Coating for forming light diffusion layer, film for projection screen, and projection screen

A paint with a base resin and rare earth phosphate fine particles forms a light diffusion layer, addressing the balance of transparency and image display issues in projection screens, providing wide viewing angles and minimal chromatic aberration.

JP7561954B2Active Publication Date: 2024-10-04RIKEN TECHNOS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023213436
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-06
Filing Date
2023-12-19
Publication Date
2024-10-04
Estimated Expiration
2039-11-06

AI Technical Summary

Technical Problem

Existing projection screen films struggle to achieve a balance between high transparency, wide viewing angle, and resistance to chromatic aberration while maintaining clear image display performance.

Method used

A paint formulation containing a base resin and rare earth phosphate fine particles, optionally with a silane coupling agent and a compound with an isocyanate group and polymerizable functional groups, is used to form a light diffusion layer that enhances transparency and image display performance.

Benefits of technology

The paint achieves a projection screen with excellent transparency, wide viewing angle, and minimal chromatic aberration, suitable for use in transparent media like glass windows.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561954000003
    Figure 0007561954000003
  • Figure 0007561954000004
    Figure 0007561954000004
  • Figure 0007561954000005
    Figure 0007561954000005
Patent Text Reader

Abstract

To provide a coating material for forming a light diffusion layer, which is a coating material capable of obtaining a projection screen excellent in balance between high transparency and high video display performance, and also to provide a film for the projection screen including the light diffusion layer formed using the coating material, and the projection screen.SOLUTION: Disclosed is a coating material for forming a light diffusion layer of a projection screen, which includes: (A)100 parts by mass of a base resin; and (B) 0.1 to 50 parts by mass of a rare earth phosphate fine particle, and further, preferably contains: (C) 1 to 30 parts by mass of silane coupling agent, and (D) 1 to 30 parts by mass of a compound having an isocyanate group and a polymerizable functional group other than the isocyanate group based on 100 parts by mass of rare earth phosphate fine particles. A component of (A) the base resin preferably contains (A1) polyfunctional poly (meth) acrylate.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating material for forming a light diffusion layer, a film for a projection screen, and a projection screen. More specifically, the present invention relates to a coating material used for forming a light diffusion layer of a projection screen, a film for a projection screen including a light diffusion layer formed using the coating material, and a projection screen. [Background technology]

[0002] In recent years, a transparent projection screen film has been attached to a medium having translucent visibility, such as glass windows and glass-covered display shelves in commercial facilities such as convenience stores, supermarkets, shopping centers, and department stores; and glass partitions in event venues. Video content such as products, services, and news is projected and displayed on the projection screen film when desired, while usually maintaining translucent visibility. A projection screen film for such use is required to have both conflicting characteristics, namely, high translucent visibility (high transparency) and a clear view of the projected and displayed image (high image displayability). In addition, a wide angle (a wide viewing angle) at which the projected and displayed image can be clearly viewed (the angle at which the projection screen is viewed), no chromatic aberration occurs in the projected and displayed image, and the projection screen film itself is required to have no color. Many proposals have been made for a transparent projection screen film (for example, Patent Documents 1 and 2). However, these technologies were not sufficiently satisfactory as a projection screen film for use as described above. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-212800 A [Patent Document 2] JP 2017-215355 A [Patent Document 3] International Publication No. 2018 / 025800 [Patent Document 4] JP 2014-201495 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a paint for forming a light diffusion layer of a projection screen, which is capable of obtaining a projection screen having an excellent balance between high transparency and high image display properties, a film for a projection screen including a light diffusion layer formed using the paint, and a projection screen.A further object of the present invention is to provide a paint for forming a light diffusion layer of a projection screen, which is capable of obtaining a projection screen having an excellent balance between high transparency and high image display properties, has a wide viewing angle, is unlikely to cause chromatic aberration (sufficiently small chromatic aberration), and is colorless (white and transparent), a film for a projection screen including a light diffusion layer formed using the paint, and a projection screen. [Means for solving the problem]

[0005] As a result of extensive research, the present inventors have found that the above object can be achieved by using a specific paint.

[0006] That is, the present invention provides a coating material for forming a light diffusion layer of a projection screen, comprising: (A) 100 parts by mass of a base resin; and (B) 0.1 to 50 parts by mass of rare earth phosphate fine particles.

[0007] A second invention is the coating material according to the first invention, wherein the component (A) base resin contains (A1) a multifunctional poly(meth)acrylate.

[0008] A third invention is the coating material according to the second invention, in which the component (A1) has a polystyrene-equivalent mass average molecular weight calculated from a differential molecular weight distribution curve measured by gel permeation chromatography of 1,000 or more.

[0009] A fourth invention is the coating material according to any one of the first to third inventions, further comprising 1 to 30 parts by mass of (C) a silane coupling agent per 100 parts by mass of the rare earth phosphate fine particles (B).

[0010] A fifth invention is a coating material according to any one of the first to fourth inventions, further comprising 1 to 30 parts by mass of (D) a compound having an isocyanate group and a polymerizable functional group other than an isocyanate group per 100 parts by mass of the rare earth phosphate fine particles (B).

[0011] A sixth invention is a film for a projection screen, comprising a light diffusing layer formed using the coating material according to any one of the first to fifth inventions.

[0012] A seventh invention is a film for a projection screen which has a light diffusion layer on at least one surface of a film substrate layer; the light diffusion layer is formed using a coating material containing (A) a substrate resin and (B) rare earth phosphate fine particles; and satisfies the following characteristics (A) to (C): (a) Total light transmittance of 85% or more; (b) Haze: 30% or less; and (c) Diffusion rate of 2% or more.

[0013] An eighth invention is a projection screen including the film for a projection screen according to the sixth invention or the seventh invention.

[0014] A ninth invention is a projection screen including a light diffusing layer formed using the coating material according to any one of the first to fifth inventions.

[0015] A tenth aspect of the present invention is a method for producing a film for a projection screen, comprising the steps of: (1) a step of mixing and stirring 100 parts by mass of (B) rare earth phosphate fine particles, 1 to 30 parts by mass of (C) a silane coupling agent, and 500 to 2000 parts by mass of (E) a solvent to obtain a mixed solution 1; (2) a step of further blending (D) a compound having an isocyanate group and a polymerizable functional group other than an isocyanate group with the mixed solution 1 obtained in the above step (1) in an amount of 1 to 30 parts by mass per 100 parts by mass of the component (B) rare earth phosphate fine particles, and mixing and stirring the mixture to obtain a mixed solution 2; (3) a step of further blending (A) a base resin with the mixed solution 2 obtained in the above step (2), mixing and stirring the mixture to obtain a coating material containing 100 parts by mass of the above component (A) base resin, and 0.1 to 50 parts by mass of the above component (B) rare earth phosphate fine particles; (4) forming a light diffusing layer on at least one surface of a film substrate using the coating material obtained in the above step (3); The production method includes the steps of: Effect of the Invention

[0016] A projection screen film including a light diffusion layer formed using the coating material of the present invention has an excellent balance between high transparency and high image display properties. A projection screen film including a light diffusion layer formed using a preferred coating material of the present invention has an excellent balance between high transparency and high image display properties, has a wide viewing angle, is less likely to cause chromatic aberration (sufficiently small chromatic aberration), and is colorless (white and transparent). Therefore, it can be suitably used as a projection screen film. In particular, it can be suitably used as a projection screen film that is attached to a medium having transmissive visibility such as a glass window and projects and displays video content when desired while normally maintaining transmissive visibility.

[0017] A projection screen including a light diffusion layer formed using the coating material of the present invention has an excellent balance between high transparency and high image display properties. A projection screen including a light diffusion layer formed using a preferred coating material of the present invention has an excellent balance between high transparency and high image display properties, has a wide viewing angle, is less likely to cause chromatic aberration (sufficiently small chromatic aberration), and is colorless (white and transparent). Therefore, it can be suitably used as a projection screen. In particular, it can be suitably used as a projection screen that usually maintains transmission visibility and projects and displays video content when desired. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] In this specification, the term "resin" is used to include a resin mixture containing two or more resins and a resin composition containing components other than resin. In this specification, the term "film" is used interchangeably or interchangeably with "sheet". In this specification, the terms "film" and "sheet" are used to refer to something that can be industrially wound into a roll. The term "plate" is used to refer to something that cannot be industrially wound into a roll. In this specification, laminating a layer and another layer in order includes both directly laminating the layers and laminating the layers with one or more layers, such as an anchor coat, interposed between the layers.

