Plasma etching of mask materials
The plasma etching method addresses the challenge of etching multiple layers with varying etch resistance in photomasks by using fluorine and halogen precursors and adjustable bias frequencies, ensuring precise and stable etching across layers.
Patent Information
- Application Number
- JP2023565492
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-28
- Filing Date
- 2022-04-07
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2042-04-07
AI Technical Summary
Conventional etching methods struggle to selectively etch multiple layers of photomask materials with varying etch resistance, leading to issues like critical dimension loss, sloped sidewalls, and misalignment in semiconductor manufacturing, particularly at advanced technology nodes.
A plasma etching method using fluorine-containing and halogen-containing precursors, adjustable bias frequencies, and controlled chamber conditions to tailor etching processes in situ, accommodating the properties of different materials within the photomask stack.
Enables precise, controlled dry etching that maintains dimensional stability and profile integrity across multiple layers, reducing misalignment and critical dimension loss, and improving device yield.
Smart Images

Figure 0007564968000001 
Figure 0007564968000002 
Figure 0007564968000003
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of and priority to U.S. Non-provisional Application No. 17 / 242,758, filed April 28, 2021, and entitled “PLASMA ETCHING OF MASK MATERIALS,” the contents of which are incorporated herein by reference in their entirety for all purposes. [Technical field]
[0002] The present technology relates to semiconductor processes and equipment, and more particularly to selectively etching mask structures. [Background technology]
[0003] Integrated circuits can be built by processes that fabricate intricately patterned layers of material on a substrate surface. To fabricate patterned materials on a substrate, a controlled method is needed to remove exposed material. Chemical etching is used for a variety of purposes including transferring patterns in photoresist to an underlying layer, thinning a layer, or reducing the lateral dimensions of features already present on the surface. It is often desirable to have an etch process that etches one material faster than another, for example to facilitate the pattern transfer process. Such an etch process is said to be selective to the first material. Due to the wide variety of materials, circuits, and processes, etch processes are developed with selectivity to a variety of materials.
[0004] Etch processes can be referred to as wet or dry based on the materials used in the process. For example, wet etches can preferentially remove some oxide dielectrics over other dielectrics and materials. However, wet processes can have difficulty penetrating some constrained trenches and can also deform the remaining materials in some cases. Dry etches, which are performed in a local plasma formed within the substrate processing region, can penetrate more constrained trenches and are less likely to deform delicate remaining structures. However, the local plasma can damage the substrate through the creation of electric arcs when the local plasma discharges.
[0005] Thus, there is a need for improved systems and methods that can be used to manufacture high quality devices and structures. These and other needs are addressed by the present technology. Summary of the Invention
[0006] An exemplary etching method can include forming a plasma of a fluorine-containing precursor to generate plasma effluents. A first bias frequency can be applied while forming the plasma. The method can include contacting a substrate contained in a processing region of the semiconductor processing chamber with the plasma effluents. The substrate can be or can include a photomask. The method can include etching a first layer of the photomask. Etching the first layer of the photomask can expose a second layer of the photomask. The method can include adjusting the first bias frequency to a second bias frequency while maintaining the plasma of the fluorine-containing precursor. The method can include etching the second layer of the photomask.
[0007] In some embodiments, the photomask can include a mirror layer, an absorber covering the mirror layer, and a capping layer disposed between the absorber and the mirror layer. The capping layer can include a metal. The photomask can include a hardmask covering the absorber. The photomask can include an anti-reflective coating layer disposed between the hardmask and the absorber. At least one of the hardmask and the anti-reflective coating layer can be or can include an oxide or nitride material. The photomask can include a layer of material disposed between the hardmask and the anti-reflective coating layer. The layer of material can be or can include a metal. The fluorine-containing precursor can include a first fluorine-containing precursor. The fluorine-containing precursor can include a second halogen-containing precursor. The first fluorine-containing precursor can include carbon and the second halogen-containing precursor can be carbon-free.
[0008] The flow ratio of the first fluorine-containing precursor to the second halogen-containing precursor may be greater than 2:1 or may be about 2:1. The method may include adjusting the flow ratio of the first fluorine-containing precursor and the second halogen-containing precursor subsequent to etching the first layer of the photomask. The fluorine-containing precursor may include a third precursor. The third precursor may include carbon. The third precursor may be utilized only during either etching the first layer of the photomask or etching the second layer of the photomask. The chamber pressure in the semiconductor processing chamber may be maintained at less than or about 50 mTorr. The third layer of the photomask may be exposed by etching the second layer of the photomask. The method may include adjusting the second bias frequency to a third bias frequency while maintaining the plasma of the fluorine-containing precursor. The applied power or effective power may be less than or about 500 W and may be provided as continuous wave, source pulsed, bias pulsed, or both source pulsed and bias pulsed.
[0009] Some embodiments of the present technology may include an etching method. The method may include forming a plasma of a first fluorine-containing precursor and a second halogen-containing precursor to generate plasma effluents. A first bias frequency may be applied while forming the plasma. The method may include contacting a substrate contained in a processing region of a semiconductor processing chamber with the plasma effluents. The substrate may be or may include a photomask. The photomask may include at least three layers between a hard mask and a mirror layer of the photomask. The method may include etching a first layer of the photomask. Etching the first layer of the photomask may expose a second layer of the photomask. The method may include at least one of adjusting the first bias frequency to a second bias frequency, adjusting a pressure in the semiconductor processing chamber, adjusting an effective power of either the source electrode or the bias electrode, or both electrodes, or adjusting a flow ratio between the first fluorine-containing precursor and the second halogen-containing precursor. The method may include etching the second layer of the photomask.
