Laminate, optical member, optical device, and manufacturing method for laminate

JP2024135394APending Publication Date: 2024-10-04NITTO DENKO CORP

Patent Information

Application Number
JP2023046050
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Benefits of technology

【0011】 本発明によれば、凹凸構造の凹部への粘接着剤の侵入が抑制されており、かつ、他の部材に対する接着力又は粘着力に優れた積層体、光学部材、光学装置及び積層体の製造方法を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135394000001_ABST
    Figure 2024135394000001_ABST
Patent Text Reader

Abstract

To provide a laminate with excellent adhesion or tackiness to other members, and capable of suppressing the intrusion of the adhesive into the recess of an uneven structure.SOLUTION: A laminate 100A is characterized by the following conditions: a first optical sheet 10a has a first principal plane 12s with an uneven structure and a second principal plane 18s of the opposite side from the first principal plane 12s; an adhesive layer 20a is arranged on the side of the first principal plane 12s of the first optical sheet 10a; the uneven structure owned by the first principal plane 12s includes multiple recesses 14 and a flat part 10s between two recesses 14 adjacent to each other among the multiple recesses 14; the flat part 10s of the first principal plane 12s is in contact with the adhesive layer 20a surface; the adhesive layer 20a includes a (meth)acrylic polymer; and the nano-indentation hardness measured by pushing an indenter by 2000 nm onto the adhesive layer 20a using a nano-indenter is equal to or greater than 0.1 MPa and is less than 2.0 MPa.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate, an optical member, an optical device, and a method for manufacturing a laminate. [Background technology]

[0002] An optical sheet having a concave-convex structure on its surface may be used with an adhesive layer disposed on the concave-convex surface. The optical sheet is used, for example, by being attached to another member such as a light guide layer by the adhesive layer (Patent Document 1).

[0003] According to Patent Document 1, when an adhesive layer is attached to a surface having a concave-convex structure of an optical sheet, the degree to which the adhesive layer penetrates (fills) the concaves of the concave-convex structure affects the function of the optical sheet. For this reason, Patent Document 1 proposes to provide an optical laminate having an adhesive layer that is restricted in the degree to which it penetrates into the concaves of the concave-convex structure of the optical sheet, and an optical device having such an optical laminate. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2022 / 176659 Summary of the Invention [Problem to be solved by the invention]

[0005] However, if the hardness of the adhesive or pressure-sensitive adhesive is increased too much in order to prevent it from penetrating into the recesses of the uneven structure, the adhesive strength may decrease, which may result in poor bonding to other components, whereas if the hardness of the adhesive or pressure-sensitive adhesive is decreased too much, the adhesive or pressure-sensitive adhesive may penetrate too far into the recesses of the uneven structure.

[0006] Therefore, an object of the present invention is to provide a laminate, an optical member, an optical device, and a method for manufacturing a laminate in which the intrusion of an adhesive into recesses of a concave-convex structure is suppressed and which has excellent adhesive strength or cohesive strength to other members. [Means for solving the problem]

[0007] In order to achieve the above object, the laminate of the present invention comprises: A first optical sheet and an adhesive layer are included, the first optical sheet has a first main surface having a concave-convex structure and a second main surface opposite to the first main surface; the adhesive layer is disposed on the first main surface side of the first optical sheet, the concave-convex structure of the first main surface includes a plurality of concave portions and a flat portion between two adjacent concave portions of the plurality of concave portions, The flat portion of the first main surface is in contact with a surface of the adhesive layer, The adhesive layer contains a (meth)acrylic polymer, The adhesive layer has a nanoindentation hardness of 0.1 MPa or more and 2.0 MPa or less, the nanoindentation hardness being measured by pressing an indenter 2000 nm into the adhesive layer using a nanoindenter.

[0008] The optical member of the present invention is characterized by including the laminate of the present invention.

[0009] The optical device of the present invention includes the optical member of the present invention.

[0010] The method for producing a laminate of the present invention includes a step of bonding the tacky adhesive layer and the first main surface of the first optical sheet. Effect of the Invention

[0011] According to the present invention, it is possible to provide a laminate, an optical member, an optical device, and a method for manufacturing a laminate in which the intrusion of an adhesive into recesses of a concave-convex structure is suppressed and which has excellent adhesive strength or cohesive strength to other members. [Brief description of the drawings]

[0012] [Figure 1A] FIG. 1A is a schematic cross-sectional view showing an example of the configuration of the optical laminate of the present invention. [Figure 1B] FIG. 1B is a schematic cross-sectional view showing another example of the configuration of the optical laminate of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an enlarged portion of the optical laminate of FIG. 1A. [Diagram 3] FIG. 3 is a schematic perspective view of a first optical sheet in the optical laminate of FIG. 1A. [Figure 4A] FIG. 4A is a schematic cross-sectional view showing an example of a lighting device including the optical laminate of FIG. 1A. [Figure 4B] FIG. 4B is a schematic cross-sectional view showing another example of a lighting device including the optical laminate of FIG. 1A. [Figure 5A] FIG. 5A is a schematic plan view showing another example of the first optical sheet in the optical laminate of the present invention. [Figure 5B] FIG. 5B is a schematic cross-sectional view of the first optical sheet of FIG. 5A. [Figure 6A] FIG. 6A is a schematic plan view showing yet another example of the first optical sheet in the optical laminate of the present invention. [Figure 6B] FIG. 6B is a schematic cross-sectional view of a recess in the first main surface of the first optical sheet in FIG. 6A. [Figure 6C] FIG. 6C is a schematic plan view of a recess in the first main surface of the first optical sheet in FIG. 6A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following description in any way.

[0014] In the present invention, the "adhesive layer" refers to a layer formed by at least one of a pressure-sensitive adhesive and an adhesive. In the present invention, unless otherwise specified, the "adhesive layer" may be an "adhesive layer" formed by a pressure-sensitive adhesive, an "adhesive layer" formed by an adhesive, or a layer containing both a pressure-sensitive adhesive and an adhesive. In addition, in the present invention, a pressure-sensitive adhesive and an adhesive may be collectively referred to as a "adhesive". In general, an agent having a relatively weak adhesive or bonding strength (e.g., an agent that allows the adherend to be peeled off again) may be called an "adhesive", and an agent having a relatively strong adhesive or bonding strength (e.g., an agent that does not allow the adherend to be peeled off again or is very difficult to peel off again) may be called an "adhesive". In the present invention, there is no clear distinction between a pressure-sensitive adhesive and an adhesive. In the present invention, there is no clear distinction between "adhesive strength" and "adhesive strength".

[0015] In the present invention, "on" or "on the surface" may refer to a state of being in direct contact with the surface or a state of being via another layer or the like.

[0016] In the laminate of the present invention, for example, the (meth)acrylic polymer may contain a nitrogen-containing monomer as a monomer unit. The nitrogen-containing monomer may be, for example, a heterocycle-containing acrylic monomer.

[0017] In the laminate of the present invention, for example, the (meth)acrylic polymer may be a (meth)acrylic polymer having a weight average molecular weight of 500,000 to 3,500,000 obtained by polymerizing, as monomer components, 3 to 20 wt % of a heterocycle-containing acrylic monomer (heterocycle-containing acrylate), 0.5 to 5 wt % of (meth)acrylic acid, 0.05 to 2 wt % of a hydroxyalkyl (meth)acrylate, and 83 to 96.45 wt % of an alkyl (meth)acrylate.

[0018] In the laminate of the present invention, for example, in the adhesive layer, the nitrogen-containing monomer may be a monomer having one or two reactive double bonds in one molecule. The monomer having one or two reactive double bonds in one molecule may be, for example, a heterocycle-containing acrylic monomer (heterocycle-containing acrylate).

[0019] In the laminate of the present invention, the gel fraction of the adhesive forming the adhesive layer may be, for example, 85% by weight or more, or may exceed 85% by weight, 90% by weight or more, 91% by weight or more, or 93% by weight or more, and may be, for example, 100% by weight or less, 99% by weight or less, or 98% by weight or less.

[0020] In the laminate of the present invention, the adhesive layer may be a layer formed by a method including, for example, a step of preparing an adhesive coating liquid containing a (meth)acrylic polymer, a step of applying the adhesive coating liquid to a substrate, and a step of drying the substrate coated with the adhesive coating liquid by heating. The laminate of the present invention may be formed, for example, from an adhesive coating liquid having a specific composition, and integrated with the void layer. This can suppress significant penetration of the adhesive layer into the void layer, especially under a long-term heat durability test. The adhesive coating liquid may further include, for example, a crosslinking agent, or may include other components as described below.

[0021] In the adhesive coating liquid for forming the adhesive layer in the laminate of the present invention, the nitrogen-containing monomer preferably has a small number of functional groups (the number of reactive double bonds in one molecule) in order to efficiently crosslink main chains in a graft reaction. For example, as described above, the number of reactive double bonds in one molecule is preferably one or two.

[0022] In addition, even if a monomer having one or two reactive double bonds is mixed during the production of the (meth)acrylic polymer, it is difficult to reduce the amount of the semi-high molecular weight polymer (which has a small molecular weight and is easily permeated into the voids of the void layer) as described above. However, according to the present invention, by using a pressure-sensitive adhesive coating liquid in which a monomer having one or two reactive double bonds is mixed into the (meth)acrylic polymer later and then crosslinking the adhesive, for example, the graft reaction as described above occurs, and the amount of the semi-high molecular weight polymer can be reduced.

[0023] In the present invention, "(meth)acrylic" means at least one of acrylic and methacrylic. For example, "(meth)acrylic acid" means at least one of acrylic acid and methacrylic acid. "(meth)acrylic acid ester" means at least one of acrylic acid ester and methacrylic acid ester. "(meth)acrylate" means at least one of methyl acrylate and methyl methacrylate.

[0024] In the present invention, the term "(meth)acrylic polymer" refers to a polymer having a structure obtained by polymerizing a component containing at least one selected from the group consisting of acrylic acid, methacrylic acid, acrylic acid esters, methacrylic acid esters, monomers having an acryloyl group, and monomers having a methacryloyl group. The component may or may not contain a substance other than at least one selected from the group consisting of acrylic acid, methacrylic acid, acrylic acid esters, methacrylic acid esters, monomers having an acryloyl group, and monomers having a methacryloyl group.

[0025] In the present invention, the "acrylic monomer" refers to, for example, a monomer including at least one selected from the group consisting of acrylic acid, an acrylic ester, and a monomer having an acryloyl group.

[0026] In the present invention, the "isocyanate-based crosslinking agent" refers to, for example, a crosslinking agent having an isocyanate group (isocyanato group) in the molecule. In the present invention, the number of isocyanate groups (isocyanato groups) in one molecule of the isocyanate-based crosslinking agent is not particularly limited, but is preferably 2 or more, and may be, for example, 2, 3, or 4, and the upper limit is not particularly limited, but is, for example, 10 or less.

[0027] In the present invention, the "epoxy crosslinking agent" refers to, for example, a crosslinking agent having an epoxy group in the molecule. In the present invention, the number of epoxy groups in one molecule of the epoxy crosslinking agent is not particularly limited, but is preferably 2 or more, and may be, for example, 2, 3, or 4, and the upper limit is not particularly limited, but is, for example, 10 or less.

[0028] [1. Laminate, optical member, and optical device] As described above, the laminate of the present invention comprises a first optical sheet and an adhesive layer, the first optical sheet having a first main surface having a concave-convex structure and a second main surface opposite the first main surface, the adhesive layer is arranged on the first main surface side of the first optical sheet, the concave-convex structure of the first main surface comprises a plurality of recesses and a flat portion between two adjacent recesses among the plurality of recesses, the flat portion of the first main surface is in contact with a surface of the adhesive layer, the adhesive layer comprises a (meth)acrylic polymer, and is characterized in that the nanoindentation hardness measured by pressing an indenter 2000 nm into the adhesive layer using a nanoindenter is 0.1 MPa or more and 2.0 MPa or less.

