Resistance Spot Welding Method

A two-step energization process with controlled current patterns and cooling steps addresses the challenge of cracking in resistance spot welding of surface-treated steel plates, enabling stable large nugget formation and robust welds.

JP7558475B2Active Publication Date: 2024-10-01JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022566087
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-30
Filing Date
2022-07-19
Publication Date
2024-10-01
Estimated Expiration
2042-07-19

AI Technical Summary

Technical Problem

Resistance spot welding of surface-treated steel plates, particularly those with zinc plating, often results in cracks due to liquid metal embrittlement and deformation, making it difficult to stably secure large nugget diameters while suppressing cracking.

Method used

A two-step energization process is employed, where the first energization forms a nugget with controlled current values and multi-stage or upslope patterns to minimize deformation, followed by a second energization with cooling steps to expand the nugget diameter, thereby stabilizing the weld without excessive deformation or cracking.

Benefits of technology

This method effectively stabilizes the formation of large nugget diameters while suppressing cracking, ensuring strong and reliable welds in surface-treated steel plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558475000006
    Figure 0007558475000006
  • Figure 0007558475000007
    Figure 0007558475000007
  • Figure 0007558475000008
    Figure 0007558475000008
Patent Text Reader

Abstract

The purpose of the present invention is to provide a resistance spot welding method. In the resistance spot welding method according to the present invention, the carbon equivalent of a high strength galvanized steel sheet used for plate assembly is 0.20% or higher and the tensile strength is 780 MPa or higher. In a first electrification step, when a current value at the beginning of electrification is denoted as Is, a current value at the end of the electrification is denoted as If, and the thickness of a thinnest steel plate of superimposed steel plates is denoted as t, a welding part having a nugget diameter of 3.0 √tmm to 4.5 √tmm is formed while the electrification is performed so that the current value If at the end of the electrification satisfies If>Is. In a second electrification step, a cooling step for maintaining a non-electrification state during 10 ms or more and less than 160 ms, and an electrification step for performing electrification with a current value Ip that is at least the current value If at the end of electrification during 20 ms or more and less than 200 ms are repeated.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resistance spot welding method. [Background technology]

[0002] In general, resistance spot welding, which is a type of lap resistance welding method, is used to join two or more overlapping steel plates. In this welding method, as shown in FIG. 1, two overlapping steel plates 1 and 2 are put together, the upper and lower sides of the plate set are sandwiched between a pair of electrodes 3 and 4, and a welding current is passed between the upper and lower electrodes while applying pressure from the upper and lower sides of the plate set with the pair of electrodes 3 and 4 to join the steel plates together. A spot-shaped weld 5 is obtained by using resistance heat generated by passing a welding current. This spot-shaped weld 5 is called a nugget, and is a portion where the two steel plates 1 and 2 melt and solidify at the contact point of the steel plates when a welding current is passed through the overlapping steel plates, and the steel plates are joined together in a spot-shaped manner. Note that FIG. 1 shows two overlapping steel plates as an example.

[0003] However, resistance spot welding of a sheet assembly in which multiple steel sheets, including surface-treated steel sheets, are overlapped has a problem that cracks may occur in the welded portion. Here, surface-treated steel sheets refer to steel sheets having a metal plating layer, such as zinc plating represented by electrolytic zinc plating and hot-dip galvanizing (including alloyed hot-dip galvanizing), or zinc alloy plating containing elements such as aluminum and magnesium in addition to zinc, on the surface of the base material (underlying steel sheet). The melting points of zinc plating and zinc alloy plating are lower than the melting point of the base material, and therefore the following problems arise.

[0004] In other words, it is believed that cracks in welds are caused by so-called liquid metal embrittlement, in which the low-melting point metal plating layer on the surface of the steel sheet melts during welding, and when the pressure from the electrodes and tensile stress due to the thermal expansion and contraction of the steel sheet are applied to the weld, the molten low-melting point metal penetrates the crystal grain boundaries of the base material of the surface-treated steel sheet, reducing the grain boundary strength and causing cracks.

[0005] Such cracks are likely to occur when a large deformation is applied to the welded portion. For example, when welding is performed under conditions that cause expulsion, they are likely to occur on the surfaces of the steel sheets 1 and 2 that are in contact with the electrodes 3 and 4 as shown in FIG. 5. On the other hand, from the viewpoint of ensuring joint strength, it is important to secure a nugget with a large nugget diameter. In actual welding, there are cases where sufficient current density cannot be secured in the area to be welded due to the influence of welding disturbances such as current shunting to a welding point located near the area to be welded and electrode wear due to continuous welding. In such cases, the heat input decreases, making it difficult to secure a predetermined nugget diameter. By setting the current value during welding to be large while taking into consideration the above-mentioned case where the heat input decreases, it is possible to secure a nugget with a large nugget diameter, but in that case, a large deformation of the welded portion occurs, as typified by the occurrence of expulsion, and the risk of cracking increases. As described above, it is difficult to stably secure a nugget with a large nugget diameter while suppressing the occurrence of cracks during welding in actual welding, which is a practical issue for surface-treated steel sheets.

