Secondary battery and manufacturing method therefor
The pre-doping of silicon-based negative electrodes with lithium in lithium secondary batteries addresses the high irreversible capacity issue, resulting in improved energy density, cycle life, and safety by minimizing volumetric expansion and enhancing conductivity.
Patent Information
- Application Number
- JP2022510936
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-19
- Filing Date
- 2020-08-19
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-08-19
AI Technical Summary
Existing lithium secondary batteries face challenges in achieving high energy density, cycle characteristics, and safety due to the high irreversible capacity of silicon-based negative electrode active materials, which lead to volumetric expansion and reduced performance.
A secondary battery design that includes a silicon-based negative electrode pre-doped with lithium to compensate for initial irreversible capacity, reducing the need for lithium in the positive electrode and minimizing volumetric expansion, combined with a carbon layer to enhance conductivity and stability.
The pre-doping method significantly increases energy density, cycle characteristics, and speed characteristics, particularly enhancing initial discharge capacity and capacity retention, while ensuring safety and stability.
Smart Images

Figure 0007560150000005 
Figure 0007560150000006 
Figure 0007560150000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a secondary battery including a negative electrode pre-doped with lithium and including a silicon-based negative electrode active material, and a method for manufacturing the same. [Background technology]
[0002] In recent years, with the development of the information and communication industry, as electronic devices become smaller, lighter, thinner, and more portable, the demand for high energy density of batteries used as power sources for these electronic devices increases. Lithium secondary batteries are the batteries that can best meet this demand, and research is being actively conducted on the application of the same to small batteries and large electronic devices, such as automobiles and power storage systems.
[0003] Lithium secondary batteries have mainly used lithium-containing transition metal oxides, such as LiCoO2 and LiMn2O4, as positive electrodes and carbon-based materials, such as graphite, as negative electrodes. However, in order to achieve excessive improvements in the charging speed of active materials, thinning of separators, or particularly high-capacity lithium secondary batteries, in recent years, high charging voltages through methods of reducing the film thickness of such constituent materials as separators have caused problems that adversely affect the safety of lithium secondary batteries.
[0004] Therefore, new materials that can achieve high energy density while achieving the reliability and safety of secondary batteries, such as alloy negative electrode active materials, such as silicon or tin and their oxides, are attracting attention as next-generation high-capacity materials. Oxide-based alloy negative electrode active materials have the advantage of having a smaller volume change than non-oxide-based negative electrode active materials and a charge and discharge capacity four times or more than that of graphite. However, oxide-based alloy negative electrode active materials have the problem of a large irreversible capacity during the first charge and discharge.
[0005] In general, a negative electrode active material made of silicon oxide undergoes an alloying reaction between a material that can reversibly absorb and release lithium and a material that cannot reversibly absorb and release lithium (irreversible material) during initial charging, resulting in a problem that the lithium ions present in the positive electrode at the time of design are reduced.
[0006] In this regard, Japanese Patent Application Publication No. 2002-313324 discloses a method for improving the initial efficiency by directly adding lithium metal to the negative electrode when preparing the negative electrode, however, when lithium metal is directly added to the negative electrode, gelation occurs during the preparation of the negative electrode active material composition, which causes process problems and performance problems of the secondary battery.
[0007] Furthermore, JP 2008-084842 A discloses a method of doping the negative electrode by contacting it with lithium metal when manufacturing a secondary battery. In such a case, however, there may be a problem in the safety of the secondary battery, since a reaction involving silicon oxide or titanium oxide, including significant heat generation, may occur.
[0008] On the other hand, lithium is dissolved in silicon oxide (SiO x , 0.9≦x≦1.6) materials are disclosed in Japanese Patent Application Publication No. 2011-222153 and Japanese Patent No. 6274253. However, the techniques disclosed in these documents either fail to obtain satisfactory secondary battery performance or have slow reaction rates, which make it difficult to mass-produce and use in practice. Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention is devised to solve the problems of the prior art. The technical problem solved by the present invention is to provide a secondary battery that can increase the energy density, cycle characteristics, and rate characteristics, and in particular, can further increase the initial discharge capacity and capacity retention rate.
[0010] Another technical problem solved by the present invention is to provide a method for manufacturing a secondary battery. [Means for solving the problem]
[0011] To achieve the above object, an embodiment of the present invention provides a secondary battery including a positive electrode, a negative electrode, and an electrolyte, wherein the positive electrode includes a metal oxide active material, the negative electrode includes a silicon-based negative electrode active material, and the negative electrode is pre-doped with lithium in an amount corresponding to an initial irreversible capacity of the negative electrode.
[0012] Another embodiment provides a method for producing a secondary battery, comprising the steps of: (1-1) applying a negative electrode active material composition comprising a silicon-based negative electrode active material to a negative electrode current collector to prepare a negative electrode; (1-2) placing a separator between the negative electrode and a lithium metal plate to prepare a cell; (1-3) electrochemically activating the cell obtained in step (1-2) to pre-dope the negative electrode with lithium; and (1-4) producing a secondary battery using the negative electrode pre-doped with lithium.
[0013] Yet another embodiment provides a method for producing a secondary battery, comprising the steps of: (2-1) applying an anode active material composition comprising a silicon-based anode active material to an anode current collector to prepare an anode; (2-2) disposing the anode and a lithium metal plate in a reactor and carrying out an oxidation-reduction reaction to pre-dope the anode with lithium; and (2-3) sequentially stacking the anode pre-doped with lithium, a separator, and a cathode comprising a metal oxide active material to prepare an electrode. Effect of the Invention
[0014] The secondary battery according to the embodiment can achieve not only safety but also a significant increase in energy density, and can improve cycle characteristics and rate characteristics. In particular, the secondary battery can further increase the initial discharge capacity and capacity retention rate. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 shows an example of a step of pre-doping a negative electrode with lithium in a method for manufacturing a secondary battery according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a graph showing the capacity characteristics of Example 3-2 and Comparative Example 3-1 with respect to the number of cycles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention is not limited to what is disclosed below, but rather it can be modified in various forms without changing the gist of the present invention.
[0017] In this specification, when a moiety is referred to as "comprising" an element, it should be understood that the moiety can also include other elements, unless otherwise indicated.
[0018] Furthermore, all numbers and expressions relating to quantities of components, reaction conditions, and the like used herein should be understood as being modified by the term "about," unless otherwise indicated.
[0019] [Secondary battery] A secondary battery according to an embodiment of the present invention includes a positive electrode, a negative electrode, and an electrolyte, the positive electrode including a metal oxide active material, the negative electrode including a silicon-based negative electrode active material, and the negative electrode being pre-doped with lithium in an amount corresponding to an initial irreversible capacity of the negative electrode.
[0020] The secondary battery according to the embodiment of the present invention includes a negative electrode including a silicon-based negative electrode active material pre-doped with lithium in an amount corresponding to the initial irreversible capacity of the negative electrode, thereby significantly increasing the energy density, cycle characteristics and rate characteristics as well as the safety of the secondary battery.
[0021] Generally, silicon-based negative electrode active materials show high capacity, but as cycling proceeds, the volume expansion rate is more than 300%, which may lead to increased resistance and increased side reactions in the liquid electrolyte. Therefore, problems caused by the formation of a solid electrolyte interface (SEI) layer, such as damage to the electrode structure, may be aggravated. Furthermore, silicon oxide-based negative electrode active materials have a volume expansion rate smaller than that of silicon-based negative electrode active materials, while the initial irreversible capacity increases, and is increased by Li2O due to oxygen in the negative electrode active material, but the energy density decreases, and the cycle characteristics and rate characteristics decrease.
[0022] According to an embodiment of the present invention, in order to obtain a secondary battery with high energy density, it is important to make the irreversible capacity of the negative electrode active material as small as possible. Therefore, a negative electrode containing a silicon-based negative electrode active material pre-doped with lithium is adopted in the present invention, which can reduce the initial irreversible capacity of the negative electrode, prevent the metal ions of the positive electrode from penetrating into the SEI of the negative electrode surface, and increase the energy density. Pre-doping compensates for the irreversible capacity, or the lithium required for charging and discharging can be included in the negative electrode even when a lithium-free active material is used in the positive electrode. Therefore, the performance of the secondary battery can be increased.
[0023] According to an embodiment of the present invention, the negative electrode can include a silicon-based negative electrode active material. The silicon-based negative electrode active material can be silicon fine particles, SiO x The inorganic filler may include at least one selected from the group consisting of a compound represented by (0.3≦x≦1.6), silicon dioxide, and a silicate containing magnesium, calcium, aluminum, or a combination thereof.
[0024] Furthermore, the silicon-based negative electrode active material can be an active material that includes a matrix of an oxide capable of absorbing and releasing lithium. The matrix can include silicon oxide, titanium oxide, or a mixture thereof.
[0025] In the negative electrode active material, the content of silicon can be 30% by weight to 80% by weight, specifically 40% by weight to 80% by weight, more specifically 40% by weight to 70% by weight, especially 40% by weight to 60% by weight, based on the total weight of the negative electrode active material. If the content of silicon is less than 30% by weight, the amount of the negative electrode active material acting during the absorption and release of lithium is small, which may reduce the charge and discharge capacity of the secondary battery. On the other hand, if it exceeds 80% by weight, the charge and discharge capacity of the secondary battery can be increased, while the expansion and contraction of the electrode during charge and discharge may be excessively increased, which may reduce the cycle characteristics.
[0026] The silicon particles can be crystalline or amorphous, specifically, amorphous or a similar phase. When the silicon particles are amorphous or a similar phase, the expansion and contraction during charging and discharging of the lithium secondary battery is small, and the battery performance, e.g., capacity characteristics, can be further increased.
[0027] Furthermore, silicon particles are SiO x At least one of the compounds represented by (0.3≦x≦1.6), silicon dioxide, and silicates containing magnesium, calcium, and aluminum, or combinations thereof, or those surrounded by them, can be present in a uniformly dispersed form. In such a case, the expansion or contraction of silicon can be suppressed, thereby increasing the performance of the secondary battery. On the other hand, when a carbon layer including a carbon film is formed on silicon fine particles, they can have a structure dispersed in the silicon oxide compound or silicate as well.
