Etching method and plasma processing apparatus
By employing a fluorine-containing and boron-containing gas mixture with a cooled substrate supporter, the method addresses shape defects in plasma etching by suppressing by-product formation and promoting decomposition, resulting in improved etching precision and reduced defects in silicon-containing films.
Patent Information
- Application Number
- JP2020188671
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-12
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-11-12
AI Technical Summary
Existing plasma etching methods for silicon-containing films result in shape defects, such as twisting or bending, of openings due to the accumulation of by-products like ammonium fluorosilicate on the sidewalls or bottom of the openings, which hinder linear etching progression.
The method involves using a processing gas containing fluorine-containing, boron-containing, and optionally phosphorus-containing gases, with the substrate supporter temperature set below 0°C, to suppress by-product generation and promote decomposition, thereby maintaining the etching's linear progression.
This approach effectively reduces shape defects in openings by preventing by-product accumulation and enhancing etching efficiency, ensuring precise and defect-free etching of silicon-containing films.
Smart Images

Figure 00000013_0000 
Figure 00000013_0001 
Figure 00000014_0000
Abstract
Description
[Technical field]
[0001] An exemplary embodiment of the present disclosure relates to an etching method. [Background technology]
[0002] In the manufacture of electronic devices, plasma etching of a silicon-containing film on a substrate is performed. In the plasma etching, the silicon-containing film is etched using plasma generated from a processing gas. JP 2016-39309 A discloses a processing gas containing hydrogen gas, a fluorohydrocarbon gas, a fluorine-containing gas, a hydrocarbon gas, a boron trichloride gas, and a nitrogen gas as a processing gas used in the plasma etching of a silicon-containing film. JP 2014-17406 A discloses a processing gas containing boron as a processing gas used in the plasma etching of a silicon-containing film. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-39309 A [Patent Document 2] JP 2014-17406 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides a technique for suppressing defects in the shape of an opening formed in a silicon-containing film during plasma etching of the silicon-containing film. [Means for solving the problem]
[0005] In one exemplary embodiment, an etching method is provided, which includes the steps of: (a) providing a substrate having a silicon-containing film, including a silicon nitride film, in a chamber; and (b) generating a plasma from a process gas in the chamber to etch the silicon-containing film. The process gas includes a fluorine-containing gas and a boron-containing gas. In the step (b), a temperature of a substrate support that supports the substrate is set to a temperature less than 0° C. Effect of the Invention
[0006] According to one exemplary embodiment, it is possible to suppress shape defects of an opening formed in a silicon-containing film during plasma etching of the silicon-containing film. [Brief description of the drawings]
[0007] [Figure 1] 1 is a flow diagram of an etching method according to an exemplary embodiment. [Diagram 2] 2 is a partially enlarged cross-sectional view of an example of a substrate to which the etching method shown in FIG. 1 can be applied. [Diagram 3] 1 is a schematic diagram of a plasma processing apparatus according to an exemplary embodiment; [Figure 4] 2 is a partially enlarged cross-sectional view of an example of a substrate to which the etching method shown in FIG. 1 is applied. [Diagram 5] FIG. 13 is a partially enlarged cross-sectional view of an example substrate for evaluating the degree of shape defects of an opening. [Figure 6] 1 is a graph showing the results of the first and second experiments. [Figure 7] 13 is a graph showing the results of the third and fourth experiments. [Figure 8] 13 is a graph showing the results of the fifth to eighth experiments. [Figure 9] 13 is a graph showing the results of the fifth to sixth and ninth to thirteenth experiments. [Figure 10] 13 is a graph showing the results of the fourteenth experiment. [Figure 11] 13 is a graph showing the results of the 15th experiment. [Figure 12] FIG. 12(a) to (c) show the results of the 16th to 18th experiments, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Various exemplary embodiments are described below.
[0009] In one exemplary embodiment, an etching method is provided, which includes the steps of: (a) providing a substrate having a silicon-containing film, including a silicon nitride film, in a chamber; and (b) generating a plasma from a process gas in the chamber to etch the silicon-containing film. The process gas includes a fluorine-containing gas and a boron-containing gas. In the step (b), a temperature of a substrate support that supports the substrate is set to a temperature less than 0° C.
