Film forming method
By adjusting the oxygen-to-inert gas ratio in a controlled plasma environment, the film formation method enhances the loading effect, ensuring consistent silicon oxide film thickness across the wafer surface.
Patent Information
- Application Number
- JP2020208755
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-16
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-12-16
AI Technical Summary
Existing methods for forming silicon oxide films on wafers face challenges in achieving optimal loading effects, particularly in terms of in-plane uniformity and film thickness consistency.
A film formation method involving alternating adsorption and oxidation steps, where the ratio of oxygen gas to inert gas is adjusted based on pressure conditions to enhance the loading effect, using a controlled plasma environment to form a silicon oxide film in a recess on a substrate.
The method improves the loading effect by optimizing the in-plane uniformity of the silicon oxide film thickness, reducing variations across the wafer surface.
Smart Images

Figure 0007563845000005 
Figure 0007563845000006 
Figure 0007563845000007
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a film forming method. By law Regarding. [Background technology]
[0002] There is known a technique for forming a silicon oxide film on a wafer W by repeatedly supplying diisopropylaminosilane and oxygen radicals alternately into a reaction tube at room temperature (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-206500 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides techniques that can improve the loading effect at a desired pressure. [Means for solving the problem]
[0005] A film formation method according to one embodiment of the present disclosure is a method for forming a silicon oxide film in a recess formed on a surface of a substrate in a processing vessel, the method comprising the steps of: (a) adsorbing a silicon-containing gas onto the substrate; (b) exposing the substrate to a plasma formed from an oxidizing gas containing oxygen gas and an inert gas at a desired pressure; and (c) repeating steps (a) and (b), wherein in step (b), a ratio of oxygen gas to inert gas is determined based on the desired pressure and corresponding information in which the ratio of oxygen gas to inert gas and information on the loading effect are associated with each pressure in the processing vessel. Effect of the Invention
[0006] The present disclosure allows for improved loading effects at desired pressures. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic vertical cross-sectional view showing an example of a film forming apparatus according to an embodiment. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of a film forming apparatus according to an embodiment. [Diagram 3] FIG. 2 is a diagram showing an example of the configuration of a control unit of a film forming apparatus according to an embodiment; [Figure 4] FIG. 1 is a diagram showing an example of a film forming method according to an embodiment; [Diagram 5] Diagram explaining the mechanism by which the loading effect improves [Figure 6] FIG. 1 shows the evaluation results of Example 1 [Figure 7] FIG. 1 shows the evaluation results of Example 2 [Figure 8] FIG. 1 shows the evaluation results of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, non-limiting exemplary embodiments of the present disclosure will be described with reference to the accompanying drawings. In all of the accompanying drawings, the same or corresponding members or parts are designated by the same or corresponding reference numerals, and duplicated descriptions will be omitted.
[0009] [Film forming equipment] An example of a film forming apparatus according to an embodiment will be described with reference to Figures 1 to 3. In this embodiment, a case in which a silicon oxide film is formed by atomic layer deposition (ALD) will be described as an example.
[0010] The film forming apparatus 1 includes a ceiling-equipped, generally cylindrical processing vessel 2 whose longitudinal direction is oriented in a vertical direction. The processing vessel 2 is made of a material having excellent heat resistance and corrosion resistance, such as quartz.
[0011] An exhaust unit 3 for exhausting gas within the processing vessel 2 is disposed on one side of the processing vessel 2. The exhaust unit 3 is formed to extend upward along the processing vessel 2 and communicates with the processing vessel 2 via an opening (not shown) provided in the sidewall of the processing vessel 2. The upper end of the exhaust unit 3 is connected to an exhaust port 4 disposed in the upper part of the processing vessel 2. An exhaust pipe (not shown) is connected to the exhaust port 4, and the exhaust pipe is provided with a pressure adjustment mechanism such as a valve (not shown) and a vacuum pump 127 described later. The pressure adjustment mechanism exhausts gas within the processing vessel 2 to the exhaust pipe via the opening, the exhaust unit 3, and the exhaust port 4, and the inside of the processing vessel 2 is controlled to a desired pressure (vacuum level).
