Friction Transmission Belt

A friction transmission belt with a fabric layer of high-tensile cellulose fibers like hemp and polyester composite yarns addresses the issues of water injection and abrasion resistance, providing long-lasting durability and cost-effectiveness.

JP7555992B2Active Publication Date: 2024-09-25MITSUBOSHI BELTING LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022069324
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-26
Filing Date
2022-04-20
Publication Date
2024-09-25
Estimated Expiration
2042-04-20

AI Technical Summary

Technical Problem

Existing friction transmission belts face challenges in maintaining water injection resistance and abrasion resistance over time, particularly due to the use of cotton fibers, which have low abrasion resistance and increase costs when combined with polyamide fibers.

Method used

The friction transmission surface is covered with a fabric containing natural cellulose fibers with a tensile strength of 4.5 cN/dtex or more, preferably hemp, and optionally blended with other natural cellulose fibers like cotton, along with polyester composite yarns, to enhance water absorption and abrasion resistance.

Benefits of technology

The solution maintains water injection resistance and abrasion resistance for a long period while reducing costs by using a combination of hemp and other cellulose fibers, ensuring durability and sound performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555992000003
    Figure 0007555992000003
  • Figure 0007555992000004
    Figure 0007555992000004
  • Figure 0007555992000005
    Figure 0007555992000005
Patent Text Reader

Abstract

To provide a friction transmission belt having a fabric-covered pulley contact portion, where the friction transmission belt can retain water-injection sounding resistance for a long time, and the friction transmission belt can be provided at low cost.SOLUTION: A V-ribbed belt 1 has a friction transmission face covered with a fabric 6, the fabric 6 containing a natural cellulose fiber with tensile strength of 4.5 cN / dtex or more, and a polyester composite yarn.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a friction transmission belt having a friction transmission surface covered with fabric. [Background technology]

[0002] Power transmission belts are widely used as a means of power transmission. Compared to gears and chains, power transmission belts have advantages such as light weight, low noise, high freedom in layout, and easy maintenance, and are used in a variety of fields including automobiles and agricultural machinery.

[0003] Power transmission belts are broadly classified into friction power transmission belts and interlocking power transmission belts based on the difference in the mechanism of power transmission. Interlocking power transmission belts include toothed belts and double-sided toothed belts. Friction power transmission belts include flat belts, wrapped V-belts, raw edge V-belts, and V-ribbed belts. Raw edge V-belts include raw edge cogged V-belts, which have irregularities (cogs) on the inner circumferential surface to improve flexibility, and raw edge double cogged V-belts, which have cogs on both the inner and outer circumferential surfaces.

[0004] These power transmission belts are formed by embedding a core (core wire, tensile member) such as a twisted cord in an elastic body such as rubber, elastomer, etc. Furthermore, some power transmission belts have a structure in which all or part of the belt surface, such as the contact portion with the pulley, is covered with a fabric (reinforcing fabric) such as a woven fabric or knitted fabric.

[0005] For example, Patent Document 1 discloses a V-ribbed belt in which a frictional power transmission surface is covered with a knitted fabric knitted with a polyester composite yarn and a cellulose-based natural spun yarn, the polyester composite yarn being a bulky processed yarn, and the knitting ratio of the cellulose-based natural spun yarn being equal to or greater than that of the polyester composite yarn. Patent Document 2 discloses a V-ribbed belt in which a frictional power transmission surface is covered with a weft-knitted multi-layered knitted fabric containing a cellulose-based natural spun yarn, a polyester composite yarn, and a polyamide yarn, and in which at least the cellulose-based natural spun yarn and the polyamide yarn are arranged in layers on the frictional power transmission surface side. It is described that the weft-knitted multi-layered knitted fabric contains a cellulose-based natural spun yarn, thereby improving the water-pour noise resistance, and contains a polyamide yarn, thereby suppressing wear of the cellulose-based natural spun yarn, thereby maintaining the water-pour noise resistance for a long period of time. Patent Document 3 discloses a frictional power transmission belt covered with a surface-coating fabric formed of a composite spun yarn containing a low water-absorbent filament fiber and a high water-absorbent staple fiber. This friction power transmission belt is described as having high transmission capacity and low wear rate even in a water-submerged environment. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-209028 A [Patent Document 2] JP 2018-197605 A [Patent Document 3] International Publication No. 2019 / 193881 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in Patent Documents 1 to 3, cotton is used as the absorbent fiber, but while cotton has excellent absorbency, it has the drawback of low abrasion resistance. In addition, in Patent Documents 2 and 3, it is thought that the effect of suppressing the abrasion of cotton is obtained by combining cotton with polyamide fiber, but there is a problem that the use of polyamide fiber increases the cost, and further improvement is required in the durability of the water-pouring noise resistance.

[0008] Therefore, an object of the present invention is to provide a friction transmission belt having a portion that comes into contact with a pulley covered with fabric, which can maintain its resistance to water-pouring noise for a long period of time, and to provide this friction transmission belt at low cost. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention provides a friction transmission surface covered with a fabric, The fabric is a friction power transmission belt, characterized in that it contains natural cellulose fibers having a tensile strength of 4.5 cN / dtex or more, and polyester-based composite yarn.

[0010] According to the above-mentioned configuration, the friction transmission belt in which the friction transmission surface, which is the portion that comes into contact with the pulley, is covered with fabric can maintain water absorption (resistance to noise caused by water pouring) and wear resistance for a long period of time.

[0011] In the friction power transmission belt of the present invention, the natural cellulose fibers contained in the fabric may be exclusively hemp.

[0012] According to the above-mentioned configuration, the friction transmission belt can maintain its water absorption (water-pouring noise resistance) for a long period of time and its wear resistance for an even longer period of time.

[0013] Moreover, in the above-mentioned friction transmission belt of the present invention, the fabric may contain hemp as the natural cellulose fiber, and further contain natural cellulose fibers other than the hemp.

[0014] According to the above configuration, by including natural cellulose fibers other than hemp in the fabric in addition to hemp, it is possible to reduce costs while fully maintaining an acceptable range of abrasion resistance for a friction transmission belt, compared to a case in which only hemp is used as the natural cellulose fiber contained in the fabric.

[0015] In the above-mentioned friction transmission belt of the present invention, the natural cellulose fiber other than hemp may be cotton.

