Electrophotographic photoreceptor, process cartridge, and image forming apparatus
Fluorine-containing resin particles with controlled carboxyl and basic compound levels improve charging stability and chargeability, addressing fogging and image density issues in electrophotographic photoreceptors.
Patent Information
- Application Number
- JP2023137377
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-07
- Filing Date
- 2023-08-25
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2039-09-24
AI Technical Summary
Conventional fluorine-containing resin particles contain carboxyl groups or basic compounds in excess amounts, leading to unstable charging characteristics, which result in issues such as fogging and decreased image density in electrophotographic photoreceptors.
Fluorine-containing resin particles are developed with controlled amounts of carboxyl groups (0 to 30 per particle) and basic compounds (0 to 3 ppm), produced without radiation irradiation, and formulated into a composition or layered material for improved chargeability.
The resin particles exhibit enhanced charging stability and chargeability, reducing fogging and maintaining image density in high-temperature, high-humidity environments.
Smart Images

Figure 0007556444000025 
Figure 0007556444000023 
Figure 0007556444000024
Abstract
Description
[Technical field]
[0001] The present invention relates to a fluorine-containing resin particle, a composition, a layered product, an electrophotographic photoreceptor, a process cartridge, and an image-forming apparatus. [Background technology]
[0002] Fluorine-containing resin particles are widely used, for example, as lubricants, etc. The fluorine-containing resin particles include particles obtained by irradiation with radiation, particles obtained by polymerization, and the like.
[0003] For example, Patent Document 1 discloses "an electrophotographic photoreceptor containing fluorine atom-containing resin particles in a photosensitive layer."
[0004] Furthermore, Patent Document 2 describes a process for producing a polytetrafluoroethylene having a complex viscosity of 1×10 at 380° C. by irradiating the polytetrafluoroethylene with radiation. The process includes the steps of: (1) charging polytetrafluoroethylene, at least one additive selected from the group consisting of hydrocarbons, chlorinated hydrocarbons, alcohols, and carboxylic acids (excluding perfluorocarboxylic acids having 8 to 14 carbon atoms), and at least one additive selected from the group consisting of inert gases (excluding the additives) and oxygen adsorbents into a sealed container; and (2) irradiating the polytetrafluoroethylene with radiation so that the complex viscosity of the polytetrafluoroethylene is 1×10 at 380° C. 2 ~7×10 5 "A method for producing low-molecular-weight polytetrafluoroethylene, comprising the step (2) of obtaining low-molecular-weight polytetrafluoroethylene having a molecular weight of 1.0 Pa·s."
[0005] In addition, Patent Document 3 states that "polytetrafluoroethylene was irradiated with radiation to obtain a melt viscosity of 1×10 at 380°C. 2 ~7×10 5 The document discloses a method for producing low-molecular-weight polytetrafluoroethylene, comprising: a step (1) of obtaining low-molecular-weight polytetrafluoroethylene having a molecular weight of Pa·s; a step (2) of pulverizing the low-molecular-weight polytetrafluoroethylene; and a step (3) of heat-treating the low-molecular-weight polytetrafluoroethylene pulverized in the step (2).
[0006] Furthermore, Patent Document 4 discloses "a low-molecular-weight polytetrafluoroethylene powder characterized in that it has a 50% average particle size of 3 μm or less as measured by a dry laser, contains powder with a particle size of 1 μm or less, has a melt viscosity of 2500 Pa s or less as measured by a flow tester method at 340°C, and is obtained by suspension polymerization."
[0007] Furthermore, Patent Document 5 discloses "a method for producing an ultrafine powder of crosslinked polytetrafluoroethylene resin, comprising the steps of: (a) irradiating a mixed solution of tetrafluoroethylene monomer and acetone with ionizing radiation to polymerize the monomer, thereby forming the solution into a gel-state dispersion of polytetrafluoroethylene in an acetone solvent; (b) separating a fine powder of polytetrafluoroethylene from the dispersion; and (c) irradiating the polytetrafluoroethylene fine powder with ionizing radiation to crosslink it." [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2009-104145 A [Patent Document 2] JP 2018-24869 A [Patent Document 3] JP 2018-24868 A [Patent Document 4] JP 2010-202741 A [Patent Document 5] JP 2000-026614 A Summary of the Invention [Problem to be solved by the invention]
[0009] Conventionally, fluorine-containing resin particles contain a carboxyl group or a basic compound due to the production method thereof, and therefore have the property that stable charging characteristics cannot be obtained due to the amount of these compounds. Therefore, the object of the present invention is to provide a method for producing a carboxyl group having 10 carbon atoms. 6 The object of the present invention is to provide fluorine-containing resin particles which have excellent electrostatic properties compared to those containing more than 30 particles per particle or containing more than 3 ppm of basic compound. [Means for solving the problem]
[0010] The above problems are solved by the following means.
[0011] <1> The number of carboxyl groups is 10 carbon atoms. 6 Fluorine-containing resin particles having 0 to 30 particles per particle and containing 0 ppm to 3 ppm of basic compounds. <2> The number of the carboxyl groups is 10 6 The number of basic compounds per particle is 0 to 20, and the amount of the basic compounds is 0 ppm to 3 ppm. <1> Fluorine-containing resin particles according to claim 1. <3> The amount of the carboxyl group is 10 6 The number of basic compounds per particle is 0 to 20, and the amount of the basic compounds is 0 ppm to 1.5 ppm. <1> Fluorine-containing resin particles according to claim 1. <4> The basic compound is an amine compound. <1> ~ <3> Fluorine-containing resin particles according to any one of claims 1 to 7. <5> The basic compound has a boiling point of 40° C. or higher and 130° C. or lower. <1> ~ <4> Fluorine-containing resin particles according to any one of claims 1 to 7. <6> The amount of perfluorooctanoic acid is between 0 ppb and 25 ppb. <1> ~ <5> Fluorine-containing resin particles according to any one of claims 1 to 7. <7> The amount of perfluorooctanoic acid is between 0 ppb and 20 ppb. <6> Fluorine-containing resin particles according to claim 1. <8> Obtained without irradiation during the manufacturing process <1> ~ <7> Fluorine-containing resin particles according to any one of claims 1 to 7. <9> <1> ~ <8> 2. A composition comprising the fluorine-containing resin particles according to claim 1. <10> Liquid or solid <9> The composition described in <11> <1> ~ <8> 2. A layered product comprising the fluorine-containing resin particles according to claim 1. <12> A conductive substrate and a photosensitive layer provided on the conductive substrate, The outermost surface layer is <11> 2. An electrophotographic photoreceptor comprising a layer made of the layered material according to claim 1. <13> The outermost layer contains a polycarbonate resin containing a structural unit represented by the following general formula (PCA) and a structural unit represented by the following general formula (PCB): <12> The electrophotographic photoreceptor according to claim 1. [ka] (In the general formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and R P4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 5 to 7 carbon atoms, or an aryl group having 6 to 12 carbon atoms. P1 represents a phenylene group, a biphenylene group, a naphthylene group, an alkylene group, or a cycloalkylene group. <14> The outermost surface layer contains a charge transport material having a butadiene structure and a triarylamine structure. <12> or <13> The electrophotographic photoreceptor according to claim 1. <15> a dispersant having fluorine atoms adhered to the surface of the fluorine-containing resin particles, The dispersant having a fluorine atom has a wave number of 1673 cm in an infrared absorption spectrum. -1 Wave number 1779cm -1 For peak areas in the range of 1020 cm -1Wave number 1308cm -1 The peak area ratio in the range is 2.7 to 4.8. <12> ~ <14> 13. The electrophotographic photoreceptor according to claim 12. <16> <12> ~ <15> The electrophotographic photoreceptor according to any one of claims 1 to 5, A process cartridge that is detachably attached to an image forming apparatus. <17> <12> ~ <15> The electrophotographic photoreceptor according to any one of the above items, a charging means for charging the surface of the electrophotographic photoreceptor; an electrostatic latent image forming means for forming an electrostatic latent image on the charged surface of the electrophotographic photoreceptor; a developing unit for developing an electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing a toner to form a toner image; a transfer means for transferring the toner image onto a surface of a recording medium; An image forming apparatus comprising: Effect of the Invention
[0012] <1> According to the invention, the number of carboxyl groups is 10 6 The fluorine-containing resin particles provided are excellent in charge stability, as compared with the case where the number of particles per particle exceeds 30 or the amount of the basic compound exceeds 3 ppm. <2> , <3> According to the invention, the number of carboxyl groups is 10 6 The fluorine-containing resin particles provided have excellent electrostatic properties compared to when the amount of the basic compound is more than 20 per particle or more than 3 ppm.
[0013] <4> or <5> According to the present invention, fluorine-containing resin particles having excellent charging properties are provided, as compared with a case in which the amount of an amine compound or a basic compound having a boiling point of 40° C. or more and 130° C. or less exceeds 3 ppm as a basic compound.
[0014] <6> or <7> According to the present invention, fluorine-containing resin particles having excellent electrostatic properties are provided, as compared with the case where the amount of perfluorooctanoic acid is more than 25 ppb.
[0015] <8> According to the present invention, there are provided fluorine-containing resin particles which are superior in electrostatic chargeability as compared with fluorine-containing resin particles which have been irradiated with radiation.
[0016] <9> According to the invention, the number of carboxyl groups is 10 6 The present invention provides a composition containing fluorine-containing resin particles that has excellent electrostatic chargeability, as compared with a composition containing fluorine-containing resin particles having more than 30 particles per particle or containing more than 3 ppm of basic compounds.
[0017] <10> or <11> According to the invention, the number of carboxyl groups is 10 6 The present invention provides a layered material containing fluorine-containing resin particles that has excellent electrostatic properties compared to the case where fluorine-containing resin particles having more than 30 particles per particle or an amount of basic compound exceeding 3 ppm are used. <12> According to the present invention, there is provided an electrophotographic photoreceptor having an outermost surface layer containing fluorine-containing resin particles having excellent electrostatic properties. <13> or <14> According to the invention, the number of carboxyl groups is 10 6 Compared to the case where more than 30 fluorine-containing resin particles are used per particle, an electrophotographic photoreceptor is provided in which density unevenness in granular images is suppressed even when a polycarbonate resin containing a structural unit represented by general formula (PCA) and a structural unit represented by general formula (PCB) is used as a binder resin. <15> According to the invention, the infrared absorption spectrum of a dispersant having a fluorine atom has a wave number of 1673 cm -1 Wave number 1779cm -1 For peak areas in the range of 1020 cm -1 Wave number 1308cm -1 In comparison with the case where the peak area ratio in the range is less than 2.8 or exceeds 4.8, an electrophotographic photoreceptor is provided which suppresses localized deterioration in cleaning performance. <16> or <17> According to the present invention, there is provided a process cartridge including an electrophotographic photoreceptor having an outermost surface layer containing fluorine-containing resin particles having excellent charging properties, or an image forming apparatus including the electrophotographic photoreceptor. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a schematic cross-sectional view illustrating an example of a layer structure of the electrophotographic photoreceptor according to the present embodiment. [Diagram 2] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic configuration diagram illustrating another example of an image forming apparatus according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment of the present invention will be described in detail.
[0020] (Fluorine-containing resin particles) The fluorine-containing resin particles according to the first embodiment have a carboxyl group having a carbon number of 10. 6 The number of particles per particle is between 0 and 30, and the amount of basic compounds is between 0 ppm and 3 ppm. The fluorine-containing resin particles according to this embodiment have the above-mentioned structure, and therefore have excellent charging properties.
[0021] Here, the fluorine-containing resin particles include particles obtained by irradiation with radiation (also referred to in this specification as "radiation-irradiated fluorine-containing resin particles"), particles obtained by polymerization (also referred to in this specification as "polymerization-type fluorine-containing resin particles"), etc.
[0022] The radiation-irradiated fluorine-containing resin particles (fluorine-containing resin particles obtained by irradiation with radiation) refer to fluorine-containing resin particles granulated during radiation polymerization, and fluorine-containing resin particles obtained by decomposing the polymerized fluorine-containing resin by irradiation to reduce the molecular weight and make it finer. The radiation-exposed fluorine-containing resin particles also contain a large amount of carboxyl groups because a large amount of carboxylic acid is produced by exposure to radiation in air.
[0023] On the other hand, the polymerized type fluorine-containing resin particles (fluorine-containing resin particles obtained by polymerization) refer to fluorine-containing resin particles which are granulated during polymerization by a suspension polymerization method, an emulsion polymerization method or the like and which are not irradiated with radiation. Polymerized fluorine-containing resin particles are produced by polymerization in the presence of a basic compound, and therefore contain the basic compound as a residue.
[0024] That is, conventional fluorine-containing resin particles contain a large amount of carboxyl groups or basic compounds.
[0025] When the fluorine-containing resin particles contain a large number of carboxyl groups, they exhibit ionic conductivity and therefore have the property of being difficult to be charged. For example, when conventional fluorine-containing resin particles containing a large amount of carboxyl groups are applied to the outermost surface layer of an electrophotographic photoreceptor, the chargeability of the photoreceptor decreases in a high-temperature and high-humidity environment, and a phenomenon in which toner adheres to non-image areas (hereinafter also referred to as "fogging") may occur.
[0026] On the other hand, if the fluorine-containing resin particles contain a large amount of a basic compound, the basic compound exhibits hole trapping properties, and therefore the particles become difficult to be charged. For example, when conventional fluorine-containing resin particles containing a large amount of a basic compound are applied to the outermost surface layer of an electrophotographic photoreceptor, the residual potential increases over time, which may result in a decrease in image density.
[0027] Therefore, the fluorine-containing resin particles according to the present embodiment have improved chargeability by restricting the amount of carboxyl groups and basic compounds to the above ranges. Note that, as long as the number of carboxyl groups and the amount of basic compounds are restricted within the above ranges, even if the number of carboxyl groups is somewhat large, as long as the amount of basic compounds is relatively large, the ionic conductivity and hole trapping property cancel each other out, and chargeability tends to improve. Therefore, for example, when the fluorine-containing resin particles according to this embodiment are applied to the outermost surface layer of an electrophotographic photoreceptor, the occurrence of fogging and a decrease in image density due to an increase in residual potential is suppressed.
[0028] The fluorine-containing resin particles according to the second embodiment are polymerized fluorine-containing resin particles, and contain a basic compound in an amount of 0 ppm or more and 3 ppm or less. The fluorine-containing resin particles according to the second embodiment are polymerized fluorine-containing resin particles, i.e., fluorine-containing resin particles which are granulated during polymerization by a suspension polymerization method, an emulsion polymerization method, or the like, and which are not irradiated with radiation, so that a large amount of carboxylic acid is not produced, and the carboxyl group is not present or is present in a small amount, and the amount of basic compound is also reduced. Therefore, the fluorine-containing resin particles according to the second embodiment also have high chargeability.
[0029] Hereinafter, the fluorine-containing resin particles according to this embodiment will be described in detail.
[0030] The fluorine-containing resin particles according to this embodiment do not contain a carboxyl group, or if they do contain a carboxyl group, the amount is small. 6 The number per particle is from 0 to 30, and from the viewpoint of improving the chargeability, the number is preferably from 0 to 20.
[0031] Here, the carboxyl group of the fluorine-containing resin particle is, for example, a carboxyl group derived from a terminal carboxylic acid contained in the fluorine-containing resin particle.
[0032] Methods for reducing the amount of carboxyl groups in fluorine-containing resin particles include 1) a method in which radiation is not applied during the particle production process, and 2) a method in which radiation is applied in the absence of oxygen or under conditions with a reduced oxygen concentration.
[0033] The amount of carboxyl groups in the fluorine-containing resin particles is measured as follows, as described in JP-A-4-20507. The fluorine-containing resin particles were preformed in a press to produce a film with a thickness of approximately 0.1 mm. The infrared absorption spectrum of the produced film was measured. The infrared absorption spectrum of the fluorine-containing resin particles, which were produced by contacting the fluorine-containing resin particles with fluorine gas to completely fluorinate the carboxylic acid terminals, was also measured, and the number of terminal carboxyl groups (10 carbon atoms) was calculated from the difference spectrum between the two using the following formula: 6 per piece) = (l × K) / t l: Absorbance K: Correction coefficient t: film thickness (mm) The absorption wave number of the carboxyl group is 3560 cm -1 , the correction coefficient is 440.