[0012] A lid body 5 is disposed below the processing vessel 2. The lid body 5 is formed of a material having excellent heat resistance and corrosion resistance, such as quartz. The lid body 5 is configured to be movable up and down by a boat elevator 128 described later. When the lid body 5 is raised by the boat elevator 128, the lower side (furnace opening portion) of the processing vessel 2 is closed, and when the lid body 5 is lowered by the boat elevator 128, the lower side (furnace opening portion) of the processing vessel 2 is opened.
[0013] The wafer boat 6 is placed on the lid 5. The wafer boat 6 is made of, for example, quartz. The wafer boat 6 is configured to be able to accommodate a plurality of wafers W at a predetermined interval in the vertical direction. A heat retaining tube for preventing a temperature drop in the processing vessel 2 from the furnace opening of the processing vessel 2 and a rotating table for rotatably mounting the wafer boat 6 housing the wafers W may be provided on the upper part of the lid 5, and the wafer boat 6 may be mounted on these. In these cases, it becomes easier to control the temperature of the wafers W accommodated in the wafer boat 6 to be uniform.
[0014] A temperature control mechanism, for example, a heater 7 for heating made of a resistance heating element, is provided around the processing vessel 2 so as to surround the processing vessel 2. The inside of the processing vessel 2 is set to a predetermined temperature by the heater 7 for heating, and as a result, the wafer W accommodated inside the processing vessel 2 is heated to the predetermined temperature.
[0015] Processing gas supply pipes 8 and 9 are inserted into the side surface of the processing chamber 2 near the bottom end thereof to supply processing gas into the processing chamber 2. In this embodiment, a source gas, an oxidizing gas, a purge gas, etc. are used as the processing gas. The source gas is a silicon-containing gas that causes the wafer W to adsorb the source (Si), and may be, for example, diisopropylaminosilane (DIPAS) gas. The source gas is used in the adsorption step described below. The oxidizing gas is a gas that oxidizes the adsorbed source (Si), and may be, for example, oxygen (O2) gas. The oxidizing gas is used in the oxidation step described below. The purge gas is a gas that dilutes the processing gas, and may be, for example, an inert gas such as nitrogen (N2) gas.
[0016] The processing gas supply pipe 8 supplies an oxidizing gas and a purge gas into the processing vessel 2. The processing gas supply pipe 8 is inserted into a plasma generating unit 10, which will be described later. Therefore, the oxidizing gas and the dilution gas supplied from the processing gas supply pipe 8 are plasma excited (activated). As the processing gas supply pipe 8, for example, a dispersion injector is used.
[0017] The processing gas supply pipe 9 supplies a source gas and a purge gas into the processing vessel 2. As shown in Fig. 2, the processing gas supply pipe 9 is disposed on the inner wall of the processing vessel 2. Therefore, the source gas and the purge gas supplied from the processing gas supply pipe 9 are not plasma-excited (activated). As the processing gas supply pipe 9, for example, a distributed injector is used.
[0018] Each of the processing gas supply pipes 8 and 9 is provided with supply holes (not shown) at a predetermined interval in the vertical direction, and the processing gas is supplied into the processing vessel 2 through the supply holes. Therefore, as shown by the arrows in FIG. 1, the processing gas is supplied into the processing vessel 2 from a plurality of points in the vertical direction. Each of the processing gas supply pipes 8 and 9 is connected to a processing gas supply source (not shown) via a mass flow controller (MFC) 125 described later. Note that FIG. 1 illustrates only the processing gas supply pipe 8 that supplies a processing gas for performing a plasma processing described later (in this embodiment, a processing gas supply pipe that supplies an oxidizing gas). Also, FIG. 2 illustrates the processing gas supply pipe 8 that supplies an oxidizing gas and the processing gas supply pipe 9 that supplies a processing gas that is not used for the plasma processing described later (in this embodiment, a processing gas supply pipe that supplies a source gas or a purge gas).
