Polarizing plate and image display device using the same

The polarizing plate design addresses the reddish reflection issue by controlling refractive index differences between layers, effectively suppressing redness and improving display performance in image display devices.

JP7557504B2Active Publication Date: 2024-09-27NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022129979
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-17
Publication Date
2024-09-27
Estimated Expiration
2042-08-17

AI Technical Summary

Technical Problem

Conventional polarizing plates used in image display devices exhibit a reddish reflection hue due to large reflection anisotropy for long wavelength light, affecting display performance.

Method used

A polarizing plate design with controlled refractive index differences between the polarizer and adhesive layer, and optionally including a protective layer and undercoat layer, to minimize reflection anisotropy and suppress redness, featuring a refractive index difference of less than 0.20 and reflectance difference of less than 0.40% between absorption and perpendicular axes.

Benefits of technology

The design effectively suppresses redness in polarizing plates even when using polarizers with large reflection anisotropy for long wavelength light, enhancing display performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557504000005
    Figure 0007557504000005
  • Figure 0007557504000004
    Figure 0007557504000004
  • Figure 0007557504000001
    Figure 0007557504000001
Patent Text Reader

Abstract

To provide a polarizing plate which uses a polarizer with large reflection anisotropy for long-wavelength light, and yet offers suppressed reddishness.SOLUTION: A polarizing plate according to an embodiment of the present invention comprises a polarizer, and a protective layer stacked on the polarizer via an adhesive layer. A difference between a refractive index n1A of the polarizer in an absorption axis direction and a refractive index n2 of the adhesive layer is 0.20 or less in absolute terms.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate and an image display device using the polarizing plate. [Background technology]

[0002] In recent years, image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices and inorganic EL display devices), have rapidly become widespread. Polarizing plates are typically used in image display devices. However, depending on the configuration of the polarizing plate, the reflection hue may become reddish, which may adversely affect the display performance of the image display device. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-127569 A [Patent Document 2] JP 2019-204083 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and its main object is to provide a polarizing plate in which redness is suppressed despite the use of a polarizer with large reflection anisotropy for long-wavelength light. [Means for solving the problem]

[0005] [1] A polarizing plate according to an embodiment of the present invention has a polarizer and a protective layer laminated on the polarizer via an adhesive layer, and has a refractive index n 1A and the refractive index n2 of the adhesive layer, the absolute value of which is 0.20 or less. [2] In the above [1], the reflectance R in the absorption axis direction of the polarizer at a wavelength of 700 nm PA and the reflectance R in the direction perpendicular to the absorption axisPT The difference is less than 0.40%. [3] In the above [1] or [2], the protective layer has an in-plane retardation Re(550) of 20 nm or less. [4] In any one of the above [1] to [3], the protective layer is made of a polycarbonate-based resin film. [5] In any one of the above [1] to [4], the polarizing plate further has an undercoat layer between the adhesive layer and the protective layer. [6] In the above [5], the refractive index n 1A and the refractive index n4 of the undercoat layer, the absolute value of which is 0.20 or less. [7] In any one of the above [1] to [6], the polarizing plate further has a retardation layer having a circular polarization function or an elliptically polarizing function on the opposite side of the polarizer to the protective layer. [8] According to another aspect of the present invention, there is provided an image display device comprising the polarizing plate according to any one of [1] to [6] above. [9] An image display device may include the polarizing plate described above in [7]. Effect of the Invention

[0006] According to the embodiments of the present invention, a polarizing plate in which redness is suppressed can be realized despite the use of a polarizer having large reflection anisotropy for light with long wavelengths. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view of a polarizing plate according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Representative embodiments of the present invention will be described below, but the present invention is not limited to these embodiments.

[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation of a film measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation of a film measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re=(nx-ny)×d, where d(nm) is the thickness of the film. (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction of a film measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction of a film measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth=(nx-nz)×d, where d(nm) is the thickness of the film. (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When angles are referred to herein, unless otherwise specified, the angles include angles in both clockwise and counterclockwise directions.

[0010] A. Overall structure of polarizing plate 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100 shown in the figure has a polarizer 10 and a protective layer 30 laminated to the polarizer 10 via an adhesive layer 20. In this embodiment of the present invention, the refractive index n 1Aand the refractive index n2 of the adhesive layer is typically 0.20 or less, preferably 0.18 or less, more preferably 0.15 or less, even more preferably 0.12 or less, and particularly preferably 0.07 or less. The smaller the absolute value of the difference, the better, and desirably it is zero. With this configuration, a polarizing plate with suppressed redness can be realized even when a polarizer with large reflection anisotropy for long-wavelength light is used. Note that the refractive index n in the absorption axis direction of the polarizer 1A is typically greater than the refractive index n2 of the adhesive layer. 1T The absolute value of the difference between the refractive index n1 of the polarizer and the refractive index n2 of the adhesive layer is not so large in most cases. The absolute value of the difference may be, for example, 0.01 to 0.10, or may be, for example, 0.02 to 0.09, or may be, for example, 0.04 to 0.06. As a result, the refractive index n 1A By controlling the absolute value of the difference between the refractive index n1 and the refractive index n2 of the adhesive layer, the effects of the embodiment of the present invention can be made significant.

[0011] In the embodiment of the present invention, the polarizing plate typically has a reflectance R PA is the reflectance R in the direction perpendicular to the absorption axis of the polarizer. PT Moreover, R PA and R PT The difference between R and R is preferably 0.40% or less, more preferably 0.39% or less, even more preferably 0.35% or less, particularly preferably 0.30% or less, particularly preferably 0.25% or less, and most preferably 0.15% or less. PA and R PT The difference between the above is, for example, 0.03% or more, and for example, 0.05% or more. With this configuration, a polarizing plate in which redness is suppressed can be realized even if a polarizer (described later) with large reflection anisotropy for long wavelength light (for example, light with a wavelength of 650 nm or more) is used.

