Directional deposition in an etching chamber

The method of simultaneous deposition and etching using a vertical growth mask with fluorocarbon and tungsten-containing gases addresses the issue of preserving critical dimensions in high aspect ratio patterning, ensuring precise and efficient semiconductor substrate processing.

JP7561123B2Active Publication Date: 2024-10-03LAM RES CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021523818
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-05
Filing Date
2019-10-29
Publication Date
2024-10-03
Estimated Expiration
2039-10-29

AI Technical Summary

Technical Problem

Existing semiconductor manufacturing techniques face challenges in preserving the critical dimensions of etch masks during high aspect ratio patterning, as dielectric spacers are susceptible to corrosion and plasma enhanced chemical vapor deposition processes lead to horizontal growth, altering feature profiles.

Method used

A method involving the simultaneous deposition and etching of a vertical growth mask over a patterned etch mask, using fluorocarbon and tungsten-containing gases with plasma ignition, to maintain the critical dimensions and prevent sidewall deposition, achieved through geometrical and material selectivity.

Benefits of technology

The method effectively preserves the critical dimensions of the etch mask, preventing corrosion and horizontal growth, thereby enhancing the precision and efficiency of semiconductor substrate processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561123000001
    Figure 0007561123000001
  • Figure 0007561123000002
    Figure 0007561123000002
  • Figure 0007561123000003
    Figure 0007561123000003
Patent Text Reader

Abstract

Described herein is a method for forming a vertical growth mask for use in etching applications. The disclosed embodiment includes introducing a tungsten-containing deposition precursor and one or more carrier gases while igniting a plasma to selectively deposit tungsten onto field regions of positive features of a patterned etch mask, while substantially avoiding deposition on sidewalls of the positive features or exposed surfaces of a target layer underlying the patterned etch mask.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [Incorporated by reference] A PCT application has been filed contemporaneously herewith as a part of this application. Each application to which this application claims benefit or priority, as identified in the contemporaneously filed PCT application, is incorporated by reference in its entirety into this application for all purposes. [Background technology]

[0002] The fabrication of semiconductor devices includes the fabrication of microprocessors, logic circuits, and memory devices. Such devices may be fabricated using a variety of techniques, including patterning techniques that create various types of masks. Some processes involve the formation of structures that include silicon oxide and silicon nitride. Some techniques for forming such structures may be limited to patterning techniques that include both etching and deposition.

[0003] The description of the background art provided herein is generally intended to illustrate the contents of the present disclosure. To the extent disclosed in this background art, the work done by the inventors disclosed in this application, and aspects of the description that may not be admitted as prior art at the time of filing, are not expressly or implicitly admitted as prior art to the present disclosure. Summary of the Invention

[0004] Methods and apparatus for processing a semiconductor substrate are described herein. One aspect relates to a method comprising: providing a semiconductor substrate having a patterned etch mask on a target layer, the patterned etch mask including spaced apart positive type features, each spaced apart positive type feature having a field region and a sidewall; and depositing a vertical growth mask selectively on the field regions of the spaced apart positive type features relative to the target layer.

[0005] In various embodiments, the vertical growth mask includes at least one feature, the critical dimension of the at least one feature of the vertical growth mask being substantially equal to a critical dimension of a corresponding spaced apart positive tone feature of the patterned etch mask.

[0006] In some embodiments, depositing the vertical growth mask over the field region is performed at a substrate temperature between about 0°C and about 160°C.

[0007] The method includes etching the target layer using both the patterned etch mask and the vertical growth mask as masks. In some embodiments, the deposition of the vertical growth mask and the etching of the target layer are performed simultaneously. In some embodiments, the deposition and etching are performed simultaneously by exposing the semiconductor substrate to a fluorocarbon gas and a tungsten-containing gas and igniting a plasma. The fluorocarbon gas and the tungsten-containing gas may be delivered at a ratio of fluorocarbon gas flow rate to tungsten-containing gas flow rate of between about 10:1 and about 1:1. In some embodiments, the fluorocarbon gas is delivered at a flow rate that is less than about 80% of the total volume of the fluorocarbon gas and the tungsten-containing gas.

[0008] In some embodiments, the target layer comprises amorphous carbon, and deposition and etching are performed simultaneously by simultaneously exposing the semiconductor substrate to an oxygen plasma and a tungsten-containing plasma.

[0009] In some embodiments, the method may further include alternating between selectively depositing a vertical growth mask and etching the target layer, hi some embodiments, the target layer comprises amorphous carbon and the etching is performed by exposing the target layer to an oxygen plasma.

[0010] In various embodiments, the size of the spaces between the spaced apart positive features of the vertical growth mask is substantially the same as the size of the spaces between the spaced apart positive features of the patterned etch mask, hi some embodiments, the size of the spaces between the spaced apart positive features of the patterned etch mask is within about 100% of the size of the spaces between the spaced apart positive features of the vertical growth mask.

[0011] In various embodiments, the spaces between the spaced apart positive features have an aspect ratio of between about 50:1 and about 100:1.

[0012] In various embodiments, the space size between two adjacent spaced apart positive features is between about 10 nm and about 200 nm.

[0013] In various embodiments, depositing the vertical growth mask selectively on the field region includes exposing the field region to a tungsten-containing gas. In some embodiments, the tungsten-containing gas is delivered with a diluent gas. The diluent gas can be one or more of argon gas, hydrogen gas, and mixtures thereof. The tungsten-containing gas can be a tungsten halide. In some embodiments, the tungsten halide is selected from the group consisting of tungsten hexafluoride and tungsten hexachloride. In some embodiments, depositing the vertical growth mask selectively on the field region further includes igniting a plasma in the atmosphere including the tungsten-containing gas. The plasma can be generated by a plasma power of about 100 W to about 500 W.

[0014] In various embodiments, selectively depositing the vertical growth mask onto the field region is performed in a process chamber having a chamber pressure between about 10 mTorr and about 100 mTorr.

[0015] In various embodiments, selectively depositing the vertical growth mask onto the field regions is accomplished by adjusting process conditions such as plasma power, chamber pressure, or substrate temperature.

[0016] In various embodiments, the patterned etch mask has a thickness from about 5 nm to about 200 nm.

[0017] In various embodiments, the patterned etch mask comprises a material selected from the group consisting of silicon oxide, silicon nitride, silicon oxynitride, and combinations thereof.

[0018] In various embodiments, the patterned etch mask comprises a photoresist. The target layer may also be formed from an anti-reflective coating. In various embodiments, the target layer has a thickness of about 500 nm to about 5000 nm.

[0019] Another aspect relates to a method comprising providing a semiconductor substrate having a patterned etch mask on a target layer, the patterned etch mask including spaced apart positive features, each spaced apart feature having a field region and a sidewall; and depositing a selectively grown tungsten-containing mask vertically relative to the target layer onto the field regions of the spaced apart positive features.

[0020] Another aspect relates to a method comprising providing a semiconductor substrate comprising a carbon-containing target layer, an antireflective layer, and a patterned photoresist; patterning the antireflective layer to form a patterned antireflective mask; exposing the semiconductor substrate to a tungsten-containing precursor and igniting a plasma under a plurality of conditions to selectively deposit the tungsten-containing mask to form a patterned tungsten-containing mask on field regions of the patterned antireflective mask; and patterning the carbon-containing target layer with the patterned antireflective mask and the patterned tungsten-containing mask.

[0021] Another aspect relates to a method comprising providing a semiconductor substrate including a target layer and a patterned etch mask having a first critical dimension; and exposing the semiconductor substrate to a plasma generated from a mixture of a tungsten-containing precursor material and argon gas and hydrogen gas with a plasma power between about 100 W and about 500 W at a substrate temperature below about 160° C., thereby forming a tungsten material on the patterned etch mask having a second critical dimension, wherein the second critical dimension is within about 150% of the first critical dimension.

[0022] Another aspect relates to an apparatus comprising: a reaction chamber including a pedestal for holding a substrate; a plasma source coupled to the reaction chamber and configured to generate a plasma; one or more first gas inlets coupled to the reaction chamber; a second gas inlet coupled to the reaction chamber; and a controller having instructions to: introduce a tungsten-containing precursor and a mixture of argon and hydrogen gases; generate the plasma using a plasma power of between about 100 W and about 500 W; and set a temperature of the pedestal to a temperature less than 160° C.

[0023] These and other aspects are further described below with reference to the drawings. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a process flow diagram illustrating steps performed by certain disclosed embodiments.

[0025] [Diagram 2] FIG. 1 is a process flow diagram illustrating steps performed by certain disclosed embodiments.

[0026] [Diagram 3] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments; [Figure 4] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments; [Diagram 5] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments; [Figure 6A] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments; [Figure 6B] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments; [Figure 7A] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments; [Figure 7B] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments; [Figure 8A] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments; [Figure 8B] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments; [Figure 8C] 1 is a schematic diagram of a substrate subjected to a process performed according to certain disclosed embodiments;

[0027] [Figure 9] FIG. 1 is a schematic diagram of an example process chamber for carrying out certain disclosed embodiments.

[0028] [Figure 10]FIG. 1 is a schematic diagram of an example of a process apparatus for carrying out certain disclosed embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] In the following description, numerous specific details are provided to provide a thorough understanding of the present embodiments. The disclosed embodiments may be practiced without some or all of these specific details. In other instances, well-known process operations have not been described in detail in order not to unnecessarily obscure the disclosed embodiments. It will be understood that while the disclosed embodiments are described in connection with the specific embodiment, it is not intended to be limited to this specific embodiment.

