Manufacturing method of cured coating film

A copolymer-based photosensitive resin composition with blocked isocyanato groups and acid groups addresses low-temperature curability and solvent resistance issues in color filters for flexible displays, ensuring stable and effective pattern formation.

JP7563509B2Active Publication Date: 2024-10-08RESONAC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023022986
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-08-03
Filing Date
2023-02-17
Publication Date
2024-10-08
Estimated Expiration
2038-07-06

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions used in color filters for flexible displays face challenges with low-temperature curability, storage stability, and solvent resistance, particularly when using plastic substrates like polyethylene terephthalate, which expand or contract during baking, and current solutions do not adequately meet these requirements.

Method used

A photosensitive resin composition comprising a copolymer with blocked isocyanato groups and acid groups, along with a hydroxyl group-containing organic solvent, reactive diluent, and photopolymerization initiator, allowing for low-temperature curing and improved solvent resistance, while maintaining storage stability.

Benefits of technology

The composition achieves good developability, storage stability, and forms a cured coating film with excellent solvent resistance even at low temperatures, suitable for flexible displays and color filters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563509000001
    Figure 0007563509000001
  • Figure 0007563509000002
    Figure 0007563509000002
  • Figure 0007563509000003
    Figure 0007563509000003
Patent Text Reader

Abstract

To provide a method for producing a photosensitive resin composition which has good developability and storage stability and gives a cured coating film which is excellent in solvent resistance even when cured at low temperature. [Solution] This is a method for producing a photosensitive resin composition, characterized by comprising the steps of synthesizing a copolymer (A) by copolymerizing a blocked isocyanato group-containing (meth)acrylate with an unsaturated carboxylic acid in the presence of a hydroxyl group-containing organic solvent (B), and then blending a reactive diluent (C) and a photopolymerization initiator (D).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition and a method for producing the same, a color filter and a method for producing the same, and an image display element. [Background technology]

[0002] In recent years, from the viewpoint of resource and energy saving, photosensitive resin compositions that can be cured by active energy rays such as ultraviolet rays and electron beams have been widely used in the fields of various coatings, printing, paints, adhesives, etc. Also, in the field of electronic materials such as printed wiring boards, photosensitive resin compositions that can be cured by active energy rays are used for solder resists, color filter resists, etc. Furthermore, the required properties of curable photosensitive resin compositions are becoming more and more diverse and sophisticated, and among them, short-time curing properties that take productivity into consideration and low-temperature curing properties that suppress thermal damage to members to which they are applied are required.

[0003] A color filter generally comprises a transparent substrate such as a glass substrate, red (R), green (G) and blue (B) pixels formed on the transparent substrate, a black matrix formed at the boundary between the pixels, and a protective film formed on the pixels and the black matrix. A color filter having such a configuration is usually manufactured by sequentially forming a black matrix, pixels and a protective film on a transparent substrate. Various methods have been proposed for forming pixels and black matrices (hereinafter, the pixels and black matrix are referred to as "colored patterns"). Among them, the pigment / dye dispersion method, which uses a photosensitive resin composition as a resist and is produced by a photolithography process in which coating, exposure, development and baking are repeated, is currently mainstream because it provides a colored pattern with excellent durability and few defects such as pinholes.

[0004] In general, photosensitive resin compositions used in photolithography contain an alkali-soluble resin, a reactive diluent, a photopolymerization initiator, a colorant, and a solvent. The pigment / dye dispersion method has the above advantages, but on the other hand, since black matrix and R, G, and B patterns are repeatedly formed, high heat resistance is required, and there are often problems such as restrictions on the types of colorants that can be used as colorants that can withstand high baking temperatures.

[0005] Patent Document 1 discloses a coloring composition that can be cured at low temperatures and has improved storage stability by using an alkali-soluble resin, a polymerizable compound having an ethylenically unsaturated bond, a radiation-sensitive polymerization initiator, a colorant, and a compound such as ethyl 3-aminobenzenesulfonate.

[0006] Patent Document 2 enables low-temperature curing by using a photosensitive resin composition containing a polymer precursor whose reaction to a final product is accelerated by a basic substance or by heating in the presence of a basic substance, and a specific base generator that generates a base by irradiation with electromagnetic waves and heating. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2013-68843 A [Patent Document 2] JP 2014-70148 A Summary of the Invention [Problem to be solved by the invention]

[0008] In recent years, flexible displays such as electronic paper have become widespread. Plastic substrates such as polyethylene terephthalate have been considered as substrates for these flexible displays. These substrates tend to expand or contract during baking, and it is necessary to lower the temperature of the baking process. However, the level achieved in Patent Document 1 is insufficient to meet the above requirements. In addition, while Patent Document 2 improves low-temperature curing properties, it has low storage stability and is difficult to put into practical use.

[0009] The present invention has been made in order to solve the above-mentioned problems, and an object of the present invention is to provide a photosensitive resin composition which has good developability and storage stability and gives a cured coating film which has excellent solvent resistance even when cured at a low temperature, and a method for producing the same. Another object of the present invention is to provide a color filter having a colored pattern with excellent solvent resistance, a method for producing the same, and an image display device equipped with the color filter. [Means for solving the problem]

[0010] That is, the present invention is represented by the following [1] to

[15] . [1] A photosensitive resin composition comprising: a copolymer (A) containing a structural unit (a) having a blocked isocyanato group and a structural unit (b) having an acid group; a hydroxyl group-containing organic solvent (B); a reactive diluent (C); and a photopolymerization initiator (D). [2] The photosensitive resin composition according to [1], wherein the structural unit (a) having a blocked isocyanato group is a structural unit derived from a blocked isocyanato group-containing (meth)acrylate, and a dissociation rate of the blocked isocyanato group of the blocked isocyanato group-containing (meth)acrylate is 5 to 99 mass % when heated at 100° C. for 30 minutes. [3] The photosensitive resin composition according to [1] or [2], wherein the blocking agent of the structural unit (a) having a blocked isocyanato group is one or more selected from the group consisting of diethyl malonate, 3,5-dimethylpyrazole, and methyl ethyl ketoxime. [4] The hydroxyl group-containing organic solvent (B) is selected from the group consisting of ethylene glycol monoalkyl ether, diethylene glycol monoalkyl ether, propylene glycol monoalkyl ether, propylene glycol monoaryl ether, dipropylene glycol monoalkyl ether, tripropylene glycol monoalkyl ether, 3-methoxy-1-butanol, 1,3-propanediol monoalkyl ether, 1,3-butanediol monoalkyl ether, 1,4-butanediol monoalkyl ether, glycerin monoalkyl ether, glycerin dialkyl ether, methanol, ethanol, propanol, C 5-6 Cycloalkanediols, C 5-6 The photosensitive resin composition according to any one of [1] to [3], wherein the compound is at least one selected from the group consisting of cycloalkane dimethanol, ethyl lactate, and diacetone alcohol. [5] The photosensitive resin composition according to any one of [1] to [4], wherein the structural unit (b) having an acid group is a structural unit derived from an unsaturated carboxylic acid. [6] The photosensitive resin composition according to any one of [1] to [5], wherein the copolymer (A) contains 1 to 40 mol % of the structural unit (a) having the blocked isocyanato group and 1 to 60 mol % of the structural unit (b) having an acid group. [7] The photosensitive resin composition according to any one of [1] to [6], wherein the molar ratio of the structural unit (a) having the blocked isocyanato group to the structural unit (b) having the acid group in the copolymer (A) is 10:90 to 50:50. [8] The copolymer (A) is selected from the group consisting of 2-(3,5-dimethylpyrazol-1-yl)carbonylaminoethyl methacrylate, 2-[O-(1'-methylpropylideneamino)carboxyamino]ethyl methacrylate, 2-[[[2-methyl-1-oxo-2-propenyl]oxy]ethyl]amino]carbonyl]-1,3 diethyl ester of malonate, 4-[[[[2-[(2-methyl-1-oxo-2-propen-1-yl)oxy]ethyl]amine]carbonyl]oxy]methyl ester of benzoate, 2-[[[[2-[(2-methyl-1-oxy-2-propen-1-yl) The photosensitive resin composition according to any one of [1] to [7], comprising at least one structural unit (a) derived from selected from the group consisting of 2-propenoic acid-2-methyl-2-[[(3,5-dimethylphenoxy)carbonyl]amine]ethyl ester, (b) a structural unit derived from (meth)acrylic acid, and (c) a structural unit derived from at least one selected from the group consisting of glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and methyl (meth)acrylate. [9] The photosensitive resin composition according to any one of [1] to [8], further comprising a colorant (E) for use in a color filter.

