Bearing rings and shafts

By employing a steel composition with a surface layer having higher nitrogen and carbon content and controlled austenite levels, the bearing ring and shaft achieve enhanced surface fatigue resistance, addressing the limitations of prior technologies.

JP7555294B2Active Publication Date: 2024-09-24NTN CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021050276
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-24
Publication Date
2024-09-24
Estimated Expiration
2041-03-24

AI Technical Summary

Technical Problem

Existing bearing rings and shafts, such as those described in Patent Documents 1 and 2, have limitations in surface fatigue resistance.

Method used

The bearing ring and shaft are made of steel with a surface layer having higher nitrogen and carbon content than the core, specific hardness distributions, and controlled amounts of retained austenite to enhance surface fatigue resistance.

Benefits of technology

The solution significantly improves surface fatigue resistance, reducing manufacturing costs and preventing fatigue failure and deformation, as demonstrated by rolling fatigue tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555294000007
    Figure 0007555294000007
  • Figure 0007555294000006
    Figure 0007555294000006
  • Figure 0007555294000003
    Figure 0007555294000003
Patent Text Reader

Abstract

To provide a bearing ring which can improve a surface fatigue resistance property.SOLUTION: A bearing ring has a surface which contacts with a roller whose diameter is equal to or larger than 1.5 mm, and equal to or smaller than 4.0 mm, and whose value obtained by dividing its length by a diameter is equal to or 4, and equal to or smaller than 10, and is formed of steel. The bearing ring comprises a surface layer part formed on the surface, and a core part existing inside the surface layer part. A content of nitrogen in the steel existing on the surface is larger than a content of nitrogen in the steel existing in the core part. In a first position in which a distance from the surface becomes 0.05 mm, and in a second position in which a distance from the surface becomes 0.20 mm, the hardness of the steel is equal to or higher than 720Hv. A value obtained by subtracting the hardness of the steel in the second position from the hardness of the steel in the first position is equal to or lower than 30Hv.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a bearing ring and a shaft. [Background technology]

[0002] Japanese Patent No. 4423754 (Patent Document 1) describes a raceway ring. In the raceway ring described in Patent Document 1, the surface (raceway surface) is subjected to carbo-nitriding and quenching. As a result, the raceway ring described in Patent Document 1 has improved surface fatigue resistance.

[0003] Japanese Patent Laid-Open Publication No. 2010-1521 (Patent Document 2) describes a shaft. The shaft described in Patent Document 2 is a pinion shaft for a planetary gear mechanism. In the shaft described in Patent Document 2, the surface (raceway surface) is subjected to carbo-nitriding and quenching. As a result, the surface fatigue resistance of the shaft described in Patent Document 2 is improved.

[0004] Additionally, a method described in Japanese Patent No. 4800444 (Patent Document 3) is known as a heat treatment for improving the surface fatigue resistance of gears and bearing parts. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4423754 [Patent Document 2] JP 2010-1521 A [Patent Document 3] Patent No. 4800444 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the race described in Patent Document 1 and the shaft described in Patent Document 2 leave room for improvement in terms of surface fatigue resistance.

[0007] The present invention has been made in view of the above-mentioned problems in the prior art. More specifically, the present invention provides a bearing ring and a shaft capable of improving surface fatigue resistance characteristics. [Means for solving the problem]

[0008] The raceway ring according to the first aspect of the present invention has a surface that contacts a roller and has a diameter of 1.5 mm to 4.0 mm and a length divided by the diameter of 4 to 10, and is made of steel. The raceway ring has a surface layer on the surface and a core layer inside the surface layer. The nitrogen content of the steel in the surface layer is higher than the nitrogen content of the steel in the core. At a first position that is 0.05 mm away from the surface and at a second position that is 0.20 mm away from the surface, the hardness of the steel is 720 Hv or more. The hardness of the steel at the first position minus the hardness of the steel at the second position is 30 Hv or less.