[0028] Furthermore, when the silicon-based negative electrode active material contains silicon particles, it is preferable because it reacts with the silicon particles to form a lithium alloy that is difficult to destroy. During charging, the silicon particles react with lithium to form Li 4。2 Si is formed and during discharge it reverts back to silicon.
[0029] Silicon particles were analyzed by X-ray diffraction (Cu-K) using copper as a cathode target. α ) analysis, and calculated by the Scherrer equation based on the full width at half maximum (FWHM) of the diffraction peak of Si (220) at approximately 2θ = 47.5 °, the crystal size can be 2 nm to 10 nm, specifically, 2 nm to 9 nm, more specifically, 2 nm to 8 nm. If the crystal size of the silicon fine particles exceeds 10 nm, cracks may occur in the negative electrode active material due to volume expansion or contraction during charging and discharging, thereby reducing cycle characteristics. Furthermore, if the crystal size of the silicon fine particles is less than 2 nm, the charge and discharge capacity may decrease, and physical properties may change during storage due to increased reactivity, which may cause problems in processability. If the crystal size of the silicon fine particles is within the above range, there is almost no area that does not contribute to charging and discharging, and it is possible to suppress the decrease in the Coulomb efficiency, which represents the ratio of the charge capacity to the discharge capacity, i.e., the charge and discharge efficiency.
[0030] When the silicon particles are further subdivided into amorphous or crystalline sizes of about 2 to 6 nm, the density of the negative electrode active material increases, so that it can approach the theoretical density, and the pores can be significantly reduced. As a result, the density of the matrix increases, the strength is increased, and cracking is suppressed; therefore, the initial efficiency or cycle life characteristics of the secondary battery can be further increased.
[0031] Furthermore, the negative electrode active material is SiO x (0.3≦x≦1.6) or a silicon oxide compound, for example, silicon dioxide. Specifically, the compound may be SiO x (0.5≦x≦1.6), silicon dioxide, or a mixture thereof. More specifically, it can be SiO x (0.7≦x≦1.2), silicon dioxide, or a mixture thereof. As such, when a silicon oxide compound is used, it can increase the capacity and reduce the volume expansion when applied to a secondary battery.
[0032] The silicon oxide compound may be amorphous when observed by energy dispersive X-ray spectroscopy (EDX) or a transmission electron microscope, or may have a structure in which silicon particles (amorphous) of a few nanometers to a few tens of nanometers are dispersed in the silicon oxide compound.
[0033] The silicon oxide compound can be obtained by a process comprising the steps of cooling and depositing silicon oxide gas produced by heating a mixture of silicon dioxide and submicron silicon powder or silicon particles having a size of 50 nm or less.
[0034] Silicon oxide compounds are amorphous and can undergo irreversible reactions with lithium ions during discharge to form Li-Si-O or Si+Li2O. Therefore, as the content of silicon dioxide in silicon oxide compounds increases, the initial irreversible reactions may increase and the initial efficiency may decrease.
[0035] The silicon oxide compound can be used in an amount of 5 mol% to 20 mol% based on the total negative electrode active material. If the content of the silicon oxide compound is less than 5 mol%, the volume expansion and life characteristics of the secondary battery may be reduced. If it exceeds 20 mol%, the initial irreversible reaction of the secondary battery may be increased.
[0036] According to an embodiment of the present invention, the negative electrode active material may not contain silicon dioxide, because when silicon is intercalated, the production of lithium silicate is inhibited, which can improve the initial efficiency; however, when silicon dioxide is contained, an irreversible reaction occurs when silicon dioxide reacts with lithium, which produces lithium silicate, thereby reducing the initial efficiency.
[0037] Furthermore, the negative electrode active material may include a silicate containing magnesium, calcium, aluminum, or a combination thereof. The magnesium, calcium, aluminum, or a combination thereof may be used in a doped form. Specifically, the negative electrode active material may include a silicate containing magnesium, in which magnesium is used in a doped form.
[0038] According to an embodiment of the present invention, the magnesium-containing silicate may include MgSiO3 crystals, Mg2SiO4 crystals, or a mixture thereof.
[0039] Furthermore, according to one embodiment, the magnesium-containing silicate may include MgSiO3 crystals and may further include Mg2SiO4 crystals.
[0040] In silicates containing magnesium, when magnesium is doped, for example, when SiO and Mg react in a 1:1 ratio, if the elements are distributed uniformly, only Si and MgO are thermodynamically present. However, if the element concentration distribution is non-uniform, not only Si and MgO but also other substances, for example, unreacted SiO and metallic Mg, may be present.
[0041] According to an embodiment of the present invention, the negative electrode active material may include Mg2SiO4 crystals and MgO, but it may substantially include a large amount of MgSiO3 crystals in order to increase the charge / discharge capacity and initial efficiency.
[0042] As used herein, the phrase "substantially comprises a major amount of a component" or "substantially comprises" a component means comprising the component as the main component or comprising primarily the component.
[0043] Specifically, the inclusion of a large amount of MgSiO3 means that the amount of MgSiO3 is greater than the amount of Mg2SiO4 crystals. For example, in an X-ray diffraction analysis, the ratio (IF / IE) of the intensity of the X-ray diffraction peak corresponding to Mg2SiO4 crystals appearing in the range of 2θ=22.3° to 23.3° to the intensity of the X-ray diffraction peak corresponding to MgSiO3 crystals appearing in the range of 2θ=30.5° to 31.5° is 1 or less.
[0044] In silicates, SiO x The magnesium content relative to the total amount of the battery may affect the initial discharge characteristics or cycle characteristics during charging and discharging.
[0045] SiO x The silicon in the MgSiO3 alloy can be alloyed with lithium atoms to significantly increase the initial discharge characteristics. On the other hand, when magnesium silicate of MgSiO3 crystal is used in a substantially large amount, the fineness of silicon particles can be maintained and the strength of the matrix can be further strengthened. Furthermore, the density can be increased, thereby forming a dense matrix. As a result, the increase in initial efficiency or the improvement effect of cycles during charging and discharging can be increased. However, when Mg2SiO4 crystal is used in a large amount, the size of silicon particles can be increased, thereby reducing the strength or density of the matrix, and the alloying of silicon atoms and lithium atoms can be reduced, which may cause a decrease in the initial discharge characteristics of the secondary battery.
[0046] When the negative electrode active material includes a silicate containing magnesium, the chemical reaction between the negative electrode active material and the binder can be suppressed compared to when lithium is doped instead of magnesium. Therefore, the use of such a negative electrode active material can increase the safety of the negative electrode active material composition, which not only improves the safety of the negative electrode but also improves the cycle characteristics of the secondary battery. Furthermore, since the silicate containing magnesium hardly reacts with lithium ions, when it is applied to an electrode, it is understood that when the lithium ions increase rapidly, the expansion / contraction of the electrode is reduced, thereby increasing the cycle characteristics. Furthermore, it is understood that the strength of the matrix, which is the continuous phase surrounding the silicon fine particles, can be increased by the silicate.
[0047] When the negative electrode active material contains silicate containing magnesium, the doping amount, i.e., the content of magnesium, can be 3 wt% to 15 wt%, specifically 4 wt% to 12 wt%, based on the total weight of the negative electrode active material. When the content of magnesium is 3 wt% or more, an increase in the initial efficiency of the secondary battery can be achieved. When it is 15 wt% or less, it can be advantageous in terms of cycle characteristics and handling safety of the secondary battery.
[0048] According to another embodiment of the present invention, when the negative electrode active material includes a silicate containing calcium, aluminum, or a combination thereof, the doping amount, i.e., the content of calcium or aluminum, may be 3 wt % to 15 wt %, specifically 4 wt % to 12 wt %, based on the total weight of the negative electrode active material.
[0049] According to an embodiment of the present invention, the magnesium, calcium, or aluminum containing silicate can be represented by the following Formula 1:
[0050] [Formula 1] M x SiO y
[0051] In formula 1, M is at least one metal selected from the group consisting of Mg, Ca, and Al, and 0.5≦x≦2, and 2.5≦y≦4.
[0052] The silicates of formula 1 are oxides that have thermodynamically more negative Gibbs free energies than silicon oxide compounds, are amorphous, and are stable to lithium, and therefore may help suppress initial irreversible reactions.
[0053] According to an embodiment of the present invention, the silicon-based negative electrode active material can include a carbon layer including a carbon film on a surface thereof, where the carbon layer can include at least one selected from the group consisting of carbon nanofibers, graphene, graphene oxide, and reduced graphene oxide.
[0054] Specifically, a carbon layer, which is flexible in terms of volume expansion due to excellent conductivity, specifically at least one selected from the group consisting of carbon nanofibers, graphene, graphene oxide, and reduced graphene oxide, is coated with a silicon-based negative electrode active material, for example, silicon fine particles, SiO x The carbon layer can be grown directly on the surface of at least one negative electrode active material selected from the group consisting of a compound represented by (0.3≦x≦1.6), silicon dioxide, and a silicate containing magnesium, calcium, aluminum, or a combination thereof. As a result, it is possible to suppress the volume expansion of the negative electrode active material, reduce the phenomenon in which the silicon-based negative electrode active material is pressed, and reduce the reduction in the SEI layer formed by the reaction between the silicon-based negative electrode active material and the electrolyte due to the carbon layer.
[0055] The carbon layer may contain carbon in an amount of 2% by weight to 10% by weight, specifically 4% by weight to 8% by weight, based on the total weight of the negative electrode active material. If the carbon content is less than 2% by weight, the conductivity of the negative electrode may deteriorate. If it exceeds 10% by weight, the carbon content may increase excessively, the capacity of the negative electrode may decrease, and it may be difficult to achieve the desired increase in energy density in the present invention. The method for forming the carbon layer may be a method of chemical vapor deposition (CVD) in organic gas and / or vapor, or a method of introducing organic gas and / or vapor into a reactor during heat treatment.