[0019] In this specification, the term "more than" in relation to a numerical range is used to mean a certain numerical value or more than a certain numerical value. For example, 20% or more means 20% or more than 20%. The term "less than" in relation to a numerical range is used to mean a certain numerical value or less than a certain numerical value. For example, 20% or less means 20% or less than 20%. Furthermore, the symbol "~" in relation to a numerical range is used to mean a certain numerical value, more than a certain numerical value and less than another certain numerical value, or another certain numerical value. Here, the other certain numerical value is a numerical value larger than the certain numerical value. For example, 10 to 90% means 10%, more than 10% and less than 90%, or 90%. Furthermore, the upper and lower limits of the numerical range can be arbitrarily combined, and an embodiment in which the values ​​are arbitrarily combined can be read. For example, from a statement regarding the numerical range of a certain characteristic such as "usually 10% or more, preferably 20% or more. On the other hand, it is usually 40% or less, preferably 30% or less" or "usually 10 to 40%, preferably 20 to 30%," it can be read that the numerical range of the certain characteristic is 10 to 40%, 20 to 30%, 10 to 30%, or 20 to 40% in one embodiment.

[0020] Other than in the examples, or where otherwise specified, all numerical values ​​used in the specification and claims should be understood to be modified by the term "about." Without attempting to limit the application of the doctrine of equivalents to the scope of the claims, each numerical value should be construed in light of the number of significant digits and by applying ordinary rounding techniques.

[0021] 1.Paint for forming light diffusion layer: The coating material of the present invention comprises (A) a base resin, and (B) rare earth phosphate fine particles. In one preferred embodiment, the coating material of the present invention further comprises (C) a silane coupling agent. In one preferred embodiment, the coating material of the present invention further comprises (D) a compound having an isocyanate group and a polymerizable functional group other than an isocyanate group. In one more preferred embodiment, the coating material of the present invention comprises (A) a base resin, (B) rare earth phosphate fine particles, (C) a silane coupling agent, and (D) a compound having an isocyanate group and a polymerizable functional group other than an isocyanate group. Each component will be described below.

[0022] (A) Base resin: The above-mentioned component (A) base resin encompasses the above-mentioned component (B) rare earth phosphate fine particles and functions to form a coating film.

[0023] Examples of the component (A) include curable resins such as active energy ray curable resins and thermosetting resins, pressure sensitive adhesives, adhesives, and thermoplastic resins. Among these, curable resins such as active energy ray curable resins and thermosetting resins are preferred from the viewpoint of dispersing the component (B) well in the component (A), of making the thickness of the light diffusion layer uniform and of uniformly expressing image display properties, and of preventing the thickness of the light diffusion layer from changing and impairing the uniformity of image display properties even if the projection screen is subjected to a physical impact.

[0024] The thermosetting resin can be polymerized and cured by heat to form a coating film. Examples of the thermosetting resin include phenol resin, urea resin, melamine resin, unsaturated polyester, epoxy resin, silicone resin, two-component curing urethane resin, and polyurethane.

[0025] The above-mentioned active energy ray-curable resin can be polymerized and cured by active energy rays such as ultraviolet rays and electron beams to form a coating film.

[0026] Examples of the active energy ray curable resin include (meth)acryloyl group-containing monofunctional reactive monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, phenyl (meth)acrylate, phenyl cellosolve (meth)acrylate, 2-methoxyethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, 2-acryloyloxyethyl hydrogen phthalate, dimethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, and trimethylsiloxyethyl methacrylate; and monofunctional reactive monomers such as N-vinylpyrrolidone and styrene. In this specification, (meth)acrylate means acrylate or methacrylate.Examples of the active energy ray-curable resin include (meth)acryloyl group-containing bifunctional reactive monomers such as diethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 2,2'-bis(4-(meth)acryloyloxypolyethyleneoxyphenyl)propane, and 2,2'-bis(4-(meth)acryloyloxypolypropyleneoxyphenyl)propane; trimethylolpropane tri(meth)acrylate, trimethylolethane ... Examples of the reactive monomer include polyfunctional (meth)acrylates such as (meth)acryloyl group-containing trifunctional reactive monomers, such as (meth)acryloyl group-containing tetrafunctional reactive monomers, such as ditrimethylolpropane tetra(meth)acrylate and pentaerythritol tetramethacrylate; (meth)acryloyl group-containing hexafunctional reactive monomers, such as dipentaerythritol hexaacrylate; and (meth)acryloyl group-containing octafunctional reactive monomers, such as tripentaerythritol octaacrylate. Examples of the active energy ray-curable resin include polyfunctional poly(meth)acrylates such as prepolymers or oligomers, such as polyurethane (meth)acrylate, polyester (meth)acrylate, polyacryl (meth)acrylate, polyepoxy (meth)acrylate, polyalkylene glycol poly(meth)acrylate, and polyether (meth)acrylate, each of which has two or more (meth)acryloyl groups in one molecule.

[0027] The curable resin may be one of these or a mixture of two or more of them.

[0028] As the curable resin, from the viewpoint of achieving a better balance between high transparency and high image display properties, the active energy ray curable resin is preferable, a polyfunctional (meth)acrylate is more preferable, and a polyfunctional poly(meth)acrylate is even more preferable.

[0029] (A1) Multifunctional poly(meth)acrylate: The above-mentioned component (A1) multifunctional poly(meth)acrylate is an oligomer or prepolymer having two or more (meth)acryloyl groups in one molecule. In this specification, a (meth)acryloyl group means an acryloyl group or a methacryloyl group. Since the above-mentioned component (A1) has two or more (meth)acryloyl groups in one molecule, it functions to form a coating film by being polymerized and cured by active energy rays such as ultraviolet rays and electron beams.

[0030] Examples of the component (A1) include prepolymers or oligomers such as polyurethane (meth)acrylate, polyester (meth)acrylate, polyacryl (meth)acrylate, polyepoxy (meth)acrylate, polyalkylene glycol poly (meth)acrylate, and polyether (meth)acrylate, each of which has two or more (meth)acryloyl groups in one molecule. Among these, polyurethane (meth)acrylates each of which has two or more (meth)acryloyl groups in one molecule are preferred from the viewpoints of surface hardness and coating appearance.

[0031] The above-mentioned polyurethane (meth)acrylate having two or more (meth)acryloyl groups in one molecule is a compound having a urethane structure (-NH-CO-O-) or a derivative thereof, and is a compound having two or more (meth)acryloyl groups in one molecule.

[0032] The polyurethane (meth)acrylate having two or more (meth)acryloyl groups in one molecule is not particularly limited, but may typically be one produced using a compound having two or more isocyanate groups (-N=C=O) in one molecule, a polyol compound, and a hydroxyl group-containing (meth)acrylate, i.e., one containing structural units derived from these compounds.

[0033] Examples of the compound having two or more isocyanate groups in one molecule include compounds having two isocyanate groups in one molecule, such as diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, tolylene diisocyanate, and methylene bis(4-cyclohexyl isocyanate). Examples of the compound having two or more isocyanate groups in one molecule include polyisocyanates such as a trimethylolpropane adduct of tolylene diisocyanate, a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, an isocyanurate of tolylene diisocyanate, an isocyanurate of hexamethylene diisocyanate, an isocyanurate of isophorone diisocyanate, and a biuret of hexamethylene diisocyanate. As the compound having two or more isocyanate groups in one molecule, one of these compounds or a mixture of two or more of them can be used.

[0034] Examples of the polyol compound include polyether polyol, polyester polyol, and polycarbonate polyol.

[0035] Examples of the polyether polyols include polyalkylene glycols such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; polyalkylene oxides such as polyethylene oxide and polypropylene oxide; copolymers of ethylene oxide and propylene oxide; copolymers of ethylene oxide and tetrahydrofuran; copolymers of dihydric phenol compounds and polyoxyalkylene glycols; and copolymers of dihydric phenols and one or more alkylene oxides having 2 to 4 carbon atoms (e.g., ethylene oxide, propylene oxide, 1,2-butylene oxide, and 1,4-butylene oxide).

[0036] Examples of the polyester polyol include poly(ethylene adipate), poly(butylene adipate), poly(neopentyl adipate), poly(hexamethylene adipate), poly(butylene azelaate), poly(butylene sebacate), and polycaprolactone.

[0037] Examples of the polycarbonate polyol include poly(butanediol carbonate), poly(hexanediol carbonate), and poly(nonanediol carbonate).

[0038] As the polyol compound, one or a mixture of two or more of these can be used.

[0039] Examples of the hydroxyl group-containing (meth)acrylate include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate; glycol-based (meth)acrylates such as dipropylene glycol (meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; glycerin-based (meth)acrylates such as glycerin di(meth)acrylate; glycidyl-based (meth)acrylates such as fatty acid-modified glycidyl (meth)acrylate; 2-hydroxyethyl Examples of the hydroxyl group-containing (meth)acrylate include phosphorus atom-containing (meth)acrylates such as acryloyl phosphate; (meth)acrylic acid adducts of esters or ester derivatives such as 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate; pentaerythritol-based (meth)acrylates such as pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, ethylene oxide-modified pentaerythritol tri(meth)acrylate, and ethylene oxide-modified dipentaerythritol penta(meth)acrylate; and caprolactone-modified (meth)acrylates such as caprolactone-modified 2-hydroxyethyl (meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, and caprolactone-modified dipentaerythritol penta(meth)acrylate. The hydroxyl group-containing (meth)acrylate may be one of these or a mixture of two or more of them.