[0009] In the race according to the first aspect of the present invention, the carbon content and the nitrogen content in the steel at the surface may be 0.6 to 0.9 weight percent and 0.3 to 0.8 weight percent, respectively. The carbon content and the nitrogen content in the steel at the surface layer may be higher than the nitrogen content and the carbon content in the steel at the core, respectively. The carbon content in the steel at the core may be 0.15 to 0.4 weight percent. The steel may contain chromium, manganese, silicon, and molybdenum. The chromium content in the steel may be 0.5 to 3.0 weight percent. The sum of the manganese content, the silicon content, and the molybdenum content in the steel may be 1.0 to 3.0 weight percent. The distance between the surface and a third position where the hardness of the steel is 653 Hv may be 0.25 to 0.60 mm.

[0010] In the bearing ring according to the first aspect of the present invention, the amount of retained austenite in the steel in the core may be 3 volume percent or less.

[0011] In the bearing ring according to the first aspect of the present invention, the amount of retained austenite in the steel on the surface may be 25 volume percent or more and 40 volume percent or less.

[0012] A shaft according to a second aspect of the present invention has a surface and is made of steel. The shaft comprises a surface layer on the surface and a core inside the surface layer. The diameter of the shaft is 6 mm or more and 30 mm or less. The nitrogen content of the steel in the surface layer is higher than the nitrogen content of the steel in the core. At a first position 0.05 mm away from the surface and at a second position 0.20 mm away from the surface, the hardness of the steel is 720 Hv or more. The value obtained by subtracting the hardness of the steel at the second position from the hardness of the steel at the first position is 30 Hv or less.

[0013] The carbon content and nitrogen content in the steel at the surface are 0.6 to 0.9 mass percent and 0.3 to 0.8 mass percent, respectively. The carbon content in the steel at the core is 0.15 to 0.4 mass percent. The steel contains chromium, manganese, silicon, and molybdenum. The chromium content in the steel is 0.5 to 3.0 mass percent. The sum of the manganese, silicon, and molybdenum contents in the steel is 1.0 to 3.0 mass percent.

[0014] In the shaft according to the second aspect of the present invention, the amount of retained austenite in the steel in the core may be 3 volume percent or less.

[0015] In the shaft according to the second aspect of the present invention, the amount of retained austenite in the steel on the surface may be 25 volume percent or more and 40 volume percent or less. The shaft according to the second aspect of the present invention may be for a planetary reducer. Effect of the Invention

[0016] According to the bearing ring according to the first aspect of the present invention and the shaft according to the second aspect of the present invention, the surface fatigue resistance can be improved. [Brief description of the drawings]

[0017] [Figure 1] 1 is a cross-sectional view of a rolling bearing 100. FIG. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of the bearing ring 10. [Diagram 3] 2 is an enlarged cross-sectional view of the shaft 40. FIG. [Figure 4] 3A to 3C are process diagrams showing a manufacturing method of the bearing ring 10. [Diagram 5] 1 is a graph showing the relationship between the distance from an outer circumferential surface 40a and the hardness of the steel in Samples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings. In the following drawings, the same or corresponding parts are designated by the same reference numerals, and redundant description will not be repeated.

[0019] A rolling bearing according to an embodiment (hereinafter referred to as "rolling bearing 100") will be described. The rolling bearing 100 is a needle roller bearing. The rolling bearing 100 is a rolling bearing used, for example, in an automobile transmission (for example, a planetary reducer). However, the rolling bearing 100 can be used for purposes other than automobile transmissions.

[0020] (Configuration of rolling bearing according to embodiment) Fig. 1 is a cross-sectional view of a rolling bearing 100. As shown in Fig. 1, the rolling bearing 100 has a race 10, a plurality of rollers 20, and a cage 30. The rolling bearing 100 is attached to a shaft 40.

[0021] The raceway 10 is ring-shaped. The central axis of the raceway 10 is defined as the central axis A. The direction of the central axis A is defined as the axial direction. The direction passing through the central axis A and perpendicular to the central axis A is defined as the radial direction. The direction along the circumference centered on the central axis A is defined as the circumferential direction.

