Film and manufacturing method thereof, roll body and manufacturing method thereof

The film design with controlled convex area ratios and resin viscosity adjustments addresses winding misalignment and sticking issues, maintaining film stability and optical properties.

JP7556386B2Active Publication Date: 2024-09-26KONICA MINOLTA INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022530000
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-12
Publication Date
2024-09-26
Estimated Expiration
2040-06-12

AI Technical Summary

Technical Problem

Existing optical films wound into rolls experience misalignment and sticking due to uneven air release during winding, leading to deterioration of optical properties.

Method used

A film design with band-shaped protrusions at both ends, where the ratio of the upper and lower convex areas (S1/S2) is controlled between 0.6 and 0.95, and the viscosity ratio of the resin compositions is adjusted to 0.00003 to 0.02, allowing controlled air retention and release.

Benefits of technology

The solution effectively suppresses winding misalignment and sticking while maintaining appropriate air retention, ensuring stable film rolls with minimal deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556386000011
    Figure 0007556386000011
  • Figure 0007556386000014
    Figure 0007556386000014
  • Figure 0007556386000013
    Figure 0007556386000013
Patent Text Reader

Abstract

The film of the present invention has belt-like convex parts at both end parts in the width direction. When the maximum height of the convex part is denoted by Tmax and when the area of the convex part located above the midpoint (Tmax / 2) of the convex part with respect to the maximum height Tmax of the convex part is denoted by S1, and the area of the convex part below said midpoint is denoted by S2, S1 and S2 satisfy formula (1) below. Formula (1): 0.6 ≤ S1 / S2 ≤ 0.95
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film and a method for producing the same, and a roll body and a method for producing the same. [Background technology]

[0002] 2. Description of the Related Art Resin films containing cycloolefin resins, (meth)acrylic resins, or the like as their main components have good transparency and dimensional stability, and are therefore used as optical films such as polarizing plate protective films.

[0003] From the viewpoints of ease of handling and production efficiency, such optical films are usually stored or transported in the form of a roll obtained by winding up a strip-shaped film into a roll.

[0004] In such a roll body, in order to prevent quality defects caused by films sticking to each other during storage or transportation, a process called embossing is usually performed on both ends in the width direction of the film to create projections and recesses (see, for example, Patent Document 1). However, the embossed portions formed by embossing are easily crushed, and it has sometimes been impossible to sufficiently prevent films from sticking to each other.

[0005] In response to this, a method is also known in which convex portions (knurling portions) are formed on both widthwise ends of a film by coating (see, for example, Patent Document 2). The knurling portions formed by coating are stronger and less prone to crushing than embossed portions, and are therefore considered to be able to effectively prevent films from sticking to each other. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2012-118238 A [Patent Document 2] JP 2012-206312 A Summary of the Invention [Problem to be solved by the invention]

[0007] In Patent Document 2, the shape of the knurling portion 2 (protrusion) in a cross section along the width direction of the film 1 is rectangular (see FIG. 6). When wound into a roll, the surface of such a knurling portion adheres closely to the back surface of the overlapping film without any gaps, so that air can be reliably trapped between the films when wound.

[0008] However, if an external impact is applied while the film is being wound, the air stored between the films is released all at once, which can easily cause winding misalignment (roll deformation) or film sticking. When such winding misalignment or film sticking occurs, the optical properties are likely to deteriorate, especially in optical films. Therefore, when the film is wound, it is desirable to allow an appropriate amount of air to escape while still retaining an appropriate amount of air between the film.

[0009] The present invention has been made in consideration of the above circumstances, and aims to provide a film and a manufacturing method thereof, and a roll body and a manufacturing method thereof, which are capable of preventing misalignment or sticking when an external impact is applied, while allowing an appropriate amount of air to be contained between the film portions. [Means for solving the problem]

[0010] The above problem can be solved by the following configuration.

[0011] The film of the present invention is a film having band-shaped convex portions at both ends in the width direction, and when the maximum height of the convex portions is Tmax, the region of the convex portions above the midpoint (Tmax / 2) of the maximum height Tmax of the convex portions is S1, and the region of the convex portions below the midpoint is S2, S1 and S2 satisfy the following formula (1): Formula (1): 0.6≦S1 / S2≦0.95

[0012] The method for producing a film of the present invention is a method for producing a film having band-shaped convex portions at both widthwise ends, and includes the steps of 1) casting a first resin composition to obtain a band-shaped film base, and 2) casting a second resin composition onto both widthwise ends of the surface of the band-shaped film base to form the band-shaped convex portions, wherein the ratio η2 / η1 of the viscosity η2 of the second resin composition during casting in step 2) to the viscosity η1 of the first resin composition during casting in step 1) is 0.00003 to 0.02.

[0013] The roll body of the present invention is a roll body formed by winding up a band-shaped film having band-shaped convex portions at both ends in the width direction, wherein when the maximum height of the convex portions is Tmax, a convex portion region S1 above a convex portion midpoint (Tmax / 2) relative to the maximum height Tmax of the convex portions and a convex portion region S2 below the midpoint are the roll body characterized in that S1 and S2 satisfy the following formula (1): Formula (1): 0.6≦S1 / S2≦0.95

[0014] The method for producing a roll body of the present invention is a method for producing a roll body by winding up a strip-shaped film having strip-shaped convex portions at both widthwise ends, and includes the steps of 1) casting a first resin composition to obtain a strip-shaped film base, and 2) casting a second resin composition onto both widthwise ends of the surface of the strip-shaped film base to form the strip-shaped convex portions, wherein a ratio η2 / η1 of a viscosity η2 of the second resin composition during casting in step 2) to a viscosity η1 of the first resin composition during casting in step 1) is 0.00003 to 0.02. Effect of the Invention

[0015] According to the present invention, it is possible to provide a roll of film that can contain an appropriate amount of air between the film portions and can suppress misalignment or sticking when an external impact is applied, and a method for manufacturing the same. [Brief description of the drawings]

[0016] [Figure 1]FIG. 1A is a plan view of a band-shaped film in the present embodiment, and FIG. 1B is a cross-sectional view taken along line 1B-1B of FIG. 1A. [Diagram 2] FIG. 2 is an enlarged view of the protrusion in FIG. 1B. [Diagram 3] FIG. 3A is a plan view of a band-shaped film in another embodiment, and FIG. 3B is a cross-sectional view taken along line 3B-3B in FIG. 3A. [Figure 4] FIG. 4A is a plan view of a band-shaped film in another embodiment, and FIG. 4B is a cross-sectional view taken along line 4B-4B in FIG. 4A. [Diagram 5] 5A to 5C are cross-sectional views showing the shape of a convex portion according to another embodiment. [Figure 6] FIG. 6 is a cross-sectional view of a conventional strip-shaped film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The inventors have discovered that by ensuring that an appropriate gap is formed between the convex portions and the back surface of the film base when the strip-shaped film is wound into a roll; specifically, by adjusting the ratio S1 / S2 of the area S1 of the upper half of the convex portion to the area S2 of the lower half of the convex portion in the width-wise cross section of the film to be 0.95 or less, it is possible to suppress misalignment and sticking when the strip-shaped film is wound into a roll.

[0018] In this way, by forming an appropriate gap between the convex portion and the back surface of the film base, it is possible to trap an appropriate amount of air between the film folds while winding the film while releasing the appropriate amount of air. As a result, the air that has accumulated between the film folds during winding is not released all at once, which is thought to suppress winding misalignment and deformation.

[0019] S1 / S2 can be adjusted by any method, for example, by the viscosity or resin concentration of the resin composition for forming the convex portions, the drying rate (or solidification rate) of the resin composition, surface treatment of the film base, etc. For example, from the viewpoint of making S1 / S2 0.95 or less, it is preferable to reduce the contact angle of the resin composition for forming the convex portions with the film base; for this purpose, it is preferable to reduce the viscosity or resin concentration of the resin composition, or increase the drying rate (or solidification rate) of the resin composition.