[0012] 2 is a schematic cross-sectional view of a polarizing plate according to another embodiment of the present invention. The polarizing plate 101 in the illustrated example further includes an undercoat layer 40 between the adhesive layer 20 and the protective layer 30. In this embodiment, the refractive index n 1A The absolute value of the difference between the refractive index n1 of the undercoat layer and the refractive index n4 of the undercoat layer is preferably 0.20 or less, more preferably 0.18 or less, even more preferably 0.15 or less, particularly preferably 0.12 or less, and particularly preferably 0.07 or less. The smaller the absolute value of the difference, the more preferable, and desirably zero. With this configuration, even if a polarizer with large reflection anisotropy for long-wavelength light is used, a polarizing plate with suppressed redness can be realized. In this case, the refractive index n1 in the absorption axis direction of the polarizer 1A The absolute value of the difference between the refractive index n1 and the refractive index n4 of the undercoat layer can be controlled. 1A It is not necessary to control the absolute value of the difference between the refractive index n1 of the adhesive layer and the refractive index n2 of the adhesive layer. As a result, the degree of freedom in selecting the adhesive layer is significantly increased. Note that, similar to the relationship with the refractive index n2 of the adhesive layer described above, the refractive index n 1A is typically greater than the refractive index n4 of the undercoat layer. 1T The absolute value of the difference between the refractive index n4 of the undercoat layer and the refractive index n5 of the polarizer in the absorption axis direction is not so large in most cases. The absolute value of the difference may be, for example, 0.01 to 0.10, or, for example, 0.02 to 0.09, or, for example, 0.04 to 0.06. As a result, the refractive index n 1A By controlling the absolute value of the difference between the refractive index n4 of the undercoat layer and the refractive index n3 of the undercoat layer, the effects of the embodiment of the present invention can be made significant.

[0013] The polarizing plate according to the embodiment of the present invention may further have a retardation layer (not shown) having a circular polarization function or an elliptical polarization function on the side opposite to the protective layer 30 of the polarizer 10, if necessary. With such a configuration, a polarizing plate (polarizing plate with a retardation layer) having excellent anti-reflection properties can be obtained. In one embodiment, the retardation layer is composed of a stretched film of a resin film. In this case, the retardation layer is typically a single layer. In another embodiment, the retardation layer is an alignment solidified layer of a liquid crystal compound (hereinafter, sometimes referred to as a liquid crystal alignment solidified layer). In this case, the retardation layer may be a single layer, or may have a two-layer structure of a first liquid crystal alignment solidified layer and a second liquid crystal alignment solidified layer.

[0014] In one embodiment, the polarizing plate (polarizing plate with retardation layer) may further have another retardation layer on the opposite side of the retardation layer to the polarizer. The other retardation layer is typically a so-called positive C plate whose refractive index characteristics show the relationship nz>nx=ny. By providing such another retardation layer, it is possible to effectively prevent reflection in an oblique direction, and the anti-reflection function can be made to have a wide viewing angle.

[0015] When the polarizing plate is disposed on the viewing side of the image display device, the protective layer 30 is typically disposed on the viewing side. Therefore, the protective layer 30 may be subjected to a surface treatment as necessary. Examples of the surface treatment include a hard coat treatment, an anti-reflection treatment, an anti-sticking treatment, and an anti-glare treatment. In the embodiment of the present invention, a hard coat treatment (formation of a hard coat layer) is preferable. The hard coat layer will be described later. The hard coat treatment may be combined with other surface treatments. In addition, the protective layer 30 may be subjected to a treatment for improving visibility when viewed through polarized sunglasses (typically, imparting an (elliptical) polarizing function or imparting an ultra-high phase difference) as necessary. By performing such a treatment, excellent visibility can be achieved even when the display screen is viewed through polarized lenses such as polarized sunglasses. Therefore, the polarizing plate may be suitably applied to an image display device that can be used outdoors.

[0016] If necessary, the polarizing plate according to the embodiment of the present invention may further have another protective layer (not shown) on the side opposite the protective layer 30 of the polarizer 10 (between the polarizer and the retardation layer, if a retardation layer is provided).

[0017] For practical purposes, the polarizing plate according to the embodiment of the present invention has an adhesive layer (not shown) as the outermost layer on the side opposite to the protective layer 30, and can be attached to an image display cell. In this case, it is preferable that a release liner is temporarily attached to the surface of the adhesive layer until the polarizing plate is used. By temporarily attaching the release liner, the adhesive layer is protected and the polarizing plate can be formed into a roll.

[0018] The components of the polarizing plate will be described below.

[0019] B. Polarizer Any appropriate polarizer can be adopted as the polarizer 10. For example, the resin film forming the polarizer may be a single-layer resin film or a laminate of two or more layers.

[0020] Specific examples of polarizers made of a single-layer resin film include hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films that have been dyed with iodine or a dichroic substance such as a dichroic dye and stretched, and polyene-based oriented films such as dehydrated PVA films and dehydrochlorinated polyvinyl chloride films. A polarizer obtained by dyeing a PVA film with iodine and uniaxially stretching it is preferably used because of its excellent optical properties.

[0021] The dyeing with iodine is carried out, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment, or may be carried out while dyeing. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based film in water and washing it with water before dyeing, it is possible to wash off dirt and antiblocking agents on the surface of the PVA-based film, and also to swell the PVA-based film and prevent uneven dyeing.

[0022] Specific examples of polarizers obtained using a laminate include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced by, for example, applying a PVA-based resin solution to the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to make the PVA-based resin layer into a polarizer. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95° C. or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of the PVA, and to achieve high optical properties. In addition, by simultaneously increasing the orientation of the PVA in advance, problems such as a decrease in the orientation of the PVA or dissolution when immersed in water in the subsequent dyeing and stretching steps can be prevented, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the orientation of the polyvinyl alcohol molecules can be disturbed and the orientation can be reduced, compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained by immersing the laminate in a liquid through a treatment process such as a dyeing treatment and an underwater stretching treatment. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage treatment.The obtained resin substrate / polarizer laminate may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or any suitable protective layer may be laminated on the peeled surface of the resin substrate / polarizer laminate after peeling the resin substrate from the resin substrate / polarizer laminate, or on the surface opposite to the peeled surface, depending on the purpose. Details of the method for producing such a polarizer are described in, for example, JP2012-73580A and JP6470455A. The entire disclosures of these publications are incorporated herein by reference.

[0023] The thickness of the polarizer is preferably 10 μm or less, more preferably 1 μm to 8 μm, and further preferably 3 μm to 7 μm. Such a very thin polarizer has a large reflection anisotropy for light of long wavelengths, more specifically, the reflectance in the absorption axis direction tends to be larger than the reflectance in the direction perpendicular to the absorption axis. Therefore, the effect of the embodiment of the present invention is remarkable in a polarizing plate having such a very thin polarizer.

[0024] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is preferably 41.0% to 46.0%, and more preferably 42.5% to 45.0%. The degree of polarization of the polarizer is preferably 98.0% or more, more preferably 99.0% or more, even more preferably 99.9% or more, and particularly preferably 99.95% or more. According to the embodiment of the present invention, even if the single transmittance is in the above-mentioned range, the degree of polarization can be maintained in such a range.