[0006] As countermeasures to such problems, for example, there are techniques described in Patent Documents 1 to 4. Patent Document 1 proposes a method for suppressing the occurrence of cracks in spot welding of high-strength plated steel sheets by appropriately adjusting the welding current duration and the holding time after the welding current is applied.

[0007] In addition, in Patent Document 2, a method is proposed in which the current pattern is three or more stages, the current flow time, welding current, and other welding conditions are adjusted so that the appropriate current range (the current range in which a nugget diameter that is equal to or larger than the desired nugget diameter and in which the residual melt pressure is equal to or larger than 0.05 mm can be stably formed) is 1.0 kA or more, preferably 2.0 kA or more, and a cooling time is provided between each stage, thereby suppressing the occurrence of cracks.

[0008] Moreover, Patent Document 3 proposes a method of suppressing the occurrence of cracks by appropriately adjusting the holding time after energization.

[0009] Furthermore, Patent Document 4 proposes a method of improving the cross tensile strength of a joint by forming a nugget by main current application and then applying a short-time post-current that does not cause the nugget to grow. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2003-103377 A [Patent Document 2] JP 2003-236676 A [Patent Document 3] JP 2017-47476 A [Patent Document 4] JP 2012-187639 A Summary of the Invention [Problem to be solved by the invention]

[0011] However, in Patent Documents 1 and 2, the influence of disturbances during construction is not considered, and in consideration of the actual construction during automobile assembly, the countermeasures may be insufficient. Furthermore, Patent Document 3 is a technology that can prevent cracks that occur between the end of current flow and the opening of the electrodes, but does not mention cracks that occur during current flow, and it can be difficult to prevent such cracks. Furthermore, Patent Document 4 does not mention cracks during welding, and under conditions for forming a large nugget diameter with this current flow, deformation of the steel sheet surface becomes large, which may cause cracks.

[0012] In addition, the problem of difficulty in reliably obtaining a nugget with a large diameter while suppressing the occurrence of cracks during welding in such surface-treated steel sheets is not limited to the case of resistance spot welding of automotive steel sheets, but also exists in resistance spot welding of other steel sheets.

[0013] The present invention has been made in consideration of the above circumstances, and has an object to provide a resistance spot welding method that can stably secure a nugget with a large nugget diameter while suppressing cracking during welding of surface-treated steel sheets. [Means for solving the problem]

[0014] The present inventors have conducted extensive research in order to achieve the above object.

[0015] Cracks during welding are likely to occur when large deformation occurs in the weld. Therefore, if it is possible to enlarge the nugget while minimizing deformation, it is possible to suppress cracks during welding and ensure a stable production of a nugget with a large diameter. In addition, one of the causes of deformation in the weld is splash, and it has been found that suppressing large splashes (i.e. splashes with a large amount of scattered liquid metal) is effective in suppressing cracks during welding.

[0016] The current flow process during welding is divided into two steps, the first current flow process and the second current flow process. In the first current flow process, current is applied within a range that does not cause excessive deformation, and a nugget with a certain nugget diameter is formed. At this time, the current value is adjusted to suppress deformation, so a sufficiently large nugget is not formed, and if there is an external disturbance that reduces the nugget diameter, for example, a problem may occur in which a nugget with the specified nugget diameter cannot be secured. Therefore, in the second current flow process, the current flow conditions are adjusted to expand the nugget so as not to cause excessive deformation in the welded part, thereby suppressing the occurrence of cracks during welding and stably securing a nugget with a large nugget diameter.

[0017] The energization conditions in the first energization step and the second energization step are shown below.

[0018] In the first current flow process, it is important to form a weld that will not cause significant deformation in the subsequent second current flow process. In this process, the heat input is adjusted by adjusting the current flow pattern to firmly bond the pressure weld (corona bond) around the nugget. This makes it possible to keep the scale of splashing (the amount of molten metal that splashes out) small in the subsequent second current flow process, which reduces deformation of the weld and, as a result, makes it possible to prevent cracks from occurring.

[0019] In the second current application process, the nugget can be enlarged by applying a current value equal to or greater than the current value in the first current application process, but applying current for a long period of time results in excessive heat input, which causes significant deformation of the welded portion. Therefore, by using a current application pattern that repeats short-time current application and short-time cooling, the nugget can be enlarged in stages while suppressing deformation of the welded portion, making it possible to suppress the occurrence of cracks during welding. In such a current application pattern, even if splashing occurs, the scale of the splashing (the amount of molten metal scattered by splashing) can be kept small by applying current for a short period of time. This reduces deformation of the welded portion, which makes it possible to suppress the occurrence of cracks during welding.

