Roll body and its manufacturing method, film and its manufacturing method
By using cycloolefin resin compositions with controlled melting temperatures and activation treatments, the roll body achieves enhanced adhesion between the film base and convex portions, preventing peeling and misalignment, thus stabilizing film unwinding.
Patent Information
- Application Number
- JP2022530001
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-12
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-06-12
AI Technical Summary
Existing roll bodies of resin films experience insufficient adhesion between the film base and convex portions, leading to peeling and winding misalignment during transportation and storage.
A roll body configuration where the film base and convex portions are made from cycloolefin resin compositions with controlled melting temperatures and activation treatments to enhance adhesion, using a crosslinkable composition with urethane or modified olefin polymers to form strong bonds.
The solution achieves high adhesion between the film base and convex portions, effectively preventing peeling and winding misalignment, ensuring stable film unwinding and reducing defects.
Smart Images

Figure 0007556387000005 
Figure 0007556387000001 
Figure 0007556387000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a roll body and a method for producing the same, and a film and a method for producing the same. [Background technology]
[0002] Resin films mainly composed of cycloolefin resins have good transparency and good moisture resistance, and therefore are used as optical films such as polarizing plate protective films, etc. From the viewpoints of ease of handling and production efficiency, these optical films are usually stored or transported in the form of a roll obtained by winding a strip-shaped film into a roll.
[0003] In such a roll body, in order to prevent quality defects caused by films sticking to each other during storage or transportation, a process called embossing is usually performed on both ends in the width direction of the film to create projections and recesses (see, for example, Patent Document 1). However, the embossed portions formed by embossing are easily crushed, and it has sometimes been impossible to sufficiently prevent films from sticking to each other.
[0004] In response to this, a method is also known in which knurling portions (convex portions) are formed by coating on both widthwise ends of a film. Specifically, a method has been proposed in which a knurling-forming liquid A containing cellulose triacetate, a plasticizer, silicon dioxide particles, and a solvent is coated on both widthwise ends of a resin film, and then dried, or a knurling-forming liquid B containing dipentaerythritol hexaacrylate and a photopolymerization initiator is photocured to form knurling portions (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-118238 A [Patent Document 2] JP 2012-206312 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the roll of Patent Document 2, sufficient adhesion was not obtained between the resin film (film base) and the knurling portion (protruding portion). Therefore, for example, when vibration is applied to the roll in the width direction, the knurling portion is likely to peel off, and misalignment of the winding is likely to occur.
[0007] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a roll of strip film and a manufacturing method thereof that have high adhesion of convex portions to the film base and can suppress peeling of the convex portions and the resulting winding misalignment. [Means for solving the problem]
[0008] The above problem can be solved by the following configuration.
[0009] The roll body of the present invention is a roll body obtained by winding a strip-shaped film in a direction perpendicular to its width direction, the film having a film base and convex portions provided at both ends in the width direction, the film base containing a first resin composition containing a cycloolefin resin, and the convex portions containing a second resin composition containing a cycloolefin resin, or a crosslinked product of a crosslinkable composition containing a urethane polymer or a modified olefin polymer having a functional group reactive with a polar group on the film base.
[0010] The method for producing a roll body of the present invention is a method for producing a roll body by winding a strip-shaped film along a direction perpendicular to its width direction, and includes the steps of 1) melt-casting a first resin composition containing a cycloolefin resin, followed by cooling and solidifying to obtain a strip-shaped film base, and 2) melt-casting a second resin composition containing a cycloolefin resin onto both widthwise ends of the strip-shaped film base, followed by cooling and solidifying to form convex portions, wherein a melting temperature T2 of the second resin composition during the melt-casting is the same as or higher than a melting temperature T1 of the first resin composition during the melt-casting.
[0011] The method for producing a roll body of the present invention is a method for producing a roll body by winding a strip-shaped film along a direction perpendicular to its width direction, and includes the steps of: 1) casting a first resin composition containing a cycloolefin resin to obtain a strip-shaped film base; 2) performing an activation treatment on both widthwise end portions of the strip-shaped film base; and 3) casting a crosslinkable composition containing a urethane polymer or a modified olefin polymer having a functional group reactive with a polar group on the film base onto the activation-treated surfaces of both widthwise end portions of the strip-shaped film base, followed by crosslinking to form convex portions.
[0012] The film of the present invention is a film having a film base and band-shaped convex portions provided on both ends thereof, wherein the film base comprises a first resin composition containing a cycloolefin resin, and the convex portions are a second resin composition containing a cycloolefin resin, or comprise a crosslinked product of a crosslinkable composition containing a urethane polymer or a modified olefin polymer having a functional group that reacts with a polar group on the film base.
[0013] The film manufacturing method of the present invention is a method for manufacturing a film having a film base and band-shaped convex portions provided on both ends thereof, and includes the steps of 1) melt-casting a first resin composition containing a cycloolefin resin, followed by cooling and solidifying to obtain a band-shaped film base, and 2) melt-casting a second resin composition containing a cycloolefin resin onto both ends of the band-shaped film base, followed by cooling and solidifying to form convex portions, wherein the melting temperature T2 of the second resin composition during the melt-casting is the same as or higher than the melting temperature T1 of the first resin composition during the melt-casting.
[0014] The method for producing a film of the present invention is a method for producing a film having a film base and strip-shaped convex portions provided at both ends thereof, and includes the steps of 1) casting a first resin composition containing a cycloolefin resin to obtain a strip-shaped film base, 2) subjecting both widthwise ends of the strip-shaped film base to an activation treatment, and 3) casting a crosslinkable composition containing a urethane polymer or a modified olefin polymer having a functional group that reacts with a polar group on the film base onto the surfaces that have been subjected to the activation treatment at both widthwise ends of the strip-shaped film base, and then crosslinking the surfaces to form convex portions. Effect of the Invention
[0015] According to the present invention, it is possible to provide a belt-shaped film roll body and a manufacturing method thereof in which the protrusions have high adhesion to the film base and peeling of the protrusions and the resulting winding misalignment can be suppressed. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1A is a plan view of a band-shaped film in the present embodiment, and FIG. 1B is a cross-sectional view taken along line 1B-1B of FIG. 1A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] (Regarding the first aspect) The inventors have discovered that, first, by using "a cycloolefin resin as the material for the convex portions" and "when producing the roll body, the melting temperature T2 of the second resin composition for obtaining the convex portions is made higher than the melting temperature T1 of the first resin composition for obtaining the film base," good adhesion of the convex portions can be obtained and winding misalignment can be suppressed.
[0018] The mechanism behind this is unclear, but is presumed to be as follows. By using the same material for the protrusions as for the film base, the adhesion between the protrusions and the film base can be improved. Furthermore, when the melting temperature T1 of the first resin composition during film formation to obtain the film base is relatively low, the density of the film base tends to be low. Therefore, the cycloolefin resin of the second resin composition for obtaining the protrusions tends to penetrate easily and the polymer chains tend to become entangled with each other, improving adhesion. On the other hand, when the melting temperature T2 of the second resin composition is relatively high, the fluidity of the cycloolefin resin increases, so that the penetration into the film base and the entanglement of the polymer chains tend to occur easily, improving adhesion between the film base and the protrusions.
[0019] (Regarding the second aspect) Secondly, the inventors discovered that by using "a urethane polymer or modified olefin polymer having functional groups that react with polar groups (e.g., hydroxyl groups or carbonyl groups) on the surface of the film base as the material for the convex portions" and by carrying out "an activation treatment for generating polar groups on both widthwise ends of the film base during production of the roll body," good adhesion of the convex portions can be obtained and winding misalignment can be suppressed.
[0020] The mechanism behind this is unclear, but is presumed to be as follows. Polar groups such as hydroxyl groups are generated on the surface of the film base that has been subjected to activation treatment such as corona treatment. For example, a cycloolefin resin containing a structural unit derived from a monomer having a norbornene structure as described below has a tertiary carbon, and therefore is prone to generating polar groups such as hydroxyl groups by corona treatment or the like. By applying a crosslinkable composition containing a polymer having a functional group that reacts with the polar group to such a treated surface, the polar group on the surface of the film base reacts with the functional group of the polymer, improving the adhesion between the film base and the convex portion.