[0040] As the component (A1), one or a mixture of two or more of these can be used.

[0041] The polystyrene-equivalent mass average molecular weight (Mw) of the component (A1) calculated from a differential molecular weight distribution curve (hereinafter sometimes abbreviated as "GPC curve") measured by gel permeation chromatography (hereinafter sometimes abbreviated as "GPC curve") may be preferably 1,000 or more, more preferably 2,000 or more, even more preferably 3,000 or more, and most preferably 4,000 or more, from the viewpoint of dispersing the component (B) well and improving the surface appearance of the coating film formed. On the other hand, from the viewpoint of the coatability of a coating material containing the component (A1), it may be preferably 100,000 or less, more preferably 70,000 or less, and even more preferably 50,000 or less.

[0042] The polystyrene-equivalent Z-average molecular weight (Mz) of the component (A1) calculated from the GPC curve may be, from the viewpoint of dispersing the component (B) well and improving the surface appearance of the coating film formed, preferably 2,000 or more, more preferably 4,000 or more, even more preferably 6,000 or more, and most preferably 8,000 or more. On the other hand, from the viewpoint of the coatability of the coating material containing the component (A1), it may be preferably 200,000 or less, more preferably 150,000 or less, and even more preferably 120,000 or less.

[0043] The GPC measurement was performed using a Tosoh Corporation high-performance liquid chromatography system "HLC-8320 (trade name)" (a system including a degasser, a liquid delivery pump, an autosampler, a column oven, and an RI (differential refractive index) detector); two Shodex GPC columns "KF-806L (trade name)" and one each of "KF-802 (trade name)" and "KF-801 (trade name)" were used as GPC columns, totaling four columns, connected in the order of KF-806L, KF-806L, KF-802, and KF-801 from the upstream side; and tetrahydrofuran (stabilizer-free) for high-performance liquid chromatography from Wako Pure Chemical Industries, Ltd. was used as the mobile phase; the conditions were a flow rate of 1.0 milliliters / minute, a column temperature of 40°C, a sample concentration of 1 milligram / milliliter, and a sample injection amount of 100 microliters. The elution amount at each retention volume can be determined from the amount detected by the RI detector, assuming that the refractive index of the measurement sample does not depend on the molecular weight. A calibration curve from retention volume to polystyrene-equivalent molecular weight can be created using standard polystyrene "EasiCal PS-1 (trade name)" from Agilent Technology Co., Ltd. (Plain A molecular weights: 6,375,000, 573,000, 117,000, 31,500, 3,480; Plain B molecular weights: 2,517,000, 270,600, 71,800, 10,750, 705). The analysis program that can be used is "TOSOH HLC-8320GPC EcoSEC (trade name)" from Tosoh Corporation. For the theory of GPC and the actual measurement, reference books such as "Size Exclusion Chromatography: High Performance Liquid Chromatography of Polymers, Author: Mori Sadao, First Edition, First Printing, December 10, 1991" published by Kyoritsu Shuppan Co., Ltd. and "Synthetic Polymer Chromatography, Editors: Otani Hajime, Takarazaki Tatsuya, First Edition, First Printing, July 25, 2013" published by Ohmsha Co., Ltd. can be referred to.

[0044] Figure 1 shows the differential molecular weight distribution curve of the following component (A1-1) used in the examples. A peak top for the main component and a peak top for the subcomponent are observed, and the polystyrene-equivalent molecular weights at the peak top positions are 3600 and 430, respectively. The polystyrene-equivalent molecular weight of the component with the highest molecular weight is observed to be 39800. The polystyrene-equivalent number average molecular weight of the entire product is 2000, the mass average molecular weight is 4800, and the Z average molecular weight is 9600.

[0045] From the viewpoint of improving the surface hardness and scratch resistance of the coating film, the number of (meth)acryloyl groups in one molecule of the above component (A1) may be preferably 3 or more, more preferably 4 or more, and even more preferably 5 or more. On the other hand, from the viewpoint of crack resistance, the number may be usually 30 or less, preferably 20 or less, more preferably 12 or less, and even more preferably 10 or less.

[0046] (B) Rare earth phosphate particles: The rare earth phosphate fine particles of component (B) are fine particles of phosphate of rare earth (scandium, yttrium, and lanthanoid (lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium)). Component (B) scatters light incident on the light diffusion layer of the projection screen, allowing image content to be projected and displayed clearly.

[0047] Without intending to be bound by theory, it is believed that because the above component (B) has a high refractive index and a high Abbe number, and the wavelength dependency of the refractive index is small, it is possible to obtain a projection screen that has a wide viewing angle and is less susceptible to chromatic aberration (sufficiently small chromatic aberration).In addition, because the above component (B) is white and transparent, it is believed that a colorless projection screen can be obtained.

[0048] The average particle size of the component (B) may be usually 20 μm or less, preferably 10 μm or less, more preferably 6 μm or less, even more preferably 3 μm or less, and most preferably 1 μm or less, from the viewpoint of maintaining the transparency of the coating film, while it may be preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.08 μm or more, from the viewpoint of enabling a clear projection and display of video content.

[0049] In this specification, the average particle size of particles is the particle size at which the cumulative amount of particles from the smallest particle is 50 mass % in a particle size distribution curve measured by a laser diffraction / scattering method. The particle size distribution curve can be measured, for example, using a laser diffraction / scattering particle size analyzer "MT3200II (product name)" manufactured by Nikkiso Co., Ltd.

[0050] As the above component (B), for example, those described in Patent Documents 3 and 4 can be preferably used.

[0051] As the component (B), one or a mixture of two or more of these can be used.

[0052] The amount of component (B) may be, from the viewpoint of enabling clear projection and display of video content, usually 0.1 parts by mass or more, preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 2 parts by mass or more, and most preferably 3 parts by mass or more, relative to 100 parts by mass of component (A). On the other hand, from the viewpoint of maintaining the transparency of the coating film, the amount may be usually 50 parts by mass or less, preferably 40 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and most preferably 15 parts by mass or less.

[0053] (C) Silane coupling agent: The silane coupling agent (C) is a silane compound having at least two different reactive groups, namely, a hydrolyzable group (e.g., an alkoxy group such as a methoxy group or an ethoxy group; an acyloxy group such as an acetoxy group; a halogen group such as a chloro group; etc.) and an organic functional group (e.g., a vinyl group, an epoxy group, a methacryloxy group, an acryloxy group, an amino group, a mercapto group, an isocyanate group, a ureido group, an isocyanurate group, etc.). The component (C) enhances the miscibility of the component (A) and the component (B), and thus improves the surface appearance and the wet heat resistance of the coating film (light diffusion layer) formed from the light diffusing coating material.

[0054] Without intending to be bound by theory, it is believed that the reason why component (C) can increase the miscibility of component (A) and component (B) is that component (C) has a hydrolyzable group and can therefore form a chemical bond with or strongly interact with component (B), and that component (C) has an organic functional group and can therefore form a chemical bond with or strongly interact with component (A).

[0055] Examples of the component (C) include a silane coupling agent having a vinyl group (a silane compound having a vinyl group and a hydrolyzable group), a silane coupling agent having an epoxy group (a silane compound having an epoxy group and a hydrolyzable group), a silane coupling agent having a (meth)acryloxy group (a methacryloxy group or an acryloxy group) (a silane compound having a (meth)acryloxy group and a hydrolyzable group), a silane coupling agent having an amino group (a silane compound having an amino group and a hydrolyzable group), a silane coupling agent having a mercapto group (a silane compound having a mercapto group and a hydrolyzable group), a silane coupling agent having an isocyanate group (a silane compound having an isocyanate group and a hydrolyzable group), a silane coupling agent having a ureido group (a silane compound having a ureido group and a hydrolyzable group), and a silane coupling agent having an isocyanurate group (a silane compound having an isocyanurate group and a hydrolyzable group).

[0056] Examples of the silane coupling agent having a vinyl group include vinyltrimethoxysilane, vinyltriethoxysilane, and p-styryltrimethoxysilane.

[0057] Examples of the silane coupling agent having an epoxy group include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.

[0058] Examples of the silane coupling agent having a (meth)acryloxy group include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane.

[0059] Examples of the silane coupling agent having an amino group include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, Examples include 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane.

[0060] Examples of the silane coupling agent having a mercapto group include 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0061] An example of the silane coupling agent having an isocyanate group is 3-isocyanatepropyltriethoxysilane.

[0062] Examples of the silane coupling agent having a ureido group include 3-ureidopropyltrimethoxysilane and 3-ureidopropyltriethoxysilane.

