Hydrolyzable nonwoven fabric, hydrolyzable nonwoven fabric laminate, and method for producing hydrolyzable nonwoven fabric

A nonwoven fabric with integrated pulp and regenerated cellulose fibers, treated by high-pressure water jetting, addresses the challenge of combining high wet tensile strength and water-disintegrability, ensuring effective use and easy disposal.

JP7559579B2Active Publication Date: 2024-10-02OJI HLDG CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021011568
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-28
Publication Date
2024-10-02
Estimated Expiration
2041-01-28

AI Technical Summary

Technical Problem

Existing water-disintegratable papers and nonwoven fabrics face challenges in achieving both high wet tensile strength and water-disintegrability, particularly in pop-up wet tissue products, where the fabric needs to maintain strength during use and disintegrate easily after use.

Method used

A water-disintegrable nonwoven fabric composed of pulp fibers and regenerated cellulose fibers, specifically flat and round rayon fibers, is produced with controlled fiber lengths and integrated through high-pressure water jet treatment, creating streaks that enhance both wet tensile strength and water-disintegrability.

Benefits of technology

The fabric achieves excellent wet tensile strength to withstand cleaning tasks without breaking and disintegrates easily in water, suitable for pop-up wet tissue products and flushable in various toilets, including water-saving models.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559579000002
    Figure 0007559579000002
  • Figure 0007559579000003
    Figure 0007559579000003
  • Figure 0007559579000001
    Figure 0007559579000001
Patent Text Reader

Abstract

To provide a water-disintegrable nonwoven fabric having both excellent wet tensile strength and water-disintegrable properties.SOLUTION: A water-disintegrable nonwoven fabric of the invention comprises interlaced pulp fibers, flat rayon fibers, and round rayon fibers. The surface of the water-disintegrable nonwoven fabric has jet stream scars caused by high-pressure water jet stream treatment, and the water-disintegrable nonwoven fabric in a wet state satisfies 70≤WT1≤500 and 2.0≤WT1 / WT2≤6.0, when the tensile strength in the direction in which jet stream scars caused by high-pressure water jet stream treatment are extended is represented as WT1 N / m, and the tensile strength in the direction perpendicular to the direction in which the jet stream scars caused by the high-pressure water jet stream treatment are extended is represented as WT2 N / m.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-disintegrable nonwoven fabric, a water-disintegrable nonwoven fabric laminate, and a method for producing a water-disintegrable nonwoven fabric. [Background technology]

[0002] Conventionally, cleaning products such as toilet cleaning wipes and wet wipes have been used. Some cleaning products can be flushed down a flush toilet after use, which makes disposal after use easy and hygienic. As such cleaning products, cleaning products made of water-disintegrable paper impregnated with water or chemicals have been put on the market.

[0003] Water-disintegrable paper is required to have the property of easily disintegrating when washed with water, while being strong enough to withstand cleaning and other operations. For this reason, inclusion of a paper strength enhancer or a resin component has been considered in order to improve the strength of water-disintegrable paper. For example, Patent Document 1 describes water-disintegrable paper containing a water-soluble binder having a carboxyl group selected from the group consisting of carboxymethyl cellulose, carboxyethyl cellulose, and carboxymethylated starch. Here, it has been considered that the carboxyl group of the water-soluble binder forms an intramolecular mixed salt with a specific polyvalent metal to increase the strength. In addition, Patent Document 2 describes a water-disintegrable nonwoven fabric in which a water-insoluble resin is partially provided on at least one surface layer of a water-disintegrable nonwoven fabric substrate, and a slit is provided in the surface layer provided with the water-insoluble resin. Here, a thermoplastic resin is used as the water-insoluble resin, thereby increasing the strength of the nonwoven fabric.

[0004] Water-decomposable nonwoven fabrics containing synthetic fibers have also been developed. For example, Patent Document 3 discloses a fiber composite material containing natural and / or synthetic fibers. Here, the use of regenerated cellulose fibers (viscose fibers) as synthetic fibers is considered. In Patent Document 3, a fleece structure is produced using round viscose fibers and flat viscose fibers. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-184984 [Patent Document 2] Japanese Patent Application Publication No. 184193 / 1983 [Patent Document 3] Special Publication No. 2008-546917 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, there has been a demand for water-disintegratable paper to have better water-disintegratability, and there are cases where a higher level of water-disintegratability is required than before.

[0007] Furthermore, in the case of pop-up wet tissue products in which the water-disintegrable paper is impregnated with water to make it moist, the water-disintegrable paper is required to have sufficient wet tensile strength in order to pull out the wet tissue that is partially sticking out from the opening.

[0008] Therefore, in order to solve such problems of the conventional techniques, the present inventors have carried out studies with the aim of providing a water-disintegrable nonwoven fabric having both excellent wet tensile strength and water-disintegrability. [Means for solving the problem]

[0009] As a result of intensive research to solve the above problems, the present inventors have found that a water-disintegrable nonwoven fabric which combines excellent wet tensile strength and water-disintegrability and which is suitable for a pop-up type wet tissue package can be obtained by using a combination of flat rayon fibers and round rayon fibers as the regenerated cellulose fibers in a water-disintegrable nonwoven fabric containing pulp fibers and regenerated cellulose fibers, setting the average fiber length of the regenerated cellulose fibers within a specified range, and entangling and integrating these fibers by high-pressure water jet stream treatment, and further setting the ratio of the tensile strength in the direction in which the streak-like jet marks formed by the high-pressure water jet stream treatment extend (the same as the papermaking direction of the papermaking machine) to the tensile strength in the direction perpendicular to the direction of the streak-like jet marks in a specific range in a wet water-disintegrable nonwoven fabric. Specifically, the present invention has the following configuration.