[0025] The iodine concentration of the polarizer is, for example, 3% by weight to 10% by weight, more preferably 4% by weight to 8% by weight, and further preferably 5% by weight to 7% by weight. A polarizer having such an iodine concentration has a large interaction between iodine and substances contained in the components of the polarizing plate, and has a large reflection anisotropy for light with a long wavelength, and more specifically, the reflectance in the absorption axis direction tends to be larger than the reflectance in the direction perpendicular to the absorption axis. Therefore, the effect of the embodiment of the present invention is remarkable in a polarizing plate having a polarizer with such an iodine concentration. In this specification, the "iodine concentration" means the amount of all iodine contained in the polarizer. More specifically, iodine in the polarizer is I - , I2, I3 - In this specification, the iodine concentration refers to the concentration of iodine including all of these forms. The iodine concentration can be calculated, for example, from the fluorescent X-ray intensity by fluorescent X-ray analysis and the film (polarizer) thickness.

[0026] Refractive index n in the absorption axis direction of the polarizer 1A and the refractive index n perpendicular to the absorption axis 1T Difference from (n 1A -n 1T ) is, for example, 0.15 to 0.20, and is, for example, 0.18 to 0.20. A polarizer having such refractive index characteristics has a large reflection anisotropy for light with a long wavelength, more specifically, the reflectance in the absorption axis direction tends to be larger than the reflectance in the direction perpendicular to the absorption axis. Therefore, the effects of the embodiment of the present invention are remarkable in a polarizing plate having a polarizer with such refractive index characteristics.

[0027] Reflectance R in the absorption axis direction of the polarizer at a wavelength of 700 nm SA is typically the reflectance R in the direction perpendicular to the absorption axis of the polarizer. ST Moreover, R SA and R ST The difference between R and R is preferably 0.5% or more, more preferably 1.0% or more, and further preferably 2.0% or more. SA and R STThe difference between the above values ​​may be, for example, 2.5% or less. According to the embodiment of the present invention, a polarizing plate in which redness is suppressed can be realized despite the use of a polarizer having such large reflection anisotropy.

[0028] C. Protective layer The in-plane retardation Re(550) of the protective layer is preferably 20 nm or less, more preferably 15 nm or less, even more preferably 10 nm or less, particularly preferably 8 nm or less, and particularly preferably 5 nm or less. The lower limit of the in-plane retardation Re(550) of the protective layer may be, for example, 0 nm. With this configuration, when an image display device to which the polarizing plate according to the embodiment of the present invention is applied is viewed through polarized sunglasses, a decrease in visibility (for example, the screen appears pitch black) can be suppressed.

[0029] The protective layer may exhibit an inverse wavelength dispersion characteristic in which the retardation value increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value hardly changes according to the wavelength of the measurement light. In one embodiment, the protective layer exhibits a flat wavelength dispersion characteristic. In this case, Re(450) / Re(550) of the protective layer is preferably 0.95 to 1.05, and more preferably 0.98 to 1.02.

[0030] The protective layer 30 may be made of any suitable resin film as long as it satisfies the above-mentioned characteristics. Examples of resins constituting the protective layer include polycarbonate-based resins, cyclic olefin-based resins, cellulose-based resins, polyester-based resins, polyvinyl alcohol-based resins, polyamide-based resins, polyimide-based resins, polyether-based resins, polystyrene-based resins, acrylic resins, and polyester carbonate-based resins. Among these, polycarbonate-based resins and polyester carbonate-based resins may be preferably used. These resins can be laser-processed, which is very advantageous, for example, when processing a polarizing plate into a modified shape. In this specification, polycarbonate-based resins and polyester carbonate resins may be collectively referred to as polycarbonate-based resins.

[0031] As the polycarbonate-based resin, any suitable polycarbonate-based resin can be used as long as the effects of the present invention can be obtained. Preferably, the polycarbonate-based resin contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from at least one dihydroxy compound selected from the group consisting of alicyclic diol, alicyclic dimethanol, di-, tri- or polyethylene glycol, and alkylene glycol or spiro glycol. Preferably, the polycarbonate-based resin contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, a structural unit derived from an alicyclic dimethanol, and / or a structural unit derived from a di-, tri- or polyethylene glycol; more preferably, it contains a structural unit derived from a fluorene-based dihydroxy compound, a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from a di-, tri- or polyethylene glycol. The polycarbonate-based resin may contain a structural unit derived from another dihydroxy compound as necessary. Details of polycarbonate-based resins are described, for example, in JP-A-2014-10291, JP-A-2014-26266, JP-A-2015-212816, JP-A-2015-212817, and JP-A-2015-212818, and the descriptions in these publications are incorporated herein by reference.

[0032] In one embodiment, a polycarbonate resin containing a unit structure derived from a dihydroxy compound represented by the following general formula (1) can be used. [ka] (In the above general formula (1), R1 to R4 each independently represent a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 6 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms; X represents a substituted or unsubstituted alkylene group having 2 to 10 carbon atoms, a substituted or unsubstituted cycloalkylene group having 6 to 20 carbon atoms, or a substituted or unsubstituted arylene group having 6 to 20 carbon atoms; and m and n each independently represent an integer of 0 to 5.)

[0033] Specific examples of the dihydroxy compound represented by the general formula (1) include 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-ethylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-propylphenyl)fluorene, 9,9-bis(4-hydroxy-3-isopropylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-sec-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-tert-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-cyclohexylphenyl)fluorene, 9,9-bis(4-hydroxy-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxy ... ,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexyl 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene, and the like.

[0034] The polycarbonate resin may contain, in addition to the structural units derived from the dihydroxy compounds, structural units derived from dihydroxy compounds such as isosorbide, isomannide, isoidet, spiroglycol, dioxane glycol, diethylene glycol (DEG), triethylene glycol (TEG), polyethylene glycol (PEG), and bisphenols.

[0035] Details of polycarbonate resins containing structural units derived from dihydroxy compounds are described, for example, in Japanese Patent No. 5204200, JP 2012-67300 A, Japanese Patent No. 3325560, WO2014 / 061677, etc. The descriptions in these patent documents are incorporated herein by reference.