[0020] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.

[0021] The film of the present invention may be a strip-shaped film or a sheet-shaped film cut out from a strip-shaped film. First, an example in which the film is a strip-shaped film (a roll of strip-shaped film) will be described.

[0022] 1. Film roll The roll body of the present invention is a strip-shaped film wound into a roll in a direction perpendicular to the width direction of the film.

[0023] Fig. 1A is a plan view of a band-shaped film in this embodiment, and Fig. 1B is a cross-sectional view taken along line 1B-1B in Fig. 1A. Fig. 2 is an enlarged view of protrusion 12 in Fig. 1B. Note that hatching of the cross section is omitted in Fig. 1B for ease of viewing.

[0024] 1A and 1B, a strip-shaped film 10 has strip-shaped convex portions 12 at both ends in the width direction. In the present embodiment, the strip-shaped film 10 has a film base 11 and convex portions 12 provided at both ends in the width direction.

[0025] 1-1.Film base 11 The film base 11 is preferably a resin film, and more preferably a resin film that can be used as an optical film.

[0026] (resin) The resin contained in the film base 11 (resin film) is preferably a thermoplastic resin. The thermoplastic resin may be any suitable resin for an optical film, and is not particularly limited, but examples thereof include cycloolefin resin, (meth)acrylic resin, polyimide, cellulose ester, polyester, polycarbonate, and the like. Among them, from the viewpoint of having good transparency, cycloolefin resin, (meth)acrylic resin, and cellulose ester are preferred, and from the viewpoint of further having low moisture absorption (high dimensional stability), cycloolefin resin and (meth)acrylic resin are more preferred.

[0027] (Cycloolefin resin) The cycloolefin resin is preferably a polymer containing a structural unit derived from a norbornene monomer. The norbornene monomer is not particularly limited as long as it is a compound having a norbornene skeleton, but when the film is formed by a solution casting method, it is preferably a norbornene monomer having a polar group.

[0028] The norbornene monomer having a polar group is preferably represented by formula (1).

[0029] [ka]

[0030] In formula (1), R 1 ~R 4 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 30 carbon atoms, or a polar group. 1 ~R 4 At least one of the groups is a polar group.

[0031] The polar group refers to a functional group in which polarization occurs due to atoms with high electronegativity such as oxygen atoms, sulfur atoms, and nitrogen atoms. Examples of such polar groups include carboxy groups, hydroxy groups, alkoxycarbonyl groups, aryloxycarbonyl groups, amino groups, amide groups, cyano groups, and groups in which these groups are bonded via a linking group such as an alkylene group. Among these, carboxy groups, hydroxy groups, alkoxycarbonyl groups, and aryloxycarbonyl groups are preferred, and alkoxycarbonyl groups and aryloxycarbonyl groups are more preferred from the viewpoint of ensuring solubility during solution casting.

[0032] From the viewpoint of making it easier to localize polar groups on the film surface, R 1 and R 2 is a hydrogen atom, and R 3 and R 4 is preferably a group other than a hydrogen atom.

[0033] p represents an integer of 0 to 2.

[0034] Examples of monomers represented by formula (1) include the following: [ka]

[0035] The content of the structural unit derived from the norbornene-based monomer having a polar group can be 50 to 100% by mass based on the total structural units constituting the cycloolefin resin.

[0036] The cycloolefin resin having a polar group may further contain a structural unit derived from a copolymerizable monomer copolymerizable with the norbornene monomer having a polar group, as necessary.

[0037] Examples of the copolymerizable monomer include norbornene monomers having no polar group and monomers having no norbornene skeleton. Examples of the monomer having no norbornene skeleton include copolymerizable monomers capable of ring-opening copolymerization (with norbornene monomers having a polar group) and copolymerizable monomers capable of addition copolymerization (with norbornene monomers having a polar group).

[0038] Examples of the copolymerizable monomer capable of ring-opening copolymerization include cycloolefins having no norbornene skeleton, such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, and dicyclopentadiene.

[0039] Examples of copolymerizable monomers capable of addition copolymerization include unsaturated double bond-containing compounds, vinyl cyclic hydrocarbon monomers, and (meth)acrylic acid esters. Examples of unsaturated double bond-containing compounds are olefin compounds having 2 to 8 carbon atoms, examples of which include ethylene, propylene, and butene. Examples of vinyl cyclic hydrocarbon monomers include vinylcyclopentene monomers such as 4-vinylcyclopentene and 2-methyl-4-isopropenylcyclopentene. Examples of (meth)acrylic acid esters include (meth)acrylic acid alkyl esters having 1 to 20 carbon atoms, such as methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate.

[0040] The weight average molecular weight (Mw) of the cycloolefin resin is preferably 20,000 to 300,000. When the Mw of the cycloolefin resin is within the above range, the film formability is not easily impaired while providing sufficient mechanical strength to the film. From the above viewpoint, the Mw of the cycloolefin resin is more preferably 40,000 to 200,000.

[0041] The Mw of the cycloolefin resin can be measured in terms of polystyrene by gel permeation chromatography (GPC). Specifically, it can be measured using a Tosoh Corporation HLC8220GPC and a column (Tosoh Corporation TSK-GEL G6000HXL-G5000HXL-G5000HXL-G4000HXL-G3000HXL in series).

[0042] The glass transition temperature (Tg) of the cycloolefin resin is usually 110° C. or higher, preferably 110 to 350° C., more preferably 120 to 250° C., and particularly preferably 120 to 220° C. If the cycloolefin resin has a Tg of 110° C. or higher, deformation due to use under high temperature conditions or secondary processing such as coating or printing is suppressed, which is preferable. In addition, if the Tg is 350° C. or lower, deterioration of the resin due to molding processing or heat during molding processing is suppressed, which is preferable.

[0043] The Tg of the cycloolefin resin can be measured using DSC (Differential Scanning Colorimetry) in accordance with JIS K 7121-2012 or ASTM D 3418-82.

[0044] ((Meth)acrylic resin) The (meth)acrylic resin is a homopolymer of a (meth)acrylic acid ester or a copolymer of a (meth)acrylic acid ester and a copolymerizable monomer copolymerizable therewith. The (meth)acrylic acid ester is preferably methyl methacrylate.

[0045] The copolymerizable monomer may be any monomer capable of copolymerizing with methyl methacrylate, and may be a copolymerizable monomer having a ring structure or a copolymerizable monomer not having a ring structure.

[0046] Examples of copolymerizable monomers having a ring structure include: (meth)acrylic acid esters having an alicyclic ring, such as dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, cyclohexyl (meth)acrylate, and six-membered ring lactone (meth)acrylic acid esters; vinyl compounds having an alicyclic ring such as vinylcyclohexane; Vinyls having aromatic rings, such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, and α-methylstyrene; and These include maleimides (compounds having an imide ring) such as N-phenylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-cyclohexylmaleimide, and No-chlorophenylmaleimide.

[0047] Examples of copolymerizable monomers having no ring structure include: (meth)acrylic acid alkyl esters having 2 to 20 carbon atoms, such as ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-octyl (meth)acrylate; Unsaturated nitriles such as (meth)acrylonitrile; Unsaturated carboxylic acids such as (meth)acrylic acid, crotonic acid, and (meth)acrylic acid; Vinyl acetate, olefins such as ethylene and propylene; Vinyl halides such as vinyl chloride, vinylidene chloride, and vinylidene fluoride; (Meth)acrylamides such as (meth)acrylamide, methyl(meth)acrylamide, ethyl(meth)acrylamide, and propyl(meth)acrylamide are included.

[0048] The copolymerizable monomer may be of one type or of a combination of two or more types.

[0049] The Mw of the (meth)acrylic resin is preferably 400,000 to 3,000,000. When the Mw is within the above range, the film is provided with sufficient mechanical strength (toughness), while the film-forming property and drying property are not easily impaired. From the above viewpoints, the Mw of the (meth)acrylic resin is more preferably 500,000 to 2,000,000. The Mw of the (meth)acrylic resin can be measured by the same method as described above.

