Method for post-treatment of silicon nitride-based dielectric films using high energy low dose plasma
By applying a helium-containing high-energy, low-dose plasma to silicon nitride films, the process addresses incomplete filling in high aspect ratio gaps and trenches, achieving denser and more uniform dielectric layers with improved mechanical properties and etch rates.
Patent Information
- Application Number
- JP2021572329
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-06
- Filing Date
- 2020-06-03
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-06-03
AI Technical Summary
Existing semiconductor manufacturing processes face challenges in completely filling high aspect ratio gaps and trenches with silicon nitride-based dielectric films due to limited solidification depth, leading to incomplete filling and inferior mechanical properties.
Exposing silicon nitride-based dielectric films to a helium-containing high-energy, low-dose plasma with controlled ion energy and flux density to break Si-H and N-H bonds, promoting crosslinking and densification of the films.
The process enhances the filling of high aspect ratio features with silicon nitride films, improving mechanical properties and etch rates without causing significant damage, resulting in denser and more uniform dielectric layers.
Smart Images

Figure 0007556891000002 
Figure 0007556891000003 
Figure 0007556891000009
Abstract
Description
[Technical field]
[0001] background Field FIELD OF THE DISCLOSURE Embodiments of the present disclosure relate generally to flowable gap-fill films and manufacturing processes thereof, and more specifically to post-treatment of the flowable films with high-energy, low-dose plasma. [Background technology]
[0002] 2. Description of Related Art The fabrication of miniaturized semiconductor devices, including shallow trench isolation (STI), intermetal dielectric (IMD) layers, interlayer dielectric (ILD) layers, premetal dielectric (PMD) layers, passivation layers, fin field effect transistors (FinFETs), etc., faces advanced lithographic challenges to pattern nanoscale gate structures. Silicon nitride is one of the primary dielectric materials used in such structures. A dielectric precursor containing silicon and nitrogen in the liquid phase is delivered to gaps and trenches on a substrate (called a flowable film) and then hardened in the solid phase to a silicon nitride (SiN)-based dielectric film, typically by vapor annealing, ultraviolet (UV) exposure, hot pressing, and sintering at high temperatures, to form void-free gaps and trenches. Filling is performed by flowable chemical vapor deposition (CVD). However, such solidification process is limited to a certain depth within the high aspect ratio feature, so that the feature is not completely filled with silicon nitride (SiN)-based dielectric film. In some cases, the flowable film is treated with a standard high density plasma (HDP) containing high energy ions to increase the solidification depth. However, it is known that such HDP treatment does not penetrate the silicon nitride (SiN)-based dielectric film and does not increase the solidification depth to the depth of the high aspect ratio feature. Thus, the wet etch selectivity of the material within the high aspect ratio feature (partially containing silicon nitride) to silicon oxide is lower than that of silicon nitride to silicon oxide.
[0003] Therefore, new solidification processes are needed to form flowable films that can fill high aspect ratio gaps and trenches and have improved mechanical properties, such as improved wet etch rate (WERR, <2:1) compared to silicon oxide. DISCLOSURE OF THEINVENTION
[0004] overview The embodiments described herein generally relate to a method for post-treating a silicon nitride (SiN)-based dielectric film formed on a surface of a substrate, the method including placing the substrate having the silicon nitride (SiN)-based dielectric film formed thereon in a processing chamber and exposing the silicon nitride (SiN)-based dielectric film to a helium-containing high-energy, low-dose plasma in the processing chamber. The energy of helium ions in the helium-containing high-energy, low-dose plasma is between 1 eV and 3.01 eV, and the flux density of helium ions in the helium-containing high-energy, low-dose plasma is greater than 5×10 15 ions / cm 2 1.37 x 10 seconds 16 ions / cm 2 -seconds.
[0005]
[0013] An embodiment of the present disclosure may further provide a method of forming and post-treating a silicon nitride (SiN)-based dielectric film on a surface of a substrate, the method comprising: delivering a silicon and nitrogen-containing dielectric precursor onto a substrate disposed in a processing region of a first chamber; providing a radical flux to the processing region of the first chamber and exposing the delivered dielectric precursor to a helium-containing high-energy low-dose plasma in a second chamber. The energy of helium ions in the helium-containing high-energy low-dose plasma is between 1 eV and 3.01 eV, and the flux density of helium ions in the helium-containing high-energy low-dose plasma is greater than 5×10 15 ions / cm 2 1.37 x 10 seconds 16 ions / cm 2 -seconds.
