Contact lenses having surfaces with different flexibility

A contact lens with a more flexible posterior surface, achieved by coating with outer hydrogel layers, addresses the issue of surface flexibility disparity, enhancing comfort and fit.

JP7564197B2Active Publication Date: 2024-10-08ALCON INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022520551
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-04
Filing Date
2020-11-03
Publication Date
2024-10-08
Estimated Expiration
2040-11-03

AI Technical Summary

Technical Problem

Existing contact lenses often lack sufficient flexibility differentiation between the anterior and posterior surfaces, leading to suboptimal wearing comfort.

Method used

Designing a contact lens with a posterior surface that is significantly more flexible than the anterior surface, achieved by coating the lens with outer hydrogel layers that have a higher indentation depth ratio, enhancing surface flexibility through specific reactive functional groups and cross-linking processes.

Benefits of technology

Improves wearing comfort by providing a softer posterior surface that better conforms to the eye, reducing friction and enhancing overall lens fit and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564197000056
    Figure 0007564197000056
  • Figure 0007564197000057
    Figure 0007564197000057
  • Figure 0007564197000058
    Figure 0007564197000058
Patent Text Reader

Abstract

The present invention relates to contact lenses, particularly SiHy contact lenses, comprising a lens bulk material having a posterior surface and an opposite anterior surface coated with an outer hydrogel layer. The outer hydrogel layer comprises a front outer hydrogel layer and a posterior outer hydrogel layer. The contact lenses of the present invention are characterized by a difference in surface flexibility between the posterior surface (BC) and the anterior surface (FC).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates generally to contact lenses having a lower surface modulus at their rear surface (base curve) than at their opposing front surface (front curve), and to methods of making such contact lenses. [Background technology]

[0002] In recent years, much effort has been expended to develop contact lenses which offer improved wearing comfort.

[0003] One example is the incorporation of a leachable wetting agent into a contact lens (see, e.g., U.S. Pat. Nos. 4,045,547; 4,042,552; 5,198,477; 5,219,965; 6,367,929; 6,822,016; 7,279,507; 8,030,369; and 9,804,295).

[0004] Another example is the incorporation of bioactive agents and hydrophobic comfort agents into contact lenses (see, for example, US Patent Application Publication No. 10,155,349).

[0005] Yet another example is the development of a new class of soft contact lenses, water gradient contact lenses. This new class of soft contact lenses was first developed and successfully introduced to the market as DAILIES® TOTAL1® (Alcon), a daily disposable contact lens. One-week or one-month disposable water gradient soft contact lenses have also been developed (see US Patent Application Publication No. 2019-0179055A1). This new class of soft contact lenses is characterized by having a water gradient structural configuration, with an increase in water content observed in the passage from the core to the surface of the contact lens, and reaching the highest water content in the area near and including the surface of the contact lens (see US Patent Application No. 8,480,227, which is incorporated herein by reference in its entirety). This unique design provides a lens surface that is very smooth and very soft, with a high water content, thus providing an excellent wearing experience to the patient.

[0006] Another example is creating contact lenses with a nano-textured surface that mimics the surface characteristics of the cornea of ​​the human eye (see, for example, US Pat. No. 9,244,195). Summary of the Invention [Means for solving the problem]

[0007] An object of the present invention is to provide a contact lens in which the posterior surface of the contact lens, which is in direct contact with the cornea, is much softer than the anterior surface, thereby improving the wearing comfort of the contact lens. The present invention, in one aspect, provides a soft contact lens, preferably a silicone hydrogel contact lens, having a posterior surface that is softer than its opposing anterior surface.

[0008] The present invention, in another aspect, provides a method for making such soft contact lenses, preferably such silicone hydrogel contact lenses.

[0009] This aspect and other aspects of the invention, including various preferred embodiments in any combination, will become apparent from the following description of the currently preferred embodiment. The following detailed description is merely exemplary in nature and is not intended to limit the scope of the invention as defined by the appended claims and their equivalents. As would be apparent to one skilled in the art, many variations and modifications of the invention may be implemented without departing from the spirit and scope of the novel concepts of the disclosure. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view of a structural configuration of a contact lens according to a preferred embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a lens holder for performing nanoindentation measurements on contact lenses using the Optics11 Puima nanoindentation instrument. [Diagram 3] 1 is a schematic diagram of a low coherence interferometer (LCI). [Figure 4] Shown is data collected with an LCI system with a scanning probe positioned above the lens. The x-axis is the relative position (or depth) measured as optical path distance (OPD) in microns; the y-axis is the signal intensity from the low coherence interferometer (LCI), in arbitrary units, which is proportional to the amount of back-reflected light from the surface. The peak signal at the FC plane comes before the BC plane. [Diagram 5] Shown is data collected with an LCI system with a scanning probe positioned below the lens. The x-axis is the relative position (or depth) measured as optical path distance (OPD) in microns; the y-axis is the signal intensity from the low coherence interferometer (LCI), in arbitrary units, which is proportional to the amount of back-reflected light from the surface. The peak signal at the BC plane comes before the FC plane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention belongs. In general, the nomenclature and laboratory procedures used herein are known and commonly employed by those skilled in the art. These procedures use conventional methods, such as those performed by those skilled in the art and commonly referred to in various ways. Where a term is given in the singular, the inventors also contemplate the plural form of that term. The nomenclature used herein and the laboratory procedures described below are known and commonly employed in the art.

[0012] In this application, the term "about" as used herein means that the number referred to as "about" includes the stated number plus or minus 1 to 10% of the stated number.

[0013] "Contact lens" refers to a structure that can be placed on or in the eye of a wearer. A contact lens can, but need not, correct, improve or alter the user's vision. Contact lenses can be of any suitable material known in the art or later developed, and they can be hard lenses, rigid gas permeable lenses, soft lenses or hybrid lenses.

[0014] As used herein, the terms "anterior surface," "front surface," "front curve surface," or "FC surface" in reference to a contact lens are interchangeable and refer to the surface of the contact lens that faces away from the eye during wear. The anterior surface (FC surface) is typically substantially convex.

[0015] As used herein, the terms "posterior surface", "back surface", "back curve surface" or "BC surface" in reference to a contact lens are interchangeable and refer to the surface of the contact lens that faces the eye during wear. The posterior surface (BC surface) is typically substantially concave.

[0016] "Hard contact lens" refers to a contact lens that contains a hard plastic (eg, polymethyl methacrylate) as the bulk (core) material.

[0017] "Rigid gas permeable contact lens" refers to a contact lens that includes a gas permeable material (eg, a material made from fluorosilicone acrylate) as the bulk (core) material.

[0018] Soft contact lenses can be non-silicone hydrogel contact lenses or silicone hydrogel contact lenses. "Non-silicone hydrogel contact lenses" refers to contact lenses that include a non-silicone hydrogel bulk (core) material. "Silicone hydrogel contact lenses" refers to contact lenses that include a silicone hydrogel bulk (core) material.

[0019] Hybrid contact lenses have a central optic zone made of a gas permeable lens material surrounded by a peripheral zone made of silicone hydrogel or conventional hydrogel lens material.

[0020] The embedded contact lens comprises a three-dimensional article and a lens bulk material consisting essentially of a non-silicone hydrogel material or a silicone hydrogel material, where the three-dimensional article is made of a non-hydrogel material and has a three-dimensional size smaller than that of the contact lens, whereby it is fully embedded within the non-silicone hydrogel material or the silicone hydrogel material. The non-hydrogel material can be any material that absorbs less than 10% by weight of water when fully hydrated (preferably about 7.5% by weight or less, more preferably about 5.0% by weight or less, and even more preferably about 2.5% by weight or less).

[0021] "Hydrogel" or "hydrogel material" refers to a crosslinked polymeric material that is insoluble in water but can retain at least 10 weight percent water in its three-dimensional polymer network (i.e., polymer matrix) when fully hydrated.

[0022] The term "non-silicone hydrogel" as used in this application refers to a hydrogel that does not contain silicon in theory.

[0023] The terms "silicone hydrogel" or "SiHy" used in this application are interchangeable and refer to a hydrogel containing silicone. Silicone hydrogel (SiHy) is typically obtained by copolymerization of a polymerizable composition containing at least one silicone-containing vinyl monomer, or at least one silicone-containing vinyl macromer, or at least one silicone-containing prepolymer having ethylenically unsaturated groups.

[0024] "Hydrophilic," as used herein, describes a material or portion thereof that tends to associate with water rather than with lipids.

[0025] "Vinyl monomer" refers to a compound that has one and only one ethylenically unsaturated group, is soluble in a solvent, and can be polymerized chemically or thermally.

[0026] As used in this application, the term "ethylenically unsaturated group" is used broadly herein and is intended to encompass any group that contains at least one >C=C< group. Exemplary ethylenically unsaturated groups include, but are not limited to, (meth)acryloyl [ka] , allyl, vinyl, styrenyl or other C=C containing groups.

[0027] The term "(meth)acrylamide" refers to methacrylamide and / or acrylamide.

[0028] The term "(meth)acrylate" refers to methacrylate and / or acrylate.

[0029] As used herein, "chemically" with respect to curing, crosslinking or polymerization of a polymerizable composition, prepolymer or material means that the curing (e.g., crosslinking and / or polymerization) is effected by actinic radiation, such as, for example, UV / visible radiation, ionizing radiation (e.g., gamma or X-ray radiation), microwave radiation, etc. Methods of thermal or chemical curing are well known to those skilled in the art.

[0030] As used herein, "hydrophilic vinyl monomer" refers to a vinyl monomer that, as a homopolymer, typically yields a polymer that is water soluble or capable of absorbing at least 10 weight percent water.

[0031] As used herein, "hydrophobic vinyl monomer" refers to a vinyl monomer that, as a homopolymer, typically results in a polymer that is water insoluble or can absorb less than 10 weight percent water.

[0032] "Blend vinyl monomer" refers to a vinyl monomer that is capable of dissolving both the hydrophilic and hydrophobic polymerizable components of the polymerizable composition to form a solution.

[0033] The term "acrylic monomer" refers to a vinyl-based monomer having one single (meth)acryloyl group.

[0034] "N-vinyl amide monomer" refers to an amide compound having a vinyl group (-CH=CH2) attached directly to the nitrogen atom of the amide group.

[0035] "Macromer" or "prepolymer" refers to a compound or polymer that contains ethylenically unsaturated groups and has a number average molecular weight greater than 700 Daltons.

[0036] The term "vinyl crosslinker" as used in this application refers to a compound having at least two ethylenically unsaturated groups. "Vinyl crosslinking agents" refers to a subclass of vinyl crosslinkers each having a number average molecular weight of about 700 Daltons or less.

[0037] The term "polymer" as used in this application means a material formed by polymerizing or crosslinking one or more monomers, macromers, prepolymers, and / or combinations thereof.

[0038] The term "molecular weight" of polymeric materials (including monomeric or macromeric materials) as used in this application refers to number average molecular weight, unless otherwise specified or different test conditions are indicated.

[0039] The "polysiloxane segment" is [ka] (In the formula, R1' and R2' are each a C1 to C 10 Alkyl, C1-C4 alkyl- or C1-C4 alkoxy-substituted phenyl, C1-C 10 Fluoroalkyl, C1-C 10 Fluoroethers, C6-C 18 Aryl radical, -alk-(OC2H4) γ1 -OR o (wherein alk is a C1-C6 alkyl diradical, R o is H or C1-C4 alkyl, and γ1 is an integer of 1 to 10, 40 Two substituents independently selected from the group consisting of organic radicals or linear hydrophobic polymer chains, each of which is C2-C 40 The organic radical has at least one functional group selected from the group consisting of a hydroxyl group (-OH), a carboxyl group (-COOH), -NR3'R4', an amino bond of -NR3'-, an amide bond of -CONR3'-, an amide of -CONR3'R4', a urethane bond of -OCONH-, and a C1 to C4 alkoxy group, and R3' and R4' are each independently hydrogen or a C1 to C4 alkoxy group. 15 (It is alkyl) "siloxane" refers to a polymer chain consisting of at least three consecutively and directly bonded siloxane units (divalent radicals), each independent of the other, having the formula:

[0040] "Polysiloxane vinyl monomer" refers to a compound that contains at least one polysiloxane segment and one and only one ethylenically unsaturated group.

[0041] "Polysiloxane vinyl crosslinker" refers to a compound that contains at least one polysiloxane segment and at least two ethylenically unsaturated groups.

[0042] "Chain-extended polysiloxane vinyl crosslinker" refers to a compound that contains at least two ethylenically unsaturated groups and at least two polysiloxane segments, each pair of which is linked by a divalent radical.

[0043] As used herein, the term "fluid" denotes a material that can flow like a liquid.

[0044] As used in this application, the term "transparent" with respect to a polymerizable composition means that the polymerizable composition is a clear solution or liquid mixture (i.e., has a light transmittance of 85% or greater in the range of 400-700 nm).

[0045] The term "alkyl" refers to a monovalent radical obtained by removing a hydrogen atom from a straight-chain or branched alkane compound. An alkyl group (radical) forms one bond with one other group in an organic compound.

[0046] The terms "alkylene divalent group," "alkylene diradical," or "alkyl diradical" are interchangeable and refer to a divalent radical obtained by removing one hydrogen atom from an alkyl. An alkylene divalent group forms two bonds with other groups in an organic compound.

[0047] The term "alkyl triradical" refers to a trivalent radical obtained by removing two hydrogen atoms from an alkyl. An alkyl triradical forms three bonds with other groups in an organic compound.

[0048] The terms "alkoxy" or "alkoxyl" refer to a monovalent radical obtained by removing a hydrogen atom from the hydroxyl group of a straight-chain or branched alkyl alcohol. An alkoxy group (radical) forms one bond with one other group in an organic compound.

[0049] The term "amino group" as used herein refers to a primary or secondary amino group of formula -NHR', where R', unless otherwise specified, is hydrogen or a C1-C 20 It refers to an unsubstituted or substituted straight-chain or branched alkyl group.

[0050] In this application, the term "substituted" with respect to an alkyl diradical or alkyl radical means that the alkyl diradical or alkyl radical contains at least one substituent replacing one hydrogen atom of the alkyl diradical or alkyl radical, which is selected from the group consisting of hydroxy (-OH), carboxy (-COOH), -NH2, sulfhydryl (-SH), C1-C4 alkyl, C1-C4 alkoxy, C1-C4 alkylthio (alkylsulfido), C1-C4 acylamino, C1-C4 alkylamino, di-C1-C4 alkylamino, halogen atoms (Br or Cl), and combinations thereof.

[0051] In this application, the term "poly(2-oxazoline-co-ethyleneimine)" means [ka] (In the formula, R 1 is hydrogen, methyl, ethyl, N-pyrrolidonylmethyl, N-pyrrolidonylethyl, N-pyrrolidonylpropyl or -alk-(OC2H4) m3 a monovalent radical of -OR" where alk is a C1-C4 alkyl diradical; R" is a C1-C4 alkyl (preferably methyl); m3 is an integer from 1 to 10 (preferably 1 to 5); x is an integer from 5 to 500; and z is an integer less than or equal to x. Poly(2-oxazoline-co-ethyleneimine) refers to a statistical copolymer or polymer segment thereof having the formula: Poly(2-oxazoline-co-ethyleneimine) can be obtained by hydrolysis of polyoxazoline.

