Acoustic resonator device, filter device, and method for manufacturing an acoustic resonator device
XBARs with a half-lambda dielectric layer address the limitations of SAW and BAW resonators by enhancing rigidity, thermal conductivity, and capacitance, enabling efficient operation in higher frequency communication bands.
Patent Information
- Application Number
- JP2021553386
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-16
- Filing Date
- 2020-03-16
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-03-16
AI Technical Summary
Existing RF filters using surface acoustic wave (SAW) resonators and bulk acoustic wave (BAW) resonators are not suitable for higher frequency communication bands proposed in future communication networks.
The use of laterally excited film bulk acoustic resonators (XBARs) with a half-lambda dielectric layer to enhance performance, including a thicker diaphragm for higher rigidity and thermal conductivity, and a larger capacitance per unit area, which are suitable for frequencies above 3 GHz.
The XBARs with a half-lambda dielectric layer provide improved electromechanical coupling, reduced spurious modes, and stable frequency tuning, enabling effective operation in higher frequency bands with reduced temperature sensitivity.
Smart Images

Figure 0007556358000004 
Figure 0007556358000010 
Figure 0007556358000009
Abstract
Description
[Technical field]
[0001] The present disclosure relates to radio frequency filters using acoustic wave resonators, and in particular to filters for use in communications devices. [Background technology]
[0002] 2. Description of Related Art A radio frequency (RF) filter is a two-port device configured to pass some frequencies and stop others, where "pass" means to transmit with relatively low signal loss and "stop" means to block or substantially attenuate. The range of frequencies that a filter passes is called the filter's "passband." The range of frequencies that a filter stops is called the filter's "stopband." A typical RF filter has at least one passband and at least one stopband. The specific requirements for passbands and stopbands depend on the particular application. For example, a "passband" may be defined as the frequency range over which the insertion loss of a filter is better than a defined value, such as 1 dB, 2 dB, or 3 dB. A "stopband" may be defined as the frequency range over which the filter's rejection is greater than a defined value, such as 20 dB, 30 dB, or 40 dB, depending on the application.
[0003] RF filters are used in communications systems that transmit information over radio links. For example, RF filters are found in cellular base stations, mobile phones and computing devices, satellite transceivers and ground stations, Internet of Things (IoT) devices, laptop computers and tablets, fixed-point wireless links, and the RF front-end of other communications systems. RF filters are also used in radar and electronic and information warfare systems.
[0004] RF filters typically require many design trade-offs to achieve the best compromise between performance parameters such as insertion loss, rejection, isolation, power handling, linearity, size, cost, etc. for each specific application. Specific design and manufacturing methods and improvements can simultaneously meet one or more of these requirements.
[0005] Improving the performance of RF filters in wireless systems has a wide impact on system performance. RF filter improvements can be leveraged to improve system performance, including larger cell size, longer battery life, higher data rates, greater network capacity, lower cost, improved security, and increased reliability. These improvements can be realized alone or in combination at many levels of a wireless system, e.g., at the RF module, RF transceiver, mobile or fixed subsystems, and network level.
[0006] The desire for wider bandwidth for communication channels inevitably leads to the use of higher frequency communication bands. Current LTE (Long Term Evolution) specifications define frequency bands from 3.3 GHz to 5.9 GHz. Some of these bands are not currently in use. Proposals for future wireless communications include millimeter wave communication bands up to 28 GHz. Summary of the Invention
[0007] High performance RF filters in current communication systems typically incorporate surface acoustic wave (SAW) resonators, bulk acoustic wave (BAW) resonators, film bulk acoustic wave resonators (FBARs) or other acoustic resonators, but these existing technologies are not suitable for use at the higher frequencies proposed for future communication networks. [Brief description of the drawings]
[0008] [Figure 1]1 includes a schematic plan view and two schematic cross-sectional views of a transversely excited film bulk acoustic resonator (XBAR). [Diagram 2] FIG. 2 is an enlarged schematic cross-sectional view of a portion of XBAR in FIG. [Diagram 3] 1 is an enlarged schematic cross-sectional view of a portion of an improved XBAR including a "half-lambda" dielectric layer. [Figure 4] 1 is a graph comparing the admittance of an XBAR having a half-lambda dielectric layer and a conventional XBAR. [Diagram 5] 1 is a cross-sectional view of an XBAR with a half-lambda dielectric layer contoured to represent stress at resonant frequency; [Figure 6] 1 is a graph comparing the admittance of three XBARs with half-lambda AlN layers. [Figure 7] 1 is a graph comparing the admittance of three XBARs with half-lambda SiO 2 layers. [Figure 8] 13 is a graph comparing the admittance of three other XBARs with half-lambda SiO 2 layers. [Figure 9] 13 is a graph showing the admittance of an XBAR having an excessively thin half-lambda SiO 2 layer. [Figure 10] 13 is a graph showing the admittance of an XBAR having an excessively thin half-lambda SiO 2 layer. [Figure 11] 1 is a graph showing the temperature coefficient of frequency of an XBAR as a function of SiO2 thickness. [Figure 12] 1 is a schematic circuit diagram and layout of a filter using XBAR. [Figure 13] 1 is a flow chart of a process for fabricating an XBAR including a half-lambda dielectric layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In this specification, features appearing in the figures are assigned three or four digit reference numbers, with the least significant two digits being unique to the feature and the most significant one or two digits being the number of the figure in which the feature is first introduced. Features not described in conjunction with a figure can be presumed to have the same characteristics and functionality as previously described features having the same reference number.