[0016] According to the above configuration, by using relatively inexpensive cotton instead of natural cellulose fibers other than hemp, procurement and manufacturing costs can be further reduced.

[0017] In the above-mentioned friction transmission belt of the present invention, the fabric may be knitted from a blended yarn obtained by blending the hemp staple fibers with staple fibers of a natural cellulose fiber other than the hemp.

[0018] According to the above configuration, by using hemp staple fibers and staple fibers of natural cellulose fibers other than hemp in the form of a blended yarn, it is possible to produce a fabric knitted in a state in which hemp and natural cellulose fibers other than hemp are uniformly dispersed, thereby enhancing the effect of suppressing wear of the natural cellulose fibers other than hemp, and making it possible to maintain water-pouring noise resistance for a longer period of time.

[0019] Moreover, in the friction power transmission belt of the present invention, the blended yarn may have a count of 20 to 60.

[0020] If the blended yarn is too thin, there is a risk of reduced abrasion resistance, whereas if the blended yarn is too thick, the balance with the polyester composite yarn will be poor, resulting in reduced elongation and physical properties of the fabric, and there is a risk of the rubber composition bleeding out or poor rib shape. Therefore, by setting the thickness of the blended yarn to 20 to 60 count, it is possible to improve the abrasion resistance of the friction transmission belt while reducing the decrease in elongation and physical properties of the fabric, and to suppress the bleeding of the rubber composition and the occurrence of defective rib shape. Effect of the Invention

[0021] A friction transmission belt having a portion that comes into contact with a pulley covered with fabric can be provided that is resistant to water-injected noise for a long period of time and can be provided at low cost. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a schematic perspective view illustrating an example of a belt transmission device using a V-ribbed belt according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of the V-ribbed belt taken along the section AA in FIG. [Diagram 3] FIG. 3 is a conceptual diagram illustrating a manufacturing method of a V-ribbed belt. [Figure 4] FIG. 4 is a conceptual diagram illustrating the friction coefficient measurement test in a dry state (a) and in a wet state (b). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] An example of an embodiment of the present invention will be described below with reference to the drawings. Fig. 1 shows an example of a belt transmission device for driving an accessory using a V-ribbed belt 1, which is a type of friction transmission belt, according to the present invention. This belt transmission device is the simplest example, including a drive pulley 21 and a driven pulley 22, with the V-ribbed belt 1 wound between the drive pulley 21 and the driven pulley 22. The endless V-ribbed belt 1 has a plurality of V-shaped ribs 2 formed on its inner periphery that extend in the belt circumferential direction, and the outer periphery of the drive pulley 21 and the driven pulley 22 has a plurality of V-shaped grooves 23 into which the ribs 2 of the V-ribbed belt 1 fit.

[0024] (V-ribbed belt 1 configuration) As shown in FIG. 2, the V-ribbed belt 1 includes a tension layer 3 forming the outer circumferential belt back surface, a compression layer 4 provided on the inner circumferential side of the tension layer 3, and a core wire 5 embedded between the tension layer 3 and the compression layer 4 and extending in the belt circumferential direction. A plurality of V-shaped rib portions 2 extending in the belt circumferential direction are formed in the compression layer 4, and the surface of the rib portion 2 serving as a friction transmission surface is covered with a fabric 6. As described later, both the tension layer 3 and the compression layer 4 are formed of a rubber composition. If necessary, an adhesive layer may be provided between the tension layer 3 and the compression layer 4. This adhesive layer is provided for the purpose of improving the adhesion of the core wire 5 to the tension layer 3 and the compression layer 4, but is not essential. The adhesive layer may be in a form in which the entire core wire 5 is embedded in the adhesive layer, or in a form in which the core wire 5 is embedded between the adhesive layer and the tension layer 3 or between the adhesive layer and the compression layer 4.

[0025] (Tension layer 3 and compression layer 4) Examples of the rubber component of the rubber composition forming the compression layer 4 include vulcanizable or crosslinkable rubbers, such as diene rubbers (natural rubber, isoprene rubber, butadiene rubber, chloroprene rubber, styrene butadiene rubber, acrylonitrile butadiene rubber, hydrogenated nitrile rubber, mixed polymers of hydrogenated nitrile rubber and metal salts of unsaturated carboxylic acids, etc.), ethylene-α-olefin elastomers, chlorosulfonated polyethylene rubber, alkylated chlorosulfonated polyethylene rubber, epichlorohydrin rubber, acrylic rubber, silicone rubber, urethane rubber, and fluororubber.

[0026] Among these, a rubber composition containing sulfur or an organic peroxide is used to form an unvulcanized rubber layer, and the unvulcanized rubber layer is preferably vulcanized or crosslinked. In particular, ethylene-α-olefin elastomers (ethylene-α-olefin rubbers) are preferred because they do not contain harmful halogens, have ozone resistance, heat resistance, and cold resistance, and are economically advantageous. Examples of ethylene-α-olefin elastomers include ethylene-α-olefin rubbers (ethylene-propylene rubbers, etc.) and ethylene-α-olefin-diene rubbers (ethylene-propylene-diene copolymers, etc.). Examples of α-olefins include propylene, butene, pentene, methylpentene, hexene, and octene. These α-olefins can be used alone or in combination of two or more. Examples of diene monomers that are raw materials for these include non-conjugated diene monomers, such as dicyclopentadiene, methylenenorbornene, ethylidenenorbornene, 1,4-hexadiene, and cyclooctadiene. These diene monomers can be used alone or in combination of two or more kinds.

[0027] In the ethylene-α-olefin elastomer, the ratio of ethylene to α-olefin (the mass ratio of the former / the latter) is preferably in the range of 40 / 60 to 90 / 10, preferably 45 / 55 to 85 / 15, and more preferably 55 / 45 to 80 / 20. The ratio of diene can be selected from the range of 4 to 15% by mass, for example, 4.2 to 13% by mass, and preferably 4.4 to 11.5% by mass. The iodine value of the ethylene-α-olefin elastomer containing the diene component is, for example, in the range of 3 to 40, preferably 5 to 30, and more preferably 10 to 20. If the iodine value is too small, the vulcanization of the rubber composition becomes insufficient, and wear and adhesion tend to occur, and if the iodine value is too large, the scorch of the rubber composition becomes short, making it difficult to handle, and the heat resistance tends to decrease. The iodine value is measured by adding an excess of iodine to the sample to be measured, allowing it to react completely (reaction between iodine and unsaturated bonds), and then quantifying the amount of remaining iodine by oxidation-reduction titration.