[0052] In this application, the term "poly(2-oxazoline-co-ethyleneimine)-epichlorohydrin" refers to a polymer obtained by reacting poly(2-oxazoline-co-ethyleneimine) with epichlorohydrin to convert all or a significant percentage (≧90%) of the secondary amine groups of poly(2-oxazoline-co-ethyleneimine) to azetidinium groups. Examples of poly(2-oxazoline-co-ethyleneimine)-epichlorohydrin are disclosed in pending U.S. Patent Application Publication No. 2016 / 0061995A1.

[0053] "Epichlorohydrin-functionalized polyamine" or "epichlorohydrin-functionalized polyamidoamine" refers to a polymer obtained by reacting a polyamine or polyamidoamine with epichlorohydrin to convert all or a significant percentage of the secondary amine groups of the polyamine or polyamidoamine to azetidinium groups.

[0054] The term "polyamidoamine-epichlorohydrin" refers to an adipic acid-diethylenetriamine copolymer functionalized with epichlorohydrin.

[0055] In this application, the term "azetidinium" or "3-hydroxyazetidinium" means [ka] "Cationic" refers to a positively charged (i.e. cationic) divalent radical (or group or moiety) of

[0056] The term "thermally crosslinkable" with respect to a polymeric material or functional group means that the polymeric material or functional group is capable of undergoing a crosslinking reaction (or coupling reaction) with another material or functional group at relatively high temperatures (about 40°C to about 140°C), but that the polymeric material or functional group is not capable of undergoing the same crosslinking reaction (or coupling reaction) with another material or functional group to a detectable extent at a temperature of about 5°C to about 15°C in a time period of about 1 hour.

[0057] The term "phosphorylcholine" as used in this application means [ka] (wherein n is an integer of 1 to 5, and R1, R2 and R3 are each independently C1 to C8 alkyl or C1 to C8 hydroxyalkyl). This refers to a zwitterionic group.

[0058] As used herein, the term "carboxyl-containing vinyl monomer" refers to any vinyl monomer having a carboxyl group (-COOH); the term "amino-containing vinyl monomer" refers to any vinyl monomer having an amino group (-NHR').

[0059] The term "non-reactive vinyl monomer" as used in this application refers to a monomer that is a carboxyl group, a primary amino group, a secondary amino group, an epoxide group, an isocyanate group, an azlactone group ( [ka] or an aziridine group ( [ka] ) wherein p is 0 or 1; 3 R and 4 R are each independently a C1-C8 alkyl; R 1 refers to any vinyl monomer that does not contain a cyclic alkyl group (which is hydrogen, methyl, or ethyl).

[0060] A free radical initiator can be either a photoinitiator or a thermal initiator. A "photoinitiator" refers to a chemical that initiates a free radical crosslinking / polymerization reaction by using light. A "thermal initiator" refers to a chemical that initiates a radical crosslinking / polymerization reaction by using thermal energy.

[0061] The inherent "oxygen permeability" of a material, Dk i is the rate at which oxygen passes through the material. As used in this application, the term "oxygen permeability (Dk)" in reference to hydrogels (silicone or non-silicone) or contact lenses refers to the corrected oxygen permeability (Dk c ), which is measured at about 34-35°C and corrected for the surface resistance to oxygen flux caused by boundary layer effects according to the procedure described in Example 1 of U.S. Patent Application Publication No. 2012 / 0026457 A1, which is incorporated by reference in its entirety. Oxygen permeability is usually expressed in units of barrer, where "barrer" is the unit [(cm 3 oxygen)(mm) / (cm 2 )(sec)(mmHg)]×10 -10 It is defined as:

[0062] The "oxygen permeability" of a lens or material, Dk / t, is the rate at which oxygen passes through a particular lens or material of average thickness t [in mm] over the area being measured. Oxygen permeability is usually expressed in units of barrer / mm, where "barrer / mm" is the unit of [(cm 3 oxygen) / (cm 2 )(sec)(mmHg)]×10 -9 It is defined as:

[0063] As used herein, "ophthalmically compatible" refers to a material or surface of a material that can be in intimate contact with the ocular environment for extended periods of time without causing significant damage to the ocular environment and without causing significant discomfort to the user.

[0064] The term "ophthalmically safe" with respect to a packaging solution for sterilizing and storing contact lenses means that a contact lens stored in the solution is safe to be placed directly on the eye without rinsing after autoclaving, and the solution is safe and sufficiently comfortable for daily contact with the eye through a contact lens. An ophthalmically safe packaging solution after autoclaving has a tonicity and pH that is compatible with the eye, and is substantially free of eye irritants or ocular cytotoxic substances in accordance with international ISO standards and U.S. FDA regulations.

[0065] The term "moisture gradient" in reference to a contact lens means that there is an increase in water content observed passing from the core to the surface of the contact lens, reaching a highest water content in regions near and including the surface of the contact lens. It is understood that the increase in water content from the core to the surface of the contact lens can be continuous and / or stepwise, so long as the water content is highest in regions near and including the surface of the contact lens.

[0066] The term "cross section" of a contact lens as used in this application refers to a lens cross section obtained by cutting the lens with a knife or cutting tool at an angle substantially perpendicular to either the anterior or posterior surface of the lens. Those skilled in the art will be familiar with the fact that contact lenses are cut manually (i.e., cut by hand) or with a Cryosta Microtome or lathe to obtain a contact lens cross section. The resulting contact lens cross section can be polished using ion etching or similar techniques.

[0067] The term "modulus" or "elastic modulus" in relation to contact lenses or materials refers to the tensile modulus, or Young's modulus, which is a measure of the stiffness of contact lenses or materials under tension.Modulus can be measured using a method according to the ANSI Z80.20 standard.Methods for measuring the elastic modulus of silicone hydrogel materials or contact lenses are known to those skilled in the art.For example, all commercially available contact lenses have a reported elastic modulus value.

[0068] As used in this application, the term "lens bulk material" in reference to a contact lens is interchangeable and means a layer that has the three-dimensional shape of the contact lens and includes a central curved surface (which divides the contact lens into two parts, one part including the anterior surface and the other part including the posterior surface) and has a variable thickness.

[0069] As used in this application, the term "exterior hydrogel layer" in reference to a contact lens means the outermost hydrogel layer underlying the surface of the contact lens, which consists of an outer anterior hydrogel layer and an outer posterior hydrogel layer, and completely covers the lens bulk material. "Exterior anterior hydrogel layer" in reference to a contact lens means the outermost hydrogel layer underlying the anterior surface of the contact lens. "Exterior posterior hydrogel layer" in reference to a contact lens means the outermost hydrogel layer underlying the posterior surface of the contact lens. It is understood that the anterior surface is composed of the same material as the outer anterior hydrogel layer, and the posterior surface is composed of the same material as the outer posterior hydrogel layer.

[0070] As used in this application, the term "transition layer" with respect to contact lenses means a layer of polymeric material located between the inner layer (or lens bulk material) and one of the outer hydrogel layers on the anterior and posterior surfaces.

[0071] The term "surface flexibility" is used in this application to mean the apparent elastic properties of a polymer-based article (hydrogel or silicone hydrogel article) at one of its surfaces, measured by the indentation depth at a compression pressure of 5 KPa of an indentation probe with a tip radius of 9.5 μm and a stiffness of 0.54 N / m in a nanoindentation test (described in Example 1). The compression pressure of 5 kPa is used to simulate the pressure of the eyelid, typically 1-5 kPa. Depending on the flexibility of the surface, other probe tip radii or cantilever stiffnesses can be used. For stiffer materials, stiffer probes can be used.

[0072] The apparent surface hardness (i.e., surface flexibility) of a contact lens having an outer hydrogel layer on one of its two surfaces depends on the surface modulus (or Young's modulus) of the outer hydrogel layer on the core at a small depression (less than 10% of the total lens thickness). As known to those skilled in the art, the surface modulus of a hydrogel correlates with the mesh size of the hydrogel, since the mesh size of the hydrogel is proportional to the length of the crosslinked chains and inversely proportional to the crosslink density of the hydrogel (see US 2018 / 0030209). Since there is a correlation between the mesh size of a hydrogel and the equilibrium water content, the surface modulus of a hydrogel can be inversely correlated with the equilibrium water content of the hydrogel. The higher the surface modulus of a hydrogel, the lower the equilibrium water content. As a result, the greater the indentation depth at 5 kPa, the lower the modulus of the outer hydrogel layer on a contact lens at one of its surfaces.

[0073] Because the outer hydrogel layer can be much softer than the lens bulk material, the apparent surface properties (i.e., surface flexibility) of a contact lens having an outer hydrogel layer on one of its two surfaces also depend on the thickness of the outer hydrogel layer below that surface: the greater the indentation depth at 5 kPa, the thicker the outer hydrogel layer of the contact lens on one of its surfaces.

[0074] Therefore, the indentation depth at a compression pressure of 5 kPa (or any fixed compression pressure) of a contact lens at one of its surfaces can be a good indicator of both the surface modulus (or equilibrium water content) and / or the thickness of the outer hydrogel layer at that surface.

[0075] In this application, the "average thickness" of the outer anterior or posterior hydrogel layer or transition layer is referred to simply as the "outer anterior hydrogel layer thickness," "outer posterior hydrogel layer thickness," or "transition layer thickness," and is measured by AFM, environmental scanning electron microscopy, confocal fluorescence microscopy, or any technique known to one of skill in the art on a cross-section of a contact lens in an indicated state (e.g., fully hydrated or fully hydrated (i.e., in phosphate buffer solution, pH about 7.3±0.2) or dry (e.g., fully oven dried)).

[0076] FIG. 1 shows a schematic representation of a contact lens of the present invention according to a preferred embodiment. According to this preferred embodiment of the present invention, the contact lens 100 has a front surface (or front curve or convex surface) 101 and an opposing rear surface (or back curve or concave surface) 102 that rests on the cornea of ​​the eye when worn by a user. The contact lens 100 comprises a lens bulk material 110, an outer front hydrogel layer 121 and an outer rear hydrogel layer 122. The lens bulk material 110 has a three-dimensional shape that closely resembles the contact lens 100. The outer anterior and rear hydrogel layers 120 are made of a substantially silicone-free (preferably completely silicone-free) hydrogel material that has a high water content compared to the water content of the inner layer 110. The outer anterior and rear hydrogel layers 120 are fused at the periphery 103 of the contact lens 100 and completely cover the inner layer 110.

[0077] As used in this application, the term "equilibrium water content" in reference to a contact lens or polymer-based material means the amount of water (expressed as a weight percent) present in a contact lens or polymer-based material when fully hydrated (equilibrated) in phosphate buffered saline (about 0.79 wt % NaCl) measured at room temperature (as defined above).

[0078] As used in this application, the terms "crosslinked coating" or "hydrogel coating" or "hydrogel layer" on a contact lens are interchangeable and are used to describe a crosslinked polymer-based material having a three-dimensional network that can contain water when fully hydrated. The three-dimensional network of the crosslinked polymer-based material can be formed by the crosslinking of two or more linear or branched polymers via crosslinks.

[0079] As used herein, "surface modification" or "surface treatment" means that, before or after formation of the article, the article has been treated with a surface treatment process (or surface modification process) in which (1) a coating is provided on the surface of the article, (2) chemical species are adsorbed or covalently attached onto the surface of the article, (3) the chemical nature (e.g., electrostatic charge) of chemical groups on the surface of the article is altered, or (4) the surface properties of the article are otherwise altered. Exemplary surface treatment processes include, but are not limited to, surface treatment with energy (e.g., plasma, electrostatic charge, irradiation or other energy sources), chemical treatment, grafting of hydrophilic vinyl monomers or macromers onto the surface of the article, mold transfer coating as disclosed in U.S. Pat. No. 6,719,929, incorporation of wetting agents into lens formulations to make contact lenses as proposed in U.S. Pat. Nos. 6,367,929 and 6,822,016, reinforced mold transfer coating as disclosed in U.S. Pat. No. 7,858,000, and hydrophilic coating by covalent bonding or physical deposition of one or more layers of one or more hydrophilic polymers onto the contact lens surface as disclosed in U.S. Pat. Nos. 8,147,897 and 8,409,599, and U.S. Patent Publication Nos. 2011 / 0134387, 2012 / 0026457, and 2013 / 0118127.

[0080] The present invention relates generally to contact lenses, and in particular to SiHy contact lenses, which are characterized by a difference in surface flexibility between their posterior (BC) and anterior (FC) surfaces. The posterior surface of the contact lens of the present invention is in direct contact with the cornea and is much softer than the anterior surface, which has a greater impact on the wearing comfort.

[0081] In one aspect, the present invention provides a contact lens comprising a lens bulk material coated with an exterior hydrogel layer and having a posterior surface and an opposing anterior surface, the exterior hydrogel layer being comprised of a front outer hydrogel layer and a posterior outer hydrogel layer, the posterior outer hydrogel layer having an indentation depth ratio of at least about 1.2 (preferably at least about 1.3, more preferably at least about 1.4, even more preferably at least about 1.5, and most preferably at least about 1.6).

number

[0082] In another aspect, the invention provides a method of making a coated contact lens, the method comprising the steps of: (1) obtaining a contact lens precursor having a concave surface and an opposing convex surface and comprising lens bulk material and first reactive functional groups on and / or adjacent to anterior and posterior surfaces, the first reactive functional groups being selected from the group consisting of carboxyl groups, amino groups, azetidinium groups, epoxide groups, aziridine groups, vinylsulfone groups, thiol groups and combinations thereof, preferably from the group consisting of carboxyl groups, amino groups, azetidinium groups, epoxide groups, vinylsulfone groups, thiol groups and combinations thereof, more preferably from the group consisting of carboxyl groups, amino groups, azetidinium groups and combinations thereof, and even more preferably from the group consisting of carboxyl groups, amino groups, azetidinium groups and combinations thereof; (2) placing the contact lens precursor in a container in a position to ensure that the concave surface of the contact lens precursor faces up while the convex surface faces down; (3) applying a coating of the contact lens precursor to the contact lens precursor while maintaining the concave surface facing up. dispensing an aqueous solution onto the concave surface of the contact lens precursor in a container in an amount to completely immerse the lens precursor in the aqueous solution, the aqueous solution having a room temperature and comprising at least one hydrophilic polymeric material, each of the at least one hydrophilic polymeric material comprising a second reactive functional group capable of reacting with one of the first reactive functional groups to form a covalent bond at a temperature higher than room temperature, the second reactive functional group being selected from the group consisting of a carboxyl group, an amino group, an azetidinium group, an epoxide group, an aziridine group, a thiol group and combinations thereof (preferably from the group consisting of a carboxyl group, an amino group, an azetidinium group, an epoxide group, a thiol group and combinations thereof, more preferably from the group consisting of a carboxyl group, an amino group, an azetidinium group and combinations thereof); and (4) raising the temperature of the aqueous solution having the contact lens precursor therein to a temperature of about 35° C. to about 140° C. to form a coated contact lens, which is a contact lens of the present invention as described in the previous aspect of the present invention.