[0022] The raceway 10 has an end face 10a, an end face 10b, an inner peripheral surface 10c, and an outer peripheral surface 10d. The end face 10a, the end face 10b, the inner peripheral surface 10c, and the outer peripheral surface 10d may be collectively referred to as the surface of the raceway 10.

[0023] The end face 10a and the end face 10b constitute axial end faces of the bearing ring 10. The end face 10b is the face opposite to the end face 10a in the axial direction.

[0024] The inner peripheral surface 10c extends in the circumferential direction. The inner peripheral surface 10c faces the central axis A. One axial end of the inner peripheral surface 10c is continuous with the end face 10a. The other axial end of the inner peripheral surface 10c is continuous with the end face 10b. The inner peripheral surface 10c is the raceway surface of the bearing ring 10. That is, the bearing ring 10 contacts the rollers 20 at the inner peripheral surface 10c.

[0025] The outer peripheral surface 10d extends in the circumferential direction. The outer peripheral surface 10d faces the opposite side to the central axis A. In other words, the outer peripheral surface 10d is the opposite surface to the inner peripheral surface 10c in the radial direction. One end of the outer peripheral surface 10d in the axial direction is continuous with the end surface 10a. The other end of the outer peripheral surface 10d in the axial direction is continuous with the end surface 10b.

[0026] The race 10 is made of steel. More specifically, the race 10 is made of hardened and tempered steel. The steel that makes up the race 10 contains chromium, manganese, silicon, and molybdenum.

[0027] The chromium content in the steel constituting the raceway ring 10 is preferably 0.5 mass percent or more from the viewpoints of improving hardenability and improving surface fatigue resistance due to carbide precipitation, and the chromium content in the steel constituting the raceway ring 10 is preferably 3.0 mass percent or less from the viewpoints of reducing steel costs.

[0028] The total content of manganese, silicon, and molybdenum in the steel constituting the raceway 10 is preferably 1.0 mass percent or more from the viewpoint of improving hardenability and heat resistance. The total content of manganese, silicon, and molybdenum in the steel constituting the raceway 10 is preferably 3.0 mass percent or less from the viewpoint of reducing steel costs.

[0029] Fig. 2 is an enlarged cross-sectional view of the raceway 10. As shown in Fig. 2, the raceway 10 has a surface layer portion 11 and a core portion 12. The surface layer portion 11 is a portion of the raceway 10 that is on the surface of the raceway 10. The core portion 12 is a portion of the raceway 10 that is on the inside of the surface layer portion 11. The nitrogen content and carbon content in the steel in the surface layer portion 11 are greater than the nitrogen content and carbon content in the steel in the core portion 12, respectively. That is, the surface of the raceway 10 has been subjected to carbo-nitriding treatment.

[0030] The nitrogen and carbon contents in the steel in the surface layer 11 decrease with increasing distance from the surface of the raceway 10. The nitrogen and carbon contents in the steel in the core portion 12 are constant regardless of position. Therefore, the nitrogen and carbon contents in the steel are measured sequentially from the surface of the raceway 10 along the depth direction (direction perpendicular to the surface of the raceway 10), and the position where the measured nitrogen and carbon contents become constant is the boundary between the surface layer 11 and the core portion 12.

[0031] When the surface of the raceway 10 is not carburized and only nitriding is performed, the carbon content in the steel in the surface layer 11 and the carbon content in the steel in the core portion 12 are the same. Therefore, in this case, the nitrogen content in the steel is measured sequentially from the surface of the raceway 10 along the depth direction, and the position where the measured nitrogen content becomes constant is the boundary between the surface layer 11 and the core portion 12.

[0032] The nitrogen content in the steel on the surface of the race 10 is preferably 0.3 mass percent or more from the viewpoints of improving temper softening resistance and improving surface fatigue resistance by increasing the amount of retained austenite. The nitrogen content in the steel on the surface of the race 10 is preferably 0.8 mass percent or less from the viewpoints of suppressing a decrease in hardness due to an excessive amount of retained austenite.

