Method for manufacturing polarizing plate, method for manufacturing image display device, and method for adjusting transmittance of polarizing film
By adjusting the transmittance of polarizing films through a method involving polyvinyl alcohol resin film processing and solvent contact, the method addresses brightness inconsistencies in image display devices, achieving consistent screen appearance.
Patent Information
- Application Number
- JP2021008759
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-22
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2041-01-22
AI Technical Summary
Existing methods do not allow for the adjustment of polarizing film transmittance after it is produced, leading to variations in brightness due to individual differences in image display cells and backlight units.
A method involving dyeing and stretching a polyvinyl alcohol resin film, followed by drying to a moisture content of 15% or less, and then contacting the surface with an aqueous solvent to adjust transmittance, including steps like auxiliary stretching, dyeing, stretching in boric acid solution, and drying shrinkage treatment.
Enables fine adjustment of polarizing film transmittance, reducing brightness variations between image display devices, ensuring consistent appearance across multiple screens.
Smart Images

Figure 0007555836000002 
Figure 0007555836000003 
Figure 0007555836000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polarizing plate, a method for producing an image display device, and a method for adjusting the transmittance of a polarizing film. [Background technology]
[0002] In recent years, image display devices such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices, inorganic EL display devices) have rapidly become widespread. Due to the image formation method used, liquid crystal display devices have polarizing plates disposed on both sides of a liquid crystal cell. It is also known that organic EL display devices can prevent problems such as external light reflection and background glare by disposing a circular polarizing plate including a λ / 4 plate on the viewing side of the organic EL cell (e.g., Patent Documents 1 and 2).
[0003] A polarizing plate generally has a structure in which a protective layer is disposed on at least one side of a polarizing film prepared by dyeing and stretching a polyvinyl alcohol-based resin film, and is attached to an image display cell such as a liquid crystal cell or an organic EL cell via an adhesive layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-311239 A [Patent Document 2] JP 2002-372622 A Summary of the Invention [Problem to be solved by the invention]
[0005] Conventionally, no method has been known for adjusting the transmittance of a polarizing film after its production, and therefore, it has not been possible to adjust the transmittance of the polarizing film after the polarizing plate is attached to an image display cell. On the other hand, since the brightness of an image display device may vary due to individual differences in the quality of image display cells, backlight units, etc., there has been a demand for the development of a method for adjusting the transmittance of the polarizing film after a protective layer is laminated thereon or after it is attached to an image display cell.
[0006] The present invention has been made to solve the above-mentioned problems in the conventional art, and a main object of the present invention is to provide a method for adjusting the transmittance of a polarizing film after its production. [Means for solving the problem]
[0007] According to one aspect of the present invention, there is provided a method for producing a polarizing plate, comprising, in order, a step of subjecting a polyvinyl alcohol-based resin film to a dyeing treatment and a stretching treatment in an aqueous boric acid solution, followed by drying until the moisture content is 15% by weight or less to obtain a primary polarizing film, and a step of contacting an aqueous solvent with the surface of the primary polarizing film to change the transmittance to obtain a secondary polarizing film. In one embodiment, the aqueous solvent is contacted with the exposed surface of the primary polarizing film, one surface of which is exposed and the other surface of which is protected. In one embodiment, the process for obtaining the primary polarizing film includes subjecting a polyvinyl alcohol-based resin film containing a halide and a polyvinyl alcohol-based resin, in the form of a laminate with a long thermoplastic resin substrate, to an air-assisted stretching process, a dyeing process, a stretching process in an aqueous boric acid solution, and a drying and shrinking process in that order, and the drying and shrinking process includes heating the laminate while transporting it in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction, and drying the polyvinyl alcohol-based resin film until its moisture content becomes 15% by weight or less. In one embodiment, the halide is iodide or sodium chloride. In one embodiment, the primary polarizing film has a thickness of 12 μm or less. According to another aspect of the present invention, there is provided a method for manufacturing an image display device, comprising the steps of: laminating a polarizing plate, which is made of a polyvinyl alcohol-based resin film containing a dichroic substance and which includes, in this order, a polarizing film having a moisture content of 15% by weight or less, a protective layer, and an adhesive layer, on an image display cell via the adhesive, so that the surface of the polarizing film opposite the side on which the protective layer is disposed is exposed; and contacting the exposed surface of the polarizing film with an aqueous solvent to change the transmittance, in this order. In one embodiment, the image display device is a liquid crystal display device or an organic EL display device. According to yet another aspect of the present invention, there is provided a method for adjusting the transmittance of a polarizing film, the method comprising the step of bringing an aqueous solvent into contact with a surface of a polarizing film made of a polyvinyl alcohol-based resin film containing a dichroic substance and having a moisture content of 15% by weight or less. Effect of the Invention
[0008] According to the present invention, the transmittance of the polarizing film can be changed after the fact by contacting an aqueous solvent with the surface of the polarizing film prepared by dyeing and stretching a polyvinyl alcohol-based resin film. In addition, the transmittance can be changed by contacting an aqueous solvent with the surface of the polarizing film in a state in which the appearance is stabilized by drying until the moisture content is equal to or less than a predetermined value after stretching in an aqueous boric acid solution, so that the transmittance can be finely adjusted. As a result, for example, the variation in brightness between image display devices can be reduced, which is useful when it is desired to align the appearance of multiple display screens, particularly when multiple display screens are combined to display an image (large public displays, digital signage, etc.). [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic diagram showing an example of a drying shrinkage treatment using a heating roll. [Figure 2A] FIG. 2 is a schematic cross-sectional view illustrating an example of a polarizing plate that can be produced in the process of producing a polarizing plate. [Figure 2B] FIG. 2 is a schematic cross-sectional view illustrating an example of a polarizing plate that can be produced in the process of producing a polarizing plate. [Figure 2C] FIG. 2 is a schematic cross-sectional view illustrating an example of a polarizing plate that can be produced in the process of producing a polarizing plate. [Figure 3A] 1 is a schematic cross-sectional view of an example of a polarizing plate that can be produced by a process of protecting an exposed surface of a secondary polarizing film. [Figure 3B] 1 is a schematic cross-sectional view of an example of a polarizing plate that can be produced by a process of protecting an exposed surface of a secondary polarizing film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments. Note that a polarizing plate obtained by the method for producing a polarizing plate according to the embodiment of the present invention includes at least a polarizing film, and preferably includes a polarizing film and a protective layer disposed on one or both sides of the polarizing film.
[0011] A. Manufacturing method of polarizing plate The method for producing a polarizing plate according to an embodiment of the present invention includes, in this order, a step of subjecting a polyvinyl alcohol (PVA)-based resin film to a dyeing treatment and a stretching treatment in a boric acid aqueous solution (stretching treatment in boric acid water), and then drying the film until the moisture content is 15% by weight or less to obtain a primary polarizing film, and a step of contacting an aqueous solvent with the surface of the primary polarizing film to change the transmittance to obtain a secondary polarizing film. According to the method for producing a polarizing plate, the transmittance can be changed afterwards to a desired value by contacting an aqueous solvent with the surface of a polarizing film (primary polarizing film) once produced to decolorize the film. In addition, by contacting the polarizing film (primary polarizing film) in a state of being highly oriented and having a stabilized appearance through the stretching treatment in boric acid water and drying treatment with an aqueous solvent, the transmittance can be suitably adjusted while avoiding excessive reduction in the degree of polarization, wrinkles, dissolution, etc.
[0012] In the method for manufacturing a polarizing plate according to an embodiment of the present invention, the transmittance may be changed by contacting only one side of the primary polarizing film with an aqueous solvent, or the transmittance may be changed by contacting both sides with an aqueous solvent.
[0013] In a method for producing a polarizing plate according to one embodiment of the present invention, the transmittance is changed by contacting an aqueous solvent with the exposed surface of a primary polarizing film in a state in which one surface is exposed and the other surface is protected. The method for producing a polarizing plate according to this embodiment may, for example, include a step of producing a polarizing plate in which one surface of the primary polarizing film is exposed and the other surface is protected by a protective layer between the steps of obtaining a primary polarizing film and obtaining a secondary polarizing film.
[0014] A-1. Process for obtaining primary polarizing film In the process of obtaining a primary polarizing film, the PVA-based resin film is dyed and stretched in boric acid water, and then dried until the moisture content is 15% by weight or less to obtain a primary polarizing film. The primary polarizing film may be prepared using a single layer of PVA-based resin film, or may be prepared using a laminate of two or more layers including a PVA-based resin layer (PVA-based resin film). A primary polarizing film prepared using a laminate of two or more layers can preferably maintain excellent optical properties (typically, single transmittance and polarization degree) while avoiding the occurrence of wrinkles, even after contact with an aqueous solvent.