[0063] An example of the silane coupling agent having an isocyanurate group is tris-(trimethoxysilylpropyl)isocyanurate.

[0064] As the component (C), one or a mixture of two or more of these can be used.

[0065] The amount of the component (C) may be usually 1 part by mass or more, preferably 4 parts by mass or more, more preferably 7 parts by mass or more, based on 100 parts by mass of the component (B), from the viewpoint of reliably obtaining the effect of improving the miscibility between the components (A) and (B). On the other hand, from the viewpoint of the coating film curability and transparency, the amount may be usually 30 parts by mass or less, preferably 20 parts by mass or less, more preferably 15 parts by mass or less.

[0066] When producing the coating material of the present invention, it is preferable to mix and stir the above-mentioned components (B) and (C) and then add the above-mentioned component (A) and further mix and stir, so that the effect of the above-mentioned component (C) in improving the miscibility of the above-mentioned components (A) and (B) can be more reliably obtained.

[0067] (D) Compounds having an isocyanate group and a polymerizable functional group other than an isocyanate group: The above-mentioned component (D) is a compound having an isocyanate group and a polymerizable functional group other than an isocyanate group, and is a compound having one or more isocyanate groups (-N=C=O) in one molecule and having one or more polymerizable functional groups other than an isocyanate group. In this specification, a compound that is a multifunctional (meth)acrylate or a multifunctional poly(meth)acrylate and has an isocyanate group is classified as the above-mentioned component (D) rather than the above-mentioned component (A). The above-mentioned component (D) functions to increase the miscibility of the above-mentioned component (A) and the above-mentioned component (B), and thus to improve the surface appearance and the wet heat resistance of the coating film (light diffusion layer) formed from the light diffusing paint.

[0068] Examples of the polymerizable functional group other than the isocyanate group contained in the component (D) include a (meth)acryloyl group, a vinyl group, an epoxy group, an amino group, and a mercapto group. Among these, a (meth)acryloyl group and a vinyl group are preferred.

[0069] The number of isocyanate groups contained in the component (D) may be preferably 1 to 3, and more preferably 1. The number of polymerizable functional groups other than the isocyanate groups contained in the component (D) may be preferably 1 to 3, and more preferably 1 to 2.

[0070] Examples of the component (D) include a compound having one isocyanate group and one polymerizable functional group other than an isocyanate group in one molecule, such as 2-isocyanatoethyl (meth)acrylate; and a compound having one isocyanate group and two polymerizable functional groups other than an isocyanate group in one molecule, such as 1,1-(bis(meth)acryloyloxymethyl)ethyl isocyanate.

[0071] As the component (D), one or a mixture of two or more of these can be used.

[0072] The amount of the component (D) may be usually 1 part by mass or more, preferably 4 parts by mass or more, more preferably 7 parts by mass or more, based on 100 parts by mass of the component (B), from the viewpoint of reliably obtaining the effect of improving the miscibility between the components (A) and (B). On the other hand, from the viewpoint of the coating film curability, the amount may be usually 30 parts by mass or less, preferably 20 parts by mass or less, more preferably 15 parts by mass or less.

[0073] When producing the coating material of the present invention, it is preferable to mix and stir the above-mentioned components (B) and (D) and then add the above-mentioned component (A) and further mix and stir, so that the effect of the above-mentioned component (D) in improving the miscibility of the above-mentioned components (A) and (B) can be more reliably obtained.

[0074] It is preferable to use the above-mentioned component (C) and the above-mentioned component (D) in combination. In this embodiment, when producing the coating material of the present invention, it is preferable to mix and stir the above-mentioned component (B) and the above-mentioned component (C), then add the above-mentioned component (D) and mix and stir, and then add the above-mentioned component (A) and mix and stir. The effect of improving the miscibility of the above-mentioned component (A) and the above-mentioned component (B) by using the above-mentioned component (C) in combination can be obtained more reliably.

[0075] Without intending to be bound by theory, the above-mentioned miscibility-improving effect is considered as follows. If the hydrolyzable groups (hereinafter referred to as "free hydrolyzable groups") of the component (C) that are not involved in chemical bonds or strong interactions with the component (B) form chemical bonds with each other (between the free hydrolyzable groups) or strongly interact with each other, the component (B) will aggregate and the dispersibility will decrease. This phenomenon is prevented by the component (D), which has an isocyanate group, forming chemical bonds with the free hydrolyzable groups or strongly interacting with them. And, since the component (D) has a polymerizable functional group, it can form chemical bonds with the component (A) or strongly interact with them, so the component (D) alone contributes to improving the miscibility between the components (A) and (B). In addition, the reason why it is preferable to mix and stir the component (C) with the component (B) before the component (D) is that a hydrolyzable group is more advantageous than an isocyanate group in terms of chemical bonding and strong interaction with the component (B).

[0076] From the viewpoint of improving the curability by active energy rays, it is preferable that the coating material of the present invention further contains a compound having two or more isocyanate groups (-N=C=O) in one molecule and / or a photopolymerization initiator.

[0077] Examples of the compound having two or more isocyanate groups in one molecule include methylene bis-4-cyclohexyl isocyanate; polyisocyanates such as trimethylolpropane adduct of tolylene diisocyanate, trimethylolpropane adduct of hexamethylene diisocyanate, trimethylolpropane adduct of isophorone diisocyanate, isocyanurate of tolylene diisocyanate, isocyanurate of hexamethylene diisocyanate, isocyanurate of isophorone diisocyanate, and biuret of hexamethylene diisocyanate; and urethane crosslinking agents such as blocked isocyanates of the above polyisocyanates. The compound having two or more isocyanate groups in one molecule may be one of these or a mixture of two or more of them. In addition, when crosslinking, a catalyst such as dibutyltin dilaurate or dibutyltin diethylhexoate may be added as necessary.

[0078] Examples of the photopolymerization initiator include benzophenone-based compounds such as benzophenone, methyl o-benzoyl benzoate, 4-methylbenzophenone, 4,4'-bis(diethylamino)benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone; benzoin-based compounds such as benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzyl methyl ketal; acetophenone, 2,2-dimethoxy-2-phenyl Examples of the photopolymerization initiator include acetophenone compounds such as acetophenone and 1-hydroxycyclohexylphenyl ketone; anthraquinone compounds such as methylanthraquinone, 2-ethylanthraquinone, and 2-amylanthraquinone; thioxanthone compounds such as thioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone; alkylphenone compounds such as acetophenone dimethyl ketal; triazine compounds; biimidazole compounds; acylphosphine oxide compounds; titanocene compounds; oxime ester compounds; oxime phenyl acetate compounds; hydroxyketone compounds; and aminobenzoate compounds. As the photopolymerization initiator, one or more of these compounds may be used.

[0079] As the photopolymerization initiator, it is preferable to use two or more acetophenone-based photopolymerization initiators, for example, 1-hydroxy-cyclohexyl-phenyl ketone and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one in combination. This allows the coating film to be cured sufficiently while suppressing coloration.

[0080] It is preferable that the coating material of the present invention further contains a leveling agent from the viewpoint of making the surface of the light diffusing layer smooth.

[0081] Examples of the leveling agent include acrylic leveling agents, silicon leveling agents, fluorine leveling agents, silicon-acrylic copolymer leveling agents, fluorine-modified acrylic leveling agents, fluorine-modified silicon leveling agents, and leveling agents into which functional groups (e.g., alkoxy groups such as methoxy and ethoxy groups, acyloxy groups, halogen groups, amino groups, vinyl groups, epoxy groups, methacryloxy groups, acryloxy groups, and isocyanate groups) have been introduced. Among these, silicon-acrylic copolymer leveling agents are preferred as the leveling agent. As the leveling agent, one or a mixture of two or more of these can be used.

[0082] The amount of the leveling agent is not particularly limited since it is an optional component. The amount of the leveling agent may be usually 0.01 parts by mass or more, preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, based on 100 parts by mass of the component (A), from the viewpoint of reliably obtaining the effect of using the leveling agent. On the other hand, the amount of the leveling agent may be usually 3 parts by mass or less, preferably 2 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, based on the viewpoint of suppressing troubles due to bleeding out.

[0083] The coating material of the present invention may contain, as desired, one or more optional components such as inorganic particles other than component (B), antistatic agents, surfactants, leveling agents, thixotropy-imparting agents, stain inhibitors, printability improvers, antioxidants, weather resistance stabilizers, light resistance stabilizers, ultraviolet absorbers, heat stabilizers, organic particles, organic colorants, and inorganic colorants.