[0006] BRIEF DESCRIPTION OF THE DRAWINGS So that the above-mentioned features of the present disclosure can be understood in detail, a more particular description of the present disclosure briefly summarized above can be had by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings illustrate only typical embodiments of the present disclosure and therefore should not be considered as limiting its scope. [Brief description of the drawings]
[0007] [Figure 1] 1 is a flow chart illustrating a method of forming a flowable film according to one embodiment. [Diagram 2] 1 is a schematic diagram of a cluster tool according to one embodiment. [Figure 3A] 1 is a schematic diagram of a deposition chamber according to one embodiment. [Figure 3B] FIG. 2 is a schematic bottom view of a showerhead according to one embodiment. [Figure 4] 1 is a schematic diagram of a plasma chamber according to one embodiment. [Figure 5A] 1 shows optical emission spectroscopy (OES) intensity of a helium-containing plasma, according to one embodiment. [Figure 5B] 1 shows optical emission spectroscopy (OES) intensity of a helium-containing plasma, according to one embodiment. [Figure 6] 1 illustrates the etch amount of a silicon nitride (SiN) based dielectric film according to one embodiment.
[0008] For clarity, where applicable, the same reference numbers have been used to designate identical elements that are common between the figures. Furthermore, elements of one embodiment may be advantageously adapted for use in other embodiments described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Detailed Description The embodiments described herein provide a method for post-treating a silicon nitride (SiN)-based dielectric film deposited on a substrate, for example, by flowable chemical vapor deposition (CVD). The silicon nitride (SiN)-based dielectric film contains silicon-nitrogen (Si-N-Si) bonds. The silicon nitride (SiN)-based dielectric film deposited on a substrate may contain a large amount of silicon-hydrogen (Si-H) and nitrogen-hydrogen (NH) bonds as a result of Si-H bridging limited near the surface of the deposited silicon nitrogen (Si-N)-based dielectric film, causing insufficient filling of gaps and trenches. The method described herein includes post-treating the silicon nitride (SiN)-based dielectric film deposited on a surface of a substrate by exposing the deposited silicon nitride (SiN)-based dielectric film to a helium-containing high energy low dose plasma. The method described herein can be used to reduce or eliminate the Si-H and NH bonds in the silicon nitride (SiN)-based dielectric film to densify the silicon nitride (SiN)-based dielectric film to a large thickness.
[0010] The embodiments described herein also provide methods for forming silicon nitride (SiN)-based dielectric films by flowable CVD to fill gaps and trenches with high aspect ratios (AR) and small dimensions (e.g., AR 8). In some embodiments, the silicon nitride (SiN)-based dielectric films formed by flowable CVD are seamless and can fill high AR gaps and trenches using liquid-phase silicon and nitrogen dielectric precursors and co-reactants (reactant gases) in radical form, such as oxygen (O2) or ammonia (NH3).
[0011] FIG. 1 is a flow chart illustrating a method 100 used to form a silicon nitride (SiN)-based dielectric film on a surface of a substrate, according to one embodiment.
[0012] In block 102, a substrate is placed in a deposition chamber. The substrate may be, for example, a metal substrate such as aluminum or stainless steel, a semiconductor substrate silicon-on-insulator (SOI) such as silicon or gallium arsenide, a glass substrate, or a plastic substrate. The semiconductor substrate may be a patterned substrate at any stage of fabrication / manufacturing in the formation of an integrated circuit. The patterned substrate may include gaps, trenches, holes, vias, etc. that are filled with a dielectric material.
[0013] In block 104, one or more dielectric precursors in liquid phase and a carrier gas, such as argon (Ar) or helium (He), are flowed into the deposition chamber via a gas delivery device, such as a dual channel showerhead (DCSH), to deliver the dielectric precursors onto a surface of a substrate disposed within the deposition chamber at a flow rate between about 250 sccm and about 5000 sccm per channel of the DCSH. The surface of the substrate can be held at a low temperature, between about 40° C. and about 150° C., for example, at about 80° C. The pressure of the deposition chamber can be maintained between about 0.5 Torr and about 3.0 Torr.