[0010] In some embodiments, the method can include detecting exposure of the second layer of the photomask while etching the first layer of the photomask. The photomask can include a mirror layer, an absorber covering the mirror layer, and a capping layer disposed between the absorber and the mirror layer. The capping layer can be or can include a metal. The absorber can be or can include at least two layers of material. Etching the second layer of the photomask can expose the third layer of the photomask. The method can include etching the third layer of the photomask. The bias frequency can be maintained between either the etching of the first layer of the photomask and the second layer of the photomask or the etching of the second layer of the photomask and the etching of the third layer of the photomask. At least one of the three layers can include a first transition metal. The hardmask can include a second metal characterized by a hardness or etch resistance less than the hardness or etch resistance of the first transition metal. The plasma can also be formed with a third precursor. The first fluorine-containing precursor can contain carbon, the second halogen-containing precursor can be carbon-free, and the third precursor can contain carbon.
[0011] Some embodiments of the present technology may include an etching method. The method may include forming a plasma of at least one fluorine-containing precursor to generate plasma effluents. A first bias frequency may be applied while forming the plasma. The method may include contacting a substrate contained in a processing region of a semiconductor processing chamber with the plasma effluents. The substrate may be or may include a photomask. Also, the photomask may include at least two layers between a hard mask and a mirror layer of the photomask. The method may include etching a first layer of the photomask. Etching the first layer of the photomask may expose a second layer of the photomask. The method may include adjusting the first bias frequency to a second bias frequency. The first bias frequency may be greater than or about 10 MHz, and the second bias frequency may be less than or about 10 MHz. Also, either or both bias frequencies may be a combination of frequencies. The method may include etching a second layer of the photomask. In some embodiments, the photomask can include a mirror layer, an absorber covering the mirror layer, and a metal-containing capping layer disposed between the absorber and the mirror layer.
[0012] Such techniques can provide many advantages over conventional systems and techniques. For example, the process can enable the performance of a precisely controlled dry etch, which can preserve various materials on the substrate. Additionally, the process can selectively tune in situ to etch subsequent materials in the stack to generate features that extend through multiple layers of the structure. These and other embodiments, along with their many advantages and features, are described in more detail in the following description and in conjunction with the accompanying figures.
[0013] A further understanding of the nature and advantages of the disclosed technology may be realized by reference to the remaining portions of the specification and the drawings. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic cross-sectional view of an exemplary processing chamber in accordance with some embodiments of the present technique. [Diagram 2] 1 illustrates an exemplary process in a method according to some embodiments of the present technology. [Figure 3A-B] 1 is a schematic cross-sectional view of an etched material in accordance with some embodiments of the present technique; [Figure 3C-D] 1 is a schematic cross-sectional view of an etched material in accordance with some embodiments of the present technique; [Figure 3E] 1 is a schematic cross-sectional view of an etched material in accordance with some embodiments of the present technique; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Some of the figures are included as schematics. It is understood that the figures are for illustrative purposes and should not be considered to scale unless expressly stated to be to scale. Furthermore, as schematics, the figures are provided to facilitate understanding and may in some cases not include all aspects or information as compared to realistic representations and may in some cases include additional or exaggerated material for illustrative purposes.
[0016] In the accompanying figures, similar components and / or features may have the same reference label. Furthermore, various components of the same type may be distinguished by a letter following the reference label, which distinguishes between the similar components. If only a first reference label is used in the specification, the description may apply to any component among the similar components having that same first reference label, regardless of the letter.
[0017] When moving to smaller technology nodes, such as the 7 nm node, and in smaller semiconductor manufacturing, improved techniques for patterning, such as extreme ultraviolet ("EUV") lithography, can be used. EUV lithography utilizes a photomask structure that is patterned using a specific integrated circuit design. The photomask is then incorporated into a lithography scanner and used to pattern an image onto a substrate. EUV lithography utilizes a composite mask structure having multiple layers including a mirror structure and an absorber. EUV technology can be characterized by several challenges, including mask 3D effects. Mask 3D effects include the protrusion of the absorber from the mirror structure, which can result in shadowing effects or imaging misalignment on the substrate during processing. These effects can result in misalignment and focus issues between one-dimensional and two-dimensional features.
[0018] In an attempt to solve the mask 3D effect, newer materials are utilized and feature sizes are adjusted, but these changes bring new problems with respect to patterning. For example, many conventional techniques utilize ion-beam etching to pattern absorber materials. Ion-beam etching essentially results in the sputter removal of material through a bombardment process using ions, such as from argon or other inert materials. However, as the range of materials sought to be incorporated into photomasks becomes wider, materials featuring different hardness values can be used in one or more layers of the mask structure. Thus, hardmasks used for patterning may have difficulty surviving the bombardment, as the etch resistance of the underlying material being etched increases. In practice, the increase in power required to etch the underlying material cannot be compensated for by a thicker hardmask, and critical dimension openings may occur. This can cause the absorber sidewalls to slope, which can result in critical dimension losses during processing, and straight sidewalls are sought to improve mask operation.
[0019] The present technology overcomes these limitations by implementing a selective etch process that can be adapted in situ to tailor the etching operation between layers of the structure. By tailoring within the chemical and multiple physical bombardment schemes, the present technology can improve selective removal and can also improve the sidewall angle of the absorber structure. While the remaining disclosure routinely identifies specific materials and semiconductor structures that utilize the disclosed technology, it will be readily understood that the systems, methods and materials are equally applicable to many other structures that can benefit from aspects of the present technology. Thus, the present technology should not be construed as being limited to use only with any particular process or material. Additionally, while an exemplary chamber is described to provide a foundation for the present technology, it should be understood that the present technology can be applied to virtually any semiconductor processing chamber that can tolerate the operations described.
[0020] FIG. 1 illustrates a schematic cross-sectional view of an exemplary processing chamber 100 according to some embodiments of the present technique. The processing chamber 100 may generally include a processing chamber body 102 having a substrate support 124 or pedestal, and a controller 146. The chamber body 102 may have a conductive wall 104 that may support a substantially flat dielectric ceiling 108. Other embodiments of the processing chamber 100 may have other types of ceilings, such as a domed ceiling or a sloped ceiling. An antenna 110 may be disposed above the ceiling 108. The antenna 110 may include one or more inductive coil elements, such as coaxial elements 110a and 110b, that may be selectively controlled. The antenna 110 may be coupled to a plasma power source 112 via a first matching network 114. The plasma power source 112 may be capable of generating up to about 3000 W at a tunable frequency ranging from about 50 kHz to about 13.56 MHz.