[0010] Detailed Description Equipment Description 1 shows a simplified schematic top view and orthogonal cross-sectional view of a transversely excited film bulk acoustic resonator (XBAR) 100 described in U.S. Patent No. 10,491,192. XBAR resonators such as resonator 100 may be used in a variety of RF filters, including band-reject filters, band-pass filters, duplexers, and multiplexers. XBARs are particularly well suited for use in filters for communication bands with frequencies above 3 GHz.
[0011] The XBAR 100 is a piezoelectric plate 110 having parallel front and back surfaces 112, 114, respectively, with thin film conductor patterns formed on the surfaces. The plate is a thin single crystal layer of piezoelectric material such as lithium niobate, lithium tantalate, lanthanum gallium silicate, gallium nitride, or aluminum nitride. The plate is cut so that the orientation of the X, Y, and Z crystal axes relative to the front and back surfaces is known and consistent. In the example presented in this patent, the plate is Z-cut, meaning that the Z axis is perpendicular to the front and back surfaces 112, 114. However, XBARs can be fabricated with piezoelectric plates of other crystallographic orientations.
[0012] The rear surface 114 of the piezoelectric plate 110 is attached to the surface of the substrate 120, except for the portion of the piezoelectric plate 110 that forms a diaphragm 115 that straddles a cavity 140 formed in the substrate. The portion of the piezoelectric plate that straddles the cavity will be referred to herein as the "diaphragm" 115 because of its physical similarity to the diaphragm of a microphone. As shown in FIG. 1, the diaphragm 115 is continuous with the remainder of the piezoelectric plate 110 around the entire perimeter 145 of the cavity 140. "Continuous" in this context means "connected in a continuous manner without any intervening material."
[0013] The substrate 120 provides mechanical support for the piezoelectric plate 110. The substrate 120 may be, for example, silicon, sapphire, quartz, or other material or combination of materials. The back surface 114 of the piezoelectric plate 110 may be bonded to the substrate 120 using a wafer bonding process. Alternatively, the piezoelectric plate 110 may be grown on the substrate 120 or attached to the substrate in other ways. The piezoelectric plate 110 may be attached directly to the substrate or to the substrate 120 via one or more intermediate layers of material.
[0014] "Cavity" has its conventional meaning of "empty space in a solid." Cavity 140 may be a hole that passes completely through substrate 120 (as shown in cross sections AA and BB) or may be a recess in substrate 120. Cavity 140 may be formed, for example, by selectively etching substrate 120 before or after attachment of piezoelectric plate 110 and substrate 120.
[0015] The conductor pattern of XBAR 100 includes an interdigital transducer (IDT) 130. IDT 130 includes a first plurality of parallel fingers, such as finger 136, extending from a first bus bar 132 and a second plurality of fingers extending from a second bus bar 134. The first and second plurality of parallel fingers are interleaved. The interleaved fingers typically overlap by a distance AP, referred to as the "aperture" of the IDT. The center-to-center distance L between the outermost fingers of IDT 130 is the "length" of the IDT.
[0016] The first and second bus bars 132, 134 serve as the terminals of the XBAR 100. A radio frequency or microwave signal applied between the two bus bars 132, 134 of the IDT 130 excites a primary acoustic mode in the piezoelectric plate 110. The primary acoustic mode is a bulk shear mode, in which acoustic energy propagates along a direction substantially perpendicular to the plane of the piezoelectric plate 110, which is also perpendicular, or transverse, to the direction of the electric field created by the IDT fingers. In this manner, the XBAR can be considered a laterally excited film bulk wave resonator.
[0017] The IDT 130 is positioned on the piezoelectric plate 110 such that at least the fingers of the IDT 130 are located in a portion 115 of the piezoelectric plate that straddles or is suspended above the cavity 140. As shown in FIG. 1, the cavity 140 has a rectangular shape with an extent that is greater than the gap AP and length L of the IDT 130. The XBAR cavity may have a variety of shapes, including regular polygons and irregular polygons. The XBAR cavity may or may not have four or more sides, and the sides may be straight or curved.
[0018] For ease of illustration in Figure 1, the geometric pitch and width of the IDT fingers are greatly exaggerated relative to the length (dimension L) and spacing (dimension AP) of the XBAR. A typical XBAR has 10 or more parallel fingers in the IDT 110. An XBAR can have hundreds, or even thousands, of parallel fingers in the IDT 110. Similarly, the thickness of the fingers in the cross-sectional view is greatly exaggerated.
[0019] Figure 2 is a detailed schematic cross-sectional view of an XBAR 200, which may be XBAR 100 of Figure 1. Piezoelectric plate 210 is a single crystal layer of piezoelectric material having a front surface 214 and a back surface 216. A thickness ts between front surface 214 and back surface 216 may be, for example, 100 nm to 1500 nm. For use in a 5G NR (fifth generation new wireless) or Wi-Fi (registered trademark) band (3.3 GHZ to 6 GHz) filter, thickness ts may be, for example, 280 nm to 550 nm.
[0020] The IDT fingers 238 may be aluminum, a substantially aluminum alloy, copper, a substantially copper alloy, tungsten, molybdenum, beryllium, gold, or other conductive material. A thin layer (relative to the total conductor thickness) of other metals such as chromium or titanium may be formed under and / or over the fingers to improve the bond between the fingers and the piezoelectric plate 210 and / or to passivate or encapsulate the fingers. The IDT busbars (132, 134 in FIG. 1) may be made of the same or different material as the fingers.