[0014] In some embodiments, the dielectric precursor is an organosilicon compound containing silicon, nitrogen, hydrogen, and chlorine such as silylamine and its derivatives, an organosilicon compound containing silicon, nitrogen, hydrogen, oxygen, or a combination thereof.
[0015] In block 106, a plasma may be generated in a remote plasma source (RPS) outside the deposition chamber and flowed into the substrate processing region of the deposition chamber along with a carrier gas (e.g., Ar, He). The plasma may be generated by dissociation of process precursor gases including molecular oxygen (O2), ozone (O3), molecular hydrogen (H2), nitrogen-hydrogen compounds (NH3, N2H4, etc.), nitrogen-oxygen compounds (NO, NO2, N2O, etc.), hydrogen-oxygen compounds (e.g., H2O, H2O2), nitrogen-hydrogen-oxygen compounds (e.g., NH4OH), carbon-oxygen compounds (e.g., CO, CO2), or combinations thereof. In the plasma, O * , H* , and / or N * Radicals including, for example, O * , H * , N * , NH3 * , N2H4 * , NH2 * , N.H. * , N * O * etc.
[0016] In some embodiments, RPS-activated radicals are flowed into the deposition chamber at a flow rate between about 1 sccm and about 1,000 sccm (referred to as the "radical flux").
[0017] In block 108, one or more radicals (also called reactive gas) in the substrate processing region react with the delivered dielectric precursor to form a silicon nitride (SiN)-based dielectric film. The composition of the formed silicon nitrogen (Si-N)-based dielectric film can be adjusted by changing the composition of the reactive gas in the radical flux. To form nitrogen-containing films such as SiON, SiCON, and SiN films, the reactive gas can be, for example, ammonia (NH3), hydrogen (H2), hydrazine (N2H4), nitrogen dioxide (NO2), or nitrogen (N2). When the reactive gas in the substrate processing region reacts with the delivered dielectric precursor, Si-H and NH bonds (weak bonds) are partially broken and replaced with Si-N, Si-NH, and / or Si-NH2 bonds (strong bonds) to form a silicon nitride (SiN) dielectric film.
[0018] In block 110, the formed silicon nitride (SiN) based dielectric film is exposed to a high energy, low dose plasma containing light ions (i.e., ionized species with low atomic numbers in the periodic table), such as helium (He), hydrogen (H2), argon (Ar), or nitrogen (N2), in a plasma chamber to harden the formed silicon nitride (SiN) based dielectric film. The plasma chamber is coupled to two power sources, an RF power source that controls the density of the ion flux (also called ion dose) via an inductive coil, and an RF power source that controls the ion energy.
[0019] When exposed to a high-energy, low-dose plasma containing light ions, the formed silicon nitride (SiN)-based dielectric film S Compounds having -H bonds and NH bonds are further cross-linked, i.e., adjacent compounds of the formed silicon nitride (SiN)-based dielectric film S When -H and NH bonds react with the photoion-containing plasma, adjacent compounds are S The -H bonds are removed and cross-linked by forming Si-N, Si-NH, and / or Si-NH2 bonds, thereby solidifying the corresponding portions of the silicon nitride (SiN)-based dielectric film.
[0020] Without intending to be bound by theory, it is believed that plasma-activated ion radicals physically collide with Si-H bonds in the silicon nitride (SiN)-based dielectric film, thereby breaking the Si-H bonds and forming Si-N, Si-NH, and / or Si-NH2 bonds. The light ions travel to a selected depth through the formed silicon nitride (SiN)-based dielectric film without substantially damaging the formed silicon nitride (SiN)-based dielectric film. This treatment with light ion radicals can perform a uniform nitridation process (e.g., formation of Si-N, Si-NH, and / or Si-NH2 bonds) to a depth of 0 nm to 4.2 nm without damaging the formed silicon nitride (SiN)-based dielectric film, but curing, e.g., by thermal annealing or UV irradiation, is necessarily limited to curing near the exposed surface of the silicon nitride (SiN)-based dielectric film.