[0033] The carbon content in the steel on the surface of the race 10 is preferably 0.6 mass percent or more and 0.9 mass percent or less. The carbon content in the steel in the core portion 12 (i.e., the carbon content in the steel before the carburizing treatment) is preferably 0.15 mass percent or more and 0.40 mass percent or less from the viewpoints of improving workability and ensuring strength by reducing the amount of retained austenite.

[0034] The balance of the steel constituting the raceway 10 is iron and unavoidable impurities. The content of each component in the steel constituting the raceway 10 is measured using an EPMA (Electron Probe Micro Analyzer).

[0035] The raceway 10 is preferably formed from the first, second or third steel material having the composition shown in Table 1. The first steel material corresponds to SCM420, a chromium molybdenum steel defined in the JIS standard (JIS G 4053:2016). The raceway 10 may be formed from the fourth steel material having the composition shown in Table 1. The third steel material corresponds to SUJ2, a high carbon chromium bearing steel defined in the JIS standard (JIS G 4805:2018).

[0036] [Table 1]

[0037] A position 0.05 mm away from the surface of the raceway 10 is designated as position P1. A position 0.20 mm away from the surface of the raceway 10 is designated as position P2. The hardness of the steel at positions P1 and P2 is 720 Hv or more. The hardness of the steel at position P1 is greater than the hardness of the steel at position P2. It is preferable that the value obtained by subtracting the hardness of the steel at position P2 from the hardness of the steel at position P1 is 30 Hv or less.

[0038] The position where the hardness of the steel is 653 Hv is designated as position P3. Position P3 is farther from the surface of the raceway 10 than position P2. More specifically, the distance between the surface of the raceway 10 and position P3 is preferably 0.25 mm or more and 0.6 mm or less.

[0039] The hardness of the steel constituting the raceway ring 10 is measured by the Vickers hardness test method defined in the JIS standard (JIS Z 2245:2009).

[0040] The amount of retained austenite in the steel on the surface of the race 10 is preferably 25 volume percent or more and 40 volume percent or less. The amount of retained austenite in the steel on the surface of the race 10 is more preferably 30 volume percent or more and 35 volume percent or less. The amount of retained austenite in the steel in the core 12 is preferably 3 volume percent or less.

[0041] The amount of retained austenite in steel is measured by X-ray diffraction. More specifically, the amount of retained austenite in steel is measured by comparing the integrated intensity of the X-ray diffraction peak of austenite in steel with the integrated intensity of the X-ray diffraction peak of other phases in the steel.

[0042] As shown in Fig. 1, roller 20 is a needle roller. Roller 20 extends in the axial direction. Roller 20 has end face 20a, end face 20b, and outer circumferential surface 20c. End face 20a and end face 20b are end faces in the axial direction. End face 20b is the opposite face to end face 20a in the axial direction.

[0043] The outer peripheral surface 20c extends in the circumferential direction. One axial end of the outer peripheral surface 20c is continuous with the end face 20a. The other axial end of the outer peripheral surface 20c is continuous with the end face 20b. The rollers 20 contact the inner peripheral surface 10c at the outer peripheral surface 20c. A plurality of rollers 20 are arranged in the circumferential direction. The rollers 20 contact the shaft 40 at the outer peripheral surface 20c. As a result, the rolling bearing 100 supports the shaft 40 rotatably around the central axis A.

[0044] The diameter of roller 20 is 1.5 mm or more and 4.0 mm or less. The value obtained by dividing the length of roller 20 by the diameter of roller 20 is 4 or more and 10 or less. The length of roller 20 is the length in the axial direction, i.e., the distance between end face 20a and end face 20b.

[0045] The rollers 20 are made of, for example, steel. The steel constituting the rollers 20 may be the same as the steel constituting the raceway 10, or may be different from the steel constituting the raceway 10. The cage 30 is disposed between the raceway 10 and the shaft 40. The cage 30 holds a plurality of rollers 20. This maintains the distance between two adjacent rollers 20 in the circumferential direction within a certain range.

[0046] The shaft 40 extends in the axial direction. The diameter of the shaft 40 is equal to or greater than 6 mm and equal to or less than 30 mm. The shaft 40 has an outer circumferential surface 40a. The outer circumferential surface 40a extends in the circumferential direction. The shaft 40 contacts the rollers 20 at the outer circumferential surface 40a. In other words, the outer circumferential surface 40a is the raceway surface of the shaft 40. The shaft 40 is made of hardened and tempered steel.