[0050] The Tg of the (meth)acrylic resin is preferably 90° C. or higher. When the Tg is 90° C. or higher, not only can the heat resistance of the film be increased, but also the drying property during film formation is easily increased. From the viewpoint of preventing the toughness of the film from being impaired, the Tg of the (meth)acrylic resin is more preferably 100 to 150° C. The Tg of the (meth)acrylic resin can be measured by the same method as described above.

[0051] (Cellulose ester) Cellulose ester is a compound in which cellulose is esterified with a carboxylic acid.

[0052] The total substitution degree of the acyl group of the cellulose ester is preferably 2 to 3, more preferably 2.2 to 2.6. The acyl group can be an acetyl group, a propionyl group, or both. The substitution degree of the acyl group of the cellulose ester can be measured by the method specified in ASTM-D817-96.

[0053] Examples of the cellulose ester include cellulose triacetate and cellulose acetate propionate.

[0054] In order to obtain a certain level of mechanical strength, the Mw of the cellulose ester is preferably from 100,000 to 500,000, and more preferably from 150,000 to 300,000. The Mw can be measured by the same method as described above.

[0055] The Tg of the cellulose ester is usually preferably from 140 to 200° C., and more preferably from 160 to 190° C. The Tg can be measured by the same method as described above.

[0056] The resin content is preferably 60% by mass or more relative to the film base 11, and can be 70 to 100% by mass.

[0057] (fine particles) The film base 11 may further contain fine particles (matting agent) as necessary, which can impart appropriate slipperiness to the surface of the resin film.

[0058] The fine particles may be inorganic fine particles or organic fine particles.

[0059] Examples of inorganic fine particles include silica particles. The average primary particle size of the silica particles is not particularly limited, but is preferably, for example, 5 to 100 nm, and more preferably 10 to 50 nm.

[0060] An example of the organic fine particles is preferably polymer fine particles having a refractive index difference with the resin of 0.01 or less. From the viewpoint of high affinity with the resin and easy adjustment of the refractive index to the above range, an example of such organic fine particles is preferably a copolymer containing a structural unit selected from the group consisting of (meth)acrylic acid esters, vinyl esters, styrenes, and olefins, more preferably a copolymer containing a structural unit derived from a (meth)acrylic acid ester and a styrene, and even more preferably a copolymer containing a structural unit derived from a (meth)acrylic acid ester, a structural unit derived from a styrene, and a structural unit derived from a polyfunctional monomer.

[0061] The glass transition temperature (Tg) of the organic fine particles is preferably not less than 80° C. The glass transition temperature (Tg) of the organic fine particles can be measured in accordance with JISK 7121-2012 or ASTM D3418-82, as described above.

[0062] The average particle size of the organic fine particles is 0.01 to 0.4 μm. If the average particle size of the organic fine particles is 0.01 μm or more, it is possible to form unevenness of appropriate size on the surface of the obtained film, making it easy to impart slipperiness, and if it is 0.4 μm or less, it is easy to suppress an increase in the internal haze of the film. From the above viewpoint, the average particle size of the organic fine particles is more preferably 0.07 to 0.28 μm.

[0063] The average primary particle size of inorganic fine particles or organic fine particles can be measured by the following procedure. 1) A cross section parallel to the in-plane slow axis of the film is observed by TEM in the same area as described above. 2) The primary particle diameters of any 10 inorganic or organic fine particles in the obtained TEM image are measured, and the average value thereof is regarded as the "average primary particle diameter."

[0064] [Physical Properties] The thickness of the film base 11 is constant. That is, the film base 11 is not embossed, and therefore does not have a thin portion formed by being crushed with an embossing roller. The thickness of the film base 11 is not particularly limited, but is preferably 3 to 40 μm, more preferably 5 to 30 μm, and further preferably 10 to 20 μm.

[0065] The length (wound length) of the film base 11 is not particularly limited, but is preferably 2000 to 15000 m, and more preferably 3000 to 12000 m. The width of the film base 11 is not particularly limited, but is preferably 950 to 3000 mm.

[0066] (Phase difference Ro and Rt) It is preferable that the film base 11 has a retardation according to the required optical properties. For example, from the viewpoint of using the protective film as a retardation film for an IPS mode, it is preferable that the retardation Ro in the in-plane direction and the retardation Rt in the thickness direction, which are measured at a wavelength of 550 nm and at 23° C. and 55% RH, respectively, satisfy the following formulas. |Ro|≦10nm |Rt|≦10nm

[0067] Ro and Rt are defined by the following formulas, respectively. Formula (I): Ro = (nx - ny) x d Formula (II): Rt = ((nx + ny) / 2 - nz) × d (In the formula, nx represents the refractive index in the in-plane slow axis direction (the direction in which the refractive index is maximum) of the film base 11, ny represents the refractive index in a direction perpendicular to the in-plane slow axis of the film base 11, nz represents the refractive index in the thickness direction of the film base 11, d represents the thickness (nm) of the film base 11.

[0068] The in-plane slow axis of the film base 11 can be confirmed by an automatic birefringence meter Axoscan (AxoScan Mueller Matrix Polarimeter, manufactured by Axometrics).

[0069] Ro and Rt can be measured in the following manner. 1) The film base 11 is conditioned for 24 hours in an environment of 23° C. and 55% RH. The average refractive index of this film base 11 is measured with an Abbe refractometer, and the thickness d is measured with a commercially available micrometer. 2) The retardations Ro and Rt of the film base 11 after humidity conditioning at a measurement wavelength of 550 nm are measured in an environment of 23° C. and 55% RH using an automatic birefringence meter Axoscan (AxoScan Mueller Matrix Polarimeter, manufactured by Axometrics).

[0070] (Internal Haze) The internal haze of the film base 11 is preferably 1.0% or less, more preferably 0.1% or less, and even more preferably 0.05% or less. The internal haze of the film base 11 can be measured in accordance with JIS K-6714 using a haze meter (HGM-2DP, Suga Test Instruments) at 25°C and 60% RH for a sample of 40 mm x 80 mm.

[0071] 1-2. Convex part 12 The protrusions 12 are knurled portions obtained by applying a resin composition to both widthwise ends of the surface of the film base 11 .

[0072] The protrusions 12 are arranged in a band shape along the longitudinal direction of the film base 11 at both ends in the width direction of the film base 11 (see FIG. 1A). The term "band shape" is not limited to a continuously extending shape, but also includes an intermittently extending shape. That is, the protrusions 12 may be arranged in a band shape continuously, or may be arranged in a band shape intermittently. In this embodiment, the protrusions 12 are arranged in a continuous shape (see FIG. 1A). The protrusions 12 may be integral with the film base 11, or may be separate.

[0073] In a cross section along the width direction of film 10 (cross section perpendicular to the extension direction of protrusions 12), when the maximum height of protrusions 12 is Tmax, the area of ​​the region of protrusions 12 that is farther from film base 11 than the height of Tmax / 2 (region above the midpoint Tmax / 2 of protrusions 12) is S1 (upper part of FIG. 2), and the area of ​​the region closer to film base 11 than the height of Tmax / 2 (region below the midpoint of protrusions 12) is S2 (lower part of FIG. 2), S1 is smaller than S2. Specifically, it is preferable that S1 and S2 satisfy the following formula (1). Formula (1): 0.6≦S1 / S2≦0.95

[0074] When S1 / S2 is 0.6 or more, the contact area between the convex portion 12 and the back surface of the film base 11 can be secured, and air can be appropriately stored between the overlapping film bases 11. When S1 / S2 is 0.95 or less, the convex portion 12 and the back surface of the film base 11 do not adhere too closely to each other, and an appropriate gap can be formed. As a result, when the film is wound up, air can be appropriately released while being contained between the overlapping film bases 11. As a result, it is possible to prevent excessive air from being contained between the overlapping film bases 11, and therefore, when an impact or the like is applied from the outside, the air accumulated between the film bases 11 is suddenly released, and the occurrence of winding misalignment or sticking can be prevented. From the same viewpoint, it is more preferable to satisfy 0.7≦S1 / S2≦0.9.

