Non-aqueous electrolyte secondary battery
A non-aqueous electrolyte secondary battery with a fixing tape having a surface roughness of 40 μm or more addresses electrode deformation by evenly distributing stress, ensuring structural stability and performance.
Patent Information
- Application Number
- JP2021545536
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-11
- Filing Date
- 2020-09-08
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-09-08
AI Technical Summary
Non-aqueous electrolyte secondary batteries experience deformation such as bending of the positive and negative electrodes due to the expansion of the electrode body during charging and discharging, which is exacerbated by the concentration of stress at the fixing tape attachment points.
The battery design incorporates a fixing tape with a base material layer having a surface roughness of 40 μm or more in a 1 mm wide area, which alleviates stress concentration and suppresses deformation by distributing it more evenly.
The solution effectively prevents bending of the electrodes by distributing stress more uniformly, thereby maintaining the structural integrity and performance of the battery.
Smart Images

Figure 0007564812000002 
Figure 0007564812000003 
Figure 0007564812000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery. [Background technology]
[0002] Conventionally, a nonaqueous electrolyte secondary battery has been widely used in which a wound electrode body, which is formed by winding a strip-shaped positive electrode and a strip-shaped negative electrode with a separator therebetween, is wound with a fixing tape at the outermost periphery and then housed in an exterior body. In this battery, the exterior body can be used as a negative electrode terminal by connecting a negative electrode lead protruding from the winding start end of the negative electrode to the exterior body. Patent Document 1 discloses a nonaqueous electrolyte secondary battery in which a negative electrode lead provided at the winding start end of the negative electrode is connected to the exterior body and further a current collector exposed portion that contacts the inner wall surface of the exterior body is provided at the winding end of the negative electrode in order to improve the output characteristics of the battery. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2016 / 147564 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the nonaqueous electrolyte secondary battery described in Patent Document 1, a certain level of contact pressure is required between the electrode body and the exterior body, and the electrode body expands after repeated charging and discharging, so the contact pressure increases. Since a fixing tape is attached to the outermost peripheral surface of the electrode body, deformation such as bending may occur in the positive electrode or negative electrode that constitutes the electrode body, starting from the end of the fixing tape where stress is likely to concentrate.
[0005] An object of the present disclosure is to provide a nonaqueous electrolyte secondary battery capable of suppressing deformation, such as bending, of the positive electrode and negative electrode originating from the fixing tape when the electrode assembly expands. [Means for solving the problem]
[0006] The nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure is a nonaqueous electrolyte secondary battery including a wound electrode assembly in which a strip-shaped positive electrode and a strip-shaped negative electrode are wound with a separator interposed therebetween, and a metal exterior body that houses the electrode assembly. The electrode assembly is characterized in that the positive electrode or the negative electrode is exposed on the outermost peripheral surface thereof, and a fixing tape having a base layer and an adhesive layer is attached to the positive electrode or the negative electrode by the adhesive layer, and the base layer has a surface roughness (Sa) of 40 μm or more in at least a region 1 mm wide from the end. Effect of the Invention
[0007] According to the nonaqueous electrolyte secondary battery according to the present disclosure, deformation such as bending of the positive electrode and negative electrode originating from the fixing tape can be suppressed when the electrode assembly expands. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is an axial cross-sectional view of a cylindrical secondary battery according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view of an electrode body included in the secondary battery shown in FIG. [Diagram 3] FIG. 3 is an explanatory diagram showing the positive electrode and negative electrode constituting the electrode assembly shown in FIG. 2 in a developed state. [Figure 4] FIG. 4 is a cross-sectional view of a fixing tape according to an example of the embodiment. [Diagram 5] FIG. 5(a) is a plan view of the stress application device, and FIG. 5(b) is a cross-sectional view taken along line AA in FIG. 5(a) as viewed in the direction of the arrow. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an example of an embodiment of a cylindrical secondary battery according to the present disclosure will be described in detail with reference to the drawings. In the following description, specific shapes, materials, values, directions, etc. are examples for facilitating understanding of the present invention, and can be appropriately changed according to the specifications of the cylindrical secondary battery. In addition, the exterior body is not limited to a cylindrical shape, and may be, for example, a rectangular shape. In addition, in the following description, when multiple embodiments and modified examples are included, it is assumed from the beginning that the characteristic parts of these embodiments and modified examples will be used in appropriate combination.
