Heavy duty pneumatic tires
A heavy-duty tire with a tread made of isoprene, butadiene, and styrene-butadiene rubber, combined with specific carbon black properties and a high land ratio, addresses wear resistance issues in heavy-duty tires, enhancing durability and reducing heat generation.
Patent Information
- Application Number
- JP2023010969
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-01-27
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2038-10-24
AI Technical Summary
Existing heavy-duty tires face challenges in achieving excellent wear resistance, particularly in large vehicles like trucks and buses, despite advancements in tread patterns and compounding for environmental considerations.
The tire's tread portion is composed of a rubber composition containing isoprene rubber, butadiene rubber, and styrene-butadiene rubber with specific particle diameters and carbon black content, along with a high land ratio, enhancing wear resistance through improved reinforcement and energy dispersion.
The tire exhibits significantly improved wear resistance and reduced heat generation, maintaining performance in actual vehicle conditions.
Smart Images

Figure 0007559847000002 
Figure 0007559847000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a heavy duty pneumatic tire. [Background technology]
[0002] In general, the tread portion of heavy duty tires used for large vehicles such as trucks and buses is provided with a plurality of main grooves extending continuously in the tire circumferential direction and land portions separated by these main grooves. From the viewpoint of environmental aspects, etc., such heavy duty tires require a total tire life and wear resistance (high severity), and improvements are being made, for example, in terms of tread patterns and compounding.
[0003] For example, Patent Document 1 discloses a heavy-duty tire having circumferential grooves in a zigzag pattern extending continuously in the tire circumferential direction in the tread portion and center inclined grooves arranged so as to separate a plurality of center blocks between the circumferential grooves, in which a predetermined shape is imparted to the center blocks, thereby obtaining excellent wear resistance, etc. Thus, from the viewpoint of environmental aspects, etc., there is a demand for providing a heavy-duty tire having excellent wear resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-088343 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to solve the above problems and to provide a heavy-duty pneumatic tire having excellent wear resistance. [Means for solving the problem]
[0006] The present invention relates to a rubber composition for a tread portion, the rubber composition comprising isoprene-based rubber, butadiene-based rubber, styrene-butadiene-based rubber, and a rubber composition having an average particle size of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area of 130 m 2 The present invention relates to a heavy-duty pneumatic tire that is made of a rubber composition containing carbon black of at least 81% by mass and has a land ratio of at least 81%.
[0007] The rubber composition further has an average particle size of more than 20 nm and not more than 25 nm and / or a cetyltrimethylammonium bromide adsorption specific surface area of 100 m 2 / g or more 130m 2 It is preferred that the carbon black contains less than 1 / g of carbon black.
[0008] The rubber composition preferably has a total styrene content of 2.0 to 11.0 mass % based on 100 mass % of the rubber component.
[0009] The rubber composition preferably has an abrasion resistance performance index of 140 or more. Effect of the Invention
[0010] According to the present invention, the tread portion is made of isoprene-based rubber, butadiene-based rubber, styrene-butadiene-based rubber, and a rubber composition having an average particle diameter of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area of 130 m 2 The heavy-duty pneumatic tire is made of a rubber composition containing carbon black of 81% or more per 1000 t / g and has a land ratio of 81% or more, so that the wear resistance is significantly improved. [Brief description of the drawings]
[0011] [Figure 1] 1 is a development view of a tread portion 2 of a tire 1 according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention relates to a rubber composition for a tread portion, the rubber composition comprising isoprene-based rubber, butadiene-based rubber, styrene-butadiene-based rubber, and a rubber composition having an average particle size of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area of 130 m 2 The heavy-duty pneumatic tire is made of a rubber composition containing carbon black of 81% or more and has a land ratio of 81% or more.
[0013] By forming the tread portion in this manner with a high land ratio shape and by using a rubber composition of a specific blend, the wear resistance performance in an actual vehicle is significantly improved.
[0014] The reason for this improvement in wear resistance (on an actual vehicle) is not clear, but it is presumed to be due to the following effects. First, by blending styrene butadiene rubber into a conventional isoprene rubber / butadiene rubber compound, the reinforcing property with carbon black is improved, and the wear resistance is improved. In addition, by blending a specific carbon black as a reinforcing filler, the reinforcing property with the polymer is secured, and the wear resistance is improved. In other words, by dispersing a small amount of styrene butadiene rubber in a polymer of isoprene rubber / butadiene rubber, a three-phase state of isoprene rubber / butadiene rubber / styrene butadiene rubber is formed, and by dispersing a specific carbon black near the boundary between each phase, the bond between each phase is strengthened, resulting in a rubber composition capable of absorbing impact, and it is presumed that the wear resistance is significantly improved. Furthermore, by increasing the land ratio to a predetermined value or more, the rigidity of the tread is increased, and energy is dispersed, thereby improving the wear resistance. It is presumed that the above-mentioned action and effect makes it possible to provide a tire with significantly (synergistically) improved wear resistance.
[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. 1 is a development view of a tread portion 2 of a tire 1 showing one embodiment of the present invention. The tire 1 of this embodiment is a pneumatic tire for heavy loads.
[0016] The tread portion 2 is provided with, for example, a plurality of main grooves 3 that extend continuously in the tire circumferential direction. In this embodiment, the main grooves 3 include a pair of crown main grooves 4, 4 arranged on both sides of the tire equator C, and a pair of shoulder main grooves 5, 5 arranged between the crown main groove 4 and the tread edge Te.
[0017] The "tread end" Te is defined as the axially outermost contact point when a tire 1 in a normal condition, that is, mounted on a normal rim, inflated to a normal internal pressure, and unloaded, is placed on a flat surface with a normal load and a camber angle of 0 degrees. In the normal condition, the distance in the axial direction between both tread ends Te, Te is defined as the tread width TW. Unless otherwise specified, the dimensions of each part of the tire are values measured in the normal condition.