[0010] [1] A water-decomposable nonwoven fabric in which pulp fibers and regenerated cellulose fibers are intertwined, The regenerated cellulose fibers include flat rayon fibers and round rayon fibers, The average fiber length of the regenerated cellulose fibers is 2 mm or more and 20 mm or less, the surface of the water-decomposable nonwoven fabric has jet marks caused by high-pressure water jet treatment; The water-decomposable nonwoven fabric in a wet state after being impregnated with 2 parts by mass of pure water per part by mass of the bone-dry water-decomposable nonwoven fabric and left for 2 days has a The tensile strength in the direction in which the streaks caused by the high-pressure water jet treatment extend is defined as WT1N / m, When the tensile strength in the direction perpendicular to the direction in which the streaks caused by the high-pressure water jet treatment extend is WT2N / m, A water-decomposable nonwoven fabric satisfying 70≦WT1≦500 and 2.0≦WT1 / WT2≦6.0. [2] The water-decomposable nonwoven fabric according to [1], wherein the content of the flat rayon fibers relative to the total mass of the regenerated cellulose fibers is P (parts by mass), and the content of the round rayon fibers relative to the total mass of the regenerated cellulose fibers is Q (parts by mass), in which P:Q=1:9 to 9:1. [3] The water-decomposable nonwoven fabric according to [1] or [2], wherein the content of the pulp fibers is 30 to 90 mass% and the content of the regenerated cellulose fibers is 10 to 50 mass% based on the total mass of the water-decomposable nonwoven fabric. [4] The water-decomposable nonwoven fabric according to any one of [1] to [3], wherein the flat rayon fibers are hollow flat rayon fibers. [5] The water-decomposable nonwoven fabric according to any one of [1] to [4], wherein the ratio of the outer edge width to the outer edge length of the cross section of the flat rayon fibers is 1:2 to 1:30. [6] The water-decomposable nonwoven fabric according to any one of [1] to [5], wherein the pulp fibers have an average fiber length of 1.5 mm or more. [7] The water-decomposable nonwoven fabric according to any one of [1] to [6], wherein the pulp fibers contain coniferous pulp fibers, and the content of hardwood pulp fibers relative to the total mass of the pulp fibers is 50 mass% or less. [8] A wet water-disintegrable nonwoven fabric obtained by impregnating the water-disintegrable nonwoven fabric according to any one of [1] to [7] with water. [9] A wet water-disintegrable nonwoven fabric laminate comprising a plurality of sheets of the wet water-disintegrable nonwoven fabric according to [8].

[10] A wet water-disintegrable nonwoven fabric laminate according to [9], wherein each leaf of the wet water-disintegrable nonwoven fabric is folded so as to overlap with each other.

[11] A package containing the wet water-disintegrable nonwoven fabric laminate according to [8] or [9], the package having an opening at an upper portion of the wet water-disintegrable nonwoven fabric laminate for removing the wet water-disintegrable nonwoven fabric, A package in which 1 part by mass of the water-disintegrable nonwoven fabric in an absolutely dry state is impregnated with 2 parts by mass of pure water and left for 2 days, and in the wet water-disintegrable nonwoven fabric, the direction in which streaks that are jet marks caused by high-pressure water jet treatment extend corresponds to the direction in which the wet water-disintegrable nonwoven fabric is taken out.

[12] A method for producing a water-decomposable nonwoven fabric, comprising the steps of forming a nonwoven fabric sheet containing pulp fibers and regenerated cellulose fibers using a wet papermaking machine, and then subjecting the nonwoven fabric sheet to a high-pressure water jet treatment, The regenerated cellulose fibers include flat rayon fibers and round rayon fibers, The average fiber length of the regenerated cellulose fibers is 2 mm or more and 20 mm or less, The water-decomposable nonwoven fabric in a wet state after being impregnated with 2 parts by mass of pure water per part by mass of the bone-dry water-decomposable nonwoven fabric and left for 2 days has a The tensile strength in the direction in which the streaks caused by the high-pressure water jet treatment extend is defined as WT1N / m, When the tensile strength in the direction perpendicular to the direction in which the streaks caused by the high-pressure water jet treatment extend is WT2N / m, A method for producing a water-decomposable nonwoven fabric, comprising adjusting a jet wire ratio so as to satisfy the conditions 70≦WT1≦500 and 2.0≦WT1 / WT2≦6.0. Effect of the Invention

[0011] According to the present invention, it is possible to obtain a water-disintegrable nonwoven fabric having both excellent wet tensile strength and water-disintegrability. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic diagram of a water-decomposable nonwoven fabric according to an embodiment of the present invention when viewed in plan, in which the vertical dotted lines represent stripes that are jet marks caused by high-pressure water jet treatment. [Diagram 2] FIG. 2 is a schematic diagram showing a state in which each leaf of a wet water-disintegrable nonwoven fabric is folded with overlapping portions in a wet water-disintegrable nonwoven fabric laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "~" means a range including the numerical values ​​before and after "~" as the lower and upper limits.

[0014] (Water-degradable nonwoven fabric) The present invention relates to a water-decomposable nonwoven fabric in which pulp fibers and regenerated cellulose fibers are entangled. The regenerated cellulose fibers include flat rayon fibers and round rayon fibers. The regenerated cellulose fibers have an average fiber length of 2 mm or more and 20 mm or less.

[0015] The water-disintegrable nonwoven fabric of the present invention has the above-mentioned constitution, and therefore has both excellent wet tensile strength and water disintegrability. Conventionally, in water-disintegrable nonwoven fabrics, wet tensile strength and water disintegrability are mutually contradictory properties, and it has been difficult to achieve both at a high level. However, the present inventors have succeeded in achieving both wet tensile strength and water disintegrability by using flat rayon fibers and round rayon fibers as regenerated cellulose fibers and setting the average fiber length of the regenerated cellulose fibers within a predetermined range.

[0016] The wet tensile strength of the water-disintegrable nonwoven fabric was measured by impregnating 1 part by mass of the water-disintegrable nonwoven fabric in an absolutely dry state with 2 parts by mass of pure water, leaving the fabric for 2 days, and then measuring the tensile strength of the wet water-disintegrable nonwoven fabric using a tensile tester. The wet water-decomposable nonwoven fabric is prepared by folding a sample having a width of 50 mm and a span length of 114 mm in half widthwise (so that the width becomes 25 mm) to prepare a measurement piece. For the water-decomposable nonwoven fabric in a wet state, the tensile strength in the direction in which the streaks resulting from the high-pressure water jet treatment extend and the tensile strength in the direction perpendicular to the direction in which the streaks resulting from the high-pressure water jet treatment extend are each measured at a pulling speed of 300 mm / min. As a tensile tester used for measuring the wet tensile strength, for example, a TENSILON universal material testing machine manufactured by A&D Co., Ltd. can be used.