[0084] The coating material of the present invention may contain a solvent as desired in order to dilute the coating material to a concentration that is easy to apply. The solvent is not particularly limited as long as it does not react with the component (A), the component (B), and other optional components, or catalyze (promote) the self-reaction (including deterioration reaction) of these components. Examples of the solvent include 1-methoxy-2-propanol, 2-propanol, ethanol, ethyl acetate, n-butyl acetate, toluene, methyl ethyl ketone, methyl isobutyl ketone, diacetone alcohol, and acetone. Among these, 1-methoxy-2-propanol, 2-propanol, and ethanol are preferred, and 1-methoxy-2-propanol and 2-propanol are more preferred, from the viewpoint of dispersibility of the component (B) and suppression of precipitation of the component (B) when the coating material is left to stand. As the solvent, one or a mixture of two or more of these can be used.

[0085] The coating material of the present invention can be obtained by mixing and stirring these components.

[0086] A preferred method for producing the coating material of the present invention is, for example, (1) a step of mixing and stirring 100 parts by mass of the component (B) rare earth phosphate fine particles, 1 to 30 parts by mass of the component (C) silane coupling agent, and 500 to 2000 parts by mass of the solvent (E) to obtain a mixed solution 1; (2) a step of further blending the component (D) a compound having an isocyanate group and a polymerizable functional group other than an isocyanate group with the mixed solution 1 obtained in the step (1) in an amount of 1 to 30 parts by mass per 100 parts by mass of the component (B) rare earth phosphate fine particles, and mixing and stirring to obtain a mixed solution 2; (3) a step of further blending the component (A) base resin with the mixed solution 2 obtained in the step (2), mixing and stirring to obtain a coating material containing 100 parts by mass of the component (A) base resin, and 0.1 to 50 parts by mass of the component (B) rare earth phosphate fine particles; The following methods can be mentioned:

[0087] The device used for mixing and stirring in the above steps (1) to (3) is not particularly limited, and any known mixing and stirring device can be used. The mixing and stirring in the above steps (1) to (3) can also be performed using ultrasonic waves.

[0088] When performing the mixing and stirring in the above steps (1) to (3), it is preferable to use small spheres such as zirconia beads to assist in the mixing and stirring. The size of the small spheres may be appropriately selected taking into consideration the average particle size of the component (B). The size of the small spheres may be usually 0.1 to 3 mm, preferably 0.3 to 1 mm, in diameter. From the viewpoint of dispersibility of the component (B) and workability, the amount of the small spheres used may be usually 1,000 to 10,000 parts by mass, preferably 2,000 to 5,000 parts by mass, per 100 parts by mass of the component (B).

[0089] The amount of component (E) blended in step (1) may be usually 500 to 2000 parts by mass, preferably 700 to 1500 parts by mass, from the viewpoints of dispersibility of component (B), suppression of settling of component (B) when the coating material is allowed to stand, and setting the solids content and viscosity of the coating material of the present invention within appropriate ranges.

[0090] 2.Projection Screen Film: The projection screen film of the present invention includes a light diffusing layer formed using the coating material of the present invention. The projection screen film of the present invention usually has a light diffusing layer formed using the coating material of the present invention on at least one side of a film substrate layer.

[0091] The coating material of the present invention has been described above. The method of forming the light diffusion layer using the coating material of the present invention is not particularly limited, and a known web coating method can be used. Examples of the method include rod coating, roll coating, gravure coating, reverse coating, roll brushing, dip coating, spray coating, spin coating, air knife coating, and die coating. Among these methods, rod coating is preferred from the viewpoint of making the thickness of the light diffusion layer uniform, and rod coating using a Mayer bar as a rod (hereinafter sometimes abbreviated as "Mayer bar method") is more preferred.

[0092] The thickness of the light diffusion layer is not particularly limited and can be any thickness as desired. From the viewpoint of imparting high image display properties, the thickness of the light diffusion layer may be usually 0.5 μm or more, preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 3 μm or more. On the other hand, from the viewpoint of maintaining good bending resistance of the projection screen film of the present invention and making it easy to handle as a film roll, the thickness may be usually 60 μm or less, preferably 30 μm or less, more preferably 20 μm or less, even more preferably 10 μm or less, and most preferably 7 μm or less.

[0093] From the viewpoint of imparting high transparency to the projection screen film of the present invention and from the viewpoint of making it colorless, the above-mentioned film base preferably has high transparency, and more preferably has high transparency and is colorless.

[0094] The total light transmittance of the film substrate (measured according to JIS K7361-1:1997) may be usually 80% or more, preferably 85% or more, more preferably 88% or more, even more preferably 90% or more, and most preferably 92% or more. A higher total light transmittance is preferable. The total light transmittance can be measured according to JIS K7361-1:1997, for example, using a turbidity meter "NDH2000 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd.

[0095] The yellowness index of the film substrate (measured according to JIS K7105:1981) may be usually 5 or less, preferably 3 or less, more preferably 2 or less, and even more preferably 1 or less. A lower yellowness index is preferable. The yellowness index can be measured according to JIS K7105:1981, for example, using a colorimeter "SolidSpec-3700 (product name)" manufactured by Shimadzu Corporation.

[0096] Examples of the film substrate include films of cellulose ester resins such as triacetyl cellulose, polyester resins such as polyethylene terephthalate, cyclic hydrocarbon resins such as ethylene norbornene copolymers, acrylic resins such as polymethyl methacrylate, polyethyl methacrylate, and vinylcyclohexane-methyl (meth)acrylate copolymers, aromatic polycarbonate resins, polyolefin resins such as polypropylene and 4-methyl-pentene-1, polyamide resins, polyarylate resins, polymeric urethane acrylate resins, and polyimide resins. These films include unstretched films, uniaxially stretched films, and biaxially stretched films. These films also include laminated films in which one or more of these films are laminated in two or more layers.

[0097] The thickness of the film substrate is not particularly limited and can be any thickness as desired. When high rigidity is not required for the projection screen film of the present invention, from the viewpoint of handling and conformity with the standard for glass shatterproof film, it may be usually 10 μm or more, preferably 30 μm or more, more preferably 50 μm or more. On the other hand, from the viewpoint of economic efficiency, it may be usually 250 μm or less, preferably 150 μm or less, more preferably 100 μm or less. When high rigidity is required for the projection screen film of the present invention, it may be usually 200 μm or more, preferably 300 μm or more, more preferably 400 μm or more. In addition, from the viewpoint of responding to the demand for thinning of the article, it may be usually 1500 μm or less, preferably 1000 μm or less, more preferably 700 μm or less.

[0098] In addition, when forming the light diffusion layer, the surface or both surfaces of the film substrate on which the light diffusion layer is to be formed may be subjected in advance to an adhesion enhancing treatment such as a corona discharge treatment or an anchor coat formation in order to increase the adhesive strength with the light diffusion layer.

[0099] The projection screen film of the present invention may have any layer other than the light diffusion layer and the film base layer, if desired. Examples of the optional layer include a hard coat, an anchor coat, a pressure sensitive adhesive layer, a transparent conductive layer, an infrared shielding layer, an infrared reflecting layer, an electromagnetic wave shielding layer, an electromagnetic wave reflecting layer, and a reflecting layer. The optional layer is not limited to one layer, and may be two or more layers. When the optional layer is two or more layers, the type is not limited to one, and may be two or more.

[0100] 2 is a conceptual cross-sectional view showing one example of an embodiment of the projection screen film of the present invention. This embodiment is a type that is attached to the outdoor side of a glass window, and has, in order from the side that is attached to the glass, an adhesive layer 1, an infrared shielding layer 2, a first anchor coat 3, a film substrate layer 4, a second anchor coat 5, a light diffusion layer 6, and a weather-resistant hard coat 7. This embodiment is a so-called transmission type, and video content is projected from the indoor side and viewed from the outdoor side.

[0101] 3 is a conceptual cross-sectional view showing one example of another embodiment of the projection screen film of the present invention. This embodiment is a type that is attached to the indoor side of a glass window, and has, in order from the side that is attached to the glass, a weather-resistant adhesive layer 8, a light diffusion layer 6, a first anchor coat 3, a film substrate layer 4, a second anchor coat 5, an infrared shielding layer 2, and a hard coat 9. This embodiment is a so-called transmission type, and video content is projected from the indoor side and viewed from the outdoor side.

[0102] 4 is a conceptual cross-sectional view showing one example of another embodiment of the projection screen film of the present invention. This embodiment is a type that is attached to the indoor side of a glass window, and has a weather-resistant adhesive layer 8, a first anchor coat 3, a film substrate layer 4, a second anchor coat 5, a reflective layer 10, a light diffusion layer 6, an infrared shielding layer 2, and a hard coat 9. This embodiment is a so-called reflective type, and video content is projected from the indoor side and viewed from the indoor side.

