Rubber composition and transmission belt

The rubber composition for power transmission belts, using ethylene-α-olefin elastomer, carbon black, and crosslinking agents, addresses conductivity and crack resistance issues, ensuring effective electrical conductivity and durability.

JP2024155743APending Publication Date: 2024-10-31MITSUBOSHI BELTING LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024038127
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2024-03-12
Publication Date
2024-10-31

Smart Images

  • Figure 2024155743000009
    Figure 2024155743000009
  • Figure 2024155743000010
    Figure 2024155743000010
  • Figure 2024155743000011
    Figure 2024155743000011
Patent Text Reader

Abstract

To provide a rubber composition capable of improving the conductivity of a transmission belt.SOLUTION: There is provided a transmission belt formed by a rubber composition comprising a polymer component, carbon black, a cross-linking agent and a co-cross-linking agent. The polymer component includes an ethylene-α-olefin elastomer. The cross-linking agent includes a sulfur-based cross-linking agent. The ratio of the carbon black is 55 to 85 pts.mass based on 100 pts.mass of the polymer component. The rubber composition may further comprise short fibers. The ratio of the short fibers may be 15 to 50 pts.mass based on 100 pts.mass of the polymer component. The short fibers may include synthetic short fibers and natural short fibers. The short fibers are a combination of at least one synthetic short fibers selected from the group consisting of polyester short fibers and aramid short fibers and cellulose short fibers and the ratio of the cellulose short fibers may be 10 to 100 pts.mass based on 100 pts.mass of the synthetic short fibers. The crosslinking agent may be a sulfur-based crosslinking agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition and a power transmission belt capable of improving the electrical conductivity of the power transmission belt. [Background technology]

[0002] A transmission belt is placed around multiple pulleys to transmit power from the driving pulley to the driven pulley. During this process, static electricity can build up on the belt as it repeatedly engages with and disengages from the pulleys, which can have a detrimental effect on surrounding electrical equipment. To avoid such adverse effects, belts with improved conductivity (electrical conductivity) have been proposed.

[0003] For example, Patent Document 1 (Japanese Patent No. 5358191) discloses a rubber composition for a transmission belt containing furnace carbon black, zinc oxide, and stearic acid. Patent Document 2 (Japanese Patent No. 5489319) discloses a rubber composition for a transmission belt containing specific amounts of conductive carbon black and furnace carbon black. These documents state that rubber compositions containing carbon black are also excellent in maintaining electrical conductivity after running. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5358191 [Patent Document 2] Patent No. 5489319 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the rubber compositions of Patent Documents 1 and 2 do not reach the level required for, for example, explosion-proof specifications, and there has been a demand for rubber compositions having higher electrical conductivity, including electrical conductivity maintenance.

[0006] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a rubber composition and a power transmission belt that can improve the electrical conductivity of the power transmission belt. [Means for solving the problem]

[0007] The present inventors considered that in order to improve the electrical conductivity of a transmission belt, it is important that carbon black is linked together in the rubber matrix to form an electrical path, and therefore investigated compounding a large amount of carbon black. However, an increase in the amount of carbon black alone is not sufficient to maintain electrical conductivity after running, and it was believed that the cause of this is that minute cracks are generated, causing the carbon black to break. As a result of further intensive investigations, the present inventors found that the electrical conductivity of a transmission belt can be improved by compounding a large amount of carbon black in an ethylene-propylene-diene terpolymer (EPDM) and combining it with a sulfur-based crosslinking agent and a co-crosslinking agent, and thus completed the present invention.

[0008] That is, the rubber composition according to embodiment [1] of the present invention is a rubber composition comprising a polymer component, carbon black, a crosslinking agent, and a co-crosslinking agent, the polymer component comprises an ethylene-α-olefin elastomer; The crosslinking agent comprises a sulfur-based crosslinking agent; and The proportion of the carbon black is 55 to 85 parts by mass with respect to 100 parts by mass of the polymer component.

[0009] An embodiment [2] of the present invention is an embodiment in which the rubber composition of the embodiment [1] further contains short fibers, and the proportion of the short fibers is 15 to 50 parts by mass per 100 parts by mass of the polymer component.

[0010] The third aspect of the present invention is the above-mentioned second aspect, wherein the staple fibers include synthetic staple fibers and natural staple fibers.

[0011] Aspect [4] of the present invention is an aspect of the above aspect [2] or [3], in which the staple fibers are a combination of at least one synthetic staple fiber selected from the group consisting of polyester staple fibers and aramid staple fibers and cellulose staple fibers, and the proportion of the cellulose staple fibers is 10 to 100 parts by mass per 100 parts by mass of the synthetic staple fibers.

[0012] Aspect [5] of the present invention is any one of aspects [1] to [4] above, wherein the crosslinking agent is a sulfur-based crosslinking agent.

[0013] Aspect [6] of the present invention is any one of aspects [1] to [5] above, further comprising clay, wherein the proportion of the clay is 20 to 60 parts by mass per 100 parts by mass of the carbon black.

[0014] The present invention also includes, as an embodiment [7], a power transmission belt including a cross-linked product of the rubber composition according to any one of the embodiments [1] to [6].

[0015] An embodiment [8] of the present invention is an embodiment in which the thickness of the power transmission belt of the embodiment [7] is 8 mm or more. Effect of the Invention

[0016] In the present invention, the electrical conductivity can be improved by combining an ethylene-α-olefin elastomer with a predetermined amount of carbon black, a sulfur-based crosslinking agent, and a co-crosslinking agent. In particular, when used in a transmission belt (particularly a compressed rubber layer), the occurrence of microcracks in the belt can be suppressed even after the belt has been running, the electrical resistance can be kept low, and the electrical conductivity of the transmission belt can be improved. Furthermore, the crack resistance and abrasion resistance of the transmission belt can also be improved. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram showing the layout of a running test for evaluating the crack resistance of the raw-edge cogged V-belt obtained in the examples. [Diagram 2]FIG. 2 is a schematic diagram showing the layout of a running test for evaluating the wear resistance of the raw-edge cogged V-belt obtained in the examples. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing the raw-edge cogged V-belt obtained in the examples placed on electrodes for measuring the electrical resistance of the belt. [Figure 4] FIG. 4 is a schematic plan view illustrating a method for measuring the electrical resistance of the raw-edge cogged V-belt obtained in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] [Rubber composition] The rubber composition of the present invention contains a polymer component (A), carbon black (B), a crosslinking agent (C) and a co-crosslinking agent (D).

[0019] (A) Polymer component (or rubber component) In the rubber composition of the present invention, the polymer component (first polymer component) (A) contains an ethylene-α-olefin elastomer because it has excellent heat resistance, cold resistance, and weather resistance.

[0020] The ethylene-α-olefin elastomer may contain ethylene units and α-olefin units as constituent units, and may further contain diene units. Therefore, the ethylene-α-olefin elastomer includes ethylene-α-olefin copolymer rubber, ethylene-α-olefin-diene terpolymer rubber, etc.

[0021] Examples of α-olefins for forming α-olefin units include linear α-C olefins such as propylene, butene, pentene, methylpentene, hexene, and octene. 3-12 Among these α-olefins, α-C such as propylene 3-4 Olefins, especially propylene, are preferred.

[0022] As the diene monomer for forming the diene unit, a non-conjugated diene monomer is usually used. Examples of the non-conjugated diene monomer include dicyclopentadiene, methylenenorbornene, ethylidenenorbornene, 1,4-hexadiene, and cyclooctadiene. Among these diene monomers, ethylidenenorbornene and 1,4-hexadiene (particularly ethylidenenorbornene) are preferred.

[0023] Representative examples of ethylene-α-olefin elastomers include ethylene-α-olefin rubbers [ethylene-propylene rubber (EPM), ethylene-butene rubber (EBM), ethylene-octene rubber (EOM), etc.] and ethylene-α-olefin-diene rubbers [ethylene-propylene-diene terpolymers (EPDM)].

[0024] These ethylene-α-olefin elastomers can be used alone or in combination of two or more. Among these, ethylene-α-C is preferred because of its excellent heat resistance, cold resistance and weather resistance. 3-4 Ethylene-α-olefin-diene terpolymer rubbers such as olefin-diene terpolymer rubbers are preferred, and EPDM is particularly preferred. Therefore, the proportion of EPDM may be 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more (particularly 95% by mass or more), or may be 100% by mass (EPDM only) based on the total ethylene-α-olefin elastomer.