[0010] FIG. 1 is an axial cross-sectional view of a cylindrical secondary battery 10 as an example of an embodiment. In the secondary battery 10 shown in FIG. 1, an electrode body 14 and a non-aqueous electrolyte (not shown) are housed in an exterior body 15. The electrode body 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. As a non-aqueous solvent (organic solvent) for the non-aqueous electrolyte, carbonates, lactones, ethers, ketones, esters, etc. can be used, and these solvents can be used in a mixture of two or more kinds. When using a mixture of two or more kinds of solvents, it is preferable to use a mixed solvent containing a cyclic carbonate and a chain carbonate. For example, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used as the cyclic carbonate, and dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), etc. can be used as the chain carbonate. The electrolyte salt of the non-aqueous electrolyte may be LiPF6, LiBF4, LiCF3SO3, or a mixture thereof. The amount of electrolyte salt dissolved in the non-aqueous solvent may be, for example, 0.5 to 2.0 mol / L. For convenience of explanation, the sealing body 16 side will be referred to as "upper" and the bottom side of the exterior body 15 as "lower".
[0011] The opening end of the exterior body 15 is closed by the sealing body 16, so that the inside of the secondary battery 10 is sealed. Insulating plates 17 and 18 are provided above and below the electrode body 14, respectively. The positive electrode lead 19 extends upward through a through hole in the insulating plate 17 and is welded to the underside of the filter 22, which is the bottom plate of the sealing body 16. In the secondary battery 10, the cap 26, which is the top plate of the sealing body 16 and is electrically connected to the filter 22, serves as the positive electrode terminal. On the other hand, the negative electrode lead 20 extends to the bottom side of the exterior body 15 through a through hole in the insulating plate 18 and is welded to the inner surface of the bottom of the exterior body 15. In the secondary battery 10, the exterior body 15 serves as the negative electrode terminal.
[0012] The exterior body 15 is a cylindrical metallic exterior can with a bottom. This makes the battery hard and resistant to deformation when subjected to external stress, and protects the inside. On the other hand, when the electrode body 14 expands due to repeated charging and discharging, the contact pressure between the electrode body 14 and the exterior body 15 increases because the metallic exterior body 15 is hard and resistant to deformation.
[0013] As described above, the exterior body 15 may be rectangular. However, the cylindrical exterior body 15 has a circular horizontal cross section, and the stress inside the battery is uniformly distributed, so that the cylindrical exterior body 15 is less likely to expand than a rectangular exterior body having a flat portion that is prone to expansion, and the contact pressure between the electrode body 14 and the exterior body 15 is likely to be large. Therefore, when the exterior body 15 is cylindrical, deformation such as bending of the positive electrode 11 and the negative electrode 12 starting from the fixing tape is likely to occur, and the effect of the present disclosure is easily achieved.
[0014] A gasket 27 is provided between the exterior body 15 and the sealing body 16 to ensure the sealing of the inside of the secondary battery 10. The exterior body 15 has a grooved portion 21 that is formed, for example, by pressing a side portion from the outside and that supports the sealing body 16. The grooved portion 21 is preferably formed in an annular shape along the circumferential direction of the exterior body 15, and supports the sealing body 16 on its upper surface via the gasket 27.
[0015] The sealing body 16 includes a filter 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cap 26, which are stacked in this order from the electrode body 14 side. Each member constituting the sealing body 16 has, for example, a disk shape or a ring shape, and each member except the insulating member 24 is electrically connected to each other. The lower valve body 23 and the upper valve body 25 are connected to each other at their respective centers, and the insulating member 24 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, for example, the lower valve body 23 breaks, and as a result, the upper valve body 25 swells toward the cap 26 and separates from the lower valve body 23, thereby cutting off the electrical connection between them. When the internal pressure further increases, the upper valve body 25 breaks, and gas is discharged from the opening 26a of the cap 26.