[0018] A "genuine rim" is a rim that is determined for each tire by the standard system that includes the standard on which the tire is based. For example, in the case of JATMA, it is called a "standard rim," in the case of TRA, it is called a "Design Rim," and in the case of ETRTO, it is called a "Measuring Rim."
[0019] "Normal internal pressure" refers to the air pressure set for each tire by each standard in the standard system on which the tire is based. For JATMA, it is the "maximum air pressure." For TRA, it is the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES." For ETRTO, it is the "INFLATION PRESSURE."
[0020] "Normal load" refers to the load that is determined for each tire by each standard in the system of standards, including the standards on which the tire is based. For JATMA, it is the "maximum load capacity." For TRA, it is the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES." For ETRTO, it is the "LOAD CAPACITY."
[0021] The crown main groove 4 and the shoulder main groove 5 extend continuously in a straight line in the circumferential direction of the tire. Such main grooves 3 effectively discharge water in the grooves rearward in the direction of travel when driving on wet roads, thereby providing excellent wet performance.
[0022] The tread portion 2 is provided with a pair of middle land portions 7, 7 separated by a crown main groove 4 and a shoulder main groove 5, a crown land portion 8 separated between the crown main grooves 4, 4, and a pair of shoulder land portions 9, 9 separated between the shoulder main groove 5 and the tread end Te.
[0023] The middle land portion 7 is provided with a middle lateral groove 30 that connects the crown main groove 4 and the shoulder main groove 5. Such a middle lateral groove 30 smoothly drains the water film on the tread surface 7e of the middle land portion 7 to the crown main groove 4 and the shoulder main groove 5.
[0024] In this embodiment, the middle lateral groove 30 includes a first portion 30a extending from the crown main groove 4 toward the axially outer side, a second portion 30b extending from the shoulder main groove 5 toward the axially inner side, and a third portion 30c connecting the first portion 30a and the second portion 30b. The third portion 30c is inclined at an angle larger than the angles of the first portion 30a and the second portion 30b with respect to the axial direction of the tire. The groove edge 30e of the third portion 30c has a tire axial component and a tire circumferential component, so that the wet performance is improved. In addition, the first portion 30a and the second portion 30b maintain high rigidity of the middle land portion 7 in the tire circumferential direction.
[0025] The crown land portion 8 is provided with a crown lateral groove 31 connecting the crown main grooves 4, 4 on both sides of the tire equator C. In this embodiment, the crown lateral groove 31 is provided with an inclination opposite to that of the middle lateral groove 30. In this specification, a "groove" is defined as a groove-like body having a groove width of 2 mm or more.
[0026] From the viewpoint of wear resistance, the tread portion 2 of the tire 1 has a land ratio of 81% or more, preferably 82% or more, and more preferably 84% or more. From the viewpoint of wet grip performance, the upper limit is preferably 95% or less, and more preferably 90% or less. The "land ratio" is the ratio (Sc / Sa) of the total surface area Sa of the tread surface when all grooves provided within the tread width TW of the tread portion 2 are assumed to be filled in the normal state, to the total area Sc of the contact surface that comes into contact with the ground.
[0027] The rubber composition constituting the tread portion 2 (middle land portion 7, crown land portion 8, shoulder land portion 9, middle lateral groove 30, crown lateral groove 31, etc.) is a rubber component containing isoprene-based rubber, butadiene-based rubber, and styrene-butadiene-based rubber, and a rubber component having an average particle diameter of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area of 130 m 2 / g or more of carbon black.
[0028] The isoprene-based rubber is not particularly limited as long as it is a polymer mainly composed of isoprene-based units (isoprene units and isoprene derivative units (epoxidized isoprene units, etc.)). Examples of the isoprene-based rubber include isoprene rubber (IR), epoxidized isoprene rubber, hydrogenated isoprene rubber, grafted isoprene rubber, natural rubber (NR), deproteinized natural rubber (DPNR), highly purified natural rubber (UPNR), epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. These may be used alone or in combination of two or more. The isoprene-based rubber has an isoprene-based unit content of 95% by mass or more, or may be 98% by mass or more, or may be 100% by mass, in 100% by mass of rubber.
[0029] In the rubber composition, the content of the isoprene-based rubber in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The upper limit is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. Within the above range, good abrasion resistance tends to be obtained.
[0030] The styrene butadiene rubber (SBR) is not particularly limited as long as it is a rubber having styrene units (styrene units and styrene derivative units) and butadiene units (butadiene units and butadiene derivative units), and examples thereof include emulsion-polymerized styrene butadiene rubber (E-SBR) and solution-polymerized styrene butadiene rubber (S-SBR). The total content of styrene units and butadiene units in 100% by mass of rubber in the styrene butadiene rubber is, for example, 95% by mass or more, and may be 98% by mass or more or 100% by mass. These may be used alone or in combination of two or more.
[0031] The styrene-butadiene rubber may be either unmodified SBR or modified SBR. The modified SBR may be any SBR having a functional group that interacts with a filler such as silica, and examples thereof include terminal-modified SBR (terminal-modified SBR having the above-mentioned functional group at the terminal) in which at least one terminal of SBR is modified with a compound (modifier) having the above-mentioned functional group, main-chain-modified SBR having the above-mentioned functional group in the main chain, main-chain-terminal-modified SBR having the above-mentioned functional group in the main chain and at least one terminal (for example, main-chain-terminal-modified SBR having the above-mentioned functional group in the main chain and modified with the above-mentioned modifier at least one terminal), and terminal-modified SBR modified (coupled) with a polyfunctional compound having two or more epoxy groups in the molecule and having a hydroxyl group or epoxy group introduced therein.
[0032] Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms), and an amide group are preferable.