[0021] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0022] 1. Film roll The roll body of the present invention is a strip-shaped film wound into a roll in a direction perpendicular to the width direction of the film.
[0023] Fig. 1A is a plan view of a band-shaped film in the present embodiment, and Fig. 1B is a cross-sectional view taken along line 1B-1B in Fig. 1A. Note that in Fig. 1B, hatching of the cross section has been omitted for ease of viewing.
[0024] As shown in FIGS. 1A and 1B, a strip-shaped film 10 has a film base 11 and protruding portions 12 provided on both ends in the width direction.
[0025] 1-1.Film base 11 The film base 11 includes a first resin composition that includes a thermoplastic resin.
[0026] The thermoplastic resin is not particularly limited as long as it is suitable for an optical film, but from the viewpoint of having good transparency and low moisture absorption, a cycloolefin resin is more preferable. That is, the film base 11 includes a first resin composition containing a cycloolefin resin.
[0027] The cycloolefin resin is preferably a polymer containing a structural unit derived from a monomer having a norbornene structure.
[0028] Examples of monomers having a norbornene structure include bicyclo[2.2.1]hept-2-ene (trivial name: norbornene), tricyclo[4.3.0.12,5]deca-3,7-diene (trivial name: dicyclopentadiene), 7,8-benzotricyclo[4.3.0.12,5]dec-3-ene (trivial name: methanotetrahydrofluorene), tetracyclo[4.4.0.12,5.17,10]dodec-3-ene (trivial name: tetracyclododecene), and derivatives thereof (e.g., those having a substituent on the ring).
[0029] Examples of the substituent include an alkyl group, an alkylene group, an alkenyl group, an alkynyl group, an alkylidene group, an aryl group, and a polar group.
[0030] The polar group may be a group containing a heteroatom selected from an oxygen atom, a nitrogen atom, a sulfur atom, a silicon atom, and a halogen atom, and examples thereof include a carboxyl group, a carbonyl group, a carbonyloxycarbonyl group, an epoxy group, a hydroxyl group, an oxy group, an ester group, a silanol group, a silyl group, an amino group, an amide group, an imide group, a nitrile group, a carbonate group, a thioester group, a thiocarbonate group, a thioether group, a thionyl oxide group, and a sulfonic acid group.
[0031] The monomer having a norbornene structure may be used alone or in combination of two or more kinds.
[0032] The content of the structural unit derived from the monomer having a norbornene structure is preferably 50 to 100% by mass, more preferably 70% by weight or more, and even more preferably 90% by weight or more, based on the total structural units constituting the cycloolefin resin. When the content of the structural unit derived from the norbornene monomer is within the above range, the transparency and heat resistance of the cycloolefin resin are good.
[0033] The cycloolefin resin may further contain a structural unit derived from a copolymerizable monomer that is copolymerizable with the monomer having a norbornene structure, as necessary.
[0034] Examples of the copolymerizable monomer include a copolymerizable monomer that does not have a norbornene structure; examples of the copolymerizable monomer that does not have a norbornene structure include a copolymerizable monomer capable of ring-opening copolymerization and a copolymerizable monomer capable of addition copolymerization.
[0035] Examples of the copolymerizable monomer capable of ring-opening copolymerization include cycloolefins such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, and dicyclopentadiene.
[0036] Examples of copolymerizable monomers capable of addition copolymerization include unsaturated double bond-containing compounds, vinyl cyclic hydrocarbon monomers, and (meth)acrylic acid esters. Examples of unsaturated double bond-containing compounds are α-olefins having 2 to 20 carbon atoms, examples of which include ethylene, propylene, and 1-butene. Examples of vinyl cyclic hydrocarbon monomers include vinylcyclopentene monomers such as 4-vinylcyclopentene and 2-methyl-4-isopropenylcyclopentene. Examples of (meth)acrylic acid esters include (meth)acrylic acid alkyl esters having 1 to 20 carbon atoms, such as methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Hereinafter, (meth)acrylic acid refers to acrylic acid or methacrylic acid.
[0037] Examples of the cycloolefin resin include a ring-opening polymer of a monomer having a norbornene structure and its hydrogenated product; an addition polymer of a monomer having a norbornene structure and its hydrogenated product. Among them, a hydrogenated product of a ring-opening polymer of a monomer having a norbornene structure is preferred from the viewpoints of moldability, heat resistance, low moisture absorption, etc.
[0038] The weight average molecular weight (Mw1) of the cycloolefin resin is not particularly limited, but is preferably from 10,000 to 100,000, more preferably from 15,000 to 80,000, and even more preferably from 20,000 to 50,000. When Mw1 is within the above range, the obtained film has an excellent balance between mechanical strength and moldability.
[0039] The Mw1 of the cycloolefin resin can be measured in terms of polystyrene by gel permeation chromatography (GPC). Specifically, it can be measured using a Tosoh Corporation HLC8220GPC) and a column (Tosoh Corporation TSK-GEL G6000HXL-G5000HXL-G5000HXL-G4000HXL-G3000HXL in series).
[0040] The glass transition temperature (Tg1) of the cycloolefin resin is usually 100° C. or higher, preferably 110 to 190° C., and more preferably 120 to 180° C. If Tg1 is 100° C. or higher, deformation due to use under high temperature conditions or secondary processing such as coating or printing can be easily suppressed, and if it is 190° C. or lower, resin deterioration due to molding processing or heat during molding processing can be easily suppressed.
[0041] The Tg1 of the cycloolefin resin can be measured using DSC (Differential Scanning Colorimetry) in accordance with JISK 7121-2012 or ASTM D3418-82.
[0042] The content of the cycloolefin resin is preferably 80% by mass or more, and can be 90 to 100% by mass, relative to the first resin composition.
[0043] (Other ingredients) The first resin composition may further contain other components other than the cycloolefin resin as necessary. Examples of the other components include fine particles (matting agents), heat stabilizers, light stabilizers, UV absorbers, antistatic agents, antioxidants, lubricants, colorants (pigments, dyes, etc.), and fluorescent whitening agents.
[0044] The fine particles (matting agent) can impart appropriate slipperiness to the film base 11. The fine particles may be inorganic fine particles or organic fine particles.
[0045] Examples of inorganic fine particles include silica particles. The average primary particle size of the silica particles is not particularly limited, but is preferably, for example, 5 to 100 nm, and more preferably 10 to 50 nm.
[0046] An example of the organic fine particles is preferably polymer fine particles having a refractive index difference with the resin of 0.01 or less. From the viewpoint of high affinity with the resin and easy adjustment of the refractive index to the above range, an example of such organic fine particles is preferably a copolymer containing a structural unit selected from the group consisting of (meth)acrylic acid esters, vinyl esters, styrenes, and olefins, more preferably a copolymer containing a structural unit derived from a (meth)acrylic acid ester and a styrene, and even more preferably a copolymer containing a structural unit derived from a (meth)acrylic acid ester, a structural unit derived from a styrene, and a structural unit derived from a polyfunctional monomer.
[0047] The glass transition temperature (Tg) of the organic fine particles is preferably not less than 80° C. The glass transition temperature (Tg) of the organic fine particles can be measured in accordance with JISK 7121-2012 or ASTM D 3418-82.
[0048] The average particle diameter of the organic fine particles is 0.01 to 0.4 μm. When the average particle diameter of the organic fine particles is 0.01 μm or more, it is possible to form unevenness of appropriate size on the surface of the obtained film, making it easy to impart slipperiness, and when it is 0.4 μm or less, it is easy to suppress an increase in the internal haze of the film. From the above viewpoint, the average particle diameter of the organic fine particles is more preferably 0.07 to 0.28 μm. The average primary particle diameter of the fine particles can be determined by 1) observing the cross section parallel to the in-plane slow axis of the film with a TEM; and 2) measuring the primary particle diameters of any 10 fine particles in the TEM image, and averaging them.