[0020] The present invention has been made based on the above findings, and the gist of the present invention is as follows. [1] A resistance spot welding method in which two or more steel sheets, including at least one high-strength zinc-based plated steel sheet, are stacked together to form a sheet assembly, the sheet assembly is clamped between a pair of welding electrodes, and current is passed through the sheet assembly while applying pressure to join the steel sheets, The high-strength zinc-based plated steel sheet has a carbon equivalent Ceq represented by the formula (1) of 0.20% or more and a tensile strength of 780 MPa or more, The energization includes a first energization step and a second energization step, In the first current application step, the current value at the start of current application is Is (kA), the current value at the end of current application is If (kA), and the thickness of the thinnest steel sheet among the overlapping steel sheets is t (mm). By passing current so that the current value If (kA) at the end of current passing satisfies equation (2), a weld with a nugget diameter of 3.0√t (mm) or more and 4.5√t (mm) or less is formed. A resistance spot welding method in which the second current flow process enlarges the nugget by repeating a cooling process in which a no-current state is maintained for a period of 10 ms or more and less than 160 ms, and a current flow process in which current is passed at a current value Ip (kA) equal to or greater than the current value If (kA) at the end of the current flow for a period of 20 ms or more and less than 200 ms. Ceq=C+Si / 30+Mn / 20+2P+4S (1) If >Is (2) Here, the element symbols in formula (1) indicate the content (mass%) of each element, and are set to 0 when the element is not contained. [2] The first current application step is a multi-stage current application having n stages (n is an integer of 2 or more), The current values ​​of each stage in the multi-stage current supply are I1 to In (kA), and the current value I1 (kA) of the first stage is the same as the current value Is (kA) at the start of the current supply and the current value In of the nth stage is the same as the current value If (kA) at the end of the current supply. The resistance spot welding method according to [1], wherein the current values ​​I1 to In (kA) of each stage satisfy formula (3). I1 < I2 < I3 <... <In (3) [3] The resistance spot welding method according to [1], wherein the first current flow step is an upslope current flow in which the current value is continuously increased from a current value Is at the start of the current flow to a current value If at the end of the current flow. [4] The resistance spot welding method according to any one of [1] to [3], wherein the cooling step and the current application step in the second current application step are repeated two or more times. [5] The diameter of the nugget formed after the completion of the first current flow process is N1 (mm), and the diameter of the nugget formed after the completion of the first current flow process and the second current flow process is N2 (mm), The resistance spot welding method according to any one of [1] to [4], wherein an amount of expansion of the nugget diameter in the second current passing step, expressed as (N2-N1), is 0.1√t (mm) or more. Effect of the Invention

[0021] According to the present invention, it is possible to stably form a nugget having a large diameter while suppressing the occurrence of cracks during welding of surface-treated steel sheets, and therefore, it is extremely effective in the industry. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of resistance spot welding according to the present invention. [Diagram 2] FIG. 2 is a diagram showing a test piece for resistance spot welding in an embodiment of the present invention, the upper side being a plan view and the lower side being a side view. [Diagram 3] FIG. 3 is a diagram showing a test piece for resistance spot welding in an embodiment of the present invention, the upper side being a plan view and the lower side being a side view. [Figure 4] FIG. 4 is a diagram showing a test piece for resistance spot welding in an embodiment of the present invention, the upper side being a plan view and the lower side being a side view. [Diagram 5] FIG. 5 is a cross-sectional view that illustrates an example of how cracks occur during conventional resistance spot welding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, the resistance spot welding method of the present invention will be described with reference to the drawings, however, the present invention is not limited to the embodiment.

[0024] The present invention is a resistance spot welding method in which two or more steel sheets are overlapped to form a sheet assembly, the sheet assembly is clamped between a pair of welding electrodes arranged above and below the sheet assembly, and current is passed through the sheet assembly in a current pattern described below while applying pressure to the sheet assembly to form a nugget and join the steel sheets together.

[0025] For example, as shown in Fig. 1, when resistance spot welding a sheet set consisting of two overlapping steel sheets, the overlapping steel sheets (lower steel sheet 2 and upper steel sheet 1) are clamped between a pair of welding electrodes, i.e., a welding electrode 4 (hereinafter sometimes referred to as the "lower electrode") arranged on the lower side of the sheet set and a welding electrode 3 (hereinafter sometimes referred to as the "upper electrode") arranged on the upper side of the sheet set, and electricity is passed through them while applying pressure. The number of overlapping steel sheets is preferably four or less.

[0026] The device for carrying out the resistance spot welding method of the present invention is not particularly limited as long as it is configured to apply pressure using a lower electrode and an upper electrode and control the pressure. For example, devices such as an air cylinder or a servo motor can be used. Furthermore, the configuration for supplying current during energization and controlling the current value is not particularly limited, and the present invention can be applied to both DC and AC. In the case of AC, "current" means "effective current."

[0027] The shape of the tip of the lower electrode and the upper electrode is not particularly limited. For example, DR type (dome radius type), R type (radius type), D type (dome type), etc. described in JIS C 9304:1999 can be mentioned. The tip diameter of each electrode is, for example, 4 mm to 16 mm. The radius of curvature is, for example, 10 mm to 400 mm, and the tip can be a flat type electrode.