[0029] The configuration of the laminate of the present invention will be described by way of examples with reference to Figures 1A, 1B, 2, 3, 4A, and 4B. Although Figures 1A, 1B, 2, 3, 4A, and 4B are cross-sectional views, hatching has been appropriately simplified or omitted for ease of viewing.

[0030] FIG. 1A shows a schematic cross-sectional view of an optical laminate 100A according to one embodiment of the present invention. FIG. 1B shows a schematic cross-sectional view of an optical laminate 101A according to another embodiment of the present invention. FIG. 2 is a schematic cross-sectional view showing an enlarged portion of the optical laminate 100A. FIG. 3 is a schematic perspective view of an optical sheet 10a included in the optical laminate 100A. FIG. 4A is a schematic cross-sectional view of an illumination device 200A including the optical laminate 100A.

[0031] As shown in FIG. 1A, the optical laminate 100A includes a first optical sheet 10a and a tacky adhesive layer 20a. The tacky adhesive layer 20a may be, for example, a pressure-sensitive adhesive layer formed of a pressure-sensitive adhesive, or an adhesive layer formed of an adhesive. The first optical sheet 10a has a first main surface 12s having an uneven structure and a second main surface 18s opposite to the first main surface 12s. The tacky adhesive layer 20a is disposed on the first main surface 12s side of the first optical sheet 10a. The uneven structure of the first main surface 12s includes a plurality of recesses 14 and a flat portion 10s between two adjacent recesses 14 among the plurality of recesses 14. The flat portion 10s of the first main surface 12s is in contact with the tacky adhesive layer 20a. The tacky adhesive layer 20a includes a (meth)acrylic polymer. The nanoindentation hardness measured by pressing an indenter 2000 nm into the adhesive layer 20a using a nanoindenter is 0.1 MPa or more and 2.0 MPa or less. In addition, as shown in Fig. 1A, the recess 14 of the first main surface forms an internal space (space) 14a between the recess 14 and the surface of the adhesive layer 20a.

[0032] The optical laminate 101A shown in FIG. 1B is an example in which the optical laminate of the present invention further includes other components in addition to the first optical sheet and the tacky adhesive layer. As shown in the figure, this optical laminate 101A has an optical laminate 100A and a second optical sheet 30 arranged on the side opposite to the first optical sheet 10a side of the tacky adhesive layer 20a. The optical laminate 100A in FIG. 1B is the same as the optical laminate 100A in FIG. 1A. The explanation of the optical laminate 100A also applies to the optical laminate 101A unless otherwise specified, so the explanation may be omitted to avoid duplication.

[0033] The second optical sheet 30 of the optical laminate 101A has a main surface 38s on the adhesive layer 20a side and a main surface 32s opposite to the main surface 38s. The main surface 38s is a flat surface. Although not shown in FIG. 1B, at least one other optical member (e.g., an optical sheet) may be disposed on the side opposite to the adhesive layer 20a in the second optical sheet 30 of the optical laminate 101A (i.e., on the main surface 32s). The other optical member (or optical sheet) is not particularly limited, and examples thereof include a diffusion plate and a light guide plate. The other optical member may be adhered to the main surface 32s of the optical sheet 30 via an adhesive layer, for example.

[0034] As described above, FIG. 2 is a schematic cross-sectional view showing an enlarged portion of the optical laminate 100A. In the examples of FIG. 1A and FIG. 2, the adhesive layer 20a does not penetrate into the recess 14. That is, the adhesive layer 20a does not exist in the space defined by the recess 14. The space defined by the recess 14 refers to a space defined by the recess 14 and a sheet surface (a surface parallel to the XY plane) including the flat portion 10s adjacent to the recess 14. Therefore, the internal space 14a defined by the surface 28s of the adhesive layer 20a on the first optical sheet 10a side and the first main surface 12s of the first optical sheet 10a coincides with the space defined by the recess 14 in this example. Hereinafter, the internal space 14a may be referred to as an air cavity or an optical cavity. The internal space 14a is typically a void portion filled with air. However, the internal space 14a may be filled with a material having a lower refractive index than the first optical sheet 10a and the tacky adhesive layer 20a instead of air. As described above, FIG. 3 is a schematic perspective view of the optical sheet 10a included in the optical laminate 100A. In a plan view (XY plane) of the optical sheet seen from the normal direction of the main surface, the multiple internal spaces may be internal spaces (e.g., triangular prism-shaped grooves extending in the X direction) that are continuous in the X direction as in the example of FIG. 3, and may be discretely provided in the Y direction, or may be discretely provided in the X direction and the Y direction as in the example of FIG. 5A described later. Note that, as shown in FIGS. 4A and 4B described later, in a lighting device having the optical laminate 100A, the light guide direction of the light guide layer 80 is the -Y direction. Although light propagates in various directions within the light-guiding layer 80, in the following, the -Y direction is referred to as the light-guiding direction, and light that has a -Y-direction component (i.e., the -Y-direction component is not zero) is defined as propagating in the -Y direction.

[0035] The optical laminate 100A functions as a light distribution structure as described in, for example, WO 2011 / 124765 or WO 2019 / 087118. That is, the optical laminate 100A has a plurality of internal spaces 14a that form interfaces that direct light in the Z direction (downward in the figure) by total internal reflection. The internal space 14a is defined by a surface 16s and a surface 17s that are part of the first main surface 12s of the first optical sheet 10a, and a surface 28s on the first optical sheet 10a side of the adhesive layer 20a. Here, the cross-sectional shape of the internal space 14a (the shape of a cross section perpendicular to the X direction and parallel to the YZ plane) is triangular. The interface formed by the inclined surface 16s functions as an interface that directs light in the Z direction (downward in the figure) by total internal reflection. Each of the recesses 14, i.e., each of the internal spaces 14a, has an inclined surface (first inclined surface) 16s that directs a part of the light propagating in the optical laminate 100A toward the second main surface 18s side of the first optical sheet 10a (Z direction in the figure) by total internal reflection, and an inclined surface (second inclined surface) 17s on the opposite side to the inclined surface 16s. The inclination angle θa of the inclined surface 16s is, for example, 10° or more and 70° or less. The lower limit is preferably 30° or more, more preferably 45° or more. If the inclination angle θa is smaller than 10°, the controllability of the light distribution may decrease, and the light extraction efficiency may also decrease. On the other hand, if the inclination angle θa exceeds 70°, for example, processing of the shaped film may become difficult. In addition, the inclination angle θb of the inclined surface 17s is, for example, 50° or more and 100° or less. The lower limit is preferably 70° or more. If the inclination angle θb is smaller than 50°, stray light may occur in an unintended direction. On the other hand, if the inclination angle θb exceeds 100°, for example, processing of a shaped film may become difficult. The inclination angle θa of the inclined surface 16s and the inclination angle θb of the inclined surface 17s are angles with respect to a direction parallel to the Y direction in a cross section of the recess 14 (a cross section perpendicular to the X direction and parallel to the YZ plane). In this example, the inclination angle θa of the inclined surface 16s is smaller than the inclination angle θb of the inclined surface 17s. In a lighting device having the optical laminate 100A (see FIG. 4A and FIG. 4B), the inclined surface 16s is disposed closer to the light source 60 than the inclined surface 17s.The cross-sectional shape of the internal space 14a (cross-sectional shape perpendicular to the X direction and parallel to the YZ plane) is determined by the inclination angle θa of the inclined surface 16s and the inclination angle θb of the inclined surface 17s, the width Wy, and the depth C. The shape of the internal space 14a (recess 14) is not limited to the illustrated one, and may be modified in various ways. By adjusting the shape, size, arrangement density, etc. of the internal space 14a (recess 14), the distribution (light distribution) of the light beams emitted from the optical laminate 100A can be adjusted (see, for example, Patent Documents 2 and 3).

[0036] The optical laminate functioning as the light distribution control structure can be configured to have one or both of the functions of a light guide layer having a plurality of internal spaces and a direction conversion layer. For example, as shown in FIG. 4A, the optical laminate 100A can be used in a lighting device 200A. As shown in FIG. 4A, the lighting device 200A includes an optical laminate 102A and a light source 60. As shown in the figure, the optical laminate 102A has the optical laminate 100A and a light guide layer 80 provided on the side opposite to the first optical sheet 10a side in the adhesive layer 20a of the optical laminate 100A. The light guide layer 80 is bonded to, for example, a surface 22s on the side opposite to the first optical sheet 10a side in the adhesive layer 20a. The light guide layer 80 has a first main surface 80a, a second main surface 80b opposite to the first main surface 80a, and a light receiving unit 80c that receives light emitted from the light source 60. The light source 60 is not particularly limited, but may be, for example, an LED device, and a plurality of LED devices may be arranged for use. A part of the light guided into the light guide layer 80 is totally internally reflected (TIR) ​​at the interface 16s and the interface 14s formed by the internal space 14a, as shown by the arrow in Fig. 4A. The light totally internally reflected at the interface 14s (the surface 28s of the adhesive layer 20a on the first optical sheet side) propagates through the light guide layer 80 and the adhesive layer 20a, and the light totally internally reflected at the inclined surface 16s is emitted to the outside of the optical laminate 102A from the second main surface 18s side of the first optical sheet 10a.

[0037] The refractive indexes of the light guide layer 80, the adhesive layer 20a, and the first optical sheet 10a are not particularly limited, but are preferably approximately equal to each other. The difference (absolute value) in the refractive index between the light guide layer 80 and the adhesive layer 20a, and the difference (absolute value) in the refractive index between the adhesive layer 20a and the first optical sheet 10a are each independently preferably 0.20 or less, more preferably 0.15 or less, and even more preferably 0.10 or less. The lower limit of the absolute value is not particularly limited, but is, for example, 0 or a numerical value exceeding 0.

[0038] The thickness of the adhesive layer 20a is not particularly limited, and may be, for example, 0.01 μm or more and 50.0 μm or less. The lower limit of the thickness of the adhesive layer 20a is preferably 1.0 μm or more. The upper limit of the thickness of the adhesive layer 20a is preferably 30.0 μm or less, and more preferably 20.0 μm or less. Unless otherwise specified, the thickness of the adhesive layer refers to the thickness on the flat portion 10s of the first main surface 12s of the first optical sheet 10a.

[0039] The haze value of the optical laminate 100A is not particularly limited, but is, for example, 5.0% or less. The lower limit of the haze value is not particularly limited, but is, for example, 0% or a value exceeding 0%. The haze value can be measured, for example, using a haze meter (device name "HZ-1", manufactured by Suga Test Instruments Co., Ltd.) under D65 light.

[0040] FIG. 4B is an example in which the light guide layer 80A in the lighting device 200A in FIG. 4A is disposed at a different position from that in the lighting device 200A in FIG. 4A. As in the lighting device 200B shown in FIG. 4B, the light guide layer 80 may be provided on the first optical sheet 10a side of the optical laminate 100A (closer to the first optical sheet 10a than the visco-adhesive layer 20a). The light guide layer 80 and the first optical sheet 10a may be attached via, for example, a visco-adhesive layer (not shown). In the lighting device 200B, too, the light totally internally reflected at the interface 14s (the surface 28s of the visco-adhesive layer 20a on the first optical sheet side) propagates through the visco-adhesive layer 20a, and the light totally internally reflected at the inclined surface 16s is emitted to the outside of the optical laminate 102B from the second main surface 18s side of the first optical sheet 10a.