[0056] Furthermore, the cumulative 50% average particle size (D 50 ) can be 0.5 μm to 15 μm, specifically 2 μm to 10 μm, and more specifically 3 μm to 10 μm or 4 μm to 8 μm. 50 If D is too small, the bulk density becomes too small, which may reduce the charge and discharge capacity per unit volume. 50 If D is too large, it is difficult to prepare the electrode layer of the secondary battery, and there may be a problem that it may peel off from the current collector material. 50 is the weight average value D in particle size distribution measurement by laser beam diffraction method 50 (i.e., the particle size or median size when the cumulative weight is 50%).
[0057] According to an embodiment of the present invention, the carbon layer may have an average thickness of 10 nm to 200 nm, specifically, 20 nm to 200 nm.
[0058] When the average thickness of the carbon layer is 10 nm or more, the conductivity can be increased. When it is 200 nm or less, the decrease in the capacity of the secondary battery can be suppressed. The average thickness of the carbon layer can be measured, for example, by the following procedure.
[0059] First, the negative electrode active material is observed under a transmission electron microscope (TEM) at an arbitrary magnification. The magnification is preferably, for example, such that it can be seen with the naked eye. Next, the thickness of the carbon layer is measured at 15 arbitrary points. In this case, it is preferable to select the measurement positions as widely and randomly as possible without concentrating on a specific area. Finally, the average value of the thickness of the carbon layer at the 15 points is calculated.
[0060] Furthermore, when the silicon-based negative electrode active material according to the embodiment of the present invention is used, the battery capacity per unit weight of the negative electrode active material can be 1,500 to 3,000 mAh / g, and as a result, a secondary battery having high conductivity and improved cycle characteristics with relatively small volume expansion can be provided. Furthermore, when it is used in combination with a carbon-based negative electrode active material, the coulombic efficiency and cycle characteristics can be increased.
[0061] The positive electrode employed in the secondary battery can include a metal oxide active material, which can include oxides having a spinel structure, including, in particular, lithium cobalt oxide, lithium manganate, or mixtures thereof.
[0062] The secondary battery according to the embodiment of the present invention satisfies the following relationship 1, and the lithium metal plate for lithium doping has a thickness (TL) of 10 μm to 30 μm and a density of 0.3 g / cm 3 ~0.8g / cm 3 The density (DA) of the powder may be 0.01 to 0.05.
[0063] [Relationship 1] 0.5<{TA×DA×CA0(100-ICE) / 100} / CLt×(CLa / CLt)}×TL×DL <TL<{TA×DA×CA0(100-ICE) / 100} / CLt×(CLa / CLt)×DL
[0064] In relation 1, TA: Thickness of negative electrode (μm) DA: Density of negative electrode (g / cm 3 ) ICE: Initial efficiency (%) CA0: first charge capacity of the negative electrode (mAh / g) CLt: Theoretical capacity of lithium (3,600mAh / g) CLa: Lithium actual capacity (mAh / g) TL: Thickness of lithium metal plate (μm) DL: Density of lithium metal plate (0.53 g / cm 3 )
[0065] Furthermore, the thickness of the lithium metal plate can be specifically 15 μm to 25 μm. When considering the pre-doping speed, a lithium metal plate having a large surface area is preferable. When considering the ease of handling, productivity, and the environment of the pre-doping process of the lithium metal plate, a lithium metal plate having a small surface area may be preferable. When the thickness of the lithium metal plate satisfies the above range, it may be preferable in terms of suppression of lithium residue, pre-doping speed, and productivity.
[0066] [Method for manufacturing a secondary battery]
[0067] A method for manufacturing a secondary battery according to an embodiment of the present invention may include the steps of: (1-1) applying a negative electrode active material composition including a silicon-based negative electrode active material to a negative electrode current collector to prepare a negative electrode; (1-2) placing a separator between the negative electrode and a lithium metal plate to prepare a cell; (1-3) electrochemically activating the cell obtained in step (1-2) to pre-dope the negative electrode with lithium; and (1-4) manufacturing a secondary battery using the negative electrode pre-doped with lithium.
[0068] Step (1-1) may include a step of applying a negative electrode active material composition containing a silicon-based negative electrode active material to a negative electrode current collector, and a step of rolling and drying the same, and may be carried out by a commonly used method.
[0069] Specifically, the negative electrode is prepared by applying a negative electrode active material composition, in which a negative electrode active material, a conductive material, and a binder are mixed, to a negative electrode current collector, and then drying the same. The negative electrode can be prepared by a method commonly used in the art. For example, a negative electrode active material composition (slurry) can be prepared by mixing and stirring a binder, a solvent, and optionally a conductive material and a dispersant with the negative electrode active material according to an embodiment of the present invention, which can be applied to a current collector, rolled up, and dried to prepare a negative electrode.
[0070] The silicon-based negative electrode active material can be used as a negative electrode active material.
[0071] In the method for manufacturing a secondary battery according to an embodiment of the present invention, the silicon-based negative electrode active material can be obtained by the steps of: mixing silicon powder and silicon dioxide powder to obtain a silicon-silicon oxide raw powder mixture; heating and depositing the raw powder mixture to obtain a silicon oxide composite material; and pulverizing and classifying the silicon oxide composite material to obtain the silicon-based negative electrode active material.
[0072] Specifically, in a method for preparing a silicon-based negative electrode active material, a first step can include mixing silicon powder and silicon dioxide powder to obtain a silicon-silicon oxide raw powder mixture.
[0073] When silicon powder and silicon dioxide powder are mixed, the mixing molar ratio of silicon dioxide powder to silicon powder, ie, the molar ratio of silicon dioxide powder / silicon powder, is greater than 0.9 and smaller than 1.1, specifically, 1.01 to 1.08.
[0074] In the method for preparing a silicon-based negative electrode active material, the second step can include heating and evaporating the raw material powder mixture to obtain a silicon oxide composite material.
[0075] The heating and deposition of the raw material powder mixture in the second step can be carried out at 500°C to 1,600°C, specifically, 600°C to 1,500°C. If the heating and deposition temperature is lower than 500°C, it may be difficult to carry out the reaction, thereby reducing the productivity. If it is higher than 1,600°C, the raw material powder mixture may melt, thereby reducing the reactivity.
[0076] In the method for preparing the silicon-based negative electrode active material, the third step can include grinding and classifying the silicon oxide composite material to obtain the silicon-based negative electrode active material.
[0077] The grinding is carried out to obtain a mean particle size (D 50 The negative electrode active material having the above-mentioned particle diameter can be obtained by crushing and classifying the negative electrode active material having the above-mentioned particle diameter. The crushing can be performed using a commonly used crusher or sieve.
[0078] Furthermore, according to an embodiment of the present invention, the method may further include a step of cooling the silicon oxide composite material between the second step and the third step.
[0079] The cooling can be performed at room temperature while injecting an inert gas, which can be at least one selected from carbon dioxide gas, argon (Ar), water vapor (H2O), helium (He), nitrogen (N2), and hydrogen (H2).
[0080] Meanwhile, according to an embodiment of the present invention, the method may further include a step of forming a carbon layer including a carbon film on a surface of the negative active material by using a chemical pyrolysis deposition method after the grinding and classification of the third step.
[0081] In the chemical pyrolysis deposition method, a carbon layer including a carbon film can be formed on the surface of a negative electrode active material by adding at least one carbon source gas selected from a compound represented by the following formula 2; a compound represented by the following formula 3; a compound represented by the following formula 4; and at least one hydrocarbon selected from acetylene, benzene, toluene, and xylene thereto, and carrying out the reaction in a gas phase state at 600°C to 1,200°C.
[0082] [Formula 2] C n H (2n+2-A) [OH] A In formula 2, n is an integer of 1 to 20, and A is 0 or 1.
[0083] [Formula 3] C m H 2m In formula 3, m is an integer from 2 to 6,
[0084] [Formula 4] C x H y O z In formula 4, x is an integer from 1 to 20, y is an integer from 0 to 20, and z is 1 or 2.
[0085] The compound represented by formula 2 can include, for example, at least one selected from methane (CH4), ethane (C2H6), propane (C3H8), methanol (CH3OH), ethanol (C2H5OH), and propanol (C3H8O). The compound represented by formula 3 can include ,workman The compound represented by formula 4 may include at least one selected from the group consisting of ethylene (C2H4), and propylene (C3H6). On the other hand, the compound represented by formula 4 is an oxygen-containing gas, and may include at least one selected from the group consisting of carbon monoxide (CO) and carbon dioxide (CO2).
[0086] Furthermore, when the carbon layer is formed, an inert gas including at least one selected from carbon dioxide gas, argon (Ar), water vapor (H2O), helium (He), nitrogen (N2), and hydrogen (H2) can be injected. According to one embodiment, when water vapor is included when the carbon layer is formed, the negative electrode active material can exhibit higher electrical conductivity. Specifically, when water vapor is included when the carbon layer is formed, a highly crystalline carbon film can be formed on the surface of the negative electrode active material by reaction with the gas mixture, and can exhibit high electrical conductivity even when a smaller amount of carbon is coated. The content of water vapor in the gas mixture is not particularly limited. For example, it can be 0.01% by volume to 10% by volume based on 100% by volume of the total carbon source gas.
[0087] According to one embodiment, when the carbon layer is formed, a mixed gas of CH4 and CO2 or a mixed gas of CH4, CO2, and H2O can be used as the carbon source gas. When a mixed gas of CH4 and CO2 is used, the molar ratio of CH4:CO2 can be about 1:0.20-0.50, specifically about 1:0.25-0.45, more specifically about 1:0.30-0.40. When a mixed gas of CH4, CO, and H2O is used, the molar ratio of CH4:CO2:H2O can be about 1:0.20-0.50:0.01-1.45, specifically about 1:0.25-0.45:0.10-1.35, more specifically about 1:0.30-0.40:0.50-1.0.
[0088] According to another embodiment, when the carbon layer is formed, CO, CO2, or a combination thereof can be used as the carbon source gas.
