Crosslinkable polymer composition and coated conductor

A crosslinkable cable coating composition using a silane-functionalized ethylene-based polymer, hindered phenol antioxidant, and aromatic amine-aromatic sulfonate addresses degradation issues in existing coatings by promoting moisture curing without isobutylene generation, ensuring safety and cost-effectiveness.

JP7561185B2Active Publication Date: 2024-10-03DOW GLOBAL TECHNOLOGIES LLC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022514657
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-09-06
Publication Date
2024-10-03
Estimated Expiration
2039-09-06

AI Technical Summary

Technical Problem

Existing cable coatings using polyolefins and hindered phenolic antioxidants for moisture curing reactions face degradation issues due to sulfonic acids, which generate toxic isobutylene.

Method used

A composition comprising a silane-functionalized ethylene-based polymer, a hindered phenol antioxidant, and an aromatic amine-aromatic sulfonate is used, which forms a crosslinkable coating that avoids degradation by using the aromatic amine-aromatic sulfonate as a catalyst to promote moisture curing without generating isobutylene.

Benefits of technology

The composition effectively crosslinks under moisture curing conditions, reducing isobutylene generation and maintaining the integrity of the coating, thereby enhancing safety and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561185000001
    Figure 0007561185000001
  • Figure 0007561185000002
    Figure 0007561185000002
  • Figure 0007561185000003
    Figure 0007561185000003
Patent Text Reader

Abstract

A composition is provided that includes (A) a silane-functionalized ethylene-based polymer, (B) a hindered phenol antioxidant, and (C) an aromatic amine-aromatic sulfonate salt. Also provided are a coated conductor that includes a conductor, and a coating on a conductor that includes the composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] Cables are frequently formed by coating the conductors with a crosslinkable coating containing a polyolefin and a hindered phenol antioxidant. An acid, such as a sulfonic acid, is included in the coating to promote the moisture cure reaction. However, the sulfonic acid is known to cause decomposition of the hindered phenol antioxidant. Decomposition of the hindered phenol antioxidant is problematic because it produces isobutylene, which is toxic.

[0002] There is a recognized need in the art for a coating composition containing a polyolefin and a hindered phenol antioxidant that is crosslinkable via a moisture cure reaction and avoids degradation of the hindered phenol antioxidant. Summary of the Invention

[0003] The present disclosure provides a composition comprising: (A) a silane-functionalized ethylene-based polymer, (B) a hindered phenol antioxidant, and (C) an aromatic amine-aromatic sulfonate.

[0004] The present disclosure also provides a process for moisture curing a silane-functionalized ethylene-based polymer, the process including: (A) providing an aromatic amine-aromatic sulfonate salt, (B) mixing the aromatic amine-aromatic sulfonate salt with a hindered phenol antioxidant to form a catalyst composition, (C) contacting the silane-functionalized ethylene-based polymer with the catalyst composition to form a crosslinkable composition, and (D) exposing the crosslinkable composition to moisture cure conditions to form a crosslinked composition.

[0005] definition Any references to the Periodic Table of the Elements are to the table as published in 1990-1991 by CRC Press, Inc. References to groups of elements in this table are to the new notation for numbering the groups.

[0006] For purposes of United States patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or the equivalent United States version thereof is so incorporated by reference), particularly with respect to the disclosure of definitions (to the extent not inconsistent with any definitions provided in this disclosure) and general knowledge in the art.

[0007] Numerical ranges disclosed herein include all values ​​from and including the lower and upper limits. Ranges containing explicit values ​​(e.g., ranges 1, or 2, or 3-5, or 6, or 7) include subranges between the two explicit values ​​(e.g., the above range 1-7 includes the subranges 1-2, 2-6, 5-7, 3-7, 5-6, etc.).

[0008] Unless otherwise stated, implicit from the context, or customary in the art, all parts and percentages are by weight and all testing methods are as of the filing date of this disclosure.

[0009] "Alkoxy" (or "alkoxy group") means -OZ 1 Refers to radicals, typical Z 1 includes alkyl, substituted alkyl, cycloalkyl, substituted cycloalkyl, heterocycloalkyl, substituted heterocycloalkyl, silyl groups, and combinations thereof. Non-limiting examples of suitable alkoxy radicals include methoxy, ethoxy, benzyloxy, and t-butoxy.

[0010] "Alkyl" and "alkyl group" refer to saturated linear, cyclic, or branched hydrocarbon groups. "Substituted alkyl" refers to an alkyl in which one or more of the hydrogen atoms bonded to any carbon of the alkyl is replaced with another group, such as halogen, aryl, substituted aryl, cycloalkyl, substituted cycloalkyl, heterocycloalkyl, substituted heterocycloalkyl, halogen, haloalkyl, hydroxy, amino, phosphido, alkoxy, amino, thio, nitro, and combinations thereof.

[0011] "Ambient environment" refers to conditions of room temperature (23-25°C) and 50% relative humidity.

[0012] "Antioxidant" refers to a type or class of chemical compounds that can be used to minimize oxidation that can occur during processing of a polymer.

[0013] "Aryl" and "aryl group" refer to an organic radical derived from an aromatic hydrocarbon by removing one hydrogen atom from the aromatic hydrocarbon. The aryl group may be a monocyclic and / or fused ring system, each of which suitably contains 5 to 7, preferably 5 or 6, atoms. Also included are structures in which two or more aryl groups are bonded via a single bond. Specific examples include, but are not limited to, phenyl, tolyl, naphthyl, biphenyl, anthryl, indenyl, fluorenyl, benzofluorenyl, phenanthryl, triphenylenyl, pyrenyl, perylenyl, chrysenyl, naphthacenyl, fluoranthenyl, and the like. "Substituted aryl" refers to an aryl in which one or more hydrogen atoms bonded to any carbon are replaced with one or more functional groups, such as alkyl, substituted alkyl, cycloalkyl, substituted cycloalkyl, heterocycloalkyl, substituted heterocycloalkyl, halogen, alkylhalo (e.g., CF3), hydroxy, amino, phosphido, alkoxy, amino, thio, nitro, and both saturated and unsaturated cyclic hydrocarbons fused to an aromatic ring, covalently linked, or linked to a common group such as a methylene or ethylene moiety. The common linking group may be a carbonyl, as in benzophenone, or an oxygen, as in diphenyl ether, or a nitrogen, as in diphenylamine.

[0014] "Alpha-olefin," "α-olefin," and like terms refer to a hydrocarbon molecule or a substituted hydrocarbon molecule (i.e., a hydrocarbon molecule containing one or more atoms other than hydrogen and carbon, such as, for example, a halogen, oxygen, nitrogen, etc.) that contains (i) only ethylenic unsaturation, the unsaturation being located between a first carbon atom and a second carbon atom, and (ii) at least 2 carbon atoms, or from 3 to 20 carbon atoms, or from 4 to 10 carbon atoms, or from 4 to 8 carbon atoms. Non-limiting examples of α-olefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-dodecene, and mixtures of two or more of these monomers.

[0015] "Blend," "polymer blend," and like terms refer to a composition of two or more polymers. Such blends may or may not be miscible. Such blends may or may not be phase separated. Such blends may or may not contain one or more domain configurations as determined from transmission electron spectroscopy, light scattering, x-ray scattering, and any other method used to measure and / or identify domain configurations.

[0016] The term "block copolymer" or "segmented copolymer" refers to a polymer containing two or more chemically distinct regions or segments (referred to as "blocks") linked in a linear fashion, i.e., a polymer containing chemically distinct units that are attached end-to-end (covalently bonded) to polymerized functional groups, rather than in a pendant or grafted manner. In one embodiment, the blocks differ in the amount or type of comonomer incorporated therein, density, amount of crystallinity, type of crystallinity (e.g., polyethylene vs. polypropylene), crystallite size attributable to polymers of such composition, type or degree of stereoregularity (isotactic or syndiotactic), regioregularity or regioirregularity, amount of branching, including long chain branching or hyperbranching, uniformity, or any other chemical or physical property.

[0017] A "cable" is at least one conductor, e.g., wire, optical fiber, etc., within a protective insulation, jacket, or sheath. A cable may be two or more wires or two or more optical fibers bound together within a common protective jacket or sheath. A combination cable may contain both electrical wires and optical fibers. The individual wires or fibers within the jacket or sheath may be bare, covered, or insulated. Cables may be designed for low, medium, and / or high voltage applications.

[0018] The term "composition" refers to a mixture of materials that comprise the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0019] The terms "comprising," "including," "having," and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether or not they are specifically disclosed. For the avoidance of any doubt, all compositions recited in claims through the use of the word "comprising" may include any additional additives, adjuvants, or compounds, whether polymerized or not, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any subsequent recitation any other component, step, or procedure, excepting those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not specifically described or listed. The term "or" refers to the listed items individually and in any combination, unless otherwise stated. The use of the singular includes the use of the plural, and vice versa.

[0020] A "conductor" is one or more wires or one or more fibers for conducting heat, light and / or electricity at any voltage (DC, AC, or transient). The conductor may be single wire / fiber or multi-wire / fiber and may be in stranded or tubular form. Non-limiting examples of suitable conductors include various metals such as carbon, silver, gold, copper, aluminum, etc. The conductor may also be optical fiber made from either glass or plastic. The conductor may or may not be disposed within a protective sheath. The conductor may be a single cable or multiple cables bundled together (i.e., cable core or cores).

[0021] "Crosslinkable" and "curable" indicate that the polymer, before or after being formed into an article, has not been cured or crosslinked, and has not been subjected to or exposed to treatments that induced substantial crosslinking, but that the polymer contains additives or functionality that result in substantial crosslinking when subjected to or exposed to such treatments (e.g., exposure to water).

[0022] "Crosslinked" and similar terms indicate that the polymer composition has a xylene or decalin extractables of 90 weight percent or less (i.e., a gel content of 10 weight percent or more) before or after it is molded into an article.

[0023] "Cured" and similar terms indicate that a polymer has been subjected to or exposed to a treatment that induces crosslinking, either before or after being formed into an article.