[0041] As described above, an example of the lighting device of the present invention is shown in FIG. 4A and FIG. 4B, respectively. The lighting device of the present invention is an example of the optical device of the present invention. However, the optical device of the present invention is not limited to only the lighting device. The optical device of the present invention and the lighting device of the present invention are not limited to the examples of FIG. 4A and FIG. 4B, and various modifications are possible. For example, a base layer may be provided on the side opposite the light guide layer 80 of the optical laminate 100A in the lighting device 200A. An anti-reflection layer may be provided instead of the base layer, and a hard coat layer (for example, having a pencil hardness of H or more) may be provided instead of the base layer. For example, one or both of the anti-reflection layer and the hard coat layer may be provided on the base layer. For example, one or both of the anti-reflection layer and the hard coat layer may be provided on the side opposite the exit surface of the light guide layer 80 (upper side in the figure). The anti-reflection layer and the hard coat layer can be formed, for example, by using a known material and a known method. Furthermore, for example, a low refractive index layer may be provided between the optical laminate 102A and the base layer (or one or both of the antireflection layer and the hard coat layer).

[0042] In the example of the lighting device 200B, a base layer may be provided on the side of the optical laminate 100A opposite to the light guide layer 80. Instead of the base layer, one or both of an antireflection layer and a hard coat layer (e.g., having a pencil hardness of H or more) may be provided, and one or both of an antireflection layer and a hard coat layer may be provided on the base layer. In addition, one or both of an antireflection layer and a hard coat layer may be provided on the exit surface side (lower side in the figure) of the light guide layer 80. A low refractive index layer may be provided between the optical laminate 102B and the base layer (or one or both of the antireflection layer and the hard coat layer).

[0043] As shown in FIG. 3, when the first optical sheet 10a of FIG. 1A, FIG. 1B, FIG. 2, FIG. 4A, and FIG. 4B is viewed in a plan view from the normal direction of the first main surface 12s, each of the multiple recesses 14 extends in the X direction and is continuous in the X direction. The multiple recesses 14 are arranged discretely in the Y direction, and flat portions 10s are provided between the recesses 14. In the Y direction, the recesses 14 are preferably arranged periodically in the Y direction, and the pitch Py is, for example, 6 μm or more and 120 μm or less. The width Wy of the recess 14 is, for example, 3 μm or more and 20 μm or less, and the width Dy of the flat portion 10s is, for example, 3 μm or more and 100 μm or less. The ratio Wy / Dy of the width Wy of the recess 14 to the width Dy of the flat portion 10s is, for example, 0.3 or more and 7 or less. The depth C (depth in the Z direction) of the recess 14 is, for example, 1 μm or more and 100 μm or less. The depth C of the recess 14 is preferably 20 μm or less, more preferably 12 μm or less. The depth C of the recess 14 is preferably 4 μm or more, more preferably 6 μm or more, and more preferably 8 μm or more.

[0044] The density of the recesses 14 is preferably 0.3% or more in terms of obtaining good brightness, in terms of the ratio (occupancy rate) of the area of ​​the recesses 14 to the area of ​​the first optical sheet 10a when the first optical sheet 10a is viewed in a plane from the normal direction of the first main surface 12s. The occupancy rate of the recesses 14 is appropriately selected depending on the application, and for example, in an application requiring transparency, it is preferably 0.3% or more and 10% or less, and more preferably 0.5% or more and 4% or less. In an application requiring higher brightness, it is preferably 30% or more and 80% or less. The occupancy rate of the recesses 14 may be uniform, or may be increased as the distance from the light source (for example, the light source 60 in FIG. 4A or FIG. 4B) increases so that the brightness does not decrease even if the distance from the light source increases.

[0045] In the laminate of the present invention, the first optical sheet is not limited to the first optical sheet 10a shown in FIG. 1A to FIG. 4B. For example, instead of the first optical sheet 10a, the unevenly shaped film 70 (optical sheet) shown in FIG. 5A and FIG. 5B may be used as the first optical sheet. The unevenly shaped film 70 has a main surface having an uneven structure, and the uneven structure has a plurality of recesses 74 and flat portions 72s between adjacent recesses 74. When the shaped film 70 is viewed in a plan view from the normal direction of the main surface (see, for example, FIG. 5A), the plurality of recesses 74 are arranged in a discrete island shape in both the X direction and the Y direction. In the shaped film 70, the size of the recesses 74 (length L, width W: see FIG. 5A and FIG. 5B) is, for example, preferably 10 μm or more and 500 μm or less for the length L and 1 μm or more and 100 μm or less for the width W. In addition, from the viewpoint of light extraction efficiency, the depth H is preferably 1 μm or more and 100 μm or less. The depth H of the recess 14 is preferably 20 μm or less, more preferably 12 μm or less. The depth H of the recess 14 is preferably 4 μm or more, more preferably 6 μm or more, and more preferably 8 μm or more. When the recesses 74 are distributed discretely and uniformly, they are preferably arranged periodically, for example, as shown in FIG. 5A. The pitch Px is preferably, for example, 10 μm or more and 500 μm or less, and the pitch Py is preferably, for example, 10 μm or more and 500 μm or less. It should be noted that the present invention is not limited to the example of FIG. 5A, and the recesses may be arranged discretely in the light guide direction of the light guide layer and in a direction intersecting the light guide direction of the light guide layer when used in a lighting device.

[0046] The density of the recesses 74 is not particularly limited, but when the shaped film 70 is viewed in a plan view from the normal direction of the main surface (FIG. 5A), the ratio of the area of ​​the recesses 74 to the area of ​​the shaped film 70 (occupancy rate) is preferably 0.3% or more from the viewpoint of obtaining good brightness. The occupancy rate of the recesses 74 is appropriately selected depending on the application to be used. For example, in an application requiring transparency, it is preferably 30% or less in order to obtain good visible light transmittance and haze value, and is preferably 1% or more in order to obtain good brightness. The upper limit is more preferably 25% or less, and in order to obtain a high visible light transmittance, it is preferably 10% or less, and more preferably 5% or less. For example, it is preferably 0.3% or more and 10% or less, and more preferably 0.5% or more and 4% or less. In an application requiring higher brightness, it is preferably 30% or more and 80% or less. The occupancy rate of the multiple recesses 74 may be uniform, or may increase with increasing distance from a light source (e.g., light source 60 in FIG. 4A or FIG. 4B) so that the brightness does not decrease even if the distance from the light source increases.

[0047] 1A to 4B show an example in which the cross-sectional shape of the recesses 14 is a triangle. However, the cross-sectional shape of the recesses 14 is not limited to this, and for example, the cross-sectional shape of the recesses 14 may be any shape having a surface that can form an interface that directs light in the Z direction by total internal reflection. The cross-sectional shape of the recesses 14 may be, for example, a quadrangle (e.g., a trapezoid), and is not limited to a polygon, and may be a shape including a curve.

[0048] The laminate of the present invention may use, for example, a concave-convex shaped film 82 (optical sheet) shown in FIG. 6A as the first optical sheet, instead of the first optical sheet 10a of FIG. 1A to FIG. 4B. FIG. 6A also shows a light source 60. The concave-convex shaped film 82 has a main surface having a concave-convex structure, and the concave-convex structure has a plurality of recesses 84 and flat portions 82s between adjacent recesses 84. Each of the plurality of recesses 84 has a first inclined surface 86s that directs a part of the light propagating in the optical laminate in the Z direction by total internal reflection, and a second inclined surface 87s on the opposite side to the first inclined surface 86s. As shown in FIG. 6A, when viewed in a plan view from the normal direction of the main surface having the concave-convex structure of the concave-convex shaped film 82, the first inclined surface 86s of the recess 84 forms a curved surface that is convex toward the light source 60 side. When a plurality of LED devices arranged in the X direction are used as the light source 60, the light emitted from each LED device has a spread in the Y direction, so that the first inclined surface 86s acts uniformly on the light if the first inclined surface 86s has a curved surface convex toward the light source 60 side. In addition, when a coupling optical system is provided between the light source 60 and the light receiving section 80c of the light guide layer 80 and light with high parallelism (light with small spread in the Y direction) is made to enter, the first inclined surface 86s may be parallel to the X direction. The preferable ranges of the size (length L, width W: see Figs. 6B and 6C), depth H (see Fig. 6B), and pitches Px and Py of the recesses 84 may be the same as those of the recesses 74 of the unevenness-forming film 70, for example.

[0049] The method for producing the optical laminate 100A is not particularly limited, but for example, the optical laminate 100A can be produced by attaching the adhesive layer 20a to the surface 12s having the uneven structure of the first optical sheet 10a by, for example, a roll-to-roll method. From the viewpoint of mass productivity, it is preferable to produce the optical laminate 100A by the roll-to-roll method.

[0050] In the adhesive layer of the laminate of the present invention, the nanoindentation hardness measured by pressing an indenter 2000 nm into the adhesive layer using a nanoindenter (hereinafter, sometimes referred to as "nanoindentation hardness") is 0.1 MPa or more and 2.0 MPa or less, as described above. The nanoindentation hardness of the adhesive layer needs to be neither too low nor too high from the viewpoint of suppressing the intrusion into the recesses of the uneven structure and maintaining the adhesive or cohesive strength to other members. The upper limit of the nanoindentation hardness of the adhesive layer may be, for example, 1.5 MPa or less, 1.0 MPa or less, 0.6 MPa or less, 0.55 MPa or less, or 0.25 MPa or less. The lower limit of the nanoindentation hardness of the adhesive layer may be, for example, 0.11 MPa or more, 0.13 MPa or more, or 0.18 MPa or more. The nanoindentation hardness of the adhesive layer is, for example, 0.11 to 2.0 MPa, 0.13 to 2.0 MPa, 0.18 to 2.0 MPa, 0.10 to 1.5 MPa, 0.11 to 1.5 MPa, 0.13 to 1.5 MPa, 0.18 to 1.5 MPa, 0.10 to 1.0 MPa, 0.11 to 1.0 MPa, 0.13 to 1.0 MPa, 0.18 to 1.0 MPa, 0 The pressure may be 0.10 to 0.6 MPa, 0.11 to 0.6 MPa, 0.13 to 0.6 MPa, 0.18 to 0.6 MPa, 0.10 to 0.55 MPa, 0.11 to 0.55 MPa, 0.13 to 0.55 MPa, 0.18 to 0.55 MPa, 0.10 to 0.25 MPa, 0.11 to 0.25 MPa, 0.13 to 0.25 MPa, or 0.18 to 0.25 MPa.

[0051] In addition, the laminate of the present invention may or may not include other components other than the first optical sheet and the tacky adhesive layer. The other components are not particularly limited, and are, for example, as described with reference to Figs. 1A to 6C. Furthermore, the other components may be any other components, for example, an optical functional layer. The optical functional layer is also not particularly limited, and may be, for example, an optical functional layer used in a general optical film, for example, a microlens film, a prism film, a diffusion film, a polarizing reflective film, a polarizing film, a retardation film, a high refractive index layer, etc.

[0052] The laminate of the present invention may have a light transmittance of 80% or more of the laminate of the first optical sheet and the adhesive layer. The laminate may have a haze of 3% or less. The light transmittance may be, for example, 82% or more, 84% or more, 86% or more, or 88% or more, and the upper limit is not particularly limited, but is ideally 100%, and may be, for example, 95% or less, 92% or less, 91% or less, or 90% or less. The haze of the laminate may be measured, for example, by the same method as that for measuring the haze of the void layer described later. The light transmittance is the transmittance of light having a wavelength of 550 nm, and may be measured, for example, by the following measurement method.

[0053] (Method of measuring light transmittance) The laminate is treated as a sample to be measured using a spectrophotometer U-4100 (trade name of Hitachi, Ltd.). The total light transmittance (light transmittance) of the sample is measured when the total light transmittance of air is taken as 100%. The total light transmittance (light transmittance) value is taken as the value measured at a wavelength of 550 nm.