[0015] A-1-1. Preparation of a primary polarizing film using a laminate of two or more layers The preparation of a primary polarizing film using a laminate of two or more layers can be carried out, for example, by a method including subjecting a PVA-based resin film containing a halide and a PVA-based resin, in the state of being laminated with a long thermoplastic resin substrate, to an air-assisted stretching treatment, a dyeing treatment, a stretching treatment in an aqueous boric acid solution, and a drying shrinkage treatment in this order. The laminate of a thermoplastic resin substrate and a PVA-based resin film can be obtained, for example, by forming a PVA-based resin layer (PVA-based resin film) containing a halide and a PVA-based resin on one side of a long thermoplastic resin substrate to form a laminate. The drying shrinkage treatment includes, for example, heating the laminate of the long thermoplastic resin substrate and the PVA-based resin film while conveying it in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction, and drying the PVA-based resin film until the moisture content becomes 15% by weight or less. The content of the halide in the PVA-based resin layer is preferably 5 to 20 parts by weight with respect to 100 parts by weight of the PVA-based resin. The drying shrinkage treatment is preferably carried out using a heated roll, and the temperature of the heated roll is preferably 60° C. to 120° C. According to such a production method, a primary polarizing film having a high degree of orientation of the PVA resin and excellent optical properties can be obtained.
[0016] A-1-1-1. Preparation of laminate Any suitable method can be adopted as a method for producing a laminate of a thermoplastic resin substrate and a PVA-based resin layer. Preferably, a coating liquid containing a halide and a PVA-based resin is applied to the surface of the thermoplastic resin substrate, and then dried to form a PVA-based resin layer on the thermoplastic resin substrate. As described above, the content of the halide in the PVA-based resin layer is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA-based resin.
[0017] Any appropriate method can be used as the coating method of the coating liquid. For example, roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, knife coating (comma coating, etc.), etc. are listed. The coating and drying temperature of the coating liquid is preferably 50° C. or higher.
[0018] The thickness of the PVA-based resin layer is preferably 3 μm to 40 μm, and more preferably 3 μm to 20 μm.
[0019] Before forming the PVA-based resin layer, the thermoplastic resin substrate may be subjected to a surface treatment (e.g., corona treatment, etc.), or an easy-adhesion layer may be formed on the thermoplastic resin substrate. By carrying out such treatment, the adhesion between the thermoplastic resin substrate and the PVA-based resin layer can be improved.
[0020] The thickness of the thermoplastic resin substrate is preferably 20 μm to 300 μm, more preferably 50 μm to 200 μm. If it is less than 20 μm, it may be difficult to form a PVA-based resin layer. If it exceeds 300 μm, for example, in the underwater stretching treatment described below, it may take a long time for the thermoplastic resin substrate to absorb water, and an excessive load may be required for stretching.
[0021] The thermoplastic resin substrate preferably has a water absorption rate of 0.2% or more, more preferably 0.3% or more. The thermoplastic resin substrate can absorb water, and the water can act as a plasticizer to plasticize the substrate. As a result, the stretching stress can be significantly reduced, and the substrate can be stretched at a high ratio. On the other hand, the water absorption rate of the thermoplastic resin substrate is preferably 3.0% or less, more preferably 1.0% or less. By using such a thermoplastic resin substrate, it is possible to prevent problems such as a significant decrease in the dimensional stability of the thermoplastic resin substrate during production, which leads to a deterioration in the appearance of the resulting polarizing film. It is also possible to prevent the substrate from breaking during underwater stretching, and the PVA-based resin layer from peeling off from the thermoplastic resin substrate. The water absorption rate of the thermoplastic resin substrate can be adjusted, for example, by introducing a modifying group into the constituent material. The water absorption rate is a value determined in accordance with JIS K 7209.
[0022] The glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 120°C or lower. By using such a thermoplastic resin substrate, the stretchability of the laminate can be sufficiently ensured while suppressing the crystallization of the PVA-based resin layer. Furthermore, in consideration of the plasticization of the thermoplastic resin substrate by water and the underwater stretching, it is more preferable that the temperature is 100°C or lower, and further 90°C or lower. On the other hand, the glass transition temperature of the thermoplastic resin substrate is preferably 60°C or higher. By using such a thermoplastic resin substrate, defects such as deformation of the thermoplastic resin substrate (e.g., generation of unevenness, sagging, wrinkles, etc.) during the application and drying of the coating liquid containing the PVA-based resin can be prevented, and a laminate can be produced satisfactorily. In addition, the stretching of the PVA-based resin layer can be satisfactorily performed at a suitable temperature (e.g., about 60°C). The glass transition temperature of the thermoplastic resin substrate can be adjusted, for example, by introducing a modifying group into the constituent material and heating using a crystallizing material. The glass transition temperature (Tg) is a value obtained in accordance with JIS K 7121.
[0023] Any suitable thermoplastic resin may be used as the material for the thermoplastic resin substrate. Examples of the thermoplastic resin include ester resins such as polyethylene terephthalate resins, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, polyamide resins, polycarbonate resins, and copolymer resins thereof. Among these, norbornene resins and amorphous polyethylene terephthalate resins are preferred.
[0024] In one embodiment, amorphous (uncrystallized) polyethylene terephthalate resins are preferably used. Among them, amorphous (hard to crystallize) polyethylene terephthalate resins are particularly preferably used. Specific examples of amorphous polyethylene terephthalate resins include copolymers further containing isophthalic acid and / or cyclohexanedicarboxylic acid as dicarboxylic acids, and copolymers further containing cyclohexanedimethanol or diethylene glycol as glycols.
[0025] In a preferred embodiment, the thermoplastic resin substrate is made of a polyethylene terephthalate resin having an isophthalic acid unit. This is because such a thermoplastic resin substrate has excellent stretchability and can suppress crystallization during stretching. This is believed to be due to the introduction of an isophthalic acid unit to impart a large bend to the main chain. The polyethylene terephthalate resin has a terephthalic acid unit and an ethylene glycol unit. The content ratio of the isophthalic acid unit is preferably 0.1 mol% or more, more preferably 1.0 mol% or more, based on the total of all repeating units. This is because a thermoplastic resin substrate with extremely excellent stretchability can be obtained. On the other hand, the content ratio of the isophthalic acid unit is preferably 20 mol% or less, more preferably 10 mol% or less, based on the total of all repeating units. By setting such a content ratio, the crystallinity can be favorably increased in the drying shrinkage treatment described below.
[0026] The thermoplastic resin substrate may be stretched in advance (before the PVA-based resin layer is formed). In one embodiment, the long thermoplastic resin substrate is stretched in the transverse direction. The transverse direction is preferably a direction perpendicular to the stretching direction of the laminate described below. In this specification, "perpendicular" also includes the case where the direction is substantially perpendicular. Here, "substantially perpendicular" includes the case where the direction is 90°±5.0°, preferably 90°±3.0°, and more preferably 90°±1.0°.
[0027] The stretching temperature of the thermoplastic resin substrate is preferably from the glass transition temperature (Tg) of Tg-10° C. to Tg+50° C. The stretching ratio of the thermoplastic resin substrate is preferably from 1.5 times to 3.0 times.
[0028] Any appropriate method may be adopted as the stretching method of the thermoplastic resin substrate. Specifically, it may be fixed end stretching or free end stretching. The stretching method may be dry or wet. The stretching of the thermoplastic resin substrate may be performed in one stage or multiple stages. When it is performed in multiple stages, the above-mentioned stretching ratio is the product of the stretching ratios of each stage.
[0029] The coating liquid contains a halide and a PVA resin as described above. The coating liquid is typically a solution in which the halide and the PVA resin are dissolved in a solvent. Examples of the solvent include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyhydric alcohols such as trimethylolpropane, and amines such as ethylenediamine and diethylenetriamine. These can be used alone or in combination of two or more. Among these, water is preferred. The concentration of the PVA resin in the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. With such a resin concentration, a uniform coating film that is in close contact with the thermoplastic resin substrate can be formed. The content of the halide in the coating liquid is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA resin.
