Photosensitive resin composition for forming partition wall, partition wall structure produced using the same, and display device including the partition wall structure
The photosensitive resin composition addresses issues in forming thick partition walls by ensuring consistent line width and improved light blocking, enhancing color conversion performance and display quality.
Patent Information
- Application Number
- JP2022555839
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-16
- Filing Date
- 2020-11-25
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-11-25
AI Technical Summary
Conventional photosensitive resin compositions struggle with forming partition walls of 7 μm to 15 μm thickness for color conversion panels, leading to changes in line width due to varying development times, difficulty in aligning mask patterns, and reduced luminous efficiency due to light scattering and absorption by barrier ribs.
A photosensitive resin composition containing an alkali-soluble resin, polymerizable compound, photopolymerization initiator, and solvent, with specific transmittance and reflectance properties, is used to form partition walls that efficiently block blue light and maintain consistent line width, enhancing color conversion characteristics.
The composition effectively blocks blue light, maintains consistent line width, and improves color conversion performance by preventing color mixing and increasing red and green light reflectance, resulting in high-quality display devices.
Smart Images

Figure 0007562692000003 
Figure 0007562692000004 
Figure 0007562692000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive resin composition for forming a partition wall, a partition wall structure produced using the same, and a display device including the partition wall structure. [Background technology]
[0002] Generally, a display device including a color conversion panel using a blue light source exhibits light blocking properties against the blue light used as a light source, and to prevent color mixing of each color conversion pixel, a partition is formed between each color conversion pixel. Depending on the conversion efficiency of the color conversion pixels, the partition between each color conversion pixel is formed to a thickness of approximately 7 μm to 15 μm.
[0003] Conventionally used photosensitive resin compositions for black matrices have no problem in forming patterns when the film thickness is 1 μm to 1.5 μm as conventionally manufactured. However, the partition walls for color conversion panels must be formed to a film thickness of 7 μm to 15 μm. When partition walls having a thickness of 7 μm or more are formed using conventional photosensitive resin compositions for black matrices, the line width of the pattern changes significantly depending on the development time in the development process due to a decrease in the transmittance of ultraviolet light in the exposure process. If the line width of the partition walls between color conversion pixels increases for the same area, the size of the color conversion pixels decreases, resulting in a problem of reduced color conversion performance of the color conversion panel.
[0004] In addition, when a conventional photosensitive resin composition for black matrix is used to manufacture a barrier rib for a color conversion panel, it is difficult to form a pattern at an accurate position because it is difficult to recognize the align key at the bottom when aligning a mask pattern in an exposure process after a coating process. Furthermore, the barrier rib formed using the conventional photosensitive resin composition for black matrix has a problem that the light scattered by the barrier rib among the red or green light scattered by the quantum dots is absorbed by the barrier rib and disappears, thereby decreasing the luminous efficiency of the color conversion panel.
[0005] Meanwhile, in the conventional technology, a colored pattern using an organic pigment is manufactured to manufacture a color filter. In this case, in order to show each desired hue, CI red pigment (CI Pigment Red) to CI orange pigment (CI Pigment Orange) are used for a pattern where red is desired, and CI green pigment (CI Pigment Green) to CI yellow pigment (CI Pigment Yellow) are used for a pattern where green is desired. Usually, the thickness of the color filter coating film is manufactured to 2 μm to 3 μm, which is different from the above-mentioned barrier rib manufacturing technology for color conversion panels, which is manufactured to a thickness of 7 μm to 15 μm. Also, in terms of optics, the color filter aims to show a specific hue on the color coordinate system, and characteristics such as brightness and contrast are important, whereas the barrier rib for color conversion panels is a display device technology manufactured by combining a display including a color conversion panel with a blue light source.
[0006] In this regard, Korean Patent Publication No. 10-2007-0094460 aims to provide a photosensitive resin composition for forming partition walls having excellent shape stability against heat, but the above-mentioned problems are not overcome at present. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made to improve the above-mentioned conventional technical problems, and has an object to provide a photosensitive resin composition for forming a partition wall, which can efficiently block blue light and improve color conversion properties for red and green light.
[0008] Another object of the present invention is to provide a photosensitive resin composition for forming partition walls, which causes little change in line width of a pattern depending on the development time in a development step.
[0009] A further object of the present invention is to provide a structure produced using the photosensitive resin composition for forming partition walls, and a display device including the partition wall structure. [Means for solving the problem]
[0010] The present invention provides a photosensitive resin composition for forming a partition wall, which comprises an alkali-soluble resin, a polymerizable compound, a photopolymerization initiator, and a solvent, wherein a cured film produced from the photosensitive resin composition has a transmittance of less than 5% at a wavelength of 450 nm and a reflectance of 30% or more at a wavelength of 640 nm when the cured film has a thickness of 7 μm to 15 μm.
[0011] The present invention also provides a partition structure for color-converting pixels, which is manufactured using the photosensitive resin composition.
[0012] The present invention further provides a display device including a color conversion panel including the color conversion pixel barrier structure. Effect of the Invention
[0013] A cured film produced using the photosensitive resin composition for forming a partition wall of the present invention satisfies the characteristics that, when the cured film has a thickness of 7 μm to 15 μm, the transmittance at a wavelength of 450 nm is less than 5% and the reflectance at a wavelength of 640 nm is 30% or more, thereby efficiently blocking blue light while at the same time increasing the reflectance for red and green light, thereby providing the effect of improving the color conversion characteristics of a color conversion panel including the same.