[0028] In this way, overlapping steel sheets (sheet set) are clamped between a pair of welding electrodes and current is applied while pressure is applied to form a nugget of a required size by resistance heating, and the overlapping steel sheets are joined to obtain a welded joint. In the present invention, this current is applied in a specific pattern described below.

[0029] The present invention is applied to a sheet assembly in which either one or both sides of the sheet assembly in contact with each welding electrode arranged on the upper and lower sides of the sheet assembly are surface-treated steel sheets having a metal plating layer. Here, the above-mentioned "both sides of the sheet assembly in contact with each welding electrode" refers to the two steel sheets arranged on the outermost side of the sheet assembly consisting of multiple steel sheets in contact with the upper electrode and the lower electrode. In addition, the above-mentioned "either one side of the sheet assembly in contact with each welding electrode" refers to either one of the two steel sheets arranged on the outermost side of the sheet assembly consisting of multiple steel sheets in contact with the upper electrode or the lower electrode. Note that it is preferable that the melting point of the metal plating layer is lower than the melting point of the base material of the surface-treated steel sheet.

[0030] As described above, the surface-treated steel sheet refers to a steel sheet having a metal plating layer, such as zinc plating represented by electrolytic zinc plating, hot-dip galvanizing (including alloyed hot-dip galvanizing), or zinc alloy plating containing elements such as aluminum and magnesium in addition to zinc, on the surface of a base material (base steel sheet). Here, such a surface-treated steel sheet is referred to as a "zinc-based plated steel sheet." Therefore, in the present invention, at least one of the multiple steel sheets constituting the above-mentioned sheet assembly is a zinc-based plated steel sheet.

[0031] The above-mentioned zinc-based plated steel sheet is a high-strength steel sheet (high-strength zinc-based plated steel sheet) having a carbon equivalent (Ceq) (%), expressed by the following formula (1), of 0.20% or more and a tensile strength of 780 MPa or more. Ceq(%)=C+Si / 30+Mn / 20+2P+4S (1) Here, the element symbols in formula (1) indicate the content (mass%) of each element, and are set to 0 when the element is not contained.

[0032] High-strength steel plates are highly susceptible to cracking, and cracking during welding is likely to be a problem. However, the effects of the present invention can be achieved even with steel plates having a tensile strength of 780 MPa or more, with the carbon equivalent adjusted to 0.20% or more. Steel plates having a carbon equivalent of less than 0.20% have low cracking susceptibility, and cracking during welding is unlikely to be a problem in the first place. From the viewpoint of achieving even greater effects, the carbon equivalent Ceq is preferably 0.25% or more, and more preferably 0.30% or more.

[0033] The upper limit of the carbon equivalent (Ceq) is not particularly specified. Since a steel sheet having an extremely high carbon equivalent, i.e., an extremely high susceptibility to cracking, may not be able to obtain a sufficient crack suppression effect even if the current application pattern of the present invention is applied, the carbon equivalent (Ceq) is preferably set to 0.60% or less, and more preferably set to 0.50% or less. The chemical composition of the high-strength zinc-based plated steel sheet used in the present invention may be appropriately adjusted so as to obtain the above-mentioned ranges of carbon equivalent (Ceq) and tensile strength.

[0034] The tensile strength of the zinc-based plated steel sheet is preferably 780 MPa or more. Steel sheets with high tensile strength tend to contain a large amount of alloy components and are easily susceptible to cracking, so the effects of the present invention are easily obtained. The tensile strength is more preferably 980 MPa or more. There is no particular upper limit for the tensile strength of the steel sheet, but the tensile strength is preferably 2500 MPa or less.

[0035] In the present invention, the thickness of the steel plate to be resistance spot welded is not particularly limited. For example, it is preferably within the range of 0.5 mm to 3.0 mm. Steel plates having a thickness within this range can be suitably used as automobile parts.

[0036] The two or more steel sheets to be resistance spot welded may be steel sheets of the same type and shape, or may be steel sheets of different types and shapes. Also, a surface-treated steel sheet having a metal plating layer and a steel sheet not having a metal plating layer may be overlapped.

[0037] Next, a current pattern in the resistance spot welding method of the present invention will be described.

[0038] In the present invention, two or more steel sheets including at least one zinc-based plated steel sheet are stacked together to form a sheet assembly, and the sheet assembly is clamped between a pair of welding electrodes and current is applied while applying pressure to form a nugget and to join the steel sheets. This current application includes a first current application step and a second current application step. In the present invention, this current application is performed in a specific pattern described below.

