 1 including the light-emitting element 4 is, for example, a micro LED display. Note that EL is an abbreviation for electroluminescence.

[0134] An example of the structure of the light emitting device 1 will be described with reference to Fig. 1. This light emitting device 1 is a top emission type. The light emitting device 1 includes a support substrate 2, a transparent substrate 3 that faces the support substrate 2 with a gap therebetween, a light emitting element 4 on the surface of the support substrate 2 that faces the transparent substrate 3, and a passivation layer 6 and a sealing material 5 that cover the light emitting element 4.

[0135] The support substrate 2 is made of, for example, but not limited to, a resin material. The transparent substrate 3 is made of a material having light-transmitting properties. The transparent substrate 3 is, for example, a glass substrate or a transparent resin substrate. The light-emitting element 4 includes, for example, a pair of electrodes 41, 43 and an organic light-emitting layer 42 between the electrodes 41, 43. The organic light-emitting layer 42 includes, for example, a hole injection layer 421, a hole transport layer 422, an organic light-emitting layer 423, and an electron transport layer 424, which are stacked in the above order.

[0136] The light emitting device 1 includes a plurality of light emitting elements 4, which form an array 9 (hereinafter referred to as element array 9) on a support substrate 2. The element array 9 also includes a partition 7. The partition 7 is located on the support substrate 2 and separates two adjacent light emitting elements 4. The partition 7 is produced, for example, by forming a photosensitive resin material using a photolithography method. The element array 9 also includes connection wiring 8 that electrically connects the electrodes 43 and the electron transport layers 424 of adjacent light emitting elements 4 to each other. The connection wiring 8 is provided on the partition 7.

[0137] The passivation layer 6 is preferably made of silicon nitride or silicon oxide, and is particularly preferably made of silicon nitride. In the example shown in FIG. 1, the passivation layer 6 includes a first passivation layer 61 and a second passivation layer 62. The first passivation layer 61 covers the element array 9 in a state of direct contact with the element array 9, thereby covering the light-emitting element 4. The second passivation layer 62 is disposed on the opposite side of the element array 9 with respect to the first passivation layer 61, and a gap is provided between the second passivation layer 62 and the first passivation layer 61. The sealant 5 is filled between the first passivation layer 61 and the second passivation layer 62. That is, the first passivation layer 61 is interposed between the light-emitting element 4 and the sealant 5 covering the light-emitting element 4.

[0138] Furthermore, a second sealing material 52 is filled between the second passivation layer 62 and the transparent substrate 3. The second sealing material 52 is made of, for example, a transparent resin material. The material of the second sealing material 52 is not particularly limited. The material of the second sealing material 52 may be the same as or different from the sealing material 5.

[0139] A method for producing the encapsulant 5 using the composition (X) and a method for producing the light emitting device 1 will be described.

[0140] In this embodiment, it is preferable to form the composition (X) by the inkjet method, and then irradiate the composition (X) with ultraviolet light to harden the composition (X), thereby producing the encapsulant 5. In this embodiment, the composition (X) can be applied and formed by the inkjet method. As described above, in this embodiment, the oxygen ratio of the composition (X) is 75 mass % or less, and therefore defects are unlikely to occur when the composition (X) is formed by the inkjet method.

[0141] When applying composition (X) by the inkjet method, if composition (X) has a sufficiently low viscosity at room temperature, for example, if the viscosity at 25°C is 20 mPa s or less, particularly 15 mPa s or less, composition (X) can be molded by applying it by the inkjet method without heating.

[0142] When composition (X) has the property of being reduced in viscosity by heating, composition (X) may be heated and then coated and molded by an inkjet method. When composition (X) has a viscosity of 20 mPa·s or less, particularly 15 mPa·s or less at 40°C, composition (X) can be reduced in viscosity by simply heating it slightly, and this reduced-viscosity composition (X) can be discharged by an inkjet method. The heating temperature for composition (X) is, for example, 20°C or higher and 50°C or lower.