[0016] Next, the electrode body 14 will be described with reference to FIG. 2. FIG. 2 is a perspective view of the electrode body 14. As described above, the electrode body 14 has a wound structure in which the positive electrode 11 and the negative electrode 12 are wound in a spiral shape with the separator 13 interposed therebetween. The positive electrode 11, the negative electrode 12, and the separator 13 are all formed in a strip shape, and are wound in a spiral shape around a winding core arranged along the winding axis, so that they are alternately stacked in the radial direction of the electrode body 14. In the radial direction, the winding axis side is called the inner circumferential side, and the opposite side is called the outer circumferential side. In the electrode body 14, the longitudinal direction of the positive electrode 11 and the negative electrode 12 is the winding direction, and the width direction of the positive electrode 11 and the negative electrode 12 is the axial direction. The positive electrode lead 19 extends in the axial direction from approximately the center in the radial direction between the center and the outermost circumference at the upper end of the electrode body 14. The negative electrode lead 20 extends in the axial direction from the vicinity of the winding axis at the lower end of the electrode body 14.
[0017] The negative electrode 12 is exposed on the outermost peripheral surface of the electrode body 14, and the fixing tape 50 is attached to the negative electrode 12 at both axial ends. The fixing tape 50 is a member for winding the electrode body 14, and is attached so as to cover at least a part of the winding end portion 12a of the negative electrode 12. The width of the fixing tape 50 is not particularly limited, but may be, for example, 3 mm to 30 mm, or 5 mm to 15 mm. The position and number of the fixing tape 50 are not particularly limited as long as the fixing tape 50 is attached so as to cover a part of the winding end portion 12a exposed on the outermost peripheral surface of the electrode body 14, and may be attached, for example, along the axial direction.
[0018] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The material of the separator 13 is preferably an olefin resin such as polyethylene or polypropylene. The thickness of the separator 13 is, for example, 10 μm to 50 μm. The separator 13 tends to be thinner as the capacity and output of the battery increase. The separator 13 has a melting point of, for example, about 130° C. to 180° C.
[0019] Next, the positive electrode 11 and the negative electrode 12 constituting the electrode body 14 will be described with reference to FIG. 3. FIG. 3 is an explanatory diagram showing the positive electrode 11 and the negative electrode 12 in a developed state. In the electrode body 14, the negative electrode 12 is formed larger than the positive electrode 11 in order to prevent lithium deposition in the negative electrode 12. Specifically, the length of the negative electrode 12 in the width direction (axial direction) is larger than the length of the positive electrode 11 in the width direction. In addition, the length of the negative electrode 12 in the longitudinal direction is larger than the length of the positive electrode 11 in the longitudinal direction. As a result, when wound into the electrode body 14, at least the entire part of the positive electrode 11 where the positive electrode mixture layer 32 is formed is disposed opposite the part of the negative electrode 12 where the negative electrode mixture layer 42 is formed via the separator 13.
[0020] The positive electrode 11 has a strip-shaped positive electrode current collector 30 and a positive electrode mixture layer 32 formed on both the inner and outer circumferential sides of the positive electrode current collector 30. For the positive electrode current collector 30, for example, a foil of a metal such as aluminum, or a film having such a metal disposed on the surface layer, is used. A suitable positive electrode current collector 30 is a foil of a metal mainly composed of aluminum or an aluminum alloy. The thickness of the positive electrode current collector 30 is, for example, 10 μm to 30 μm.
[0021] The positive electrode active material layer 32 is preferably formed over the entire area of both surfaces of the positive electrode current collector 30, excluding the positive electrode current collector exposed portions 34 described later. The positive electrode active material layer 32 preferably contains a positive electrode active material, a conductive agent, and a binder. The positive electrode 11 is produced by applying a positive electrode active material slurry containing a positive electrode active material, a conductive agent, a binder, and a solvent such as N-methyl-2-pyrrolidone (NMP) to both surfaces of the positive electrode current collector 30, and then drying and compressing the positive electrode active material layer 32.
[0022] Examples of the positive electrode active material include lithium-containing transition metal oxides containing transition metal elements such as Co, Mn, and Ni. The lithium-containing transition metal oxide is not particularly limited, but is preferably a composite oxide represented by the general formula Li 1+x MO2 (wherein -0.2 < x ≦ 0.2, and M contains at least one of Ni, Co, Mn, and Al).