[0047] 3 is an enlarged cross-sectional view of shaft 40. Shaft 40 has a surface layer portion 41 and a core portion 42. Surface layer portion 41 is a portion of shaft 40 on the outer circumferential surface 40a. Core portion 42 is a portion of shaft 40 on the inside of surface layer portion 41. The nitrogen content and carbon content in the steel in surface layer portion 41 are greater than the nitrogen content and carbon content in the steel in core portion 42, respectively. That is, the outer circumferential surface 40a has been subjected to carbo-nitriding treatment.

[0048] However, the outer peripheral surface 40a does not need to be carburized. In this case, the carbon content in the steel in the surface layer 41 is the same as the carbon content in the steel in the core .

[0049] The steel constituting the shaft 40 contains chromium, manganese, silicon, and molybdenum. The chromium content in the steel constituting the shaft 40 is preferably 0.5 mass percent or more and 3.0 mass percent or less. The total of the manganese content, silicon content, and molybdenum content in the steel constituting the shaft 40 is preferably 1.0 mass percent or more and 3.0 mass percent or less.

[0050] The carbon content in the steel at the outer circumferential surface 40a is preferably 0.6 mass percent or more and 0.9 mass percent or less. The carbon content in the steel at the core 42 is preferably 0.15 mass percent or more and 0.40 mass percent or less. The nitrogen content in the steel at the outer circumferential surface 40a is preferably 0.3 mass percent or more and 0.8 mass percent or less. The remainder of the steel constituting the shaft 40 is iron and unavoidable impurities.

[0051] The shaft 40 is preferably made of the first steel material, the second steel material, or the third steel material. The shaft 40 may be made of the fourth steel material.

[0052] A position 0.05 mm away from the outer peripheral surface 40a is designated as position P4. A position 0.20 mm away from the outer peripheral surface 40a is designated as position P5. The hardness of the steel at positions P4 and P5 is 720 Hv or more. The hardness of the steel at position P4 is greater than the hardness of the steel at position P5. It is preferable that the value obtained by subtracting the hardness of the steel at position P5 from the hardness of the steel at position P4 is 30 Hv or less.

[0053] The position where the hardness of the steel is 653 Hv is designated as position P6. Position P6 is farther from the outer peripheral surface 40a than position P5. More specifically, the distance between the surface of the bearing ring 10 and position P3 is preferably 0.25 mm or more and 0.6 mm or less.

[0054] The amount of retained austenite in the steel at the outer peripheral surface 40a is preferably 25 volume percent or more and 40 volume percent or less. More preferably, the amount of retained austenite in the steel at the outer peripheral surface 40a is 30 volume percent or more and 35 volume percent or less. The amount of retained austenite in the steel at the core 42 is preferably 3 volume percent or less.

[0055] <Method of Manufacturing Bearing Ring 10> Fig. 4 is a process diagram showing a manufacturing method of the bearing ring 10. As shown in Fig. 4, the manufacturing method of the bearing ring 10 includes a preparation step S1, a carbo-nitriding step S2, a quenching step S3, a tempering step S4, and a post-treatment step S5. The carbo-nitriding step S2 is performed after the preparation step S1. The quenching step S3 is performed after the carbo-nitriding step S2. The tempering step S4 is performed after the quenching step S3. The post-treatment step S5 is performed after the tempering step S4.

[0056] In the preparation step S1, a workpiece to be processed is prepared. The workpiece is ring-shaped. The workpiece is prepared by, for example, forming a base material into a shape close to the race 10 by machining such as forging and turning.

[0057] In the carbo-nitriding step S2, a carbo-nitriding treatment is performed on the surface of the workpiece. The carbo-nitriding treatment is performed by holding the workpiece at a predetermined heat treatment temperature in a heat treatment gas. For example, an endothermic transformer gas (RX gas) to which a nitrogen source gas (e.g., ammonia gas) is added is used as the heat treatment gas. The predetermined heat treatment temperature is, for example, a temperature equal to or higher than the A1 transformation point of the steel constituting the workpiece. Note that instead of the carbo-nitriding step S2, only the nitriding treatment may be performed.