[0143] More specifically, for example, first, a support substrate 2 is prepared. On one surface of the support substrate 2, partition walls 7 are fabricated by photolithography using, for example, a photosensitive resin material. Next, a plurality of light-emitting elements 4 are provided on one surface of the support substrate 2. The light-emitting elements 4 can be fabricated by an appropriate method such as a vapor deposition method or a coating method. In particular, it is preferable to fabricate the light-emitting elements 4 by a coating method such as an inkjet method. In this way, an element array 9 is fabricated on the support substrate 2.

[0144] Next, a first passivation layer 61 is provided on the element array 9. The first passivation layer 61 can be formed by a deposition method such as a plasma CVD method.

[0145] Next, the composition (X) is formed on the first passivation layer 61 by, for example, an inkjet method to form a coating film. If the inkjet method is used for both the formation of the light emitting element 4 and the application of the composition (X), the manufacturing efficiency of the light emitting device 1 can be particularly improved. Next, the coating film of the composition (X) is cured by irradiating it with ultraviolet light to form the encapsulant 5. The thickness of the encapsulant 5 is, for example, 5 μm or more and 50 μm or less.

[0146] When irradiating the composition (X) with ultraviolet rays, the composition (X) may be irradiated with ultraviolet rays under an atmosphere containing oxygen, such as an air atmosphere, or may be irradiated with ultraviolet rays under an inert atmosphere, such as a nitrogen atmosphere. In this embodiment, as described above, the oxygen ratio of the composition (X) is 75 mass% or less, so that oxygen inhibition is unlikely to occur, even if the photopolymerizable compound (A) contains the radical polymerizable compound (A1). Therefore, even if the composition (X) is irradiated with ultraviolet rays under an atmosphere containing oxygen, the composition (X) is easily cured.

[0147] Next, a second passivation layer 62 is provided on the sealing material 5. The second passivation layer 62 can be formed by a deposition method such as a plasma CVD method.

[0148] Next, an ultraviolet-curable resin material is provided on one surface of the support substrate 2 so as to cover the second passivation layer 62, and then the transparent substrate 3 is placed on the resin material. The transparent substrate 3 is, for example, a glass substrate or a transparent resin substrate.

[0149] Next, ultraviolet light is irradiated from the outside toward the transparent substrate 3. The ultraviolet light passes through the transparent substrate 3 and reaches the ultraviolet-curable resin material. As a result, the ultraviolet-curable resin material is cured, and the second sealing material 52 is produced.

[0150] In this embodiment, as described above, it is possible to make it difficult for a decrease in luminous efficiency caused by the passivation layer 6 and the sealing material 5 in the light emitting device 1 to occur.

[0151] The thickness of the sealing material 5 is, for example, 1 μm or more and 20 μm or less. The thickness of the sealing material 5 may be 15 μm or less. In this case, by thinning the sealing material 5, the light emitting device 1 can be thinned, and it is also possible to obtain a flexible light emitting device 1. Furthermore, even if the thickness of the sealing material 5 is 10 μm or less, in this embodiment, a decrease in luminous efficiency caused by the passivation layer 6 and the sealing material 5 in the light emitting device 1 is unlikely to occur. It is more preferable that the thickness of the sealing material 5 be 8 μm or less. In order to effectively prevent moisture from entering the light emitting element 4 by the sealing material 5, the thickness of the sealing material 5 is preferably 3 μm or more, and more preferably 5 μm or more.

[0152] The thickness of the passivation layer 6 overlapping the sealing material 5 is, for example, 0.1 μm or more and 2 μm or less. When the passivation layer 6 includes the first passivation layer 61 and the second passivation layer 62 as described above, it is preferable that the thickness of each of the first passivation layer 61 and the second passivation layer 62 is 0.1 μm or more and 2 μm or less.

[0153] The use of the composition (X) according to this embodiment is not limited to the preparation of the encapsulant 5 for the light-emitting element 4. The composition (X) can be used to prepare various optical components that transmit light emitted by a light source. For example, the optical component may be a color resist. That is, for example, a phosphor may be contained in the composition (X), and a color resist in a color filter may be prepared from this composition (X). This color filter can be provided in a display device such as an organic EL display or a micro LED display, which is a light-emitting device. EXAMPLES

[0154] 1. Preparation of the Composition Compositions of the examples and comparative examples were prepared by mixing the components shown in Tables 1 to 3 below.