[0025] In the ethylene-α-olefin elastomer, the ethylene content (proportion of ethylene units) in the ethylene-α-olefin elastomer may be 45% by mass or more, for example, 45 to 80% by mass, preferably 48 to 70% by mass, and more preferably 50 to 60% by mass. If the ethylene content is too low, when used in a transmission belt, the abrasion resistance may decrease, and if the ethylene content is too high, the processability and crack resistance may decrease.

[0026] In the present application, the ethylene content means the mass ratio of ethylene units in all units constituting the ethylene-α-olefin elastomer, and can be measured by a conventional method, but may be a ratio based on ethylene as a monomer.

[0027] Furthermore, in the present application, when there are multiple types of ethylene-α-olefin elastomers, the ethylene content means an average value based on the mass ratio (average ethylene content), that is, the average ethylene content is the sum of the products of the ethylene contents and the mass fractions of the respective ethylene-α-olefin elastomers.

[0028] In the ethylene-α-olefin elastomer, the ratio (mass ratio) of ethylene to α-olefin (former / latter) is 40 / 60 to 90 / 10, preferably 45 / 55 to 80 / 20, further preferably 50 / 50 to 70 / 30, and further preferably 55 / 45 to 60 / 40.

[0029] The diene content (particularly, the ethylidene norbornene content) of the ethylene-α-olefin elastomer (particularly, the ethylene-α-olefin-diene ternary copolymer rubber such as EPDM) is, for example, 0.1 to 15 mass%, preferably 1 to 10 mass%, further preferably 2 to 7 mass%, more preferably 3 to 6 mass%, and most preferably 4 to 5 mass%. If the diene content is too high, there is a risk that high heat resistance cannot be ensured. If the diene content is too low, there is a risk that the processability and crack resistance will decrease when used in a transmission belt, and conversely, if the diene content is too high, there is a risk that the abrasion resistance will decrease.

[0030] In the present application, the diene content means the mass ratio of diene monomer units in all units constituting the ethylene-α-olefin elastomer, and can be measured by a conventional method, but may be a ratio based on the monomer.

[0031] The iodine value of the ethylene-α-olefin elastomer containing a diene monomer is, for example, 3 to 40, preferably 5 to 30, and more preferably 10 to 20. If the iodine value is too small, the crosslinking of the rubber composition becomes insufficient, and wear and adhesion tend to occur, whereas if the iodine value is too large, the scorch of the rubber composition tends to be short, making it difficult to handle, and the heat resistance tends to decrease.

[0032] In the present application, the iodine value of the ethylene-α-olefin elastomer can be measured by a conventional method, for example, infrared spectroscopy.

[0033] The Mooney viscosity [ML(1+4)125°C] of the uncrosslinked ethylene-α-olefin elastomer may be 15 or more, for example, 15 to 85, preferably 20 to 70, further preferably 25 to 60, more preferably 30 to 50, and most preferably 35 to 45. If the Mooney viscosity is too low, when used in a transmission belt, there is a risk of the abrasion resistance decreasing, and conversely, if it is too high, there is a risk of the processability and crack resistance decreasing.

[0034] In this application, the Mooney viscosity can be measured by a method conforming to JIS K 6300-1 (2013), and the test conditions are as follows: an L-shaped rotor is used, the test temperature is 125°C, preheating is 1 minute, and the rotor operation time is 4 minutes. The Mooney viscosity is used as an index of the fluidity (ease of processing) of rubber by filling an uncrosslinked ethylene-α-olefin elastomer in a cavity so that it is in contact with a rotor with grooves on its surface, and measuring the torque required to rotate the rotor.

[0035] Furthermore, in the present application, when there are multiple types of ethylene-α-olefin elastomers, the Mooney viscosity means an average value based on the mass ratio (average Mooney viscosity). In other words, the average Mooney viscosity is the sum of the products of the Mooney viscosities of the respective ethylene-α-olefin elastomers and the mass fractions.

[0036] The proportion of the ethylene-α-olefin elastomer in the polymer component (A) may be 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and most preferably 100% by mass (only ethylene-α-olefin elastomer). If the proportion of the ethylene-α-olefin elastomer in the polymer component is too low, there is a risk of the heat resistance and cold resistance decreasing.

[0037] The polymer component (A) may contain, in addition to the ethylene-α-olefin elastomer, other polymer components, for example, diene rubbers [natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), chloroprene rubber (CR), butyl rubber (IIR), styrene butadiene rubber (SBR), vinylpyridine-styrene-butadiene copolymer rubber, acrylonitrile-butadiene rubber (nitrile rubber: NBR), acrylonitrile-chloroprene rubber; hydrogenated products of the diene rubbers, such as hydrogenated nitrile rubber (HNBR, including a mixed polymer of hydrogenated nitrile rubber and an unsaturated carboxylic acid metal salt)], olefin rubbers [polyoctenylene rubber, ethylene-vinyl acetate copolymer rubber, chlorosulfonated polyethylene rubber (CSM), alkylated chlorosulfonated polyethylene rubber (ACSM)], epichlorohydrin rubber, acrylic rubber, silicone rubber, urethane rubber, fluororubber, and the like, as long as the effects of the present invention are not impaired. These rubber components may be carboxylated, such as carboxylated SBR, carboxylated NBR, etc. The hydrogenated nitrile rubber is not limited to hydrogenated nitrile rubber alone, and may be a composite polymer of hydrogenated nitrile rubber and an unsaturated carboxylic acid metal salt. These polymer components may be used alone or in combination of two or more.

[0038] The proportion of the other polymer component in the polymer component (A) may be 50% by mass or less, preferably 20% by mass or less, and more preferably 10% by mass or less.

[0039] When polymer component (A) contains other polymer components, the Mooney viscosity of the uncrosslinked polymer components can be selected from the viscosity ranges described above for the Mooney viscosity of ethylene-α-olefin elastomers, including the preferred ranges.

[0040] (B) Carbon black The rubber composition of the present invention contains carbon black (B) as an inorganic filler in order to improve electrical conductivity. In the present invention, the rubber composition contains a large amount of carbon black (B), thereby improving electrical conductivity.

[0041] Carbon black is classified by ASTM as "N0**" to "N9**" (classified based on iodine adsorption), and has been classified into SAF, HAF, GPF, etc. based on the performance of rubber products. N110 (SAF), N220 (ISAF), N330 (HAF), etc., which have small primary particle diameters, are called hard carbon, and N550 (FEF), N660 (GPF), N762 (SRF), etc., which have large primary particle diameters, are sometimes called soft carbon. These carbon blacks can be used alone or in combination of two or more. Of these, hard carbon blacks such as ISAF are preferred.

[0042] The average primary particle size of carbon black (B) can be selected from the range of 5 to 200 nm (e.g., 10 to 100 nm), for example, 10 to 70 nm, preferably 13 to 50 nm, further preferably 15 to 40 nm, and more preferably 20 to 30 nm. If the average primary particle size of carbon black (B) is too small, the dispersibility of carbon black (B) in the rubber composition may decrease, whereas if it is too large, the reinforcing properties of carbon black (B) may decrease.

[0043] In the present application, the average primary particle size of the carbon black (B) can be measured on a number basis using, for example, a transmission electron microscope.

[0044] The DBP absorption of the carbon black (B) can be selected, for example, from the range of about 60 to 500 mL / 100 g, preferably 80 mL / 100 g or more, more preferably 100 mL / 100 g or more, and may be 100 to 200 mL / 100 g. If the DBP absorption is too small, the electrical conductivity of the crosslinked rubber may decrease.

[0045] In this application, the DBP absorption amount of carbon black (B) means a value (OAN) that can be measured on an uncompressed sample in accordance with JIS K 6217-4 (2017).

[0046] The iodine adsorption amount of carbon black (B) is, for example, 5 to 200 g / kg, preferably 10 to 180 g / kg, further preferably 50 to 150 g / kg, and further preferably 100 to 130 g / kg. If the iodine adsorption amount is too small, the hardness and modulus of the crosslinked rubber may decrease, whereas if it is too large, it may become difficult to prepare carbon black (B) itself.

[0047] In the present application, the iodine adsorption amount of carbon black (B) can be measured in accordance with the standard test method of ASTM D1510-17.

[0048] The BET specific surface area of ​​carbon black (B) is, for example, 50 to 400 m 2 / g, preferably 70 to 300m 2 / g, more preferably 80 to 200m 2 / g, more preferably 100 to 150m 2 / g.