[0033] Modifiers used in modified SBR include, for example, polyglycidyl ethers of polyhydric alcohols such as ethylene glycol diglycidyl ether, glycerin triglycidyl ether, trimethylolethane triglycidyl ether, and trimethylolpropane triglycidyl ether; polyglycidyl ethers of aromatic compounds having two or more phenol groups, such as diglycidylated bisphenol A; polyepoxy compounds, such as 1,4-diglycidylbenzene, 1,3,5-triglycidylbenzene, and polyepoxidized liquid polybutadiene; Epoxy group-containing tertiary amines such as 4,4'-diglycidyl-diphenylmethylamine and 4,4'-diglycidyl-dibenzylmethylamine; diglycidyl amino compounds such as diglycidyl aniline, N,N'-diglycidyl-4-glycidyloxyaniline, diglycidyl orthotoluidine, tetraglycidyl meta-xylylenediamine, tetraglycidyl aminodiphenylmethane, tetraglycidyl-p-phenylenediamine, diglycidyl aminomethylcyclohexane, and tetraglycidyl-1,3-bisaminomethylcyclohexane;
[0034] Amino group-containing acid chlorides such as bis-(1-methylpropyl)carbamic acid chloride, 4-morpholinecarbonyl chloride, 1-pyrrolidinecarbonyl chloride, N,N-dimethylcarbamic acid chloride, and N,N-diethylcarbamic acid chloride; epoxy group-containing silane compounds such as 1,3-bis-(glycidyloxypropyl)-tetramethyldisiloxane and (3-glycidyloxypropyl)-pentamethyldisiloxane;
[0035] Sulfide group-containing silane compounds such as (trimethylsilyl)[3-(trimethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(triethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(tripropoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(tributoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(methyldimethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(methyldiethoxysilyl)propyl]sulfide, (trimethylsilyl)[3-(methyldipropoxysilyl)propyl]sulfide, and (trimethylsilyl)[3-(methyldibutoxysilyl)propyl]sulfide;
[0036] N-substituted aziridine compounds such as ethyleneimine and propyleneimine; alkoxysilanes such as methyltriethoxysilane, N,N-bis(trimethylsilyl)-3-aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)-3-aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminoethyltrimethoxysilane, and N,N-bis(trimethylsilyl)aminoethyltriethoxysilane; amino groups and / or substituted amino groups such as 4-N,N-dimethylaminobenzophenone, 4-N,N-di-t-butylaminobenzophenone, 4-N,N-diphenylaminobenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(diphenylamino)benzophenone, and N,N,N',N'-bis-(tetraethylamino)benzophenone. (Thio)benzophenone compounds having a group; benzaldehyde compounds having an amino group and / or a substituted amino group, such as 4-N,N-dimethylaminobenzaldehyde, 4-N,N-diphenylaminobenzaldehyde, and 4-N,N-divinylaminobenzaldehyde; N-methyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, N-phenyl-2-pyrrolidone, Nt-butyl-2-pyrrolidone, and N-methyl-5-methyl N-substituted pyrrolidones such as 2-pyrrolidone, N-substituted piperidones such as N-methyl-2-piperidone, N-vinyl-2-piperidone, and N-phenyl-2-piperidone; N-substituted lactams such as N-methyl-ε-caprolactam, N-phenyl-ε-caprolactam, N-methyl-ω-laurylolactam, N-vinyl-ω-laurylolactam, N-methyl-β-propiolactam, and N-phenyl-β-propiolactam; and
[0037] Examples of such compounds include N,N-bis-(2,3-epoxypropoxy)-aniline, 4,4-methylene-bis-(N,N-glycidylaniline), tris-(2,3-epoxypropyl)-1,3,5-triazine-2,4,6-triones, N,N-diethylacetamide, N-methylmaleimide, N,N-diethylurea, 1,3-dimethylethyleneurea, 1,3-divinylethyleneurea, 1,3-diethyl-2-imidazolidinone, 1-methyl-3-ethyl-2-imidazolidinone, 4-N,N-dimethylaminoacetophene, 4-N,N-diethylaminoacetophenone, 1,3-bis(diphenylamino)-2-propanone, and 1,7-bis(methylethylamino)-4-heptanone. The modification with the above compound (modifying agent) can be carried out by a known method.
[0038] As the styrene-butadiene rubber, for example, SBR manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., and the like can be used.
[0039] The styrene content of the styrene butadiene rubber is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and particularly preferably 20% by mass or more. The styrene content is preferably 60% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 25% by mass or less. By keeping it within the above range, good abrasion resistance and heat resistance tend to be obtained. The styrene content of the styrene butadiene rubber is 1 It is calculated by H-NMR measurement.
[0040] In the rubber composition, the content of the styrene-butadiene rubber in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass or more. By making it equal to or more than the lower limit, good abrasion resistance tends to be obtained. In addition, the upper limit is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, and particularly preferably 35% by mass or less. There is a concern that the use of a large amount of styrene-butadiene rubber may deteriorate heat generation performance, but by making it equal to or less than the upper limit, deterioration of heat generation performance tends to be suppressed.
[0041] The butadiene rubber (BR) is not particularly limited as long as it is a polymer mainly composed of butadiene units (butadiene units and butadiene derivative units), and for example, BR with a high cis content, BR with a low cis content, BR containing syndiotactic polybutadiene crystals, etc. can be used. These may be used alone or in combination of two or more. The butadiene rubber has a butadiene unit content of, for example, 95% by mass or more, 98% by mass or more, or 100% by mass, in 100% by mass of rubber. Rubber containing butadiene units and styrene units corresponds to the styrene butadiene rubber, but does not correspond to the butadiene rubber.
[0042] The cis content of BR is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more, with no particular upper limit. When it is within the above range, the effect tends to be better. The cis content of BR can be measured by infrared absorption spectroscopy.
[0043] The butadiene rubber may be either unmodified BR or modified BR. The modified BR may be the modified BR into which the above-mentioned functional groups have been introduced.
[0044] As the butadiene-based rubber, for example, products of Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Corporation, etc. can be used.