[0054] In the laminate of the present invention, for example, the 180° peel adhesion of the adhesive layer to PMMA (polymethyl methacrylate) (hereinafter, sometimes simply referred to as "PMMA adhesion" or "PMMA adhesive strength") is preferably, for example, 1.0 N / 20 mm or more. From the viewpoint of the risk of peeling during handling when the laminate of the present invention is attached to another member (e.g., another layer), it is preferable that the PMMA adhesive strength is not too low. The PMMA adhesive strength may be, for example, 2.0 N / 20 mm or more, 3.0 N / 20 mm or more, 4.0 N / 20 mm or more, 5.0 N / 20 mm or more, or 6.0 N / 20 mm or more, and may be, for example, 50 N / 20 mm or less, 40 N / 20 mm or less, 30 N / 20 mm or less, 20 N / 20 mm or less, or 10 N / 20 mm or less. The PMMA adhesive strength in the laminate of the present invention can be measured, for example, as follows.

[0055] <Method for Measuring Adhesion of PMMA> Cut the laminate of the present invention into a width of 20 mm to expose the adhesive layer disposed on the first main surface side of the first optical sheet. This is used as a test piece, and the PMMA adhesion force (mN / 20 mm) is measured. Alternatively, instead of this test piece, the PMMA adhesion force (mN / 20 mm) may be measured in the same manner using an alternative test piece manufactured as follows. The manufacturing method of the alternative test piece is as follows: First, on one side of a separator film (for example, a polyethylene terephthalate film treated with a silicone-based release agent: manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., MRF38), the same adhesive layer as the adhesive layer disposed on the first main surface side of the first optical sheet in the laminate of the present invention is formed. Next, the adhesive layer is bonded to a polyethylene terephthalate (PET) film with a thickness of 25 μm (for example, trade name "Lumirror S-10", manufactured by Toray Industries, Inc.). It is cut into a width of 20 mm, the peeled PET film is peeled off, and the surface of the exposed adhesive layer is bonded to a polymethyl methacrylate (PMMA) plate (for example, trade name "Acrylite", manufactured by Mitsubishi Chemical Corporation) to obtain the alternative test piece, and the PMMA adhesion force (mN / 20 mm) is measured. Specifically, the method for measuring the PMMA adhesion force (mN / 20 mm) is as follows: When bonding to the PMMA plate, crimping is performed once with a 2 kg roller, and 30 minutes after bonding, a tensile-compression tester (device name "AGS-50NX", manufactured by Shimadzu Corporation) is used to measure the 180° peel adhesion force under the following conditions. The measured value of this peel adhesion force is taken as the PMMA adhesion force. Peeling speed: 300 mm / min Measurement conditions: Temperature: 23 ± 2°C, Humidity: 65 ± 5%RH

[0056] The laminate of the present invention may be formed on a substrate such as a film. The film may be, for example, a resin film. In general, those with a relatively small thickness are called "films", and those with a relatively large thickness are called "sheets" for distinction, but in the present invention, there is no particular distinction between "films" and "sheets".

[0057] The substrate is not particularly limited, and for example, a substrate made of a thermoplastic resin, a substrate made of glass, an inorganic substrate such as silicon, a plastic molded from a thermosetting resin, an element such as a semiconductor, a carbon fiber material such as a carbon nanotube, etc. can be preferably used, but is not limited thereto. The form of the substrate can be, for example, a film, a plate, etc. Examples of the thermoplastic resin include polyethylene terephthalate (PET), acrylic, cellulose acetate propionate (CAP), cycloolefin polymer (COP), triacetyl cellulose (TAC), polyethylene naphthalate (PEN), polyethylene (PE), polypropylene (PP), etc.

[0058] The optical member of the present invention is not particularly limited, and may be, for example, an optical film including the laminate of the present invention.

[0059] The optical apparatus (optical device) of the present invention is not particularly limited, and may be, for example, an image display apparatus or a lighting apparatus. Examples of the image display apparatus include a liquid crystal display, an organic EL (Electro Luminescence) display, and a micro LED (Light Emitting Diode) display. Examples of the lighting apparatus include an organic EL lighting apparatus.

[0060] [3. Adhesive coating fluid] In the laminate of the present invention, the adhesive layer can be formed, for example, using an adhesive coating liquid, as described above. In the present invention, the "adhesive" and the "adhesive" are not necessarily clearly distinguishable, as described below. In the present invention, the term "adhesive" includes both the "adhesive" and the "adhesive" unless otherwise specified. The adhesive coating liquid may be, for example, an adhesive coating liquid containing the (meth)acrylic polymer, or may be, for example, an adhesive coating liquid further containing a crosslinking agent (e.g., an isocyanate crosslinking agent), or may further contain, for example, a monomer having one or two reactive double bonds in one molecule and an organic peroxide. The adhesive coating liquid is not particularly limited, but is, for example, as shown below.

[0061] In the adhesive layer of the laminate of the present invention, the (meth)acrylic polymer may be substantially free of a (meth)acrylic polymer having a polystyrene-equivalent molecular weight of 100,000 or less.

[0062] In the laminate of the present invention, for example, the content of the (meth)acrylic polymer having a polystyrene-equivalent molecular weight of 100,000 or less in the (meth)acrylic polymer may be 10% by weight or less, 5% by weight or less, 1% by weight or less, 0.5% by weight or less, or less than 0.1% by weight. The lower limit of the content of the (meth)acrylic polymer having a polystyrene-equivalent molecular weight of 100,000 or less in the (meth)acrylic polymer is not particularly limited, but is, for example, 0% by weight (i.e., does not include the (meth)acrylic polymer having a polystyrene-equivalent molecular weight of 100,000 or less) or a value exceeding 0% by weight.

[0063] In the laminate of the present invention, for example, the (meth)acrylic polymer may be substantially free of a (meth)acrylic polymer having a polystyrene-equivalent molecular weight of 30 million or more.

[0064] In the laminate of the present invention, for example, the content of the (meth)acrylic polymer having a polystyrene-equivalent molecular weight of 30 million or more in the (meth)acrylic polymer may be 10% by weight or less, 5% by weight or less, 1% by weight or less, 0.5% by weight or less, or less than 0.1% by weight. The lower limit of the content of the (meth)acrylic polymer having a polystyrene-equivalent molecular weight of 30 million or more in the (meth)acrylic polymer is not particularly limited, but is, for example, 0% by weight (i.e., does not include the (meth)acrylic polymer having a polystyrene-equivalent molecular weight of 30 million or more) or a value exceeding 0% by weight.

[0065] The (meth)acrylic polymer may contain, for example, 1 to 30% by weight, and preferably 3 to 25% by weight or 3 to 20% by weight, of a nitrogen-containing monomer as a monomer unit. The (meth)acrylic polymer may have, for example, a polydispersity (weight average molecular weight (Mw) / number average molecular weight (Mn)) of 3.0 or less. The lower limit of the polydispersity is not particularly limited, and is, for example, 1.0 or more, 1.5 or more, or 2.0 or more. The adhesive coating liquid may be, for example, an adhesive coating liquid containing the (meth)acrylic polymer.

[0066] The pressure-sensitive adhesive coating liquid may be, for example, a (meth)acrylic polymer containing, as monomer components, 3 to 20% by weight of a heterocycle-containing acrylic monomer, a (meth)acrylic polymer having a polymerizable functional group, 0.5 to 5% by weight of (meth)acrylic acid, 0.05 to 2% by weight of a hydroxyalkyl (meth)acrylate, and 83 to 96.45% by weight of an alkyl (meth)acrylate, and this (meth)acrylic polymer may be used as a base polymer.

[0067] As the heterocycle-containing acrylic monomer, for example, one having a polymerizable functional group and a heterocycle can be used without any particular limitation. Examples of the polymerizable functional group include a (meth)acryloyl group and a vinyl ether group. Among these, a (meth)acryloyl group is preferred. Examples of the heterocycle include a morpholine ring, a piperidine ring, a pyrrolidine ring, and a piperazine ring. Examples of the heterocycle-containing acrylic monomer include N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, and N-acryloylpyrrolidine. Among these, N-acryloylmorpholine is preferred. The heterocycle-containing acrylic monomer can improve both the heat resistance and the moisture resistance of the adhesive layer (adhesive layer) when the adhesive layer is thinned. In the following, N-acryloylmorpholine may be referred to as "ACMO".

[0068] In addition, the heterocycle-containing acrylic monomer is preferable in that it can improve the adhesive strength of the pressure-sensitive adhesive layer (adhesive layer) to the optical film. In particular, it is preferable in that it can improve the adhesive strength to cyclic polyolefins such as norbornene-based resins, and is suitable when cyclic polyolefins are used as the optical film.

[0069] The heterocycle-containing acrylic monomer is used, for example, at a ratio of 3 to 20% by weight based on the total amount of monomer components forming the (meth)acrylic polymer. The ratio of the heterocycle-containing acrylic monomer may be, for example, 4 to 19% by weight or 6 to 18% by weight. The ratio of the heterocycle-containing acrylic monomer is preferably not less than the above range from the viewpoint of heat resistance and moisture resistance when the pressure-sensitive adhesive layer (adhesive layer) is thinned. In addition, the ratio of the heterocycle-containing acrylic monomer is preferably not more than the above range from the viewpoint of moisture resistance when the pressure-sensitive adhesive layer (adhesive layer) is thinned. In addition, the ratio of the heterocycle-containing acrylic monomer is preferably not more than the above range from the viewpoint of improving the adhesion of the pressure-sensitive adhesive layer (adhesive layer). In addition, the ratio of the heterocycle-containing acrylic monomer is preferably not more than the above range from the viewpoint of adhesive strength.

[0070] As the (meth)acrylic acid, acrylic acid is particularly preferred.

[0071] The (meth)acrylic acid is used, for example, in a proportion of 0.5 to 10% by weight based on the total amount of monomer components forming the (meth)acrylic polymer. The proportion of (meth)acrylic acid may be, for example, 1 to 8% by weight or 1.5 to 7% by weight. From the viewpoint of heat resistance when the pressure-sensitive adhesive layer (adhesive layer) is thinned, the proportion of (meth)acrylic acid is preferably not less than the above range. Moreover, from the viewpoint of adhesive strength, the proportion of (meth)acrylic acid is preferably not more than the above range.

[0072] As the hydroxyalkyl (meth)acrylate, for example, those having a polymerizable functional group and a hydroxyl group can be used without any particular limitation.As the hydroxyalkyl (meth)acrylate, for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, etc. are suitable.

[0073] The hydroxyalkyl (meth)acrylate is used, for example, in a proportion of 0.05 to 2% by weight based on the total amount of monomer components forming the (meth)acrylic polymer. The proportion of the hydroxyalkyl (meth)acrylate may be, for example, 0.075 to 1.5% by weight or 0.1 to 1% by weight. From the viewpoint of heat resistance when the pressure-sensitive adhesive layer (adhesive layer) is thinned, the proportion of the hydroxyalkyl (meth)acrylate is preferably not less than the above range. Moreover, from the viewpoint of adhesive strength, the proportion of the hydroxyalkyl (meth)acrylate is preferably not more than the above range.

[0074] The alkyl (meth)acrylate may have an average carbon number of about 1 to 12 in the alkyl group of the alkyl (meth)acrylate. The (meth)acrylate refers to acrylate and / or methacrylate, and (meth) in the present invention has the same meaning. Specific examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate, etc., which can be used alone or in combination. Among these, alkyl (meth)acrylates having an alkyl group with 1 to 9 carbon atoms are preferred.

[0075] The alkyl (meth)acrylate is used in an amount of, for example, 83 to 96.45% by weight based on the total amount of monomer components forming the (meth)acrylic polymer. The alkyl (meth)acrylate is usually the remainder other than the heterocycle-containing acrylic monomer, (meth)acrylic acid, and hydroxyalkyl (meth)acrylate.