[0039] <First energization process> First, in the first current flow process, assuming that the current value at the start of current flow is Is (kA), the current value at the end of current flow is If (kA), and the thickness of the thinnest of the overlapping steel sheets is t (mm), current is passed so that the current value Is (kA) at the start of current flow and the current value If (kA) at the end of current flow satisfy the relationship in equation (2), thereby forming a weld with a nugget diameter of 3.0√t (mm) or more and 4.5√t (mm) or less. If >Is (2)

[0040] When the relationship between the current value Is at the start and the current value If at the end of current application is If≦Is, the heat input to the pressure-welded portion is insufficient. As a result, the pressure-welded portion around the nugget cannot be firmly welded in the first current application process, and the effect of reducing the scale of expulsion that may occur in the subsequent second current application process cannot be obtained. In addition, it is difficult to grow the nugget sufficiently, and there is a possibility that the nugget diameter in the above-mentioned range cannot be obtained. The current value If at the end of current application is preferably (Is+1)(kA) or more, and more preferably (Is+3)(kA) or more. The upper limit of the current value If at the end of energization is not particularly specified, but from the viewpoint of suppressing the occurrence of spattering due to a sudden increase in current in the first energization step, the current value If at the end of energization is preferably (Is+10) (kA) or less, and more preferably (Is+8) (kA) or less. In order to form a nugget without expulsion in the first current-passing step and to significantly suppress expulsion in the second current-passing step, the current value If at the end of current passing is preferably set in the range of 5 to 15 kA.

[0041] If the nugget diameter formed is less than 3.0√t (mm), the nugget diameter formed in the first current flow process is too small, making it difficult to effectively expand the nugget in the subsequent second current flow process. As a result, it becomes difficult to ensure a large nugget diameter. Also, if the nugget diameter formed exceeds 4.5√t (mm), the heat input due to current flow becomes excessive, causing the weld to deform and prone to cracking. Therefore, the nugget diameter formed in the first current flow process should be 3.0√t (mm) or more and 4.5√t (mm) or less.

[0042] The nugget diameter formed in the first current application step is preferably in the range of 4.0√t(mm) to 4.5√t(mm). If it is in the range of 4.0√t(mm) to 4.5√t(mm), the effect of increasing the nugget diameter in the subsequent second current application step can be more significantly obtained. The above "t" refers to the thickness of the steel plate. Specifically, the thickness of the thinnest steel plate among the overlapping steel plates that make up the plate assembly is taken as t. For example, when the thicknesses of the multiple steel plates that make up the plate assembly are different, the thickness of the thinnest steel plate among them is taken as t.

[0043] In the present invention, as described above, it is important to form a welded portion in the first current application process that does not cause large deformation in the subsequent second current application process. For this purpose, the current during current application in the first current application process is controlled to satisfy formula (2) and is made variable. Examples of a method for controlling the current to be variable include multi-stage current application and upslope current application. By controlling the current to be variable so that it increases in this way, the pressure welded portion around the nugget is firmly joined in the first current application process and the scale of expulsion in the subsequent second current application process can be kept small, so that deformation of the welded portion is reduced, and as a result, it is possible to suppress the occurrence of cracks. An example of a specific method will be described below.

[0044] [Multi-stage energization] The current in the first current application step is n-stage (n is an integer of 2 or more) multi-stage current application. When the current value in each stage in this multi-stage current application is I1 to In (kA), and the current value I1 (kA) in the first stage is the same as the current value Is (kA) at the start of the current application and the current value In in the nth stage is the same as the current value If (kA) at the end of the current application, it is preferable that the current values ​​I1 to In (kA) in each stage satisfy formula (3). I1 <I2 < I3 <···< In (3) In the case of n-stage multi-stage current application, if the current value I1 (kA) of the first stage, the current value I2 (kA) of the second stage, the current value I3 (kA) of the third stage, ..., the current value In (kA) of the nth stage do not satisfy the formula (3), the heat input to the pressure welded portion will be insufficient. As a result, the pressure welded portion around the nugget cannot be firmly welded in the first current application process, and the effect of reducing the scale of expulsion that may occur in the subsequent second current application process cannot be obtained. In addition, it is difficult to grow the nugget sufficiently, and it may not be possible to obtain a nugget diameter in the above-mentioned range.

[0045] The number of stages, "n", is an integer equal to or greater than 2. From the viewpoint of preventing the management of welding conditions during construction from becoming too complicated, it is preferable that n be 5 or less.

[0046] [Upslope energization] The current flow in the first current flow step is preferably an up-slope current flow in which the current value is continuously increased from the current value Is at the start of current flow to the current value If at the end of current flow. This makes it possible to firmly join the pressure-welded portion around the nugget in the first current flow step, and to keep the scale of expulsion small in the subsequent second current flow step, thereby reducing deformation of the welded portion. As a result, it becomes possible to suppress the occurrence of cracks.

