Toner manufacturing method
By changing the volume average particle size of coarsely pulverized material and using a controlled trajectory through a swirl chamber, the method addresses the challenge of in-machine fusion and enhances toner productivity in producing smaller toner particles.
Patent Information
- Application Number
- JP2020146450
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-01
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-09-01
AI Technical Summary
Existing mechanical pulverizers face challenges in producing smaller toner particles while suppressing in-machine fusion and ensuring stable particle size, particularly when increasing rotor speed or reducing the gap between rotor and stator leads to temperature rises and potential fusion.
A method involving melt-kneading a binder resin and colorant mixture, followed by coarse grinding, and then using a pulverizing means with a rotor and stator arrangement that allows for changing the volume average particle size of the coarsely pulverized material during the pulverization process, utilizing a swirl chamber to control the trajectory of the coarsely pulverized material.
This method effectively suppresses in-machine fusion and improves toner productivity by stabilizing the particle size of finely pulverized products, even when producing smaller particles.
Smart Images

Figure 0007562339000004 
Figure 0007562339000005 
Figure 0007562339000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an image forming method for visualizing an electrostatic image in electrophotography, and a method for producing a toner for use in a toner jet. [Background technology]
[0002] In electrophotography and image forming methods for visualizing electrostatic images, toners are used to develop electrostatic images. Toner manufacturing methods are roughly divided into pulverization and polymerization, and pulverization is a simple manufacturing method. In a general manufacturing method using the pulverization method, a binder resin and a colorant, and optionally a charge control agent, a release agent, a fluidity imparting agent, and a magnetic material are added and mixed, melted and kneaded, cooled and solidified, and then the kneaded material is pulverized by a pulverizing means. Thereafter, if necessary, a process of classifying the particles to a desired particle size distribution and a process of adding a fluidizing agent are carried out to obtain a toner to be used for image formation. In the case of a toner used in a two-component development method, the toner is mixed with various magnetic carriers and then used for image formation. As the crushing means, various crushing devices are used, but in recent years, energy saving of the device is required to reduce CO2 emissions, and mechanical crushers with low power consumption are often used. For example, a mechanical crusher is known that includes a rotor supported by a central rotating shaft and having multiple convex and concave portions on its outer circumferential surface in a casing having an inlet and an outlet for the material to be crushed, and a stator disposed outside the rotor with a predetermined gap from the outer circumferential surface of the rotor and having multiple convex and concave portions on its inner circumferential surface, and when the material to be crushed passes through a processing section where the rotor and the stator face each other on the air flow flowing from the inlet to the outlet, it collides with the convex or concave portions of the rotor or the stator to crush the material to be crushed. In recent years, there has been a demand for smaller toner particle size in order to improve image quality. In order to reduce the particle size of toner, in the mechanical grinding machine described above, it is effective to rotate the rotor at high speed or narrow the gap between the rotor and the stator. However, when the rotor is rotated at high speed, the temperature of the material to be ground and the temperature of the air in the grinding chamber rise due to frictional heat during grinding, and fusion inside the machine is likely to occur. In addition, fusion inside the machine is also likely to occur when the gap between the rotor and the stator is narrowed. In order to produce toner particles with smaller diameters, a mechanical pulverizer in which the shape of the grooves in the stator is devised has been disclosed (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-21768 A Summary of the Invention [Problem to be solved by the invention]
[0004] The mechanical grinding machine described in Patent Document 1 is capable of producing toner particles with a smaller particle size by devising a groove shape for the stator. However, it has been found that the mechanical grinding machine described in Patent Document 1 has room for improvement in terms of suppressing fusion within the machine when producing toner particles with smaller particle diameters. When the rotor rotation speed is increased in order to grind toner particles into smaller particle sizes and obtain a finely ground product, or when the amount of material to be ground per unit time is increased as a means of improving productivity, the temperature inside the machine and the temperature of the material to be ground become more significant, making it more likely that adhesion will occur inside the machine. Furthermore, if the temperature inside the machine and the temperature of the material to be pulverized rise significantly, the surface of the material to be pulverized may partially melt and the particles of the material to be pulverized may bond together, causing the particle size of the finely pulverized product to become unstable. The present invention has been made to solve the above-mentioned problems, and provides a method for producing toner particles that can suppress in-machine fusion and achieve improvement in toner productivity when producing toner particles having a smaller particle size. [Means for solving the problem]