[0019] A plasma generating unit 10 is provided on the other side of the processing vessel 2, i.e., on the opposite side of the one side of the processing vessel 2 on which the exhaust unit 3 is disposed. The plasma generating unit 10 includes a pair of electrodes 11 and the like. A processing gas supply pipe 8 is inserted between the pair of electrodes 11. The pair of electrodes 11 are connected to a high-frequency power source, a matching box (not shown), and the like. By applying high-frequency power between the pair of electrodes 11 from the high-frequency power source via the matching box, the processing gas supplied between the pair of electrodes 11 is excited (activated) into plasma, and oxygen radicals (O * ) is generated. * ) are supplied into the processing vessel 2 from the plasma generating unit 10.
[0020] In the processing vessel 2, a plurality of temperature sensors 122, for example made up of thermocouples, for measuring the temperature in the processing vessel 2 and a plurality of pressure gauges 123 for measuring the pressure in the processing vessel 2 are arranged.
[0021] The film forming apparatus 1 includes a control unit 100 that controls each unit of the apparatus. An example of the configuration of the control unit 100 is shown in FIG.
[0022] Connected to the control unit 100 are an operation panel 121, temperature sensor(s) 122, pressure gauge(s) 123, a heater controller 124, an MFC 125, a valve control unit 126, a vacuum pump 127, a boat elevator 128, a plasma control unit 129, and the like.
[0023] The operation panel 121 includes a display screen and operation buttons, and transmits operation instructions from the operator to the control unit 100, and also displays various information from the control unit 100 on the display screen.
[0024] The temperature sensor(s) 122 measure the temperatures of various parts, such as the inside of the processing chamber 2 and the inside of the exhaust piping, and notify the control unit 100 of the measured temperatures.
[0025] The pressure gauge(s) 123 measure the pressures in the processing chamber 2, the exhaust pipes, and the like, and notify the control unit 100 of the measured values.
[0026] The heater controller 124 is for individually controlling the heating heaters 7, and in response to instructions from the control unit 100, energizes the heating heaters 7 to heat them, and also measures the power consumption of the heating heaters 7 individually and notifies the control unit 100.
[0027] The MFC 125 is disposed in each pipe such as the process gas supply pipes 8 and 9, and controls the flow rate of the gas flowing through each pipe to an amount instructed by the control unit 100. The MFC 125 also measures the actual flow rate of the gas and notifies the control unit 100.
[0028] Valve control unit 126 is arranged on each pipe, and controls the opening degree of the valve arranged on each pipe to a value instructed by control unit 100.
[0029] The vacuum pump 127 is connected to an exhaust pipe and exhausts gas from within the processing chamber 2 .
[0030] The boat elevator 128 loads the wafer boat 6 (wafers W) into the processing vessel 2 by raising the lid body 5, and unloads the wafer boat 6 (wafers W) from the processing vessel 2 by lowering the lid body 5.
[0031] The plasma control unit 129 is for controlling the plasma generating unit 10, and controls the plasma generating unit 10 in response to an instruction from the control unit 100, and activates, for example, oxygen supplied into the plasma generating unit 10 to generate oxygen radicals (O * ) etc.
[0032] The control unit 100 is made up of a recipe storage unit 111, a ROM 112, a RAM 113, an I / O port 114, a CPU 115, and a bus 116 that interconnects these components.
[0033] The recipe storage unit 111 stores a setup recipe and a plurality of process recipes. At the beginning of manufacturing the film forming apparatus 1, only the setup recipe is stored. The setup recipe is executed when generating a thermal model or the like corresponding to each processing apparatus. The process recipe is a recipe prepared for each heat treatment (process) that the user actually performs. The process recipe specifies the temperature change of each part, the pressure change in the processing vessel 2, the timing of starting and stopping the supply of the processing gas and the supply flow rate, etc., from the time when the wafer W is loaded into the processing vessel 2 to the time when the processed wafer W is unloaded.