[0155] The details of the components shown in Tables 1 to 3 are as follows. The viscosity of each of the components was measured using a rheometer (Anton Paar Japan, model number DHR-2) at a temperature of 25°C and a shear rate of 1000 s -1 The values ​​were measured under the following conditions. -ACMO: Acryloylmorpholine, boiling point 265°C, viscosity 12 mPa·s, glass transition temperature 145°C. -Morpholin-4-yl acrylate: boiling point 290°C, viscosity 16 mPa·s, glass transition temperature 115°C. -N-vinyl-ε-caprolactam: Manufactured by BASF, boiling point 245°C, viscosity 6 mPa·s, glass transition temperature 90°C. -Isobornyl acrylate: boiling point 245℃, viscosity 8mPa·s, glass transition temperature 97℃. -Phenoxyethyl acrylate: boiling point 290℃, viscosity 13mPa·s, glass transition temperature 2℃. - FAM201: Fujifilm, a polyfunctional acrylic compound represented by formula (51), boiling point of 300°C or higher, solid at room temperature. - FAM301: Fujifilm, a polyfunctional acrylic compound represented by formula (52), boiling point of 300°C or higher, solid at room temperature. - FAM401: Fujifilm, a polyfunctional acrylic compound represented by formula (53), boiling point of 300°C or higher, solid at room temperature. - FAM402: Fujifilm, a polyfunctional acrylic compound represented by formula (54), boiling point of 300°C or higher, solid at room temperature. -3G: Triethylene glycol dimethacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd., boiling point 290, viscosity 8 mPa·s. -BD: 1,4-butanediol dimethacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd., boiling point 280, viscosity 7 mPa·s. -SR351S: Trimethylolpropane triacrylate, boiling point above 300°C, viscosity 106 mPa·s. -Irgacure TPO: BASF, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0156] 2.Evaluation Test The following evaluation tests were carried out on the examples and comparative examples. The results are shown in Tables 1 to 3.

[0157] (1) Viscosity at 25℃ The viscosity of the composition was measured using a rheometer (Anton Paar Japan, model number DHR-2) at a temperature of 25 °C and a shear rate of 1000 s -1 The measurements were performed under the following conditions.

[0158] (2) 40℃ viscosity The viscosity of the composition was measured using a rheometer (Anton Paar Japan, model number DHR-2) at a temperature of 40 °C and a shear rate of 1000 s -1 The measurements were performed under the following conditions.

[0159] (3) UV curing in air (touch test) The composition was applied to prepare a coating film. The coating film was irradiated with ultraviolet light at an intensity of 5 W / cm using a Unijet E075IIHD (peak wavelength 395 nm) manufactured by Ushio Inc. in an air atmosphere. 2 , and the cumulative light intensity is 1500mJ / cm 2 The coating was photocured to produce a film with a thickness of 10 μm by irradiating the coating under the conditions of ultraviolet irradiation intensity of 0.5 W / cm. 2 , and the cumulative light intensity is 1500mJ / cm 2 When the temperature was changed to 100° C., a film was prepared in the same manner.

[0160] The film was subjected to a touch test with a light intensity of 5W / cm 2 and 0.5W / cm 2 When no tack was observed in any of the cases, it was marked "A"; when the irradiation intensity was 5 W / cm 2 In the case of 0.5W / cm, tack was observed, but 2 In the case of , when no tack was observed, it was marked as "B" and the irradiation intensity was 5W / cm 2 and 0.5W / cm 2 When tack was observed in any of the above cases, the sample was rated as "C."

[0161] (4) UV curing in air (pencil strength) The composition was applied to prepare a coating film. The coating film was irradiated with ultraviolet light at an intensity of 5 W / cm using a Unijet E075IIHD (peak wavelength 395 nm) manufactured by Ushio Inc. in an air atmosphere. 2 , and the cumulative light intensity is 1500mJ / cm 2 The coating was photocured under the conditions of 10 μm thick. The pencil hardness of this film was measured according to the scratch hardness (pencil method) of JIS K5600-5-4:1999.