[0024] An "ethylene-based polymer" is a polymer that contains greater than 50 weight percent polymerized ethylene monomer (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer. Ethylene-based polymers include ethylene homopolymers and ethylene copolymers (meaning units derived from ethylene and one or more comonomers). The terms "ethylene-based polymer" and "polyethylene" may be used interchangeably. Non-limiting examples of ethylene-based polymers (polyethylenes) include low density polyethylene (LDPE), medium density polyethylene (MDPE), and linear polyethylene. Non-limiting examples of linear polyethylene include linear low density polyethylene (LLDPE), ultra low density polyethylene (ULDPE), very low density polyethylene (VLDPE), multicomponent ethylene-based copolymers (EPE), ethylene / α-olefin multiblock copolymers (also known as olefin block copolymers (OBC)), single-site catalyzed linear low density polyethylene (m-LLDPE), substantially linear or linear plastomers / elastomers, and high density polyethylene (HDPE). In general, polyethylene can be produced in gas phase, fluidized bed reactors, liquid phase slurry process reactors, or liquid phase solution process reactors using heterogeneous catalyst systems such as Ziegler-Natta catalysts, homogeneous catalyst systems including group 4 transition metals and ligand structures such as metallocenes, nonmetallocene metal centers, heteroaryls, heterovalent aryloxy ethers, phosphinimines, and others. A combination of heterogeneous and / or homogeneous catalysts may also be used in either a single reactor or dual reactor configuration. In one embodiment, the ethylene-based polymer does not contain an aromatic comonomer polymerized therein.

[0025] "Ethylene plastomer / elastomer" refers to a polymer that contains units derived from ethylene and at least one C3-C 10It is a substantially linear or linear ethylene / α-olefin copolymer containing a uniform distribution of short chain branches including units derived from an α-olefin comonomer. The ethylene plastomer / elastomer has a density of 0.870 g / cc to 0.917 g / cc. Non-limiting examples of ethylene plastomers / elastomers include AFFINITY™ plastomers and elastomers (available from Dow Chemical Company), EXACT™ plastomers (available from ExxonMobil Chemical), Tafmer™ (available from Mitsui), Nexlene™ (available from SK Chemicals Co.), and Lucene™ (available from LG Chem Ltd.).

[0026] "High density polyethylene" (or "HDPE") is a polymer consisting of ethylene homopolymer or at least one C4-C 10 An ethylene / α-olefin copolymer having an α-olefin comonomer and a density greater than 0.94 g / cc to 0.98 g / cc. HDPE can be a unimodal or multimodal copolymer. A "unimodal ethylene copolymer" is an ethylene / C4-C6 copolymer having one distinct peak in gel permeation chromatography (GPC) showing the molecular weight distribution. 10 A multimodal ethylene copolymer is an α-olefin copolymer that has at least two distinct peaks in the molecular weight distribution measured by GPC. 10 It refers to α-olefin copolymers. Multimodality includes copolymers with two peaks (bimodal) as well as copolymers with three or more peaks. Non-limiting examples of HDPE include DOW™ high density polyethylene (HDPE) resins, ELITE™ reinforced polyethylene resins, and CONTINUUM™ bimodal raw polyethylene resins, each available from The Dow Chemical Company, LUPOLEN™ available from LyondellBasell, and HDPE products from Borealis, Ineos, and ExxonMobil.

[0027] The terms "hydrocarbyl" and "hydrocarbon" refer to substituents containing only hydrogen and carbon atoms, including branched or unbranched, saturated or unsaturated, cyclic, polycyclic or acyclic species. Non-limiting examples include alkyl, cycloalkyl, alkenyl, alkadienyl, cycloalkenyl, cycloalkadienyl, aryl, and alkynyl groups.

[0028] "Hydrolyzable silane groups" are silane groups that react with water. These include alkoxysilane groups on monomers or polymers that can be hydrolyzed to give silanol groups, which can then condense to crosslink the monomer or polymer.

[0029] "Interpolymers" are polymers prepared by the polymerization of at least two different monomers. This generic term includes copolymers, which are commonly used to refer to polymers prepared from two different monomers, and polymers prepared from three or more different monomers, such as terpolymers, tetrapolymers, etc.

[0030] A "jacket" is the outermost covering of a conductor. If a conductor includes a single covering, the covering may function as both the jacket and the insulation on the conductor.

[0031] "Linear low density polyethylene" (or "LLDPE") is a polyethylene that is a mixture of units derived from ethylene and at least one C3-C 10It is a linear ethylene / α-olefin copolymer containing a uniform distribution of short chain branches with units derived from an α-olefin comonomer. LLDPE is characterized by little, if any, long chain branching, in contrast to conventional LDPE. LLDPE has a density of 0.910 g / cc to 0.940 g / cc. Non-limiting examples of LLDPE include TUFLIN™ Linear Low Density Polyethylene Resins and DOWLEX™ Polyethylene Resins, each available from The Dow Chemical Company, and MARLEX™ Polyethylene (available from Chevron Phillips).

[0032] "Low density polyethylene" (or "LDPE") is defined as any ethylene homopolymer or copolymer having a density between 0.915 g / cc and 0.940 g / cc and containing at least one C3-C4 long chain branch having a broad MWD. 10 It consists of ethylene / α-olefin copolymers with an α-olefin comonomer. LDPE is typically produced by high pressure free radical polymerization (tubular reactor or autoclave using a free radical initiator). Non-limiting examples of LDPE include MarFlex™ (Chevron Phillips), LUPOLEN™ (LyondellBasell), as well as LDPE products from Borealis, Ineos, ExxonMobil, etc.

[0033] "Medium density polyethylene" (or "MDPE") refers to ethylene homopolymer or at least one C3-C6 copolymer having a density between 0.926 g / cc and 0.940 g / cc. 10 It is an ethylene / α-olefin copolymer that contains an α-olefin comonomer.

[0034] "Multicomponent ethylene-based copolymers" (or "EPEs") are copolymers that contain units derived from ethylene and at least one C3-C6 copolymer, such as those described in patent documents USP 6,111,023, USP 5,677,383, and USP 6,984,695. 10It contains units derived from an α-olefin comonomer. The EPE resin has a density of 0.905 g / cc to 0.962 g / cc. Non-limiting examples of EPE resins include ELITE™ reinforced polyethylene and ELITE AT™ advanced technology resins, each available from The Dow Chemical Company, SURPASS™ polyethylene (PE) resins available from Nova Chemicals, and SMART™ available from SK Chemicals Co.

[0035] As used herein, an "olefin-based polymer" is a polymer that contains greater than 50 mole percent polymerized olefin monomers (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer. Non-limiting examples of olefin-based polymers include ethylene-based polymers and propylene-based polymers.

[0036] A "polymer" is a compound prepared by polymerization of monomers, whether of the same or different kinds, which, in polymerized form, provide a plurality and / or repeating "units" or "structural units" that make up the polymer. Thus, the generic term polymer encompasses the term homopolymer, which is usually used to refer to a polymer prepared from only one type of monomer, and the term copolymer, which is usually used to refer to a polymer prepared from at least two types of monomer. It also encompasses all forms of copolymers, e.g., random, block, etc. The terms "ethylene / α-olefin polymer" and "propylene / α-olefin polymer" refer to the above-mentioned copolymers prepared from polymerizing ethylene or propylene, respectively, and one or more additional polymerizable α-olefin monomers. It should be noted that while polymers are often referred to as "made from" one or more specified monomers, such as "based on" the specified monomers or types of monomers and "containing" the specified monomer content, in this context the term "monomer" is understood to refer to the polymerized residue of the specified monomer and not to the non-polymerized species. Generally, polymers herein are referred to in terms of "units" which are the polymerized form of the corresponding monomers.

[0037] A "propylene-based polymer" is a polymer that contains more than 50 mole percent polymerized propylene monomers (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer. Propylene-based polymers include propylene homopolymers and propylene copolymers (meaning units derived from propylene and one or more comonomers). The terms "propylene-based polymer" and "polypropylene" may be used interchangeably. Non-limiting examples of propylene-based polymers (polypropylenes) include those that contain at least one C2- or C4-C 10 It is a propylene / α-olefin copolymer with an α-olefin comonomer.

[0038] "Sheath" is a generic term and when used in reference to a cable includes insulating covering or layer, protective jacket, and the like.

[0039] "Single-site catalyzed linear low density polyethylene" (or "m-LLDPE") is a polyethylene that is a mixture of units derived from ethylene and at least one C3-C 10 It is a linear ethylene / α-olefin copolymer containing a uniform distribution of short chain branches with units derived from an α-olefin comonomer. m-LLDPE has a density of 0.913 g / cc to 0.940 g / cc. Non-limiting examples of m-LLDPE include EXCEED™ Metallocene PE (available from ExxonMobil Chemical), LUFLEXEN™ m-LLDPE (available from LyondellBasell), and ELTEX™ PF m-LLDPE (available from Ineos Olefins & Polymers).

[0040] "Ultra-low density polyethylene (or "ULDPE")" and "very low density polyethylene (or "VLDPE")" are each made of units derived from ethylene and at least one C3-C 10 They are linear ethylene / α-olefin copolymers containing a heterogeneous distribution of short chain branches including units derived from the α-olefin comonomer. ULDPE and VLDPE each have a density of 0.885 g / cc to 0.915 g / cc. Non-limiting examples of ULDPE and VLDPE include ATTANE™ ULDPE resins and FLEXOMER™ VLDPE resins, each available from The Dow Chemical Company.

[0041] A "wire" is a single strand of conductive metal, such as copper or aluminum, or a single strand of optical fiber.

[0042] Test Method Density is measured according to ASTM D792, Method B. Results are reported in grams per cubic centimeter (g) (g / cc or g / cm 3 ) to record.

[0043] Gel content is measured by extraction with boiling decalin at 180° C. for 5 hours according to ASTM 2765. Results are reported as a percentage (%) based on the total weight of the composition. The percentage of gel typically increases with increasing crosslinking level.

[0044] High temperature creep is measured according to IEC-60811-2-1. Thermal deformation at 200°C is measured as a percentage (%) under a load of 0.2 MPa. High temperature creep in water bath is measured after the specimens are cured in a water bath at 90°C for 1, 3, and 6 hours. High temperature creep in ambient environment is measured after the specimens are cured at room temperature (23-25°C) and 50% relative humidity for 69, 90, 100, 168, and 230 hours.

[0045] Melt index (MI) (also known as I2) was measured in accordance with ASTM D1238, condition 190° C. / 2.16 kilogram (kg) weight, and is reported in grams dissolved per 10 minutes (g / 10 min).

[0046] Isobutylene Measurement Samples are prepared for isobutylene measurement according to two methods.