[0034] In the fluorine-containing resin particles according to the present embodiment, basic compound is not contained, or even if it is contained, it is a small amount. Specifically, the amount of basic compound in the fluorine-containing resin particles is 0 ppm or more and 3 ppm or less, and from the viewpoint of improving charging property, it is preferably 0 ppm or more and 1.5 ppm or less, and more preferably 0 ppm or more and 1.2 ppm or less. Here, ppm is based on mass.
[0035] Here, examples of the basic compound of the fluorine-containing resin particles include 1) a basic compound derived from a polymerization initiator used when forming the fluorine-containing resin particles into particles during polymerization, 2) a basic compound used in the step of aggregating the particles after polymerization, and 3) a basic compound used as a dispersion aid for stabilizing the dispersion after polymerization.
[0036] Examples of the basic compound include amine compounds, hydroxides of alkali metals or alkaline earth metals, oxides of alkali metals or alkaline earth metals, acetates, and the like (e.g., particularly amine compounds). The basic compound is, for example, a basic compound having a boiling point (boiling point under normal pressure (1 atmosphere)) of 40°C or higher and 130°C or lower (preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 90°C or lower).
[0037] The amine compound may be a primary, secondary, or tertiary amine compound. Examples of the primary amine compound include methylamine, ethylamine, propylamine, isopropylamine, n-butylamine, isobutylamine, t-butylamine, hexylamine, 2-ethylhexylamine, secondary butylamine, allylamine, and methylhexylamine.
[0038] Examples of secondary amine compounds include dimethylamine, diethylamine, di-n-propylamine, diisopropylamine, di-n-butylamine, diisobutylamine, di-t-butylamine, dihexylamine, di(2-ethylhexyl)amine, N-isopropyl-N-isobutylamine, di(2-ethylhexyl)amine, di-secondary butylamine, diallylamine, N-methylhexylamine, 3-pipecoline, 4-pipecoline, 2,4-lupetidine, 2,6-lupetidine, 3,5-lupetidine, morpholine, and N-methylbenzylamine.
[0039] Tertiary amine compounds include trimethylamine, triethylamine, tri-n-propylamine, triisopropylamine, tri-n-butylamine, triisobutylamine, tri-t-butylamine, trihexylamine, tri(2-ethylhexyl)amine, N-methylmorpholine, N,N-dimethylallylamine, N-methyldiallylamine, triallylamine, N,N-dimethylallylamine, N,N,N',N'-tetramethyl-1,2-diaminoethane, N,N,N',N'-tetramethyl-1,3-diaminopropane, N,N,N',N'-tetraallyl-1,4-diaminobutane, and N-methylpiperidine. , pyridine, 4-ethylpyridine, N-propyl diallylamine, 3-dimethylaminopropanol, 2-ethylpyrazine, 2,3-dimethylpyrazine, 2,5-dimethylpyrazine, 2,4-lutidine, 2,5-lutidine, 3,4-lutidine, 3,5-lutidine, 2,4,6-collidine, 2-methyl-4-ethylpyridine, 2-methyl-5-ethylpyridine, N,N,N',N'-tetramethylhexamethylenediamine, N-ethyl-3-hydroxypiperidine, 3-methyl-4-ethylpyridine, 3-ethyl-4-methylpyridine, 4-(5-nonyl)pyridine, imidazole, N-methylpiperazine, and the like.
[0040] Examples of hydroxides of alkali metals or alkaline earth metals include NaOH, KOH, Ca(OH)2, Mg(OH)2, Ba(OH)2, and the like. Examples of the oxides of alkali metals or alkaline earth metals include CaO and MgO. Examples of acetates include zinc acetate and sodium acetate.
[0041] Methods for reducing the amount of basic compounds in fluorine-containing resin particles include: 1) washing the particles with water, an organic solvent (alcohols such as methanol, ethanol, isopropanol, tetrahydrofuran, etc.) after production; and 2) heating the particles after production (for example, heating to 200°C or higher and 250°C or lower) to decompose or vaporize the basic compounds and remove them.
[0042] The amount of the basic compound in the fluorine-containing resin particles is measured as follows. -Pretreatment- When a layered material containing fluorine-containing resin particles is to be measured, the layered material is immersed in a solvent (e.g., tetrahydrofuran) and all substances other than the fluorine-containing resin particles and substances insoluble in the solvent are dissolved in the solvent (e.g., tetrahydrofuran), then the material is dropped into pure water and the precipitate is filtered off. The solution containing PFOA obtained at this time is collected. The insoluble matter obtained by filtration is further dissolved in a solvent, then the material is dropped into pure water and the precipitate is filtered off. This process is repeated five times to obtain fluorine-containing resin particles as a measurement sample. When a composition containing fluorine-containing resin particles is to be measured, the composition is subjected to the same treatment as in the case of the layered material to obtain fluorine-containing resin particles as a measurement sample. When the fluorine-containing resin particles themselves are to be measured, the fluorine-containing resin particles are subjected to the same treatment as in the case of the layered material to obtain fluorine-containing resin particles as a measurement sample.
[0043] -measurement- On the other hand, a basic compound solution (methanol solvent) with a known concentration is used, and a calibration curve (calibration curve from 0 ppm to 100 ppm) is obtained from the basic compound concentration and peak area value of the basic compound solution (methanol solvent) with a known concentration using gas chromatography. The measurement sample is then measured by gas chromatography, and the amount of the basic compound in the fluorine-containing resin particles is calculated from the obtained peak area and a calibration curve. The measurement conditions are as follows.
[0044] -Measurement conditions- Headspace sampler: (HP7694, manufactured by Hewlett-Packard Company) Measuring instrument: Gas chromatograph (HP6890 series, manufactured by HP) Detector: Flame ionization detector (FID) Column: HP19091S-433, manufactured by HP) Sample heating time: 10 min Split Ratio: 300:1 ·Flow rate: 1.0ml / min Column temperature setting: 60℃ (3min), 60℃ / min, 200℃ (1min)
[0045] In the fluorine-containing resin particles according to the present embodiment, from the viewpoint of improving the chargeability, the amount of perfluorooctanoic acid (hereinafter also referred to as "PFOA") is preferably 0 ppb or more and 25 ppb or less, more preferably 0 ppb or more and 20 ppb or less, and more preferably 0 ppb or more and 15 ppb or less, relative to the fluorine-containing resin particles. Here, "ppb" is based on mass.
[0046] Here, PFOA is used or generated as a by-product in the production process of fluorine-containing resin particles (particularly fluorine-containing resin particles such as polytetrafluoroethylene particles, modified polytetrafluoroethylene particles, and perfluoroalkyl ether / tetrafluoroethylene copolymer particles), and therefore fluorine-containing resin particles often contain PFOA. In addition, PFOA has a carboxyl group that causes a decrease in the electrostatic charge of the particles, and therefore, it is preferable that the fluorine-containing resin particles do not contain PFOA, or if they do contain it, the amount is small.
[0047] Methods for reducing the amount of PFOA include thoroughly washing fluorine-containing resin particles with pure water, alkaline water, alcohols (methanol, ethanol, isopropanol, etc.), ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.), esters (ethyl acetate, etc.), other common organic solvents (toluene, tetrahydrofuran, etc.), etc. Washing may be performed at room temperature, but it can be reduced more efficiently by performing it under heating.
[0048] The amount of PFOA is measured by the following method. -Sample pretreatment- When a layered material containing fluorine-containing resin particles is to be measured, the layered material is immersed in a solvent (e.g., tetrahydrofuran) and all substances other than the fluorine-containing resin particles and substances insoluble in the solvent are dissolved in the solvent (e.g., tetrahydrofuran), then the material is dropped into pure water and the precipitate is separated by filtration. The solution containing PFOA obtained at this time is collected. The insoluble matter obtained by filtration is further dissolved in a solvent, and the solution is dropped into pure water and the precipitate is separated by filtration. The process of collecting the solution containing PFOA obtained at this time is repeated five times, and the aqueous solution collected in all steps is regarded as a pretreated aqueous solution. When a composition containing fluorine-containing resin particles is to be measured, the composition is subjected to the same treatment as in the case of the layered material to obtain a pretreated aqueous solution. When the fluorine-containing resin particles themselves are to be measured, the fluorine-containing resin particles are subjected to the same treatment as in the case of the layered material to obtain a pretreated aqueous solution.
[0049] -measurement- The pretreated aqueous solution obtained by the above method is used to prepare and measure the sample solution in accordance with the method shown in "Analysis of Perfluorooctane Sulfone Acid (PFOS) and Perfluorooctane Acid (PFOA) in Environmental Water, Sediment, and Organisms, Iwate Prefectural Environmental Health Research Center."
[0050] Examples of the fluorine-containing resin particles according to this embodiment include particles of a fluoroolefin homopolymer, and particles of a copolymer of two or more types of fluoroolefins, that is, a copolymer of one or more types of fluoroolefins with a non-fluorine-based monomer (i.e., a monomer that does not have a fluorine atom).
[0051] Examples of fluoroolefins include perhaloolefins such as tetrafluoroethylene (TFE), perfluorovinyl ether, hexafluoropropylene (HFP), and chlorotrifluoroethylene (CTFE), and non-perfluoroolefins such as vinylidene fluoride (VdF), trifluoroethylene, and vinyl fluoride. Among these, VdF, TFE, CTFE, and HFP are preferred.
[0052] On the other hand, examples of non-fluorine-based monomers include hydrocarbon olefins such as ethylene, propylene, and butene; alkyl vinyl ethers such as cyclohexyl vinyl ether (CHVE), ethyl vinyl ether (EVE), butyl vinyl ether, and methyl vinyl ether; alkenyl vinyl ethers such as polyoxyethylene allyl ether (POEAE) and ethyl allyl ether; organic silicon compounds having reactive α,β-unsaturated groups such as vinyltrimethoxysilane (VSi), vinyltriethoxysilane, and vinyltris(methoxyethoxy)silane; acrylic acid esters such as methyl acrylate and ethyl acrylate; methacrylic acid esters such as methyl methacrylate and ethyl methacrylate; vinyl esters such as vinyl acetate, vinyl benzoate, and "Veova" (trade name, vinyl ester manufactured by Shell); and the like. Among these, alkyl vinyl ethers, allyl vinyl ethers, vinyl esters, and organic silicon compounds having reactive α,β-unsaturated groups are preferred.
[0053] Among these, as the fluorine-containing resin particles, particles with a high fluorination rate are preferred, and particles such as polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), and ethylene-chlorotrifluoroethylene copolymer (ECTFE) are more preferred, with PTFE, FEP, and PFA particles being particularly preferred.
[0054] The fluorine-containing resin particles according to the present embodiment are preferably polymerized fluorine-containing resin particles, which are granulated during polymerization by a suspension polymerization method, an emulsion polymerization method, or the like, and are not irradiated with radiation, as described above. Here, the production of fluorine-containing resin particles by the suspension polymerization method is, for example, a method in which additives such as a polymerization initiator and a catalyst are suspended together with a monomer for forming a fluorine-containing resin in a dispersion medium, and then the monomer is polymerized while the polymer is granulated. Furthermore, the production of fluorine-containing resin particles by emulsion polymerization is a method in which, for example, additives such as a polymerization initiator, a catalyst, and the like are emulsified in a dispersion medium together with a monomer for forming a fluorine-containing resin using a surfactant (i.e., an emulsifier), and then the monomer is polymerized while the polymerized product is granulated. In particular, the fluorine-containing resin particles are preferably particles obtained without being exposed to radiation during the production process. However, the fluororesin particles may also be radiation-exposed fluororesin particles that have been irradiated with radiation in the absence of oxygen or at a reduced oxygen concentration.
[0055] The average particle size of the fluorine-containing resin particles according to the present embodiment is not particularly limited, but is preferably 0.2 μm to 4.5 μm, more preferably 0.2 μm to 4 μm. Fluorine-containing resin particles (especially fluorine-containing resin particles such as PTFE particles) with an average particle size of 0.2 μm to 4.5 μm tend to contain a lot of PFOA. Therefore, fluorine-containing resin particles with an average particle size of 0.2 μm to 4.5 μm tend to have low electrostatic chargeability. However, by suppressing the amount of PFOA within the above range, even fluorine-containing resin particles with an average particle size of 0.2 μm to 4.5 μm can have high electrostatic chargeability.
[0056] The average particle size of the fluorine-containing resin particles is a value measured by the following method. Observe with a SEM (scanning electron microscope) at a magnification of, for example, 5000 times or more, measure the maximum diameter of the fluorine-containing resin particles (secondary particles formed by aggregation of primary particles), and take the average value of 50 particles as the average particle size of the fluorine-containing resin particles. Note that a JEOL JSM-6700F is used as the SEM, and secondary electron images are observed at an accelerating voltage of 5 kV.
[0057] From the viewpoint of dispersion stability, the specific surface area (BET specific surface area) of the fluorine-containing resin particles according to this embodiment is 5 m 2 / g or more 15m 2 / g or less, and 2 / g or more 13m 2 It is more preferable that the molecular weight is not more than 1 / g. The specific surface area is a value measured by a nitrogen substitution method using a BET type specific surface area measuring device (Shimadzu Corporation: Flow Soap II 2300).
[0058] The apparent density of the fluorine-containing resin particles according to this embodiment is preferably from 0.2 g / ml to 0.5 g / ml, more preferably from 0.3 g / ml to 0.45 g / ml, from the viewpoint of dispersion stability. The apparent density is a value measured in accordance with JIS K6891 (1995).
[0059] The melting temperature of the fluorine-containing resin particles according to this embodiment is preferably 300° C. or more and 340° C. or less, and more preferably 325° C. or more and 335° C. or less. The melting temperature is a melting point measured in accordance with JIS K6891 (1995).
[0060] The fluorine-containing resin particles according to this embodiment may have a dispersant having fluorine atoms (hereinafter, also referred to as a "fluorine-containing dispersant") attached to the surface.
[0061] The fluorine-containing dispersant may be a polymer obtained by homopolymerizing or copolymerizing a polymerizable compound having a fluorinated alkyl group (hereinafter also referred to as a "fluorinated alkyl group-containing polymer").
[0062] Specific examples of the fluorine-containing dispersant include homopolymers of (meth)acrylates having a fluoroalkyl group, random or block copolymers of (meth)acrylates having a fluoroalkyl group and monomers not having fluorine atoms, etc. Note that (meth)acrylate refers to both acrylate and methacrylate.
[0063] Examples of the (meth)acrylate having a fluorinated alkyl group include 2,2,2-trifluoroethyl (meth)acrylate and 2,2,3,3,3-pentafluoropropyl (meth)acrylate.
[0064] Examples of monomers not having a fluorine atom include (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isooctyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 2-ethoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, and ethyl carbitol (meth). p)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxy (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, hydroxyethyl o-phenylphenol (meth)acrylate, o-phenylphenol glycidyl ether (meth)acrylate.
[0065] Other specific examples of the fluorine-containing dispersant include block or branched polymers disclosed in U.S. Patent No. 5,637,142 and Japanese Patent No. 4,251,662. Further specific examples of the fluorine-containing dispersant include fluorine-based surfactants.
[0066] Among these, as the fluorine-containing dispersant, a fluorinated alkyl group-containing polymer having a structural unit represented by the following general formula (FA) is preferred, and a fluorinated alkyl group-containing polymer having a structural unit represented by the following general formula (FA) and a structural unit represented by the following general formula (FB) is more preferred.
[0067] Hereinafter, a fluorinated alkyl group-containing polymer having a structural unit represented by the following general formula (FA) and a structural unit represented by the following general formula (FB) will be described.