[0010] According to the above etching method, in the plasma etching of the silicon-containing film, the shape defect of the opening formed in the silicon-containing film can be suppressed. The mechanism by which the shape defect of the opening is suppressed is considered to be as follows, but is not limited thereto. When the temperature of the substrate support is low (for example, less than 0°C), by-products (for example, ammonium silicofluoride ((NH4)2SiF6)) generated by etching are difficult to volatilize. As a result, the by-products are deposited on the sidewall or bottom of the opening during etching, and the etching does not proceed linearly in the depth direction. This causes the sidewall of the opening to bend, which may cause the shape defect of the opening. However, when the process gas contains a boron-containing gas, the generation of by-products is suppressed and the decomposition of the by-products is promoted. Therefore, the shape defect of the opening caused by the by-products is suppressed.
[0011] In one exemplary embodiment, the process gas may further include a phosphorus-containing gas. When the process gas includes a phosphorus-containing gas, the generation of by-products generated by etching is promoted. Even in such a case, when the process gas includes a boron-containing gas, the generation of by-products is suppressed and the decomposition of the by-products is promoted.
[0012] The fluorine-containing gas may include at least one of a fluorocarbon gas, a hydrofluorocarbon gas, a hydrogen fluoride gas, a nitrogen trifluoride gas, and a sulfur hexafluoride gas. In this case, defects in the shape of the opening formed in the silicon-containing film can be further suppressed.
[0013] The ratio of the flow rate of the boron-containing gas to the flow rate of the processing gas may be 6% or less, in which case the flow rate of the boron-containing gas can be reduced.
[0014] The silicon-containing film may further include a silicon oxide film.
[0015] In another exemplary embodiment, an etching method is provided that includes: (a) providing a substrate having a silicon-containing film in a chamber, the silicon-containing film comprising a silicon nitride film; and (b) generating a plasma in the chamber from a process gas comprising a phosphorus-containing gas, a fluorine-containing gas, and a boron-containing gas to etch the silicon-containing film.
[0016] According to the above etching method, in the plasma etching of the silicon-containing film, the shape defect of the opening formed in the silicon-containing film can be suppressed. The mechanism by which the shape defect of the opening is suppressed is considered to be as follows, but is not limited to this. When the processing gas contains a phosphorus-containing gas, the generation of by-products (e.g., ammonium silicofluoride ((NH4)2SiF6)) generated by etching is promoted. As a result, the by-products are deposited on the sidewall or bottom of the opening during etching, and the etching does not proceed linearly in the depth direction. This causes the sidewall of the opening to bend, which may cause the shape defect of the opening. However, when the processing gas contains a boron-containing gas, the generation of by-products is suppressed and the decomposition of the by-products is promoted. Therefore, the shape defect of the opening caused by the by-products is suppressed.
[0017] In the step (b), the temperature of a substrate support that supports the substrate may be set to a temperature below 0° C. When the temperature of the substrate support is low (for example, below 0° C.), by-products generated by etching are less likely to volatilize. Even in such a case, when the process gas contains a boron-containing gas, the generation of by-products is suppressed and decomposition of the by-products is promoted.
[0018] The ratio of the flow rate of the boron-containing gas to the flow rate of the processing gas may be 6% or less, in which case the flow rate of the boron-containing gas can be reduced.
[0019] The silicon-containing film may further include a silicon oxide film.
[0020] Various exemplary embodiments will now be described in detail with reference to the drawings, in which the same or corresponding parts are designated by the same reference numerals.
[0021] 1 is a flow diagram of an etching method according to one exemplary embodiment. The etching method shown in FIG. 1 (hereinafter referred to as "Method MT") is applied to a substrate having a silicon-containing film. In Method MT, the silicon-containing film is etched.
[0022] Fig. 2 is a partially enlarged cross-sectional view of an example of a substrate to which the etching method shown in Fig. 1 can be applied. The substrate W shown in Fig. 2 can be used in the manufacture of devices such as DRAM and 3D-NAND. The substrate W has a silicon-containing film SF. The substrate W may further have a base region UR. The silicon-containing film SF can be provided on the base region UR.