[10] The photosensitive resin composition according to [9], comprising 10 to 100 parts by mass of the copolymer (A), 30 to 1,000 parts by mass of the hydroxyl group-containing organic solvent (B), more than 0 to 90 parts by mass of the reactive diluent (C), 0.1 to 30 parts by mass of the photopolymerization initiator (D), and 5 to 80 parts by mass of the colorant (E), relative to 100 parts by mass of the total amount of the copolymer (A) and the reactive diluent (C).

[11] The photosensitive resin composition according to [9] or

[10] , wherein the colorant (E) contains a pigment.

[0011]

[12] A color filter having a colored pattern made of a cured product of the photosensitive resin composition according to any one of [9] to

[11] .

[0012]

[13] An image display device comprising the color filter according to

[12] .

[0013]

[14] A method for producing a color filter, comprising the steps of applying the photosensitive resin composition according to any one of [9] to

[11] to a substrate, exposing the composition to light, developing the composition with an alkali, and baking the composition at a temperature of 160°C or lower to form a colored pattern.

[0014]

[15] A method for producing a photosensitive resin composition, comprising the steps of: synthesizing a copolymer (A) by copolymerizing a blocked isocyanato group-containing (meth)acrylate with an unsaturated carboxylic acid in the presence of a hydroxyl group-containing organic solvent (B); and then blending a reactive diluent (C) and a photopolymerization initiator (D). Effect of the Invention

[0015] According to the present invention, it is possible to provide a photosensitive resin composition which has good developability and storage stability and which forms a cured coating film which has excellent solvent resistance even when cured at a low temperature, and a method for producing the same. Furthermore, according to the present invention, it is possible to provide a color filter having a colored pattern with excellent solvent resistance, a method for producing the same, and an image display device equipped with the color filter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] <Photosensitive resin composition> The photosensitive resin composition of the present invention is characterized by containing a copolymer (A) containing a structural unit (a) having a blocked isocyanato group and a structural unit (b) having an acid group, a hydroxyl group-containing organic solvent (B), a reactive diluent (C), and a photopolymerization initiator (D).

[0017] <Copolymer (A)> <Structural Unit (a) Having a Blocked Isocyanato Group> The structural unit (a) having a blocked isocyanato group contained in the copolymer (A) is a structural unit derived from a monomer containing a blocked isocyanato group. Examples of the monomer include a monomer having an ethylenically unsaturated bond and a blocked isocyanato group, such as a compound in which an isocyanato group in an isocyanate compound having a vinyl group, a (meth)acryloyloxy group, or the like in the molecule is blocked with a blocking agent. The reaction between the isocyanate compound and the blocking agent can be carried out regardless of the presence or absence of a solvent. When a solvent is used, it is necessary to use a solvent that is inactive against the isocyanato group. In the blocking reaction, an organic metal salt such as tin, zinc, or lead, or a tertiary amine may be used as a catalyst. The reaction can generally be carried out at -20 to 150°C, but is preferably carried out at 0 to 100°C. Examples of the isocyanate compound include a compound represented by the following formula (1).

[0018] [ka]

[0019] In the above formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 -CO-, -COOR 3 - (where R 3 is an alkylene group having 1 to 6 carbon atoms) or -COO-R 4 O-CONH-R 5 - (where R 4 is an alkylene group having 2 to 6 carbon atoms, R 5 R represents an alkylene group having 2 to 12 carbon atoms or an arylene group having 6 to 12 carbon atoms, which may have a substituent. 2 is preferably -COOR 3 - where R 3 is preferably an alkylene group having 1 to 4 carbon atoms.

[0020] Specific examples of the isocyanate compound represented by the above formula (1) include 2-isocyanatoethyl (meth)acrylate, 2-isocyanatopropyl (meth)acrylate, 3-isocyanatopropyl (meth)acrylate, 2-isocyanato-1-methylethyl (meth)acrylate, 2-isocyanato-1,1-dimethylethyl (meth)acrylate, 4-isocyanatocyclohexyl (meth)acrylate, and methacryloyl isocyanate. In addition, an equimolar (1 mol:1 mol) reaction product of a 2-hydroxyalkyl (meth)acrylate and a diisocyanate compound can also be used. The alkyl group of the 2-hydroxyalkyl (meth)acrylate is preferably an ethyl group or an n-propyl group, more preferably an ethyl group. Examples of the diisocyanate compound include hexamethylene diisocyanate, 2,4-(or 2,6-)tolylene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), 3,5,5-trimethyl-3-isocyanatomethylcyclohexyl isocyanate (IPDI), m-(or p-)xylene diisocyanate, 1,3-(or 1,4-)bis(isocyanatomethyl)cyclohexane, and lysine diisocyanate.

[0021] Among these isocyanate compounds, 2-isocyanatoethyl (meth)acrylate, 2-isocyanatopropyl (meth)acrylate, 3-isocyanatopropyl (meth)acrylate, 2-isocyanato-1-methylethyl (meth)acrylate, 2-isocyanato-1,1-dimethylethyl (meth)acrylate, 4-isocyanatocyclohexyl (meth)acrylate and methacryloyl isocyanate are preferred, and 2-isocyanatoethyl (meth)acrylate and 2-isocyanatopropyl (meth)acrylate are more preferred.

[0022] In this specification, the term "(meth)acrylate" means either acrylate or methacrylate, and the term "(meth)acrylic acid" means either acrylic acid or methacrylic acid.

[0023] Examples of blocking agents for blocking the isocyanato group in the isocyanate compound include lactam-based agents such as ε-caprolactam, δ-valerolactam, γ-butyrolactam, and β-propiolactam; alcohol-based agents such as methanol, ethanol, propanol, butanol, ethylene glycol, methyl cellosolve, butyl cellosolve, methyl carbitol, benzyl alcohol, phenyl cellosolve, furfuryl alcohol, and cyclohexanol; phenol-based agents such as phenol, cresol, 2,6-xylenol, 3,5-xylenol, ethylphenol, o-isopropylphenol, and butylphenols such as p-tert-butylphenol, p-tert-octylphenol, nonylphenol, dinonylphenol, styrenated phenol, methyl 2-hydroxybenzoate, methyl 4-hydroxybenzoate, thymol, p-naphthol, p-nitrophenol, and p-chlorophenol; active methylenes such as butyl mercaptan, ethyl acetoacetate, and acetylacetone; mercaptans such as butyl mercaptan, thiophenol, and tert-dodecyl mercaptan; amines such as diphenylamine, phenylnaphthylamine, aniline, and carbazole; acid amides such as acetanilide, acetaniside, acetate, and benzamide; acid imides such as succinimide and maleimide; imidazoles such as imidazole, 2-methylimidazole, and 2-ethylimidazole; pyrazo Examples of blocking agents include pyrazole-based agents such as 3,5-dimethylpyrazole, urea-based agents such as urea, thiourea, ethyleneurea, carbamate-based agents such as N-phenylcarbamate phenyl, 2-oxazolidone, imine-based agents such as ethyleneimine, polyethyleneimine, oxime-based agents such as formaldoxime, acetaldoxime, acetoxime, methylethylketoxime, methylisobutylketoxime, cyclohexanoneoxime, bisulfite-based agents such as sodium bisulfite, potassium bisulfite, etc. These blocking agents may be used alone or in combination of two or more.

[0024] The blocking agent protects the highly reactive isocyanato groups, but the blocked isocyanato groups are dissociated by heating to regenerate the isocyanato groups. In the present invention, the isocyanato groups react with reactive functional groups contained in the copolymer (A) and the reactive diluent (C), i.e., acid groups and optionally contained hydroxyl groups and amino groups, to form a cured product with high crosslink density.

[0025] From the viewpoint of low-temperature curing property and storage stability of the photosensitive resin composition described later, it is preferable to use a blocked isocyanato group-containing (meth)acrylate as a monomer that gives a structural unit (a) having a blocked isocyanato group. It is preferable to use a blocked isocyanato group-containing (meth)acrylate that has a dissociation rate of the blocked isocyanato group of preferably 5 to 99 mass%, more preferably 8 to 97 mass%, and most preferably 10 to 95 mass% when heated at 100°C for 30 minutes. The dissociation rate of the blocked isocyanato group of the blocked isocyanato group-containing (meth)acrylate is a value measured by HPLC analysis of the mass reduction rate of the blocked isocyanato group-containing (meth)acrylate after preparing an n-octanol solution containing the blocked isocyanato group-containing (meth)acrylate at a concentration of 20 mass%, adding 1 mass% of dibutyltin laurate and 3 mass% of phenothiazine (polymerization inhibitor) to the solution, and then heating at 100°C for 30 minutes. By using a blocked isocyanato group-containing (meth)acrylate with a dissociation rate in the above range, the stability of the copolymer during synthesis can be sufficiently ensured, the baking temperature during the preparation of the cured coating film can be sufficiently reduced, and the solvent resistance of the cured coating film can be sufficiently ensured. Examples of blocking agents for blocked isocyanato group-containing (meth)acrylates having such a dissociation rate include γ-butyrolactam, 1-methoxy-2-propanol, 2,6-dimethylphenol, diisopropylamine, methylethylketoxime, 3,5-dimethylpyrazole, and diethyl malonate. Among these blocking agents, diethyl malonate, 3,5-dimethylpyrazole, and methylethylketoxime are more preferred from the viewpoint of low-temperature curing properties.