[0030] In the manufacture of semiconductor devices, masking methods are used to pattern and etch substrates. As the aspect ratio of substrates increases, the demand for more selective hard masks also increases. Various patterning schemes include the formation of positive features such as dielectric spacers that are used as masks to etch target layers. However, some dielectric spacers may be susceptible to erosion, especially when the aspect ratio of the gap between the dielectric spacers is very large, which may result in a large gap depth, which may result in a long etching period for etching the target layer with the dielectric spacers. Thus, some dielectric spacers may erode during etching of the target layer.

[0031] There are several methods to prevent etch masks from eroding during etching, including plasma-enhanced chemical vapor deposition (PECVD) processes that cause bread-loafing growth on the etch mask, thereby reducing the critical dimension of the negative features between the masks and changing the profile of the features. This is particularly problematic for features with very high aspect ratios and for long etching times.

[0032] Techniques for forming these masks involve alternating etching of an underlying layer, such as a target layer, and deposition of additional mask material that is applied to the mask during etching; such processes involve different types of process gases and, optionally, different tools, which increases processing time when transferring the wafer between stations or tools.

[0033] Provided herein is a method for depositing a mask onto a field area of ​​a patterned substrate while substantially preserving the critical dimensions of the mask. In various embodiments, deposition of the mask can occur while selectively etching a target layer into the negative features of the mask.

[0034] The vertically grown masks described herein are deposited with little or no lateral deposition as the mask is deposited. That is, deposition on the field regions of the positive substrate results in the sidewalls of the vertically grown mask being nearly vertical, without changing the size of the spaces between the positive features of the patterned mask. The deposition occurs substantially without deposition on the sidewalls of the positive substrate, with most or all deposition occurring only on the field regions. As the mask grows vertically, additional deposition mask material is deposited in large amounts on the existing mask material, and the growth is substantially vertical. That is, little or no mask material is deposited on the sidewalls of the deposited mask, and the vertically grown mask can be grown to a variety of thicknesses appropriate for each particular application. The deposition is selective, preferentially forming new material on the positive features, particularly on the tops of each positive feature. The selective deposition can proceed such that the new material forms vertically on the tops of the positive features without substantially extending horizontally. Thus, one particular advantage of certain disclosed embodiments is the ability to preserve the critical dimension of the features, i.e., the width of the space between the positive features on which the vertical growth mask is deposited, such that the deposited vertical growth mask is substantially the same width as the underlying etch mask on which it is deposited. For purposes of greater clarity, the material on which the vertical growth mask is deposited will be referred to as the "underlying etch mask" or "etch mask", although it will be understood that a variety of materials can be used to form the etch mask, including polymeric, dielectric, and semiconductor materials. It will be understood that the etch mask can be a patterned photoresist. It will also be understood that the etch mask can be a patterned antireflective coating, such as a bottom antireflective coating (BARC) layer or a dielectric antireflective coating (DARC) layer. The term "vertical growth mask" is used to refer to a material that is deposited on an underlying etch mask, and as a result, preserves the critical dimension and mask width of the features.An advantage of certain disclosed embodiments is the ability to avoid trimming or thinning of the formed mask structures, where thinning or trimming is defined as a reduction in a critical dimension of more than 2% of the critical dimension, or any concavity or roughness in the sidewalls.

[0035] The vertical growth mask may be a tungsten-containing material, such as tungsten metal. In many embodiments, the tungsten-containing metal may not be pure tungsten metal, but may contain some impurities. Although tungsten is described herein as an example material, it will be understood that other metal-containing or metal-free materials may be used by employing appropriate reactive materials and process conditions to achieve vertical growth.

[0036] Further disclosed herein is a method for simultaneously depositing a vertical growth mask while etching an underlying layer during the same processing period. The process conditions used to deposit the vertical growth mask can also be used to etch the underlying target material, such as an anti-reflective layer or an amorphous carbon layer, such that each time the substrate is exposed to process conditions, including but not limited to precursor gases, plasma conditions, temperature and pressure, the underlying target material below the underlying etch mask is etched in addition to forming a vertical growth mask on the underlying etch mask. In other words, one process simultaneously forms a vertical mask on the field region and etches the target material into the feature.

[0037] The disclosed embodiments involve selecting the process window and geometry of the underlying mask pattern to achieve vertical growth of the vertical growth mask, etching the underlying target material, or both.

[0038] Without being bound to a particular theory, it is believed that feature size selectivity, material selectivity, or both contribute to the ability of certain disclosed embodiments to achieve selective vertical growth and, in some cases, parallel etching of the underlying target material. Feature size selectivity refers to the selectivity achieved by depositing more material on one area of ​​the substrate having a first feature size characteristic than on another area of ​​the substrate having a second feature size characteristic, the areas being defined as locations on the substrate based on the exposed substrate size or topography. This form of selectivity is based solely on feature size, without requiring different materials to selectively promote or inhibit deposition. Thicker deposition in one area versus another is determined by the deposition rate (thickness deposited per unit time) in each region. Feature size selectivity can be achieved by the aspect ratio of the negative features on the substrate, and can result in a deposition rate on the field region of the substrate (i.e., on either side of the feature opening of the negative features) that exceeds the deposition rate on the sidewall or bottom area of ​​the negative features. In certain disclosed embodiments, it is believed that vertical growth is achievable due to the high aspect ratio of the negative features between the positive features defined by the underlying etch mask.

[0039] Material selectivity refers to the deposition of one material on a substrate relative to another material on a substrate due to differences in the chemical, physical, or morphological (e.g., composition, lattice structure, or other properties) of the materials. That is, for example, the deposition rate of a dielectric material may be greater than the deposition rate of a conductive material. In certain disclosed embodiments, it is believed that vertical growth can be achieved by material selectivity between the surface of the underlying etch mask (or the surface of the deposited material of the vertical growth mask) and the surface of the target material underlying the underlying etch mask. In addition, once the vertical growth mask is deposited, it is believed that in certain disclosed embodiments, vertical growth can be achieved by material selectivity between the surface of the deposited material of the vertical growth mask and the surfaces of the target material underlying the underlying etch mask and the underlying etch mask. This form of selectivity is based solely on material differences without the need for different surface geometries to selectively promote or inhibit deposition. Of course, in some cases, selectivity can be imparted by a combination of compositional differences and geometric differences on the exposed surfaces.

[0040] FIG. 1 is a process flow diagram illustrating the steps performed by certain disclosed embodiments.

[0041] In step 120, a patterned semiconductor substrate is provided having a patterned etch mask over a target layer.

[0042] The semiconductor substrate may be a silicon wafer, e.g., a 200 mm wafer, a 300 mm wafer, or a 450 mm wafer, including wafers having one or more layers of material deposited thereon, e.g., a dielectric, conductive, or semiconducting material. Non-limiting examples of underlayers include dielectric layers and conductive layers, e.g., silicon oxide, silicon nitride, silicon carbide, metal oxides, metal nitrides, metal carbides, and metal layers (e.g., copper, aluminum, tungsten, cobalt, ruthenium, molybdenum, tantalum, etc.).

[0043] The patterned etch mask may be referred to herein as an "underlying etch mask." The patterned etch mask may include spaced apart positive features (as opposed to recessed). During etching, the spaced apart features are transferred onto the substrate, i.e., directly onto the target layer or onto an intermediate layer above the target layer. The size of the positive features may be characterized by a critical dimension, which is the width measured horizontally across the positive feature at the shortest distance from one sidewall to another in the cross section of the positive feature. Each positive feature includes sidewalls and an exposed field area. The exposed field area is the top horizontal area of ​​the feature. The field area may be defined by a patterned etch mask, e.g., a mask previously used to pattern a patterned photoresist, and during etching, the mask is used to pattern the patterned etch mask and the mask is removed, leaving the exposed field area of ​​the patterned etch mask feature. In various embodiments, the average critical dimension of the positive features on the substrate is between about 10 nm and about 200 nm.

[0044] The separation distance of adjacent features is the feature pitch, which is measured from the center of a first space between positive features of the mask to the adjacent space on the other side of the positive features. The distance between positive features may be referred to herein as a "negative feature" that has a "negative feature opening" measured horizontally across the space between two positive features when measured from the sidewall of one positive feature to the sidewall of an adjacent positive feature. In some embodiments, the negative features have an average aspect ratio of at least about 1:1, or between about 50:1 and about 100:1. It will be appreciated that in some embodiments, there may be a variety of feature sizes and / or aspect ratios across the surface of the substrate. It will also be appreciated that in some embodiments, there may be the same and / or similar feature dimensions across the surface of the substrate.

[0045] In one embodiment, the patterned etch mask has an average thickness of about 5 nm to about 3000 nm, as measured by taking the average of the thicknesses measured vertically for each feature from the field area of ​​the positive feature to the top of the adjacent underlying layer of the mask.

[0046] In some embodiments, the patterned etch mask is a dielectric material, silicon, carbon, or a polymeric material.