[0005] The present invention relates to a method for melt-kneading a mixture containing a binder resin and a colorant. The process of , The obtained kneaded product is cooled, and then the cooled product is By coarse grinding machine Coarsely crush to obtain coarsely crushed material Process , A step of finely pulverizing the coarsely pulverized material by a fine pulverizing means. 、 A method for producing a toner comprising the steps of: The fine grinding means comprises: a powder inlet for introducing the coarsely pulverized material into the fine pulverization means; a stator having a plurality of protrusions and recesses on an inner circumferential surface; a rotor attached to a central rotating shaft and having a plurality of protrusions and recesses on an outer circumferential surface; a powder outlet for discharging the finely pulverized powder from the fine pulverization means; The stator contains the rotor, and the rotor is disposed so that a surface of the stator and a surface of the rotor face each other with a predetermined gap therebetween; The volume average particle size of the coarsely pulverized material to be fed into the fine pulverization means is The finely pulverizing step Changed in death, The volume average particle size of the coarsely pulverized product is changed by changing the pulverization conditions of the coarse pulverizer. The present invention relates to a method for producing a toner. Effect of the Invention
[0006] According to the present invention, it is possible to provide a method for producing toner particles that can suppress in-machine fusion when producing toner particles having a smaller particle size, and achieves improvement in toner productivity. [Brief description of the drawings]
[0007] [Figure 1]FIG. 1 is a schematic diagram of a mechanical grinder which is a fine grinding means used in the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of the particle size distribution of the coarsely pulverized material used in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In the present invention, the expressions "xx or more and xx or less" and "xx to xx" expressing a numerical range mean a numerical range including the lower and upper limit endpoints, unless otherwise specified.
[0009] The method for producing toner particles of the present invention is a method for producing toner, comprising the steps of melt-kneading a mixture containing a binder resin and a colorant, cooling the resulting kneaded mixture, coarsely pulverizing the cooled mixture to obtain a coarsely pulverized product, and finely pulverizing the coarsely pulverized product by a fine pulverizing means, The fine grinding means comprises: a powder inlet for introducing the coarsely pulverized material into the fine pulverization means; a stator having a plurality of protrusions and recesses on an inner circumferential surface; a rotor attached to a central rotating shaft and having a plurality of protrusions and recesses on an outer circumferential surface; a powder outlet for discharging the finely pulverized powder from the fine pulverization means; The stator contains the rotor, and the rotor is disposed so that a surface of the stator and a surface of the rotor face each other with a predetermined gap therebetween; The volume average particle size of the coarsely pulverized material fed into the fine pulverizing means is changed during production.
[0010] According to the investigations of the present inventors, the above-mentioned production method can provide a method for producing toner particles that can suppress in-machine fusion when producing toner particles having a smaller particle size, and achieves improved toner productivity.
[0011] The reason why the method for producing toner particles provides superior effects not seen in the past is believed to be as follows.
[0012] When a predetermined amount of coarsely pulverized material (material to be pulverized) is fed into the powder supply port (powder inlet) 101 of the mechanical fine grinder shown in Figure 1, the coarsely pulverized material is introduced into the grinding processing chamber, which is the gap between the rotor 103 and the stator 104.
[0013] The powder is then instantly crushed by the impact generated between a rotor with many grooves on its surface, which rotates at high speed in the crushing chamber, and a stator with many grooves on its surface.The powder is then discharged through the powder discharge port 106.
[0014] The coarsely ground material fed from the powder supply port is subjected to a force parallel to the central rotation axis by the airflow from the powder supply port to the powder discharge port, and a force in the normal direction to the rotor's outer circumference by collision with the convex and concave parts of the rotor. As a result, the material to be ground is considered to be ground while moving along a single spiral trajectory in the direction of the rotor's rotation, starting from the gap between the rotor and the stator near the powder supply port and ending near the powder discharge port. This trajectory is determined by the airflow generated in the fine grinder and the particle size (weight) of the coarsely ground material. The airflow in the fine grinder is determined by operating conditions such as the rotation speed of the rotor 103, the minimum gap between the rotor 103 and the stator 104, and the flow rate of the suction blower. The position at which the coarsely ground material is easily introduced into the grinding chamber is determined by the flow of this airflow for each particle size of the coarsely ground material. As a result, for example, when coarsely pulverized material of 60 μm size as shown in FIG. 2 is pulverized by the above-mentioned mechanical fine pulverizer, it is thought that the material will follow a single trajectory that has a certain degree of expansion centered on the trajectory of the 60 μm coarsely pulverized material and enter the pulverization processing chamber.