[0047] Sample Preparation Method 1. One gram of catalyst master batch pellets are sealed into an HSGC vial within 10 minutes of pelletization. The vial is sealed and stored at room temperature (23-25°C) for 2 weeks. Isobutylene evolution is then measured.

[0048] Sample Preparation Method 2. The catalyst masterbatch pellets are placed into a polyethylene bag within 10 minutes of pelletization. The bag is sealed and stored at room temperature (23-25°C) for 2 weeks. A 1 gram sample is then removed from the bag and placed into an HSGC vial, which is then sealed and measured for isobutylene evolution.

[0049] Measurement. Isobutylene evolved from the catalyst masterbatch is measured by (i) headspace gas chromatography (HSGC) according to the conditions in Table A below, or (ii) gas chromatography (GC) according to the conditions in Table B below. In either case, the peak area at a retention time of 1.8 minutes is recorded. [Table 1] [Table 2] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0050] The present disclosure provides a composition comprising: (A) a silane-functionalized ethylene-based polymer, (B) a hindered phenol antioxidant, and (C) an aromatic amine-aromatic sulfonate.

[0051] In one embodiment, the (C) aromatic amine-aromatic sulfonate salt has the following structure (I): [ka] In the formula, Y is an integer from 1 to 2 or 3; R 1 is selected from an aryl group, a substituted aryl group, an alkyl group, or a substituted alkyl group; R 2 is selected from aryl groups and substituted aryl groups; R 3 is selected from an aryl group, a substituted aryl group, an alkyl group, a substituted alkyl group, or hydrogen; R 4 is selected from aryl groups and substituted aryl groups, and X is an integer from 1 to 2, or 3, or 4.

[0052] A. Silane-Functionalized Ethylene-Based Polymers The composition comprises a silane-functionalized ethylene-based polymer. A "silane-functionalized ethylene-based polymer" is a polymer that contains a silane and 50% or more by weight, or a majority, of polymerized ethylene, based on the total weight of the polymer. Non-limiting examples of suitable silane-functionalized polyolefins include ethylene / silane copolymers, silane-grafted polyolefins (Si-g-PE), and combinations thereof.

[0053] "Ethylene / silane copolymer" is formed by copolymerization of ethylene and hydrolyzable silane monomers, such as vinylalkoxysilane monomers. In one embodiment, the ethylene / silane copolymer is prepared by copolymerization of ethylene, hydrolyzable silane monomers, and, optionally, an unsaturated ester. The preparation of ethylene / silane copolymers is described, for example, in USP 3,225,018 and USP 4,574,133, each of which is incorporated herein by reference.

[0054] "Silane-grafted polyethylene" (or "Si-g-PE") is formed by grafting hydrolyzable silane monomers (such as vinyl alkoxysilane monomers) onto the backbone of a base polyethylene. In one embodiment, the grafting is performed in the presence of a free radical generator such as a peroxide. The hydrolyzable silane monomers can be grafted onto the backbone of the base polyethylene (i) prior to incorporating or compounding the Si-g-PE into a composition used to make a final article such as a coated conductor (also known as the SIOPLAS™ process), or (ii) simultaneously with the extrusion of the composition that forms the final article (also known as the MONOSIL™ process, where the Si-g-PE is formed in situ during melt blending and extrusion). In one embodiment, the Si-g-PE is formed before the Si-g-PE is compounded with the aromatic amine-aromatic sulfonate, the hindered phenol antioxidant, and other optional components. In another embodiment, the Si-g-PE is formed in situ by combining polyethylene, hydrolyzable silane monomers, and peroxide initiators with aromatic amine-aromatic sulfonate, hindered phenol antioxidant, and other optional components.

[0055] The base polyethylene of the Si-g-PE can be any ethylene-based polymer disclosed herein. Non-limiting examples of suitable ethylene-based polymers include ethylene homopolymers and ethylene-based interpolymers containing one or more polymerizable comonomers, such as unsaturated esters and / or α-olefins. In one embodiment, the ethylene-based polymer is selected from low density polyethylene (LDPE), high density polyethylene (HDPE), and combinations thereof.

[0056] The hydrolyzable silane monomers used to make the ethylene / silane copolymers or Si-g-PEs are silane-containing monomers that will effectively copolymerize with ethylene to form ethylene / silane copolymers or graft onto ethylene-based polymers to form Si-g-PEs. An exemplary hydrolyzable silane monomer has the following structure (A): [ka] wherein R' is a hydrogen atom or a methyl group, x and y are 0 or 1, with the proviso that when x is 1, y is 1, n is an integer from 1 to 12, inclusive, or n is an integer from 1 to 4, and each R" is independently a hydrolyzable organic group such as an alkoxy group having 1 to 12 carbon atoms (e.g., methoxy, ethoxy, butoxy), an aryloxy group (e.g., phenoxy), an aroxy group (e.g., benzyloxy), an aliphatic acyloxy group having 1 to 12 carbon atoms (e.g., formyloxy, acetyloxy, propanoyloxy), an amino or substituted amino group (alkylamino, arylamino), or a lower alkyl group having 1 to 6 carbon atoms, inclusive, with the proviso that not more than one of the three R" groups is alkyl.

[0057] Non-limiting examples of suitable hydrolyzable silane monomers include silanes having an ethylenically unsaturated hydrocarbyl group, such as a vinyl, allyl, isopropenyl, butenyl, cyclohexenyl, or gamma-(meth)acryloxyallyl group, and a hydrolyzable group, such as, for example, a hydrocarbyloxy, hydrocarbonyloxy, or hydrocarbylamino group. Examples of hydrolyzable groups include methoxy, ethoxy, formyloxy, acetoxy, proprionyloxy, and alkyl or arylamino groups.

[0058] In one embodiment, the hydrolyzable silane monomer is an unsaturated alkoxysilane such as vinyltrimethoxysilane (VTMS), vinyltriethoxysilane, vinyltriacetoxysilane, gamma-(meth)acryloxy, propyltrimethoxysilane, and mixtures of these silanes.

[0059] Non-limiting examples of suitable unsaturated esters used to make the ethylene / silane copolymer include alkyl acrylates, alkyl methacrylates, or vinyl carboxylates. Non-limiting examples of suitable alkyl groups include methyl, ethyl, n-propyl, i-propyl, n-butyl, t-butyl, and the like. In one embodiment, the alkyl group has 1, or 2 to 4, or 8 carbon atoms. Non-limiting examples of suitable alkyl acrylates include ethyl acrylate, methyl acrylate, t-butyl acrylate, n-butyl acrylate, and 2-ethylhexyl acrylate. Non-limiting examples of suitable alkyl methacrylates include methyl methacrylate and n-butyl methacrylate. In one embodiment, the carboxylate group has 2 to 5, or 6, or 8 carbon atoms. Non-limiting examples of suitable vinyl carboxylates include vinyl acetate, vinyl propionate, and vinyl butanoate.

[0060] In one embodiment, the silane-functionalized ethylene-based polymer contains 0.1%, or 0.5%, or 1.0%, or 1.5% to 2.0%, or 2.5%, or 3.0%, or 4.0%, or 5.0% by weight of the silane, based on the total weight of the silane-functionalized ethylene-based polymer.

[0061] In one embodiment, the silane-functionalized ethylene-based polymer contains, consists essentially of, or consists of: (i) 50%, or 60%, or 70%, or 80%, or 90%, or 95% to 97%, or 98%, or 99%, or less than 100% by weight ethylene, and (ii) the inverse amount of silane, or greater than 0%, or 1%, or 2%, or 3%, to 5%, or 10%, or 20%, or 30%, or 40%, or 50% by weight silane, based on the total weight of the silane-functionalized ethylene-based polymer.

[0062] In one embodiment, the silane-functionalized ethylene-based polymer has a density from 0.850 g / cc, or 0.910 g / cc, or 0.920 g / cc to 0.922 g / cc, or 0.925 g / cc, or 0.930 g / cc, or 0.950 g / cc, or 0.965 g / cc. In another embodiment, the silane-functionalized ethylene-based polymer has a density from 0.850 g / cc to 0.965 g / cc, or 0.900 g / cc to 0.950 g / cc, or 0.920 g / cc to 0.925 g / cc.

[0063] In one embodiment, the silane-functionalized ethylene-based polymer has a melt index (MI) of 0.1 g / 10 min, or 0.5 g / 10 min, or 1.0 g / 10 min, or 1.5 g / 10 min to 2 g / 10 min, or 5 g / 10 min, or 10 g / 10 min, or 15 g / 10 min, or 20 g / 10 min, or 30 g / 10 min, or 40 g / 10 min, or 50 g / 10 min. In another embodiment, the functionalized ethylene-based polymer has a melt index (MI) of 0.1 g / 10 min to 50 g / 10 min, or 0.5 g / 10 min to 10 g / 10 min, or 0.5 g / 10 min to 5 g / 10 min.

[0064] In one embodiment, the silane-functionalized ethylene-based polymer is an ethylene / silane copolymer. The ethylene / silane copolymer contains ethylene and hydrolyzable silane monomers as the only monomer units. In another embodiment, the ethylene / silane copolymer is optionally a C3, or C4-C6, or C8, or C 10 , or C 12 , or C 16 , or C 18 , or C 20 α-olefins, unsaturated esters, and combinations thereof. In one embodiment, the ethylene / silane copolymer is an ethylene / unsaturated ester / silane reactor copolymer. Non-limiting examples of suitable ethylene / silane copolymers include SI-LINK™ DFDA-5451 NT and SI-LINK™ AC DFDB-5451 NT, each available from The Dow Chemical Company.

[0065] The ethylene / silane reactor copolymer can comprise two or more embodiments disclosed herein.

[0066] In one embodiment, the silane-functionalized ethylene-based polymer is Si-g-PE.

[0067] The base ethylene-based polymer of the Si-g-PE contains 50% by weight, or 55% by weight, or 60% by weight, or 65% by weight, or 70% by weight, or 80% by weight, or 90% by weight, or 95% to 97% by weight, or 98% by weight, or 99% by weight, or 100% by weight ethylene, based on the total weight of the base ethylene-based polymer.