[0021] Typically, but not intended to be limiting, curing of the dielectric precursor (block 110) occurs in a chamber (such as a plasma chamber) separate from the deposition chamber in which the dielectric precursor is delivered and reacted with reactive gases (blocks 104-108). In general, the sequence of operations (e.g., blocks 104-108) may be repeated over multiple cycles to form an entirely thick film.
[0022] Embodiments of the deposition system can be incorporated into a larger manufacturing system for producing integrated circuit chips. Figure 2 shows one such cluster tool 1001 including processing chambers 1008a-f, according to one embodiment. In Figure 2, a pair of front-opening unified pods (FOUPs) 1002 deliver substrates (e.g., 300 mm diameter wafers) that are received by a robotic arm 1004 and placed in a low-pressure holding area 1006. A second robotic arm 1010 can be used to transport substrates between the low-pressure holding area 1006 and the processing chambers 1008a-f.
[0023] 3A is a schematic diagram of a processing chamber 300 having a chamber body 302 and a lid assembly 304, according to one embodiment. The lid assembly 304 generally includes a remote plasma source (RPS) 306, a lid 308, and a dual channel showerhead (DCSH) 310. The RPS 306 can process process precursor gases provided from a process precursor gas source 312. A plasma formed in the RPS 306 can then be delivered to a chamber plasma region 318 through a gas inlet assembly 314 and a baffle 316 coupled to the lid 308. A carrier gas (e.g., Ar, He) can be delivered to the chamber plasma region 318. The lid (i.e., conductive top) 308 and the dual channel showerhead (DCSH) 310 are disposed with an insulating ring 310 therebetween, which allows an AC potential to be applied to the lid 308 with respect to the DCSH 310.
[0024] The DCSH 310 is disposed between the chamber plasma region 318 and the substrate processing region 324, and allows plasma-activated radicals present in the chamber plasma region 318 to pass through a number of through-holes 326 and enter the substrate processing region 324. The flow of radicals (radical flux) is indicated by solid arrows "A" in FIG. 3A. The substrate 328 is disposed on a substrate support 330 disposed in the substrate processing region 324. The DCSH 310 also has one or more hollow volumes 332 that can be filled with a dielectric precursor provided from a precursor source 334. The dielectric precursor passes from the one or more hollow volumes 332 through small holes 336 into the substrate processing region 324 and bypasses the chamber plasma region 318. The flow of the dielectric precursor is indicated by dotted arrows in FIG. 3A. The exhaust ring 338 is used to uniformly evacuate the substrate processing region 324 by using an exhaust pump 340. The DCSH 310 may be thicker than the length of the smallest diameter of the through-holes 326. The length of the minimum diameter of the through-hole 326 may be limited by forming a larger diameter portion of the through-hole 326 partially through the DCSH 310 to maintain a flow of radical flux from the chamber plasma region 318 to the substrate processing region 324. In some embodiments, the length of the minimum diameter of the through-hole 326 may be on the same order of magnitude or less than the minimum diameter of the through-hole 326.
[0025] In some embodiments, a pair of processing chambers (e.g., 1008c-d) (referred to as a twin chamber) of FIG. 2 can be used to deposit a dielectric precursor on a substrate. Each processing chamber (e.g., 1008c-d) can have the cross-sectional structure of processing chamber 300 shown in FIG. 3A. The flow rates per channel of the DCSHs listed above correspond to the flow rates into each chamber (e.g., 1008c-d) through the corresponding DCSH 310.
[0026] 3B is a schematic bottom view of the DCSH 310 according to one embodiment. The DCSH 310 can provide a radical flux and a carrier gas present in the chamber plasma region 318 via through-holes 326.
[0027] In some embodiments, the number of through holes 326 can be between about 60 and about 2,000. The through holes 326 can have a round shape or a variety of shapes. In some embodiments, the minimum diameter of the through holes 326 can be between about 0.5 mm and about 20 mm, or between about 1 mm and about 6 mm. The cross-sectional shape of the through holes 326 can be conical, cylindrical, or a combination of the two shapes. In some embodiments, a number of small holes 336 can be used to introduce the dielectric precursor to the substrate processing region 324, and can be between about 100 and about 5,000, or between about 500 and about 2,000. The diameter of the small holes 336 can be between about 0.1 mm and about 2 mm.