[0034] The ROM 112 is composed of an EEPROM, a flash memory, a hard disk, etc., and is a recording medium that stores the operation program of the CPU 115, etc.
[0035] The RAM 113 functions as a work area for the CPU 115 .
[0036] The I / O port 114 is connected to an operation panel 121, a temperature sensor 122, a pressure gauge 123, a heater controller 124, an MFC 125, a valve control unit 126, a vacuum pump 127, a boat elevator 128, a plasma control unit 129, etc., and controls the input and output of data and signals.
[0037] A CPU (Central Processing Unit) 115 constitutes the core of the control unit 100 and executes a control program stored in a ROM 112. The CPU 115 also controls the operation of the film forming apparatus 1 according to a recipe (process recipe) stored in a recipe storage unit 111 in response to an instruction from an operation panel 121. That is, the CPU 115 causes a temperature sensor(s) 122, a pressure gauge(s) 123, an MFC 125, etc. to measure the temperature, pressure, flow rate, etc. of each part inside the processing vessel 2 and the exhaust piping, etc. The CPU 115 also outputs control signals, etc. to a heater controller 124, an MFC 125, a valve control unit 126, a vacuum pump 127, etc. based on the measurement data, and controls the above-mentioned parts to follow the process recipe.
[0038] The bus 116 transfers information between each section.
[0039] [Film formation method] An example of a film formation method of the embodiment will be described with reference to Fig. 4. In the film formation method of the embodiment, a case in which a silicon oxide film is formed on a wafer W by an ALD method using the above-mentioned film formation apparatus 1 will be described as an example.
[0040] The film forming method of the embodiment is a method for forming a silicon oxide film having a desired thickness on a wafer W by performing (repeating) a cycle including an adsorption step and an oxidation step a predetermined number of times (e.g., 100 times). The adsorption step is a step for adsorbing a silicon-containing material (hereinafter referred to as "silicon" or "Si") including silicon (Si) onto the surface of the wafer W. The oxidation step is a step for oxidizing the Si adsorbed onto the surface of the wafer W. In this embodiment, DIPAS gas is used as a source gas, O2 gas is used as an oxidation gas, and N2 gas is used as a purge gas.
[0041] In the following description, the operation of each part constituting the film forming apparatus 1 is controlled by the control unit 100 (CPU 115). As described above, the control unit 100 (CPU 115) controls the heater controller 124 (heating heater 7), MFC 125 (processing gas supply pipes 8, 9), valve control unit 126, vacuum pump 127, plasma control unit 129 (plasma generation unit 10), etc., to set the temperature, pressure, gas flow rate, etc. in the processing vessel 2 in each process to conditions according to the recipe shown in FIG.
[0042] First, the wafers W are loaded into the processing vessel 2. Specifically, the inside of the processing vessel 2 is maintained at a predetermined load temperature by the temperature-raising heater 7, and a predetermined amount of N2 gas is supplied into the processing vessel 2. In addition, the wafer boat 6 containing the wafers W is placed on the lid 5. Then, the boat elevator 128 raises the lid 5, and the wafers W (wafer boat 6) are loaded into the processing vessel 2.
[0043] After the loading step, an adsorption step is performed. The adsorption step is a process of supplying a source gas to the wafer W to adsorb Si to the surface of the wafer W. In this embodiment, DIPAS gas is supplied to the wafer W to adsorb Si to the wafer W.
[0044] In the adsorption step, first, the inside of the processing vessel 2 is set to a predetermined temperature (for example, room temperature). In this embodiment, since the inside of the processing vessel 2 is set to room temperature, the inside of the processing vessel 2 is not heated by the temperature raising heater 7. In addition, DIPAS gas and N2 gas are supplied into the processing vessel 2 from the processing gas supply pipe 9, and N2 gas is supplied into the processing vessel 2 from the processing gas supply pipe 8 (flow process).