[0030] Additives may be added to the coating liquid. Examples of additives include plasticizers and surfactants. Examples of plasticizers include polyhydric alcohols such as ethylene glycol and glycerin. Examples of surfactants include nonionic surfactants. These can be used to further improve the uniformity, dyeability, and stretchability of the resulting PVA-based resin layer.
[0031] Any suitable resin can be used as the PVA resin. Examples include polyvinyl alcohol and ethylene-vinyl alcohol copolymer. Polyvinyl alcohol is obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer is obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of the PVA resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree can be determined in accordance with JIS K 6726-1994. By using a PVA resin with such a saponification degree, a polarizing film with excellent durability can be obtained. If the saponification degree is too high, gelation may occur.
[0032] The average degree of polymerization of the PVA resin can be appropriately selected depending on the purpose. The average degree of polymerization is usually 1000 to 10000, preferably 1200 to 4500, and more preferably 1500 to 4300. The average degree of polymerization can be determined in accordance with JIS K 6726-1994.
[0033] Any suitable halide may be used as the halide. For example, iodide and sodium chloride may be used. For example, iodide may be potassium iodide, sodium iodide, and lithium iodide. Among these, potassium iodide is preferred.
[0034] The amount of the halide in the coating solution is preferably 5 to 20 parts by weight per 100 parts by weight of the PVA-based resin, and more preferably 10 to 15 parts by weight per 100 parts by weight of the PVA-based resin. If the amount of the halide exceeds 20 parts by weight per 100 parts by weight of the PVA-based resin, the halide may bleed out, causing the final polarizing film to become cloudy.
[0035] Generally, the orientation of polyvinyl alcohol molecules in the PVA-based resin layer increases when the PVA-based resin layer is stretched, but when the stretched PVA-based resin layer is immersed in a liquid containing water, the orientation of polyvinyl alcohol molecules may be disturbed and the orientation may decrease. In particular, when a laminate of a thermoplastic resin substrate and a PVA-based resin layer is stretched in boric acid water, the tendency of the orientation degree to decrease is significant when the laminate is stretched in boric acid water at a relatively high temperature to stabilize the stretching of the thermoplastic resin substrate. For example, the stretching of a PVA film alone in boric acid water is generally performed at 60°C, whereas the stretching of a laminate of A-PET (thermoplastic resin substrate) and a PVA-based resin layer is performed at a high temperature of about 70°C, in which case the orientation of PVA at the initial stage of stretching may decrease before it increases due to underwater stretching. In response to this, a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate is prepared, and the laminate is stretched at high temperature (auxiliary stretching) in air before being stretched in boric acid water, so that the crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after the auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the orientation of the polyvinyl alcohol molecules is disturbed and the orientation is reduced, compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the polarizing film obtained through a process in which the laminate is immersed in a liquid, such as a dyeing process and an underwater stretching process.
[0036] A-1-1-2. Aerial supplementary stretching process In particular, in order to obtain high optical properties, a two-stage stretching method is selected, which combines dry stretching (auxiliary stretching) and stretching in boric acid water. By introducing auxiliary stretching like two-stage stretching, it is possible to stretch while suppressing the crystallization of the thermoplastic resin substrate, which solves the problem of the thermoplastic resin substrate being excessively crystallized and reduced in stretchability in the subsequent stretching in boric acid water, and the laminate can be stretched at a higher magnification. Furthermore, when applying a PVA-based resin onto a thermoplastic resin substrate, in order to suppress the influence of the glass transition temperature of the thermoplastic resin substrate, it is necessary to lower the application temperature compared to when applying a PVA-based resin onto a normal metal drum, which may result in a problem that the crystallization of the PVA-based resin is relatively low and sufficient optical properties cannot be obtained. In contrast, by introducing auxiliary stretching, it is possible to increase the crystallinity of the PVA-based resin even when applying a PVA-based resin onto a thermoplastic resin substrate, and it is possible to achieve high optical properties. At the same time, by increasing the orientation of the PVA-based resin in advance, problems such as a decrease in the orientation of the PVA-based resin or dissolution when the resin is immersed in water during subsequent dyeing or stretching processes can be prevented, making it possible to achieve high optical properties.
[0037] The stretching method of the auxiliary air stretching may be fixed end stretching (for example, a method of stretching using a tenter stretching machine) or free end stretching (for example, a method of uniaxially stretching the laminate by passing it between rolls with different peripheral speeds), but in order to obtain high optical properties, free end stretching may be actively adopted. In one embodiment, the air stretching process includes a heated roll stretching step in which the laminate is stretched by the difference in peripheral speed between heated rolls while being transported in its longitudinal direction. The air stretching process typically includes a zone stretching step and a heated roll stretching step. The order of the zone stretching step and the heated roll stretching step is not limited, and the zone stretching step may be performed first, or the heated roll stretching step may be performed first. The zone stretching step may be omitted. In one embodiment, the zone stretching step and the heated roll stretching step are performed in this order. In another embodiment, the laminate is stretched in a tenter stretching machine by gripping the ends of the laminate and widening the distance between the tenters in the machine direction (the increase in the distance between the tenters is the stretching ratio). At this time, the distance between the tenters in the width direction (perpendicular to the machine direction) is set to be arbitrarily close. Preferably, it can be set to be closer to the free end stretching ratio in the machine direction. In the case of free end stretching, the shrinkage ratio in the width direction = (1 / stretching ratio) 1 / 2 It is calculated as follows.
[0038] The auxiliary air-drawing may be performed in one step or in multiple steps. When the auxiliary air-drawing is performed in multiple steps, the draw ratio is the product of the draw ratios in each step. The draw direction in the auxiliary air-drawing is preferably approximately the same as the draw direction in the underwater drawing.
[0039] The stretching ratio in the auxiliary air-stretching is preferably 2.0 to 3.5 times. The maximum stretching ratio in the case of combining the auxiliary air-stretching and the underwater stretching is preferably 5.0 times or more, more preferably 5.5 times or more, and even more preferably 6.0 times or more, based on the original length of the laminate. In this specification, the "maximum stretching ratio" refers to the stretching ratio just before the laminate breaks, and refers to a value 0.2 lower than the stretching ratio at which the laminate breaks, which is determined separately.
[0040] The stretching temperature of the auxiliary air stretching can be set to any appropriate value depending on the material of the thermoplastic resin substrate, the stretching method, etc. The stretching temperature is preferably equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin substrate, more preferably equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin substrate + 10°C, and particularly preferably equal to or higher than Tg + 15°C. On the other hand, the upper limit of the stretching temperature is preferably 170°C. By stretching at such a temperature, the crystallization of the PVA resin can be suppressed from progressing rapidly, and defects due to the crystallization (for example, the orientation of the PVA resin layer due to stretching can be suppressed). The crystallization index of the PVA resin after the auxiliary air stretching is preferably 1.3 to 1.8, more preferably 1.4 to 1.7. The crystallization index of the PVA resin can be measured by the ATR method using a Fourier transform infrared spectrophotometer. Specifically, the measurement is performed using polarized light as the measurement light, and the crystallization index at 1141 cm of the obtained spectrum is suppressed. -1 and 1440cm -1 The crystallization index is calculated according to the following formula using the intensity of Crystallization index=(I C / I R ) however, I C : 1141cm when measuring with incident measuring light -1 Intensity I R : 1440cm when measuring with incident measuring light -1 Intensity It is.
[0041] A-1-1-3. Insolubilization treatment If necessary, an insolubilization treatment is carried out after the auxiliary air stretching treatment and before the underwater stretching treatment or the dyeing treatment. The insolubilization treatment is typically carried out by immersing the PVA-based resin layer in an aqueous boric acid solution. By carrying out the insolubilization treatment, water resistance is imparted to the PVA-based resin layer, and it is possible to prevent a decrease in the orientation of PVA when immersed in water. The concentration of the aqueous boric acid solution is preferably 1 part by weight to 4 parts by weight with respect to 100 parts by weight of water. The liquid temperature of the insolubilization bath (aqueous boric acid solution) is preferably 20°C to 50°C.
[0042] A-1-1-4. Dyeing process The dyeing treatment is typically carried out by dyeing the PVA-based resin layer with a dichroic substance (typically iodine). Specifically, the dyeing treatment is carried out by adsorbing iodine to the PVA-based resin layer. Examples of the adsorption method include a method of immersing the PVA-based resin layer (laminate) in a dyeing solution containing iodine, a method of applying the dyeing solution to the PVA-based resin layer, and a method of spraying the dyeing solution onto the PVA-based resin layer. A preferred method is to immerse the laminate in a dyeing solution (dye bath), because iodine can be well adsorbed by this method.