[0045] The content of the butadiene rubber in 100% by mass of the rubber component is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more. The upper limit is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less. Within the above range, good abrasion resistance is obtained and processability tends to be easily ensured.
[0046] The rubber composition may contain rubber components other than isoprene-based rubber, butadiene-based rubber, and styrene butadiene-based rubber. Examples of other rubber components that may be contained include diene rubbers such as styrene isoprene butadiene rubber (SIBR), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), acrylonitrile butadiene rubber (NBR), and butyl rubber (IIR). The rubber components may be used alone or in combination of two or more.
[0047] In the rubber composition, the total styrene content (total content of styrene parts contained in the total amount of rubber components) in 100% by mass of the rubber components is preferably 2.0% by mass or more, more preferably 4.0% by mass or more, and even more preferably 6.0% by mass or more. The upper limit is preferably 11.0% by mass or less, more preferably 10.0% by mass or less, and even more preferably 9.0% by mass or less. Within the above range, good wear resistance and heat resistance tend to be obtained. Here, the total styrene amount (mass%) in 100% by mass of the rubber component is Σ(content (mass%) of each styrene-containing rubber × styrene content (mass%) of each styrene-containing rubber / 100). For example, when the rubber component is composed of 30% by mass of NR, 30% by mass of SBR (styrene content 23.5% by mass), and 40% by mass of BR, the total styrene amount in 100% by mass of the rubber component is 7.05% by mass (=30×23.5 / 100).
[0048] The rubber composition has an average particle size of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of 130 m 2 / g or more of carbon black (also referred to as carbon black (A)).
[0049] From the viewpoint of abrasion resistance, the average particle size of the carbon black (A) is preferably 20 nm or less, more preferably 17 nm or less, and even more preferably 15 nm or less. Although there is no particular lower limit, from the viewpoint of dispersibility, etc., the average particle size is preferably 5 nm or more, more preferably 10 nm or more. The average particle size of carbon black is a number average particle size, and is measured by a transmission electron microscope.
[0050] From the viewpoint of wear resistance, the CTAB of the carbon black (A) is preferably 130m 2 / g or more, more preferably 140m 2 / g or more, more preferably 145m 2 / g or more, particularly preferably 150m 2 The upper limit is not particularly limited, but from the viewpoint of dispersibility, etc., it is preferably 250 m 2 / g or less, more preferably 200m 2 / g or less, more preferably 180m 2 / g or less. In this specification, the CTAB of carbon black is a value measured in accordance with JIS K6217-3:2001.
[0051] The nitrogen adsorption specific surface area (N 2 SA) is preferably 125 mm from the viewpoint of wear resistance. 2 / g or more, more preferably 145m 2 / g or more, more preferably 150m 2 / g or more, particularly preferably 155m 2 The upper limit is not particularly limited, but from the viewpoint of dispersibility, etc., it is preferably 250 m 2 / g or less, more preferably 200m 2 / g or less, more preferably 180m 2 / g or less. In addition, the N of carbon black 2 SA is determined according to JIS K 6217-2:2001.
[0052] The iodine adsorption amount (IA) (mg / g) of the carbon black (A) is preferably 120 mg / g or more, more preferably 125 mg / g or more, even more preferably 130 mg / g or more, and particularly preferably 140 mg / g or more from the viewpoint of abrasion resistance. The upper limit is not particularly limited, but is preferably 200 mg / g or less, more preferably 180 mg / g or less, and even more preferably 160 mg / g or less from the viewpoint of dispersibility, etc.
[0053] The ratio (CTAB / IA) of the cetyltrimethylammonium bromide adsorption specific surface area (CTAB) to the iodine adsorption amount (IA) (mg / g) of the carbon black (A) is preferably 0.85 to 1.35 m from the viewpoint of wear resistance. 2 / mg, more preferably 0.92 to 1.30m 2 / mg, more preferably 1.00 to 1.25m 2 / mg. In this specification, the iodine adsorption amount (IA) of carbon black is a value measured in accordance with JIS K6217-1:2001.
[0054] The surface activity index represented by CTAB / IA can be considered as an index of the crystallinity (graphitization rate) of carbon black. In other words, the higher the CTAB / IA, the less crystallized the carbon black is, and the greater the interaction between the carbon black and the rubber component tends to be. CTAB / IA is also considered as a parameter for evaluating the amount of acidic functional groups present on the carbon black surface. The acidic functional groups on the carbon black surface contribute to the interaction with the rubber component, and the higher the CTAB / IA, the more acidic functional groups are present on the carbon black surface. Therefore, when the CTAB / IA is within the above range, a more significant reinforcing effect can be achieved for the rubber component, and excellent wear resistance can be obtained.
[0055] From the viewpoint of abrasion resistance, the dibutyl phthalate oil absorption (DBP) of the carbon black (A) is preferably 120 cm 3 / 100g or more, preferably 125cm 3 / 100g or more, more preferably 135cm 3 The upper limit is not particularly limited, but from the viewpoint of dispersibility, etc., it is preferably 180 cm 3 / 100g or less, more preferably 170cm 3 / 100g or less, more preferably 160cm 3 / 100g or less. The DBP of carbon black is measured in accordance with JIS K 6217-4:2001.
[0056] Examples of carbon black (A) include SAF. These carbon blacks may be used alone or in combination of two or more. Carbon black (A) can also be produced by the production methods described in JP-A-200-319539 and JP-T-8-507555.
[0057] The content of carbon black (A) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the rubber component. If it is above the lower limit, good abrasion resistance tends to be obtained. In addition, from the viewpoint of dispersibility, the content is preferably 70 parts by mass or less, more preferably 60 parts by mass or less, even more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less.
[0058] The rubber composition preferably further contains a carbon black other than the carbon black (A) (also referred to as other carbon black), which can synergistically improve the abrasion resistance.