[0045] The flow process of the adsorption step is performed for a predetermined time (e.g., 1 to 10 seconds), and when a predetermined amount of Si is adsorbed on the surface of the wafer W, the supply of DIPAS gas and N2 gas from the process gas supply pipe 9 and the supply of N2 gas from the process gas supply pipe 8 are stopped. Then, the gas in the process vessel 2 is discharged, and a predetermined amount of N2 gas is supplied into the process vessel 2 from the process gas supply pipes 8 and 9, for example, to discharge the gas in the process vessel 2 to the outside of the process vessel 2 (purge, vacuum process).
[0046] After the adsorption step, an oxidation step is performed in which the wafer W on which Si is adsorbed is exposed to plasma formed from an oxidizing gas to oxidize the Si.
[0047] In the oxidation step, the inside of the processing vessel 2 is set to a predetermined temperature (for example, room temperature). Furthermore, O2 gas and N2 gas are supplied into the processing vessel 2 from the processing gas supply pipe 8 at a predetermined ratio, and N2 gas is supplied into the processing vessel 2 from the processing gas supply pipe 9. Then, high-frequency power with a predetermined output is applied between the electrodes 11 from a high-frequency power source (not shown) via a matching box (not shown). As a result, the O2 gas and N2 gas supplied between the electrodes 11 are plasma-excited (activated), and oxygen radicals (O * ) is generated. The oxygen radicals generated in this manner are supplied from the plasma generating unit 10 into the processing vessel 2. When the oxygen radicals are supplied into the processing vessel 2, the Si adsorbed on the wafer W is oxidized, and a silicon oxide film is formed on the wafer W (flow process). Note that the flow process is performed, for example, while the inside of the processing vessel 2 is pumped only by the vacuum pump 127.
[0048] In the flow process, O2 gas and N2 gas are supplied from the process gas supply pipe 8 into the process vessel 2 at a ratio determined based on a desired pressure and corresponding information in which the ratio of O2 gas and N2 gas and information on the loading effect are associated with each pressure in the process vessel 2. This allows a silicon oxide film to be formed under conditions that improve the loading effect at the desired pressure. The corresponding information is calculated, for example, by experiments and simulations according to the embodiments described below, and is stored in the recipe storage unit 111, the ROM 112, etc. in advance. The loading effect is an index of the in-plane uniformity when a silicon oxide film is formed on a wafer W on which a pattern is formed. The improvement of the loading effect means that the in-plane uniformity of the film thickness, for example, the drop in the film thickness at the center of the wafer W, is improved. In this embodiment, the loading effect is evaluated using the largest value among the values of the following formula (1) as an index value.
[0049]
number
[0050] In formula (1), the film thickness on a bare wafer is the film thickness when a silicon oxide film is formed on a bare wafer with no pattern formed thereon. The film thickness on a patterned wafer is the film thickness when a silicon oxide film is formed on a patterned wafer with a pattern including recesses formed thereon under the same process conditions as for a bare wafer. The loading effect is calculated by measuring each film thickness at multiple positions on the diameter of the wafer W, and using formula (1) at each film thickness measurement position. The smaller the loading effect index value, the smaller the difference in film thickness with the bare wafer, and the better the loading effect.
[0051] The flow process of the oxidation step is performed for a predetermined time (e.g., 5 to 100 seconds), and when a desired silicon oxide film is formed on the wafer W, the supply of O2 gas from the process gas supply pipe 8 is stopped, and the application of high frequency power from the high frequency power source (not shown) is stopped. The supply of N2 gas from the process gas supply pipes 8 and 9 is also stopped. Then, the gas in the process vessel 2 is discharged, and a predetermined amount of N2 gas is supplied from the process gas supply pipes 8 and 9 into the process vessel 2 to discharge the gas in the process vessel 2 to the outside of the process vessel 2 (purge, vacuum process).