[0047] In some embodiments, the dielectric material is silicon oxide, silicon nitride, silicon oxynitride (S i ON), or combinations thereof. The dielectric material may be deposited by thermal or plasma-assisted techniques using silicon-containing precursors and one or more oxygen-containing and / or nitrogen-containing reactants. As an example, the dielectric material may be etched using fluorocarbon-containing chemistries, optionally with a plasma.

[0048] "Silicon oxide" as used herein means Si x O y where x and y include integer values ​​as well as non-integer values. For example, "silicon oxide" is a compound of the formula SiO n where n is 1≦n≦2, and n can have integer or non-integer values. "Silicon oxide" includes compositions having SiO 1.8 "Silicon oxide" also includes silicon dioxide (SiO2) and silicon monoxide (SiO). "Silicon oxide" also includes both natural and synthetic variants, and further includes any and all crystal and molecular structures that include tetrahedral coordination of oxygen atoms surrounding a central silicon atom. "Silicon oxide" also includes amorphous silicon oxides and silicates.

[0049] "Silicon nitride" is used herein as Si xN y where x and y include integer values ​​(x=3, y=4) as well as non-integer values. For example, "silicon nitride" has the formula SiN n where n is 1≦n≦2, and n can have integer or non-integer values. "Silicon nitride" includes compositions having the formula: SiN 1.8 "Silicon nitride" also includes Si3N4, silicon nitride with traces of and / or interstitial hydrogen (SiNH), and silicon nitride with traces of and / or interstitial oxygen (SiON). "Silicon nitride" also includes both natural and synthetic variants and includes any and all lattice, crystal and molecular structures including trigonal alpha silicon nitride, hexagonal beta silicon nitride and cubic gamma silicon nitride. Silicon nitride also includes amorphous silicon nitride and can further include silicon nitride with trace impurities.

[0050] In some embodiments, the polymeric material has the formula C x H y O z and may be pre-deposited by spin-on techniques and patterned using etching chemistries including oxygen and fluorocarbons and / or plasma. In some embodiments, the polymeric material is a photoresist that is patterned by exposure to radiation and developing using lithography techniques such as EUV lithography.

[0051] In some embodiments, the patterned etch mask is a patterned photoresist.

[0052] In some embodiments, the patterned etch mask can be pre-patterned by using a developed photoresist as a mask. In some embodiments, the patterned etch mask can be or can include an antireflective layer. For example, the patterned etch mask can be a BARC layer or a DARC layer.

[0053] In step 140, a vertical growth mask is deposited on the exposed field regions of the patterned etch mask. The vertical growth mask is deposited using precursor materials and process conditions such that the mask increases in thickness over time with deposition of the mask, without substantial deposition on the sidewalls of the patterned etch mask or on the sidewalls of the vertical growth mask. This behavior is referred to as "vertical growth", although it is understood that "vertical" is used only as a term to describe the phenomenon when the substrate has its active surface oriented horizontally. In some embodiments, precursor materials and process conditions can be selectively used to modify the profile of the material deposited on the vertical growth mask. In some embodiments, the vertical growth mask is a patterned tungsten-containing mask.

[0054] The vertical growth mask may be a metal-containing or non-metallic material. Example materials for the vertical growth mask include silicon-containing materials, such as silicon, carbon-containing materials, boron-containing materials, titanium-containing materials, ruthenium-containing materials, and tungsten-containing materials, such as tungsten metal and tungsten metal with impurities.

[0055] The vertical growth mask may be deposited by introducing one or more process gases and igniting a plasma. The one or more process gases used depend on the material for depositing the vertical growth mask. In various embodiments, the one or more process gases include a metal-containing gas. In some embodiments, the metal-containing gas is a metal halide. In some embodiments, the metal-containing gas is a metal carbonyl gas. The metal-containing gas includes a tungsten-containing gas. Examples of tungsten-containing gases include tungsten halides, such as tungsten pentachloride, tungsten hexachloride, tungsten pentafluoride, and tungsten pentachloride. In some embodiments, the metal-containing gas includes titanium chloride (TCl). i In some embodiments, the metal-containing gas includes a titanium-containing gas such as triruthenium dodecacarbonyl (Ru(CO) 12 In various embodiments, the one or more process gases include a carbon-containing gas or a boron-containing gas. Examples of carbon-containing gases include methane (CH4), acetylene (C2H2), and propylene (C3H6). Examples of boron-containing gases include diborane (B2H6). In various embodiments, a tungsten-containing gas is used to deposit a tungsten-containing vertical growth mask. In various embodiments, a carbon-containing gas is used to deposit a carbon-containing vertical growth mask. In various embodiments, a boron-containing gas is used to deposit a boron-containing vertical growth mask. In various embodiments, a titanium-containing gas is used to deposit a titanium-containing vertical growth mask. In various embodiments, a ruthenium-containing gas is used to deposit a ruthenium-containing vertical growth mask.

[0056] In some embodiments, the plasma is ignited in an atmosphere of one or more process gases. For example, in some embodiments, the plasma is ignited in an atmosphere of a tungsten-containing gas. Although deposition processes using plasma are described herein, in some embodiments, thermal processes without plasma can also be used by selecting process conditions such as chamber pressure, gas flows, temperature, etc.

[0057] In some embodiments, depending on the material of the vertical growth mask, the one or more process gases include a non-metal gas, such as a silicon-containing gas or a carbon-containing gas.

[0058] The one or more process gases for depositing the vertical growth mask may be delivered with one or more carrier gases and / or dilution gases. In some embodiments, the carrier gas may be diverted before being delivered into the process chamber containing the substrate. In some embodiments, the carrier gas is delivered into the process chamber with one or more process gases. Examples of carrier gases include argon, hydrogen, helium, and combinations thereof.

[0059] A dilution gas, which may have the same composition as the carrier gas, may be used with the process gas for depositing the vertical growth mask or may be introduced in a separate step. The dilution gas may be used to limit etching or trimming due to halogen species that may decompose from the metal halide used to deposit the vertical growth mask. The dilution gas may be ignited with the plasma to facilitate scavenging of the halogen species.

[0060] The composition of the gas delivered to deposit the vertical growth mask may affect the deposition profile of the deposited vertical growth mask. In particular, the ratio of process gases can be used to adjust the directionality and growth rate of the vertical growth mask. For example, in some embodiments, the ratio of tungsten hexafluoride to hydrogen is between about 1:0 and about 1:5 to achieve a vertically deposited vertical growth mask with a critical dimension within about 150% of the critical dimension of the patterned etch mask.

[0061] In particular, in some embodiments, the vertical growth mask may be deposited by introducing tungsten hexafluoride with a mixture of argon and hydrogen and igniting a plasma.

[0062] The plasma is ignited using process conditions selected, but not limited to plasma power or frequency, to expose the field regions of the patterned mask to the plasma in a process gas atmosphere over time, thereby resulting in an increase in thickness of the vertical growth mask while making the critical dimensions of the vertical growth mask substantially the same as the critical dimensions of the patterned etch mask, for example within about 10% or about 5%.

[0063] In some embodiments, a plasma is ignited for the deposition process, and the process gas reacts with the field regions of the patterned etch mask. In some embodiments, the process gas reacts with the substrate or is adsorbed onto the surface of the field regions of the patterned etch mask. In various embodiments, deposition occurs preferentially or selectively such that deposition occurs faster in the field regions of the patterned etch mask than on the sidewalls of the patterned etch mask. In some embodiments, substantially no deposition occurs on the sidewalls of the patterned etch mask. In various embodiments, the process gas is introduced into the chamber in gaseous form, and may optionally be introduced by a carrier gas such as argon, helium, hydrogen, or combinations thereof. Species originating from the process gas plasma may be generated directly by forming a plasma in a process chamber containing the substrate, or they may be generated remotely in a process chamber not containing the substrate and delivered inside the process chamber containing the substrate.

[0064] In some embodiments, the plasma is formed in situ, whereby the plasma is formed directly on the substrate surface in the chamber. In various embodiments, the plasma is an inductively coupled plasma or a capacitively coupled plasma. In some embodiments, a bias (voltage) of between about 0V and about 500V is applied to a pedestal holding the substrate to directionally move charged plasma species toward the substrate.

[0065] In various embodiments, the plasma power for a single wafer is between about 100 W and about 500 W. The plasma can be generated using high frequency and / or low frequency plasmas.

[0066] In step 140, the substrate temperature may be set to a temperature between about 20° C. and about 80° C. It will be understood that the substrate temperature is a temperature set for the pedestal that holds the semiconductor substrate in order to heat or cool the substrate itself, and is not necessarily the exact temperature of the substrate itself at any given time.

[0067] Step 140 may be performed in a process chamber with the chamber pressure set between about 10 mTorr and about 100 mTorr, which may be adjusted as needed to obtain a given deposition rate and a particular deposition profile, in some embodiments, adjusted to increase vertical growth such that the critical dimensions of the vertical growth mask are within about 150% of the critical dimensions of the patterned etch mask.

[0068] In various embodiments, the deposition rate, deposition profile, and directionality of deposition (i.e., achieving a predetermined shape for the deposited vertical growth mask) are achieved by modifying process conditions such as plasma power, chamber pressure, substrate temperature, and / or gas flow composition and / or gas flow rates and / or gas flow ratios of the multiple gases flowed to deposit the vertical growth mask. The selectivity of the deposition also depends on the material on which the vertical growth mask is deposited and other exposed areas on the substrate.