[0058] The carbon content and nitrogen content in the steel on the surface of the race 10 and the depth of the surface layer 11 can be adjusted by the carbon potential and nitrogen potential in the heat treatment gas and the holding time.

[0059] In the quenching step S3, the workpiece is quenched. The quenching is carried out by holding the workpiece at a temperature equal to or higher than the A1 transformation point of the steel constituting the workpiece, and then quenching the M of the steel constituting the workpiece. S The workpiece is quenched to a temperature equal to or lower than the transformation point. The workpiece is quenched, for example, by water cooling or oil cooling.

[0060] In the tempering step S4, the workpiece is tempered. Tempering is performed by holding the workpiece at a temperature below the A1 transformation point of the steel that constitutes the workpiece. In the post-treatment step S5, the workpiece is post-treated. This post-treatment includes machining (grinding, polishing, etc.) and cleaning of the surface of the workpiece. In this manner, the race 10 having the structure shown in Figs. 1 and 2 is manufactured.

[0061] (Method of manufacturing the shaft 40) The method for manufacturing the shaft 40 includes a preparation step S1, a carbo-nitriding step S2, a quenching step S3, a tempering step S4, and a post-treatment step S5, similar to the method for manufacturing the race 10. However, the method for manufacturing the shaft 40 differs from the method for manufacturing the race 10 in the shape of the workpiece prepared in the preparation step S1.

[0062] (Effect of raceway 10) Rolling bearings used in automobile transmissions are sometimes used in a state where a sufficient oil film is not formed between the raceway surface and the roller surface due to the low viscosity of lubricating oil and the reduced supply of lubricating oil to improve fuel efficiency. In particular, in needle roller bearings, the rollers are long and slender, and it is difficult to ensure the machining accuracy of the roller surface, so that it is difficult to form an oil film between the raceway surface and the roller surface. As a result, in needle roller bearings, fatigue failure is likely to occur on the roller surface and the raceway surface due to metal contact with the raceway surface and the roller surface.

[0063] In needle roller bearings, the maximum contact pressure between the raceway and roller surface is usually about 3500 MPa. Therefore, the maximum shear stress caused by contact between the raceway and roller surface is applied at a position up to about 0.10 mm away from the raceway. This maximum shear stress affects the surface fatigue resistance of the raceway.

[0064] In the raceway 10, there is a position where maximum shear stress occurs between positions P1 and P2. In the raceway 10, the hardness of the steel at positions P1 and P2 is 720 Hv or more. In addition, in the raceway 10, the hardness of the steel at positions P1 minus the hardness of the steel at positions P2 is 30 Hv or less. In this way, in the raceway 10, the hardness of the steel is sufficiently ensured in the vicinity of the position where maximum shear stress occurs, and the hardness distribution is highly uniform, improving the surface fatigue resistance characteristics.

[0065] When the distance between the position P3 and the surface of the raceway 10 is set to 0.25 mm or more and 0.60 mm or less, the penetration depth of carbon and nitrogen is shortened. Therefore, by setting the distance between the position P3 and the surface of the raceway 10 to 0.25 mm or more and 0.60 mm or less, the carbo-nitriding step S2 can be shortened, thereby reducing the manufacturing cost.

[0066] When the amount of retained austenite in the steel in the core portion 12 is 3 volume percent or less, it is possible to suppress deterioration of the raceway 10 over time due to creep of the retained austenite. When the amount of retained austenite in the steel on the surface of the raceway 10 is 25 volume percent or more and 40 volume percent or less, fatigue flaking originating from indentations formed on the surface of the raceway 10 due to hard foreign matter (such as wear powder) becoming trapped is suppressed, thereby further improving surface fatigue resistance.