[0026] It is also preferable to use a blocked isocyanato group-containing (meth)acrylate in which the dissociation temperature of the blocked isocyanato group is 80° C. or higher. When a blocked isocyanato group-containing (meth)acrylate with a dissociation temperature of 80° C. or higher is used, the stability of the copolymer during synthesis can be sufficiently ensured, and unintended crosslinking reactions can be reduced during the modification reaction described below. On the other hand, when the dissociation temperature of the blocked isocyanato group is 160° C. or lower, the baking temperature can be sufficiently reduced, and the solvent resistance of the cured coating film can be sufficiently ensured. The dissociation temperature of the blocked isocyanato group of the blocked isocyanato group-containing (meth)acrylate is determined by preparing an n-octanol solution having a concentration of 20% by mass of the blocked isocyanato group-containing (meth)acrylate, adding 1% by mass of dibutyltin laurate and 3% by mass of phenothiazine (polymerization inhibitor) to the solution, heating the solution at a predetermined temperature, and measuring the mass loss rate of the blocked isocyanato group-containing (meth)acrylate after 30 minutes by HPLC analysis. The dissociation temperature of the blocked isocyanato group is determined as the temperature at which the mass loss rate becomes 80% by mass or more.

[0027] Examples of the blocked isocyanato group-containing (meth)acrylate include methacrylates such as Karenz (registered trademark) MOI-DEM (a reaction product of methacryloyloxyethyl isocyanate and diethyl malonate, manufactured by Showa Denko K.K., dissociation temperature of blocked isocyanato group: 90° C., dissociation rate: 90% by mass) represented by the following formula (2), Karenz MOI-BP (a reaction product of methacryloyloxyethyl isocyanate and 3,5-dimethylpyrazole, manufactured by Showa Denko K.K., dissociation temperature of blocked isocyanato group: 110° C., dissociation rate: 70% by mass) represented by the following formula (3), and Karenz MOI-BM (a reaction product of methacryloyloxyethyl isocyanate and methyl ethyl ketoxime, manufactured by Showa Denko K.K., dissociation temperature of blocked isocyanato group: 130° C., dissociation rate: 18% by mass) represented by the following formula (4), and corresponding acrylates. These blocked isocyanato group-containing (meth)acrylates may be used alone or in combination of two or more kinds.

[0028] [ka]

[0029] [ka]

[0030] [ka]

[0031] The proportion of the structural unit (a) having a blocked isocyanato group contained in the copolymer (A) is not particularly limited, but is preferably 1 to 40 mol%, more preferably 2 to 30 mol%, and most preferably 3 to 25 mol%. When the proportion of the structural unit (a) having a blocked isocyanato group is 1 to 40 mol%, the solvent resistance of the cured coating film is improved and the storage stability of the copolymer (A) is maintained.

[0032] <Structural unit (b) having an acid group> The structural unit (b) having an acid group contained in the copolymer (A) is a structural unit derived from an acid group-containing monomer (excluding the structural unit (a) having the blocked isocyanato group). Examples of the acid group include a carboxyl group, a sulfo group, and a phospho group, and among these, a carboxyl group is preferred in terms of availability. Examples of the monomer that gives the structural unit (b) having an acid group include a monomer having a polymerizable unsaturated bond and an acid group, such as an unsaturated carboxylic acid or an anhydride thereof, an unsaturated sulfonic acid, or an unsaturated phosphonic acid. Specific examples of preferred monomers include unsaturated carboxylic acids or anhydrides thereof such as (meth)acrylic acid, α-bromo(meth)acrylic acid, β-furyl(meth)acrylic acid, crotonic acid, propiolic acid, cinnamic acid, α-cyanocinnamic acid, maleic acid, maleic anhydride, monomethyl maleate, monoethyl maleate, monoisopropyl maleate, fumaric acid, itaconic acid, itaconic anhydride, citraconic acid, and citraconic anhydride; unsaturated sulfonic acids such as 2-acrylamido-2-methylpropanesulfonic acid, tert-butylacrylamidosulfonic acid, and p-styrenesulfonic acid; unsaturated phosphonic acids such as vinylphosphonic acid; and the like. These monomers may be used alone or in combination of two or more. Among these, from the viewpoints of excellent alkali developability and easy availability, unsaturated carboxylic acids are preferred, and (meth)acrylic acid is more preferred.

[0033] In the present invention, by containing the structural unit (b) having an acid group in the copolymer (A), the alkali developability is significantly improved when the copolymer (A) is used as a photosensitive material.

[0034] The proportion of the structural unit (b) having an acid group contained in the copolymer (A) is not particularly limited, but is preferably 1 to 60 mol%, more preferably 10 to 50 mol%, and most preferably 15 to 40 mol%. When the proportion of the structural unit (b) having an acid group is 1 to 60 mol%, an appropriate alkaline development speed is obtained, and a precise pattern can be formed.

[0035] In the copolymer (A), the molar ratio of the structural unit (a) having a blocked isocyanato group to the structural unit (b) having an acid group can be, for example, 1:99 to 99:1, and from the viewpoints of the solvent resistance of the cured coating film and the storage stability of the copolymer (A), it is more preferably 5:95 to 75:25, and most preferably 10:90 to 50:50.

[0036] <Other structural units (c)> In the present invention, the copolymer (A) may contain, as structural units, other structural units (c) copolymerizable with the structural units (a) having a blocked isocyanato group and the structural units (b) having an acid group (excluding those corresponding to the structural units (a) having a blocked isocyanato group and the structural units (b) having an acid group). Specific examples of the other structural units (c) include a structural unit (c-1) having an epoxy group, a structural unit (c-2) having a hydroxyl group, and a structural unit (c-3) other than (c-1) and (c-2). The proportion of the other structural units (c) contained in the copolymer (A) is not particularly limited, but is preferably 0 to 80 mol%, more preferably 0 to 70 mol%, and most preferably 0 to 60 mol%.

[0037] Examples of monomers used to introduce the structural unit (c-1) having an epoxy group include monomers having a polymerizable unsaturated bond and an epoxy group, such as (meth)acrylic acid ester derivatives containing an epoxy group, such as oxiranyl (meth)acrylate, glycidyl (meth)acrylate, 2-methylglycidyl (meth)acrylate, 2-ethylglycidyl (meth)acrylate, 2-oxiranylethyl (meth)acrylate, 2-glycidyloxyethyl (meth)acrylate, 3-glycidyloxypropyl (meth)acrylate, and glycidyloxyphenyl (meth)acrylate; Examples of the (meth)acrylic acid ester derivatives include those containing an epoxy group-containing alicyclic carbon ring such as a 3,4-epoxycyclohexane ring, such as 4-epoxycyclohexyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 2-(3,4-epoxycyclohexyl)ethyl (meth)acrylate, 2-(3,4-epoxycyclohexylmethyloxy)ethyl (meth)acrylate, and 3-(3,4-epoxycyclohexylmethyloxy)propyl (meth)acrylate; vinyl ether compounds containing an epoxy group; and allyl ether compounds containing an epoxy group. These monomers may be used alone or in combination of two or more. Among these, epoxy group-containing (meth)acrylates such as oxiranyl (meth)acrylate, glycidyl (meth)acrylate, 2-methylglycidyl (meth)acrylate, 2-ethylglycidyl (meth)acrylate, 2-oxiranylethyl (meth)acrylate, 2-glycidyloxyethyl (meth)acrylate, 3-glycidyloxypropyl (meth)acrylate, and glycidyloxyphenyl (meth)acrylate are preferred, with glycidyl (meth)acrylate being more preferred.

[0038] By including the structural unit (c-1) having an epoxy group in the copolymer (A), the solvent resistance of the copolymer (A) is significantly improved when the copolymer (A) is used as a photosensitive material.

[0039] When the structural unit (c-1) having an epoxy group is introduced into the copolymer (A), the proportion of the structural unit (c-1) having an epoxy group is not particularly limited, but is preferably from more than 0 mol% to 60 mol%, more preferably from more than 0 mol% to 50 mol%, and most preferably from more than 0 mol% to 40 mol%.