[0068] [ka]
[0069] In the general formulas (FA) and (FB), R F1 , R F2 , R F3 and R F4 each independently represents a hydrogen atom or an alkyl group. X F1 represents an alkylene chain, a halogen-substituted alkylene chain, -S-, -O-, -NH-, or a single bond. Y F1 is an alkylene chain, a halogen-substituted alkylene chain, -(C fx H 2fx-1 (OH))- or a single bond. Q F1 represents -O- or -NH-. Each of fl, fm and fn independently represents an integer of 1 or more. fp, fq, fr and fs each independently represent an integer of 0 or 1 or more. ft represents an integer between 1 and 7. fx represents an integer of 1 or greater.
[0070] In the general formulas (FA) and (FB), R F1 , R F2 , R F3 and R F4 The group represented by the formula (I) is preferably a hydrogen atom, a methyl group, an ethyl group, a propyl group, or the like, more preferably a hydrogen atom or a methyl group, and even more preferably a methyl group.
[0071] In the general formulas (FA) and (FB), X F1 and Y F1 The alkylene chain (unsubstituted alkylene chain, halogen-substituted alkylene chain) represented by the formula (I) is preferably a linear or branched alkylene chain having 1 to 10 carbon atoms. Y F1 Represents -(C fx H 2fx-1 It is preferable that fx in (OH)- represents an integer of 1 or more and 10 or less. It is preferable that fp, fq, fr and fs each independently represent 0 or an integer of 1 or more and 10 or less. It is preferable that fn is, for example, 1 or more and 60 or less.
[0072] Here, in the fluorine-containing dispersant, the ratio of the structural unit represented by general formula (FA) to the structural unit represented by general formula (FB), i.e., fl:fm, is preferably in the range of 1:9 to 9:1, and more preferably in the range of 3:7 to 7:3.
[0073] The fluorine-containing dispersant may further have a structural unit represented by general formula (FC) in addition to the structural unit represented by general formula (FA) and the structural unit represented by general formula (FB). The content ratio of the structural unit represented by general formula (FC) is preferably in the range of 10:0 to 7:3, more preferably in the range of 9:1 to 7:3, in terms of the ratio (fl+fm:fz) to the total of the structural units represented by general formulas (FA) and (FB), i.e., fl+fm.
[0074] [ka]
[0075] In the general formula (FC), R F5 , and R F6 each independently represents a hydrogen atom or an alkyl group, and fz represents an integer of 1 or greater.
[0076] In the general formula (FC), R F5 , and R F6 The group represented by the formula (I) is preferably a hydrogen atom, a methyl group, an ethyl group, a propyl group, or the like, more preferably a hydrogen atom or a methyl group, and even more preferably a methyl group.
[0077] Commercially available fluorine-containing dispersants include, for example, GF300, GF400 (manufactured by Toagosei Co., Ltd.), Surflon series (manufactured by AGC Seimi Chemical Co., Ltd.), Ftergent series (manufactured by Neos Corporation), PF series (manufactured by Kitamura Chemical Co., Ltd.), Megafac series (manufactured by DIC), and FC series (manufactured by 3M).
[0078] The weight average molecular weight Mw of the fluorine-containing dispersant is preferably from 20,000 to 200,000, more preferably from 50,000 to 200,000, from the viewpoint of improving the dispersibility of the fluorine-containing resin particles.
[0079] The weight average molecular weight of a fluorine-containing dispersant is a value measured by gel permeation chromatography (GPC). For example, molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120 as a measuring device, a Tosoh TSKgel GMHHR-M + TSKgel GMHHR-M (7.8mm I.D. 30cm) column, and a chloroform solvent, and the molecular weight is calculated from the measurement results using a molecular weight calibration curve prepared with a monodisperse polystyrene standard sample.
[0080] The content of the fluorine-containing dispersant is, for example, preferably from 0.5% by mass to 10% by mass, and more preferably from 1% by mass to 7% by mass, based on the fluorine-containing resin particles. The fluorine-containing dispersant may be used alone or in combination of two or more kinds.
[0081] Here, the method for adhering fluorine-containing resin particles to the fluorine-containing resin particles according to this embodiment is as follows: 1) A method in which fluorine-containing resin particles and a fluorine-containing dispersant are mixed in a dispersion medium to prepare a dispersion of the fluorine-containing resin particles, and then the dispersion medium is removed from the dispersion. 2) A method in which fluorine-containing resin particles and a fluorine-containing dispersant are mixed using a dry powder mixer to adhere the fluorine-containing dispersant to the fluorine-containing resin particles. 3) A method in which a fluorine-containing dispersant dissolved in a solvent is dropped onto the fluorine-containing resin particles while they are being stirred, and then the solvent is removed. etc.
[0082] Here, the fluorine-containing dispersant is a fluorine-containing dispersant having a wave number of 1673 cm in the infrared absorption spectrum. -1 Wave number 1779cm -1 For peak areas in the range of 1020 cm -1 Wave number 1308cm -1 Also included are fluorine-based graft polymers having a peak area ratio in the range of from 2.7 to 4.8 (hereinafter also referred to as "specific fluorine-based graft polymers").
[0083] When the fluorine-containing resin particles having this specific fluorine-based graft polymer adhered to the surface are contained in the outermost layer of an electrophotographic photoreceptor, local deterioration in cleaning performance is suppressed. The reason for this is presumed to be as follows.
[0084] Conventionally, fluorine-containing resin particles are blended in the surface layer of an electrophotographic photoreceptor for the purpose of improving the cleaning property, and a dispersant such as a fluorine-based graft polymer is used to improve the dispersibility of the fluorine-containing resin particles.
[0085] However, even if a dispersant is blended together with the fluorine-containing resin particles in a coating liquid for forming a surface layer of an electrophotographic photoreceptor to enhance the dispersibility of the fluorine-containing resin particles, the dispersibility decreases over time, and settling or re-aggregation of the fluorine-containing resin particles may occur. When the surface layer of the electrophotographic photoreceptor is formed using a coating liquid in which the dispersibility of the fluorine-containing resin particles is reduced, the dispersibility of the fluorine-containing resin particles in the surface layer is reduced, which may cause localized cleaning defects. Furthermore, after the coating liquid is applied, the dispersibility of the fluorine-containing resin particles is reduced due to changes in component concentration due to drying of the coating film, etc., which may cause localized deterioration in cleaning properties.
[0086] In the fluorine-based graft polymer used as a dispersant, the fluorine components in the polymer (specifically, fluorinated alkyl groups, etc.) tend to interact strongly with the fluorine-containing resin particles. On the other hand, the ester skeleton (i.e., >C=O), which is a polar group in the fluorine-based graft polymer, tends to interact strongly with the vehicle of the coating liquid (specifically, the binder resin (e.g., binder resin such as polycarbonate resin or polyarylate resin) and the solvent).
[0087] The dispersion stabilization of the fluorine-containing resin particles by the fluorine-based graft polymer is called stabilization by steric hindrance, and is determined by the balance between the affinity between the fluorine-based graft polymer and the fluorine-containing resin particles, and the affinity between the fluorine-based graft polymer and the vehicle of the coating liquid.
[0088] If the affinity between the fluorine-based graft polymer and the fluorine-containing resin particles is too higher than the affinity between the fluorine-based graft polymer and the vehicle of the coating liquid, the fluorine-based graft polymer attached to the fluorine-containing resin particles will not dissolve and spread in the dispersion liquid, and the stabilization of the fluorine-containing resin particles due to the steric hindrance of the fluorine-based graft polymer will be easily reduced. On the other hand, if the affinity between the fluorine-based graft polymer and the fluorine-containing resin particles is too lower than the affinity between the fluorine-based graft polymer and the vehicle of the coating liquid, the fluorine-based graft polymer will be difficult to adhere to the fluorine-containing resin particles, and will be difficult to function as a dispersant.
[0089] In this state, for example, due to mechanical load caused by circulation of the coating liquid for forming a surface layer, temperature change during storage of the coating liquid, changes over time in the components of the coating liquid such as evaporation of the solvent, changes in component concentrations during drying of the coating liquid, and the like, the dispersibility of the fluorine-containing resin particles decreases over time, making the fluorine-containing resin particles prone to settling or re-aggregation. As a result, the dispersibility of the fluorine-containing particles in the surface layer of the photoreceptor decreases, causing uneven concentration of the fluorine-containing particles in the surface layer of the photoreceptor, which may result in localized cleaning defects in areas with low concentration of fluorine-containing particles.
[0090] In contrast, in a specific fluorine-based graft polymer, the wave number is 1020 cm -1 Wave number 1308cm -1 The peak in this range corresponds to the peak derived from the fluorine component of the fluorine-based graft polymer. In other words, this peak area corresponds to the amount of the fluorine component of the fluorine-based graft polymer. On the other hand, the wave number is 1673 cm -1 Wave number 1779cm -1 The peak in the range corresponds to the peak derived from the ester skeleton (i.e., >C=O) of the fluorine-based graft polymer. In other words, this peak area corresponds to the amount of the ester skeleton of the fluorine-based graft polymer. Therefore, the ratio of the peak areas of both corresponds to the ratio of the amount of fluorine components to the amount of ester skeletons in the fluorine-based graft polymer.
[0091] And the peak area ratio of both (wave number 1020 cm -1 Wave number 1308cm -1 Peak area / wavenumber in the range of 1673cm -1 Wave number 1779cm -1 When the peak area in the range of (a) is within the above range, a balance is achieved between the affinity between the fluorine-based graft polymer and the fluorine-containing resin particles, and the affinity between the fluorine-based graft polymer and the vehicle of the coating liquid. This balance ensures the adhesion of the fluorine-based graft polymer to the fluorine-containing resin particles, while also ensuring the affinity of the fluorine-based graft polymer to the vehicle of the coating liquid, and the stabilization of the fluorine-containing resin particles due to the steric hindrance of the fluorine-based graft polymer is exhibited.
[0092] Therefore, even if mechanical load due to circulation of the coating liquid for forming a surface layer occurs, temperature change during storage of the coating liquid, changes over time in the components of the coating liquid such as evaporation of the solvent, changes in the concentrations of the components during drying of the coating liquid, and the like, a decrease in dispersibility of the fluorine-containing resin particles over time is suppressed, and settling or re-aggregation of the fluorine-containing resin particles is unlikely to occur. As a result, the dispersibility of the fluorine-containing particles in the surface layer of the photoreceptor is improved, and localized cleaning defects are suppressed.
[0093] In a specific fluorine-based graft polymer, the peak area ratio (wave number 1020 cm -1 Wave number 1308cm -1 Peak area / wavenumber in the range of 1673cm -1 Wave number 1779cm -1 From the viewpoint of suppressing a local decrease in cleaning performance, the peak area in the range of (a) is preferably 2.8 or more and 4.8 or less, and more preferably 3.5 or more and 4.8 or less.
[0094] The infrared absorption spectrum of the specific fluorine-based graft polymer is measured by the following method. First, the fluorine-based graft polymer to be measured is made into a fine powder or film to prepare a measurement sample for the ATR method (attenuated total reflection measurement method). The measurement sample is then subjected to 64 integrations and a resolution of 4 cm using an infrared spectrophotometer (JASCO Corporation: FT / IR-6100, ATR unit, with ZnSe window material). -1 Under the condition of 650 cm -1 More than 4000cm -1 After measuring the following range, ATR correction is performed to obtain an infrared absorption spectrum. And the wave number is 1673 cm -1 Wave number 1779cm -1 The peak area in this range is determined as the carbonyl group in the fluorine-based graft polymer. Similarly, the wave number is 1020 cm -1 Wave number 1308cm -1 The peak area in this range is calculated as the sum of the CF groups and COC groups in the fluorine-based graft polymer.
[0095] When the infrared absorption spectrum of a specific fluorine-based graft polymer is measured from the outermost surface layer containing the fluorine-based graft polymer, the fluorine-based graft polymer as a measurement sample is collected as follows. The outermost surface layer is dissolved in a soluble solvent such as tetrahydrofuran, and the fluorine-containing fine particles are filtered through a 0.1 μm mesh filter. Next, the fluorine-containing fine particles obtained by filtration are heated at 100° C. or less in an aromatic hydrocarbon such as toluene or xylene, or a halogen solvent such as fluorocarbon, perfluorocarbon, hydrochlorofluorocarbon, methylene chloride, or chloroform, an ester solvent such as ethyl acetate or butyl acetate, a ketone solvent such as acetone, methyl ethyl ketone, methyl isobutyl ketone, or cyclopentanone, or a mixed solvent of two or more of these, and then filtered and dried to elute and collect the fluorine-based graft polymer adsorbed on the surface of the fluorine-containing fine particles.
[0096] The fluorine-based graft polymer having the above peak area ratio can be, for example, a copolymer of a polymerizable compound having a fluorinated alkyl group and a polymerizable compound having an ester group but not having a fluorinated alkyl group. The fluorine-based graft polymer having the peak area ratio can be obtained by adjusting the ratio of the amounts of these two polymerizable compounds.
[0097] Specific examples of the specific fluorine-based graft polymer include random or block copolymers of (meth)acrylates having a fluorinated alkyl group and monomers having no fluorinated alkyl group and an ester group (>C=0). Note that (meth)acrylate refers to both acrylate and methacrylate.
[0098] Examples of the (meth)acrylate having a fluorinated alkyl group include 2,2,2-trifluoroethyl (meth)acrylate and 2,2,3,3,3-pentafluoropropyl (meth)acrylate.
[0099] Examples of monomers that do not have a fluorinated alkyl group and have an ester group (>C=0) include methoxypolyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, and (meth)acrylate of phenoxypolyethylene glycol (meth)acrylate.
[0100] As the specific fluorine-based graft polymer, in particular, a fluorinated alkyl group-containing polymer having a structural unit represented by the above general formula (FA) and a structural unit represented by the above general formula (FB) is preferred.
[0101] Here, in the specific fluorine-based graft polymer, the ratio of the structural unit represented by general formula (FA) to the structural unit represented by general formula (FB), i.e., fl:fm, is preferably in the range of 1:9 to 9:1, and more preferably in the range of 3:7 to 7:3.
[0102] The specific fluorine-based graft polymer may further have a structural unit represented by the above general formula (FC) in addition to the structural unit represented by the general formula (FA) and the structural unit represented by the general formula (FB). The content ratio of the structural unit represented by the general formula (FC) is preferably in the range of 10:0 to 7:3, more preferably in the range of 9:1 to 7:3, in terms of the ratio (fl+fm:fz) to the total of the structural units represented by the general formulas (FA) and (FB), i.e., fl+fm.
[0103] The weight average molecular weight Mw of the specific fluorine-based graft polymer is preferably from 20,000 to 200,000, more preferably from 50,000 to 200,000, and even more preferably from 80,000 to 150,000, from the viewpoint of improving the dispersibility of the fluorine-containing resin particles (i.e., from the viewpoint of suppressing local deterioration in cleaning performance).
[0104] <Composition> The composition according to this embodiment contains the fluorine-containing resin according to this embodiment. The composition according to the present embodiment may contain a fluorine-containing dispersant. The composition containing a fluorine-containing dispersant may be a composition prepared by mixing dispersant-attached fluorine-containing resin particles having a fluorine-containing dispersant attached to the surface thereof with other components (e.g., a dispersion medium, resin particles other than PTFE particles, etc.), or may be a composition prepared by mixing fluorine-containing resin particles, a fluorine-containing dispersant, and other components (e.g., a dispersion medium, resin particles other than PTFE particles, etc.) separately.
[0105] The composition according to the present embodiment may be either a liquid composition or a solid composition. Examples of the liquid composition include a fluorine-containing resin particle dispersion containing fluorine-containing resin particles and a dispersion medium, and a layer-forming coating liquid obtained by blending a resin with a fluorine-containing resin particle dispersion. The solid composition may be a composition containing fluorine-containing resin particles and resin particles (for example, toner particles, powder coating particles, etc.).
[0106] <Layered material> The layered product according to the present embodiment includes the fluorine-containing resin particles according to the present embodiment. Specifically, the layered product according to the present embodiment is, for example, a layer formed from the composition according to the present embodiment.
[0107] Examples of the layered product according to the present embodiment include the outermost layer of an electrophotographic photoreceptor, a toner image, a powder coating layer, a sliding layer, and the like.