[0023] Examples of the above-mentioned conductive agent include carbon materials such as carbon black (CB), acetylene black (AB), ketjen black, and graphite. Examples of the above-mentioned binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide (PI), acrylic resins, and polyolefin resins. Further, these resins may be used in combination with carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), etc. These may be used alone or in combination of two or more.
[0024] In the example shown in FIG. 3, a positive electrode current collector exposed portion 34 is provided at the central portion in the longitudinal direction of the positive electrode 11 over the entire length in the width direction. The positive electrode current collector exposed portion 34 is a portion where the surface of the positive electrode current collector 30 is not covered by the positive electrode active material layer 32. The positive electrode current collector exposed portion 34 is provided, for example, by intermittent coating in which the positive electrode active material slurry is not applied to a part of the positive electrode current collector 30.
[0025] One end of the positive electrode lead 19 is connected to the positive electrode current collector exposed portion 34 by ultrasonic welding or the like. From the viewpoint of the workability of the connection work of the positive electrode lead 19, it is preferable that the positive electrode current collector exposed portion 34 is provided on both sides of the positive electrode 11 so as to overlap in the thickness direction of the positive electrode 11. From the viewpoint of current collection, it is preferable that the positive electrode lead 19 is provided at a position approximately equidistant from the winding start end and the winding end end 11a. When wound into the electrode body 14, the other end of the positive electrode lead 19 extends upward from the end face in the width direction at the radial middle position of the electrode body 14. The arrangement position of the positive electrode lead 19 is not particularly limited to the example shown in FIG. 3, and the positive electrode current collector exposed portion 34 can be provided according to the arrangement position of the positive electrode lead 19.
[0026] The negative electrode 12 has a strip-shaped negative electrode current collector 40 and a negative electrode mixture layer 42 formed on both sides of the negative electrode current collector 40. For the negative electrode current collector 40, for example, a foil of a metal such as copper, or a film having such a metal disposed on its surface layer, etc. is used. The thickness of the negative electrode current collector 40 is, for example, 5 μm to 30 μm.
[0027] The negative electrode mixture layer 42 is preferably formed on the entire area of both sides of the negative electrode current collector 40 except for a negative electrode current collector exposed portion 44 described later. The negative electrode mixture layer 42 preferably contains a negative electrode active material and a binder. The negative electrode 12 is produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, water, and the like to both sides of the negative electrode current collector 40, and then drying and compressing the negative electrode mixture layer 42.
[0028] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions, and can be, for example, a carbon material such as natural graphite or artificial graphite, a metal that alloys with lithium such as Si or Sn, or an alloy or oxide containing these. For example, the same resin as that in the positive electrode 11 is used as the binder contained in the negative electrode mixture layer 42. When preparing the negative electrode mixture slurry using an aqueous solvent, styrene-butadiene rubber (SBR), CMC or a salt thereof, polyacrylic acid or a salt thereof, polyvinyl alcohol, etc. can be used. These materials can be used alone or in combination of two or more.
[0029] 3, a negative electrode current collector exposed portion 44 is provided over the entire length of the current collector in the width direction at the winding start end and winding end portion 12a in the longitudinal direction of the negative electrode 12. The negative electrode current collector exposed portion 44 is a portion of the surface of the negative electrode current collector 40 that is not covered with the negative electrode mixture layer 42. The negative electrode current collector exposed portion 44 is provided, for example, by intermittent application in which the negative electrode mixture slurry is not applied to a part of the negative electrode current collector 40.
[0030] One end of the negative electrode lead 20 is connected to the negative electrode current collector exposed portion 44 at the winding start end by ultrasonic welding or the like. From the viewpoint of workability in connecting the negative electrode lead 20, it is preferable that the negative electrode current collector exposed portion 44 is provided on both sides of the negative electrode 12 so as to overlap in the thickness direction of the negative electrode 12. When wound into the electrode body 14, the other end of the negative electrode lead 20 extends downward from the end face in the width direction near the center of the winding axis of the electrode body 14. The position of the negative electrode lead 20 is not particularly limited to the example shown in FIG. 3, and the negative electrode current collector exposed portion 44 can be provided in accordance with the position of the negative electrode lead 20.