[0067] (Effect of Shaft 40) In shaft 40, the hardness of the steel at position P4 and the hardness of the steel at position P5 are 720 Hv or more, and the hardness of the steel at position P4 minus the hardness of the steel at position P5 is 30 Hv or less, thereby improving the surface fatigue resistance.

[0068] When the distance between the position P6 and the outer peripheral surface 40a is 0.25 mm or more and 0.60 mm or less, the manufacturing cost can be reduced by shortening the time for the carbo-nitriding step S2.

[0069] When the amount of retained austenite in the steel in the core portion 42 is 3 volume percent or less, it is possible to suppress changes over time in the shaft 40 due to creep of the retained austenite (more specifically, bending of the shaft 40). When the amount of retained austenite in the steel in the outer circumferential surface 40a is 25 volume percent or more and 40 volume percent or less, fatigue flaking originating from indentations formed on the outer circumferential surface 40a due to the entrapment of hard foreign matter is suppressed, thereby further improving the surface fatigue resistance.

[0070] (Example) A rolling fatigue test was conducted to confirm the effect of the shaft 40. In the rolling fatigue test, the diameter of the rollers 20 was set to 4 mm, and the length of the rollers 20 was set to 19 mm. In the rolling fatigue test, Samples 1 to 4 were prepared as shaft 40 samples, as shown in Table 2. Sample 1 was formed from the fourth steel material. Sample 2 was formed from the second steel material. Sample 3 was formed from the third steel material. Sample 4 was formed from the first steel material.

[0071] [Table 2]

[0072] Samples 1 and 2 were tempered by holding at 180°C. Sample 3 was tempered by holding at 160°C. Sample 4 was tempered by holding at 170°C. Sample 1 was subjected to only nitriding treatment. Samples 2 to 4 were subjected to carbo-nitriding treatment.

[0073] In sample 1, the carbon content and nitrogen content in the steel on the outer peripheral surface 40a were 1.0 mass percent and 0.13 mass percent, respectively. In sample 2, the carbon content and nitrogen content in the steel on the outer peripheral surface 40a were 0.80 mass percent and 0.45 mass percent, respectively. In sample 3, the carbon content and nitrogen content in the steel on the outer peripheral surface 40a were 0.65 mass percent and 0.55 mass percent, respectively. In sample 4, the carbon content and nitrogen content in the steel on the outer peripheral surface 40a were 0.75 mass percent and 0.55 mass percent, respectively.

[0074] In sample 1, the amount of retained austenite in the steel in the core 42 was 13 volume percent. In sample 2, the amount of retained austenite in the steel in the core 42 was 2 volume percent. In sample 3, the amount of retained austenite in the steel in the core 42 was 4 volume percent. In sample 4, the amount of retained austenite in the steel in the core 42 was 2 volume percent.

[0075] Fig. 5 is a graph showing the relationship between the distance from the outer peripheral surface 40a and the hardness of the steel in Samples 1 to 4. As shown in Fig. 5, in Sample 1, the hardness of the steel at position P4 was 756 Hv, the hardness of the steel at position P5 was 751 Hv, and the distance from the outer peripheral surface 40a to position P6 was more than 0.6 mm. In Sample 2, the hardness of the steel at position P4 was 742 Hv, the hardness of the steel at position P5 was 701 Hv, and the distance from the outer peripheral surface 40a to position P6 was 0.48 mm.

[0076] In sample 3, the hardness of the steel at position P4 was 740 Hv, the hardness of the steel at position P5 was 732 Hv, and the distance from the outer peripheral surface 40a to position P6 was 0.55 mm. In sample 4, the hardness of the steel at position P4 was 733 Hv, the hardness of the steel at position P5 was 723 Hv, and the distance from the outer peripheral surface 40a to position P6 was 0.39 mm.

[0077] Rolling fatigue life (L 10 The rolling fatigue life of each sample was evaluated as a ratio relative to the rolling fatigue life of sample 2. The rolling fatigue life of sample 1 was 3.52 times that of sample 2. The rolling fatigue life of sample 3 was 7.89 times that of sample 2. The rolling fatigue life of sample 4 was 3.90 times that of sample 2.