[0014] In addition, the photosensitive resin composition of the present invention can form a structure in which the line width of a pattern changes little due to changes in development time in a development process, and thus can form color conversion pixels of a constant size, thereby providing the effect of preventing a decrease in color conversion performance due to a decrease in the size of the color conversion pixels.
[0015] Furthermore, the partition structure manufactured using the photosensitive resin composition of the present invention can be effectively applied to a color conversion panel using a blue light source and a display device including the same, thereby providing a high-quality display device. [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 is a diagram showing the transmission spectra of cured films produced using the photosensitive resin compositions according to Example 3 and Example 6 of the present invention, and Comparative Example 5. [Diagram 2] FIG. 2 is a diagram showing the reflectance spectra of cured films produced using the photosensitive resin compositions according to Example 3 and Example 6 of the present invention, and Comparative Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention provides a photosensitive resin composition for forming a partition wall, which comprises an alkali-soluble resin, a polymerizable compound, a photopolymerization initiator, and a solvent, and a cured film produced from the photosensitive resin composition has a transmittance of less than 5% at a wavelength of 450 nm and a reflectance of 30% or more at a wavelength of 640 nm when the cured film has a thickness of 7 μm to 15 μm. The present invention also provides a partition wall structure produced from the photosensitive resin composition, and a display device including the same.
[0018] The cured film produced from the photosensitive resin composition may preferably have a maximum transmittance at a wavelength of 450 nm of less than 4%, and more preferably less than 3%, when the cured film has a thickness of 7 μm to 15 μm.
[0019] Furthermore, the cured film produced from the photosensitive resin composition may preferably have a reflectance of 33% or more, and more preferably 36% or more, at a wavelength of 640 nm when the cured film has a thickness of 7 μm to 15 μm.
[0020] Furthermore, the cured film produced from the photosensitive resin composition may have a reflectance at a wavelength of 550 nm of 30% or more, preferably 35% or more, and more preferably 40% or more, when the cured film has a thickness of 7 μm to 15 μm.
[0021] When the cured film satisfies the above-mentioned conditions of specific transmittance and specific reflectance at a specific wavelength, it can efficiently block blue light used as a light source on the rear surface and can efficiently reflect red and green light, and can exhibit excellent light blocking properties and color conversion properties in a display device using a blue light source including the cured film as a partition structure.
[0022] A display device including a color conversion panel uses quantum dots in color conversion pixels to convert blue (high energy) light into green (low energy) or red (low energy) light to realize an image. The barrier structure used in this case has a very important technical purpose of blocking interference between pixels of a blue light source used as a light source and preventing color mixing of blue, green, and red pixels generated in each pixel, and is technically different from the barrier structure used in a color filter that realizes colors by transmitting light of a specific wavelength using a white light source.
[0023] On the other hand, in a display device including a color conversion panel, the thickness of each color conversion pixel is formed to be thick, about 10 μm, in order to increase the light absorbance of the color conversion layer and obtain sufficient light conversion efficiency. Therefore, the partition structure for the color conversion panel needs to be formed to a thickness of 7 μm to 15 μm according to the thickness of the color conversion pixel.
[0024] In addition, the barrier rib structure according to the prior art is generally formed in black, but in the case of a thickness of 7 μm to 15 μm, which is not the commonly used thickness of 1 μm to 2 μm, the thickness is too thick in the exposure process, and the ultraviolet transmittance is reduced, so that photocuring cannot be induced deep inside. If photocuring is not formed deep inside the coating film, there is a problem that the line width of the pattern changes due to a change in the development time in the development process, and in severe cases, the bottom end of the pattern is developed and the pattern disappears. Therefore, there is a limit to the use of black photosensitive resin compositions such as conventional photosensitive resin compositions for black matrices as a material for forming a barrier rib structure.
[0025] The photosensitive resin composition according to the present invention can form a red, yellow, or orange partition structure, and has the advantage that it can induce sufficient photocuring deep into the film even when a cured film having a thickness of 7 μm to 15 μm is formed, and therefore it can provide a partition structure with little change in line width of the pattern due to changes in development time in the development process. In this case, the line width of the pattern is formed to be 10 μm to 50 μm.
[0026] The present invention will be described in detail below. <Photosensitive resin composition> The photosensitive resin composition for forming partition walls according to the present invention contains an alkali-soluble resin, a polymerizable compound, a photopolymerization initiator, and a solvent, and may further contain one or more selected from a colorant and a scattering particle.
[0027] The photosensitive resin composition according to the present invention can be characterized as being for forming partition walls of a color conversion panel that uses a blue light source.
[0028] Alkali-soluble resin The alkali-soluble resin can be selected from resins known in this field without any particular restrictions, so long as it has reactivity due to the action of light or heat, is alkali-soluble, acts as a dispersion medium for the solid content contained in the photosensitive resin composition, and functions as a binder resin.
[0029] Specifically, the alkali-soluble resin is preferably a copolymer of an unsaturated carboxyl group-containing monomer and another monomer copolymerizable therewith.
[0030] Examples of the unsaturated carboxyl group-containing monomer include unsaturated carboxylic acids having one or more carboxyl groups in the molecule, such as unsaturated monocarboxylic acids, unsaturated dicarboxylic acids, and unsaturated polycarboxylic acids.