[0075] The height of the protrusions 12 refers to the height from the surface of the film base 11 (the height in the normal direction to the surface of the film base 11).

[0076] The sum of the areas S1 and S2 of the protrusions 12 is 0.0006 to 0.07 mm 2 It is preferable that the thickness is 0.0013 to 0.03 mm. 2 It is more preferable that the sum of the areas S1 and S2 of the protrusions 12 is equal to or greater than the lower limit, the winding is likely to shift, and if it is equal to or less than the upper limit, the winding is likely to contain excessive air. When the protrusions 12 are formed intermittently, the sum of S1 and S2 is calculated by measuring the sum of S1 and S2 for each of the multiple protrusions 12 and averaging them.

[0077] The areas S1 and S2 of the protrusions 12, the maximum height Tmax, and the maximum width Wmax of the protrusions in a cross section along the width direction of the film 10 can be measured using a laser microscope. As the laser microscope, for example, a laser microscope VK-X1000 manufactured by Keyence Corporation can be used. Specifically, the areas S1 and S2 of the protrusions 12 are measured by measuring the areas of the upper and lower halves of the protrusions 12 with a laser microscope in an area of ​​100 mm in the length direction of the film and 15 mm in the width direction of the film centered on one row of protrusions, and the average values ​​thereof can be calculated as the "areas S1 and S2 of the protrusions 12." When there are multiple rows (lines) of protrusions 12, the value is for one row (line) of protrusions 12. When applying with a dispenser or intermittently applying, the value is the average value of the measured values ​​for the multiple protrusions 12 present in the above region.

[0078] The ratio (%) of the total area (S1+S2) of the convex portions to the area of ​​the film base in the cross section of the optical film in the width direction is not particularly limited, but is preferably 0.005 to 0.06%, and more preferably 0.01 to 0.04%. When there are multiple convex portions in the cross section of the optical film in the width direction, the ratio refers to the ratio of the total area of ​​those convex portions to the area of ​​the film base.

[0079] The shape of the convex portion 12 is not particularly limited as long as it is a shape that allows for an appropriate gap to be formed between the convex portion 12 and the back surface of the film base portion 11 when the film 10 is wound up, specifically, a shape in which S1 / S2 satisfies the above range.

[0080] For example, the height of the center of the protrusions 12 (in the width direction of the film base 11) may be higher than the height of both ends of the protrusions 12 (see FIG. 2 and FIG. 5A described below), may be the same as the height of both ends of the protrusions 12 (see FIG. 5B described below), or may be lower than the height of both ends of the protrusions 12 (see FIG. 5C described below). In particular, it is preferable that the height of the center of the protrusions 12 is higher than the height of both ends of the protrusions 12 or is the same as the height of both ends of the protrusions 12. In this embodiment, the height of the center of the protrusions 12 is higher than the height of both ends of the protrusions 12 (see FIG. 2).

[0081] Specifically, in a cross section along the width direction of the film 10, the shape of the protrusions 12 may be either an arch (circular segment) or a polygon. An arch shape is a shape in which both ends of a circular or elliptical arc are connected by a straight line, and examples thereof include a semicircle and a semiellipse. Examples of polygons include a trapezoid (see FIG. 5B described below) and a staircase shape (see FIG. 5A described below).

[0082] The maximum height Tmax of the protrusions 12 is not particularly limited, but is preferably 0.8 to 35%, more preferably 1.0 to 15%, and even more preferably 2.5 to 7.0% of the thickness of the film base 11. Specifically, the maximum height Tmax of the protrusions 12 is preferably 0.3 to 4.0 μm, and more preferably 0.5 to 2.0 μm.

[0083] The maximum width Wmax of the protrusions 12 in the width direction of the film base 11 is not particularly limited, but is preferably 0.05 to 5%, more preferably 0.05 to 3%, and even more preferably 0.05 to 1% of the width of the film base 11. Specifically, the maximum width Wmax of the protrusions 12 is preferably 0.5 to 50 mm, and more preferably 1 to 30 mm.

[0084] The position of the apex of the protrusions 12 in the width direction of the film 10 is not particularly limited, but is preferably within a range of 0.3Wmax to 0.7Wmax from one end of the protrusions 12 in the width direction.

[0085] The protrusions 12 are obtained from a second resin composition described below, and contain a resin.

[0086] The resin contained in the protrusions 12 can be the same as the resin contained in the film base 11. That is, the resin contained in the film base 11 and the resin contained in the protrusions 12 may be the same type or different types. In particular, from the viewpoint of improving the adhesion between the protrusions 12 and the film base 11, it is preferable that the resin contained in the film base 11 and the resin contained in the protrusions 12 are the same type. That is, when the resin contained in the film base 11 is a cycloolefin resin, it is preferable that the resin contained in the protrusions 12 is also a cycloolefin resin.

[0087] The Mw of the resin contained in the protrusions 12 is preferably lower than the Mw of the resin contained in the film base 11. Specifically, the Mw of the cycloolefin resin contained in the protrusions 12 is preferably 10,000 to 50,000. When the Mw of the cycloolefin resin is within the above range, it is difficult to excessively increase the viscosity of the knurling solution, and it is easy to adjust the maximum height Tmax of the protrusions to within the above range. From the above viewpoint, the Mw of the cycloolefin resin is more preferably 20,000 to 40,000. The Mw of the cycloolefin resin can be measured by the same method as described above.

[0088] The resin content is not particularly limited, but is preferably 60% by mass or more, and more preferably 70 to 100% by mass, based on the entire protrusion 12.

[0089] The protrusions 12 may further contain the same components (e.g., fine particles) as the film base 11, if necessary. However, from the viewpoint of preventing slippage between the protrusions 12 and the back surface of the film base 11 when the film 10 is wound up and facilitating appropriate adhesion between them, it is preferable that the content of fine particles in the protrusions 12 is less than the content of fine particles in the film base 11, and it is more preferable that the protrusions 12 do not contain fine particles.

[0090] 2. Manufacturing method of roll body The roll body of the present invention can be obtained through a process of 1) casting a first resin composition onto a support to obtain a strip-shaped film base 11, and 2) casting a second resin composition onto both widthwise ends of the strip-shaped film base 11 to form convex portions.

[0091] 1) Process for obtaining the film base 11 The first resin composition is cast to obtain a strip-shaped film base 11.

[0092] The casting of the first resin composition may be performed by a melt casting method or a solution casting method, among which, from the viewpoint of being able to use a high molecular weight resin, the casting of the first resin composition is preferably performed by a solution casting method.

[0093] That is, the film base 11 can be obtained through the steps of 1A) obtaining a first resin composition (dope), 1B) casting the obtained dope onto a support, drying and peeling it off to obtain a film-like material, and 1C) stretching the obtained film-like material.

[0094] Regarding step 1A A first resin composition is prepared by dissolving a resin in a solvent.

[0095] The solvent used includes at least an organic solvent (good solvent) capable of dissolving the resin. Examples of the good solvent include chlorine-based organic solvents such as dichloromethane; and non-chlorine-based organic solvents such as methyl acetate, ethyl acetate, acetone, and tetrahydrofuran. Among them, methylene chloride is preferable.

[0096] The solvent used may further include a poor solvent. Examples of the poor solvent include linear or branched aliphatic alcohols having 1 to 4 carbon atoms. When the ratio of alcohol in the dope is high, the film-like material is likely to gel and is likely to be easily peeled off from the metal support. Examples of linear or branched aliphatic alcohols having 1 to 4 carbon atoms include methanol, ethanol, n-propanol, iso-propanol, n-butanol, sec-butanol, and tert-butanol. Among them, methanol and ethanol are preferred from the viewpoints of stability and drying property.