[0023] The silicon-containing film SF may be a silicon-containing dielectric film. The silicon-containing dielectric film may include a silicon oxide film or a silicon nitride film. The silicon-containing dielectric film may be a film having other film types as long as it is a dielectric film containing silicon. The silicon-containing film SF may also include a silicon film (e.g., a polycrystalline silicon film). The silicon-containing film SF may also include at least one of a silicon nitride film, a polycrystalline silicon film, a carbon-containing silicon film, and a low-k film. The carbon-containing silicon film may include a SiC film and / or a SiOC film. The low-k film contains silicon and may be used as an interlayer insulating film. The silicon-containing film SF may also include two or more silicon-containing films having different film types. The two or more silicon-containing films may include a silicon oxide film and a silicon nitride film. The silicon-containing film SF may be, for example, a multilayer film including one or more silicon oxide films and one or more silicon nitride films that are alternately stacked. The silicon-containing film SF may also be a multilayer film including a plurality of silicon oxide films and a plurality of silicon nitride films that are alternately stacked. Alternatively, the two or more silicon-containing films may include a silicon oxide film and a silicon film. The silicon-containing film SF may be, for example, a multilayer film including one or more silicon oxide films and one or more silicon films that are alternately stacked. The silicon-containing film SF may be a multilayer film including a plurality of silicon oxide films and a plurality of polycrystalline silicon films that are alternately stacked. Alternatively, the two or more silicon-containing films may include a silicon oxide film, a silicon nitride film, and a silicon film.
[0024] The substrate W may further include a mask MK. The mask MK is provided on the silicon-containing film SF. The mask MK is formed of a material having an etching rate lower than that of the silicon-containing film SF in step ST2. The mask MK may be formed of an organic material. That is, the mask MK may contain carbon. The mask MK may be formed of, for example, an amorphous carbon film, a photoresist film, or a spin-on carbon film (SOC film). Alternatively, the mask MK may be formed of a silicon-containing film such as a silicon-containing anti-reflective film. Alternatively, the mask MK may be a metal-containing mask formed of a metal-containing material such as titanium nitride, tungsten, or tungsten carbide. The mask MK may have a thickness of 3 μm or more.
[0025] The mask MK is patterned. That is, the mask MK has a pattern to be transferred to the silicon-containing film SF in step ST2. When the pattern of the mask MK is transferred to the silicon-containing film SF, an opening OP (see FIG. 4) such as a hole or a trench is formed in the silicon-containing film SF. The opening OP may be a recess. The opening OP may penetrate the silicon-containing film SF in the thickness direction. When the silicon-containing film SF is a multilayer film including a plurality of silicon oxide films and a plurality of silicon nitride films alternately stacked, the opening OP may penetrate the multilayer film in the thickness direction. The aspect ratio of the opening OP formed in the silicon-containing film SF in step ST2 may be 20 or more, 30 or more, 40 or more, or 50 or more. The mask MK may have a line and space pattern.
[0026] In the method MT, a plasma processing apparatus is used for etching the silicon-containing film SF. FIG. 3 is a schematic diagram of a plasma processing apparatus according to an exemplary embodiment. The plasma processing apparatus 1 shown in FIG. 3 includes a chamber 10. The chamber 10 provides an internal space 10s therein. The chamber 10 includes a chamber body 12. The chamber body 12 has a substantially cylindrical shape. The chamber body 12 is formed of, for example, aluminum. A corrosion-resistant film is provided on the inner wall surface of the chamber body 12. The corrosion-resistant film may be formed of a ceramic such as aluminum oxide or yttrium oxide.
[0027] A passage 12p is formed in a sidewall of the chamber body 12. The substrate W is transferred between the internal space 10s and the outside of the chamber 10 through the passage 12p. The passage 12p is opened and closed by a gate valve 12g. The gate valve 12g is provided along the sidewall of the chamber body 12.
[0028] A support 13 is provided on the bottom of the chamber body 12. The support 13 is made of an insulating material. The support 13 has a generally cylindrical shape. The support 13 extends upward from the bottom of the chamber body 12 in the internal space 10s. The support 13 supports a substrate support 14. The substrate support 14 is configured to support a substrate W in the internal space 10s.
[0029] The substrate support 14 has a lower electrode 18 and an electrostatic chuck 20. The substrate support 14 may further have an electrode plate 16. The electrode plate 16 is made of a conductor such as aluminum and has a substantially disk-like shape. The lower electrode 18 is provided on the electrode plate 16. The lower electrode 18 is made of a conductor such as aluminum and has a substantially disk-like shape. The lower electrode 18 is electrically connected to the electrode plate 16.