[0078] Condition A1 is that the hardness of the steel at position P4 and the hardness of the steel at position P5 are 720 Hv or more. Condition A2 is that the value obtained by subtracting the hardness of the steel at position P5 from the hardness of the steel at position P4 is 30 Hv or more. Condition B is that the distance between the outer circumferential surface 40a and position P6 is 0.25 mm or more and 0.60 mm or less.

[0079] Sample 2 did not satisfy conditions A1 and A2. On the other hand, Samples 1, 3, and 4 satisfied conditions A1 and A2. From this comparison, it was experimentally revealed that the surface fatigue resistance of the shaft 40 was improved by satisfying conditions A1 and A2.

[0080] The amount of bending of Sample 1, Sample 3, and Sample 4 was evaluated as a magnification relative to the ratio of the amount of bending of Sample 2. The amount of bending of Sample 1 was 4.33 times the amount of bending of Sample 2. The amount of bending of Sample 3 was 2.66 times the amount of bending of Sample 2. The amount of bending of Sample 4 was 1.00 times the amount of bending of Sample 2.

[0081] Condition C states that the amount of retained austenite in the steel in core portion 42 is 3 volume percent or less. Condition C was satisfied in samples 2 and 4, but not in samples 1 and 3. From this comparison, it was experimentally demonstrated that satisfying condition C suppresses deformation (bending) of shaft 40.

[0082] Although the embodiment of the present invention has been described above, the above-mentioned embodiment can be modified in various ways. The scope of the present invention is not limited to the above-mentioned embodiment. The scope of the present invention is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0083] 10 bearing ring, 10a, 10b end surface, 10c inner surface, 10d outer surface, 11 surface layer, 12 core section, 20 rollers, 20a, 20b end surface, 20c outer surface, 30 cage, 40 shaft, 40a outer surface, 41 surface layer, 42 core section, 100 rolling bearing, A Center axis, P1, P2, P3, P4, P5, P6 position, S1 preparation process, S2 carbo-nitriding process, S3 quenching process, S4 tempering process, S5 post-treatment process.

Claims

1. A steel raceway having a surface that contacts rollers and has a diameter of 1.5 mm or more and 4.0 mm or less, and a length divided by the diameter that is 4 or more and 10 or less, A surface layer portion on the surface; A core portion located inside the surface layer portion, The nitrogen content in the steel in the surface layer is higher than the nitrogen content in the steel in the core layer, At a first position that is 0.05 mm away from the surface and at a second position that is 0.20 mm away from the surface, the hardness of the steel is 720 Hv or more; The hardness of the steel at the first position minus the hardness of the steel at the second position is 30 Hv or less; The carbon content and the nitrogen content in the steel at the surface are 0.6 to 0.9 weight percent and 0.3 to 0.8 weight percent, respectively; the carbon content and the nitrogen content in the steel in the surface layer portion are higher than the nitrogen content and the carbon content in the steel in the core portion, respectively; The carbon content in the steel in the core is 0.15 mass percent or more and 0.4 mass percent or less, the steel contains chromium, manganese, silicon and molybdenum; In the steel, the chromium content is 0.5 mass percent or more and 3.0 mass percent or less, In the steel, the total content of manganese, silicon, and molybdenum is 1.0 mass% or more and 3.0 mass% or less, A raceway, the distance between the surface and a third location where the hardness of the steel is 653 Hv being 0.25 mm or more and 0.60 mm or less.

2. 2. The raceway of claim 1, wherein the amount of retained austenite in the steel in the core is 3 volume percent or less.

3. 3. The raceway according to claim 1, wherein the amount of retained austenite in the steel at the surface is between 25 volume percent and 40 volume percent.

Citation Information

Patent Citations

  • Rolling element and method of producing the same

    JP2004027260A

  • Needle roller bearing and needle roller

    JP2009057589A

  • Shaft and pinion shaft

    JP2010001521A

  • Bearing parts, rolling bearing, and process for production of bearing parts

    JP2010222678A

  • Constituent member of bearing, process for production of same, and ball-and-roller bearing provided with the constituent member

    JP2010248612A