[0097] Regarding step 1B Next, the obtained first resin composition is cast onto a support. The first resin composition can be cast by discharging it from a casting die. The temperature of the first resin composition during casting is usually 15 to 30°C, and preferably room temperature (23°C).

[0098] Next, after the solvent in the first resin composition cast onto the support is appropriately evaporated (after drying), the composition is peeled off from the support to obtain a film-like material.

[0099] The amount of the residual solvent in the first resin composition at the time of peeling is, for example, preferably 25% by mass or more, more preferably 30 to 37% by mass, and even more preferably 30 to 35% by mass. When the amount of the residual solvent at the time of peeling is 25% by mass or more, the solvent can be easily evaporated from the film-like material after peeling at once. In addition, when the amount of the residual solvent at the time of peeling is 37% by mass or less, excessive stretching of the film-like material due to peeling can be suppressed.

[0100] The amount of the remaining solvent in the first resin composition at the time of peeling is defined by the following formula: The same applies hereinafter. Residual solvent amount (mass%)=(mass of first resin composition before heat treatment−mass of first resin composition after heat treatment) / mass of first resin composition after heat treatment×100 The heat treatment used in measuring the amount of residual solvent refers to a heat treatment at 140°C for 15 minutes.

[0101] The amount of residual solvent at the time of peeling can be adjusted by the drying temperature and drying time of the first resin composition on the support, the temperature of the support, and the like.

[0102] 1C) Process The obtained film-like material is then dried. The drying may be performed in one step or multiple steps. The drying may be performed while stretching the film, if necessary.

[0103] The stretching may be carried out according to the desired optical properties. It is preferable to stretch in at least one direction, and it may be performed in two mutually perpendicular directions (for example, biaxial stretching in the width direction (TD) of the film and the transport direction (MD) perpendicular thereto).

[0104] The stretching ratio can be 1.01 to 2 times, for example, from the viewpoint of use as a retardation film for IPS. The stretching ratio is defined as (stretching direction size of film after stretching) / (stretching direction size of film before stretching). When performing biaxial stretching, it is preferable to set the above stretching ratios for each of the TD direction and MD direction.

[0105] The in-plane slow axis direction of the film (the direction in which the refractive index is maximum in the plane) is usually the direction in which the stretching ratio is maximum.

[0106] When the glass transition temperature of the resin is Tg, the drying temperature (stretching temperature) during stretching is preferably from (Tg-65)° C. to (Tg+60)° C., and more preferably from (Tg-50)° C. to (Tg+50)° C. When the stretching temperature is at or above a certain level, the solvent is easily volatilized appropriately, making it easy to adjust the stretching tension to an appropriate range, whereas when the temperature is below a certain level, the solvent does not volatilize too much, making it difficult for stretchability to be impaired.

[0107] The stretching temperature can be specified as either (a) the ambient temperature such as the temperature inside the stretching machine or the hot air temperature when drying is performed using a non-contact heating type such as a tenter stretching machine, (b) the temperature of the contact heating part when drying is performed using a contact heating type such as a hot roller, or (c) the surface temperature of the film-like material (surface to be dried).

[0108] The amount of residual solvent in the film at the start of stretching is preferably about the same as the amount of residual solvent in the film at the time of peeling, for example, preferably 20 to 30% by mass, more preferably 25 to 30% by mass.

[0109] The film can be stretched in the TD (width) direction by, for example, fixing both ends of the film with clips or pins and widening the distance between the clips or pins in the traveling direction (tenter method).The film can be stretched in the MD direction by, for example, applying a peripheral speed difference between multiple rolls and utilizing the roll peripheral speed difference between them (roll method).

[0110] From the viewpoint of further reducing the amount of residual solvent, it is preferable to further dry (post-dry) the film obtained after stretching. For example, it is preferable to further dry the film obtained after stretching while conveying it with a roll or the like (with a certain tension applied).

[0111] The drying temperature (the drying temperature without stretching or the drying temperature after stretching) is preferably (Tg-30) to (Tg+30)°C, and more preferably (Tg-20) to Tg°C, where Tg is the glass transition temperature of the resin. If the drying temperature is above a certain level, the evaporation rate of the solvent from the film-like material after stretching is easily increased, and therefore the drying efficiency is easily improved, whereas if the drying temperature is below a certain level, deformation due to stretching of the film-like material is easily suppressed. The drying temperature can be specified in the same manner as described above.

[0112] 2) About the process of forming the convex parts Next, a second resin composition is cast onto both widthwise ends of the obtained film base 11 to form convex portions.

[0113] The casting of the second resin composition may be a melt casting method or a solution casting method. From the viewpoint of improving production efficiency, when the first resin composition is cast by a solution casting method in the above step 1), it is preferable to form the second resin composition by a solution casting method as well.

[0114] That is, the convex portions 12 can be formed by applying a second resin composition (knurling solution) containing a resin and a solvent to both widthwise ends of the film base 11 and then drying the same.

[0115] (Second resin composition) The resin contained in the second resin composition may be the same as the resin contained in the dope.

[0116] The solvent contained in the second resin composition includes at least an organic solvent (good solvent) capable of dissolving the resin. Examples of the good solvent include chlorine-based organic solvents such as methylene chloride; and non-chlorine-based organic solvents such as methyl acetate, ethyl acetate, acetone, tetrahydrofuran, cyclopentanone, and toluene. Among them, methylene chloride, cyclopentanone, and toluene are preferable from the viewpoint of easily dissolving the cycloolefin resin. Among them, ketones such as cyclopentanone and methylene chloride are more preferable from the viewpoint of high volatilization speed due to high saturated vapor pressure and easy adjustment of S1 / S2 of the convex portion to the above range.

[0117] The solvent contained in the second resin composition may further contain a poor solvent, which may be the same as the poor solvent contained in the dope.

[0118] From the viewpoint of adjusting S1 / S2 of the convex portions to the above range, the viscosity of the second resin composition (knurling solution) during casting is preferably lower than the viscosity of the first resin composition (dope) during casting in the above step 1). Specifically, the ratio η2 / η1 of the viscosity η2 of the second resin composition during casting in the step 2) to the viscosity η1 of the first resin composition during casting in the step 1) is preferably 0.00003 to 0.01. When η2 / η1 is 0.00003 or more, S1 / S2 of the convex portions 12 tends to be 0.6 or more, and when η2 / η1 is 0.02 or less, S1 / S2 of the convex portions 12 tends to be 0.9 or less.

[0119] The viscosity η1 of the first resin composition during casting is preferably, for example, 10,000 to 100,000 mPa·s, and the viscosity η2 of the second resin composition is preferably 1 to 300 mPa·s. The viscosities can be measured with a viscometer (for example, a viscometer RE-80L manufactured by Toki Sangyo Co., Ltd.).

[0120] The viscosity during casting can be adjusted, for example, by the resin concentration or the molecular weight of the resin in the solution casting method; it is preferable to adjust, for example, by the melting temperature or the molecular weight of the resin in the melt casting method.

[0121] In the solution casting method, the resin concentration of the second resin composition is preferably lower than that of the first resin composition, and is preferably 50% by mass or less of the resin concentration of the first resin composition. Specifically, the resin concentration of the second resin composition is preferably more than 2% by mass and 10% by mass or less, and more preferably 3 to 7% by mass.

[0122] (Grant) The second resin composition can be applied by any method, for example, casting using a die (preferably a reduced pressure die) or coating using a dispenser.

[0123] When a reduced pressure die is used, the slit gap may be adjusted according to the thickness of the convex portion, and the slit width may be adjusted according to the width of the convex portion. The slit gap is preferably, for example, 100 to 300 μm, and the slit width is preferably, for example, 3 to 20 mm. When a dispenser is used, the discharge amount is preferably, for example, 1 to 100 μg / shot, and the discharge pitch is preferably, for example, 0.2 to 30 mm.