[0031] Examples of the unsaturated monocarboxylic acid include acrylic acid, methacrylic acid, crotonic acid, α-chloroacrylic acid, and cinnamic acid.
[0032] Examples of the unsaturated dicarboxylic acid include maleic acid, fumaric acid, itaconic acid, citraconic acid, and mesaconic acid.
[0033] The unsaturated polycarboxylic acid may be an acid anhydride, and specifically, examples thereof include maleic anhydride, itaconic anhydride, and citraconic anhydride. The unsaturated polycarboxylic acid may be a mono(2-methacryloyloxyalkyl)ester thereof, and examples thereof include mono(2-acryloyloxyethyl) succinate, mono(2-methacryloyloxyethyl) succinate, mono(2-acryloyloxyethyl) phthalate, and mono(2-methacryloyloxyethyl) phthalate. The unsaturated polycarboxylic acid may be a mono(meth)acrylate of a dicarboxy polymer at both ends thereof, and examples thereof include ω-carboxypolycaprolactone monoacrylate and ω-carboxypolycaprolactone monomethacrylate.
[0034] The unsaturated carboxyl group-containing monomers may be used alone or in combination of two or more.
[0035] Examples of other monomers copolymerizable with the unsaturated carboxyl group-containing monomer include aromatic vinyl compounds such as styrene, α-methylstyrene, o-vinyltoluene, m-vinyltoluene, p-vinyltoluene, p-chlorostyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-vinylbenzyl methyl ether, m-vinylbenzyl methyl ether, p-vinylbenzyl methyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, and indene;Methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-propyl acrylate, n-propyl methacrylate, i-propyl acrylate, i-propyl methacrylate, n-butyl acrylate, n-butyl methacrylate, i-butyl acrylate, i-butyl methacrylate, sec-butyl acrylate, sec-butyl methacrylate, t-butyl acrylate, t-butyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl acrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl acrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, allyl acrylate, allyl methacrylate, benzyl acrylate, benzyl methacrylate, silyl unsaturated carboxylic acid esters such as cyclohexyl acrylate, cyclohexyl methacrylate, phenyl acrylate, phenyl methacrylate, 2-methoxyethyl acrylate, 2-methoxyethyl methacrylate, 2-phenoxyethyl acrylate, 2-phenoxyethyl methacrylate, methoxydiethylene glycol acrylate, methoxydiethylene glycol methacrylate, methoxytriethylene glycol acrylate, methoxytriethylene glycol methacrylate, methoxypropylene glycol acrylate, methoxypropylene glycol methacrylate, methoxydipropylene glycol acrylate, methoxydipropylene glycol methacrylate, isobornyl acrylate, isobornyl methacrylate, dicyclopentadienyl acrylate, dicyclopentadiethyl methacrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl methacrylate, glycerol monoacrylate, and glycerol monomethacrylate;Unsaturated carboxylic acid aminoalkyl esters such as 2-aminoethyl acrylate, 2-aminoethyl methacrylate, 2-dimethylaminoethyl acrylate, 2-dimethylaminoethyl methacrylate, 2-aminopropyl acrylate, 2-aminopropyl methacrylate, 2-dimethylaminopropyl acrylate, 2-dimethylaminopropyl methacrylate, 3-aminopropyl acrylate, 3-aminopropyl methacrylate, 3-dimethylaminopropyl acrylate, and 3-dimethylaminopropyl methacrylate; unsaturated carboxylic acid glycidyl esters such as glycidyl acrylate and glycidyl methacrylate; carboxylic acid vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl benzoate; vinyl methyl ether, vinyl ethyl ether, and allyl glycidyl ether unsaturated ethers such as acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, vinylidene cyanide, and other vinyl cyanide compounds; unsaturated amides such as acrylamide, methacrylamide, α-chloroacrylamide, N-2-hydroxyethyl acrylamide, and N-2-hydroxyethyl methacrylamide; unsaturated imides such as maleimide, N-benzylmaleimide, N-phenylmaleimide, and N-cyclohexylmaleimide; aliphatic conjugated dienes such as 1,3-butadiene, isoprene, and chloroprene; and macromonomers having a monoacryloyl group or monomethacryloyl group at the end of the polymer molecular chain of polystyrene, polymethyl acrylate, polymethyl methacrylate, poly-n-butyl acrylate, poly-n-butyl methacrylate, and polysiloxane. Each of these monomers can be used alone or in a mixture of two or more kinds.
[0036] The content of the alkali-soluble resin is 20 to 70% by weight, preferably 30 to 60% by weight, based on the total weight of the solid content in the photosensitive resin composition. When the content of the alkali-soluble resin is within the above range, the solubility in the developer is sufficient, the formation of a cured film is easy, and the reduction in the film in the pixel portion of the exposed portion during development is prevented, resulting in good loss of the non-exposed portion, which is preferable.
[0037] In the present invention, the total weight of solids in the photosensitive resin composition means the total weight of the remaining components excluding the solvent in the photosensitive resin composition.
[0038] polymerizable compound The polymerizable compound is a compound that can be polymerized by light and heat, and any polymerizable compound known in this field can be selected and used without any particular limitation as long as it can be polymerized by light and heat. Specifically, a monofunctional monomer, a bifunctional monomer, other polyfunctional monomers, etc. can be used.