[0036] In one embodiment, a polycarbonate resin containing an oligofluorene structural unit may be used. Examples of the polycarbonate resin containing an oligofluorene structural unit include a resin containing a structural unit represented by the following general formula (2) and / or a structural unit represented by the following general formula (3). [ka] (In the above general formula (2) and the above general formula (3), R5 and R6 are each independently a direct bond or a substituted or unsubstituted alkylene group having 1 to 4 carbon atoms (preferably an alkylene group having 2 to 3 carbon atoms on the main chain). R7 is a direct bond or a substituted or unsubstituted alkylene group having 1 to 4 carbon atoms (preferably an alkylene group having 1 to 2 carbon atoms on the main chain). R8 to R 13 are each independently a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms (preferably 1 to 4, more preferably 1 to 2), a substituted or unsubstituted aryl group having 4 to 10 carbon atoms (preferably 4 to 8, more preferably 4 to 7), a substituted or unsubstituted acyl group having 1 to 10 carbon atoms (preferably 1 to 4, more preferably 1 to 2), a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms (preferably 1 to 4, more preferably 1 to 2), a substituted or unsubstituted aryloxy group having 1 to 10 carbon atoms (preferably 1 to 4, more preferably 1 to 2), a substituted or unsubstituted acyloxy group having 1 to 10 carbon atoms (preferably 1 to 4, more preferably 1 to 2), a substituted or unsubstituted amino group, a substituted or unsubstituted vinyl group having 1 to 10 carbon atoms (preferably 1 to 4), a substituted or unsubstituted ethynyl group having 1 to 10 carbon atoms (preferably 1 to 4), a sulfur atom having a substituent, a silicon atom having a substituent, a halogen atom, a nitro group, or a cyano group. R8~R13 At least two adjacent groups among these may be bonded to each other to form a ring.)

[0037] In one embodiment, the fluorene ring contained in the oligofluorene structural unit is 13 are all hydrogen atoms, or R and / or R 13 is any one selected from the group consisting of a halogen atom, an acyl group, a nitro group, a cyano group, and a sulfo group, and R 12 is a hydrogen atom.

[0038] Details of the polycarbonate-based resin containing an oligofluorene structural unit are described, for example, in JP 2015-212816 A. The description of this publication is incorporated herein by reference.

[0039] The thickness of the protective layer is preferably 15 μm to 60 μm, and more preferably 25 μm to 45 μm.

[0040] D. Hard Coat Layer The hard coat layer may be made of any suitable material as long as the effect of the embodiment of the present invention can be obtained. The hard coat layer is, for example, a cured layer of any suitable thermosetting resin or active energy ray (for example, ultraviolet light, visible light, electron beam) curable resin. UV curable resin is preferred. This is because the hard coat layer can be formed with simple operation and high efficiency. Specific examples of UV curable resins include polyester-based, (meth)acrylic-based, urethane-based, amide-based, silicone-based, epoxy-based, and unsaturated polyester-based UV curable resins. (Meth)acrylic UV curable resins include urethane (meth)acrylate, polyester (meth)acrylate, and epoxy (meth)acrylate. UV curable resins may include UV curable monomers, oligomers, and polymers. Preferred UV curable resins include resin compositions containing acrylic monomer or oligomer components having preferably 2 or more, more preferably 3 to 6 UV polymerizable functional groups. Typically, a photopolymerization initiator is blended into the UV curable resin.

[0041] The hard coat layer preferably has a pencil hardness of H or more, more preferably 2H or more, and even more preferably 3H or more. On the other hand, the pencil hardness of the hard coat layer is preferably 6H or less, more preferably 5H or less. If the pencil hardness of the hard coat layer is in this range, excellent surface protection performance can be imparted when the polarizing plate is applied to an image display device. The pencil hardness can be measured based on the "Pencil Hardness Test" of JIS K 5400.

[0042] The thickness of the hard coat layer is preferably 5 μm or less, more preferably 0.5 μm to 4 μm, and further preferably 1 μm to 3.5 μm. If the thickness of the hard coat layer is within this range, excellent scratch resistance can be achieved.

[0043] The hard coat layer can be formed by any suitable method. The hard coat layer can be preferably formed by coating a resin composition for forming a hard coat layer on a protective layer, drying the composition, and curing the dried coating film by irradiating it with ultraviolet light.

[0044] Details of the hard coat layer are described in, for example, JP-A-2011-237789 and JP-A-2016-224443, the disclosures of which are incorporated herein by reference.

[0045] E. Adhesive layer E-1. When no undercoat layer is applied The refractive index n2 of the adhesive layer is preferably 1.50 to 1.70, and more preferably 1.60 to 1.70. When the refractive index of the adhesive layer is within this range, the refractive index n 1A and the refractive index n2 of the adhesive layer can be set in the desired range.

[0046] The adhesive constituting the adhesive layer may be any suitable adhesive having a high refractive index as described above. Such an adhesive having a high refractive index may be prepared by blending a refractive index adjuster (e.g., titanium oxide) with any suitable adhesive.

[0047] E-2. When applying a primer layer When an undercoat layer is provided, the effect of the embodiment of the present invention can be obtained by controlling the refractive index n4 of the undercoat layer. Therefore, it is not necessary to precisely control the refractive index n2 of the adhesive layer. In other words, an adhesive having appropriate properties according to the purpose can be used as the adhesive constituting the adhesive layer.

[0048] The adhesive layer may be made of, for example, an active energy ray curable adhesive. Examples of the active energy ray curable adhesive include an ultraviolet ray curable adhesive and an electron beam curable adhesive. From the viewpoint of the curing mechanism, examples of the active energy ray curable adhesive include a radical curable adhesive, a cationic curable adhesive, an anionic curable adhesive, and a hybrid of a radical curable adhesive and a cationic curable adhesive. Typically, a radical curable ultraviolet ray curable adhesive may be used. This is because it is versatile and the characteristics (composition) can be easily adjusted.

[0049] The active energy ray curable adhesive typically contains a monofunctional component, a polyfunctional component (curing component), and a photopolymerization initiator. The monofunctional component and the polyfunctional component are typically radical polymerizable compounds. Preferred monofunctional components include, for example, higher alkyl esters of (meth)acrylic acid and modified products thereof. Specific examples include isostearyl acrylate, lauryl acrylate, acryloylmorpholine, and unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone. Preferred polyfunctional components include, for example, monomers and / or oligomers having two or more functional groups such as (meth)acrylate groups and (meth)acrylamide groups. Specific examples include polyethylene glycol diacrylate, trimethylpropane triacrylate, and glycerin triacrylate. Specific examples of monofunctional or polyfunctional components other than those mentioned above include tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, phenoxydiethylene glycol acrylate, cyclic trimethylolpropane formal acrylate, dioxane glycol diacrylate, EO-modified diglycerin tetraacrylate, γ-butyrolactone acrylate, N-methylpyrrolidone, hydroxyethyl acrylamide, N-methylol acrylamide, N-methoxymethyl acrylamide, N-ethoxymethyl acrylamide, and 9-vinyl carbazole. In one embodiment, the monofunctional or polyfunctional component has a ring structure. Specific examples include acryloyl morpholine, γ-butyrolactone acrylate, unsaturated fatty acid hydroxyalkyl ester-modified ε-caprolactone, N-methylpyrrolidone, and 9-vinyl carbazole. Each of the monofunctional or polyfunctional components may be used alone or in combination of two or more.