[0059] Other examples of carbon black include carbon black having an average particle size of more than 20 nm and not exceeding 25 nm and / or a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of 100 m 2 / g or more 130m 2 Carbon black having a molecular weight of less than 1000 kJ / g (also referred to as carbon black (B)) can be suitably used.
[0060] The average particle size of the carbon black (B) is more than 20 nm and not more than 25 nm (greater than 20 nm and not more than 25 nm), but the lower limit is preferably 21 nm or more from the viewpoint of dispersibility, etc. The upper limit is preferably 24 nm or less, more preferably 23 nm or less, from the viewpoint of abrasion resistance.
[0061] From the viewpoint of wear resistance, the CTAB of the carbon black (B) is preferably 105m 2 / g or more, more preferably 110m 2 The upper limit is not particularly limited, but from the viewpoint of dispersibility, etc., it is preferably 125 m 2 / g or less, more preferably 120m 2 / g or less.
[0062] The average particle size, CTAB, of other carbon blacks such as carbon black (B) can be measured by the same method as described above.
[0063] The content of carbon black (B) is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 30 parts by mass or more, based on 100 parts by mass of the rubber component. If it is above the lower limit, good abrasion resistance tends to be obtained. In addition, from the viewpoint of dispersibility, the content is preferably 100 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 60 parts by mass or less.
[0064] Other carbon blacks include, but are not limited to, N220, N234, N219, N339, N330, N326, N351, N550, N762, etc. For example, products from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., etc. can be used. These may be used alone or in combination of two or more. From the viewpoints of wear resistance and cost, N220 is particularly preferred.
[0065] The carbon black content (total content of carbon black (A) and other carbon black) is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, even more preferably 45 parts by mass or more, and particularly preferably 50 parts by mass or more, per 100 parts by mass of the rubber component. If the content is above the lower limit, good abrasion resistance tends to be obtained. From the viewpoint of dispersibility, the content is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 70 parts by mass or less.
[0066] The content of carbon black (A) in 100% by mass of carbon black is preferably 5% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more. The upper limit of the content is preferably 80% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less. Within the above range, good abrasion resistance tends to be obtained.
[0067] The rubber composition may contain silica. When silica is compounded in the rubber composition, the content is preferably 3.0 parts by mass or more, more preferably 5.0 parts by mass or more, based on 100 parts by mass of the rubber component, from the viewpoint of grip performance. The content is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less.
[0068] The nitrogen adsorption specific surface area of silica (N 2 SA) is preferably 80m 2 / g or more, more preferably 115m 2 / g or more, more preferably 150m 2 By making it equal to or higher than the lower limit, good grip performance tends to be obtained. 2 / g or less, more preferably 270m 2 / g or less, more preferably 250m 2 By setting the content to the upper limit or less, good silica dispersibility tends to be obtained. In addition, the N of silica 2SA is a value measured by the BET method in accordance with ASTM D3037-93.
[0069] The silica is not particularly limited, and for example, dry process silica (anhydrous silica) or wet process silica (hydrated silica) can be used, but wet process silica (hydrated silica) is preferred because it has a large number of silanol groups. Commercially available products include those from Degussa, Tosoh Silica Co., Ltd., Solvay Japan Co., Ltd., Tokuyama Co., Ltd., etc. These may be used alone or in combination of two or more.
[0070] The rubber composition may contain other fillers in addition to carbon black and silica, such as calcium carbonate, talc, alumina, clay, aluminum hydroxide, and mica.
[0071] When the rubber composition contains silica, it is preferable that the rubber composition contains a silane coupling agent together with the silica. The silane coupling agent may be any silane coupling agent that has been conventionally used in combination with silica in the rubber industry, and is not particularly limited. Examples of the silane coupling agent include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxy ... mercapto-based compounds such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and Momentive's NXT and NXT-Z; vinyl-based compounds such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based compounds such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based compounds such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based compounds such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based compounds such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. Commercially available products include those from Degussa, Momentive, Shin-Etsu Silicone, Tokyo Chemical Industry, Azumax, and Dow Corning Toray. These may be used alone or in combination of two or more. Of these, sulfide-based and mercapto-based products are preferred.
[0072] When the rubber composition contains a silane coupling agent, the content is preferably 2 parts by mass or more, more preferably 5 parts by mass or more, based on 100 parts by mass of silica. By making the content equal to or more than the lower limit, the effect of compounding the silane coupling agent tends to be obtained. Also, the content is preferably 20 parts by mass or less, more preferably 15 parts by mass or less. By making the content equal to or less than the upper limit, the effect commensurate with the compounding amount is obtained, and good processability during kneading tends to be obtained.
[0073] The rubber composition may contain a softener (a softener that is in a liquid state at room temperature (25° C.)) such as oil or a liquid diene polymer.
[0074] Examples of the oil include process oils such as paraffin-based, aromatic, and naphthenic process oils.
[0075] The liquid diene polymer has a weight average molecular weight (Mw) of 1.0×10 based on polystyrene standards, as measured by gel permeation chromatography (GPC). 3 ~2.0×10 5 Preferably, it is 3.0×10 3 ~1.5×10 4 It is more preferable that the content is equal to or more than the lower limit. By setting the content to be equal to or more than the lower limit, good abrasion resistance and fracture properties can be obtained, and sufficient durability can be secured. On the other hand, by setting the content to be equal to or less than the upper limit, the viscosity of the polymerization solution can be good, and excellent productivity can be obtained. In the present invention, the Mw of the liquid diene polymer is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0076] Examples of liquid diene polymers include liquid styrene butadiene copolymers (liquid SBR), liquid butadiene polymers (liquid BR), liquid isoprene polymers (liquid IR), liquid styrene isoprene copolymers (liquid SIR), liquid styrene butadiene styrene block copolymers (liquid SBS block polymers), liquid styrene isoprene styrene block copolymers (liquid SIS block polymers), liquid farnesene polymers, and liquid farnesene butadiene copolymers. These may be modified at the ends or main chains with polar groups. Of these, liquid IR and liquid SBR are preferred.
