Sulfide solid electrolyte, electric storage element, and method for producing sulfide solid electrolyte

A sulfide solid electrolyte with a unique crystal structure and composition, produced by controlled heat-treatment of a sulfide glass, addresses the need for improved ionic conductivity in power storage elements, enhancing their charging and discharging capabilities.

JP7563033B2Active Publication Date: 2024-10-08GS YUASA CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020134094
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-06
Publication Date
2024-10-08
Estimated Expiration
2040-08-06

AI Technical Summary

Technical Problem

There is a need for sulfide solid electrolytes with improved ionic conductivity for use in power storage elements, particularly in hybrid electric vehicles and hybrid industrial machinery, to enhance their performance.

Method used

A sulfide solid electrolyte with a specific crystal structure, characterized by diffraction peaks at 2θ=17.8°±0.5°, 19.1°±0.5°, 21.7°±0.5°, and 23.8°±0.5°, and 30.85°±0.5°, and containing lithium, sulfur, phosphorus, and chlorine, is produced by heat-treating a sulfide glass with a pentavalent phosphorus valence, ensuring a temperature difference of 20°C to 45°C from the crystallization temperature to suppress crystalline phases with low ionic conductivity.

Benefits of technology

The resulting sulfide solid electrolyte exhibits excellent ionic conductivity, improving charge/discharge performance, especially at high rates, making it suitable for advanced power storage elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563033000002
    Figure 0007563033000002
  • Figure 0007563033000003
    Figure 0007563033000003
  • Figure 0007563033000004
    Figure 0007563033000004
Patent Text Reader

Abstract

To provide a sulfide solid electrolyte that is excellent in ionic conductivity, an electricity storage element that contains a sulfide solid electrolyte excellent in ionic conductivity, and a method for producing a sulfide solid electrolyte excellent in ionic conductivity.SOLUTION: The sulfide solid electrolyte contains lithium, sulfur, phosphorus and chlorine, has a crystalline structure that has diffraction peaks at 2θ=17.8°±0.5°, 19.1°±0.5°, 21.7°±0.5°, 23.8°±0.5°, and 30.85°±0.5° in X-ray diffraction measurement using CuKα ray, and in which the valence of the phosphorus is 5, and the sulfide solid electrolyte has virtually no crystalline phase of β-Li3 PS4.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sulfide solid electrolyte, an electricity storage element, and a method for producing the sulfide solid electrolyte. [Background technology]

[0002] Lithium ion secondary batteries are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc., due to their high energy density. The lithium ion secondary battery generally has a pair of electrodes electrically isolated by a separator and a non-aqueous electrolyte interposed between the electrodes, and is configured to charge and discharge by transferring lithium ions between the electrodes. In addition, capacitors such as lithium ion capacitors are also widely used as storage elements other than lithium ion secondary batteries.

[0003] In recent years, with the aim of improving the safety of non-aqueous electrolyte secondary batteries, all-solid-state batteries have been proposed that use a sulfide solid electrolyte or the like as the non-aqueous electrolyte instead of a liquid electrolyte such as an organic solvent (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-340257 A Summary of the Invention [Problem to be solved by the invention]

[0005] For energy storage elements used in hybrid electric vehicles (hereinafter also referred to as "HEVs") and hybrid industrial machinery (heavy machinery, construction machinery, etc.), sulfide solid electrolyte materials with further improved ionic conductivity are desired.

[0006] The present invention has been made in light of the above circumstances, and has an object to provide a sulfide solid electrolyte having excellent ion conductivity, an energy storage element containing a sulfide solid electrolyte having excellent ion conductivity, and a method for producing a sulfide solid electrolyte having excellent ion conductivity. [Means for solving the problem]

[0007] One aspect of the present invention is a sulfide solid electrolyte that contains lithium, sulfur, phosphorus, and chlorine, and has a crystal structure having diffraction peaks at 2θ=17.8°±0.5°, 19.1°±0.5°, 21.7°±0.5°, 23.8°±0.5°, and 30.85°±0.5° in X-ray diffraction measurement using CuKα radiation, in which the valence of the phosphorus is pentavalent, and which is substantially free of a β-Li3PS4 crystal phase.

[0008] Another aspect of the present invention is an electricity storage element containing the sulfide solid electrolyte according to one aspect of the present invention.

[0009] Another aspect of the present invention is a method for producing a sulfide solid electrolyte, comprising heat treating a sulfide glass containing lithium, sulfur, phosphorus, and chlorine, wherein the phosphorus has a valence of five, wherein the heat treatment temperature is lower than a crystallization temperature of the sulfide glass, and a difference between the crystallization temperature and the heat treatment temperature is 20°C or more and 45°C or less. Effect of the Invention

[0010] According to one aspect of the present invention, it is possible to provide a sulfide solid electrolyte having excellent ion conductivity, an energy storage element containing a sulfide solid electrolyte having excellent ion conductivity, and a method for producing a sulfide solid electrolyte having excellent ion conductivity. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view of an all-solid-state battery which is one embodiment of the energy storage element of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an energy storage device formed by assembling a plurality of energy storage elements according to one embodiment of the present invention. [Diagram 3] FIG. 3 is an X-ray diffraction diagram for each of the solid electrolytes of Examples 2 to 4 and Comparative Examples 2 to 4. [Figure 4] FIG. 4 is an X-ray diffraction diagram of each of the solid electrolytes of Examples 1, 3, 5 to 7, and Comparative Examples 1 and 5. [Diagram 5] FIG. 5 shows X-ray diffraction patterns of the solid electrolytes of Example 3, Comparative Example 6, and Reference Example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The sulfide solid electrolyte according to one aspect of the present invention contains lithium, sulfur, phosphorus, and chlorine, and has a crystal structure having diffraction peaks at 2θ=17.8°±0.5°, 19.1°±0.5°, 21.7°±0.5°, 23.8°±0.5°, and 30.85°±0.5° in X-ray diffraction measurement using CuKα radiation, the valence of the phosphorus is pentavalent, and the electrolyte is substantially free of a β-Li3PS4 crystal phase.

[0013] The present inventors have focused on the fact that, among halogen atoms, chlorine has superior electrochemical stability compared to bromine and iodine in order to improve the battery performance of an energy storage element, and have come up with the present invention based on the idea that a chlorine-containing Li2S-P2S5-LiCl-based glass ceramic solid electrolyte does not have a crystal structure with low ion conductivity, but has a specific crystal structure, thereby making it possible to obtain a sulfide solid electrolyte with excellent ion conductivity. The sulfide solid electrolyte contains lithium, sulfur, pentavalent phosphorus and chlorine, and is substantially free of the β-Li3PS4 crystal phase, which has low ionic conductivity.Instead, the sulfide solid electrolyte has a crystal structure having diffraction peaks at 2θ=17.8°±0.5°, 19.1°±0.5°, 21.7°±0.5°, 23.8°±0.5°, and 30.85°±0.5° in X-ray diffraction measurement using CuKα rays, which is considered to be a crystalline phase with high ionic conductivity, and thus has excellent ionic conductivity. In the present invention, "substantially free of β-Li3PS4 crystal phase" includes not only the case where the crystal phase is not contained at all in the structure, but also the case where the content is so low that it is below the detection limit in X-ray diffraction measurement. Note that the above "case where it is below the detection limit in X-ray diffraction measurement" also includes the case where it is below the detection limit in X-ray diffraction measurement, but the β-Li3PS4 crystal phase is detected in observation with a transmission electron microscope (TEM).