[0049] Examples of the antioxidant include phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants. Among them, phenol-based antioxidants are preferred, and alkyl-substituted phenol-based antioxidants are more preferred. The content of the antioxidant is not particularly limited, but may be 0.001 to 5 parts by mass, preferably 0.01 to 3 parts by mass, per 100 parts by mass of the cycloolefin resin.
[0050] Examples of the ultraviolet absorbing agent include a benzotriazole-based ultraviolet absorbing agent, a benzoate-based ultraviolet absorbing agent, a benzophenone-based ultraviolet absorbing agent, an acrylate-based ultraviolet absorbing agent, and a metal complex-based ultraviolet absorbing agent. Examples of the light stabilizer include a hindered amine-based light stabilizer.
[0051] Examples of dyes include oil-soluble dyes (various CI solvent dyes). Examples of pigments include diarylide pigments, azo lake pigments, condensed azo pigments, benzimidazolone pigments, quinacridone pigments, perylene pigments, and anthraquinone pigments.
[0052] Examples of the antistatic agent include long-chain alkyl alcohols such as stearyl alcohol and behenyl alcohol, and fatty acid esters of polyhydric alcohols such as glycerin monostearate and pentaerythritol monostearate.
[0053] [Physical Properties] The thickness of the film base 11 is constant. That is, the film base 11 is not embossed, and therefore does not have a thin portion formed by being crushed by an embossing roller. The thickness of the film base 11 is not particularly limited, but is preferably 10 to 40 μm, more preferably 10 to 30 μm, and even more preferably 15 to 20 μm.
[0054] The length (wound length) of the film base 11 is not particularly limited, but is preferably 2000 to 15000 m, and more preferably 3000 to 12000 m. The width of the film base 11 is not particularly limited, but is preferably 1000 to 3000 mm.
[0055] 1-2. Convex part 12 The protrusions 12 are arranged in a strip shape along the longitudinal direction of the film base 11 at both ends in the width direction of the film base 11 (see FIG. 1A). The protrusions 12 may be arranged continuously or intermittently. In the present embodiment, the protrusions 12 are arranged continuously (see FIG. 1A).
[0056] In the cross section of the width direction of the film 10, the shape of the protrusions 12 is not particularly limited and may be a polygon or a circular segment. A circular segment is a shape in which both ends of a circular or elliptical arc are connected by a straight line, and examples thereof include a semicircle and a semiellipse. Examples of a polygon include a rectangle and a trapezoid.
[0057] The height T of the protrusions 12 is not particularly limited, but is preferably 1.0 to 25%, and more preferably 2.5 to 10%, of the thickness of the film base 11. Specifically, the height T of the protrusions 12 is preferably 0.3 to 4.0 μm, and more preferably 0.5 to 2.0 μm. The height of the protrusions 12 refers to the height from the surface of the film base 11 (the height in the normal direction to the surface of the film base 11).
[0058] The width W of the protrusions 12 is not particularly limited, but is preferably 0.2 to 2.0%, and more preferably 0.4 to 1.5%, of the width of the film base 11. Specifically, the width W of the protrusions 12 is preferably 5 to 20 mm, and more preferably 10 to 15 mm.
[0059] The height T and width W of the protrusions 12 in the cross section in the width direction of the film 10 can be measured using a laser microscope. As the laser microscope, for example, a Laser Microscope VK-X1000 manufactured by Keyence Corporation can be used.
[0060] The protrusions 12 contain a second resin composition containing a cycloolefin resin, or a crosslinked product of a crosslinkable composition containing a polymer having a functional group that reacts with a polar group on the film base 11 .
[0061] <Second resin composition> The cycloolefin resin contained in the second resin composition (constituting the protrusions 12) may be the same as the cycloolefin resin contained in the first resin composition (constituting the film base 11).
[0062] The weight average molecular weight (Mw2) of the cycloolefin resin contained in the second resin composition is preferably smaller than the weight average molecular weight (Mw1) of the cycloolefin resin contained in the first resin composition. When the convex portion 12 is formed by, for example, a melt casting method, if the molten cycloolefin resin has a low molecular weight, it is likely to penetrate into the gaps between the polymer chains of the cycloolefin resin contained in the film base 11, and the effect of improving adhesion due to entanglement is likely to be obtained. Specifically, (Mw1-Mw2) is preferably 10,000 or more, and more preferably 20,000 to 90,000.
[0063] The Mw2 of the cycloolefin resin contained in the second resin composition is not particularly limited as long as it satisfies the above relationship, but is preferably from 10,000 to 100,000. When Mw2 is 10,000 or more, the mechanical strength of the resulting protrusions 12 is easily obtained, and when Mw2 is 100,000 or less, the viscosity is unlikely to become high during melt extrusion, and moldability is unlikely to be impaired.
[0064] The content of the cycloolefin resin in the second resin composition is preferably 80% by mass or more, and more preferably 90 to 100% by mass.
[0065] The second resin composition may further contain other components as necessary. Examples of the other components include the same components as those contained in the first resin composition, such as fine particles (matting agents).
[0066] <Crosslinkable composition> The crosslinkable composition includes a polymer having functional groups. The polymer may be an oligomer or a polymer.
[0067] The functional group is preferably a group that reacts with a polar group on the surface of the film base 11, and examples of such polar groups include a hydroxyl group. Examples of functional groups that react with a hydroxyl group include a carboxyl group, a group derived from a carboxylic acid anhydride residue, a carboxylate group, an ammonium group, an amino group, and an isocyanate group. Among these, a carboxyl group, a group derived from a carboxylic acid anhydride residue, and an isocyanate group are preferred.
[0068] That is, the polymer having a functional group is preferably a urethane polymer having a functional group reactive with a hydroxyl group, or a modified olefin polymer having a functional group reactive with a hydroxyl group.
[0069] (Urethane polymer having functional groups) The urethane polymer having a functional group may be, for example, a polyurethane obtained by reacting (i) a polyhydric alcohol component having two or more hydroxyl groups in one molecule with (ii) a polyisocyanate component, or a polyurethane obtained by chain-extending an isocyanate group-containing prepolymer obtained by reacting the components (i) and (ii) with a chain extender. Also, a part of the above (i) may be replaced with a component having an acid structure (iii).
[0070] (i) Ingredients: The component (i) is not particularly limited, but examples thereof include alkylene polyols, polyether polyols, polyester polyols, polyether ester polyols, and polycarbonate polyols. These may be used alone or in combination of two or more.
[0071] (1) Alkylene polyol Examples of polyoxyalkylene polyols include ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, 1,5-pentanediol, neopentyl glycol, 1,6-hexane glycol, 2,5-hexanediol, dipropylene glycol, tricyclodecane dimethanol, 1,4-cyclohexane dimethanol, 2,2-dimethylpropanediol, 1,4-butanediol, and the like.
[0072] (2) Polyether polyol Examples of polyether polyols include alkylene oxide adducts of alkylene polyols; ring-opening (co)polymers of alkylene oxides and cyclic ethers (e.g., tetrahydrofuran); polyethylene glycol, polypropylene glycol, ethylene glycol-propylene glycol copolymers; glycols such as polytetramethylene glycol, polyhexamethylene glycol, and polyoctamethylene glycol.
[0073] (3) Polyester polyol Examples of polyester polyols include those obtained by polycondensing a dicarboxylic acid or its anhydride with a polyol under conditions of excess hydroxyl groups. Examples of dicarboxylic acids include adipic acid, succinic acid, sebacic acid, glutaric acid, maleic acid, fumaric acid, phthalic acid, or anhydrides thereof. Examples of polyols include the polyalkylene polyols described above in (1).
[0074] Examples of the polyester polyol include ethylene glycol-adipic acid condensate, butanediol-adipic acid condensate, hexamethylene glycol-adipic acid condensate, and ethylene glycol-propylene glycol-adipic acid condensate.