[0015] According to the present invention, by changing the particle size of the coarsely pulverized material during production, the trajectory of the coarsely pulverized material in the pulverization chamber can be changed, and the entire pulverization chamber can be effectively used. This makes it possible to suppress local temperature rises in the device, and to prevent adhesion in the device and an increase in the particle size of the finely pulverized product. The change in particle size of the coarsely pulverized material in the present invention is not within the range of so-called manufacturing fluctuations, but is intentionally changed by changing the operating conditions of the coarse pulverization device.
[0016] If the orbit of the coarsely crushed material remains constant during crushing, the flow of the coarsely crushed material in the crushing chamber becomes localized. Therefore, when the coarsely crushed material is crushed, the frictional heat generated during crushing may cause a significant increase in the temperature inside the crusher and in the coarsely crushed material. As a result, the toner may melt inside the machine starting from the temperature rise point, or the surface of the coarsely crushed material may melt partially, causing the crushed material to bond together, resulting in an unstable particle size of the finely crushed product.
[0017] In order to change the trajectory of the coarsely pulverized material in the pulverization chamber, it is possible to change the air flow in the above-mentioned device. However, if the operating conditions such as the rotation speed of the rotor 103 are changed, the particle size of the finely pulverized material also changes significantly, making it impossible to produce products with the desired particle size.
[0018] On the other hand, the inventors have found through intensive research that changing the particle size of the coarsely pulverized material has almost no effect on the particle size of the finely pulverized material. The reason for this is believed to be as follows. The energy required for pulverization can be considered to be the change in surface area that occurs during pulverization. In this case, there is almost no difference in the change in surface area between when a pulverized material with a particle size of 50 μm is pulverized to 6 μm and when a pulverized material with a particle size of 100 μm is pulverized to 6 μm (because the surface area of 6 μm is overwhelmingly large). Therefore, it is believed that even when the particle size of the coarsely pulverized material is changed, almost the same particle size of the finely pulverized product can be obtained under the same operating conditions.
[0019] It is preferable to change the particle size of the coarsely pulverized material every time the device is operated for a certain period of time. The longer the time that the coarsely pulverized material is continuously supplied at the same particle size, the higher the risk of adhesion inside the device.
[0020] In the present invention, the difference in the volume average particle size of the coarsely pulverized products before and after the change is preferably 50 μm or more. By making the difference 50 μm or more, the trajectories of the coarsely pulverized products of each particle size passing through the device can be made farther apart, and the effect of the present invention can be clearly achieved.
[0021] In addition, it is preferable that the mechanical fine grinding machine is provided with a swirl chamber 1021 communicating with the supply port 101 as shown in Fig. 1. The coarsely ground material entering through the supply port 101 rotates along the wall of the swirl chamber 1021, and as it continues to rotate, it is introduced into the grinding chamber according to the particle size of the coarsely ground material. In other words, compared to a machine without a swirl chamber, it is considered that the flow straightening effect is stronger and it is easier for the material to enter from the desired location according to its particle size. Since the present invention aims to intentionally change the particle size of the coarsely ground material and change its trajectory within the machine, it is preferable to have a swirl chamber in which the location of entry can be easily controlled depending on the particle size.
[0022] Next, a procedure for producing toner particles according to the production method of the present invention will be described.
[0023] First, in the raw material mixing process, at least a binder resin and a colorant are weighed out in a predetermined amount as toner internal additives, and then mixed. If necessary, a release agent that suppresses the occurrence of hot offset during heat fixing of the toner, a dispersant that disperses the release agent, a charge control agent, etc. may be mixed. Examples of mixing devices include a double con mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, etc.