[0076] As the monomer components forming the (meth)acrylic polymer, for example, in addition to the above-mentioned monomers, any other monomers can be used within a range of 10% or less of the total amount of monomers, as long as the object of the present invention is not impaired.

[0077] Examples of the optional monomer include acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride, caprolactone adducts of acrylic acid, sulfonic acid group-containing monomers such as styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid, and phosphoric acid group-containing monomers such as 2-hydroxyethyl acryloyl phosphate. Nitrogen-containing vinyl monomers are also included. For example, maleimide, N-cyclohexylmaleimide, N-phenylmaleimide; (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide and other (N-substituted) amide monomers; aminoethyl(meth)acrylate, aminopropyl(meth)acrylate, N,N(meth)acrylic acid -dimethylaminoethyl, t-butylaminoethyl (meth)acrylate, 3-(3-pyridyl)propyl (meth)acrylate and other alkylaminoalkyl (meth)acrylate monomers; methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate and other alkoxyalkyl (meth)acrylate monomers; and succinimide monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, N-(meth)acryloyl-8-oxyoctamethylene succinimide.

[0078] Furthermore, vinyl monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinyl carboxylic acid amides, styrene, α-methylstyrene, and N-vinylcaprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as glycidyl (meth)acrylate; glycol-based acrylic ester monomers such as polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate; and acrylic ester monomers such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, silicone (meth)acrylate, and 2-methoxyethyl acrylate can also be used.

[0079] Further, as copolymerizable monomers other than the above, there may be mentioned silane-based monomers containing silicon atoms, etc. Examples of the silane-based monomers include 3-acryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyltriethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyltriethoxysilane, 10-methacryloyloxydecyltrimethoxysilane, 10-acryloyloxydecyltrimethoxysilane, 10-methacryloyloxydecyltriethoxysilane, 10-acryloyloxydecyltriethoxysilane, etc.

[0080] The (meth)acrylic polymer used in the adhesive layer in the laminate of the present invention may have a weight average molecular weight (Mw) of, for example, 700,000 to 4,000,000. The weight average molecular weight may be, for example, 1,500,000 to 4,000,000, for example, 1,800,000 to 3,800,000, 2,000,000 to 3,500,000, or 2,200,000 to 3,300,000. In addition, the weight average molecular weight may be, for example, 800,000 to 3,500,000, for example, 1,500,000 to 3,400,000, or 2,000,000 to 3,300,000. The weight average molecular weight is preferably not smaller than the above range in terms of heat resistance and moisture resistance when the adhesive layer (adhesive layer) is thinned. In addition, the weight average molecular weight is preferably not larger than the above range in terms of durability, lamination property, and adhesive strength when the adhesive layer is thinned. In the present invention, the weight average molecular weight refers to a value measured by, for example, GPC (gel permeation chromatography) and calculated in terms of polystyrene.

[0081] The method for producing such a (meth)acrylic polymer is not particularly limited, and can be appropriately selected from known production methods such as solution polymerization, bulk polymerization, emulsion polymerization, various radical polymerizations, etc. The obtained (meth)acrylic polymer may be any of a random copolymer, a block copolymer, a graft copolymer, etc.

[0082] In the solution polymerization, for example, ethyl acetate, toluene, etc. are used as a polymerization solvent. In a specific example of the solution polymerization, the reaction is carried out under a stream of an inert gas such as nitrogen, with the addition of a polymerization initiator, at a temperature of about 50 to 70° C., for example, for about 1 to 30 hours.

[0083] The polymerization initiator, chain transfer agent, emulsifier, etc. used in the radical polymerization are not particularly limited and can be appropriately selected and used. The weight average molecular weight of the (meth)acrylic polymer can be controlled by the amount of the polymerization initiator and chain transfer agent used and the reaction conditions, and the amount used is appropriately adjusted depending on the type of these.

[0084] Examples of the polymerization initiator include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-amidinopropane)dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis(2-methylpropionamidine)disulfate, 2,2'-azobis(N,N'-dimethyleneisobutylamidine), and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate (VA-057, manufactured by Wako Pure Chemical Industries, Ltd.); persulfates such as potassium persulfate and ammonium persulfate; di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butyl ... Examples of the initiator include, but are not limited to, peroxide initiators such as dicarbonate, t-butyl peroxyneodecanoate, t-hexyl peroxypivalate, t-butyl peroxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, dibenzoyl peroxide, t-butyl peroxyisobutyrate, 1,1-di(t-hexylperoxy)cyclohexane, t-butyl hydroperoxide, and hydrogen peroxide; and redox initiators combining a peroxide and a reducing agent, such as a combination of a persulfate and sodium hydrogen sulfite, or a combination of a peroxide and sodium ascorbate.

[0085] The polymerization initiator may be used alone or in combination of two or more kinds. The total content of the polymerization initiator may be, for example, about 0.005 to 1 part by weight or about 0.02 to 0.5 part by weight based on 100 parts by weight of the monomer.

[0086] In addition, when a (meth)acrylic polymer having the above weight average molecular weight is produced using, for example, 2,2'-azobisisobutyronitrile as a polymerization initiator, the amount of the polymerization initiator used may be, for example, about 0.06 to 0.2 parts by weight or about 0.08 to 0.175 parts by weight relative to 100 parts by weight of the total amount of the monomer components.

[0087] Examples of the chain transfer agent include lauryl mercaptan, glycidyl mercaptan, mercaptoacetic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, and 2,3-dimercapto-1-propanol. The chain transfer agent may be used alone or in combination of two or more. The total content of the chain transfer agent is, for example, about 0.1 parts by weight or less relative to 100 parts by weight of the total amount of the monomer components.

[0088] Examples of emulsifiers used in emulsion polymerization include anionic emulsifiers such as sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzenesulfonate, polyoxyethylene alkyl ether ammonium sulfate, and sodium polyoxyethylene alkyl phenyl ether sulfate, and nonionic emulsifiers such as polyoxyethylene alkyl ether, polyoxyethylene alkyl phenyl ether, polyoxyethylene fatty acid ester, and polyoxyethylene-polyoxypropylene block polymer. These emulsifiers may be used alone or in combination of two or more.

[0089] Furthermore, as reactive emulsifiers, emulsifiers having radical polymerizable functional groups such as propenyl groups and allyl ether groups are specifically exemplified by Aqualon HS-10, HS-20, KH-10, BC-05, BC-10, and BC-20 (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and Adeka Reasoap SE10N (manufactured by Asahi Denka Kogyo Co., Ltd.). Reactive emulsifiers are preferred because they are incorporated into the polymer chain after polymerization, improving water resistance. The amount of emulsifier used is 0.3 to 5 parts by weight, and more preferably 0.5 to 1 part by weight, based on 100 parts by weight of the total amount of monomer components, in terms of polymerization stability and mechanical stability.

[0090] The content of the (meth)acrylic polymer in the adhesive coating liquid is not particularly limited, and may be, for example, 3 mass % or more, or 5 mass % or more, and may be, for example, 30 mass % or less, 20 mass % or less, or 10 mass % or less, relative to the total mass of the adhesive coating liquid.

[0091] The adhesive coating liquid may or may not contain a monomer having one or two reactive double bonds in one molecule. The monomer having one or two reactive double bonds in one molecule is not particularly limited, but from the viewpoint of the reaction rate of the graft reaction, acrylic monomers, vinyl monomers, methacrylic monomers, and allyl monomers are preferred, and acrylic monomers are more preferred. The acrylic monomer is not particularly limited, but may be, for example, the same as the monomer exemplified as the monomer component of the acrylic polymer. In the monomer having one or two reactive double bonds in one molecule, the structure of the side chain is not particularly limited, but a heterocycle-containing monomer is preferred from the viewpoint of simultaneously achieving a high elastic modulus and a reduction in the amount of semi-high molecular weight polymer within an appropriate range.

[0092] In a case where the adhesive coating liquid contains a monomer having one or two reactive double bonds in one molecule, the content thereof is not particularly limited, and may be, for example, 0.1 mass % or more, 0.5 mass % or more, or 1 mass % or more, and may be, for example, 30 mass % or less, 20 mass % or less, or 10 mass % or less, relative to the total mass of the (meth)acrylic polymer in the adhesive coating liquid.

[0093] The adhesive coating liquid may or may not contain a crosslinking agent, as described above. The crosslinking agent is not particularly limited, but examples thereof include isocyanate-based crosslinking agents and epoxy-based crosslinking agents. The isocyanate-based crosslinking agent is not particularly limited, but examples thereof include aromatic isocyanates such as tolylene diisocyanate and xylylene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate. The epoxy crosslinking agent is not particularly limited, but examples thereof include bisphenol A-epichlorohydrin type epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl erythritol, diglycerol polyglycidyl ether, 1,3'-bis(N,N-diglycidylaminomethyl)cyclohexane, and N,N,N',N'-tetraglycidyl-m-xylylenediamine.

[0094] More specifically, the isocyanate-based crosslinking agent may be, for example, lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate, alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate, aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl isocyanate, trimethylolpropane / tolylene diisocyanate trimer adduct (Japan Examples of such polyisocyanates include isocyanate adducts such as a trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., product name: Coronate L), a trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., product name: Coronate HL), and an isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., product name: Coronate HX); polyether polyisocyanates, polyester polyisocyanates, and adducts of these with various polyols; and polyisocyanates which have been multifunctionalized with an isocyanurate bond, a biuret bond, an allophanate bond, or the like.

[0095] More specifically, examples of the epoxy crosslinking agent include "Tetrad C" manufactured by Mitsubishi Gas Chemical Company, Inc., "Tetrad X" manufactured by Mitsubishi Gas Chemical Company, Inc., and "S-610" manufactured by Synasia.

[0096] The crosslinking agent (e.g., isocyanate-based crosslinking agent or epoxy-based crosslinking agent) may be used alone or in a mixture of two or more kinds, and the total content may be, for example, 0.02 to 2 parts by mass, 0.04 to 1.5 parts by mass, or 0.05 to 1 part by mass of the crosslinking agent relative to 100 parts by mass of the (meth)acrylic polymer. The content of the isocyanate-based crosslinking agent is preferably 0.02 parts by mass or more from the viewpoint of cohesive strength, while it is preferably 2 parts by mass or less from the viewpoint of suppressing or preventing a decrease in adhesive strength due to excessive crosslinking. The content of the epoxy-based crosslinking agent is preferably 0.01 parts by mass or more from the viewpoint of void residual rate, while it is preferably 1.0 part by mass or less from the viewpoint of peeling durability.

[0097] In the adhesive coating liquid, the crosslinking agent may be, for example, only an isocyanate-based crosslinking agent, or may or may not contain other crosslinking agents other than the isocyanate-based crosslinking agent. Examples of the other crosslinking agents include organic crosslinking agents and polyfunctional metal chelates. Examples of the organic crosslinking agents include epoxy crosslinking agents and imine crosslinking agents. The organic crosslinking agents are preferably isocyanate crosslinking agents or epoxy crosslinking agents. The polyfunctional metal chelate is a polyvalent metal covalently bonded or coordinately bonded to an organic compound. Examples of polyvalent metal atoms include Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, Ti, etc. Examples of atoms in the organic compound that are covalently bonded or coordinately bonded include oxygen atoms, etc., and examples of the organic compounds include alkyl esters, alcohol compounds, carboxylic acid compounds, ether compounds, and ketone compounds.

[0098] The adhesive coating liquid may or may not contain an organic peroxide. The organic peroxide is not particularly limited, but examples thereof include di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, dibenzoyl peroxide, t-butylperoxyisobutyrate, 1,1-di(t-hexylperoxy)cyclohexane, and t-butyl hydroperoxide. Only one type may be used, or multiple types may be used in combination.