[0069] For example, deposition of a tungsten vertical growth mask is performed on the exposed carbon-containing material over the DARC material. In particular, deposition of a tungsten vertical growth mask can be achieved on the exposed amorphous carbon-containing material over the silicon oxynitride material. In some embodiments, deposition of a vertical growth mask can be achieved on the exposed DARC material over the polymeric BARC material.

[0070] Selective deposition can also be achieved with certain feature geometry. For example, the aspect ratio of the space between the positive features of the patterned etch mask before deposition can range from about 50:1 to about 200:1. Selective deposition of the vertical growth mask can be achieved when the width of the negative features between the positive features of the patterned etch mask before deposition is about 10 nm to about 200 nm. Selective deposition of the vertical growth mask can be achieved when the depth of the negative features between the positive features of the patterned etch mask is at least about 20 nm.

[0071] Step 140 may be performed by simultaneously introducing one or more process gases and one or more carrier gases and igniting a plasma in a plasma-enhanced atomic layer deposition (PECVD) type process.

[0072] Step 140 may be performed by introducing one or more process gases and one or more carrier gases in alternating pulses and igniting a plasma during at least one or both of the process gas and / or carrier gas introductions in a plasma-enhanced atomic layer deposition (PEALD) type process.

[0073] Alternating pulse deposition is performed by repeating a cycle, which may include one pulse of a first gas and one pulse of a second, different gas, where during the pulse of the first gas, the second gas is not flowed and during the pulse of the second gas, the first gas is not flowed.

[0074] In one example, the deposition cycle performed during step 140 is one pulse of tungsten hexafluoride and one pulse of an argon / hydrogen mixture.

[0075] Each pulse in a deposition cycle can be of a specific duration. The pulse of the first gas and the pulse of the second gas can have different durations. The pulse of the first gas and the pulse of the second gas can have the same duration. In one example, a pulse of tungsten hexafluoride can be between about 100 milliseconds and about 10 seconds, while a pulse of argon / hydrogen mixture can be between about 100 milliseconds and about 10 milliseconds.

[0076] In some embodiments, the second gas is used to scavenge or treat the substrate. For example, in some embodiments, prolonged exposure of a particular patterned etch mask to tungsten hexafluoride may result in degradation of the patterned etch mask and / or prolonged exposure of a target layer disposed beneath the patterned etch mask to tungsten hexafluoride may result in degradation of the target layer. Alternating the introduction of tungsten hexafluoride with the introduction of a carrier gas or mixture of carrier gases capable of scavenging the surface of the substrate may prevent undesired etching or trimming of the patterned etch mask and the target layer. A plasma may be ignited during the pulse of carrier gas.

[0077] In various embodiments of the cyclic deposition, the various cycles of alternating process gas and carrier gas pulses are, for example, at least about 2 cycles, or from about 3 cycles to about 20 cycles. In addition, the time of each pulse can vary, so the number of cycles can depend on the desired thickness of the vertical growth mask as well as the duration of each pulse.

[0078] In some embodiments, the process conditions may vary between cycles depending on the desired deposition profile.

[0079] Returning to FIG. 1, in step 160, the target layer located below the patterned etching mask is etched using the patterned etching mask and the deposited vertical growth mask as masks. The patterned etching mask and the deposited vertical growth mask have similar critical dimensions while the pitch is kept the same and the spaces between the features of the mask are flanked by sidewalls that include both the patterned etching mask material and the vertical growth mask material. Etching is performed by using these features as a mask with a chemical that is selectively used to etch the target layer, so that the etch rate of the target layer is substantially greater than the etch rate of the vertical growth mask. The etch rate depends on the composition of the etching gas used and the process conditions. The etching gas depends on the material of the target layer and the depth to which the target layer can be etched.

[0080] In one example, the target layer is an amorphous carbon layer and the etching gas used comprises a fluorocarbon having a chemical formula of CxFyHz, where x is 1-4, y is 1-8, and z is 1-6. A plasma may be ignited during etching. The plasma may be ignited using a plasma power of between about 50 W and about 3000 W for a single wafer. The etch rate of amorphous carbon using a CF4 plasma ignited using a plasma power of 300 W may be at least about 1.5 times greater than the etch rate of a tungsten vertical growth mask.

[0081] The etch may be selective such that the target layer etches faster than the mask, although it will be appreciated that in some embodiments the vertical growth mask may be degraded by prolonged exposure of the target layer to the etching chemistry. In various embodiments, the etching of the target layer may be temporarily stopped to deposit an additional vertical growth mask by repeating step 140 and then continuing the etching in step 160.

[0082] In some embodiments, steps 140 and 160 are performed simultaneously. That is, in some embodiments, deposition of the vertical growth mask can occur by introducing a selection of process gases and adjusting process conditions, including temperature and plasma power, to reduce depletion of the vertical growth mask during etching of the target layer. Specific examples are further described below.

[0083] Simultaneous etching of the target layer and deposition of the vertical growth mask has many advantages. First, the gases used to deposit the vertical growth mask can be delivered and the etching gases used to etch the target layer can be simultaneously flowed into the same chamber used to etch the target layer, thereby increasing efficiency and avoiding movement of the wafer between chambers, stations, or tools for forming the mask and etching the target layer. Second, since the vertical growth mask deposition chemistry is introduced continuously, there is little or no risk of degrading the mask when etching the target layer. This can allow etching of very thick materials that involve long exposure to the etching chemistry without degrading the mask when etching the very thick material. For example, the target layer to be etched can have a thickness of about 500 nm to about 5000 nm. Third, by carefully adjusting the process conditions, the deposited vertical growth mask can have substantially the same critical dimensions as the patterned etch mask, so that even if the target layer is exposed to various gases for depositing the vertical growth mask, the vertical growth mask will only deposit on the field regions of the patterned etch mask or on the field regions of the deposited vertical growth mask, with little or no deposition on the sidewalls of the space between the patterned etch mask and the vertical growth mask.

[0084] Simultaneously etching and depositing the vertical growth mask includes adjusting process conditions and gas flows to achieve an acceptable etch rate of the target layer while maintaining a thickness of the vertical growth mask and preventing degradation of the mask during etching of the target layer. In some embodiments, simultaneously performing steps 140 and 160 includes introducing one or more gases suitable for etching the target layer and one or more gases suitable for depositing the vertical growth mask together. The one or more gases suitable for etching the target layer are described above with respect to step 160. The one or more gases suitable for depositing the vertical growth mask are described above with respect to step 140. In some embodiments, the one or more gases suitable for etching the target layer include a fluorocarbon gas. In some embodiments, the one or more gases suitable for depositing the vertical growth mask include a tungsten-containing gas. In various embodiments, the ratio of the flow rate of the tungsten-containing gas to the flow rate of the fluorocarbon gas affects the etch rate of the target layer and the deposition rate of the vertical growth mask. In various embodiments, when the target layer is amorphous carbon and the vertical growth mask is a tungsten mask deposited on a SiON patterned etch mask, the ratio of the flow rate of the carbon tetrafluoride gas to the flow rate of the tungsten hexafluoride gas is between about 20:1 and about 1:1. In some embodiments, the fluorocarbon gas is delivered at a flow rate that is less than about 80% of the total flow rate of all gases delivered. In various embodiments, simultaneous etching and deposition can result in a net etch rate of the target layer of 1 nm / sec for a net deposition rate of 0.5 nm / sec for the vertical growth mask.

[0085] In one example, the target layer is an amorphous carbon layer and the vertical growth mask is a tungsten mask deposited on a SiON patterned etch mask having a critical dimension of 50 nm, the vertical growth mask being deposited by performing three cycles at a substrate temperature of 60° C. and a chamber pressure of 20 mTorr, each cycle including one pulse of tungsten hexafluoride with a flow rate of 30 sccm for 10 seconds and one pulse of argon / hydrogen plasma with an argon flow rate of 200 sccm and a hydrogen flow rate of 200 sccm, ignited with a plasma power of 300 W at a substrate temperature of 60° C. and a chamber pressure of 20 mTorr. The deposited vertical growth mask has a critical dimension of 50 nm and a thickness of 50 nm, with no tungsten mask deposited on the sidewalls of the SiON patterned etch mask.

[0086] In another example, the target layer is an amorphous carbon layer and the vertical growth mask is a tungsten mask deposited on a SiON etch patterned mask having a critical dimension of 50 nm. The amorphous carbon layer is etched while the vertical growth mask is deposited. The vertical growth mask is deposited by introducing tungsten hexafluoride at a flow rate of about 10 sccm, fluorocarbon gas (e.g., CH2F2 and SF6) at a flow rate of 50 sccm, and igniting a helium plasma with a helium flow rate of 300 sccm at a substrate temperature of 40° C., a chamber pressure of 10 mTorr, and a plasma power of 300 W. The deposited vertical growth mask has a critical dimension of 50 nm and a thickness of 50 nm, no tungsten mask is deposited on the sidewalls of the SiON etch patterned mask, and the amount of the amorphous carbon layer etched is less than 20 A.

[0087] In some embodiments, steps 140 and 160 are performed as alternating sequential steps, with a cycle including step 140 followed by step 160, and the cycle repeated multiple times. In some embodiments, step 140 is performed after step 160 has been performed for a period of time, such that step 140 functions to regenerate any vertical growth mask that was degraded during step 160.

[0088] Specific examples are further described below.