[0043] The dyeing solution is preferably an aqueous iodine solution. The amount of iodine to be mixed is preferably 0.05 to 0.5 parts by weight relative to 100 parts by weight of water. In order to increase the solubility of iodine in water, it is preferable to mix an iodide in the aqueous iodine solution. Examples of iodides include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide. Among these, potassium iodide is preferable. The amount of iodide to be mixed is preferably 0.1 to 10 parts by weight, more preferably 0.3 to 5 parts by weight, relative to 100 parts by weight of water. The temperature of the dyeing solution during dyeing is preferably 20°C to 50°C in order to suppress dissolution of the PVA resin. When the PVA-based resin layer is immersed in the dye solution, the immersion time is preferably 5 seconds to 5 minutes, and more preferably 30 seconds to 90 seconds, in order to ensure the transmittance of the PVA-based resin layer.
[0044] The dyeing conditions (concentration, liquid temperature, immersion time) can be set so that the single transmittance of the finally obtained polarizing film is a desired value. As such dyeing conditions, preferably, an iodine aqueous solution is used as the dyeing solution, and the content ratio of iodine and potassium iodide in the iodine aqueous solution is 1:5 to 1:20. The content ratio of iodine and potassium iodide in the iodine aqueous solution is preferably 1:5 to 1:10. This makes it possible to obtain a primary polarizing film having the optical properties described below.
[0045] When a dyeing process is performed continuously after a process (typically, an insolubilization process) in which the laminate is immersed in a treatment bath containing boric acid, the boric acid concentration of the dyeing bath may change over time due to the boric acid contained in the treatment bath being mixed into the dyeing bath, resulting in unstable dyeability. In order to suppress the above-mentioned instability of dyeability, the upper limit of the boric acid concentration of the dyeing bath is adjusted to be preferably 4 parts by weight, more preferably 2 parts by weight, relative to 100 parts by weight of water. On the other hand, the lower limit of the boric acid concentration of the dyeing bath is preferably 0.1 parts by weight, more preferably 0.2 parts by weight, and even more preferably 0.5 parts by weight, relative to 100 parts by weight of water. In one embodiment, the dyeing process is performed using a dyeing bath in which boric acid has been blended in advance. This can reduce the rate of change in the boric acid concentration when the boric acid of the treatment bath is mixed into the dyeing bath. The amount of boric acid preliminarily mixed into the dye bath (i.e., the content of boric acid not derived from the treatment bath) is preferably 0.1 to 2 parts by weight, and more preferably 0.5 to 1.5 parts by weight, per 100 parts by weight of water.
[0046] A-1-1-5. Cross-linking treatment If necessary, a crosslinking treatment is carried out after the dyeing treatment and before the underwater stretching treatment. The crosslinking treatment is typically carried out by immersing the PVA-based resin layer in an aqueous boric acid solution. The crosslinking treatment imparts water resistance to the PVA-based resin layer, and prevents the orientation of the PVA from decreasing when the layer is immersed in high-temperature water in the subsequent underwater stretching. The concentration of the aqueous boric acid solution is preferably 1 to 5 parts by weight per 100 parts by weight of water. In addition, when the crosslinking treatment is carried out after the dyeing treatment, it is preferable to further add an iodide. By adding an iodide, it is possible to suppress the elution of iodine adsorbed to the PVA-based resin layer. The amount of the iodide to be added is preferably 1 to 5 parts by weight per 100 parts by weight of water. Specific examples of the iodide are as described above. The liquid temperature of the crosslinking bath (aqueous boric acid solution) is preferably 20°C to 50°C.
[0047] A-1-1-6. Underwater stretching treatment The underwater stretching treatment is performed by immersing the laminate in a stretching bath. The underwater stretching treatment allows stretching at a temperature lower than the glass transition temperature (typically about 80° C.) of the thermoplastic resin substrate or the PVA-based resin layer, and allows the PVA-based resin layer to be stretched at a high magnification while suppressing crystallization. As a result, a polarizing film having excellent optical properties can be produced.
[0048] The stretching method of the laminate can be any appropriate method. Specifically, it may be fixed end stretching or free end stretching (for example, a method of uniaxially stretching the laminate by passing it between rolls having different peripheral speeds). Preferably, free end stretching is selected. The stretching of the laminate may be performed in one stage or multiple stages. When performing the stretching in multiple stages, the stretching ratio (maximum stretching ratio) of the laminate described below is the product of the stretching ratios in each stage.
[0049] The underwater stretching is typically performed by immersing the laminate in an aqueous solution of boric acid (underwater stretching in boric acid). By using an aqueous solution of boric acid as the stretching bath, it is possible to impart to the PVA-based resin layer rigidity that can withstand the tension applied during stretching and water resistance that does not dissolve in water. Specifically, boric acid can generate tetrahydroxyborate anions in the aqueous solution and crosslink with the PVA-based resin through hydrogen bonds. As a result, the PVA-based resin layer is imparted with rigidity and water resistance, and can be stretched well, making it possible to produce a primary polarizing film with excellent optical properties.
[0050] The boric acid aqueous solution is preferably obtained by dissolving boric acid and / or a borate in water as a solvent. The boric acid concentration is preferably 1 to 10 parts by weight, more preferably 2.5 to 6 parts by weight, and particularly preferably 3 to 5 parts by weight, relative to 100 parts by weight of water. By setting the boric acid concentration to 1 part by weight or more, dissolution of the PVA-based resin layer can be effectively suppressed, and a polarizing film with higher characteristics can be produced. In addition to boric acid or a borate, an aqueous solution obtained by dissolving a boron compound such as borax, glyoxal, glutaraldehyde, or the like in a solvent can also be used.
[0051] Preferably, an iodide is added to the stretching bath (boric acid aqueous solution). By adding an iodide, it is possible to suppress the elution of iodine adsorbed in the PVA resin layer. Specific examples of the iodide are as described above. The concentration of the iodide is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 8 parts by weight, relative to 100 parts by weight of water.
[0052] The stretching temperature (liquid temperature of the stretching bath) is preferably 40°C to 85°C, more preferably 60°C to 75°C. At such a temperature, the laminate can be stretched at a high ratio while suppressing dissolution of the PVA-based resin layer. Specifically, as described above, the glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 60°C or higher in relation to the formation of the PVA-based resin layer. In this case, if the stretching temperature is lower than 40°C, there is a risk that the substrate cannot be stretched well even when the plasticization of the thermoplastic resin substrate by water is taken into consideration. On the other hand, the higher the temperature of the stretching bath, the higher the solubility of the PVA-based resin layer, and there is a risk that excellent optical properties cannot be obtained. The immersion time of the laminate in the stretching bath is preferably 15 seconds to 5 minutes.
[0053] The stretching ratio in the underwater stretching is preferably 1.5 times or more, more preferably 3.0 times or more. The total stretching ratio of the laminate is preferably 5.0 times or more, more preferably 5.5 times or more, based on the original length of the laminate. By achieving such a high stretching ratio, a primary polarizing film with extremely excellent optical properties can be produced. Such a high stretching ratio can be achieved by employing an underwater stretching method (stretching in boric acid water).
[0054] A-1-1-7. Drying shrinkage treatment The drying shrinkage treatment includes, for example, heating the laminate of the long thermoplastic resin substrate and the PVA-based resin film while transporting it in the longitudinal direction, thereby shrinking it in the width direction by 2% or more, and drying the PVA-based resin film until the moisture content of the film is 15% by weight or less. From the viewpoint of obtaining a stable appearance, it is preferable to dry the laminate until the moisture content is 12% by weight or less, more preferably 10% by weight or less, and even more preferably 1 to 5% by weight.
[0055] The drying shrinkage treatment may be performed by zone heating in which the entire zone is heated, or by heating the transport roll (using a so-called heating roll) (heat roll drying method). Preferably, both are used. By drying using a heating roll, it is possible to efficiently suppress the heat curl of the laminate and produce a primary polarizing film with excellent appearance. Specifically, by drying the laminate in a state where it is aligned with the heating roll, it is possible to efficiently promote the crystallization of the thermoplastic resin substrate and increase the crystallinity, and even at a relatively low drying temperature, it is possible to satisfactorily increase the crystallinity of the thermoplastic resin substrate. As a result, the rigidity of the thermoplastic resin substrate increases and it becomes in a state where it can withstand the shrinkage of the PVA-based resin layer due to drying, and curling is suppressed. In addition, by using a heating roll, it is possible to dry the laminate while maintaining it in a flat state, so that it is possible to suppress not only curling but also wrinkles. At this time, the optical properties of the laminate can be improved by shrinking it in the width direction by the drying shrinkage treatment. This is because the orientation of the PVA and the PVA / iodine complex can be effectively increased. The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment is preferably 1% to 10%, more preferably 2% to 8%, and particularly preferably 4% to 6%. By using a heating roll, the laminate can be continuously shrunk in the width direction while being transported, thereby achieving high productivity.