[0049] In the present application, the BET specific surface area means a specific surface area measured by the BET method using nitrogen gas.

[0050] The rubber composition of the present invention contains a large amount of carbon black, and therefore the electrical conductivity and electrical conductivity retention can be improved without using special carbon blacks (e.g., ketjen black, acetylene black, etc.) classified as conductive carbon blacks. Therefore, the carbon black (B) may be a general-purpose carbon black (non-conductive carbon black). Furthermore, as the carbon black, non-conductive carbon black is preferable because it can improve the abrasion resistance and crack resistance.

[0051] The proportion of carbon black (B) is 55 to 85 parts by mass, preferably 60 to 83 parts by mass, and more preferably 70 to 80 parts by mass, based on 100 parts by mass of polymer component (A). If the proportion of carbon black (B) is too low, the electrical conductivity and electrical conductivity retention of the rubber composition will decrease, whereas if the proportion is too high, poor dispersion of carbon black (B) will easily occur, making it difficult to roll the rubber composition into a sheet.

[0052] The proportion of conductive carbon black may be 1000 parts by mass or less (e.g., 1 to 1000 parts by mass) relative to 100 parts by mass of non-conductive carbon black, and is preferably 500 parts by mass or less (e.g., 10 to 500 parts by mass), and may be 300 parts by mass or less, preferably 100 parts by mass or less, more preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and most preferably 10 parts by mass or less, from the viewpoint of improving abrasion resistance and crack resistance. Carbon black (B) is preferably substantially free of conductive carbon black, and particularly preferably free of conductive carbon black, from the viewpoint of improving abrasion resistance and crack resistance.

[0053] (C) Crosslinking agent (vulcanizing agent) The rubber composition of the present invention further contains a crosslinking agent (C). In the present invention, the crosslinking agent (C) contains a sulfur-based crosslinking agent, and is combined with a co-crosslinking agent (D) described below, so that when the rubber composition is used in a transmission belt, the occurrence of microcracks can be suppressed and the electrical conductivity retention after running can be improved.

[0054] Examples of sulfur-based crosslinking agents include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, and sulfur chlorides (sulfur monochloride, sulfur dichloride, etc.). These sulfur-based crosslinking agents can be used alone or in combination of two or more. Among these, powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, and highly dispersible sulfur are preferred, and powdered sulfur is particularly preferred.

[0055] The proportion of the sulfur-based crosslinking agent in the crosslinking agent (C) may be 50% by mass or more, preferably 80% by mass or more, further preferably 90% by mass or more, and even more preferably 100% by mass. If the proportion of the sulfur-based crosslinking agent is too small, the flex fatigue resistance of the crosslinked product (or the crack resistance of the transmission belt) may decrease.

[0056] The crosslinking agent (C) may further contain an organic peroxide in addition to the sulfur-based crosslinking agent, so long as the effect of the present invention is not impaired. The organic peroxide may be an organic peroxide that is usually used for crosslinking rubber or resin, such as diacyl peroxide (e.g., dilauroyl peroxide, dibenzoyl peroxide, etc.), peroxyketal (e.g., 1,1-di(t-butylperoxy)cyclohexane, 2,2-di(t-butylperoxy)butane, etc.), alkyl peroxy ester (t-butylperoxybenzoate, etc.), dialkyl peroxide (di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, etc.), or a mixture thereof. peroxy)hexyne-3, 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,3-bis(2-t-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, etc., diaralkyl peroxides (dicumyl peroxide, t-butylcumyl peroxide, etc.), peroxycarbonates (t-butylperoxyisopropyl carbonate, t-butylperoxy-2-ethyl-hexyl carbonate, t-amylperoxy-2-ethyl-hexyl carbonate, etc.), etc.

[0057] These organic peroxides can be used alone or in combination of two or more. Furthermore, the organic peroxide is preferably a peroxide having a decomposition temperature of about 150 to 250° C. (for example, 175 to 225° C.) that provides a half-life of one minute due to thermal decomposition.

[0058] The ratio of the organic peroxide may be 100 parts by mass or less, preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the sulfur-based crosslinking agent. If the ratio of the organic peroxide is too high, the electrical conductivity retention of the transmission belt may decrease. It is particularly preferable that the crosslinking agent (C) does not substantially contain an organic peroxide, and it is most preferable that the crosslinking agent (C) does not contain an organic peroxide.

[0059] The proportion of the crosslinking agent (C) (particularly, the sulfur-based crosslinking agent) can be selected from the range of, for example, about 1 to 10 parts by mass relative to 100 parts by mass of the polymer component (A), and is preferably 1.2 parts by mass or more, for example, 1.2 to 5 parts by mass, preferably 1.3 to 3 parts by mass, more preferably 1.5 to 2.5 parts by mass, more preferably 1.6 to 2.3 parts by mass, and most preferably 1.8 to 2.2 parts by mass. If the proportion of the sulfur-based crosslinking agent is too small, there is a risk that the rubber hardness, lateral pressure resistance, and abrasion resistance will decrease, and if it is too large, there is a risk that the flex fatigue resistance of the crosslinked product will decrease and there is also a risk of blooming (precipitation on the surface) occurring.

[0060] (D) Co-crosslinking agent The rubber composition of the present invention further contains a co-crosslinking agent (D). Examples of the co-crosslinking agent (co-vulcanizing agent) (D) include known co-crosslinking agents, such as polyfunctional (iso)cyanurates [e.g., triallyl isocyanurate (TAIC), triallyl cyanurate (TAC), etc.], polydiene (e.g., 1,2-polybutadiene, etc.), metal salts of unsaturated carboxylic acids [e.g., (meth)acrylic acid polyvalent metal salts such as zinc (meth)acrylate and magnesium (meth)acrylate], oximes (e.g., quinone dioxime, etc.), guanidines (e.g., diphenyl guanidine, etc.), polyfunctional (meth)acrylates [e.g., alkane diol di(meth)acrylate such as ethylene glycol di(meth)acrylate and butane diol di(meth)acrylate, trimethylol propane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, etc.], and the like. alkane polyol poly(meth)acrylates such as thritol tetra(meth)acrylate, bismaleimides [for example, alkylene bismaleimides such as N,N'-1,2-ethylene dimaleimide, N,N'-hexamethylene bismaleimide, 1,6'-bismaleimide-(2,2,4-trimethyl)cyclohexane; N,N'-m-phenylene dimaleimide (MPBM), 4-methyl-1,3-phenylene dimaleimide, 4,4'-diphenylmethane dimaleimide, arene bismaleimides such as 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, 4,4'-diphenyl ether dimaleimide, 4,4'-diphenyl sulfone dimaleimide, 1,3-bis(3-maleimidophenoxy)benzene, etc.].

[0061] These co-crosslinking agents can be used alone or in combination of two or more. Among these, bismaleimides such as MPBM are preferred.

[0062] The proportion of the co-crosslinking agent (D) is, for example, 0.1 to 10 parts by mass (particularly 0.7 to 10 parts by mass), preferably 0.2 to 5 parts by mass, further preferably 0.3 to 3 parts by mass, more preferably 0.5 to 1.5 parts by mass, and most preferably 0.8 to 1.2 parts by mass, relative to 100 parts by mass of the polymer component (A). If the proportion of the co-crosslinking agent (D) is too low, the abrasion resistance may decrease and the modulus of the crosslinked rubber may decrease, whereas if it is too high, the flex fatigue resistance of the crosslinked product may decrease.

[0063] (E) Short Fiber The rubber composition of the present invention may further contain short fibers (E) in order to improve wear resistance. Examples of the short fibers (E) include polyolefin short fibers (polyethylene short fibers, polypropylene short fibers, etc.), polyamide short fibers [aliphatic polyamide short fibers (nylon short fibers) such as polyamide 6 short fibers, polyamide 66 short fibers, and polyamide 46 short fibers, and aramid short fibers, etc.], polyester short fibers [polyalkylene arylate-based short fibers (e.g., polyethylene terephthalate (PET) short fibers, polytrimethylene terephthalate (PTT) short fibers, polybutylene terephthalate (PBT) short fibers, polyethylene naphthalate (PEN) short fibers, etc. C short fibers, etc. 2-4 Alkylene C 8-14 arylate staple fibers); completely aromatic polyester staple fibers such as polyarylate staple fibers and liquid crystal polyester staple fibers; synthetic staple fibers such as vinylon staple fibers, polyvinyl alcohol staple fibers, and polyparaphenylene benzobisoxazole (PBO) staple fibers; natural staple fibers such as cotton, hemp, and wool, regenerated cellulose staple fibers such as rayon, cellulose ester staple fibers, and inorganic staple fibers such as carbon staple fibers and glass staple fibers. These staple fibers can be used alone or in combination of two or more.