[0050] The refractive index n2 of the adhesive layer made of the above-mentioned active energy ray-curable adhesive may be, for example, 1.45 to 1.49.

[0051] The thickness of the adhesive layer, regardless of the presence or absence of an undercoat layer, is preferably 0.1 μm to 3.0 μm, and more preferably 0.5 μm to 2.0 μm.

[0052] F. Undercoat layer The undercoat layer is typically a solidified layer of a coating film of an aqueous resin. A preferred example of the aqueous resin is a urethane resin. Therefore, the undercoat layer can preferably be a solidified layer of a coating film of an aqueous dispersion (undercoat agent) containing a urethane resin. The aqueous system is more environmentally friendly than the solvent system, and can also be excellent in workability.

[0053] The urethane resin is typically obtained by reacting a polyol with a polyisocyanate. The polyol is not particularly limited as long as it has two or more hydroxyl groups in the molecule, and any appropriate polyol can be used. Specific examples include polyacrylic polyol, polyester polyol, and polyether polyol. These can be used alone or in combination of two or more.

[0054] Examples of polyisocyanates include aliphatic diisocyanates such as tetramethylene diisocyanate, dodecamethylene diisocyanate, 1,4-butane diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, and 3-methylpentane-1,5-diisocyanate; isophorone diisocyanate, hydrogenated xylylene diisocyanate, 4,4'-cyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, and 1,3-bis(isocyanate methyl)silane diisocyanate. Examples of the diisocyanates include alicyclic diisocyanates such as cyclohexane, aromatic diisocyanates such as tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, and 1,4-phenylene diisocyanate, and aromatic aliphatic diisocyanates such as dialkyl diphenylmethane diisocyanate, tetraalkyl diphenylmethane diisocyanate, and α,α,α,α-tetramethyl xylylene diisocyanate. These may be used alone or in combination of two or more.

[0055] The urethane resin preferably has a carboxyl group. By having a carboxyl group, an undercoat layer having excellent adhesion to a polarizer (particularly under high temperature and high humidity) can be obtained. The urethane resin having a carboxyl group can be obtained, for example, by reacting the above-mentioned polyol and the above-mentioned polyisocyanate with a chain lengthening agent having a free carboxyl group. Examples of the chain lengthening agent having a free carboxyl group include dihydroxycarboxylic acid and dihydroxysuccinic acid. Examples of the dihydroxycarboxylic acid include dialkylolalkanoic acid such as dimethylolalkanoic acid (e.g., dimethylolacetic acid, dimethylolbutanoic acid, dimethylolpropionic acid, dimethylolbutyric acid, and dimethylolpentanoic acid). These can be used alone or in combination of two or more.

[0056] The number average molecular weight of the urethane resin is preferably 5,000 to 600,000, and more preferably 10,000 to 400,000. The acid value of the urethane resin is preferably 10 or more, more preferably 10 to 50, and particularly preferably 20 to 45. When the acid value is within this range, the adhesion to the polarizer can be more excellent.

[0057] The undercoat agent preferably includes a crosslinking agent. Any suitable crosslinking agent may be used as the crosslinking agent. Specifically, when the urethane resin has a carboxyl group, the crosslinking agent preferably includes a polymer having a group that can react with the carboxyl group. Examples of the group that can react with the carboxyl group include an organic amino group, an oxazoline group, an epoxy group, and a carbodiimide group. Preferably, the crosslinking agent has an oxazoline group. The crosslinking agent having an oxazoline group has a long pot life at room temperature when mixed with the urethane resin, and the crosslinking reaction proceeds by heating, so that the workability is good.

[0058] The undercoat agent preferably does not contain fine particles. With such a configuration, an undercoat layer with small retardation unevenness can be realized. As a result, a polarizing plate with significantly suppressed redness can be realized even when a polarizer with large reflection anisotropy for long wavelength light is used due to a synergistic effect with the effect of the small in-plane retardation of the protective layer. The undercoat agent may contain a leveling agent as necessary. By including a leveling agent, the smoothness of the coating film can be further improved, and as a result, an undercoat layer with small thickness variation can be formed. Examples of the leveling agent include isopropyl alcohol (IPA), ethylene glycol, and propylene glycol. The content of the leveling agent in the undercoat agent may be, for example, 1.0% by weight to 3.5% by weight.

[0059] The undercoat agent preferably contains a refractive index adjuster. A representative example of the refractive index adjuster is a high refractive index material. An example of the high refractive index material is titanium oxide. By adjusting the type (and therefore the refractive index) and the amount of the refractive index adjuster, it is possible to obtain an undercoat agent capable of forming an undercoat layer having a desired refractive index.

[0060] The undercoat agent may further contain any suitable additive. Examples of the additive include antiblocking agents, dispersion stabilizers, thixotropic agents, antioxidants, UV absorbers, defoamers, thickeners, dispersants, surfactants, catalysts, fillers, lubricants, and antistatic agents. The type, number, combination, and amount of additives may be appropriately set according to the purpose.

[0061] Details of the urethane resin and the undercoat agent are described, for example, in JP-A-2010-055062 and JP-A-2021-047235. The descriptions in the publications are incorporated herein by reference.

[0062] The thickness of the undercoat layer is preferably 150 nm to 600 nm, more preferably 200 nm to 500 nm, and further preferably 250 nm to 400 nm. With such a configuration, breakage during formation of the undercoat layer on the protective layer can be suppressed.

[0063] The refractive index n4 of the undercoat layer is preferably 1.50 to 1.70, more preferably 1.60 to 1.70. If the refractive index of the undercoat layer is within such a range, the absolute value of the difference between the refractive index n 1A in the absorption axis direction of the polarizer and the refractive index n4 of the undercoat layer can be within the above desired range.