[0014] The sulfide solid electrolyte preferably has a composition represented by the general formula (100-z)(yLi2S (1-y)P2S5) zLiCl αM (wherein 0.74≦y≦0.78, 5≦z≦55, and 0≦α≦30. M represents one or more elements other than Li, P, S, and Cl). When the sulfide solid electrolyte has a composition represented by the general formula, the ionic conductivity can be further increased.

[0015] The ionic conductivity of the sulfide solid electrolyte at 25°C is 6.0×10 -4 When the ionic conductivity of the sulfide solid electrolyte at 25° C. is equal to or higher than the above value, the charge / discharge performance, such as the high-rate charge / discharge performance, of an energy storage element containing the sulfide solid electrolyte can be improved.

[0016] An electric storage element according to another aspect of the present invention contains the sulfide solid electrolyte.

[0017] The energy storage element according to another aspect of the present invention contains the sulfide solid electrolyte, and therefore has excellent ion conductivity and can improve charge / discharge performance, such as high-rate charge / discharge performance.

[0018] A method for producing a sulfide solid electrolyte according to another aspect of the present invention includes heat treating a sulfide glass containing lithium, sulfur, phosphorus, and chlorine, where the phosphorus has a valence of five, wherein the heat treatment temperature is lower than a crystallization temperature of the sulfide glass, and a difference between the crystallization temperature and the heat treatment temperature is 20°C or more and 45°C or less.

[0019] When Li2S-P2S5-LiCl-based glass is heated, the β-Li3PS4 crystal phase, which is a phase with low ion conductivity, tends to precipitate along with the precipitation of the β-Li3PS4 crystal phase, which is a phase with high ion conductivity. The present inventors have found that by heating Li2S-P2S5-LiCl-based glass under certain conditions, the precipitation of the β-Li3PS4 crystal phase, which is a phase with low ion conductivity, can be suppressed, and the composition range in which the β-Li3PS4 crystal phase precipitates with high ion conductivity can be expanded. The method for producing a sulfide solid electrolyte includes heat treating a sulfide glass having the above composition, and the temperature of the heat treatment is lower than the crystallization temperature of the sulfide glass, and the difference between the crystallization temperature and the heat treatment temperature is 20°C or more and 45°C or less, so that a sulfide solid electrolyte having a crystal phase with high ion conductivity and substantially no β-Li3PS4 crystal phase with low ion conductivity can be produced. Therefore, the production method can produce a sulfide solid electrolyte with excellent ion conductivity.

[0020] In addition, in the Li2S-P2S5-LiCl-based glass, which is the raw material used in the manufacturing method of the sulfide solid electrolyte, the valence of phosphorus (P) is +5. Therefore, in the sulfide glass of the above composition, PS4 3- When this sulfide glass is heat-treated at a temperature higher than the crystallization temperature of the sulfide glass, the same PS4 3- On the other hand, sulfide glass made from phosphorus with a valence other than +5, such as 0 or +3, is likely to undergo a phase transition to PS4. 3- In addition to the unit, P2S6 4-It is known that units are generated (Solid State Ionics 262 (2014) 733-737, JP 2018-174130 A, etc.). When this sulfide glass is heat-treated, it is assumed that it is difficult to undergo a phase transition to the β-Li3PS4 phase even under high temperature conditions, and that it changes to another crystal phase. Therefore, it is assumed that the phenomenon of the generation of the β-Li3PS4 phase when heat-treated at a temperature higher than the crystallization temperature of the sulfide glass is remarkable when the valence of phosphorus contained in the sulfide glass, which is the raw material of the sulfide solid electrolyte, is substantially only +5.

[0021] The sulfide glass preferably has a composition represented by the general formula (100-z)(yLi2S (1-y)P2S5) zLiCl αM (wherein 0.74≦y≦0.78, 5≦z≦55, and 0≦α≦30; M represents one or more elements other than Li, P, S, and Cl). When the sulfide glass has a composition represented by the general formula, a sulfide solid electrolyte having higher ion conductivity can be produced.

[0022] Hereinafter, embodiments of the sulfide solid electrolyte and the all-solid-state battery according to the present invention will be described in detail.

[0023] <Sulfide solid electrolyte> The sulfide solid electrolyte according to one embodiment of the present invention contains lithium, sulfur, phosphorus, and chlorine, and has a crystal structure (hereinafter also referred to as crystalline phase A) having diffraction peaks at 2θ=17.8°±0.5°, 19.1°±0.5°, 21.7°±0.5°, 23.8°±0.5°, and 30.85°±0.5° in an X-ray diffraction measurement using CuKα radiation, the valence of the phosphorus is pentavalent, and the sulfide solid electrolyte does not substantially have a β-Li3PS4 crystal phase. The sulfide solid electrolyte can be used for any application requiring excellent ion conductivity. In particular, the sulfide solid electrolyte is preferably used for a lithium storage element.

[0024] The sulfide solid electrolyte contains lithium, sulfur, phosphorus, and chlorine, and has a crystalline structure. The valence of the phosphorus is pentavalent. Here, "having a crystalline structure" means that a peak derived from the crystalline structure of the sulfide solid electrolyte is observed in an X-ray diffraction pattern in an X-ray diffraction measurement. The sulfide solid electrolyte having a crystalline structure can be obtained, for example, by crystallizing an amorphous sulfide glass solid electrolyte by heat treatment or the like.

[0025] The sulfide solid electrolyte is substantially free of a β-Li3PS4 crystal phase, which has low ionic conductivity, and has a crystal structure having diffraction peaks at 2θ=17.8°±0.5°, 19.1°±0.5°, 21.7°±0.5°, 23.8°±0.5°, and 30.85°±0.5° in X-ray diffraction measurement using CuKα rays, which is considered to be a crystalline phase with high ionic conductivity, and therefore has excellent ionic conductivity.

[0026] The diffraction peak in the first crystal structure may be within the range of ±0.3°, or may be within the range of ±0.1° of the range of 2θ.

[0027] The crystal phase of the above β-Li3PS4 is the same as the crystal phase reported in Electrochemistry Communications 5 (2003) 111-114, and in X-ray diffraction measurement using the above CuKα radiation, it has diffraction peaks at 2θ=17.5°±0.5°, 18.6°±0.5°, 29.1°±0.5°, 29.9°±0.5°, and 31.2°±0.5°. Therefore, the sulfide solid electrolyte does not have a diffraction peak that can be identified with the β-Li3PS4 crystal phase in an X-ray diffraction diagram using CuKα radiation.