[0021] The substrate pedestal 124 may operate as a cathode in some embodiments and may be coupled to a biasing power supply 140 via a second matching network 142. The biasing power supply 140 may provide up to about 600 W at a tunable continuous wave as well as pulsed frequencies ranging from about 100 Hz to about 10 kHz. The biasing power supply 140 may generate a pulsed RF power output, or the biasing power supply 140 may generate a pulsed DC power output. As previously mentioned, the power supply 140 may also provide a constant DC and / or RF power output. The substrate support 124 may include an electrostatic chuck 160. The electrostatic chuck 160 may include at least one clamping electrode 132 and may be controlled by a chuck power supply 166. In some embodiments, the substrate support 124 may include additional substrate retention mechanisms such as a susceptor clamp ring, a vacuum chuck, a mechanical chuck, or any other mechanical or other configuration for maintaining the substrate in place during processing or etching operations.
[0022] A gas panel 120 can be coupled to the processing chamber 100 to provide process gases and / or other gases to the interior of the processing chamber body 102. In some illustrated embodiments, the gas panel 120 can be coupled to one or more inlets 116 formed in a channel 118 in the conductive wall 104 of the chamber body 102. The one or more inlets 116 can also be provided elsewhere, such as the ceiling 108 of the processing chamber. The pressure of the processing chamber 100 can be controlled using a throttle valve 162 and a vacuum pump 164. The vacuum pump 164 and the throttle valve 162 may be capable of maintaining a chamber pressure ranging from about 1 mTorr to about 50 mTorr during processing operations. The temperature of the wall 104 can be controlled using liquid-containing conduits that can be run through the wall 104 in any number of continuous or segmented patterns. The wall temperature can be typically maintained at room temperature, above room temperature, or below room temperature. In some embodiments, the chamber walls 104 may be formed from or include a metal such as aluminum, stainless steel, or other metals used in semiconductor processing chambers, and the chamber walls 104 may be coupled to an electrical ground 106. The processing chamber 100 may also include a number of additional systems for process control, internal diagnostics, endpoint detection, or other operations that may facilitate semiconductor processing, each of which is collectively referred to as support systems 154.
[0023] A reticle adapter 182 may be used to secure a substrate, such as a reticle or other substrate 122, onto the substrate support 124. The reticle adapter 182 may typically include a bottom portion 184 machined to cover an upper surface of the substrate support 124, such as the electrostatic chuck 160, and a top portion 186 having an opening 188 sized and shaped to hold the substrate 122. The opening 188 may be generally or substantially centered relative to the substrate support 124. The adapter 182 may typically be formed from a single piece of etch-resistant, high-temperature resistant material, such as polyimide ceramic or quartz. An edge ring 126 may cover the adapter 182 and / or secure the adapter 182 to the pedestal 124, as shown. A lifting mechanism 138 may be used to lower or raise the adapter 182 so that the substrate 122 may be placed on or removed from the substrate support 124. Generally, the lifting mechanism 138 may be or may include a number of lift pins, such as the illustrated lift pin 130 , which may move through respective guide holes 136 .
[0024] During processing, the temperature of the substrate 122 can be controlled by stabilizing the temperature of the substrate support 124. In some embodiments, the substrate support 124 can include a heater 144 and / or an optional heat sink 128. The heater 144 can be one or more fluid conduits configured to receive and direct a heat transfer fluid through a channel to maintain a temperature. Additionally, the heater 144 can be or include at least one heating element 134 that can be regulated by a heater power supply 168. A backside gas, such as helium or any other gas, from a gas source 156 can be provided through a gas conduit 158 to a channel that can be formed on a pedestal surface below the substrate 122. The backside gas can be used to facilitate heat transfer between the substrate support 124 and the substrate 122. During processing, the substrate support 124 can be heated to a steady state temperature by the embedded heater 144, which, in combination with the helium backside gas, can facilitate uniform heating of the substrate 122.
[0025] The controller 146 may include a central processing unit ("CPU") 150, a memory 148 for the CPU 150, and support circuits 152, which may facilitate control of the components of the processing chamber 100 and etch processes, such as the processes or operations discussed in more detail below. The controller 146 may be one of any form of general-purpose computer processor and sub-processors that may be used in industrial settings to control various chambers. The memory 148 of the CPU 150 may be one or more of readily available memories, such as random-access memory, read-only memory, floppy disk, hard disk, or any other form of digital storage, local or remote memory. The support circuits 152 may be coupled to the CPU 150 to support the processor in any number of ways that will be readily understood by those skilled in the art. The support circuits may include cache, power supplies, clock circuits, input / output circuitry and subsystems, and any other computing components. The processes or operations may typically be stored in the memory 148 or other computer-readable medium that is accessible to the CPU 150 as software routines. Alternatively, the software routines may also be stored and / or executed by a second CPU that is located remotely from the hardware being controlled by CPU 150.
[0026] The chambers already discussed can be used to perform exemplary methods, including etching methods. Referring to FIG. 2, an exemplary process in a method 200 according to an embodiment of the present technology is shown. The method 200 can include one or more processes prior to the start of the method, including front-end processing, deposition, etching, polishing, cleaning, or any other process that can be performed prior to the described processes. The method can include many optional processes that may or may not be specifically associated with some embodiments of the method according to an embodiment of the present technology. For example, many of the operations are described to provide a broader scope of processes that may be performed, but are not critical to the technology or may be performed in an alternative manner as discussed further below. The method 200 can describe the process shown generally in FIGS. 3A-3E, and the illustrations of FIGS. 3A-3E will be described in connection with the process of the method 200. It should be understood that the figures are merely partially schematic illustrations, and that the substrate can include any number of additional materials and features having various properties and aspects as illustrated in the figures.