[0089] According to another embodiment, when the carbon layer is formed, a carbon source gas containing CH4 and N2 as an inert gas can be used. The molar ratio of CH4 and N2 in the mixed gas can be about 1:0.20-0.50, specifically about 1:0.25-0.45, more specifically about 1:0.30-0.40.
[0090] According to one embodiment, no inert gas may be included.
[0091] Additionally, during the reaction, the heat treatment temperature, the composition of the gas mixture, etc. can be selected in view of the desired amount of carbon film.
[0092] When the carbon layer is formed, the heat treatment temperature can be 600°C to 1,200°C, specifically 700°C to 1,100°C, and more specifically 700°C to 1,000°C.
[0093] Furthermore, the pressure during the heat treatment can be controlled by adjusting the amount of the gas mixture introduced. For example, the pressure during the heat treatment can be 1 atm or more, for example, but is not limited to, 1 atm to 5 atm.
[0094] Furthermore, the heat treatment time is not limited, but it can be appropriately adjusted according to the heat treatment temperature, the pressure during the heat treatment, the composition of the gas mixture, and the desired amount of carbon coating. For example, the heat treatment time can be 10 minutes to 100 hours, specifically 30 minutes to 90 hours, more specifically 50 minutes to 40 hours. According to one embodiment, as the heat treatment time increases, the thickness of the carbon film formed can increase. When the thickness is adjusted to a moderate degree, the electrical properties of the negative electrode active material can be increased.
[0095] According to an embodiment of the present invention, the carbon film is preferably formed uniformly and thinly over the entire surface of the negative electrode active material, and it is preferable that a substantially large amount of carbon nanofibers, graphene, graphene oxide, or reduced graphene oxide is formed as the carbon film.
[0096] Furthermore, a carbon layer containing a uniform carbon film can be formed on the surface of the negative electrode active material through the gas phase reaction of the carbon source gas even at a relatively low temperature. In the negative electrode active material, the carbon film thus formed does not easily peel off. Furthermore, a carbon film having high crystallinity can be formed through the gas phase reaction; therefore, when it is used as the negative electrode active material, the electrical conductivity of the negative electrode active material can be increased without changing the structure.
[0097] The carbon layer can include at least one selected from the group consisting of carbon nanofibers, graphene, graphene oxide, and reduced graphene oxide.
[0098] The structure of the carbon layer can be a layer, a nanosheet type, or a structure mixed with several flakes.
[0099] The layer may refer to the form of a film in which graphene is continuously and uniformly formed on the surface of at least one selected from silicon particles, silicon oxide compounds, magnesium silicate, and reduction products thereof.
[0100] Furthermore, the nanosheets may be made of carbon nanofibers or graphene-containing materials, silicon particles, SiO x (0.3≦x≦1.6), silicon dioxide, and silicates containing magnesium, calcium, aluminum, or a combination thereof.
[0101] Additionally, flakes can refer to when a portion of the nanosheet or membrane is damaged or deformed.
[0102] After the carbon layer is formed, the method may further include crushing and classifying. The average particle size (D 50The average particle diameter (D) of the negative electrode active material on which the carbon layer is formed can be 0.5 μm to 15 μm, specifically, 2 μm to 10 μm, and more specifically, 3 μm to 10 μm or 4 μm to 8 μm. 50 ) is 0.5 μm, the bulk density is too small and the charge and discharge capacity per unit volume may decrease. 50 If the average particle size (D) exceeds 15 μm, it is difficult to prepare the electrode layer, and as a result, it may peel off from the current collector material. 50 ) is the weighted average value D 50 That is, it is the value measured as the particle size or median diameter when the cumulative weight is 50% in particle size distribution measurement by laser beam diffraction method.
[0103] The average particle size (D 50 ) can be achieved by the above-mentioned grinding. Furthermore, the average particle size (D 50 After grinding to 0.1 mm, classification can be carried out to achieve particle size distribution, for which dry classification, wet classification, or filtration can be used. In dry classification, the processes of dispersion, separation (separation of fine particles and defective particles), accumulation (separation of solids and gases), and discharge are carried out successively or simultaneously using airflow, and pretreatment (adjustment of moisture, dispersibility, humidity, etc.) can be carried out prior to classification in order not to reduce the classification efficiency due to interference between particles, particle shape, airflow disturbance, velocity distribution, and static electricity effects, etc., thereby adjusting the moisture or oxygen concentration in the airflow used. Furthermore, the desired particle size distribution can be obtained by carrying out grinding and classification at once.
[0104] When a negative electrode active material having an average particle size is achieved by the grinding and classification process, the initial efficiency of the cycle characteristics can be increased by about 10% to 20% compared to before classification. max In such a case, the specific surface area of the negative electrode active material may be reduced; as a result, the lithium that is accommodated in the SEI layer may be reduced.
[0105] Furthermore, the negative electrode active material is 2m 2 / g~20m 2 / g. The specific surface area of the negative electrode active material may be 2 m 2 If it is less than 20m / g, the rate characteristics of the secondary battery may be deteriorated. 2 If the surface area exceeds 3 m / g, the contact area with the electrolyte increases, which may cause problems such as accelerating the decomposition reaction of the electrolyte or causing side reactions in the battery. 2 / g~15m 2 / g, more specifically, 3m 2 / g~10m 2 / g. The specific surface area can be measured by BET using nitrogen adsorption. For example, a specific surface area measuring device commonly used in the art (Macsorb HM (model 1210) of MOUNTECH, Belsorp-mini II of MicrotracBEL, etc.) can be used.
[0106] The negative electrode active material is 1.8 g / cm 3 ~3.2g / cm 3 , specifically, 2.5 g / cm 3 ~3.2g / cm 3 As the specific gravity increases, the number of pores in the negative electrode active material decreases, which can increase the conductivity and the strength of the matrix increases, which can increase the initial efficiency or cycle life characteristics. In this specification, specific gravity can refer to true specific gravity, density, or true density. For measuring specific gravity, for example, measuring specific gravity by a dry density meter, Acupick II 1340 manufactured by Shimadzu Corporation can be used as a dry density meter. The purge gas used can be helium gas, and the measurement can be performed after 200 purges in a sample holder set at a temperature of 23 ° C.
[0107] According to an embodiment of the present invention, in the case of a negative electrode active material including a carbon layer, particularly a carbon layer having excellent flexibility in conductivity and volume expansion, particularly a carbon nanofiber or graphene-containing material, the carbon layer grows directly on the negative electrode active material, thereby suppressing volume expansion and reducing the phenomenon in which silicon particles, silicon oxide compounds, or silicates are pressed and contracted. Furthermore, since the direct reaction between the silicon contained in the negative electrode active material and the electrolyte can be controlled by the carbon nanofiber or graphene, it is possible to reduce the formation of an SEI layer of the electrode. When the negative electrode active material including the carbon layer is used, even if a binder is not used in the preparation of the negative electrode active material composition, it is possible to suppress structural collapse due to the volume expansion of silicon particles, silicon oxide compounds, and silicates, and to minimize the increase in resistance, and thus it can be advantageously used in the manufacture of an electrode and a lithium secondary battery having excellent electrical conductivity and capacity characteristics.
[0108] Furthermore, according to an embodiment of the present invention, the negative electrode active material may further include a carbon-based negative electrode material.
[0109] Specifically, the negative electrode active material can be used as a mixture of a silicon-based negative electrode active material and a carbon-based negative electrode material. In such a case, the electrical resistance of the negative electrode active material can be reduced, and the expansion stress involved in charging can be simultaneously alleviated. The carbon-based negative electrode material can include at least one selected from the group consisting of natural graphite, synthetic graphite, soft carbon, hard carbon, mesocarbon, carbon fiber, carbon nanotube, pyrolytic carbon, coke, glass carbon fiber, sintered organic polymer compound, and carbon black.
[0110] The content of the carbon-based negative electrode material, for example, the graphite-based negative electrode material, can be 30% by weight to 95% by weight, specifically 30% by weight to 90% by weight, more specifically 50% by weight to 80% by weight, based on the total weight of the negative electrode active material. In particular, when the negative electrode active material contains silicon fine particles, the silicon fine particles do not cause volume expansion; therefore, a secondary battery with excellent cycle characteristics can be obtained when the carbon-based negative electrode material is mixed for use.
[0111] The binder is not particularly limited. For example, it can be at least one selected from the group consisting of fluorine-based resins, such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HEP), polyvinylidene fluoride, polytetrafluoroethylene; rubber-based materials, such as fluorine rubber and styrene-butylene rubber (SBR); polyolefins, such as polyethylene and polypropylene; acrylic resins; and polyimide-based resins. Since silicon-based negative electrode active materials have a large volume change during charging and discharging, materials with excellent adhesive properties may be more preferable. For example, it can include polyimide-based resins, including polyimide, polyamide-imide, or mixtures thereof. Furthermore, when the negative electrode is prepared, the amount of mixing with the binder can be determined in consideration of the type, particle size, shape, and mixing of the composition of the negative electrode active material of the present invention. By appropriately mixing in consideration of the strength and adhesiveness of the negative electrode, good cycle characteristics of the secondary battery can be obtained.
[0112] Conductive material is not particularly limited as long as it has conductivity without undergoing chemical change in battery.For example, it can be graphite, such as natural graphite and synthetic graphite; carbon black, such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fiber, such as carbon fiber and metal fiber; metal powder, such as fluorocarbon, aluminum, and nickel powder; conductive whisker, such as zinc oxide and potassium titanate; conductive metal oxide, such as titanium oxide; conductive material, such as polyphenylene derivative.
[0113] The dispersant can be an aqueous dispersant or an organic dispersant, for example, N-methyl-2-pyrrolidone.
[0114] The negative electrode current collector is not particularly limited. Examples include copper foil, stainless steel foil, and titanium foil. In addition, a surface embossed current collector or a porous current collector, such as expanded metal, meshed or perforated metal, can be used.
[0115] Furthermore, the method for manufacturing a secondary battery can include a step (1-2) of preparing a cell by placing a separator between the negative electrode and a lithium metal plate.