[0028] Examples of organic peroxides that crosslink the unvulcanized rubber layer include diacyl peroxides, peroxy esters, dialkyl peroxides (dicumyl peroxide, t-butylcumyl peroxide, 1,1-di-butylperoxy-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(t-butylperoxy)-hexane, 1,3-bis(t-butylperoxy-isopropyl)benzene, di-t-butyl peroxide, etc.). These organic peroxides can be used alone or in combination of two or more. Furthermore, the organic peroxides have a half-life of 1 minute due to thermal decomposition in a temperature range of 150°C to 250°C, preferably about 175°C to 225°C.

[0029] The proportion of the vulcanizing agent or crosslinking agent (especially organic peroxide) in the unvulcanized rubber layer is 1 to 10 parts by mass, preferably 1.2 to 8 parts by mass, and more preferably 1.5 to 6 parts by mass, calculated as solid content per 100 parts by mass of the rubber component (such as ethylene-α-olefin elastomer).

[0030] The rubber composition may contain a vulcanization accelerator. Examples of the vulcanization accelerator include thiuram-based accelerators, thiazole-based accelerators, sulfenamide-based accelerators, bismaleimide-based accelerators, and urea-based accelerators. These vulcanization accelerators can be used alone or in combination of two or more. The ratio of the vulcanization accelerator (meaning the total amount when multiple types are combined, and the same applies hereinafter when multiple types are combined) is 0.5 to 15 parts by mass, preferably 1 to 10 parts by mass, and more preferably 2 to 5 parts by mass, based on the solid content, relative to 100 parts by mass of the rubber component.

[0031] In addition, the rubber composition may further contain a co-crosslinking agent (crosslinking aid or co-vulcanizing agent) in order to increase the degree of crosslinking and prevent adhesion wear and the like. Examples of the co-crosslinking agent include conventional crosslinking aids, such as polyfunctional (iso)cyanurates (triallyl isocyanurate, triallyl cyanurate, etc.), polydiene (1,2-polybutadiene, etc.), metal salts of unsaturated carboxylic acids (zinc (meth)acrylate, magnesium (meth)acrylate, etc.), oximes (quinone dioxime, etc.), guanidines (diphenyl guanidine, etc.), polyfunctional (meth)acrylates (ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, etc.), bismaleimides (N,N'-m-phenylene bismaleimide, etc.). These crosslinking aids can be used alone or in combination of two or more. The proportion of the crosslinking aid is 0.01 to 10 parts by mass, preferably 0.05 to 8 parts by mass, based on 100 parts by mass of the rubber component, calculated as solid content.

[0032] The rubber composition may contain short fibers as necessary. Examples of short fibers include cellulosic fibers (cotton, rayon, etc.), polyester fibers (PET, PEN fibers, etc.), aliphatic polyamide fibers (nylon 6 fibers, nylon 66 fibers, nylon 46 fibers, etc.), aromatic polyamide fibers (p-aramid fibers, m-aramid fibers, etc.), vinylon fibers, polyparaphenylene benzobisoxazole (PBO) fibers, etc. These short fibers may be subjected to a conventional adhesion treatment or surface treatment, for example, treatment with RFL liquid, etc., in order to improve dispersibility and adhesiveness in the rubber composition. The proportion of the short fibers is 1 to 50 parts by mass, preferably 5 to 40 parts by mass, and more preferably 10 to 35 parts by mass, based on 100 parts by mass of the rubber component.

[0033] Furthermore, the rubber composition may contain, as necessary, conventional additives such as vulcanization aids, vulcanization retarders, reinforcing agents (carbon black, silicon oxides such as hydrated silica, etc.), fillers (clay, calcium carbonate, talc, mica, etc.), metal oxides (zinc oxide, magnesium oxide, calcium oxide, barium oxide, iron oxide, copper oxide, titanium oxide, aluminum oxide, etc.), plasticizers (oils such as paraffinic oil, naphthenic oil, process oil, etc.), processing agents or processing aids (stearic acid, stearic acid metal salts, wax, paraffin, fatty acid amides, etc.), age inhibitors (antioxidants, heat age inhibitors, flex crack inhibitors, ozonation inhibitors, etc.), colorants, tackifiers, coupling agents (silane coupling agents, etc.), stabilizers (ultraviolet absorbers, antioxidants, ozonation inhibitors, heat stabilizers, etc.), lubricants (graphite, molybdenum disulfide, ultra-high molecular weight polyethylene, etc.), flame retardants, antistatic agents, etc. The metal oxide may act as a crosslinking agent. These additives may be used alone or in combination of two or more. The proportions of these additives may be selected from the conventional ranges depending on the type. For example, the proportion of the reinforcing agent (carbon black, silica, etc.) is 10 to 200 parts by mass (preferably 20 to 150 parts by mass), the proportion of the metal oxide (zinc oxide, etc.) is 1 to 15 parts by mass (preferably 2 to 10 parts by mass), the proportion of the plasticizer (oils such as paraffin oil, etc.) is 1 to 30 parts by mass (preferably 5 to 25 parts by mass), and the proportion of the processing agent (stearic acid, etc.) is 0.1 to 5 parts by mass (preferably 0.5 to 3 parts by mass) per 100 parts by mass of the rubber component.

[0034] The tension layer 3 may be formed of the same rubber composition as the compression layer 4 (a rubber composition containing a rubber component such as ethylene-α-olefin elastomer) or may be formed of a fabric (reinforcing fabric) such as canvas. Examples of reinforcing fabrics include woven fabrics, wide-angle canvases, knitted fabrics, and nonwoven fabrics. Among these, woven fabrics woven in a plain weave, twill weave, satin weave, and other forms, and wide-angle canvases and knitted fabrics with a crossing angle between the warp and weft threads of about 90° to 130° are preferred. The same fibers as the short fibers can be used as the fibers constituting the reinforcing fabric. The reinforcing fabric may be treated (dipped, etc.) with an RFL liquid and then coated to form a rubber-attached canvas.

[0035] The tension layer 3 is preferably formed of the same rubber composition as the compression layer 4. The rubber component of this rubber composition often uses the same type or rubber of the same system as the rubber component of the compression layer 4. The proportions of additives such as vulcanizing agents or crosslinking agents, co-crosslinking agents, vulcanization accelerators, etc. can also be selected from the same ranges as the rubber composition of the compression layer 4.