[0028] The X-ray diffraction measurement using CuKα radiation is carried out according to the following procedure. The solid electrolyte powder to be measured is filled into an airtight sample holder for X-ray diffraction measurement in an argon atmosphere with a dew point of -50°C or less. Powder X-ray diffraction measurement is carried out using an X-ray diffraction device (MiniFlex II, manufactured by Rigaku). The radiation source is CuKα radiation, the tube voltage is 30 kV, the tube current is 15 mA, and the diffracted X-rays are passed through a 30 μm thick Kβ filter and detected by a high-speed one-dimensional detector (model number: D / teX Ultra 2). The sampling width is 0.01°, the scan speed is 5° / min, the divergence slit width is 0.625°, the receiving slit width is 13 mm (OPEN), and the scattering slit width is 8 mm.

[0029] As the sulfide solid electrolyte, the sulfide glass preferably has a composition represented by the general formula (100-z)(yLi2S·(1-y)P2S5)·zLiCl·αM (wherein 0.74≦y≦0.78, 5≦z≦55, and 0≦α≦30. M represents one or more elements other than Li, P, S, and Cl). When the sulfide solid electrolyte has a composition represented by the general formula, the ionic conductivity can be further increased.

[0030] The lower limit of z in the above general formula is preferably 10, more preferably 12, and even more preferably 15. The upper limit of z is preferably 50, more preferably 40, and even more preferably 30. When z in the above general formula is within the above range, the ionic conductivity at 25° C. can be further increased.

[0031] The lower limit of y in the above general formula is preferably 0.75. The upper limit of y is preferably 0.77. When the content ratios of Li2S and P2S5 in the sulfide solid electrolyte are within the above ranges, the sulfide solid electrolyte has high ionic conductivity.

[0032] In the above general formula, α is preferably 0. When α=0 in the above general formula, the ionic conductivity can be further improved.

[0033] The element M in the above general formula may be any of the elements belonging to the second to fifth periods of groups 13 to 17 of the periodic table. Among these, N, O, F, Br and I are preferred. When the element M in the above general formula is any of the elements in the above ranges of the periodic table, it is possible to improve performance such as water resistance, reduction resistance, and ion conductivity.

[0034] The lower limit of the ionic conductivity of the sulfide solid electrolyte at 25°C is 6.0 × 10 -4 S / cm is preferred, 8.0×10 -4 S / cm is more preferable, 9.0×10 -4 S / cm is more preferable, and 1.0×10 -3 When the sulfide solid electrolyte has an ionic conductivity at 25° C. of not less than the above value, the charge / discharge performance, such as the high-rate charge / discharge performance, of the energy storage device can be improved.

[0035] The ionic conductivity of the sulfide solid electrolyte is determined by measuring the AC impedance using the following method. In an argon atmosphere with a dew point of -50°C or less, 120 mg of sample powder is placed in a powder molder with an inner diameter of 10 mm, and then uniaxially pressurized at 50 MPa or less using a hydraulic press. After releasing the pressure, 120 mg of SUS316L powder is placed on the upper surface of the sample as a current collector, and then uniaxially pressurized again at 50 MPa or less using a hydraulic press. Next, 120 mg of SUS316L powder is placed on the lower surface of the sample as a current collector, and then uniaxially pressurized at 360 MPa for 5 minutes to obtain a pellet for measuring ionic conductivity. The pellet for measuring ionic conductivity is inserted into a HS cell manufactured by Hosen Co., Ltd., and AC impedance is measured at a specified temperature. The measurement conditions are an applied voltage amplitude of 20 mV, a frequency range of 1 MHz to 100 mHz, and a measurement temperature of 25°C.

[0036] The ratio of the lithium content to the chlorine content (Li / Cl) is preferably less than 16.0 and 1.5 or more in molar ratio. By setting the ratio of the lithium content to the chlorine content (Li / Cl) in the above range, a crystal phase with high ionic conductivity is easily precipitated, and ionic conductivity tends to be increased.

[0037] The ratio of the sulfur content to the chlorine content (S / Cl) is preferably less than 19.0 and 2.0 or more in molar ratio. By setting the ratio of the lithium content to the chlorine content (Li / Cl) in the above range, a crystal phase with high ionic conductivity is easily precipitated, and ionic conductivity tends to be increased.

[0038] The shape of the solid electrolyte is not particularly limited, and is usually granular, block, or the like.

[0039] The sulfide solid electrolyte has excellent ion conductivity. The sulfide solid electrolyte can be suitably used as an electrolyte for a storage element such as a lithium ion secondary battery, particularly for a lithium ion storage element. In particular, the sulfide solid electrolyte can be suitably used as an electrolyte for an all-solid-state battery. The solid electrolyte can be used for any of a positive electrode layer, a separator layer, a negative electrode layer, etc. in a storage element.

[0040] <Electricity storage element> As an embodiment of the energy storage element of the present invention, an all-solid-state battery will be specifically described below. The energy storage element 10 shown in FIG. 1 is an all-solid-state battery, and is a secondary battery in which a positive electrode layer 1 and a negative electrode layer 2 are arranged with an isolating layer 3 interposed therebetween. The positive electrode layer 1 has a positive electrode substrate 4 and a positive electrode active material layer 5, and the positive electrode substrate 4 is the outermost layer of the positive electrode layer 1. The negative electrode layer 2 has a negative electrode substrate 7 and a negative electrode active material layer 6, and the negative electrode substrate 7 is the outermost layer of the negative electrode layer 2. In the energy storage element 10 shown in FIG. 1, the negative electrode active material layer 6, the isolating layer 3, the positive electrode active material layer 5, and the positive electrode substrate 4 are laminated in this order on the negative electrode substrate 7.

[0041] The energy storage element 10 contains a sulfide solid electrolyte according to an embodiment of the present invention in at least one of the positive electrode layer 1, the negative electrode layer 2, and the separator layer 3. More specifically, the solid electrolyte according to an embodiment of the present invention is contained in at least one of the positive electrode active material layer 5, the negative electrode active material layer 6, and the separator layer 3. Since the energy storage element 10 contains the sulfide solid electrolyte having excellent ion conductivity, it has excellent ion conductivity and can improve charge / discharge performance such as high-rate charge / discharge performance.

[0042] The energy storage element 10 may be configured to use a solid electrolyte other than the solid electrolyte according to one embodiment of the present invention. Examples of the other solid electrolyte include sulfide solid electrolytes other than the sulfide solid electrolyte, oxide-based solid electrolytes, dry polymer electrolytes, gel polymer electrolytes, and pseudo-solid electrolytes, and the sulfide solid electrolyte is preferred. In addition, a single layer in the energy storage element 10 may contain multiple different types of solid electrolytes, or each layer may contain a different solid electrolyte.