[0068] In one embodiment, the base ethylene-based polymer of the Si-g-PE is an ethylene / α-olefin copolymer. The α-olefin contains 3, or 4 to 6, or 8, or 12, or 20 carbon atoms. Non-limiting examples of suitable α-olefins include propylene, butene, hexene, and octene. In one embodiment, the ethylene-based copolymer is an ethylene / octene copolymer. When the ethylene-based copolymer is an ethylene / α-olefin copolymer, the Si-g-PE is a silane-grafted ethylene / α-olefin copolymer. Non-limiting examples of suitable ethylene / α-olefin copolymers useful as base ethylene-based polymers for the Si-g-PE include ENGAGE™ and INFUSE™ resins available from Dow Chemical Company.

[0069] Blends of silane-functionalized ethylene-based polymers can also be used, where the silane-functionalized ethylene-based polymer can be diluted with one or more other polyolefins to the extent that the polyolefins are (i) miscible or compatible with each other, and (ii) the silane-functionalized ethylene-based polymer constitutes 30% by weight, or 40% by weight, or 50% by weight, or 55% by weight, or 60% by weight, or 70% by weight, or 80% by weight, or 90% by weight, or 95% by weight, or 99% by weight to less than 100% by weight of the blend (based on the combined weight of the polyolefins, including the silane-functionalized ethylene-based polymer).

[0070] The silane-functionalized ethylene-based polymer can comprise two or more embodiments disclosed herein.

[0071] B. Hindered phenol antioxidants The composition contains a hindered phenol antioxidant.

[0072] "Hindered phenol antioxidants" are primary antioxidants that act as radical scavengers. Hindered phenol antioxidants contain a phenol group. Non-limiting examples of suitable hindered phenol antioxidants include pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), 1,3,5-trimethyl-2,4,6-tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-benzene, pentaerythrityl tetrakis-3(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate, n-octadecyl-3(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate, 4, Examples of such hindered phenol antioxidants include 4'-methylenebis(2,6-tert-butyl-phenol), 4,4'-thiobis(6-tert-butyl-o-cresol), 2,6-di-tert-butylphenol, 6-(4-hydroxyphenoxy)-2,4-bis(n-octyl-thio)-1,3,5 triazine, di-n-octylthio)ethyl 3,5-di-tert-butyl-4-hydroxy-benzoate, and sorbitol hexa[3-(3,5-di-tert-butyl-4-hydroxy-phenyl)-propionate], and combinations thereof. Such hindered phenol antioxidants are commercially available from BASF and include IRGANOX™ 565, 1010, 1076, and 1726.

[0073] In one embodiment, the hindered phenol antioxidant is pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), commercially available as IRGANOX™ 1010 from BASF.

[0074] The hindered phenol antioxidant may comprise two or more embodiments disclosed herein.

[0075] C. Aromatic amine-aromatic sulfonate The composition comprises an aromatic amine-aromatic sulfonate salt.

[0076] "Aromatic amine-aromatic sulfonate" or "AS-ASAS" is a salt compound formed from an aromatic amine and an aromatic sulfonic acid. The AS-ASAS may be a monoamine, diamine, or triamine. AS-ASAS excludes salt compounds formed from linear amines and / or branched amines. Additionally, AS-ASAS excludes salt compounds formed from linear sulfonic acids and / or branched sulfonic acids.

[0077] An "aromatic amine" is a compound having the following structure (II): [ka] In the formula, R 5 is selected from an aryl group, a substituted aryl group, an alkyl group, or a substituted alkyl group; R 6 is selected from aryl groups and substituted aryl groups; R 7 is selected from an aryl group, a substituted aryl group, an alkyl group, a substituted alkyl group, or hydrogen; and X is an integer from 1 to 2, or 3, or 4.

[0078] In one embodiment, in structure (II), R 5 is C6-C 40 Aryl groups, substituted C6-C 40 Aryl groups, C1-C 40 Alkyl or substituted C1-C 40 alkyl groups; R 6 is C6-C 40 Aryl groups, and substituted C6-C 40 aryl group, R 7 is C6-C 40 Aryl groups, substituted C6-C 40 Aryl groups, C1-C 40 Alkyl groups, substituted C1-C 40 an alkyl group, or hydrogen; and X is an integer from 1 to 2, or 3, or 4.

[0079] Non-limiting examples of suitable aromatic amines include 4,4'-bis(alpha,alpha-dimethylbenzyl)diphenylamine, N1-(4-methylpentan-2-yl)-N4-phenylbenzene-1,4-diamine, N,N'-diphenyl-p-phenylenediamine, di([1,1'-biphenyl]-4-yl)amine, (2,2,4-trimethyl-1,2-dihydroquinoline), 9,9-dimethyl-9,10-dihydroacridine, N-phenyl-2-naphthylamine, N1,N4-di(naphthalen-2-yl)benzene-1,4-diamine, N,N'-bis-(1,4-dimethylpentyl)-p-phenylenediamine, N,N'-di-sec-butyl-1,4-phenylenediamine, N-isopropyl-N'-phenyl-1,4-phenylenediamine, 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, and combinations thereof.

[0080] An "aromatic sulfonic acid" is a compound having the following structure (III): [ka] In the formula, R 8 is selected from aryl groups and substituted aryl groups.

[0081] Non-limiting examples of suitable aromatic sulfonic acids include naphthalenesulfonic acid, dodecylbenzenesulfonic acid (DBSA), 4-methylbenzenesulfonic acid, naphthalene-2-sulfonic acid, 4-dodecylbenzenesulfonic acid, P-toluenesulfonic acid, 2,4,6-trimethylbenzenesulfonic acid, 2,4,6-trichlorobenzenesulfonic acid, naphthalene-2-sulfonic acid, naphthalene-1-sulfonic acid, 4-methylbenzenesulfonic acid, benzenesulfonic acid, substituted naphthalene-1-sulfonic acids, substituted naphthalene-2-sulfonic acids, 4-(tert-butyl)benzenesulfonic acid, and combinations thereof.

[0082] AS-ASAS has the following structure (I): [ka] In the formula, Y is an integer from 1 to 2 or 3; R 1 is selected from an aryl group, a substituted aryl group, an alkyl group, or a substituted alkyl group; R 2 is selected from an aryl group and a substituted aryl group; R 3 is selected from an aryl group, a substituted aryl group, an alkyl group, a substituted alkyl group, or hydrogen; R 4 is selected from aryl groups and substituted aryl groups, and X is an integer from 1 to 2, or 3, or 4.

[0083] In one embodiment, in structure (I): Y is 1 to 2, X is 1 to 2, or 1 to 3, or 1 to 4, and R 1 is C6-C 40 , or C6-C 20 , or C6-C 15 or a C6 aryl group; a substituted C6-C 40 , or C6-C 20 , or C6-C 15 or C6 aryl group; C1-C 40 , or C1-C 20 , or C1-C 10 or a C4-C8 alkyl group; or a substituted C1-C 20 , or C1-C 10 or a C4-C8 alkyl group; R 2 is C6-C 40 , or C6-C 20 , or C6-C 15 , or C6 aryl groups, and substituted C6-C 40 , or C6-C 20 , or C6-C 15 or a C6 aryl group; R 3 is C6-C 40 , or C6-C 20 , or C6-C 15 or a C6 aryl group; a substituted C6-C 40 , or C6-C 20 , or C6-C 15or C6 aryl group; C1-C 40 , or C1-C 20 , or C1-C 10 or a C4-C8 alkyl group; 40 , or C1-C 20 , or C1-C 10 or a C4-C8 alkyl group; or hydrogen; 4 is C6-C 40 , or C6-C 20 , or C6-C 15 , or C6 aryl groups, and substituted C6-C 40 , or C6-C 20 , or C6-C 15 or a C6 aryl group.

[0084] In one embodiment, the AS-ASAS has a sulfur to nitrogen molar ratio of 0.8:1, or from 1:1 to 1.3:1, In another embodiment, the AS-ASAS has a sulfur to nitrogen molar ratio of 1:1.

[0085] Non-limiting examples of suitable AS-ASAS are shown in Table C below and include structures (IV)-(XI), and combinations thereof. [Table 3]

[0086] In one embodiment, the AS-ASAS is selected from structure (IV), structure (V), structure (VI), structure (VII), structure (VIII), and structure (XI).

[0087] In one embodiment, the AS-ASAS is selected from structure (IV), structure (V), structure (VI), and structure (VII).

[0088] In one embodiment, the AS-ASAS is selected from structure (IX) and structure (X).

[0089] In one embodiment, the AS-ASAS is selected from structure (IV) and structure (IX).

[0090] In one embodiment, the AS-ASAS is selected from structure (VI), structure (VIII), structure (X), and structure (XI).

[0091] AS-ASAS is not polymeric, in other words, it is free or substantially free of dimers, trimers, and tetramers of aromatic amines.

[0092] In one embodiment, AS-ASAS is synthesized by mixing aromatic amines with aromatic sulfonic acids in an organic solvent or wax at room temperature (23-25° C.) for 1 hour, or 2-3 hours, or 4 hours, or 5 hours, or 6 hours. Non-limiting examples of suitable organic solvents include dichloromethane, toluene, and combinations thereof.

[0093] The aromatic amine-aromatic sulfonate (AA-ASAS) may comprise two or more embodiments disclosed herein.

[0094] D. Optional Additives In one embodiment, the composition comprises (A) a silane-functionalized ethylene-based polymer, (B) a hindered phenol antioxidant, (C) an aromatic amine-aromatic sulfonate, and (D) one or more optional additives.

[0095] Non-limiting examples of suitable optional additives include antioxidants (other than (B) hindered phenol antioxidants), colorants, corrosion inhibitors, lubricants, waxes, silanol condensation catalysts, ultraviolet (UV) absorbers or stabilizers, antiblocking agents, coupling agents, compatibilizers, plasticizers, fillers, processing aids, moisture scavengers, scorch retarders, metal deactivators, siloxanes, crosslinking aids, extending oils, and polyolefins (other than (A) silane-functionalized ethylene-based polymers), and combinations thereof.

[0096] In one embodiment, the composition includes an antioxidant different from the (B) hindered phenol antioxidant. A non-limiting example of a suitable antioxidant is a phosphite antioxidant, such as IRGAFOS™ 168 available from BASF. In one embodiment, the composition contains 0 wt.%, or 0.01 wt.% to 0.5 wt.%, or 1.0 wt.%, or 2.0 wt.%, or 3.0 wt.% of the antioxidant, based on the total weight of the composition.