[0021] Dimension p is the center-to-center spacing or "pitch" of the IDT fingers, sometimes referred to as the IDT pitch and / or the XBAR pitch. Dimension w is the width or "mark" of the IDT fingers. XBAR IDTs are substantially different from IDTs in surface acoustic wave (SAW) resonators, where the IDT pitch is 1 / 2 the acoustic wavelength at the resonant frequency. Furthermore, the mark-to-pitch ratio of SAW resonator IDTs is typically close to 0.5 (i.e., the width of the marks or fingers is approximately 1 / 4 the acoustic wavelength at resonance). In XBARs, the IDT pitch p is typically 2-20 times the finger width w. Additionally, the IDT pitch p is typically 2-20 times the thickness ts of the piezoelectric plate 210. The width of the XBAR IDT fingers is not constrained to 1 / 4 the acoustic wavelength at resonance. For example, the width of the XBAR IDT fingers can be 500 nm or more so that the IDTs can be fabricated using optical lithography. The thickness tm of the IDT fingers can be from 100 nm to approximately equal to the width w. The thickness of the IDT busbars (132, 134 in FIG. 1) can be the same as or greater than the thickness tm of the IDT fingers.
[0022] A shear bulk acoustic wave (BAW) propagating perpendicular to the plane of a piezoelectric plate will reflect off the surface and form a resonance, or standing wave, when the thickness ts of the plate is an integer multiple of 1 / 2 the wavelength λ of the acoustic wave. The longest wavelength / lowest frequency at which such a resonance occurs is the frequency f0, with a wavelength λ equal to twice the thickness ts of the piezoelectric plate. 0, s is the shear BAW fundamental resonance. 0, "s" means the wavelength of the fundamental (0th order) shear BAW resonance of the piezoelectric plate within the piezoelectric plate. The same acoustic wave (i.e., shear BAW propagating in the same direction at the same frequency) may have a different wavelength in other materials. Note that the frequency f0 is the velocity of the shear BAW of the piezoelectric plate, expressed as the wavelength λ 0, The shear BAW fundamental resonance of the piezoelectric plate is not the same as the resonance of the XBAR element 200, which is influenced by the IDT structure.
[0023] FIG. 3 is a detailed schematic cross-sectional view of an XBAR incorporating a "half-lambda" dielectric layer. FIG. 3 specifically shows an XBAR 300 having a thick dielectric layer 350 on the front side of the piezoelectric plate 310 (i.e., the side facing away from the substrate, the top side as shown in FIG. 3). Instead of the dielectric layer 350, it is also possible to use an equivalent dielectric layer on the back side 316 of the piezoelectric plate 310. On a larger scale, the XBAR 300 having the thick dielectric layer 350 is similar to the XBAR 100 of FIG. 1. FIG. 3 also shows two IDT fingers 338 as previously described. Dimension p is the center-to-center spacing or "pitch" of the IDT fingers, and dimension w is the width or "mark" of the IDT fingers.
[0024] The piezoelectric plate 310 is a thin single crystal layer of a piezoelectric material such as lithium niobate or lithium tantalate. The piezoelectric plate 310 is cut so that the orientations of the X, Y, and Z crystal axes relative to the front and back surfaces 314, 316 are known and consistent. The thickness ts of the piezoelectric plate 310 may be, for example, between 100 nm and 1500 nm.
[0025] The dielectric layer 350 can be nearly any dielectric material, such as SiO2, Si3N4, Al2O3, AlN, or other materials. As will be described below, particular advantages may be obtained when the dielectric material is or includes AlN and when the dielectric material is SiO2.
[0026] The thickness ts of the piezoelectric plate 310 and the thickness td of the dielectric layer 350 are configured such that the shear BAW propagating perpendicular to the faces 316 and 352 forms a full-period standing wave between the faces 316 and 352 at a predetermined frequency that may be slightly less than the desired resonant frequency of the XBAR device 300. That is, a second harmonic resonance of the shear BAW occurs at the predetermined frequency. By definition, the thickness ts of the piezoelectric plate is equal to or greater than λ, which is the wavelength of the fundamental shear BAW resonance of the piezoelectric plate 310 without the dielectric layer 350, as discussed above. 0, Nominally, the thickness td of the dielectric layer 350 is λ 0,d 1 / 2 of λ 0,dis the wavelength of the same bulk BAW in the dielectric layer 350. In this case, each of the piezoelectric plate 310 and the dielectric layer 350 contains a standing wave with a half period of f0, which is the frequency of the current second harmonic resonance. 0,d is the ratio of the velocity of the shear acoustic wave in the dielectric layer 350 to the velocity of the shear acoustic wave in the piezoelectric plate 310, λ 0,s For a relatively slow dielectric material such as SiO2, λ 0,d is λ 0,s In this case, the thickness td of the dielectric layer 350 may be the same as or slightly larger than ts. For relatively fast dielectric materials such as Si3N4 and AlN, λ 0,d is λ 0,s In this case, the thickness td of the dielectric layer 350 is proportionally greater than ts.
[0027] In this specification, the dielectric layer 350 is referred to as a "half-lambda" dielectric layer, but the thickness t of the dielectric layer is exactly λ. 0,d The total thickness of the piezoelectric plate 310 and the dielectric layer 350 is such that the second harmonic resonance of the bulk shear wave occurs at a given frequency, and the thickness td is λ 0,d The results of the simulations are as follows: 0.85λ 0,d ≦2td≦1.15λ 0,d (1) A range of dielectric layer thicknesses defined by will result in an XBAR with stable electromechanical coupling with low spurious modes. Values of td outside this range will result in weaker electromechanical coupling and an increase in spurious modes. Varying td within this range can tune the resonant frequency of the XBAR by about 10%, which is sufficient to establish the required frequency offset between the shunt and series resonators in many filter applications.
[0028] 3, the dielectric layer 350 is shown deposited over and between the IDT fingers 338. In other embodiments, the half-lambda dielectric layer may be formed only between the IDT fingers. The half-lambda dielectric layer 350 may be a single layer or two or more layers of different dielectric materials with similar acoustic impedance.