[0103] The projection screen film of the present invention has a total light transmittance (measured according to JIS K7361-1:1997) of preferably 85% or more, more preferably 88% or more, even more preferably 90% or more, and most preferably 91% or more. Since the total light transmittance is 85% or more, the projection screen film of the present invention is a projection screen film that is used by being attached to a medium having transmission visibility such as a glass window, and can be suitably used as a film for a projection screen that projects and displays video content when desired while usually maintaining transmission visibility. The higher the total light transmittance, the more preferable it is. The total light transmittance can be measured according to JIS K7361-1:1997, for example, using a turbidity meter "NDH2000 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd.

[0104] The projection screen film of the present invention may have a haze (measured according to JIS K7136:2000 under conditions of light incidence from the surface on the light diffusion layer side) of preferably 30% or less, more preferably 25% or less, even more preferably 20% or less, even more preferably 15% or less, and most preferably 12% or less. By having a haze of 30% or less, transparency can be maintained when video content is not projected and displayed. From the viewpoint of maintaining transparency, a lower haze is preferable. The haze can be measured according to JIS K7136:2000 under conditions of light incidence from the surface on the light diffusion layer side, for example, using a turbidity meter "NDH2000 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd.

[0105] The projection screen film of the present invention has a diffusion rate of 2% or more, preferably 4% or more, and more preferably 7% or more. From the viewpoint of image display properties, a higher diffusion rate is preferable. The diffusion rate here is a value measured and calculated according to the diffusion rate test (C) in the following Examples.

[0106] The projection screen film of the present invention may have a viewing angle (angle at which a projected image can be clearly seen) of preferably 100° or more, more preferably 120° or more, even more preferably 140° or more, and most preferably 160° or more. From the viewpoint of image display, the wider the viewing angle, the better. The viewing angle here refers to the maximum angle that results in a △ or O rating when evaluated according to the viewing angle test (iv) in the following examples.

[0107] The yellowness index (measured according to JIS K7105:1981) of the hard coat laminate film of the present invention in the projection screen film of the present invention is preferably 5 or less, more preferably 3 or less, even more preferably 2 or less, and most preferably 1.6 or less. A lower yellowness index is preferable. When the yellowness index is 5 or less, the film can be suitably used as a projection screen film. The yellowness index can be measured according to JIS K7105:1981 using, for example, a colorimeter "SolidSpec-3700 (product name)" manufactured by Shimadzu Corporation.

[0108] 3.Projection Screen: The projection screen of the present invention includes a light diffusion layer formed using the coating material of the present invention. In a typical embodiment, the projection screen of the present invention is a projection screen film of the present invention bonded to a part or all of a medium having transmissive visibility such as a glass window. In another typical embodiment, the projection screen of the present invention is a projection screen in which a light diffusion layer is formed directly or via an anchor coat using the coating material of the present invention on a part or all of a medium having transmissive visibility such as a glass window.

[0109] The medium having the above-mentioned transmissive visibility may be a transparent resin plate (including a laminate). By using the transparent resin plate, the problems of glass (e.g., low impact resistance and easy breakage, low processability, high specific gravity, heavy, etc.) can be fundamentally improved. In addition, by using the transparent resin plate as the above-mentioned medium, it becomes easy to manufacture a product having a curved surface shape with good productivity. EXAMPLES

[0110] The present invention will be described below with reference to examples, but the present invention is not limited to these.

[0111] Measurement method (a) Total light transmittance: In accordance with JIS K7361-1:1997, the turbidity was measured using a turbidity meter "NDH2000 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd., under the condition that light was incident on the surface on the light diffusion layer side.

[0112] (b) Haze: In accordance with JIS K7136:2000, a turbidity meter "NDH2000 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd. was used to measure the turbidity under the condition that light was incident on the surface on the light diffusion layer side.

[0113] (C) Diffusion rate: Using a goniophotometer "GC5000L (product name)" manufactured by Nippon Denshoku Industries Co., Ltd., light was incident on the surface on the light diffusion layer side at a projection angle of 0°, and the transmittance and reflectance were measured at 1° intervals from a receiving angle of -85° to 85°. The diffusivity was then calculated using the program built into the goniophotometer (calculation formula below). Diffusion rate=(L 20 +L 70 ) / (2 L5)=(T 20 / cos20°+T 70 / cos70°) / (2·T5 / cos5°) Here, L 20 is the reflectance when the light receiving angle is 20°, L 70 is the reflectance when the receiving angle is 70°, L5 is the reflectance when the receiving angle is 5°, T 20is the transmittance when the light receiving angle is 20°, T 70 is the transmittance when the light receiving angle is 70°, and T5 is the transmittance when the light receiving angle is 5°.

[0114] (d) Viewing angle: 100 parts by mass of Shin-Etsu Chemical Co., Ltd.'s addition reaction type silicon-based adhesive "KR-3704 (trade name)", 0.5 parts by mass of Shin-Etsu Chemical Co., Ltd.'s platinum compound-based addition reaction catalyst "CAT-PL-50T (trade name)", and 20 parts by mass of toluene were mixed and stirred to obtain a coating material for forming an adhesive layer. Next, the coating material for forming an adhesive layer was applied to the surface of the projection screen film opposite to the surface on which the light diffusion layer was formed so that the thickness after curing was 30 μm, and the coating material was heated and cured at 130° C. for 1 minute to form an adhesive layer. Next, the adhesive layer side surface of the projection screen film was bonded to a float plate glass (thickness 3 mm) specified in JIS R3202:2011 of Test Piece Co., Ltd. to prepare a projection screen. Next, a projection screen was created by attaching a projector "ZenBeam" of ASUS Co., Ltd. from the glass surface side of the projection screen. E1 (product name) was used to project an image in a dark place under the conditions of an incidence angle of 0° and a distance of 30 cm between the glass surface and the projector lens, and a visual acuity chart was displayed at a predetermined position so that the Landolt ring of the visual acuity chart was a predetermined size (a size that would be judged as 1.0 visual acuity if distinguished from a position 4 m away (hereinafter abbreviated as the size for 1.0 visual acuity), or a size that would be judged as 1.5 visual acuity if distinguished from a position 4 m away (hereinafter abbreviated as the size for 1.5 visual acuity). Next, the projection screen was The subject (with corrected visual acuity of 1.0 for the eye used for the test (the eye not used was covered with an eye shield)) was waiting at a distance of 60 cm and at an angle of 80° (the angle between the line normal to the light diffusion layer side of the projection screen, passing through the Landolt ring display, and the line connecting the Landolt ring display and the subject's waiting location is 80°, which is equivalent to a visual field angle of 160°; the same applies below) and was asked to answer the position of the gap in the displayed Landolt ring. Evaluation was based on the following criteria. ○: Landolt rings of any size were distinguishable. △: The Landolt ring of a size for visual acuity of 1.0 was distinguishable, but the Landolt ring of a size for visual acuity of 1.5 was not distinguishable. ×: No size of Landolt ring could be identified.

[0115] Similarly, tests were also conducted in which the angle of the area where the subjects waited was changed to an angle of 70° (140° field of view), 60° (120° field of view), 50° (100° field of view), and 40° (80° field of view).

[0116] (E) Chromatic aberration: A projection screen was created in the same manner as in the above test (iv), and an image was projected onto the projection screen in the same manner as in the above test (iv), to display a blue and red checkered pattern in a square shape with a side length of 3 mm. Next, the checkered pattern was visually observed from a position at an angle of 0° and a distance of 60 cm from the display location of the checkered pattern on the projection screen, and evaluated according to the following criteria. ○: No chromatic aberration was observed. △: Slight chromatic aberration was observed. ×: Chromatic aberration was clearly observed.

[0117] (F) Yellowness index: According to JIS K7105:1981, the measurement was carried out using a colorimeter "SolidSpec-3700 (product name)" manufactured by Shimadzu Corporation under the condition that light was incident on the surface on the light diffusion layer side.

[0118] (g) Pencil hardness: According to JIS K5600-5-4:1999, the light diffusion layer side of the projection screen film was measured using a "Uni" (product name) pencil manufactured by Mitsubishi Pencil Co., Ltd. under conditions of a test length of 25 mm and a load of 200 g. The presence or absence of scratches was judged by visually observing the sample surface under a fluorescent lamp at a position 50 cm away from the lamp.

[0119] (H) Surface appearance: The surface of the projection screen film on the side of the light diffusion layer was visually observed while shining light from a fluorescent lamp at various angles of incidence, and evaluated according to the following criteria. A: There were no ripples or scratches on the surface. Even when I looked closely at it through the light, it had a uniform transparency. B: There were no ripples or scratches on the surface. However, when viewed up close and through the light, there were some areas with slightly different transparency. C: There were no scratches on the surface. However, when viewed up close, slight undulations were observed on the surface. Also, when viewed up close through a light, there were areas with different transparency. D: Waviness and scratches were observed on the surface. There were also areas with clearly different transparency.