[0064] Of these staple fibers, synthetic staple fibers and / or natural staple fibers (particularly polyester staple fibers and / or cellulose staple fibers) are widely used. A combination of synthetic staple fibers and natural staple fibers is preferred from the viewpoint of improving abrasion resistance while maintaining the flexural fatigue resistance of the crosslinked product, a combination of polyester staple fibers and / or aramid staple fibers and cellulose staple fibers is even more preferred from the viewpoint of improving crack resistance, a combination of polyester staple fibers and cellulose staple fibers is even more preferred, and a combination of polyalkylene arylate staple fibers such as PET staple fibers and cellulose staple fibers such as cotton staple fibers is most preferred.

[0065] When the short fibers (E) are a combination of synthetic and natural short fibers, the proportion of the natural short fibers (particularly, cellulose short fibers) can be selected from the range of about 1 to 1000 parts by mass per 100 parts by mass of the synthetic short fibers (particularly, polyester short fibers), and is, for example, 5 to 200 parts by mass, preferably 10 to 100 parts by mass, further preferably 20 to 80 parts by mass, more preferably 30 to 70 parts by mass, and most preferably 40 to 60 parts by mass. If the proportion of the natural short fibers is too low, there is a risk that the flex fatigue resistance of the crosslinked product (particularly, the crack resistance of the transmission belt) cannot be improved, and if it is too high, there is a risk that the abrasion resistance cannot be improved.

[0066] When the staple fibers (E) contain polyester staple fibers and cellulose staple fibers, the proportion of polyamide staple fibers (particularly aliphatic polyamide fibers) may be 100 parts by mass or less, preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the total of polyester staple fibers and cellulose staple fibers. It is particularly preferable that the staple fibers (E) are substantially free of polyamide staple fibers (particularly aliphatic polyamide fibers), and it is most preferable that they are free of polyamide staple fibers (particularly aliphatic polyamide fibers). If the proportion of polyamide staple fibers is too high, there is a risk of reduced crack resistance.

[0067] The short fibers (E) have an average fiber diameter of, for example, 1 to 1000 μm, preferably 3 to 100 μm, further preferably 5 to 50 μm, and further preferably 10 to 30 μm. If the average fiber diameter is too large, the hardness and modulus of the crosslinked product of the rubber composition may decrease, whereas if the average fiber diameter is too small, it may be difficult to disperse the short fibers uniformly.

[0068] The short fibers (E) have an average fiber length of, for example, 1 to 20 mm, preferably 1.5 to 10 mm, more preferably 2 to 7 mm, and even more preferably 2.5 to 6 mm. If the average length of the short fibers is too short, there is a risk that the mechanical properties (e.g., modulus) in the grain direction of the power transmission belt cannot be sufficiently improved, whereas if the average length is too long, there is a risk that the dispersibility of the short fibers in the rubber composition decreases.

[0069] From the viewpoint of dispersibility and adhesiveness of the short fibers (E) in the rubber composition, it is preferable that at least the short fibers (E) are subjected to an adhesion treatment (or surface treatment). It is not necessary that all the short fibers are adhesion treated, and adhesion-treated short fibers and non-adhesive short fibers (untreated short fibers) may be mixed or used in combination.

[0070] In the adhesive treatment of the short fibers (E), various adhesive treatments can be used, for example, a treatment liquid containing an initial condensation product of phenols and formalin (such as a prepolymer of novolac or resol-type phenolic resin), a treatment liquid containing a rubber component (or latex), a treatment liquid containing the initial condensation product and a rubber component (latex), a treatment liquid containing a reactive compound (adhesive compound) such as a silane coupling agent, an epoxy compound (such as an epoxy resin), or an isocyanate compound. In a preferred adhesive treatment, the short fibers are treated with a treatment liquid containing the initial condensation product and a rubber component (latex), particularly with at least a resorcinol-formalin-latex (RFL) liquid. Such treatment liquids may be used in combination, and for example, the short fibers may be pretreated with a conventional adhesive component, for example, a reactive compound (adhesive compound) such as an epoxy compound (such as an epoxy resin), or an isocyanate compound, and then treated with an RFL liquid.

[0071] The proportion of the short fibers (E) (the proportion of the total amount when multiple types are combined) is, for example, 10 to 100 parts by mass, preferably 15 to 50 parts by mass, more preferably 20 to 40 parts by mass, and even more preferably 25 to 35 parts by mass, per 100 parts by mass of the polymer component. If the proportion of the short fibers (E) is too low, the hardness and modulus of the cured product of the rubber composition may decrease, whereas if the proportion is too high, it may become difficult to disperse the short fibers uniformly.

[0072] (F) Crosslinking accelerator The rubber composition of the present invention may further contain a crosslinking accelerator (F) in order to improve the electrical conductivity maintaining property of the transmission belt.

[0073] Examples of the crosslinking accelerator (F) include thiuram accelerators [e.g., tetramethylthiuram monosulfide (TMTM), tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), tetrabutylthiuram disulfide (TBTD), dipentamethylenethiuram tetrasulfide (DPTT), N,N'-dimethyl-N,N'-diphenylthiuram disulfide (MPTD)], sulfenamide accelerators [e.g., N-cyclohexyl-2-benzothiazylsulfenamide (CBS), N,N'-dicyclohexyl-2-benzothiazylsulfenamide (DCBS), Nt-butyl-2-benzothiazylsulfenamide (TBBS)], thiomorpholine accelerators [e.g., 4,4'-dithiodimorpholine (DTDM), 2-(4' -morpholinodithio)benzothiazole (MBSS), etc.], thiazole-based accelerators [e.g., 2-mercaptobenzothiazole (MBT), zinc salt of MBT (ZMBT), dibenzothiazyl disulfide (MBTS), etc.], urea-based or thiourea-based accelerators [e.g., ethylenethiourea (ETU), trimethylthiourea (TMU), diethylthiourea (DETU), etc.], guanidine-based accelerators [e.g., diphenylguanidine (DPG), di-o-tolylguanidine (DOTG), etc.], dithiocarbamic acid-based accelerators [e.g., sodium dimethyldithiocarbamate (SDMC), zinc diethyldithiocarbamate (ZDEC), zinc dibutyldithiocarbamate (ZDBC), etc.], xanthogenate-based accelerators [zinc isopropylxanthogenate (ZIX), etc.], etc. These crosslinking accelerators can be used alone or in combination of two or more. Of these crosslinking accelerators, TMTD, DPTT, CBS, MBTS, etc. are commonly used.

[0074] Among them, a combination of a thiuram accelerator, a sulfenamide accelerator, and a thiazole accelerator is preferred. In these combinations, the ratio of the thiuram accelerator may be 5 to 40 mass% (particularly 10 to 30 mass%) in the crosslinking accelerator (F). The ratio of the sulfenamide accelerator may be 20 to 60 mass% (particularly 30 to 50 mass%) in the crosslinking accelerator (F). The ratio of the thiazole accelerator may be 20 to 60 mass% (particularly 30 to 50 mass%) in the crosslinking accelerator (F).

[0075] The proportion of the crosslinking accelerator (F) is, for example, 0.2 to 10 parts by mass, preferably 0.5 to 7 parts by mass, further preferably 1 to 5 parts by mass, more preferably 1.5 to 4 parts by mass, and most preferably 2 to 3 parts by mass, relative to 100 parts by mass of the polymer component (A). If the proportion of the crosslinking accelerator (F) is too low, the lateral pressure resistance of the power transmission belt may decrease, whereas if it is too high, the scorch resistance, rolling property, and crack resistance may decrease.

[0076] (G) Clay The rubber composition of the present invention may further contain clay (G) as an inorganic filler in order to improve rollability.

[0077] The pH of the clay (G) is 5.5 or more (particularly 6 or more), for example, 6 to 10 (e.g., 6 to 7.5), preferably 6 to 8 (e.g., 6.2 to 7.2), further preferably 6 to 7.3 (e.g., 6 to 7), more preferably 6 to 6.7, and most preferably 6 to 6.5. If the pH of the clay (G) is low, scorch is likely to occur and rollability is also reduced.