[0075] (4) Polyetherester polyol Examples of polyetherester polyols include ether group-containing polyols (e.g., polyether polyols and diethylene glycol as described in (2) above) or mixtures of these with other glycols, which are then reacted with dicarboxylic acids or their anhydrides as described in (3) above, and alkylene oxides. More specifically, polytetramethylene glycol-adipic acid condensates are exemplified.
[0076] (5) Polycarbonate polyol The polycarbonate polyol may be a compound represented by the formula: HO-R-(OC(O)-OR)x-OH (R represents a saturated fatty acid polyol residue having 1 to 12 carbon atoms, x represents the number of repeating units in the molecule and is usually an integer of 5 to 50.
[0077] Polycarbonate polyols can be obtained by a transesterification method in which a saturated aliphatic polyol is reacted with a substituted carbonate (e.g., diethyl carbonate, diphenyl carbonate) under conditions in which hydroxyl groups are in excess; or by a method in which a saturated aliphatic polyol is reacted with phosgene, or, if necessary, further reacted with a saturated aliphatic polyol.
[0078] (ii) Ingredients: The component (ii) is a polyisocyanate component having two or more isocyanate groups in one molecule.
[0079] Examples of the polyisocyanate component include aliphatic diisocyanates having 1 to 12 carbon atoms, such as hexamethylene diisocyanate, 2,2,4-trimethylhexane diisocyanate, and hexane diisocyanate (HDI); alicyclic diisocyanates having 4 to 18 carbon atoms, such as 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, isophorone diisocyanate (IPDI), and dicyclohexylmethane diisocyanate (HMDI); and aromatic isocyanates, such as tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate.
[0080] (iii) Ingredients: The component (iii) is a polyol having an acidic group. The acidic group can be a carboxyl group or a sulfonic acid group. Examples of polyols having an acidic group include dimethylolalkanoic acids such as dimethylolacetic acid, dimethylolpropionic acid, and dimethylolbutyric acid.
[0081] As described above, the polyurethane can be prepared by reacting (i) a polyhydric alcohol component with (ii) a polyvalent isocyanate component, or by subjecting (i) and (ii) components to a urethane reaction in an organic solvent under an isocyanate group excess condition to obtain an isocyanate group-containing prepolymer, neutralizing the prepolymer, and chain extending the prepolymer using a chain extender. Also, an acid structure can be introduced by replacing a part of (i) component with (iii) an acid group-containing component.
[0082] The method for extending the chain of the isocyanate group-containing prepolymer may be a known method. For example, water, a water-soluble polyamine, a glycol or the like may be used as a chain extender, and the isocyanate group-containing prepolymer and the chain extender may be reacted, if necessary, in the presence of a catalyst.
[0083] When the urethane resin has an acidic group, at least a part of the acidic group may be neutralized. Neutralizing the acidic group can improve the water dispersibility of the urethane resin. Examples of the neutralizing agent include organic amines such as trimethylamine, triethylamine, and tripropylamine; and inorganic bases such as sodium hydroxide, potassium hydroxide, and ammonia.
[0084] (Modified olefin polymer having functional groups) The modified olefin polymer is a polyolefin having a functional group obtained by modifying a polyolefin with a compound (modifier) having a functional group. Among them, the modified olefin polymer is more preferably an acid-modified olefin polymer. The acid-modified olefin polymer is obtained by reacting an olefin polymer with an unsaturated carboxylic acid or its anhydride to introduce a carboxyl group or a group derived from a carboxylic acid anhydride (graft modification).
[0085] The olefin polymer may be a homopolymer of an olefin monomer, or a copolymer of an olefin monomer and another monomer.
[0086] The olefin monomer is preferably an α-olefin having 2 to 8 carbon atoms. Examples of the α-olefin having 2 to 8 carbon atoms include ethylene, propylene, 1-butene, isobutylene, and 1-hexene, and preferably ethylene or propylene. Examples of monomers other than the olefin monomer include vinyl acetate, (meth)acrylic acid ester, styrene, etc.
[0087] Examples of polyolefins include very low density polyethylene (VLDPE), low density polyethylene (LDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), linear low density polyethylene, polypropylene (PP), ethylene-propylene copolymer, olefin elastomer (TPO), ethylene-vinyl acetate copolymer (EVA), ethylene-(meth)acrylic acid copolymer, and ethylene-(meth)acrylic acid ester copolymer, and preferably ethylene-(meth)acrylic acid copolymer.
[0088] The modifier may be an unsaturated carboxylic acid or anhydride thereof. Examples of the unsaturated carboxylic acid or anhydride thereof include maleic acid, fumaric acid, itaconic acid, citraconic acid, glutaconic acid, tetrahydrophthalic acid, aconitic acid, maleic anhydride, itaconic anhydride, glutaconic anhydride, citraconic anhydride, aconitic anhydride, norbornene dicarboxylic anhydride, and tetrahydrophthalic anhydride, and preferably maleic anhydride.
[0089] (Common matters) The weight average molecular weight (Mw3) of the polymer having a functional group contained in the crosslinkable composition is not particularly limited, but is preferably larger than the weight average molecular weight (Mw1) of the cycloolefin resin contained in the first resin composition. Specifically, (Mw3-Mw1) is preferably 30,000 or more, and more preferably 50,000 to 100,000.
[0090] In this way, by making the Mw3 of the polymer contained in the crosslinkable composition larger than the Mw1 of the cycloolefin resin contained in the first resin composition, the polymer chains of the polymer contained in the crosslinkable composition (of the protrusions 12) tend to become entangled with the polymer chains of the cycloolefin resin contained in the first resin composition (of the film base 11). Therefore, the polymer chains of the cycloolefin resin of the film base 11 are indirectly bonded via the polymer, providing a reinforcing effect, which is believed to enhance the adhesion between the film base 11 and the protrusions 12.
[0091] The Mw3 of the polymer is not particularly limited as long as it satisfies the above relationship, but is preferably from 40,000 to 200,000, and more preferably from 80,000 to 160,000. When Mw3 is at least the lower limit, the mechanical strength of the resulting protrusions 12 is easily obtained, and when Mw3 is at most the upper limit, the viscosity of the solution during molding does not become too high, and moldability is less likely to be impaired.
[0092] The content of the above polymer is preferably 60% by mass or more, and more preferably 80 to 100% by mass, based on the solid content of the crosslinkable composition.
[0093] The crosslinkable composition may further contain other components as necessary. Examples of the other components include the same components as those contained in the first resin composition, such as fine particles (matting agent).
[0094] 2. Manufacturing method of roll body The roll body of the present invention can be obtained through 1) a step of obtaining a strip-shaped film base 11, and 2) a step of forming convex portions on both widthwise ends of the strip-shaped film base 11.
[0095] 1) Process for obtaining the film base 11 The first resin composition is cast to obtain a strip-shaped film base 11.
[0096] The casting of the first resin composition may be performed by a melt casting method or a solution casting method, among which the melt casting method is preferred from the viewpoints of not requiring a solvent and of the associated reduction in equipment load and reduction in environmental load.
[0097] That is, the film base 11 can be obtained through a process in which a first resin composition containing a cycloolefin resin is melt-kneaded, then cast onto a support, and cooled and solidified.
[0098] The melt kneading can be carried out by any method, but is preferably carried out by extrusion molding from the viewpoint of being able to uniformly thin the thickness, etc. The melting temperature T1 is preferably lower than the melting temperature T2 of the second resin composition described later.
[0099] Specifically, when the glass transition temperature of the cycloolefin resin contained in the first resin composition is Tg1, the melting temperature T1 of the first resin composition is preferably (Tg1+90) to (Tg1+150)°C. When the melting temperature T1 is (Tg1+90)°C or higher, the fluidity during extrusion is good, and when it is (Tg1+150)°C or lower, the quality deterioration due to thermal deterioration of the resin is unlikely to occur. From the same viewpoint, the melting temperature T1 is more preferably (Tg1+110) to (Tg1+130)°C. Specifically, it is 220 to 300°C, preferably 240 to 290°C, and more preferably 260 to 280°C.