[0116] The lithium metal plate can have a thickness of 10 μm to 30 μm, specifically, 15 μm to 25 μm. When considering the pre-doping speed, a lithium metal plate having a large surface area is preferable. When considering the ease of handling the lithium metal plate, productivity, and the environment of the pre-doping process, a lithium metal plate having a small surface area is preferable. When the thickness of the lithium metal plate satisfies the above range, it can be preferable in terms of suppressing lithium residue, pre-doping speed, and productivity. Furthermore, the lithium metal plate has a density of 0.3 g / cm 3 ~0.8g / cm 3 The density of the powder may be 0.01 to 0.01.
[0117] On the other hand, the separator may be a conventional porous polymer film used as a conventional separator, for example, a porous polymer film prepared from a polyolefin-based polymer, for example, an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, which may be used alone or in a laminate. In addition, an insulating thin film having high ion permeability and mechanical strength may be used. The separator may include a safety-enhanced separator (SRS), in which a ceramic material is thinly coated on the surface of the separator.
[0118] Furthermore, a conventional porous nonwoven fabric can be used, for example, a nonwoven fabric made of high melting point glass fiber, polyethylene terephthalate fiber, etc., but is not limited thereto. The separator can have a thickness of 10 μm to 30 μm, specifically, 15 μm to 25 μm.
[0119] The method for producing the secondary battery may include a step (1-3) of electrochemically activating the cell obtained in step (1-2) to pre-dope the negative electrode with lithium.
[0120] In this specification, pre-doping refers to doping of lithium by absorbing and supporting lithium in the negative electrode prior to normal charging and discharging between the positive and negative electrodes.
[0121] In order to obtain a secondary battery with high energy density as desired in the present invention, it is important to make the irreversible capacity of the negative electrode active material as small as possible. Since it is theoretically impossible to reduce it below a certain level, high energy density can be increased by pre-doping the negative electrode with lithium. Pre-doping compensates for irreversible capacity, or the lithium required for charging and discharging can be included in the negative electrode even when a lithium-free active material is used in the positive electrode.
[0122] As a pre-doping method according to an embodiment of the present invention, a method of pre-doping lithium onto a negative electrode active material can be used, in which a lithium metal plate adopted as a counter electrode is electrochemically activated in an electrolyte solution used in a secondary battery. The pre-doping can include a step of pre-doping the negative electrode with lithium in an amount corresponding to the initial irreversible capacity of the negative electrode by electrochemically causing the adsorption and desorption of lithium during contacting the negative electrode and the lithium metal plate. Specifically, once a lithium metal plate as a negative electrode and a counter electrode are adopted, and a separator is placed between the negative electrode and the lithium metal plate to prepare a cell, it is electrochemically activated in a liquid electrolyte to pre-dope the negative electrode with an amount of lithium corresponding to the first irreversible capacity. The liquid electrolyte can include a non-aqueous electrolyte, a polymer electrolyte, or a polymer gel electrolyte.
[0123] Furthermore, electrochemical activation can be performed by charging and discharging the cell, for example, but not limited to, after the voltage reaches 0.005 V at a constant current of 0.1 C, charging is performed at a constant voltage of 0.005 C, and discharging is performed at a constant current of 0.1 C until the voltage reaches 1.5 V.
[0124] As described above, since the separator is placed between the negative electrode and the lithium metal plate in the liquid electrolyte, the negative electrode and the lithium metal plate are not in direct contact with each other, but are pre-doped with lithium through the electrochemical contact between the negative electrode and the lithium metal plate; therefore, it is possible to solve the problem that needle-like crystals (dendrites) formed by directly attaching or depositing the lithium metal plate on the negative electrode adversely affect the separator. As a result, the safety of the secondary battery can be guaranteed.
[0125] Furthermore, the pre-doping method according to another embodiment of the present invention can be a method in which excess lithium (the amount of irreversible capacity remaining in the negative electrode) after doping is also removed by de-doping. The pre-doping process includes the steps of doping the negative electrode with lithium in an amount equivalent to the initial irreversible capacity of the negative electrode by causing lithium adsorption and desorption while the negative electrode and the lithium metal plate are in electrochemical contact to dope lithium; and releasing (de-doping) an amount of lithium other than the amount of the initial irreversible capacity of the negative electrode.
[0126] Specifically, once lithium metal plates as negative and counter electrodes are employed, a separator is sandwiched between the negative and lithium metal plates, and a cell is prepared, it is electrochemically activated in a liquid electrolyte, for example, a non-aqueous liquid electrolyte, to pre-dope the negative electrode with an amount of lithium corresponding to the first irreversible capacity; and release (de-doping) an amount of lithium other than the amount of initial irreversible capacity of the negative electrode. When the negative electrode is pre-doped with an amount of lithium corresponding to the irreversible capacity, particularly when pre-doped by de-doping, it is possible to achieve an initial efficiency close to 100%. As a result, the capacity ratio of the negative electrode / positive electrode (N / P ratio) can approach 1.0, and the capacity of the secondary battery itself can be increased. Furthermore, although a large exothermic reaction may be involved during pre-doping with lithium, the current during doping with lithium can be controlled, thereby controlling its rate, which may be a great advantage in terms of safety.
[0127] Therefore, according to the present invention, since the negative electrode is doped and de-doped with lithium by electrochemical doping or pre-doping method, it is possible to pre-dope the negative electrode with lithium in an amount corresponding to the irreversible capacity. As a result, the volume expansion of the negative electrode involved in the absorption and release of lithium can be reduced. Furthermore, since the doping rate can be controlled by controlling the current, the safety of doping can also be ensured by suppressing the generation of large amounts of heat. In particular, when doping is performed in large quantities, the temperature can be controlled, so that the method can be advantageous for mass production.
[0128] Lithium salts commonly used as electrolytes for lithium secondary batteries can be used as electrolytes in the present invention without limitation. For example, the anion of the lithium salt is F - , Cl - , Br - , I - , NO 3- , N(CN) 2- , B.F. 4- , ClO4 - , P.F. 6- , (CF3)2PF 4- , (CF3)3PF 3- , (CF3)4PF 2- , (CF3)5PF - , (CF3)6P - , CF3SO 3- , CF3CF2SO 3- , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO 3- , CF3CO 2- , CHCO 2- , SCN-, and (CF3CF2SO2)2N - It can be any one selected from the group consisting of:
[0129] Organic solvents that are commonly used in liquid electrolytes for lithium secondary batteries can be used in the liquid electrolyte of the present invention without any restrictions. As a representative example, any one or a mixture of two or more selected from the group consisting of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, dipropyl carbonate, dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylidene carbonate, sulfolane, gamma-butyrolactone, propylene sulfite, methyl acetate, methyl formate, and tetrahydrofuran can be commonly used. The concentration of the liquid electrolyte is not particularly limited, but can be, for example, 0.5 to 2 mol / L. It is preferable that the liquid electrolyte has a water content of 100 ppm or less. Meanwhile, the term "non-aqueous liquid electrolyte" used in this specification refers to a concept that extends not only to non-aqueous liquid electrolytes and organic liquid electrolytes, but also to gel-like and solid electrolytes.
[0130] In the secondary battery including the lithium pre-doped negative electrode and the silicon-based negative electrode active material according to the embodiment of the present invention, the energy density can be significantly increased, and the cycle characteristics and rate characteristics can be improved. In particular, the initial discharge capacity and capacity retention of the secondary battery can be further increased.
[0131] The method for producing a secondary battery can include the step (1-4) of producing a secondary battery using a negative electrode pre-doped with lithium.
[0132] Specifically, upon electrochemical activation in step (1-3), the cell is separated to produce a secondary battery using a negative electrode pre-doped with lithium, a positive electrode including a positive electrode active material, and a separator.
[0133] When the secondary battery is manufactured, the positive electrode active material used in the positive electrode is not particularly limited as long as it is a material that can electrochemically absorb and release lithium.For example, it can include a metal oxide active material containing lithium that can be electrochemically released.Specifically, it can include an oxide having a spinel structure, including lithium cobalt oxide, lithium manganate, or a mixture thereof.
[0134] Furthermore, the positive electrode active material may include at least one selected from the group consisting of lithium complex cobalt oxide, lithium complex nickel oxide, lithium complex manganese oxide, and lithium complex titanium oxide. An active material in which at least one different metal element is added to a complex oxide may be used. Furthermore, at least one selected from the group consisting of at least one metal oxide selected from the group consisting of manganese, vanadium, and iron, a disulfide-based compound, a polyacene-based compound, and activated carbon may be used as those that do not contain electrochemically releasable lithium.
[0135] Furthermore, as the separator, a separator that is commonly used can be used, and the separator described in step (1-2) can be used.
[0136] A method for manufacturing a secondary battery according to another embodiment includes the steps of: (2-1) applying an anode active material composition including a silicon-based anode active material to an anode current collector to prepare an anode; (2-2) placing the anode and a lithium metal plate in a reactor and performing an oxidation-reduction reaction to pre-dope the anode with lithium; and (2-3) successively stacking the anode pre-doped with lithium, a separator, and a cathode including a metal oxide active material to prepare an electrode.
[0137] Step (2-1) is a step of preparing a negative electrode by applying a negative electrode active material composition containing a silicon-based negative electrode active material to a negative electrode current collector. Furthermore, step (2-1) can further include a step of rolling and drying the negative electrode current collector after applying the negative electrode active material composition to the negative electrode current collector, which can be performed by a commonly used method.
[0138] In the method for preparing a secondary battery according to an embodiment of the present invention, the method for preparing the silicon-based negative electrode active material is as described above.
[0139] Further, step (2-2) is a step of placing a negative electrode and a lithium metal plate in a reactor to carry out an oxidation-reduction reaction to pre-dope the negative electrode with lithium.
[0140] Specifically, referring to FIG. 1, once the negative electrode (10) prepared in step (2-1) and the lithium metal plate (30) are placed in a reactor, an oxidation-reduction reaction can be carried out. In such a case, the oxidation-reduction reaction can be carried out in a liquid electrolyte (20). The liquid electrolyte (20) can include a non-aqueous electrolyte, a polymer electrolyte, or a polymer gel electrolyte. The oxidation-reduction reaction is carried out, for example, by doping the negative electrode with lithium in the non-aqueous liquid electrolyte together with the lithium metal plate via a reduction reaction at 0.0003-0.001 V, and carrying out an oxidation reaction until 1.0-2.0 V for dedoping.