[0036] The rubber composition of the tension layer 3 may contain short fibers similar to those of the compression layer 4 in order to suppress the generation of abnormal noise due to adhesion of the back rubber during back drive. The short fibers may be linear or partially bent (for example, milled fibers described in JP 2007-120507 A). When the V-ribbed belt 1 runs, cracks may occur in the tension layer 3 in the belt circumferential direction, which may cause the V-ribbed belt 1 to break. This can be prevented by orienting the short fibers in the belt width direction or random directions. In addition, in order to suppress the generation of abnormal noise during back drive, an uneven pattern may be provided on the surface of the tension layer 3 (back of the belt). Examples of uneven patterns include a knitted fabric pattern, a woven fabric pattern, a woven sudare fabric pattern, and an embossed pattern (for example, a dimple shape), and the size and depth are not particularly limited.

[0037] (Core 5) The core wire 5 is not particularly limited, and may be a cord formed of polyester fiber (polybutylene terephthalate fiber, polyethylene terephthalate fiber, polytrimethylene terephthalate fiber, polyethylene naphthalate fiber, etc.), aliphatic polyamide (nylon) fiber (nylon 6 fiber, nylon 66 fiber, nylon 46 fiber, etc.), aromatic polyamide (aramid) fiber (copolyparaphenylene-3,4'-oxydiphenylene-terephthalamide fiber, poly-p-phenylene terephthalamide fiber, etc.), polyarylate fiber, glass fiber, carbon fiber, PBO fiber, etc. These fibers may be used alone or in combination of two or more. These fibers are appropriately selected according to the expansion coefficient of the flexible jacket 51 described later. For example, in the case of high elongation such as an expansion coefficient exceeding 2%, polyester fiber (particularly low elasticity polybutylene terephthalate fiber) and nylon fiber (particularly nylon 66 fiber and nylon 46 fiber) having a low elastic modulus are preferable. This is because, with fibers having a high elastic modulus such as aramid fibers and PBO fibers, the fibers cannot stretch sufficiently even when the flexible jacket 51 expands, causing the pitch line of the core wires 5 embedded in the V-ribbed belt 1 to become unstable and preventing the formation of an appropriate shape for the rib portion 2. For this reason, when using fibers having a high elastic modulus, it is preferable to set the expansion rate of the flexible jacket 51 low (for example, about 1%).

[0038] (Fabric 6) The fabric 6 may be any fabric including woven fabric, wide-angle canvas, nonwoven fabric, knitted fabric, etc., and it is preferable to use knitted fabric, particularly weft-knitted multi-layered fabric, as necessary. Weft-knitted fabric has excellent elasticity, so it can be easily attached to the friction transmission surface formed with unevenness by the rib portion 2 (the shape of the rib portion 2 is less likely to be deformed). In addition, by using a multi-layered knitted fabric, it is possible to more reliably prevent the rubber component of the compression layer 4 from seeping out, and the desired characteristics can be obtained by changing the exposed ratio of the yarn between the friction transmission surface side and the compression layer 4 side. Examples of weft-knitted multi-layered fabrics that are knitted in multiple layers by weft knitting include smooth knit, interlock knit, double rib knit, single pique knit, ponte Roma knit, Milano rib knit, double jersey knit, and pique knit (front pique, back pique, double pique).

[0039] The fabric 6 is knitted to contain natural cellulose fibers having a tensile strength of 4.5 cN / dtex or more and polyester composite yarns. The fabric 6 contains natural cellulose fibers having a tensile strength of 4.5 cN / dtex or more, which allows the fabric 6 to have both water absorption and abrasion resistance. Furthermore, the fabric 6 contains polyester composite yarns, which allows the rubber composition forming the compression layer 4 to be prevented from seeping out onto the friction transmission surface.

[0040] For natural cellulose fibers with a tensile strength of 4.5 cN / dtex or more, the fiber length is preferably about 1 to 200 mm, particularly 10 to 50 mm, because if the fiber length is too short, the abrasion resistance may decrease, and if the fiber length is too long, the water absorbency may decrease.

[0041] Furthermore, the fiber diameter of natural cellulose fibers having a tensile strength of 4.5 cN / dtex or more is preferably about 5 to 100 μm, particularly 10 to 30 μm, because if the fiber diameter is too small, the abrasion resistance may decrease, and if the fiber diameter is too large, the water absorbency may decrease.

[0042] The tensile strength of natural cellulose fibers is measured according to JIS L1069 (2002) by measuring the tensile strength of a single fiber and converting it into a value per dtex. The pulling speed is 1 mm / min.

[0043] As the natural cellulose fiber having a tensile strength of 4.5 cN / dtex or more contained in the fabric 6, hemp is preferable, and specifically, bast fibers such as hemp, ramie, flax, linen, jute, and kenaf, and vein fibers such as Manila hemp and sisal can be used. In particular, flax is preferable because it has a good balance of abrasion resistance, water absorbency, and cost.

[0044] The fabric 6 may contain other kinds of natural cellulose fibers in addition to hemp as the above-mentioned natural cellulose fiber having a tensile strength of 4.5 cN / dtex or more. For example, examples of natural cellulose fibers other than hemp include bamboo fiber, sugarcane fiber, seed hair fiber (cotton fiber (cotton linter), kapok, etc.), wool, silk, animal-derived cellulose fibers such as sea squirt cellulose, bacterial cellulose fiber, and algae cellulose.

[0045] Here, it is preferable to use only hemp as the natural cellulose fiber contained in the fabric 6 from the viewpoint of improving abrasion resistance. That is, it is preferable that the fabric 6 is composed only of hemp and polyester composite yarn. However, since hemp is relatively expensive, the cost can be reduced by including natural cellulose fibers other than hemp in the fabric 6 in addition to hemp within a range in which a decrease in abrasion resistance can be tolerated. In particular, it is preferable to use cotton, which has high water absorption and is inexpensive as a natural cellulose fiber other than hemp, in combination with hemp. Note that the tensile strength of cotton is less than 4.5 cN / dtex, so it is not an essential component in the fabric 6 of the V-ribbed belt 1 of this embodiment.