[0029] The primary advantage of incorporating half-lambda dielectric layer 350 into XBAR 300 is the increased thickness of the diaphragm. Depending on the material used for half-lambda dielectric layer 350, the thickness of the diaphragm of XBAR 300 may be two to three times the thickness of diaphragm 115 of XBAR 100 of Figure 1. A thicker diaphragm has higher stiffness and is less likely to warp or distort due to temperature changes.
[0030] The thicker diaphragm of XBAR300 also has higher thermal conductivity, especially when half-lambda dielectric layer 350 is or includes a highly thermally conductive dielectric material such as aluminum nitride. Higher thermal conductivity allows heat to be removed from the diaphragm more efficiently, allowing a smaller resonator area to be used for a given thermal load or power dissipation.
[0031] The XBAR300 also has a larger capacitance per unit area compared to the XBAR100 in Figure 1 (for the same IDT pitch). The capacitance of the resonator is a circuit design issue. RF filters, especially those using acoustic resonators, are usually required to have the input and output impedance of the filter match a specified value (usually 50 Ω). This requirement determines the minimum capacitance value of some or all of the resonators in the filter. The larger capacitance per unit area of the XBAR300 with its partial Bragg reflector allows the use of a smaller resonator area for the required capacitance value.
[0032] An XBAR (not shown) with a half-lambda dielectric layer on the back side of the piezoelectric plate 310 improves stiffness and thermal conductivity, but only slightly increases the capacitance per unit area.
[0033] FIG. 4 is a graph 400 comparing the admittance of an XBAR with a half-lambda dielectric layer to a conventional XBAR. The data in FIG. 4 and in FIGS. 6 and 7, discussed below, are the result of a finite element simulation of an XBAR device. The solid line 410 plots the magnitude of admittance as a function of frequency for an XBAR including a half-lambda dielectric layer. The piezoelectric plate is 400 nm thick lithium niobate. The IDT is 100 nm thick aluminum. The IDT finger pitch and mark are 4.25 μm and 1.275 μm, respectively. The half-lambda dielectric layer is composed of a 350 nm thick Si3N4 layer and a 350 nm thick AlN layer. The resonant frequency is 4.607 GHz and the anti-resonant frequency is 4.862 GHz. The difference between the anti-resonant and resonant frequencies is 255 MHz, which is about 5.4% of the average of the resonant and anti-resonant frequencies.
[0034] Dashed line 420 is a plot of the magnitude of admittance as a function of frequency for a conventional XBAR. The piezoelectric plate is 400 nm thick lithium niobate. The IDT is 100 nm thick aluminum. The IDT finger pitch and marks are 3.7 μm and 0.47 μm, respectively. The resonant frequency is 4.71 GHz and the anti-resonant frequency is 5.32 GHz. The difference between the anti-resonant and resonant frequencies is 610 MHz, which is about 12.2% of the average of the resonant and anti-resonant frequencies. The admittance of the conventional XBAR (dashed line 420) shows several spurious modes between the resonant and anti-resonant frequencies that are not present in the admittance of the XBAR with a half-lambda dielectric layer (solid line 410).
[0035] The incorporation of a half-lambda dielectric layer into the XBAR device 300 provides a stiffer diaphragm with higher thermal conductivity and potentially less excitation of spurious modes compared to conventional XBAR devices, with the benefit of reduced electromechanical coupling and associated smaller difference between resonant and anti-resonant frequencies.
[0036] Figure 5 is a cross-sectional view of an XBAR 500 with a half-lambda dielectric layer with contours showing stress at resonant frequency. The piezoelectric plate 510 is 400 nm thick lithium niobate. The IDT fingers 538 are 100 nm thick aluminum. The half-lambda dielectric layer 550 is composed of a 350 nm thick Si3N4 layer 552 and a 350 nm thick AlN layer 554.
[0037] The stress in XBAR 500 at the resonant frequency reflects a full-period standing wave between the faces of the device. The stress corresponds to the peaks of the two half-periods of the standing wave and is highest near the center of the thickness of the piezoelectric plate 510 and near the center of the dielectric layer 550. The stress is lowest near the faces of the device, near the boundary between the piezoelectric plate 510 and the dielectric layer 550 near the center, corresponding to the zero crossings of the standing wave.
[0038] FIG. 6 is a graph 600 illustrating the use of pitch and dielectric layer thickness to tune the resonant and anti-resonant frequencies of an XBAR with a half-lambda dielectric layer. The solid line 610 is a plot of admittance magnitude as a function of frequency for an XBAR with pitch and mark of 4.25 μm and 1.275 μm, respectively. The piezoelectric plate is 400 nm thick lithium niobate. The IDT is 100 nm thick aluminum. The half-lambda dielectric layer is composed of a 700 nm thick layer of Si3N4. The resonant frequency is 4.513 GHz and the anti-resonant frequency is 4.749 GHz. The difference between the anti-resonant and resonant frequencies is 236 MHz, which is about 5.1% of the average of the resonant and anti-resonant frequencies.
[0039] The dotted line 620 is a plot of the magnitude of admittance as a function of frequency for a similar XBAR with the same structure except that the IDT finger pitch and marks are 3.75 μm and 1.31 μm, respectively. The resonant frequency is 4.557 GHz and the anti-resonant frequency is 4.795 GHz. Changing the IDT pitch from 4.25 μm to 3.75 μm increases the resonant and anti-resonant frequencies by about 45 MHz. Varying the pitch from 3 μm to 5 μm provides a tuning range of about 200 MHz.