[0031] The negative electrode current collector exposed portion 44 of the winding end portion 12a is located on the outermost peripheral surface of the electrode body 14 and is in contact with the exterior body 15. This ensures a current path to the negative electrode terminal in addition to the negative electrode lead 20, improving the output characteristics of the battery.
[0032] By exposing the negative electrode 12 on the outermost peripheral surface of the electrode body 14, a current path to the negative terminal at the winding end portion 12a is ensured, but it is preferable that the negative electrode current collector 40 is exposed as in one example of the embodiment. It is more preferable that the negative electrode current collector 40 is exposed on the entire outermost peripheral surface of the electrode body 14. This increases the contact area between the negative electrode current collector exposed portion 44 and the exterior body 15, improving the output characteristics of the battery. When the negative electrode current collector 40 is exposed on the entire outermost peripheral surface of the electrode body 14, the longitudinal length of the negative electrode current collector exposed portion 44 may be greater than the outermost peripheral length of the electrode body 14.
[0033] In the above, in FIG. 3, the case where the exterior body 15 is a negative electrode terminal has been described, but when the exterior body 15 is a positive electrode terminal, the positive electrode 11 may be exposed at the outermost peripheral surface of the electrode body 14. This ensures a current path to the positive electrode terminal at the winding end 11a of the positive electrode 11. The fixing tape 50 is attached so as to cover at least a part of the winding end 11a of the positive electrode 11 exposed at the outermost peripheral surface of the electrode body 14. As in the case where the negative electrode 12 is exposed at the outermost peripheral surface of the electrode body 14, it is preferable that a positive electrode current collector exposed portion 34 is provided at the winding end 11a of the positive electrode 11, and the positive electrode current collector 30 is exposed at the outermost peripheral surface of the electrode body 14.
[0034] Next, the fixing tape 50, which is a member for winding up the electrode body 14, will be described with reference to Fig. 4. Fig. 4 is a cross-sectional view of the fixing tape 50 in one example of the embodiment. The fixing tape 50 has a base layer 52 and an adhesive layer 54, and is attached to the positive electrode 11 or negative electrode 12 exposed on the outermost peripheral surface of the electrode body 14 by the adhesive layer 54.
[0035] The base layer 52 has an uneven surface as shown in Fig. 4. The period of the uneven surface of the base layer 52 may be regular or irregular. Although the uneven surface of the base layer 52 may have unevenness in a specific direction, it is preferable that the uneven surface of the base layer 52 has unevenness in all directions.
[0036] The base material layer 52 has a surface roughness (Sa) of 40 μm or more in at least a region 1 mm wide from the end. By setting the surface roughness (Sa) to 40 μm or more near the end of the fixing tape 50, where stress due to contact pressure between the electrode body 14 and the exterior body 15 is likely to concentrate, the stress is alleviated and deformation such as bending of the positive electrode 11 and the negative electrode 12 can be suppressed. Here, the surface roughness (Sa) is defined in ISO25178 and can be measured using a commercially available microscope such as the VR-3200 manufactured by KEYENCE Corporation.
[0037] The surface roughness (Sa) of the entire surface of the base material layer 52 is preferably 40 μm or more. This allows stress to be relieved not only in the vicinity of the ends of the base material layer 52 but also over the entire surface of the base material layer 52, so that deformation such as bending of the positive electrode 11 and the negative electrode 12 can be more reliably suppressed.
[0038] From the viewpoint of maintaining the battery characteristics, the surface roughness (Sa) of the base material layer 52 is preferably 150 μm or less. If the surface roughness (Sa) of the base material layer 52 is increased, the thickness of the fixing tape 50 increases, and the space for accommodating the electrode body 14 and the electrolyte within the exterior body 15 decreases.
[0039] The base material layer 52 can be appropriately selected from the viewpoints of strength, resistance to the electrolyte, processability, cost, etc., and can be made of, for example, PP (polypropylene), PI (polyimide), PET (polyethylene terephthalate), etc. The adhesive layer 54 is preferably made of a resin having adhesiveness at room temperature, and can be made of, for example, an acrylic resin or a rubber resin.