[0162] (5) Glass transition temperature The composition was applied to prepare a coating film, and the coating film was then irradiated with ultraviolet light at 5 W / cm using a Unijet E075IIHD (peak wavelength 395 nm) manufactured by Ushio Electric Co., Ltd. in an air atmosphere. 2 , and the cumulative light intensity is 1500mJ / cm 2 The coating was photocured by irradiating under the conditions of , and a film with a thickness of 200 μm was produced. The glass transition temperature of a sample cut out from this film was measured using a viscoelasticity measuring device (manufactured by Hitachi High-Tech Science Corporation, model number DMA7100).

[0163] (6) Adhesion The composition was applied onto a piece of quartz glass (dimensions: 50 mm × 25 mm × 1 mm) to produce a coating film with a thickness of 50 μm. Another piece of quartz glass was placed on top of this coating film so that the dimensions of the area where the two pieces contacted each other were 12.5 mm × 25 mm. The composition was exposed to ultraviolet light at an intensity of 5 W / cm2 using a Unijet E075IIHD (peak wavelength: 395 nm) manufactured by Ushio Electric Co., Ltd. in an air atmosphere. 2 , and the cumulative light intensity is 3000mJ / cm 2 The coating was then irradiated under the conditions of

[0164] Next, the adhesive strength between the two quartz glass pieces was measured by a tensile shear test (tensile speed 5 mm / min) in accordance with JIS K 6850. The results were evaluated according to the following criteria. A: 15MPa or more. B: Less than 15MPa.

[0165] (7) Outgassing evaluation The outgassing when the cured product of the composition was heated was sampled by the headspace method and measured by gas chromatography. In detail, 100 mg of the composition was placed in a headspace vial with a volume of 22 mL. Next, the composition was irradiated with ultraviolet light at an intensity of 5 W / cm using a Unijet E075IIHD (peak wavelength 395 nm) manufactured by Ushio Inc. under an atmospheric condition. 2 , and the cumulative light intensity is 1500mJ / cm 2 The composition was cured by irradiating the composition under the conditions of 1000 nm to 1000 nm, and the vial was then sealed. The composition was then heated at 80°C for 30 minutes, and the gas phase in the vial was then introduced into a gas chromatograph for analysis. The concentration of outgassing from the composition was determined based on the peak area of ​​the resulting gas chromatogram. The concentration of outgassing is the volume fraction of outgassing in the gas phase of the vial relative to the volume of the vial (22 mL).

[0166] The outgas concentrations were determined using toluene as a reference substance. Specifically, two reference samples with toluene concentrations of 1000 ppm and 100 ppm were prepared by volatilizing toluene in a vial. Each reference sample was introduced into a gas chromatograph for analysis. From the peak areas of the two chromatograms obtained in this way, the relationship between the peak area and the concentration was determined, and the above outgas concentrations were determined based on these results.

[0167] As a result, outgassing concentrations (volume fraction) of 60 ppm or less were rated as "A," those between 60 ppm and 100 ppm or less were rated as "B," those between 100 ppm and 200 ppm or less were rated as "C," and those over 200 ppm were rated as "D."

[0168] (8) Inkjet compatibility The composition was placed in the cartridge of an inkjet printer (Fujifilm, Model DMP2831), and droplets of the composition were ejected from the nozzle of the inkjet printer at a temperature of 30° C. and a frequency of 1 kHz. The droplets were observed with a high-speed camera, and were rated as "A" when neither mist nor satellites were observed, and "B" when at least one of mist or satellites was observed.

[0169] (9) Storage stability The composition was left to stand for 2 months at 60°C in a nitrogen atmosphere. The viscosity change rate Rμ was calculated from the viscosity μ0 of the composition before the test and the viscosity μ1 of the composition after the test using the following formula (M1). A rate of change of less than 10% was rated as "A", a rate of change of 10% or more but less than 20% was rated as "B", and a rate of change of 20% or more was rated as "C". Rμ={(μ1-μ0) / μ0}×100(%) …(M1)

[0170] [Table 1]

[0171] [Table 2]