[0047] The energization time and pressure in the first energization step can be appropriately selected so as to ensure the above-mentioned nugget diameter. In the present invention, from the viewpoint of forming a nugget having the above-mentioned nugget diameter without causing splashing, the energization time is preferably set to 100 to 700 ms as a condition of resistance spot welding in the first energization step. If the energization time is 100 ms or less, it is difficult to obtain the effect of firmly joining the pressure-welded portion around the nugget. If the energization time is 700 ms or more, the heat input becomes excessive, which may cause excessive deformation of the welded portion. Here, when the first energization step is a multi-stage energization, the energization time in this step is controlled so that the total energization time in each stage is within the above-mentioned range. More preferably, it is in the range of 100 to 500 mms. The pressure in the first current passing step is preferably in the range of 1.5 kN to 8.0 kN.

[0048] <Second energization process> After the above-mentioned first current application step, a second current application step is performed. In the second current application step, a cooling step in which a no-current state is maintained for 10 ms or more and less than 160 ms, and a current application step in which a current value Ip (kA) equal to or greater than the current value If (kA) at the end of the first current application step is applied for 20 ms or more and less than 200 ms are repeated to enlarge the nugget.

[0049] In the present invention, in order to ensure sufficient joint strength, the nugget diameter of the welded portion obtained after the second current passing step is preferably set to a target diameter in the range of 4.5√t(mm) to 6.0√t(mm).

[0050] [Cooling process] If the no-current time in the cooling process is less than 10 ms, the weld cannot achieve a sufficient cooling effect, and the weld is likely to deform significantly during the subsequent current application process. As a result, cracks are likely to occur in the weld. On the other hand, if the no-current time in the cooling process is 160 ms or more, the impact of nugget shrinkage during cooling is too large, and the effect of enlarging the nugget by repeatedly applying current to the cooling process and current application process cannot be fully achieved. Therefore, the no-current time in the cooling process is set to be 10 ms or more and less than 160 ms.

[0051] [Electrification process] If the current application time in the current application process is less than 20 ms, the nugget cannot be enlarged sufficiently due to insufficient heat input. On the other hand, if the current application time in the current application process is 200 ms or more, excessive heat input is applied in one current application, which makes it easy for large deformation of the welded portion to occur and for cracks to occur in the welded portion. Therefore, the current application time in the current application process is set to 20 ms or more and less than 200 ms. The current application time in this current application process is preferably set to 160 ms or less, and more preferably set to 150 ms or less.

[0052] In order to obtain a more significant effect of stably increasing the nugget diameter while suppressing deformation of the welded portion, it is preferable to set the non-energization time of the cooling step in the second current application step to 10 to 80 ms and the current application time of the current application step in the second current application step to 20 to 100 ms, and more preferably to set the non-energization time of the cooling step to 60 ms or less. More preferably, the de-energization time in the cooling step is 20 ms or more, and even more preferably, the energization time in the energization step is 40 ms or more.

[0053] In addition, if the current value Ip (kA) in the current application process is less than the current value If (kA) at the end of the first current application process, the effect of enlarging the nugget cannot be obtained due to insufficient heat input. Therefore, the current value Ip (kA) in the current application process is set to be equal to or greater than the current value If (kA) at the end of the first current application process. There is no particular upper limit for the current value Ip in the current application process. Under conditions of extremely large current, excessive heat input may cause large deformation of the welded portion, resulting in cracks. Therefore, the current value Ip (kA) is preferably set to be equal to or less than (4×If) (kA), more preferably equal to or less than (3×If) (kA), and even more preferably equal to or less than (1.5×If) (kA).

[0054] In the present invention, the number of repetitions of the cooling step and the current application step in the second current application step may be one, but is preferably two or more. If the number of repetitions is less than two, the effect of enlarging the nugget diameter may not be sufficiently obtained. There is no particular upper limit to the number of repetitions. However, if the number of repetitions exceeds 10, the effect of enlarging the nugget becomes saturated, making it difficult to obtain a large effect, and the total time of the entire welding process becomes long, so from the viewpoint of construction efficiency, 10 times or less is preferable. A more preferable number of repetitions is 5 times or less. The repeated energization in the second energization step is performed at a constant rate.

[0055] In addition, from the viewpoint of ensuring a large diameter nugget in the present invention, when the nugget diameter formed after the first current application step is N1 (mm) and the nugget diameter formed after the first current application step and the second current application step is N2 (mm), the value of (N2-N1), which is the amount of expansion of the nugget diameter in the second current application step, is preferably 0.1√t (mm) or more. The value of (N2-N1) is more preferably 0.3√t (mm) or more, and even more preferably 0.5√t (mm) or more. In addition, if the expansion of the nugget diameter in the second current application step is extremely large, the deformation of the welded part may become large due to excessive heat input, and cracks may occur, so the above expansion amount is preferably 3.0√t (mm) or less. The value of (N2-N1) is more preferably 2.5√t (mm) or less, and even more preferably 2.0√t (mm) or less.