[0046] When hemp and natural cellulose fibers other than hemp are used in combination in the fabric 6, they can be used as separate yarns. In this case, it is preferable to use the hemp staple fibers and the natural cellulose fibers other than hemp staple fibers in the form of a blended yarn. For example, the fabric 6 is knitted with a blended yarn in which hemp staple fibers and cotton staple fibers are blended. By knitting the fabric 6 in the form of a blended yarn in this way, the hemp and the natural cellulose fibers other than hemp are more uniformly dispersed, so that the effect of suppressing the wear of the natural cellulose fibers other than hemp is enhanced, and the water-pouring noise resistance can be maintained for a long period of time. In addition, the hemp and cotton blended yarn is in a state where hemp staple fibers and cotton staple fibers are blended, and hemp and cotton staple fibers are not present in the form of long fibers. In this way, by blending the hemp and cotton staple fibers, the hemp and cotton are more uniformly dispersed, improving the wear resistance.

[0047] In addition, in a blended yarn obtained by blending hemp staple fibers and cotton staple fibers, the ratio (mass ratio) of hemp to cotton can be selected from the range of about cotton / hemp = 1 / 99 to 80 / 20. A high ratio of hemp improves abrasion resistance but increases costs, while a high ratio of cotton reduces costs but may reduce abrasion resistance. From the viewpoint of being able to reduce costs while fully maintaining an acceptable range of abrasion resistance, the ratio (mass ratio) of hemp to cotton is preferably cotton / hemp = 30 / 70 to 80 / 20 (particularly 50 / 50 to 80 / 20), and more preferably 60 / 40 to 80 / 20 (particularly 65 / 35 to 75 / 25).

[0048] The blended yarn and spun yarn constituting the fabric 6 preferably have a count of 20 to 60, and more preferably have a count of 30 to 50 (particularly 30 to 40). If the yarn is too thin, there is a risk of reduced abrasion resistance, whereas if the yarn is too thick, the balance with the polyester composite yarn will be poor, resulting in reduced elongation and physical properties of the fabric, and there is a risk of the rubber composition bleeding out or poor rib shape. Therefore, by setting the thickness of the blended yarn and spun yarn constituting the fabric 6 to 20 to 60 count, it is possible to improve the abrasion resistance of the friction transmission belt while reducing the decrease in the elongation and physical properties of the fabric, and to suppress the bleeding of the rubber composition and the occurrence of defective rib shape. In this application, the thickness of blended yarns and spun yarns is expressed in terms of cotton count, regardless of the type of fiber (cotton, linen, nylon, etc.). Cotton count is defined as a thread that weighs 1 pound (453.6 grams) and is 840 yards (768.1 meters) long as number 1, with a count of 30 being a thread that weighs 1 pound and is 840 x 30 yards long, and a count of 50 being a thread that weighs 1 pound and is 840 x 50 yards long. In other words, the higher the number, the thinner the thread.

[0049] In addition, bulky processed yarn can be used as the polyester composite yarn contained in the fabric 6. Bulky processed yarn is processed yarn that has a large cross-sectional bulk by causing the fibers to shrink (shrink) or by covering the core yarn with another yarn. Bulky processed yarn includes conjugate yarn, covered yarn, shrink-processed yarn, woolly processed yarn, taslan processed yarn, and interlaced processed yarn, but conjugate yarn and covered yarn are preferred as the polyester composite yarn that is a bulky processed yarn.

[0050] The conjugate yarn preferably has a cross-sectional structure in which two or more polymers with different thermal shrinkage rates are bonded together in the fiber axis direction. When heat is applied to a conjugate yarn having such a structure during production or processing, shrinkage occurs due to the difference in the shrinkage rate (thermal shrinkage rate) of each polymer, resulting in a bulky yarn. For example, there is a composite yarn (PTT / PET conjugate yarn) in which polytrimethylene terephthalate (PTT) and polyethylene terephthalate (PET) are conjugated, and a composite yarn (PBT / PET conjugate yarn) in which polybutylene terephthalate (PBT) and polyethylene terephthalate (PET) are conjugated. As described above, by using a conjugate yarn containing polyethylene terephthalate (PET) as a polyester-based composite yarn, the elasticity, bulkiness, and abrasion resistance of the fabric 6 can be improved. In addition, the conjugate yarn containing polyethylene terephthalate is easily available, so the cost can be reduced. In addition, covered yarn is a yarn in which the bulk of the cross section of the entire yarn is increased by covering (covering) the periphery of the core yarn with another yarn. For example, there is a composite yarn (PET / PU covered yarn) in which a polyurethane (PU) yarn with excellent elasticity is used as the core and the surface is covered with polyethylene terephthalate (PET), and a composite yarn (PA / PU covered yarn) in which a PU core is covered with polyamide (PA). Among these composite yarns, a PTT / PET conjugate yarn with excellent elasticity and abrasion resistance is preferred.

[0051] In addition, a surfactant or a hydrophilic softener can be contained or attached to the fabric 6 as a hydrophilic treatment agent. When a hydrophilic treatment agent is contained or attached to the fabric 6 in this way, when water droplets adhere to the friction transmission surface (fabric 6), the water droplets quickly wet and spread over the hydrophilically treated surface of the fabric 6 to form a water film, and are further absorbed by the cellulose-based natural spun yarn of the fabric 6, so that the water film disappears on the friction transmission surface. Therefore, the decrease in the friction coefficient of the friction transmission surface in a wet state is further suppressed.

[0052] As the hydrophilic treatment agent, a surfactant or a hydrophilic softener can be used. As a method for incorporating or attaching these hydrophilic treatment agents to the fabric 6, a method for spraying the hydrophilic treatment agent on the fabric 6, a method for coating the hydrophilic treatment agent on the fabric 6, or a method for immersing the fabric 6 in the hydrophilic treatment agent can be adopted. In addition, when using a surfactant as the hydrophilic treatment agent, a method for incorporating the surfactant in the fabric 6 by applying the surfactant to the surface of a cylindrical outer mold having a plurality of rib patterns engraved on the inner peripheral surface during the production of the V-ribbed belt 1 and vulcanizing the molded product can also be adopted. Among these methods, the method for immersing the fabric 6 in the hydrophilic treatment agent is preferred because it is possible to incorporate or attach the hydrophilic treatment agent simply and more uniformly.

[0053] A surfactant is a general term for a substance that has a hydrophilic group, which is compatible with water, and a hydrophobic group (lipophilic group), which is compatible with oil, in its molecule. In addition to having the function of uniformly mixing polar and non-polar substances, surfactants also have the effect of reducing surface tension to increase wettability, and of reducing interfacial friction by interposing between substances.