[0027] Method 200 may or may not include optional processing for deploying the semiconductor structure in a particular manufacturing process. It should be understood that method 200 may be performed on any number of semiconductor structures, including photomask 300, as illustrated in FIG. 3A, which may be a photolithographic reticle or photomask, as illustrated. For example, the exemplary photomask structure may include one or more layers that may be utilized or patterned. The exposed material at any time during the etch process may be or include a metal material, one or more dielectric materials, an alloy layer, a hardmask material, or any other material that may be used for a photomask or other substrate. While any number of photomasks or other semiconductor structures may be encompassed by the present technique, in some embodiments, photomask 300 may be an EUV photomask that may be patterned by some embodiments of the present technique.
[0028] For example, Figure 3A can illustrate a photomask structure that can be patterned to produce a reticle for photolithography. The remaining disclosure will refer to the illustrated EUV mask structure, but it should be understood that the materials can include any number of alternatives as described by the embodiments of the present technology, and the described process can include etching one or more layers of the structure that can be formed from any number of materials. It should be understood that the structures mentioned are not intended to be limiting, and that any of a variety of other semiconductor structures including alternative photomask structures, as well as any number of semiconductor layers incorporating the described materials, are similarly encompassed.
[0029] The technique can include a process for etching one or more layers including absorbers of an EUV photomask structure. As illustrated, the photomask structure can include many layers formed in succession to produce a structure, some of which can be etched to produce a photomask. As shown, a photomask 300, which can be a photomask structure, can include a quartz or low thermal expansion material substrate 305 that can form a base for an overlying structure. The substrate 305 can include a conductive backside coating 307 formed on the backside of the substrate, which can be or include one or more transition metal-containing materials, such as chromium, tantalum, or some other material, and which can include oxides or nitrides of these materials. The substrate 305 can be covered with a mirror layer 310, which can be a set of layers of alternating materials to produce a Bragg reflector. In embodiments of the present technology, the mirror layer may be or include any number of materials typically used in photomasks, and in one non-limiting example, the mirror layer may include alternating layers of molybdenum and silicon in any number of pairs, such as 40 pairs, also as a non-limiting example.
[0030] The mirror layer can be covered with a capping layer 312, which can protect the mirror layer from contact by the etchant during processing. The capping layer can be or include any metal, including any transition metal, such as ruthenium, as an example, and in any case, in some embodiments, can include both a metal layer and a buffer layer covering the metal layer. An absorber layer 315 can be disposed over the capping layer 312 and can be etched during embodiments of the present technology. The absorber can be characterized by a thin thickness to limit mask 3D effects, in some embodiments, the absorber can be characterized by a thickness of less than or about 50 nm, less than or about 40 nm, less than or about 30 nm, or less than 30 nm. In some embodiments, the absorber layer can include two or more layers of material, including a second layer 317, as illustrated and depicted by the hatched lines as shown. In some embodiments, the absorber can have consistent metals, such as particular transition metals, in individual layers and can also have one or more non-metallic materials, although in some embodiments including absorbers with multiple layers, the layers can include different metals, including different transition metals.
[0031] An anti-reflective coating layer 320 may be formed over the absorber layer, and in some embodiments, an additional metal layer 325 may be optionally formed over the anti-reflective coating layer 320. A hard mask 330 may be formed on top of the mask, followed by a resist 335, which may be patterned by a preceding photolithography operation. The method 200 may include, in some embodiments, optionally patterning the hard mask using a photoresist in optional operation 205, which may produce a patterned hard mask 330 over the photomask structure, as illustrated in FIG.
[0032] As previously discussed, conventional ion-beam etching can have difficulty patterning through the photomask layers between the hard mask 330 and the capping layer 312 while maintaining the feature critical dimensions. Furthermore, many mask layer materials may contain many additional metals, metal oxides, metal nitrides, or other metal-containing materials to meet the requirements of future nodes. Although ion-beam etching can etch through one or two tantalum layers while maintaining feature or pitch widths at feature sizes of tens of nanometers or more, ion-beam etching has proven unable to etch through advanced absorber and photomask materials without the pitch width becoming too wide or damaging one or more layers. For example, newer materials may include a combination of more etch resistant and less etch resistant materials throughout the layer stack, which may include two, three, four, or more layers of material as illustrated. More etch resistant or less etch resistant can mean both being physically more resistant to etching, such as by having a greater hardness, as well as being chemically more resistant to the etch process. Because ion-beam etching is limited to a high energy sputtering etch process, less etch resistant materials can be substantially over-etched as the process attempts to penetrate the more etch resistant material. This can result in extensive loss of anisotropic etch profile maintenance, which can affect absorber performance and otherwise cause device yield loss. Furthermore, as the number of material layers increases, ion-beam etching may not be able to selectively control the loss of the hard mask layer, requiring increased mask thickness, which may not be compatible with future nodes.
[0033] To overcome the problem of being unable to selectively etch multiple layers while maintaining dimensional stability, the present technique can perform a plasma etch that can be selectively adapted in situ to tailor specific stack layers. As mentioned above, by utilizing end-point detection in the processing chamber, subsequent layers of the stack can be identified and etch corrections can be performed as necessary to maintain the etch process. Although many examples will be discussed in connection with the methodology performed, it should be understood that the present technique can be performed using many variations to accommodate many different materials as well as the relationships between the materials of the stack being processed. Thus, the examples mentioned are not intended to limit the present technique, and it should be understood that the present technique encompasses multiple material combinations as further described below.
[0034] The material etched between the hard mask and the capping layer can include many layers and materials. For example, the layers can include one or more of the metal layer 325, the anti-reflective coating layer 320, and one or more layers of material for the absorber 315 according to embodiments of the present technology. Exemplary materials can include one or more transition metals from any of a variety of groups. For example, any of the layers of materials can include one or more metals, including alloys, and one or more non-metals. The layers can include any combination of metals and / or non-metals in embodiments of the present technology. One or more of the layers, for example the absorber layer, can include tantalum, either as a tantalum-based alloy, or as any combination of these, such as an oxide, nitride, carbide, boride, or oxynitride.