[0040] The dashed line 630 plots the magnitude of admittance as a function of frequency for a similar XBAR. The IDT finger pitch and mark are 4.25 μm and 1.275 μm, respectively, and the dielectric layer includes a 700 nm thick Si3N4 layer plus a 50 nm SiO2 layer. The resonant frequency is 4.400 GHz and the anti-resonant frequency is 4.626 GHz. The addition of a 50 nm "tuning layer" reduces the resonant and anti-resonant frequencies by about 110 MHz.
[0041] FIG. 7 is another graph 700 illustrating the use of pitch and dielectric layer thickness to tune the resonant and anti-resonant frequencies of an XBAR with a half-lambda dielectric layer. The solid line 710 plots the magnitude of admittance as a function of frequency for an XBAR with pitch and mark of 4.25 μm and 1.275 μm, respectively. The piezoelectric plate is 400 nm thick lithium niobate. The IDT is 100 nm thick aluminum. The half-lambda dielectric layer is composed of a 400 nm thick layer of SiO2. The resonant frequency is 4.705 GHz and the anti-resonant frequency is 5.108 GHz. The difference between the anti-resonant and resonant frequencies is 403 MHz, which is about 8.2% of the average of the resonant and anti-resonant frequencies.
[0042] The dotted line 720 plots the magnitude of admittance as a function of frequency for a similar XBAR with the same structure except that the IDT finger pitch and marks are 3.75 μm and 1.31 μm, respectively. The resonant frequency is 4.740 GHz and the anti-resonant frequency is 5.137 GHz. Changing the IDT pitch from 4.25 μm to 3.75 μm increases the resonant and anti-resonant frequencies by about 35 MHz. Varying the pitch from 3 μm to 5 μm provides a tuning range of about 100 MHz.
[0043] Dashed line 730 plots the magnitude of admittance as a function of frequency for a similar XBAR with the same structure except that the IDT finger pitch and marks are 4.25 μm and 1.275 μm, respectively, and the dielectric layer is 450 nm thick SiO2. The resonant frequency is 4.512 GHz and the anti-resonant frequency is 4.905 GHz. The difference between the anti-resonant and resonant frequencies is 393 MHz, which is about 8.3% of the average resonant and anti-resonant frequencies. Increasing the thickness of the dielectric layer by 50 nm reduces the resonant and anti-resonant frequencies by about 190 MHz without reducing the electromechanical coupling.
[0044] FIG. 8 is another graph 800 illustrating the use of dielectric layer thickness to tune the resonant and anti-resonant frequencies of an XBAR with a half-lambda dielectric layer. The dotted line 810 is a plot of admittance magnitude as a function of frequency for an XBAR with pitch and mark of 4.25 μm and 1.275 pm, respectively. The piezoelectric plate is 400 nm thick lithium niobate. The IDT is 100 nm thick aluminum. The half-lambda dielectric layer is comprised of a 425 nm thick layer of SiO2. In this example, the dielectric layer thickness td is λ. 0,d / 2.
[0045] The solid line 820 plots the magnitude of admittance as a function of frequency for a similar XBAR of the same structure except that the dielectric layer is SiO2 with a thickness of 375 nm. In this case, td=0.88(λ 0,d / 2). The dashed line 830 plots the magnitude of admittance as a function of frequency for a similar XBAR of the same structure except that the dielectric layer is SiO2 with a thickness of 475 nm. In this case, td=1.12(λ 0,d Changing the SiO2 from 375 nm to 475 nm shifts the resonant and antiresonant frequencies by about 400 MHz while maintaining electromechanical coupling and without introducing objectionable spurious modes.
[0046] Assuming a lithium niobate piezoelectric plate with a thickness of 400 nm, the range of td expressed by formula (1) corresponds to approximately 350 nm to 500 nm. This range can be expressed as follows in terms of the thickness ts of the piezoelectric plate: 0.875ts≦td≦1.25ts (2) This range is believed to apply to any thickness of the lithium niobate piezoelectric plate.
[0047] Figure 9 is a graph 900 illustrating the effect of an overly thin "half-lambda" dielectric layer. The solid line 910 plots the magnitude of admittance as a function of frequency for an XBAR having the same structure as the device of Figure 8, but with the SiO2 dielectric layer thickness reduced to 325 nm. In this case, td=0.76(lambda 0,d This reduction in the thickness of the dielectric layer reduces the electromechanical coupling and generates very large spurious modes below the resonant frequency of the device.
[0048] FIG. 10 is a graph 1000 illustrating the effect of making a "half-lambda" dielectric layer too thick. The solid line 910 plots the magnitude of admittance as a function of frequency for an XBAR having the same structure as the device of FIG. 8, but with the SiO2 dielectric layer thickness increased to 525 nm. In this case, td=1.24(λ 0,d Increasing the thickness of the dielectric layer in this way reduces the electromechanical coupling and generates very large spurious modes that exceed the resonant frequency of the device.
[0049] The temperature coefficients of frequency for SiO2 and lithium niobate are similar in magnitude and opposite in sign, and XBAR devices using SiO2 half-lambda for the dielectric layer exhibit substantially less frequency change with temperature than conventional XBAR devices.
[0050] FIG. 11 is a graph showing the temperature coefficient of frequency of an XBAR as a function of SiO2 thickness. Specifically, solid line 1110 plots the temperature coefficient of the anti-resonant frequency of the XBAR device whose admittance characteristics were previously shown in FIGS. 7 and 8. Dashed line 1120 plots the temperature coefficient of the resonant frequency of the same device. Simulations have shown that a conventional XBAR device without a dielectric layer has a temperature coefficient of frequency of approximately -113 ppm / °C. The presence of a SiO2 half-lambda dielectric layer reduces the magnitude of the temperature coefficient of frequency by approximately a factor of three.