[0097] In one embodiment, the composition comprises a wax. Wax can be used to reduce the melt viscosity of the composition. Non-limiting examples of suitable waxes include ethylene-based polymer waxes, propylene-based polymer waxes, paraffin waxes, microcrystalline waxes, by-product polyethylene waxes, Fischer-Tropsch waxes, oxidized Fischer-Tropsch waxes, functionalized waxes such as hydroxystearamide waxes and fatty acid amide waxes, and combinations thereof.

[0098] In one embodiment, the composition includes a silanol condensation catalyst, such as Lewis and Bronsted acids and bases. The "silanol condensation catalyst" promotes crosslinking of silanol-functionalized polyolefins. A Lewis acid is a chemical species that can accept an electron pair from a Lewis base. A Lewis base is a chemical species that can donate an electron pair to a Lewis acid. Non-limiting examples of suitable Lewis acids include tin carboxylates, such as dibutyltin dilaurate (DBTDL), and various other organometallic compounds, such as lead naphthenate, zinc caprylate, and cobalt naphthenate. Non-limiting examples of suitable Lewis bases include primary, secondary, and tertiary amines. These catalysts are typically used in moisture curing applications. In one embodiment, the composition includes 0 wt. %, or 0.001 wt. % to 0.1 wt. %, or 1.0 wt. % of a silanol condensation catalyst, based on the total weight of the composition. During the MONOSIL™ process, a silanol condensation catalyst is typically added to the reaction extruder so that it is present during the grafting reaction of the silane to the polyolefin backbone to form the Si-g-PE in situ. Thus, the silane-functionalized ethylene-based polymer may undergo some coupling (photocrosslinking) before exiting the extruder, and crosslinking is completed after it exits the extruder when it is exposed to moisture (e.g., sauna baths or cooling baths) and / or humidity typically present in the environment in which it is stored, transported, or used.

[0099] In one embodiment, the composition includes an ultraviolet (UV) light absorber or stabilizer. Non-limiting examples of suitable UV stabilizers include 1,3,5-triazine-2,4,6-triamine, N,N-1,2-ethanediylbisN-3-4,6-bisbutyl(1,2,2,6,6-pentamethyl-4-piperidinyl)amino-1,3,5-triazin-2-ylaminopropyl-N,N-dibutyl-N,N-bis(1,2,2,6,6-pentamethyl-4-piperidinyl)-1,5,8,12-tetrakis[4,6-bis(n-butyl-n-1,2,2,6,6-pentamethyl-4-piperidylamino)-1,3,5-triazin-2-yl]-1,5,8,12-tetraazadodecane (SABO SpA of Levate, Italy, available under the trademark SABO STAB). and hindered amine light stabilizers (HALS), such as UV-119 (commercially available as UV-119). In one embodiment, the composition contains 0 wt. %, or 0.001 wt. % to 0.01 wt. %, or 1.0 wt. %, or 3.0 wt. % of a UV absorber or stabilizer, based on the total weight of the composition.

[0100] In one embodiment, the composition includes a metal deactivator. The metal deactivator suppresses the catalytic activity of metal surfaces and trace metal minerals. The metal deactivator converts trace metals and metal surfaces to an inactive form, for example, by sequestering. Non-limiting examples of suitable metal deactivators include 1,2-bis(3,5-di-tert-butyl-4-hydroxyhydrocinnamoyl)hydrazine, 2,2'-oxamindobis[ethyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and oxalyl bis(benzylidene hydrazide) (OABH). In one embodiment, the composition contains 0% by weight, or greater than 0% by weight, or between 0.01% by weight and 0.05% by weight, or 1% by weight, or 10% by weight, of the metal deactivator, based on the total weight of the composition.

[0101] In one embodiment, the composition includes a filler. Non-limiting examples of suitable fillers include zinc oxide, zinc borate, zinc molybdate, zinc sulfide, carbon black, organoclay, and combinations thereof. The filler may or may not have flame retardant properties. In one embodiment, the filler is coated with a material (such as stearic acid) that prevents or retards the tendency of the filler to otherwise have to interfere with the silane cure reaction. In one embodiment, the composition contains 0 wt%, or 0.01 wt% to 1.0 wt%, or 3.0 wt%, or 5.0 wt% of the filler, based on the total weight of the composition.

[0102] In one embodiment, the composition includes a processing aid. Non-limiting examples of suitable processing aids include oils, organic acids (such as stearic acid), and metal salts of organic acids (such as zinc stearate). In one embodiment, the composition contains 0 wt.%, or 0.01 wt.% to 1.0 wt.%, or 3.0 wt.% of the processing aid based on the total weight of the composition.

[0103] In one embodiment, the composition includes a moisture scavenger. The moisture scavenger removes or inactivates unwanted water in the composition to prevent unwanted (premature) crosslinking and other water-initiated reactions in the composition during storage or extrusion conditions. Non-limiting examples of moisture scavengers include organic compounds selected from silanes such as orthoesters, acetals, ketals, or alkoxysilanes. In one embodiment, the moisture scavenger is an alkoxysilane (e.g., hexadecyltrimethoxysilane). The alkoxysilane moisture scavenger is not grafted or copolymerized to the polyolefin. The moisture scavenger is present in an amount of 0 wt%, or greater than 0 wt%, or between 0.01 wt% and 0.2 wt%, or 1.0 wt%, based on the total weight of the composition.

[0104] In one embodiment, the composition comprises a siloxane. A non-limiting example of a suitable siloxane is polydimethylsiloxane (PDMS), such as dimethylvinylsilyl-terminated polydimethylsiloxane. In one embodiment, the composition contains 0.2 wt.%, or 0.5 wt.% to 1.0 wt.%, or 5.0 wt.% of the siloxane, based on the total weight of the composition.

[0105] In one embodiment, the composition includes a crosslinking coagent. A "crosslinking coagent" is a substance that improves the crosslinking efficiency of the composition. A non-limiting example of a suitable crosslinking coagent is triallyl isocyanurate (TAIC). In one embodiment, the composition contains 0 wt.%, or greater than 0 wt.%, or 0.1 wt.% to 0.5 wt.%, or 1.0 wt.% of a crosslinking coagent based on the total weight of the composition.

[0106] In one embodiment, the composition includes a polyolefin different from (A) the silane-functionalized ethylene-based polymer. Non-limiting examples of suitable polyolefins include ethylene-based polymers, propylene-based polymers, and combinations thereof. Non-limiting examples of suitable ethylene-based polymers include LDPE, ethylene / ethyl acrylate (EEA) copolymers, and combinations thereof. In one embodiment, the polyolefin is not functionalized. In one embodiment, the composition contains 0 wt%, or 1 wt%, or 3 wt% to 5 wt%, or 10 wt%, or 15 wt%, or 20 wt%, or 50 wt%, or 70 wt% polyolefin based on the total weight of the composition. In another embodiment, the composition contains 1 wt% to 70 wt%, or 1 wt% to 10 wt%, or 1 wt% to 5 wt% polyolefin (such as LDPE and / or EEA copolymer) based on the total weight of the composition. In one embodiment, the polyolefin is a carrier polyolefin that is combined with (B) a hindered phenol antioxidant and / or (C) an AS-ASAS to form a catalyst masterbatch, and the catalyst masterbatch is then combined with (A) a silane-functionalized ethylene-based polymer to form the composition.

[0107] In one embodiment, the composition contains 0 wt.%, or greater than 0 wt.%, or between 0.001 wt.% and 0.01 wt.%, or 0.1 wt.%, or 0.5 wt.%, or 1.0 wt.%, or 2.0 wt.%, or 5.0 wt.%, or 10.0 wt.%, or 15.0 wt.%, or 20.0 wt.% of the additive based on the total weight of the composition.

[0108] The additive may comprise two or more embodiments disclosed herein.

[0109] E. Composition The composition contains (A) a silane-functionalized ethylene-based polymer, (B) a hindered phenol antioxidant, (C) an aromatic amine-aromatic sulfonate (AS-ASAS), and, optionally, (D) an additive. In one embodiment, the AS-ASAS has the structure (I):

[0110] In one embodiment, the composition is a crosslinkable composition. In a further embodiment, the composition is a moisture-curable composition. In other words, the composition can crosslink when exposed to moisture (e.g., sauna bath or cold bath) and / or moisture present in the environment in which it is stored, transported, or used. Moisture-curing conditions include the presence of water (e.g., as moisture present in a bath or environment) and a temperature of 20°C, or 23°C to 25°C to 30°C.

[0111] In one embodiment, the composition is a crosslinked composition. The crosslinked composition is formed by crosslinking the crosslinkable composition. In one embodiment, crosslinking of the crosslinkable polymer composition begins in an extruder. In another embodiment, crosslinking is delayed until the crosslinkable composition is extruded, such as onto a conductor. Crosslinking of the crosslinkable composition is initiated and / or accelerated through exposure to a moist environment (e.g., curing at ambient conditions or in a sauna or water bath). In one embodiment, crosslinking of the crosslinkable composition is initiated and / or accelerated through exposure to moisture. The crosslinked composition comprises bonds between silane-functionalized ethylene-based polymer chains.

[0112] In one embodiment, the composition contains, consists essentially of, or consists of (A) a silane-functionalized ethylene-based polymer, (B) a hindered phenol antioxidant, (C) an AS-ASAS, and, optionally, (D) an additive.

[0113] In one embodiment, the composition contains 30%, or 40%, or 50%, or 60%, or 70%, or 80%, or 90% to 95%, or 97%, or 98%, or 99% by weight of the silane-functionalized ethylene-based polymer, based on the total weight of the composition.

[0114] In one embodiment, the composition contains 0.03 wt.%, or 0.05 wt.%, or 0.09 wt.% to 0.10 wt.%, or 0.2 wt.%, or 0.5 wt.%, or 1.0 wt.% of a hindered phenol antioxidant based on the total weight of the composition.

[0115] In one embodiment, the composition contains 0.05%, or 0.08%, or 0.10%, or 0.11% to 0.16%, or 0.20%, or 0.50%, or 1.0%, or 2.0%, or 3.0%, or 4.0%, or 5.0% by weight of AS-ASAS, based on the total weight of the composition.

[0116] In one embodiment, the composition comprises, based on the total weight of the composition, (A) 30 wt% to 99 wt%, or 50 wt% to 99 wt%, or 80 wt% to 99 wt%, or 90 wt% to 99 wt%, or 90 wt% to 95 wt% of a functionalized ethylene-based polymer (such as an ethylene / silane copolymer); (B) 0.03 wt% to 1.0 wt%, or 0.03 wt% to 0.5 wt%, or 0.05 wt% to 0.2 wt%, or 0.09 wt% to 0.10 wt% of a hindered phenyl group. % of an AS-ASAS having structure (I), and (D) from 0 to 20 wt. %, or from greater than 0 to 20 wt. %, or from greater than 0 to 10 wt. % of an additive. In a further embodiment, the composition is a crosslinkable composition.