[0100] Next, the molten first resin composition is extruded from a slit-shaped discharge port of a T-die, and solidified by a cooling roll (support) to form a film.
[0101] The temperature of the cooling roll is preferably from 50 to 100°C, and more preferably from 70 to 90°C.
[0102] If necessary, the obtained film may be stretched.
[0103] The stretching may be carried out according to the desired optical properties. It is preferable to stretch in at least one direction, and it may be performed in two mutually perpendicular directions (for example, biaxial stretching in the width direction (TD) of the film and the transport direction (MD) perpendicular thereto).
[0104] When the glass transition temperature of the cycloolefin resin is Tg1, the heating temperature during stretching (stretching temperature) is preferably from (Tg1+5)° C. to (Tg1+150)° C., and more preferably from (Tg1+15)° C. to (Tg1+100)° C. When the stretching temperature is at least a certain level, it is easy to adjust the stretching tension to an appropriate range.
[0105] The film can be stretched in the TD (width) direction by, for example, fixing both ends of the film with clips or pins and widening the distance between the clips or pins in the traveling direction (tenter method).The film can be stretched in the MD direction by, for example, applying a peripheral speed difference between multiple rolls and utilizing the roll peripheral speed difference between them (roll method).
[0106] 2) Step of forming the protrusion 12 Next, convex portions are formed on both widthwise ends of the obtained film base 11.
[0107] The formation of the convex portion may be performed by any method depending on the type of material, and may be performed by melt casting or solution casting. For example, the formation of the convex portion containing the second resin composition containing a cycloolefin resin is preferably performed by melt casting; the formation of the convex portion containing the crosslinked product of the crosslinkable composition containing a polymer having a functional group is preferably performed by solution casting.
[0108] <When the second resin composition is used> A second resin composition containing a cycloolefin resin is melt-cast onto both widthwise ends of the film base 11, and then cooled and solidified to form convex portions.
[0109] The melt casting can be performed in the same manner as described above. In particular, the melting temperature T2 of the second resin composition during melt casting is preferably the same as or higher than the melting temperature T1 of the first resin composition during melt casting. This is because when T2 is the same as or higher than T1, the adhesion of the convex portion 12 to the film base 11 is easily increased. Specifically, when the difference (T1-Tg1) between the melting temperature T1 of the first resin composition and the Tg1 of the cycloolefin resin of the first resin composition is ΔT1, and the difference (T2-Tg2) between the melting temperature T2 of the second resin composition and the Tg2 of the cycloolefin resin of the second resin composition is ΔT2, it is preferable that ΔT2-ΔT1≧20°C is satisfied, and more preferably ΔT2-ΔT1≧40°C is satisfied.
[0110] This is presumably due to the following phenomenon. When the melting temperature T1 of the first resin composition during film formation is relatively low, the fluidity of the cycloolefin resin decreases, and the packing of the polymer chains becomes difficult to proceed. As a result, the density of the obtained film base 11 becomes low (the gaps between the polymer chains increase), and the penetration of the cycloolefin resin of the second resin composition (constituting the protrusions 12) and the entanglement of the polymer chains are likely to occur, which is presumably why the adhesion is improved. Furthermore, when the melting temperature T2 of the second resin composition is relatively high, the fluidity of the cycloolefin resin increases, facilitating penetration into the film base 11 and entanglement of the cycloolefin resin with itself, which tends to improve adhesion.
[0111] The melting temperature T2 is preferably (Tg2+110) to (Tg2+170)°C. When the melting temperature T2 is (Tg2+110)°C or higher, the fluidity during extrusion is good, and when the melting temperature T2 is (Tg2+170)°C or lower, not only is quality deterioration due to thermal deterioration of the resin unlikely to occur, but also deterioration in adhesion due to deterioration in strength of the protrusions and the resulting winding deviation can be sufficiently suppressed. From the same viewpoint, the melting temperature T2 is more preferably (Tg2+135) to (Tg2+160)°C.
[0112] The second resin composition thus cast is then cooled and solidified. The cooling method and the cooling temperature may be the same as those for the first resin composition.
[0113] <When a crosslinkable composition is used> First, it is preferable to subject the surface of the film base 11 onto which the crosslinkable composition is to be applied to an activation treatment.
[0114] The activation treatment is preferably a treatment for imparting polar groups such as hydroxyl groups to the surface of the film base 11. This makes it possible to react with the polymer contained in the crosslinkable composition, and enhances the adhesion between the film base 11 and the protrusions 12.
[0115] Examples of the activation treatment include corona treatment, plasma treatment and saponification treatment, preferably corona treatment and plasma treatment, more preferably corona treatment.
[0116] The conditions of the activation treatment are not particularly limited as long as they can increase the adhesion of the protrusions 12. For example, in the case of corona treatment, the irradiation amount is 200 to 1000 (W·min / m 2 ), and 300 to 900 (W·min / m 2 ) is more preferable.
[0117] Next, a crosslinkable composition containing a polymer having a functional group is applied to the activation-treated surfaces at both ends in the width direction of the film base 11.
[0118] (Crosslinkable composition) The crosslinkable composition contains the polymer having the functional group. From the viewpoint of reducing the environmental load, the crosslinkable composition is preferably an aqueous dispersion in which the polymer is dispersed in water or a water-soluble organic solvent.
[0119] Examples of the water-soluble organic solvent include alcohols (straight-chain or branched-chain alcohols having 1 to 4 carbon atoms, such as methanol, ethanol, n-propanol, iso-propanol, n-butanol, sec-butanol, and tert-butanol). Among these, methanol and ethanol are preferred from the viewpoints of stability and drying properties.
[0120] The aqueous dispersion can be prepared by synthesizing the medium and dispersing it in water by a standard method, or a commercially available product can be used. For example, aqueous dispersions of polyurethane resins include Superflex 830, 460, 870, 420, 420NS (product names: polyurethanes manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), Bondic 1370NS, 1320NS (product names: polyurethanes manufactured by Dainippon Ink and Chemicals, Inc.), Olester UD-350, Takenate WD220 (product names: polyurethanes manufactured by Mitsui Chemicals, Inc.), and the like.
[0121] The resin concentration of the crosslinkable composition is preferably 70% by mass or less, and more preferably 10 to 50% by mass.
[0122] (Grant) The crosslinkable composition can be applied by any method, for example, casting using a die (preferably a reduced pressure die) or coating using a dispenser.
[0123] (Dry) The crosslinkable composition can be dried by any method, for example, hot air drying or heating and drying by electromagnetic waves.
[0124] The drying temperature is not particularly limited, but is preferably moderately high. Specifically, the drying temperature may be a temperature at which the solvent (including water) contained in the crosslinkable composition can be volatilized and removed, and is preferably, for example, 40 to 250°C, and more preferably 40 to 200°C.
[0125] In this way, polar groups such as hydroxyl groups may be generated on the surface of the activated film base 11. By applying a crosslinkable composition containing a polymer having a functional group that reacts with the polar group to such a treated surface, it is presumed that the polar group on the film base 11 will bond with the functional group of the polymer, thereby enhancing the adhesion between the film base 11 and the protrusions 12. During drying, the urethane oligomers also polymerize with each other to form a urethane resin, which provides many reaction sites with the polymer chains of the cycloolefin resin that constitutes the film base 11, which is believed to further increase the adhesion between the layers.
[0126] As a result, a film 10 is obtained that has a film base 10 and protruding portions 12 disposed at both ends in the width direction of the film base 10. The obtained film 10 is wound up in a roll shape along the longitudinal direction.
[0127] 3) Winding process The obtained film base 11 is wound up in the longitudinal direction (direction perpendicular to the width direction) of the film 10 using a winding machine. This makes it possible to obtain the film wound up in a roll around a core, i.e., a roll of the film 10.
[0128] The winding method is not particularly limited, and may be a constant torque method, a constant tension method, a taper tension method, or the like.