[0024] Furthermore, the toner raw materials blended and mixed as described above are melt-kneaded to melt the resins and disperse the colorant therein. In the melt-kneading step, for example, a batch-type kneader such as a pressure kneader or a Banbury mixer, or a continuous kneader can be used. In recent years, single-screw or twin-screw extruders have become mainstream due to their advantages such as continuous production, and for example, a KTK twin-screw extruder manufactured by Kobe Steel, Ltd., a TEM twin-screw extruder manufactured by Toshiba Machine Co., Ltd., a twin-screw extruder manufactured by KCK Corporation, and a Co-kneader manufactured by Buss Co., Ltd. are commonly used. Furthermore, the colored resin composition obtained by melt-kneading the toner raw materials is rolled with a two-roller or the like after melt-kneading, and cooled through a cooling step in which it is cooled with water or the like.
[0025] The cooled colored resin composition obtained above is coarsely pulverized to a desired particle size in a coarse pulverization step. In the coarse pulverization step, a pulverizer such as a crusher, a hammer mill, or a feather mill is usually used, but in the toner manufacturing method of the present invention, the volume average particle size of the coarsely pulverized product to be supplied to the fine pulverization step is preferably in the range of 20 μm to 300 μm both before and after the above change, and more preferably in the range of 20 μm to 200 μm.
[0026] If the particle size of the coarsely pulverized product supplied to the fine pulverization process exceeds 300 μm, there may be no effect of improving productivity in terms of fine particle size. This is because if the particle size of the coarsely pulverized product is too large, the load applied locally to the fine pulverization device becomes too large, and even if the trajectory of the coarsely pulverized product in the device is changed as in the present invention, there may be a risk of fusion. On the other hand, if the particle size of the coarsely pulverized product is less than 20 μm, the impact on the fine pulverization process is small, but stable production in the coarse pulverization process becomes difficult, which is not preferable for toner production.
[0027] In the toner manufacturing method of the present invention, it is preferable that the coarse pulverizer used in the coarse pulverization step has a primary pulverization means and a secondary pulverization means. In particular, the primary pulverization means has a plurality of rotary strikers for primary pulverization attached to the central rotating shaft for primary pulverization, and the secondary pulverization means has a rotor made of a rotor having irregularities attached to the central rotating shaft for secondary pulverization, and a stator having irregularities arranged around the rotor with a certain distance from the rotor surface, and these pulverization zones are contained within one unit, and it is more preferable to use a coarse pulverizer in which the primary pulverization rotating shaft and the secondary pulverization rotating shaft are coaxial and operated at the same rotation speed during manufacturing. When this coarse pulverizer is used, the desired coarse pulverization particle size can be obtained by changing the rotation speed, so it is suitable for controlling the coarse pulverization particle size. It is preferable that the rotation of the rotating shaft in the primary pulverization and the secondary pulverization is performed by a common power source.
[0028] Next, the raw materials of the toner particles containing at least the binder resin and the colorant used in the present invention will be described.
[0029] <Binding resin> As the binder resin used in the toner used in electrophotography, a general resin can be used. For example, polyester resin, styrene-acrylic acid copolymer, polyolefin resin, vinyl resin, fluororesin, phenol resin, silicone resin, epoxy resin, etc. Among these, from the viewpoint of improving low-temperature fixing property, amorphous polyester resin is used, and from the viewpoint of achieving both low-temperature fixing property and hot offset resistance, it is known to use low-molecular-weight polyester and high-molecular-weight polyester in combination. In addition, from the viewpoint of further improving low-temperature fixing property and blocking resistance during storage, crystalline polyester may be used as a plasticizer.
[0030] <Coloring agent> Colorants that can be contained in the toner include the following.
[0031] The colorant may be a known organic pigment or oil-based dye, carbon black, or a magnetic material.
[0032] Examples of cyan colorants include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds.
[0033] Examples of magenta colorants include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds.
[0034] Examples of yellow colorants include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds.
[0035] Examples of black colorants include carbon black, magnetic materials, and those toned to black using the above-mentioned yellow colorants, magenta colorants, and cyan colorants.
[0036] The colorants may be used alone or in combination of two or more.
[0037] <Release agent> If necessary, a release agent for suppressing the occurrence of hot offset during the heat fixing of the toner may be used. Typical examples of the release agent include low molecular weight polyolefins, silicone wax, fatty acid amides, ester waxes, carnauba wax, and hydrocarbon waxes.
[0038] <Method for measuring particle size distribution of finely ground particles> The particle size distribution of the finely ground product was measured as follows.