[0108] In the layered material according to this embodiment, the content of the fluorine-containing resin particles is preferably from 0.1% by mass to 40% by mass, more preferably from 1% by mass to 30% by mass, based on the layered material.
[0109] <Electrophotographic photoreceptor> The electrophotographic photoreceptor (hereinafter also referred to as "photoreceptor") according to this embodiment has a conductive substrate and a photosensitive layer provided on the conductive substrate, and the outermost surface layer is a layer made of the layered material according to this embodiment. The outermost layer made of this layered material may be a charge transport layer of a laminated type photosensitive layer, a single-layer type photosensitive layer, a surface protective layer, or the like.
[0110] Hereinafter, the electrophotographic photoreceptor according to the present embodiment will be described with reference to the drawings. 1 may be, for example, a photoreceptor 7 having a structure in which an undercoat layer 1, a charge generation layer 2, and a charge transport layer 3 are laminated in this order on a conductive support 4. The charge generation layer 2 and the charge transport layer 3 constitute a photosensitive layer 5.
[0111] The electrophotographic photoreceptor 7 may have a layer structure in which the undercoat layer 1 is not provided. The electrophotographic photoreceptor 7 may be a photoreceptor having a single-layer type photosensitive layer in which the functions of the charge generating layer 2 and the charge transport layer 3 are integrated. In the case of a photoreceptor having a single-layer type photosensitive layer, the single-layer type photosensitive layer constitutes the outermost layer. The electrophotographic photoreceptor 7 may be a photoreceptor having a surface protective layer on the charge transport layer 3 or on the single-layer photoreceptor. In the case of a photoreceptor having a surface protective layer, the surface protective layer constitutes the outermost surface layer.
[0112] Hereinafter, each layer of the electrophotographic photoreceptor according to the present embodiment will be described in detail, with the reference numerals omitted.
[0113] (Conductive substrate) Examples of conductive substrates include metal plates, metal drums, and metal belts containing metals (aluminum, copper, zinc, chromium, nickel, molybdenum, vanadium, indium, gold, platinum, etc.) or alloys (stainless steel, etc.). Examples of conductive substrates include paper, resin films, belts, etc. coated, vapor-deposited, or laminated with conductive compounds (e.g., conductive polymers, indium oxide, etc.), metals (e.g., aluminum, palladium, gold, etc.) or alloys. Here, "conductive" refers to a material having a volume resistivity of 10 13 This means that the resistance is less than Ωcm.
[0114] When the electrophotographic photoreceptor is used in a laser printer, the surface of the conductive substrate is preferably roughened to a center line average roughness Ra of 0.04 μm to 0.5 μm in order to suppress interference fringes that occur when irradiating with laser light. When non-interfering light is used as the light source, roughening to prevent interference fringes is not particularly necessary, but it is suitable for extending the life of the conductive substrate since it suppresses the occurrence of defects due to unevenness on the surface.
[0115] Examples of methods for roughening the surface include wet honing, which involves spraying an abrasive suspended in water onto the conductive substrate; centerless grinding, in which the conductive substrate is pressed against a rotating grindstone and continuously ground; and anodizing.
[0116] As a method for roughening the surface, there can be mentioned a method in which, without roughening the surface of the conductive substrate, a conductive or semiconductive powder is dispersed in a resin to form a layer on the surface of the conductive substrate, and the surface is roughened by the particles dispersed in the layer.
[0117] In the roughening treatment by anodization, an oxide film is formed on the surface of a conductive substrate made of metal (e.g., aluminum) by anodizing the substrate in an electrolyte solution using the substrate as the anode. Examples of electrolyte solutions include sulfuric acid solution and oxalic acid solution. However, the porous anodic oxide film formed by anodization is chemically active in its original state, easily contaminated, and has a large resistance variation depending on the environment. Therefore, it is preferable to perform a sealing treatment on the porous anodic oxide film, in which the micropores of the oxide film are filled by volume expansion caused by hydration reaction in pressurized steam or boiling water (metal salts such as nickel may be added) to change the film into a more stable hydrated oxide.
[0118] The thickness of the anodic oxide film is preferably, for example, from 0.3 μm to 15 μm. If the thickness is within this range, the film tends to exhibit a barrier property against injection and tends to suppress an increase in residual potential due to repeated use.
[0119] The conductive substrate may be subjected to a treatment with an acidic treatment solution or a boehmite treatment. Treatment with an acid treatment liquid is carried out, for example, as follows. First, an acid treatment liquid containing phosphoric acid, chromic acid, and hydrofluoric acid is prepared. The compounding ratios of phosphoric acid, chromic acid, and hydrofluoric acid in the acid treatment liquid are, for example, in the range of 10% by mass to 11% by mass for phosphoric acid, 3% by mass to 5% by mass for chromic acid, and 0.5% by mass to 2% by mass for hydrofluoric acid, and the total concentration of these acids is preferably in the range of 13.5% by mass to 18% by mass. The treatment temperature is preferably, for example, 42° C. to 48° C. The film thickness of the coating is preferably 0.3 μm to 15 μm.
[0120] The boehmite treatment is carried out, for example, by immersing the material in pure water at 90°C to 100°C for 5 to 60 minutes, or by contacting the material with heated steam at 90°C to 120°C for 5 to 60 minutes. The thickness of the coating is preferably 0.1 μm to 5 μm. This may be further anodized using an electrolyte solution having low coating solubility, such as adipic acid, boric acid, borates, phosphates, phthalates, maleates, benzoates, tartrates, or citrates.
[0121] (subbing layer) The undercoat layer is, for example, a layer containing inorganic particles and a binder resin.
[0122] As inorganic particles, for example, powder resistivity (volume resistivity) of 10 2 Ωcm or more 10 11 Examples of such particles include inorganic particles with a particle size of Ωcm or less. Among these, examples of inorganic particles having the above-mentioned resistance value include metal oxide particles such as tin oxide particles, titanium oxide particles, zinc oxide particles, and zirconium oxide particles, and zinc oxide particles are particularly preferred.
[0123] The specific surface area of inorganic particles by the BET method is, for example, 10 m 2 / g or higher is preferable. The volume average particle size of the inorganic particles is, for example, from 50 nm to 2000 nm (preferably from 60 nm to 1000 nm).
[0124] The content of the inorganic particles is, for example, preferably from 10% by mass to 80% by mass, more preferably from 40% by mass to 80% by mass, based on the binder resin.
[0125] The inorganic particles may be surface-treated. Two or more types of inorganic particles having different surface treatments or different particle sizes may be used in combination.
[0126] Examples of the surface treatment agent include a silane coupling agent, a titanate coupling agent, an aluminum coupling agent, a surfactant, etc. In particular, a silane coupling agent is preferred, and a silane coupling agent having an amino group is more preferred.
[0127] Examples of silane coupling agents having an amino group include, but are not limited to, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, and N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane.
[0128] Silane coupling agents may be used in combination of two or more kinds. For example, a silane coupling agent having an amino group may be used in combination with another silane coupling agent. Examples of other silane coupling agents include, but are not limited to, vinyltrimethoxysilane, 3-methacryloxypropyl-tris(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, and 3-chloropropyltrimethoxysilane.
[0129] The surface treatment method using the surface treatment agent may be any known method, and may be either a dry method or a wet method.
[0130] The amount of the surface treatment agent to be used is preferably, for example, 0.5% by mass or more and 10% by mass or less based on the inorganic particles.
[0131] Here, it is preferable that the undercoat layer contains an electron accepting compound (acceptor compound) together with the inorganic particles, from the viewpoints of improving the long-term stability of electrical properties and carrier blocking properties.
[0132] Examples of the electron-accepting compound include electron-transporting substances such as quinone compounds such as chloranil and bromoanil; tetracyanoquinodimethane compounds; fluorenone compounds such as 2,4,7-trinitrofluorenone and 2,4,5,7-tetranitro-9-fluorenone; oxadiazole compounds such as 2-(4-biphenyl)-5-(4-t-butylphenyl)-1,3,4-oxadiazole, 2,5-bis(4-naphthyl)-1,3,4-oxadiazole and 2,5-bis(4-diethylaminophenyl)-1,3,4-oxadiazole; xanthone compounds; thiophene compounds; and diphenoquinone compounds such as 3,3',5,5'-tetra-t-butyldiphenoquinone. In particular, the electron-accepting compound is preferably a compound having an anthraquinone structure. Examples of the compound having an anthraquinone structure include hydroxyanthraquinone compounds, aminoanthraquinone compounds, and aminohydroxyanthraquinone compounds, and more specifically, anthraquinone, alizarin, quinizarin, anthrarufin, and purpurin.
[0133] The electron accepting compound may be contained in the undercoat layer in a dispersed state together with the inorganic particles, or may be contained in a state of being attached to the surfaces of the inorganic particles.
[0134] The method for attaching the electron accepting compound to the surface of the inorganic particles may be, for example, a dry method or a wet method.
[0135] The dry method is, for example, a method in which an electron-accepting compound is attached to the surface of inorganic particles by dropping an electron-accepting compound directly or dissolved in an organic solvent or spraying it together with dry air or nitrogen gas while stirring inorganic particles with a mixer or the like that exerts a large shearing force. The dropping or spraying of the electron-accepting compound is preferably performed at a temperature below the boiling point of the solvent. After dropping or spraying the electron-accepting compound, baking may be performed at 100° C. or higher. The temperature and time of baking are not particularly limited as long as electrophotographic properties can be obtained.
[0136] The wet method is a method in which, for example, an electron-accepting compound is added while dispersing inorganic particles in a solvent by stirring, ultrasonic waves, a sand mill, an attritor, a ball mill, etc., and the inorganic particles are stirred or dispersed, and then the solvent is removed to attach the electron-accepting compound to the surface of the inorganic particles. The solvent is removed, for example, by filtration or distillation. After the solvent is removed, baking may be performed at 100°C or higher. The baking temperature and time are not particularly limited as long as electrophotographic properties are obtained. In the wet method, moisture contained in the inorganic particles may be removed before adding the electron-accepting compound, and examples of such methods include a method of removing the moisture while stirring and heating in a solvent, and a method of removing the moisture by azeotropy with the solvent.
[0137] The attachment of the electron accepting compound may be carried out before or after the inorganic particles are subjected to a surface treatment with a surface treatment agent, or the attachment of the electron accepting compound and the surface treatment with the surface treatment agent may be carried out simultaneously.
[0138] The content of the electron accepting compound is, for example, from 0.01% by mass to 20% by mass, and preferably from 0.01% by mass to 10% by mass, based on the inorganic particles.
[0139] Examples of the binder resin used in the undercoat layer include known materials such as acetal resins (e.g., polyvinyl butyral, etc.), polyvinyl alcohol resins, polyvinyl acetal resins, casein resins, polyamide resins, cellulose resins, gelatin, polyurethane resins, polyester resins, unsaturated polyester resins, methacrylic resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate-maleic anhydride resins, silicone resins, silicone-alkyd resins, urea resins, phenol resins, phenol-formaldehyde resins, melamine resins, urethane resins, alkyd resins, and epoxy resins; zirconium chelate compounds; titanium chelate compounds; aluminum chelate compounds; titanium alkoxide compounds; organic titanium compounds; and silane coupling agents. Examples of the binder resin used in the undercoat layer include charge transporting resins having charge transporting groups, conductive resins (such as polyaniline, etc.), and the like.
[0140] Among these, the binder resin used in the undercoat layer is preferably a resin that is insoluble in the coating solvent of the upper layer, and in particular, a resin obtained by reacting at least one resin selected from the group consisting of thermosetting resins such as urea resins, phenol resins, phenol-formaldehyde resins, melamine resins, urethane resins, unsaturated polyester resins, alkyd resins, and epoxy resins, with a curing agent is preferred. When two or more of these binder resins are used in combination, the mixing ratio is set as necessary.
[0141] The undercoat layer may contain various additives for improving electrical properties, environmental stability, and image quality. Examples of the additives include known materials such as polycyclic condensation and azo-based electron transport pigments, zirconium chelate compounds, titanium chelate compounds, aluminum chelate compounds, titanium alkoxide compounds, organic titanium compounds, silane coupling agents, etc. As described above, silane coupling agents are used for surface treatment of inorganic particles, and may also be added to the undercoat layer as an additive.
[0142] Examples of silane coupling agents as additives include vinyltrimethoxysilane, 3-methacryloxypropyl-tris(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, and the like.
[0143] Examples of the zirconium chelate compound include zirconium butoxide, zirconium ethyl acetoacetate, zirconium triethanolamine, acetylacetonate zirconium butoxide, ethyl acetoacetate zirconium butoxide, zirconium acetate, zirconium oxalate, zirconium lactate, zirconium phosphonate, zirconium octanoate, zirconium naphthenate, zirconium laurate, zirconium stearate, zirconium isostearate, methacrylate zirconium butoxide, stearate zirconium butoxide, and isostearate zirconium butoxide.
[0144] Examples of titanium chelate compounds include tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetra(2-ethylhexyl) titanate, titanium acetylacetonate, polytitanium acetylacetonate, titanium octylene glycolate, titanium lactate ammonium salt, titanium lactate, titanium lactate ethyl ester, titanium triethanolamine, and polyhydroxytitanium stearate.
[0145] Examples of aluminum chelate compounds include aluminum isopropylate, monobutoxyaluminum diisopropylate, aluminum butyrate, diethylacetoacetate aluminum diisopropylate, and aluminum tris(ethylacetoacetate).
[0146] These additives may be used alone or as a mixture or polycondensation product of a plurality of compounds.
[0147] The undercoat layer preferably has a Vickers hardness of 35 or more. The surface roughness (ten-point average roughness) of the undercoat layer is preferably adjusted to between 1 / (4n) (n is the refractive index of the upper layer) and 1 / 2 of the wavelength λ of the exposure laser used in order to suppress moire images. Resin particles or the like may be added to the undercoat layer to adjust the surface roughness. Examples of the resin particles include silicone resin particles and crosslinked polymethyl methacrylate resin particles. The surface of the undercoat layer may be polished to adjust the surface roughness. Examples of the polishing method include buffing, sandblasting, wet honing, grinding, and the like.
[0148] The formation of the undercoat layer is not particularly limited, and a well-known formation method can be used. For example, the undercoat layer can be formed by forming a coating film of a coating solution for forming the undercoat layer in which the above-mentioned components are added to a solvent, drying the coating film, and heating it as necessary.
[0149] Examples of the solvent for preparing the coating liquid for forming the undercoat layer include known organic solvents, such as alcohol-based solvents, aromatic hydrocarbon solvents, halogenated hydrocarbon solvents, ketone-based solvents, ketone alcohol-based solvents, ether-based solvents, and ester-based solvents. Specific examples of these solvents include ordinary organic solvents such as methanol, ethanol, n-propanol, iso-propanol, n-butanol, benzyl alcohol, methyl cellosolve, ethyl cellosolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, ethyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, methylene chloride, chloroform, chlorobenzene, and toluene.
[0150] Examples of the method for dispersing the inorganic particles when preparing the coating liquid for forming the undercoat layer include known methods such as those using a roll mill, a ball mill, a vibrating ball mill, an attritor, a sand mill, a colloid mill, and a paint shaker.
[0151] Examples of the method for applying the coating liquid for forming the undercoat layer onto the conductive substrate include ordinary methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating, and curtain coating.
[0152] The thickness of the undercoat layer is set, for example, preferably at least 15 μm, and more preferably within the range of from 20 μm to 50 μm.
[0153] (Middle class) Although not shown, an intermediate layer may be further provided between the undercoat layer and the photosensitive layer. The intermediate layer is, for example, a layer containing a resin. Examples of the resin used in the intermediate layer include polymer compounds such as acetal resins (e.g., polyvinyl butyral, etc.), polyvinyl alcohol resins, polyvinyl acetal resins, casein resins, polyamide resins, cellulose resins, gelatin, polyurethane resins, polyester resins, methacrylic resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate-maleic anhydride resins, silicone resins, silicone-alkyd resins, phenol-formaldehyde resins, and melamine resins. The intermediate layer may be a layer containing an organometallic compound. Examples of the organometallic compound used in the intermediate layer include organometallic compounds containing metal atoms such as zirconium, titanium, aluminum, manganese, and silicon. The compounds used in the intermediate layer may be used alone or as a mixture or polycondensation product of a plurality of compounds.