[0117] In one embodiment, the composition has a high temperature creep of less than 160%, or less than 130%, or less than 110%, or less than 100%, or less than 50%, or 0%, or 40% to 50%, or 100%, or 110%, or 120%, or 160%, after curing in a water bath at 90° C. for 1 hour. In one embodiment, the composition has a high temperature creep of less than 150%, or less than 130%, or less than 110%, or less than 100%, or less than 80%, or less than 70%, or less than 40%, or 0%, or 20%, or 30% to 40%, or 70%, or 80%, or 100%, or 110%, or 130%, or 150%, after curing in a water bath at 90° C. for 3 hours. In one embodiment, the composition has a high temperature creep of less than 150%, or less than 100%, or less than 80%, or 0%, or less than 20%, or 50%, or 70%-75%, or 80%, or 100%, or 150%, after curing in a 90° C. water bath for 6 hours.

[0118] In one embodiment, the composition has a high temperature creep of less than 100%, or less than 70%, or 0%, or 20%, or 50% to 70%, or 100% after 69 hours of ambient curing. In one embodiment, the composition has a high temperature creep of less than 110%, or less than 100%, or less than 80%, or 0%, or 20%, or 50% to 70%, or 105%, or 110% after 90 hours of ambient curing. In one embodiment, the composition has a high temperature creep of less than 140%, or 0%, or 20%, or 50%, or 70% to 130%, or 150% after 100 hours of ambient curing. In one embodiment, the composition has a high temperature creep of less than 140%, or less than 100%, or less than 90%, or less than 60%, or 0%, or 20%, or 50% to 60%, or 95%, or 100%, or 130%, or 140% after curing at ambient for 168 hours. In one embodiment, the composition has a high temperature creep of less than 100%, or less than 80%, or less than 60%, or less than 55%, or 0%, or 20% to 55%, or 60%, or 80%, or 100% after curing at ambient for 230 hours.

[0119] In one embodiment, the composition has a high temperature creep in a 90° C. water bath of (i) less than 160%, or less than 130%, or less than 110%, or less than 100%, or less than 50% after 1 hour of curing, and / or (ii) less than 150%, or less than 130%, or less than 110%, or less than 100%, or less than 80%, or less than 70%, or less than 40% after 3 hours of curing, and / or (iii) less than 150%, or less than 100%, or less than 80% after 6 hours of curing. In one embodiment, the composition has a high temperature creep at ambient conditions of (i) less than 100%, or less than 70% after 69 hours of cure, and / or (ii) less than 110%, or less than 100%, or less than 80% after 90 hours of cure, and / or (iii) less than 140% after 100 hours of cure, and / or (iv) less than 140%, or less than 100%, or less than 90%, or less than 60% after 168 hours of cure, and / or (v) less than 100%, or less than 80%, or less than 60%, or less than 55% after 230 hours of cure. Low high temperature creep is advantageous for wire and cable applications because it indicates that the composition is crosslinked (i.e., cured).

[0120] In one embodiment, the AS-ASAS, the hindered phenol antioxidant, and the carrier polyolefin are combined to form a masterbatch. The masterbatch is then combined with a silane-functionalized ethylene-based polymer to form a composition. In one embodiment, the masterbatch (also referred to as a "catalyst masterbatch") contains, based on the total weight of the masterbatch, (i) 0.05 wt.%, or 0.10 wt.%, or 0.50 wt.%, or 1.0 wt.%, or 2.0 wt.%, or 2.3 wt.% to 3.2 wt.%, or 4.0 wt.%, or 5.0 wt.%, or 10 wt.% AS-ASAS; (ii) 0.03 wt.%, or 0.05 wt.%, or 0.10 wt.%, or 0.50 wt.%, or 1.0 wt.%, or 2.0 wt.%, or 2.3 wt.% to 3.2 wt.%, or 4.0 wt.%, or 5.0 wt.%, or 10 wt.% AS-ASAS; %, or 1.0 wt%, or 1.50 wt%, or 1.90 wt% to 2.0 wt%, or 3.0 wt%, or 4.0 wt% of a hindered phenol antioxidant, and (iii) 86 wt%, or 90 wt%, or 94 wt% to 96 wt%, or 99 wt%, or 99.92 wt% of a carrier polyolefin (such as an EEA copolymer and / or LDPE). In a further embodiment, the carrier polyolefin is a blend of an EEA copolymer and LDPE in a 1:1 weight ratio, based on the total weight of the blend.

[0121] In one embodiment, the composition or masterbatch exhibits at least 50% isobutylene reduction compared to the same composition or masterbatch containing the aromatic sulfonic acid of the aromatic amine-aromatic sulfonate salt instead of the salt, as measured by HSGC using Sample Preparation Method 1. In another embodiment, the composition or masterbatch exhibits at least 50% isobutylene reduction compared to the same composition or masterbatch containing the aromatic sulfonic acid of the aromatic amine-aromatic sulfonate salt instead of the salt, as measured by HSGC using Sample Preparation Method 2.

[0122] In one embodiment, the composition, or masterbatch, has a molecular weight of less than 6,000,000 per gram (g) as measured by HSGC using Sample Preparation Method 1. -1 ), or 5,000,000g -1 Less than or 4,000,000g -1 Less than or 0g -1 ~6,000,000g -1 , or 1,000g -1 ~6,000,000g -1 , or 500,000g -1 ~6,000,000g -1 , or 500,000g -1 ~5,000,000g -1 The isobutylene generation peak area is 1.018.

[0123] In one embodiment, the composition, or masterbatch, has a 1.4×10 mercury per mole sulfur content as measured by HSGC using Sample Preparation Method 1. 11 Less than (mol -1 ), or 1.2×10 11 Mole -1 Less than or 1.0×10 11 Mole -1 Less than or 5.0 x 10 10 Mole -1 Less than or 0 moles -1 ~1.4x10 11 Mole -1 , or 1.0×10 7 Mole -1 ~1.4×10 11 Mole -1 , or 1.0×10 10 Mole -1 ~1.4×10 11 Mole -1 The isobutylene generation peak area is 1.018.

[0124] In one embodiment, the composition, or masterbatch, has a molecular weight of less than 1,000,000 per gram (g) as measured by HSGC using Sample Preparation Method 2. -1 ) or 100,000g-1 Less than or 80,000g -1 Less than or 75,000g -1 Less than or 0g -1 ~1,000,000g -1 , or 100g -1 ~100,000g -1 , or 100g -1 ~80,000g -1 , or 100g -1 ~75,000g -1 The isobutylene generation peak area is 1.018.

[0125] In one embodiment, the composition, or masterbatch, has a 1.8×10 mercury per mole sulfur content as measured by HSGC using Sample Preparation Method 2. 9 Less than (mol -1 ), or 1.7×10 9 Mole -1 Less than or equal to 1.6×10 9 Mole -1 Less than or equal to 1.5 x 10 9 Mole -1 Less than or 0 moles -1 ~1.8x10 9 Mole -1 , or 1.0×10 6 Mole -1 ~1.80×10 9 Mole -1 , or 1.0×10 6 Mole -1 ~1.70×10 9 Mole -1 The isobutylene generation peak area is 1.018.

[0126] Since isobutylene is toxic, the amount of isobutylene generated is small (for example, 6,000,000 g when measured by HSGC using sample preparation method 1). -1 Peak area less than 1.4 x 10 11 Mole -1The reduction in isobutylene generation is advantageously greater than 100% (peak area less than 100%). Thus, the reduction in isobutylene generation leads to improved safety in handling the compositions and masterbatches, as well as reduced production costs. Moreover, isobutylene is generated in the compositions and masterbatches of the present invention as a result of the decomposition of the hindered phenolic antioxidant. Thus, the reduction in isobutylene generation indicates that the decomposition of the hindered phenolic antioxidant is advantageously reduced or avoided.