[0129] The winding tension when winding the film base 11 can be about 50 to 170 N. The longer the winding length, the greater the total amount of air stored between the film particles when viewed as a whole roll when wound into a roll, and the more likely it is that the air will be released and the film will shift when wound. Even in such a case, the adhesion of the protrusions 12 to the film base 11 can be increased by adjusting the composition of the protrusions 12 and the conditions for forming the protrusions 12, thereby preventing the protrusions 12 from peeling off or shifting when wound.
[0130] When the obtained film 10 is used, the portion where the convex portion 12 is formed is removed, and the film 10 is used as an optical film for a display device such as a liquid crystal display device or an organic EL display device. Examples of optical films include polarizing plate protective films (including retardation films and brightness enhancement films), transparent substrate films, and light diffusion films. Among these, the film 10 is preferably used as a polarizing plate protective film.
[0131] 3. Film and its manufacturing method As described above, the film of the present invention may be a belt-shaped film or a roll thereof, or may be a sheet-shaped film cut from a belt-shaped film. That is, the film of the present invention may be a film cut from the roll 10 of the present invention.
[0132] As described above, such a film has a film base (corresponding to the above-mentioned film base 11) and band-shaped convex portions (corresponding to the above-mentioned convex portions 12) provided at both ends in the width direction of the film base.
[0133] The shape, height T, width W, and material of the protrusions in the cross section of the film perpendicular to the direction in which the belt-like protrusions extend are as described above. The shape (no recesses) of the film base 11, the thickness of the film base, and the material of the film base are also as described above.
[0134] Such a film can be produced by a method similar to the method for producing the roll body described above, except that it does not include the winding step 3) above, or it further includes a step of cutting out the strip-shaped film unwound from the roll body after the winding step 3) above.
[0135] [Variations] In the above embodiment, the protrusions 12 are arranged continuously along the longitudinal direction of the film base 11, but the present invention is not limited to this. For example, the protrusions 12 may be arranged intermittently along the longitudinal direction of the film base 11.
[0136] In the above embodiment, one protrusion 12 is disposed on each of both ends in the width direction of the film base 11, but the present invention is not limited to this, and a plurality of protrusions may be disposed on each end.
[0137] Furthermore, in the above embodiment, an example has been shown in which the protrusions 12 are disposed on only one surface of the film base 11, but this is not limiting, and the protrusions 12 may be disposed on both surfaces.
[0138] In the above embodiment, the film base 11 is formed by melt casting, but the present invention is not limited to this, and the film base 11 may be formed by solution casting. EXAMPLES
[0139] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0140] 1. Material Preparation <Preparation of Cycloolefin Resin 1 Pellets> (polymerization) Under a nitrogen atmosphere, 5.0 parts by mass of tetracyclo[4.4.0.12,5.17,10]dodec-3-ene (TCD) and 5.0 parts by mass of tricyclo[4.3.0.12,5]deca-3,7-diene (DCP) were dissolved in 300 parts by mass of cyclohexane, and 0.30 parts by mass of 1-hexene was added as a molecular weight regulator. A mixture of 1.1 parts by mass of a 10% by mass solution of triisobutylaluminum in cyclohexane and 0.043 parts by mass of isobutyl alcohol was added to this solution. While keeping this solution at 40°C, 45.0 parts by mass of TCD, 45.0 parts by mass of DCP, and 11 parts by mass of a 0.6% by mass solution of tungsten hexachloride in cyclohexane were continuously added over a period of 2 hours to polymerize. 0.067 parts by weight of butyl glycidyl ether and 0.20 parts by mass of isopropyl alcohol were added to the polymerization solution to inactivate the polymerization catalyst. The polymerization conversion was 100%, and the weight ratio of TCD / DCP in the polymer was 50 / 50.
[0141] (Hydrogenation) To 200 parts by mass of the polymerization reaction solution, 2.4 parts by mass of a diatomaceous earth-supported nickel catalyst (Nissan Girdler; G-96D, nickel support rate 58% by mass) and 20 parts by mass of cyclohexane were added, and the mixture was stirred in a pressure-resistant reactor at 170°C and a hydrogen pressure of 45 kgf / cm. 2 The hydrogenation reaction was carried out at 200°C for 2 hours. This solution was filtered using a pressure filter (Ishikawajima-Harima Heavy Industries, Ltd., leaf filter) with diatomaceous earth as a filter aid to remove the catalyst. 200 parts by mass of the reaction solution containing the obtained polymer hydrogenation product was poured into 400 parts by mass of isopropyl alcohol under stirring to precipitate the hydrogenation product, which was then filtered and recovered. After washing with 200 parts by weight of acetone, the product was dried at 100°C for 24 hours in a vacuum dryer reduced to 1 mmHg or less to obtain 23 parts by mass of a norbornene ring-opening polymer hydrogenation product (cycloolefin resin 1). The remainder of the reaction solution containing cycloolefin resin 1 was stored at 25°C under a nitrogen atmosphere. The weight average molecular weight of the obtained cycloolefin resin 1 was 50,000 (in cyclohexane, polyisoprene equivalent), the glass transition temperature was 130°C, and the hydrogenation rate was 99.9% or more.
[0142] (Pellet preparation) To 100 parts by mass of cycloolefin resin 1, 0.1 parts by weight of tetrakis(methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenylpropionate)methane was added as an antioxidant, and the mixture was melt-kneaded at a cylinder temperature of 240°C using a twin-screw extruder (Toshiba Machine Co., Ltd., TEM-35B), extruded from a die in the form of strands, and cut using a pelletizer to obtain 95 parts by mass of pellets of cycloolefin resin 1.
[0143] <Preparation of Pellets of Cycloolefin Resins 2 to 5> The charge amount, reaction conditions and purification conditions were adjusted so that the weight average molecular weight of the resulting cycloolefin resin would be the value shown in Table 1, and pellets of cycloolefin resins 2 to 5 were obtained.
[0144] <Preparation of Water Dispersion of Urethane Resin 1> In a 2000 ml four-neck flask equipped with a thermometer, a stirrer, a nitrogen inlet tube and a cooling tube, 840 g of polyester polyol Maximol FSK-2000 (manufactured by Kawasaki Chemical Industries, Ltd., hydroxyl value 56 mg KOH / g), 119 g of tolylene diisocyanate as a polyvalent isocyanate component, and 200 g of methyl ethyl ketone as a solvent were placed, and reacted at 75 ° C for 1 hour while introducing nitrogen. After the reaction was completed, it was cooled to 60 ° C, and 35.6 g of dimethylolpropionic acid was added to introduce an acid structure, and reacted at 75 ° C to obtain an aqueous urethane resin solution having an acid structure with an isocyanate group content of 0.5%. Next, this acid structure-containing aqueous urethane resin solution was cooled to 40 ° C, and 1500 g of water and 10.6 g of sodium hydroxide as a neutralizing agent were added, and emulsification was performed by high-speed stirring with a homomixer. Methyl ethyl ketone was distilled off from this emulsion under heating and reduced pressure, and then water was added thereto so that the solid content concentration became 40%, followed by neutralization treatment, whereby an aqueous dispersion of urethane resin 1 was obtained.
[0145] <Preparation of Water Dispersions of Urethane Resins 2 to 4> The amounts of ingredients, reaction conditions and purification conditions were adjusted so that the weight average molecular weight of the resulting urethane resin would be the value shown in Table 1, thereby obtaining aqueous dispersions of urethane resins 2 to 4.
[0146] <Modified olefin resin> An ethylene-acrylic acid copolymer (Mw: 100,000) having a carboxyl group was synthesized by a standard method (see the examples in JP 2003-119328 A), and an aqueous dispersion was prepared by combining it with water so that the solid concentration was 40% (content of the above polymer in the solid content: 99%).
[0147] <Preparation of acrylic resin pellets> Polymethyl methacrylate (Mw: 200,000) synthesized by a conventional method was dried at 70°C under reduced pressure in a vacuum Nauta mixer for 3 hours, and then cooled to room temperature. This was melt-kneaded at 235°C in a twin-screw extruder and extruded into a strand shape. The molten material extruded into a strand shape was water-cooled and then cut to obtain pellets of acrylic resin.