[0043] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-P2S5-Li3N, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, and Li2S-P2S5-Z. m S 2n (where m and n are positive numbers, and Z is Ge, Zn, or Ga.), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (where x and y are positive numbers, and M is P, Si, Ge, B, Al, Ga, or In.) Li 10 GeP2S 12 etc. can be mentioned.

[0044] [Positive electrode layer] The positive electrode layer 1 includes a positive electrode substrate 4 and a positive electrode active material layer 5 laminated on the surface of the positive electrode substrate 4. The positive electrode layer 1 may have an intermediate layer between the positive electrode substrate 4 and the positive electrode active material layer 5. The intermediate layer may be, for example, a layer containing conductive particles and a resin binder.

[0045] (Positive electrode substrate) The positive electrode substrate 4 has electrical conductivity. The term "electrically conductive" means that the volume resistivity measured in accordance with JIS-H-0505 (1975) is 107 "Non-conductive" means that the volume resistivity is 10 7 It means that the resistance is more than Ω·cm. As the material of the positive electrode substrate 4, metals such as aluminum, titanium, tantalum, indium, stainless steel, etc., or alloys thereof are used. Among these, aluminum or aluminum alloys are preferred from the viewpoints of potential resistance, high conductivity, and cost. As the positive electrode substrate 4, foils, vapor deposition films, etc. are mentioned, and foils are preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate 4. Examples of aluminum or aluminum alloys include A1085P, A3003P, etc. specified in JIS-H-4000 (2014).

[0046] The average thickness of the positive electrode substrate 4 is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, further preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate 4 within the above range, it is possible to increase the strength of the positive electrode substrate 4 while increasing the energy density per volume of the energy storage element 10. The "average thickness" of the positive electrode substrate 4 and the negative electrode substrate 7 described later refers to the value obtained by dividing the mass of the substrate of a given area by the true density and area of ​​the substrate.

[0047] The intermediate layer is a layer disposed between the positive electrode substrate 4 and the positive electrode active material layer 5. The intermediate layer contains conductive particles such as carbon particles, thereby reducing the contact resistance between the positive electrode substrate 4 and the positive electrode active material layer 5. The configuration of the intermediate layer is not particularly limited, and includes, for example, a resin binder and conductive particles.

[0048] (Cathode active material layer) The positive electrode active material layer 5 includes a positive electrode active material. The positive electrode active material layer 5 can be formed from a so-called positive electrode mixture including a positive electrode active material. The positive electrode active material layer 5 may include a mixture or a composite including a positive electrode active material and a solid electrolyte. The positive electrode active material layer 5 may include optional components such as a conductive agent, a binder, a thickener, and a filler, as necessary. One or more of these optional components may not be substantially contained in the positive electrode active material layer 5.

[0049] The positive electrode active material contained in the positive electrode active material layer 5 can be appropriately selected from known positive electrode active materials that are commonly used in lithium ion secondary batteries and all-solid-state batteries. As the positive electrode active material, a material capable of absorbing and releasing lithium ions is usually used. Examples of the positive electrode active material include lithium transition metal composite oxides having an α-NaFeO2 crystal structure, lithium transition metal composite oxides having a spinel crystal structure, polyanion compounds, chalcogen compounds, and sulfur. Examples of lithium transition metal composite oxides having an α-NaFeO2 crystal structure include Li[Li x Ni 1-x ]O2(0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), etc. Lithium transition metal composite oxides with spinel crystal structure include Li x Mn2O4, Li x Ni γ Mn (2-γ) O4, etc. Examples of polyanion compounds include LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. Examples of chalcogen compounds include titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. Atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surface of the positive electrode active material may be coated with an oxide such as lithium niobate, lithium titanate, or lithium phosphate. In the positive electrode active material layer, one of these positive electrode active materials may be used alone, or two or more may be mixed and used.

[0050] The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material to the above lower limit or more, the positive electrode active material can be easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above upper limit or less, the electronic conductivity of the positive electrode active material layer 5 is improved. Here, the "average particle size" refers to a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).

[0051] In order to obtain particles of a predetermined shape, a pulverizer, a classifier, etc. are used. Examples of the pulverization method include a method using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, or a sieve. During pulverization, wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, etc. are used as necessary for both the dry and wet methods.

[0052] The content of the positive electrode active material in the positive electrode active material layer 5 is preferably 10 mass % or more and 95 mass % or less, more preferably 30 mass % or more, and further preferably 50 mass % or more. By setting the content of the positive electrode active material within the above range, the electric capacity of the energy storage element 10 can be increased.

[0053] When the positive electrode active material layer 5 contains a solid electrolyte, the content of the solid electrolyte is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more and 70% by mass or less, and even more preferably 50% by mass or less. By setting the content of the solid electrolyte within the above range, the electric capacity of the storage element can be increased. When the solid electrolyte according to one embodiment of the present invention is used for the positive electrode active material layer 5, the content of the solid electrolyte according to one embodiment of the present invention relative to the total solid electrolyte in the positive electrode active material layer 5 is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and even more preferably substantially 100% by mass.

[0054] The mixture of the positive electrode active material and the solid electrolyte is a mixture prepared by mixing the positive electrode active material and the solid electrolyte by mechanical milling or the like. For example, the mixture of the positive electrode active material and the solid electrolyte can be obtained by mixing a particulate positive electrode active material and a particulate solid electrolyte. The composite of the positive electrode active material and the solid electrolyte includes a composite having a chemical or physical bond between the positive electrode active material and the solid electrolyte, a composite in which the positive electrode active material and the solid electrolyte are physically combined, and the like. The composite includes a composite in which the positive electrode active material and the solid electrolyte are present in one particle, and examples of the composite include a composite in which the positive electrode active material and the solid electrolyte form an aggregated state, and a composite in which a solid electrolyte-containing coating is formed on at least a part of the surface of the positive electrode active material.

[0055] The conductive agent is not particularly limited as long as it is a material having electrical conductivity. Examples of such conductive agents include carbonaceous materials, metals, conductive ceramics, and the like. Examples of carbonaceous materials include graphitized carbon, non-graphitized carbon, graphene-based carbon, and the like. Examples of non-graphitized carbon include carbon nanofibers, pitch-based carbon fibers, carbon black, and the like. Examples of carbon black include furnace black, acetylene black, ketjen black, and the like. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, and the like. Examples of the shape of the conductive agent include powder and fiber. As the conductive agent, one of these materials may be used alone, or two or more of them may be mixed and used. In addition, these materials may be used in a composite form. For example, a material in which carbon black and CNT are composited may be used. Among these, carbon black is preferable from the viewpoint of electronic conductivity and coatability, and acetylene black is preferable among them.