[0077] In the rubber composition, the content of the softener (total amount of softener) is preferably 1.0 to 50 parts by mass, more preferably 2.0 to 30 parts by mass, further preferably 2.0 to 20 parts by mass, and particularly preferably 2.0 to 10 parts by mass, per 100 parts by mass of the rubber component, from the viewpoint of abrasion resistance. In this specification, the content of the softener includes the amount of oil contained in the oil-extended rubber.
[0078] The rubber composition may contain a resin that is in a solid state at room temperature (25° C.) The content of the resin is preferably 3 to 50 parts by mass, and more preferably 7 to 40 parts by mass, based on 100 parts by mass of the rubber component.
[0079] Examples of resins include aromatic vinyl polymers, coumarone-indene resins, indene resins, rosin resins, terpene resins, and acrylic resins. Commercially available products include those from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Co., Ltd., Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JX Energy Corporation, Arakawa Chemical Industries Co., Ltd., Taoka Chemical Co., Ltd., and Toagosei Co., Ltd. These may be used alone or in combination of two or more. Among these, aromatic vinyl polymers, coumarone-indene resins, terpene resins, and rosin resins are preferred.
[0080] The aromatic vinyl polymer may be a resin obtained by polymerizing α-methylstyrene and / or styrene, such as a homopolymer of styrene, a homopolymer of α-methylstyrene, a copolymer of α-methylstyrene and styrene, etc. Among these, a copolymer of α-methylstyrene and styrene is preferred.
[0081] The coumarone-indene resin is a resin containing coumarone and indene as main monomer components constituting the resin skeleton (main chain), and monomer components contained in the skeleton other than coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc.
[0082] The indene resin is a resin that contains indene as a main monomer component that constitutes the skeleton (main chain) of the resin.
[0083] The rosin-based resins (rosins) can be classified according to whether they are modified or not, and can be classified into unmodified rosin (unmodified rosin) and modified rosin (rosin derivatives). Examples of unmodified rosin include tall rosin (also known as tall oil rosin), gum rosin, wood rosin, disproportionated rosin, polymerized rosin, hydrogenated rosin, and other chemically modified rosins. Modified rosin is a modification of unmodified rosin, and examples of the modified rosin include rosin esters, unsaturated carboxylic acid modified rosin esters, unsaturated carboxylic acid modified rosin esters, rosin amide compounds, and rosin amine salts.
[0084] The rosin resin preferably has a moderate acid value without an excessively high carboxyl group content. Specifically, the acid value of the rosin resin is usually more than 0 mgKOH / g, for example, 200 mgKOH / g or less, preferably 100 mgKOH / g or less, more preferably 30 mgKOH / g or less, and further preferably 10 mgKOH / g or less. The acid value can be measured according to the examples described later. If the acid value is excessively high, the acid value can be adjusted to the above range by reducing the number of carboxyl groups in the rosin through a known esterification treatment.
[0085] As the terpene resin, a polyterpene resin obtained by polymerizing a terpene compound, an aromatic modified terpene resin obtained by polymerizing a terpene compound and an aromatic compound, etc. can be used. Hydrogenated products of these resins can also be used.
[0086] The polyterpene resin is a resin obtained by polymerizing a terpene compound. The terpene compound is a polyterpene resin having a molecular weight of 1,000 to 1,0 .... 5 H 8 ) n The hydrocarbons and their oxygen-containing derivatives represented by the composition 10 H 16 ), sesquiterpenes (C 15 H 24 ), diterpenes (C 20 H 32 ), and examples thereof include α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, and γ-terpineol.
[0087] Examples of the polyterpene resin include pinene resin, limonene resin, dipentene resin, pinene / limonene resin, etc., which are made from the above-mentioned terpene compounds. Among them, pinene resin is preferred because it is easy to polymerize and is inexpensive because it is made from natural pine resin. Pinene resin usually contains both α-pinene and β-pinene, which are isomers, but depending on the components contained, it is classified into β-pinene resin containing β-pinene as the main component and α-pinene resin containing α-pinene as the main component.
[0088] Examples of the aromatic modified terpene resin include terpene phenol resins made from the above terpene compounds and phenolic compounds, and terpene styrene resins made from the above terpene compounds and styrene compounds. Terpene phenol styrene resins made from the above terpene compounds, phenolic compounds, and styrene compounds can also be used. Examples of the phenolic compounds include phenol, bisphenol A, cresol, and xylenol. Examples of the styrene compounds include styrene and α-methylstyrene.
[0089] The rubber composition preferably contains sulfur (a sulfur vulcanizing agent). Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0090] The content of the sulfur (sulfur vulcanizing agent) per 100 parts by mass of the rubber component is preferably 0.3 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1.0 parts by mass or more. By making it equal to or more than the lower limit, good wear resistance tends to be obtained. The upper limit is not particularly limited, but is preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, even more preferably 2.5 parts by mass or less, and particularly preferably 2.0 parts by mass or less.
[0091] The rubber composition preferably contains a vulcanization accelerator. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide (DM(2,2'-dibenzothiazolyl disulfide)), and N-cyclohexyl-2-benzothiazylsulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); Examples of the vulcanization accelerator include sulfenamide-based vulcanization accelerators such as hexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenyl guanidine, di-orthotolyl guanidine, and orthotolyl biguanidine. These may be used alone or in combination of two or more. Among them, sulfenamide-based and guanidine-based vulcanization accelerators are preferred.
[0092] The content of the vulcanization accelerator is preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more, based on 100 parts by mass of the rubber component, from the viewpoint of vulcanization characteristics, etc. Also, the content is preferably 8.0 parts by mass or less, more preferably 5.0 parts by mass or less, and even more preferably 3.0 parts by mass or less.