[0035] Furthermore, the present technology can be applied to advanced absorber materials that can include additional transition metal materials as well as non-metals. For example, any of the absorber 315, anti-reflective coating layer 320, and metal layer 325 can include, by way of non-limiting example, one or more of tantalum, ruthenium, cobalt, nickel, niobium, iridium, aluminum, chromium, molybdenum, tungsten, hafnium, rhenium, osmium, vanadium, titanium, platinum, tin, silver, zinc, gold, antimony, iron, silicon, and copper. Materials can be included as alloys such as nickel-aluminum, ruthenium-tungsten, chromium-nickel, any other metal-metal combination of many metals, and the like. Materials can also include one or more non-metals such as zinc telluride, silicon oxide, silicon nitride, tantalum oxynitride, tantalum oxide, tantalum nitride, chromium oxynitride, tantalum borate, tin oxide, and any other combination of metals and non-metals, as well as combinations of non-metals and non-metals.
[0036] Due to variations in advanced absorber materials, as well as hardmasks and layers between the hardmask and absorber, many stack combinations may have alternating layers characterized by different hardness qualities that may affect etching. As one non-limiting example, some embodiments may include a set of layers, where one or more layers include a metal characterized by a greater etch resistance than the hardmask layer. To accommodate etching of these structures, the present technology may provide in-situ modification of etching parameters, which may facilitate maintaining the etch profile while adjusting between layers. Additionally, the present technology may perform a combination of physical and chemical etching, which may be further adapted to accommodate various stacks of advanced photomasks.
[0037] The technique can perform the plasma etch independent of the material stack and can be further adapted using one or more parameters to accommodate different layer properties. For example, in some embodiments, the method 200 can include forming a plasma of a halogen-containing precursor in operation 210, which plasma can provide plasma effluents. In some embodiments, the plasma can be characterized by a first source power, a first bias power, and a first bias frequency. In operation 215, the plasma effluents can contact a substrate or a photomask, such as in a processing region of a semiconductor processing chamber as previously described. In operation 220, the plasma effluents can etch a first layer of the mask through the mask material. Etching can be maintained until the pattern in the hard mask is transferred through the first mask layer, thereby exposing a second layer of the photomask. Endpoint detection, as previously described, can be used to identify when the first layer of the mask has been completely etched and / or when the second layer of the mask has been exposed. Identification can occur in the processing chamber during etching of the first layer as well as during etching of any subsequent layers as described below. As illustrated in Figure 3C, a hard mask pattern may be applied through the first layer, and in some embodiments, the hard mask may be substantially maintained during the transfer or etching process. While the first layer may be metal layer 325 as illustrated, it should be understood that in some embodiments the first layer may be an anti-reflective coating layer, such as layer 320, or the first layer may be one of multiple layers of absorber material according to some embodiments of the present technology.
[0038] In operation 225, one or more parameters of the plasma etch can be performed while the substrate can be maintained in the processing chamber. In some embodiments, the parameters can be adjusted while the plasma is maintained to provide an adjustment in the etch process, although in some embodiments, the plasma can be stopped and then ignited following the adjustment. As described further below, the adjustment can include one or more operations including adjusting the first bias frequency to a second bias frequency, adjusting the pressure in the processing chamber, and / or adjusting the flow ratio of one or more precursors used in the etch process. Following the adjustment, the etch process can continue and a second layer of the photomask can be etched in operation 230. As shown in FIG. 3D, the etch can continue in the same chamber and the anti-reflective coating layer 320 can be etched, although as mentioned above, the second layer can be an absorber layer in some embodiments.
[0039] Method 200 may include one or more adjustments of the plasma or process parameters and may continue etching the third layer in optional operation 235. The plasma or process conditions may be the same or different while etching the second layer and may include multiple adjustments as previously described. Additionally, method 200 may include etching additional layers to continue through the stack of layers until the capping layer is exposed. As illustrated in FIG. 3E, the process may continue through any number of layers, including multiple absorber layers, until the capping layer or a buffer layer overlying the capping layer is exposed. Thus, in some embodiments, the etch parameters may be modified in situ and layer by layer as the etch process progresses through the stack of materials until the individual layers between the hard mask and the capping layer are etched. Although FIG. 3E illustrates a remaining hard mask, in some embodiments the hard mask may be partially left or removed during the etch process. Unlike ion-beam etching processes, the technique allows the profile to be substantially or essentially maintained layer by layer despite differences in material properties between the layers.
[0040] The etch process can provide the mentioned etch advantages by utilizing precursors and process parameters that facilitate protection of the exposed layers of material during the individual etch operations and can also accommodate the material properties in the individual layers. For example, if the hard mask material includes a harder, i.e., more etch-resistant metal, such as osmium, ruthenium, tungsten, iridium, or hafnium, and the underlayer includes a less etch-resistant metal, such as chromium, titanium, or niobium, characterized by a lower hardness, a more reactive bombardment etch can be performed that penetrates the individual layers while maintaining the hard mask. Furthermore, many parameters can be adjusted when different layers include different material properties. Unlike the case of ion-beam etching, which may be essentially limited to physical removal, the present technique can utilize both physical and chemical etching, and both physical and chemical etching properties can be adjusted in situ and between material layers. Thus, material differences can be accommodated to ensure that the profile is maintained and that the material is sufficiently etched during the process.