[0083] According to all the various aspects of the present invention, the lens bulk material of the contact lens of the present invention can be obtained directly from a preformed contact lens. A preformed contact lens can be any contact lens that has not undergone surface treatment after being manufactured according to any lens manufacturing process, or any contact lens that has undergone plasma treatment or chemical or physical surface modification treatment, or any commercially available contact lens as long as there is no hydrogel coating on the surface of the preformed contact lens. Those skilled in the art are very familiar with how to make a preformed contact lens. Those skilled in the art are very familiar with how to make a preformed contact lens. For example, a preformed contact lens can be manufactured in a conventional "spin casting mold" as described in, for example, U.S. Pat. No. 3,408,429, or by a complete cast molding process in static form as described in U.S. Pat. Nos. 4,347,198; 5,508,317; 5,583,463; 5,789,464; and 5,849,810, or by lathe cutting of a button of polymer-based material as used to make customized contact lenses. In casting, a polymerizable composition (ie, lens formulation) is typically dispensed into a mold and cured (ie, polymerized and / or crosslinked) in the mold to produce a contact lens.

[0084] Lens molds for making contact lenses are well known to those skilled in the art and are used, for example, for casting or spin casting. For example, a mold (for casting) usually includes at least two mold pieces (or parts) or mold halves, namely a first and a second mold half. The first mold half defines a first molding (or optical) surface, and the second mold half defines a second molding (or optical) surface. The first and second mold halves are configured to receive each other such that a lens-forming cavity is formed between the first and second molding surfaces. The molding surface of the mold half is the cavity-forming surface of the mold and is in direct contact with the polymerizable composition.

[0085] The method of manufacturing mold pieces for mold casting contact lenses is generally known to those skilled in the art. The method of the present invention is not limited to a specific method of forming a mold. In fact, any method of forming a mold can be used in the present invention. The first and second mold halves can be formed by various techniques, such as injection molding or lathing. Examples of suitable processes for forming mold halves are described in U.S. Patent Nos. 4,444,711; 4,460,534; 5,843,346; and 5,894,002.

[0086] To make the mold for making contact lenses, virtually all materials known in the art for making molds can be used.For example, polymer-based materials such as polyethylene, polypropylene, polystyrene, PMMA, Topas® COC grade 8007-S10 (transparent amorphous copolymer of ethylene and norbornene, Ticona GmbH, Frankfurt, Germany and Summit, New Jersey) can be used.Other materials that allow UV light to pass through can also be used, such as quartz glass and sapphire.

[0087] In a preferred embodiment, a reusable mold is used and the lens-forming composition is chemically cured under the spatial confinement of actinic radiation to form a contact lens. Examples of preferred reusable molds are those disclosed in U.S. Patent Nos. 6,627,124, 6,800,225, 7,384,590 and 7,387,759. Reusable molds can be made of quartz, glass, sapphire, CaF2, cyclic olefin copolymers (e.g., Topas® COC grade 8007-S10 (a transparent amorphous copolymer of ethylene and norbornene) from Ticona GmbH, Frankfurt, Germany and Summit, New Jersey, Zeonex® and Zeonor® from Zeon Chemicals LP, Louisville, KY), polymethyl methacrylate (PMMA), polyoxymethylene from DuPont (Delrin), Ultem® (polyetherimide) from GE Plastics, PrimoSpire®, and the like.

[0088] According to the present invention, the polymerizable composition can be introduced (dispensed) into the cavity formed by the mold according to any known method.

[0089] After the polymerizable composition is dispensed into the mold, it is polymerized to produce a contact lens. Crosslinking can be initiated thermally or chemically, preferably by exposing the polymerizable composition in the mold to spatially confined actinic radiation to crosslink the polymerizable components in the polymerizable composition.

[0090] Opening the mould so that the moulded article can be removed from it can be effected in a manner known per se.

[0091] To remove unpolymerized polymerizable components, molded contact lenses can be subjected to lens extraction. The extraction solvent can be any solvent known to those skilled in the art. Examples of suitable extraction solvents are those described below.

[0092] In a preferred embodiment, the preformed contact lens is a hard contact lens that includes a hard plastic material as the lens bulk material. Preferably, the hard plastic material is crosslinked polymethyl acrylate. Those skilled in the art are familiar with methods for making hard plastic materials such as crosslinked polymethyl methacrylate.

[0093] In another preferred embodiment, the preformed contact lens is a rigid gas permeable contact lens. Those skilled in the art know how to make rigid gas permeable lenses.

[0094] In another preferred embodiment, the preformed contact lens is a hybrid contact lens having a central optic zone made of a rigid gas permeable lens material and surrounded by a peripheral zone made of a hydrogel material.

[0095] In another preferred embodiment, the preformed contact lenses are non-silicone hydrogel contact lenses (or so-called conventional hydrogel contact lenses).

[0096] The preformed non-silicone hydrogel contact lenses may be any commercially available non-silicone hydrogel contact lens or may be manufactured according to any known method. For example, in the manufacture of preformed non-silicone hydrogel contact lenses, the non-silicone hydrogel lens formulation for making the rods used in cast or spin cast molding or lathe cutting of the contact lenses is typically one of the following: (1) (a) at least one hydrophilic vinyl monomer (e.g., hydroxyethyl methacrylate, glycerol methacrylate, N-vinylpyrrolidone or combinations thereof) and (b) a crosslinking agent, a hydrophobic vinyl monomer, a lubricant (or a so-called internal wetting agent that is incorporated into the lens formulation), a free radical initiator (photoinitiator or thermal initiator), a UV absorbing vinyl monomer, a high energy violet light ("HEVL") absorbing vinyl monomer, a visibility colorant (e.g., or (2) an aqueous solution comprising one or more water-soluble prepolymers and at least one component selected from the group consisting of hydrophilic vinyl monomers, crosslinkers, hydrophobic vinyl monomers, lubricants (or so-called internal wetting agents that are incorporated into the lens formulation), free radical initiators (photoinitiators or thermal initiators), UV absorbing vinyl monomers, HEVL absorbing vinyl monomers, visibility colorants (e.g., reactive dyes, polymerizable dyes, pigments or mixtures thereof), antimicrobial agents (e.g., preferably silver nanoparticles), bioactive agents, and combinations thereof. The resulting preformed hydrogel contact lens may then be extracted with an extraction solvent to remove unpolymerized components from the resulting lens and subjected to a hydration process, as known to those skilled in the art. It is understood that the lubricant present in a hydrogel lens formulation can improve the lubricity of a preformed hydrogel contact lens compared to the lubricity of a control preformed hydrogel contact lens obtained from a control hydrogel lens formulation without the lubricant.

[0097] Preferred examples of water-soluble prepolymers include, but are not limited to, the water-soluble crosslinkable poly(vinyl alcohol) prepolymers described in US Pat. Nos. 5,583,163 and 6,303,687.

[0098] Numerous non-silicone hydrogel lens formulations have been described in numerous patents and patent applications published up to the filing date of this application and have been used to manufacture commercially available non-silicone hydrogel contact lenses. Examples of commercially available non-silicone hydrogel contact lenses include, but are not limited to, alphafilcon A, acofilcon A, deltafilcon A, etafilcon A, focofilcon A, herfilcon A, herfilcon B, hilafilcon B, hyoxifilcon A, hyoxifilcon B, hyoxifilcon D, metafilcon A, metafilcon B, nelfilcon A, nesofilcon A, ocfilcon A, ocfilcon B, ocfilcon C, ocfilcon D, omafilcon A, femfilcon A, polymacon, sanfilcon A, terfilcon A, tetrafilcon A, and bifilcon A.

[0099] In a preferred embodiment, the inner layer is comprised of a non-silicone hydrogel material that comprises at least 50 mole % of repeat units of at least one hydroxyl-containing vinyl monomer selected from the group consisting of hydroxyethyl (meth)acrylate, glycerol (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-amino-2-hydroxypropyl (meth)acrylate, N-2-hydroxyethyl (meth)acrylamide, N-3-hydroxypropyl (meth)acrylamide, N-2-hydroxypropyl (meth)acrylamide, N-2,3-dihydroxypropyl (meth)acrylamide, N-tris(hydroxymethyl)methyl (meth)acrylamide, vinyl alcohol, allyl alcohol, and combinations thereof, more preferably selected from the group consisting of hydroxyethyl (meth)acrylate, glycerol (meth)acrylate, and vinyl alcohol. The mole percentage of repeat units can be calculated based on the non-silicone hydrogel lens formulation for making the non-silicone hydrogel contact lens.

[0100] In another preferred embodiment, the preformed contact lenses are silicone hydrogel contact lenses.

[0101] The preformed silicone hydrogel contact lens can be any commercially available silicone hydrogel contact lens or can be manufactured according to any known method. For example, in the manufacture of preformed silicone hydrogel (SiHy) contact lenses, the SiHy lens formulation for making the SiHy rod used for cast molding or spin casting molding or lathe cutting of contact lenses usually contains at least one component selected from the group consisting of silicone-containing vinyl monomers, polysiloxane vinyl-based crosslinkers, silicone-containing prepolymers, hydrophilic vinyl monomers, hydrophobic vinyl monomers, non-silicone vinyl-based crosslinkers, free radical initiators (photoinitiators or thermal initiators), silicone-containing prepolymers, and combinations thereof, as known to those skilled in the art. The resulting preformed SiHy contact lens can then be extracted with an extraction solvent to remove unpolymerized components from the resulting lens and subjected to a hydration process, as known to those skilled in the art. In addition, the preformed SiHy contact lens can be a colored contact lens (i.e., a SiHy contact lens with at least one colored pattern printed thereon, as known to those skilled in the art).

[0102] According to the present invention, silicone-containing vinyl monomer can be any silicone-containing vinyl monomer known to those skilled in the art.The preferred silicone-containing vinyl monomer examples include but are not limited to the vinyl monomers having bis(trialkylsilyloxy) alkylsilyl group or tris(trialkylsilyloxy) silyl group, polysiloxane vinyl monomer, 3-methacryloxypropyl pentamethyldisiloxane, t-butyldimethyl-siloxyethyl vinyl carbonate, trimethylsilylethyl vinyl carbonate and trimethylsilylmethyl vinyl carbonate, and their combinations.

[0103] Preferred polysiloxane vinyl monomers, including those of formula (M1), are described later in this application and can be obtained from commercial sources (e.g., Shin-Etsu, Gelest, etc.) and can be prepared, for example, according to the procedures described in U.S. Pat. Nos. 5,070,215, 6,166,236, 6,867,245, 8,415,405, 8,475,529, 8,614,261 and 9,217,813; They can be prepared by reacting ethylene glycol with monoepoxypropyloxypropyl terminated polydimethylsiloxane; by reacting glycidyl (meth)acrylate with monocarbinol terminated polydimethylsiloxane, monoaminopropyl terminated polydimethylsiloxane or monoethylaminopropyl terminated polydimethylsiloxane; or by reacting isocyanatoethyl (meth)acrylate with monocarbinol terminated polydimethylsiloxane according to coupling reactions well known to those skilled in the art.

[0104] Preferred silicone-containing vinyl monomers having bis(trialkylsilyloxy)alkylsilyl or tris(trialkylsilyloxy)silyl groups, respectively, including those of formula (M2), are described later in this application and can be obtained from commercial sources (e.g., Shin-Etsu, Gelest, etc.) and can be prepared according to the procedures described, for example, in U.S. Pat. Nos. 5,070,215, 6,166,236, 7,214,809, 8,475,529, 8,658,748, 9,097,840, 9,103,965, and 9,475,827.

[0105] Any suitable polysiloxane vinyl crosslinker can be used in the present invention. Examples of preferred polysiloxane vinyl crosslinkers include di-(meth)acryloyl-terminated polydimethylsiloxane; divinyl carbonate-terminated polydimethylsiloxane; divinyl carbamate-terminated polydimethylsiloxane; N,N,N',N'-tetrakis(3-methacryloxy-2-hydroxypropyl)-alpha,omega-bis-3-aminopropyl-polydimethylsiloxane; Macromer A, Macromer B, and Macromer C, as described in U.S. Pat. No. 5,760,100. Polysiloxane-containing macromers selected from the group consisting of Macromer C and Macromer D; U.S. Pat. Nos. 4,136,250, 4,153,641, 4,182,822, 4,189,546, 4,343,927, 4,254,248, 4,355,147, 4,276,402, 4,327,203, 4,341,889, 4,486,577, and 4,543,398; Specification, Specification No. 4605712, Specification No. 4661575, Specification No. 4684538, Specification No. 4703097, Specification No. 4833218, Specification No. 4837289, Specification No. 4954586, Specification No. 4 Specification No. 954587, Specification No. 5010141, Specification No. 5034461, Specification No. 5070170, Specification No. 5079319, Specification No. 5039761, Specification No. 5346946, Specification No. 5358995. the polysiloxane-containing macromers disclosed in U.S. Pat. Nos. 5,387,632, 5,416,132, 5,451,617, 5,486,579, 5,962,548, 5,981,675, 6,039,913, and 6,762,264; the polysiloxane-containing macromers disclosed in U.S. Pat. Nos. 4,259,467, 4,260,725, and 4,261,875.

[0106] One class of preferred polysiloxane vinyl crosslinkers is a polysiloxane having dimethylsiloxane units and one monovalent C4-C siloxane with one methyl substituent and two to six hydroxyl groups. 40and hydrophilized siloxane units each having an organic radical substituent, more preferably a polysiloxane vinyl crosslinker of formula (I), which are described later in this application and may be prepared according to the procedures disclosed in U.S. Pat. No. 1,008,1697.

[0107] Another class of preferred polysiloxane vinyl crosslinkers is the vinyl crosslinker of formula (1), which is described later in this application and is available from commercial sources; and can be prepared by reacting glycidyl (meth)acrylate (meth)acryloyl chloride with diamino-terminated polydimethylsiloxane or dihydroxyl-terminated polydimethylsiloxane; can be prepared by reacting isocyanatoethyl (meth)acrylate with dihydroxyl-terminated polydimethylsiloxane, can be prepared by reacting an amino-containing acrylic monomer with a dicarboxyl-terminated polydimethylsiloxane in the presence of a coupling agent (carbodiimide); can be prepared by reacting a carboxyl-containing acrylic monomer with a diamino-terminated polydimethylsiloxane in the presence of a coupling agent (carbodiimide); or can be prepared by reacting a hydroxyl-containing acrylic monomer with a dihydroxyl-terminated polydisiloxane in the presence of a diisocyanate or diepoxy coupling agent.

[0108] Another class of preferred polysiloxane vinyl crosslinkers is the chain extended polysiloxane vinyl crosslinker of any one of formulas (2)-(7), which are described later in this application and can be prepared according to the procedures described in U.S. Pat. Nos. 5,034,461, 5,416,132, 5,449,729, 5,760,100, 7,423,074, 8,529,057, 8,835,525, 8,993,651 and 10,301,451 and U.S. Patent Publication No. 2018-0100038 A1.