[0052] This completes one cycle of the ALD method, which includes the adsorption step and the oxidation step.
[0053] Next, one cycle of the ALD method is started again, starting from the adsorption step. Then, this cycle is repeated a predetermined number of times. As a result, Si is adsorbed onto the surface of the wafer W, and the adsorbed Si is oxidized to form a silicon oxide film. As a result, a silicon oxide film having a desired film thickness is formed on the wafer W.
[0054] When a silicon oxide film having a desired thickness is formed on the wafer W, the wafer W is unloaded. Specifically, a predetermined amount of N2 gas is supplied from the process gas supply pipes 8 and 9 into the process vessel 2 to return the pressure inside the process vessel 2 to normal pressure, and the temperature inside the process vessel 2 is maintained at a predetermined temperature by the temperature increasing heater 7. Then, the boat elevator 128 lowers the lid 5, thereby unloading the wafer W.
[0055] 〔mechanism〕 The mechanism by which the loading effect is improved by the film forming method of the embodiment will be described with reference to FIG.
[0056] FIG. 5(a) shows that oxygen radicals (O * 1 is a diagram for explaining a surface reaction of the wafer W when the flow rate of the N2 gas supplied to the wafer W (the flow rate of the N2 gas supplied from the process gas supply pipe 8) is appropriate together with the O *When the flow rate of N2 gas supplied to the wafer W is appropriate, the N2 gas is * Contributing to the transport of O * It is presumed that the loading effect is improved because the mean free path of the catalyst is lengthened and the oxidation reaction is promoted.
[0057] FIG. 5(b) shows that in the oxidation step, O * 1 is a diagram for explaining a surface reaction of the wafer W when the flow rate of the N2 gas supplied to the wafer W (the flow rate of the N2 gas supplied from the process gas supply pipe 8) is low. * When the flow rate of N2 gas supplied to the wafer W is small, O * The contribution of O to the transport is small. * The mean free path of the O * It is presumed that this causes the enzyme to become inactive, resulting in a deterioration in the loading effect.
[0058] FIG. 5(c) shows that in the oxidation step, O * 1 is a diagram for explaining a surface reaction of the wafer W when the flow rate of N2 gas supplied to the wafer W (the flow rate of N2 gas supplied from the process gas supply pipe 8) is high. * When the flow rate of N2 gas supplied to the wafer W is large, the O * It is presumed that the loading effect is deteriorated because the N2 gas inhibits the loading.
[0059] From the above, it can be said that adjusting the flow rate ratio of O2 gas and N2 gas is an effective method for improving the loading effect.
[0060] [Example] In Example 1, the influence on the loading effect when the pressure inside the processing vessel 2 (hereinafter also referred to as "furnace pressure") was changed in the film forming apparatus 1 was evaluated. In Example 1, a silicon oxide film was formed on each of a bare wafer and a patterned wafer under the process conditions (conditions A and B) shown in Table 1 below.
[0061] [Table 1]
[0062] In Table 1, "DIPAS" and "IP-N2(Si)" respectively indicate the flow rates of DIPAS gas and N2 gas supplied from the process gas supply pipe 9 into the process vessel 2. In Table 1, "O2" and "IP-N2(O2)" respectively indicate the flow rates of O2 gas and N2 gas supplied from the process gas supply pipe 8 into the process vessel 2. In Table 1, "RF" indicates the output of high-frequency power applied between the pair of electrodes 11 from the high-frequency power source, and "Pressure" indicates the pressure inside the furnace.
[0063] As shown in Table 1, in Condition A and Condition B, the furnace pressure in the flow process of the oxidation step was set to 55.0 Pa and 36.5 Pa, respectively, and all other conditions except for the furnace pressure were the same.
[0064] Fig. 6 is a diagram showing the evaluation results of Example 1, showing the relationship between the furnace pressure and the loading effect. In Fig. 6, the horizontal axis shows the furnace pressure [Pa] in the flow process of the oxidation step, and the vertical axis shows the loading effect [%]. The loading effect was calculated by the above-mentioned formula (1).