[0051] FIG. 12 is a schematic circuit diagram of a bandpass filter 1200 using five XBARs X1-X5. The filter 1200 may be, for example, a bandpass filter for band n79 used in a communication device. The filter 1200 has a conventional ladder filter structure including three series resonators X1, X3, X5 and two shunt resonators X2, X4. The three series resonators X1, X3, X5 are connected in series between a first port and a second port. In FIG. 12, the first port and the second port are shown with "In" and "Out", respectively. However, the filter 1200 is bidirectional, and either port may function as the input or output of the filter. The two shunt resonators X2, X4 are connected from the node between the series resonators to ground. All the shunt resonators and the series resonators are XBARs.
[0052] The three series resonators X1, X3, X5 and the two shunt resonators X2, X4 of the filter 1200 may be formed on a single plate 1230 of piezoelectric material bonded to a silicon substrate (not visible). Each resonator includes a respective IDT (not shown), with at least the fingers of the IDT disposed over a cavity in the substrate. In this context or a similar context, the word "respective" means "each to each related," i.e., one-to-one correspondence. In FIG. 12, the cavities are shown generally as dashed rectangles (such as rectangle 1235). In this example, the IDT of each resonator is disposed over a respective cavity. In other filters, the IDTs of two or more resonators may be disposed over a common cavity. Also, the resonators may be cascaded into multiple IDTs, and multiple cavities may be formed with multiple IDTs.
[0053] Each of the resonators X1 to X5 has a resonant frequency and an anti-resonant frequency. Simply put, each resonator is effectively short-circuited at its resonant frequency and effectively open-circuited at its anti-resonant frequency. Each of the resonators X1 to X5 creates a "zero transmittance" where the transmittance between the input and output ports of the filter is very low. Note that the transmittance at the "zero transmittance" is not actually zero due to effects such as energy leakage due to parasitic components. The three series resonators X1, X3, and X5 create zero transmittance at their respective anti-resonant frequencies (each resonator is effectively an open circuit). The two shunt resonators X2 and X4 form zero transmittance at their respective resonant frequencies (each resonator is effectively short-circuited). In a typical bandpass filter using acoustic resonators, the anti-resonant frequency of the series resonators is higher than the upper end of the passband, so the series resonators create zero transmittance above the passband. The resonant frequency of the shunt resonators is lower than the lower end of the passband, so the shunt resonators create zero transmittance below the passband.
[0054] Referring to the admittance vs. frequency data in Figures 7 and 8, it can be seen that the frequency offset between the resonant and anti-resonant frequencies of an XBAR with a 400 nm lithium niobate piezoelectric plate and a half lambda dielectric layer is about 400 MHz. This frequency separation is not sufficient for bandpass filtering in communication bands such as n79 (4400 MHz to 5000 MHz) and n77 (3300 MHZ to 4200 MHz). U.S. Patent No. 10,491,192 describes depositing a dielectric layer on the shunt resonator to lower the resonant frequency of the shunt resonator relative to the resonant frequency of the series resonator. Patent No. 10,491,192 describes a filter in which the series resonator has a very thin or no dielectric layer and the shunt resonator has a dielectric layer that is about 0.25 times the thickness of the piezoelectric plate.
[0055] A similar approach can be used to lower the resonant frequency of the shunt resonator relative to the resonant frequency of the series resonator if the resonators are XBARs with half-lambda dielectric layers. In this case, the thickness of the dielectric layer on the series resonator, tds, and the thickness of the dielectric layer on the shunt (parallel) resonator, tdp, are given by: 0.85 λ 0,d ≦2tds<2tdp≦1.15λ 0,d (3)
[0056] Returning to FIG. 8, solid curve 820 is the admittance of an XBAR with a 375 nm SiO2 layer on a 400 nm lithium niobate piezoelectric plate. Dashed curve 830 is the admittance of an XBAR with a 475 nm SiO2 layer on a 400 nm lithium niobate piezoelectric plate. A filter such as filter 1200 can be fabricated using a 400 nm lithium niobate piezoelectric plate with a 375 nm SiO2 layer on the series resonator and a 475 nm SiO2 layer on the shunt resonator. In this case, the frequency separation between the resonant frequency of the shunt resonator and the anti-resonant frequency of the series resonator is about 800 MHz, which is sufficient for a bandpass filter in band n79. The frequency separation increases in proportion to the thickness of the piezoelectric plate.
[0057] The thickness range of the SiO2 layer covering the series resonator and the shunt resonator can be expressed as follows in terms of the thickness ts of the lithium niobate piezoelectric plate: 0.875ts≦tds <tdp≦1.25ts (4) tds is the thickness of the SiO2 layer on the series resonator, and tdp is the thickness of the SiO2 layer on the shunt (parallel) resonator.
[0058] Show me how FIG. 13 is a simplified flow chart illustrating a method 1300 for fabricating an XBAR including a partial Bragg reflector, or a filter incorporating such an XBAR. The method 1300 begins at 1305 with a thin piezoelectric plate disposed on a sacrificial substrate 1302 and a device substrate 1304. The method 1300 ends at 1395 with a completed XBAR or filter. Only major process steps are included in the flow chart of FIG. 13. Various conventional process steps (e.g., surface preparation, cleaning, inspection, baking, annealing, monitoring, testing, etc.) may be performed before, between, after, and during the steps illustrated in FIG. 13.
[0059] 13 shows three variations of a method 1300 for manufacturing XBARs that differ in when and how the cavities are formed in the substrate. The cavities may be formed in steps 1310A, 1310B, or 1310C. Only one of these steps is performed in each of the three variations of method 1300.