[0056] 1 is a schematic diagram showing an example of the drying shrinkage treatment. In the drying shrinkage treatment, the laminate 200 is dried while being transported by transport rolls R1 to R6 heated to a predetermined temperature and guide rolls G1 to G4. In the illustrated example, the transport rolls R1 to R6 are arranged so as to alternately and continuously heat the surface of the PVA-based resin layer and the surface of the thermoplastic resin substrate, but, for example, the transport rolls R1 to R6 may be arranged so as to continuously heat only one surface of the laminate 200 (for example, the thermoplastic resin substrate surface).
[0057] Drying conditions can be controlled by adjusting the heating temperature of the transport rolls (temperature of the heating rolls), the number of heating rolls, the contact time with the heating rolls, etc. The temperature of the heating rolls is preferably 60°C to 120°C, more preferably 65°C to 100°C, and particularly preferably 70°C to 80°C. The crystallinity of the thermoplastic resin can be favorably increased, curling can be favorably suppressed, and an optical laminate with extremely excellent durability can be produced. The temperature of the heating rolls can be measured by a contact thermometer. In the illustrated example, six transport rolls are provided, but there is no particular restriction as long as there are multiple transport rolls. The number of transport rolls is usually 2 to 40, preferably 4 to 30. The contact time (total contact time) between the laminate and the heating rolls is preferably 1 to 300 seconds, more preferably 1 to 20 seconds, and even more preferably 1 to 10 seconds.
[0058] The heating roll may be provided in a heating furnace (for example, an oven) or in a normal production line (under room temperature environment). It is preferably provided in a heating furnace equipped with a blowing means. By using drying with a heating roll in combination with hot air drying, it is possible to suppress abrupt temperature changes between the heating rolls, and it is possible to easily control shrinkage in the width direction. The hot air drying temperature is preferably 30°C to 100°C. The hot air drying time is preferably 1 second to 300 seconds. The hot air speed is preferably about 10 m / s to 30 m / s. The wind speed is the wind speed in the heating furnace, and can be measured by a mini-vane type digital anemometer.
[0059] A-1-1-8.Other processing Preferably, after the underwater stretching treatment and before the drying shrinkage treatment, a washing treatment is carried out. The washing treatment is typically carried out by immersing the PVA-based resin layer in an aqueous potassium iodide solution.
[0060] A-1-2. Preparation of a primary polarizing film using a single layer of PVA-based resin film The primary polarizing film using a single-layer PVA-based resin film can be produced by dyeing and stretching (typically, uniaxial stretching using a roll stretching machine) a long PVA-based resin film having self-supporting properties (i.e., not requiring support by a substrate) in boric acid water, and then drying until the moisture content is 15% by weight or less, preferably 12% by weight or less, more preferably 10% by weight or less, and even more preferably 1 to 5% by weight. The dyeing is carried out, for example, by immersing the PVA-based resin film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment or while the film is being dyed. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based resin film is subjected to a swelling treatment, a crosslinking treatment, a washing treatment, or the like. For example, by immersing the PVA-based resin film in water and washing it before dyeing, it is possible to wash off dirt and antiblocking agents on the surface of the PVA-based resin film, and also to swell the PVA-based resin film to prevent uneven dyeing, etc.
[0061] A-1-3. Primary polarizing film The primary polarizing film preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The transmittance (single transmittance: Ts) of the primary polarizing film is preferably 41.5% or more, more preferably 42.0% or more, and even more preferably 42.5% or more. On the other hand, the transmittance of the primary polarizing film is preferably 46.0% or less, more preferably 45.0% or less. The degree of polarization of the primary polarizing film is preferably 98.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more. On the other hand, the degree of polarization of the primary polarizing film is preferably 99.998% or less. The transmittance is typically a Y value measured using an ultraviolet-visible spectrophotometer and corrected for luminosity. The degree of polarization is typically calculated by the following formula based on the parallel transmittance Tp and crossed transmittance Tc measured using an ultraviolet-visible spectrophotometer and corrected for luminosity. Degree of polarization (%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100
[0062] In one embodiment, the transmittance of a thin polarizing film of 12 μm or less is typically measured using an ultraviolet-visible spectrophotometer with a laminate of a polarizing film (refractive index of surface: 1.53) and a protective layer (protective film) (refractive index: 1.50) as the measurement target. Depending on the refractive index of the surface of the polarizing film and / or the refractive index of the surface in contact with the air interface of the protective layer, the reflectance at the interface of each layer may change, and as a result, the measured transmittance may change. Therefore, for example, when a protective layer with a refractive index other than 1.50 is used, the measured transmittance may be corrected depending on the refractive index of the surface in contact with the air interface of the protective layer. Specifically, the corrected value C of the transmittance is expressed by the following formula using the reflectance R1 (transmission axis reflectance) of polarized light parallel to the transmission axis at the interface between the protective layer and the air layer. C=R1-R0 R0 = ((1.50-1) 2 / (1.50+1) 2 )×(T1 / 100) R1 = ((n1-1) 2 / (n1+1) 2 )×(T1 / 100) Here, R0 is the transmission axis reflectance when a protective layer with a refractive index of 1.50 is used, n1 is the refractive index of the protective layer used, and T1 is the transmittance of the polarizing film. For example, when a base material with a surface refractive index of 1.53 (such as a cycloolefin film or a film with a hard coat layer) is used as a protective layer, the correction amount C is about 0.2%. In this case, by adding 0.2% to the transmittance obtained by measurement, it is possible to convert a polarizing film with a surface refractive index of 1.53 into the transmittance when a protective layer with a refractive index of 1.50 is used. According to the calculation based on the above formula, when the transmittance T1 of the polarizing film is changed by 2%, the change in the correction value C is 0.03% or less, and the influence of the transmittance of the polarizing film on the value of the correction value C is limited. In addition, when the protective layer has absorption other than surface reflection, an appropriate correction can be made according to the amount of absorption.
[0063] The thickness of the primary polarizing film is typically 25 μm or less, preferably 12 μm or less, more preferably 1 μm to 8 μm, even more preferably 1 μm to 7 μm, and even more preferably 2 μm to 5 μm. A small thickness has the advantage that the polarizing film is less likely to wrinkle when it is brought into contact with an aqueous solvent.
[0064] The moisture content of the primary polarizing film is typically 15% by weight or less, preferably 12% by weight or less, more preferably 10% by weight or less, and further preferably 1 to 5% by weight. If the moisture content is within the above range, the transmittance can be changed without significant deterioration of the appearance when the film is brought into contact with an aqueous solvent.
[0065] A-2. Process for producing polarizing plates In the process of preparing a polarizing plate, a polarizing plate having a structure in which a protective layer and an optional functional layer are laminated on one side of a primary polarizing film, and the other side is an exposed surface, is prepared. Any appropriate functional layer can be selected according to the purpose as the functional layer, and specific examples thereof include a retardation layer, an adhesive layer, and the like. The process of preparing the polarizing plate is an optional process. Therefore, according to the purpose, a laminate having a structure of [thermoplastic resin substrate / primary polarizing film] prepared by the method described in A-1-1 or a primary polarizing film prepared using a single layer PVA-based resin film described in A-1-2 can be directly subjected to the process of obtaining a secondary polarizing film.
[0066] 2A to 2C are schematic cross-sectional views for explaining an example of a polarizing plate that can be produced in the process of producing a polarizing plate. The polarizing plate 100A shown in FIG. 2A includes a polarizing film (primary polarizing film) 10 and a protective layer 20 disposed on one side thereof, and the side of the polarizing film (primary polarizing film) 10 opposite to the side on which the protective layer 20 is provided is an exposed surface. The polarizing plate 100A can be obtained, for example, by bonding a protective layer via an adhesive layer or a pressure-sensitive adhesive layer to the primary polarizing film side surface of a laminate having a configuration of [thermoplastic resin substrate / primary polarizing film] produced by the method described in A-1-1, and then peeling off the thermoplastic resin substrate. Alternatively, the polarizing plate 100A can be obtained by bonding a protective layer via an adhesive layer or a pressure-sensitive adhesive layer to one surface of the primary polarizing film produced by the method described in A-1-2.