[0124] The temperature of the second resin composition during casting is, for example, 10 to 30° C., and is preferably room temperature (23° C.).

[0125] (Dry) The second resin composition can be dried by any method, for example, hot air drying, heating and drying by electromagnetic waves (for example, heating and drying by an infrared (IR) heater), etc. From the viewpoint of adjusting S1 / S2 of the convex portions 12 to the above range, a high drying speed is preferable, and heating and drying by electromagnetic waves is more preferable.

[0126] From the viewpoint of adjusting S1 / S2 of the convex portions 12 to the above range, it is preferable to dry the second resin composition as quickly as possible after it is applied to the film base 11. The drying depends on the composition of the resin composition, but it is preferable to dry it within 5 seconds after it is applied, for example.

[0127] The drying temperature is not particularly limited, but is preferably high from the viewpoint of adjusting S1 / S2 of the protrusions 12 to the above range. Specifically, the drying temperature is preferably 40 to (Tg-20)°C, and more preferably 80 to (Tg-10)°C, where Tg is the glass transition temperature of the resin contained in the second resin composition. Specifically, the drying temperature is preferably 40 to 120°C, and more preferably 80 to 100°C.

[0128] The resulting film 10 is then wound into a roll along the longitudinal direction.

[0129] 3) Winding process The obtained film base 11 is wound up in the longitudinal direction (direction perpendicular to the width direction) of the film 10 using a winding machine. This makes it possible to obtain the film wound up in a roll around a core, i.e., a roll of the film 10.

[0130] The winding method is not particularly limited, and may be a constant torque method, a constant tension method, a taper tension method, or the like.

[0131] The winding tension when winding the film base 11 can be about 50 to 170 N. Thus, the longer the winding length, the more likely it is that the air stored between the film filaments will be released all at once when the film is wound into a roll, causing misalignment and sticking. Even in such cases, by adjusting S1 / S2 of the protrusions 12 to fall within the above range, the film can be wound while appropriately releasing excess air (while appropriately storing air between the film), thereby preventing misalignment and sticking.

[0132] When the obtained film 10 is used, the portion where the convex portion 12 is formed is removed, and the film 10 is used as an optical film for a display device such as a liquid crystal display device or an organic EL display device. Examples of optical films include polarizing plate protective films (including retardation films and brightness enhancement films), transparent substrate films, and light diffusion films. Among these, the film 10 is preferably used as a polarizing plate protective film.

[0133] 3. Film and its manufacturing method As described above, the film of the present invention may be cut out from a roll of the strip-shaped film 10, and has strip-shaped convex portions at both ends in the width direction.

[0134] Specifically, the film has a film base (corresponding to the above-mentioned film base 11) and band-shaped convex portions (corresponding to the above-mentioned convex portions 12) provided at both ends of the surface in the width direction. In a cross section of the film perpendicular to the extending direction of the band-shaped convex portions, S1 and S2 of the convex portions satisfy the relationship of the above-mentioned formula (1), and more preferably satisfy 0.7≦S1 / S2≦0.9.

[0135] In the cross section of the film perpendicular to the extension direction of the belt-like protrusions, the shape of the protrusions, the total area of ​​S1 and S2, the maximum height Tmax and maximum width Wmax of the protrusions, and the ratio of the total area of ​​S1 and S2 to the area of ​​the film base are as described above. In the cross section of the film perpendicular to the extension direction of the belt-like protrusions, the shape of the film base 11 (having no recesses) and the thickness of the film base are also as described above.

[0136] The film can be produced in the same manner as the above-mentioned method for producing a roll body, except that it does not include the winding step 3) above, or it further includes a step of cutting out the strip-shaped film unwound from the roll body after the winding step 3) above.

[0137] [Variations] In the above embodiment, the protrusions 12 are arranged continuously along the longitudinal direction of the film base 11, but the present invention is not limited to this. For example, the protrusions 12 may be arranged intermittently along the longitudinal direction of the film base 11.

[0138] Fig. 3A is a plan view of a strip-shaped film in another embodiment, Fig. 3B is a cross-sectional view taken along line 3B-3B in Fig. 3A, Fig. 4A is a plan view of a strip-shaped film in another embodiment, and Fig. 4B is a cross-sectional view taken along line 4B-4B in Fig. 4A.

[0139] That is, the protrusions 12 may be arranged intermittently along the longitudinal direction of the film base 11 (see FIG. 3A). The length of the protrusions 12 (the length in the longitudinal direction of the film base 11) may be about 0.04 to 10.0% of the width of the film base 11. The gap between the multiple band-shaped protrusions 12 may be about 0.02 to 1.0% of the length of the protrusions 12.

[0140] The protrusions 12 may be arranged in an island shape along the longitudinal direction of the film base 11 (see FIG. 4A). Such protrusions 12 can be formed by intermittently discharging from a dispenser. The discharging conditions can be as described above.

[0141] In the above embodiment, the shape of the protrusion 12 is as shown in FIG. 2 (see FIG. 2), but the shape is not limited to this.

[0142] 5A to 5C are diagrams showing modified shapes of protrusions 12 in a cross section along the width direction of film 10. That is, the shape of protrusions 12 may be stepped (see FIG. 5A) or trapezoidal (see FIG. 5B). Also, protrusions 12 may have a shape in which the height of the center of protrusions 12 is lower than the height of both ends of protrusions 12 (see FIG. 5C).

[0143] In the above embodiment, one protrusion 12 is disposed on each of both ends in the width direction of the film base 11, but the present invention is not limited to this, and a plurality of protrusions may be disposed on each end.

[0144] Furthermore, in the above embodiment, an example has been shown in which the protrusions 12 are disposed on only one surface of the film base 11, but this is not limiting, and the protrusions 12 may be disposed on both surfaces.

[0145] In the above embodiment, the convex portion 12 is formed by applying a knurling solution containing a resin and a solvent and then drying it (solution casting method), but the present invention is not limited to this. The convex portion 12 may be formed by applying a molten resin composition and then cooling and solidifying it (melt casting method).

[0146] That is, in the melt casting method, the roll body can be obtained through the steps of 1) casting a molten first resin composition, cooling and solidifying it to obtain a strip-shaped film base, and 2) applying a molten second resin composition to both widthwise ends of the strip-shaped film base 11, cooling and solidifying it to form convex portions. In this case, the first resin composition and the second resin composition are the same as the above-mentioned first resin composition and second resin composition, respectively, except that they do not contain a solvent.

[0147] The melt viscosity of the second resin composition during casting is preferably lower than the melt viscosity of the first resin composition during formation of the film base 11. The melt viscosity can be adjusted by the melting temperature, the weight average molecular weight of the resin, and the like. For example, from the viewpoint of adjusting S1 / S2 to the above range, it is preferable that the Mw of the resin contained in the second resin composition is lower than the Mw of the resin in the first resin composition, and the melting temperature of the second resin composition during casting may be made higher than the melt viscosity of the first resin composition during formation of the film base 11.

[0148] In the above embodiment, the method of adjusting the shape of the protrusions 12 includes adjusting the viscosity or resin concentration of the second resin composition, the application method, the drying conditions, etc., but is not limited thereto. For example, the shape may be adjusted by cutting (machining) both ends after casting the second resin composition, or by subjecting the film base 11 to a surface treatment (such as hydrophilization treatment). EXAMPLES

[0149] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.

[0150] 1. Preparation of cycloolefin resin film (film base) <Preparation of Cycloolefin Resin Film 1> (Preparation of Microparticle Dispersion) 10 parts by mass of R218 and 80 parts by mass of ethanol were mixed and stirred in a dissolver for 30 minutes, and then dispersed using a Manton-Gaulin. 80 parts by mass of dichloromethane was added to the resulting solution while stirring, and the mixture was mixed and stirred in a dissolver for 30 minutes, and then filtered with a filter (Advantec Toyo Co., Ltd.: polypropylene wound cartridge filter TCW-PPS-1N) to obtain a fine particle dispersion.