[0017] The wet tensile strength of the water-decomposable nonwoven fabric of the present invention is, when the tensile strength in the direction in which the streaks resulting from the high-pressure water jet treatment extend is defined as WT1N / m, and the tensile strength in the direction perpendicular to the direction in which the streaks resulting from the high-pressure water jet treatment extend is defined as WT2N / m, The conditions 70≦WT1≦500 and 2.0≦WT1 / WT2≦6.0 are satisfied. With regard to WT1, it is more preferable that 80≦WT1≦500, and further preferably 90≦WT3≦500. With regard to WT1 / WT2, it is more preferable that 2.0≦WT1 / WT2≦4.0.

[0018] The water-disintegrable nonwoven fabric of the present invention has excellent wet tensile strength. Therefore, when the water-disintegrable nonwoven fabric is impregnated with water or a chemical solution to form a wet water-disintegrable nonwoven fabric, it can exhibit sufficient strength to withstand cleaning work, etc. Therefore, the wet water-disintegrable nonwoven fabric does not break unintentionally during cleaning work, and the fibers of the wet water-disintegrable nonwoven fabric do not come off during use.

[0019] In addition, since the water-disintegrable nonwoven fabric of the present invention has excellent water disintegrability, it is easily disintegrated by a water flow or a large amount of water, and the disintegrated state is maintained. Therefore, when the water-disintegrable nonwoven fabric of the present invention is flushed down a flush toilet, it will not clog the drain of the flush toilet. In recent years, the demand for water-saving flush toilets has been increasing, but the water-disintegrable nonwoven fabric of the present invention is easily disintegrated even in water-saving flush toilets, so it can be flushed down any flush toilet. Here, the water disintegrability of the water-disintegrable nonwoven fabric is measured in accordance with "4.5 Ease of disintegration" of JIS P 4501:1993, after impregnating the water-disintegrable nonwoven fabric with pure water so that the mass ratio of the bone-dry water-disintegrable nonwoven fabric to pure water is 1:2 (nonwoven fabric:pure water) to obtain a wet water-disintegrable nonwoven fabric, which is then left in a sealed state at room temperature for 2 days.

[0020] In this specification, a water-disintegrable nonwoven fabric in an absolutely dry state is a nonwoven fabric having a moisture content of 1% by mass or less relative to the total mass of the water-disintegrable nonwoven fabric. The water-disintegrability of the water-disintegrable nonwoven fabric is preferably 100 seconds or less, more preferably 80 seconds or less, even more preferably 70 seconds or less, even more preferably 67 seconds or less, and particularly preferably 65 seconds or less. The lower limit of the water-disintegrability of the water-disintegrable nonwoven fabric is not particularly limited, but is preferably 15 seconds or more.

[0021] In addition, the water-disintegrability of the water-disintegrable nonwoven fabric is preferably 95% or more, and more preferably 99% or more, when the water-disintegrable nonwoven fabric is impregnated with pure water so that the mass ratio of the bone-dry water-disintegrable nonwoven fabric to the water is 1:2 (nonwoven fabric:water) to obtain a wet water-disintegrable nonwoven fabric, which is then left in a sealed state at room temperature for 2 days and then measured in accordance with the water-disintegrability test set by the International Water Services Flushability Group (IWSFG).

[0022] The chemical solution to be impregnated into the water-decomposable nonwoven fabric may be one containing water as the main component and various cosmetic materials (water-soluble solvents, antibacterial agents, antifungal agents, fragrances, surfactants, preservatives, humectants, drugs with desired medicinal effects, etc.) at a ratio of about 10% by mass or less of the total. For example, the chemical solution may be one having a mass ratio of dipropylene glycol: polyaminopropyl biguanide: disodium phosphate: benzoic acid: cetylpyridinium chloride: water of 1.00:0.20:0.15:0.15:0.05:98.45.

[0023] The water-decomposable nonwoven fabric contains pulp fibers and regenerated cellulose fibers. In the water-decomposable nonwoven fabric, the pulp fibers and the regenerated cellulose fibers are entangled, and thus the pulp fibers and the regenerated cellulose fibers are integrated together. Such a structure is formed by subjecting a nonwoven fabric sheet containing pulp fibers and regenerated cellulose fibers, which is formed by a wet papermaking method, to a high-pressure water jet stream treatment. By subjecting the pulp fibers and the regenerated cellulose fibers to a twisted, bent, and turned state, the fibers are entangled and integrated together. In other words, the water-decomposable nonwoven fabric can be said to be a nonwoven fabric in which the pulp fibers and the regenerated cellulose fibers are entangled and integrated together by the high-pressure water jet stream treatment.

[0024] In the water-disintegrable nonwoven fabric, the state in which the pulp fibers and the regenerated cellulose fibers are entangled and integrated can be seen by observing the surface of the nonwoven fabric under magnification, from the state in which each fiber is randomly oriented and entangled. In addition, since the water-disintegrable nonwoven fabric of the present invention is a nonwoven fabric in which the pulp fibers and the regenerated cellulose fibers are entangled and integrated by high-pressure water jet processing, the water-disintegrable nonwoven fabric has continuous streaky jet marks in the flow direction (MD) of the nonwoven fabric. That is, in the present invention, the presence of such jet marks can also be used to determine that the pulp fibers and the regenerated cellulose fibers are entangled. The jet marks are fine marks where the high-pressure water jet stream is applied, and the density of the fibers that make up the water-disintegrable nonwoven fabric is higher in the jet marks than in the areas where the high-pressure water jet stream is not applied.

[0025] The basis weight of the water-decomposable nonwoven fabric of the present invention is 15 g / m 2 It is preferable that the thickness is 20 g / m or more. 2 More preferably, it is 30 g / m or more. 2 The basis weight of the water-decomposable nonwoven fabric is preferably 100 g / m or more. 2 It is preferable that the thickness is less than 80 g / m 2 More preferably, it is 60 g / m or less. 2 It is more preferable that the basis weight of the water-disintegrable nonwoven fabric is within the above range, so that the impregnated tensile strength and water disintegrability can be more effectively improved. In this specification, the basis weight of the water-disintegrable nonwoven fabric is measured in accordance with JIS P 8124.

[0026] The thickness of the water-disintegrable nonwoven fabric of the present invention is preferably 100 μm or more, more preferably 150 μm or more, and is preferably 400 μm or less, more preferably 350 μm or less.