[0054] The type of surfactant is not particularly limited, and an ionic surfactant, a nonionic surfactant, etc. can be used. The nonionic surfactant may be a polyethylene glycol type nonionic surfactant or a polyhydric alcohol type nonionic surfactant.

[0055] Polyethylene glycol-type nonionic surfactants are nonionic surfactants in which ethylene oxide is added to a hydrophobic base component having a hydrophobic group, such as a higher alcohol, an alkylphenol, a higher fatty acid, a polyhydric alcohol higher fatty acid ester, a higher fatty acid amide, or a polypropylene glycol, to impart a hydrophilic group.

[0056] In addition, the fabric 6 may be subjected to an adhesion treatment in order to improve adhesion to the rubber composition constituting the compressible layer 4 (the rubber composition forming the surface of the rib portion 2). Examples of the adhesion treatment of the fabric 6 include immersion treatment in a resin-based treatment liquid in which an epoxy compound or an isocyanate compound is dissolved in an organic solvent (toluene, xylene, methyl ethyl ketone, etc.), immersion treatment in a resorcin-formalin-latex liquid (RFL liquid), and immersion treatment in a rubber paste in which a rubber composition is dissolved in an organic solvent. Other adhesion treatment methods include, for example, a friction treatment in which the fabric 6 and the rubber composition are passed through a calendar roll to rub the rubber composition into the fabric 6, a spreading treatment in which rubber paste is applied to the fabric 6, and a coating treatment in which a rubber composition is laminated on the fabric 6. By performing an adhesion treatment on the fabric 6 in this way, it is possible to improve adhesion to the compressible layer 4 and prevent the fabric 6 from peeling off during the running of the V-ribbed belt 1. Furthermore, the adhesive treatment can improve the abrasion resistance of the rib portion 2.

[0057] It is preferable that the rubber composition constituting the compression layer 4 is bonded to the fabric 6 by the above-mentioned adhesion treatment, and that the rubber composition does not bleed onto the friction transmission surface of the fabric 6 (the surface that contacts the driving pulley 21 and the driven pulley 22). If the rubber composition bleeds out from the fabric 6 onto the friction transmission surface side, the water absorption property decreases, so that the friction coefficient in wet conditions decreases significantly, and the water-pouring noise resistance decreases. Therefore, by preventing the rubber composition from bleed-out onto the friction transmission surface of the fabric 6, sufficient water absorption can be ensured, and the water-pouring noise resistance can be improved.

[0058] (Manufacturing method of V-ribbed belt 1) A manufacturing method of the V-ribbed belt 1 will be described below with reference to Fig. 3. First, as shown in Fig. 3(a), an unvulcanized sheet 3S for an extension layer is wound around a cylindrical inner mold 52 having a flexible jacket 51 attached to its outer circumferential surface, and a core wire 5 is spirally spun thereon. An unvulcanized sheet 4S for a compression layer and a fabric 6 are sequentially wound (covered) thereon to produce a molded body 10. Thereafter, the inner mold 52 around which the molded body 10 is wound is set concentrically on the inner periphery side of an outer mold 53 having a plurality of rib patterns 53a engraved on its inner periphery. At this time, a predetermined gap is provided between the inner periphery of the outer mold 53 and the outer periphery of the molded body 10.

[0059] Here, as described above, when forming the V-ribbed belt 1, the fabric 6 needs to be formed into a cylindrical shape so as to fit the outer circumference of the compression layer sheet 4S. For this purpose, there is a method of preparing a seamless fabric without joints using a circular knitting machine or the like, but in that case, it is necessary to prepare a seamless fabric corresponding to the length (circumference) of the V-ribbed belt 1. In this case, if a fabric 6 that is too long (too large circumference) is used for the length of the V-ribbed belt 1, the fabric 6 may overlap due to being dangling, which may cause quality abnormalities. Conversely, if a fabric 6 that is too short (too small circumference) is used, problems such as a defective shape of the molded rib portion 2 or a decrease in water-pouring noise resistance due to the rubber composition of the compression layer sheet 4S seeping out onto the friction transmission surface are expected. Therefore, if it is attempted to manufacture V-ribbed belts 1 of various lengths, it is necessary to have the same number of work-in-process products, which is likely to be wasted.

[0060] Therefore, in order to mold the fabric 6 into a cylindrical shape so as to fit the outer periphery of the compression layer sheet 4S, it is preferable to adopt a method of manufacturing a cylindrical fabric 6 by joining both ends of a square-shaped fabric 6 according to the length of the V-ribbed belt 1. In this case, the quality is stable because the fabric 6 can be prepared (adjusted) with an optimal perimeter regardless of the length of the V-ribbed belt 1. Furthermore, a flat knitting machine can be used in addition to a circular knitting machine, so there is a high degree of freedom, and only one type of work-in-progress is required, so there is no waste.

[0061] Examples of methods for joining both ends of the fabric 6 include a method of cutting the fabric 6 with a blade heated to a temperature near the melting point of the yarn that constitutes the fabric 6 and simultaneously welding the cut surface (hot melt, heat welding), a method of cutting and welding simultaneously by pressing with a blade that is ultrasonically vibrated (ultrasonic welding), sewing machine jointing, overlocking, butting, etc. The timing for joining both ends of the fabric 6 may be before the V-ribbed belt 1 is molded, or may be during the molding of the V-ribbed belt 1 (for example, the both ends of the fabric 6 are joined on the compression layer sheet 4S wrapped around the inner mold 52). When joining is performed before the molding of the V-ribbed belt 1, hot melt, ultrasonic welding, sewing machine jointing, and overlocking can be conveniently applied, and when joining is performed during the molding of the V-ribbed belt 1, butting can be conveniently applied. Among these, ultrasonic welding and butting are preferred because they provide a good appearance to the seam of the fabric 6. Furthermore, the fabric 6 may have one or more joints. From the standpoint of reducing the number of steps and improving the appearance, the fabric 6 preferably has one or two joints.

[0062] Next, as shown in FIG. 3(b), the flexible jacket 51 is expanded toward the inner surface of the outer mold 53 at a predetermined expansion rate (e.g., 1 to 6%), and the compression layer sheet 4S and fabric 6 of the molded body 10 are pressed into the rib mold 53a of the outer mold 53, and a vulcanization treatment (e.g., 160°C, 30 minutes) is performed in that state.