[0151] (Preparation of dope) Next, a dope having the following composition was prepared. First, methylene chloride was added to a pressurized dissolution tank, and then the following cycloolefin resin was added while stirring. Next, the fine particle dispersion liquid prepared above was further added to this, heated to 60°C, and completely dissolved while stirring. The heating temperature was increased from room temperature at 5°C / min, and after dissolving for 30 minutes, the temperature was decreased at 3°C / min. This was filtered using SHP150 manufactured by ROKI TECHNO CO., LTD. at a filtration flow rate of 300 L / m. 2 ·h, filtration pressure 1.0×10 6 The mixture was filtered at 1000 Pa to obtain a dope. JSR Corporation G7810 (cycloolefin resin containing a structural unit represented by the following formula, weight average molecular weight 40,000, glass transition temperature 170°C): 100 parts by mass Methylene chloride: 150 parts by mass Ethanol: 20 parts by weight Fine particle dispersion: 150 parts by mass [ka]

[0152] (Film forming) The obtained dope was uniformly cast on a stainless steel belt support of an endless belt casting apparatus at room temperature (23°C). The temperature of the stainless steel belt was 28°C, and the conveying speed of the stainless steel belt was 20 m / min. Next, the solvent was evaporated until the residual solvent amount in the cast film was 25% by mass on the stainless steel belt support, and then the film was peeled off from the stainless steel belt support to obtain a film. Next, the obtained film-like material was stretched in the width direction by 1.2 times under the condition of (Tg-15)°C (Tg: Tg of the cycloolefin resin) using a tenter. Next, the stretched film was transported by rolls and further dried at (Tg-10)°C until the amount of residual solvent measured by the headspace gas chromatography described above was within the range of 30 to 600 mass ppm. The ends held by the tenter clips were then slit with a laser cutter and wound up to obtain a cycloolefin resin film having a width of 1450 mm, a length of 4000 m and a thickness of 20 μm.

[0153] <Preparation of Cycloolefin Resin Films 2 to 4> Cycloolefin resin films 2 to 4 were obtained in the same manner as in the production of cycloolefin resin film 1, except that the stretching ratio was changed so that the film thickness became 10 μm, 40 μm, and 60 μm.

[0154] 2. Preparation of convex portion forming solution (second resin composition) <Preparation of solutions 1-3, 6-9 and 11-14> Convex portion forming solutions 1 to 3, 6 to 9, and 11 to 14 were obtained by mixing the resin and solvent shown in Table 1 to obtain the resin concentration shown in Table 1. Of these, silica particles (R218) were added to solution 12 in an amount equal to the amount of silica particles in the film.

[0155] <Preparation of solution 4> Polymethyl methacrylate (PMMA, weight average molecular weight 1,000,000) was dissolved in a solvent shown in Table 1 at 35° C. to obtain a convexity forming solution 4.

[0156] <Preparation of solutions 5 and 10> Cellulose triacetate (TAC, weight average molecular weight 130,000) was dissolved in a solvent shown in Table 1 to obtain convexity forming solutions 5 and 10.

[0157] Table 1 shows the compositions and physical properties of the resulting convex portion forming solutions 1 to 14.

[0158] [Table 1]

[0159] 3. Preparation of the roll body <Examples 1 to 6, 8, 10, 11, and 16, and Comparative Examples 1, 3, 5, and 6> The solutions shown in Table 2 were continuously applied to both widthwise ends of the cycloolefin resin film prepared above from a reduced pressure die (a die in the comparative example) at room temperature (23°C) under the conditions shown in Table 2, and then dried to form the convex portions shown in Figures 1A and 1B.

[0160] <Example 9> 3A and 3B were formed in the same manner as in Example 1, except that the solution shown in Table 2 was applied intermittently under the conditions shown in Table 2. The length of the protrusions (in the longitudinal direction of the cycloolefin resin film) was 100 mm, and the pitch between the protrusions was 10 mm.

[0161] <Examples 7 and 13 to 15> The solution shown in Table 2 was applied to both ends of the width direction of the cycloolefin resin film prepared above using a dispenser under the conditions shown in the same table, and then dried to form the convex portions shown in Figures 4A and 4B. In Example 12, convex portions were formed on both sides of the film. The dispenser used was a SUPER HI JET manufactured by Musashi Engineering Co., Ltd.

[0162] <Example 12> Convex portions were formed in the same manner as in Example 3, except that the application shape of the convex portions was changed as shown in Table 2.

[0163] <Comparative Example 2> The cycloolefin resin film thus produced was embossed at both ends in the width direction on one side thereof to form an embossed portion. The embossing was performed by applying pressure with a heated metal ring having a pattern of convexo-concave patterns (nine convexo-concave patterns in the width direction). The processing pressure of the metal ring was 200 kPa, and the temperature was 230°C. The obtained embossed portion had a thin portion that was thinner than the thickness of the central portion in the width direction of the film. The area ratio S1' / S2' of the portion above the thin portion (corresponding to the convex portion) was measured and found to be 0.48.

[0164] <Comparative Example 4> The cycloolefin resin film thus prepared was irradiated with laser light by a laser marker on both ends in the width direction on one side to form a laser irradiated portion. The laser irradiated portion had a thinner portion that was thinner than the thickness of the central portion in the width direction of the film. The area ratio S1' / S2' of the portion above the thinner portion (corresponding to the convex portion) was measured and found to be 0.47.

[0165] <Evaluation> (viscosity ratio) In Examples 1 to 16 and Comparative Examples 1 to 6, the viscosity of the dope for the film when being cast and the viscosity of the convexity forming solution when being cast were measured using a viscometer RE-80L manufactured by Toki Sangyo Co., Ltd. The viscosity of the dope (first resin composition) when being cast into a film (23° C.) was 27,000 mPa s, and the viscosity of the convexity forming solution (second resin composition) was a viscosity that satisfied the viscosity ratio in Table 3.

[0166] Furthermore, the physical properties of the protrusions of the roll bodies obtained in Examples 1 to 16 and Comparative Examples 1 to 6, the shape of the roll body, and the presence or absence of deformation of the film were evaluated by the following methods.

[0167] <Physical properties of convex parts> The areas S1 and S2 of the convex portions, the maximum height Tmax, and the maximum width Wmax of the convex portions in the cross section in the width direction of the film were measured using a laser microscope, a Keyence VK-X1000 laser microscope. Specifically, the maximum height and maximum width of the protrusions were measured over a 15 mm-wide area 100 mm long in the longitudinal direction of the film, centered on one row of protrusions, and the average values ​​were taken as the "maximum height Tmax and maximum width Wmax of the protrusions." Similarly, for a region 100 mm long in the length direction of the film and 15 mm wide centered on one row of convexities, the lower half area and the upper half area were measured with a laser microscope with a height of Tmax / 2 as the border, and their average values ​​were taken as "areas S1 and S2 of convexity 12." When there are multiple rows (lines) of convexities, the values ​​for one row (line) of convexities are shown. In addition, in the case of dispenser coating or intermittent coating, the average values ​​of the measurements for multiple convexities present in the above region were taken.

[0168] (Roll Shape) The shape of the roll was measured using Keyence's XG-X2900 and CA-HL08MX (line scan camera) and CA-DZW50X (pattern lighting). Specifically, when observing the surface of the roll, the area of ​​deformations of 200 μm x 200 μm or more was measured and totaled, and judged as the area ratio (%) to the outermost surface of the roll (the area of ​​one turn of the outermost film). ◎: Less than 0.3% ○: 0.3% or more and less than 0.5% ○△: 0.5% or more and less than 1.0% △: Less than 1.0% Less than 2.0% ×: 2.0% or more If it was 〇△ or better, it was judged to be good.