[0040] Examples of monomers used to introduce the structural unit (c-2) having a hydroxyl group include monomers having a polymerizable unsaturated bond and a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 4-hydroxybutyl acrylate, 2-acryloyloxyethyl-succinic acid, 2-acryloyloxyethylhexahydrophthalic acid, 2-acryloyloxyethyl phthalic acid, 2-acryloyloxyethyl-2-hydroxyethyl-phthalic acid, etc. These monomers may be used alone or in combination of two or more. Among these, (meth)acrylic acid ester derivatives containing a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl acrylate, and 4-hydroxybutyl acrylate, are preferred, with 2-hydroxyethyl (meth)acrylate being more preferred.

[0041] By including the structural unit (c-2) having a hydroxyl group in the copolymer (A), the solvent resistance of the copolymer (A) is significantly improved when it is used as a photosensitive material.

[0042] When the structural unit (c-2) having a hydroxyl group is introduced into the copolymer (A), the proportion of the structural unit (c-2) having a hydroxyl group is not particularly limited, but is preferably from more than 0 mol% to 50 mol%, more preferably from more than 0 mol% to 40 mol%, and most preferably from more than 0 mol% to 30 mol%.

[0043] Specific examples of monomers used to introduce the structural unit (c-3) other than the structural unit (c-1) having an epoxy group and the structural unit (c-2) having a hydroxyl group described above include aromatic vinyl compounds such as styrene, α-methylstyrene, o-vinyltoluene, m-vinyltoluene, p-vinyltoluene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, p-nitrostyrene, p-cyanostyrene, and p-acetylaminostyrene; norbornene (bicyclo[2.2.1]hept-2-ene), 5-methylbicyclo[2.2.1]hept-2-ene, 5-ethylbicyclo[2.2.1]hept-2-ene, tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-methyltetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethyltetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, dicyclopentadiene, tricyclo[5.2.1.0 2,6 ]dec-8-ene, tricyclo[5.2.1.0 2,6 ]dec-3-ene, tricyclo[4.4.0.1 2,5 ]undec-3-ene, tricyclo[6.2.1.0 1,8 ]undec-9-ene, tricyclo[6.2.1.0 1,8 ]undec-4-ene, tetracyclo[4.4.0.1 2,5 .1 7,10 .0 1,6 ]dodec-3-ene, 8-methyltetracyclo[4.4.0.1 2,5 .1 7,10 .0 1,6 ]dodec-3-ene, 8-ethylidenetetracyclo[4.4.0.1 2,5 .1 7,12 ]dodec-3-ene, 8-ethylidenetetracyclo[4.4.0.1 2,5 .1 7,10 .0 1,6 ]dodec-3-ene, pentacyclo[6.5.1.1 3,6 .0 2,7 .0 9,13]Pentadec-4-ene, Pentacyclo[7.4.0.1 2,5 .1 9,12 .0 8,13] Cyclic olefins having a norbornene structure such as pentadec-3-ene; dienes such as butadiene, isoprene, and chloroprene; methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, neopentyl (meth)acrylate, and benzyl (meth)acrylate, Isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, ethylcyclohexyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, rosin (meth)acrylate, norbornyl (meth)acrylate, 5-methylnorbornyl (meth)acrylate, 5-Ethylnorbornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl acrylate isobornyl (meth)acrylate, adamantyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 1,1,1-trifluoroethyl (meth)acrylate, perfluoroethyl (meth)acrylate, perfluoro-n-propyl (meth)acrylate, perfluoro-isopropyl (meth)acrylate, 3-(N,N-di (Meth)acrylic acid esters such as methylamino)propyl (meth)acrylate, triphenylmethyl (meth)acrylate, phenyl (meth)acrylate, cumyl (meth)acrylate, 4-phenoxyphenyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, nonylphenoxypolyethylene glycol mono(meth)acrylate, biphenyloxyethyl (meth)acrylate, naphthalene (meth)acrylate, and anthracene (meth)acrylate;(meth)acrylic acid amides such as (meth)acrylic acid amide, (meth)acrylic acid N,N-dimethylamide, (meth)acrylic acid N,N-diethylamide, (meth)acrylic acid N,N-dipropylamide, (meth)acrylic acid N,N-di-isopropylamide, and (meth)acrylic acid anthracenylamide; vinyl compounds such as (meth)acrylic acid anilide, (meth)acrylonitrile, acrolein, vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, N-vinylpyrrolidone, vinylpyridine, vinyl acetate, and vinyl toluene; unsaturated dicarboxylic acid diesters such as diethyl citraconic acid, diethyl maleic acid, diethyl fumaric acid, and diethyl itaconate; monomaleimides such as N-phenylmaleimide, N-cyclohexylmaleimide, N-laurylmaleimide, and N-(4-hydroxyphenyl)maleimide; and the like. Among these, (meth)acrylic acid esters are preferred, and methyl (meth)acrylate and dicyclopentanyl (meth)acrylate are particularly preferred. These monomers may be used alone or in combination of two or more kinds.

[0044] <Method for producing copolymer (A)> The proportions of the blocked isocyanato group-containing monomer (a0) and the acid group-containing monomer (b0) used in producing the copolymer (A) are not particularly limited, but are preferably 1 to 40 mol % of (a0) and 1 to 60 mol % of (b0), more preferably 2 to 30 mol % of (a0) and 10 to 50 mol % of (b0), and most preferably 3 to 25 mol % of (a0) and 15 to 40 mol % of (b0). When the copolymer (A) further contains other structural units (c), the proportions of the blocked isocyanato group-containing monomer (a0), the acid group-containing monomer (b0) and the other monomer (c0) used in the production of the copolymer (A) are preferably (a0) 1 to 40 mol%, (b0) 1 to 60 mol%, and (c0) more than 0 mol% to 80 mol%, more preferably (a0) 2 to 30 mol%, (b0) 10 to 50 mol%, and (c0) more than 0 mol% to 70 mol%, and most preferably (a0) 3 to 25 mol%, (b0) 15 to 40 mol%, and (c0) more than 0 mol% to 60 mol%.

[0045] The copolymerization reaction of the blocked isocyanato group-containing monomer (a0), the acid group-containing monomer (b0) and the other monomer (c0) can be carried out in the presence or absence of a polymerization solvent according to a radical polymerization method known in the art, but it is preferable to carry out the copolymerization reaction in the presence of a hydroxyl group-containing organic solvent (B) described later from the viewpoint of preventing abnormal polymerization and stably carrying out the polymerization reaction. By carrying out the copolymerization reaction in the presence of the hydroxyl group-containing organic solvent (B), even if the blocked isocyanato group is dissociated to generate an isocyanato group, the isocyanato group reacts with the hydroxyl group of the hydroxyl group-containing organic solvent (B), preventing abnormal polymerization. In the copolymer (A) thus obtained, it is considered that a part of the blocking agent that blocked the isocyanato group is replaced by the hydroxyl group-containing organic solvent (B). For example, after dissolving these monomers in the hydroxyl group-containing organic solvent (B), a polymerization initiator may be added to the solution, and the polymerization reaction may be carried out at 50 to 100°C for 1 to 20 hours. In this case, if the polymerization reaction is carried out at a temperature at which the blocked isocyanato group of the blocked isocyanato group-containing monomer (a0) dissociates, the isocyanato group generated upon dissociation of the blocked isocyanato group will react with an acid group to produce a gel. Therefore, it is preferable to carry out the polymerization at a temperature lower than the dissociation temperature of the blocked isocyanato group, preferably at a temperature about 20 to 50° C. lower than the dissociation temperature of the blocked isocyanato group.

[0046] In addition, the polymerization initiator that can be used in this copolymerization reaction is not particularly limited, but examples thereof include azobisisobutyronitrile, azobisisovaleronitrile, benzoyl peroxide, and t-butylperoxy-2-ethylhexanoate. These polymerization initiators may be used alone or in combination of two or more. The amount of the polymerization initiator used is generally 0.5 to 20 parts by mass, preferably 1.0 to 10 parts by mass, when the total amount of the monomers charged is 100 parts by mass.

[0047] The weight average molecular weight of the copolymer (A) in terms of polystyrene is not particularly limited, but the above-mentioned production method can provide a copolymer (A) having a weight average molecular weight of preferably 1,000 to 50,000, more preferably 3,000 to 40,000. When the weight average molecular weight of the copolymer (A) is 1,000 or more, chipping of the colored pattern after alkali development when used as a photosensitive resin composition is unlikely to occur. On the other hand, when the weight average molecular weight of the copolymer (A) is 50,000 or less, the development time becomes appropriate, and practicality is ensured.