[0056] The above explanation has mainly been given of the case where two steel sheets are overlapped and resistance spot welded, but the present invention is also applicable to the case where three or more steel sheets are overlapped and welded, and the above-mentioned effects can be obtained in the same way. EXAMPLES

[0057] The operation and effects of the present invention will be described below using examples, but the present invention is not limited to the following examples. In this example, two steel sheets including a zinc-based plated steel sheet were used, and the steel sheets were overlapped to form a sheet assembly (see Table 1). Here, as the upper and lower steel sheets, a galvannealed (GA) steel sheet and a cold-rolled steel sheet were used, whose carbon equivalent (Ceq) expressed by the above formula (1), tensile strength, and sheet thickness are shown in Table 1. The sheet assembly was subjected to resistance spot welding under the conditions shown in Table 2-1 or Table 3-1 to produce a welded joint. Table 2-1 shows the conditions for the first current flow process to be "multi-stage current flow", and Table 3-1 shows the conditions for the first current flow process to be "up-slope current flow". In Table 2-1, in multi-stage current flow, the "first stage current value I1 (kA)" refers to the "current value Is (kA) at the start of current flow", and the "final stage (nth stage) current value In (kA)" refers to the "current value If (kA) at the end of current flow". In other words, in the case of multi-stage current flow with n=3, the current value of the third stage, which is the final stage, is the current value at the end of current flow. Resistance spot welding was performed at room temperature, with the welding electrodes (lower electrode, upper electrode) constantly water-cooled. Both the lower electrode and upper electrode were DR-type electrodes made of chromium copper, with a tip diameter (tip diameter) of 6 mm and a curvature radius of 40 mm. The upper electrode was driven by a servo motor to control the pressure, and a DC power source was supplied when electricity was applied. Welded joints were produced under three disturbance conditions for each welding condition: "no disturbance", "with plate gap", and "with existing weld point". The nugget diameter and the occurrence of cracks (LME cracks) were observed for each welded joint. The amount of expansion of the nugget diameter (N2-N1) was also observed. Here, the case of producing a welded joint under the above three disturbance conditions will be described with reference to Figures 2 to 4. Each figure shows a test specimen in a state where steel plates are resistance spot welded together, with the upper figure being a plan view and the lower figure being a side view. The welded joints with the disturbance condition of "no disturbance" were prepared as follows. As shown in FIG. 2, two steel plates (upper steel plate 1, lower steel plate 2) with a size of 30 mm x 100 mm (short side x long side) were prepared from the above steel plate, and the steel plates were stacked to prepare a test specimen. The welded portion 6 in the center of the test specimen was welded under the conditions shown in Table 2-1 or Table 3-1 to prepare a welded joint. The welded portion 6 of the obtained welded joint was observed for the nugget diameter and the occurrence of cracks. The amount of enlargement of the nugget diameter was also observed. The welded joints with the disturbance condition of "with plate gap" were prepared as follows. As shown in FIG. 3, two steel plates (upper steel plate 1, lower steel plate 2) with a size of 30 mm x 100 mm (short side x long side) were prepared from the above steel plate, and spacers 7 and 8 with a thickness of 1.6 mm and a size of 30 mm x 25 mm (long side x short side) were sandwiched between the two steel plates at both ends of the steel plate to prepare a test specimen. The welded portion 6 in the center of the test specimen was welded under the conditions shown in Table 2-1 or Table 3-1 to prepare a welded joint. The welded portion 6 of the obtained welded joint was used to observe the nugget diameter and the occurrence of cracks. In addition, the amount of enlargement of the nugget diameter was observed. The test specimens with the disturbance condition of "already welded" were prepared as follows. As shown in FIG. 4, two steel plates (upper steel plate 1, lower steel plate 2) with a size of 30 mm x 100 mm (short side x long side) were prepared from the above steel plate, and the steel plates were stacked to prepare the test specimen. Already welded points 9 and 10 with a nugget diameter of 5 mm were placed at positions 20 mm away from the center of the test specimen in the longitudinal direction, and then the welded portion 6 in the center of the test specimen was welded under the conditions shown in Table 2-1 or Table 3-1 to prepare a welded joint. The welded portion 6 of the obtained welded joint was used to observe the nugget diameter and the occurrence of cracks. The amount of enlargement of the nugget diameter was also observed. The nugget diameter, the amount of enlargement of the nugget diameter, and the occurrence or absence of cracks were evaluated and judged as follows. [Evaluation of nugget diameter and enlargement of nugget diameter] Regarding the nugget diameter (N1) after the first current flow process, a welding test was conducted in advance under each of the above disturbance conditions, with only the first current flow process, and the nugget diameter was measured by observing the cross section. Here, the cross section of the cut weld was etched and then observed with an optical microscope to measure the nugget diameter between the steel sheets. The obtained measurements are shown in the "Nugget diameter N1 after the first current flow process" column in Tables 2-2 and 3-2. The nugget diameter (N2) after the second current application process was measured in the same manner as described above using each welded joint obtained by conducting the welding test under the above three disturbance conditions. The measured values ​​are shown in the "Nugget diameter N2 after the second current application process" column in Tables 2-2 and 3-2. Further, the values ​​calculated by (N2-N1), which indicate the amount of increase in the nugget diameter in the second current application process, are shown in the "N2-N1" column in Table 2. [Evaluation of cracks] The evaluation of cracks (LME cracks) was performed using each welded joint obtained by conducting welding tests under the three disturbance conditions mentioned above. When the cross section of the weld was observed with an optical microscope, if a crack of 200 μm or more was observed on the surface of the weld, it was evaluated as "cracks present." On the other hand, if no cracks of 200 μm or more were observed, it was evaluated as "no cracks." If "cracks present," it was entered as "present" in the "LME cracks" column in Table 2-2, and if "no cracks" were observed, it was entered as "no" in the same column. 〔judgement〕 Regarding the evaluation, under all three disturbance conditions, the nugget diameter (N2) was 4.5√t (mm) or more and no cracks were generated, and it was evaluated as "〇 (pass)". On the other hand, the other cases were evaluated as "× (fail)". The evaluation results are shown in Table 2-2 and Table 3-2. [Table 1] [Table 2-1] [Table 2-2] [Table 3-1] [Table 3-2] As is clear from Tables 2-2 and 3-2, in the examples of the present invention, good welded joints were obtained that were free of cracks and had a nugget diameter that was the target diameter, regardless of the disturbance conditions, whereas in the comparative examples, good welded joints were not obtained. [Explanation of symbols]