[0056] The content of the conductive agent in the positive electrode active material layer 5 is preferably from 1 mass % to 10 mass %, and more preferably from 3 mass % to 9 mass %. By setting the content of the conductive agent in the above range, the electric capacity of the energy storage element 10 can be increased.

[0057] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.

[0058] The content of the binder in the positive electrode active material layer 5 is preferably from 1 mass % to 10 mass %, and more preferably from 3 mass % to 9 mass %. By setting the binder content within the above range, the active material can be stably held.

[0059] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. When the thickener has a functional group that reacts with lithium or the like, this functional group may be deactivated in advance by methylation or the like.

[0060] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, aluminum oxide, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, and artificial products thereof.

[0061] The positive electrode active material layer 5 may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.

[0062] The average thickness of the positive electrode active material layer 5 is preferably 30 μm or more and 1,000 μm or less, and more preferably 60 μm or more and 500 μm or less. By setting the average thickness of the positive electrode active material layer 5 to be equal to or more than the above lower limit, it is possible to obtain a storage element 10 having a high energy density. By setting the average thickness of the positive electrode active material layer 5 to be equal to or less than the above upper limit, it is possible to reduce the size of the storage element 10. The average thickness of the positive electrode active material layer 5 is the average value of thicknesses measured at any five positions. The same applies to the average thicknesses of the negative electrode active material layer 6 and the separator layer 3 described later.

[0063] [Negative electrode layer] The negative electrode layer 2 has a negative electrode substrate 7 and a negative electrode active material layer 6 disposed directly or via an intermediate layer on the negative electrode substrate 7. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode layer 1, for example.

[0064] (Negative electrode substrate) The negative electrode substrate 7 is conductive. Metals such as copper, nickel, stainless steel, nickel-plated steel, and aluminum, or alloys thereof are used as the material of the negative electrode substrate 7. Among these, copper or a copper alloy is preferable. Examples of the negative electrode substrate include foils and vapor-deposited films, and foils are preferable from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferable as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.

[0065] The average thickness of the negative electrode substrate 7 is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate 7 to be equal to or greater than the lower limit, the strength of the negative electrode substrate 7 can be increased. By setting the average thickness of the negative electrode substrate 7 to be equal to or less than the upper limit, the energy density per volume of the energy storage element 10 can be increased.

[0066] (Negative electrode active material layer) The negative electrode active material layer 6 includes a negative electrode active material. The negative electrode active material layer 6 can be formed from a so-called negative electrode mixture including a negative electrode active material. The negative electrode active material layer 6 may include a mixture or a composite including a negative electrode active material and a solid electrolyte. The negative electrode active material layer 6 includes optional components such as a conductive agent, a binder, a thickener, and a filler as necessary. The types and suitable contents of these optional components in the negative electrode active material layer 6 are the same as those of each optional component in the positive electrode active material layer 5 described above. One or more of these optional components may not be substantially contained in the negative electrode active material layer 6.

[0067] The negative electrode active material layer 6 may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.

[0068] The negative electrode active material can be appropriately selected from known negative electrode active materials that are commonly used in lithium ion secondary batteries and all-solid-state batteries. As the negative electrode active material, a material capable of absorbing and releasing lithium ions is usually used. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li4Ti5O 12 , LiTiO 2、Examples of the material include titanium-containing oxides such as TiNb2O7, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitized carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. In the negative electrode active material layer 6, one of these materials may be used alone, or two or more of them may be used in combination.

[0069] "Graphite" refers to graphite that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of availability of materials with stable physical properties.

[0070] "Non-graphitic carbon" refers to carbon that has an average lattice spacing (d 002 ) is 0.34 nm or more and 0.42 nm or less. Non-graphitic carbon includes non-graphitizable carbon and graphitizable carbon. Non-graphitic carbon includes, for example, resin-derived materials, petroleum pitch-derived materials, and alcohol-derived materials.

[0071] Here, the "discharged state" refers to a state in which the open circuit voltage is 0.7 V or more in a single-electrode battery using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and metallic Li as a counter electrode. Since the potential of the metallic Li counter electrode in the open circuit state is approximately equal to the redox potential of Li, the open circuit voltage in the single-electrode battery is approximately equal to the potential of the negative electrode containing the carbon material relative to the redox potential of Li. In other words, the open circuit voltage of 0.7 V or more in the single-electrode battery means that lithium ions capable of being absorbed and released during charging and discharging are sufficiently released from the carbon material, which is the negative electrode active material.

[0072] "Non-graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.36 nm or more and 0.42 nm or less.

[0073] "Graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.34 nm or more and less than 0.36 nm.

[0074] The negative electrode active material is usually a particle (powder). The average particle size of the negative electrode active material can be, for example, 1 nm or more and 100 μm or less. When the negative electrode active material is, for example, a carbon material, the average particle size may be preferably 1 μm or more and 100 μm or less. When the negative electrode active material is a metal, a semi-metal, a metal oxide, a semi-metal oxide, a titanium-containing oxide, a polyphosphate compound, or the like, the average particle size may be preferably 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to the above lower limit or more, the production or handling of the negative electrode active material becomes easy. By setting the average particle size of the negative electrode active material to the above upper limit or less, the electronic conductivity of the active material layer is improved. In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, or the like is used. The pulverization method and the powder classification method can be selected from, for example, the methods exemplified for the positive electrode layer 1.

[0075] The content of the negative electrode active material in the negative electrode active material layer 6 is preferably 10% by mass or more and 95% by mass or less, more preferably 30% by mass or more, and further preferably 50% by mass or more. By setting the content of the negative electrode active material within the above range, the electric capacity of the energy storage element 10 can be increased.

[0076] When the negative electrode active material layer 6 contains a solid electrolyte, the content of the solid electrolyte is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more and 70% by mass or less, and even more preferably 50% by mass or less. By setting the content of the solid electrolyte within the above range, the electric capacity of the storage element 10 can be increased. When the solid electrolyte according to one embodiment of the present invention is used in the negative electrode active material layer 6, the content of the solid electrolyte according to one embodiment of the present invention relative to the total solid electrolyte in the negative electrode active material layer 6 is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and even more preferably substantially 100% by mass.

[0077] The mixture or composite of the negative electrode active material and solid electrolyte may be the mixture or composite of the positive electrode active material and solid electrolyte described above, in which the positive electrode active material is replaced with a negative electrode active material.

[0078] The average thickness of the negative electrode active material layer 6 is preferably 30 μm or more and 1,000 μm or less, and more preferably 60 μm or more and 500 μm or less. By setting the average thickness of the negative electrode active material layer 6 to be equal to or more than the above lower limit, it is possible to obtain an energy storage element 10 having a high energy density. By setting the average thickness of the negative electrode active material layer 6 to be equal to or less than the above upper limit, it is possible to reduce the size of the energy storage element 10.