[0127] In one embodiment, the composition comprises: (i) 1 wt. % to 5 wt. %, or 10 wt. %, or 20 wt. %, or 40 wt. %, or 50 wt. % of a catalyst masterbatch, based on the total weight of the composition, and (a) 0.05 wt. %, or 0.10 wt. %, or 0.50 wt. %, or 1.0 wt. %, or 2.0 wt. %, or 2.3 wt. % to 3.2 wt. %, or 4.0 wt. %, or 5.0 wt. %, or 10 wt. % of an AS-ASAS (such as an AS-ASAS having structure (I) and a 1:1 molar ratio of sulfur to nitrogen), based on the total weight of the masterbatch; (b) 0.03 wt. %, or 0.50 wt. %, or 1.0 wt. %, or 2.0 wt. %, or 2.3 wt. % to 3.2 wt. %, or 4.0 wt. %, or 5.0 wt. %, or 10 wt. % of an AS-ASAS (such as an AS-ASAS having structure (I) and a 1:1 molar ratio of sulfur to nitrogen), based on the total weight of the masterbatch; %, or 0.05%, or 0.10%, or 0.50%, or 1.0%, or 1.50%, or 1.90% to 2.0%, or 3.0%, or 4.0% by weight of a hindered phenol antioxidant; and (c) 86%, or 90%, or 94% to 96%, or 99%, or 99.92% by weight of a carrier polyolefin (such as an EEA copolymer and / or LDPE); (ii) containing, consisting essentially of, or consisting of 50%, or 60%, or 80%, or 90%, or 95% to 99% by weight of a silane-functionalized ethylene-based polymer (e.g., an ethylene / silane copolymer); The catalyst masterbatch has the following properties: (a) at least a 50% isobutylene reduction as measured by HSGC using Sample Preparation Method 1, compared to the same masterbatch containing an aromatic sulfonic acid of an aromatic amine-aromatic sulfonate salt instead of the salt, and / or (b) at least a 50% isobutylene reduction as measured by HSGC using Sample Preparation Method 2, compared to the same masterbatch containing an aromatic sulfonic acid of an aromatic amine-aromatic sulfonate salt instead of the salt, and / or (c) at least a 50% isobutylene reduction as measured by HSGC using Sample Preparation Method 1, compared to the same masterbatch containing an aromatic sulfonic acid of an aromatic amine-aromatic sulfonate salt instead of the salt, and / or (d) at least a 50% isobutylene reduction as measured by HSGC using Sample Preparation Method 2, compared to the same masterbatch containing an aromatic sulfonic acid of an aromatic amine-aromatic sulfonate salt instead of the salt, -1 ~6,000,000g -1 , or 1,000g -1 ~6,000,000g -1 , or 500,000g -1 ~6,000,000g -1 , or 500,000g -1 ~5,000,000g -1 and / or (d) an isobutylene onset peak area of ​​0 mol% or less when measured by HSGC using Sample Preparation Method 1. -1 ~1.4×10 11 Mole -1 , or 1.0×10 7 Mole -1 ~1.4×10 11 Mole -1 , or 1.0×10 10 Mole -1 ~1.4×10 11 Mole -1 and / or (e) an isobutylene generation peak area of ​​0 g when measured by HSGC using Sample Preparation Method 2. -1 ~1,000,000g -1 , or 100g -1 ~100,000g -1 , or 100g -1 ~80,000g -1 , or 100g -1 ~75,000g -1 and / or (f) an isobutylene onset peak area of ​​0 mol% or less when measured by HSGC using Sample Preparation Method 2. -1 ~1.8×10 9Mole -1 , or 1.0×10 6 Mole -1 ~1.80×10 9 Mole -1 , or 1.0×10 6 Mole -1 ~1.70×10 9 Mole -1 and having one, some, or all of the isobutylene onset peak areas: The composition has the following properties: (A) in a 90° C. water bath, (A1) after 1 hour cure, less than 160%, or less than 130%, or less than 110%, or less than 100%, or less than 50% and / or (A2) after 3 hours cure, less than 150%, or less than 130%, or less than 110%, or less than 100%, or less than 80%, or less than 70%, or less than 40%, and / or (A3) after 6 hours cure, less than 150%, or less than 100%, or less than 80%, and / or (B) in an ambient environment, (B1) and / or (B1) less than 100%, or less than 70%, after 69 hours cure, and / or (B2) less than 110%, or less than 100%, or less than 80%, after 90 hours cure, and / or (B3) less than 140%, or less than 100%, or less than 90%, or less than 60%, after 168 hours cure, and / or (B5) less than 100%, or less than 80%, or less than 60%, or less than 55%, after 230 hours cure.

[0128] It is understood that the sum of the components in each of the above compositions totals 100 weight percent (wt %).

[0129] In one embodiment, the composition is free or substantially free of propylene-based polymers, such as silane-functionalized propylene-based polymers and maleic acid-functionalized propylene-based polymers.

[0130] In one embodiment, the composition is free or substantially free of sulfonate esters and / or esters of sulfonic acids.

[0131] In one embodiment, the composition is free or substantially free of epoxy resins.

[0132] The composition may comprise two or more embodiments disclosed herein.

[0133] F. Coated Conductor The present disclosure provides a coated conductor comprising a conductor and a coating on the conductor, the coating comprising a composition containing (A) a silane-functionalized ethylene-based polymer, (B) a hindered phenol antioxidant, (C) an AS-ASAS, and, optionally, (D) an additive.

[0134] The composition can be any composition disclosed herein.

[0135] In one embodiment, the composition is a crosslinked composition.

[0136] In one embodiment, the coating is an insulating sheath for the conductor, hi another embodiment, the coating is a jacket for the conductor.

[0137] The process for making coated conductors includes heating the composition to at least the melting temperature of the silane-functionalized ethylene-based polymer and then extruding the polymer melt blend onto the conductor. The term "on" includes direct or indirect contact between the polymer melt blend and the conductor. The polymer melt blend is in an extrudable state. During and / or after extrusion, crosslinking occurs to form a crosslinked composition.

[0138] The coating is on the conductor. The coating can be one or more inner layers, such as an insulating layer. The coating can cover or otherwise surround or encase the conductor in whole or in part. The coating can be the only component surrounding the conductor. If the coating is the only component surrounding the conductor, the coating can function as a jacket and / or insulation. In one embodiment, the coating is the outermost layer of the coated conductor. Alternatively, the coating can be one layer of a multi-layer jacket or sheath that encases the metal conductor. In one embodiment, the coating is in direct contact with the conductor. In another embodiment, the coating is in direct contact with an insulating layer that surrounds the conductor.

[0139] In one embodiment, the coating is in direct contact with the conductor. As used herein, the term "direct contact" refers to a coating configuration in which the coating is disposed directly adjacent to the conductor, the coating contacts the conductor, and no intervening layers, coatings, and / or structures are present between the coating and the conductor.

[0140] In one embodiment, the coating is in indirect contact with the conductor. As used herein, the term "indirect contact" refers to a coating configuration in which an intervening layer, coating, or structure is between the coating and the conductor. Non-limiting examples of suitable intervening layers, coatings, and structures include an insulating layer, a moisture barrier, a buffer tube, and combinations thereof. Non-limiting examples of suitable insulating layers include a foamed insulating layer, a thermoplastic insulating layer, a cross-linked insulating layer, and combinations thereof.

[0141] In one embodiment, the composition contains carbon black and the coating is a semiconductive layer on a conductor.

[0142] The coating is crosslinked. In one embodiment, crosslinking of the crosslinkable composition begins in the extruder, but only to a small extent. In another embodiment, crosslinking is delayed until the crosslinkable composition is extruded onto the conductor. Crosslinking of the crosslinkable polymer composition can be initiated and / or accelerated through exposure to a moist environment (e.g., curing at ambient conditions or in a sauna or water bath). In one embodiment, crosslinking of the crosslinkable composition is initiated and / or accelerated through exposure to moisture.

[0143] In one embodiment, the coated conductor is selected from fiber optic cable, communication cable (such as a telephone cable, a local area network (LAN) cable, or a small form factor pluggable (SFP) cable), power cable, wiring for consumer electronics, charger wires for mobile phones and / or computers, computer data cords, power cords, internal equipment wiring materials, interior wiring materials, consumer electronics accessory cords, and any combination thereof.

[0144] The coated conductor may include two or more embodiments disclosed herein.

[0145] G. Process The present disclosure provides a process for moisture curing a silane-functionalized ethylene-based polymer, the process including: (A) providing an aromatic amine-aromatic sulfonate (AS-ASAS), (B) mixing the aromatic amine-aromatic sulfonate with a hindered phenol antioxidant to form a catalyst composition, (C) contacting the silane-functionalized ethylene-based polymer with the catalyst composition to form a crosslinkable composition, and (D) exposing the crosslinkable composition to moisture cure conditions to form a crosslinked composition.

[0146] Moisture cure conditions include the presence of water (eg, as moisture present in a bath or environment) and a temperature of 20°C, or 23°C to 25°C to 30°C.

[0147] In one embodiment, (B) mixing the AS-ASAS with the hindered phenol antioxidant to form the catalyst composition and (C) contacting the silane-functionalized ethylene-based polymer with the catalyst composition to form the crosslinkable composition occur simultaneously. In other words, the AS-ASAS, the hindered phenol antioxidant, and the silane-functionalized ethylene-based polymer are blended simultaneously to form the crosslinkable composition.

[0148] In one embodiment, mixing (B) AS-ASAS with a hindered phenol antioxidant to form a catalyst composition includes forming a masterbatch containing, consisting essentially of, or consisting of (i) an AS-ASAS having a 1:1 molar ratio of sulfur to nitrogen (such as an AS-ASAS having structure (I)), (ii) a hindered phenol antioxidant, and (iii) a carrier polyolefin. The masterbatch and carrier polyolefin can be any respective masterbatch (also referred to as a catalyst masterbatch) and carrier polyolefin disclosed herein. In one embodiment, the carrier polyolefin is a blend of an EEA copolymer and LDPE.

[0149] In one embodiment, the process involves synthesizing AS-ASAS by mixing an aromatic amine with an aromatic sulfonic acid in an organic solvent or wax at room temperature (23-25° C.) for 1 hour, or 2-3 hours, or 4 hours, or 5 hours, or 6 hours. Non-limiting examples of suitable organic solvents include dichloromethane, toluene, and combinations thereof.

[0150] The process may include two or more embodiments disclosed herein.

[0151] By way of example and not by way of limitation, several embodiments of the present disclosure will now be detailed in the following examples. EXAMPLES

[0152] The materials used in the examples are provided in Table 1 below. [Table 4]

[0153] A. Synthesis of catalyst salt The catalyst salts in Table 2 are synthesized by combining 10 mmol of amine with 10 mmol of acid in a reaction flask containing 100 mL of dichloromethane. For amines containing multiple amino groups, the amount of acid in the reaction mixture is varied to achieve the desired stoichiometric ratio between the sulfonic acid and amino groups.

[0154] Stir the reaction mixture at room temperature (23-25 ​​°C) for 2 h. Then evaporate the solution at 35 °C for 15 min using a rotary evaporator under reduced pressure of 0.1 MPa to obtain the catalyst salt solid product, which is vacuum-dried at room temperature (23-25 ​​°C) for 6 h.

[0155] The amines, acids, and resulting catalyst salts are provided in Table 2. As shown in Table 2, Example Salts 1-4, Example Salt 7, Example Salt 9, Example Salt 11, and Example Salt 15 are each AA-ASAS.

[0156] B. Preparation of Catalyst Salt Masterbatch and Pelletization DXM-205 (EEA copolymer) and DXM-446 (LDPE) are fed in equal amounts (i.e., 1:1 weight ratio) to a Brabender mixer set at a temperature of 120° C. and a rotation speed of 15 revolutions per minute (rpm). One of the catalyst salts from Table 2 and IRGANOX™ 1010 (hindered phenol antioxidant) are then fed to the mixer and the masterbatch composition is mixed for 3 minutes at a temperature of 120° C. and a rotation speed of 50 rpm.

[0157] After mixing, the catalyst salt masterbatch is fed into a Brabender single screw extruder set at 120° C. and pelletized.

[0158] Each catalyst salt master batch contains 4.4 mmol / 100 g of sulfonic acid groups based on the respective catalyst salt master batch. The composition of each catalyst salt master batch is provided in Table 3 below.

[0159] The catalyst salt masterbatches in Table 3 are measured for isobutylene by HSGC or by GC after Sample Preparation Method 1 or Sample Preparation Method 2 described above in the Test Methods section. The results are provided below in Tables 4A and 4B. "NM" in the tables indicates that the value was not measured.