[0039] The type of the monofunctional monomer is not particularly limited, and examples thereof include nonylphenylcarbitol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-ethylhexylcarbitol acrylate, 2-hydroxyethyl acrylate, and N-vinylpyrrolidone.
[0040] The type of the bifunctional monomer is not particularly limited, and examples thereof include 1,6-hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, bis(acryloyloxyethyl)ether of bisphenol A, and 3-methylpentanediol di(meth)acrylate.
[0041] The type of the polyfunctional monomer is not particularly limited, and examples thereof include trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, ethoxylated dipentaerythritol hexa(meth)acrylate, propoxylated dipentaerythritol hexa(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0042] Commercially available examples of the polymerizable compound include, but are not limited to, Miramer M600 from Miwon Trading Co., Ltd.
[0043] The content of the polymerizable compound is 5 to 50% by weight, preferably 10 to 40% by weight, based on the total weight of the solid content in the photosensitive resin composition. When the content of the polymerizable compound is within the above range, it is preferable in terms of the strength and smoothness of the pixel portion.
[0044] Photoinitiator The photopolymerization initiator may be selected from among photopolymerization initiators known in the art without any particular limitations, such as acetophenone-based, benzophenone-based, triazine-based, thioxanthate-based, oxime-based, benzoin-based, and biimidazole-based compounds.
[0045] For example, the oxime compound may be o-ethoxycarbonyl-α-oxyimino-1-phenylpropan-1-one, and commercially available products include OXE-01 and OXE-02 from Ciba, but are not limited thereto.
[0046] The photopolymerization initiators can be used alone or in combination of two or more. The content of the photopolymerization initiator is 0.01 to 10% by weight, preferably 0.01 to 5% by weight, based on the total weight of solids in the photosensitive resin composition. When the content of the photopolymerization initiator is within the above range, the photopolymerization reaction rate is appropriate, the increase in the overall process time is prevented, and the deterioration of the physical properties of the final cured film due to overreaction can be prevented, which is preferable.
[0047] The photosensitive resin composition according to the present invention may further include a photopolymerization initiator assistant in addition to the photopolymerization initiator. When the photopolymerization initiator and the photopolymerization initiator are used together, the photosensitive resin composition becomes more sensitive, which is preferable since it improves productivity.
[0048] The photopolymerization initiator auxiliary is a compound used to promote the polymerization of the polymerizable compound initiated by the photopolymerization initiator, and one or more compounds selected from the group consisting of amines and carboxylic acid compounds can be preferably used.
[0049] When the photopolymerization initiation assistant is contained, the content thereof is usually more than 0 mole and 10 moles or less, and preferably 0.01 mole to 5 moles, relative to 1 mole of the photopolymerization initiator. When the photopolymerization initiation assistant is contained within the above range, it is preferable because the photopolymerization efficiency can be improved and the effect of improving productivity can be expected.
[0050] solvent As the solvent, any organic solvent known in this field can be used without any particular limitation.
[0051] Specific examples of the solvent include ethylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; diethylene glycol dialkyl ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; ethylene glycol alkyl ether acetates such as methyl cellosolve acetate and ethyl cellosolve acetate; propylene glycol monomethyl ether acetate; Examples of the alkylene glycol alkyl ether acetate include alkylene glycol alkyl ether acetates such as ether acetate, propylene glycol monopropyl ether acetate, methoxybutyl acetate, and methoxypentyl acetate; aromatic hydrocarbons such as benzene, toluene, xylene, and mesitylene; ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, and glycerin; esters such as ethyl 3-ethoxypropionate and methyl 3-methoxypropionate; and cyclic esters such as γ-butyrolactone.
[0052] In terms of coatability and drying property, the solvent is preferably an organic solvent having a boiling point of 100°C to 200°C, more preferably an alkylene glycol alkyl ether acetate, a ketone, or an ester such as ethyl 3-ethoxypropionate or methyl 3-methoxypropionate, and even more preferably propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, cyclohexanone, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, or the like.
[0053] The above solvents may be used alone or in combination of two or more kinds. The content of the solvent is 60 to 90% by weight, preferably 70 to 85% by weight, based on the total weight of the photosensitive resin composition. When the content of the solvent is within the above range, it is preferable because it provides an effect of improving coatability when applied by a coating device such as a roll coater, a spin coater, a slit and spin coater, a slit coater (sometimes called a die coater), or an inkjet.
[0054] Coloring agent The photosensitive resin composition according to the present invention may contain a colorant.
[0055] The colorant preferably includes at least one selected from the group consisting of CI red pigment (CI Pigment Red), CI yellow pigment (CI Pigment Yellow), and CI orange pigment (CI Pigment Orange), and thus the photosensitive resin composition according to the present invention can form a red, yellow, or orange partition structure. The red, yellow, or orange partition structure thus formed can absorb blue light and reflect red and / or green light. Therefore, in a display device using a blue light source, it is possible to prevent the intrusion of blue light and improve the red and / or green light emission characteristics.
[0056] Preferably, the CI red pigment (CI Pigment Red) may be one or more selected from diketopyrrole-based, anthraquinone-based, perylene-based, and azo-based pigments, the CI yellow pigment (CI Pigment Yellow) may be one or more selected from anthraquinone-based, isoindolinone-based, and azo-based pigments, and the CI orange pigment (CI Pigment Orange) may be one or more selected from quinophthalone-based, isoindolinone-based, and diketopyrrole-based pigments.