[0079] [Isolation layer] The isolating layer 3 contains a solid electrolyte. As the solid electrolyte contained in the isolating layer 3, in addition to the solid electrolyte according to one embodiment of the present invention described above, various solid electrolytes exemplified in the positive electrode active material layer 5 can be used, and among them, it is preferable to use a sulfide solid electrolyte. The content of the solid electrolyte in the isolating layer 3 is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 99% by mass or more, and even more preferably substantially 100% by mass. In addition, when the solid electrolyte according to one embodiment of the present invention is used in the isolating layer 3, the content of the solid electrolyte according to one embodiment of the present invention in the total solid electrolyte in the isolating layer 3 is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and even more preferably substantially 100% by mass.

[0080] The separator 3 may contain optional components such as a binder, a thickener, a filler, etc. The optional components such as a binder, a thickener, a filler, etc. can be selected from the materials exemplified for the positive electrode active material layer 5.

[0081] The average thickness of the isolating layer 3 is preferably 1 μm or more and 50 μm or less, and more preferably 3 μm or more and 20 μm or less. By setting the average thickness of the isolating layer 3 to be equal to or more than the above lower limit, it is possible to reliably insulate the positive electrode layer 1 from the negative electrode layer 2. By setting the average thickness of the isolating layer 3 to be equal to or less than the above upper limit, it is possible to increase the energy density of the energy storage element 10.

[0082] The energy storage element of the present embodiment can be mounted as an energy storage unit (battery module) formed by assembling a plurality of energy storage elements in a power source for an automobile such as an electric vehicle (EV), a hybrid vehicle (HEV), or a plug-in hybrid vehicle (PHEV), a power source for electronic devices such as a personal computer or a communication terminal, or a power storage power source, etc. In this case, it is sufficient that the technology according to one embodiment of the present invention is applied to at least one energy storage element included in the energy storage unit.

[0083] 2 shows an example of an energy storage device 30 in which energy storage units 20, each of which is an assembly of two or more electrically connected energy storage elements 10, are further assembled. The energy storage device 30 may include a bus bar (not shown) that electrically connects two or more energy storage elements 10, a bus bar (not shown) that electrically connects two or more energy storage units 20, and the like. The energy storage units 20 or the energy storage device 30 may include a status monitoring device (not shown) that monitors the status of one or more energy storage elements.

[0084] <Method of manufacturing sulfide solid electrolyte> A method for producing a sulfide solid electrolyte according to one embodiment of the present invention includes heat treating a sulfide glass containing lithium, sulfur, phosphorus, and chlorine, where the phosphorus has a valence of five (heat treatment step). The method for producing a sulfide solid electrolyte preferably includes, prior to the heat treatment, other steps, for example, preparing a composition containing lithium, phosphorus, sulfur, and chlorine (preparation step), and reacting the composition to produce sulfide glass containing lithium, sulfur, phosphorus, and chlorine, where the phosphorus has a valence of five (sulfide glass production step).

[0085] (preparation process) In this process, a composition containing lithium, phosphorus, sulfur, and chlorine is prepared. The composition is usually a mixture of two or more compounds containing at least one element selected from lithium, phosphorus, sulfur, and chlorine. The composition (mixture) may contain the elements lithium, phosphorus, sulfur, and chlorine. Two or more elements selected from lithium, phosphorus, sulfur, and chlorine may be contained in one compound. For example, Li2S, which will be described later, is an example of a compound containing lithium and sulfur, P2S5, which will be described later, is an example of a compound containing phosphorus and sulfur, and LiCl, which will be described later, is an example of a compound containing lithium and chlorine.

[0086] Examples of the compound containing lithium include Li2S and metallic lithium. In addition, LiCl, which will be described later, may be used. Among these, Li2S is preferable. The compound containing lithium may be used alone or in combination of two or more.

[0087] An example of the phosphorus-containing compound is P2S5, etc. The phosphorus-containing compound may be used alone or in combination of two or more.

[0088] Examples of compounds containing sulfur include Li2S and P2S. 5、 Elemental sulfur and the like are exemplified. Among these, Li2S and P2S5 are preferred. The sulfur-containing compounds and the like may be used alone or in combination of two or more.

[0089] An example of the chlorine-containing compound is LiCl. The chlorine-containing compound may be used alone or in combination of two or more.

[0090] For example, in one embodiment, the composition is preferably a mixture of Li2S, P2S5, and LiCl.

[0091] The specific and preferred contents of each element (lithium, phosphorus, sulfur, and chlorine) in the composition are the same as the specific and preferred contents of each element (lithium, phosphorus, sulfur, and chlorine) in the sulfide solid electrolyte according to one embodiment of the present invention described above.

[0092] (Sulfide glass manufacturing process) In this process, for example, sulfide glass containing lithium, sulfur, phosphorus, and chlorine, and the phosphorus has a valence of five, is prepared by the following procedure. In this process, a composition containing lithium, phosphorus, sulfur, and chlorine is reacted by treating the composition by, for example, mechanical milling to obtain sulfide glass. The sulfide glass has a composition represented by the general formula (100-z)(yLi2S·(1-y)P2S5)·zLiCl·αM (where 0.74≦y≦0.78, 5≦z≦55, 0≦α≦30. M represents one or more elements other than Li, P, S, and Cl), and thus a sulfide solid electrolyte having higher ion conductivity can be produced. Note that the preferred ranges of y, z, and α in the general formula are as described above. The means for obtaining the sulfide glass are not limited to this, and may be obtained by other methods. For example, instead of the mechanical milling method, a melt quenching method or the like may be performed. "Sulfide glass" refers to a sulfide solid electrolyte that includes an amorphous structure.

[0093] The treatment by mechanical milling may be either dry or wet, but wet is preferred since the raw material compounds can be mixed more uniformly. Examples of the apparatus for performing the treatment by mechanical milling include a container-driven mill, a media-agitating mill, a high-speed rotary grinder, a roller mill, and a jet mill. Examples of the container-driven mill include a rotary mill, a vibration mill, and a planetary ball mill. Examples of the media-agitating mill include an attritor and a bead mill. Examples of the high-speed rotary grinder include a hammer mill and a pin mill. Among these, a container-driven mill is preferred, and a planetary ball mill is particularly preferred.

[0094] (Heat treatment process) In this step, sulfide glass containing lithium, sulfur, phosphorus, and chlorine, and in which the valence of phosphorus is 5, is heat-treated. This causes the sulfide glass to crystallize, and sulfide glass ceramics can be produced. The heat treatment may be performed under a reduced pressure atmosphere or an inert gas atmosphere.