[0060] Thin plates of single crystal piezoelectric material bonded to a non-piezoelectric substrate are commercially available. At the time of this application, both lithium niobate and lithium tantalate plates bonded to a variety of substrates, such as silicon, quartz, and fused silica, are available. Thin plates of other piezoelectric materials may be used now or in the future. The thickness of the piezoelectric plate may be between 300 nm and 1000 nm. Examples of piezoelectric plates include Z-cut, rotated Z-cut, and rotated Y-cut lithium niobate and lithium tantalate. The piezoelectric plate may be of other materials and cuts. The substrate may be silicon. If the substrate is silicon, a SiO2 layer may be disposed between the piezoelectric plate and the substrate. The substrate may be of other materials that can be etched or otherwise processed to form deep cavities.
[0061] In one variation of method 1300, one or more cavities are formed in the substrate at 1310A before the piezoelectric plate is bonded to the substrate at 1330. Other cavities may be formed for each resonator in the filter device. The one or more cavities may be formed using conventional photolithography and etching techniques. For example, the cavities may be formed using deep reactive ion etching (DRIE). Typically, the cavities formed at 1310A do not extend all the way through the substrate.
[0062] At 1330, the piezoelectric plate of the sacrificial substrate 1302 and the device substrate 1304 may be bonded. The piezoelectric plate of the sacrificial substrate 1302 and the device substrate 1304 may be bonded using a wafer bonding process such as direct bonding, surface or plasma activated bonding, electrostatic bonding, or some other bonding technique. The device substrate may be coated with a bonding layer such as SiO2 prior to the wafer bonding process.
[0063] After the piezoelectric plate of the sacrificial substrate 1302 and the device substrate 1304 are bonded, the sacrificial substrate and any intervening layers are removed at 1340 to expose the face of the piezoelectric plate (the face that previously faced the sacrificial substrate). The sacrificial substrate can be removed, for example, by a wet etch, a dry etch, or other process depending on the material. The exposed face of the piezoelectric plate may be polished or otherwise processed at 1340 to prepare the face and control the thickness of the piezoelectric plate.
[0064] Conductive patterns and dielectric layers defining one or more XBAR devices are formed at 1350. Typically, a filter device will have two or more conductive layers that are deposited and patterned in sequence. The conductive layers include bond pads, gold, or solder bumps, or other means for connecting the device to external circuitry. The conductive layers may be, for example, aluminum, aluminum alloys, copper, copper alloys, molybdenum, tungsten, beryllium, gold, or other conductive metals. Optionally, one or more layers of other materials may be disposed below (i.e., between) and / or above the conductive layers. For example, thin films of titanium, chromium, or other metals may be used to improve adhesion between the conductive layers and the piezoelectric plates. The conductive layers include bond pads, gold bumps, solder bumps, or other means for connecting the device to external circuitry.
[0065] The conductor pattern may be formed at 1350 by depositing a conductor layer on the face of the piezoelectric plate and removing excess metal by etching through a patterned photoresist. Alternatively, the conductor pattern may be formed at 1350 using a lift-off process. Photoresist may be deposited on the piezoelectric plate and patterned to define the conductor pattern. A conductor layer may be deposited in turn on the face of the piezoelectric plate. The photoresist may then be removed to remove excess material, leaving the conductor pattern.
[0066] At 1360, a half-lambda dielectric layer may be formed on the front side of the piezoelectric layer. The half-lambda dielectric layer may be deposited on the conductor pattern or may be formed only between the IDT fingers. In some filter devices, the first dielectric layer may be deposited on / between all the IDT fingers and the second dielectric may be selectively formed on only portions of the IDTs, e.g., only the IDTs of the shunt resonators. The first dielectric layer is thicker than the second dielectric layer. The first and second dielectric layers may be the same or different materials. Either the first or second dielectric layer may be deposited first.
[0067] In a second variation of process 1300, after all of the conductor patterns and dielectric layers have been formed in 1350 and 1360, one or more cavities are formed in the backside of the substrate in 1310B. A separate cavity may be formed for each resonator in the filter device. The one or more cavities may be formed by drilling holes through the backside of the substrate to the piezoelectric plate using anisotropic or orientation dependent dry or wet etching.
[0068] In a third variation of process 1300, one or more cavities in the form of recesses may be formed in the substrate in 1310C by etching the substrate with an etchant introduced through openings in the piezoelectric plate and the half-lambda dielectric layer. A separate cavity may be formed for each resonator in the filter device. The cavity or cavities formed in 1310C do not extend all the way through the substrate.
[0069] In all variations of process 1300, the filter device is completed at 1370. Operations that may occur at 1370 include depositing an encapsulation / passivation layer, such as SiO2 or SiO4, over all or a portion of the device, and / or forming bond pads or solder bumps, or other means for making connections between the device and external circuitry, if these steps were not performed at 1350. Other operations at 1370 include removing individual devices from a wafer containing multiple devices, other packaging steps, and testing. Other operations that may occur at 1370 are tuning the resonant frequency of resonators in the device by adding or removing metal or dielectric material on the front side of the device. Once the filter device is completed, the process ends at 1395.
[0070] A variation of process 1300 starts at 1302 with a single crystal piezoelectric wafer instead of a thin piezoelectric plate on a sacrificial substrate of a different material. Ions are implanted (not shown in FIG. 13) to a controlled depth below the surface of the piezoelectric wafer. The portion of the wafer from the surface to the depth of the ion implantation is (or becomes) the thin piezoelectric plate, and the remaining portion of the wafer is the sacrificial substrate. The piezoelectric wafer and device substrate are bonded at 1330 as previously described. At 1340, the piezoelectric wafer may be split (e.g., using thermal shock) at the ion implanted surface, exposing a thin plate of piezoelectric material and leaving it bonded to an acoustic Bragg reflector. The thickness of the thin plate of piezoelectric material is determined by the energy (i.e., depth) of the implanted ions. The process of ion implantation followed by separation of the thin plate is commonly referred to as "ion slicing." After splitting the piezoelectric wafer, the exposed surface of the piezoelectric plate may be planarized and reduced in thickness, for example, by chemical-mechanical polishing.