[0057] More preferably, the CI Red Pigment may be one or more selected from the group consisting of CI Red Pigments 9, 81, 97, 105, 122, 123, 144, 149, 150, 155, 166, 168, 171, 175, 176, 177, 179, 180, 185, 192, 202, 208, 209, 214, 215, 216, 220, 222, 224, 242, 254, 255, 264, 269, 270, and 272; The CI Yellow pigment may be one or more selected from the group consisting of CI Yellow Pigments 11, 13, 20, 24, 31, 53, 83, 86, 93, 94, 95, 99, 108, 109, 110, 117, 125, 128, 129, 138, 139, 147, 148, 150, 151, 154, 155, 166, 167, 173, 180, 185, and 199; The CI Orange pigment may be one or more selected from the group consisting of CI Orange pigments 13, 15, 31, 36, 38, 40, 42, 43, 51, 55, 59, 61, 64, 65, and 71.
[0058] Most preferably, the CI Red Pigment is one or more selected from the group consisting of CI Red Pigment 177, 179, 254, 264 and 269, the CI Yellow Pigment is one or more selected from the group consisting of CI Yellow Pigment 138, 139, 150 and 185, and the CI Orange Pigment may be one or more selected from the group consisting of CI Orange Pigment 64 and 71.
[0059] In addition, the present invention has a feature that it can efficiently block blue light even without containing a black colorant. For this reason, the colorant of the present invention preferably does not contain a black colorant. However, if necessary, it can contain up to 10% by weight, more preferably up to 5% by weight, based on the total weight of the colorant. If the black colorant is contained in excess as a colorant, it is not preferable because there is a problem that inverse taper occurs due to insufficient deep curing, and the light-emitting efficiency of the display device decreases due to a decrease in reflectance.
[0060] Specifically, the black colorant may include black organic / inorganic pigments and dyes such as carbon black, titanium black, aniline black, lactam black, and perylene black, and is understood as including a concept that includes a combination of a plurality of colorants that can exhibit black color.
[0061] When the photosensitive resin composition for forming a partition wall according to the present invention contains the colorant, the content thereof is 1 to 30% by weight, preferably 1.5 to 25% by weight, based on the total weight of the solid content in the photosensitive resin composition. When the colorant is contained within the above range, the light-shielding property for blue light is improved, and the reflectance for red and / or green light is increased, thereby improving the light-emitting property of the display device.
[0062] On the other hand, the pigment can be used as a pigment dispersion in which the pigment particle size is uniformly dispersed. An example of a method for uniformly dispersing the pigment particle size is a method in which a pigment dispersant is added and a dispersion treatment is performed, and the pigment dispersion in which the pigment is uniformly dispersed in the solution can be obtained by the above method.
[0063] The pigment dispersant is added to deflocculate the pigment and maintain its stability, and any dispersant commonly used in the art can be used without limitation. Specific examples of the pigment dispersant include cationic, anionic, nonionic, amphoteric, polyester, and polyamine surfactants, and these can be used alone or in combination of two or more.
[0064] The pigment dispersant preferably contains an acrylate-based dispersant containing butyl methacrylate (BMA) or N,N-dimethylaminoethyl methacrylate (DMAEMA), and in addition to the acrylate-based dispersant, other resin-type pigment dispersants may be used. The resin-type pigment dispersants may be used alone or in combination with two or more of the acrylate-based dispersants, and may be used in combination with the acrylate-based dispersants.
[0065] scattering particles The photosensitive resin composition for forming partition walls according to the present invention may contain scattering particles.
[0066] The scattering particles may be selected from scattering particles known in the art without any particular restrictions. Specifically, the scattering particles may include one or more oxides selected from the group consisting of Li, Be, B, Na, Mg, Al, Si, K, Ca, Sc, V, Cr, Mn, Fe, Ni, Cu, Zn, Ga, Ge, Rb, Sr, Y, Mo, Cs, Ba, La, Hf, W, Tl, Pb, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Ti, Sb, Sn, Zr, Nb, Ce, Ta, In, and combinations thereof. For example, the scattering particles may include one or more selected from the group consisting of Al2O3, SiO2, ZnO, ZrO2, BaTiO3, TiO2, Ta2O5, Ti3O5, ITO, IZO, ATO, ZnO-Al, Nb2O3, SnO, and MgO, and if necessary, a material that has been surface-treated with a compound having an unsaturated bond, such as an acrylate, may also be used.
[0067] The scattering particles may have a limited average particle size and a limited content in the entire composition so as to maximize the luminous intensity of the color filter.
[0068] In the present invention, the "average particle size" may be a number-average particle size, and may be determined, for example, from an image observed by a field emission scanning electron microscope (FE-SEM) or a transmission electron microscope (TEM). Specifically, it can be obtained by extracting several samples from the observation image of the FE-SEM or TEM, measuring the diameters of these samples, and taking the arithmetic average value.
[0069] For example, in one embodiment of the present invention, the scattering particles may have an average particle size of 30 to 500 nm, preferably 30 to 300 nm. When the average particle size of the scattering particles satisfies the above range, the scattering effect is enhanced, and the photosensitive resin composition including the scattering particles may easily ensure the reflectance of red and / or green light.
[0070] When the photosensitive resin composition for forming partition walls according to the present invention contains the scattering particles, the content thereof is 0.1 to 50% by weight, preferably 0.5 to 20% by weight, based on the total weight of the solid content in the photosensitive resin composition. When the scattering particles are contained within the above range, it is easy to ensure the reflectance for red and / or green light, and deterioration of the stability of the composition can be suppressed, which is preferable.