[0067] The polarizing plate 100B shown in FIG. 2B includes a polarizing film (primary polarizing film) 10, a protective layer 20, a retardation layer 30, and an adhesive layer 40 in this order, and the side of the polarizing film (primary polarizing film) 10 opposite to the side on which the protective layer 20 is provided is an exposed surface. The polarizing plate 100B can be obtained, for example, by bonding the retardation layer 30 to the protective layer 20 side surface of the polarizing plate 100A via an adhesive layer or an adhesive layer, and then providing an adhesive layer 40 on the surface of the retardation layer 30. Alternatively, the polarizing plate 100B can also be obtained by bonding the retardation layer 30 to the thermoplastic resin substrate side surface of a laminate having the above-mentioned [thermoplastic resin substrate / primary polarizing film] via an adhesive layer or an adhesive layer, and then providing an adhesive layer 40 on the surface of the retardation layer 30. In this case, the thermoplastic resin substrate functions as the protective layer 20. The retardation layer 30 in the illustrated example may have a single layer structure or a laminate structure in which two or more retardation layers are laminated.
[0068] The polarizing plate 100C shown in FIG. 2C includes a polarizing film (primary polarizing film) 10, a protective layer 20, and a pressure-sensitive adhesive layer 40 in this order, and the side of the polarizing film (primary polarizing film) 10 opposite to the side on which the protective layer 20 is provided is an exposed surface. The polarizing plate 100C can be obtained, for example, by providing a pressure-sensitive adhesive layer 40 on the surface of the polarizing plate 100A on the protective layer 20 side. Alternatively, the polarizing plate 100C can also be obtained by providing a pressure-sensitive adhesive layer 40 on the surface of the thermoplastic resin substrate side of a laminate having the above-mentioned [thermoplastic resin substrate / primary polarizing film] configuration. In this case, the thermoplastic resin substrate functions as the protective layer 20.
[0069] Although not shown, it is preferable that a release film is temporarily attached to the surface of the adhesive layer 40 until the polarizing plate is used.
[0070] The protective layer 20 is formed of any suitable film that can be used as a protective layer for a polarizing film. The retardation layer 30 can be, for example, a thermoplastic resin film or a liquid crystal alignment solidified layer. In addition, any suitable adhesive can be used as the adhesive for forming the adhesive layer 40, and among them, an acrylic adhesive having an acrylic polymer as a base polymer is preferably used. Such protective layers, retardation layers, and adhesive layers are well known to those skilled in the art, so detailed descriptions thereof will be omitted.
[0071] A-3. Process for obtaining secondary polarizing film In the process of obtaining the secondary polarizing film, the transmittance of the primary polarizing film is changed by contacting the surface of the primary polarizing film with an aqueous solvent. Specifically, the primary polarizing film is bleached by contacting with the aqueous solvent, thereby obtaining a secondary polarizing film having a desired transmittance.
[0072] As the aqueous solvent, any suitable aqueous solvent can be used as long as it can dissolve the dichroic material from the primary polarizing film. The aqueous solvent can be, for example, water or a mixture of water and a water-soluble organic solvent. Preferred examples of the water-soluble organic solvent include lower monoalcohols having 1 to 4 carbon atoms, such as methanol, ethanol, n-propyl alcohol, and isopropyl alcohol, and polyhydric alcohols, such as glycerin and ethylene glycol.
[0073] The content of the water-soluble organic solvent in the aqueous solvent is, for example, 20% by weight or less, preferably 10% by weight or less, and more preferably 5% by weight or less.
[0074] The method of contacting with the aqueous solvent is not particularly limited, and any appropriate method such as immersion, spraying, coating, etc. can be used. Spraying or coating is preferred for adjusting the transmittance partially, and immersion is preferred for adjusting the transmittance overall.
[0075] The contact time with the aqueous solvent and the temperature of the aqueous solvent during contact can be appropriately set according to the desired change in transmittance. The change in transmittance tends to increase by increasing the contact time or the temperature of the aqueous solvent. The contact time can be, for example, 10 minutes or less, preferably 1 second to 5 minutes, and more preferably 2 seconds to 3 minutes. The temperature of the aqueous solvent can be preferably 20°C to 70°C, more preferably 30°C to 65°C, and even more preferably 40°C to 60°C.
[0076] If necessary, the polarizing film may be dried after contact with the aqueous solvent. The drying temperature may be, for example, 30° C. to 100° C., and preferably 30° C. to 80° C. The moisture content of the polarizing film (secondary polarizing film) after drying is typically 15% by weight or less, preferably 12% by weight or less, more preferably 10% by weight or less, and further preferably 1% by weight to 5% by weight.
[0077] The secondary polarizing film preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The transmittance (single transmittance: Ts) of the secondary polarizing film can be appropriately adjusted depending on the purpose. The transmittance of the secondary polarizing film is preferably 41.5% or more, more preferably 42% or more, and even more preferably 42.5% or more. On the other hand, the transmittance of the secondary polarizing film is, for example, 70% or less, preferably 50% or less, and more preferably 46% or less. In one embodiment, the secondary polarizing film may have a transmittance higher than that of the primary polarizing film by, for example, 0.1% to 1.5%. The polarization degree of the secondary polarizing film is, for example, 90% or more, preferably 92.0% or more, more preferably 94.0% or more, even more preferably 96.0% or more, even more preferably 99.0% or more, even more preferably 99.5% or more, and preferably 99.998% or less. The transmittance and polarization degree are values obtained in the same manner as the transmittance and polarization degree of the primary polarizing film.
[0078] The thickness of the secondary polarizing film is typically 25 μm or less, preferably 12 μm or less, more preferably 1 μm to 8 μm, even more preferably 1 μm to 7 μm, and even more preferably 2 μm to 5 μm. The thickness of the secondary polarizing film can be substantially the same as that of the primary polarizing film.
[0079] A-4. Other processes The method for producing the polarizing plate may further include any appropriate step as necessary. For example, after the step of obtaining a secondary polarizing film, the method may further include a step of changing the transmittance by contacting an aqueous solvent with the surface of the secondary polarizing film. The step of changing the transmittance may be repeated two or more times. In addition, for example, the method may include a step of laminating any appropriate layer (protective layer, retardation layer, adhesive layer, etc.) on the exposed surface of the finally obtained polarizing film (e.g., secondary polarizing film) to protect the exposed surface.
[0080] 3A and 3B are schematic cross-sectional views of an example of a polarizing plate obtained after a step of protecting the exposed surface of the polarizing film. The polarizing plate 100D includes a first protective layer 20a, a polarizing film (secondary polarizing film) 10, a second protective layer 20b, a retardation layer 30, and an adhesive layer 40 in this order. The polarizing plate 100D can be obtained, for example, by providing a second protective layer 20b, a retardation layer 30, and an adhesive layer 40 in this order on the exposed surface of the polarizing film 10 of the polarizing plate 100A (FIG. 2A) that has undergone a step of obtaining a secondary polarizing film. Alternatively, the polarizing plate 100D can be obtained by laminating a first protective layer 20a on the exposed surface of the polarizing film 10 of the polarizing plate 100B (FIG. 2B) that has undergone a step of obtaining a secondary polarizing film.
[0081] The polarizing plate 100E includes a first protective layer 20a, a polarizing film (secondary polarizing film) 10, a second protective layer 20b, and an adhesive layer 40 in this order. In the polarizing plate 100E, the second protective layer 20b may have a desired phase difference and function as a phase difference layer (e.g., a λ / 4 plate) as described later. The polarizing plate 100E can be obtained, for example, by providing the second protective layer 20b and the adhesive layer 40 in this order on the exposed surface of the polarizing film 10 of the polarizing plate 100A (FIG. 2A) that has been subjected to a process of changing the transmittance. Alternatively, the polarizing plate 100E can be obtained by bonding the first protective layer 20a to the exposed surface of the polarizing film 10 of the polarizing plate 100C (FIG. 2C) that has been subjected to a process of changing the transmittance.
[0082] In one embodiment, the adhesive layer 40 is used to attach the polarizing plates 100D and 100E to an image display cell (e.g., a liquid crystal cell, an organic EL cell). In this embodiment, the first protective layer 20a becomes a protective layer (outer protective layer) disposed on the opposite side to the image display cell when the polarizing plate is applied to an image display device, and the second protective layer 20b becomes a protective layer (inner protective layer) disposed on the image display cell side.