[0028] 4 is a schematic diagram of a plasma chamber 400 having a chamber body 402 and a lid assembly 404, according to one embodiment. The lid assembly 404 includes a gas supply assembly 406 and a lid 408. The lid 408 has an opening 410 to allow the inlet of one or more process precursor gases. The gas supply assembly 406 is disposed on the lid 408 through the opening 410. The gas supply assembly 406 can be connected to a gas source 412 via a gas inlet 414 to supply one or more process precursor gases to a substrate processing region 424. A substrate 428 is disposed within the substrate processing region 424 and disposed on a substrate support 430 coupled to a bias power supply (not shown). The one or more process precursor gases can exit the substrate processing region 424 by using an exhaust ring 438 and an exhaust pump 440.
[0029] In the lid assembly 404, an inner coil 442, a middle coil 444, and an outer coil 446 are disposed on the lid 408. The inner coil 442 and the outer coil 446 are coupled to an RF power source 448 through a matching network 450. Power applied from the RF power source 448 to the outer coil 446 is inductively coupled through the lid 408 to generate a plasma from process precursor gases provided from a gas source 412 in the substrate processing region 424. The RF power source 448 supplies currents at different frequencies to control the plasma density (i.e., number of ions per cc) in the plasma, and therefore the density of the ion flux (ions / cm 2 sec). The bias power supply controls the voltage between the substrate 428 and the plasma, and therefore the energy and directionality of the ions. Thus, both the ion flux and ion energy can be controlled independently.
[0030] Thus, both the ion flux and the ion energy can be controlled independently. The heater assembly 452 can be secured to the lid 408 by clamping members 454,456.
[0031] The surface of the substrate may be maintained at a temperature between about 100° C. and about 400° C. The pressure in the plasma chamber may be maintained between about 5 mTorr and about 500 mTorr.
[0032] Below, experimental measurements of process parameters used to treat the deposited films are provided as examples to illustrate aspects of the embodiments of the present disclosure described herein, and are not intended to limit the scope of the present disclosure.
[0033] In experimental measurements, silicon nitride (SiN)-based dielectric films formed according to the method 100 described above were exposed to a helium-containing high-energy low-dose plasma at a pressure between 15 and 150 mT for a time between about 2 minutes and about 3.5 minutes. The power applied by the bias power supply to an electrode disposed within the substrate support (referred to as bias power) was varied between 100 W and 700 W, and the applied bias power varied the energy of the helium ions (i.e., ions generated in the plasma) used to bombard the surface of the substrate. The power applied to the RF power supply, an ICP plasma source in this example, was varied between 0 kW and 2.7 kW to vary the density of the helium ions generated in the plasma (i.e., lower power corresponds to lower flux density). The formed silicon nitride (SiN)-based dielectric films were bombarded by helium ions and densified (i.e., nitrided) to a depth between 2.6 Å and 4.2 Å per cycle and to an overall depth between 3 nm and 4.2 nm. A summary of some process parameters that can be used in one or more embodiments described herein is summarized below. TIFF0007556891000001.tif88170
[0034] Figure 5A shows optical emission spectroscopy (OES) intensities of helium-containing plasma measured between wavelengths 200-900 nm at powers of RF power source (referred to as RF source power) of (i) 2.7 kW (see line 591) and (ii) 700 W (see line 592). The major emission lines in Figure 5A indicate metastable helium (He) atoms (e.g., 388.8 nm, 402.6 nm, 447.1 nm, 501.5 nm, 587.5 nm, 667.8 nm, 706.5 nm, and 728.1 nm). Additionally, the reactive species detected in relation to nitrogen are excited nitrogen molecules with emission spectrum wavelengths between 300 and 400 nm. The OES intensities corresponding to metastable helium (He) atoms in the case of 700 W RF source power (see line 591) are approximately 10-1,000 times smaller than in the case of 2.7 kW RF source power (see line 592). Therefore, the plasma density of the helium ion containing plasma is 10 to 1,000 times smaller than that for the 700 W RF source power.