[0078] In the present application, the pH of the clay (G) can be measured by a conventional method, for example, a method in accordance with JIS K 5101-17-2 (2004), and in detail, the method described in the examples below.

[0079] The clay (G) is not particularly limited as long as it is a clay containing aluminum silicate, but kaolin clay, pyrophyllite clay, and calcined clay are preferred.

[0080] Kaolin clay is hydrated aluminum silicate (Al2O3·2SiO2·2H2O) obtained by crushing kaolinite, a natural clay mineral. Kaolin clay forms plate-like particles with a repeating unit of a two-layer structure of silica and alumina. Furthermore, the surface of the particles contains many acidic active groups (OH groups), and many of them exhibit acidity.

[0081] Rouseki clay, sometimes called catalpo, is a hydrated aluminum silicate (Al2O3·4SiO2·H2O) obtained by crushing pyrophyllite. Rouseki clay forms plate-like particles with a repeating unit of a triple-layer structure of silica / alumina / silica. Rouseki clay has fewer acidic active groups on the particle surface compared to kaolin clay, and many of them exhibit a slightly acidic nature.

[0082] Calcined clay is anhydrous aluminum silicate (Al2O3·2SiO2) that has had structural water removed by heating kaolin clay at around 400-1000°C. It is also believed that calcined clay loses its crystal structure by losing structural water, and that the number of acidic active groups is also reduced.

[0083] The average primary particle size of the clay (G) is, for example, about 0.1 to 20 μm, preferably about 1 to 10 μm, and more preferably about 1.5 to 5 μm. The smaller the particle size of the clay particles, the higher the reinforcing property tends to be. The clay (G) may be distinguished between clays with high reinforcing properties called hard clays and clays with low reinforcing properties called soft clays.

[0084] Clay (G) also includes surface-modified clays that have been surface-modified using surface active groups. Clay (G) may also be classified as wet type (wet clay, wet kaolin) or dry type (dry clay, dry kaolin) depending on the purification and classification methods.

[0085] In the present application, the average primary particle size of the clay (G) can be measured, for example, by a laser diffraction method.

[0086] The shape of the clay (G) may be, for example, plate-like, granular, rod-like, irregular, etc. Among these, the plate-like (scale-like) shape is preferred.

[0087] These clays can be used alone or in combination of two or more kinds. Among these, pyrophyllite clay and calcined clay are preferred from the viewpoint of suppressing scorch and improving rollability, and calcined clay is particularly preferred from the viewpoint of improving durability of the transmission belt.

[0088] The proportion of the clay (G) is, for example, 1 to 100 parts by mass, preferably 3 to 80 parts by mass, further preferably 5 to 50 parts by mass, more preferably 10 to 30 parts by mass, and most preferably 15 to 25 parts by mass, relative to 100 parts by mass of the polymer component (A). If the proportion of the clay (G) is too low, the rollability may decrease, whereas if it is too high, the crack resistance of the transmission belt may decrease.

[0089] The ratio of clay (G) may be 100 parts by mass or less (e.g., 1 to 100 parts by mass) relative to 100 parts by mass of carbon black (B), and is, for example, 5 to 80 parts by mass, preferably 10 to 70 parts by mass, further preferably 15 to 65 parts by mass, more preferably 20 to 60 parts by mass, and most preferably 25 to 40 parts by mass. If the ratio of clay (G) to carbon black (B) is too low, the crack resistance of the transmission belt may decrease, and conversely, if it is too high, the crack resistance of the transmission belt may decrease.

[0090] (H) Inorganic filler The rubber composition of the present invention may further contain an inorganic filler (another inorganic filler or filler) (H) other than carbon black and clay. Examples of the filler (H) include carbonaceous materials other than carbon black (graphite, etc.), metal compounds or synthetic ceramics (metal oxides such as magnesium oxide, calcium oxide, barium oxide, iron oxide, copper oxide, zinc oxide, titanium oxide, and aluminum oxide; metal silicates such as calcium silicate; metal carbides such as silicon carbide and tungsten carbide; metal nitrides such as titanium nitride, aluminum nitride, and boron nitride; metal carbonates such as magnesium carbonate and calcium carbonate; metal sulfates such as calcium sulfate and barium sulfate, etc.), and mineral materials other than clay (zeolite, diatomaceous earth, calcined diatomaceous earth, activated clay, alumina, silica, talc, mica, sericite, bentonite, montmorillonite, smectite, etc.). Metal oxides such as zinc oxide may act as crosslinking assistants. These fillers can be used alone or in combination of two or more.

[0091] Among these inorganic fillers, metal oxides such as magnesium oxide and zinc oxide are preferred, with zinc oxide being particularly preferred.

[0092] The proportion of the inorganic filler (H) is, for example, 1 to 30 parts by mass, preferably 2 to 20 parts by mass, more preferably 3 to 10 parts by mass, and even more preferably 4 to 8 parts by mass, relative to 100 parts by mass of the polymer component (A).

[0093] (I) Antioxidants The rubber composition of the present invention may further contain an antioxidant (I) in order to improve resistance to heat aging.

[0094] Examples of the antioxidant (I) include benzimidazole metal salt-based antioxidants, diarylamine-based antioxidants, and p-phenylenediamine-based antioxidants. These antioxidants can be used alone or in combination of two or more. Among these, diarylamine-based antioxidants are preferred. Examples of diarylamine-based antioxidants include 4,4'-di(C)-phenylenediamine such as 4,4'-dioctyldiphenylamine (ODPA). 4-18 Alkyl C 6-10 aryl)amines; bis(aralkyl-aryl)amines such as 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (DCD); styrenated diphenylamine (SDPA), and the like.

[0095] The proportion of the antioxidant (I) is, for example, 0.01 to 30 parts by mass, preferably 0.05 to 10 parts by mass, further preferably 0.1 to 5 parts by mass, more preferably 0.2 to 3 parts by mass, and most preferably 0.3 to 1 part by mass, relative to 100 parts by mass of the polymer component (A). If the proportion of the antioxidant (I) is too low, there is a risk of the heat aging resistance decreasing, whereas if it is too high, there is a risk of the flex fatigue resistance decreasing.

[0096] (J) Softener The rubber composition of the present invention may further contain a softener (processing agent or processing aid) (J). The softener (J) can be roughly classified into, for example, mineral oil-based softeners, vegetable oil-based softeners, and synthetic softeners.

[0097] Examples of mineral oil-based softeners include petroleum-based softeners [paraffin-based oils, alicyclic oils (naphthene-based oils), aromatic oils, etc.], and coal tar-based softeners (coal tar, coumarone-indene resin, etc.).

[0098] Examples of vegetable oil-based softeners include fatty oil-based softeners (fatty acids such as stearic acid or metal salts thereof, fatty acid esters, fatty acid amides, fatty oils, etc.).

[0099] Examples of synthetic softeners include synthetic resin softeners (phenol-aldehyde resins, liquid ethylene-α-olefin copolymers and other hydrocarbon synthetic oils, liquid polybutene, liquid polybutadiene, liquid isoprene rubber and other liquid rubbers), synthetic plasticizers (dioctyl phthalate and other phthalic acid diesters, polyester plasticizers, dioctyl sebacate and other C 6-18 Alkane-dicarboxylic acid esters, etc.

[0100] These softeners can be used alone or in combination of two or more. Among these, petroleum-based softeners such as paraffin-based oils and vegetable oil-based softeners such as stearic acid are preferred, and a combination of a petroleum-based softener and a vegetable oil-based softener is particularly preferred. In this case, the proportion of the vegetable oil-based softener is, for example, 1 to 100 parts by mass, preferably 5 to 50 parts by mass, and more preferably 10 to 40 parts by mass, relative to 100 parts by mass of the petroleum-based softener.

[0101] The proportion of the softener (J) is, for example, 0.1 to 50 parts by mass, preferably 0.5 to 40 parts by mass, further preferably 1 to 30 parts by mass, more preferably 2 to 10 parts by mass, and most preferably 3 to 5 parts by mass, relative to 100 parts by mass of the polymer component (A). If the proportion of the softener (J) is too high, the modulus of the crosslinked rubber may decrease, whereas if it is too low, the flex fatigue resistance may decrease.