[0039] The measurement device used is a precision particle size distribution measurement device using the pore electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 50 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000.
[0040] The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).
[0041] Before performing measurements and analysis, the dedicated software is set up as follows.
[0042] In the "Change Standard Measurement Method (SOM)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particles 10.0 μm" (Beckman Coulter).
[0043] Press the "Threshold / Noise Level Measurement Button" to automatically set the threshold and noise level. Also, set the current to 1600μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement."
[0044] In the "Pulse to particle size conversion setting" screen of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 1 μm to 30 μm.
[0045] The specific measurement method is as follows.
[0046] (1) Pour about 200 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the dedicated software to remove dirt and air bubbles from inside the aperture tube. (2) Place about 30 mL of the electrolyte solution in a 100 mL flat-bottom glass beaker. Add about 0.3 mL of a solution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made from a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted about three times by mass with ion-exchanged water as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees, and has an electrical output of 120 W. Place approximately 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank, and add approximately 2 mL of Contaminon N to this tank. (4) Set the beaker (2) in the beaker fixing hole of the ultrasonic disperser, operate the ultrasonic disperser, and adjust the height of the beaker so that the resonance state of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, the electrolytic solution (5) in which the toner is dispersed is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) Analyze the measurement data using the dedicated software that comes with the device to calculate the weight-average particle size (D4). Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4).
[0047] <Method for measuring particle size distribution of coarsely ground particles> The particle size distribution of the coarsely ground material was measured using a particle size distribution measuring device LA-950V2 (manufactured by Horiba, Ltd.). This device uses a laser scattering method to measure particle sizes from 0.01 μm to 3000 μm. The volume average particle size of the coarsely ground material was measured by wet measurement using this device. For the wet measurement method, the coarsely ground material was mixed with an aqueous medium, and ultrasonically dispersed using "Contaminon N" as a dispersant in the same way as the Coulter Counter, and then introduced into the device.
[0048] The measurements were performed using a refractive index of 1.53 for the sample (coarsely ground product) and a refractive index of 1.33 for the dispersion medium. EXAMPLES
[0049] The present invention will be specifically described below by way of examples, but the present invention is not limited to these examples.
[0050] <Production Example of Amorphous Polyester Resin L> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane: 72.0 parts by mass (0.20 moles; 100.0 mol% based on the total number of moles of polyhydric alcohol) Terephthalic acid: 28.0 parts by mass (0.17 moles; 100.0 mol% based on the total number of moles of polycarboxylic acids) Tin 2-ethylhexanoate (esterification catalyst): 0.5 parts by mass The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the reaction was carried out for 4 hours at a temperature of 200°C with stirring.
[0051] The pressure inside the reaction vessel was then reduced to 8.3 kPa and maintained for 1 hour, after which the vessel was cooled to 180° C. and returned to atmospheric pressure. Trimellitic anhydride: 3 parts by mass (0.01 mole; 4.0 mol% based on the total number of moles of polycarboxylic acids) tert-Butylcatechol (polymerization inhibitor): 0.1 parts by mass Thereafter, the above materials were added, the pressure in the reaction tank was reduced to 8.3 kPa, and the reaction was carried out for 1 hour while maintaining the temperature at 180°C. After it was confirmed that the softening point measured in accordance with ASTM D36-86 reached 90°C, the temperature was reduced to stop the reaction, and an amorphous polyester resin L was obtained as a binder resin.
[0052] <Production Example of Amorphous Polyester Resin H> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane: 72.3 parts by mass (0.20 moles; 100.0 mol% based on the total number of moles of polyhydric alcohol) Terephthalic acid: 18.3 parts by mass (0.11 moles; 65.0 mol% based on the total number of moles of polycarboxylic acids) Fumaric acid: 2.9 parts by mass (0.03 moles; 15.0 mol% based on the total number of moles of polycarboxylic acids) Tin 2-ethylhexanoate (esterification catalyst): 0.5 parts by mass The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the reaction was carried out for 2 hours at a temperature of 200°C with stirring.