[0109] Any hydrophilic vinyl monomer can be used in the present invention. Examples of preferred hydrophilic vinyl monomers are alkyl(meth)acrylamides (described later in this application), hydroxyl-containing acrylic monomers (described later in this application), amino-containing acrylic monomers (described later in this application), carboxyl-containing acrylic monomers (described later in this application), N-vinylamide monomers (described later in this application), methylene-containing pyrrolidone monomers (i.e. pyrrolidone derivatives having a methylene group linked to the pyrrolidone ring at the 3- or 5-position, respectively) (described later in this application), acrylic monomers having C1-C4 alkoxyethoxy groups (described later in this application), vinyl ether monomers (described later in this application), allyl ether monomers (described later in this application), phosphorylcholine-containing vinyl monomers (described later in this application), N-2-hydroxyethyl vinyl carbamate, N-carboxyvinyl-β-alanine (VINAL), N-carboxyvinyl-α-alanine, and combinations thereof.

[0110] According to the present invention, any hydrophobic vinyl monomer can be included in the present invention.Preferred examples of hydrophobic vinyl monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, styrene, chloroprene, vinyl chloride, vinylidene chloride, (meth)acrylonitrile, 1-butene, butadiene, vinyl toluene, vinyl ethyl ether, perfluorohexylethyl-thio-carbonyl-aminoethyl-methacrylate, isobornyl (meth)acrylate, trifluoroethyl (meth)acrylate, hexafluoroisopropyl (meth)acrylate, hexafluorobutyl (meth)acrylate and combinations thereof.

[0111] According to the present invention, any non-silicone vinyl crosslinker can be included in the present invention. Examples of preferred non-silicone vinyl crosslinkers are described later in this application.

[0112] Any thermal polymerization initiator can be used in the present invention. Suitable thermal polymerization initiators are known to those skilled in the art and include, for example, peroxides, hydroperoxides, azo-bis(alkyl- or cycloalkylnitriles), persulfates, percarbonates, or mixtures thereof.Examples of suitable thermal polymerization initiators include, but are not limited to, benzoyl peroxide, t-butyl peroxide, t-amyl peroxybenzoate, 2,2-bis(tert-butylperoxy)butane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane, 2,5-bis(tert-butylperoxy)-2,5-dimethyl-3-hexyne, bis(1-(tert-butylperoxy)-1-methylethyl)-1,2-bis(tert-butylperoxy ... tert-butyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, di-t-butyl-dipyroxyphthalate, t-butyl hydroperoxide, t-butyl peracetate, t-butyl peroxybenzoate, t-butyl peroxyisopropyl carbonate, acetyl peroxide, lauroyl peroxide, decanoyl peroxide, dicetyl peroxydicarbonate, di(4-t-butylcyclohexyl) peroxydicarbonate (Perkadox 16S), di(2-ethylhexyl) peroxydicarbonate, t-butyl peroxypivalate (Lupersol 11); t-butyl peroxy-2-ethylhexanoate (Trigonox 21-C50), 2,4-pentanedione peroxide, dicumyl peroxide, peracetic acid, potassium persulfate, sodium persulfate, ammonium persulfate, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (VAZO33), 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (VAZO44), 2,2'-azobis(2-amidinopropane) dihydrochloride (VAZO50), 2,2'-azobis(2,4-dimethyl VAZO52), 2,2'-azobis(isobutyronitrile) (VAZO64 or AIBN), 2,2'-azobis-2-methylbutyronitrile (VAZO67), 1,1-azobis(1-cyclohexanecarbonitrile) (VAZO88); 2,2'-azobis(2-cyclopropylpropionitrile), 2,2'-azobis(methylisobutyrate), 4,4'-azobis(4-cyanovaleric acid) and combinations thereof.Preferably, the thermal initiator is 2,2'-azobis(isobutyronitrile) (AIBN or VAZO64).

[0113] Suitable photoinitiators are benzoin methyl ether, diethoxyacetophenone, benzoylphosphine oxide, 1-hydroxycyclohexylphenyl ketone and Darocur and Irgacur types, preferably Darocur 1173® and Darocur 2959®, germanium-based Norrish Type I photoinitiators (e.g., those described in U.S. Pat. No. 7,605,190). Examples of benzoylphosphine initiators include 2,4,6-trimethylbenzoyldiphenylphosphine oxide; bis-(2,6-dichlorobenzoyl)-4-N-propylphenylphosphine oxide; and bis-(2,6-dichlorobenzoyl)-4-N-butylphenylphosphine oxide. Reactive photoinitiators that can be incorporated into macromers or used as special monomers are also suitable. Examples of reactive photoinitiators are those disclosed in EP 632329.

[0114] The SiHy contact lens formulations may also include other necessary ingredients known to those of skill in the art, such as, for example, UV absorbing vinyl monomers, HEVL absorbing vinyl monomers, visibility colorants (e.g., reactive dyes, polymerizable dyes, pigments, or mixtures thereof known to those of skill in the art), antimicrobial agents (e.g., preferably silver nanoparticles), bioactive agents, leachable lubricants (e.g., non-polymerizable hydrophilic polymers, etc.), leachable tear stabilizing agents (e.g., phospholipids, monoglycerides, diglycerides, triglycerides, glycolipids, glyceroglycolipids, sphingolipids, sphingoglycolipids, etc.), and mixtures thereof.

[0115] The polymerizable composition (SiHy lens formulation), as known to those skilled in the art, may be a solvent-free clear liquid prepared by mixing all of the polymerizable components with other necessary ingredients, or it may be a solution prepared by dissolving all of the desired components in any suitable solvent, such as a mixture of water and one or more water-miscible solvents, an organic solvent, or a mixture of one or more organic solvents. The term "solvent" refers to a chemical that cannot participate in a free radical polymerization reaction.

[0116] Solventless lens SiHy lens formulations typically include at least one blend vinyl monomer as a reactive solvent to dissolve all other polymerizable components of the solventless SiHy lens formulation. Examples of preferred blend vinyl monomers are described later in this application. Preferably, methyl methacrylate is used as the blend vinyl monomer in the preparation of the solventless SiHy lens formulation.

[0117] In the present invention, any solvent can be used. Examples of preferred organic solvents include, but are not limited to, tetrahydrofuran, tripropylene glycol methyl ether, dipropylene glycol methyl ether, ethylene glycol n-butyl ether, ketones (e.g., acetone, methyl ethyl ketone, etc.), diethylene glycol n-butyl ether, diethylene glycol methyl ether, ethylene glycol phenyl ether, propylene glycol methyl ether, propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol n-propyl ether, dipropylene glycol n-propyl ether, tripropylene glycol n-butyl ether, propylene glycol n-butyl ether, dipropylene glycol n-butyl ether, tripropylene glycol n-butyl ether, ... glycol phenyl ether, dipropylene glycol dimethyl ether, polyethylene glycol, polypropylene glycol, ethyl acetate, butyl acetate, amyl acetate, methyl lactate, ethyl lactate, i-propyl lactate, methylene chloride, 2-butanol, 1-propanol, 2-propanol, menthol, cyclohexanol, cyclopentanol and exonorborneol, 2-pentanol, 3-pentanol, 2-hexanol, 3-hexanol, 3-methyl-2-butanol, 2-heptanol, 2-octanol, 2-nonanol, 2-decanol, 3-octanol, norborneol, tert-butanol, tert-amyl alcohol, 2-methyl-2-pentanol, 2,3-dimethyl-2-butanol, 3-methyl-3-pentanol, 1-methylcyclohexanol, 2-methyl-2-hexanol, 3,7-Dimethyl-3-octanol, 1-chloro-2-methyl-2-propanol, 2-methyl-2-heptanol, 2-methyl-2-octanol, 2-2-methyl-2-nonanol, 2-methyl-2-decanol, 3-methyl-3-hexanol, 3-methyl-3-heptanol, 4-methyl-4-heptanol, 3-methyl-3-octanol, 4-methyl-4-octanol, 3-methyl-3-nonanol, 4-methyl-4-nonanol, 3-methyl-3-octanol, 3-ethyl-3-hexanol, 3-methyl-3-heptanol, 4-ethyl-4-heptanol, 4-propyl-4-heptanol, 4-isopropyl-4-heptanol, 2,4-dimethyl-2-pentanol, 1-methylcyclopentanol, Examples of suitable cyclopentanol include ethanol, 1-ethylcyclopentanol, 1-ethylcyclopentanol, 3-hydroxy-3-methyl-1-butene, 4-hydroxy-4-methyl-1-cyclopentanol, 2-phenyl-2-propanol, 2-methoxy-2-methyl-2-propanol, 2,3,4-trimethyl-3-pentanol, 3,7-dimethyl-3-octanol, 2-phenyl-2-butanol, 2-methyl-1-phenyl-2-propanol and 3-ethyl-3-pentanol, 1-ethoxy-2-propanol, 1-methyl-2-pyrrolidone, N,N-dimethylpropionamide, dimethylformamide, dimethylacetamide, dimethylpropionamide, N-methylpyrrolidone and mixtures thereof.

[0118] Numerous SiHy lens formulations have been described in numerous patents and patent applications published up to the filing date of this application and have been used in the manufacture of commercially available SiHy contact lenses. Examples of commercially available SiHy contact lenses include, but are not limited to, asmofilcon A, balafilcon A, confilcon A, delefilcon A, eflofilcon A, enfilcon A, funfilcon A, galyfilcon A, lotrafilcon A, lotrafilcon B, narafilcon A, narafilcon B, senofilcon A, senofilcon B, senofilcon C, sumafilcon A, somofilcon A, and stenfilcon A.

[0119] The SiHy lens formulation (ie, the polymerizable composition) can be thermally or chemically cured (polymerized), preferably in a mold for casting the contact lens, as known to those skilled in the art.

[0120] The thermal polymerization is conveniently carried out at a temperature of, for example, 25 to 120° C., preferably 40 to 100° C. The reaction time may vary within a wide range, but is conveniently, for example, 1 to 24 hours, or preferably 2 to 12 hours. It is advantageous to previously degas the components and solvents used in the polymerization reaction and to carry out the copolymerization reaction under an inert atmosphere, for example under an atmosphere of nitrogen or argon.

[0121] Actinic polymerization can then be induced by actinic radiation, such as light, especially UV or visible light of suitable wavelengths. If necessary, suitable photosensitizers can be added to provide appropriate control of the spectral requirements.

[0122] In accordance with the present invention, the lens formulation can be introduced (dispensed) into the cavity formed by the mold according to any known method.

[0123] After the lens formulation is dispensed into the mold, it is polymerized to produce a contact lens. Polymerization can be initiated thermally or chemically, preferably by exposing the lens formulation in the mold to spatially confined actinic radiation to crosslink polymerizable components in the lens formulation.

[0124] Opening the mould so that the moulded article can be removed from it can be effected in a manner known per se.

[0125] To remove unpolymerized polymerizable components, the molded contact lenses can be subjected to lens extraction. The extraction solvent can be any solvent known to those skilled in the art. Examples of suitable extraction solvents are described above.

[0126] According to the present invention, the silicone hydrogel material of the lens bulk material has an oxygen permeability of about 50 barrer (preferably about 60, more preferably about 70, even more preferably about 90 barrer, and most preferably at least about 100 barrer) to about 180 barrer. The silicone hydrogel material can also have an equilibrium water content of about 10% by weight (preferably about 20% by weight, more preferably about 30% by weight; even more preferably about 40% by weight) to about 80% by weight. The silicone hydrogel material can further have a bulk modulus (i.e., bulk Young's modulus) of about 0.3 MPa to about 1.8 MPa, preferably 0.4 MPa to about 1.5 MPa, and more preferably about 0.4 MPa to about 1.2 MPa. The oxygen permeability, elastic modulus, and water content of the silicone hydrogel material of the contact lens of the present invention can be determined by measuring the oxygen permeability, elastic modulus, and water content of a preformed contact lens. Those skilled in the art are familiar with methods for determining the elastic modulus and equilibrium water content of a silicone hydrogel material or a SiHy contact lens. For example, oxygen permeability, modulus and water content values ​​are reported for all commercially available SiHy contact lenses.

[0127] The outer posterior hydrogel layer of the present contact lenses is preferably thicker than the outer anterior hydrogel layer, with the ratio of the thickness of the outer posterior hydrogel layer to the outer anterior hydrogel layer being at least about 1.2, preferably at least about 1.3, more preferably at least about 1.4, and even more preferably at least about 1.5.

[0128] In various preferred embodiments, the separate outer front and back hydrogel layers and the outer hydrogel layer are crosslinked polymer-based materials that include a variety of different polymer chains having different compositions, as described later in this application.

[0129] According to a preferred embodiment, the outer anterior and posterior hydrogel layers of the present contact lenses, independent of one another, comprise an equilibrium water content of at least 80% by weight, preferably at least 85% by weight, more preferably at least about 90% by weight, and even more preferably at least 95% by weight.

[0130] According to the present invention, each of the outer front and rear hydrogel layers is substantially free of silicone, preferably completely free of silicone. However, confirmation of the presence or absence of silicon in the outer hydrogel layers using X-ray photoelectron spectroscopy (XPS) (typically at a probing depth of 1.5-6 Nm) shows that silicon is present in, for example, Goodfellow's polyethylene sheet (1.3±0.2%) and Alcon's DAILIES® AquaComfortPlus TM It is well known that samples are inevitably contaminated by environmental silicon, as shown by the detection of silicon by XPS on the surface of samples that are theoretically free of any silicon atoms, such as contact lenses (1.7±0.9%) or Johnson & Johnson's ACUVUE® Moist (2.8±0.9%). Therefore, the outer hydrogel layer of each of the SiHy contact lenses of the present invention is substantially silicon-free, as characterized by having a silicon atomic percentage of less than about 5%, preferably less than about 4%, and more preferably less than about 3% of the total elemental percentage, as measured by XPS analysis of the contact lens in the dry state.

[0131] The composition of the layered structure of the contact lenses of the present invention can be revealed by analysis of cross-sections of contact lenses in a fully hydrated state (i.e., directly in water or in buffered saline) by atomic force microscopy (AFM), environmental scanning electron microscopy, confocal fluorescence microscopy, or any other known technique, as known to those skilled in the art.

[0132] In any one of the above-described preferred embodiments of the various aspects of the present invention, the contact lenses of the present invention have a UVB transmittance of about 10% or less (preferably about 5% or less, more preferably about 2.5% or less, and even more preferably about 1% or less) at 280 to 315 nanometers, a UVA transmittance of about 30% or less (preferably about 20% or less, more preferably about 10% or less, and even more preferably about 5% or less) at 315 to 380 nanometers, and an ultraviolet transmittance of 0% to about 70%, preferably 5% to about 60%, more preferably 5% to about 50%, and even more preferably about 5% to about 40% at 380 to 440 nanometers.

[0133] The contact lenses of the present invention may be obtained according to any method known or to be developed by those skilled in the art.

[0134] In accordance with the present invention, a contact lens precursor is a preformed contact lens that naturally contains or has been modified to contain first reactive functional groups on and / or near its surface.