[0027] In this specification, the water-disintegrable nonwoven fabric is a nonwoven fabric in a dry state (absolutely dry state) that can be impregnated with moisture or medicine. The present invention also relates to a wet water-disintegrable nonwoven fabric obtained by impregnating a water-disintegrable nonwoven fabric with moisture or medicine. In addition to moisture, the wet water-disintegrable nonwoven fabric may further contain a wetting agent such as propylene glycol, alcohol or parabenzoic acid esters such as antibacterial agents, antifungal agents, fragrances, medicines having desired medicinal effects, and the like. The wet water-disintegrable nonwoven fabric is preferably used as a wet product such as wet tissues, baby wipes, wipers, and the like.

[0028] The wet thickness of the water-disintegrable nonwoven fabric of the present invention (thickness of wet water-disintegrable nonwoven fabric) is preferably 100 μm or more, more preferably 150 μm or more, even more preferably 200 μm or more, even more preferably 250 μm or more, and particularly preferably 270 μm or more. The wet thickness of the water-disintegrable nonwoven fabric (thickness of wet water-disintegrable nonwoven fabric) is preferably 1000 μm or less, more preferably 800 μm or less, and even more preferably 600 μm or less. By making the wet thickness of the water-disintegrable nonwoven fabric within the above range, the feeling of use when using the wet water-disintegrable nonwoven fabric can be further improved. Specifically, the touch can be improved and the softness can be improved. The cleaning effect of the wet water-disintegrable nonwoven fabric can also be improved.

[0029] <Pulp fiber> The water-decomposable nonwoven fabric of the present invention contains pulp fibers. Examples of pulp fibers include fibers made of wood pulp, non-wood pulp, and deinked pulp. Examples of wood pulp include hardwood pulp (hardwood kraft pulp (LBKP)), softwood pulp (softwood kraft pulp (NBKP)), sulfite pulp (SP), dissolving pulp (DP), soda pulp (AP), unbleached kraft pulp (UKP), oxygen bleached kraft pulp (OKP), and other chemical pulps. Semi-chemical pulp (SCP), chemical ground wood pulp (CGP), and other semi-chemical pulp, ground wood pulp (GP), and mechanical pulp such as thermomechanical pulp (TMP, BCTMP) can also be used. Examples of non-wood pulp include cotton pulp such as cotton linters and cotton lint, non-wood pulp such as hemp, straw, and bagasse, and cellulose, chitin, and chitosan isolated from sea squirts and seaweed. Examples of deinked pulp include deinked pulp made from waste paper. The above pulps may be used alone or in combination of two or more.

[0030] Among them, as the pulp fiber, it is preferable to use at least one selected from hardwood pulp (hardwood kraft pulp (LBKP)) and softwood pulp (softwood kraft pulp (NBKP)), and it is particularly preferable to use softwood pulp (softwood kraft pulp (NBKP)). By using softwood pulp (softwood kraft pulp (NBKP)), it becomes easier to suppress the falling off of pulp fibers when producing a water-decomposable nonwoven fabric, and production efficiency can be improved. In addition, by using softwood pulp (softwood kraft pulp (NBKP)) as the pulp fiber, it is possible to increase the thickness of the water-decomposable nonwoven fabric when wet, and to improve the feeling of use and cleaning effect when using the wet water-decomposable nonwoven fabric.

[0031] In the present invention, softwood pulp and hardwood pulp may be used in combination as the pulp fibers, in which case the content of hardwood pulp fibers relative to the total mass of the pulp fibers is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less. Note that the pulp fibers do not need to contain hardwood pulp, and the content of hardwood pulp fibers relative to the total mass of the pulp fibers may be 0% by mass.

[0032] The average fiber length of the pulp fibers is preferably 1.5 mm or more, more preferably 1.8 mm or more, and even more preferably 2.0 mm or more. The average fiber length of the pulp fibers is preferably 20.0 mm or less, more preferably 10.0 mm or less, and even more preferably 7.0 mm or less. Here, in this specification, the average fiber length of the pulp fibers means the length-weighted average fiber length. The length-weighted average fiber length of the pulp fibers is the fiber length calculated by the following measurement method. First, a water-decomposable nonwoven fabric is disintegrated in water to prepare a fiber dispersion slurry. This is filtered through a nylon mesh screen and separated into a residue (rayon) and a filtrate (pulp dispersion liquid). The pulp dispersion liquid is treated with a disintegrator at 4500 rpm and sufficiently disintegrated to obtain a fiber dispersion slurry. The obtained fiber dispersion slurry is diluted to 0.01 mass% or more and 0.02 mass% or less to prepare a dilution liquid. The projected length of the fiber components contained in 10 ml of this dilution solution is measured using a fiber length measuring device (Kajaani Fiber Lab Ver. 4.0, manufactured by Metso Automation), and the length-weighted average value of the disintegrated fibers is calculated.

[0033] The upper and lower limits of the freeness of the pulp fiber are not particularly limited, but are preferably 350 ml or more, more preferably 400 ml or more, and even more preferably 450 ml or more. It is also preferable that the freeness is about 700 ml.

[0034] Freeness is a value indicated by Canadian Standard Freeness (CSF) specified in JIS P 8121, and indicates the degree of beating of fibers. Beating of fibers can be performed on a paper stock (slurry) in which fibers are dispersed, using a known beating machine such as a beader or a disk refiner. Usually, the smaller the freeness value of the fibers, the stronger the degree of beating, and the greater the damage to the fibers caused by beating, leading to the progress of fibrillation. As the fibrillation of fibers progresses, the number of bonding points between fibers increases, improving the strength, but decreasing the water disintegratability. In the present invention, it is also preferable to appropriately adjust the freeness in order to set the wet strength and water disintegratability in the preferred ranges.

[0035] The content of pulp fibers relative to the total mass of the water-decomposable nonwoven fabric is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more. The content of pulp fibers relative to the total mass of the water-decomposable nonwoven fabric is preferably 90% by mass or less, and more preferably 80% by mass or less. By setting the content of pulp fibers within the above range, the impregnation tensile strength and water disintegratability of the water-decomposable nonwoven fabric can be more effectively increased.