[0172] [Table 3] < / laquatwin>

Claims

1. The present invention comprises an acrylic compound (Y) including a polyfunctional acrylic compound (Y1) having a nitrogen atom and a polyfunctional acrylic compound (Y21) other than the polyfunctional acrylic compound (Y1) having two or more radically polymerizable functional groups including a (meth)acryloyl group in one molecule, and a photopolymerization initiator (B), the polyfunctional acrylic compound (Y1) contains a polyfunctional acrylamide compound (Y11) having two or more (meth)acrylamide groups in one molecule, The polyfunctional acrylamide compound (Y11) contains at least one selected from the group consisting of a compound represented by the following formula (51), a compound represented by the following formula (52), a compound represented by the following formula (53), and a compound represented by the following formula (54), 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 The proportion of the polyfunctional acrylic compound (Y1) relative to the total amount of the acrylic compound (Y) is 3% by mass or more and 40% by mass or less, The polyfunctional acrylic compound (Y21) contains a compound (Y211) having a structure represented by the following formula (200): CH 2 =CR 1 -COO-(R 3 -O) n -CO-CR 2 =CH 2 ...(200) In formula (200), each of R 1 and R 2 is a hydrogen atom or a methyl group, n is an integer of 1 or more, R 3 is an alkylene group having 1 or more carbon atoms, and when n is 2 or more, multiple R 3 s in one molecule may be the same or different from each other; the amount of the polyfunctional acrylic compound (Y21) is 20 parts by mass or more relative to 92 parts by mass of the total acrylic compound (Y), and the ratio of the polyfunctional acrylic compound (Y21) to the total acrylic compound (Y) is 70% by mass or less, the total ratio of the polyfunctional acrylamide compound (Y1) and the polyfunctional acrylic compound (Y21) to the entire acrylic compound (Y) is 50 mass% or more; UV curable resin composition.

2. UV curable in air. The ultraviolet-curable resin composition according to claim 1 .

3. To produce an optical component that transmits light emitted by a light source, The ultraviolet-curable resin composition according to claim 1 or 2.

4. Formed by the inkjet method, The ultraviolet-curable resin composition according to claim 1 .

5. Contains no solvent or has a solvent content of 1% by mass or less; The ultraviolet-curable resin composition according to claim 1 .

6. At least one of the viscosity at 25°C and the viscosity at 40°C is 30 mPa·s or less; The ultraviolet-curable resin composition according to claim 1 .

7. The glass transition temperature of the cured product is 80° C. or higher. The ultraviolet-curable resin composition according to claim 1 .

8. The rate of outgassing generated when the cured product is heated at 80°C for 30 minutes is 60 ppm or less. The ultraviolet-curable resin composition according to claim 1 .

9. The polyfunctional acrylic compound (Y1) contains a compound having at least one amide group in one molecule. The ultraviolet-curable resin composition according to claim 1 .

10. Further containing a monofunctional acrylic compound (Y222) having a nitrogen atom, The ultraviolet-curable resin composition according to claim 1 .

11. The photopolymerization initiator (B) contains a photopolymerization initiator having photobleaching properties. The ultraviolet-curable resin composition according to claim 1 .

12. A cured product of the ultraviolet-curable resin composition according to any one of claims 1 to 11. Optical components.

13. A method for producing an optical component, comprising: molding the ultraviolet-curable resin composition according to claim 1 by an inkjet method; and then curing the ultraviolet-curable resin composition by irradiating it with ultraviolet light.

14. The ultraviolet-curable resin composition is irradiated with ultraviolet light in an atmospheric environment. The method for producing the optical component according to claim 13 .

15. A light source and an optical component that transmits light emitted by the light source, the optical component including a cured product of the ultraviolet-curable resin composition according to any one of claims 1 to 11. Light emitting device.

16. A method for manufacturing a light emitting device including a light source and an optical component that transmits light emitted by the light source, comprising the steps of: The optical component is manufactured by a method according to claim 13 or 14. A method for manufacturing a light emitting device.

Citation Information

Patent Citations

  • Photocurable composition for imprint, article having fine pattern on surface thereof and method for producing the same

    JP2018127522A

  • Photocurable composition and display

    JP2018127597A

  • Curable resin composition, cured product and printed wiring board

    JP2019179222A

  • Radical polymerization initiator, composition containing same, cured product of composition, production method for cured product, and compound

    WO2019160079A1