[0040] 4, t indicates the thickness of the fixing tape 50. t is the thickness from the apex of the base layer 52 to the surface of the adhesive layer 54. The size of t is, for example, 20 μm to 200 μm, and preferably 50 μm to 100 μm.
[0041] The method for producing the uneven surface of the base layer 52 is not particularly limited, but for example, the fixing tape 50 having an interleaf paper attached to the adhesive layer 54 can be produced by pressing the fixing tape 50 against a roller having an uneven surface. The surface roughness (Sa) of the base layer 52 can be adjusted by the surface roughness (Sa) of the roller and the magnitude of the pressing pressure of the roller. For example, a fixing tape 50 having a surface roughness (Sa) of 40 μm or more can be produced by pressing a roller having a surface roughness (Sa) of 200 μm to 400 μm with a linear pressure of 10 kgf / cm to 100 kgf / cm. EXAMPLES
[0042] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0043] <Example 1> [Preparation of test specimens] 95 parts by mass of graphite, 5 parts by mass of SiO, 1 part by mass of carboxymethyl cellulose (CMC), and 1 part by mass of styrene butadiene rubber (SBR) were mixed, and an appropriate amount of water was added to prepare a negative electrode mixture slurry. Next, the negative electrode mixture slurry was applied to one side of a belt-shaped negative electrode current collector made of copper foil with a thickness of 8 μm, and then the coating film was dried. The dried coating film was compressed using a roller, and then cut to a predetermined electrode plate size to prepare a negative electrode in which a negative electrode mixture layer was formed on one side of the negative electrode current collector.
[0044] A flat tape was produced by applying a 10 μm thick layer of acrylic adhesive onto a 20 μm thick polypropylene (PP) base layer. A polypropylene (PP) slip sheet coated with a release agent was then attached to the adhesive layer, and a roller with an uneven surface and a surface roughness of 320 μm was pressed against the base layer side with a linear pressure of 60 kgf / cm, after which the tape was cut to a width of 10 mm to produce a fixed tape with unevenness over the entire surface of the base layer side.
[0045] The fixing tape from which the insert paper had been peeled off was attached to the surface of the negative electrode on which the negative electrode mixture layer was not formed, to prepare a test piece.
[0046] <Example 2> A test piece was prepared in the same manner as in Example 1, except that the linear pressure applied to compress the flat tape with the roller was 40 kgf / cm.
[0047] <Example 3> A test piece was prepared in the same manner as in Example 1, except that the linear pressure applied to compress the flat tape with the roller was 20 kgf / cm.
[0048] <Comparative Example 1> A test piece was prepared in the same manner as in Example 1, except that the linear pressure applied to compress the flat tape with the roller was 5 kgf / cm.
[0049] <Comparative Example 2> A test specimen was prepared in the same manner as in Example 1, except that the flat tape was not compressed with a roller.
[0050] [Measurement of surface roughness (Sa) of base layer] The surface roughness (Sa) of each of the fixing tapes produced in Examples 1 to 3 and Comparative Examples 1 and 2 was measured at a magnification of 25 times using a VR-3200 manufactured by KEYENCE Corporation before being attached to the negative electrode.
[0051] [Stress application test] For the test pieces of Examples 1 to 3 and Comparative Examples 1 and 2, a stress application test was performed using a stress application device shown in Fig. 5 to evaluate the possibility of deformation such as bending of the positive electrode and negative electrode caused by the fixing tape. Details of the stress application test are as follows.
[0052] FIG. 5(a) is a plan view of the stress application device 60, and FIG. 5(b) is a cross-sectional view of the line AA in FIG. 5(a) as viewed from the direction of the arrow. The stress application device 60 has a test stand 70, a chloroprene rubber sheet 72 as a buffer material, and an indenter 74. As shown in FIG. 5(b), the test piece 62 was placed on the chloroprene rubber sheet 72 so that the negative electrode mixture layer 42 was facing downward and the fixing tape 50 was facing upward. As shown in FIG. 5(a), the test piece 62 has a 10 mm wide fixing tape 50 covering a part of the negative electrode current collector 40. After placing the test piece 62, a stress of 4 kN was applied for 10 seconds with a 20 mm square indenter to a range including the boundary between the negative electrode current collector 40 and the fixing tape 50. In this test, a stress larger than the stress actually received by the outer periphery 15 of the electrode body 14 was applied to the test piece 62. Therefore, when the fixing tape 50 has a large effect on deformation such as bending of the positive and negative electrodes, the negative electrode current collector 40 breaks at a break evaluation portion 76 corresponding to the boundary between the negative electrode current collector 40 and the fixing tape 50. On the other hand, when the fixing tape 50 has a small effect on deformation such as bending of the positive and negative electrodes, breakage of the negative electrode current collector 40 at the break evaluation portion 76 is suppressed. Therefore, in this test, the possibility of occurrence of deformation such as bending of the positive and negative electrodes caused by the fixing tape 50 was evaluated by observing the presence or absence of breakage of the negative electrode current collector 40 at the break evaluation portion 76 after the test.