[0036] <Regenerated cellulose fiber> The water-decomposable nonwoven fabric of the present invention contains regenerated cellulose fibers. The average fiber length of the regenerated cellulose fibers may be 2 mm or more, preferably 3 mm or more, and more preferably 5 mm or more. The average fiber length of the regenerated cellulose fibers may be 20 mm or less, preferably 15 mm or less, and more preferably 10 mm or less. The average fiber length is the average fiber length of the flat rayon fibers and the round rayon fibers combined. The average fiber length of the regenerated cellulose fibers is based on the measurement method of average fiber length JIS L-1015 8.4.1. By setting the fiber length of the regenerated cellulose fibers within the above range, both wet strength and water decomposability can be achieved. In particular, by setting the fiber length of the regenerated cellulose fibers to the above upper limit value or less, a water-decomposable nonwoven fabric that can maintain a bulky state even in a wet state can be easily obtained, and by setting the fiber length to the above lower limit value or more, a water-decomposable nonwoven fabric with high wet strength can be easily obtained.

[0037] The regenerated cellulose fiber contains flat rayon fiber and round rayon fiber. When the content of the flat rayon fiber relative to the total mass of the regenerated cellulose fiber is P (parts by mass), and the content of the round rayon fiber relative to the total mass of the regenerated cellulose fiber is Q (parts by mass), the ratio P:Q is preferably 1:9 to 9:1, more preferably 3:7 to 9:1, and even more preferably 3:7 to 8:2.

[0038] The flat rayon fiber has a flat cross-sectional shape. The cross-sectional shape of the fiber refers to the shape of a cut surface perpendicular to the length direction of the rayon fiber. In this specification, the flat shape refers to a shape in which the cross-sectional shape of the fiber has a major axis defined by the maximum length passing through the center point and a minor axis defined by the minimum length passing through the center point, and refers to a shape in which the ratio of the outer edge length to the outer edge width of the cross-section of the flat rayon fiber (outer edge length / outer edge width) is 2 or more. The ratio of the outer edge width to the outer edge length of the cross-section of the flat rayon fiber is preferably 1:2 to 1:30, and more preferably 1:2 to 1:20. Here, the ratio of the outer edge width to the outer edge length of the cross-section of the flat rayon fiber can be measured by observing the flat cross-sections of 10 different flat rayon fibers with a microscope from the vertical direction and using a microscale as a reference. The flat shape can be, for example, a cocoon shape, an oval shape, an ellipse shape, etc.

[0039] As the flat rayon fiber, a solid flat rayon fiber or a hollow flat rayon fiber can be used. Among them, the flat rayon fiber is preferably a hollow flat rayon fiber. As the hollow flat rayon fiber, a commercially available product can be used, for example, SBH manufactured by Daiwabo Rayon Co., Ltd.

[0040] The fineness of the flat rayon fiber is preferably 1.2 dtex or more and 7.0 dtex or less, more preferably 1.2 dtex or more and 5.0 dtex or less, and even more preferably 1.2 dtex or more and 2.0 dtex or less. By making the fineness of the flat rayon fiber within the above range, re-aggregation of the fiber components after hydrolysis can be suppressed, and thus the hydrolysis property can be more effectively improved.

[0041] Round rayon fibers have a round cross-sectional shape. Here, round refers to a cross-sectional shape of a fiber that does not substantially have a major axis and a minor axis, and the ratio of the peripheral length to the peripheral width of the cross-section of the rayon fiber (peripheral length / peripheral width) is less than 2. That is, round rayon fibers include fibers having an elliptical cross-section in which the ratio of the peripheral length to the peripheral width of the cross-section of the rayon fiber is small. In addition, fibers having a chrysanthemum-shaped or polygonal cross-section are also included in round rayon fibers. In the present invention, it is preferable to use chrysanthemum-shaped rayon fibers as the round rayon fibers. As the chrysanthemum-shaped rayon fibers, commercially available products can be used, for example, Corona SB manufactured by Daiwabo Rayon Co., Ltd.

[0042] The content of regenerated cellulose fibers relative to the total mass of the water-decomposable nonwoven fabric is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more. The content of regenerated cellulose fibers relative to the total mass of the water-decomposable nonwoven fabric is preferably 50% by mass or less, and more preferably 45% by mass or less. By setting the content of regenerated cellulose fibers within the above range, the wet strength and water disintegrability of the water-decomposable nonwoven fabric can be more effectively improved.

[0043] The regenerated cellulose fibers may include, in addition to the flat rayon fibers and round rayon fibers described above, for example, cupra fibers and lyocell fibers.

[0044] <Optional ingredients> The water-decomposable nonwoven fabric of the present invention may contain other optional components. Examples of optional components include dry strength agents, wet strength agents, and softeners. Examples of dry strength agents include cationic starch, polyacrylamide (PAM), and carboxymethyl cellulose (CMC). Examples of wet strength agents include polyamide epichlorohydrin, urea, melamine, and thermally crosslinked polyacrylamide. Examples of softeners include anionic surfactants, nonionic surfactants, and cationic surfactants. The above optional components may be used alone or in combination of two or more.

[0045] However, the content of the heat-meltable resin in the water-disintegrable nonwoven fabric of the present invention is preferably 5% by mass or less, more preferably 1% by mass or less, based on the total mass of the water-disintegrable nonwoven fabric. It is preferable that the water-disintegrable nonwoven fabric of the present invention does not substantially contain a heat-meltable resin, and it is particularly preferable that the content of the resin component is 0% by mass. In this specification, the heat-meltable resin is, for example, at least one selected from polyethylene, polypropylene, polyamide, thermoplastic polyester, and ethylene-vinyl acetate copolymer.

[0046] The water-disintegrable nonwoven fabric of the present invention exhibits excellent performance particularly in a package (so-called wet tissue package) containing a wet water-disintegrable nonwoven fabric laminate in which a plurality of wet water-disintegrable nonwoven fabrics are laminated. In order to prevent evaporation of moisture from the wet tissues, it is preferable that the opening area of ​​the wet tissue package is as small as possible.

[0047] When attempting to remove a water-disintegrable nonwoven fabric from a small opening, the water-disintegrable nonwoven fabric is easily torn, and therefore it is necessary to increase the wet tensile strength, but simply increasing the wet tensile strength alone makes it difficult to achieve compatibility with water disintegrability. In the package of the present invention, the surface of the water-disintegrable nonwoven fabric in a wet state has jet marks caused by the high-pressure water jet treatment, and the direction in which the streaks of the jet marks caused by the high-pressure water jet treatment extend, i.e., the direction in which the tensile strength is maximized, coincides with the direction in which the wet water-disintegrable nonwoven fabric is taken out, thereby preventing the water-disintegrable nonwoven fabric from tearing when it is taken out.