[0154] Among these, the intermediate layer is preferably a layer containing an organometallic compound containing zirconium atoms or silicon atoms.
[0155] The formation of the intermediate layer is not particularly limited, and a well-known formation method can be used. For example, the intermediate layer can be formed by forming a coating film of a coating liquid for forming an intermediate layer in which the above components are added to a solvent, drying the coating film, and heating it if necessary. The intermediate layer can be formed by any of the usual coating methods, such as dip coating, push-up coating, wire bar coating, spray coating, blade coating, knife coating and curtain coating.
[0156] The thickness of the intermediate layer is preferably set in the range of, for example, 0.1 μm to 3 μm. The intermediate layer may also be used as an undercoat layer.
[0157] (Charge generation layer) The charge generation layer is, for example, a layer containing a charge generation material and a binder resin. The charge generation layer may also be a vapor deposition layer of the charge generation material. The vapor deposition layer of the charge generation material is suitable for use with a non-coherent light source such as an LED (Light Emitting Diode) or an organic EL (Electro-Luminescence) image array.
[0158] Examples of the charge generating material include azo pigments such as bisazo and trisazo; condensed aromatic pigments such as dibromoanthanthrone; perylene pigments; pyrrolopyrrole pigments; phthalocyanine pigments; zinc oxide; and trigonal selenium.
[0159] Among these, in order to correspond to the laser exposure in the near infrared region, it is preferable to use a metal phthalocyanine pigment or a metal-free phthalocyanine pigment as the charge generating material.Specifically, for example, hydroxygallium phthalocyanine disclosed in JP-A-5-263007, JP-A-5-279591, etc., chlorogallium phthalocyanine disclosed in JP-A-5-98181, etc., dichlorotin phthalocyanine disclosed in JP-A-5-140472, JP-A-5-140473, etc., and titanyl phthalocyanine disclosed in JP-A-4-189873, etc. are more preferable.
[0160] On the other hand, in order to accommodate laser exposure in the near ultraviolet region, preferred charge generating materials include condensed aromatic pigments such as dibromoanthanthrone, thioindigo pigments, porphyrazine compounds, zinc oxide, trigonal selenium, and the bisazo pigments disclosed in JP-A-2004-78147 and JP-A-2005-181992.
[0161] The above charge generating materials may be used when using incoherent light sources such as LEDs and organic EL image arrays that emit light at a central wavelength of 450 nm to 780 nm, but from the viewpoint of resolution, when using a thin photosensitive layer of 20 μm or less, the electric field strength in the photosensitive layer becomes high, and a decrease in charging due to charge injection from the substrate, so-called black spots, is likely to occur as an image defect. This becomes more noticeable when using charge generating materials that are p-type semiconductors such as trigonal selenium and phthalocyanine pigments and are prone to generating dark current.
[0162] In contrast, when an n-type semiconductor such as a fused aromatic pigment, a perylene pigment, or an azo pigment is used as the charge generating material, dark current is unlikely to occur, and image defects called black spots can be suppressed even when the material is a thin film. Examples of n-type charge generating materials include, but are not limited to, compounds (CG-1) to (CG-27) described in paragraphs
[0288] to
[0291] of JP-A-2012-155282. The n-type is determined by the polarity of the photocurrent that flows using the commonly used time-of-flight method, and those that easily pass electrons as carriers rather than holes are considered to be n-type.
[0163] The binder resin used in the charge generating layer may be selected from a wide range of insulating resins, and may also be selected from organic photoconductive polymers such as poly-N-vinylcarbazole, polyvinylanthracene, polyvinylpyrene, polysilane, and the like. Examples of the binder resin include polyvinyl butyral resin, polyarylate resin (polycondensation product of bisphenols and aromatic dicarboxylic acid, etc.), polycarbonate resin, polyester resin, phenoxy resin, vinyl chloride-vinyl acetate copolymer, polyamide resin, acrylic resin, polyacrylamide resin, polyvinylpyridine resin, cellulose resin, urethane resin, epoxy resin, casein, polyvinyl alcohol resin, polyvinylpyrrolidone resin, etc. Here, "insulating" means a material having a volume resistivity of 10 13 This means that the resistance is Ωcm or more. These binder resins may be used alone or in combination of two or more.
[0164] The compounding ratio of the charge generating material to the binder resin is preferably within a range of 10:1 to 1:10 by mass.
[0165] The charge generating layer may contain other well-known additives.
[0166] The formation of the charge generation layer is not particularly limited, and a known formation method is used, for example, by forming a coating film of a coating solution for forming a charge generation layer in which the above-mentioned components are added to a solvent, drying the coating film, and heating it as necessary. The formation of the charge generation layer may be performed by vapor deposition of a charge generation material. The formation of the charge generation layer by vapor deposition is particularly suitable when a condensed ring aromatic pigment or a perylene pigment is used as the charge generation material.
[0167] Examples of the solvent for preparing the coating liquid for forming the charge generating layer include methanol, ethanol, n-propanol, n-butanol, benzyl alcohol, methyl cellosolve, ethyl cellosolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, methylene chloride, chloroform, chlorobenzene, toluene, etc. These solvents may be used alone or in combination of two or more.
[0168] Examples of methods for dispersing particles (e.g., charge generating material) in the coating liquid for forming a charge generating layer include media dispersers such as ball mills, vibration ball mills, attritors, sand mills, and horizontal sand mills, and medialess dispersers such as stirrers, ultrasonic dispersers, roll mills, and high-pressure homogenizers. Examples of high-pressure homogenizers include a collision method in which the dispersion liquid is dispersed by liquid-liquid collision or liquid-wall collision under high pressure, and a penetration method in which the dispersion liquid is dispersed by penetrating a fine flow path under high pressure. During this dispersion, it is effective to adjust the average particle size of the charge generating material in the coating liquid for forming the charge generating layer to 0.5 μm or less, preferably 0.3 μm or less, and more preferably 0.15 μm or less.
[0169] Examples of a method for applying the coating liquid for forming the charge generating layer onto the undercoat layer (or onto the intermediate layer) include conventional methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating, and curtain coating.
[0170] The thickness of the charge generating layer is set, for example, preferably in the range of 0.1 μm or more and 5.0 μm or less, and more preferably in the range of 0.2 μm or more and 2.0 μm or less.
[0171] (charge transport layer) The charge transport layer is, for example, a layer containing a charge transport material and a binder resin, and may be a layer containing a polymer charge transport material.
[0172] Examples of the charge transport material include electron transporting compounds such as quinone compounds such as p-benzoquinone, chloranil, bromanil, and anthraquinone; tetracyanoquinodimethane compounds; fluorenone compounds such as 2,4,7-trinitrofluorenone; xanthone compounds; benzophenone compounds; cyanovinyl compounds; and ethylene compounds. Examples of the charge transport material include hole transporting compounds such as triarylamine compounds, benzidine compounds, arylalkane compounds, aryl-substituted ethylene compounds, stilbene compounds, anthracene compounds, and hydrazone compounds. These charge transport materials may be used alone or in combination, but are not limited to these.
[0173] As the charge transport material, from the viewpoint of charge mobility, a triarylamine derivative represented by the following structural formula (a-1) and a benzidine derivative represented by the following structural formula (a-2) are preferred.
[0174] [ka]
[0175] In structural formula (a-1), Ar T1 , Ar T2 , and ArT3 each independently represents a substituted or unsubstituted aryl group, -C6H4-C(R T4 )=C(R T5 )(R T6 ), or -CH-CH=CH-CH=C(R T7 )(R T8 ) is shown. T4 , R T5 , R T6 , R T7 , and R T8 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group. Examples of the substituent for each of the above groups include a halogen atom, an alkyl group having from 1 to 5 carbon atoms, and an alkoxy group having from 1 to 5 carbon atoms. Examples of the substituent for each of the above groups also include a substituted amino group substituted with an alkyl group having from 1 to 3 carbon atoms.
[0176] [ka]
[0177] In structural formula (a-2), R T91 and R T92 R each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms. T101 , R T102 , R T111 and R T112 each independently represents a halogen atom, an alkyl group having from 1 to 5 carbon atoms, an alkoxy group having from 1 to 5 carbon atoms, an amino group substituted with an alkyl group having from 1 to 2 carbon atoms, a substituted or unsubstituted aryl group, -C(R T12 )=C(R T13 )(R T14 ), or -CH=CH-CH=C(R T15 )(R T16 ) and R T12 , R T13 , R T14 , R T15 and R T16each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group. Tm1, Tm2, Tn1, and Tn2 each independently represent an integer of 0 or more and 2 or less. Examples of the substituent for each of the above groups include a halogen atom, an alkyl group having from 1 to 5 carbon atoms, and an alkoxy group having from 1 to 5 carbon atoms. Examples of the substituent for each of the above groups also include a substituted amino group substituted with an alkyl group having from 1 to 3 carbon atoms.
[0178] Among the triarylamine derivatives represented by the structural formula (a-1) and the benzidine derivatives represented by the structural formula (a-2), in particular, "-C6H4-CH=CH-CH=C(R T7 )(R T8 )" and triarylamine derivatives having "-CH=CH-CH=C(R T15 )(R T16 ) is preferred from the viewpoint of charge mobility.
[0179] As the polymer charge transport material, known materials having charge transport properties such as poly-N-vinylcarbazole and polysilane are used. In particular, polyester-based polymer charge transport materials disclosed in JP-A-8-176293 and JP-A-8-208820 are particularly preferred. The polymer charge transport material may be used alone or in combination with a binder resin.
[0180] Among these charge transport materials, from the viewpoint of suppressing density unevenness in grainy images, charge transport materials having a butadiene structure and a triarylamine structure (hereinafter also referred to as "butadiene-based charge transport material") are preferred. An example of a butadiene-based charge transport material is a compound in which an organic group having a diphenylmethane structure (=C(Ph)2, Ph=benzene ring) is linked to at least one of the three benzene rings of a triarylamine structure via an aliphatic group having a butadiene structure. Specifically, the butadiene-based charge transport material may be represented by the following general formula (CT1).
[0181] [ka]
[0182] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 each independently represents a hydrogen atom, a halogen atom, an alkyl group having from 1 to 20 carbon atoms, an alkoxy group having from 1 to 20 carbon atoms, or an aryl group having from 6 to 30 carbon atoms, and two adjacent substituents may be bonded to each other to form a hydrocarbon ring structure. n and m each independently represent 0, 1 or 2.
[0183] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 Examples of the halogen atom represented by include a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc. Among these, as the halogen atom, a fluorine atom and a chlorine atom are preferred, and a chlorine atom is more preferred.
[0184] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 The alkyl group represented by the formula (I) includes a linear or branched alkyl group having 1 to 20 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of the straight-chain alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, an n-hexadecyl group, an n-heptadecyl group, an n-octadecyl group, an n-nonadecyl group, and an n-icosyl group. Specific examples of branched alkyl groups include isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, isohexyl, sec-hexyl, tert-hexyl, isoheptyl, sec-heptyl, tert-heptyl, isooctyl, sec-octyl, tert-octyl, isononyl, sec-nonyl, tert-nonyl, isodecyl, sec-decyl, tert-decyl, isoundecyl, sec-undecyl, tert-undecyl, neoundecyl, isododecyl, sec-dodecyl, tert-dodecyl, neododecyl, isotridecyl, sec-tridecyl, tert-tridecyl, neotridecyl, isotetradecyl, group, sec-tetradecyl group, tert-tetradecyl group, neotetradecyl group, 1-isobutyl-4-ethyloctyl group, isopentadecyl group, sec-pentadecyl group, tert-pentadecyl group, neopentadecyl group, isohexadecyl group, sec-hexadecyl group, tert-hexadecyl group, neohexadecyl group, 1-methylpentadecyl group, isoheptadecyl group, sec Examples of the isooctadecyl group include a 1-heptadecyl group, a tert-heptadecyl group, a neoheptadecyl group, an isooctadecyl group, a sec-octadecyl group, a tert-octadecyl group, a neooctadecyl group, an isononadecyl group, a sec-nonadecyl group, a tert-nonadecyl group, a neononadecyl group, a 1-methyloctyl group, an isoicosyl group, a sec-icosyl group, a tert-icosyl group, and a neoicosyl group. Among these, the alkyl group is preferably a lower alkyl group such as a methyl group, an ethyl group, or an isopropyl group.
[0185] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 The alkoxy group represented by the formula (I) includes a linear or branched alkoxy group having 1 to 20 carbon atoms (preferably 1 to 6, more preferably 1 to 4). Specific examples of linear alkoxy groups include a methoxy group, an ethoxy group, an n-propoxy group, an n-butoxy group, an n-pentyloxy group, an n-hexyloxy group, an n-heptyloxy group, an n-octyloxy group, an n-nonyloxy group, an n-decyloxy group, an n-undecyloxy group, an n-dodecyloxy group, an n-tridecyloxy group, an n-tetradecyloxy group, an n-pentadecyloxy group, an n-hexadecyloxy group, an n-heptadecyloxy group, an n-octadecyloxy group, an n-nonadecyloxy group, and an n-icosyloxy group. Specific examples of branched alkoxy groups include an isopropoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an isopentyloxy group, a neopentyloxy group, a tert-pentyloxy group, an isohexyloxy group, a sec-hexyloxy group, a tert-hexyloxy group, an isoheptyloxy group, a sec-heptyloxy group, a tert-heptyloxy group, an isooctyloxy group, a sec-octyloxy group, a tert-octyloxy group, an isononyloxy group, a se c-nonyloxy group, tert-nonyloxy group, isodecyloxy group, sec-decyloxy group, tert-decyloxy group, isoundecyloxy group, sec-undecyloxy group, tert-undecyloxy group, neoundecyloxy group, isododecyloxy group, sec-dodecyloxy group, tert-dodecyloxy group, neododecyloxy group, isotridecyloxy group, sec-tridecyloxy group, tert-tridecyloxy group, neotridecyloxy group, isotetradecyloxy group, hexadecyloxy group, sec-hexadecyloxy group, tert-hexadecyloxy group, neohexadecyloxy group, 1-methylpentadecyloxy group, isohept ...tert-hexadecyloxy group, neohexadecyloxy group, 1-methylpentadecyloxy group, isoheptadecyloxy group, sec-hexadecyloxy group, tert-hexadecyloxy group, neohex Examples of such an aryloxy group include a heptadecyloxy group, a tert-heptadecyloxy group, a neoheptadecyloxy group, an isooctadecyloxy group, a sec-octadecyloxy group, a tert-octadecyloxy group, a neooctadecyloxy group, an isononadecyloxy group, a sec-nonadecyloxy group, a tert-nonadecyloxy group, a neononadecyloxy group, a 1-methyloctyloxy group, an isoicosyloxy group, a sec-icosyloxy group, a tert-icosyloxy group, and a neoicosyloxy group. Among these, the alkoxy group is preferably a methoxy group.
[0186] In general formula (CT1), R C11 , R C12, R C13 , R C14 , R C15 , and R C16 The aryl group represented by the formula (I) includes an aryl group having 6 or more and 30 or less carbon atoms (preferably 6 or more and 20 or less, more preferably 6 or more and 16 or less). Specific examples of the aryl group include a phenyl group, a naphthyl group, a phenanthryl group, and a biphenylyl group. Among these, the aryl group is preferably a phenyl group or a naphthyl group.
[0187] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 Each of the above-mentioned substituents represented by also includes a group having a further substituent. The substituent includes the above-mentioned atoms and groups (e.g., halogen atoms, alkyl groups, alkoxy groups, aryl groups, etc.).
[0188] In general formula (CT1), R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 Two adjacent substituents (e.g., R C11 and R C12 Fellow, R C13 and R C14 Fellow, R C15 and R C16 In the hydrocarbon ring structure in which the substituents (atomic groups) are linked to each other, examples of the group linking the substituents to each other include a single bond, a 2,2'-methylene group, a 2,2'-ethylene group, and a 2,2'-vinylene group. Among these, a single bond and a 2,2'-methylene group are preferred. Specific examples of the hydrocarbon ring structure include a cycloalkane structure, a cycloalkene structure, and a cycloalkanepolyene structure.