[0083] The thickness of the outer protective layer is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm. When a surface treatment is applied, the thickness of the outer protective layer includes the thickness of the surface treatment layer.
[0084] The thickness of the inner protective layer is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and further preferably 10 μm to 60 μm.
[0085] In one embodiment, the inner protective layer is optically isotropic. In this specification, "optically isotropic" means that the in-plane retardation Re(550) is 0 nm to 10 nm, and the thickness direction retardation Rth(550) is -10 nm to +10 nm. Here, "Re(550)" is the in-plane retardation measured with light having a wavelength of 550 nm at 23°C, and is calculated by the formula: Re = (nx-ny) x d. Also, "Rth(550)" is the thickness direction retardation measured with light having a wavelength of 550 nm at 23°C, and is calculated by the formula: Rth(λ) = (nx-nz) x d. Here, "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), "nz" is the refractive index in the thickness direction, and "d" is the thickness (nm) of the layer (film).
[0086] In another embodiment, the inner protective layer is a retardation layer having any appropriate retardation value. The in-plane retardation Re(550) of the inner protective layer in this embodiment can be, for example, 110 nm to 150 nm. By disposing such an inner protective layer such that the angle between its slow axis and the absorption axis of the polarizing film is, for example, 35° to 55°, preferably 38° to 52°, more preferably 40° to 50°, further preferably 42° to 48°, and particularly preferably 44° to 46°, clockwise or counterclockwise, the inner protective layer can function as a circular polarizing plate.
[0087] The retardation layer 30 may be a retardation layer having a desired in-plane retardation and / or thickness retardation depending on the purpose. For example, when the inner protective layer is optically isotropic, the in-plane retardation Re(550) of the retardation layer may be 110 nm to 150 nm. Such a retardation layer may function as a circular polarizer by arranging the retardation layer such that the angle between its slow axis and the absorption axis of the polarizing film is, for example, 35° to 55°, preferably 38° to 52°, more preferably 40° to 50°, further preferably 42° to 48°, and particularly preferably 44° to 46°, clockwise or counterclockwise.
[0088] B. Manufacturing method of image display device The method for producing an image display device according to an embodiment of the present invention includes the steps of: (I) laminating a polarizing plate, which is made of a polyvinyl alcohol-based resin film containing a dichroic material and contains a polarizing film having a moisture content of 15% by weight or less, a protective layer, and an adhesive layer, in this order, on an image display cell via the adhesive layer, and making the surface of the polarizing film opposite to the side on which the protective layer is disposed an exposed surface; and (II) contacting the exposed surface of the polarizing film with an aqueous solvent to change the transmittance. According to this method for producing an image display device, the transmittance of the polarizing film can be adjusted after being attached to the image display cell, and therefore an image display device having a desired brightness can be obtained regardless of individual quality differences in the image display cell, backlight unit, etc.
[0089] B-1. Process (I) The polarizing plate laminated on the image display cell may have any configuration as long as it is made of a polyvinyl alcohol-based resin film containing a dichroic material, contains a polarizing film having a moisture content of 15% by weight or less, a protective layer, and a pressure-sensitive adhesive layer in this order, and the surface of the polarizing film on which the protective layer is not disposed can be exposed. For example, the polarizing plate may be attached to the image display cell in a state where the exposed surface of the polarizing film is protected with a surface protective film, and the surface protective film may be peeled off before contact with an aqueous solvent to expose the polarizing film.
[0090] In one embodiment, the polarizing plate laminated on the image display cell may further include a retardation layer. The polarizing plate laminated on the image display cell may be exemplified by the polarizing plates having the configurations illustrated in Figures 2B and 2C. The polarizing film, protective layer, retardation layer, and adhesive layer included in the polarizing plate may be the same as the primary polarizing film, protective layer, retardation layer, and adhesive layer described in Section A.
[0091] The image display device manufactured by the above manufacturing method can preferably be a liquid crystal display device or an organic EL display device. Therefore, the image display cell can preferably be a liquid crystal cell or an organic EL cell. A plurality of image display devices may be combined to display one image as a whole and used as a digital signage.
[0092] B-2. Process (II) In the step of changing the transmittance, an aqueous solvent is brought into contact with the exposed surface of the polarizing film to change the transmittance. Specifically, the transmittance of the polarizing film can be changed and adjusted to a desired value by decolorizing the dichroic material through contact with the aqueous solvent. The same explanation as in A-3 can be applied to the step of changing the transmittance. In order to prevent the image display cell from coming into contact with the aqueous solvent, coating or spraying can be preferably used as a method of contacting the aqueous solvent. The explanation of the secondary polarizing film in A-3 can be applied to the polarizing film after the transmittance has been changed.
[0093] The method for producing an image display device may further include, as necessary, a step of protecting an exposed surface of the polarizing film after the step of changing the transmittance. The exposed surface of the polarizing film may be protected by laminating a protective layer, a support substrate, or the like on the exposed surface via an adhesive layer such as an adhesive layer or a pressure-sensitive adhesive layer.
[0094] C. How to adjust the transmittance of a polarizing film According to another aspect of the present invention, there is provided a method for adjusting the transmittance of a polarizing film, the method comprising the step of contacting an aqueous solvent with a surface of a polarizing film made of a PVA-based resin film containing a dichroic material and having a moisture content of 15% by weight or less. According to the method for adjusting the transmittance of a polarizing film, the polarizing film is decolorized by contact with the aqueous solvent, and as a result, the transmittance of the polarizing film can be adjusted to a desired value (typically increased).
[0095] As the polarizing film to be brought into contact with the aqueous solvent, the primary polarizing film described in A-1 is preferably used. The same explanation as in A-3 can be applied to the contact between the polarizing film and the aqueous solvent. EXAMPLES
[0096] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified. (1) Thickness The thickness was measured using an interference film thickness meter (Otsuka Electronics Co., Ltd., product name "MCPD-3000"). (2) Single unit transmittance and polarization degree For the laminate (polarizing plate) of the polarizing film and the protective layer obtained in the examples and comparative examples, the single transmittance Ts, parallel transmittance Tp, and crossed transmittance Tc measured from the polarizing film side using an ultraviolet-visible spectrophotometer (Otsuka Electronics Co., Ltd. "LPF-200") were taken as Ts, Tp, and Tc of the polarizing film, respectively. These Ts, Tp, and Tc are Y values measured with a 2-degree visual field (C light source) according to JIS Z8701 and corrected for luminosity. The refractive index of the protective layer was 1.53, and the refractive index of the surface of the polarizing film opposite to the protective layer was 1.53. From the obtained Tp and Tc, the degree of polarization P was calculated according to the following formula. Polarization degree P(%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100 It should be noted that equivalent measurements can also be made using a spectrophotometer such as the "V-7100" manufactured by JASCO Corporation, and it has been confirmed that equivalent measurement results can be obtained regardless of which spectrophotometer is used. (3) Moisture content The primary polarizing film immediately after drying (when stretched as a laminate, the stretched substrate peels off) was cut into a size of 100 mm x 100 mm or more, and the weight before the treatment was measured using an electronic balance. It was then placed in a heating oven maintained at 120°C for 2 hours, and the weight after removal (weight after treatment) was measured, and the moisture content was calculated using the following formula. Moisture content [%] = (weight before treatment - weight after treatment) / weight before treatment x 100
[0097] [Example 1-1] A long roll of a 30 μm thick PVA resin film (manufactured by Kuraray, product name "PE3000") was stretched 2.2 times in the conveying direction while immersed in a 30° C. water bath, and then stretched 3 times based on the original length of the film that was not stretched at all while dyeing it by immersing it in a 30° C. aqueous solution with an iodine concentration of 0.04% by weight and a potassium concentration of 0.3% by weight. Next, this stretched film was further stretched to 3.3 times based on the original length while immersing it in a 30° C. aqueous solution with a boric acid concentration of 3% by weight and a potassium iodide concentration of 3% by weight, and then further stretched to 6 times based on the original length while immersing it in a 60° C. aqueous solution with a boric acid concentration of 4% by weight and a potassium iodide concentration of 5% by weight, and finally dried for 5 minutes in an oven maintained at 60° C. to produce a polarizing film (primary polarizing film) with a thickness of 12 μm. The moisture content of the obtained primary polarizing film was 10% by weight. The single transmittance of the polarizing film was 42.5%. Next, a PVA resin solution (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER (registered trademark) Z-200", resin concentration: 3% by weight) was applied to one side of the polarizing film, and a cycloolefin film (manufactured by Nippon Zeon Co., Ltd., Zeonor, thickness: 25 μm) was attached to obtain a polarizing plate (before treatment) having a configuration of [primary polarizing film / protective layer].