[0160] As shown in Table 4B, catalyst master batch MB21 (containing DBSA) generates twice the amount of isobutylene as catalyst master batch MB19 (containing naphthalene sulfonic acid) as measured by GC and sample preparation method 2. This suggests that DBSA tends to degrade hindered phenol antioxidants at a faster rate than naphthalene sulfonic acid. However, as shown in Table 4A, catalyst master batch MB2 (containing AA-ASAS formed using example salt 2, DBSA and NAUGARD™ 445) surprisingly generates much less isobutylene compared to catalyst master batch MB19 (containing naphthalene sulfonic acid). Without wishing to be bound by any particular theory, it is believed that at least 50% isobutylene reduction can be achieved by using aromatic amine-aromatic sulfonate salts instead of the corresponding sulfonic acids. [Table 5-1] [Table 5-2] [Table 6] [Table 7] [Table 8]

[0161] C. Preparation of the Composition SI-LINK™ DFDA-5451 NT (ethylene / silane copolymer) pellets and catalyst salt masterbatch (Table 3) pellets are dry blended to form a dry blend of 95 wt. % SI-LINK™ DFDA-5451 NT and 5 wt. % catalyst salt masterbatch, based on the total weight of the dry blend. The dry blend is fed into a Brabender single screw extruder set at 160° C. and mixed until the composition is in a molten form. The composition is then extruded into a tape having a thickness of 1 mm.

[0162] At least one tape per sample is placed in a water bath set at a temperature of 90° C. The samples are left in the water bath for 1 hour, 3 hours, and 6 hours before being tested for high temperature creep. Sample compositions that are crosslinkable are cured in the water bath.

[0163] At least one tape per sample is placed on a bench in an ambient environment (room temperature 23-25°C, 50% relative humidity). The samples are left in the ambient environment for 69, 90, 100, 168, and 230 hours and then tested for high temperature creep. Sample compositions that are crosslinkable are cured in the ambient environment.

[0164] The composition of each sample, and the results are provided in Table 5 below.

[0165] As shown in Table 5, CS6, CS8, CS13, and CS14 each contain (A) an ethylene / silane copolymer (SI-LINK™ DFDA-5451 NT), (B) a hindered phenol antioxidant (IRGANOX™ 1010), and (C) an aromatic amine-linear sulfonate (CS salt 6, CS salt 8, CS salt 13, and CS salt 14). CS6, CS8, CS13, and CS14 each lack aromatic amine-aromatic sulfonate. CS6, CS8, CS13, and CS14 each failed during high temperature creep testing at all lengths of time - indicating that the compositions are not cured. As a result, CS6, CS8, CS13, and CS14 are not moisture crosslinkable compositions. [Table 9-1] [Table 9-2]

[0166] CS16 and CS17 each contain (A) an ethylene / silane copolymer (SI-LINK™ DFDA-5451 NT), (B) a hindered phenol antioxidant (IRGANOX™ 1010), and (C) a linear amine-aromatic sulfonate (CS salt 16 and CS salt 17). CS16 and CS17 each lack the aromatic amine-aromatic sulfonate. CS16 and CS17 each failed during high temperature creep testing at all lengths of time - indicating that the compositions are not cured. As a result, CS16 and CS17 are not moisture crosslinkable compositions.

[0167] CS18 contains (A) an ethylene / silane copolymer (SI-LINK™ DFDA-5451 NT), (B) a hindered phenol antioxidant (IRGANOX™ 1010), and (C) a polymeric aromatic amine-aromatic sulfonate (CS salt 18). CS18 is devoid of non-polymeric aromatic amine-aromatic sulfonate. CS18 failed during high temperature creep testing at all lengths of time - indicating that the composition is not cured. As a result, CS18 is not a moisture crosslinkable composition.

[0168] CS19 contains (A) an ethylene / silane copolymer (SI-LINK™ DFDA-5451 NT), (B) a hindered phenol antioxidant (IRGANOX™ 1010), and (C) an aromatic sulfonic acid (NACURE™ B201). CS19 lacks aromatic amine-aromatic sulfonate. As shown in Tables 4A and 4B, the catalyst master batch contained in CS19 (MB19) exhibits an isobutylene onset peak area of ​​greater than 6,000,000 per gram (8,190,000 per gram) as measured by HSGC and Sample Preparation Method 1. As a result, the production and handling of CS19 is hazardous.

[0169] CS10, CS12, and CS14 each contain (A) an ethylene / silane copolymer (SI-LINK™ DFDA-5451 NT), (B) a hindered phenol antioxidant (IRGANOX™ 1010), and (C) an aromatic amine-aromatic sulfonate salt (CS salt 10, CS salt 12, and CS salt 14) having a sulfur to nitrogen molar ratio of greater than 1.3:1 (2:1). CS10, CS12, and CS14 each failed during high temperature creep testing at all lengths of time - indicating that the compositions are not cured. As a result, CS10, CS12, and CS14 are not moisture crosslinkable compositions.

[0170] In contrast, compositions containing (A) an ethylene / silane copolymer (SI-LINK™ DFDA-5451 NT), (B) a hindered phenol antioxidant (IRGANOX™ 1010), and (C) an aromatic amine-aromatic sulfonate salt having a sulfur to nitrogen molar ratio of greater than 1:1 (Examples 1-4, 7, 9, 11, and 15) surprisingly exhibit favorable high temperature creep (e.g., high temperature creep of 130% or less after 168 hours of ambient storage) (indicating the compositions are crosslinkable) while exhibiting safe levels of isobutylene generation (e.g., isobutylene generation peak area of ​​less than 6,000,000 per gram as measured by HSGC and Sample Preparation Method 1). It is expressly intended that the present disclosure is not limited to the embodiments and examples contained herein, but includes modifications of these embodiments, including portions of the embodiments and combinations of elements of different embodiments, as falling within the scope of the following claims. (Aspect) (Aspect 1) 1. A composition comprising: (A) a silane-functionalized ethylene-based polymer; (B) a hindered phenol antioxidant; and (C) an aromatic amine-aromatic sulfonate salt. (Aspect 2) the aromatic amine-aromatic sulfonate salt having the structure (I): [ka] In the formula, Y is an integer of 1 to 3, R 1 is selected from the group consisting of an aryl group, a substituted aryl group, an alkyl group, or a substituted alkyl group; R 2 is selected from the group consisting of aryl groups and substituted aryl groups; R 3 is selected from the group consisting of an aryl group, a substituted aryl group, an alkyl group, a substituted alkyl group, or hydrogen; R 4 is selected from the group consisting of aryl groups and substituted aryl groups; 2. The composition of embodiment 1, wherein X is an integer from 1 to 4. (Aspect 3) 3. The composition of any one of the preceding claims, wherein the aromatic amine-aromatic sulfonate has a sulfur to nitrogen molar ratio of 1:1. (Aspect 4) The composition of any one of the preceding embodiments, wherein the silane-functionalized polyolefin is selected from the group consisting of silane-grafted ethylene-based polymers and ethylene / silane copolymers. (Aspect 5) (A) 30% to 99% by weight of a silane-functionalized ethylene-based polymer; (B) 0.03 wt % to 1 wt % of a hindered phenol antioxidant; and (C) 0.05% by weight to 5% by weight of an aromatic amine-aromatic sulfonate salt. (Aspect 6) The composition of any one of aspects 1 to 5, wherein the composition is crosslinkable. (Aspect 7) 7. The composition of any one of the preceding claims, wherein the composition has a high temperature creep of less than 100% after curing in a 90° C. water bath for 3 hours. (Aspect 8) 8. The composition of any one of the preceding claims, wherein the composition has a high temperature creep of less than 100% after curing at ambient for 168 hours. (Aspect 9) The composition of any one of the preceding aspects, wherein the composition exhibits at least 50% isobutylene reduction as compared to the same composition containing an aromatic sulfonic acid of the aromatic amine-aromatic sulfonate salt instead of a salt. (Aspect 10) A coated conductor comprising: A conductor; a coating on the conductor, the coating comprising the composition according to any one of embodiments 1 to 9. (Aspect 11) 1. A process for moisture curing a silane-functionalized ethylene-based polymer comprising: (A) providing an aromatic amine-aromatic sulfonate salt; (B) mixing the aromatic amine-aromatic sulfonate salt with a hindered phenol antioxidant to form a catalyst composition; (C) contacting a silane-functionalized ethylene-based polymer with said catalyst composition to form a crosslinkable composition; (D) exposing the crosslinkable composition to moisture cure conditions to form a crosslinked composition. (Aspect 12) The process of embodiment 11, wherein the mixing of (B) and the contacting of (C) occur simultaneously. (Aspect 13) The mixing of (B) the aromatic amine-aromatic sulfonate salt; the hindered phenol antioxidant; 12. The process of embodiment 11, comprising forming a masterbatch comprising: (Aspect 14) (A) providing the aromatic amine-aromatic sulfonate salt having structure (I),

change

Claims

1. 1. A process for moisture curing a silane-functionalized ethylene-based polymer having hydrolyzable silane groups, comprising: (A) providing an aromatic amine-aromatic sulfonate salt; (B) mixing the aromatic amine-aromatic sulfonate salt with a hindered phenol antioxidant to form a catalyst composition; (C) contacting a silane-functionalized ethylene-based polymer with said catalyst composition to form a crosslinkable composition; (D) exposing the crosslinkable composition to moisture cure conditions to form a crosslinked composition; The aromatic amine-aromatic sulfonate has one or a combination of the following structures (IV) to (XI): 【Chemistry 1】 The aromatic amine-aromatic sulfonate has a sulfur to nitrogen molar ratio of from 0.8:1 to 1.3:

1.

2. 2. The process of claim 1, wherein said mixing of (B) and said contacting of (C) occur simultaneously.

3. The mixing of (B) the aromatic amine-aromatic sulfonate salt; the hindered phenol antioxidant; 10. The process of claim 1 comprising forming a masterbatch comprising:

4. 4. The process of any one of claims 1 to 3, comprising: (A) providing said aromatic amine-aromatic sulfonate salt having a sulfur to nitrogen molar ratio of 1:1.

Citation Information

Patent Citations

  • Moisture Crosslinkable Polymer Compositions - Improved Heat Aging Performance

    JP2008533280A

  • Semi-crystalline polyolefin-based additive masterbatch composition

    WO2018085241A1