[0099] In a case where the adhesive coating liquid contains the organic peroxide, the content thereof is not particularly limited, and may be, for example, 0.02 mass % or more, 0.1 mass % or more, 0.5 mass % or more, 1 mass % or more, or 2.5 mass % or more relative to the total mass of the (meth)acrylic polymer in the adhesive coating liquid, and may be, for example, 20 mass % or less, 10 mass % or less, 8 mass % or less, or 6 mass % or less.

[0100] The pressure-sensitive adhesive coating liquid may further contain a solvent, etc. The solvent is not particularly limited, but for example, the polymerization solvent used in the solution polymerization in the production of the (meth)acrylic polymer may be used as it is.

[0101] Furthermore, the adhesive coating liquid may contain, as necessary, tackifiers, plasticizers, fillers made of glass fibers, glass beads, metal powders, other inorganic powders, pigments, colorants, fillers, antioxidants, ultraviolet absorbers, silane coupling agents, etc., and various additives may also be appropriately used within the scope of the object of the present invention. Also, the adhesive layer (adhesive layer) may contain fine particles and exhibit light diffusibility.

[0102] The adhesive layer in the laminate of the present invention can be formed by using the adhesive coating liquid, for example, by the method described below. The adhesive layer may have a weight average molecular weight of 30,000 to 600,000 in a molecular weight measurement of the adhesive layer by gel permeation chromatography. In addition, the content of low molecular weight components having a molecular weight of 10,000 or less in the sol component of the adhesive layer may be 20% by weight (mass%) or less in a molecular weight measurement of the adhesive layer by gel permeation chromatography. By setting the weight average molecular weight of the sol component or the content of low molecular weight components having a molecular weight of 10,000 or less in the sol component to the specific range, the adhesive is further less likely to penetrate into the voids of the void layer. The weight average molecular weight of the sol component may be, for example, 50,000 or more, for example, 550,000 or less or 500,000 or less, for example, 50 to 550,000 or 60 to 500,000. The content (ratio) of the component having a molecular weight of 10,000 or less in the sol fraction may be, for example, 20% by weight or less, as described above, and may be, for example, 15% by weight or less or 10% by weight or less, relative to the total amount of the sol fraction (100% by weight). The lower limit of the content (ratio) of the component having a molecular weight of 10,000 or less in the sol fraction is not particularly limited, and may be, for example, 0% by weight or more or a value exceeding 0% by weight, and may be, for example, 3% by weight or more. The content (ratio) of the component having a molecular weight of 10,000 or less in the sol fraction may be, for example, 3 to 15% by weight or 3 to 10% by weight.

[0103] [4. Manufacturing method of laminate] The method for producing the laminate of the present invention is not particularly limited, and can be, for example, the production method described below. However, the following description is merely an example and does not limit the present invention in any way.

[0104] As described above, the method for producing the laminate of the present invention includes a step of bonding the tacky adhesive layer to the first main surface of the first optical sheet (hereinafter, sometimes referred to as a "bonding step"). However, the method for producing the laminate of the present invention is not limited thereto. For example, instead of the bonding step of bonding the tacky adhesive layer to the first main surface of the first optical sheet, the tacky adhesive layer may be formed by applying a tacky adhesive to the first main surface of the first optical sheet. However, from the viewpoint of suppressing the intrusion of the tacky adhesive into the recesses of the first main surface, the bonding step is preferable to the step of forming the tacky adhesive layer by applying a tacky adhesive to the first main surface.

[0105] In addition, the method for producing the laminate of the present invention (for example, the method for producing the laminate of the present invention) may further include, for example, a step of producing the adhesive layer. The method for producing the adhesive layer may include, for example, a step of applying the adhesive coating liquid to a substrate, and a step of heating and drying the substrate to which the adhesive coating liquid has been applied. For example, the adhesive layer side of an adhesive tape or the like having the adhesive layer of the present invention laminated on a substrate may be attached to the first optical sheet of the present invention to form the adhesive layer on the first optical sheet of the present invention. In this case, the substrate such as the adhesive tape may be left attached as it is, or may be peeled off from the adhesive layer. In particular, by peeling off the substrate to form a first optical sheet-containing adhesive sheet having no substrate (substrate-less), the thickness can be significantly reduced, and an increase in the thickness of a device or the like can be suppressed. In the present invention, the "adhesive" and the "adhesive layer" refer to, for example, an agent or layer that is intended to be peeled off from an adherend. In the present invention, the "adhesive" and the "adhesive layer" refer to, for example, an agent or layer that is not intended to be removably peeled from an adherend. However, in the present invention, a "pressure-sensitive adhesive" and an "adhesive" are not necessarily clearly distinguishable from each other, and a "pressure-sensitive adhesive layer" and an "adhesive layer" are not necessarily clearly distinguishable from each other. In the present invention, the pressure-sensitive adhesive layer can be produced, for example, by using the pressure-sensitive adhesive coating liquid as described above.

[0106] The adhesive layer manufacturing step can be carried out, for example, as follows. First, the adhesive coating liquid is manufactured by a mixing step of mixing all the components of the adhesive coating liquid. The adhesive coating liquid may contain, for example, the (meth)acrylic polymer as described above, and may or may not further contain a crosslinking agent (for example, an isocyanate-based crosslinking agent or an epoxy-based crosslinking agent). The adhesive coating liquid may contain, for example, the (meth)acrylic polymer, a monomer having one or two reactive double bonds in one molecule, a crosslinking agent, and an organic peroxide. At this time, when the adhesive coating liquid contains other components, the other components may also be mixed together. For example, the polymerization solvent used in the production of the (meth)acrylic polymer may be mixed as it is as a component of the adhesive coating liquid without removing it. In addition, the manufacturing method of the adhesive coating liquid may include other steps other than the mixing step, but may not include them, and may simply mix all the components of the adhesive coating liquid in the mixing step.

[0107] Next, the adhesive coating liquid is applied to a substrate (adhesive coating liquid application step). The substrate is not particularly limited, and may be, for example, a substrate such as a film. The substrate may be, for example, a substrate made of a thermoplastic resin, a substrate made of glass, an inorganic substrate such as silicon, a plastic formed from a thermosetting resin, an element such as a semiconductor, or a carbon fiber-based material such as a carbon nanotube, but is not limited thereto. The substrate may be, for example, a film or a plate. The thermoplastic resin may be, for example, polyethylene terephthalate (PET), acrylic, cellulose acetate propionate (CAP), cycloolefin polymer (COP), triacetyl cellulose (TAC), polyethylene naphthalate (PEN), polyethylene (PE), polypropylene (PP), or the like. In the adhesive coating liquid application step, the thickness of the adhesive coating liquid is not particularly limited, and may be appropriately adjusted so that the thickness of the adhesive layer after drying is a predetermined thickness. The thickness of the adhesive layer after drying is also not particularly limited, and may be, for example, as described below.

[0108] Next, the substrate coated with the adhesive coating liquid is heated and dried (heat drying step). In this heat drying step, the temperature of the heat drying is not particularly limited, but may be, for example, 50°C or more, 80°C or more, 100°C or more, or 155°C or more, and may be, for example, 200°C or less, 180°C or less, or 160°C or less. The time of the heat drying is not particularly limited, but may be, for example, 0.5 minutes or more, 1 minute or more, or 3 minutes or more, and may be, for example, 60 minutes or less, 30 minutes or less, 20 minutes or less, or 10 minutes or less. In this heat drying step, for example, a crosslinking reaction and graft polymerization occur between the (meth)acrylic polymer and the crosslinking agent. As a result, for example, as described above, the amount of the semi-high molecular weight polymer present in the adhesive coating liquid is reduced, and the adhesive layer is less likely to penetrate into the recesses of the first optical sheet. In this manner, the adhesive layer used in the laminate of the present invention can be produced.

[0109] Next, as described above, the adhesive layer is bonded to the first main surface of the first optical sheet (bonding step). This method is not particularly limited, but for example, as described above, the adhesive layer side of an adhesive tape or the like in which the adhesive layer of the present invention is laminated on a substrate may be bonded to the first optical sheet of the present invention to form the adhesive layer on the first optical sheet of the present invention. In this manner, the laminate of the present invention can be manufactured.

[0110] The thickness of the adhesive layer is not particularly limited, and is, for example, 0.1 to 100 μm, 5 to 50 μm, 10 to 30 μm, or 12 to 25 μm.

[0111] The laminate of the present invention thus obtained may be further laminated with another film (layer) to form a laminate structure including the first optical sheet, for example, as described above. In this case, in the laminate structure, each component may be laminated via the adhesive layer (adhesive or adhesive) as described above.

[0112] The lamination of the respective components may be performed, for example, efficiently by continuous processing (so-called Roll to Roll, etc.) using a long film as described above, or when the substrate is a molded product, element, etc., the components may be laminated after batch processing. EXAMPLES

[0113] Next, examples of the present invention will be described, but the present invention is not limited to the following examples.

[0114] In the following Reference Examples, Examples, and Comparative Examples, the number of parts (relative amount used) of each substance is in parts by mass (parts by weight) unless otherwise specified. In the following Reference Examples, Examples, and Comparative Examples, a pressure-sensitive adhesive (pressure-sensitive adhesive composition) described below was used as the pressure-sensitive adhesive. In the following Reference Examples, Examples, and Comparative Examples, the term "pressure-sensitive adhesive layer" corresponds to the "pressure-sensitive adhesive layer". That is, in the following Reference Examples, Examples, and Comparative Examples, the terms "pressure-sensitive adhesive layer" and "pressure-sensitive adhesive layer" are synonymous unless otherwise specified.

[0115] In the following Reference Examples, Examples, and Comparative Examples, the molecular weight of the (meth)acrylic polymer, the weight average molecular weight (Mw) of the (meth)acrylic polymer, the thickness of each layer, the gel fraction of the adhesive layer, the weight average molecular weight (Mw) of the sol fraction of the adhesive layer, the nanoindentation hardness, and the PMMA adhesive strength (180° peel adhesive strength to polymethyl methacrylate) were each measured by the following measurement methods.

[0116] <Method for measuring molecular weight of (meth)acrylic polymer> The weight-average molecular weight (Mw), polydispersity (Mw / Mn), proportion (weight percentage) of low molecular weight components with a molecular weight of 100,000 or less, and proportion (weight percentage) of high molecular weight components with a molecular weight of 30 million or more of the (meth)acrylic polymer were calculated from the molecular weight distribution curve measured by gel permeation chromatography (GPC). ·Analyzer: Waters, Alliance Column: Tosoh Corporation, G7000HXL+GMHXL+GMHXL Column size: 7.8mmφ×30cm each, total 90cm Column temperature: 40℃ ·Flow rate: 0.8mL / min ·Injection volume: 100μL ·Eluent: THF (acid added) Detector: Differential refractometer (RI) Standard sample: polystyrene

[0117] <How to measure thickness> The thickness of the adhesive layer was determined by measuring the thickness at five points on the adhesive layer using a dial gauge and taking the average value. The thickness of the intermediate layer was determined by taking the thickness of the intermediate layer, which is a part of the adhesive layer with a different contrast between the adhesive layer and the low refractive index layer in the SEM image, as the average value of the thickness measured at two points on the SEM image.