[0048] The wet water-disintegrable nonwoven fabric laminate is preferably formed by folding each leaf so that each leaf overlaps the other. By forming the laminate in this manner, when one leaf is taken out, the next leaf partially protrudes from the opening of the package, which eliminates the need to insert fingers into the package to pick out the wet water-disintegrable nonwoven fabric.

[0049] (Production method of water-disintegrable nonwoven fabric) The method for producing a water-decomposable nonwoven fabric of the present invention includes a step of subjecting a nonwoven fabric sheet containing pulp fibers and regenerated cellulose fibers formed by a wet papermaking method to a high-pressure water jet treatment. Here, the regenerated cellulose fibers include flat rayon fibers and round rayon fibers. The average fiber length of the regenerated cellulose fibers is preferably 2 mm or more and 20 mm or less.

[0050] In the production of the water-decomposable nonwoven fabric of the present invention, the wet tensile strength is adjusted to satisfy 70≦WT1≦500 and 2.0≦WT1 / WT2≦6.0, where WT1 N / m is the strength of pulling in the direction in which streaks resulting from the high-pressure water jet treatment extend (corresponding to the machine direction (papermaking direction) of the papermaking machine) and WT2 N / m is the strength of pulling in the direction perpendicular to the direction in which streaks resulting from the high-pressure water jet treatment extend. With regard to WT1, it is more preferable that 80≦WT1≦500, and further preferably 90≦WT1≦500. With regard to WT1 / WT2, it is more preferable that 2.0≦WT1 / WT2≦4.0. The WT1 / WT2 can be adjusted by adjusting the ratio of the raw material discharge speed to the wire speed (jet wire ratio) during papermaking.

[0051] In the manufacturing process of water-decomposable nonwoven fabric, first, a slurry containing pulp fibers and regenerated cellulose fibers is obtained. The slurry is then wet-laid using a known papermaking machine such as a cylinder papermaking machine, a short wire papermaking machine, an inclined wire papermaking machine, or a fourdrinier papermaking machine to form a nonwoven sheet (wet web). The fiber orientation of the nonwoven sheet (wet web) can be controlled by adding a viscous agent such as polyethylene oxide to the slurry, adjusting the line speed of the papermaking machine, or adjusting the ratio of the raw material discharge speed to the wire speed (jet wire ratio) in the wire part of the papermaking process.

[0052] In the step of subjecting the nonwoven fabric sheet to a high-pressure water jet stream treatment, the obtained nonwoven fabric sheet (wet web) is subjected to a high-pressure water jet stream treatment. The high-pressure water jet stream treatment can be carried out by a known method. Specifically, the nonwoven fabric sheet (wet web) is placed on a porous support, and water is jetted from the upper surface of the nonwoven fabric sheet (wet web) at a water pressure of 15 to 150 kg / cm through a nozzle having a large number of pores with a pore diameter of about 0.08 to 0.30 mm. 2 The high-pressure water is sprayed at a water pressure of 0.01 kWh / kg / m or more, and the fibers constituting the nonwoven fabric sheet (wet web) are entangled with each other. The energy imparted to the nonwoven fabric sheet (wet web) by the high-pressure water jet stream treatment is expressed by the high-pressure water jet stream energy of the following (Equation 3). The high-pressure water jet stream energy is preferably 0.005 kWh / kg / m or more, more preferably 0.010 kWh / kg / m or more, and even more preferably 0.015 kWh / kg / m or more. The high-pressure water jet stream energy is preferably 0.50 kWh / kg / m or less, more preferably 0.40 kWh / kg / m or less, and even more preferably 0.30 kWh / kg / m or less. By setting the high-pressure water jet stream energy within the above range, it is possible to increase the wet strength of the water-disintegratable nonwoven fabric while improving its water disintegratability. V=(2×g×(P-Ap)×10000 / (ρ×1000)) 1 / 2 ×60...(Formula 1) V: Flow velocity of water discharged from the nozzle (m / min) g:Gravity acceleration=9.8m / s 2 P: Water pressure at the nozzle (kgf / cm 2 ) A: Area of ​​one nozzle hole (mm 2 ) p: Atmospheric pressure (kgf / cm 2 ) ρ: density of water (g / cm 3 ) F=(A / 100)×V×100...(Formula 2) F: Flow rate of water discharged from one nozzle hole (cm 3 / min) A: Area of ​​one nozzle hole (mm 2 ) V: Flow velocity of water discharged from the nozzle (m / min) E=P×(F / 100)×0.163 (Formula 3) E: High pressure water jet energy (kWh / kg / m)

[0053] When high-pressure water is sprayed onto the water-disintegrable nonwoven fabric through the nozzle, streaky jet marks are formed on the surface of the water-disintegrable nonwoven fabric.

[0054] The high-pressure water jet treatment may be carried out online immediately after the formation of a web by wet papermaking, or the wet papermaking web may be dried and then subjected to the high-pressure water jet treatment online or offline.

[0055] The nonwoven fabric sheet that has been subjected to the high-pressure water jet treatment is then pressed and dried in the subsequent steps.

[0056] (Application) The water-decomposable nonwoven fabric of the present invention is impregnated with a wetting agent such as water or propylene glycol, or with an antibacterial agent, antifungal agent, fragrance, or drug having a desired medicinal effect such as alcohol or parabenzoic acid esters, and is used as a wet product such as wet tissue, baby wipes, or wipes. The water-decomposable nonwoven fabric of the present invention may also be used as a surface material for sanitary materials. In this case, the nonwoven fabric may be subjected to a treatment to increase hydrophilicity or water repellency as desired. EXAMPLES

[0057] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0058] Example 1 The fiber raw materials were mixed so that the total weight of the fibers was 19% by mass of hollow flat rayon fiber (trade name: Corona SBH, manufactured by Daiwabo Rayon Co., Ltd., ratio of outer edge width to outer edge length (flatness), 1:15) with a fineness of 1.7 dtex and an average fiber length of 7 mm, 6% by mass of chrysanthemum-shaped rayon fiber (trade name: Corona SB, manufactured by Daiwabo Rayon Co., Ltd.) with a fineness of 1.1 dtex and an average fiber length of 5 mm, and 75% by mass of unbeaten softwood kraft pulp (NBKP, freeness measured in accordance with JIS P 8121-2:2012 is 673 ml, average fiber length: 2.33 mm), and the fiber raw materials were dispersed in water to obtain a pulp slurry with a solid content concentration of 1.0% by mass. A nonwoven sheet was produced from the pulp slurry using an inclined wire-type fourdrinier papermaking machine at a jet wire ratio of 0.80 and a paper speed of 133 m / min. Next, a high-pressure water jet was sprayed onto the nonwoven fabric sheet using a water jet device (high-pressure water jet processing device) installed at the rear of the wire so that the load energy was 0.012 kWh / kg / m. The nonwoven fabric sheet that had been subjected to the high-pressure water jet processing was dried, and the basis weight after drying was 43.0 g / m. 2 A water-decomposable nonwoven fabric was obtained.