[0148] <Preparation of polyester pellets> Polyethylene terephthalate (Mw: 70,000) synthesized by a conventional method was dried at 70°C under reduced pressure in a vacuum Nauta mixer for 3 hours, and then cooled to room temperature. This was melt-kneaded at 270°C in a twin-screw extruder and extruded into a strand shape. The molten material extruded into a strand shape was water-cooled and then cut to obtain polyester pellets.
[0149] <Preparation of polyvinyl acetal> Polyvinyl acetal (Mw: 80,000) was synthesized by a standard method, and mixed with a mixed solvent of water and ethanol (water:ethanol = 50 mass %: 50 mass %) to prepare a solution with a solid concentration of 40%.
[0150] The physical properties of the obtained resin are shown in Table 1.
[0151] [Table 1]
[0152] 2. Preparation of the roll body <Preparation of Roll Body 1-1> (Preparation of film base) The obtained pellets of cycloolefin resin 1 were fed into a single-screw extruder and melt-kneaded at 240°C under a nitrogen atmosphere. Then, the pellets were extruded from the die onto a first cooling roll having a surface temperature of 90°C. Then, the resin extruded onto the first cooling roll was pressed with a touch roll. The surface temperature of the touch roll was set to 80°C. Then, the obtained resin was further cooled and solidified on the second and third cooling rolls to obtain a film. The obtained film was stretched 1.4 times in the conveying direction (MD direction) at 150°C by zone stretching and 1.5 times in the width direction (TD direction) at 150°C by tenter stretching to adjust the film thickness to 40 μm, and then slit to obtain Film 1 (film base) with a width of 2000 mm and a roll length of 4000 m.
[0153] (Formation of protrusions) First, a cellulose resin solution was prepared according to the description of Experiment 1 (paragraph 0079) of JP 2012-206312 A.
[0154] The obtained cellulose resin solution was cast using a die and then solidified by applying dry air at 80°C to form continuous convex portions along the length of the film 1 on both ends in the width direction of the prepared film 1. The height of the convex portions was 1 μm, and the width of the convex portions was 15 mm.
[0155] <Preparation of Roll Body 1-2> (Preparation of film base) A film 1 was prepared in the same manner as in the roll body 1-1.
[0156] (Formation of protrusions) Acrylic resin pellets were placed in a single-screw extruder and melt-kneaded at 250° C. in a nitrogen atmosphere. On the other hand, the film 1 (film base) prepared above was slit to a predetermined width, and then both ends in the width direction were heated to 90°C for 5 seconds or more with a heat gun. Next, melt-kneaded acrylic resin was extruded from a die onto both ends in the width direction of the heated film 1, and the molten resin was pressed from above and below with touch rolls to adjust the width to 15 mm and the thickness to 1 μm, and cooled with cooling air to form continuous convex portions. The convex portions were formed on one side of the film 1. Thereafter, the obtained film was wound around a core to obtain a roll body with a winding length of 4000 m.
[0157] <Preparation of Roll Body 1-3> (Preparation of film base) A film 1 was prepared in the same manner as in the roll body 1-1.
[0158] (Formation of protrusions) Pellets of polyethylene terephthalate (PET) were charged into a single screw extruder and melt-kneaded at 280°C under a nitrogen atmosphere. On the other hand, the film 1 (film base) prepared above was slit to a predetermined width, and then both widthwise ends of the film 1 were heated to 120°C for 5 seconds or more with a heat gun. Convex portions were formed on both widthwise ends of the heated film 1 in the same manner as for roll body 1-2, except that molten kneaded polyethylene terephthalate was extruded from a die, and the film was wound up to obtain a roll body with a winding length of 4,000 m.
[0159] <Preparation of Roll Body 1-4> (Preparation of film base) A film 1 was prepared in the same manner as in the roll body 1-1.
[0160] (Formation of protrusions) A polyvinyl acetal solution was used, and convex portions were formed in the same manner as in roll body 1-1, except that the drying temperature was 95° C., to obtain a roll body having a wound length of 4,000 m.
[0161] <Preparation of Roll Body 1-5> (Preparation of film base) A film 1 was prepared in the same manner as in the roll body 1-1.
[0162] (Formation of protrusions) Pellets of cycloolefin resin 1 were placed in a single-screw extruder and melt-kneaded at 260°C (Tg+130°C) in a nitrogen atmosphere. On the other hand, the prepared film 1 (film base) was slit to a predetermined width, and then both widthwise ends of the film 1 were heated to 125°C for 5 seconds or more with a heat gun. Convex portions were formed on both widthwise ends of the heated film 1 in the same manner as for roll body 1-2, except that molten kneaded cycloolefin resin 1 was extruded from a die, and the film was wound up to obtain a roll body with a winding length of 4000 m.
[0163] <Preparation of Roll Body 1-6> (Preparation of film base) A film 1 was prepared in the same manner as in the roll body 1-1.
[0164] (Formation of protrusions) First, the surface of both ends in the width direction of the prepared film 1 (film base) was subjected to a corona discharge treatment (activation treatment). At this time, the electron irradiation dose in the corona discharge was 500 W / m 2 / min.
[0165] Next, the aqueous dispersion of the urethane resin 1 was cast using a die onto the corona discharge-treated surface of the film 1, and applied to a width of 15 mm and a thickness of 1 μm after drying, and then dried at 95° C. to form convex portions. The film obtained was then wound up to obtain a roll having a length of 4000 m.
[0166] <Preparation of Roll Body 1-7> (Preparation of film base) A film 1 was prepared in the same manner as in the roll body 1-1.
[0167] (Formation of protrusions) Next, silica particles were added to the aqueous dispersion of the urethane resin 1 so that the amount was 4% by mass relative to the resin, to obtain a dispersion liquid.
[0168] Convex portions were formed in the same manner as in Roll 1-6, except that the dispersion prepared above was applied to the corona discharge treated surface of the prepared Film 1 (film base), and the film was wound up to obtain a roll with a wound length of 4000 m.
[0169] <Preparation of Roll Body 1-8> (Preparation of film base) A film 1 was prepared in the same manner as in the roll body 1-1.
[0170] (Formation of protrusions) Convex portions were formed on both widthwise ends of the prepared film 1 (film base) in the same manner as in roll body 1-6, except that an aqueous dispersion of ethylene-acrylic acid copolymer was used as the modified polyolefin, and the film was wound up to obtain a roll body with a winding length of 4,000 m.
[0171] <Evaluation> The obtained roll bodies 1-1 to 1-8 were evaluated for winding misalignment and adhesion of the protrusions by the following methods.
[0172] (1) Winding misalignment The obtained roll body was stored at a temperature of 40°C and a humidity of 80% for about 10 days, and then subjected to a vibration test at 5.8 m / s 2 An acceleration of 100000 was applied in the width direction for 30 minutes, and the amount of left and right deviation was measured. The vibration tester used was a TR1000 made by IMV Corporation. Evaluation was based on the following criteria. ◎: The amount of misalignment is less than 1 mm, and no misalignment occurs ○: The amount of misalignment is between 1mm and 2mm, and there is almost no misalignment. △: The amount of misalignment is between 2 mm and 4 mm, and there is a slight misalignment, but it is not a problem for practical use. ×: The amount of misalignment is 4 mm or more, and misalignment occurs in the winding, to a level that is problematic in practical use. If it was rated △ or better, it was judged to be good.
[0173] (2) Adhesion of protruding parts After the evaluation of winding misalignment, the film was unwound from the roll, and the remaining 100 m of the film between 300 m and 200 m of the core was visually inspected for the presence or absence of any portions where the protrusions had peeled off from the base of the film. The evaluation was based on the following criteria. ◎: No peeling ○: Peeling is not a problem in 1 or 2 places △: Peeling occurred in 3 to 4 places, no practical problems ×: Peeling occurred in 5 or more places, which is a practical problem. If it was rated △ or better, it was judged to be good.
[0174] Table 2 shows the evaluation results of the roll bodies 1-1 to 1-8.