[0098] The polarizing plate (before treatment) was cut to a size of 100 mm x 100 mm, and attached to a glass plate via an acrylic adhesive layer (thickness 15 μm) so that the surface on the primary polarizing film side was exposed. In this state, the plate was immersed in water at 55° C. for 6 minutes. It was then dried at 50° C. for 5 minutes to obtain a polarizing plate (after treatment) having a configuration of [secondary polarizing film / protective layer].
[0099] [Example 1-2] A polarizing plate (after processing) having a [secondary polarizing film / protective layer] structure was obtained in the same manner as in Example 1-1, except that instead of immersing in 55°C water for 6 minutes, the plate was immersed in 55°C water for 9 minutes.
[0100] [Examples 1-3] A polarizing plate (after processing) having a [secondary polarizing film / protective layer] structure was obtained in the same manner as in Example 1-1, except that instead of immersing in 55°C water for 6 minutes, the plate was immersed in 60°C water for 4 minutes.
[0101] [Examples 1-4] A polarizing plate (after processing) having a [secondary polarizing film / protective layer] structure was obtained in the same manner as in Example 1-1, except that instead of immersing in water at 55°C for 6 minutes, the plate was immersed in water at 65°C for 3 minutes.
[0102] [Example 2-1] As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of about 75° C. was used, and one side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a ratio of 9:1, and dissolving the mixture in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched 2.4 times in the machine direction (longitudinal direction) in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the final polarizing plate would be 42.3% (dyeing process). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4% by weight, potassium iodide concentration: 5% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, while drying in an oven maintained at about 90° C., it was brought into contact with a SUS heated roll whose surface temperature was maintained at about 75° C. (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 2%. In this way, a polarizing film (primary polarizing film) having a moisture content of 4.5% by weight and a thickness of 5 μm was formed on the resin substrate, and a cycloolefin film (Zeonor, manufactured by Zeon Corporation, thickness: 25 μm) was bonded to the surface of the primary polarizing film using a UV-curable adhesive (thickness: 1.0 μm).The resin substrate was then peeled off to obtain a polarizing plate (before processing) having a configuration of [primary polarizing film / protective layer].
[0103] The polarizing plate (before treatment) was cut to a size of 100 mm x 100 mm, and attached to a glass plate via an acrylic adhesive layer (thickness 15 μm) so that the surface on the primary polarizing film side was exposed, and in this state, immersed in water at 50° C. for 9 minutes. Then, by drying at 50° C. for 5 minutes, a polarizing plate (after treatment) having a configuration of [secondary polarizing film / protective layer] was obtained.
[0104] [Example 2-2] A polarizing plate (after processing) having a [secondary polarizing film / protective layer] structure was obtained in the same manner as in Example 2-1, except that instead of immersing in 50°C water for 9 minutes, the plate was immersed in 55°C water for 3 minutes.
[0105] [Example 2-3] A polarizing plate (after processing) having a [secondary polarizing film / protective layer] structure was obtained in the same manner as in Example 2-1, except that instead of immersing in 50°C water for 9 minutes, the plate was immersed in 60°C water for 1 minute.
[0106] [Example 2-4] A polarizing plate (after processing) having a [secondary polarizing film / protective layer] structure was obtained in the same manner as in Example 2-1, except that instead of immersing in 50°C water for 9 minutes, the plate was immersed in 60°C water for 2 minutes.
[0107] [Example 2-5] A polarizing plate (after processing) having a [secondary polarizing film / protective layer] structure was obtained in the same manner as in Example 2-1, except that instead of immersing in 50°C water for 9 minutes, the plate was immersed in 60°C water for 3 minutes.
[0108] [Example 3-1] A polarizing plate (before treatment) having a structure of [primary polarizing film / protective layer] was obtained in the same manner as in Example 2-1, except that the iodine concentration of the dye bath was changed and the transmittance of the obtained polarizing film was adjusted to 44.3%. The moisture content of the obtained primary polarizing film was 4.5% by weight.
[0109] The polarizing plate (before treatment) was cut to a size of 100 mm x 100 mm, and attached to a glass plate via an acrylic adhesive layer (thickness 15 μm) so that the surface on the primary polarizing film side was exposed, and in this state, immersed in water at 50° C. for 6 minutes. Then, by drying at 50° C. for 5 minutes, a polarizing plate (after treatment) having a configuration of [secondary polarizing film / protective layer] was obtained.
[0110] [Example 3-2] A polarizing plate (after processing) having a [secondary polarizing film / protective layer] structure was obtained in the same manner as in Example 3-1, except that instead of immersing in 50°C water for 6 minutes, the plate was immersed in 55°C water for 3 minutes.
[0111] The transmittance and polarization degree of the polarizing plate (before treatment) and the polarizing plate (after treatment) obtained in the above example were measured. The results are shown in Table 1. [Table 1]
[0112] As is clear from Table 1, according to the manufacturing method of the examples, the transmittance of the polarizing film can be changed after a protective layer is laminated to produce a polarizing plate. [Industrial Applicability]
[0113] The method for producing a polarizing plate of the present invention is suitably used in the production of an image display device. [Explanation of symbols]
[0114] 10 Polarizing film 20 protective layer 30 Retardation layer 40 Adhesive layer 100 Polarizing Plate
Claims
1. A step of subjecting the polyvinyl alcohol-based resin film to a dyeing treatment and a stretching treatment in an aqueous boric acid solution, and then drying the film until the moisture content is 15% by weight or less to obtain a primary polarizing film; and a step of contacting a surface of the primary polarizing film with an aqueous solvent to change the transmittance and obtain a secondary polarizing film; in that order, The method for producing a polarizing plate, wherein the secondary polarizing film has a single-piece transmittance that is 0.1% to 3.2% higher than that of the primary polarizing film.
2. The method for producing a polarizing plate according to claim 1 , wherein the aqueous solvent is brought into contact with an exposed surface of the primary polarizing film in a state in which one surface is entirely exposed and the other surface is entirely protected.
3. the step of obtaining the primary polarizing film includes subjecting a polyvinyl alcohol-based resin film containing a halide and a polyvinyl alcohol-based resin, in a state of being laminated with a long thermoplastic resin substrate, to an air-assisted stretching treatment, a dyeing treatment, a stretching treatment in an aqueous boric acid solution, and a drying shrinkage treatment in this order; 3. The method for producing a polarizing plate according to claim 1 or 2, wherein the drying and shrinking treatment comprises heating the laminate while transporting it in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction and drying the laminate until the moisture content of the polyvinyl alcohol-based resin film becomes 15% by weight or less.
4. The method for producing a polarizing plate according to claim 3 , wherein the halide is iodide or sodium chloride.
5. The method for producing a polarizing plate according to claim 1 , wherein the primary polarizing film has a thickness of 12 μm or less.
6. a step of laminating a polarizing plate including a polarizing film, which is made of a polyvinyl alcohol-based resin film containing a dichroic material and has a moisture content of 15% by weight or less, a protective layer, and a pressure-sensitive adhesive layer, in this order, on an image display cell via the pressure-sensitive adhesive layer, and making the surface of the polarizing film opposite to the side on which the protective layer is disposed an exposed surface; contacting an exposed surface of the polarizing film with an aqueous solvent to change the transmittance; A method for manufacturing an image display device, comprising the steps of:
7. The method for manufacturing an image display device according to claim 6 , wherein the image display device is a liquid crystal display device or an organic EL display device.
8. A method for adjusting the transmittance of a polarizing film, the method comprising the step of contacting an aqueous solvent with a surface of a polarizing film which is made of a polyvinyl alcohol-based resin film containing a dichroic material and has a moisture content of 15% by weight or less, The method for adjusting the single transmittance of the polarizing film is made 0.1% to 3.2% higher than that before contact with the aqueous solvent.
Citation Information
Patent Citations
Quarter-wave plate, circularly polarizing plate and display device
JP2002311239A
Composite optical retardation plate, circularly polarizing plate and liquid crystal display, organic el display device
JP2002372622A
Long adhesive film
JP2016027136A
Polarizer, polarization plate, and image display device
WO2015163401A1
Polarizing film and polarizing plate with retardation layer
WO2019235107A1