[0120] (i) Mandrel test (index of crack resistance): In accordance with JIS K5600-5-1:1999, a bending resistance test was conducted using a cylindrical mandrel method using a sample taken from a projection screen film, with dimensions of 100 mm in the machine direction and 50 mm in the horizontal direction. The diameter of the smallest mandrel among the mandrels that did not cause cracks in the coating film (light diffusion layer) was determined. Evaluation was based on the following criteria. A: 10mm or less. B: 12mm, 16mm, or 20mm. C: 25mm or 32mm. D: Cracks occurred even when the mandrel diameter was 32 mm.

[0121] (J) Curl resistance: A sample of 10 cm in the machine direction x 10 cm in the horizontal direction was taken from a film roll of projection screen film, and the height of lift due to curling at the four corners was measured when the sample was placed on a horizontal surface with the light diffusion layer side facing up. The largest lift height among the four corners was recorded as the value of the height of lift due to curling. Evaluation was based on the following criteria. A: 2mm or less. B: More than 2mm, less than 5mm. C: More than 5mm, less than 10mm. D: More than 10mm.

[0122] (k) Moisture and heat resistance (cross-cut test after moist heat treatment): The projection screen film was treated for 500 hours in a thermohygrostat at a temperature of 60°C and a relative humidity of 90%. Next, in accordance with JIS K 5600-5-6:1999, 100 squares (1 square = 1 mm x 1 mm) were cut into the grid pattern on the light diffusion layer side of the treated projection screen film. Next, an adhesion test tape was attached to the grid pattern, squeezed with fingers, and then peeled off. The evaluation criteria were in accordance with Table 1 of the above JIS standard. Category 0: The edges of the cut are completely smooth and there are no peeling marks on any of the grids. Category 1: Small separations of the coating at the intersections of cuts. No more than 5% of the cross-cut area is affected. Category 2: The coating has flaked along the edges of the cuts and / or at the intersections. Clearly more than 5% but not more than 15% of the cross-cut area is affected. Category 3: The coating has suffered partial or complete major flaking along the edges of the cuts and / or partial or complete flaking of various areas of the mesh. Cross-cut areas are affected in areas significantly greater than 15% but not more than 35%. Category 4: The coating has suffered partial or complete major flaking along the edges of the cuts and / or partial or complete flaking in several areas. Cross-cut areas are clearly more than 35% affected but not more than 65% affected. Category 5: When the degree of peeling exceeds category 4.

[0123] Raw materials used (A) Base resin: (A1) Multifunctional poly(meth)acrylate: (A1-1) Negami Chemical Industries Co., Ltd.'s polyurethane acrylate "Art Resin UN-954 (product name)". Polystyrene equivalent number average molecular weight 2000, mass average molecular weight 4800, Z average molecular weight 9600. Number of acryloyl groups 6. Solid content 60 mass%. (A1-2) Negami Chemical Industries Co., Ltd.'s polyurethane acrylate "Art Resin UN-952 (product name)". Polystyrene equivalent number average molecular weight 2500, mass average molecular weight 9100, Z average molecular weight 23000. Number of acryloyl groups 10. Solid content 60 mass%. (A1-3) Negami Chemical Industries Co., Ltd.'s polyurethane acrylate "Art Resin UN-953 (product name)". Polystyrene equivalent number average molecular weight 2000, mass average molecular weight 26000, Z average molecular weight 110000. Number of acryloyl groups 20. Solid content 40 mass%.

[0124] (A-4) Dipentaerythritol hexaacrylate "KAYARAD DPHA (product name)" from Nippon Kayaku Co., Ltd. (A-5) Amorphous polyester resin "Vylon 240SS (product name)" manufactured by Toyobo Co., Ltd.

[0125] (B) Rare earth phosphate particles: (B-1) Yttrium phosphate from Mitsui Mining & Smelting Co., Ltd. Average particle size: 0.085 μm.

[0126] (C) Silane coupling agent: (C-1) Vinyltrimethoxysilane "KBM-1003 (product name)" from Shin-Etsu Chemical Co., Ltd.

[0127] (D) Compounds having an isocyanate group and a polymerizable functional group other than an isocyanate group: (D-1) 2-isocyanatoethyl acrylate "Karenz AOI (product name)" from Showa Denko K.K.

[0128] (E) Solvent: (E-1) 1-Methoxy-2-propanol.

[0129] (F)Other: (F-1) BASF's acetophenone-based photopolymerization initiator (1-hydroxycyclohexyl phenyl ketone) "IRGACURE184 (product name)". (F-2) Acetophenone-based photopolymerization initiator (2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one) "IRGACURE127 (trade name)" manufactured by BASF. (F-3) "Coronate HX (product name)," a compound having two or more isocyanate groups per molecule, manufactured by Tosoh Corporation. (F-4) Silicone-acrylic copolymer leveling agent "Disparlon NSH-8430HF (product name)" from Kusumoto Chemicals Co., Ltd. Solid content: 10% by mass.

[0130] Example 1 (a) Preparation of paint for forming light diffusion layer: 100 parts by mass of the above (B-1), 10 parts by mass of the above (C-1), and 900 parts by mass of the above (E-1) were mixed, and 2500 parts by mass of zirconia beads (diameter 0.60 mm) were added to assist mixing and stirring, and the mixture was stirred for 15 minutes using a tube mixer. Next, 10 parts by mass of the above component (D-1) was added, and ultrasonic treatment was performed for another 30 minutes, after which the zirconia beads were filtered off to obtain a suspension. Next, 167 parts by mass of (A1-1) (100 parts by mass equivalent to solids content), 45.9 parts by mass of the suspension (4.5 parts by mass of (B-1) above, 0.45 parts by mass of (C-1) above, 0.45 parts by mass of (D-1) above, and 40.5 parts by mass of (E-1) above), 70.5 parts by mass of (E-1) above, 2.4 parts by mass of (F-1) above, 0.6 parts by mass of (F-2) above, and 2 parts by mass of (F-4) (0.2 parts by mass equivalent to solids content) were mixed and stirred to obtain a coating material for forming a light diffusion layer.

[0131] (b) Creating films for projection screens: The coating material for forming a light diffusion layer obtained in (a) above was applied to one side of a 50 μm-thick, double-sided, easily adhesive biaxially stretched polyethylene terephthalate resin film "Lumirror (product name)" manufactured by Toray Industries, Inc., using a Mayer bar type coating device so that the thickness after curing would be 5 μm, and the coating was dried and cured by exposure to ultraviolet light to form a light diffusion layer.

[0132] The above tests (a) to (j) were carried out. The results are shown in Table 1. In addition, all values ​​shown in the table are calculated as solids, except for the solvent (above (E-1)). The value of (E-1) shown in the table is the sum of the amount of (E-1) contained in the suspension and the amount of (E-1) newly added when mixing the suspension with components other than the suspension, such as component (A). The same applies to the following examples.

[0133] Examples 2-4 The same procedure as in Example 1 was repeated, except that the component (A) shown in Table 1 was used instead of the component (A1-1) and the amount of the component (E-1) added when mixing the suspension with the components other than the suspension was appropriately adjusted so that the viscosity of the coating material for forming a light diffusion layer was appropriate. The results are shown in Table 1.

[0134] Example 5 100 parts by mass of the component (A-5), 45.9 parts by mass of the suspension prepared in Example 1 (4.5 parts by mass of the (B-1), 0.45 parts by mass of the (C-1), 0.45 parts by mass of the (D-1), and 40.5 parts by mass of the (E-1)), 0.5 parts by mass of the (E-1), 10 parts by mass of the (F-3), and 2 parts by mass of the (F-4) (0.2 parts by mass in terms of solid content) were mixed and stirred to obtain a coating material for forming a light diffusion layer. Next, the coating material was applied to one side of a 50 μm-thick double-sided easy-adhesion biaxially stretched polyethylene terephthalate resin film "Lumirror (trade name)" manufactured by Toray Industries, Inc., using a Mayer bar type coating device so that the thickness after drying would be 5 μm, and then dried to form a light diffusion layer. The above tests (a) to (j) were performed. The results are shown in Table 1.

[0135] Examples 6-9 The same procedure as in Example 1 was carried out except that the blending amounts of the above components (B) to (E) were changed as shown in Table 1 or 2 by changing the blending amount of the above suspension and appropriately adjusting the amount of the above (E-1) newly blended when mixing the above suspension with components other than the above suspension so that the viscosity of the coating material for forming a light diffusion layer becomes appropriate. The results are shown in Table 1 or 2.

[0136] Examples 10-12 The same procedure as in Example 1 was carried out except that the preparation of the coating material for forming the light diffusing layer was changed as follows. The results are shown in Tables 1 and 2.