[0102] (K) Other ingredients The rubber composition of the present invention may further contain other components (K). Examples of the other components include antioxidants, flex crack inhibitors, antiozonants, colorants, tackifiers, lubricants, coupling agents (such as silane coupling agents), stabilizers (such as ultraviolet absorbers and heat stabilizers), flame retardants, and antistatic agents. These other components may be used alone or in combination of two or more.

[0103] The total proportion of the other components (K) relative to 100 parts by mass of the polymer component (A) is, for example, 0.1 to 100 parts by mass, preferably 0.2 to 50 parts by mass, more preferably 0.3 to 20 parts by mass, and even more preferably 0.5 to 10 parts by mass.

[0104] (L) Characteristics of crosslinked rubber composition The crosslinked product of the rubber composition of the present invention may have a low electrical resistance of 1 MΩ or less, for example, 0.5 MΩ or less, preferably 0.1 MΩ or less, further preferably 0.05 MΩ or less, more preferably 0.03 MΩ or less, and most preferably 0.01 MΩ or less, for example, about 0.001 to 0.03 MΩ. If the electrical resistance is too high, the crosslinked product is easily charged.

[0105] In the present application, the electrical resistance value of the crosslinked product can be measured in accordance with the laboratory method specified in ISO1813 (2014), and in detail, can be measured by the method described in the examples described later.

[0106] The rubber hardness Hs (type A) of the crosslinked product of the rubber composition of the present invention may be 88 degrees or more, for example, 88 to 96 degrees, preferably 90 to 96 degrees, further preferably 92 to 96 degrees, and further preferably 93 to 95 degrees. If the rubber hardness is too low, the wear resistance of the belt may decrease, and if the rubber hardness is too high, the crack resistance may decrease.

[0107] In this application, the rubber hardness of the crosslinked product indicates the value Hs (type A) measured using a type A durometer in accordance with the spring type durometer hardness test specified in JIS K 6253 (2012) (vulcanized rubber and thermoplastic rubber - Determination of hardness) and may be simply referred to as rubber hardness. In detail, it can be measured by the method described in the examples below.

[0108] (M) Method for producing rubber composition The rubber composition of the present invention can be prepared by mixing (or kneading) each component by a conventional method. In order to mix them uniformly, it is preferable to knead a raw material (or raw material composition) containing the polymer component (A), carbon black (B), crosslinking agent (C) and co-crosslinking agent (D).

[0109] The kneading may be performed by kneading all the compounding ingredients at once (one-pass kneading), but in order to prevent scorching (unintended crosslinking), it may be performed in two stages: a primary kneading (A kneading) in which the components other than the crosslinking agent and the co-crosslinking agent are kneaded, and a final kneading (B kneading) in which the crosslinking agent and the co-crosslinking agent are added to the primary kneaded rubber composition and kneaded. By kneading in two stages, it becomes easy to uniformly disperse the compounding ingredients in the rubber composition while preventing scorching. Kneading may be performed under heating or cooling to prevent scorching or to keep the viscosity of the rubber composition appropriate. In the case of the primary kneading, the temperature of the rubber composition is preferably 130°C or less, more preferably 70 to 130°C, even more preferably 80 to 120°C, and most preferably 90 to 110°C. In the final kneading, the temperature of the rubber composition is preferably 100°C or less, more preferably 50 to 100°C, even more preferably 65 to 95°C, and most preferably 70 to 90°C. If the temperature of the rubber composition during kneading is too high, there is a risk of scorching, whereas if the temperature is too low, there is a risk of the dispersibility of the compounding ingredients decreasing.

[0110] The kneading method may be a conventional kneading method, for example, a method using a mixing roller, a kneader, a Banbury mixer, an extruder (such as a single-screw or twin-screw extruder), or the like.

[0111] The rubber composition of the present invention is used as a crosslinked product obtained by crosslinking the rubber composition according to the application. The crosslinking temperature is, for example, 120 to 200° C. (particularly, 150 to 180° C.).

[0112] [Power transmission belt] The cross-linked product of the rubber composition of the present invention can be used for various molded articles formed with a polymer component containing an ethylene-α-olefin elastomer. Since the ethylene-α-olefin elastomer is combined with carbon black, the cross-linked product is also excellent in electrical conductivity, heat resistance, cold resistance, weather resistance, hardness, abrasion resistance, and crack resistance, and is therefore preferably used for a transmission belt.

[0113] The type of the power transmission belt (power transmission belt) of the present invention is not particularly limited as long as it is a belt that contacts a pulley to transmit power, and may be a friction power transmission belt or a meshing power transmission belt.

[0114] Examples of friction transmission belts include flat belts, V-belts (wrapped V-belts, raw edge V-belts, raw edge cogged V-belts in which cogs are formed on the inner circumference side of the raw edge V-belt, raw edge double cogged V-belts in which cogs are formed on both the inner and outer circumference sides of the raw edge V-belt, etc.), V-ribbed belts, and resin block belts.

[0115] Examples of the intermeshing power transmission belt include a toothed belt and a double-sided toothed belt.

[0116] These power transmission belts may contain a cross-linked product of the rubber composition, but it is preferable that the belt body (particularly the compressed rubber layer and / or the tensile rubber layer) is formed of a cross-linked product of the rubber composition.

[0117] Among the above-mentioned power transmission belts, the application to V-belts in which the mass ratio of the rubber composition in the entire belt is large is preferred.Furthermore, raw edge V-belts are preferred because the contact surface with the pulley is made of rubber and static electricity can be easily released, and raw edge cogged V-belts are particularly preferred because improved crack resistance is required to prevent cog valley cracks.

[0118] The raw edge cogged V-belt of the present invention may comprise an adhesive rubber layer in contact with at least a portion of the core wire extending in the longitudinal direction of the belt, an tension rubber layer formed on one side of the adhesive rubber layer, and a compression rubber layer formed on the other side of the adhesive rubber layer, the compression rubber layer having a plurality of convex portions (cogs) formed on its inner circumferential surface at predetermined intervals along the longitudinal direction of the belt and frictionally engaging with a pulley on its side. Such raw edge cogged V-belts include raw edge cogged V-belts in which the cogs are formed only in the compression rubber layer, and raw edge double cogged V-belts in which similar cogs are formed on the outer circumferential surface of the tension rubber layer in addition to the compression rubber layer.

[0119] The transmission belt of the present invention is preferably applied to a thick belt. This is because a thick transmission belt is easily cracked due to a large distortion caused by bending, and the electrical conductivity retention is easily reduced. Therefore, when the rubber composition of the present invention is used, the electrical conductivity retention can be improved even in a thick transmission belt.

[0120] The thickness (average thickness) of the power transmission belt of the present invention may be 8 mm or more (for example, about 8 to 30 mm), preferably 9 mm or more (for example, about 9 to 20 mm), further preferably 10 mm or more, and further preferably 11 mm or more.

[0121] In this application, the thickness of a power transmission belt means the maximum thickness, for example, in a raw edge cogged V-belt, it means the shortest distance between the top and bottom of a cog portion.

[0122] [Manufacturing method of power transmission belt] The method for producing the power transmission belt of the present invention is not particularly limited, and any conventional method can be used depending on the type of belt.

[0123] For example, a typical manufacturing method of a raw edge cogged V-belt will be described below. First, a laminate of a reinforcing cloth (lower cloth) and a sheet for a compressed rubber layer (uncrosslinked rubber sheet) is placed in contact with a flat cog-equipped mold in which teeth and grooves corresponding to the cog portion (cog crest portion 1a and cog bottom portion 1b) are alternately arranged, with the reinforcing cloth facing downward, and pressed at a temperature of about 60 to 100°C (particularly 70 to 80°C) to produce a cog pad (a pad that is not completely crosslinked but is in a semi-crosslinked state) with a shaped cog portion. Then, both ends of this cog pad are cut vertically from appropriate positions (particularly the tops of the cog crest portions) to obtain the required length.

[0124] Next, an inner mold, in which teeth and grooves corresponding to the cog portions are arranged alternately, is placed over the outer periphery of a cylindrical mold, and a cog pad is wrapped around it by engaging the teeth and grooves of the inner mold and joining both ends (particularly the tops of the cog peaks).A sheet for the first adhesive rubber layer (lower adhesive rubber: uncrosslinked rubber sheet) is then laminated around the outer periphery of this cog pad, and the core wire (twisted cord) that forms the core body is spun spirally, and a sheet for the second adhesive rubber layer (upper adhesive rubber: uncrosslinked rubber sheet) and a sheet for the tension rubber layer (uncrosslinked rubber sheet) are sequentially wrapped around the outer periphery of this sheet to produce an uncrosslinked molded body.