[0089] 2 is a process flow diagram illustrating steps performed by certain disclosed embodiments, which provides an example of a process flow for transferring a pattern of a patterned photoresist onto an antireflective layer, selectively depositing a vertical mask onto the patterned antireflective mask to form a multi-layer mask including both an antireflective layer and a vertical mask, and etching a target layer using the multi-layer mask.

[0090] A patterned semiconductor substrate is provided having a patterned photoresist on an antireflective layer on the target layer in step 220. It will be appreciated that in some embodiments, in addition to two or more antireflective layers, other layers may be provided on the substrate, such as cap layers, barrier layers, etc.

[0091] Figure 3 is a schematic diagram illustrating one example of a semiconductor substrate that may be provided in step 220. Although particular materials are described herein and particular layer stack configurations are illustrated in Figure 3, it will be understood that other semiconductor substrates may be provided in step 220 of Figure 2.

[0092] 3 includes a target layer 300, which may be any suitable material. In some embodiments, target layer 300 may be an amorphous carbon layer. Overlying target layer 300 is a DARC layer 302, which in some embodiments may be any one or more of a silicon-containing material, such as silicon oxide, silicon nitride, or silicon oxynitride. Formed on DARC layer 302 is a BARC layer 305, which may be a polymeric material deposited by a spin-on method. The top surface of BARC layer 305 includes a patterned photoresist 307, which may be lithographically patterned and may include silicon, carbon, or both.

[0093] Returning to Figure 2, in step 230, the antireflective layer is etched to form a patterned etch mask. Step 230 includes delivering an appropriate etching gas to etch the antireflective layer and, depending on the material forming the layer, optionally igniting a plasma and applying a bias (voltage). The etch is selective to layers underneath the antireflective layer, preventing the layers from being etched.

[0094] Figures 4 and 5 are schematic diagrams illustrating an example semiconductor substrate after the antireflective etch in step 230. Figure 4 shows a substrate having target layer 300 and DARC layer 302, where BARC layer 305 of Figure 3 is etched to form patterned BARC layer 405. This forms a patterned etch mask that includes patterned BARC layer 405, which can then be used to etch an underlying layer, such as DARC layer 302.

[0095] In some embodiments, step 230 further includes etching DARC layer 302. Figure 5 shows a substrate having target layer 300 where BARC layer 305 is etched to form patterned BARC layer 405, and then DARC layer 302 is etched to form patterned DARC layer 502. Patterned photoresist 307 is removed and / or degraded by etching the distinct antireflective layer, thereby forming a patterned etch mask that includes both patterned BARC layer 405 and patterned DARC layer 502.

[0096] Returning to Figure 2, in step 240, a vertical growth mask is deposited over the exposed field regions of the patterned etch mask formed in step 230. Step 240 may be performed using any of the suitable process gases, process conditions, and other features described with respect to step 140, as described above with respect to Figure 1. For example, the vertical growth mask may be deposited using one or more alternating cycles of a tungsten-containing precursor material and an argon and hydrogen gas mixture while igniting a plasma.

[0097] 6A and 6B show an example of selectively depositing a vertical mask without depositing it on or etching the target layer 300. FIG 6A continues from FIG 5 and shows a substrate including the target layer 300, a patterned BARC layer 405, and a patterned DARC layer 502. A vertical growth mask 600, which may be tungsten, is deposited on the field regions of the patterned BARC layer 405, with little or none of the vertical growth mask 600 being deposited on the sidewalls of the patterned BARC layer 405 or the patterned DARC layer 502, or on the exposed surfaces of the target layer 300.

[0098] 2 has been performed for a period of time sufficient to form a thicker vertical growth mask 620. As shown in FIG. 6B, the substrate can be exposed to process gases and process conditions that allow for selective vertical deposition of vertical mask 620 without depositing vertical growth mask 600 on the sidewalls of patterned BARC layer 405 or patterned DARC layer 502, or on exposed surfaces of target layer 300. The critical dimensions of thicker vertical growth mask 620 are approximately the same as the critical dimensions of patterned DARC layer 502 and patterned BARC layer 405.

[0099] 2, in step 260, the target layer 300 is etched using the patterned etch mask and the vertical mask as a mask. Step 260 can be performed using any of the suitable process gases, process conditions, and other features described with respect to step 160 described above with respect to FIG.

[0100] 1, steps 240 and 260 may be performed simultaneously or as separate steps and may be repeated in multiple cycles. The variations on simultaneous, sequential, and repeated steps discussed above with respect to steps 140 and 160 may also be applied to steps 240 and 260.

[0101] 7A and 7B show an example of selectively forming a vertical mask deposition without depositing on a target layer and without etching the target layer, and simultaneously etching the target layer.

[0102] 5, a substrate is shown. As shown, the substrate includes target layer 300, patterned BARC layer 405, and patterned DARC layer 502. A vertical growth mask 700, which may be tungsten, is deposited on the field regions of BARC layer 405, with little or none of vertical growth mask 700 deposited on the sidewalls of patterned BARC layer 405 or patterned DARC layer 502, or on the exposed surfaces of target layer 300.

[0103] FIG. 7B illustrates a substrate where steps 240 and 260 of FIG. 2 are performed simultaneously for a sufficient period of time to etch a majority of the target layer 300 to form an etched target layer 307 to form a negative feature 702 in the target layer 300. During this time, the thickness of the vertical growth mask 700 is maintained and / or added. By sequentially exposing the substrate to both the various gases for depositing the vertical growth mask 700 and the various gases for etching the target layer 300, the above results can be achieved. The thickness of the vertical growth mask 700 illustrated in FIG. 7B is approximately the same as the thickness of the vertical growth mask 700 illustrated in FIG. 7A. However, it should be understood that in some embodiments, the thickness of the vertical growth mask 700 can be different (thicker or thinner) than the thickness of the vertical growth mask 700 after sequentially exposing the substrate to both the various gases for etching the target layer 300 and the various gases for depositing the vertical growth mask 700.

[0104] 8A and 8B show an example where deposition of a vertical mask and etching of a target layer are performed with alternating pulses in a cyclic process, where the vertical mask is selectively formed without deposition on the target layer and without etching the target layer.

[0105] 8A shows the substrate following FIG. 5 after step 260, where the profile of the pre-etch vertical growth mask 800 is exposed to an etchant to etch the target layer 300 using the patterned BARC layer 405 and the patterned DARC layer 502 as a mask to form a partially etched target layer 308. The amount of the target layer 300 that is etched in this step is indicated by arrow 801, while the vertical growth mask 800 may have some material etched away, resulting in etching of the vertical growth mask 810. This may occur if the etch rate of the vertical growth mask 800 is substantially slower than the etch rate of the target layer 300, but the exposure time is long enough to etch away some of the vertical growth mask 800.

[0106] FIG. 8B illustrates the substrate following FIG. 8A where step 240 is repeated to replenish vertical growth mask 820 without etching the partially etched target layer 308 or depositing a vertical growth mask material, such as tungsten, on the sidewalls of the patterned BARC layer 405 and patterned DARC layer 502 or on the surface of the partially etched target layer 308.

[0107] FIG. 8C shows the substrate following FIG. 8B where step 260 is repeated to further etch the partially etched target layer 308 to form an additionally etched target layer 318, which is further reduced in thickness as indicated by arrow 802. The etching may further remove a portion of the refilled vertical growth mask 820 to form an additionally etched vertical growth mask 821. Steps 240 and 260 may be repeated in a cyclical alternating fashion to refill the vertical growth mask while continuing to etch the target layer. In some embodiments, the vertical growth mask is deposited to a sufficient thickness such that redeposition of the vertical growth mask is not performed. In some embodiments, the vertical growth mask is deposited to a thickness such that redeposition of the vertical growth mask occurs only once per thickness of the etched target layer, which may vary depending on the composition and thickness of the deposited vertical growth mask. In some embodiments, it is possible to deposit a thick vertical growth mask and then etch the target layer without the need for additional redeposition of the vertical growth mask, particularly when the deposited etch chemistry is highly selective to etching the target layer relative to the material for the vertical growth mask.

[0108] Various embodiments described herein can be used in a variety of applications, including extreme ultraviolet (EUV) patterning, 3D NAND mask etching, such as etching carbon-containing or doped carbon-containing materials, and punch-out applications. One example of a punch-out application is the process of etching high aspect ratio hole and trench patterns to "punch-out" the target film at the bottom of the hole or trench with minimal film loss at the top of the feature. Some of the examples described above for etching carbon-containing layers on stacks with BARC and DARC layers may correspond to EUV patterning processes.

[0109] [Device] An inductively coupled plasma (ICP) reactor may be suitable for carrying out certain disclosed embodiments, including both deposition of a vertical growth mask and etching of a target layer using the vertical mask, in some embodiments. Such an ICP reactor is also described in U.S. Patent Application Publication No. 2014 / 0170853, filed December 10, 2013, entitled "IMAGE REVERSAL WITH AHM GAP FILL FOR MULTIPLE PATTERNING," which is incorporated by reference in its entirety for all purposes. Although an ICP reactor is disclosed herein, it should be understood that in some embodiments, a capacitively coupled plasma reactor may be used.