[0137] Preparation of the paint for forming the light diffusion layer used in Example 10: 100 parts by mass of the above (B-1), 10 parts by mass of the above (C-1), and 900 parts by mass of the above (E-1) were mixed, and in order to further assist in mixing and stirring, 2,500 parts by mass of zirconia beads (diameter 0.60 mm) were added. The mixture was stirred for 15 minutes using a tube mixer, and then ultrasonically treated for 30 minutes. Thereafter, the zirconia beads were filtered off to obtain a suspension. Next, 167 parts by mass of (A1-1) (100 parts by mass equivalent to solids content), 45.45 parts by mass of the suspension (4.5 parts by mass of (B-1) above, 0.45 parts by mass of (C-1) above, and 40.5 parts by mass of (E-1) above), 70.5 parts by mass of (E-1) above, 2.4 parts by mass of (F-1) above, 0.6 parts by mass of (F-2) above, and 2 parts by mass of (F-4) (0.2 parts by mass equivalent to solids content) were mixed and stirred to obtain a coating material for forming a light diffusion layer.

[0138] Preparation of the paint for forming the light diffusing layer used in Example 11: 100 parts by mass of the above (B-1), 10 parts by mass of the above (D-1), and 900 parts by mass of the above (E-1) were mixed, and in order to further assist in mixing and stirring, 2,500 parts by mass of zirconia beads (diameter 0.60 mm) were added. The mixture was stirred for 15 minutes using a tube mixer, and then ultrasonically treated for 30 minutes. Thereafter, the zirconia beads were filtered off to obtain a suspension. Next, 167 parts by mass of (A1-1) (100 parts by mass equivalent to solids content), 45.45 parts by mass of the suspension (4.5 parts by mass of (B-1) above, 0.45 parts by mass of (D-1) above, and 40.5 parts by mass of (E-1) above), 70.5 parts by mass of (E-1) above, 2.4 parts by mass of (F-1) above, 0.6 parts by mass of (F-2) above, and 2 parts by mass of (F-4) (0.2 parts by mass equivalent to solids content) were mixed and stirred to obtain a coating material for forming a light diffusion layer.

[0139] Preparation of the paint for forming the light diffusing layer used in Example 12: 100 parts by mass of the (B-1) and 900 parts by mass of the (E-1) were mixed, and 2500 parts by mass of zirconia beads (diameter 0.60 mm) were added to aid in mixing and stirring, and the mixture was stirred for 15 minutes using a tube mixer, and then ultrasonic treatment was performed for 30 minutes. The zirconia beads were then filtered off to obtain a suspension. Subsequently, 167 parts by mass of the (A1-1) (100 parts by mass in terms of solid content), 45 parts by mass of the suspension (4.5 parts by mass of the (B-1) and 40.5 parts by mass of the (E-1)), 70.5 parts by mass of the (E-1), 2.4 parts by mass of the (F-1), 0.6 parts by mass of the (F-2), and 2 parts by mass of the (F-4) (0.2 parts by mass in terms of solid content) were mixed and stirred to obtain a coating material for forming a light diffusion layer.

[0140] [Table 1]

[0141] [Table 2]

[0142] Example 13 167 parts by mass (100 parts by mass in terms of solid content) of the above (A1-1), 11.25 parts by mass (4.5 parts by mass in terms of solid content) of a dispersion of zirconium oxide fine particles (average particle diameter 0.1 μm) in methyl isobutyl ketone / 2-methylpropyl alcohol (mixture of 7 / 3 by volume), 100 parts by mass of the above (E-1), 2.4 parts by mass of the above (F-1), 0.6 parts by mass of the above (F-2), and 2 parts by mass (0.2 parts by mass in terms of solid content) of the above (F-4) were mixed and stirred to obtain a coating material for forming a light diffusion layer. The coating material for forming a light diffusion layer was applied to one side of a 50 μm thick double-sided easy-adhesion biaxially stretched polyethylene terephthalate resin film "Lumirror (trade name)" of Toray Industries, Inc., using a Meyer bar type coating device so that the thickness after curing was 5 μm, dried, and cured by ultraviolet irradiation to form a light diffusion layer. When the above tests (a) to (c) were carried out, the total light transmittance was 86.9%, the haze was 2.5%, and the diffusion rate was 1.3%.

[0143] A projection screen film having a light diffusion layer formed using the coating material of the present invention had excellent image display properties (high diffusion rate), high transparency, a wide viewing angle, little chromatic aberration, and no color (low yellowness index). A projection screen film having a light diffusion layer formed using a preferred coating material of the present invention also had high surface hardness and good surface appearance. In addition, the results of the mandrel test, curl resistance, and moist heat resistance show that the film is easy to work with when attached to a glass window, and it is expected that problems such as cracks in the light diffusion layer will not occur easily over time. [Brief description of the drawings]

[0144] [Figure 1] 2 is a GPC curve of the above component (A1-1) used in the examples. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of an embodiment of a projection screen film of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing an example of another embodiment of the projection screen film of the present invention. [Figure 4] FIG. 2 is a schematic cross-sectional view showing an example of another embodiment of the projection screen film of the present invention. [Explanation of symbols]

[0145] 1: Adhesive layer 2: Infrared shielding layer 3: First Anchor Court 4: Film base layer 5: 2nd Anchor Court 6: Light diffusion layer 7: Weather-resistant hard coat 8: Weather-resistant adhesive layer 9: Hard court 10: Reflective layer

Claims

1. A method for producing a projection screen film, comprising the steps of: (1) a step of mixing and stirring 100 parts by mass of (B) rare earth phosphate fine particles, 1 to 30 parts by mass of (C) a silane coupling agent, and 500 to 2,000 parts by mass of (E) a solvent to obtain a mixed solution 1; (2) A step of further blending (D) a compound having an isocyanate group and a polymerizable functional group other than an isocyanate group with the mixed solution 1 obtained in the above step (1) in an amount of 1 to 30 parts by mass per 100 parts by mass of the component (B) rare earth phosphate fine particles, and mixing and stirring to obtain a mixed solution 2; (3) A process of further blending (A) a base resin with the mixed solution 2 obtained in the above process (2), mixing and stirring to obtain a coating material containing 100 parts by mass of the above component (A) base resin, and 0.1 to 50 parts by mass of the above component (B) rare earth phosphate fine particles; (4) forming a light diffusing layer on at least one surface of a film substrate using the coating material obtained in the above step (3); The above production method.

2. A method for producing a projection screen film, comprising the steps of: (1) a step of mixing and stirring 100 parts by mass of (B) rare earth phosphate fine particles, 1 to 30 parts by mass of (C) a silane coupling agent, and 500 to 2,000 parts by mass of (E) a solvent to obtain a mixed solution 1; (2) A step of further blending (D) a compound having an isocyanate group and a polymerizable functional group other than an isocyanate group with the mixed solution 1 obtained in the above step (1) in an amount of 1 to 30 parts by mass per 100 parts by mass of the component (B) rare earth phosphate fine particles, and mixing and stirring to obtain a mixed solution 2; (3) A process of further blending (A) an active energy ray curable resin with the mixed liquid 2 obtained in the above process (2), mixing and stirring the mixture to obtain a coating material containing: 100 parts by mass of the active energy ray curable resin (A); and 0.1 to 50 parts by mass of the rare earth phosphate fine particles (B); (4) forming a light diffusing layer on at least one surface of a film substrate using the coating material obtained in the above step (3); The above production method.

3. A method for producing a film for a projection screen as described in claim 2, wherein the component (A) active energy ray curable resin contains a polyfunctional (meth)acrylate.

4. A method for producing a film for a projection screen as described in claim 2 or 3, wherein the component (A) active energy ray curable resin contains (A1) a multifunctional poly(meth)acrylate.

5. A method for producing a film for a projection screen as described in claim 4, wherein the component (A1) multifunctional poly(meth)acrylate includes a polyurethane (meth)acrylate having two or more (meth)acryloyl groups in one molecule.

6. A method for producing a film for a projection screen as described in claim 4 or 5, wherein the component (A1) multifunctional poly(meth)acrylate has a polystyrene-equivalent mass average molecular weight of 1,000 or more calculated from a differential molecular weight distribution curve measured by gel permeation chromatography.

7. A method for producing a film for a projection screen described in any one of claims 1 to 6, wherein the polymerizable functional group other than an isocyanate group possessed by the component (D) compound having an isocyanate group and a polymerizable functional group other than an isocyanate group is one or more types selected from the group consisting of a (meth)acryloyl group, a vinyl group, an epoxy group, an amino group, and a mercapto group.

8. A method for producing a film for a projection screen described in any one of claims 1 to 6, wherein the polymerizable functional group other than an isocyanate group possessed by the component (D) compound having an isocyanate group and a polymerizable functional group other than an isocyanate group is one or more types selected from the group consisting of a (meth)acryloyl group and a vinyl group.

Citation Information

Patent Citations

  • JP2014‐201495A

  • JP2015‐212800A

  • JP2017‐215355A

  • Coating composition for transparent film screen, transparent film screen comprising thereof and method of manufacturing the transparent film screen

    KR1020130038694A

  • Light-transmissive transparent screen, image displaying system, and image displaying method