[0059] Example 2 A water-decomposable nonwoven fabric of Example 2 was obtained in the same manner as in Example 1, except that the fiber raw materials were mixed so as to obtain 16 mass% of hollow flat rayon fiber (product name: Corona SBH, manufactured by Daiwabo Rayon Co., Ltd.) having a fineness of 1.7 dtex and an average fiber length of 7 mm, 6 mass% of chrysanthemum-shaped rayon fiber (product name: Corona SB, manufactured by Daiwabo Rayon Co., Ltd.) having a fineness of 1.1 dtex and an average fiber length of 5 mm, and 78 mass% of unbeaten softwood kraft pulp (NBKP, freeness measured in accordance with JIS P 8121-2:2012 is 673 ml).

[0060] Example 3 In Example 1, the machine speed was 100 m / min, and the basis weight after drying was 60.0 g / m 2 A water-decomposable nonwoven fabric of Example 3 was obtained in the same manner as in Example 1, except that:

[0061] Example 4 A water-decomposable nonwoven fabric of Example 4 was obtained in the same manner as in Example 1, except that the fiber raw materials were mixed so as to obtain 16 mass% of hollow flat rayon fiber (product name: Corona SBH, manufactured by Daiwabo Rayon Co., Ltd.) having a fineness of 1.7 dtex and an average fiber length of 7 mm, 3 mass% of chrysanthemum-shaped rayon fiber (product name: Corona SB, manufactured by Daiwabo Rayon Co., Ltd.) having a fineness of 1.1 dtex and an average fiber length of 10 mm, and 81 mass% of unbeaten softwood kraft pulp (NBKP, freeness measured in accordance with JIS P 8121-2:2012 is 673 ml).

[0062] Comparative Example 1 A water-decomposable nonwoven fabric of Comparative Example 1 was obtained in the same manner as in Example 2, except that the jet wire ratio of the inclined wire type Fourdrinier papermaking machine was changed to 1.04.

[0063] Comparative Example 2 A water-decomposable nonwoven fabric of Comparative Example 2 was obtained in the same manner as in Example 2, except that the load energy of the water jet device (high-pressure water jet treatment device) was set to 0.006 kWh / kg / m.

[0064] (evaluation) (Water degradable 1) The water-disintegrable nonwoven fabrics obtained in the examples and comparative examples were dried, and then impregnated with pure water so that the mass ratio of the water-disintegrable nonwoven fabric in the dried state to the pure water was 1:2 (nonwoven fabric:pure water). The wet water-disintegrable nonwoven fabric (wet water-disintegrable nonwoven fabric) was sealed and left for 2 days. Thereafter, the water-disintegrability of the wet water-disintegrable nonwoven fabric was measured in accordance with "4.5 Ease of disintegration" of JIS P 4501:1993. If the "ease of disintegration" was within 100 seconds, the water-disintegrability was considered to be good.

[0065] (water decomposability 2) The water-decomposable nonwoven fabrics obtained in the Examples and Comparative Examples were cut into a plurality of pieces each having a size of 110 mm×200 mm, and the mass after drying (initial dry mass) was measured. The water-disintegrable nonwoven fabric was then impregnated with pure water so that the mass ratio of the dried water-disintegrable nonwoven fabric to pure water was 1:2 (nonwoven fabric:pure water), sealed, and left for 2 days to produce a wet water-disintegrable nonwoven fabric (wet water-disintegrable nonwoven fabric). The water disintegrability of the wet water disintegratable nonwoven fabric was measured in accordance with "IWSFG PAS 3:2018 Water disintegratability test method using a slosh box" described in the public specification "PAS 1:2018 Certification standard for products that can be flushed down the toilet" published by IWSFG. Specifically, the wet water-disintegrable nonwoven fabric was hydrolyzed in a slosh box for 30 minutes, and then the test pieces and water in the water tank were poured into a sieve with a mesh size of 25 mm, and the sieve was rinsed with a shower for 1 minute, after which the test pieces remaining on the sieve were collected.The sieve passing rate was calculated by (initial dry mass - dry mass of test pieces remaining on the sieve) / initial dry mass x 100. If the passing rate is 95% by mass or more, the water decomposability is said to be good.

[0066] (Wet tensile strength) The water-disintegrable nonwoven fabrics obtained in the Examples and Comparative Examples were impregnated with pure water so that the mass ratio of bone-dry water-disintegrable nonwoven fabric to pure water was 1:2 (nonwoven fabric:pure water), sealed, and left for 2 days to prepare wet water-disintegrable nonwoven fabrics (wet water-disintegrable nonwoven fabrics). A sample having a width of 50 mm and a span length of 114 mm was cut out from the wet water-decomposable nonwoven fabric, and folded in half widthwise (so the width was 25 mm). The tensile strength was measured at a tensile speed of 300 mm / min using a TENSILON universal material testing machine manufactured by A&D Corporation. The tensile strength (WT1) of the wet water-decomposable nonwoven fabric in the direction in which the streaks formed by the high-pressure water jet treatment extend, and the tensile strength (WT2) in the direction perpendicular to the direction in which the streaks formed by the high-pressure water jet treatment extend were measured, and WT1 / WT2 was calculated.