[0041] As one non-limiting example, if the capping layer 312 and metal layer 325 are included, each of them may include ruthenium or a ruthenium-containing material, which may be a physically harder material that may be more difficult to etch compared to a less etch-resistant material metal. However, the anti-reflective coating layer and one or more of the absorber layers may be or include a less etch-resistant metal, such as tantalum, or may include a more etch-resistant metal, such as iridium. Thus, the plasma characteristics used to etch the individual layers may be modified to accommodate the film. Also as a non-limiting example, if the anti-reflective coating layer includes tantalum, such as tantalum oxynitride, tantalum boron oxide, or some other material, while the absorber includes iridium, iridium alloy, or doped iridium, such as silicon-doped iridium, challenges may arise during etching if the plasma parameters are kept constant. For example, if a higher energy etch is performed across the stack, the more etch-resistant iridium-containing layer will result in a slower etch, while the tantalum-containing layer can be more easily etched. At least a portion of the antireflective coating layer can be exposed during the etching of the absorber so that, if the plasma properties are maintained, potentially critical dimension gain occurs in the antireflective coating layer resulting in sloped sidewalls on the absorber or resulting in incorrect dimensions due to overetching, etc. By adjusting one or more aspects of the physical and / or chemical etching, the technique can accommodate both conditions where the underlying film is harder than the overlying film and the underlying film is softer than the overlying film, or where the underlying film is more etch resistant than the overlying film and the underlying film is less etch resistant than the overlying film.
[0042] For example, a processing chamber such as the processing chamber 100 previously described can provide switchable bias frequencies while etching between two or more bias frequencies as well as utilizing multi-frequency operation on either electrode. For example, one or more etching operations can be performed at a first bias frequency or a first combined frequency, while one or more additional etching operations can be performed at a second bias frequency or a second combined frequency. The combined frequency can also include a ratio between two frequencies, such as 25% of the first frequency and 75% of the second frequency, in one non-limiting example, although it should be understood that these two frequencies can be any two percentages. The first bias frequency can include a higher frequency, such as greater than or about 10 MHz, and can also be greater than or about 13.56 MHz, greater than or about 27 MHz, greater than or about 40 MHz, or even higher. The second bias frequency can include a lower frequency, such as less than or about 10 MHz, and may be less than or about 7 MHz, less than or about 5 MHz, less than or about 2 MHz, less than or about 1 MHz, less than or about 500 kHz, less than or about 400 kHz, or even lower. The combination frequency can also include any second frequency. The first layer can be etched at either a higher or lower frequency while the underlying layer can be etched at another frequency, or vice versa. Thus, the first frequency can be either higher or lower than the second frequency while etching the subsequent layer where the bias frequency is adjusted. Similarly, when a subsequent layer, such as a third layer, is etched, additional adjustments can be made and a third bias frequency can be used.The third bias frequency may be the maintained second bias frequency, the third bias frequency may be a return to the first bias frequency, or in some embodiments a third bias frequency different from the first bias frequency or the second bias frequency may be applied.
[0043] By changing the bias frequency or the combination ratio in situ, the concentration of ions and neutrons can be modified, which can affect the amount of physical etching that is performed. At a bias frequency of, for example, 13.56 MHz, the plasma can be characterized by a smaller ion energy, which can increase the chemical etching or control the sputtering component of the material layer. At a lower bias frequency, for example, 2 MHz, the plasma can be characterized by a larger ion energy, which can enhance the bombardment and facilitate the etching of more etch-resistant films. A lower frequency can increase the etch rate based on the larger ion energy, but the enhanced bombardment can further thin the overlying film. For example, if the hard mask layer includes an oxide, oxynitride, or nitride, or a less etch-resistant material such as titanium, chromium, or niobium, while the absorber layer includes ruthenium or iridium, a lower frequency can increase the removal of the hard mask material to facilitate the etching of the underlying more etch-resistant film. Thus, in this and other similar material mismatches, additional processing aspects can be adjusted while maintaining process operation.
[0044] The precursors may include a first fluorine-containing precursor during each process, and may also include a second halogen-containing precursor in some embodiments, and may also include a third precursor that may or may not be a halogen-containing precursor. In some embodiments, chlorine-containing precursors, bromine-containing precursors, iodine-containing precursors, or other halogen-containing precursors may be used as the second halogen-containing precursor as well as another fluorine-containing precursor or combination of precursors. Exemplary halogen-containing precursors may include one or more of fluorine or chlorine in some embodiments, as well as any other halogen. Some exemplary precursors that may be utilized as fluorine-containing precursors may include halides, including any organic fluorine, such as hydrogen fluoride, nitrogen trifluoride, or carbon tetrafluoride or other fluorinated carbons, as well as hydrofluorocarbons, such as fluoromethane, difluoromethane, or trifluoromethane. Precursors may include diatomic fluorine, bromine trifluoride, chlorine trifluoride, sulfur hexafluoride, xenon difluoride, boron trichloride, tungsten pentachloride, tungsten hexachloride, diatomic chlorine, or any other chlorine-containing or fluorine-containing precursor. The precursors can also be flowed together in various combinations and flow ratios. The precursors can also be flowed with any number of additional precursors or carrier gases, including diatomic hydrogen or hydrogen-containing precursors, nitrogen, argon, helium, or any number of additional materials, although in some embodiments the precursors may be limited to control side reactions or other aspects that may affect selectivity.
[0045] In some embodiments, multiple fluorine-containing precursors may be used and may include one or more polymerized precursors as well as one or more non-polymerized precursors, which may or may not include halogens, for example. For example, if the precursor contains carbon or contains carbon and hydrogen, by-products may form along the sidewalls of the features being fabricated. Exemplary precursors may include halogens such as carbon tetrafluoride, or if they cannot include carbon tetrafluoride, may include halogens such as carbonyl sulfide or any other carbon-containing precursor or carbon and hydrogen-containing precursor. This allows the etched material to be more easily protected, while the more etch-resistant material is etched with a higher ion energy. As a non-limiting example, if the anti-reflective coating layer contains a material that can be etched more easily than the absorber, simply lowering the bias frequency between layer etches may open up the coating layer, and even the hard mask, further, which may affect the dimensional stability of the etch process. However, if a higher amount of polymerized precursor is utilized, the exposed sidewalls of the overlying layer may be protected, since the more etch-resistant underlying layer can be removed using a more physical etch.