[0141] The lithium metal plate can have a thickness of 10 μm to 30 μm, specifically, 15 μm to 25 μm. When considering the pre-doping speed, a lithium metal plate having a large surface area is preferable. When considering the ease of handling, productivity, and the environment of the pre-doping process of the lithium metal plate, a lithium metal plate having a small surface area may be preferable. When the thickness of the lithium metal plate satisfies the above range, it may be preferable in terms of suppression of lithium residue, pre-doping speed, and productivity. Furthermore, the lithium metal plate has a density of 0.3 g / cm 3 ~0.8g / cm 3 The density of the powder may be 0.01 to 0.01.
[0142] The negative electrode can be pre-doped with lithium by a redox reaction.
[0143] According to an embodiment of the present invention, in order to obtain a secondary battery with high energy density, it is important that the irreversible capacity of the negative electrode active material is as small as possible. Therefore, the negative electrode containing the silicon-based negative electrode active material is pre-doped with lithium in the present invention, which can reduce the initial irreversible capacity of the negative electrode, prevent the metal ions of the positive electrode from penetrating into the SEI of the negative electrode surface, and increase the energy density. Pre-doping compensates for the irreversible capacity, or even when a lithium-free active material is used in the positive electrode, the lithium required for charging and discharging can be included in the negative electrode. Therefore, the performance of the secondary battery can be increased.
[0144] As a pre-doping method according to an embodiment of the present invention, a method of doping the negative electrode with lithium in an amount corresponding to the irreversible capacity can be used, in which a redox reaction using a lithium metal plate as a counter electrode is carried out in the liquid electrolyte used in the secondary battery.
[0145] As described above, the negative electrode 10 and the lithium metal plate 30 are placed in the liquid electrolyte 20, and an oxidation-reduction reaction is carried out, thereby ensuring the safety of the secondary battery compared to a method in which a lithium metal plate is directly attached or vapor-deposited on the negative electrode. In the method in which a lithium metal plate is directly attached or vapor-deposited on the negative electrode, needle-like crystals (dendrites) formed by directly attaching or vapor-depositing a lithium metal plate on the negative electrode may adversely affect the separator, thereby compromising safety.
[0146] Furthermore, the pre-doping method according to another embodiment of the present invention can be a method in which excess lithium (remaining in the amount of irreversible capacity in the negative electrode) is removed by de-doping of lithium after doping. Pre-doping can include a method in which once the negative electrode is pre-doped with lithium through a reduction reaction, the amount of lithium other than the initial irreversible capacity is removed by releasing (de-doping) lithium through an oxidation reaction. For example, the redox reaction can be carried out in a non-aqueous liquid electrolyte, the negative electrode can be doped with lithium in an amount corresponding to the initial irreversible capacity, and the amount of lithium other than the amount of the initial irreversible capacity can be released (de-doped). When the negative electrode is pre-doped with an amount of lithium corresponding to the irreversible capacity by the pre-doping method, it is possible to achieve an initial efficiency close to 100% by de-doping in particular. As a result, the capacity ratio of the negative electrode / positive electrode (N / P ratio) can approach 1.0, which can increase the capacity of the secondary battery itself. Furthermore, although an exothermic reaction may be involved during pre-doping with lithium, the current during doping with lithium can be controlled, thereby controlling its rate, which may be a great advantage in terms of safety.
[0147] Therefore, according to the present invention, since the negative electrode is doped with lithium or doped and de-doped through an oxidation-reduction reaction by the pre-doping method, it is possible to pre-dope the negative electrode with lithium in an amount corresponding to the irreversible capacity of lithium. As a result, it is possible to reduce the volume expansion of the negative electrode involved in the absorption and release of lithium. Furthermore, since the doping rate can be controlled by controlling the current, the safety of doping can also be ensured by suppressing the generation of large amounts of heat. In particular, when large amounts of doping are performed, the temperature can be controlled, so the method can be advantageous for mass production.
[0148] Furthermore, in the step (2-2), after pre-doping, an oxidation-reduction reaction can be carried out one or more times to remove lithium doped in an excess amount in the negative electrode.
[0149] The lithium salt and organic solvent that can be used as the electrolyte in the present invention are as described above.
[0150] In a secondary battery including a silicon-based negative electrode active material pre-doped with lithium according to an embodiment of the present invention, its energy density can be significantly increased, and its cycle characteristics and rate characteristics can be further improved.
[0151] Step (2-3) is a step of preparing an electrode by successively stacking a negative electrode pre-doped with lithium, a separator, and a positive electrode containing a metal oxide active material.
[0152] When a secondary battery is manufactured, the positive electrode and separator, and the secondary battery manufacturing process are as described above.
[0153] The shape and size of the secondary battery of the present invention are not particularly limited, but it may include a cylindrical type, a square type, a pouch type, a film type, or a coin type according to each application.
[0154] The secondary battery according to the embodiment includes a negative electrode including a silicon-based negative electrode active material pre-doped with lithium, which not only achieves the safety of the secondary battery, but also significantly increases the energy density and improves the cycle characteristics and rate characteristics.
[0155] EMBODIMENTS FOR CARRYING OUT THEINVENTION
[0156] The present invention will be described in more detail with reference to the following examples, however, these examples are provided to illustrate the present invention and the scope of the examples is not limited thereto.
[0157] Example 1-1
[0158] A carbon layer including a carbon film was provided, and a silicon-based negative electrode active material (manufactured by DAEJOO) having the following physical properties, Super-P (TIMCAL) as a conductive material, and polyacrylic acid (PAA, Sigma-Aldrich) as a binder were mixed in a weight ratio of 80:10:10 to prepare a negative electrode active material composition.
[0159] SiO x , x=1.0 Carbon content: 5.1% by weight Average particle size of the negative electrode active material (D 50 ): 5.3μm
[0160] The negative electrode active material composition was applied to a copper foil having a thickness of 18 μm and dried to a thickness of 40 μm and a mass of 1.35 g / cm 3 The negative electrode was punched out into a circular shape having a diameter of 14 mm, and dried under vacuum at 80° C. for 12 hours to obtain a negative electrode (step 1-1).
[0161] On the other hand, a porous polypropylene sheet (25 μm) was placed as a separator in a glove box, and the negative electrode and a lithium metal plate having a thickness of 20 μm were placed thereon to prepare a cell (Step 1-2).
[0162] The cell obtained in step 1-2 was placed in a reactor, and a lithium non-aqueous liquid electrolyte, containing 1MLiPF6 in a mixed solvent of ethylene carbonate (EC) and diethylene carbonate (DEC) at a volume ratio of 1:1, was used to charge at a constant current of 0.1C until the voltage reached 0.005V, and then discharge at a constant current of 0.1C until the voltage reached 1.5V, to pre-do the negative electrode with lithium via electrochemical activation (step 1-3).
[0163] The cells were separated, and a secondary battery was prepared using the lithium pre-doped negative electrode (steps 1-4). Specifically, the negative electrode, separator, and positive electrode were stacked in this order in a glove box, and the same non-aqueous liquid electrolyte was used to prepare a lithium secondary battery. The positive electrode active material used in the positive electrode was LiCoO2, 20 μm aluminum foil was used as the current collector, and a porous polypropylene sheet (25 μm) was used as the separator.
[0164] Example 1-2
[0165] The negative electrode (40 μm thick and 1.5 g / cm) was fabricated using the same silicon-based negative electrode active material as in Example 1-1 and a carbon-based negative electrode material made of natural graphite (average particle size: 11 μm) mixed in a weight ratio of 50:50. 3 The density) and secondary battery were prepared in the same manner as in Example 1-1.
[0166] Examples 1-3
[0167] The negative electrode and secondary battery are made of silicon-based negative electrode active material (SiO x , x=1.0, particle size of negative electrode active material (D 50 The preparation was carried out in the same manner as in Example 1-1, except that a 5.6 μm SiO 2 : ...
[0168] Example 2-1
[0169] <Preparation of negative electrode>
[0170] A silicon-based negative electrode active material (manufactured by DAEJOO) having the following physical properties and provided with a carbon layer, Super-P (TIMCAL) as a conductive material, and polyacrylic acid (PAA, Sigma-Aldrich) as a binder were mixed in a weight ratio of 80:10:10 to prepare a negative electrode active material composition.
[0171] SiO x , x=1.0 Carbon content: 5.1% by weight Average particle size of the negative electrode active material (D 50 ): 5.3μm
[0172] The negative electrode active material composition was applied to a copper foil having a thickness of 18 μm, dried and rolled to a thickness of 40 μm and a thickness of 1.35 g / cm 3 A negative electrode having a density of 1000 g / cm2 was prepared.
[0173] The negative electrode was pre-doped with lithium via reduction reaction with a 20 μm lithium metal plate at 0.0005 V in a lithium non-aqueous liquid electrolyte containing 1 M LiPF6 in a mixed solvent of ethylene carbonate (EC) and diethylene carbonate (DEC) in a 1:1 volume ratio, de-doped via oxidation reaction up to 1.5 V, and dried via electrochemical activation to obtain a lithium pre-doped negative electrode.
[0174] <Preparation of positive electrode>
[0175] LiNi as the positive electrode active material 0.8 Co 0.2 A positive electrode active material composition (slurry) was prepared using O2, Super-P as a conductive material, and polyvinylidene fluoride (PVdF, Solvay) as a binder. The positive electrode active material composition was coated on a 15 μm aluminum foil, dried, and rolled to obtain a positive electrode.
[0176] <Secondary battery manufacturing>
[0177] A porous polypropylene sheet separator (25 μm) was placed between the lithium pre-doped negative and positive electrodes and rolled up to prepare a jelly roll, which was then placed in a cylindrical can, sealed, and a liquid electrolyte, containing 1 M LiPF6 in a mixed solvent of ethylene carbonate (EC) and diethylene carbonate (DEC) in a 1:1 volume ratio, was injected into it to prepare a 1 Ah-class secondary battery.