[0071] Additives The photosensitive resin composition according to the present invention may further contain additives as necessary, and the type of additive is determined according to the needs of the user and is not particularly limited in the present invention, but examples thereof include fillers, other polymer compounds, heat curing agents, surfactants, adhesion promoters, antioxidants, anti-aggregation agents, dispersants, etc. The additives exemplified above may be used alone or in combination of two or more kinds.
[0072] Specific examples of the other polymer compounds include curable resins such as epoxy resins and maleimide resins; and thermoplastic resins such as polyvinyl alcohol, polyacrylic acid, polyethylene glycol monoalkyl ether, polyfluoroalkyl acrylate, polyester, and polyurethane.
[0073] The antioxidant may include at least one selected from the group consisting of phosphorus-based antioxidants, sulfur-based antioxidants, and phenol-based antioxidants, and in this case, it is possible to suppress discoloration that may occur at high temperatures during the process or yellowing caused by a light source after display fabrication. The antioxidant may include at least one selected from the group consisting of phenolic compounds, phosphorus-based compounds, and sulfur-based compounds, and these can be used in combination as phenolic-phosphorus compounds, phenolic-sulfur compounds, phosphorus-sulfur compounds, or phenolic-phosphorus-sulfur compounds.
[0074] The content of the antioxidant is 0.1 to 30% by weight, preferably 0.5 to 20% by weight, based on the total weight of the solid content in the photosensitive resin composition. When the content of the antioxidant is within the above range, it is preferable in terms of solving the problem of a decrease in luminescence intensity.
[0075] The dispersant is added to maintain the dispersion stability of the pigment, and any dispersant generally used in the relevant field can be used without any restrictions.
[0076] In the case of the additives whose contents are not exemplified among the additives, those skilled in the art can add them appropriately within the range that does not impair the effects of the present invention. For example, the additives can be used in an amount of 0.05 to 10% by weight, preferably 0.1 to 10% by weight, more preferably 0.1 to 5% by weight, based on the total weight of the photosensitive resin composition, but are not limited thereto.
[0077] The photosensitive resin composition of the present invention can be produced by a conventional method known in the art, and is not particularly limited in the present invention. For example, the composition can be produced by the following method.
[0078] The colorant and / or scattering particles are mixed with a solvent in advance and dispersed using a bead mill or the like until the average particle size of the colorant becomes 30 to 300 nm. At this time, a dispersant can be additionally used as necessary, and a part or all of the alkali-soluble resin may be blended. The remaining alkali-soluble resin, the polymerizable compound, and the photopolymerization initiator, as well as additional additives as necessary and additional solvent as necessary are further added to the obtained dispersion (hereinafter sometimes referred to as mill base) to a predetermined concentration, to obtain the desired photosensitive resin composition.
[0079] <Bulkhead structure and display device> The present invention provides a barrier rib structure prepared using the photosensitive resin composition and a display device including the same.
[0080] In a display device including a color conversion panel, each pixel is driven to form a hue, so a partition structure that can distinguish each pixel must be formed. A display device including a partition structure for a color conversion panel formed using the photosensitive resin composition of the present invention is advantageous for forming fine patterns as color mixing between pixels is prevented, and it is possible to manufacture partitions with little change in line width due to changes in development time in the development process. When the line width of the partition is little changed, there is an advantage that the color conversion pixels can secure sufficient space, thereby realizing a high-quality image.
[0081] The display device may include, but is not limited to, a liquid crystal display device, an organic light emitting diode, a flexible display, etc., and may be any display device known in the art that is applicable.
[0082] The partition structure including the color conversion panel can be produced by applying the above-mentioned photosensitive resin composition of the present invention onto a substrate, photocuring and developing the composition to form a cured film.
[0083] First, a photosensitive resin composition is applied onto a substrate, and then heated and dried to remove volatile components such as the solvent, thereby obtaining a smooth coating film.
[0084] The coating method can be, for example, spin coating, casting coating, roll coating, slit and spin coating, or slit coating. After coating, the coating is heated and dried (pre-baked), or dried under reduced pressure, and then heated to volatilize volatile components such as the solvent. The heating temperature is usually 70 to 150°C, preferably 80 to 130°C. The thickness of the coating film after drying is usually about 7 to 15 μm. The coating film thus obtained is irradiated with ultraviolet light through a mask for forming a desired pattern. At this time, it is preferable to use a device such as a mask aligner or a stepper so that the entire exposed area is uniformly irradiated with parallel light and the mask and the substrate are accurately aligned. When ultraviolet light is irradiated, radicals are formed by the photopolymerization initiator at the area irradiated with ultraviolet light, which reacts with the polymerizable compound to cause photocuring.
[0085] As the ultraviolet ray, g-ray (wavelength: 436 nm), h-ray, i-ray (wavelength: 365 nm), etc. can be used. The amount of ultraviolet ray irradiation can be appropriately selected as necessary, and is not limited thereto in the present invention. The coating film after photocuring is brought into contact with a developer to dissolve the unexposed areas and develop the coating film, thereby obtaining the desired pattern shape.