[0048] The acid value (JIS K6901 5.3) of the copolymer (A) can be appropriately selected, but when it is incorporated into a photosensitive resin composition, it is preferably in the range of 20 to 300 KOHmg / g, more preferably 30 to 200 KOHmg / g. When the acid value of the copolymer (A) is 20 KOHmg / g or more, the alkaline developability is good when used as a photosensitive resin composition. On the other hand, when the acid value of the copolymer (A) is 300 KOHmg / g or less, the exposed portion (photocured portion) is difficult to dissolve in an alkaline developer, so that the pattern shape is good.

[0049] In the present invention, the copolymer (A) contains a blocked isocyanato group in the molecule. The content of the blocked isocyanato group may be appropriately selected, but is usually selected within a range such that the blocked isocyanato group equivalent is 400 to 6,000, preferably 1,000 to 5,000. The blocked isocyanato group equivalent is the mass of the polymer per mole of the blocked isocyanato group contained in the polymer, and can be determined by dividing the mass of the polymer by the number of moles of the blocked isocyanato group contained in the polymer (g / mol). In the present invention, the blocked isocyanato group equivalent is a theoretical value calculated from the amount of the blocked isocyanato group-containing monomer charged.

[0050] <Hydroxyl-containing organic solvent (B)> The hydroxyl group-containing organic solvent (B) may be any organic solvent containing a hydroxyl group, and examples thereof include ethylene glycol monoalkyl ethers, diethylene glycol monoalkyl ethers, propylene glycol monoalkyl ethers, propylene glycol monoaryl ethers, dipropylene glycol monoalkyl ethers, tripropylene glycol monoalkyl ethers, 3-methoxy-1-butanol, 1,3-propanediol monoalkyl ethers, 1,3-butanediol monoalkyl ethers, 1,4-butanediol monoalkyl ethers, glycerin monoalkyl ethers, glycerin dialkyl ethers, methanol, ethanol, propanol, C 5-6 Cycloalkanediols, C 5-6 Examples of the hydroxyl group-containing organic solvent (B) include cycloalkane dimethanol, ethyl lactate, and diacetone alcohol. Among these, from the viewpoints of film-forming property during the production of a cured coating film and ease of availability, ethyl lactate, diacetone alcohol, 3-methoxy-1-butanol, and propylene glycol monomethyl ether are preferred, and propylene glycol monomethyl ether is particularly preferred. These hydroxyl group-containing organic solvents (B) may be used alone or in combination of two or more.

[0051] In the present invention, the storage stability of the photosensitive resin composition is improved by using in combination the copolymer (A) containing the structural unit (a) having a blocked isocyanato group and the structural unit (b) having an acid group and the hydroxyl group-containing organic solvent (B).

[0052] In the photosensitive resin composition of the present invention, a solvent other than the hydroxyl group-containing organic solvent (B) may be used in combination.

[0053] <Reactive diluent (C)> The reactive diluent (C) is a compound having at least one polymerizable ethylenically unsaturated group as a polymerizable functional group in the molecule, and among them, a compound having a plurality of polymerizable functional groups is preferable. By using such a reactive diluent (C) in combination with the copolymer (A), it is possible to adjust the viscosity, and improve the strength of the cured product formed and the adhesion to the substrate.

[0054] Examples of monofunctional monomers used as the reactive diluent (C) include (meth)acrylamide, methylol (meth)acrylamide, methoxymethyl (meth)acrylamide, ethoxymethyl (meth)acrylamide, propoxymethyl (meth)acrylamide, butoxymethoxymethyl (meth)acrylamide, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-phenoxy-2-hydroxypropyl (meth)acrylate, 5-hydroxypropyl (meth)acrylate, 6-hydroxypropyl (meth)acrylate, 7-hydroxypropyl (meth)acrylate, 8-hydroxypropyl (meth)acrylate, 9-hydroxypropyl (meth)acrylate, 10-hydroxypropyl (meth)acrylate, 11-hydroxypropyl (meth)acrylate, 12-hydroxypropyl (meth)acrylate, 13-hydroxypropyl (meth)acrylate, 14-hydroxypropyl (meth)acrylate, 15-hydroxypropyl (meth)acrylate, 16-hydroxypropyl (meth)acrylate, 17-hydroxypropyl (meth)acrylate, 18-hydroxypropyl (meth)acrylate, 19-hydroxypropyl (meth)acrylate, 20-hydroxypropyl (meth)acrylate, 21-hydroxypropyl (meth)acrylate, 22-hydroxypropyl (meth)acrylate, 23-hydroxypropyl (meth)acrylate, 24-hydroxypropyl (meth)acrylate, 25-hydroxypropyl (meth)acrylate, 26-hydroxypropyl (meth)acrylate, 27-hydroxypropyl (meth)acrylate, 28-hydroxypropyl (meth)acrylate, 29-hydroxypropyl (meth)acrylate, 30-hydroxypropyl (meth)acrylate, 31-hydroxypropyl (meth)acrylate, 32-hydroxypropyl (meth)acrylate, 33-hydroxypropyl (meth)acrylate, 34-hydroxypropyl (meth)acrylate, 35-hydroxypropyl (meth)acrylate, 36-hydroxypropyl (meth)acrylate, 37-hydroxy Examples of the monomer include (meth)acrylates such as propyl (meth)acrylate, 2-(meth)acryloyloxy-2-hydroxypropyl phthalate, glycerin mono(meth)acrylate, tetrahydrofurfuryl (meth)acrylate, glycidyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, and half (meth)acrylate of phthalic acid derivative; aromatic vinyl compounds such as styrene, α-methylstyrene, α-chloromethylstyrene, and vinyl toluene; and carboxylic acid esters such as vinyl acetate and vinyl propionate. These monomers may be used alone or in combination of two or more.

[0055] Examples of polyfunctional monomers used as the reactive diluent (C) include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexane glycol di(meth)acrylate, and trimethylol propane. (meth)acrylate, glycerin di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 2,2-bis(4-(meth)acryloxydiethoxyphenyl)propane, 2,2-bis(4-(meth)acryloxypolyethoxyphenyl)propane, 2-hydroxy-3-(meth)acryloyloxypropyl(meth)acrylate Examples of the (meth)acrylates include acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, phthalic acid diglycidyl ester di(meth)acrylate, glycerin triacrylate, glycerin polyglycidyl ether poly(meth)acrylate, urethane (meth)acrylate (i.e., tolylene diisocyanate), reaction products of trimethylhexamethylene diisocyanate, hexamethylene diisocyanate, etc. with 2-hydroxyethyl (meth)acrylate, and tris(hydroxyethyl)isocyanurate tri(meth)acrylate; aromatic vinyl compounds such as divinylbenzene, diallyl phthalate, and diallyl benzene phosphonate; dicarboxylic acid esters such as divinyl adipate; triallyl cyanurate, methylene bis(meth)acrylamide, (meth)acrylamide methylene ether, and condensates of polyhydric alcohol and N-methylol (meth)acrylamide. These monomers may be used alone or in combination of two or more kinds.

[0056] <Photopolymerization initiator (D)> The photopolymerization initiator (D) is not particularly limited, and examples thereof include benzoins such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin butyl ether; acetophenones such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 4-(1-t-butyldioxy-1-methylethyl)acetophenone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1; 2-methylanthraquinone, 2-amino-1-(4-morpholinophenyl)butanone-1; Examples of the photopolymerization initiator (D) include anthraquinones such as 1-chloroanthraquinone, 2-t-butylanthraquinone, and 1-chloroanthraquinone; thioxanthones such as xanthone, thioxanthone, 2,4-dimethylthioxanthone, 2,4-diisopropylthioxanthone, and 2-chlorothioxanthone; ketals such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzophenones such as 4-(1-t-butyldioxy-1-methylethyl)benzophenone and 3,3',4,4'-tetrakis(t-butyldioxycarbonyl)benzophenone; and acylphosphine oxides. These photopolymerization initiators (D) may be used alone or in combination of two or more.

[0057] In addition to the above components, the photosensitive resin composition of the present invention may contain known additives such as known coupling agents, leveling agents, thermal polymerization inhibitors, etc. The amount of these additives to be added is not particularly limited as long as it does not impair the effects of the present invention.

[0058] <Photosensitive resin composition for color filters> The photosensitive resin composition of the present invention can further contain a colorant (E) to form a photosensitive resin composition for color filters.

[0059] The colorant (E) is not particularly limited as long as it dissolves or disperses in the hydroxyl group-containing organic solvent (B), and examples thereof include dyes, pigments, etc. As the dye, it is preferable to use an acid dye having an acidic group such as a carboxylic acid or sulfonic acid, a salt of an acid dye with a nitrogen compound, a sulfonamide of an acid dye, etc., from the viewpoints of solubility in the hydroxyl group-containing organic solvent (B) or an alkaline developer, interaction with other components in the photosensitive resin composition, heat resistance, etc.