[0030] The electrostatic chuck 20 is provided on the lower electrode 18. The substrate W is placed on the upper surface of the electrostatic chuck 20. The electrostatic chuck 20 has a body and an electrode. The body of the electrostatic chuck 20 has a substantially disk shape and is formed from a dielectric material. The electrode of the electrostatic chuck 20 is a film-like electrode and is provided in the body of the electrostatic chuck 20. The electrode of the electrostatic chuck 20 is connected to a DC power supply 20p via a switch 20s. When a voltage from the DC power supply 20p is applied to the electrode of the electrostatic chuck 20, an electrostatic attractive force is generated between the electrostatic chuck 20 and the substrate W. The substrate W is attracted to the electrostatic chuck 20 by the electrostatic attractive force and is held by the electrostatic chuck 20.
[0031] An edge ring 25 is disposed on the substrate support 14. The edge ring 25 is a ring-shaped member. The edge ring 25 may be made of silicon, silicon carbide, quartz, or the like. The substrate W is disposed on the electrostatic chuck 20 and within a region surrounded by the edge ring 25.
[0032] A flow path 18f is provided inside the lower electrode 18. A heat exchange medium (e.g., a coolant) is supplied to the flow path 18f from a chiller unit provided outside the chamber 10 via a pipe 22a. The heat exchange medium supplied to the flow path 18f is returned to the chiller unit via a pipe 22b. In the plasma processing apparatus 1, the temperature of the substrate W placed on the electrostatic chuck 20 is adjusted by heat exchange between the heat exchange medium and the lower electrode 18.
[0033] The plasma processing apparatus 1 is provided with a gas supply line 24. The gas supply line 24 supplies a heat transfer gas (for example, He gas) from a heat transfer gas supply mechanism to the gap between the upper surface of the electrostatic chuck 20 and the back surface of the substrate W.
[0034] The plasma processing apparatus 1 further includes an upper electrode 30. The upper electrode 30 is provided above the substrate support 14. The upper electrode 30 is supported on the upper part of the chamber body 12 via a member 32. The member 32 is made of an insulating material. The upper electrode 30 and the member 32 close the upper opening of the chamber body 12.
[0035] The upper electrode 30 may include a top plate 34 and a support 36. The bottom surface of the top plate 34 is the bottom surface on the side of the internal space 10s and defines the internal space 10s. The top plate 34 may be formed of a low-resistance conductor or semiconductor that generates little Joule heat. The top plate 34 has a plurality of gas discharge holes 34a penetrating the top plate 34 in its plate thickness direction.
[0036] The support 36 detachably supports the top plate 34. The support 36 is made of a conductive material such as aluminum. A gas diffusion chamber 36a is provided inside the support 36. The support 36 has a plurality of gas holes 36b extending downward from the gas diffusion chamber 36a. The plurality of gas holes 36b are connected to the plurality of gas discharge holes 34a, respectively. A gas inlet 36c is formed in the support 36. The gas inlet 36c is connected to the gas diffusion chamber 36a. A gas supply pipe 38 is connected to the gas inlet 36c.
[0037] A gas source group 40 is connected to the gas supply pipe 38 via a flow rate controller group 41 and a valve group 42. The flow rate controller group 41 and the valve group 42 configure a gas supply unit. The gas supply unit may further include a gas source group 40. The gas source group 40 includes a plurality of gas sources. The plurality of gas sources include sources of processing gases used in the method MT. The flow rate controller group 41 includes a plurality of flow rate controllers. Each of the plurality of flow rate controllers in the flow rate controller group 41 is a mass flow controller or a pressure-controlled flow rate controller. The valve group 42 includes a plurality of opening and closing valves. Each of the plurality of gas sources in the gas source group 40 is connected to the gas supply pipe 38 via a corresponding flow rate controller in the flow rate controller group 41 and a corresponding opening and closing valve in the valve group 42.
[0038] In the plasma processing apparatus 1, a shield 46 is detachably provided along the inner wall surface of the chamber body 12 and the outer periphery of the support part 13. The shield 46 prevents reaction by-products from adhering to the chamber body 12. The shield 46 is formed by forming a corrosion-resistant film on the surface of a base material made of, for example, aluminum. The corrosion-resistant film may be made of a ceramic such as yttrium oxide.
[0039] A baffle plate 48 is provided between the support 13 and the side wall of the chamber body 12. The baffle plate 48 is formed, for example, by forming a corrosion-resistant film (a film of yttrium oxide or the like) on the surface of a member made of aluminum. A plurality of through holes are formed in the baffle plate 48. An exhaust port 12e is provided below the baffle plate 48 and at the bottom of the chamber body 12. An exhaust device 50 is connected to the exhaust port 12e via an exhaust pipe 52. The exhaust device 50 includes a pressure regulating valve and a vacuum pump such as a turbo molecular pump.