[0086] The shape of the pattern thus obtained can be hardened by a post-curing step, and the heating temperature is usually 150 to 250° C., preferably 180 to 230° C. The heating time is usually 5 to 30 minutes, preferably 15 to 20 minutes. EXAMPLES
[0087] The present invention will be described in more detail below based on examples, but the embodiments of the present invention disclosed below are merely illustrative, and the scope of the present invention is not limited to these embodiments. The scope of the present invention is set forth in the claims, and further includes all modifications within the scope and meaning equivalent to the claims. In the following examples and comparative examples, the "%" and "parts" indicating the content are based on mass unless otherwise specified.
[0088] <Example> Synthesis Example 1: Synthesis of alkali-soluble resin A flask equipped with a stirrer, a thermometer, a reflux condenser, and a dropping funnel, and a nitrogen inlet tube were prepared. On the one hand, 15 parts by weight of N-benzylmaleimide, 30 parts by weight of acrylic acid, 50 parts by weight of cyclohexyl methacrylate, 5 parts by weight of methyl methacrylate, 4 parts by weight of t-butylperoxy-2-ethylhexanoate, and 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) were added and stirred and mixed to prepare a monomer dropping funnel, and 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added and stirred and mixed to prepare a chain transfer agent dropping funnel.
[0089] Thereafter, 395 parts by weight of PGMEA was introduced into the flask, the atmosphere in the flask was replaced from air to nitrogen, and the temperature of the flask was raised to 90°C while stirring. Next, the monomer and chain transfer agent were added dropwise from the dropping funnel. The dropping was continued for 2 hours while maintaining the temperature at 90°C, and after 1 hour, the temperature was raised to 110°C and maintained for 3 hours. Then, a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen = 5 / 95 (v / v) was started.
[0090] Next, 20 parts by weight of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask, and the reaction was continued at 110°C for 6 hours. Thereafter, the mixture was cooled to room temperature to obtain an alkali-soluble resin having a weight average molecular weight of 3,800 and an acid value based on solid content of 83 mgKOH / g.
[0091] The weight average molecular weight (Mw) of the alkali-soluble resin was measured by GPC using an HLC-8120GPC (manufactured by Tosoh Corporation).
[0092] The measurement conditions were as follows: TSK-GELG4000HXL and TSK-GELG2000HXL columns were connected in series, and the column temperature was 40°C. Tetrahydrofuran was used as the mobile phase solvent, and the measurement was performed at a flow rate of 1.0 mL / min. The concentration of the measurement sample was 0.6 wt%, the injection amount was 50 μl, and the analysis was performed using an RI detector. TSK STANDARD POLYSTYRENE F-40, F-4, F-1, A-2500, and A-500 (manufactured by Tosoh Corporation) were used as calibration standards, and the weight average molecular weight of the alkali-soluble resin obtained under the above conditions was measured.
[0093] Examples 1 to 11 and Comparative Examples 1 to 7: Production of Photosensitive Resin Compositions Photosensitive resin compositions of Examples 1 to 11 and Comparative Examples 1 to 7 were produced according to the compositions and contents in Table 1 below.
[0094] [Table 1]
[0095] -R177: CI Red Pigment 177 -R179: CI Red Pigment 179 -R254: CI Red Pigment 254 -R264: CI Red Pigment 264 -R269: CI Red Pigment 269 -Y138: CI Yellow Pigment 138 -Y139: CI Yellow Pigment 139 -Y150: CI Yellow Pigment 150 -Y185: CI Yellow Pigment 185 -O64: CI Orange Pigment 64 -O71: CI Orange Pigment 71 -B7: CI Black Pigment 7 -OB: Organic black pigment -G36: CI Green Pigment 36 -B15:6:CI Blue Pigment 15:6 -Scattering particles: TiO2 -Alkali-soluble resin: Alkali-soluble resin according to Synthesis Example 1 -Photopolymerizable compound: Dipentaerythritol hexaacrylate (Kayarad DPHA, manufactured by Nippon Kagaku) -Photopolymerization initiator: Irgacure OXE-02 (manufactured by Basf) -Dispersant: DISPERBYK-110 (BYK) -Solvent: Propylene glycol monomethyl ether acetate (PGMEA) Experimental Example (1) Manufacturing of barrier rib pattern cured film A 5 cm x 5 cm glass substrate (Corning) was washed with a neutral detergent and water, and then dried. On the glass substrate, each of the photosensitive resin compositions according to Examples 1 to 11 and Comparative Examples 1 to 7 was spin-coated to a final film thickness of 10 μm, pre-baked at 100°C, and dried for 2 minutes to remove the solvent. Then, a mask including a 1 to 100 μm line / space pattern or a 40 mm x 40 mm pattern was applied at an exposure dose of 50 mJ / cm. 2The non-exposed portion was removed using an alkaline aqueous solution. The prepared cured film was then post-baked at 230° C. for 20 minutes to prepare a barrier rib pattern cured film having a thickness of 10 μm.
[0096] (2) Measurement of transmittance and reflectance The transmittance and reflectance of the 40 mm x 40 mm patterned cured film manufactured to a thickness of 10 μm were measured by wavelength using a spectrophotometer (Spectrophotometer, CM-3700d). When the transmittance at a wavelength of 450 nm was less than 5%, it was marked as O, when it was 5% or more, it was marked as X, when the reflectance at a wavelength of 640 nm was 30% or more, it was marked as O, when it was less than 30%, when it was 30% or more, it was marked as O, and when it was less than 30%, it was marked as X. The results are shown in Table 2, Figures 1 and 2 below.