[0175] [Table 2]
[0176] As shown in Table 2, it is understood that the rolls 1-5 to 1-8 in which the protrusions are made of cycloolefin resin, polyurethane resin or modified polyolefin have good adhesion of the protrusions and little winding misalignment.
[0177] In contrast, it is found that the rolls 1-1 to 1-4, in which the protrusions are made of cellulose resin, acrylic resin, or polyester resin, have low adhesion at the protrusions and also suffer from winding misalignment.
[0178] <Preparation of Roll Bodies 2-1 to 2-6> Convex portions were formed on both widthwise ends of the above-mentioned film 1 in the same manner as in roll body 1-5, except that the weight-average molecular weight Mw1 of the resin constituting the film base (first resin composition) and the weight-average molecular weight Mw2 of the resin constituting the convex portions (second resin composition) were changed as shown in Table 3, to obtain a roll body.
[0179] <Preparation of Roll Bodies 2-7 to 2-13> Convex portions were formed on both widthwise ends of the above film 1 in the same manner as in roll body 1-5, except that the melting temperature T1 (°C) when forming the film base (first resin composition) and the melting temperature T2 (°C) when forming the convex portions (second resin composition) were changed as shown in Table 3, to obtain a roll body.
[0180] <Preparation of Roll Bodies 3-1 to 3-4> Convex portions were formed on both widthwise ends of the above-mentioned film 1 in the same manner as in roll body 1-5, except that the type and weight average molecular weight Mw3 of the resin constituting the convex portions (second resin composition) were changed as shown in Table 4, to obtain a roll body.
[0181] The obtained roll bodies were evaluated for winding slippage and adhesion by the same methods as described above. The evaluation results of roll bodies 2-1 to 2-13 are shown in Table 3, and the evaluation results of roll bodies 3-1 to 3-4 are shown in Table 4.
[0182] [Table 3]
[0183] [Table 4]
[0184] As shown in Table 3, when the resin constituting the convex portions is a cycloolefin resin, by making Mw2 smaller than Mw1, the adhesion of the convex portions of the roll body is further improved and the winding misalignment is further reduced (comparison of roll bodies 2-1 to 2-6).
[0185] In addition, by making the melting temperature T2 when forming the convex portions higher than the melting temperature T1 when forming the film base, it can be seen that the adhesion of the convex portions of the roll body is further improved and winding misalignment is further reduced (comparison of roll bodies 2-7 to 2-13).
[0186] On the other hand, as shown in Table 4, when the resin constituting the convex portions is a urethane resin, by making Mw3 larger than Mw1, the adhesion of the convex portions of the roll body is further improved and the winding misalignment is further reduced (comparison of roll bodies 3-1 to 3-4). [Industrial Applicability]
[0187] According to the present invention, it is possible to provide a belt-shaped film roll having protrusions that have high adhesion to the film base and that can suppress peeling of the protrusions and the resulting misalignment of the film, and a method for manufacturing the same. [Explanation of symbols]
[0188] 10 Strip of film 11 Film base 12 Convex part
Claims
1. A roll body obtained by winding a strip-shaped film in a direction perpendicular to the width direction of the film, The film has a base portion and protruding portions provided at both ends in a width direction of the base portion, The film base includes a first resin composition including a cycloolefin resin, the protrusions include a second resin composition including a cycloolefin resin, The weight average molecular weight Mw2 of the cycloolefin resin contained in the second resin composition is smaller than the weight average molecular weight Mw1 of the cycloolefin resin contained in the first resin composition. Roll body.
2. (Mw1-Mw2) is 10,000 or more; The roll body according to claim 1 .
3. The thickness of the film base is 10 to 40 μm. The roll body according to claim 1 or 2.
4. The film base is an optical film. The roll body according to any one of claims 1 to 3.
5. A method for manufacturing a roll body by winding a strip-shaped film along a direction perpendicular to the width direction of the film, comprising the steps of: 1) a step of melt-casting a first resin composition containing a cycloolefin resin, followed by cooling and solidifying the first resin composition to obtain a strip-shaped film base; 2) forming convex portions of the second resin composition on the surface of the strip-shaped film base by melt-casting a second resin composition containing a cycloolefin resin onto both widthwise ends of the strip-shaped film base and cooling and solidifying the second resin composition; Including, The melting temperature T2 of the second resin composition during the melt casting is higher than the melting temperature T1 of the first resin composition during the melt casting. A method for manufacturing a roll body.
6. When the glass transition temperature of the cycloolefin resin contained in the first resin composition is Tg1 and the glass transition temperature of the cycloolefin resin contained in the second resin composition is Tg2, The melting temperature T1 is (Tg1+90) to (Tg1+150) ° C. The melting temperature T2 is (Tg2+110) to (Tg2+170) ° C. A method for producing the roll body according to claim 5 .
7. A method for manufacturing a roll body by winding a strip-shaped film along a direction perpendicular to the width direction of the film, comprising the steps of: 1) a step of melt-casting a first resin composition containing a cycloolefin resin, followed by cooling and solidifying the first resin composition to obtain a strip-shaped film base; 2) A step of melt-casting a second resin composition containing a cycloolefin resin onto both widthwise ends of the strip-shaped film base, followed by cooling and solidifying the composition to form convex portions. Including, a melting temperature T2 of the second resin composition during the melt casting is equal to or higher than a melting temperature T1 of the first resin composition during the melt casting, When the glass transition temperature of the cycloolefin resin contained in the first resin composition is Tg1 and the glass transition temperature of the cycloolefin resin contained in the second resin composition is Tg2, The melting temperature T1 is (Tg1+90) to (Tg1+150) ° C. The melting temperature T2 is (Tg2+110) to (Tg2+170) ° C., When T1-Tg1 is ΔT1 and T2-Tg2 is ΔT2, (ΔT2-ΔT1) is 20° C. or more. A method for manufacturing a roll body.
8. A method for manufacturing a roll body by winding a strip-shaped film along a direction perpendicular to the width direction of the film, comprising the steps of: 1) a step of melt-casting a first resin composition containing a cycloolefin resin, followed by cooling and solidifying the first resin composition to obtain a strip-shaped film base; 2) A step of melt-casting a second resin composition containing a cycloolefin resin onto both widthwise ends of the strip-shaped film base, followed by cooling and solidifying the composition to form convex portions. Including, a melting temperature T2 of the second resin composition during the melt casting is equal to or higher than a melting temperature T1 of the first resin composition during the melt casting, The weight average molecular weight Mw2 of the cycloolefin resin contained in the second resin composition is smaller than the weight average molecular weight Mw1 of the cycloolefin resin contained in the first resin composition. A method for manufacturing a roll body.
9. (Mw1-Mw2) is 10,000 or more; The method for producing the roll body according to claim 8 .
10. A film having a base portion and band-shaped convex portions provided at both ends thereof, The film base includes a first resin composition including a cycloolefin resin, the protrusions include a second resin composition including a cycloolefin resin, The weight average molecular weight Mw2 of the cycloolefin resin contained in the second resin composition is smaller than the weight average molecular weight Mw1 of the cycloolefin resin contained in the first resin composition. film.
11. A method for producing a film having a base film and band-shaped convex portions provided at both ends thereof, comprising the steps of: 1) a step of melt-casting a first resin composition containing a cycloolefin resin, followed by cooling and solidifying the first resin composition to obtain a strip-shaped film base; 2) forming convex portions of the second resin composition on the surface of the strip-shaped film base by melt-casting a second resin composition containing a cycloolefin resin onto both ends of the strip-shaped film base and cooling and solidifying the second resin composition; Including, The melting temperature T2 of the second resin composition during the melt casting is higher than the melting temperature T1 of the first resin composition during the melt casting. A method for manufacturing a film.
Citation Information
Patent Citations
Optical film, optical film roll, and method for manufacturing optical film
JP2012118238A
Method for forming knurling, device for forming knurling, method for forming film using solution and polymer film
JP2012206312A
Protection film laminate
JP2017121777A
Film for molding
WO2014103988A1
Long film
WO2017145718A1