[0064] G. Retardation layer As described above, the retardation layer typically has a circular polarization function or an elliptical polarization function. Further, as described above, the retardation layer may be composed of a stretched film of a resin film or may be a liquid crystal alignment cured layer.

[0065] G-1. Stretched film of resin film When the retardation layer is composed of a stretched film of a resin film, the retardation layer is typically a single layer and can function as a so-called λ / 4 plate. In this case, Re(550) of the retardation layer is preferably 100 nm to 200 nm, more preferably 110 nm to 180 nm, still more preferably 120 nm to 160 nm, and particularly preferably 130 nm to 150 nm. The retardation layer preferably satisfies the relationship of Re(450) < Re(550), and preferably further satisfies the relationship of Re(550) < Re(650). That is, the retardation layer exhibits an inverse dispersion wavelength dependence in which the retardation value increases according to the wavelength of the measurement light. Re(450) / Re(550) of the retardation layer is, for example, more than 0.5 and less than 1.0, preferably 0.7 to 0.95, more preferably 0.75 to 0.92, and still more preferably 0.8 to 0.9. Re(650) / Re(550) is preferably 1.0 or more and less than 1.15, more preferably 1.03 to 1.1. Further, the angle formed by the slow axis of the retardation layer and the absorption axis of the polarizer is preferably 40° to 50°, more preferably 42° to 48°, still more preferably 44° to 46°, and particularly preferably about 45°.

[0066] Since the retardation layer has in-plane retardation as described above, it has a relationship of nx > ny. As long as the retardation layer has a relationship of nx > ny, it exhibits any appropriate refractive index characteristics. The refractive index characteristics of the retardation layer typically show a relationship of nx > ny ≥ nz. Here, "ny = nz" includes not only the case where ny and nz are exactly equal but also the case where they are substantially equal. Therefore, within a range that does not impair the effects of the present invention, ny < nz may occur. The Nz coefficient of the retardation layer is preferably from 0.9 to 2.0, more preferably from 0.9 to 1.5, and even more preferably from 0.9 to 1.2.

[0067] The thickness of the retardation layer can be set so as to function most appropriately as a quarter-wave plate. In other words, the thickness can be set so as to obtain a desired in-plane retardation. Specifically, the thickness is preferably from 15 μm to 60 μm, more preferably from 20 μm to 55 μm, and most preferably from 25 μm to 50 μm.

[0068] The retardation layer can be composed of any appropriate material as long as it can satisfy the above-described characteristics. The retardation layer typically contains a resin containing at least one bonding group selected from the group consisting of carbonate bonds and ester bonds. In other words, the retardation layer contains a polycarbonate-based resin, a polyester-based resin, or a polyester carbonate-based resin. In one embodiment, the retardation layer can be composed of a film that uses the material described in Item C above for the protective layer and is appropriately processed (e.g., stretching treatment) to satisfy the above characteristics. In one embodiment, the retardation layer may be composed of a film containing a blend of a polycarbonate-based resin and an acrylic-based resin. The acrylic-based resin preferably contains a structural unit derived from methyl methacrylate as a main structural unit. The content of the acrylic-based resin in the retardation layer can be, for example, from 0.5% by mass to 2.0% by mass.

[0069] G-2. Liquid Crystal Alignment固化Layer If the retardation layer is a liquid crystal alignment solidified layer, the polarizing plate (polarizing plate with retardation layer) can be significantly thinner. In this case, as described above, the retardation layer may be a single layer, or may have a two-layer structure of a first liquid crystal alignment solidified layer and a second liquid crystal alignment solidified layer. In this specification, the "alignment solidified layer" refers to a layer in which liquid crystal compounds are aligned in a predetermined direction within the layer and the alignment state is fixed. The "alignment solidified layer" is a concept that includes an alignment hardened layer obtained by hardening a liquid crystal monomer. In the retardation layer, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the retardation layer (homogeneous alignment).

[0070] G-2-1. Single layer When the liquid crystal alignment solidified layer is a single layer, its characteristics are the same as those described in section G-1 regarding the stretched resin film, except for the thickness. When the liquid crystal alignment solidified layer is a single layer, its thickness can be, for example, 1.0 μm to 5.0 μm, or, for example, 1.0 μm to 3.0 μm.

[0071] Specific examples of the liquid crystal compound constituting the retardation layer of the present embodiment are described in, for example, JP 2006-163343 A, JP 2006-178389 A, and WO 2018 / 123551 A. The descriptions in these publications are incorporated herein by reference.

[0072] G-2-2. Two-layer structure consisting of a first liquid crystal alignment solidified layer and a second liquid crystal alignment solidified layer When the retardation layer has a two-layer structure of a first liquid crystal alignment solidified layer and a second liquid crystal alignment solidified layer from the polarizer side, the first liquid crystal alignment solidified layer can typically function as a λ / 2 plate, and the second liquid crystal alignment solidified layer can typically function as a λ / 4 plate. Specifically, the Re(550) of the first liquid crystal alignment solidified layer is preferably 200 nm to 300 nm, more preferably 230 nm to 290 nm, and even more preferably 250 nm to 280 nm; the Re(550) of the second liquid crystal alignment solidified layer is as described in section G-1 regarding the stretched film of the resin film. The thickness of the first liquid crystal alignment solidified layer can be adjusted so that a desired in-plane retardation of the λ / 2 plate is obtained. Specifically, the thickness can be, for example, 2.0 μm to 4.0 μm. The thickness of the second liquid crystal alignment solidified layer can be adjusted so that a desired in-plane retardation of the λ / 4 plate is obtained. Specifically, the thickness may be, for example, 1.0 μm to 2.5 μm. In this embodiment, the angle between the slow axis of the first liquid crystal alignment solidified layer and the absorption axis of the polarizer is preferably 10° to 20°, more preferably 12° to 18°, and even more preferably 14° to 16°; the angle between the slow axis of the second liquid crystal alignment solidified layer and the absorption axis of the polarizer is preferably 70° to 80°, more preferably 72° to 78°, and even more preferably 74° to 76°. The arrangement order of the first liquid crystal alignment solidified layer and the second liquid crystal alignment solidified layer may be reversed, and the angle between the slow axis of the first liquid crystal alignment solidified layer and the absorption axis of the polarizer and the angle between the slow axis of the second liquid crystal alignment solidified layer and the absorption axis of the polarizer may be reversed. The first liquid crystal alignment solidified layer and the second liquid crystal alignment solidified layer may exhibit an inverse dispersion wavelength characteristic in which the retardation value increases depending on the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases depending on the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value changes very little depending on the wavelength of the measurement light.