[0125] Thereafter, the uncrosslinked molded body is covered with a jacket and placed in a known crosslinking device (such as a vulcanizing can) and crosslinked at a temperature of 120 to 200°C (particularly 150 to 180°C) to produce a crosslinked belt sleeve. Then, the uncrosslinked molded body is cut into a V shape using a cutter or the like to obtain an endless raw edge cogged V belt.

[0126] In this case, the reinforcing fabric and the sheet for the compressed rubber layer may be laminated on the outer periphery of the inner mold without preparing a cog pad. In this method, the reinforcing fabric and the sheet for the compressed rubber layer are pressed into the grooves of the inner mold during crosslinking molding to form the cog portion.

[0127] In the case of a raw-edge cogged V-belt not including a reinforcing fabric, a laminate may be prepared in advance by pressing a sheet for the compressed rubber layer and a sheet for the first adhesive rubber layer.

[0128] In addition, in the sheet for the tension rubber layer and the sheet for the compression rubber layer, the method of orienting the short fibers in the belt width direction can be a conventional method, for example, a method of rolling the rubber into a sheet by passing it between a pair of calendar rolls with a predetermined gap, cutting both sides of the rolled sheet with the short fibers oriented in the rolling direction in a direction parallel to the rolling direction, cutting the rolled sheet in a direction perpendicular to the rolling direction so as to have the belt forming width (length in the belt width direction), and joining the sides cut in the direction parallel to the rolling direction. For example, the method described in JP-A-2003-14054 can be used. The uncrosslinked sheet in which the short fibers are oriented by such a method can be arranged so that the short fibers are oriented in the belt width direction and crosslinked by the above method. EXAMPLES

[0129] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Details of the materials used are shown below.

[0130] [Materials used] (Polymers and Fillers) EPDM: "EP24" manufactured by JSR Corporation, ethylene content 54% by mass, diene (ethylidene norbornene) content 4.5% by mass, Mooney viscosity 42ML (1+4) 125℃ Short cotton fibers: Hashimoto's "cut cotton yarn", average fiber length 6 mm Polyester staple fiber: "PET cut yarn" manufactured by Koyo Short Fiber Co., Ltd., average fiber length 3 mm Para-aramid staple fiber: Teijin Limited's "Twaron (registered trademark)", average fiber length 3 mm Carbon black ISAF: "Seast 6" manufactured by Tokai Carbon Co., Ltd., DBP absorption capacity 114 mL / 100 g, BET specific surface area 119 m 2 / g, iodine adsorption capacity 121g / kg Conductive carbon black (acetylene black): "Denka Black" manufactured by Denka Co., Ltd., DBP absorption capacity 210 mL / 100 g, BET specific surface area 69 m 2 / g, iodine adsorption capacity 93g / kg Carbon black FEF: Cabot "Show Black N550" Silica: Evonik Degussa "Ultrasil VN3", BET specific surface area 175m 2 / g Clay (calcined clay): Imerys Performance Minerals "PoleStar", pH 6.2

[0131] (Crosslinking accelerator) Crosslinking accelerator TMTD (tetramethylthiuram disulfide): "Noccela TT" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Crosslinking accelerator CBS (N-cyclohexyl-2-benzothiazolylsulfenamide): "Noccela CZ" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Crosslinking accelerator MBTS (2,2'-dibenzothiazolyl disulfide): "Noccela DM" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0132] (Crosslinking agent and co-crosslinking agent) Co-crosslinking agent MPBM (N,N'-m-phenylenedimaleimide): "Valnoc PM" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Sulfur (powdered sulfur): "MIDAS" manufactured by Bigen Chemical Co., Ltd. Organic peroxide: 1,3-bis(t-butylperoxyisopropyl)benzene

[0133] (Other ingredients) Paraffin oil: "Diana Process Oil PW90" manufactured by Idemitsu Kosan Co., Ltd. Antioxidant DCD (4,4'-bis(α,α-dimethylbenzyl)diphenylamine): "Nocrac CD" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Anti-aging agent ODPA (octyldiphenylamine): "Nonflex OD-3" manufactured by Seiko Chemical Co., Ltd. Zinc oxide: "Zinc oxide type 2" manufactured by Sakai Chemical Industry Co., Ltd. Stearic acid: NOF Corp. "Camellia Stearate" Adhesion improver A (resorcinol-formaldehyde co-condensate): "Penacolite Resin (B-18-S)" manufactured by INDSPEC Chemical Corporation Adhesion improver B (hexamethoxymethylmelamine): SINGH PLASTICISER & RESINS "POWERPLAST PP-1890S"

[0134] [Core (processing code)] A core wire made by aligning multiple PET fiber bundles (raw yarns) with 384 filaments and 1220 dtex and twisting them in the S direction with a twist factor of 3.0 to make a first twisted yarn, and then aligning multiple first twisted yarns and twisting them in the Z direction with a twist factor of 3.0 to make a twisted cord (plied yarns) and then gluing the resulting cord. The core wire composition, total fineness, and core wire diameter are shown in Table 1. The first number in the composition indicates the number of raw yarns contained in the first twisted yarn (number of raw yarns pulled together), and the second number indicates the number of first twisted yarns contained in the plied yarn (number of first twisted yarns pulled together). The twist factor TF is a value calculated using the following formula.

[0135] TF=TN×D 0.5 / 960 [In the formula, TN indicates the number of twists per meter, and D indicates the fineness (tex) of the yarn.]

[0136] [Table 1]

[0137] [Reinforcing fabric covering the outer surface (treated canvas)] The treated canvas used to cover the outer surface of the belt is made of untreated cotton woven fabric [20s / 2 (20 count, 2-ply) cotton yarn with a warp density of 70 / 5cm and a weft density of 70 / 5cm, with a basis weight of approximately 180g / m 2The treated canvas (approximately 820 g / m2) was immersed in a treatment liquid (black dye liquid) shown in Table 2 containing a carbon black aqueous dispersion (solid content 25% by mass) and an RFL liquid (resorcinol, formalin, and latex mixture) for 10 seconds, subjected to a wide-angle treatment at 120° using a tenter, and then heat-treated at 150°C for 4 minutes. One side of the treated canvas was then coated with adhesive rubber (composition shown in Table 3 below). 2 A 1000mm thick plate was used.

[0138] [Table 2]

[0139] Examples 1 to 12, Comparative Examples 1 to 2, and Reference Examples 1 to 2 [Belt manufacturing] A laminate obtained by laminating an uncrosslinked compression rubber layer sheet having the composition shown in Tables 6 and 7 and an uncrosslinked first adhesive rubber layer sheet having the composition shown in Table 3 was wrapped around the outer periphery of a cog-equipped mold having alternating tooth portions and groove portions, with the compression rubber layer sheet facing the mold side. A core wire was then spirally wound around the outer periphery of the uncrosslinked first adhesive rubber layer sheet, and a laminate obtained by laminating an uncrosslinked second adhesive rubber layer sheet having the composition shown in Table 3 and an uncrosslinked tensile rubber layer sheet having the composition shown in Tables 6 and 7 was then wrapped around the outer periphery of the uncrosslinked second adhesive rubber layer sheet, with the uncrosslinked second adhesive rubber layer sheet facing the core wire side. A laminate was then produced by wrapping a treated canvas around the outer periphery of the tensile rubber layer sheet with the adhesive rubber coated surface facing the inner periphery side. After covering the outer periphery of the laminate with a flexible jacket, the mold was placed in a vulcanizer and steam was injected around the flexible jacket and into the inside of the mold to pressurize and heat (about 170°C) for 40 minutes to produce a belt sleeve. The produced belt sleeve was cut into a V shape with a cutter to produce a raw edge cogged V-belt with cogs on the inner periphery of the belt. The sizes of the produced belts are shown in Table 4. These belts are equivalent to narrow V-belts such as SPZ type and SPA type specified in ISO4184 (1992), and X indicates that the belt has cogs on the inner periphery of the belt.

[0140] [Table 3]

[0141] [Table 4]

[0142] [hardness] A Type A durometer as specified in JIS K 6253 (2012) (vulcanized rubber and thermoplastic rubber - Determination of hardness) was pressed against the compressed rubber layer on the side of the raw edge cogged V-belt, and the value was immediately read.