[0135] If the preformed contact lens originally contains a first reactive functional group on and / or near its surface, it can be obtained by polymerizing a polymerizable composition (i.e., a non-silicone hydrogel lens formulation or a silicone hydrogel lens formulation) containing a vinyl monomer, which further contains at least one first reactive functional group selected from the group consisting of, for example, a carboxyl group, an amino group, an azetidinium group, an epoxide group, an aziridine group, and combinations thereof. Examples of carboxyl-, amino-, azetidinium-, epoxy-, and aziridine-containing vinyl monomers are known in the art and can be obtained from commercial sources or prepared according to known procedures. The lens formulation preferably contains from about 0.1% to about 10%, more preferably from about 0.25% to about 7%, even more preferably from about 0.5% to about 5%, and most preferably from about 0.75% to about 3% by weight of such a vinyl monomer having at least one first reactive functional group.

[0136] If a preformed contact lens naturally contains amino groups on and / or near its surface, it can be chemically modified by reacting it with a divinyl sulfone compound according to a thiol Michael addition reaction to covalently bond vinyl sulfone groups through the amino groups, or by reacting it with a thiolactone to covalently bond thiol groups through the amino groups.

[0137] Examples of preferred divinyl sulfone compounds include, but are not limited to, divinyl sulfone, bis(vinylsulfonyl) C1-C6 alkanes, 1,3-bis(vinylsulfonyl)-2-propanol, 1,1-bis(vinylsulfonyl)-1-propanol, 1,5-bis(vinylsulfonyl)-3-pentanol, 1,1-bis(vinylsulfonyl)-3-methoxypropane, 1,5-bis(vinylsulfonyl)-2,4-dimethylbenzene, and 1,4-bis(vinylsulfonyl)-2,3,5,6-tetrafluorobenzene.

[0138] Examples of preferred commercially available thiolactones include, but are not limited to, 4-butyrothiolactone (or dihydro-2(3H)-thiophenone), 3-methyldihydro-2(3H)-thiophenone, 3-ethyldihydro-2(3H)-thiophenone, 3-(1-methylethyl)dihydro-2(3H)-thiophenone, 3,3-dimethyldihydro-2(3H)-thiophenone, 3-ethyl-3-methyldihydro-2(3H)-thiophenone, 3-acetyldihydro-2(3H)-thiophenone, N-acetylhomocysteine ​​thiolactone, N-propionylhomocysteine ​​thiolactone, N-butyrylhomocysteine ​​thiolactone, and N-carboxybutyrylhomocysteine ​​thylactone (or 4-oxo-4-[(tetrahydro-2-oxo-3-thienyl)amino]-butanoic acid).

[0139] The preformed contact lens may be subjected to any surface treatment to have first reactive functional groups on and / or near its surface. Any suitable surface treatment may be used in the present invention. Examples of surface treatment include, but are not limited to, plasma treatment; chemical treatment; chemical vapor deposition; grafting (covalent bonding) of a compound having at least one reactive functional group onto the surface of the article (modified or unmodified); graft polymerization of a vinyl monomer having at least one first reactive functional group onto the surface of the article (modified or unmodified); layer-by-layer ("LbL") deposition of one or more hydrophilic materials having first reactive functional groups onto the surface of the article (modified or unmodified) (i.e., LbL coating formation process); covalent bonding of one or more hydrophilic polymer-based materials having first reactive functional groups onto the surface of the article (modified or unmodified); or combinations thereof.

[0140] Plasma treatment refers to the process of exposing a contact lens to a plasma to chemically modify the surface of the contact lens. The term "plasma" refers to an ionized gas (e.g., formed by an electrical glow discharge that may consist of electrons, ions of either polarity, gas atoms and molecules in the earth or any higher state of any form of excitation and photons). The excited species interact with the solid surface of an article placed in the plasma, chemically and physically modifying the material surface. When the plasma is generated by exposing a gas in a vacuum chamber to a charge, typically radio frequency (rf) (or microwave or other frequency), it is often called a "low temperature plasma". When the plasma is generated by an atmospheric pressure discharge (e.g., an arc discharge) and maintained at ambient atmospheric pressure, it is a "high temperature plasma" or "atmospheric pressure plasma". Atmospheric pressure plasma can be generated by atmospheric pressure discharge.

[0141] For reviews of plasma processing and its uses, see R. Hartmann “Plasma polymerisation: Grundlagen, Technik und Anwendung, Jahrb. Oberflaechentechnik (1993) 49, pp. 283-296, Battelle-Inst. eV Frankfurt / Main Germany; H. Yasuda, “Glow Discharge Polymerization”, Journal of Polymer Science: Macromolecular Reviews, vol. 16 (1981), pp. 199-293; H. Yasuda, “Plasma Polymerization”, Academic Press, Inc. (1985); Frank Jansen, “Plasma Deposition Processes”, in “Plasma Deposited Thin Films”, ed. by T. Mort and F. Jansen, CRC Press Boca Raton (19); O. Auciello et al. (ed.) “Plasma-Surface Interactions and Processing of Materials” publ. by Kluwer Academic Publishers in NATO ASI Series; Series E: Applied Sciences, vol. 176 (1990), pp. 377-399; and N. Dilsiz and G. Akovali “Plasma Polymerization of Selected Organic Compounds”, Polymer, vol. 37 (1996) pp. 333-341 are references.

[0142] Known plasma treatments under low pressure include plasma deposition, plasma-induced polymerization, plasma grafting, plasma oxidation, etc. Plasma treatments under low pressure are used in commercial products such as Focus NIGHT&DAY® and AIR OPTIX® (Alcon) and PUREVISION® (Bausch&Lomb). The advantages of plasma coatings, such as those found in Focus NIGHT&DAY®, are their durability, relatively high hydrophilicity / wettability, and low susceptibility to lipid and protein deposition and adsorption. Examples of plasma treatments are those disclosed in U.S. Pat. Nos. 4,143,949; 4,312,575; 5,464,667; 6,881,269; and 7,078,074 (incorporated herein by reference in their entirety). It is understood that preformed contact lenses must typically be dried before plasma treatment under low pressure.

[0143] Those skilled in the art are well aware that a plasma (i.e., an electric glow discharge plasma) is a partially ionized gas consisting of a high concentration of excited atomic, molecular, ionic and free radical species, which is produced by exposing the gas in a vacuum chamber to an electric field, typically radio frequency (rf) (or microwave or other frequency).

[0144] As an example of plasma treatment of silicone hydrogel contact lenses under low pressure, one or more preformed silicone hydrogel contact lenses are placed in a reactor chamber between opposing electrodes. The chamber is then sealed and depressurized by a vacuum system. A significant amount of time is required to pump the system to the operating pressure. Once the appropriate pressure is obtained in the chamber, a process gas is introduced inside the chamber and the electrodes are activated. The resulting plasma cloud can apply a thin layer of polymer (or polymer coating) to the lens and / or modify the chemical composition of the top layer of the lens surface depending on the process gas used. After a suitable time, the electrodes are turned off and the reactor chamber is returned to atmospheric pressure, allowing the lens to be removed.

[0145] Low pressure plasma processing systems are known to those skilled in the art and have been disclosed in patents and papers. For example, Peng Ho and Yasuda in their paper "Ultrathin Coating Of Plasma Polymer Of Methane Applied On The Surface Of Silicone Contact Lenses," Journal of Biomedical Materials Research, Vol. 22, 919-937 (1988), the entirety of which is incorporated herein by reference, disclose a batch-type low pressure plasma processing system (or rotary plasma system) including a bell-shaped vacuum chamber in which opposing aluminum electrodes are arranged and a rotatable aluminum plate is arranged between the electrodes and driven by an induction motor in the system. Matsuzawa and Winterton in U.S. Patent No. 6,881,269, the entirety of which is incorporated herein by reference, disclose a linear low pressure plasma system.

[0146] In accordance with the present invention, a dry, preformed contact lens is treated with a low pressure plasma generated in a plasma gas (i.e., atmosphere) comprised of a mixture of air, N2, O2, CO2 or a C1-C6 hydrocarbon and a secondary gas selected from the group consisting of air, N2, O2, CO2 and combinations thereof (preferably a mixture of CO2 or a C1-C4 hydrocarbon gas and a secondary gas selected from the group consisting of air, CO2, N2 and combinations thereof, more preferably a mixture of CO2 or methane and a secondary gas selected from the group consisting of air, CO2, N2 and combinations thereof, even more preferably a mixture of CO2 or methane and CO2).

[0147] In the present invention, preferably, atmospheric pressure plasma surface treatment is used as disclosed in U.S. Patent No. 9,156,213, which is incorporated herein by reference in its entirety, in which the contact lens can be brought to a fully hydrated state.

[0148] Those skilled in the art are familiar with methods for grafting (covalently bonding) compounds having at least one first reactive functional group (such as carboxyl, amino, azetidinium, epoxide, aziridine, vinylsulfone, thiol, and combinations thereof) to the surface of a contact lens according to known coupling reactions.

[0149] As used herein, "LbL coating" refers to a coating that is not covalently bonded to the polymer matrix of a contact lens and is obtained by layer-by-layer ("LbL") deposition of one or more polymeric materials onto the lens. The LbL coating can be composed of one or more layers. The LbL coating on a contact lens can be obtained according to the methods described in U.S. Pat. Nos. 6,451,871, 6,719,929, 6,793,973, 6,811,805, 6,896,926, 8,044,112, 8,158,192 and 8,147,897. Preferably, the LbL coating comprises at least one layer of one or more polyanionic polymers each containing carboxyl groups and, optionally, a polyanionic polymer chemically modified to contain a first reactive functional group other than carboxyl groups. The polyanionic polymer is preferably a polyanionic polymer selected from the group consisting of polyacrylic acid, polymethacrylic acid, polyethylacrylic acid, poly(acrylic acid-co-methacrylic acid), poly(acrylic acid-co-ethacrylic acid), poly(methacrylic acid-co-ethacrylic acid) and mixtures thereof, more preferably a polyanionic polymer which is polyacrylic acid, polymethacrylic acid, poly(acrylic acid-co-methacrylic acid) or mixtures thereof. It is well known to chemically modify a polyanionic polymer by reacting it with a compound having at least one first reactive functional group other than a carboxyl group.

[0150] By contacting the contact lens with the polymer solution, an LbL coating of a polyanionic polymer having carboxyl groups can be formed on the contact lens. The contact lens can be contacted with the polymer coating solution by immersing the contact lens in the coating solution or by spraying the coating solution on the contact lens. One contacting process involves only immersing the contact lens in a bath of the coating solution for a certain period of time, or alternatively, immersing the contact lens in a series of baths of the coating solution sequentially for shorter periods of time in each bath. Another contacting process involves only spraying the coating solution. However, multiple alternatives include various combinations of spraying and immersion steps, which can be designed by one skilled in the art. The contact time of the contact lens with the reactive polymer coating solution can last for a maximum of about 10 minutes, preferably about 5 to about 360 seconds, more preferably about 5 to about 250 seconds, and even more preferably about 5 to about 200 seconds.

[0151] A solution of polyanionic polymer for forming a coating on a contact lens can be prepared by dissolving one or more polymers in water, a mixture of water and a water-miscible organic solvent, an organic solvent, or a mixture of one or more organic solvents. Preferably, the polymer is dissolved in a mixture of water and one or more organic solvents, an organic solvent, or a mixture of one or more organic solvents. It is believed that a solvent system including at least one organic solvent can increase the durability of the coating by swelling the contact lens, thereby allowing a portion of the reactive polymer to penetrate the contact lens. Examples of organic solvents are described above. The pH of the polyanionic polymer solution is preferably about 1.5 to about 4.0 to form a relatively thick and stable LbL coating. The temperature of the coating solution is preferably about 20°C to about 70°C.

[0152] Those skilled in the art know how to covalently bond one or more polymers having a first reactive functional group to the surface of a contact lens. Exemplary methods for covalently bonding one or more hydrophilic polymers to a medical device are described in U.S. Patents 5,599,576, 5,766,158, 6,087,415, 6,096,726, 6,340,465, 6,440,571, 6,500,481, 6,534,559, 6,623,747, 6,726,735, 6,746,747, 6,750,765, 6 ...776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,158, 6,776,15 Nos. 6,683,062, 6,838,491, 6,866,936, 6,923,978 and 8,529,057, and U.S. Patent Application Publication Nos. 2009-0145086A1, 2009-0145091A1, 2008-0142038A1 and 2007-0122540A1.

[0153] The graft polymerization of one or more vinyl monomers having at least one first reactive functional group (e.g., carboxyl, amino, azetidinium, epoxide, aziridine groups, and combinations thereof) in the presence or absence of a vinyl-based crosslinking agent to form a hydrophilic polymer coating has been described in many patents, such as U.S. Pat. Nos. 6,099,122, 6,436,481, 6,440,571, 6,447,920, 6,465,056, 6,521,352, 6,586,038, 6,730,366, 6,734,321, 6,835,410, and 6,878,399, and JP2001075060A. For example, a dry preformed contact lens is first subjected to plasma treatment in a plasma atmosphere of a compound having at least one reactive functional group (e.g., primary or secondary amino, carboxyl, epoxy, azlactone, aziridine or isocyanate group) to form a plasma coating having reactive functional groups. The plasma treated contact lens is reacted with a compound having a free radical initiator site (e.g., a thermal initiator or a photoinitiator) or preferably a living polymerization initiator site (e.g., an atom transfer radical polymerization (ATRP) initiator or a reversible addition-fragmentation chain transfer polymerization (RAFT) initiator) and a functional group that co-reacts with the functional groups of the plasma coating on the contact lens in the presence or absence of a coupling agent under coupling reaction conditions known to those skilled in the art. The resulting contact lens having free radical initiator sites thereon is immersed in a solution of one or more vinyl monomers having at least one first functional group and exposed to conditions that initiate the free radical polymerization of these vinyl monomers to form a layer of grafted polymer containing the first reactive functional group.

[0154] According to the present invention, the hydrophilic polymer-based material (i.e., cross-linked hydrophilic coating) for forming the exterior hydrogel layer or the exterior front and rear hydrogel layers comprises a second reactive functional group. Preferably, the hydrophilic polymer-based material is a highly branched hydrophilic polymer-based material that comprises a three-dimensional network (i.e., the highly branched hydrophilic polymer-based material is soluble or dispersible in water due to the polymer chains cross-linked by a limited amount of one or more cross-linking agents) and a second reactive functional group.

[0155] An example of such a highly branched hydrophilic polymer-based material is shown in Scheme I. [ka] (wherein X1 is -S-*, -OC(=O)-* or -NR'-*, and R' is hydrogen or a C1-C 20 where * represents an organic radical. The polymer is a partial reaction product of at least one azetidinium-containing polymer having an azetidinium group and at least one hydrophilic polymer having a carboxyl, primary amine, secondary amine, or thiol group according to the crosslinking reaction shown in Figure 2. The resulting highly branched hydrophilic polymer contains azetidinium groups and, optionally, carboxyl, primary amine, secondary amine, thiol groups, or combinations thereof.