[0169] (Film deformation) The film deformation was evaluated by unwinding the roll and counting the number of deformation defects using the XG-X2900, CA-HL08MX (line scan camera), and CA-DZW50X (pattern lighting) at a line speed of 5 m / min. The number of deformation defects was counted as one defect for every deformation of 100 μm x 100 μm or more. The film deformation was evaluated based on the following criteria. ◎: Less than 10 pieces / 1000m ○: Less than 50 pieces / 1000m ○△: Less than 100 pieces / 1000m △: Less than 200 pieces / 1000m ×:200 pieces / 1000m or more If it was rated as 〇△ or above, it was judged to be good.

[0170] Table 2 shows the conditions for producing the roll bodies of Examples 1 to 16 and Comparative Examples 1 to 6, and Table 3 shows the evaluation results.

[0171] [Table 2]

[0172] [Table 3]

[0173] As shown in Table 3, the roll bodies of Examples 1 to 16 all showed little misalignment or sticking, and little change in the shape of the roll body, and little deformation of the film.

[0174] In particular, it can be seen that by lowering the resin concentration of the convex portion forming solution, S1 / S2 can be appropriately reduced, and deformation of the roll body and deformation of the film can be further reduced (Comparison between Examples 3 and 9, Comparison between Examples 8 and 11).

[0175] It is also found that by using ketones such as cyclopentane as the solvent composition of the convex portion forming solution, S1 / S2 can be appropriately reduced, and deformation of the roll body and deformation of the film can be reduced (comparison between Examples 2, 3, and 10). This is believed to be due to the high saturated vapor pressure and high evaporation rate.

[0176] It is also found that applying the convex portion-forming solution with a dispenser can reduce deformation of the roll body and the film compared to applying the solution with a reduced pressure die (comparison between Examples 1 and 14 to 15). This is thought to be because dispenser coating can reduce curling of the base of the film caused by heat during drying compared to reduced pressure die coating.

[0177] In contrast, in Comparative Examples 1 and 3, in which S1 / S2 was greater than 0.95, deformation of the roll body and film occurred in both cases. This is believed to be because the protrusions were in close contact with the back surface of the base film during winding, preventing air from escaping, and as a result, the trapped air was periodically released, periodically causing misalignment during winding and film sticking.

[0178] In addition, it is found that the roll body of Comparative Example 2 which was embossed and the roll body of Comparative Example 4 in which the convex parts were formed by laser irradiation both deformed the roll body and the film. This is thought to be because the area S2 was low, so the embossed parts or the laser irradiated parts were crushed by stress, and the roll shape could not be maintained, resulting in sticking, etc.

[0179] <Examples 17 to 21> A roll body was formed in the same manner as in Example 3, except that the slit gap was changed as shown in Table 4.

[0180] <Examples 22 to 24> A roll body was formed in the same manner as in Example 7, except that the number of rows (number of lines) of convex portions and the pitch between convex portions (in the longitudinal direction of the film) were changed as shown in Table 4.

[0181] <Examples 25 to 27> A roll body was formed in the same manner as in Example 3, except that the winding length of the film was changed as shown in Table 4.

[0182] <Examples 28 to 30> A roll body was formed in the same manner as in Example 3, except that the thickness of the film was changed as shown in Table 4.

[0183] <Example 31> A roll body was formed in the same manner as in Example 3, except that the discharge width was changed as shown in Table 4.

[0184] <Examples 32 and 33> A roll body was formed in the same manner as in Example 7, except that the discharge amount and the pitch between the convex portions (in the longitudinal direction of the film) were changed as shown in Table 4.

[0185] The shape of the roll and the deformation of the film in Examples 17 to 33 were evaluated in the same manner as described above.

[0186] Table 4 shows the conditions for producing the roll bodies of Examples 17 to 33, and Table 5 shows the evaluation results.

[0187] [Table 4]

[0188] [Table 5]

[0189] As shown in Table 5, the roll bodies of Examples 17 to 33 all had little winding misalignment or sticking, and showed little change in the shape of the roll body. [Industrial Applicability]

[0190] According to the present invention, it is possible to provide a film roll body that is resistant to crushing due to winding pressure and that can suppress misalignment or sticking when an external impact is applied by maintaining an appropriate amount of air between the film sections, and a method for manufacturing the same. [Explanation of symbols]

[0191] 10 Strip of film 11 Film base 12 Convex part

Claims

1. A film having a film base and band-shaped convex portions fixed on a surface of both ends in a width direction of the film base, In a cross section of the film perpendicular to the extending direction of the belt-like convex portion, The upper surface shape of the protrusion is an arc shape in which the height of a central portion of the protrusion is higher than the height of both ends of the protrusion, A film characterized in that, when the maximum height of the convex portions is Tmax, a convex region S1 above a convex midpoint (Tmax / 2) relative to the maximum height Tmax of the convex portions is S1, and a convex region below the midpoint is S2, S1 and S2 satisfy the following formula (1): Formula (1): 0.6≦S1 / S2≦0.95

2. Tmax is 0.3 to 4.0 μm. The film of claim 1.

3. The film base does not have a recess. The film according to claim 1 or 2.

4. The thickness of the film base is 3 to 40 μm. The film according to any one of claims 1 to 3.

5. The film base is a resin film. The film according to any one of claims 1 to 4.

6. The resin film is an optical film. The film of claim 5.

7. The resin film contains a cycloolefin resin or a (meth)acrylic resin. The film according to claim 5 or 6.

8. A method for producing a film having band-shaped convex portions at both ends in a width direction, comprising the steps of: 1) A step of casting a first resin composition to obtain a strip-shaped film base; 2) casting a second resin composition onto both widthwise ends of the surface of the belt-shaped film base to form the belt-shaped convex portions; Including, a ratio η2 / η1 of a viscosity η2 of the second resin composition at the time of casting in the step 2) to a viscosity η1 of the first resin composition at the time of casting in the step 1) is 0.00003 to 0.02; A method for manufacturing a film.

9. Each of the first resin composition and the second resin composition contains a resin and a solvent, The resin concentration of the second resin composition is lower than the resin concentration of the first resin composition; A method for producing the film according to claim 8.

10. The resin concentration of the second resin composition is more than 2% by mass and not more than 10% by mass. A method for producing the film according to claim 9.

11. The thickness of the film base is 3 to 40 μm. A method for producing the film according to any one of claims 8 to 10.

12. The film base is an optical film. A method for producing the film according to any one of claims 8 to 11.

13. A roll body formed by winding up a strip-shaped film having a film base and strip-shaped convex portions fixed on a surface of both widthwise ends of the film base, In a cross section of the film perpendicular to the extending direction of the belt-like convex portion, The upper surface shape of the protrusion is an arc shape in which the height of a central portion of the protrusion is higher than the height of both ends of the protrusion, A roll body characterized in that, when the maximum height of the convex portions is Tmax, a convex portion region S1 above a convex portion midpoint (Tmax / 2) relative to the maximum height Tmax is S1, and a convex portion region below the midpoint is S2, S1 and S2 satisfy the following formula (1): Formula (1): 0.6≦S1 / S2≦0.95

14. A method for manufacturing a roll body in which a strip-shaped film having strip-shaped convex portions at both ends in a width direction is wound up, comprising the steps of: 1) A step of casting a first resin composition to obtain a strip-shaped film base; 2) casting a second resin composition onto both widthwise ends of the surface of the belt-shaped film base to form the belt-shaped convex portions; Including, a ratio η2 / η1 of a viscosity η2 of the second resin composition at the time of casting in the step 2) to a viscosity η1 of the first resin composition at the time of casting in the step 1) is 0.00003 to 0.02; A method for manufacturing a roll body.

Citation Information

Patent Citations

  • Casting apparatus, solution film forming equipment, and solution film forming method

    JP2009184136A

  • Manufacturing method for optical film

    JP2009234169A

  • Optical film, optical film roll, and method for manufacturing optical film

    JP2012118238A

  • Method for forming knurling, device for forming knurling, method for forming film using solution and polymer film

    JP2012206312A

  • Roll body of optical film, manufacturing method therefor, package, polarization plate and liquid crystal display device