[0118] <Method for measuring weight average molecular weight (Mw) of (meth)acrylic polymer> The weight average molecular weight (Mw) of the (meth)acrylic polymer was measured by gel permeation chromatography (GPC) under the following conditions. The polydispersity (Mw / Mn) of the (meth)acrylic polymer was also measured in the same manner. ·Analyzer: Waters, Alliance Column: Tosoh Corporation, G7000HXL+GMHXL+GMHXL Column size: 7.8mmφ×30cm each, total 90cm Column temperature: 40℃ ·Flow rate: 0.8mL / min ·Injection volume: 100μL ·Eluent: THF (acid added) Detector: Differential refractometer (RI) Standard sample: polystyrene

[0119] <Method for measuring gel fraction of adhesive layer> About 0.1 g was scraped off from the pressure-sensitive adhesive composition layer and used as sample 1. Sample 1 was wrapped in a Teflon (registered trademark) film (trade name "NTF1122", manufactured by Nitto Denko Corporation) having a diameter of 0.2 μm, and then tied with a kite string, which was used as sample 2. The weight of sample 2 before being subjected to the following test was measured and this was used as weight A. The weight A is the total weight of sample 1 (pressure-sensitive adhesive layer), the Teflon (registered trademark) film, and the kite string. The total weight of the Teflon (registered trademark) film and the kite string was used as weight B. Next, sample 2 was placed in a 50 ml container filled with ethyl acetate and left to stand at 23° C. for one week. Thereafter, sample 2 was taken out of the container and dried in a dryer at 130° C. for 2 hours to remove the ethyl acetate, and the weight of sample 2 was measured. The weight of sample 2 after being subjected to the above test was measured and this was used as weight C. Then, the gel fraction was calculated from the following formula. Gel fraction (%) = (CB) / (AB) x 100

[0120] <Method for measuring the weight average molecular weight (Mw) of the sol component of the adhesive layer> The weight average molecular weight (Mw) of the sol content contained in the adhesive layer was measured by GPC (gel permeation chromatography). The adhesive layer was immersed in 10 mM phosphoric acid / tetrahydrofuran overnight to extract the sol content. At this time, taking into account the gel fraction of the adhesive layer, the sol content of the solution after extraction was adjusted to 0.1 wt%. The solution after extraction was filtered through a 0.45 μm membrane filter, and the filtrate was subjected to GPC measurement. Analytical equipment: Waters, Alliance Column: Tosoh Corporation, G7000HXL+GMHXL+GMHXL Column size: 7.8mmφ×30cm each, total 90cm Column temperature: 40℃ ·Flow rate: 0.8mL / min ·Injection volume: 100μL Eluent: 10mM phosphoric acid / tetrahydrofuran Detector: Differential refractometer (RI) Standard sample: polystyrene

[0121] <Method for Measuring Nanoindentation Hardness> The measurement sample was cut out to about 1 cm square and fixed to a predetermined support, and the nanoindentation hardness of the adhesive layer was measured under the following conditions. The nanoindentation hardness was measured by the nanoindentation method. · Analyzer: Triboindenter manufactured by Hysitron Inc. · Indenter used: Conical (sphere: diameter 20 μm) · Measurement method: Single indentation measurement · Measurement temperature: Room temperature · Indentation depth: 2000 nm

[0122] From the maximum load (Pmax) and the contact projected area (A) obtained by the measurement, the nanoindentation hardness was calculated by the following formula. Nanoindentation hardness = Pmax / A

[0123] In this example, the nanoindentation hardness of the adhesive layer surface was measured, but there was no difference in the measured values even when the adhesive layer cross-section was measured.

[0124] <Method for Measuring PMMA Adhesion> The PMMA adhesive strength, i.e., the 180° peeling adhesive strength to PMMA (polymethyl methacrylate), was measured as follows. First, the adhesive layer side of a laminate (a laminate having a laminated structure of the separator film / adhesive layer) in which an adhesive layer (adhesive layer) was formed on the surface of a separator film (polyethylene terephthalate film treated with a silicone-based release agent: manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., MRF38) produced in each of the Examples and Comparative Examples described below was bonded to a polyethylene terephthalate (PET) film (trade name "Lumirror S-10", manufactured by Toray Industries, Inc.) having a thickness of 25 μm. The laminate was cut to a width of 20 mm, the PET film was peeled off, and the exposed surface of the adhesive layer was bonded to a polymethyl methacrylate (PMMA) plate (trade name "Acrylite", manufactured by Mitsubishi Chemical Co., Ltd.) to prepare a test piece, and the adhesive strength to the PMMA plate (mN / 20 mm) was measured. Specifically, the pressure bonding when bonding to the PMMA plate was performed by rolling a 2 kg roller back and forth once, and 30 minutes after bonding, the 180° peel adhesive strength was measured under the following conditions using a tension and compression tester (device name "AGS-50NX", manufactured by Shimadzu Corporation). The measured peel adhesive strength was taken as the PMMA adhesive strength. Peeling speed: 300mm / min Measurement conditions: Temperature: 23±2℃, Humidity: 65±5%RH

[0125] The measured peel adhesive strength (PMMA adhesive strength) (mN / 20 mm) obtained by the above measurement method was evaluated on a four-level scale as follows. ×: Less than 1.0mN / 20mm △: 1.0mN / 20mm or more, less than 2.0mN / 20mm ○: 2.0mN / 20mm or more and less than 6.0mN / 20mm ◎: 6.0mN / 20mm or more

[0126] <Method of measuring and calculating air cavity remaining rate> In each of the examples and comparative examples described below, the shape of the air cavity (recess of the first optical sheet) of the laminate having a laminated structure of the unevenness-imparting film (first optical sheet) / adhesive layer (tacky adhesive layer) / acrylic resin film was observed and measured using a laser microscope (VK-X1100 manufactured by Keyence Corporation). Furthermore, the shape of the air cavity (recess of the first optical sheet) of the unevenness-imparting film alone (first optical sheet) was also observed and measured using the same equipment and method. Then, the air cavity remaining rate was calculated using the following formula (1). R=(L 1 / L 2 )×100 (1) In the formula (1), R is the air cavity remaining rate (%). L 1 is the measured length of the long side of the air cavity (the recess of the first optical sheet) of the laminate. L 2 is the measured length of the long side of the air cavity (the recess of the first optical sheet) of the unevenly shaped film (first optical sheet) alone.

[0127] In the adhesive layers in the following Reference Examples, Examples, and Comparative Examples, it is presumed that the polymer (acrylic polymer) is crosslinked by the crosslinking agent through heating and drying of the applied adhesive, thereby forming a crosslinked structure, but the crosslinked structure has not been confirmed.

[0128] [Reference Example 1: Preparation of (meth)acrylic polymer (A1)] A monomer mixture containing 83 parts of butyl acrylate, 13 parts of N-acryloylmorpholine, 3 parts of acrylic acid, and 1 part of 4-hydroxybutyl acrylate was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.06 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 50 parts of ethyl acetate relative to 100 parts of the monomer mixture, and nitrogen gas was introduced to replace the atmosphere with nitrogen while gently stirring. The liquid temperature in the flask was kept at about 55°C, and a polymerization reaction was carried out for 3 hours to prepare a solution of a (meth)acrylic polymer (A1) having a weight average molecular weight (Mw) of 3,000,000 and Mw / Mn=2.8.

[0129] [Reference Example 2: Preparation of (meth)acrylic polymer (A2)] The composition of the monomer mixture charged in Reference Example 1 (preparation of (meth)acrylic polymer (A1)) was changed to 73 parts of butyl acrylate, 20 parts of N-acryloylmorpholine, 6 parts of acrylic acid, and 1 part of 4-hydroxybutyl acrylate. Otherwise, the same procedure as in Reference Example 1 was repeated to prepare a solution of (meth)acrylic polymer (A2) having a weight average molecular weight (Mw) of 2.5 million and Mw / Mn=2.4.

[0130] [Reference Example 3: Preparation of (meth)acrylic polymer (A3)] The composition of the monomer mixture charged in Reference Example 1 (preparation of (meth)acrylic polymer (A1)) was changed to 95 parts of butyl acrylate, 1 part of N-acryloylmorpholine, 3 parts of acrylic acid, and 1 part of 4-hydroxybutyl acrylate, and the polymerization reaction time was changed to 8 hours. The other conditions were the same as in Reference Example 1, and a solution of (meth)acrylic polymer (A3) with a weight average molecular weight (Mw) of 1,700,000 and Mw / Mn=5.2 was prepared.

[0131] [Reference Example 4: Preparation of (meth)acrylic polymer (A4)] The composition of the monomer mixture charged in Reference Example 1 (preparation of (meth)acrylic polymer (A1)) was changed to 63 parts of butyl acrylate, 30 parts of N-acryloylmorpholine, 6 parts of acrylic acid, and 1 part of 4-hydroxybutyl acrylate. Otherwise, the same procedure as in Reference Example 1 was repeated to prepare a solution of (meth)acrylic polymer (A4) having a weight average molecular weight (Mw) of 2,300,000 and Mw / Mn=2.8.

[0132] [Reference Example 5: Production of textured film (first optical sheet)] The unevenly shaped film was produced according to the method described in JP-A-2013-524288. Specifically, the surface of a PMMA (polymethyl methacrylate) film (manufactured by Nippon Tokushu Kogaku Jushi Co., Ltd., product name LPV90-0.01S) was first coated with lacquer (manufactured by Sanyo Chemical Industries Co., Ltd., product name "Fine Cure RM-64"), an optical pattern was embossed on the film surface containing the lacquer, and then the lacquer was cured to produce the desired unevenly shaped film (first optical sheet). The total thickness of this unevenly shaped film was 125 μm, and the haze value was 0.8%.

[0133] FIG. 5A shows a plan view of a part of the produced unevenness-imparting film (first optical sheet) seen from the uneven surface (first main surface). FIG. 5B shows a cross-sectional view of the unevenness-imparting film of FIG. 5A taken along line 8B-8B'. As shown in the figure, this unevenness-imparting film had a plurality of recesses 74 with a triangular cross section, a length L of 80 μm, a width W of 17.3 μm, and a depth H of 10 μm, arranged at intervals of width E (260 μm) in the X-axis direction. Furthermore, a pattern of such recesses 74 was arranged at intervals of width D (160 μm) in the Y-axis direction. Px in FIG. 5A is 340 μm, and Py is 174 μm. The density of the recesses 74 on the surface of the unevenness-imparting film was 2426 pieces / cm 2 5B, the inclination angle θa was about 60°, and the inclination angle θb was 85°. The occupied area ratio of the recesses 74 when the film was viewed in plan from the uneven surface side was 3.4%.

[0134] [Example 1: Production of laminate] The laminate of Example 1 was produced by the following method.

[0135] (1) Preparation of Pressure Sensitive Adhesive Composition A solution of an acrylic pressure-sensitive adhesive composition was prepared by blending 0.3 parts of an isocyanate crosslinking agent (trade name "Coronate L" manufactured by Nippon Polyurethane Industry Co., Ltd., an adduct of trimethylolpropane and tolylene diisocyanate) and 0.1 parts by mass of 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (trade name "TETRAD-C" manufactured by Mitsubishi Gas Chemical Co., Inc.) with 100 parts of the solid content of the solution of the (meth)acrylic polymer (A1) prepared (manufactured) in Reference Example 1.

[0136] (2) Formation of adhesive layer Next, the solution of the acrylic pressure-sensitive adhesive composition prepared in (1) above was applied to one side of a polyethylene terephthalate film (separator film: MRF38, manufactured by Mitsubishi Chemical Polyester Film Co., Ltd.) treated with a silicone-based release agent so that the thickness of the pressure-sensitive adhesive layer after drying would be 10 μm, and the coating was dried at 155° C. for 1 minute to form a pressure-sensitive adhesive layer on the surface of the separator film. This pressure-sensitive adhesive layer corresponds to the "adhesive layer" disposed on the first main surface side of the first optical sheet in the laminate of the present invention.