[0156] Any suitable azetidinium-containing polymer can be used in the present invention. Examples of azetidinium-containing polymers include, but are not limited to, epichlorohydrin-functionalized polyamines, homopolymers of azetidinium-containing vinyl monomers, and copolymers of azetidinium-containing vinyl monomers with one or more vinyl monomers.

[0157] Preferably, the azetidinium-containing polymer is epichlorohydrin-functionalized polyamine.Epichlorohydrin-functionalized polyamine can be obtained by reacting epichlorohydrin with polyamine polymer or secondary amino group-containing polymer.For example, poly(alkyleneimine) or poly(amidoamine) (e.g., adipic acid-diethylenetriamine copolymer), which is a polycondensate derived from polyamine and dicarboxylic acid, can be reacted with epichlorohydrin to form epichlorohydrin-functionalized polymer;monoalkylaminoalkyl(meth)acrylate or monoalkylaminoalkyl(meth)acrylamide homopolymer or copolymer can also be reacted with epichlorohydrin to form epichlorohydrin-functionalized polyamine;poly(2-oxazoline-co-ethyleneimine) copolymer can be reacted with epichlorohydrin to form epichlorohydrin-functionalized polyamine (i.e., poly(2-oxazoline-co-ethyleneimine)-epichlorohydrin). The reaction conditions for epichlorohydrin functionalization of polyamine or polyamidoamine polymers are described in EP 1465931. The preferred epichlorohydrin-functionalized polyamines are polyamidoamine-epichlorohydrin (PAE) or poly(2-oxazoline-co-ethyleneimine)-epichlorohydrin.

[0158] Polyamidoamine-epichlorohydrin is commercially available, for example, Kymene® or Polycup® resins (epichlorohydrin functionalized adipic acid-diethylenetriamine copolymers) from Hercules.

[0159] Poly(2-oxazoline-co-ethyleneimine)-epichlorohydrin can be prepared according to the procedures described in US Patent Application Publication No. 2016 / 0061995A1.

[0160] Homopolymers and copolymers of azetidinium-containing vinyl monomers can be obtained according to the procedures described in US 2013 / 03371600 A1.

[0161] Any suitable hydrophilic polymer can be used in the present invention, so long as it is compatible with the eye and contains at least one amino group, at least one carboxyl group, and / or at least one thiol group, preferably at least one carboxyl group, at least one thiol group, or a combination thereof.

[0162] Hydrophilic polymeric materials containing azetidinium groups can be prepared according to the processes disclosed in US Patent Application Publication Nos. 2016 / 0061995 A1 and 2013 / 0337160 A1 and U.S. Patent No. 8,529,057.

[0163] Another example of such a highly branched hydrophilic polymer-based material is the partial reaction product of at least one polymer having an epoxy group with at least one hydrophilic polymer having a carboxyl, primary amine, secondary amine or thiol group by known coupling reactions. The resulting highly branched hydrophilic polymer contains epoxy groups and, optionally, carboxyl, primary amine, secondary amine, thiol groups or combinations thereof. For example, a multi-armed polyethylene glycol having a terminal epoxy group can be partially reacted with a multi-armed polyethylene glycol having a terminal thiol group (or carboxyl or amino group). Alternatively, a copolymer of an epoxy-containing vinyl monomer (i.e., a vinyl monomer having an epoxy group) and one or more hydrophilic vinyl monomers can be reacted with a hydrophilic polymer having a thiol, carboxyl or amino group. Such a hydrophilic polymer-based material can be prepared according to the process disclosed in US Pat. No. 9,244,195.

[0164] Another example of such a highly branched hydrophilic polymer-based material is the partial reaction product of at least one polymer having an aziridine group (or an azlactone group) with at least one hydrophilic polymer having a carboxyl, primary amine, secondary amine or thiol group, by known coupling reactions. The resulting highly branched hydrophilic polymer contains an aziridine group (or an azlactone group) and, optionally, a carboxyl, primary amine, secondary amine, thiol group or a combination thereof. Examples of hydrophilic polymers containing aziridine or azlactone groups include copolymers of an aziridine-containing vinyl monomer (i.e., a vinyl monomer having an aziridine group) or an azlactone-containing vinyl monomer (i.e., a vinyl monomer having an azlactone group) with one or more hydrophilic vinyl monomers.

[0165] Another example of such a highly branched hydrophilic polymer-based material is the partial reaction product of at least one polymer having a vinyl sulfone group and at least one hydrophilic polymer having a thiol group by the well-known Michael addition reaction. The resulting highly branched hydrophilic polymer contains a vinyl sulfone group and / or a thiol group. Examples of hydrophilic polymers containing vinyl sulfone groups include multi-armed polyethylene glycols having terminal sulfone groups, polymers containing monomer units each having a thiol group and obtained by reacting a thiolactone with a monomer unit each having an amino group (i.e., derived from amino-containing vinyl monomers).

[0166] According to the present invention, the concentration ratio of the hydrophilicity enhancer to the azetidinium-containing polymer in the aqueous reactive solution must be selected so as not to render the resulting water-soluble thermally crosslinkable polymeric material water-insoluble (i.e., solubility of less than 0.005 g per 100 ml of water at room temperature) and so as not to consume more than about 99%, preferably about 98%, more preferably about 97%, and even more preferably about 96% of the azetidinium groups of the azetidinium-containing polymer.

[0167] In accordance with the present invention, a preformed contact lens having first reactive functional groups thereon is heated in an aqueous solution containing a hydrophilic polymer-based material having second reactive functional groups at a temperature of from about 40° C. to about 140° C. for a time to crosslink the hydrophilic polymer-based material while covalently bonding the crosslinked hydrophilic polymer-based material onto the preformed contact lens to form a hydrogel coating on the surface of the preformed contact lens.

[0168] Preferably, when the first reactive functional group is not a vinyl sulfone group, the heating step is performed by autoclaving the preformed contact lens having the first reactive functional group thereon, which is immersed in an aqueous packaging solution (i.e., an aqueous buffer solution having a pH of 6.7 to 7.6) in a sealed lens package, at a temperature of about 115° C. to about 125° C. for about 20 to 90 minutes. During autoclaving, it is believed that those azetidinium groups (or epoxy, aziridine or azlactone groups) that are not involved in the crosslinking reaction may be hydrolyzed to 2,3-dihydroxypropyl (HO-CH2-CH(OH)-CH2-) groups (or hydroxyl, amino or carboxyl groups) and that the azetidinium-containing polymeric material (or epoxy, aziridine or azlactone-containing polymeric material), if applicable, present in the lens packaging solution may be converted to a non-reactive polymeric wetting agent that may improve the wear comfort of the lens. As a result, the packaging solution is ophthalmically safe after autoclaving.

[0169] Lens packages (or containers) are well known to those skilled in the art for autoclaving and storing contact lenses. Any lens package can be used in the present invention. Preferably, the lens package is a blister package comprising a base and a cover, the cover being removably sealed to the base, and the base comprising a cavity for receiving a sterile packaging solution and a contact lens.

[0170] The lenses are packaged in individual packages, sealed, and sterilized (e.g., by autoclaving at or above about 120° C. under pressure for at least 30 minutes) before being distributed to users. Those skilled in the art will be familiar with methods of sealing and sterilizing lens packages.

[0171] In accordance with the present invention, the packaging solution contains at least one buffer and one or more other ingredients known to those skilled in the art, including, but not limited to, tonicity agents, surfactants, antibacterial agents, preservatives, and lubricants (e.g., cellulose derivatives, polyvinyl alcohol, polyvinylpyrrolidone).

[0172] The packaging solution contains a sufficient amount of buffer to maintain the pH of the packaging solution within a desired range, for example, within a physiologically acceptable range, preferably from about 6.5 to about 7.5. Any known physiologically compatible buffer may be used. Suitable buffers as components of contact lens care compositions according to the present invention are known to those skilled in the art. Examples include boric acid, borates such as sodium borate, citric acid, citrates such as potassium citrate, bicarbonates such as sodium bicarbonate, TRIS (i.e. 2-amino-2-hydroxymethyl-1,3-propanediol), Bis-Tris [i.e. bis-(2-hydroxyethyl)-imino-tris-(hydroxymethyl)-methane], Bis-Trispropane [i.e. 1,3-bis(tris(hydroxymethyl)methylamino)propane], bis-aminopolyols, triethanolamine, ACES [i.e. N-(2-hydroxyethyl)-2-aminoethanesulfonic acid], BES [i.e. N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid], HEPES [i.e. Examples of suitable buffers include 4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid], MES [i.e. 2-(N-morpholino)ethanesulfonic acid], MOPS [i.e. 3-[N-morpholino]-propanesulfonic acid], PIPES [i.e. piperazine-N,N'-bis(2-ethanesulfonic acid], TES {i.e. N-[tris(hydroxymethyl)methyl]-2-aminoethanesulfonic acid}, salts thereof, phosphate buffers such as Na2HPO4, NaH2PO4 and KH2PO4 or mixtures thereof. The amount of each buffer in the aqueous packaging solution is preferably 0.001% to 2% by weight, preferably 0.01% to 1% by weight; most preferably about 0.05% to about 0.30% by weight.

[0173] The packaging aqueous solution has a tonicity of about 200 to about 450 milliosmoles (mOsm), preferably about 250 to about 350 mOsm. The tonicity of the packaging aqueous solution can be adjusted by adding organic or inorganic substances that affect tonicity. Suitable ophthalmically acceptable tonicity agents include, but are not limited to, sodium chloride, potassium chloride, glycerol, propylene glycol, polyols, mannitol, sorbitol, xylitol, and mixtures thereof.

[0174] The packaging solution of the present invention has a viscosity at 25°C of about 1 centipoise to about 5 centipoise.

[0175] In a preferred embodiment, the packaging solution contains from about 0.01% to about 2%, more preferably from about 0.05% to about 1.5%, even more preferably from about 0.1% to about 1%, and most preferably from about 0.2% to about 0.5% by weight of a hydrophilic polymeric material having a second reactive functional group.

[0176] Although various embodiments of the present invention have been described using specific terms, devices and methods, such descriptions are for illustrative purposes only. The terms used are terms of description rather than of limitation. As will be apparent to those skilled in the art, many variations and modifications of the present invention may be made by those skilled in the art without departing from the spirit and scope of the novel concepts of the present disclosure. In addition, it should be understood that aspects of the various embodiments of the present invention may be interchanged in whole or in part, or may be combined in any manner and / or used together, as set forth below: 1. A contact lens comprising a lens bulk material coated with an exterior hydrogel layer and having a posterior surface and an opposite anterior surface, the exterior hydrogel layer being comprised of a front outer hydrogel layer and a posterior outer hydrogel layer, the posterior outer hydrogel layer having an indentation depth ratio of at least about 1.2.

number

number

number

number

number

number

[0177] The above disclosure enables those skilled in the art to carry out the present invention.Various modifications, alterations and combinations can be made to the various embodiments described herein.In order to better enable the reader to understand specific embodiments and their advantages, reference to the following examples is proposed.It is intended that the present specification and examples are considered as illustrative. EXAMPLES

[0178] Example 1 Measurement of oxygen permeability Apparent oxygen permeability (Dk app ), apparent oxygen permeability (Dk / t), intrinsic (or edge-corrected) oxygen permeability (Dk c ) is determined according to the procedure described in Example 1 of US Patent Application Publication No. 2012 / 0026457A1.

[0179] Surface Wettability Test The water contact angle (WCA) of contact lenses is a general measure of the surface wettability of contact lenses. In particular, a lower water contact angle corresponds to a more wettable surface. The dynamic captive bubble contact angle of contact lenses is measured using an FDS instrument from Future Digital Scientific Corp. The FDS instrument is capable of measuring advancing and receding contact angles. Measurements are performed on hydrated contact lenses at room temperature. The contact lenses are removed from the vial, immersed in approximately 40 mL of fresh PBS, shaken for at least 30 minutes, then replaced with fresh PBS and soaked and shaken for another 30 minutes unless otherwise specified. The contact lenses are then placed on lens paper and tapped to remove surface water, then placed on the lens holder with the front curve up and the top of the lens holder screwed on. The securely fastened lens holder is placed in a glass cell cuvette filled with filtered PBS. The glass cell cuvette is placed on the stage of the FDS instrument. The stage height and the syringe needle are adjusted to distribute air bubbles on the lens surface. Three dispense / withdraw cycles are repeated for each lens to obtain advancing and receding contact angles, which are reported in the examples below.

[0180] Water Break Time (WBUT) Test The surface hydrophilicity of the lenses (after autoclaving) is assessed by measuring the time it takes for the water film to begin to break down on the lens surface. Lenses exhibiting a WBUT ≥ 10 seconds are considered to have a hydrophilic surface and are expected to exhibit sufficient wettability (ability to support a tear film) on the eye.

[0181] The lenses are prepared for water-shedding measurements by removing the lenses from the blisters with flexible plastic tweezers (e.g., from Menicon) and placing the lenses in test tubes containing phosphate-buffered saline. The tubes contain 10 mL of phosphate-buffered saline per lens, with one lens per tube. Allow the lenses to soak overnight (at least 16 hours) before testing.

[0182] WBUT is measured at room temperature as follows: the lens is removed from the test tube and placed on a platform submerged in PBS. The platform is then lifted out of the PBS solution (t=0) and the fluid flowing from the lens surface is observed with a video camera. When the fluid on the lens surface disappears, this WBUT time is recorded. Optionally, a stopwatch can be used to measure the time from when the platform is lifted out of the PBS to when the fluid on the lens surface disappears. The platform is withdrawn and the lens is pulled under the surface of the PBS. At least three spots are measured per lens, and at least three lenses are measured to obtain an average WBUT measurement for each lens group.

[0183] equilibrium moisture content The equilibrium water content (EWC) of a contact lens is determined as follows.

[0184] The amount of water (expressed as weight percent) present in hydrated hydrogel contact lenses that have been fully equilibrated with saline is measured at room temperature. After quickly stacking the lenses and wiping the lenses with a cloth, transfer the stack of lenses to an aluminum pan on an analytical balance. The number of lenses in each sample pan is typically five. Record the hydrated weight of the pan + lenses. Cover the pan with aluminum foil. Place the pan in a laboratory oven at 100 ± 2 °C and dry for 16-18 hours. Remove the pan + lenses from the oven and cool in a desiccator for at least 30 minutes. Remove one pan from the desiccator and discard the aluminum foil. Weigh the pan + dry lens sample on an analytical balance. Repeat for all pans. The wet and dry weights of the lens samples can be calculated by subtracting the weight of the empty weighing pan.

[0185] Elasticity The elastic modulus of contact lenses is determined using an MTS Insight instrument. The contact lenses are first cut into 3.12 mm wide strips using a Precision Concept two-stage cutter. Five thickness values ​​are measured within a gauge length of 6.5 mm. The strips are attached to the grips of the instrument and submerged in PBS at a controlled temperature of 21±2° C. Typically, a 5 N load cell is used for testing. A constant force and rate is applied to the sample until it breaks. Force and displacement data are collected by the TestWorks software. The elastic modulus value is calculated by the TestWorks software, which is the slope or tangent of the stress versus strain curve near zero elongation in the elastic deformation region.