[0093] The rubber composition may contain a wax. The wax is not particularly limited, and examples thereof include petroleum waxes such as paraffin wax and microcrystalline wax; natural waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene, etc. Commercially available products include those from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. These may be used alone or in combination of two or more kinds. Among them, petroleum waxes are preferred, and paraffin wax is more preferred.
[0094] The amount of the wax per 100 parts by mass of the rubber component is preferably 0.5 part by mass or more, more preferably 1 part by mass or more, and preferably 10 parts by mass or less, more preferably 6 parts by mass or less.
[0095] The rubber composition may contain an antioxidant. The antioxidant is not particularly limited, and examples thereof include naphthylamine-based antioxidants such as phenyl-α-naphthylamine; diphenylamine-based antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylene Examples of the antioxidant include p-phenylenediamine antioxidants such as diamines; quinoline antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Commercially available products include those from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd. These may be used alone or in combination of two or more. Among them, p-phenylenediamine antioxidants (more preferably, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) are preferred.
[0096] The amount of the antioxidant per 100 parts by mass of the rubber component is preferably 0.3 parts by mass or more, more preferably 1 part by mass or more, and is preferably 7 parts by mass or less, more preferably 6 parts by mass or less, and further preferably 5 parts by mass or less.
[0097] The rubber composition may also contain a fatty acid, in particular stearic acid. As the stearic acid, any conventionally known product can be used, for example, products available from NOF Corporation, NOF Corporation, Kao Corporation, Fujifilm Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., and the like.
[0098] The amount of the fatty acid is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and further preferably 2.5 parts by mass or more, based on 100 parts by mass of the rubber component. The amount is preferably 10 parts by mass or less, and more preferably 5 parts by mass or less.
[0099] The rubber composition may contain zinc oxide. As the zinc oxide, any known zinc oxide can be used, for example, products available from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., and the like.
[0100] The amount of zinc oxide per 100 parts by mass of the rubber component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and is preferably 5 parts by mass or less, more preferably 4 parts by mass or less.
[0101] In addition to the above-mentioned components, the rubber composition may contain additives that are generally used in the tire industry, such as surfactants.
[0102] The rubber composition can be produced by a known method, for example, by kneading the components using a rubber kneading device such as an open roll, a Banbury mixer, or a kneader, and then vulcanizing the mixture.
[0103] As for the kneading conditions, in the base kneading step in which additives other than the crosslinking agent (vulcanizing agent) and the vulcanization accelerator are kneaded, the kneading temperature is usually 100 to 180°C, preferably 120 to 170°C. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 120°C or lower, preferably 85 to 110°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 140 to 190°C, preferably 150 to 185°C.
[0104] The rubber composition (rubber composition after vulcanization) preferably has an abrasion resistance performance index of not less than 140. The larger the abrasion resistance performance index, the more preferable, with 150 or more being more preferable, and 160 or more being even more preferable. The abrasion resistance performance index is a value obtained by the method described in the Examples section below.
[0105] The heavy-duty pneumatic tire of the present invention is manufactured by a conventional method using the above-mentioned rubber composition. That is, the rubber composition containing the above-mentioned components is extruded in an unvulcanized state to match the shape of a tread (a component that comes into contact with the road surface, such as a single-layer tread or a cap tread of a multi-layer tread) and other components, and molded in a conventional method on a tire building machine together with other tire components to form an unvulcanized tire. The unvulcanized tire is heated and pressurized in a vulcanizer to obtain a tire. The tire can be used for trucks, buses, etc. EXAMPLES
[0106] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.
[0107] (Production Example 1) Fine particle carbon black 1 was produced by the method described in Example 3 of JP-A-8-507555.
[0108] (Production Example 2) A carbon black reactor was used in which a combustion zone having an inner diameter of 800 mm and a length of 1600 mm and equipped with an air inlet duct and a combustion burner, a raw material introduction zone consisting of a narrow-diameter section having an inner diameter of 145 mm and a length of 1000 mm connected to the combustion zone and having a raw material nozzle penetrating from the periphery, and a rear reaction zone having an inner diameter of 400 mm and a length of 3000 mm and equipped with a quenching device were successively connected, and C heavy oil was used as the fuel and creosote oil as the raw material hydrocarbon, and each condition was set to produce fine particle carbon black 2.
[0109] Various chemicals used in the examples and comparative examples will be collectively described below. NR:TSR20 SBR: SBR1502 (styrene content: 23.5% by mass) manufactured by Sumitomo Chemical Co., Ltd. BR: BR150B (cis content: 95% by mass) manufactured by Ube Industries, Ltd. Fine particle carbon black 1: Production example 1 (average particle size 16 nm, CTAB 170 m 2 / g, N 2 SA174m 2 / g, IA163mg / g, CTAB / IA1.04, DBP154cm 3 / 100g) Fine particle carbon black 2: Production example 2 (average particle size 16 nm, CTAB 158 m 2 / g, N 2 SA170m 2 / g, IA145mg / g, CTAB / IA1.09, DBP138cm 3 / 100g) Fine particle carbon black 3: N134 (average particle size 18 nm, CTAB130m 2 / g, N 2 SA148m 2 / g, IA144mg / g, CTAB / IA0.90, DBP123cm 3 / 100g) Carbon black 4: N220 (average particle size 22 nm, CTAB115m 2 / g, N 2 SA115m 2 / g, IA118mg / g, CTAB / IA0.97, DBP113cm 3 / 100g) Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Anti-aging agent: Nocrac 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Stearic acid: stearic acid manufactured by NOF Corporation Zinc oxide: Two types of zinc oxide manufactured by Mitsui Mining & Smelting Co., Ltd. Oil: TDAE oil manufactured by Japan Energy Corporation Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator: Noccela NS (N-tert-butyl-2-benzothiazylsulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0110] Examples and Comparative Examples According to the compounding recipe shown in Table 1, chemicals other than sulfur and vulcanization accelerator were kneaded for 5 minutes at 150°C using a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. Next, sulfur and vulcanization accelerator were added to the kneaded product obtained, and the mixture was kneaded for 5 minutes at 80°C using an open roll to obtain an unvulcanized rubber composition. The resulting unvulcanized rubber composition was press-vulcanized at 150° C. for 35 minutes to obtain a vulcanized rubber sheet.