[0060] Examples of such dyes are: acid alizarin violet N; acid black 1, 2, 24, 48; acid blue 1, 7, 9, 25, 29, 40, 45, 62, 70, 74, 80, 83, 90, 92, 112, 113, 120, 129, 147; acid chrome violet K; acid Fuchsin; acid green 1, 3, 5, 25, 27, 50; acid orange 6, 7, 8, 10, 12, 50, 51, 52, 56, 63, 74, 95; acid red1, 4, 8, 14, 17, 18, 26, 27, 29, 31, 34, 35, 37, 42, 44, 50, 51, 52, 57, 69, 73, 80, 87, 88, 91, 92, 94, 97, 103, 111, 11 4,129,133,134,138,143,145,150,151,158,176,183,198,211,215,216,217,249,252,257,260,266,274;acid violet 6B, 7, 9, 17, 19;acid Yellow 1, 3, 9, 11, 17, 23, 25, 29, 34, 36, 42, 54, 72, 73, 76, 79, 98, 99, 111, 112, 114, 116; Food Yellow 3 and derivatives thereof. Among these, azo-based, xanthene-based, anthraquinone-based or phthalocyanine-based acid dyes are preferred. These dyes may be used alone or in combination of two or more types depending on the color of the desired pixel.

[0061] Examples of pigments include yellow pigments such as CI Pigment Yellow 1, 3, 12, 13, 14, 15, 16, 17, 20, 24, 31, 53, 83, 86, 93, 94, 109, 110, 117, 125, 128, 137, 138, 139, 147, 148, 150, 153, 154, 166, 173, 194, 214; orange pigments such as CI Pigment Orange 13, 31, 36, 38, 40, 42, 43, 51, 55, 59, 61, 64, 65, 71, 73; and CI Pigment Red 9, 97, 105, 122, 123, 144, 149, 166, 168. , red pigments such as CI Pigment Blue 15, 15:3, 15:4, 15:6, 60; violet pigments such as CI Pigment Violet 1, 19, 23, 29, 32, 36, 38; green pigments such as CI Pigment Green 7, 36, 58, 59; brown pigments such as CI Pigment Brown 23, 25; black pigments such as CI Pigment Black 1, 7, carbon black, titanium black, iron oxide, etc.

[0062] These colorants (E) may be used alone or in combination of two or more depending on the color of the desired pixel. The above dyes and pigments may also be used in combination depending on the color of the desired pixel.

[0063] When a pigment is used as the colorant (E), a known dispersant may be blended in the photosensitive resin composition from the viewpoint of improving the dispersibility of the pigment. As the dispersant, it is preferable to use a polymer dispersant having excellent dispersion stability over time. Examples of the polymer dispersant include urethane-based dispersants, polyethyleneimine-based dispersants, polyoxyethylene alkyl ether-based dispersants, polyoxyethylene glycol diester-based dispersants, sorbitan aliphatic ester-based dispersants, and aliphatic modified ester-based dispersants. As such a polymer dispersant, those commercially available under the trade names EFKA (manufactured by EFKA Chemicals BV), Disperbyk (manufactured by BYK-Chemie), Disparlon (manufactured by Kusumoto Chemicals Co., Ltd.), and SOLSPERSE (manufactured by Zeneca) may be used. The blending amount of the dispersant may be appropriately set according to the type of pigment used, etc.

[0064] The blending amounts of the copolymer (A), the hydroxyl group-containing organic solvent (B), the reactive diluent (C), the photopolymerization initiator (D) and the colorant (E) in the photosensitive resin composition for color filters are, relative to 100 parts by mass of the total amount of the copolymer (A) and the reactive diluent (C) in the photosensitive resin composition for color filters, 10 to 100 parts by mass of the copolymer (A), 30 to 1,000 parts by mass of the hydroxyl group-containing organic solvent (B), more than 0 to 90 parts by mass of the reactive diluent (C), 0.1 to 30 parts by mass of the photopolymerization initiator (D), and 0.1 to 30 parts by mass of the colorant (E). The amount is 5 to 80 parts by mass, preferably 20 to 80 parts by mass of copolymer (A), 50 to 800 parts by mass of hydroxyl-containing organic solvent (B), 20 to 80 parts by mass of reactive diluent (C), 0.5 to 20 parts by mass of photopolymerization initiator (D), and 5 to 70 parts by mass of colorant (E). More preferably, the amount is 30 to 75 parts by mass of copolymer (A), 100 to 700 parts by mass of hydroxyl-containing organic solvent (B), 25 to 70 parts by mass of reactive diluent (C), 1 to 15 parts by mass of photopolymerization initiator (D), and 10 to 60 parts by mass of colorant (E). If the blending amount is within this range, a photosensitive resin composition for color filters having an appropriate viscosity is obtained. In addition, even in the case of a photosensitive resin composition that does not contain a colorant (E), the blending amounts of copolymer (A), hydroxyl-containing organic solvent (B), reactive diluent (C), and photopolymerization initiator (D) can be applied within the above numerical range.

[0065] <Production of Photosensitive Resin Composition> The photosensitive resin composition of the present invention can be produced by mixing the above-mentioned components using a known mixing device. It is also possible to produce the composition by copolymerizing a blocked isocyanato group-containing (meth)acrylate with an unsaturated carboxylic acid in the presence of a hydroxyl group-containing organic solvent (B) to prepare a composition containing the copolymer (A) and the hydroxyl group-containing organic solvent (B), and then mixing the reactive diluent (C), the photopolymerization initiator (D) and the optional colorant (E).

[0066] The photosensitive resin composition obtained as described above has alkaline developability, and is therefore suitable as a resist. The photosensitive resin composition can be cured by appropriately selecting a baking temperature within the range of 250°C or less. However, since the copolymer (A) used in the present invention has excellent curing properties at low temperatures, the baking temperature can be lowered compared to conventional materials. When a pigment is used as the colorant (E) in the photosensitive resin composition, sufficient curing properties can be obtained even at a baking temperature of 160°C or less. The photosensitive resin composition of the present invention is advantageous in terms of energy consumption because the crosslinking reaction proceeds sufficiently even at a low baking temperature. In addition, it becomes possible to use colorants (E) and substrates with poor heat resistance, and the inherent properties of the colorant can be obtained and application to various substrates becomes possible. From this viewpoint, the baking temperature is preferably 160°C or less, and more preferably 150°C or less. The lower limit of the baking temperature is not necessarily uniform depending on the type of the blocked isocyanato group contained in the copolymer (A), but it must be equal to or higher than the dissociation temperature of the blocked isocyanato group, and is usually 80°C or higher, preferably 90°C or higher, and more preferably 100°C or higher. If the baking temperature is too low, it becomes difficult to sufficiently improve the solvent resistance of the coating film. The baking time can be appropriately selected, but is usually 10 minutes to 4 hours, preferably 20 minutes to 2 hours.

[0067] The photosensitive resin composition of the present invention is suitable as a resist used for producing various resists, particularly color filters to be incorporated in organic EL displays (for black PDL), liquid crystal displays, solid-state imaging devices such as CCD and CMOS, etc. In addition, the photosensitive resin composition of the present invention gives a cured coating film excellent in solvent resistance, low-temperature curing properties, etc., and can therefore also be used as various coatings, adhesives, binders for printing inks, etc.

[0068] The photosensitive resin composition of the present invention has good developability and storage stability, and can form a colored pattern with excellent solvent resistance even if the baking temperature during pattern formation is low, so that it is extremely useful as a photosensitive material for color filters. In addition, the photosensitive resin composition of the present invention can contribute to the development of flexible displays, the reduction of energy consumption in the manufacturing process, and the relaxation of restrictions on colorants used, due to its low-temperature curing.

[0069] <Color filter> Next, a color filter having a color pattern made of a cured product of the photosensitive resin composition for color filters of the present invention will be described. The color filter of the present invention has a color pattern formed using the above-mentioned photosensitive resin composition for color filters. A color filter is usually composed of a substrate, RGB pixels formed thereon, a black matrix formed at the boundaries between the respective pixels, and a protective film formed on the pixels and the black matrix. In this configuration, except that the pixels and the black matrix (color pattern) are formed using the above-mentioned photosensitive resin composition for color filters, other configurations may be known.

[0070] Next, an embodiment of a method for manufacturing a color filter will be described. First, a colored pattern is formed on a substrate. Specifically, a black matrix and RGB pixels are sequentially formed on the substrate. The material of the substrate is not particularly limited, and a glass substrate, a silicon substrate, a polycarbonate substrate, a polyester substrate, a polyamide substrate, a polyamideimide substrate, a polyimide substrate, an aluminum substrate, a printed wiring substrate, an array substrate, etc. can be appropriately used.