[0186] Contact lens surface flexibility All surface modified contact lenses can have a surface modulus that is different from their bulk properties. In particular, contact lenses with a soft hydrogel coating thereon have a softer surface modulus than the bulk. The apparent surface modulus properties of a contact lens in the near-surface and surface-containing regions can be characterized in a nanoindentation test by measuring the indentation depth of an indentation probe with a tip radius of 9.5 μm and a stiffness of 0.54 N / m at a compressive pressure of 5 KPa against one surface of the contact lens. For surface moduli between 1 and 500 kPa, this cantilever stiffness is recommended. For harder or softer surface samples, a different cantilever could be used.

[0187] Nanoindentation Testing In a microindentation test, the indentation depth of an indentation probe with a tip radius of 9.5 μm and a stiffness of 0.54 N / m is measured at a compressive pressure of 5 KPa against one surface of a contact lens as follows.

[0188] An Optics11 Piuma instrument is used to determine the indentation depth function of displacement. Before performing the indentation, the Piuma probe is calibrated in the selected test solution (i.e. PuriLens plus, OPTIFREE Replenish vehicle, PBS) according to the instructions in the manual (see https: / / optics11life.com / wp-content / uploads / 2019 / 05 / Piuma-Nanoindenter-Manual.pdf). This calibration consists of first calibrating the optical sensor with the probe submerged in the test solution but not in contact with the substrate surface. Then, a test indentation is performed on a glass slide, followed by a second cantilever calibration. The lens is rinsed in the test solution to wash away excess lens package solution (30-50 ml of test solution for 10-20 min). The bottom of the lens holder (shown in Figure 2) is filled with 25 ml of test solution and degassed for at least 5 min. After immersion, the lens is placed (test side up) on the center post of the lens holder bottom. The lens should be placed so that the edge of the lens faces away from the holder. The lens is then inverted onto the post to minimize any air bubbles or excess test fluid remaining.

[0189] Place the upper piece over the lower piece and lock it into place to ensure the lens is held in place. Then place the holder on the test stage and align the center of the lens with the probe. Add enough test solution to completely submerge the sample.

[0190] Finally, move the Piuma probe just above the lens surface (approximately 1-2 mm away) and submerge the probe in the test solution. Continue dripping the solution onto the probe surface until the cantilever is fully immersed and the signal is stable.

[0191] The nanoindentation "surface probing" routine is performed according to the manufacturer's typical procedures. The indentation routine consists of a 10 μm indentation at a speed of 1 μm / sec. The probe is moved to the surface and the contact point is determined by the first deflection detected by the cantilever. Typically, three indentations are made at multiple spots (i.e. 16) on the lens surface with a large distance between spots (i.e. 250 microns), and five lenses of each lens type are typically tested.

[0192] A typical Piuma probe used to characterize surface moduli from 1 to 500 kPa has a stiffness of 0.54 N / m and a tip radius of 9.5 μm. cap ) can be calculated by the following formula: S cap =2πRh (where "R" is the tip radius and h is the indentation depth).

[0193] Once indentation is performed, both the indentation depth and the indentation force are recorded. To calculate the indentation depth at 5 kPa, the indentation pressure is calculated by dividing the indentation force by the contact area of ​​the ball-crown. From this data set, the indentation distance at 5 kPa (typically, eyelid pressures are between 1 and 5 kPa) can be reported.

[0194] All raw data is processed using MATLAB and analyzed using Excel.

[0195] chemicals In the examples below, the following abbreviations are used: AMA stands for allyl methacrylate; NVP stands for N-vinylpyrrolidone; MMA stands for methyl methacrylate; TEGDMA stands for triethylene glycol dimethacrylate; EGMA stands for ethylene glycol methyl ether methacrylate; VAZO64 stands for 2,2'-dimethyl-2,2'azodipropiononitrile; Nobloc is 2-[3-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]ethyl methacrylate from Aldrich; RB247 is Reactive Blue 247; TAA stands for tert-amyl alcohol; PAA stands for polyacrylic acid; PAE stands for polyamidoamine-epichlorohydrin (also known as polyamine-epichlorohydrin). % NaH2PO4·H2, about 0.388 wt.% Na2HPO4·2H2O, and about 0.79 wt.% NaCl; wt.% stands for weight percent; mSi1 stands for monobutyl terminated monomethacryloxypropyl terminated polydimethylsiloxane (from Gelest, Mw about 600-800 g / mol); "GA" macromer stands for dimethacryloyloxypropyl terminated polysiloxane of formula (A) (Mn about 6.8 Kg / mol, OH content about 1.2 meq / g). [ka]

[0196] Example 2 Preparation of the polymerizable composition Lens formulation (polymerizable composition) is prepared to have the following composition (parts): mSil (34 parts by weight); GA (6 parts by weight); NVP (40 parts by weight); MMA (10 parts by weight); EGMA (10 parts by weight); TEGDMA (0.4 parts by weight); AMA (0.1 parts by weight); Nobloc (1 part by weight); VAZO64 (0.5 parts by weight); RB247 (0.01 parts by weight); TAA (1 part by weight). The formulation is prepared by placing the listed components in their target amounts in a clean bottle and mixing with a stir bar at room temperature for 30 minutes at 600 rpm. After all solids are dissolved, the formulation is filtered using a 2.7 μm glass microfiber filter (GMF).

[0197] Cast molded silicone hydrogel contact lenses The lens formulation is purged with nitrogen at room temperature for 30-35 minutes. The N2 purged lens formulation is placed into a polypropylene mold and heat cured under the following cure conditions: room temperature to 55°C at approximately 7°C / min; hold at 55°C for approximately 30 minutes; ramp from 55°C to 80°C at approximately 7°C / min; hold at 55°C for approximately 30 minutes; ramp from 80°C to 100°C at approximately 7°C / min; hold at 100°C for approximately 30 minutes. The mold is opened and the molded lens is removed from the mold.

[0198] Prior to lens characterization, the resulting silicone hydrogel (SiHy) contact lenses (uncoated SiHy lenses) are subjected to the following post-molding treatment: After demolding, the SiHy lenses prepared above are immersed in PBS twice at room temperature for about 60 minutes. After rinsing with PBS for 5 minutes, the lenses are placed in polypropylene lens packaging shells (or blisters) (one lens per shell) containing 0.6 mL of PBS. The blisters are then sealed with foil and autoclaved at about 121° C. for about 45 minutes. The SiHy lenses have an oxygen permeability (measured according to polarographic methods) of about 83 barrer, a bulk modulus of about 0.67 MPa, a water content of about 50% by weight, a relative ion permeability of about 11.0 relative to Alsacon lenses, and a WBUT of zero seconds.

[0199] Example 3 Preparation of PAA aqueous solution An aqueous solution of polyacrylic acid (PAA) is prepared by adding an appropriate amount of PAA (Mn approx. 450 kD) in water (distilled or deionized water). After the PAA is completely dissolved, the pH is adjusted to approx. 2 by adding approx. 1.85% formic acid to the aqueous PAA solution. The target concentration of PAA is approx. 0.1 wt.%. The prepared aqueous PAA solution is filtered to remove any particulate matter or foreign matter.

[0200] Phosphate-buffered saline (PBS) Phosphate buffered saline is prepared by dissolving NaH2PO4·H2O, Na2HPO4·2H2O in a predetermined amount of purified water (distilled or deionized) to have the following composition: approximately 0.044 w / w% NaH2PO4·H2O, approximately 0.388 w / w / % Na2HPO4·2H2O, and approximately 0.79 w / w% NaCl.

[0201] Phosphate buffer (PB) without NaCl (PB, without NaCl) PB is prepared using the same procedure as for preparing PBS, but without the addition of NaCl.

[0202] IPC Saline IPC saline is prepared by dissolving / mixing appropriate amounts of poly(AAm-co-AA) (90 / 10), PAE, NaH2PO4·H2O, Na2HPO4·2H2O and NaCl in DI (deionized) water and then adjusting the pH to about 7.3 to have the following concentrations: about 0.132 wt% poly(AAm-co-AA); about 0.11 wt% PAE; about 0.044 wt% NaH2PO4·H2O, about 0.388 wt% Na2HPO4·2H2O and about 0.79 wt% NaCl. Poly(AAm-co-AA) (90 / 10) partial sodium salt, poly(AAm-co-AA) 90 / 10, Mw 200,000) is purchased from Polysciences, Inc. and used as received. The prepared solution is pretreated at 65 °C for about 6 h. After heat pretreatment, the IPC saline is cooled to room temperature. Up to 5 ppm hydrogen peroxide can be added to the final IPC saline to prevent bioburden growth, and the IPC saline is filtered using a 0.22 micron membrane filter.

[0203] SiHy lenses with PAA base coat After removal from the mold, the SiHy contact lenses (made in Example 2) are placed in an appropriate tray. The tray with the lenses is then immersed in the PAA solution for a period of time, either 120 minutes in one bath of PAA or 30 minutes in the first bath and then 90 minutes in the second bath of two consecutive baths of PAA. The PAA immersion solution is heated above room temperature, for example to 40° C. Sufficient agitation (e.g., horizontal shaking or up-and-down motion) can be used to ensure proper flow of the PAA solution during the immersion process.

[0204] After PAA soaking, the lenses are typically transferred to a bath of PB for up to about 1 hour at room temperature. Sufficient agitation (e.g., horizontal shaking or up-and-down motion) can be used to ensure adequate flow of PB during the soaking process.

[0205] The lenses are then transferred to a bath of water, typically at room temperature for about 5-10 minutes. Sufficient agitation (e.g., horizontal shaking or up-and-down motion) may be used to ensure adequate flow of water during the soaking process.

[0206] SiHy contact lenses having a hydrogel coating thereon The SiHy lenses having the PAA-based coating thereon prepared above are placed into polypropylene lens packaging shells (one lens per shell) containing about 0.15-0.3 mL of IPC saline in one of three positions: position I (posterior surface facing down, anterior surface facing up); position II (posterior surface facing up, anterior surface facing down); and position III (inverted posterior surface facing down, inverted anterior surface facing up). About 0.35-0.5 mL of IPC saline is placed into the concave surface (i.e., posterior surface or inverted anterior surface), allowing some overflow of the IPC saline in the packaging shell. The blister (packaging shell) is then sealed with foil and autoclaved at about 121° C. for about 45 minutes to form a SiHy contact lens having a crosslinked hydrophilic coating (i.e., hydrogel coating) thereon. The shell is maintained horizontally during autoclaving to ensure that the anterior and posterior surfaces of the contact lens are in the designated positions.

[0207] Surface properties of SiHy contact lenses with a hydrogel layer thereon The resulting SiHy contact lenses (autoclaved at position I) taken directly from the package have a WBUT greater than 10 seconds and a sessile drop (static) water contact angle less than 55 degrees.

[0208] Example 4 The surface flexibility of the contact lenses is determined according to the procedure described in Example 1. The flexibility of the uncoated contact lenses (EWC about 50%; bulk modulus about 0.69 MPa) prepared in Example 2, the coated contact lenses (EWC about 50%; bulk modulus about 0.69 MPa) prepared in Example 3, and the commercially available contact lens BioTrue TM(EWC about 78%; bulk modulus about 0.49 MPa, Bausch & Lamb) is used in this example. The results are reported in Table 1.

[0209] [Table 1]

[0210] As mentioned above, it should be noted that the indentation depth value measured on the lens surface in the nanoindentation test with an indentation probe having a tip radius of 9.5 μm and a stiffness of 0.54 N / m at a compressive pressure of 5 KPa reflects the apparent hardness (i.e., flexibility) of the surface: the higher the value, the softer the surface.

[0211] Table 1 shows that even though BioTrue lenses have a lower bulk modulus (0.49 MPa) than the coated lenses, both the posterior and anterior surfaces of the coated lenses are much softer than BioTrue lenses; both the posterior and anterior surfaces of the coated lenses are much softer than uncoated lenses; and that the autoclave position of the lens within the lens package can directly affect the flexibility of the posterior and anterior surfaces of coated contact lenses within the package during autoclaving.

[0212] Example 5 This example illustrates a method for qualitatively determining whether the posterior and anterior surfaces of a contact lens have different surface material and / or structural properties according to low coherence interferometry (LCI) as shown in FIG.

[0213] Similar to ultrasound, LCI uses a fine beam of light (beam width approximately 40 μm) to measure the thickness of multi-layer products. It relies on light reflected from the surfaces between the layers. The surfaces of multiple layers of material are detected as peaks in the depth-scanned signal. The central location of each peak defines the location of the surface (interface). The peak intensity is proportional to the light reflected from the surface. In the test, a contact lens is placed in a cuvette or wet cell filled with saline and placed on a flat window with the rear surface facing down. The scanning probe can be placed above the lens or below the lens.

[0214] If a contact lens has identical material and mechanical properties at the two lens surfaces, the FC and BC signal peaks are expected to be of the same intensity (e.g., see peak 1FC and peak 1BC, respectively, for the FC and BC surfaces of a commercially available AIR Optix Plus Hydraglyde lens (Alcon) in Figure 4).

[0215] In the commercially available DAILIES® TOTAL 1 lens (Alcon) tested, the FC signal peak 2FC is slightly lower than the BC signal peak 2BC (Figure 4).

[0216] However, for the coated contact lens produced in Example 3 at autoclave position II, the FC signal peak 3FC is much larger than the BC signal peak 3BC (Figure 4). The dramatic difference (or difference in signal intensity) between the FC and BC surface signals reflects the difference in optical properties between the FC and BC surfaces. Considering the nanoindentation measurement results of Example 4 on a similar contact lens, these results indicate that the simple optical detection results correlate with the surface flexibility of the surface, i.e., the surface flexibility of the posterior and anterior surfaces with different material and structural properties.

[0217] 5 also shows LCI data collected on lenses made in Example 3 but in autoclave position III (i.e., the contact lens was inverted before being placed in the lens package and autoclave). The signal intensities are inverted: the peak signals 4FC and 5FC on the FC side are much weaker than the peak signals 4BC and 5BC on the BC side. This result further supports that the autoclave position of the lens in the lens package during autoclaving directly impacts the flexibility of the posterior and anterior surfaces of the coated contact lens in the package during autoclaving.

[0218] All publications and patents cited herein are incorporated by reference in their entirety.