[0058] 1 Upper steel plate 2 Lower steel plate 3 Upper electrode 4 Lower electrode 5. Nugget 6 Welding 7, 8 Spacer 9, 10 Already welded

Claims

1. A resistance spot welding method comprising overlapping two or more steel sheets including at least one high-strength zinc-based plated steel sheet to form a sheet assembly, clamping the sheet assembly between a pair of welding electrodes, and passing current through the sheet assembly while applying pressure to the sheet assembly to join the steel sheets, the method comprising the steps of: The high-strength zinc-based plated steel sheet has a carbon equivalent represented by formula (1) of 0.20% or more and a tensile strength of 780 MPa or more, The current application includes a first current application process for forming a nugget having a nugget diameter of 3.0√t (mm) or more and 4.5√t (mm) or less, and a second current application process for expanding the nugget, In the first current application step, when the current value at the start of current application is Is (kA), the current value at the end of current application is If (kA), and the sheet thickness of the thinnest steel sheet among the overlapping steel sheets is t (mm), A variable current is continuously applied from the start of current application to the end of current application in the first current application step so that the current value If (kA) at the end of current application satisfies formula (2), thereby forming a weld having a nugget diameter of 3.0√t (mm) or more and 4.5√t (mm) or less; In the second current application step, a cooling step of maintaining a current-free state for 10 ms or more and less than 160 ms and a current application step of applying a current at a current value Ip (kA) equal to or more than the current value If (kA) at the end of the current application for 20 ms or more and less than 200 ms are repeated with constant current application to enlarge the nugget, When the nugget diameter formed after the completion of the first current application process is N1 (mm), and the nugget diameter formed after the completion of the first current application process and the second current application process is N2 (mm), The resistance spot welding method according to claim 1, wherein an expansion amount of the nugget diameter in the second current application step, represented by (N2-N1), is 0.1√t (mm) or more. Ceq=C+Si / 30+Mn / 20+2P+4S (1) If>Is (2) Here, the element symbols in formula (1) indicate the content (mass%) of each element, and when an element is not contained, it is set to 0.

2. The first current application step is a multi-stage current application having n stages (n is an integer of 2 or more), Let the current values ​​of each stage in the multi-stage current supply be I1 to In (kA), and let the current value I1 (kA) of the first stage be the same as the current value Is (kA) at the start of the current supply and the current value In of the nth stage be the same as the current value If (kA) at the end of the current supply.

2. The resistance spot welding method according to claim 1, wherein the current values ​​I1 to In (kA) of each stage satisfy formula (3). I1 < I2 < I3 <...< In (3)

3. 2. The resistance spot welding method according to claim 1, wherein the first current flow step is upslope current flow in which a current value is continuously increased from a current value Is at a start of the current flow to a current value If at a termination of the current flow.

4. 2. The resistance spot welding method according to claim 1, wherein the cooling step and the current applying step are repeated two or more times in the second current applying step.

5. 3. The resistance spot welding method according to claim 2, wherein the cooling step and the current applying step are repeated two or more times in the second current applying step.

6. The resistance spot welding method according to claim 3 , wherein the cooling step and the current applying step are repeated two or more times in the second current applying step.

Citation Information

Patent Citations

  • Spot welding method for high strength plated steel plate

    JP2003103377A

  • Method for spot-welding high tensile strength galvanized base steel sheet

    JP2003236676A

  • Resistance spot welding method for high-strength steel sheet

    JP2012187639A

  • Spot welding method

    JP2017047476A

  • Resistance spot welding method

    JP2021079416A