[0053] Table 1 shows the surface roughness (Sa) of each of the fixing tapes used in Examples 1 to 3 and Comparative Examples 1 and 2, and the presence or absence of breakage in each test piece after testing.
[0054] [Table 1]
[0055] In Comparative Examples 1 and 2, in which the surface roughness (Sa) of the fixing tape was small, the negative electrode current collector broke at the break evaluation site, whereas in Examples 1 to 3, in which the surface roughness (Sa) of the fixing tape was large, the negative electrode current collector did not break. That is, in Examples 1 to 3, the fixing tape had little effect on deformation such as bending of the positive and negative electrodes, so the possibility of deformation of the positive and negative electrodes caused by the fixing tape was low. This shows that by increasing the surface roughness (Sa) of the fixing tape, deformation such as bending of the negative and positive electrodes can be suppressed even when contact pressure occurs between the electrode body and the exterior body. [Explanation of symbols]
[0056] 10 secondary battery, 11 positive electrode, 12 negative electrode, 12a winding end portion, 13 separator, 14 electrode body, 15 exterior body, 16 sealing body, 17, 18 insulating plate, 19 positive electrode lead, 20 negative electrode lead, 21 grooved portion, 22 filter, 23 lower valve body, 24 insulating member, 25 upper valve body, 26 cap, 26a opening, 27 gasket, 30 positive electrode current collector, 32 positive electrode mixture layer, 34 positive electrode current collector exposed portion, 40 negative electrode current collector, 42 negative electrode mixture layer, 44 negative electrode current collector exposed portion, 50 fixing tape, 52 base material layer, 54 adhesive layer, 60 stress application device, 62 test piece, 70 test stand, 72 chloroprene rubber sheet, 74 indenter, 76 fracture evaluation portion
Claims
1. A nonaqueous electrolyte secondary battery comprising: a wound electrode assembly in which a strip-shaped positive electrode and a strip-shaped negative electrode are wound with a separator interposed therebetween; and a metal exterior body that houses the electrode assembly, the positive electrode or the negative electrode is exposed on the outermost peripheral surface of the electrode body, and a fixing tape having a base layer and an adhesive layer is attached to the positive electrode or the negative electrode by the adhesive layer; The nonaqueous electrolyte secondary battery, wherein the substrate layer has a surface roughness (Sa) of 40 μm or more in at least a region having a width of 1 mm from an end portion.
2. The nonaqueous electrolyte secondary battery according to claim 1 , wherein the exterior body is cylindrical.
3. the positive electrode has a positive electrode current collector and a positive electrode mixture layer formed on a surface of the positive electrode current collector, the negative electrode has a negative electrode current collector and a negative electrode mixture layer formed on a surface of the negative electrode current collector, 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the positive electrode current collector or the negative electrode current collector is exposed at the outermost peripheral surface of the electrode assembly.
4. 4. The nonaqueous electrolyte secondary battery in accordance with claim 3, wherein the negative electrode current collector is exposed over the entire outermost peripheral surface of the electrode assembly.
5. 5. The nonaqueous electrolyte secondary battery according to claim 1, wherein the surface roughness (Sa) of the entire surface of the base layer is 40 μm or more.
Citation Information
Patent Citations
Lithium ion secondary battery
JP2007184234A
sealing tape
JP2016532752A
Secondary battery
JP2017016806A
Lithium ion rechargeable battery
US20070154789A1
Non-aqueous electrolyte secondary battery
WO2016147564A1