Claims

1. A method for producing a coated contact lens, comprising the steps of: (1) obtaining a contact lens precursor having a posterior surface that is concave and an opposite anterior surface that is convex, the contact lens precursor comprising lens bulk material and first reactive functional groups on and / or adjacent the anterior and posterior surfaces, the first reactive functional groups being selected from the group consisting of carboxyl groups, amino groups, azetidinium groups, epoxide groups, thiol groups, and combinations thereof; (2) placing the Contact Lens Precursor within a container in a position to ensure that the posterior surface of the Contact Lens Precursor faces up while the anterior surface faces down; (3) administering an aqueous solution to the posterior surface of the contact lens precursor, while maintaining the posterior surface facing upward, in an amount to completely immerse the contact lens precursor in the aqueous solution that is a packaging solution in the container, the aqueous solution having a room temperature and comprising at least one hydrophilic polymer-based material, the at least one hydrophilic polymer-based material each comprising a second reactive functional group capable of reacting with one first reactive functional group to form a covalent bond at a temperature higher than the room temperature, the second reactive functional group being selected from the group consisting of a carboxyl group, an amino group, an azetidinium group, an epoxide group, a thiol group, and combinations thereof; (4) sealing the container containing the contact lens precursor completely immersed in the aqueous solution while maintaining the rear surface facing upward; and (5) autoclaving the sealed container containing the contact lens precursor therein at a temperature of 115° C. to 125° C. for 20 to 90 minutes while maintaining the rear surface facing upward to form a coated contact lens. Including, The contact lens includes the lens bulk material coated with an outer hydrogel layer, the outer hydrogel layer being comprised of an outer anterior hydrogel layer and an outer posterior hydrogel layer, the outer posterior hydrogel layer having an indentation depth ratio of at least 1.

2. [0010] wherein (Id) is a hydrogel layer having a hydrogel thickness of about 100 mm, more flexible than said outer front hydrogel layer, as characterized by having PS is the indentation depth measured in a nanoindentation test using an indentation probe having a tip radius of 9.5 μm and a stiffness of 0.54 N / m at a compressive pressure of 5 KPa against the rear surface, and (Id) AS is the indentation depth measured in a nanoindentation test using an indentation probe having a tip radius of 9.5 μm and a stiffness of 0.54 N / m at a compressive pressure of 5 KPa against the anterior surface, and the contact lens has a water break-off time of at least 10 seconds.

2. 10. The method of claim 1, wherein the lens bulk material is a preformed hard contact lens made essentially of a hard plastic material that is crosslinked polymethacrylate.

3. 10. The method of claim 1, wherein the lens bulk material is a preformed rigid gas permeable contact lens made essentially of a rigid gas permeable lens material.

4. The method of claim 2 or 3, wherein the outer front and rear hydrogel layers, independently of each other, have a thickness of from 0.2 μm to 20 μm when fully hydrated.

5. 10. The method of claim 1, wherein the lens bulk material is a preformed hybrid contact lens having a central optic zone made essentially of a hard gas permeable lens material and surrounded by a peripheral zone made essentially of a non-silicone hydrogel material.

6. 2. The method of claim 1, wherein the lens bulk material is a preformed embedded contact lens, the lens bulk material consisting essentially of a three-dimensional article and a non-silicone hydrogel material, the three-dimensional article being made of a non-hydrogel material and having a three-dimensional size smaller than that of the contact lens, whereby the three-dimensional article is fully embedded within the non-silicone hydrogel material.

7. 10. The method of claim 1, wherein the lens bulk material is a preformed non-silicone hydrogel contact lens made essentially of a non-silicone hydrogel material, the non-silicone hydrogel material comprising at least 50 mole percent repeat units of at least one hydroxyl-containing vinyl monomer, and the non-silicone hydrogel material has an equilibrium water content of 10% to 80% by weight.

8. 10. The method of claim 1, wherein the lens bulk material is a preformed hybrid contact lens having a central optic zone made essentially of a hard gas permeable lens material and surrounded by a peripheral zone made essentially of a silicone hydrogel material.

9. 2. The method of claim 1, wherein the lens bulk material is a preformed embedded contact lens, the lens bulk material consisting essentially of a three-dimensional article and a silicone hydrogel material, the three-dimensional article being made of a non-hydrogel material and having a three-dimensional size smaller than that of the preformed embedded contact lens, whereby the three-dimensional article is fully embedded within the silicone hydrogel material.

10. The method of claim 1 , wherein the lens bulk material is a preformed non-silicone hydrogel contact lens made essentially of a silicone hydrogel material.

11. The method of any one of claims 8 to 10, wherein the silicone hydrogel material has an equilibrium water content of 10% to 80% by weight and an oxygen permeability of 50 barrers to 180 barrers.

12. 12. The method of any one of claims 5 to 11, wherein the outer front and rear hydrogel layers, independently of each other, have a thickness of from 0.05 μm to 20 μm when fully hydrated.

13. The outer front and rear hydrogel layers may each independently comprise: (1) an alkyl(meth)acrylamide selected from the group consisting of (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-ethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-3-methoxypropyl(meth)acrylamide, and combinations thereof; (2) an alkyl(meth)acrylamide selected from the group consisting of N-2-hydroxyethyl(meth)acrylamide, N,N-bis(hydroxyethyl)(meth)acrylamide, N-3-hydroxypropyl(meth)acrylamide, N-2-hydroxypropyl(meth)acrylamide, N-2,3-dihydroxypropyl(meth)acrylamide, N-tris(hydroxymethyl)methyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, 3-hydroxypropyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, glycerol methacrylate, di(ethylene glycol) meth ... (3) a hydroxyl-containing acrylic monomer selected from the group consisting of 2-(meth)acrylamidoglycolic acid, (meth)acrylic acid, ethylacrylic acid, 3-(meth)acrylamidopropionic acid, 5-(meth)acrylamidopentanoic acid, 4-(meth)acrylamidobutanoic acid, 3-(meth)acrylamido-2-methylbutanoic acid, 3-(meth)acrylamido-3-methylbutanoic acid, 2-(meth)acrylamido-2-methyl-3,3-dimethylbutanoic acid, 3-(meth)acrylamidohexanoic acid, 4-(meth)acrylamido-3,3-dimethylhexanoic acid, and combinations thereof;(4) An amino-containing acrylic monomer selected from the group consisting of N-2-aminoethyl(meth)acrylamide, N-2-methylaminoethyl(meth)acrylamide, N-2-ethylaminoethyl(meth)acrylamide, N-2-dimethylaminoethyl(meth)acrylamide, N-3-aminopropyl(meth)acrylamide, N-3-methylaminopropyl(meth)acrylamide, N-3-dimethylaminopropyl(meth)acrylamide, 2-aminoethyl(meth)acrylate, 2-methylaminoethyl(meth)acrylate, 2-ethylaminoethyl(meth)acrylate, 3-aminopropyl(meth)acrylate, 3-methylaminopropyl(meth)acrylate, 3-ethylaminopropyl(meth)acrylate, 3-amino-2-hydroxypropyl(meth)acrylate, trimethylammonium 2-hydroxypropyl(meth)acrylate hydrochloride, dimethylaminoethyl(meth)acrylate, and combinations thereof;(5) N-vinylpyrrolidone, N-vinyl-3-methyl-2-pyrrolidone, N-vinyl-4-methyl-2-pyrrolidone, N-vinyl-5-methyl-2-pyrrolidone, N-vinyl-6-methyl-2-pyrrolidone, N-vinyl-3-ethyl-2-pyrrolidone, N-vinyl-4,5-dimethyl-2-pyrrolidone, N-vinyl-5,5-dimethyl-2-pyrrolidone, N-vinyl-3,3,5-trimethyl-2-pyrrolidone, N-vinylpiperidone, N-vinyl-3-methyl-2-piperidone, N-vinyl-4-methyl-2-piperidone, N-vinyl N-vinyl-5-methyl-2-piperidone, N-vinyl-6-methyl-2-piperidone, N-vinyl-6-ethyl-2-piperidone, N-vinyl-3,5-dimethyl-2-piperidone, N-vinyl-4,4-dimethyl-2-piperidone, N-vinylcaprolactam, N-vinyl-3-methyl-2-caprolactam, N-vinyl-4-methyl-2-caprolactam, N-vinyl-7-methyl-2-caprolactam, N-vinyl-7-ethyl-2-caprolactam, N-vinyl-3,5-dimethyl-2-caprolactam, N-vinyl-4,6-dimethyl (5) N-vinyl amide monomers selected from the group consisting of 1-methyl-3-methylene-2-pyrrolidone, 1-ethyl-3-methylene-2-pyrrolidone, 1-methyl-5-methylene-2-pyrrolidone, 1-ethyl-5-methyl ... methylene-containing pyrrolidone monomers selected from the group consisting of 1-n-propyl-3-methylene-2-pyrrolidone, 1-n-propyl-5-methylene-2-pyrrolidone, 1-isopropyl-3-methylene-2-pyrrolidone, 1-isopropyl-5-methylene-2-pyrrolidone, 1-n-butyl-3-methylene-2-pyrrolidone, 1-tert-butyl-3-methylene-2-pyrrolidone, and combinations thereof; (7) C; 1 ~C 4 C having an alkoxyethoxy group and having a number average molecular weight of 1500 or less, such as ethylene glycol methyl ether (meth)acrylate, di(ethylene glycol) methyl ether (meth)acrylate, tri(ethylene glycol) methyl ether (meth)acrylate, tetra(ethylene glycol) methyl ether (meth)acrylate, 1 ~C 4 - acrylic monomers selected from alkoxy poly(ethylene glycol) (meth)acrylates, methoxy-poly(ethylene glycol) ethyl (meth)acrylamides having a number average molecular weight of up to 1500, and combinations thereof; (8) vinyl ether monomers selected from the group consisting of ethylene glycol monovinyl ether, di(ethylene glycol) monovinyl ether, tri(ethylene glycol) monovinyl ether, tetra(ethylene glycol) monovinyl ether, poly(ethylene glycol) monovinyl ether, ethylene glycol methyl vinyl ether, di(ethylene glycol) methyl vinyl ether, tri(ethylene glycol) methyl vinyl ether, tetra(ethylene glycol) methyl vinyl ether, poly(ethylene glycol) methyl vinyl ether, and combinations thereof; (9) ethylene glycol monoallyl ether, di(ethylene glycol) monoallyl ether, tri(ethylene glycol) monoallyl ether, tetra(ethylene glycol) monoallyl ether, poly(ethylene glycol) monoallyl ether, (10) an allyl ether monomer selected from the group consisting of ethylene glycol methyl allyl ether, di(ethylene glycol) methyl allyl ether, tri(ethylene glycol) methyl allyl ether, tetra(ethylene glycol) methyl allyl ether, poly(ethylene glycol) methyl allyl ether, and combinations thereof; (11) an allyl ether monomer selected from the group consisting of (meth)acryloyloxyethyl phosphorylcholine, (meth)acryloyloxypropyl phosphorylcholine, 4-((meth)acryloyloxy)butyl-2'-(trimethylammonio)ethyl ethyl phosphate, 2-[(meth)acryloylamino]ethyl-2'-(trimethylammonio)-ethyl phosphate, 3-[(meth)acryloylamino]propyl-2'-(trimethylammonio)ethyl phosphate, 4-[(meth)acryloylamino]butyl-2'-(trimethylammonio)ethyl phosphate, 5-((meth)acryloyloxy)pentyl-2'-(trimethylammonio)ethyl phosphate, 6-((meth)acryloyloxy)hexyl-2'-(trimethylammonio)-ethyl phosphate,2-((meth)acryloyloxy)ethyl-2'-(triethylammonio)ethyl phosphate, 2-((meth)acryloyloxy)ethyl-2'-(tripropylammonio)ethyl phosphate, 2-((meth)acryloyloxy)ethyl-2'-(tributylammonio)ethyl phosphate, 2-((meth)acryloyloxy)propyl-2'-(trimethylammonio)-ethyl phosphate, 2-((meth)acryloyloxy)butyl-2'- (Trimethylammonio)ethyl phosphate, 2-((meth)acryloyloxy)pentyl-2'-(trimethylammonio)ethyl phosphate, 2-((meth)acryloyloxy)hexyl-2'-(trimethylammonio)ethyl phosphate, 2-(vinyloxy)ethyl-2'-(trimethylammonio)ethyl phosphate, 2-(allyloxy)ethyl-2'-(trimethylammonio)ethyl phosphate, 2-(vinyloxycarbonyl)ethyl 13. The method of any one of claims 1 to 12, wherein the crosslinked hydrophilic polymer-based material is a crosslinked hydrophilic polymer-based material comprising a polymer chain comprising repeating monomer units of at least one hydrophilic vinyl monomer comprising: phosphorylcholine-containing vinyl monomer selected from the group consisting of aryl-2'-(trimethylammonio)ethyl phosphate, 2-(allyloxycarbonyl)ethyl-2'-(trimethylammonio)-ethyl phosphate, 2-(vinylcarbonylamino)ethyl-2'-(trimethylammonio)ethyl phosphate, 2-(allyloxycarbonylamino)ethyl-2'-(trimethylammonio)ethyl phosphate, 2-(butenoyloxy)ethyl-2'-(trimethylammonio)ethyl phosphate, and combinations thereof; (11) allyl alcohol; (12) N-2-hydroxyethyl vinyl carbamate; (13) N-carboxyvinyl-β-alanine; (14) N-carboxyvinyl-α-alanine; (15) or combinations thereof.

14. The outer front and rear hydrogel layers are, independently of one another, crosslinked hydrophilic polymeric materials comprising poly(ethylene glycol) chains, the poly(ethylene glycol) chains being (1)-NH 2 (2) poly(ethylene glycol) having one unique functional group selected from the group consisting of -NH, -SH, -COOH, and epoxy groups; 2 (3) poly(ethylene glycol) having two terminal functional groups selected from the group consisting of -NH 2 13. The method of any one of claims 1 to 12, wherein the aryl group is a multi-arm poly(ethylene glycol) having one or more functional groups selected from the group consisting of -COOH, -SH, epoxy groups, and combinations thereof; or (4) directly derived from combinations thereof.

15. The method of any one of claims 1 to 14, wherein the outer front and rear hydrogel layers, independently of each other, have an equilibrium water content of at least 80% by weight.

16. The method of any one of claims 1 to 15, wherein the contact lens precursor inherently comprises first reactive functional groups on and / or adjacent to the anterior and posterior surfaces.

17. 16. The method of any one of claims 1 to 15, wherein the contact lens precursor is obtained by subjecting a preformed contact lens to a surface treatment to have the first reactive functional groups, the surface treatment comprising at least one process selected from the group consisting of: plasma treatment; chemical treatment; chemical vapor deposition; grafting (covalent bonding) of one or more compounds, each having at least one reactive functional group, onto the preformed contact lens; graft polymerization of one or more vinyl monomers, having at least one first reactive functional group, onto the preformed contact lens; layer-by-layer ("LbL") deposition of one or more polymer-based materials, having a first reactive functional group, onto the preformed contact lens; covalent bonding of one or more polymer-based materials, having a first reactive functional group, onto the preformed contact lens; and combinations thereof.

18. The method according to any one of claims 1 to 17, wherein the at least one hydrophilic polymer-based material is a highly branched hydrophilic polymer-based material comprising the second reactive functional group.

19. The method of claim 1, wherein the first reactive functional group is selected from the group consisting of a carboxyl group, an amino group, and combinations thereof, and the second reactive functional group is an azetidinium group.

Citation Information

Patent Citations

  • Silicone hydrogel lenses with a surface that has a high moisture content

    JP2013533517A

  • Contact lenses with a hydrophilic layer

    JP2015534106A

  • Weekly and monthly disposable water gradient contact lenses

    WO2019116139A1