[0110] FIG. 9 shows a schematic cross-sectional view of an inductively coupled plasma integrated etch and deposition apparatus 900 suitable for carrying out embodiments herein, such as the Kiyo® Reactor manufactured by Lam Research Corp, Fremont, Calif. The inductively coupled plasma apparatus 900 includes an overall process chamber 901 that is structurally defined by chamber walls 901 and windows 911. The chamber walls 901 may be manufactured from stainless steel or aluminum. The windows 911 may be manufactured using quartz or other dielectric materials. An optional internal plasma grid 950 divides the overall process chamber 901 into an upper sub-chamber 902 and a lower sub-chamber 903. In most embodiments, the plasma grid 950 may be removed, thereby utilizing the chamber space consisting of the sub-chambers 902 and 903. A chuck 917 is positioned within the lower sub-chamber 903 near a bottom inner surface. The chuck 917 is configured to receive and hold a semiconductor wafer 919 as the etch and deposition processes are carried out. The chuck 917 can be an electrostatic chuck for supporting the wafer 919 when present. In some embodiments, an edge ring (not shown) surrounds the chuck 917 and has a top surface that is generally flush with a top surface of the wafer 919 when present on the chuck 917. The chuck 917 further includes an electrostatic electrode for gripping and unclasping the wafer. For this purpose, a filter and a DC clamp power supply (not shown) may be provided. Other control systems for lifting the wafer 919 from the chuck 917 may also be used. An RF power supply 923 may be used to charge the chuck 917. The RF power supply 923 is connected to a matching circuit 921 via connection 927. The matching circuit 921 is connected to the chuck 917 via connection 925. In this manner, the RF power supply 923 is connected to the chuck 917.

[0111] The components for generating a plasma include a coil 933 positioned above the window 911. In some embodiments, the disclosed embodiments do not use a coil. The coil 933 is fabricated from a conductive material and includes at least one complete turn. An example cross section of the coil 933 shown in FIG. 9 includes three turns. The cross section of the coil 933 is illustrated by symbols, where the coil with an "X" rotates into the page, while the coil with a "●" rotates out of the page. The components for generating a plasma also include an RF output power source 941 for delivering RF power to the coil 933. Generally, the RF output power source 941 is connected to a matching circuit 939 via a coupling 945. The matching circuit 939 is connected to the coil 933 via a connection 943. In this manner, the RF output power source 941 is connected to the coil 933. An optional Faraday shield 949 is positioned between the coil 933 and the window 911. The Faraday shield 949 is maintained in a spaced apart relationship relative to the coil 933. A Faraday shield 949 is disposed directly above the window 911. The coil 933, the Faraday shield 949, and the window 911 are each configured to be substantially parallel to one another. The Faraday shield may prevent metals or other species from depositing on the dielectric window of the plasma chamber 901.

[0112] Process gases (e.g., metal halides such as tungsten hexafluoride, argon, hydrogen, fluorocarbons, etc.) may be flowed into the process chamber 901 through one or more main gas inlets 960 and / or one or more side gas inlets 970 located in the upper chamber 902. Similarly, similar gas inlets may be provided to deliver process gases to a capacitively coupled plasma processing chamber, not shown. A vacuum pump, such as a single or two stage mechanical dry pump and / or turbomolecular pump 940, may be used to draw process gases from the process chamber 901 and maintain pressure within the process chamber 901. The pump may be used to purge gases within the chamber 901 and evacuate the chamber 901, for example, in a scavenging step to prevent halogen species from trimming or etching a mask. A valve controlled conduit may be used to fluidly connect the vacuum pump to the process chamber 901, thereby selectively controlling the application of a vacuum atmosphere by the vacuum pump. This can be done by employing a closed loop flow control device such as a throttle valve (not shown) or a pendulum valve (not shown) during plasma processing. Similarly, a vacuum pump and valve controlled fluid connections may be employed for a capacitively coupled plasma processing chamber.

[0113] During operation of the apparatus, one or more process gases may be delivered into the process chamber 901 through the gas inlet 960 and / or the gas inlet 970. In some embodiments, the process gases may be delivered only through the main gas inlet 960 or only through the side gas inlet 970. In some cases, the gas inlets shown in the figures may be replaced with more complex gas inlets, such as one or more showerheads. The Faraday shield 949 and / or the optional grid 950 may include internal channels and holes that allow process gases to be delivered to the chamber 901. Either or both of the Faraday shield 949 and / or the optional grid 950 may function as a showerhead for delivering process gases. In some embodiments, a liquid vapor delivery system may be located upstream of the chamber 901, such that once the liquid reactant or precursor material is vaporized, the vaporized reactant or precursor material is introduced into the chamber 901 through the gas inlet 960 and / or the gas inlet 970.

[0114] Radio frequency power is delivered from an RF power supply 941 to the coil 933, causing an RF current to flow through the coil 933. The RF current flowing through the coil 933 generates an electromagnetic field around the coil 933. The electromagnetic field generates an induced current in the upper sub-chamber 902. Physical and chemical reactions of the generated ions and radicals with the wafer 919 selectively etch features and deposit layers on the wafer.

[0115] When a plasma grid is used with both the upper subchamber 902 and lower subchamber 903 present, the induced current reacts with the gas present in the upper subchamber 902, generating an electron-ion plasma in the upper subchamber 902. The optional internal plasma grid 950 limits the amount of hot electrons in the lower subchamber 903. In some embodiments, the apparatus is designed and operated such that the plasma generated in the lower subchamber 903 exists as an ion-ion plasma.

[0116] Both the upper electron-ion plasma and the lower ion-ion plasma may contain positive and negative ions, but the ion-ion plasma has more negative ions relative to positive ions. Volatile by-products of etching and / or deposition are removed from the lower sub-chamber 903 through outlet 922. Herein, the chuck 917 may operate at an elevated temperature range of about 10° C. to about 250° C. The temperature depends on the process step and the specific recipe.

[0117] The chamber 901 may be coupled to equipment (not shown) when installed in a clean room or manufacturing facility. The equipment includes plumbing for delivering process gases, a vacuum generator, temperature control, and atmospheric particle control. These equipment are coupled to the chamber 901 when installed in the target manufacturing facility. Additionally, the chamber 901 may be coupled to a transfer chamber that allows robotics to transfer semiconductor wafers in and out of the chamber 901 using typical automation.

[0118] In some embodiments, a system controller 930 (which may include one or more physical or logical controllers) controls some or all of the processes in the processing chambers. The system controller 930 may include one or more memory devices and one or more processors. In some embodiments, the apparatus includes a switching system to control the flow rates and time during which the disclosed embodiments are performed. In some embodiments, the apparatus has a switching time of up to about 500 ms to up to about 750 ms. The switching time may depend on the chemicals flowing, the recipe selected, the reactor configuration, and other factors.

[0119] In some installations, the controller 930 is part of a system, which may be some of the examples described above. Such systems may include semiconductor processing equipment, including a processing tool or tools, a chamber or chambers, a platform or platforms for processing, and / or specific processing components (wafer pedestal, gas flow systems, etc.). These systems may be integrated with electronics that control the system before, during, or after processing of a semiconductor wafer or substrate. The electronics may be a "controller," and the controller may control various components or subparts of the system or systems. The controller 930 may be programmed to control any of the processes disclosed in the embodiments, depending on the process parameters and / or type of system, including, for example, delivery of process gases, temperature settings (e.g., heating / cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow settings, fluid delivery settings, position and process settings, wafer transfer to and from the tool, other transfers of the tool, and / or coupling or locking of loads for coupling to a particular system.

[0120] Broadly, the controller 930 can be defined as electronic equipment having various integrated circuits, logic circuits, memory, and / or software that receive instructions, issue instructions, control processing, enable clean processing, and enable terminal measurements. The integrated circuits can include chips as firmware that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute the program instructions (e.g., software). The program instructions can be instructions communicated to the controller in the form of various individual settings (or program files) and can be instructions that define process parameters for performing a particular process on or for a semiconductor wafer or for a system. In some embodiments, the process parameters can be part of a recipe defined by a process engineer to accomplish one or more process steps during the manufacture of one or more of the layers, process wafer materials, metals, oxides, silicon, silicon oxides, surfaces, circuits, and / or dies of the wafer.

[0121] In some implementations, the controller 930 may be integrated or coupled with the system, i.e., part of or coupled with a computer networked with the system, or a combination thereof. For example, the controller 930 may reside in the "cloud" or be all or part of a fab host computer system, which allows remote access to the wafer processing. The computer may allow remote access to the system to monitor the current progress of a manufacturing process, review the history of a manufacturing process to date, review trends and performance metrics based on multiple manufacturing processes, change parameters of a current process, set process steps to align with a current process, or start a new process. In some cases, a remote computer (e.g., a server) may provide process recipes to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that allows input or programming of parameters and / or settings that are then transferred from the remote computer to the system. In some examples, the controller 930 receives instructions in the form of data, which specifies parameters to be used for each processing step to be performed during one or more processes. It should be understood that the parameters may be specific to the type of process to be performed and the type of tool with which the controller is configured to interact or control. Thus, as noted above, the controller 930 may be distributed, consisting of one or more distributed controllers networked together to perform a common purpose of processing, such as, for example, processing and controlling as disclosed herein. One example of a distributed controller for such purposes is one or more integrated circuits on the chamber that communicate with one or more integrated circuits located remotely (at the platform level or as part of a remote computer) to cooperatively control the processes associated with the chamber.