[0097] (3) Measurement of line width change The line width of the 100 μm line mask pattern was measured using an optical microscope (ECLIPSE LV100POL, Nikon Corporation) for each of the substrates developed for 80 seconds and 160 seconds in the barrier rib pattern cured film manufacturing process (1). The line width of the pattern of the substrate developed for 80 seconds and the line width change of the pattern of the substrate developed for 160 seconds were measured, and the case where the line width change was 5.0 μm or more was indicated as X. The results are shown in Table 2 below.
[0098] [Table 2]
[0099] It can be seen that the cured films prepared using the photosensitive resin compositions of Examples 1 to 11 have a transmittance of less than 5% at a wavelength of 450 nm, a reflectance of 30% or more at a wavelength of 640 nm, and excellent line width change of the pattern.
[0100] In particular, it can be confirmed that the cured films produced using the photosensitive resin compositions according to Examples 6 to 9, which contain a yellow pigment as a colorant, have a reflectance of 30% or more at a wavelength of 550 nm.
[0101] In contrast, the cured films prepared using the photosensitive resin compositions of Comparative Examples 1 and 2, which did not contain scattering particles, showed a transmittance of less than 5% at a wavelength of 450 nm, but a reflectance of less than 30% at a wavelength of 640 nm, and it was confirmed that the line width change of the pattern was also very large.
[0102] In addition, it can be seen that the cured film prepared using the photosensitive resin composition of Comparative Example 3, which does not contain a colorant, exhibited a reflectance of 30% or more at a wavelength of 640 nm, but a transmittance of more than 5% at a wavelength of 450 nm, and the change in line width of the pattern was also very large.
[0103] In particular, the cured films prepared using the photosensitive resin compositions according to Comparative Examples 4 and 5, which contained only a black colorant, not a red, yellow, or orange colorant, showed a transmittance of less than 5% at a wavelength of 450 nm, but showed a reflectance of less than 30% at a wavelength of 640 nm, despite the inclusion of scattering particles, and thus failed to achieve the effect aimed at by the present invention.
Claims
1. The ink includes a colorant, scattering particles, an alkali-soluble resin, a polymerizable compound, a photopolymerization initiator, and a solvent, The colorant includes at least one selected from the group consisting of C.I. red pigment (C.I. Pigment Red), C.I. yellow pigment (C.I. Pigment Yellow), and C.I. orange pigment (C.I. Pigment Orange), and does not include a black or blue colorant, A cured film produced from the photosensitive resin composition has a transmittance of less than 5% at a wavelength of 450 nm and a reflectance of 30% or more at a wavelength of 640 nm when the cured film has a thickness of 7 μm to 15 μm.
2. The photosensitive resin composition for forming partition walls according to claim 1, wherein the C.I. Pigment Red is at least one selected from the group consisting of diketopyrrole-based, anthraquinone-based, perylene-based, and azo-based pigments.
3. The photosensitive resin composition for forming partition walls according to claim 1, wherein the C. I. Pigment Yellow is at least one selected from anthraquinone-based, isoindolinone-based, and azo-based pigments.
4. The photosensitive resin composition for forming partition walls according to claim 1, wherein the C. I. Pigment Orange is at least one selected from the group consisting of quinophthalone, isoindolinone, and diketopyrrole pigments.
5. The C.I. red pigment is one or more selected from the group consisting of C.I. red pigments 177, 179, 254, 264, and 269; The C.I. yellow pigment is one or more selected from the group consisting of C.I. yellow pigments 138, 139, 150, and 185; The photosensitive resin composition for forming partition walls according to claim 1, wherein the C.I. orange pigment is at least one selected from the group consisting of C.I. orange pigments 64 and 71.
6. The scattering particles are Al 2 O 3 , SiO 2 , ZnO, ZrO 2 , BaTiO 3 , TiO 2 , Ta 2 O 5 , Ti 3 O 5 , ITO, IZO, ATO, ZnO-Al, Nb 2 O 3 2. The photosensitive resin composition for forming partition walls according to claim 1, further comprising at least one selected from the group consisting of SnO and MgO.
7. 2. The photosensitive resin composition for forming partition walls according to claim 1, which is used for forming partition walls of a color conversion panel using a blue light source.
8. Relative to the total weight of solids in the photosensitive resin composition, 20 to 70% by weight of said alkali-soluble resin; 5 to 50% by weight of the polymerizable compound; 0.01 to 10% by weight of the photopolymerization initiator; and 2. The photosensitive resin composition for forming partition walls according to claim 1, wherein the photosensitive resin composition contains 60 to 90% by weight of a solvent based on the total weight of the photosensitive resin composition.
9. 2. The photosensitive resin composition for forming partition walls according to claim 1, wherein a cured film produced from the photosensitive resin composition has a reflectance of 30% or more at a wavelength of 550 nm when the cured film has a thickness of 7 μm to 15 μm.
10. A partition structure produced from the photosensitive resin composition according to any one of claims 1 to 9.
11. A display device comprising the partition structure according to claim 10.
Citation Information
Patent Citations
Semiconductor light-emitting device
JP2004055632A
Transparent plate with light-shielding layer
JP2019144338A
Transparent plate with light shielding layer
JP2019191340A
Resin composition, light-blocking film, method for producing light-blocking film, and substrate having partitioning wall attached thereto
WO2020008969A1