[0046] To promote polymerization, in some embodiments, the adjusted parameter may be the flow ratio between the first fluorine-containing precursor, which may contain carbon or carbon and hydrogen, and the second halogen-containing precursor, which may be free of both carbon and hydrogen. The flow ratio may be greater than 1:1 or about 1:1, greater than 2:1 or about 2:1, greater than 3:1 or about 3:1, greater than 4:1 or about 4:1, greater than 5:1 or about 5:1, greater than 6:1 or about 6:1, greater than 7:1 or about 7:1, greater than 8:1 or about 8:1, greater than 9:1 or about 9:1, greater than 10:1 or about 10:1 or more. Additionally, a third precursor may be incorporated, which may have an even higher polymerization potential. For example, the first fluorine-containing precursor can include carbon, and the third precursor can include carbon and / or hydrogen. The third precursor can be included in any of the ratios mentioned above with respect to either the first fluorine-containing precursor or the second halogen-containing precursor, and any precursor can be in a higher ratio. Similarly, if a successive layer can be etched more easily with respect to the overlying layer, the ratio of the second halogen-containing precursor can be increased to any of the ratios mentioned above with respect to the first fluorine-containing precursor, and / or the delivery of the third precursor can be stopped, which can limit polymerization. This can increase the etch rate through the layers, which can further enhance the selectivity of removal between layers. The flow rate ratio can be modified between any two layers, which can affect the etch rate and etch selectivity in embodiments of the present technology.
[0047] Other process conditions can affect and facilitate etching according to embodiments of the present technology. For example, the temperature at which the process is performed can affect the extent to which reactions can occur. Higher temperatures can increase the etching of some materials, such as materials that are not very etch-resistant, and the temperature can be controlled to limit or increase the etching of these materials. As one non-limiting example, in some embodiments, the hard mask material can be or include materials that are more sensitive to temperature, such as those containing chromium or silicon, which can be more easily removed at higher temperatures. Thus, the etch process can be performed at a temperature of, for example, less than about 100° C. throughout the etch process, thereby protecting the hard mask from over-etching. Additionally, the temperature can be increased if the mask material is not likely to be removed as much and the underlying film can be more easily etched at a higher temperature. Thus, in embodiments, the process temperature can be maintained between about 20° C. or less and about 150° C. or more during processing. The temperature may be adjusted between treatments in some embodiments, and the temperature may also be maintained within these ranges, within narrower ranges encompassed by these ranges, or at any temperature between any of these ranges.
[0048] The pressure in the chamber can also affect the processes being performed. Maintaining a lower pressure during one or more etching processes, such as while etching a film that features a more etch-resistant material, can facilitate enhanced interactions at the substrate surface. Lower pressures can lengthen the mean free path between atoms, thereby increasing the energy and enhancing interactions at the film surface. Similarly, utilizing a higher pressure during some processes, such as when a film that can be more easily sputtered can be exposed, can slow the etch rate while enhancing the chemical interaction between the etchant and the material being removed. Thus, in some embodiments, the pressure can be maintained at any pressure between about 0.5 mTorr and about 50 mTorr for any process during the method. The pressure can also be adjusted between processes in some embodiments, and the pressure can be maintained at any pressure within these ranges, narrower ranges encompassed by these ranges, or between any of these ranges.
[0049] The power of the source and / or bias can be controlled, which can provide enhanced control over the overall depth of the etching process and can affect the layers exposed during the etching process. Thus, during any process, the plasma power on either or both the source and bias can be maintained at less than about 500 W. By maintaining a lower plasma power, sputtering can be controlled and interactions can be limited to surface chemical reactions, which can better limit the extent of etching through the material. Thus, in some embodiments, the plasma power on either or both the source and bias can be maintained at or below 450 W, 400 W, 350 W, 300 W, 250 W, 200 W, 150 W, 100 W, or less.
[0050] In some embodiments, the source and / or bias power can be pulsed at any of the frequencies already mentioned, thereby allowing for a certain amount of "off" time for certain aspects of the process. This can allow for chemical interactions to be maintained or can allow time for polymer by-products to deposit, thereby protecting the material to be maintained. Thus, the bias power can be pulsed during any process during the method according to an embodiment of the present technology. When pulsing, power can be applied at a level higher than any of the power values mentioned above, but can maintain effective power at or below 500 W throughout the pulsing. By adjusting the plasma and / or process parameters during the etching process, the present technology can be used to sequentially etch through multiple layers of material without long dwell times or the need to transfer the substrate between chambers. Additionally, processing can enhance profile control during etching such that an absorber featuring any of the materials already mentioned can be characterized, within measurement tolerances, by a sidewall angle of greater than or about 80°, greater than or about 82°, greater than or about 84°, greater than or about 85°, greater than or about 85°, greater than or about 86°, greater than or about 87°, greater than or about 88°, greater than or about 88°, greater than or about 88.5°, greater than or about 89°, greater than or about 89.5°, or substantially or essentially a 90° sidewall angle, thereby improving processing as a photomask absorber.
[0051] In the above description, for purposes of explanation, numerous details are set forth in order to provide an understanding of various embodiments of the present technology. However, it will be apparent to one skilled in the art that particular embodiments may be practiced without some of these details or with additional details.
[0052] Although several embodiments have been disclosed, those skilled in the art will recognize that various modifications, alternative structures, and equivalents may be used without departing from the spirit of the embodiments. Additionally, many well-known processes and elements have not been described to avoid unnecessarily obscuring the technology. Thus, the above description should not be taken as limiting the scope of the technology. Additionally, although a method or process is described in some cases as a sequence or in steps, it should be understood that the operations may be performed simultaneously or in a different order than listed.
[0053] Where a range of values is provided, it is understood that each intervening value between the upper and lower limits of that range, to the smallest fraction of the unit of the lower limit, is also expressly disclosed, unless the context clearly indicates otherwise. Any narrower range between any stated or unstated intervening value in a stated range and any other stated or intervening value in that stated range is included. The upper and lower limits of these smaller ranges may be independently included or excluded within the range, and each range in which either limit is included, neither limit is included, or both limits are included, is also encompassed within the technology, subject to any specifically excluded limit in the stated range. If a stated range includes one or both of the limits, then ranges excluding either or both of those included limits are also included.