[0122] Without being limited thereto, example systems may include plasma etch chambers or modules, deposition chambers or modules, spin rinse chambers or modules, metal plating chambers or modules, clean chambers or modules, bevel edge etch chambers or modules, physical vapor deposition (PVD) chambers or modules, chemical vapor deposition (CVD) chambers or modules, ALD chambers or modules, ALE chambers or modules, ion implantation chambers or modules, track chambers or modules, and other semiconductor processing systems that may be associated with or used in the manufacturing and / or fabrication of semiconductor wafers.

[0123] As described above, depending on the process step or steps performed by the tool, the controller may be in communication with one or more other tool circuits or modules, other tool components, cluster tools, other tool interfaces, nearby tools, adjacent tools, tools located throughout the factory, main computers, other controllers in a semiconductor manufacturing factory, tools used for material transfer to move containers of wafers between tool locations and / or fill ports.

[0124] FIG. 10 illustrates a semiconductor process cluster architecture with various modules that interact with a vacuum transfer module 1038 (VTM). The transfer module mechanism that "transfers" wafers between multiple storage facilities and processing modules may be referred to as a "cluster tool architecture" system. An airlock 1030, also known as a loadlock or transfer module, is shown in the VTM 1038 with four processing modules 1020a-1020d, which may be individually optimized to perform various manufacturing processes. By way of example, the processing modules 1020a-1020d may be implemented to perform substrate etching, deposition, ion implantation, wafer cleaning, sputtering, and / or other semiconductor processes. In some embodiments, any of the vertical mask deposition, patterned etch mask etching, and target layer etching are performed in the same module. In some embodiments, any of the vertical mask deposition, patterned etch mask etching, and target layer etching are performed in different modules of the same tool. For example, one or more substrate etch processing modules (any of 1020a-1020d) may be implemented for vertical mask deposition, patterned etch mask etching, target layer etching, and other suitable functions in accordance with the disclosed specification. The airlock 1030 and process modules 1020 may be referred to as "stations." Each station has a surface 1036 for allowing the station to interact with a VTM 1038. Sensors 1-18 are provided within each surface and are used to detect the passage of the wafer 1026 as it moves between the stations.

[0125] The robot 1022 transfers the wafer 1026 between the stations. In one embodiment, the robot 1022 has one arm, and in another embodiment, the robot 1022 has two arms, where each arm has an end effector 1024 that picks up the wafer 1026 for transfer. In the atmospheric transfer module (ATM) 1040, a tip robot 1032 is used to transfer the wafer 1026 from a cassette or front opening unified pod (FOUP) 1034 in a load port module (LPM) 1042 to the airlock 1030. The module center 1028 inside the process module 1020 is one location for positioning the wafer 1026. An aligner 1044 in the ATM 1040 is used to align the wafer.

[0126] In the exemplary process, the wafer is positioned in one of the FOUPs 1034 in the LPM 1042. The tip robot 1032 transfers the wafer from the FOUP 1034 to an aligner 1044, which allows the wafer 1026 to be properly centered before being etched or otherwise processed. Once aligned, the wafer 1026 is moved by the tip robot 1032 to the airlock 1030. The airlock module has the ability to match the environment between the ATM and the VTM, so the wafer 1026 can be moved between the two pressure environments without damage. The wafer 1026 is moved by the robot 1022 from the airlock module 1030 through the VTM 1038 to one of the process modules 1020a-1020d. To accomplish this wafer transfer, the robot 1022 uses an end effector 1024 on each of its arms. Once the wafer 1026 has been processed, it is moved by the robot 1022 from the process modules 1020a-1020d to the airlock module 1030. The wafer 1026 can then be moved by the front end robot 1032 to one of the FOUPs 1034 or to the aligner 1044.

[0127] It should be noted that the computer controlling the wafer movement can be local to the cluster structure, can be located outside the cluster structure on the manufacturing floor, or can be coupled to the cluster structure via a network at a remote location. As has been described with reference to Figure 9, the controller described above can be installed with the tool of Figure 10.

[0128] The implementations disclosed herein deposit material onto a substrate, such as a wafer, substrate, or other workpiece. The workpiece may be of various shapes, sizes, and materials. In this application, the terms "semiconductor wafer," "wafer," "substrate," "wafer substrate," and "partially fabricated integrated circuit" are used interchangeably. Those skilled in the art will appreciate that the term "partially fabricated integrated circuit" may refer to a silicon wafer during any of a number of stages of fabrication of an integrated circuit on a silicon wafer.

[0129] [Conclusion] Although the foregoing embodiments have been described in some detail for a clear understanding of the invention, it will be apparent that certain changes and modifications can be made within the scope of the appended claims. It should be noted that there are many alternative ways of implementing the process, system, and apparatus according to the present embodiments. Thus, the present embodiments should be considered as illustrative rather than restrictive, and the embodiments should not be limited to the details set forth herein. The present invention can be realized, for example, in the following manner. Application example 1: 1. A method comprising: providing a semiconductor substrate having a patterned etch mask on a target layer, the patterned etch mask including spaced apart positive tone features, each spaced apart positive tone feature having a field region and a sidewall; and depositing a vertical growth mask onto the target layer selectively over the field regions of the spaced apart positive tone features. Application example 2: The method of Application Example 1, wherein the vertical growth mask includes at least one feature, and a critical dimension of the at least one feature of the vertical growth mask is substantially equal to a critical dimension of a corresponding spaced apart positive feature of the patterned etching mask. Application example 3: The method of application example 1, further comprising etching the target layer using both the patterned etching mask and the vertical growth mask as masks. Application example 4: The method of application example 3, wherein the deposition of the vertical growth mask and the etching of the target layer are performed simultaneously. Application example 5: The method of Application Example 1, wherein the size of the spaces between the spaced-apart positive features of the vertical growth mask is substantially the same as the size of the spaces between the spaced-apart positive features of the patterned etching mask. Application example 6: 1. A method comprising: providing a semiconductor substrate having a patterned etch mask on a target layer, the patterned etch mask including spaced apart positive type features, each spaced apart positive type feature having a first critical dimension, a field area, and a sidewall; depositing a mask on the target layer having a second critical dimension over the field regions of the corresponding spaced apart positive features; The method of depositing the mask such that the second critical dimension is maintained within about 150% of the first critical dimension as the deposition thickness of the mask is increased. Example 7: 1. A method comprising: providing a semiconductor substrate having a patterned etch mask on a target layer, the patterned etch mask including spaced apart positive features, each spaced apart positive feature having a field region and a sidewall; and depositing, on the target layer, a tungsten-containing mask selectively grown vertically onto the feed regions of the spaced-apart positive features. Application example 8: 1. A method comprising: Providing a semiconductor substrate having a carbon-containing target layer, an antireflective layer, and a patterned photoresist; patterning the antireflective layer to form a patterned antireflective mask; exposing the semiconductor substrate to a tungsten-containing precursor and igniting a plasma under a plurality of conditions to selectively deposit a tungsten-containing mask to form a patterned tungsten-containing mask over field regions of the patterned antireflective mask; patterning the carbon-containing target layer with the patterned antireflective mask and the patterned tungsten-containing mask. Example 9: 1. A method comprising: providing a semiconductor substrate including a target layer and a patterned etch mask having a first critical dimension; forming a tungsten material having a second critical dimension on the patterned etch mask by exposing the semiconductor substrate to a plasma generated from a mixture of a tungsten-containing precursor and argon gas and hydrogen gas with a plasma power of between about 100 W and about 500 W at a substrate temperature below about 160° C. The method, wherein the second critical dimension is within about 150% of the first critical dimension. Example 10: An apparatus comprising: a reaction chamber including a pedestal for holding a substrate; a plasma source coupled to the reaction chamber and configured to generate a plasma; one or more first gas inlets coupled to the reaction chamber; a second gas inlet coupled to the reaction chamber; A controller comprising: introducing a tungsten-containing precursor material and a mixture of argon and hydrogen gas; generating the plasma using a plasma output of between about 100 W and about 500 W; setting the temperature of the pedestal to a temperature lower than 160°C; and a controller having instructions to cause the device to perform the steps.

Claims

1. 1. A method comprising: providing a semiconductor substrate having a patterned etch mask on a target layer, the patterned etch mask including spaced apart positive tone features, each spaced apart positive tone feature having a field region and a sidewall; depositing a vertical growth mask onto the target layer selectively over the field regions of the spaced apart positive features, the depositing of the vertical growth mask including depositing the vertical growth mask substantially without deposition on sidewalls of the positive features; and etching the target layer using both the patterned etching mask and the vertical growth mask as masks; The method, wherein the deposition and the etching are performed in one or more cycles, and the deposition of the vertical growth mask includes replenishing the vertical growth mask to allow for continuation of the etching of the target layer.

2. 2. The method of claim 1 , wherein the vertical growth mask includes at least one feature, a critical dimension of the at least one feature of the vertical growth mask being substantially equal to a critical dimension of a corresponding spaced apart positive tone feature of the patterned etch mask.

3. 10. The method of claim 1, wherein the deposition of the vertical growth mask and the etching of the target layer occur simultaneously.

4. 2. The method of claim 1, wherein the size of the spaces between the spaced-apart positive features of the vertical growth mask is substantially the same as the size of the spaces between the spaced-apart positive features of the patterned etch mask.