[0071] The colored pattern can be formed by photolithography. Specifically, the photosensitive resin composition is applied onto a substrate to form a coating film, and then the coating film is exposed to light through a photomask having a predetermined pattern to photocure the exposed portion. The unexposed portion is then developed with an alkaline aqueous solution, followed by baking to form a predetermined colored pattern.

[0072] The method of applying the photosensitive resin composition is not particularly limited, but may be a screen printing method, a roll coating method, a curtain coating method, a spray coating method, a spin coating method, or the like. After applying the photosensitive resin composition, the hydroxyl-containing organic solvent (B) may be volatilized by heating using a heating means such as a circulation oven, an infrared heater, or a hot plate, if necessary. The heating conditions are not particularly limited, and may be appropriately set depending on the type of the photosensitive resin composition used. In general, heating at a temperature of 50°C to 120°C for 30 seconds to 30 minutes may be used.

[0073] Next, the formed coating film is partially exposed by irradiating it with active energy rays such as ultraviolet rays and excimer laser light through a negative mask. The amount of energy radiation to be irradiated may be appropriately selected depending on the composition of the photosensitive resin composition, and may be, for example, 30 to 2000 mJ / cm. 2 The light source used for exposure is not particularly limited, but may be a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, a xenon lamp, a metal halide lamp, or the like.

[0074] The alkaline aqueous solution used for development is not particularly limited, but may be an aqueous solution of sodium carbonate, potassium carbonate, calcium carbonate, sodium hydroxide, potassium hydroxide, or the like; an aqueous solution of an amine compound such as ethylamine, diethylamine, or dimethylethanolamine; or an aqueous solution of a p-phenylenediamine compound such as tetramethylammonium, 3-methyl-4-amino-N,N-diethylaniline, 3-methyl-4-amino-N-ethyl-N-β-hydroxyethylaniline, 3-methyl-4-amino-N-ethyl-N-β-methanesulfonamidoethylaniline, 3-methyl-4-amino-N-ethyl-N-β-methoxyethylaniline, or a sulfate, hydrochloride, or p-toluenesulfonate thereof. In addition, a defoamer or a surfactant may be added to these aqueous solutions as necessary. In addition, after development with the alkaline aqueous solution, it is preferable to wash with water and dry.

[0075] The baking conditions are not particularly limited, and the heat treatment may be performed according to the type of the photosensitive resin composition used. In the conventional photosensitive resin composition, when the baking temperature is 200° C. or less, the solvent resistance of the colored pattern is insufficient, but in the photosensitive resin composition for color filters of the present invention, a colored pattern exhibiting sufficient solvent resistance can be formed even when baked at a temperature of 120° C. or less. Therefore, the baking temperature can be lowered, and when baking at a high temperature, the processing time can be shortened, which is a great advantage in manufacturing. From this viewpoint, the baking temperature is usually 210° C. or less, preferably 160° C. or less, more preferably 120° C. or less, and the baking time is usually 10 minutes to 4 hours, preferably 20 minutes to 2 hours.

[0076] The above-mentioned coating, exposure, development and baking are repeated in sequence using the photosensitive resin composition for the black matrix and the photosensitive resin compositions for the red, green and blue pixels, thereby forming a desired colored pattern. Although the above describes a method for forming a colored pattern by photocuring, if a photosensitive resin composition containing a curing accelerator and a known epoxy resin is used instead of the photopolymerization initiator (D), the desired colored pattern can be formed by applying the composition by the inkjet method and then heating. Next, a protective film is formed on the colored pattern (each pixel of RGB and the black matrix). The protective film is not particularly limited, and may be formed using a known material.

[0077] The color filter produced in this manner has excellent sensitivity and developability, and is produced using a photosensitive resin composition that can be cured at low temperatures and gives a colored pattern with excellent solvent resistance, and therefore has an excellent colored pattern with little color change.

[0078] <Image display element> The image display element of the present invention is an image display element equipped with the above-mentioned color filter, and specific examples thereof include a liquid crystal display element, an organic EL display element, and a solid-state imaging element such as a CCD element or a CMOS element. The image display element of the present invention may be manufactured according to a conventional method, except for using the above-mentioned color filter. For example, when manufacturing a liquid crystal display element, the above-mentioned color filter is formed on a substrate, and then electrodes, spacers, etc. are formed in sequence. Then, electrodes, etc. are formed on another substrate, and the two are bonded together, and a predetermined amount of liquid crystal is injected and sealed. EXAMPLES

[0079] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In these examples, parts and percentages are all based on mass unless otherwise specified. In addition, the acid value and weight average molecular weight are measured as follows. (1) Acid value: The acid value of the copolymer (A) measured in accordance with JIS K6901 5.3, and means the number of milligrams of potassium hydroxide required to neutralize the acidic components contained in 1 g of the copolymer (A). (2) The weight average molecular weight (Mw) means the weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions in terms of standard polystyrene. Column: Showdex (registered trademark) LF-804 + LF-804 (manufactured by Showa Denko K.K.) Column temperature: 40℃ Sample: 0.2% solution of copolymer in tetrahydrofuran Developing solvent: Tetrahydrofuran Detector: Differential refractometer (Shodex RI-71S) (manufactured by Showa Denko K.K.) Flow rate: 1mL / min

[0080] [Synthesis Example 1] In a flask equipped with a stirrer, a dropping funnel, a condenser, a thermometer and a gas inlet tube, 149.3 g of propylene glycol monomethyl ether was placed, and the mixture was stirred while replacing with nitrogen and heated to 78° C. Next, a monomer mixture consisting of 22.4 g of dicyclopentanyl methacrylate, 17.2 g of methacrylic acid and 50.2 g of 2-(3,5-dimethylpyrazol-1-yl)carbonylaminoethyl methacrylate (Karenz MOI-BP, manufactured by Showa Denko K.K., dissociation rate of blocked isocyanato group: 70 mass%) and 11.2 g of 2,2′-azobis(2,4-dimethylvaleronitrile) (polymerization initiator) added and dissolved in 62.8 g of propylene glycol monomethyl ether acetate were each dropped into the flask from the dropping funnel. After the dropwise addition, the mixture was stirred at 78° C. for 3 hours to carry out a copolymerization reaction, thereby producing a copolymer, and thus obtaining a polymer composition (concentration of components other than the solvent: 35% by mass) of sample No. 1. The weight-average molecular weight of the copolymer in the obtained polymer composition was 9,100, and the acid value was 121.5 KOHmg / g.

[0081] [Synthesis Examples 2 to 9 and Comparative Synthesis Examples 1 to 2] Copolymerization reaction was carried out under the same conditions as in Synthesis Example 1, except that the raw materials shown in Tables 1 and 2 were used, to obtain polymer compositions of Samples Nos. 2 to 11 (concentration of components other than the solvent: 35% by mass). The weight average molecular weight and acid value of the copolymer in the obtained polymer composition are shown in Tables 1 and 2. In Tables 1 and 2, 2-[O-(1'-methylproplideneamino)carboxyamino]ethyl methacrylate was Karenz MOI-BM, manufactured by Showa Denko K.K., dissociation rate of blocked isocyanato group: 18% by mass; 2-[[[2-methyl-1-oxo-2-propenyl]oxy]ethyl]amino]carbonyl]-1,3 diethyl malonate was Karenz MOI-DEM, manufactured by Showa Denko K.K., dissociation rate of blocked isocyanato group: 90% by mass; and 4-[[[[2-[(2-methyl-1-oxo-2 2-[[[2-[(2-methyl-1-oxy-2-propen-1-yl)oxy]ethyl]amine]carbonyl]oxy]methyl ester of benzoic acid has a dissociation rate of blocked isocyanato groups: 75% by mass, and 2-propenoic acid-2-methyl-2-[[(3,5-dimethylphenoxy)carbonyl]amine]ethyl ester has a dissociation rate of blocked isocyanato groups: 28% by mass.

[0082] [Table 1]

[0083] [Table 2]

[0084] [Examples 1 to 9 and Comparative Examples 1 to 2] <Preparation of photosensitive resin composition (pigment type)> A green pigment dispersion was prepared by adding 100 parts by mass of CI Pigment Green 36 (colorant), 44.98 parts by mass of propylene glycol monomethyl ether acetate, and 25 parts by mass of a dispersant (Disperbyk-161, manufactured by Big Chemie Japan Co., Ltd.) to a stainless steel container filled with 200 g of zirconia beads having a diameter of 0.5 mm, and mixing and dispersing the mixture for 2 hours using a paint shaker. This green pigment dispersion was mixed with other ingredients shown in Table 3 (i.e., polymer composition, reactive diluent, photopolymerization initiator, and solvent) to prepare a photosensitive resin composition. The mixing ratio of each ingredient is as shown in Table 3. The photosensitive resin compositions of Examples 1 to 9 were prepared using the polymer compositions of Samples Nos. 1 to 9, respectively, and the photosensitive resin compositions of Comparative Examples 1 and 2 were prepared using the polymer compositions of Samples Nos. 10 to 11, respectively. The amount of polymer composition includes the solvent contained at the end of the copolymerization reaction, and the amount of solvent contained in each sample is also included in the solvent as an ingredient.