[0035] FIG. 5B shows the OES intensity of a helium-containing plasma at various bias powers, such as between 100 W and 500 W, and a pressure of 150 mTorr. The RF source power was kept at 0 W, and thus a helium-containing plasma was generated by application of a bias applied to the substrate support electrode. As can be seen from FIG. 5B, the OES intensity corresponding to the major emission line in FIG. 5A increases linearly with the applied bias power and thus the energy of the helium ions. Thus, in this example, a high energy, low dose plasma was provided with a low RF source power (e.g., 700 W) and a high bias power (e.g., 100-500 W).
[0036] A helium-containing plasma, in which the plasma density and energy of the helium ions can be controlled as described above, can be used to densify formed deposition layers, such as silicon nitride (SiN)-based dielectric films. A helium-containing plasma, having a low plasma density and containing high energy helium ions, can bombard the substrate surface and penetrate deep into the silicon nitride (SiN)-based dielectric film without significant damage to the film due to excessive bombardment of the film surface created in higher plasma density processes and the use of higher atomic weight gases typically used in conventional plasma processes. A helium-containing plasma, having a low plasma density and containing high energy helium ions, can result in a thickness densification with less overall damage in the formed silicon nitride (SiN)-based dielectric film. For example, silicon and nitride-containing flowable films deposited within high aspect ratio features can be treated with such a high energy low dose helium-containing plasma to densify the flowable film and form a silicon nitride (SiN)-based dielectric film that is densified to an increased depth within the high aspect ratio feature without significant damage to the formed flowable film layer.
[0037] FIG. 6 shows the amount of silicon nitride (SiN)-based dielectric film removed using a dilute HF (DHF) solution prepared by diluting 1% HF with deionized water for 5 minutes. Silicon nitride (SiN)-based dielectric films were formed according to the method 100 described above and then exposed to a helium-containing plasma at a pressure between 150 mTorr and 300 mTorr with an RF source power of 2.7 kW (high dose) and 700 W (low dose), and a bias power of 300 W (low energy) and 700 W (high energy). As can be seen in FIG. 6, a lower dose (i.e., at a lower RF source power) and a higher energy (i.e., at a higher bias power) of helium ions in the plasma increased the amount of etching of the silicon nitride-based dielectric film, and the formed silicon nitride (SiN)-based dielectric film had a nitride (densified) portion to a deeper depth, and the etch rate was improved to 12.5 Å / min. The lower pressure also leads to higher energy of the helium ions in the plasma and therefore improved etch rates.
[0038] As described above, post-treatment of silicon nitride (SiN)-based flowable films with helium-containing high-energy low-dose plasma can increase nitridation depth and improve wet etching rate (WERR) without damaging the flowable film. It should be noted that the above specific exemplary embodiments are only some possible examples of silicon nitride (SiN)-based dielectric films that can be post-treated with high-energy low-dose plasma according to the present disclosure, and do not limit the possible configurations, specifications, deposition methods, etc. of silicon nitride (SiN)-based dielectric films. For example, post-treatment with light ion-containing high-energy low-dose plasma can be applied to doped or undoped SiCOH, SiCON, SiO, and SiN films.
[0039] While the forgoing is directed to specific embodiments, other and further embodiments may be devised without departing from the basic scope thereof, which is determined by the following claims.
Claims
1. 1. A method for post-treating a silicon nitride (SiN) based dielectric film formed on a surface of a substrate, comprising: placing the substrate having the silicon nitride (SiN) based dielectric film formed thereon in a processing chamber; exposing the silicon nitride (SiN) based dielectric film to a helium-containing high energy low dose plasma in the processing chamber; the energy of helium ions in the helium-containing high-energy low-dose plasma is between 1 eV and 3.01 eV; The flux density of the helium ions in the helium-containing high-energy low-dose plasma is 5×10 15 ions / cm 2 Seconds and 1.37 x 10 16 ions / cm 2 - A method between seconds.