[0065] As shown in Fig. 6, the loading effect was 25.63% and 10.63% when the furnace pressure in the flow process of the oxidation step was set to 55.0 Pa and 36.5 Pa, respectively. This result shows that the loading effect is improved by lowering the furnace pressure.
[0066] In Example 2, the influence on the loading effect was evaluated when the flow rate of N2 gas (hereinafter referred to as "IP-N2(O2)") supplied together with O2 gas from the processing gas supply pipe 8 into the processing chamber 2 in the flow process of the oxidation step in the film forming apparatus 1 was changed. In Example 2, similar to Example 1, a silicon oxide film was formed on each of a bare wafer and a patterned wafer under the process conditions (conditions C to E) shown in Table 2 below.
[0067] [Table 2]
[0068] In Table 2, "DIPAS" and "IP-N2(Si)" respectively indicate the flow rates of DIPAS gas and N2 gas supplied from the process gas supply pipe 9 into the process vessel 2. In Table 2, "O2" and "IP-N2(O2)" respectively indicate the flow rates of O2 gas and N2 gas supplied from the process gas supply pipe 8 into the process vessel 2. In Table 2, "RF" indicates the output of high-frequency power applied between the pair of electrodes 11 from the high-frequency power source, and "Pressure" indicates the pressure inside the furnace.
[0069] As shown in Table 2, conditions C, D, and E are conditions in which the flow rate of IP-N2(O2) in the flow process of the oxidation step is set to 0.5 slm, 1 slm, and 2 slm, respectively, and all other conditions except for the flow rate of IP-N2(O2) are the same.
[0070] FIG. 7 shows the evaluation results of Example 2, where FIG. 7(a) shows the relationship between the flow rate of IP-N2 (O2) and the loading effect, and FIG. 7(b) shows the relationship between the flow rate of IP-N2 (O2) and the pressure inside the furnace. In FIG. 7(a), the horizontal axis shows the flow rate [slm] of IP-N2 (O2), and the vertical axis shows the loading effect [%]. In FIG. 7(b), the horizontal axis shows the flow rate [slm] of IP-N2 (O2), and the vertical axis shows the pressure inside the furnace in the oxidation step [Pa]. The loading effect was calculated by the above-mentioned formula (1).
[0071] As shown in Fig. 7(a), the loading effect was 9.62%, 7.43%, and 10.14% when the flow rate of IP-N2(O2) was set to 0.5 slm, 1 slm, and 2 slm, respectively. Also, as shown in Fig. 7(b), the furnace pressure was 36.27 Pa, 38.13 Pa, and 41.67 Pa when the flow rate of IP-N2(O2) was set to 0.5 slm, 1 slm, and 2 slm, respectively. This result shows that the loading effect can be improved by changing the flow rate of IP-N2(O2), even under high furnace pressure conditions.
[0072] In Example 3, in the film forming apparatus 1, the total flow rate of O2 gas and N2 gas supplied from the process gas supply pipe 8 into the process vessel 2 in the flow process of the oxidation step was fixed at 5.5 slm, and the influence on the loading effect when the ratio of O2 gas to N2 gas was changed was evaluated. In Example 3, similar to Example 1, a silicon oxide film was formed on each of a bare wafer and a patterned wafer under the process conditions (conditions F to J) shown in Table 3 below.
[0073] [Table 3]
[0074] In Table 3, "DIPAS" and "IP-N2(Si)" respectively indicate the flow rates of DIPAS gas and N2 gas supplied from the processing gas supply pipe 9 into the processing vessel 2. In Table 3, "O2" and "IP-N2(O2)" respectively indicate the flow rates of O2 gas and N2 gas supplied from the processing gas supply pipe 8 into the processing vessel 2. In Table 1, "O2:IP-N2(O2)" indicates the ratio of O2 gas and N2 gas supplied from the processing gas supply pipe 8 into the processing vessel 2. In Table 3, "RF" indicates the output of high-frequency power applied between the pair of electrodes 11 from the high-frequency power source, and "pressure" indicates the pressure inside the furnace.