[0111] According to the land ratio shown in Table 1, the obtained unvulcanized rubber composition was molded into a tread shape, and laminated together with other tire components to prepare an unvulcanized tire. The tire was press-vulcanized at 150°C for 20 minutes to obtain a test tire (size: 225 / 70R19.5 (for heavy load)) having the basic pattern shown in FIG. 1.
[0112] The obtained test tires and vulcanized rubber sheets were evaluated as follows, and the results are shown in Table 1.
[0113] <Wear resistance (rubber composition after vulcanization)> Using an LAT tester (Laboratery Abration and Skid Tester, a rubber abrasion tester "LAT100" manufactured by Hiraizumi Yoko Co., Ltd.), the volume loss of each vulcanized rubber sheet (rubber composition after vulcanization) was measured under conditions of a load of 40 N, a speed of 20 km / h, and a slip angle of 6°. The volume loss of the compounded rubber of Comparative Example 1 was set to 100, and the abrasion resistance performance index of each compound was calculated according to the following calculation formula. The larger the value, the more excellent the abrasion resistance performance. (Wear resistance performance index) = (Volume loss amount of the compounding of Comparative Example 1) / (Volume loss amount of each compounding) × 100
[0114] <Fever> Using a spectrometer manufactured by Ueshima Seisakusho Co., Ltd., tan δ of each vulcanized rubber sheet (rubber composition after vulcanization) was measured at a dynamic strain amplitude of 1%, a frequency of 10 Hz, and a temperature of 50° C. The reciprocal value of tan δ was expressed as an index (heat generation index) with Comparative Example 2 being set at 100. A larger value indicates less heat generation and better low heat generation properties.
[0115] <Wear resistance performance (actual vehicle)> A 2D vehicle fitted with each test tire was driven on an asphalt surface on a general road for a total of 10,000 km, after which the groove depth of each of the four main grooves on each of the two front tires was measured and averaged. The results are expressed as an index with Comparative Example 1 set to 100, and the higher the value, the better the wear resistance on an actual vehicle.
[0116] [Table 1]
[0117] From Table 1, the examples in which the tread portion was made of a rubber composition containing isoprene-based rubber, butadiene-based rubber, styrene-butadiene-based rubber, and carbon black having a predetermined average particle size and / or cetyltrimethylammonium bromide adsorption specific surface area, and the land ratio of the tread portion was adjusted to a predetermined value or more, were extremely excellent in wear resistance performance on an actual vehicle. Heat generation was also suppressed. On the other hand, Comparative Example 2, which had a small land ratio, and Comparative Example 3, which did not contain SBR, were inferior in these performances. [Explanation of symbols]
[0118] 1. Tires (pneumatic tires for heavy loads) 2 Tread section 3 Main groove 4 Crown main groove 5 Shoulder main groove 7 Middle Land Section 7e Middle land tread 8 Crown Land Division 9 Shoulder Land Section 30 Middle Yokomizo 30a Middle Yokomizo Part 1 30b Middle Yokomizo Part 2 30c Middle Yokomizo Part 3 30e Middle lateral groove edge 31 Crown lateral groove Te tread edge TW tread width
Claims
1. The tread portion is made of isoprene-based rubber, butadiene-based rubber, styrene-butadiene-based rubber, and a rubber composition having an average particle diameter of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area of 130 m 2 A heavy-duty pneumatic tire comprising a rubber composition containing carbon black of 100% or more and having a land ratio of 81% or more, The rubber composition comprises a content of the isoprene-based rubber in 100% by mass of the rubber component is 5% by mass or more and 30% by mass or less, a content of the butadiene-based rubber is 10% by mass or more, and a content of the styrene-butadiene-based rubber is 5% by mass or more, The heavy-duty pneumatic tire has a carbon black content of 5 parts by mass or more and 30 parts by mass or less based on 100 parts by mass of a rubber component.
2. A heavy-duty pneumatic tire having a tread portion made of a rubber composition containing isoprene-based rubber, butadiene-based rubber, styrene-butadiene-based rubber, and carbon black having an average particle size of 20 nm or less and / or a cetyltrimethylammonium bromide adsorption specific surface area of 130 m2 / g or more, and having a land ratio of 81% or more, The rubber composition comprises the content of the isoprene-based rubber is 5% by mass or more and 30% by mass or less, the content of the butadiene-based rubber is 10% by mass or more and 60% by mass or less, and the content of the styrene-butadiene-based rubber is 5% by mass or more and 60% by mass or less, based on 100% by mass of the rubber component; The heavy-duty pneumatic tire has a carbon black content of 5 parts by mass or more and 30 parts by mass or less based on 100 parts by mass of a rubber component.
3. 3. The heavy-duty pneumatic tire according to claim 1, wherein the rubber composition has a total styrene content of 6.0 to 11.0 mass % based on 100 mass % of the rubber component.
4. The rubber composition further has an average particle size of more than 20 nm and not more than 25 nm and / or a cetyltrimethylammonium bromide adsorption specific surface area of 100 m 2 / g or more 130m 2 4. The heavy-duty pneumatic tire according to claim 1, further comprising carbon black of less than 0.1 g / g.
5. The heavy duty pneumatic tire according to any one of claims 1 to 4, wherein the rubber composition has an abrasion resistance performance index of 140 or more.
Citation Information
Patent Citations
Tread rubber composition for retreaded tire
JP1994192480A
Tread rubber composition for heavy load tire or its retreaded tire
JP2000219778A
Pneumatic tire
JP2003252009A
Pneumatic tire for heavy load
JP2005232407A
Rubber composition for flap and pneumatic tire
JP2010275359A