[0189] In the general formula (CT1), n and m are preferably 1.
[0190] In the general formula (CT1), from the viewpoint of forming a photosensitive layer (charge transport layer) having high charge transport ability, R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms, and preferably, m and n each represent 1 or 2; R C11 , R C12 , R C13 , R C14 , R C15 , and R C16 It is more preferable that m and n each represent 1. That is, the butadiene-based charge transport material (CT1) is more preferably a charge transport material represented by the following structural formula (CT1A) (exemplary compound (CT1-3)).
[0191] [ka]
[0192] Specific examples of the butadiene-based charge transport material (CT1) are shown below, but the present invention is not limited thereto.
[0193] [ka]
[0194] The abbreviations in the above exemplary compounds have the following meanings: The numbers before the substituents indicate the substitution positions on the benzene ring. -CH3: Methyl group -OCH3: Methoxy group
[0195] The butadiene-based charge transport material (CT1) may be used alone or in combination of two or more kinds.
[0196] Examples of the binder resin used in the charge transport layer include polycarbonate resin, polyester resin, polyarylate resin, methacrylic resin, acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl acetate resin, styrene-butadiene copolymer, vinylidene chloride-acrylonitrile copolymer, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinyl acetate-maleic anhydride copolymer, silicone resin, silicone alkyd resin, phenol-formaldehyde resin, styrene-alkyd resin, poly-N-vinylcarbazole, polysilane, etc. Among these, polycarbonate resin or polyarylate resin is suitable as the binder resin. These binder resins are used alone or in combination of two or more.
[0197] Here, it is preferable to use polycarbonate resin as the binder resin from the viewpoint of durability and high image quality. On the other hand, if fluorine-containing resin particles having many carboxyl groups are used together with polycarbonate resin, the dispersibility of the fluorine-containing resin particles tends to deteriorate. If the dispersibility of the fluorine-containing resin particles deteriorates, the surface of the outermost layer becomes rough, and density unevenness of the grainy image is easily generated. The reason for this phenomenon is presumed to be as follows: The carbonate group (-OC(=O)O-) of the polycarbonate resin interacts with the carboxyl group of the fluorine-containing resin particle, blocking the site in the fluorine-containing resin particle where the fluorine-containing dispersant is adsorbed. Then, due to the steric hindrance of the polycarbonate resin, it becomes difficult for the fluorine-containing dispersant to be adsorbed on the surface of the fluorine-containing resin particle. As a result, it is presumed that the fluorine-containing resin particle deteriorates, and image defects are more likely to occur due to the expansion of the dot area. In particular, when a polycarbonate resin containing a structural unit represented by the following general formula (PCA) and a structural unit represented by the following general formula (PCB), which has a large amount of carbonate groups (-OC(=O)O-) per unit mole, is used, the dispersibility of the fluorine-containing resin particles deteriorates, and image defects tend to occur due to the expansion of the dot area. Therefore, when a polycarbonate resin containing a structural unit represented by the following general formula (PCA) and a structural unit represented by the following general formula (PCB) is used, the number of carboxyl groups is 10 or less. 6 By using 0 to 30 fluorine-containing resin particles per image, density unevenness in a grainy image is suppressed.
[0198] [ka]
[0199] In the general formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and R P4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 5 to 7 carbon atoms, or an aryl group having 6 to 12 carbon atoms. P1 represents a phenylene group, a biphenylene group, a naphthylene group, an alkylene group, or a cycloalkylene group.
[0200] In the general formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and R P4 The alkyl group represented by the formula (I) includes a linear or branched alkyl group having 1 to 6 carbon atoms (preferably 1 to 3 carbon atoms). Specific examples of the straight-chain alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, and an n-hexyl group. Specific examples of branched alkyl groups include an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, an isohexyl group, a sec-hexyl group, and a tert-hexyl group. Among these, the alkyl group is preferably a lower alkyl group such as a methyl group or an ethyl group.
[0201] In the general formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and R P4 Examples of the cycloalkyl group represented by the formula (I) include cyclopentyl, cyclohexyl, and cycloheptyl.
[0202] In the general formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and R P4 Examples of the aryl group represented by the formula (I) include a phenyl group, a naphthyl group, and a biphenylyl group.
[0203] In the general formula (PCA) and (PCB), X P1 The alkylene group represented by the formula (I) includes a linear or branched alkylene group having 1 to 12 carbon atoms (preferably 1 to 6 carbon atoms, more preferably 1 to 3 carbon atoms). Specific examples of the linear alkylene group include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, an n-pentylene group, an n-hexylene group, an n-heptylene group, an n-octylene group, an n-nonylene group, an n-decylene group, an n-undecylene group, and an n-dodecylene group. Specific examples of branched alkylene groups include isopropylene, isobutylene, sec-butylene, tert-butylene, isopentylene, neopentylene, tert-pentylene, isohexylene, sec-hexylene, tert-hexylene, isoheptylene, sec-heptylene, tert-heptylene, isooctylene, sec-octylene, tert-octylene, isononylene, sec-nonylene, tert-nonylene, isodecylene, sec-decylene, tert-decylene, isoundecylene, sec-undecylene, tert-undecylene, neoundecylene, isododecylene, sec-dodecylene, tert-dodecylene, and neododecylene. Among these, the alkylene group is preferably a lower alkyl group such as a methylene group, an ethylene group, or a butylene group.
[0204] In the general formula (PCA) and (PCB), X P1 The cycloalkylene group represented by the formula (I) includes a cycloalkylene group having 3 to 12 carbon atoms (preferably 3 to 10 carbon atoms, more preferably 5 to 8 carbon atoms). Specific examples of the cycloalkyl group include a cyclopropyl group, a cyclopentyl group, a cyclohexyl group, a cyclooctyl group, and a cyclododecanyl group. Of these, the cycloalkyl group is preferably a cyclohexyl group.
[0205] In the general formulas (PCA) and (PCB), R P1 , R P2 , R P3 , R P4 , and X P1 Each of the above-mentioned substituents represented by also includes groups having a further substituent. Examples of the substituent include a halogen atom (e.g., a fluorine atom, a chlorine atom), an alkyl group (e.g., an alkyl group having 1 to 6 carbon atoms), a cycloalkyl group (e.g., a cycloalkyl group having 5 to 7 carbon atoms), an alkoxy group (e.g., an alkoxy group having 1 to 4 carbon atoms), and an aryl group (e.g., a phenyl group, a naphthyl group, a biphenylyl group, etc.).
[0206] In the general formula (PCA), R P1 , and R P2 each independently preferably represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; R P1 , and R P2 More preferably, represents a hydrogen atom. In the general formula (PCB), R P3 , and R P4 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; X P1 It is preferred that represents an alkylene group or a cycloalkylene group.
[0207] Specific examples of BP polycarbonate resins include, but are not limited to, the following: In the example compounds, pm and pn indicate the copolymerization ratio.
[0208] [ka]
[0209] Here, in the P polycarbonate resin, the content (copolymerization ratio) of the structural unit represented by general formula (PCA) is preferably in the range of 5 mol % or more and 95 mol % or less with respect to all structural units constituting the polycarbonate resin, and from the viewpoint of suppressing density unevenness in grainy images, it is preferably in the range of 5 mol % or more and 50 mol % or less, and more preferably in the range of 15 mol % or more and 30 mol % or less. Specifically, in the above example compounds of BP polycarbonate resin, pm and pn indicate the copolymerization ratio (molar ratio), and pm:pn is in the range of 95:5 to 5:95, 50:50 to 5:95, and more preferably 15:85 to 30:70.
[0210] The compounding ratio of the charge transport material to the binder resin is preferably from 10:1 to 1:5 by mass.
[0211] The charge transport layer may contain other well-known additives.
[0212] The formation of the charge transport layer is not particularly limited, and a known formation method can be used. For example, the charge transport layer can be formed by forming a coating film of a coating liquid for forming the charge transport layer in which the above components are added to a solvent, drying the coating film, and heating it as necessary.
[0213] Examples of solvents for preparing the coating liquid for forming the charge transport layer include ordinary organic solvents such as aromatic hydrocarbons such as benzene, toluene, xylene, and chlorobenzene, ketones such as acetone and 2-butanone, halogenated aliphatic hydrocarbons such as methylene chloride, chloroform, and ethylene chloride, and cyclic or linear ethers such as tetrahydrofuran and ethyl ether. These solvents may be used alone or in combination of two or more.
[0214] Examples of a coating method for coating the coating liquid for forming the charge transport layer on the charge generating layer include ordinary methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating and curtain coating.
[0215] The thickness of the charge transport layer is set, for example, preferably in the range of 5 μm or more and 50 μm or less, and more preferably in the range of 10 μm or more and 30 μm or less.
[0216] (protective layer) A protective layer is provided on the photosensitive layer as necessary for the purpose of, for example, preventing chemical changes in the photosensitive layer when the photosensitive layer is charged and further improving the mechanical strength of the photosensitive layer. Therefore, it is preferable to apply a layer composed of a cured film (crosslinked film) as the protective layer. Examples of such a layer include the following layers 1) and 2).
[0217] 1) A layer composed of a cured film of a composition containing a reactive group-containing charge transport material having a reactive group and a charge transport skeleton in the same molecule (i.e., a layer containing a polymer or crosslinked product of the reactive group-containing charge transport material). 2) A layer composed of a cured film of a composition containing a non-reactive charge transport material and a reactive group-containing non-charge transport material that does not have a charge transport skeleton and has a reactive group (i.e., a layer containing a non-reactive charge transport material and a polymer or crosslinked body of the reactive group-containing non-charge transport material).
[0218] The reactive group of the reactive group-containing charge transport material may be a chain polymerizable group, an epoxy group, -OH, -OR (wherein R represents an alkyl group), -NH2, -SH, -COOH, or -SiR. Q1 3-Qn (OR Q2 ) Qn [However, R Q1 represents a hydrogen atom, an alkyl group, or a substituted or unsubstituted aryl group; R Q2 represents a hydrogen atom, an alkyl group, or a trialkylsilyl group; Qn represents an integer of 1 to 3.
[0219] The chain polymerizable group is not particularly limited as long as it is a functional group capable of radical polymerization, and is, for example, a functional group having a group containing at least a carbon double bond.Specific examples include a group containing at least one selected from a vinyl group, a vinyl ether group, a vinyl thioether group, a styryl group (vinyl phenyl group), an acryloyl group, a methacryloyl group, and derivatives thereof.Among them, the chain polymerizable group is preferably a group containing at least one selected from a vinyl group, a styryl group (vinyl phenyl group), an acryloyl group, a methacryloyl group, and derivatives thereof, because of its excellent reactivity.
[0220] The charge transporting skeleton of the reactive group-containing charge transporting material is not particularly limited as long as it is a known structure in electrophotographic photoreceptors, and examples thereof include a skeleton derived from a nitrogen-containing hole transporting compound such as a triarylamine compound, a benzidine compound, a hydrazone compound, etc., and a structure conjugated with a nitrogen atom. Among these, a triarylamine skeleton is preferred.
[0221] The reactive group-containing charge transport material having a reactive group and a charge transporting skeleton, the non-reactive charge transport material, and the reactive group-containing non-charge transport material may be selected from well-known materials.
[0222] The protective layer may contain other well-known additives.
[0223] The formation of the protective layer is not particularly limited, and a well-known formation method can be used. For example, the protective layer can be formed by forming a coating film of a coating liquid for forming the protective layer in which the above components are added to a solvent, drying the coating film, and, if necessary, subjecting it to a curing treatment such as heating.
[0224] Examples of solvents for preparing a coating solution for forming a protective layer include aromatic solvents such as toluene and xylene, ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone, ester solvents such as ethyl acetate and butyl acetate, ether solvents such as tetrahydrofuran and dioxane, cellosolve solvents such as ethylene glycol monomethyl ether, and alcohol solvents such as isopropyl alcohol and butanol. These solvents may be used alone or in combination of two or more. The protective layer-forming coating liquid may be a solvent-free coating liquid.
[0225] Examples of a method for applying the protective layer-forming coating liquid onto a photosensitive layer (e.g., a charge transport layer) include conventional methods such as dip coating, push-up coating, wire bar coating, spray coating, blade coating, knife coating, and curtain coating.
[0226] The thickness of the protective layer is set, for example, preferably in the range of 1 μm or more and 20 μm or less, and more preferably in the range of 2 μm or more and 10 μm or less.
[0227] (single-layer photosensitive layer) The single-layer type photosensitive layer (charge generation / charge transport layer) is, for example, a layer containing a charge generation material, a charge transport material, and, if necessary, a binder resin and other well-known additives. Note that these materials are the same as those described for the charge generation layer and the charge transport layer. The content of the charge generating material in the single-layer photosensitive layer is preferably 0.1% by mass to 10% by mass, more preferably 0.8% by mass to 5% by mass, based on the total solid content. The content of the charge transport material in the single-layer photosensitive layer is preferably 5% by mass to 50% by mass, based on the total solid content. The method for forming the single-layer type photosensitive layer is the same as the method for forming the charge generating layer and the charge transport layer. The thickness of the single-layer photosensitive layer is, for example, 5 μm or more and 50 μm or less, and preferably 10 μm or more and 40 μm or less.
[0228] <Image forming apparatus (and process cartridge)> The image forming apparatus according to the present embodiment includes an electrophotographic photoreceptor, a charging unit for charging the surface of the electrophotographic photoreceptor, an electrostatic latent image forming unit for forming an electrostatic latent image on the surface of the charged electrophotographic photoreceptor, a developing unit for developing the electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing toner to form a toner image, and a transfer unit for transferring the toner image to the surface of a recording medium. The electrophotographic photoreceptor according to the present embodiment is applied as the electrophotographic photoreceptor.
[0229] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as an apparatus provided with a fixing means for fixing a toner image transferred onto the surface of a recording medium; an apparatus of a direct transfer type for directly transferring a toner image formed on the surface of an electrophotographic photosensitive member onto a recording medium; an apparatus of an intermediate transfer type for primarily transferring a toner image formed on the surface of an electrophotographic photosensitive member onto the surface of an intermediate transfer member, and then secondarily transferring the toner image transferred onto the surface of the intermediate transfer member onto the surface of a recording medium; an apparatus provided with a cleaning means for cleaning the surface of an electrophotographic photosensitive member before charging after the transfer of a toner image; an apparatus provided with a discharging means for irradiating the surface of an electrophotographic photosensitive member with discharging light to discharge the surface before charging after the transfer of a toner image; and an apparatus provided with an electrophotographic photosensitive member heating member for increasing the temperature of the electrophotographic photosensitive member and reducing the relative temperature.
[0230] In the case of an intermediate transfer type device, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the electrophotographic photosensitive body onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.
[0231] The image forming apparatus according to the present embodiment may be either a dry development type image forming apparatus or a wet development type image forming apparatus (a development type using a liquid developer).
[0232] In the image forming apparatus according to the present embodiment, for example, a portion including an electrophotographic photosensitive member may be a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge including an electrophotographic photosensitive member according to the present embodiment is preferably used. In addition to the electrophotographic photosensitive member, the process cartridge may include at least one selected from the group consisting of a charging means, an electrostatic latent image forming means, a developing means, and a transfer means.
[0233] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.
[0234] FIG. 2 is a schematic diagram showing an example of the image forming apparatus according to the present embodiment. As shown in FIG. 2, the image forming apparatus 100 according to the present embodiment includes a process cartridge 300 including an electrophotographic photoreceptor 7, an exposure device 9 (an example of an electrostatic latent image forming means), a transfer device 40 (a primary transfer device), and an intermediate transfer body 50. In the image forming apparatus 100, the exposure device 9 is disposed at a position where it can expose the electrophotographic photoreceptor 7 from the opening of the process cartridge 300, the transfer device 40 is disposed at a position facing the electrophotographic photoreceptor 7 via the intermediate transfer body 50, and the intermediate transfer body 50 is disposed with a part of it in contact with the electrophotographic photoreceptor 7. Although not shown, the image forming apparatus 100 also includes a secondary transfer device that transfers the toner image transferred to the intermediate transfer body 50 to a recording medium (e.g., paper). The intermediate transfer body 50, the transfer device 40 (a primary transfer device), and the secondary transfer device (not shown) correspond to an example of a transfer means.