[0053] The pressure in the reactor was then reduced to 8.3 kPa and maintained for 1 hour, after which it was cooled to 180 and returned to atmospheric pressure. Trimellitic anhydride: 6.5 parts by mass (0.03 moles; 20.0 mol% based on the total number of moles of polycarboxylic acids) tert-Butylcatechol (polymerization inhibitor): 0.1 parts by mass Thereafter, the above materials were added, the pressure in the reaction tank was reduced to 8.3 kPa, and the reaction was carried out for 15 hours while maintaining the temperature at 160°C. After it was confirmed that the softening point measured in accordance with ASTM D36-86 reached 137°C, the temperature was reduced to stop the reaction, and an amorphous polyester resin H was obtained as a binder resin.
[0054] <Crystalline polyester resin> 1,6-Hexanediol: 34.5 parts by mass (0.29 moles; 100.0 mol% based on the total number of moles of polyhydric alcohol) Dodecanedioic acid: 65.5 parts by mass (0.28 moles; 100.0 mol% based on the total number of moles of polycarboxylic acids) Tin 2-ethylhexanoate: 0.5 parts by weight The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. After replacing the atmosphere in the flask with nitrogen gas, the temperature was gradually raised with stirring, and the reaction was carried out for 3 hours at a temperature of 140°C with stirring.
[0055] Next, the above materials were added, the pressure in the reaction vessel was reduced to 8.3 kPa, and the temperature was maintained at 200° C. while the reaction was carried out for 4 hours.
[0056] Furthermore, the pressure in the reaction tank was gradually released to return to normal pressure, and then one or more aliphatic compounds selected from the group consisting of aliphatic monocarboxylic acids and aliphatic monoalcohols were added in an amount of 7.0 mol% relative to 100.0 mol% of the raw material monomer, and the mixture was reacted at 200°C for 2 hours under normal pressure.
[0057] Thereafter, the pressure inside the reaction vessel was reduced again to 5 kPa or less, and the mixture was reacted at 200° C. for 3 hours to obtain a crystalline polyester resin.
[0058] <Toner manufacturing example> Amorphous polyester resin L 80 parts by weight Amorphous polyester resin H 20 parts by weight Crystalline polyester resin 5 parts by weight Fischer-Tropsch wax (hydrocarbon wax, maximum endothermic peak temperature 90°C) 5 parts by mass CI Pigment Blue 15:3 7 parts by weight The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes at 100° C., the mixture was kneaded in a twin-screw kneader (PCM-92, manufactured by Ikegai Corporation). The barrel temperature during kneading was set so that the outlet temperature of the kneaded product was 120° C. The outlet temperature of the kneaded product was directly measured using a handy type thermometer HA-200E manufactured by Anritsu Keiki Co., Ltd. The kneaded product was then cooled.
[0059] Example 1 In this example, the fine pulverization process was carried out while changing the particle size of the coarsely pulverized material. Specifically, the rotation speed of the coarse pulverizer was changed to 2900 rpm, 2300 rpm, and 1800 rpm to obtain the coarsely pulverized material. The volume average particle size of the coarsely pulverized material obtained at each rotation speed is shown in Table 1.
[0060] In this embodiment, as shown in Table 2, the conditions are a cycle of 2900 rpm for 20 minutes, 2300 rpm for 15 minutes, and 1800 rpm for 10 minutes. The obtained coarsely ground toner product was ground in a grinder (modified Turbo Mill T800 manufactured by Turbo Kogyo Co., Ltd.) shown in FIG. 1 to obtain toner particles.
[0061] In this embodiment, the minimum gap between the rotor 103 and the stator 104 of the pulverizer is set to 1.0 mm, the temperature of the air introduced into the mechanical fine pulverizer is set to -20°C, and the flow rate of the suction blower is set to 25 m 3 / min, and the supply rate of the coarsely ground material was 250 kg / hr.
[0062] The rotation speed of the rotor 103 was set under the following conditions. <Condition 1> The rotation speed of the rotor 103 was set to 170 m / sec, and production was carried out continuously for 4 hours. <Condition 2> The rotation speed of the rotor 103 was set to 180 m / sec, and production was carried out continuously for 4 hours.
[0063] [Evaluation of in-machine adhesion] After four hours of continuous production, the device was stopped and the degree of toner adhesion (dirt) on the rotor and stator was visually confirmed.
[0064] The evaluation ranks are as follows: A: Almost no adhesion, very good. B: Some adhesion is observed, but at a level that does not cause problems in practical use. C: Adhesion was observed and there was a problem in practical use.