[0071] Concluding remarks Throughout this specification, the illustrated embodiments and examples should be considered as illustrations, rather than limitations of the disclosed or claimed apparatus and procedures. While many of the examples presented herein include specific combinations of method acts or system configurations, it should be understood that those acts and those configurations can be combined in other ways to accomplish the same purpose. With respect to flow charts, additional or fewer steps may be taken, and illustrated steps may be combined or further refined to achieve the methods described herein. Acts, configurations, and features discussed only in relation to one embodiment are not intended to exclude a similar role in other embodiments.
[0072] As used herein, "plurality" means two or more. As used herein, a "set" of an item can include one or more of such items. As used herein, whether in the detailed description or the claims, terms such as "comprising," "including," "carrying," "having," "containing," "involving," and the like, are to be understood without restriction, i.e., meaning including but not limited to. With respect to the claims, only the transitional phrases "consisting of" and "consisting only of" are closed or semi-closed transitional phrases. The use of ordinal numbers such as "first," "second," "third," and the like to modify claim features in the claims does not, in itself, imply a priority, precedence, or chronological order in which the actions of a method are performed of a claim feature relative to others, but is merely used as a marker to distinguish a claim feature having a certain name from other features having the same name (but where an ordinal number is used). As used herein, "and / or" means that the listed items are alternatives, but the alternatives also include any combination of the listed items.
Claims
1. A substrate; a piezoelectric plate attached to the substrate directly or via at least one intermediate layer of material, a portion of the piezoelectric plate forming a diaphragm above the cavity; an interdigital transducer (IDT) formed on the piezoelectric plate, the interleaved fingers of the IDT being positioned on the diaphragm; a dielectric layer formed on the piezoelectric plate; The thickness ts of the piezoelectric plate and the thickness td of the dielectric layer are defined as follows: 2ts=λ0,s 0.88 minutes 0,d ≦2td≦1.12l 0,d λ 0,s is the wavelength of the fundamental shear bulk acoustic wave (BAW) resonance in the piezoelectric plate; λ 0,d is the wavelength of the fundamental shear BAW resonance in the dielectric layer.
2. The dielectric layer is made of SiO 2 , Si 3 N 4 , Al 2 O 3 2. The acoustic resonator device of claim 1, wherein the material is one or more of: GaN;
3. the piezoelectric plate is lithium niobate; The dielectric layer is made of SiO 2 2. The acoustic resonator device according to claim 1 .
4. 4. The acoustic resonator according to claim 3, wherein the temperature coefficient of frequency of the acoustic resonator is −32 ppm / ° C. to −42 ppm / ° C. at the resonant frequency and −20 ppm / ° C. to −36 ppm / ° C. at the anti-resonant frequency.
5. A substrate; a piezoelectric plate having a thickness ts and attached to the substrate directly or via at least one intermediate layer of material; a conductor pattern formed on the piezoelectric plate, the conductor pattern including a plurality of interdigital transducers (IDTs) of respective resonators including shunt resonators and series resonators, interleaved fingers of each of the plurality of IDTs being disposed in a respective portion of the piezoelectric plate above one or more cavities; a first dielectric layer disposed between the fingers of the series resonator and having a thickness tds; a second dielectric layer disposed between the fingers of the shunt resonator and having a thickness tdp; ts, tds, and tdp are 2ts=λ 0,s and 0.88 minutes 0,d ≦2tdfs<2tdfp≦1.12l 0,d It is expressed by the formula, λ 0,s is the wavelength of the fundamental shear bulk acoustic wave (BAW) resonance in the piezoelectric plate, λ 0,d is the wavelength of the shear BAW fundamental resonance in the dielectric layer of the filter device.
6. 1. A method of manufacturing an acoustic resonator device in a piezoelectric plate that is attached to a substrate, either directly or through one or more intermediate layers of material, comprising the steps of: forming a cavity in the substrate such that a portion of the piezoelectric plate forms a diaphragm above the cavity; forming an interdigital transducer (IDT) on the piezoelectric plate, the interleaved fingers of the IDT being disposed on the diaphragm; forming a dielectric layer on the piezoelectric plate; The thickness ts of the piezoelectric plate and the thickness td of the dielectric layer are defined as follows: 2ts=λ0,s 0.88 minutes 0,d ≦2td≦1.12l 0,d λ 0,s is the wavelength of the fundamental shear bulk acoustic wave (BAW) resonance in the piezoelectric plate; λ 0,d is the wavelength of the fundamental shear BAW resonance in the dielectric layer.
7. Forming the dielectric layer includes SiO 2 , Si 3 N 4 , Al 2 O 3 The method of claim 6 , further comprising depositing one or more of: SiO 2 ; and AlN.
8. the piezoelectric plate is lithium niobate; Forming the dielectric layer includes forming a SiO 2 7. A method for manufacturing an acoustic resonator device as claimed in claim 6, comprising depositing
Citation Information
Patent Citations
Elastic surface wave apparatus
JP1978062964A
Filter and demultiplexer
JP2008079227A
Elastic wave device and electronic component
JP2010233210A
Surface acoustic wave device
JP2012169760A
Broadband acoustically coupled thin-film BAW filter
JP2013528996A