[0054] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to a "precursor" includes a plurality of such precursors, reference to a "layer" includes reference to one or more layers and equivalents thereof known to those skilled in the art, and so forth.
[0055] Additionally, the words "comprises," "comprising," "containing," "containing," "including," and "comprising," when used in this specification and the following claims, are intended to specify the presence of a stated feature, integer, component or operation, but they do not preclude the presence or addition of one or more other features, integers, components, operations, acts or groups.
Claims
1. 1. An etching method comprising the steps of: forming a plasma of a fluorine-containing precursor to generate plasma effluents, wherein a first bias frequency is applied while forming the plasma; contacting a substrate contained in a processing region of a semiconductor processing chamber with the plasma effluents, the substrate comprising a photomask; etching a first layer of the photomask, where etching the first layer of the photomask exposes a second layer of the photomask; adjusting the first bias frequency to a second bias frequency while maintaining the plasma of the fluorine-containing precursor; Etching the second layer of the photomask. An etching method comprising:
2. The photomask is A mirror layer; an absorber covering the mirror layer; a capping layer disposed between the absorber and the mirror layer, the capping layer comprising a metal; The etching method of claim 1 , comprising:
3. The photomask is a hard mask covering the absorber; an anti-reflective coating layer disposed between the hard mask and the absorber; Further equipped with The etching method of claim 2 , wherein at least one of the hard mask and the anti-reflective coating layer comprises an oxide or nitride material.
4. The photomask is a layer of material disposed between the hard mask and the antireflective coating layer; 4. The etching method of claim 3, further comprising: wherein the layer of material comprises a metal.
5. The fluorine-containing precursor is a first fluorine-containing precursor; a second halogen-containing precursor; 2. The etching method of claim 1, wherein the first fluorine-containing precursor comprises carbon and the second halogen-containing precursor is carbon-free.
6. 6. The etching method of claim 5, wherein a flow ratio of the first fluorine-containing precursor to the second halogen-containing precursor is greater than or about 2:
1.
7. adjusting a flow ratio of the first fluorine-containing precursor and the second halogen-containing precursor subsequent to etching the first layer of the photomask. The etching method of claim 5 further comprising:
8. The fluorine-containing precursor is A third precursor containing carbon The etching method of claim 5 further comprising:
9. 9. The etching method of claim 8, wherein the third precursor is utilized only during either etching the first layer of the photomask or etching the second layer of the photomask.
10. 10. The etching method of claim 1, wherein a chamber pressure in the semiconductor processing chamber is maintained at less than or about 50 mTorr.
11. The second layer of the photomask is etched to expose a third layer of the photomask, and the method further comprises: adjusting the second bias frequency to a third bias frequency while maintaining the plasma of the fluorine-containing precursor. The etching method of claim 1 further comprising:
12. 1. An etching method comprising the steps of: forming a plasma of a first fluorine-containing precursor and a second halogen-containing precursor to generate plasma effluents, wherein a first bias frequency is applied while forming the plasma; contacting a substrate contained in a processing region of a semiconductor processing chamber with the plasma effluents, the substrate comprising a photomask, the photomask comprising at least three layers between a hard mask and a mirror layer of the photomask; etching a first layer of the photomask, where etching the first layer of the photomask exposes a second layer of the photomask; To adjust, adjusting the first bias frequency to a second bias frequency; adjusting the pressure in the semiconductor processing chamber; Adjusting the effective power of the source electrodes and / or bias electrodes; or adjusting a flow ratio between the first fluorine-containing precursor and the second halogen-containing precursor; adjusting, Etching the second layer of the photomask. An etching method comprising:
13. Detecting exposure of the second layer of the photomask while etching the first layer of the photomask. The etching method of claim 12 further comprising:
14. The photomask is A mirror layer; an absorber covering the mirror layer; a capping layer disposed between the absorber and the mirror layer, the capping layer comprising a metal; The etching method of claim 12 comprising:
15. The etching method of claim 14 , wherein the absorber comprises at least two layers of material.
16. The second layer of the photomask is etched to expose a third layer of the photomask, and the method further comprises: Etching the third layer of the photomask, wherein a bias frequency is maintained between either the etching of the first layer of the photomask and the second layer of the photomask, or the etching of the second layer of the photomask, and the etching of the third layer of the photomask. The etching method of claim 12 further comprising:
17. 13. The etching method of claim 12, wherein at least one of the three layers comprises a first metal and the hard mask comprises a second metal characterized by a hardness less than a hardness of the first metal.
18. 13. The etching method of claim 12, wherein the plasma is further formed with a third precursor, the first fluorine-containing precursor comprising carbon, the second halogen-containing precursor being carbon-free, and the third precursor comprising carbon.
19. 1. An etching method comprising the steps of: forming a plasma of at least one fluorine-containing precursor to generate plasma effluents, wherein a first bias frequency is applied while forming the plasma; contacting a substrate contained in a processing region of a semiconductor processing chamber with the plasma effluents, the substrate comprising a photomask, the photomask comprising at least two layers between a hard mask and a mirror layer of the photomask; etching a first layer of the photomask, where etching the first layer of the photomask exposes a second layer of the photomask; adjusting the first bias frequency to a second bias frequency, the first bias frequency being greater than or about 10 MHz and the second bias frequency being less than or about 10 MHz; Etching the second layer of the photomask. An etching method comprising:
20. The photomask is A mirror layer; an absorber covering the mirror layer; a capping layer disposed between the absorber and the mirror layer, the capping layer comprising a metal; 20. The etching method of claim 19, comprising:
Citation Information
Patent Citations
Method of etching extreme ultraviolet light (EUV) photomasks
JP2008072127A
Method for etching EUV material layers utilized to form a photomask
US20140154615A1
Method for Extreme Ultraviolet Lithography Mask Treatment
US20190324364A1
Reflective mask blank for EUV lithography
WO2012105508A1