[0178] Example 2-2
[0179] The negative electrode and secondary battery were prepared in the same manner as in Example 2-1, except that a polyimide resin was used as the binder.
[0180] Example 2-3
[0181] Negative electrode (thickness 37 μm and 1.10 g / cm 3 A secondary battery was prepared in the same manner as in Example 2-2, except that the same silicon-based negative electrode active material as in Example 2-2 and a carbon-based negative electrode material of natural graphite (average particle size: 7.5 μm) were mixed in a weight ratio of 50:50.
[0182] Example 3-1
[0183] A silicon-based negative electrode active material composition was prepared by mixing a silicon-based negative electrode active material (manufactured by DAEJOO) having the following physical properties provided with a carbon layer, Super-P (TIMCAL) as a conductive material, and polyacrylic acid (PAA, Sigma-Aldrich) as a binder in a weight ratio of 80:10:10.
[0184] SiO x , x=1.0 Carbon content: 5% by weight Average particle size of silicon-based negative electrode active material (D 50 ): 7.0μm
[0185] The silicon-based negative electrode active material composition was applied to a copper foil having a thickness of 18 μm and dried to a thickness of 41 μm and a mass of 1.3 g / cm 3 A negative electrode having a density of 1.0 mm was prepared. The negative electrode was punched out to a diameter of 14 mmφ and dried under vacuum at 80° C. for 12 hours to obtain a negative electrode. When the thus prepared negative electrode was wound or not wound around a shaft of 4 mmφ, the negative electrode active material did not peel off from the current collector, and therefore it was confirmed that it had sufficient strength for electrochemical evaluation.
[0186] Then, a porous polypropylene sheet (30 μm) was placed as a separator between the negative electrode and a lithium metal plate having a thickness of 20 μm in a glove box to prepare a cell. The cell was placed in a reactor and a constant current of 1.5 mA was applied to the lithium non-aqueous liquid electrolyte, which contained 1 M LiPF6 in a mixed solvent of ethylene carbonate (EC) and diethylene carbonate (DEC) in a volume ratio of 1:1, for a predetermined time after reaching 1 mV and 1 mV with respect to the potential of the lithium metal plate. The negative electrode was then pre-doped with lithium by performing a de-doping (release of lithium) at a constant current of 0.6 mA with respect to the potential of the lithium metal plate until 2.0 V with respect to the potential of the lithium metal plate, thereby increasing the initial efficiency of the negative electrode. The initial efficiency measured was therefore 76.1%.
[0187] The cells were separated and a secondary battery was prepared using the negative electrode pre-doped with lithium.
[0188] Specifically, a positive electrode active material composition was prepared by mixing LiCoO2 as a positive electrode active material, Super-P (TIMCAL) as a conductive material, and polyacrylic acid (PAA, Sigma-Aldrich) as a binder in a weight ratio of 80:10:10. The positive electrode active material composition was applied to an aluminum current collector and punched out to 16 mmφ to prepare a positive electrode. A separator with a lithium metal plate having a thickness of 15 μm was laminated on the positive electrode, with the lithium metal plate placed facing the positive electrode. The separator used was a porous polypropylene sheet (25 μm). A negative electrode pre-doped with lithium was stacked on the separator to prepare a cell, and a secondary battery was manufactured using a non-aqueous liquid electrolyte. When the secondary battery was manufactured, the same non-aqueous liquid electrolyte was used as the non-aqueous liquid electrolyte used in the method for increasing the initial efficiency of the negative electrode.
[0189] Example 3-2
[0190] A carbon layer was provided, and a silicon-based negative active material (manufactured by DAEJOO) and a polyimide resin (manufactured by Ube Industries, Ltd., U-varnish A, NMP (N-methyl-2-pyrrolidone) solution, 18.1 wt % solid content) were used as a binder. The silicon-based negative active material and the binder were mixed in a weight ratio of 90:10 (based on the solid content) and the viscosity was adjusted with NMP to prepare a negative active material, which was used in the same manner as in Example 3-1 to a thickness of 37 μm and a thickness of 1.03 g / cm. 3 A lithium pre-doped silicon-based anode and secondary battery were prepared in the same manner as in Example 3-1, except that the anode was punched to 16 mmφ and dried under vacuum at 200°C for 10 hours, and a lithium non-aqueous liquid electrolyte containing 1M LiPF6 in a mixed solvent of ethylene carbonate (EC) and methyl ethylene carbonate in a volume ratio of 3:7 was used as the electrolyte.
[0191] SiO x , x=1.0 Carbon content: 5.1% by weight Average particle size of silicon-based negative electrode active material (D 50 ): 5.3μm
[0192] Example 3-3
[0193] Negative electrode (thickness 37 μm and 1.00 g / cm 3 The negative electrode active material having the following physical properties (KSC801, Shin-Etsu Chemical) and the binder were used in a weight ratio of 85:15 (based on the solid content) in the same manner as in Example 3-1.
[0194] SiO x , x=1.0 SiO x Amount of carbon composite in: SiO x 5% by weight SiO x Particle size of carbon composite material (D 50 ): 7.0μm
[0195] The negative electrode was punched to a diameter of 17 mm and dried under vacuum at 80° C. for 10 hours. A cell was prepared containing the negative electrode, a separator, and a 20 μm lithium metal plate. A lithium non-aqueous liquid electrolyte containing 1 M LiPF6 in a mixed solvent of ethylene carbonate and methyl ethyl carbonate in a volume ratio of 3:7 was poured as the electrolyte and left there for 60 hours to pre-dope the negative electrode with lithium.
[0196] On the other hand, LiNi 0.8 Co 0.2 O2, acetylene black as a conductive material, and polyvinylidene fluoride (PVdF, Solvay) as a binder were mixed in a weight ratio of 92:4:4 in NMP (N-methylpyrrolidone) solvent to prepare a positive electrode active material composition (slurry). The positive electrode active material composition was coated on a 20 μm aluminum foil, dried, and rolled to obtain a positive electrode. The initial charge and discharge characteristics of the positive electrode showed a capacity of 175 mAh / g from 4.3 V to 2.7 V.
[0197] A secondary battery was obtained in the same manner as in Example 3-1, using a silicon-based negative electrode having a thickness of 40 μm (dried at 200° C. under vacuum for 10 hours) prepared in the same manner as above.
[0198] <Evaluation of the performance of secondary batteries using silicon-based negative electrodes>
[0199] In the lithium pre-doped negative electrode of Example 3-3, the thickness of the lithium pre-doped negative electrode was 60 μm. Therefore, the fact that the thickness corresponding to the lithium metal plate (20 μm) increased indicates that no gaps were generated due to the loss of the lithium metal plate.
[0200] The secondary battery of Example 3-3 was charged to 4.3 V at a current of 3 mA, and a constant voltage of 4.3 V was applied to charge the battery for 8 hours. It was then discharged to 2.0 V (negative electrode voltage equivalent to about 0.7 V relative to the lithium potential) at a constant current of 3 mA. The secondary battery had a charge capacity of 18.0 mAh, a discharge capacity of 14.9 mAh, and an average discharge voltage of 3.60 V. Furthermore, the discharge capacity to 3.0 V was 14.0 mAh.
[0201] Comparative Example 1-1
[0202] The negative electrode and secondary battery were prepared in the same manner as in Example 1-1, except that the negative electrode was not pre-doped with lithium.
[0203] Comparative Example 1-2
[0204] The negative electrode and secondary battery were prepared in the same manner as in Example 1-2, except that the negative electrode was not pre-doped with lithium.
[0205] Comparative Example 1-3
[0206] The negative electrode and secondary battery are made of silicon-based negative electrode active material (SiO x , x=1.0, particle size of negative electrode active material (D 50 It was prepared in the same manner as in Comparative Example 1-1, except that a 5.8 μm PEFC was used.
[0207] Comparative Example 2-1
[0208] The negative electrode and secondary battery were prepared in the same manner as in Example 2-1, except that the negative electrode was not pre-doped with lithium.
[0209] Comparative Example 2-2
[0210] The negative electrode and secondary battery were prepared in the same manner as in Example 2-2, except that the negative electrode was not pre-doped with lithium.
[0211] Comparative Example 2-3
[0212] The negative electrode and secondary battery were prepared in the same manner as in Example 2-3, except that the negative electrode was not pre-doped with lithium.
[0213] Comparative Example 3-1
[0214] The negative electrode and secondary battery were prepared in the same manner as in Example 3-1, except that the negative electrode was not pre-doped with lithium and the positive electrode and the lithium metal plate were not in contact.
[0215] Comparative Example 3-2
[0216] The negative electrode and secondary battery were prepared in the same manner as in Example 3-3, except that the silicon-based negative electrode having a thickness of 40 μm was not pre-doped with lithium and the positive electrode and the lithium metal plate were not in contact.
[0217] The secondary battery prepared using the negative electrode was charged at a current of 1 mA to 4.3 V, and a constant voltage of 4.3 V was applied to charge the battery for 20 hours. It was then discharged at a constant current of 2 mA to 3.0 V (negative electrode voltage equivalent to about 0.7 V relative to the lithium potential). The secondary battery had a charge capacity of 18.2 mAh, a discharge capacity of 10.6 mAh, and an average discharge voltage of 3.57 V.
[0218] Comparative Example 3-3
[0219] The negative electrode and secondary battery were prepared in the same manner as in Example 3-1, except that the same silicon-based negative electrode active material as in Example 3-1 and the carbon-based negative electrode material of natural graphite (average particle size: 11 μm) were mixed in a weight ratio of 50:50, the negative electrode was not doped with lithium, and a silicon-based negative electrode having a thickness of 30 μm was used. The secondary battery had a charge capacity of 17.8 mAh, a discharge capacity of 11.0 mAh, and an average discharge voltage of 3.59 V.