2. The method of claim 1, wherein the silicon nitride (SiN) based dielectric film contains Si-H bonds.
3. The method of claim 1, wherein the silicon nitride (SiN) based dielectric film comprises N-H bonds.
4. 10. The method of claim 1, wherein the substrate is at a temperature between 100° C. and 400° C. during exposure of the silicon nitride (SiN) based dielectric film to the helium-containing high-energy low-dose plasma.
5. 10. The method of claim 1, wherein the substrate is at a pressure between 5 mTorr and 300 mTorr during exposure of the silicon nitride (SiN) based dielectric film to the helium-containing high energy low dose plasma.
6. The method of claim 1 , wherein the substrate is made of a material selected from the group consisting of metals, semiconductors, and plastics.
7. 1. A method for post-treating a silicon-based film formed on a surface of a substrate, comprising: placing the substrate having the silicon-based film formed thereon in a processing chamber; exposing the silicon-based film to a helium-containing high energy, low dose plasma in the processing chamber; the energy of helium ions in the helium-containing high-energy low-dose plasma is between 1 eV and 3.01 eV; The flux density of the helium ions in the helium-containing high-energy low-dose plasma is 5×10 15 ions / cm 2 Seconds and 1.37 x 10 16 ions / cm 2 - A method between seconds.
8. The method of claim 7 , wherein the silicon-based film comprises silicon nitride (SiN).
9. The method of claim 7, wherein the silicon-based film comprises Si-H bonds.
10. The method of claim 7, wherein the silicon-based film comprises N--H bonds.
11. 8. The method of claim 7, wherein the substrate is at a temperature between 100° C. and 400° C. during exposure of the silicon-based film to the helium-containing high-energy low-dose plasma.
12. 8. The method of claim 7, wherein the substrate is at a pressure between 5 mTorr and 300 mTorr during exposure of the silicon-based film to the helium-containing high energy low dose plasma.
13. The method of claim 7 , wherein the substrate is made of a material selected from the group consisting of metals, semiconductors, and plastics.
14. 1. A method for forming and post-treating a silicon nitride (SiN) based dielectric film on a surface of a substrate, comprising: delivering a dielectric precursor comprising silicon and nitrogen onto the substrate disposed in a processing region of a first chamber; providing a radical flux to the processing region of the first chamber; exposing the delivered dielectric precursor to a helium-containing high energy low dose plasma in a second chamber; the energy of helium ions in the helium-containing high-energy low-dose plasma is between 1 eV and 3.01 eV; The flux density of helium ions in the helium-containing high-energy low-dose plasma is 5×10 15 ions / cm 2 Seconds and 1.37 x 10 16 ions / cm 2 - A method between seconds.
15. 15. The method of claim 14, wherein the substrate is at a temperature between 100° C. and 400° C. during exposure of the silicon nitride (SiN) based dielectric film to the helium-containing high-energy low-dose plasma.
16. 15. The method of claim 14, wherein the substrate is at a pressure between 5 mTorr and 300 mTorr during exposure of the silicon nitride (SiN) based dielectric film to the helium-containing high energy low dose plasma.
17. The method of claim 14 , wherein the substrate is made of a material selected from the group consisting of metals, semiconductors, and plastics.
18. 15. The method of claim 14, wherein the dielectric precursor is an organosilicon compound containing silicon, nitrogen, hydrogen, and chlorine.
19. 15. The method of claim 14, wherein the dielectric precursor is an organosilicon compound containing silicon, nitrogen, hydrogen, and oxygen.
20. The radical flux is oxygen (O 2 ), ozone (O 3 ), water (H 2 O), ammonia (NH 3 ), hydrazine (N 2 H 4 ), nitrogen dioxide (NO 2 ), and nitrogen (N 2 15. The method of claim 14, further comprising a radical gas selected from the group consisting of:
Citation Information
Patent Citations
Method of manufacturing semiconductor device, active matrix substrate, and electronic apparatus
JP2005203800A
Method for curing low dielectric constant film by electron beam
JP2005524983A
Method for separating thin films at medium temperature after co-implantation
JP2006505928A
Manufacturing method for thin film
JP2007251172A
Curing of insulating film under reduction atmosphere
JP2008010877A