[0073] The retardation layer of the present embodiment is formed, for example, using a composition containing any suitable liquid crystal monomer. As the liquid crystal monomer, for example, polymerizable mesogen compounds described in JP-A-2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, and GB2280445 can be used. Specific examples of such polymerizable mesogen compounds include BASF's product name LC242, Merck's product name E7, and Wacker-Chem's product name LC-Sillicon-CC3767. As the liquid crystal monomer, for example, a nematic liquid crystal monomer is preferable.

[0074] H. Image display device The polarizing plate described in the above items A to G can be applied to an image display device. Therefore, the embodiment of the present invention also includes an image display device using such a polarizing plate. Representative examples of image display devices include liquid crystal display devices and organic EL display devices. The image display device according to the embodiment of the present invention typically includes the polarizing plate described in the above items A to G on the viewing side. The polarizing plate is disposed so that the protective layer 30 is on the viewing side. EXAMPLES

[0075] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The evaluation items and measurement methods in the examples are as follows.

[0076] (1) Refractive index Regarding the refractive index of the adhesive layer, a single film sample was prepared from the adhesive constituting the adhesive layer, and the refractive index of the sample was measured using a multi-wavelength Abbe refractometer (manufactured by Atago Co., Ltd.). Refractive index n in the absorption axis direction of the polarizer 1A and the refractive index n perpendicular to the absorption axis 1Twas measured and calculated as follows. A polarizer was transferred from the polarizing plate having the resin substrate / polarizer configuration obtained in the Examples and Comparative Examples to the surface of the adhesive layer of a blackboard provided with an adhesive layer to obtain a test sample. Using this test sample, the reflectance R SA and the reflectance R in the direction perpendicular to the absorption axis ST was measured using a spectrophotometer (Hitachi U-4100). SA is the reflectance when the vibration direction of the linearly polarized light from the light source of the spectrophotometer is parallel to the absorption axis direction; R ST is the reflectance when the vibration direction of the linearly polarized light from the light source of the spectrophotometer is perpendicular to the absorption axis direction. Using equations (I) and (II), R SA and R ST From 1A and n 1T The measurement wavelength was 700 nm. R SA =(1-n 1A ) 2 / (1+n 1A ) 2 (I) R ST =(1-n 1T ) 2 / (1+n 1T ) 2 (II)

[0077] (2) In-plane phase difference Re(550) The resin films constituting the protective layers used in the examples and comparative examples were measured using Axoscan (manufactured by Axometrics).

[0078] (3)Reflectance The polarizing plates obtained in the examples and comparative examples were attached to a blackboard via an acrylic adhesive to prepare measurement samples. The reflectance R of the measurement sample in the absorption axis direction of the polarizer PA and the reflectance R in the direction perpendicular to the absorption axis PT was measured using a spectrophotometer (Hitachi, Ltd., U-4100) in the same manner as in (1) above.

[0079] (4) Reflective hue The measurement sample prepared in the same manner as in (3) above was measured using a spectrophotometer / colorimeter (CM-26d, manufactured by Konica Minolta).

[0080] (5) Redness The color of the measurement sample prepared in the same manner as in (3) above was visually observed and evaluated according to the following criteria. Good: No redness was noted Poor: Redness was noticed

[0081] [Production Example 1: Preparation of polarizing plate] As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of about 75° C. was used, and one side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a ratio of 9:1, and dissolving the mixture in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched 2.4 times in the machine direction (longitudinal direction) in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the finally obtained polarizer would be the desired value (dyeing treatment). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4% by weight, potassium iodide concentration: 5% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, the film was dried in an oven maintained at about 90° C. while being brought into contact with a SUS heated roll whose surface temperature was maintained at about 75° C. (drying shrinkage treatment). In this way, a polarizer having a thickness of about 5 μm was formed on the resin substrate, and a polarizing plate having a resin substrate / polarizer structure was obtained. The single transmittance Ts of the polarizer was 42.6% and the polarization degree P was 99.99%. The refractive index n 1A is 1.70, and the refractive index in the direction perpendicular to the absorption axis, n 1T The reflectance R SA is 6.7%, and the reflectance R ST is 4.3%, and R SA and R ST The difference was 2.4%.

[0082] [Production Example 2: Preparation of resin film constituting protective layer] Polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with an agitator and a reflux condenser controlled at 100° C. Bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane (compound 3) 29.60 parts by mass (0.046 mol), ISB 29.21 parts by mass (0.200 mol), SPG 42.28 parts by mass (0.139 mol), DPC 63.77 parts by mass (0.298 mol), and calcium acetate monohydrate 1.19×10 as a catalyst. -2 Part of mass (6.78×10 -5mol) was charged. After the inside of the reactor was purged with nitrogen under reduced pressure, heating was performed with a heat medium, and stirring was started when the inside temperature reached 100 ° C. 40 minutes after the start of the temperature increase, the inside temperature was reached 220 ° C., and while controlling to maintain this temperature, the pressure was reduced and 90 minutes after reaching 220 ° C., the pressure was reduced to 13.3 kPa. Phenol vapor by-produced with the polymerization reaction was led to a reflux condenser at 100 ° C., a small amount of monomer components contained in the phenol vapor were returned to the reactor, and the uncondensed phenol vapor was led to a condenser at 45 ° C. and recovered. Nitrogen was introduced into the first reactor to restore the pressure to atmospheric pressure, and the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, the temperature increase and pressure reduction in the second reactor were started, and the inside temperature was set to 240 ° C. and the pressure to 0.2 kPa in 50 minutes. Thereafter, polymerization was allowed to proceed until the specified stirring power was reached. When the predetermined power was reached, nitrogen was introduced into the reactor to restore pressure, and the polyester carbonate produced was extruded into water and the strands were cut to obtain pellets. The obtained polycarbonate resin was vacuum-dried at 80°C for 5 hours, and then a polycarbonate-based resin film having a thickness of 13 μm was produced using a film-forming device equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 300 mm, setting temperature: 250°C), a chill roll (setting temperature: 120-130°C) and a winder. The in-plane retardation Re (550) of the obtained polycarbonate-based resin film was 1 nm. Finally, a hard coat layer (thickness 2 μm) was formed on one surface of the polycarbonate-based resin film.