[0220] Evaluation of capacity characteristics and initial efficiency of secondary batteries
[0221] The lithium secondary batteries obtained in the examples and comparative examples were each aged for 12 hours. Then, using a charge and discharge tester (WonATech), they were each charged at a constant current of 0.1 C until the voltage reached 4.2 V, and discharged at a constant current of 0.1 C until the voltage reached 2.5 V. This charge / discharge test was repeated 50 times to obtain the capacity retention rate.
[0222] After cycling, the initial discharge capacity and capacity retention were calculated as follows, and the results are shown in Table 1.
[0223] Initial discharge capacity: Discharge capacity at one cycle
[0224] Capacity retention: (discharge capacity at 50th cycle) / (discharge capacity at 1st cycle) x 100
[0225] [Table 1]
[0226] As can be seen from Table 1, the secondary batteries of Examples 1-1 to 1-3 in which the negative electrodes were pre-doped with lithium had initial discharge capacities of 8.8 mAh to 12.9 mAh, while the secondary batteries of Comparative Examples 1-1 to 1-3 in which the negative electrodes were not pre-doped with lithium had initial discharge capacities of 8.6 mAh or less, which was significantly reduced compared to the secondary batteries of Examples 1-1 to 1-3.
[0227] Furthermore, the secondary batteries of Examples 1-1 to 1-3 had capacity retention rates of 97% or more, the secondary batteries of Examples 1-1 and 1-2 had capacity retention rates of 99%, while the secondary battery of Comparative Example 1-3 had a value of 95%, which was significantly reduced compared to the capacity retention rates of the secondary batteries of Examples 1-1 to 1-3, especially Examples 1-1 and 1-2.
[0228] [Table 2]
[0229] As can be seen from Table 2, the secondary batteries of Examples 2-1 to 2-3 in which the negative electrode was pre-doped with lithium were superior in secondary battery characteristics to the secondary batteries of Comparative Examples 2-1 to 2-3 in which the negative electrode was not pre-doped with lithium.
[0230] In particular, the secondary batteries of Examples 2-1 to 2-3 had efficiencies of 86% or more, while those of Comparative Examples 2-1 to 2-3 had efficiencies of less than 69%. The secondary battery of Example 2-1 had an efficiency of 86.4%, which was an increase of more than 20% compared to the secondary battery of Comparative Example 2-1 having an efficiency of 68.7%. Furthermore, the secondary batteries of Examples 2-1 and 2-2 had capacities of about 1.0 mAh or more, while those of Comparative Examples 2-1 to 2-3 had capacities of less than 0.8 mAh.
[0231] On the other hand, the secondary batteries of the examples and comparative examples were left at room temperature overnight. Then, they were charged and discharged at 0.5 mA / cm using a charge and discharge tester (manufactured by Nagano Co., Ltd.) until the voltage of the test battery reached 4.2 V. 2 Each was charged at a constant current of 0.5 mA / cm. 2 The discharge was terminated when the cell voltage reached 2.5 V. The discharge capacity was then measured. This charge and discharge test was repeated 50 times to measure the capacity retention.
[0232] The discharge capacity and capacity retention after cycling were calculated as above, and the results are shown in Table 3.
[0233] [Table 3]
[0234] As can be seen from Table 3, the secondary batteries of Examples 2-1 to 2-3 in which the negative electrodes were pre-doped with lithium had initial discharge capacities of 11 mAh to 13.2 mAh, while the secondary batteries of Comparative Examples 2-1 to 2-3 in which the negative electrodes were not pre-doped with lithium had initial discharge capacities of 8.5 mAh or less, which was a 20% to 50% decrease compared to the secondary batteries of Examples 2-1 to 2-2.
[0235] Meanwhile, the initial efficiency and capacity retention of the lithium secondary batteries obtained in Examples 3-1 to 3-3 and Comparative Examples 3-1 to 3-3 were measured by the above-mentioned methods. The results are shown in FIG.
[0236] [Table 4]
[0237] As can be seen from Table 4, the secondary batteries of Examples 3-1 to 3-3 in which the negative electrodes were pre-doped with lithium had initial efficiencies of 88% to 89% and capacity retention rates of 98% to 99% after 50 cycles.
[0238] In contrast, the secondary batteries of Comparative Examples 3-1 to 3-3, in which the negative electrode was not pre-doped with lithium and the lithium metal plate was not in contact with the positive electrode, had initial efficiencies of 58% to 62%, which was reduced by about 20% or more compared to the secondary batteries of Examples. Furthermore, the secondary batteries of Comparative Examples 3-1 to 3-3 also had reduced capacity retention rates compared to the secondary batteries of Examples.
[0239] Meanwhile, Fig. 2 shows the capacity characteristics of the secondary batteries of Example 3-2 and Comparative Example 3-1 with respect to the number of cycles. As can be seen from Fig. 2, the secondary battery of Example 3-2 was increased by about 20% or more compared to the secondary battery of Comparative Example 3-1 even after 50 repeated charge and discharge tests. [Explanation of symbols]
[0240] 10: Negative electrode 20:Liquid electrolyte 30: Lithium metal plate [Industrial Applicability]
[0241] The secondary battery according to the embodiment can not only achieve safety, but also significantly increase the energy density, and improve cycle characteristics and rate characteristics. In particular, the secondary battery can further increase the initial discharge capacity and capacity retention rate; therefore, it can be advantageously used in the field of secondary batteries.
Claims
1. A secondary battery including a positive electrode, a negative electrode, and an electrolyte, the positive electrode including a metal oxide active material, the negative electrode including a silicon-based negative electrode active material, and the negative electrode being doped with lithium in an amount corresponding to an initial irreversible capacity of the negative electrode, the silicon-based negative electrode active material including a carbon layer including a carbon film on a surface thereof, and a cumulative 50% average particle size (D 50 the silicon-based negative electrode active material contains MgSiO 3 crystals and Mg 2 SiO 4 crystals, and in an X-ray diffraction analysis, the ratio (IF / IE) of the intensity of an X-ray diffraction peak corresponding to Mg 2 SiO 4 crystals appearing in the range of 2θ=22.3° to 23.3° to the intensity of an X-ray diffraction peak corresponding to MgSiO 3 crystals appearing in the range of 2θ=30.5° to 31.5° is 1 or less.
2. 2. The secondary battery of claim 1, wherein the metal oxide active material comprises an oxide having a spinel structure including lithium cobalt oxide, lithium manganate, or a mixture thereof.
3. The silicon-based negative electrode active material is made of silicon fine particles, SiO x 2. The secondary battery of claim 1, comprising at least one selected from the group consisting of a compound represented by (0.3≦x≦1.6), silicon dioxide, and a silicate containing magnesium, calcium, aluminum, or a combination thereof.
4. 2. The secondary battery of claim 1, wherein the carbon layer contains carbon in an amount of 2% by weight to 10% by weight based on the total weight of the negative electrode active material.
5. The secondary battery of claim 1 , wherein the carbon layer includes at least one selected from the group consisting of carbon nanofibers, graphene, and reduced graphene oxide.
6. The following relationship 1 is satisfied, and the lithium metal plate for lithium doping has a thickness of 10 μm to 30 μm and a thickness of 0.3 g / cm 3 ~0.8g / cm 3 The secondary battery of claim 1 having a density of [Relationship 1] 0.5<{TA×DA×CA0(100-ICE) / 100} / CLt×(CLa / CLt)}×TL×DL<TL<{TA×DA×CA0(100-ICE) / 100} / CLt×(CLa / CLt)×DL In relation 1, TA: thickness of negative electrode (μm) DA: Density of negative electrode (g / cm 3 ) ICE: Initial efficiency (%) CA0: first charge capacity of the negative electrode (mAh / g) CLt: theoretical capacity of lithium (3,600 mAh / g) CLa: actual capacity of lithium (mAh / g) TL: thickness of lithium metal plate (μm) DL: density of lithium metal plate (0.53 g / cm 3 )
7. (1-1) applying a negative electrode active material composition containing a silicon-based negative electrode active material to a negative electrode current collector to prepare a negative electrode; (1-2) preparing a cell by placing a separator between the negative electrode and a lithium metal plate; (1-3) electrochemically activating the cell obtained in step (1-2) to pre-dope the negative electrode with lithium; and (1-4) A process for producing a secondary battery using a negative electrode pre-doped with lithium 2. A method for manufacturing the secondary battery of claim 1, comprising:
8. The method for producing a secondary battery according to claim 7, further comprising the step of pre-doping the negative electrode with lithium in an amount corresponding to the initial irreversible capacity of the negative electrode by causing adsorption and desorption of lithium during electrochemical contact of the negative electrode and the lithium metal plate in step (1-3).
9. In the step (1-3), once the negative electrode is electrochemically pre-doped with lithium, an amount of lithium other than the amount of lithium corresponding to the initial irreversible capacity of the negative electrode is released to perform pre-doping. The method for producing a secondary battery according to claim 7.
10. (2-1) applying a negative electrode active material composition containing a silicon-based negative electrode active material to a negative electrode current collector to prepare a negative electrode; (2-2) placing the negative electrode and a lithium metal plate in a reactor and carrying out an oxidation-reduction reaction to pre-dope the negative electrode with lithium; and (2-3) A step of preparing an electrode by successively stacking a negative electrode pre-doped with lithium, a separator, and a positive electrode containing a metal oxide active material.
2. A method for manufacturing the secondary battery of claim 1, comprising:
11. The method for manufacturing a secondary battery according to claim 10, wherein in the step (2-2), the oxidation-reduction reaction is carried out one or more times to remove excess lithium doped in the negative electrode after pre-doping.
12. The method for producing a secondary battery according to claim 7 or 10, wherein the silicon-based negative electrode active material is obtained by the steps of: mixing silicon powder and silicon dioxide powder to obtain a silicon-silicon oxide raw powder mixture; heating and vapor-depositing the raw powder mixture to obtain a silicon oxide composite material; and pulverizing and classifying the silicon oxide composite material to obtain the silicon-based negative electrode active material.
Citation Information
Patent Citations
Manufacturing method for lithium ion secondary battery
JP2008004466A
Negative electrode active material grain powder for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery
JP2017091778A
Silicon composite oxide for lithium secondary battery negative electrode material and production method thereof
JP2018156922A