[0063] 3(c), the inner mold 52 is removed from the outer mold 53, and the vulcanized rubber sleeve 10A having the multiple ribs 2 is removed from the outer mold 53. After that, the vulcanized rubber sleeve 10A is cut to a predetermined width along the circumferential direction using a cutter to finish the V-ribbed belt 1. Note that the method for manufacturing the V-ribbed belt 1 is not limited to the above method, and other known methods disclosed in, for example, JP 2004-82702 A can also be used.

[0064] As described above, in the V-ribbed belt 1 in which the friction transmission surfaces, which are the contact portions with the drive pulley 21 and the driven pulley 22, are covered with the fabric 6, the fabric 6 contains natural cellulose fibers having a tensile strength of 4.5 cN / dtex or more, and polyester-based composite yarn, so that the water absorption (resistance to noise caused by water pouring) and abrasion resistance can be maintained for a long period of time.

[0065] In particular, by using only hemp as the natural cellulose fiber having a tensile strength of 4.5 cN / dtex or more contained in the fabric 6, the water absorption (water-pouring noise resistance) of the V-ribbed belt 1 can be maintained for a long period of time, while the abrasion resistance can be maintained for an even longer period of time.

[0066] Also, like the above V-ribbed belt 1, the fabric 6 may be configured to contain hemp as a natural cellulose fiber of 4.5 cN / dtex or more, and further contain natural cellulose fibers other than the hemp (without any limitation on tensile strength). By including natural cellulose fibers other than hemp in addition to hemp in the fabric 6, it is possible to reduce costs while sufficiently maintaining the acceptable abrasion resistance of the V-ribbed belt 1, compared to a case in which only hemp is used as the natural cellulose fiber contained in the fabric 6. In particular, by using relatively inexpensive cotton as the natural cellulose fiber other than hemp, it is possible to further reduce procurement and manufacturing costs.

[0067] Furthermore, by knitting the fabric 6 with a blended yarn in which short fibers of hemp and short fibers of natural cellulose fibers other than hemp are mixed, the fabric 6 can be knitted in a state in which the hemp and the natural cellulose fibers other than hemp are uniformly dispersed. This enhances the effect of suppressing wear of the natural cellulose fibers other than hemp, and the water-pouring noise resistance of the V-ribbed belt 1 can be maintained for a longer period of time.

[0068] (others) In the above embodiment, the V-ribbed belt 1 has been described as an example of a friction transmission belt, but the fabric 6 can also be used for other types of friction transmission belts such as flat belts, wrapped V-belts, and raw edge V-belts, and can also be used for transmission belts in general. EXAMPLES

[0069] Next, as shown in Table 1, V-ribbed belts according to Examples 1 to 8 and Comparative Examples 1 to 3 were produced and subjected to a friction coefficient measurement test and an abrasion resistance test. Furthermore, a friction coefficient measurement test was performed again on each of the V-ribbed belts subjected to the abrasion resistance test.

[0070] Examples 1 to 8 and Comparative Examples 1 to 3 all use a double pique weft-knitted two-layered fabric (woven fabric), and the compressed layer side of the weft-knitted two-layered fabric is formed of yarn C (PTT / PET conjugate yarn), which is common to all of them. There is a difference in the yarn on the frictional power transmission surface side (pulley contact surface side) of the weft-knitted two-layered fabric. A blended yarn with a different mass ratio of hemp and cotton was used on the frictional power transmission surface side (pulley contact surface side) of Examples 1 to 3. A 100% hemp yarn was used on the frictional power transmission surface side (pulley contact surface side) of Example 4. An alternating knit in which 100% cotton yarn and 100% hemp yarn were alternately knitted was used on the frictional power transmission surface side (pulley contact surface side) of Example 5. Examples 6 and 8 used a blended yarn with a thicker yarn than Example 1. Example 7 used an alternating knit with a thicker yarn than Example 5. 100% cotton yarn was used on the frictional power transmission surface side (pulley contact surface side) of Comparative Example 1. Alternating knitting of 100% cotton yarn and 100% nylon yarn was used on the frictional power transmission surface side (pulley contact surface side) of Comparative Example 2. A blended yarn of cotton and nylon was used on the frictional power transmission surface side (pulley contact surface side) of Comparative Example 3.

[0071] (Friction coefficient measurement test) The friction coefficient measurement test was performed using a testing machine equipped with a driving pulley (Dr.) with a diameter of 121.6 mm, an idler pulley (IDL.1) with a diameter of 76.2 mm, an idler pulley (IDL.2) with a diameter of 61.0 mm, an idler pulley (IDL.3) with a diameter of 76.2 mm, an idler pulley (IDL.4) with a diameter of 77.0 mm, and a driven pulley (Dn.) with a diameter of 121.6 mm, as shown in Figure 4, and each V-ribbed belt was suspended around each of these pulleys.

[0072] As shown in (a) of Figure 4, in tests under dry conditions simulating normal driving, the driving pulley (Dr.) rotation speed was set to 400 rpm, the belt winding angle α around the driven pulley (Dn.) was set to π / 9 radians (20°) under room temperature conditions (23°C), and each V-ribbed belt was run with a constant load (180 N / 6 rib) applied, and the torque of the driven pulley (Dn.) was gradually increased. The friction coefficient μ was calculated using equation (1) from the torque value of the driven pulley (Dn.) when the slippage speed of V-ribbed belt 1 relative to the driven pulley (Dn.) reached its maximum (100% slip). μ = ln(T 1 / T 2 ) / α (1) Here, T 1 is tension side tension, T 2 is the slack side tension. Slack side tension T of driven pulley (Dn.) 2 is equal to the constant load (180N / 6rib), and the tension on the exit side T 1 is this constant load plus the tension due to the torque of the driven pulley (Dn.).

[0073] As shown in (b) of Figure 4, in the test under wet conditions simulating driving in the rain, the rotation speed of the driving pulley (Dr.) was set to 800 rpm, the belt winding angle α around the driven pulley (Dn.) was set to π / 4 radians (45°), and 300 ml of water was continuously poured per minute near the inlet of the driven pulley (Dn.). The other conditions were the same as in the test under dry conditions, and the friction coefficient μ was calculated using equation (1).