[0067] (Wet tissue pop-up suitability evaluation) The water-disintegrable nonwoven fabrics obtained in the Examples and Comparative Examples were impregnated with the drug solution (dipropylene glycol: polyaminopropyl biguanide: disodium phosphate: benzoic acid: cetylpyridinium chloride: water, the mass ratio of which was 1.00:0.20:0.15:0.15:0.05:98.45) in a bone-dry state so that the mass ratio of the water-disintegrable nonwoven fabric to the drug solution was 1:2 (nonwoven fabric: drug solution), and the fabric was left for 2 days in this state. Then, as shown in FIG. 1, 30 pieces were cut into pieces having a size of 200 mm parallel to the direction of the streaks resulting from the high-pressure water jet treatment and 180 mm in the direction perpendicular to the direction of the streaks resulting from the high-pressure water jet treatment, and mountain and valley folds were performed.

[0068] Next, the folded samples were stacked so that each water-decomposable nonwoven fabric was sandwiched between the other samples as shown in Figure 2 to produce a bundle of 30 wet tissues. In addition, a stack of wet tissues was wrapped in plastic film, a rounded rectangular shape (27 mm x 59 mm) was opened at the top, and 30 wet tissues were removed from the opening. The pop-up property was visually evaluated according to the following criteria. In addition, the occurrence of tearing of the wet tissue when the wet tissue was taken out from the opening was visually evaluated. 〇: When you take out one sheet, the next sheet comes out partway from the outlet. ×: When you remove one sheet, the next sheet does not come out.

[0069] [Table 1]

[0070] The water-disintegrable nonwoven fabrics of Examples 1 to 4 were excellent in water disintegrability, and when used in wet tissue packages, they did not tear when taken out, and were therefore excellent in pop-up suitability.

Claims

1. A water-decomposable nonwoven fabric in which softwood pulp fibers and regenerated cellulose fibers are intertwined, The regenerated cellulose fibers include hollow flat rayon fibers and chrysanthemum-shaped rayon fibers, The average fiber length of the regenerated cellulose fibers is 2 mm or more and 20 mm or less, The content of the softwood pulp fibers is 50 to 90% by mass based on the total mass of the water-decomposable nonwoven fabric, the surface of the water-decomposable nonwoven fabric has jet marks caused by high-pressure water jet treatment; The water-decomposable nonwoven fabric in a wet state after being impregnated with 2 parts by mass of pure water per part by mass of the bone-dry water-decomposable nonwoven fabric and left for 2 days has a The tensile strength in the direction in which the streaks caused by the high-pressure water jet treatment extend is WT 1 N / m, The tensile strength in the direction perpendicular to the direction in which the streaks caused by the high-pressure water jet treatment extend is WT. 2 When expressed as N / m, 80≦WT 1 ≦190, and 2.0≦WT 1 / W.T. 2 A water-decomposable nonwoven fabric satisfying a moisture content of ≦4.

0.

2. 2. The water-decomposable nonwoven fabric according to claim 1, wherein the content of the hollow flat rayon fibers relative to the total mass of the regenerated cellulose fibers is P (parts by mass), and the content of the chrysanthemum-shaped rayon fibers relative to the total mass of the regenerated cellulose fibers is Q (parts by mass), in which P:Q is 7:3 to 9:

1.

3. 3. The water-decomposable nonwoven fabric according to claim 1, wherein the content of the regenerated cellulose fibers is 10 to 50% by mass.

4. The water-decomposable nonwoven fabric according to any one of claims 1 to 3, wherein the ratio of the outer edge width to the outer edge length of the cross section of the flat rayon fibers is 1:2 to 1:

30.

5. The water-decomposable nonwoven fabric according to any one of claims 1 to 4, wherein the pulp fibers have an average fiber length of 1.5 mm or more.

6. The water-decomposable nonwoven fabric according to any one of claims 1 to 5, wherein the pulp fibers contain softwood pulp fibers, and a content of hardwood pulp fibers relative to a total mass of the pulp fibers is 50 mass% or less.

7. A wet water-disintegrable nonwoven fabric obtained by impregnating the water-disintegrable nonwoven fabric according to any one of claims 1 to 6 with water.

8. A wet water-disintegrable nonwoven fabric laminate comprising a plurality of sheets of the wet water-disintegrable nonwoven fabric according to claim 7 laminated together.

9. 9. The wet water-disintegrable nonwoven fabric laminate according to claim 8, wherein each leaf of the wet water-disintegrable nonwoven fabric is folded with overlapping portions.

10. A package containing the wet water-disintegrable nonwoven fabric laminate according to claim 8 or 9, the package having an opening at an upper portion of the wet water-disintegrable nonwoven fabric laminate for removing the wet water-disintegrable nonwoven fabric, A package in which 1 part by mass of the water-disintegrable nonwoven fabric in an absolutely dry state is impregnated with 2 parts by mass of pure water and left for 2 days, and in the wet water-disintegrable nonwoven fabric, the direction in which streaks that are jet marks caused by high-pressure water jet treatment extend corresponds to the direction in which the wet water-disintegrable nonwoven fabric is taken out.

11. A method for producing a water-decomposable nonwoven fabric, comprising the steps of forming a nonwoven fabric sheet containing softwood pulp fibers and regenerated cellulose fibers using a wet papermaking machine, and then subjecting the nonwoven fabric sheet to a high-pressure water jet treatment, The regenerated cellulose fibers include hollow flat rayon fibers and chrysanthemum-shaped rayon fibers, The average fiber length of the regenerated cellulose fibers is 2 mm or more and 20 mm or less, The content of the softwood pulp fibers is 50 to 90% by mass based on the total mass of the water-decomposable nonwoven fabric, Furthermore, in the case of the water-decomposable nonwoven fabric in a wet state after impregnating 2 parts by mass of pure water with 1 part by mass of the bone-dry water-decomposable nonwoven fabric and leaving it for 2 days, The tensile strength in the direction in which the streaks caused by the high-pressure water jet treatment extend is WT 1 N / m, The tensile strength in the direction perpendicular to the direction in which the streaks caused by the high-pressure water jet treatment extend is WT. 2 When expressed as N / m, 80≦WT 1 ≦190, and 2.0≦WT 1 / W.T. 2 A method for producing a water-decomposable nonwoven fabric, comprising adjusting a jet wire ratio so as to satisfy the condition of ≦4.0.

Citation Information

Patent Citations

  • Water dispersible nonwoven fabric

    JP1987184193A

  • Water-disintegrable paper

    JP1994184984A

  • Water-disintegrable nonwoven fabric and its production

    JP1999093055A

  • Nonwoven fabric, method for producing the same and use of the same

    JP2001146664A

  • Water-disintegratable paper

    JP2001234457A