5. 1. A method comprising: providing a semiconductor substrate having a patterned etch mask on a target layer, the patterned etch mask including spaced apart positive tone features, each spaced apart positive tone feature having a first critical dimension, a field region, and a sidewall; depositing, on the target layer, a mask having a second critical dimension over the field regions of corresponding spaced apart positive features, substantially without deposition of the mask on sidewalls of the spaced apart positive features, the mask deposition comprising using one or more cycles of alternating pulses of (i) a first gas and (ii) a mixture of a second gas and a third gas; depositing the mask to replenish the mask while etching the target layer using the patterned etch mask and the mask to form an etched target layer; The method of depositing the mask such that the second critical dimension is maintained within 150% of the first critical dimension as the deposition thickness of the mask is increased.

6. 1. A method comprising: providing a semiconductor substrate having a patterned etch mask on a target layer, the patterned etch mask including spaced apart positive tone features, each spaced apart positive tone feature having a field region and a sidewall; depositing a tungsten-containing mask selectively grown vertically onto the target layer over the field regions of the spaced apart positive features, the deposition of the tungsten-containing mask occurring substantially without deposition on sidewalls of the spaced apart positive features; and etching the target layer using the patterned etch mask and the tungsten-containing mask. The method of claim 1, wherein the depositing and the etching are performed in one or more cycles, and the depositing of the tungsten-containing mask includes replenishing the tungsten-containing mask to a thickness sufficient to continue the etching of the target layer.

7. 1. A method comprising: Providing a semiconductor substrate having a carbon-containing target layer, an antireflective layer, and a patterned photoresist; patterning the antireflective layer to form a patterned antireflective mask; exposing the semiconductor substrate to a tungsten-containing precursor and igniting a plasma under a plurality of conditions to selectively deposit a tungsten-containing mask to form a patterned tungsten-containing mask over field regions of the patterned antireflective mask; patterning the carbon-containing target layer with the patterned antireflective mask and the patterned tungsten-containing mask.

8. 1. A method comprising: providing a semiconductor substrate including a carbon-containing target layer and a patterned etch mask having a first critical dimension; forming a tungsten material having a second critical dimension on the patterned etch mask by exposing the semiconductor substrate to a plasma generated from one or more pulses of a tungsten-containing precursor and one or more pulses of a mixture of argon and hydrogen gas with a plasma power between 100 W and 500 W at a substrate temperature below 160° C.; patterning the carbon-containing target layer with the patterned etch mask and the tungsten material; A method comprising: The method, wherein the second critical dimension is within 150% of the first critical dimension.

9. An apparatus comprising: a reaction chamber including a pedestal for holding a substrate, the substrate having a patterned etch mask having a first critical dimension; a plasma source coupled to the reaction chamber and configured to generate a plasma; one or more first gas inlets coupled to the reaction chamber; a second gas inlet coupled to the reaction chamber; A controller comprising: introducing a tungsten-containing precursor and a mixture of argon and hydrogen gas; generating said plasma using a plasma power of between 100 W and 500 W; setting the temperature of the pedestal at a temperature less than 160° C. to form a tungsten material on the patterned etch mask having a second critical dimension; patterning a carbon-containing target layer using the patterned etching mask and the tungsten material; a controller having instructions configured to cause the controller to perform one or more operations including The device, wherein the second critical dimension is within 150% of the first critical dimension.

10. 2. The method of claim 1 , The method, wherein depositing the vertical growth mask comprises using cycles of one or more pulses of (i) a first gas, and (ii) a mixture of a second gas and a third gas.

11. 11. The method of claim 10, The method of claim 1, wherein the first gas comprises a tungsten-containing precursor and the mixture of the second and third gases comprises a mixture of argon and hydrogen gas.

12. 2. The method of claim 1 , The method, wherein the vertical growth mask comprises a width that is within 150% of a width of the patterned etch mask.

13. 10. The method of claim 1 further comprising: Etching the vertical growth mask and the target layer; selectively depositing an additional vertical growth mask on the etched vertical growth mask; The method comprising:

14. 6. The method of claim 5, The method of claim 1, wherein the second critical dimension is maintained within 150% of the first critical dimension without substantial deposition on the sidewalls of the spaced apart positive features.

15. 6. The method of claim 5, The method of claim 1, wherein the first gas comprises a tungsten-containing precursor and the mixture of the second and third gases comprises a mixture of argon and hydrogen gas.

16. 7. The method of claim 6, further comprising: patterning the target layer with at least the patterned etch mask and the vertically selectively grown tungsten-containing mask.

17. 17. The method of claim 16, The method of claim 1, wherein depositing the vertically selectively grown tungsten-containing mask and patterning the target layer are performed simultaneously.

18. 17. The method of claim 16, The method of claim 1, wherein depositing the vertically selectively grown tungsten-containing mask and patterning the target layer are alternated in cycles.

19. 9. The method of claim 8, The method, wherein the one or more pulses of the mixture of argon and hydrogen gas have a duration between 100 milliseconds and 10 seconds.

20. 9. The method of claim 8, The method, wherein the one or more pulses of tungsten-containing precursor comprise a duration of from about 100 milliseconds to about 10 seconds.

21. 9. The method of claim 8, the one or more pulses of the tungsten-containing precursor and the one or more pulses of the mixture of argon and hydrogen gas comprise multiple alternating pulses of the tungsten-containing precursor and the mixture of argon and hydrogen gas.

22. 22. The method of claim 21, the plurality of alternating pulses comprises a quantity of cycles selected based on a duration of each of the plurality of alternating pulses of the tungsten-containing precursor and the mixture of argon and hydrogen gas, a desired thickness of the tungsten material, or a combination thereof.

23. 23. The method of claim 22, The method, wherein the number of cycles is between about 3 cycles and about 20 cycles.

24. 9. The method of claim 8, The method of claim 1, wherein the forming of the tungsten material and the patterning of the carbon-containing target layer occur simultaneously.

25. 9. The method of claim 8, The method, wherein the forming of the tungsten material and the patterning of the carbon-containing target layer are performed in cycles.

26. 8. The method of claim 7, 13. The method of claim 12, wherein the deposition of the tungsten-containing mask comprises using one or more cycles of (i) a pulse of a first gas and (ii) a pulse of a mixture of a second gas and a third gas.

27. 27. The method of claim 26, the first gas comprises a tungsten-containing precursor and the mixture of the second and third gases comprises a mixture of argon and hydrogen gas.

28. 27. The method of claim 26 further comprising: selecting an amount of the one or more cycles based on a duration of the pulse of the first gas, a duration of the pulse of a mixture of the second and third gases, a desired thickness of the tungsten-containing mask, or a combination thereof.

29. 8. The method of claim 7, the forming of the patterned tungsten-containing mask and the patterning of the carbon-containing target layer occur simultaneously.

30. 8. The method of claim 7, The method, wherein the forming of the patterned tungsten-containing mask and the patterning of the carbon-containing target layer are performed in cycles.

31. An apparatus comprising: one or more process chambers configured to receive a semiconductor substrate and to receive one or more precursor gases; A controller, providing said semiconductor substrate comprising a carbon-containing target layer, an antireflective layer, and a patterned photoresist; patterning the antireflective layer to form a patterned antireflective mask; exposing the semiconductor substrate to a tungsten-containing precursor and igniting a plasma under a plurality of conditions to selectively deposit a tungsten-containing mask to form a patterned tungsten-containing mask over field regions of the patterned antireflective mask; patterning the carbon-containing target layer with the patterned antireflective mask and the patterned tungsten-containing mask; a controller configured to cause the device to An apparatus comprising:

32. 32. The apparatus of claim 31 , The method, wherein the deposition of the tungsten-containing mask comprises using one or more cycles of (i) a pulse of a first gas and (ii) a pulse of a mixture of a second gas and a third gas.

33. 33. The apparatus of claim 32, the first gas comprises the tungsten-containing precursor, and the mixture of the second gas and third gas comprises a mixture of argon and hydrogen gas.

34. 33. The apparatus of claim 32, the controller is further configured to cause the apparatus to select an amount of the one or more cycles based on a duration of the pulse of the first gas, a duration of the pulse of a mixture of the second and third gases, a desired thickness of the tungsten-containing mask, or a combination thereof.

35. 32. The apparatus of claim 31 , an apparatus wherein said forming said patterned tungsten-containing mask and said patterning said carbon-containing target layer occur simultaneously.

36. 32. The apparatus of claim 31 , an apparatus wherein the forming of the patterned tungsten-containing mask and the patterning of the carbon-containing target layer are performed in cycles.

37. 10. The apparatus of claim 9, The device, wherein the patterned etch mask is between about 5 nm and about 3000 nm thick.

38. 10. The apparatus of claim 9, The apparatus, wherein the patterned etch mask comprises a photoresist.

39. 10. The apparatus of claim 9, The carbon-containing target layer comprises an anti-reflective coating.

40. 10. The apparatus of claim 9, The apparatus, wherein the carbon-containing target layer is between about 500 nm and about 5000 nm thick.

41. 10. The apparatus of claim 9, An apparatus wherein a tungsten-containing precursor is introduced in one or more pulses and said mixture of argon and hydrogen gas is introduced in one or more pulses.

Citation Information

Patent Citations

  • Thin film forming method

    JP1993094970A

  • Method for forming mask structure, film forming device, and memory medium

    JP2015110830A