[0074] (Wear resistance test) For the wear resistance test, a test machine (not shown) was used, which was equipped with a driving pulley (Dr.) with a diameter of 120 mm, an idler pulley (IDL.1) with a diameter of 75 mm, a tension pulley (Ten.) with a diameter of 60 mm, and a driven pulley (Dn.) with a diameter of 120 mm, in that order. Each V-ribbed belt was hung on each of these pulleys, and in an atmosphere of 120°C, the driving pulley (Dr.) was rotated at a speed of 4900 rpm, and an axial load of 890 N was applied to the tension pulley (Ten.) as an initial load. The belt mass was measured before and after the test, and the wear rate was calculated using formula (2). Wear rate = (mass before test - mass after test) / mass before test x 100 (%) (2) The lower the wear rate, the more excellent the wear resistance.

[0075] (Friction coefficient measurement test after wear resistance test) In the friction coefficient measurement test after the wear resistance test, the above-mentioned friction coefficient measurement test was performed again for each V-ribbed belt after the wear resistance test to determine the friction coefficient μ in a dry state and the friction coefficient μ in a wet state. In addition, the durability of the water noise resistance was evaluated. Specifically, when Δμ, which is the difference between the friction coefficient μ in a dry state and the friction coefficient μ in a wet state after the wear resistance test, is less than 0.4, it was determined that the durability of the water noise resistance was good.

[0076] Table 1 shows the configurations of the V-ribbed belts according to Examples 1 to 8 and Comparative Examples 1 to 3, and the test results thereof.

[0077] [Table 1]

[0078] (Materials used) Cotton yarn, linen yarn, cotton / linen blend yarn: Spun yarn made by twisting various staples together PTT / PET conjugate yarn: Toray Industries, 84dtex Nylon thread: Toray Industries, nylon 66, 110dtex filament thread Cotton / nylon blended yarn: Nylon 66 filament and cotton staple 50 count (cotton count) blended yarn Hemp fiber (linen): average fiber length 30 mm, average fiber diameter 20 μm, tensile strength 5 cN / dtex Cotton fiber: average fiber length 20mm, average fiber diameter 20μm, tensile strength 3cN / dtex

[0079] (Rubber compound for tension and compression layers) [Table 2]

[0080] EPDM: Dow Chemical's "Nodel IP4640", ethylene content 55% by mass, propylene content 40% by mass, ethylidene norbornene (ENB) content 5% by mass Zinc oxide: "Zinc oxide type 3" manufactured by Seido Chemical Industry Co., Ltd. Stearic acid: NOF Corp. "Camellia Stearate" Carbon black HAF: "Seast V" manufactured by Tokai Carbon Co., Ltd., average primary particle size 55 nm Anti-aging agent: "Nocrac MB" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Softener (paraffin oil): "NS-90" manufactured by Idemitsu Kosan Co., Ltd. Organic peroxide: NOF Corp. "Perkmyl D-40"

[0081] (Discussion of each test result) Examples 1 to 8, which contain hemp on the friction transmission surface side (pulley contact surface side) of the weft-knitted two-layered fabric (woven fabric), had small Δμ after the abrasion resistance test and were able to maintain water-pouring noise resistance for a long period of time.Comparative Examples 1 to 3 had large Δμ after the abrasion resistance test and were unable to maintain water-pouring noise resistance for a long period of time.

[0082] There was no difference in Δμ after the abrasion resistance test among Examples 1 to 8, and Example 4, which used 100% hemp yarn, had the best abrasion resistance. However, the abrasion resistance of the other Examples was also at an acceptable level, and Examples 1, 6, and 8, which have a high proportion of cotton, are preferable from a cost perspective. Among them, Example 8 is particularly preferable because it can achieve both cost reduction and abrasion resistance.

[0083] Comparing Example 1 and Comparative Example 3, Comparative Example 3, which was a blend of cotton and nylon, had a small abrasion rate, but the Δμ after the abrasion resistance test was large, resulting in a low durability of water-pouring noise resistance.

[0084] In Example 1, which used hemp, the wear rate was relatively large, but Δμ after the wear resistance test was small, and the durability of the water-pour noise resistance was high. A similar tendency was confirmed in a comparison between Example 5 and Comparative Example 2. This shows that the durability of the water-pour noise resistance cannot be improved simply by having good wear resistance, and it can be said that this result shows the superiority of using hemp, which has a good balance between wear resistance and water absorption.

[0085] A comparison between Example 2 and Example 5 reveals that the use of a blended yarn of cotton and linen provides superior abrasion resistance compared to alternating knitting of 100% cotton yarn and 100% linen yarn.

[0086] A comparison of Examples 1, 6, and 8 showed that the abrasion resistance was improved by increasing the thickness of the cotton and linen blended yarn. Also, a comparison of Examples 5 and 7 showed that the abrasion resistance was improved by increasing the thickness of the cotton and linen yarns, even in the case of alternating knitting with cotton and linen yarns. [Explanation of symbols]

[0087] 1 V-ribbed belt 2 Rib section 3 stretch layers 4. Compression Layer 5 core wire 6 Fabric 10 Molded body 21 Drive pulley 22 Driven pulley 23 V-shaped groove 51 Flexible Jacket 52 Inner mold 53 External mold 53a Ribbed

Claims

1. The friction transmission surface is covered with fabric, The fabric contains hemp, which is a natural cellulose fiber having a tensile strength of 4.5 cN / dtex or more, a natural cellulose fiber other than the hemp, and a polyester-based composite yarn, The friction transmission belt is characterized in that the hemp and the natural cellulose fibers other than hemp are knitted with a blended yarn obtained by blending the hemp staple fibers with the natural cellulose fibers other than the hemp staple fibers.

2. 2. The friction power transmission belt according to claim 1, wherein the natural cellulose fiber other than hemp is cotton.

3. The friction transmission belt according to claim 2, wherein the blended yarn obtained by blending the hemp staple fibers and the cotton staple fibers has a mass ratio within the range of "cotton / hemp = 1 / 99 to 80 / 20".

4. 2. The friction power transmission belt according to claim 1, wherein the blended yarn has a count of 20 to 60.

Citation Information

Patent Citations

  • V-ribbed belt

    JP2014209028A

  • V-ribbed belt and its manufacturing method

    JP2018197605A

  • Friction transmission belt and manufacturing method thereof

    JP2019120402A

  • Friction transmission belt

    WO2019193881A1