[0075] As shown in Table 3, Condition F, Condition G, Condition H, Condition I, and Condition J are conditions in which the ratio of O2 gas to N2 gas supplied from the processing gas supply pipe 8 into the processing vessel 2 is set to 10:1, 5:1, 4:1, 3:1, and 2:1, respectively, and all other conditions except for the ratio are the same.
[0076] FIG. 8 is a diagram showing the evaluation results of Example 3. FIG. 8(a) shows the relationship between the ratio of O2 gas and N2 gas supplied from the processing gas supply pipe 8 into the processing vessel 2 and the loading effect, and FIG. 8(b) shows the relationship between the ratio of O2 gas and N2 gas supplied from the processing gas supply pipe 8 into the processing vessel 2 and the pressure inside the furnace. In FIG. 8(a), the horizontal axis shows the ratio of O2 gas and N2 gas supplied from the processing gas supply pipe 8 into the processing vessel 2, and the vertical axis shows the loading effect [%]. In FIG. 8(b), the horizontal axis shows the ratio of O2 gas and N2 gas supplied from the processing gas supply pipe 8 into the processing vessel 2, and the vertical axis shows the pressure inside the furnace [Pa]. The loading effect was calculated by the above-mentioned formula (1).
[0077] As shown in FIG. 8(a), the loading effect when O2:IP-N2(O2) was set to 10:1, 5:1, 4:1, 3:1, and 2:1 was 9.62%, 6.8%, 5.82%, 5.74%, and 6.47%, respectively. Also, as shown in FIG. 8(b), the furnace pressure when O2:IP-N2(O2) was set to 10:1, 5:1, 4:1, 3:1, and 2:1 was 36.27 Pa, 36.27 Pa, 36.23 Pa, 36.07 Pa, and 35.90 Pa, respectively. From this result, it was shown that the loading effect was improved without changing the furnace pressure by changing the ratio of O2 gas and N2 gas supplied from the processing gas supply pipe 8 into the processing vessel 2. Specifically, it was shown that the loading effect was improved by setting O2:IP-N2(O2) to 5:1 to 2:1. In particular, it was shown that the loading effect was particularly improved by adjusting the O2:IP-N2(O2) ratio to 3:1.
[0078] In the above embodiment, the process gas supply pipes 8 and 9 are an example of a gas supply unit, and the wafer W is an example of a substrate.
[0079] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]
[0080] 1 Film deposition equipment 2. Treatment vessel 3 Exhaust section 8. Processing gas supply pipe 9. Processing gas supply pipe 100 Control section
Claims
1. 1. A method for forming a silicon oxide film in a recess formed on a surface of a substrate in a processing chamber, comprising: (a) adsorbing a silicon-containing gas onto a substrate; (b) exposing the substrate to a plasma formed from an oxidizing gas, including oxygen gas and an inert gas, at a desired pressure; (c) repeating the steps (a) and (b); having In the step (b), a ratio of oxygen gas to an inert gas is determined based on the desired pressure and correspondence information in which a ratio of oxygen gas to an inert gas and information on a loading effect are associated with each other for each pressure in the processing vessel. Film formation method.
2. The step (b) is performed in a state where the inside of the processing vessel is vacuum pumped. The film forming method according to claim 1 .
3. The inert gas is nitrogen gas, The ratio of oxygen gas to nitrogen gas is 5:1 to 2:
1. The film forming method according to claim 1 or 2.
Citation Information
Patent Citations
Plasma processing device
JP2009038155A
Thin film forming method and apparatus, and program
JP2009206500A
Method of forming hard mask of metal oxide
JP2012142574A
Film forming method and film forming apparatus
JP2012175057A
Integrating atomic scale ald (atomic layer deposition) process and ale (atomic layer etching) process
JP2016131238A