[0085] [Table 3]

[0086] <Evaluation of Photosensitive Resin Composition> (1) Alkaline developability Each of the photosensitive resin compositions of Examples 1 to 9 and Comparative Examples 1 and 2 was spin-coated onto a 5 cm square glass substrate (alkali-free glass substrate) so that the thickness after exposure was 2.5 μm, and then the substrate was heated at 90° C. for 3 minutes to volatilize the solvent. Next, a photomask with a predetermined pattern was placed at a distance of 100 μm from the coating film, and the coating film was exposed through this photomask (exposure amount 150 mJ / cm 2) and the exposed parts were photocured. Next, an aqueous solution containing 0.1 mass % sodium carbonate was sprayed at a temperature of 23°C and a pressure of 0.3 MPa to dissolve and develop the unexposed parts, and then the film was baked at 100°C for 20 minutes to form a predetermined pattern. The residue after the alkali development was confirmed by observing the pattern after the alkali development using an electron microscope S-3400 manufactured by Hitachi High-Technologies Corporation. The evaluation criteria are as follows: ○: No residue ×: Residue present The evaluation results of alkaline developability are shown in Table 4.

[0087] (2) Evaluation of solvent resistance Each of the photosensitive resin compositions of Examples 1 to 9 and Comparative Examples 1 to 2 was spin-coated on a 5 cm square glass substrate (alkali-free glass substrate) so that the thickness after baking was 2.5 μm, and then heated at 90° C. for 3 minutes to volatilize the solvent. Next, the coating film was exposed to light with a wavelength of 365 nm, the exposed part was photocured, and then the coating film was left in a dryer with a baking temperature of 100° C. for 20 minutes to produce a cured coating film. 200 mL of propylene glycol monomethyl ether acetate was placed in a 500 mL glass bottle with a lid and left at 80° C. The test piece with the cured coating film was immersed in the solution and then left at 80° C. for 5 minutes. The color change (ΔE * ab) was measured using a spectrophotometer UV-1650PC (Shimadzu Corporation). ΔE * The measurement results of ab are shown in Table 4. ΔE * If ab is 1.5 or less, it can be said that the solvent resistance is excellent.

[0088] (3) Evaluation of storage stability The copolymers of Synthesis Examples 1 to 9 and Comparative Synthesis Examples 1 to 2 were weighed out in equal amounts into glass containers and the openings were sealed with aluminum foil to prevent dust and the like from entering. Next, these samples were placed in an incubator maintained at 23°C, and the weight average molecular weight (Mw) of the samples was measured after one month. The rate of change in Mw after one month is shown in Table 5. If the rate of change in Mw after one month is within 20%, the storage stability of the copolymer can be said to be excellent.

[0089] [Table 4]

[0090] [Table 5]

[0091] As can be seen from the results in Table 4, the photosensitive resin compositions of Examples 1 to 9 using the polymer compositions of Samples No. 1 to 9 had good alkali developability and solvent resistance. Furthermore, since the storage stability of a copolymer correlates with the storage stability of the photosensitive resin composition containing it, it can be said from the results in Table 5 that the photosensitive resin compositions of Examples 1 to 9 using the polymer compositions of Samples No. 1 to 9 also had good storage stability. In contrast, the photosensitive resin compositions of Comparative Examples 1 and 2 using the polymer compositions of Samples No. 10 and 11 had good storage stability, but the photosensitive resin composition of Comparative Example 1 using the polymer composition of Sample No. 10 had insufficient solvent resistance, and the photosensitive resin composition of Comparative Example 2 using the polymer composition of Sample No. 11 had insufficient alkali developability and solvent resistance.

[0092] As is apparent from the above results, the present invention can provide a photosensitive resin composition that has good developability, as well as excellent solvent resistance and storage stability.

[0093] This international application claims priority to Japanese Patent Application No. 2017-150502, filed on August 3, 2017, the entire contents of which are incorporated herein by reference.

Claims

1. The method includes a step of synthesizing a copolymer (A) by copolymerizing a monomer mixture containing a blocked isocyanato group-containing (meth)acrylate, an unsaturated carboxylic acid, and a monomer having a polymerizable unsaturated bond and a hydroxyl group in the presence of a hydroxyl group-containing organic solvent (B), and then blending a reactive diluent (C) and a photopolymerization initiator (D), the blocked isocyanato group-containing (meth)acrylate is at least one selected from the group consisting of 2-(3,5-dimethylpyrazol-1-yl)carbonylaminoethyl methacrylate, 2-[O-(1'-methylpropylideneamino)carboxyamino]ethyl methacrylate, 2-[[[2-methyl-1-oxo-2-propenyl]oxy]ethyl]amino]carbonyl]-1,3-diethyl malonate, 4-[[[[2-[(2-methyl-1-oxo-2-propen-1-yl)oxy]ethyl]amine]carbonyl]oxy]methyl benzoate, 2-[[[[2-[(2-methyl-1-oxy-2-propen-1-yl)oxy]ethyl]amine]carbonyl]oxy]methyl benzoate, and 2-methyl-2-[[(3,5-dimethylphenoxy)carbonyl]amine]ethyl 2-propenoate; The method for producing a cured coating film includes a step of applying a photosensitive resin composition obtained by the method for producing a photosensitive resin composition, in which the hydroxyl group-containing organic solvent (B) is one or more selected from the group consisting of ethylene glycol monoalkyl ether, diethylene glycol monoalkyl ether, propylene glycol monoalkyl ether, propylene glycol monoaryl ether, dipropylene glycol monoalkyl ether, tripropylene glycol monoalkyl ether, 3-methoxy-1-butanol, 1,3-propanediol monoalkyl ether, 1,3-butanediol monoalkyl ether, 1,4-butanediol monoalkyl ether, glycerin monoalkyl ether, and glycerin dialkyl ether, to a substrate, exposing the composition to light, developing the composition with an alkali, and baking the resulting mixture at a temperature of 160° C. or less to form a pattern.

2. 2. The method for producing a cured coating film according to claim 1, wherein the hydroxyl group-containing organic solvent (B) is a propylene glycol monoalkyl ether.

3. The method for producing a cured coating film according to claim 1 or 2, wherein the copolymer (A) contains 1 to 40 mol % of structural units derived from the blocked isocyanato group-containing (meth)acrylate, 1 to 60 mol % of structural units derived from the unsaturated carboxylic acid, and more than 0 mol % to 50 mol % of structural units derived from the monomer having a polymerizable unsaturated bond and a hydroxyl group.

4. The method for producing a cured coating film according to any one of claims 1 to 3, wherein a molar ratio of the structural units derived from the blocked isocyanato group-containing (meth)acrylate and the structural units derived from the unsaturated carboxylic acid in the copolymer (A) is from 10:90 to 50:

50.

5. The method for producing a cured coating film according to any one of claims 1 to 4, wherein the unsaturated carboxylic acid is (meth)acrylic acid, and the monomer having a polymerizable unsaturated bond and a hydroxyl group is at least one selected from the group consisting of 2-hydroxyethyl (meth)acrylate.

6. The method for producing a cured coating film described in any one of claims 1 to 5, wherein the photosensitive resin composition further contains a colorant (E), and the cured coating film is a color filter.

7. 7. The method for producing a cured coating film according to claim 6, wherein, relative to 100 parts by mass of the total amount of the copolymer (A) and the reactive diluent (C), the copolymer (A) is contained in an amount of 10 to 100 parts by mass, the hydroxyl group-containing organic solvent (B) is contained in an amount of 30 to 1,000 parts by mass, the reactive diluent (C) is contained in an amount of more than 0 to 90 parts by mass, the photopolymerization initiator (D) is contained in an amount of 0.1 to 30 parts by mass, and the colorant (E) is contained in an amount of 5 to 80 parts by mass.

8. The method for producing a cured coating film according to claim 6 or 7, wherein the colorant (E) contains a pigment.

Citation Information

Patent Citations

  • Curable resin composition for columnar spacer, the columnar spacer and liquid crystal display element

    JP2006189584A

  • Color filter, liquid crystal display element, and manufacturing method of color filter

    JP2013068843A

  • Production method of molded body and curing method of photosensitive resin composition

    JP2014070148A

  • Resin composition containing specified hardening acceleration catalyst

    JP2015174877A

  • Curable resin composition, color filter, image display element and manufacturing method of color filter

    JP2016084464A