[0095] The temperature of the heat treatment is lower than the crystallization temperature of the sulfide glass. The lower limit of the difference between the crystallization temperature and the heat treatment temperature is 20°C, preferably 23°C, and more preferably 25°C. On the other hand, the upper limit of the difference between the crystallization temperature and the heat treatment temperature is 45°C, preferably 42°C, and more preferably 40°C. By setting the temperature of the heat treatment lower than the crystallization temperature of the sulfide glass and the difference between the crystallization temperature and the heat treatment temperature within the above range, the precipitation of the β-Li3PS4 crystal phase having low ion conductivity is suppressed, and a sulfide solid electrolyte having a crystal phase having high ion conductivity can be produced. In addition, in the Li2S-P2S5-LiCl-based solid electrolyte, a crystal phase having high ion conductivity can be precipitated in a relatively wide composition range, so that the variation in characteristics due to composition unevenness during mass production can be suppressed.

[0096] The crystallization temperature can be determined by differential scanning calorimetry (DSC).

[0097] <Method of manufacturing energy storage element> The method for producing an electric storage element according to an embodiment of the present invention can be performed by a generally known method, except that the solid electrolyte according to an embodiment of the present invention is used to prepare at least one of the positive electrode layer, the separator layer, and the negative electrode layer. Specifically, the method for producing an electric storage element according to an embodiment of the present invention includes, for example, (1) preparing a positive electrode mixture, (2) preparing a separator layer material, (3) preparing a negative electrode mixture, and (4) stacking the positive electrode layer, the separator layer, and the negative electrode layer. Each step will be described in detail below.

[0098] (1) Positive electrode mixture preparation process In this step, a positive electrode mixture for forming a positive electrode layer (positive electrode active material layer) is usually prepared. The method for preparing the positive electrode mixture is not particularly limited and can be appropriately selected according to the purpose. For example, a mechanical milling method for treating the material of the positive electrode mixture, compression molding of the positive electrode active material, sputtering using a target material of the positive electrode active material, etc. can be mentioned. When the positive electrode mixture contains a mixture or composite containing a positive electrode active material and a solid electrolyte, this step can include, for example, mixing the positive electrode active material and the solid electrolyte using a mechanical milling method or the like to prepare a mixture or composite of the positive electrode active material and the solid electrolyte.

[0099] (2) Preparation of materials for the isolation layer In this step, a material for forming an isolation layer is usually prepared. When the storage element is a lithium ion storage element, the isolation layer material is usually a solid electrolyte. The solid electrolyte as the isolation layer material can be prepared by a conventionally known method. For example, it can be obtained by processing a predetermined material by a mechanical milling method. The isolation layer material may be prepared by heating a predetermined material to a melting temperature or higher by a melt quenching method, melting and mixing the two at a predetermined ratio, and quenching. Other methods for synthesizing the isolation layer material include, for example, a solid phase method in which the material is sealed under reduced pressure and fired, a liquid phase method such as dissolution deposition, a gas phase method (PLD), and firing under an argon atmosphere after mechanical milling. In addition, when the isolation layer material is the sulfide solid electrolyte, the isolation layer material is prepared by a method for producing the sulfide solid electrolyte.

[0100] (3) Negative electrode mixture preparation process In this step, a negative electrode mixture for forming a negative electrode layer (negative electrode active material layer) is usually prepared. The specific method for preparing the negative electrode mixture is the same as that for the positive electrode mixture. When the negative electrode mixture contains a mixture or composite containing a negative electrode active material and a solid electrolyte, this step can include, for example, mixing the negative electrode active material and the solid electrolyte using a mechanical milling method or the like to prepare a mixture or composite of the negative electrode active material and the solid electrolyte.

[0101] (Lamination process) In this process, for example, a positive electrode layer having a positive electrode substrate and a positive electrode active material layer, an isolation layer, and a negative electrode layer having a negative electrode substrate and a negative electrode active material layer are laminated. In this process, the positive electrode layer, the isolation layer, and the negative electrode layer may be formed in this order, or may be formed in the reverse order, and the order of formation of each layer is not particularly limited. The positive electrode layer is formed, for example, by pressure molding the positive electrode substrate and the positive electrode mixture, the isolation layer is formed by pressure molding the isolation layer material, and the negative electrode layer is formed by pressure molding the negative electrode substrate and the negative electrode mixture. The positive electrode layer, the isolation layer, and the negative electrode layer may be laminated by pressure molding the positive electrode substrate, the positive electrode mixture, the isolation layer material, the negative electrode mixture, and the negative electrode substrate at once. The positive electrode layer and the negative electrode layer may be molded in advance, respectively, and then pressure molded and laminated with the isolation layer.

[0102] [Other embodiments] The present invention is not limited to the above-mentioned embodiment, and can be embodied in various modified and improved forms in addition to the above-mentioned forms. For example, the electric storage element according to the present invention may include layers other than the positive electrode layer, the separator layer, and the negative electrode layer. The electric storage element according to the present invention may contain a liquid in one or more of the layers. The electric storage element according to the present invention may be a capacitor, etc., in addition to the electric storage element being a secondary battery.

[0103] The configuration of the all-solid-state battery according to the present invention is not particularly limited, and may include layers other than the negative electrode layer, the positive electrode layer, and the separator layer, such as an intermediate layer or an adhesive layer.

[0104] <Example> The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0105] [Examples 1 to 7 and Comparative Examples 1 to 5] The sulfide solid electrolytes of Examples 1 to 7 and Comparative Examples 1 to 5 were synthesized by the following treatment. (preparation process) Li2S (purity 99.98%, manufactured by Aldrich), P2S5 (purity 99%, manufactured by Aldrich), and LiCl (purity 99.998%, manufactured by Aldrich) were mixed in a mortar in a glove box in an argon atmosphere with a dew point of −50° C. or less to prepare a composition containing Li, P, S, and Cl. (Sulfide glass manufacturing process) 1.0 g of the above composition was placed in a sealed 80 mL zirconia pot containing 900 zirconia balls with a diameter of 4 mm. The mixture was subjected to mechanical milling using a planetary ball mill (FRITSCH, model number Premium line P-7) at an orbital speed of 510 rpm for 10 to 25 hours to obtain a sulfide glass. (Heat treatment process) The sulfide glass was heated from room temperature to a temperature shown in Table 1 at a heating rate of 2° C. / min, and then heat-treated at the temperature shown in Table 1 for 2 hours to synthesize the sulfide solid electrolytes of Examples 1 to 7 and Comparative Examples 1 to 5.

[0106] [Comparative Example 6] In the preparation step, Li2S (purity 99.98%, manufactured by Aldrich) and P2S5 (purity 99%, manufactured by Aldrich) were mixed in a mortar in a glove box with an argon atmosphere having a dew point of −50° C. or less to prepare a composition containing Li, P and S. The same treatment as in Example 1 was carried out.

[0107] [Reference example 1] In the preparation step, Li2S (purity 99.98%, manufactured by Aldrich), P2S5 (purity 99%, manufactured by Aldrich), and LiBr (purity 99.999%, manufactured by Aldrich) were mixed in a mortar in a glove box with an argon atmosphere having a dew point of −50° C. or less to prepare a composition containing Li, P, S, and Br. The same treatment as in Example 1 was performed.