[0143] [Evaluation of crack resistance (time until cracks occur)] The crack resistance of raw edge cogged V-belts was evaluated using a three-axis running test machine equipped with a driving (Dr.) pulley, a driven (Dn.) pulley, and a tension (Ten.) pulley, as shown in Figure 1. The diameter of each pulley, initial tension, and driven pulley load were changed according to the belt shape, as shown in Table 5. The belt was run at a driving pulley speed of 4900 rpm and an ambient temperature of 85°C, and the time until cracks of 1.0 mm or more in depth appeared was measured. The shorter the time until cracks appeared, the better the crack resistance was judged to be, and a time of 170 hours or more was considered to be acceptable. The evaluation results using SPBX are shown in Tables 6 and 7.

[0144] [Table 5]

[0145] [Wear resistance evaluation (wear rate)] The wear resistance of the SPBX-type belt was evaluated using a two-axis running test machine consisting of a driving (Dr.) pulley with a diameter of 180 mm and a driven (Dn.) pulley with a diameter of 180 mm, as shown in Figure 2. In detail, a raw-edge cogged V-belt was hung on each pulley, and the belt was run for 100 hours at an ambient temperature of 23°C with an axle load of 1800 N, a driving pulley rotation speed of 1140 rpm, and a load on the driven pulley of 70 N·m. The mass of the belt was measured before and after the run, and the mass change rate (wear rate) was evaluated. The smaller the wear rate, the better the wear resistance, and a rate of 0.6% or less was considered to be acceptable. The evaluation results are shown in Tables 6 and 7.

[0146] Wear rate (%) = [(W0-W1) / W0] x 100 [In the formula, W0 represents the mass (g) of the belt before running, and W1 represents the mass (g) of the belt after running]

[0147] [Measurement of electrical resistance] The measurements were performed in accordance with the laboratory method specified in ISO1813 (2014). More specifically, as shown in the schematic cross-sectional view (cross-sectional view perpendicular to the belt length direction) in Figure 3, a pair of brass electrodes 2 (contact surface length 25 mm) were placed 100 mm apart on an insulating resin plate 1, and a raw edge cogged V-belt 3 was placed before running (unused) on the electrodes of the device, and a load of 1 N per 1 mm of belt width (upper width) was applied from above the belt. As shown in the schematic plan view in Figure 4, a voltage of 500 V was applied after the terminals of an insulation resistance meter 4 were attached to the electrodes 2, and the electrical resistance value was measured 5 seconds after the voltage application. The measurements were performed at room temperature of 23°C and relative humidity of 50%. Before placing the belt on the electrodes, the belt was cleaned with fuller's earth (Algital's "Green Clay Powder Active"), and a conductive paint (Pluscoat Co., Ltd.'s "Polycarm PCS-1201S") was applied between the belt and the electrodes. The electrical resistance was measured at 5 equal points along the length of the belt, and the average value was used. The smaller the electrical resistance, the better the effect of preventing static electricity in the belt. The results are shown in Tables 6 and 7.

[0148] [Conductivity maintenance (rate of change in electrical resistance)] The electrical resistance of the raw-edge cogged V-belt after running (the belt after the crack resistance evaluation) was measured in the same manner as the measurement of the electrical resistance of the belt before running (unused) and the rate of change in electrical resistance was calculated using the following formula. The smaller the rate of change in electrical resistance, the better the electrical conductivity retention, and a rate of change of 200% or less was considered to be acceptable. The results are shown in Tables 6 and 7.

[0149] Rate of change in electrical resistance (%) = [(R1-R0) / R0] x 100 [In the formula, R0 represents the electrical resistance value (MΩ) of the belt before running (unused), and R1 represents the electrical resistance value (MΩ) of the belt after running (after evaluating crack resistance)]

[0150] [Table 6]

[0151] [Table 7]

[0152] Tables 6 and 7 show the evaluation results of the SPBX type belt. Examples 1 to 5 had a small rate of change in electrical resistance and were excellent in abrasion resistance and crack resistance. Example 4 is an example in which the short fibers do not contain natural short fibers, but the crack resistance was reduced compared to Example 1. Example 5 is an example in which the short fibers do not contain synthetic short fibers, but the abrasion resistance was reduced compared to Example 1.

[0153] On the other hand, Comparative Example 1 in which crosslinking was performed with an organic peroxide instead of sulfur, and Comparative Example 2 in which no co-crosslinking agent was included, had low crack resistance and a large rate of change in electrical resistance value.

[0154] Reference Example 1, which contained a small amount of carbon black, had low abrasion resistance and a large electrical resistance value before and after running, and a large rate of change in electrical resistance value. Reference Example 2, which contained a large amount of carbon black, had low crack resistance.

[0155] In Examples 6 and 7, the short fibers in Example 1 were changed to aramid short fibers, but compared to Example 1, the crack resistance was reduced.

[0156] Example 8 is an example in which the amount of the co-crosslinking agent was reduced from that of Example 1, and the abrasion resistance was reduced compared to that of Example 1.

[0157] Examples 9 and 10 are examples in which part of the carbon black in Example 1 was changed to conductive carbon black. Compared with Example 1, however, the abrasion resistance and crack resistance were reduced.

[0158] Examples 11 and 12 are examples in which the amount of carbon black was reduced and the amount of clay was increased from Example 1, but compared to Example 1, the crack resistance was reduced.

[0159] Next, the rate of change in electrical resistance was measured for the SPZX, SPAX, and SPCX type belts, and the results are shown in Table 8. The rubber composition was the same as that of Example 1 in Table 6.

[0160] [Table 8]

[0161] As is clear from the results in Table 8, the rate of change in electrical resistance value was small for all belts, confirming that they had excellent electrical conductivity retention. [Industrial Applicability]

[0162] The rubber composition of the present invention can be used for various molded articles, such as tires, hoses, power transmission belts, and conveyor belts, but is particularly preferably used for power transmission belts. The power transmission belts can be used, for example, friction power transmission belts such as flat belts, V-belts (wrapped V-belts, low-edge V-belts, low-edge cogged V-belts, low-edge double cogged V-belts, etc.), V-ribbed belts, and resin block belts; meshing power transmission belts such as toothed belts and double-sided toothed belts, etc. In particular, when used as a compressed rubber layer of a power transmission belt, it is useful for the compressed rubber layer of a speed change belt (low-edge cogged V-belts, low-edge double cogged V-belts, etc.) used in motorcycles, four-wheeled buggies, snowmobiles, agricultural machines, etc., which are becoming increasingly powerful, because of its excellent wear resistance and crack resistance.

Claims

1. A rubber composition comprising a polymer component, carbon black, a crosslinking agent and a co-crosslinking agent, the polymer component comprises an ethylene-α-olefin elastomer; The crosslinking agent comprises a sulfur-based crosslinking agent; and The rubber composition has a ratio of the carbon black of 55 to 85 parts by mass per 100 parts by mass of the polymer component.

2. 2. The rubber composition according to claim 1, further comprising short fibers, the proportion of said short fibers being 15 to 50 parts by mass per 100 parts by mass of said polymer component.

3. 3. The rubber composition according to claim 2, wherein said staple fibers comprise synthetic staple fibers and natural staple fibers.

4. 4. The rubber composition according to claim 2 or 3, wherein the staple fibers are a combination of at least one synthetic staple fiber selected from the group consisting of polyester staple fibers and aramid staple fibers and cellulose staple fibers, and the proportion of the cellulose staple fibers is 10 to 100 parts by mass per 100 parts by mass of the synthetic staple fibers.

5. 3. The rubber composition according to claim 1, wherein the crosslinking agent is a sulfur-based crosslinking agent.

6. 3. The rubber composition according to claim 1, further comprising clay, the proportion of said clay being 20 to 60 parts by mass per 100 parts by mass of said carbon black.

7. A power transmission belt comprising a crosslinked product of the rubber composition according to claim 1 or 2.

8. 8. The power transmission belt according to claim 7, which has a thickness of 8 mm or more.

Citation Information

Patent Citations

  • Transmission belt

    JP2006064174A

  • Drive belt and its manufacturing method

    JP2009024757A

  • Rubber composition and power transmitting belt

    JP2009249519A

  • Friction transmission belt and method of manufacturing the same

    JP2013185678A

  • Transmission belt

    JP2016211589A