[0235] 2 supports an electrophotographic photoreceptor 7, a charging device 8 (an example of a charging means), a developing device 11 (an example of a developing means), and a cleaning device 13 (an example of a cleaning means) integrally within a housing. The cleaning device 13 has a cleaning blade (an example of a cleaning member) 131, which is disposed so as to come into contact with the surface of the electrophotographic photoreceptor 7. The cleaning member may not be in the form of the cleaning blade 131, but may be a conductive or insulating fibrous member, which may be used alone or in combination with the cleaning blade 131.
[0236] FIG. 2 shows an example of an image forming apparatus equipped with a fibrous member 132 (roll-shaped) that supplies lubricant 14 to the surface of electrophotographic photosensitive member 7, and a fibrous member 133 (flat brush-shaped) that assists in cleaning, which may be arranged as needed.
[0237] Hereinafter, each configuration of the image forming apparatus according to this embodiment will be described.
[0238] -Charging device- As the charging device 8, for example, a contact type charger using a conductive or semiconductive charging roller, charging brush, charging film, charging rubber blade, charging tube, etc. Also, a non-contact type roller charger, a scorotron charger or corotron charger that utilizes corona discharge, or other chargers known per se, can be used.
[0239] -Exposure equipment- The exposure device 9 may be, for example, an optical device that exposes the surface of the electrophotographic photoreceptor 7 with light such as semiconductor laser light, LED light, or liquid crystal shutter light in a predetermined image. The wavelength of the light source is within the spectral sensitivity range of the electrophotographic photoreceptor. The wavelength of the semiconductor laser is mainly near infrared light having an oscillation wavelength of about 780 nm. However, it is not limited to this wavelength, and a laser having an oscillation wavelength of 600 nm or a blue laser having an oscillation wavelength of 400 nm to 450 nm may also be used. In addition, a surface-emitting laser light source capable of outputting multiple beams is also effective for forming a color image.
[0240] -Developing device- The developing device 11 may be, for example, a general developing device that develops by contacting or non-contacting a developer. The developing device 11 is not particularly limited as long as it has the above-mentioned functions, and may be selected according to the purpose. For example, it may be a known developing device that has a function of attaching a one-component developer or a two-component developer to the electrophotographic photoreceptor 7 using a brush, roller, or the like. Among them, it is preferable to use a developing roller that holds a developer on its surface.
[0241] The developer used in the developing device 11 may be a one-component developer containing only toner, or may be a two-component developer containing toner and a carrier. The developer may be magnetic or non-magnetic. Well-known developers are used.
[0242] -Cleaning device- The cleaning device 13 is a cleaning blade type device equipped with a cleaning blade 131 . In addition to the cleaning blade system, a fur brush cleaning system or a simultaneous development and cleaning system may also be used.
[0243] -Transfer device- Examples of the transfer device 40 include known transfer chargers such as a contact type transfer charger using a belt, roller, film, rubber blade, etc., and a scorotron transfer charger or corotron transfer charger that utilizes corona discharge.
[0244] -Intermediate transfer body- A belt-like intermediate transfer belt containing semiconductive polyimide, polyamideimide, polycarbonate, polyarylate, polyester, rubber, etc. is used as the intermediate transfer body 50. The intermediate transfer body may be in the form of a drum other than a belt.
[0245] FIG. 3 is a schematic diagram showing another example of the image forming apparatus according to the present embodiment. 3 is a tandem-type multi-color image forming apparatus equipped with four process cartridges 300. In the image forming apparatus 120, the four process cartridges 300 are arranged in parallel on the intermediate transfer body 50, and one electrophotographic photosensitive body is used for each color. The image forming apparatus 120 has the same configuration as the image forming apparatus 100, except that it is a tandem type.
[0246] <Other uses of fluorine-containing resin particles> The fluorine-containing resin particles according to this embodiment are suitably used as an external additive for toners, an external additive for powder paints, an additive for paints, an additive for functional coating materials, and an additive for the surface layer of an electrophotographic photoreceptor. For example, when the fluorine-containing resin particles are used as an external additive for toner, the toner may be an electrostatic image developing toner having toner particles and fluorine-containing resin particles as an external additive. The toner particles contain a resin (binder resin). The toner particles may contain other additives such as a colorant and a release agent, if necessary. When the fluorine-containing resin particles are used as an external additive for powder coating, the powder coating may be, for example, a powder coating having powder particles and fluorine-containing resin particles as an external additive. The powder particles include a thermosetting resin and a thermosetting agent. The powder particles may include other additives such as a colorant, if necessary. EXAMPLES
[0247] Examples of the present invention will be described below, but the present invention is not limited to the following examples. In addition, "parts" and "%" are based on mass unless otherwise specified.
[0248] <Example 1> -Production of fluorine-containing resin particles (1)- Fluorine-containing resin particles (1) were produced as follows. 100 parts by mass of commercially available homopolytetrafluoroethylene fine powder (standard specific gravity 2.175 measured according to ASTM D 4895 (2004)) and 2.4 parts by mass of ethanol as an additive were placed in a bag made of barrier nylon, and the entire bag was replaced with nitrogen. After that, it was irradiated with 150 kGy of cobalt-60 gamma rays at room temperature to obtain a low molecular weight polytetrafluoroethylene powder. The obtained powder was pulverized to obtain fluorine-containing resin particles (1).
[0249] <Example 2> -Production of fluorine-containing resin particles (2)- 100 parts by mass of fluorine-containing resin particles (1) and 400 parts by mass of methanol were collected, washed with a stirrer at 250 rpm for 10 minutes while irradiating with ultrasonic waves, and the supernatant was filtered. After repeating this operation three times, the filtrate was dried under reduced pressure at 60°C for 17 hours to produce fluorine-containing resin particles (2).
[0250] <Example 3> -Production of fluorine-containing resin particles (3)- Fluorine-containing resin particles (3) were produced in the same manner as in the production of fluorine-containing resin particles (1), except that the entire bag was replaced with nitrogen so that the oxygen concentration was 10%.
[0251] <Example 4> -Production of fluorine-containing resin particles (4)- Fluorine-containing resin particles (4) were produced in the same manner as in the production of the fluorine-containing resin particles (2), except that the fluorine-containing resin particles (3) were used instead of the fluorine-containing resin particles (1) in the production of the fluorine-containing resin particles (2).
[0252] <Example 5> -Production of fluorine-containing resin particles (5)- In the autoclave, 3 liters of deionized water, 3.0 g of ammonium perfluorooctanoate, and 120 g of paraffin wax (manufactured by Nippon Oil Corporation) as an emulsion stabilizer were charged, and the system was replaced with nitrogen three times and with TFE (tetrafluoroethylene) twice to remove oxygen, and then the internal pressure was set to 1.0 MPa with TFE, and the internal temperature was kept at 70°C while stirring at 250 rpm. Next, 150 cc of ethane as a chain transfer agent at normal pressure and 20 ml of an aqueous solution in which 300 mg of ammonium persulfate as a polymerization initiator was dissolved were charged into the system to start the reaction. During the reaction, the temperature in the system was kept at 70°C, and TFE was continuously supplied so that the internal pressure of the autoclave was always kept at 1.0 ± 0.05 MPa. When the amount of TFE consumed in the reaction after the addition of the initiator reached 1000 g, the supply of TFE and stirring were stopped, and the reaction was terminated. The particles were then separated by centrifugation, and 400 parts by mass of methanol was collected and washed for 10 minutes at 250 rpm with ultrasonic irradiation, and the supernatant was filtered. This procedure was repeated three times, and the filtrate was dried under reduced pressure at 60°C for 17 hours. Through the above steps, fluorine-containing resin particles (5) were produced.
[0253] <Example 6> -Production of fluorine-containing resin particles (6)- Fluorine-containing resin particles (6) were produced in the same manner as in the production of fluorine-containing resin particles (5) except that 5 g of triethylamine was added after the end of the reaction.
[0254] <Comparative Example 1> -Production of fluorine-containing resin particles (C1)- Fluorine-containing resin particles (C1) were produced in the same manner as in the production of fluorine-containing resin particles (1), except that the radiation exposure was carried out in air. <Comparative Example 2> -Production of fluorine-containing resin particles (C2)- Fluorine-containing resin particles (C2) were produced in the same manner as in the production of the fluorine-containing resin particles (2), except that the fluorine-containing resin particles (C1) were used instead of the fluorine-containing resin particles (1).
[0255] <Comparative Example 3> -Production of fluorine-containing resin particles (C3)- Fluorine-containing resin particles (C3) were produced in the same manner as in the production of fluorine-containing resin particles (6), except that the washing step was carried out once.
[0256] <Evaluation> (Various measurements) The fluorine-containing resin particles were measured for the following properties according to the methods described above. Carboxyl group (indicated as "COOH" in the table) with 10 carbon atoms 6 Number of pieces per piece (pieces) Amount of basic compounds (ppm) PFOA content (ppb)
[0257] (Actual machine evaluation) -Preparation of photoconductor- Using the obtained fluorine-containing resin particles, a photoreceptor was produced as follows.
[0258] Zinc oxide: (average particle size 70 nm: manufactured by Teika Co., Ltd.: specific surface area value 15 m 2 100 parts of zinc oxide (100 parts by weight / g) was mixed with 500 parts of tetrahydrofuran and stirred, and 1.3 parts of a silane coupling agent (KBM503: manufactured by Shin-Etsu Chemical Co., Ltd.) was added and stirred for 2 hours. Thereafter, the toluene was distilled off by reduced pressure distillation, and the mixture was baked at 120°C for 3 hours to obtain zinc oxide surface-treated with a silane coupling agent. 110 parts of zinc oxide that had been subjected to the surface treatment was mixed with stirring in 500 parts of tetrahydrofuran, and a solution in which 0.6 parts of alizarin was dissolved in 50 parts of tetrahydrofuran was added, followed by stirring for 5 hours at 50° C. Thereafter, the zinc oxide to which alizarin had been added was filtered out by filtration under reduced pressure, and further dried under reduced pressure at 60° C. to obtain zinc oxide to which alizarin had been added. A mixed solution was obtained by mixing 60 parts of this alizarin-added zinc oxide, 13.5 parts of a curing agent (blocked isocyanate Sumidur 3175, manufactured by Sumitomo Bayern Urethane Co., Ltd.), 15 parts of butyral resin (S-LEC BM-1, manufactured by Sekisui Chemical Co., Ltd.), and 85 parts of methyl ethyl ketone. 38 parts of this mixed solution and 25 parts of methyl ethyl ketone were mixed, and dispersed for 2 hours in a sand mill using 1 mmφ glass beads, to obtain a dispersion solution. To the resulting dispersion, 0.005 parts of dioctyltin dilaurate as a catalyst and 45 parts of silicone resin particles (Tospearl 145, Momentive Performance Materials Japan LLC) were added to obtain a coating solution for the undercoat layer. This coating solution was applied to a cylindrical aluminum substrate by dip coating, and dried and cured at 170°C for 30 minutes to obtain a 22μm thick undercoat layer.
[0259] Next, 1 part of hydroxygallium phthalocyanine, which has strong diffraction peaks at Bragg angles (2θ±0.2°) of 7.5°, 9.9°, 12.5°, 16.3°, 18.6°, 25.1°, and 28.3° in the X-ray diffraction spectrum, was mixed with 1 part of polyvinyl butyral (S-LEC BM-S, manufactured by Sekisui Chemical Co., Ltd.) and 80 parts of n-butyl acetate, and the mixture was dispersed together with glass beads using a paint shaker for 1 hour to prepare a coating solution for the charge generation layer. The resulting coating solution was dip-coated on the conductive support on which the undercoat layer had been formed, and dried by heating at 100°C for 10 minutes to form a charge generation layer with a thickness of 0.15 μm.
[0260] 45 parts of a benzidine compound represented by the following formula (CTM1) as a charge transport material, and 55 parts of a polymer compound (viscosity average molecular weight: 40,000) having a repeating unit represented by the following formula (PCZ1) as a binder resin were dissolved in 350 parts of toluene and 150 parts of tetrahydrofuran, and 10 parts of fluorine-containing resin particles and 1 part of fluorine-containing dispersant GF400 (manufactured by Toa Gosei Co., Ltd.) were added, and the mixture was treated five times with a high-pressure homogenizer to prepare a coating liquid for a charge generation layer. The obtained coating liquid was applied onto the charge generation layer by a dip coating method, and heated at 130°C for 45 minutes to form a charge transport layer with a thickness of 13 μm.
[0261] [ka]
[0262] [ka]
[0263] Through the above steps, each photoreceptor was produced.
[0264] -Image forming device for evaluation- The obtained electrophotographic photoreceptor was mounted on a DocuCentre-V C7775 manufactured by Fuji Xerox Co., Ltd. In addition, a surface potential probe was provided in the area to be measured at a position 1 mm away from the surface of the photoreceptor using a surface potential meter (Trek 334 manufactured by Trek Corporation). This apparatus was used as an image forming apparatus for evaluation.
[0265] -Evaluation of electrostatic charge- The chargeability of the resulting photoreceptor was evaluated as follows. After setting the surface potential after charging to -700V using the image forming device for evaluation, 70,000 full-surface halftone images with an image density of 30% were output onto A4 paper in a high temperature and high humidity environment (temperature 28°C, humidity 85% RH environment).Then, the surface potential was measured using a surface potential meter and evaluated according to the following criteria. 5: Surface potential is between -700V and -690V 4: Surface potential is between -690V and -675V 3: Surface potential is between -675V and -660V (level that does not pose a problem in practical use) 2: Surface potential is between -660V and -640V 1: Surface potential is -640V or more
[0266] -Evaluation of residual potential- The residual potential of the resulting photoreceptor was evaluated as follows. Using the evaluation image forming device, the surface potential after charging was set to -700V, and then 70,000 full-surface halftone images with an image density of 30% were printed on A4 paper in a high temperature and high humidity environment (temperature 28°C, humidity 85% RH). Then, using a surface potential meter, the initial residual potential of the photoconductor that had been de-electrified after 100 sheets were printed, and the residual potential of the photoconductor that had been de-electrified over time after 70,000 sheets were measured, and the difference (absolute value) was calculated and evaluated according to the following criteria. 5: Residual potential difference is less than 5V 4: Residual potential difference is 5V or more and less than -10V 3: Residual potential difference is 10V or more but less than -20V (level that does not cause any problems in practical use) 2: Residual potential difference is 20V or more and less than 50V 1: Residual potential difference is 50V or more
[0267] [Table 1]
[0268] From the above results, it is understood that the charging property and residual potential of the photoconductor in this embodiment are better than those in the comparative example. Therefore, it is understood that the fluorine-containing resin particles of this example have excellent charging properties. As shown in Examples 1 and 2, when the number of carboxyl groups and the amount of basic compound are controlled within a specific range, even if the number of carboxyl groups is somewhat large, as long as the amount of basic compound is relatively large, the ionic conductivity and hole trapping property cancel each other out, and the charging property tends to improve.
[0269] <Examples 11 to 17, Comparative Examples 11 to 12> Photoreceptors of Examples 11 to 17 and Comparative Examples 11 and 12 were produced in the same manner as described above using the fluorine-containing resin particles shown in Table 2. However, for the charge transport layer, the charge transport material (CTM type) and binder resin (indicated as "PC type" in the table) shown in Table 2 were used.