[0108] [Reference example 2] In the preparation step, Li2S (purity 99.98%, manufactured by Aldrich), P2S5 (purity 99%, manufactured by Aldrich), and LiI (purity 99.999%, manufactured by Aldrich) were mixed in a mortar in a glove box with an argon atmosphere having a dew point of −50° C. or less to prepare a composition containing Li, P, S, and I. The same treatment as in Example 1 was performed.

[0109] Crystallization temperature T C The value was determined by DSC measurement using the following method: A DSC apparatus (Rigaku Thermo Plus DSC8230) was used, and a steel sealed pan was heated from room temperature to 400° C. at a rate of 10° C. / min.

[0110] [evaluation] (1)XRD analysis X-ray diffraction measurements were carried out by the method described above.

[0111] 3 to 5 show X-ray diffraction patterns in the range of 2θ=10° to 40° for the examples and comparative examples. Table 1 shows the crystal structures identified from the X-ray diffraction patterns.

[0112] (2) Ionic conductivity (σ) The ionic conductivity (σ 25 ) was determined by measuring AC impedance by the above-mentioned method using "VMP-300" manufactured by Bio-Logic Co., Ltd. Table 1 shows the ionic conductivity at 25°C of the examples and comparative examples.

[0113] [Table 1]

[0114] As shown in FIG. 3 to FIG. 5, the sulfide solid electrolytes of Examples 1 to 7, Comparative Examples 2 to 6, Reference Examples 1 and 2 were confirmed to have a crystalline structure by observing peaks in the X-ray diffraction measurement. In the heat treatment step, by setting the difference between the crystallization temperature and the heat treatment temperature to 20° C. or more and 45° C. or less, the sulfide solid electrolytes of Examples 1 to 7 having a crystalline structure (crystalline phase A) having diffraction peaks at 2θ=17.8°±0.5°, 19.1°±0.5°, 21.7°±0.5°, 23.8°±0.5°, and 30.85°±0.5° in the X-ray diffraction measurement could be obtained. On the other hand, the sulfide solid electrolytes of Comparative Examples 1 to 5 obtained by setting the difference between the crystallization temperature and the heat treatment temperature to less than 20° C. or more than 45° C. had a crystalline phase of β-Li3PS4 having low ionic conductivity or had an amorphous phase. Furthermore, as shown in Table 1 and FIG. 5, Comparative Example 6, which did not contain chlorine and had a composition represented by 75Li2S·25P2S5, had a β-Li3PS4 crystal phase with low ionic conductivity.

[0115] As shown in Table 1, the sulfide solid electrolytes of Examples 1 to 7 had good ionic conductivity at 25°C. On the other hand, it can be seen that the sulfide solid electrolytes of Comparative Examples 1 to 6 had lower ionic conductivity than those of Examples 1 to 7. Note that the favorable range of ionic conductivity of a sulfide solid electrolyte usually varies depending on the composition constituting the sulfide solid electrolyte. For example, when z=15, the favorable range of ionic conductivity of a sulfide solid electrolyte containing a composition represented by the general formula (100-z)(yLi2S·(1-y)P2S5)·zLiCl is 7.0×10 -4 S / cm or more 3.0×10 -3 S / cm or less, and for z=30, it is 6.0×10 -4 S / cm or more 2.0×10 -3 S / cm or less, and for z=50, it is 4.0×10 -4 S / cm or more 1.0×10 -3 It is considered to be less than S / cm.

[0116] Furthermore, Reference Example 1 having a composition represented by 85(0.75Li2S 0.25P2S5) 15LiBr and Reference Example 2 having a composition represented by 85(0.75Li2S 0.25P2S5) 15LiI had a crystal structure including a crystal phase (referred to as crystal phase B in Table 1) different from crystal phase A of the sulfide solid electrolyte. That is, although the difference between the crystallization temperature and the heat treatment temperature was 20°C or more and 45°C or less, the above Comparative Example 6, Reference Examples 1 and 2 had a crystal phase different from crystal phase A of the sulfide solid electrolyte, and it is understood that crystal phase A is a crystal phase specific to the sulfide solid electrolyte containing chlorine.

[0117] The above results demonstrate that the sulfide solid electrolyte according to the present invention has excellent ion conductivity. [Industrial Applicability]

[0118] The solid electrolyte according to the present invention is suitably used as a solid electrolyte for an electricity storage element such as an all-solid-state battery. [Explanation of symbols]

[0119] 1 Positive electrode layer 2. Negative electrode layer 3 isolation layer 4. Positive electrode substrate 5 Cathode active material layer 6 Negative electrode active material layer 7. Negative electrode substrate 10 Energy storage element (solid-state battery) 20 Energy Storage Unit 30 Energy storage device

Claims

1. Contains lithium, sulfur, phosphorus and chlorine, It has a crystal structure having diffraction peaks at 2θ=17.8°±0.5°, 19.1°±0.5°, 21.7°±0.5°, 23.8°±0.5°, and 30.85°±0.5° in X-ray diffraction measurement using CuKα radiation, The phosphorus has a valence of five; β-Li 3 P.S. 4 The sulfide solid electrolyte is substantially free of a crystalline phase.

2. General formula (100-z) (yLi 2 S (1-y)P 2 S 5 2. The sulfide solid electrolyte according to claim 1, having a composition represented by the formula: y·zLiCl·αM (wherein 0.74≦y≦0.78, 5≦z≦55, and 0≦α≦30. M represents one or more elements other than Li, P, S, and Cl).

3. Ionic conductivity at 25°C is 6.0 x 10 -4 The sulfide solid electrolyte according to claim 1 or 2, having a specific surface area of ​​1.5 S / cm or more.

4. An electric storage element comprising the sulfide solid electrolyte according to claim 1, 2 or 3.

5. The present invention comprises heat treating a sulfide glass containing lithium, sulfur, phosphorus, and chlorine, the phosphorus having a valence of five, the temperature of the heat treatment is lower than the crystallization temperature of the sulfide glass; The method for producing a sulfide solid electrolyte, wherein the difference between the crystallization temperature and the heat treatment temperature is 20° C. or more and 45° C. or less.

6. The sulfide glass has the general formula (100-z) (yLi 2 S (1-y)P 2 S 5 6. The method for producing a sulfide solid electrolyte according to claim 5, having a composition represented by the formula: y·zLiCl·αM (wherein 0.74≦y≦0.78, 5≦z≦55, and 0≦α≦30; M represents one or more elements other than Li, P, S, and Cl).

Citation Information

Patent Citations

  • Lithium secondary battery

    JP2000340257A

  • Solid electrolyte

    JP2013201110A

  • Solid electrolyte material and method for producing the same

    JP2018174129A

  • Solid electrolyte material and method for producing the same

    JP2018174130A

  • All-solid secondary battery and solid electrolyte material

    JP2020087525A