[0083] [Production Example 3-1: Preparation of Adhesive Constituting Adhesive Layer] 61.5 parts by weight of unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone (Daicel Corporation, Plaxel FA1DDM), 30.8 parts by weight of acryloylmorpholine (KJ Chemicals, ACMO), 7.7 parts by weight of polyethylene glycol diacrylate (Kyoeisha Chemical, Light Acrylate 9EG-A), 15.3 parts by weight of acrylic oligomer (Toagosei, ARUFON UP-1190), and 7.0 parts by weight of radical polymerization initiator were mixed to prepare ultraviolet curable adhesive A. The refractive index of adhesive A after curing was 1.49.

[0084] [Production Example 3-2: Preparation of adhesive constituting adhesive layer] A refractive index adjuster (titanium oxide, "A-190" manufactured by Sakai Chemical Industry Co., Ltd.) was added to the ultraviolet-curable adhesive A to prepare an ultraviolet-curable adhesive B having a refractive index of 1.53 after curing.

[0085] [Production Example 3-3: Preparation of adhesive constituting adhesive layer] A refractive index adjuster (titanium oxide, "A-190" manufactured by Sakai Chemical Industry Co., Ltd.) was added to the ultraviolet-curable adhesive A to prepare an ultraviolet-curable adhesive C having a refractive index of 1.60 after curing.

[0086] [Production Example 4-1: Preparation of Undercoat Agent Constituting Undercoat Layer] Undercoat agent X was prepared by mixing 16.8 parts by weight of polyester urethane (manufactured by Daiichi Kogyo Seiyaku, product name: Superflex 210, solids content: 33%), 4.2 parts by weight of a crosslinker (oxazoline-containing polymer, manufactured by Nippon Shokubai, product name: Epocross WS-700, solids content: 25%), and 2.0 parts by weight of 1% by weight ammonia water, and adding pure water and isopropyl alcohol (IPA, leveling agent) to adjust the solids concentration to 1% by weight and the IPA concentration to 2.5% by weight. The refractive index of the undercoat layer formed from undercoat agent X was 1.51.

[0087] [Production Example 4-2: Preparation of undercoat agent constituting undercoat layer] A refractive index adjuster (titanium oxide, "A-190" manufactured by Sakai Chemical Industry Co., Ltd.) was used in Primer X to prepare Primer Y, which would give a refractive index of the resulting primer layer of 1.60.

[0088] [Production Example 4-3: Preparation of undercoat agent constituting undercoat layer] A refractive index adjuster (titanium oxide, "A-190" manufactured by Sakai Chemical Industry Co., Ltd.) was used in Primer X to prepare Primer Z, which would give a refractive index of the resulting primer layer of 1.70.

[0089] [Example 1] The undercoat agent X of Production Example 4-1 was applied to the surface of the polycarbonate-based resin film obtained in Production Example 2 on which the hard coat (HC) layer was not formed, and dried to form an undercoat layer, thereby obtaining a laminate of HC layer / polycarbonate-based resin film / undercoat layer. The undercoat layer of the laminate was attached to the polarizer side of the laminate of the resin substrate / polarizer obtained in Production Example 1 via the adhesive A of Production Example 3-1 (thickness after curing: 1 μm). Finally, the resin substrate was peeled off to obtain a polarizing plate having a configuration of HC layer / polycarbonate-based resin film (protective layer) / undercoat layer / adhesive layer / polarizer. The obtained polarizing plate was subjected to the above evaluations (3) to (5). The results are shown in Table 1.

[0090] [Examples 2 to 5, Comparative Examples 1 to 2] A polarizing plate was produced in the same manner as in Example 1, except that the adhesive layer and the undercoat layer were combined as shown in Table 1. The obtained polarizing plate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0091] [Table 1]

[0092] [evaluation] As is clear from Table 1, according to the examples of the present invention, a polarizing plate in which redness is suppressed can be realized despite the use of a polarizer with large reflection anisotropy for light with long wavelengths. [Industrial Applicability]

[0093] The polarizing plate according to the embodiment of the present invention can be suitably used in image display devices (typically, liquid crystal display devices and organic EL display devices). [Explanation of symbols]

[0094] 10 Polarizer 20 Adhesive layer 30 protective layer 40 Undercoat layer 100 Polarizing Plate 101 Polarizing plate

Claims

1. A polarizing plate having a polarizer made of a polyvinyl alcohol-based resin film containing iodine and a protective layer laminated on the polarizer via an adhesive layer, The refractive index n of the polarizer in the absorption axis direction 1A and the refractive index n of the adhesive layer 2 The absolute value of the difference between The reflectance R of the polarizer in the absorption axis direction at a wavelength of 700 nm SA and the reflectance R in the direction perpendicular to the absorption axis ST The difference between the The reflectance R of the polarizing plate in the absorption axis direction of the polarizer at a wavelength of 700 nm PA and the reflectance R in the direction perpendicular to the absorption axis PT The difference between the Polarizing plate.

2. The refractive index n of the adhesive layer 2 2. The polarizing plate according to claim 1, wherein the polarizing angle .theta. is 1.50 to 1.

70.

3. A polarizing plate having a polarizer made of a polyvinyl alcohol-based resin film containing iodine, a protective layer laminated on the polarizer via an adhesive layer, and an undercoat layer provided between the adhesive layer and the protective layer, The refractive index n of the polarizer in the absorption axis direction 1A and the refractive index n of the undercoat layer 4 The absolute value of the difference between The reflectance R of the polarizer in the absorption axis direction at a wavelength of 700 nm SA and the reflectance R in the direction perpendicular to the absorption axis ST The difference between the The reflectance R of the polarizing plate in the absorption axis direction of the polarizer at a wavelength of 700 nm PA and the reflectance R in the direction perpendicular to the absorption axis PT The difference between the Polarizing plate.

4. The refractive index n of the undercoat layer 4 The polarizing plate according to claim 3, wherein the σ is 1.50 to 1.

70.

5. 5. The polarizing plate according to claim 1, wherein the protective layer has an in-plane retardation Re(550) of 20 nm or less.

6. The polarizing plate according to claim 5 , wherein the protective layer is made of a polycarbonate-based resin film.

7. The polarizing plate according to claim 1 , further comprising a retardation layer having a circular polarization function or an elliptically polarizing function on the opposite side of the polarizer to the protective layer.

8. An image display device comprising the polarizing plate according to claim 1 .

9. An image display device comprising the polarizing plate according to claim 7 .

Citation Information

Patent Citations

  • Polarizing plate and liquid crystal display device using the same

    JP2013127569A

  • Polarization plate

    JP2018151603A

  • Manufacturing method of decorative glass member

    JP2019107830A

  • Optical laminate, display panel, and display device

    JP2019204083A

  • Polarizing plate with surface protective film

    JP2020086237A