[0270] Details of the abbreviations in Table 2 are as follows. · BPZ1: The following polycarbonate resin (pm:pn = 0.2:0.8, viscosity average molecular weight = 55,000) [ka] · BPZ2: The following polycarbonate resin (pm:pn = 0.3:0.7, viscosity average molecular weight = 50,000) [ka] PCZ1: Polycarbonate resin (viscosity average molecular weight = 40,000) [ka] CTM1: The following compound [ka] CTM2: The following compound (charge transport material represented by structural formula (CT1A) (example compound (CT1-3))) [ka] <Evaluation> The photoreceptors of Examples 11 to 17 and Comparative Examples 11 and 12 were evaluated as follows. (dispersibility) The dispersibility of the fluorine-containing resin particles was evaluated visually and by the following method. From the substrate of the photoreceptor obtained in each example, a slice of the laminate from the undercoat layer to the surface charge transport layer 1 was cut using a single-edged trimming razor (manufactured by Nisshin EM Co., Ltd.), and the slice was embedded in a photocurable acrylic resin (product name D-800: manufactured by JEOL Datum Co., Ltd.). Next, the slice was cut using a microtome method (microtome device: manufactured by LEICA Co., Ltd.) using a diamond knife so that the cross section of the slice of the laminate was revealed. The cross section of the slice was observed with a laser microscope OLS-1100 manufactured by Olympus Optical Co., Ltd. under the condition of a step amount of 0.01 μm. The evaluation criteria are as follows: A: Both visual and laser microscope evaluations show that the particles are uniformly dispersed, with no aggregation. B: Laser microscope evaluation reveals weak localized aggregation (less than 5% of the area), but this is not problematic. C: Laser microscope evaluation revealed some aggregation (less than 10% of the area), but this was not problematic for practical use. D: Strong aggregation is observed, to the extent that a slight abnormal noise occurs when the machine is stopped. E: Strong agglomeration occurs overall. The level is such that obvious abnormal noise occurs during machine operation.
[0271] (image quality) The image quality (graininess and uneven density of an image) was evaluated as follows. A 50% halftone image was formed in an environment of room temperature 28°C and humidity 85%, and the graininess of the image was observed visually and with a magnifying glass. The evaluation criteria are as follows: A: No uneven density. B: When magnified with a loupe, there is some unevenness in density (less than 5% of the area), but this does not cause any problems in actual use. C: When magnified with a loupe (area less than 10%), uneven density can be seen, but this does not pose a problem in practical use. D: Unevenness in density was confirmed by visual inspection (area of 10% or more), and there was a problem with the image quality when using high-resolution equipment such as color machines. E: Visible unevenness in density is observed. Problematic for practical use.
[0272] (scratch) The surface of the photoreceptor (the surface of the charge transport layer, which is the outermost layer) was evaluated for scratches as follows. After forming 10,000 images in an environment with a room temperature of 28°C and a humidity of 85%, the surface of the photoconductor was observed visually and with a microscope (digital microscope, Keyence Corporation, model number: VHX-700) at 500 times magnification. The evaluation criteria are as follows: A: No scratches on the photoconductor surface B: Minor scratches can be observed under a microscope. C: Scratches are clearly visible under a microscope, but not visible to the naked eye. No problems in practical use. D: Minor scratches are visible to the naked eye, causing problems in terms of image quality. E: Scratches are clearly visible to the naked eye. Image quality is questionable.
[0273] [Table 2]
[0274] From the above results, the number of carboxyl groups is 10 6 It can be seen that when 0 to 30 fluorine-containing resin particles are used, the dispersibility of the fluorine-containing resin particles is high and the image quality (uneven density of grainy images) is good, even when a polycarbonate resin containing a structural unit represented by the general formula (PCA) and a structural unit represented by the general formula (PCB) is used. It can also be seen that scratches on the surface of the photoconductor (surface of the charge transport layer, which is the outermost layer) are suppressed.
[0275] <Examples 21 to 39> (Production of Fluorine-Based Graft Polymer (1)) Fluorine-based graft polymer (1) was synthesized as follows. 5 parts by mass of methyl isobutyl ketone was placed in a 500 mL reaction vessel equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen gas inlet, and the solution temperature in the reaction vessel was maintained at 80° C. under a nitrogen gas atmosphere. A mixed solution of 9 parts by mass of perfluorohexyl ethyl acrylate, 21 parts by mass of macromonomer AA-6 (manufactured by Toagosei Co., Ltd.), 0.25 parts by mass of Perhexyl O (manufactured by NOF Corporation) as a polymerization initiator, and 45 parts by mass of methyl isobutyl ketone was dripped into the reaction vessel over 2 hours using a syringe drip pump. After the dripping was completed, stirring was continued for another 2 hours, and then the solution temperature was raised to 90° C. and stirred for another 2 hours. 400 ml of methanol was added dropwise to the methyl isobutyl ketone resin solution obtained after the reaction to precipitate a fluorine-based graft polymer. The precipitated solid was filtered and dried to obtain 21.2 g of a fluorine-based graft polymer (1).
[0276] (Production of Fluorine-Based Graft Polymer (2)) Fluorine-based graft polymer (2) (24.1 g) was obtained by synthesizing fluorine-based graft polymer (1) in the same manner as in the synthesis of fluorine-based graft polymer (1), except that the amount of perhexyl O was changed from 0.25 parts by mass to 0.2 parts by mass.
[0277] (Production of Fluorine-Based Graft Polymer (3)) The synthesis of fluorine-based graft polymer (3) (19.8 g) was obtained in the same manner as in the synthesis of fluorine-based graft polymer (1), except that Perhexyl O was replaced with Purble PV (manufactured by NOF Corporation).
[0278] (Production of Fluorine-Based Graft Polymer (4)) In the synthesis of the fluorine-based graft polymer (1), the amount of perfluorohexylethyl acrylate was changed from 9 parts by mass to 11 parts by mass, and the amount of the macromonomer AA-6 was changed from 21 parts by mass to 19 parts by mass, but the same procedure as in the synthesis of the fluorine-based graft polymer (1) was repeated to produce 23 g of a fluorine-based graft polymer (4).
[0279] (Production of Fluorine-Based Graft Polymer (5)) In the synthesis of the fluorine-based graft polymer (1), the amount of perfluorohexyl ethyl acrylate was changed from 9 parts by mass to 11 parts by mass, the amount of macromonomer AA-6 was changed from 21 parts by mass to 19 parts by mass, and the amount of methyl isobutyl ketone was changed from 45 parts by mass to 40 parts by mass, but the same procedure was carried out as in the synthesis of the fluorine-based graft polymer (1), to produce 20.2 g of a fluorine-based graft polymer (5).
[0280] (Production of Fluorine-Based Graft Polymer (6)) 21.5 g of fluorine-based graft polymer (6) was produced in the same manner as in the synthesis of fluorine-based graft polymer (1), except that the amount of methyl isobutyl ketone was changed from 45 parts by mass to 60 parts by mass.
[0281] (Production of Fluorine-Based Graft Polymer (7)) In the synthesis of the fluorine-based graft polymer (1), the amount of Perhexyl O was changed from 0.25 parts by mass to 0.2 parts by mass, and the stirring time after the completion of the dropwise addition was changed from 2 hours to 5 hours. In the same manner as in the synthesis of the fluorine-based graft polymer (1), 24 g of a fluorine-based graft polymer (7) was produced.
[0282] (Production of Fluorine-Based Graft Polymer (8)) Fluorine-based graft polymer (8) (17 g) was produced in the same manner as in the synthesis of fluorine-based graft polymer (1), except that perfluorobutyl ethyl acrylate was used instead of perfluorohexyl ethyl acrylate.
[0283] (Production of Fluorine-Based Graft Polymer (C1)) 400 g of methanol was added dropwise to 150 g (solid content 25 wt%) of fluorine-based graft polymer "GF400 (Toagosei Co., Ltd.)" and the precipitated fluorine-based graft polymer was collected by filtration and dried to obtain 31 g of fluorine-based graft polymer. This refined product was designated as a fluorine-based graft polymer (C1).
[0284] (Production of Fluorine-Based Graft Polymer (C2)) The solvent was distilled off from 50 g of fluorine-based graft polymer "GF400 (Toagosei Co., Ltd.)" to obtain 12.6 g of fluorine-graft polymer. This was named fluorine-based graft polymer (C2).
[0285] (Production of Fluorine-Based Graft Polymer (C3)) In the synthesis of the fluorine-based graft polymer (1), 26 g of a fluorine-based graft polymer (C3) was produced in the same manner as in the synthesis of the fluorine-based graft polymer (1), except that after the reaction, 400 ml of methanol was added and the solvent was distilled off without purification treatment.
[0286] (Production of Fluorine-Based Graft Polymer (C4)) 50 g of fluorine-based graft polymer "LE-604 (Kyoeisha Chemical Co., Ltd.)" was dropped into 250 ml of hexane, and the precipitated fluorine-based graft polymer was filtered and purified. This refined product was designated as a fluorine-based graft polymer (C4).
[0287] (Production of Fluorine-Based Graft Polymer (C5)) In the synthesis of the fluorine-based graft polymer (1), the amount of perfluorohexylethyl acrylate was changed from 9 parts by mass to 16 parts by mass, and the amount of macromonomer AA-6 was changed from 21 parts by mass to 14 parts by mass. In the same manner as in the synthesis of the fluorine-based graft polymer (1), 14 g of a fluorine-based graft polymer (C5) was produced.
[0288] Photoreceptors of Examples 21 to 39 were produced in the same manner as the photoreceptor of Example 1, except that the obtained fluorine-based graft polymer was used as a fluorine-containing dispersant.
[0289] <Evaluation> (Various measurements) The following properties of the fluorine-based graft polymer were measured according to the methods described above. Peak area ratio in infrared absorption spectrum (wave number 1020cm -1 Wave number 1308cm -1 Peak area / wavenumber in the range of 1673cm -1 Wave number 1779cm -1 (In the table, this is indicated as "peak area ratio F / C=O") ·Weight average molecular weight Mw
[0290] (Evaluation of dispersion stability of fluorine-containing resin particles (centrifugal separation test)) The dispersion stability of the fluorine-containing resin particles (centrifugal separation test) was evaluated as follows. Using the types and amounts of fluorine-containing resin particles and fluorine-based graft polymers shown in Table 1, a dispersion coating liquid similar to that used in the preparation of the charge transport layer of the electrophotographic photoreceptor 1 was prepared. This dispersion coating liquid was placed in a 1.5 ml sample tube and centrifuged at 6,000 rpm for 5 minutes using a centrifuge. The results were visually evaluated according to the following criteria. A++: The entire sample tube is opaque and there is absolutely no settling of fluorine-containing resin particles. A+: The entire sample tube is opaque, but there is a slight difference in concentration between the top and bottom, but this is not a problem. A: The entire inside of the sample tube is opaque, but a small amount of fluorine-containing resin particle deposits are visible at the bottom, but this is acceptable. B: The sample tube was transparent, and there was clearly a deposit of fluorine-containing resin particles at the bottom, resulting in poor dispersion stability. C: The entire sample tube was transparent, with most of the fluorine-containing resin particles deposited at the bottom, and the dispersion stability was poor.
[0291] (Cleaning performance evaluation) The cleaning ability of the photoreceptor was evaluated as follows. The photoreceptor of each example was mounted on an image forming apparatus (manufactured by Fuji Xerox Co., Ltd.: product name ApeosPort-IVC3375). Using this apparatus, halftone images with an image density of 5% were formed on A4 paper (210×297 mm, manufactured by Fuji Xerox Co., Ltd., P paper) in the initial state and under a high temperature and high humidity environment (28° C., 85 RH%) until the cumulative number of rotations of the photoreceptor reached 100,000 cycles. After that, 20 halftone images with an image density of 50% were output continuously, and the image on the 20th sheet was visually observed to evaluate whether or not image defects such as streaks occurred. And the evaluation was performed according to the following criteria. A+: No problems whatsoever with image quality. A: There are minor streak defects, but they do not affect the image quality. B: There is a clear streak defect and it is at a problematic level. C: There is a streak defect on the front surface, which is at a problematic level.
[0292] [Table 3]
[0293] [Table 4]
[0294] From the above results, it is understood that Examples 21 to 32, in which a specific fluorine-based graft polymer was used as a fluorine-containing dispersant, are superior in terms of the dispersion stability of the fluorine-containing resin particles as well as the cleaning properties, compared with Examples 33 to 39. [Explanation of symbols]
[0295] REFERENCE SIGNS LIST 1 undercoat layer, 2 charge generating layer, 3 charge transport layer, 4 conductive substrate, 7A, 7 electrophotographic photoreceptor, 8 charging device, 9 exposure device, 11 developing device, 13 cleaning device, 14 lubricant, 40 transfer device, 50 intermediate transfer body, 100 image forming apparatus, 120 image forming apparatus, 131 cleaning blade, 132 fibrous member (roll type), 133 fibrous member (flat brush type), 300 process cartridge
Claims
1. A conductive substrate and a photosensitive layer provided on the conductive substrate, The outermost layer has a carboxyl group with a carbon number of 10 6 the layer is made of a layered material containing fluorine-containing resin particles, the number of which is from 0 to 30 per particle and the amount of a basic compound is from 0 ppm to 3 ppm, a dispersant having fluorine atoms adhered to the surface of the fluorine-containing resin particles, The fluorine-containing dispersant has an infrared absorption spectrum in which the peak area ratio in the wavenumber range of 1020 cm -1 to 1308 cm -1 to the peak area in the wavenumber range of 1673 cm -1 to 1779 cm -1 is 2.7 to 4.
8.
2. The number of the carboxyl groups is 10 6 2. The electrophotographic photoreceptor according to claim 1, wherein the number of particles per particle is from 0 to 20, and the amount of the basic compound is from 0 ppm to 3 ppm.
3. The amount of the carboxyl group is 10 6 2. The electrophotographic photoreceptor according to claim 1, wherein the number of particles per particle is from 0 to 20, and the amount of the basic compound is from 0 ppm to 1.5 ppm.
4. 4. The electrophotographic photoreceptor according to claim 1, wherein the basic compound is an amine compound.
5. 5. The electrophotographic photoreceptor according to claim 1, wherein the basic compound has a boiling point of 40° C. or higher and 130° C. or lower.
6. 6. The electrophotographic photoreceptor according to claim 1, wherein the amount of perfluorooctanoic acid is from 0 ppb to 25 ppb.
7. 7. The electrophotographic photoreceptor according to claim 6, wherein the amount of perfluorooctanoic acid is from 0 ppb to 20 ppb.
8. The electrophotographic photoreceptor according to claim 1, wherein the outermost layer comprises a polycarbonate resin.
9. The electrophotographic photoreceptor according to any one of claims 1 to 8, wherein the outermost layer contains a polycarbonate resin containing a structural unit represented by the following general formula (PCA) and a structural unit represented by the following general formula (PCB): 【Chemistry 1】 (In the general formulas (PCA) and (PCB), R P1 , R P2 , R P3 , and R P4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 5 to 7 carbon atoms, or an aryl group having 6 to 12 carbon atoms. P1 represents a phenylene group, a biphenylene group, a naphthylene group, an alkylene group, or a cycloalkylene group.
10. 10. The electrophotographic photoreceptor according to claim 1, wherein the outermost layer contains a charge transport material having a butadiene structure and a triarylamine structure.
11. The electrophotographic photoreceptor according to claim 1, wherein the weight average molecular weight of the dispersant having a fluorine atom is from 20,000 to 200,000.
12. The electrophotographic photoreceptor according to any one of claims 1 to 11 is provided, A process cartridge that is detachably attached to an image forming apparatus.
13. The electrophotographic photoreceptor according to any one of claims 1 to 11, a charging means for charging the surface of the electrophotographic photoreceptor; an electrostatic latent image forming means for forming an electrostatic latent image on the charged surface of the electrophotographic photoreceptor; a developing unit for developing an electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing a toner to form a toner image; a transfer means for transferring the toner image onto a surface of a recording medium; An image forming apparatus comprising:
Citation Information
Patent Citations
Electrophotographic sensitive body
JP1989255862A
Electrophotographic photoreceptor
JP1995134435A
Ultrafine powdery crosslinked polytetrafluoroethylene resin and preparation thereof
JP2000026614A
Electrophotographic photoreceptor, method for manufacturing electrophotographic photoreceptor, process cartridge, and image forming apparatus
JP2004191869A
Electrophotographic photosensitive member, method of manufacturing electrophotographic photosensitive member, process cartridge, and electrophotographic apparatus
JP2009104145A