[0137] (3) Formation of the laminate Next, the surface of the pressure-sensitive adhesive layer (adhesive layer) was bonded to an acrylic resin film (thickness: 30 μm), and then the separator film (PET film) was peeled off to bond the exposed pressure-sensitive adhesive layer to the unevenness-imparting film of Reference Example 5. Autoclaving was then performed at 50°C, 0.5 MPa, and 15 minutes to obtain an optical laminate having a laminated structure of unevenness-imparting film (first optical sheet) / pressure-sensitive adhesive layer (adhesive layer) / acrylic resin film.

[0138] [Examples 2 to 3 and Comparative Examples 1 to 2: Production of Laminates] The laminates of Examples 2 and 3 and Comparative Examples 1 and 2 were produced as follows.

[0139] In producing the laminates of Examples 2 to 3 and Comparative Examples 1 to 2, either the same (meth)acrylic polymer (A1) as in Example 1 was used (Example 3), or any of the (meth)acrylic polymers (A2) to (A4) produced in Reference Examples 2 to 4 were used instead of the (meth)acrylic polymer (A1) as shown in Table 1 below (Example 2 and Comparative Examples 1 to 2).

[0140] The preparation (production) method and production conditions of the (meth)acrylic polymers (A2) to (A4) are as described in the above Reference Examples 2 to 4. In the preparation method of the (meth)acrylic polymers (A2) to (A4), the types of monomers and their blending ratios are as described in the above Reference Examples 2 to 4, and are as shown in the following Table 1. In addition, the polymer properties (weight average molecular weight (MW), polydispersity (Mw / Mn)) of the (meth)acrylic polymers (A2) to (A4) are as shown in the following Table 1.

[0141] In Example 2 and Comparative Example 1, except that the (meth)acrylic polymer (A2) or (meth)acrylic polymer (A3) was used instead of the (meth)acrylic polymer (A1), respectively, a solution of an acrylic pressure-sensitive adhesive composition was prepared in the same manner as in "(1) Preparation of pressure-sensitive adhesive composition" described in Example 1. Furthermore, laminates of Example 2 and Comparative Example 1 were produced in the same manner as Example 1 except for the above.

[0142] In Example 3, 0.3 parts of an isocyanate crosslinking agent (trade name "Coronate L" manufactured by Nippon Polyurethane Industry Co., Ltd., an adduct of tolylene diisocyanate of trimethylolpropane), 10 parts by mass of an ultraviolet-curable urethane acrylate resin A in terms of solid content, and 1.0 part by mass of 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone (trade name "Omnirad2959" manufactured by IGM Japan LLC) as a photopolymerization initiator were mixed with respect to 100 parts by solid content of the (meth)acrylic polymer (A1) solution. The solution of the acrylic adhesive composition was prepared in the same manner as in "(1) Preparation of adhesive composition" described in Example 1. Furthermore, an adhesive layer was prepared in the same manner as in Example 1 using the solution of the acrylic adhesive composition. Thereafter, the adhesive layer was attached to the release-treated surface of a 50 μm-thick polyethylene film that had been subjected to a silicone release treatment. Furthermore, ultraviolet light was irradiated from the top surface (polyethylene film side) to cure the curable resin in the adhesive layer, and then the polyethylene film was peeled off. The ultraviolet light was irradiated using an LED lamp (Quark Technology Co., Ltd., peak illuminance: 200 mW / cm 2 , cumulative light intensity 1500mJ / cm 2 (wavelength 345-365 nm) was used, and the illuminance of ultraviolet light was measured using a UV Power Puck (manufactured by Fusion UV Systems Japan Co., Ltd.). In this way, the adhesive layer (adhesive layer) obtained by curing the curable resin in the adhesive layer was used as the "adhesive layer" in the laminate of this embodiment (Example 3). Thereafter, the laminate of Example 3 was produced in the same manner as in "(3) Formation of Laminate" in Example 1.

[0143] A laminate of Comparative Example 2 was produced in exactly the same manner as in Example 3, except that the (meth)acrylic polymer (A4) was used in place of the (meth)acrylic polymer (A1).

[0144] [Evaluation of properties of laminates in examples and comparative examples] The laminates of Examples 1 to 3 and Comparative Examples 1 and 2 produced as described above were measured and evaluated for their properties by the methods described above. The results are summarized in Table 1 below. In Table 1 below, "Polymer composition" indicates the composition of each of the (meth)acrylic polymers (A1) to (A4) used in producing the laminates. "BA" indicates butyl acrylate. "ACMO" indicates N-acryloylmorpholine. "AA" indicates acrylic acid. "4HBA" indicates 4-hydroxybutyl acrylate.

[0145] [Table 1]

[0146] As shown in Table 1, the laminates of Examples 1 to 3, in which the nanoindentation hardness of the adhesive layer is within the range of the present invention (0.1 MPa or more and 2.0 MPa or less), all had a high PMMA adhesive strength of 1.0 mN / 20 mm or more, and also had a high air cavity residual rate of 90% or more. A high PMMA adhesive strength means that the adhesive strength or adhesion to other members is excellent. A high air cavity residual rate means that the intrusion of the adhesive into the recesses of the uneven structure of the first optical sheet is suppressed. That is, the laminates of Examples 1 to 3 all had the adhesive strength or adhesion to other members that were suppressed from intruding into the recesses of the uneven structure. In contrast, the laminate of Comparative Example 1, in which the nanoindentation hardness of the adhesive layer was too small (too soft), had a high PMMA adhesive strength, but a lower air cavity residual rate than the Examples. On the other hand, the laminate of Comparative Example 2, in which the nanoindentation hardness of the adhesive layer was too large (too hard), had a high air cavity residual rate, but could not be bonded to PMMA because the adhesive strength (bonding strength) of the adhesive layer was low, and therefore the PMMA adhesive strength could not be measured.

[0147] The present invention can be described, for example, as follows: However, the following notes are merely examples, and the present invention is not limited to these forms.

[0148] (Appendix 1) A first optical sheet and an adhesive layer are included, the first optical sheet has a first main surface having a concave-convex structure and a second main surface opposite to the first main surface; the adhesive layer is disposed on the first main surface side of the first optical sheet, the concave-convex structure of the first main surface includes a plurality of concave portions and a flat portion between two adjacent concave portions of the plurality of concave portions, The flat portion of the first main surface is in contact with a surface of the adhesive layer, The adhesive layer contains a (meth)acrylic polymer, A laminate characterized in that the nanoindentation hardness, measured by pressing an indenter 2000 nm into the adhesive layer using a nanoindenter, is 0.1 MPa or more and 2.0 MPa or less. (Appendix 2) In the first optical sheet, The recess of the first main surface forms a space between the surface of the adhesive layer and the recess. 2. The laminate of claim 1. (Appendix 3) 3. The laminate according to claim 1 or 2, wherein the (meth)acrylic polymer contains, as a monomer unit, 1 to 30% by weight of a nitrogen-containing monomer. (Appendix 4) 4. The laminate according to claim 3, wherein the (meth)acrylic polymer has a polydispersity (weight average molecular weight (Mw) / number average molecular weight (Mn)) of 3.0 or less. (Appendix 5) 5. The laminate according to claim 3 or 4, wherein the nitrogen-containing monomer is a heterocycle-containing acrylic monomer. (Appendix 6) the adhesive layer is formed from an adhesive containing the (meth)acrylic polymer and a crosslinking agent, 6. The laminate according to any one of claims 1 to 5, wherein the pressure-sensitive adhesive has a gel fraction of more than 85%. (Appendix 7) 7. The laminate according to any one of claims 1 to 6, wherein the (meth)acrylic polymer is substantially free of a (meth)acrylic polymer having a polystyrene-equivalent molecular weight of 100,000 or less. (Appendix 8) 8. The laminate according to any one of claims 1 to 7, wherein the (meth)acrylic polymer has a weight average molecular weight (Mw) of 1.5 million to 4 million. (Appendix 9) An optical member comprising the laminate according to any one of claims 1 to 8. (Appendix 10) 10. An optical device comprising the optical member according to claim 9. (Appendix 11) 9. A method for producing a laminate according to any one of claims 1 to 8, comprising the step of bonding the adhesive layer and the first main surface of the first optical sheet. [Industrial Applicability]

[0149] As described above, according to the present invention, it is possible to provide a laminate, an optical member, an optical device, and a method for manufacturing a laminate, in which the intrusion of a pressure-sensitive adhesive into the recesses of the uneven structure is suppressed and which has excellent adhesive strength or adhesion to other members. The use of the present invention is not particularly limited. For example, the optical device of the present invention is not particularly limited, and examples thereof include image display devices and lighting devices. Examples of the image display devices include liquid crystal displays, organic EL displays, micro LED displays, and the like. Examples of the lighting devices include organic EL lighting, and the like. Furthermore, the use of the laminate of the present invention is not limited to the optical member and optical device of the present invention, and is arbitrary, and can be used for a wide range of uses. [Explanation of symbols]

[0150] 10a First optical sheet 12s, 18s main surface (front) 20a adhesive layer 60 light source 80 Light guiding layer 100A, 101A, 102A, 102B Optical laminate 200A, 200B lighting equipment

Claims

1. A first optical sheet and an adhesive layer are included, the first optical sheet has a first main surface having a concave-convex structure and a second main surface opposite to the first main surface; the adhesive layer is disposed on the first main surface side of the first optical sheet, The uneven structure of the first main surface includes a plurality of recesses and a flat portion between two adjacent recesses among the plurality of recesses, The flat portion of the first main surface is in contact with a surface of the adhesive layer, The adhesive layer contains a (meth)acrylic polymer, A laminate characterized in that the nanoindentation hardness measured by pressing an indenter into the adhesive layer by 2000 nm using a nanoindenter is 0.1 MPa or more and 2.0 MPa or less.

2. In the first optical sheet, The recess of the first main surface forms a space between the surface of the adhesive layer and the recess. The laminate of claim 1.

3. 2. The laminate according to claim 1, wherein the (meth)acrylic polymer contains, as monomer units, 1 to 30% by weight of a nitrogen-containing monomer.

4. 4. The laminate according to claim 3, wherein the (meth)acrylic polymer has a polydispersity (weight average molecular weight (Mw) / number average molecular weight (Mn)) of 3.0 or less.

5. 4. The laminate according to claim 3, wherein the nitrogen-containing monomer is a heterocycle-containing acrylic monomer.

6. the adhesive layer is formed from an adhesive containing the (meth)acrylic polymer and a crosslinking agent, The laminate according to claim 1 , wherein the pressure-sensitive adhesive has a gel fraction of more than 85%.

7. 2. The laminate according to claim 1, wherein the (meth)acrylic polymer is substantially free of a (meth)acrylic polymer having a molecular weight of 100,000 or less in terms of polystyrene.

8. 2. The laminate according to claim 1, wherein the (meth)acrylic polymer has a weight average molecular weight (Mw) of 1.5 million to 4 million.

9. An optical member comprising the laminate according to claim 1 .

10. An optical device comprising the optical member according to claim 9.

11. The method for producing a laminate according to claim 1 , further comprising: bonding the adhesive layer to the first main surface of the first optical sheet.

Citation Information

Patent Citations

  • Adhesive sheet and liquid crystal display

    JP2011026361A

  • Sealing member for light guide plates and method for producing light guide plate using the same

    JP2019178283A

  • Adhesive layer, laminate, optical laminate, method for producing optical laminate, and optical device

    WO2021167090A1

  • Adhesive composition layer, layered product, optical layered product, optical device, and method for producing optical layered product

    WO2021167091A1

  • Optical laminate and optical device

    WO2022176659A1

Cited By

  • Optical member inspection method and optical member manufacturing method

    CN122793736A

  • Method for inspecting optical components, and method for manufacturing optical components

    JP2026155377A

  • Method for inspecting optical member and method for manufacturing optical member

    KR1020260142023A