[0065] The evaluation results are shown in Table 3.
[0066] [Evaluation of particle size stability] The finely pulverized product produced was sampled every 30 minutes, and the weight average particle size (D4) was measured to evaluate the particle size stability of the finely pulverized product.
[0067] The evaluation was performed by calculating the difference between the maximum and minimum particle sizes sampled, and ranking the particles as follows. A: Less than 0.2 μm, which is good. B: Between 0.2 μm and 0.4 μm, a level that does not pose a problem for practical use. C: 0.4 μm or more, which is a problematic level for practical use.
[0068] The evaluation results are shown in Table 3.
[0069] [Examples 2 to 8] The conditions of the coarse pulverizer are shown in Table 2. The volume average particle size of the coarsely pulverized product versus the rotation speed of the coarse pulverizer is shown in Table 1. The other conditions were the same as in Example 1, and the evaluation was performed.
[0070] The evaluation results are shown in Table 3.
[0071] [Comparative Examples 1 to 3] The rotation speed of the coarse crusher was kept constant. The conditions are shown in Table 2. The other conditions were the same as in Example 1, and the evaluation was performed.
[0072] The evaluation results are shown in Table 3.
[0073] [Table 1]
[0074] [Table 2]
[0075] [Table 3] [Explanation of symbols]
[0076] 101: grinding supply port (powder inlet), 1021: volute chamber, 1022: volute chamber outlet, 103: rotor, 104: stator, 105: rear chamber, 106: powder outlet, 107: rotating shaft, 108: cold air generator, 109: cold water supply port, 110: cold water outlet
Claims
1. A step of melt-kneading a mixture containing a binder resin and a colorant; a step of cooling the obtained kneaded product and then coarsely pulverizing the cooled product using a coarse pulverizer to obtain a coarsely pulverized product; a step of finely pulverizing the coarsely pulverized product by a fine pulverizing means; A method for producing a toner comprising the steps of: The fine grinding means comprises: a powder inlet for introducing the coarsely pulverized material into the fine pulverization means; a stator having a plurality of protrusions and recesses on an inner circumferential surface; a rotor attached to a central rotating shaft and having a plurality of protrusions and recesses on an outer circumferential surface; a powder outlet for discharging the finely pulverized powder from the fine pulverization means; The stator contains the rotor, and the rotor is disposed so that a surface of the stator and a surface of the rotor face each other with a predetermined gap therebetween; The volume average particle size of the coarsely pulverized material fed into the pulverizing means is changed during the pulverizing step; A method for producing a toner, wherein the volume average particle size of the coarsely pulverized product is changed by changing the pulverization conditions of the coarse pulverizer.
2. 2. The method for producing a toner according to claim 1, wherein the volume average particle size of the coarsely pulverized product before and after the change is within the range of 20 μm to 200 μm.
3. 3. The method for producing a toner according to claim 1, wherein the volume average particle size of the coarsely pulverized material fed into the fine pulverization means is changed every time the fine pulverization means operates for a certain period of time.
4. The coarse crusher has a primary crushing means and a secondary crushing means, The primary crushing means has a plurality of rotary strikers for primary crushing attached to a central rotary shaft for primary crushing, The secondary crushing means has a rotor made of a rotor having projections and recesses attached to a central rotating shaft for secondary crushing, and a stator having projections and recesses disposed around the rotor while maintaining a constant distance from the rotor surface; The primary grinding rotating shaft and the secondary grinding rotating shaft are coaxially arranged and are operated at the same rotation speed during production, 4. The method for producing a toner according to claim 1, wherein the volume average particle size of the coarsely pulverized product is changed by changing the rotation speed of the primary pulverization rotating shaft and the secondary pulverization rotating shaft.
5. 5. The method for producing a toner according to claim 1, wherein the difference in volume average particle size of the coarsely pulverized product before and after the change is 50 μm or more.
6. 6. The method for producing a toner according to claim 1, wherein the fine pulverizing means has a swirl chamber communicating with the powder inlet.
Citation Information
Patent Citations
Mechanical pulverizer
JP2004042029A
Pulverizing mill and its fine powder product
JP2005021768A
Method for manufacturing electrostatic charge image developing toner
JP2005249988A
Method and apparatus for manufacturing toner particle
JP2007187689A
Crushing device
JP2013086023A