[0040] The plasma processing apparatus 1 includes a high-frequency power supply 62 and a bias power supply 64. The high-frequency power supply 62 is a power supply that generates high-frequency power HF. The high-frequency power HF has a first frequency suitable for generating plasma. The first frequency is, for example, a frequency within a range of 27 MHz to 100 MHz. The high-frequency power supply 62 is connected to the lower electrode 18 via a matching device 66 and the electrode plate 16. The matching device 66 has a circuit for matching the impedance of the load side (lower electrode 18 side) of the high-frequency power supply 62 to the output impedance of the high-frequency power supply 62. The high-frequency power supply 62 may be connected to the upper electrode 30 via the matching device 66. The high-frequency power supply 62 constitutes an example of a plasma generating unit.
[0041] The bias power supply 64 is a power supply that generates an electric bias. The bias power supply 64 is electrically connected to the lower electrode 18. The electric bias has a second frequency. The second frequency is lower than the first frequency. The second frequency is, for example, a frequency in the range of 400 kHz to 13.56 MHz. When the electric bias is used together with the high frequency power HF, it is applied to the lower electrode 18 to attract ions to the substrate W. When the electric bias is applied to the lower electrode 18, the potential of the substrate W placed on the substrate support 14 fluctuates within a period defined by the second frequency.
[0042] In one embodiment, the electric bias may be a high frequency power LF having a second frequency. When the high frequency power LF is used together with the high frequency power HF, it is used as a high frequency bias power for attracting ions to the substrate W. A bias power supply 64 configured to generate the high frequency power LF is connected to the lower electrode 18 via a matching box 68 and the electrode plate 16. The matching box 68 has a circuit for matching the impedance of the load side (lower electrode 18 side) of the bias power supply 64 to the output impedance of the bias power supply 64.
[0043] It is also possible to generate plasma using high frequency power LF without using high frequency power HF, that is, using only a single high frequency power. In this case, the frequency of the high frequency power LF may be a frequency higher than 13.56 MHz, for example, 40 MHz. In this case, the plasma processing apparatus 1 does not need to include the high frequency power supply 62 and the matching box 66. In this case, the bias power supply 64 constitutes an example of a plasma generating unit.
[0044] When plasma processing is performed in the plasma processing apparatus 1, a gas is supplied from a gas supply unit to the internal space 10s. In addition, a high-frequency electric field is generated between the upper electrode 30 and the lower electrode 18 by supplying high-frequency power HF and / or an electric bias. The generated high-frequency electric field generates plasma from the gas in the internal space 10s.
[0045] The plasma processing apparatus 1 may further include a control unit 80. The control unit 80 may be a computer including a processor, a storage unit such as a memory, an input device, a display device, a signal input / output interface, and the like. The control unit 80 controls each part of the plasma processing apparatus 1. In the control unit 80, an operator can use the input device to input commands and the like to manage the plasma processing apparatus 1. In addition, the control unit 80 can visualize and display the operating status of the plasma processing apparatus 1 using the display device. Furthermore, the storage unit stores a control program and recipe data. The control program is executed by the processor to execute various processes in the plasma processing apparatus 1. The processor executes the control program and controls each part of the plasma processing apparatus 1 according to the recipe data.
[0046] Referring again to Fig. 1, the method MT will be described below taking as an example a case where the method MT is applied to a substrate W shown in Fig. 2 using a plasma processing apparatus 1. When the plasma processing apparatus 1 is used, the method MT can be executed in the plasma processing apparatus 1 by controlling each part of the plasma processing apparatus 1 by a control unit 80. In the following description, the control of each part of the plasma processing apparatus 1 by the control unit 80 for executing the method MT will also be described.
[0047] In the following description, in addition to Fig. 1, Fig. 4 will be referred to. Fig. 4 is a partially enlarged cross-sectional view of an example of a substrate to which the etching method shown in Fig. 1 is applied.
[0048] 1, the method MT starts with step ST1. In step ST1, a substrate W is provided in a chamber 10. The substrate W is placed on an electrostatic chuck 20 in the chamber 10 and held by the electrostatic chuck 20. The substrate W may have a diameter of 300 mm.
[0049] In the method MT, step ST2 is then performed. In step ST2, the silicon-containing film SF is etched by chemical species from a plasma generated from a processing gas in the chamber 10. The chemical species may be a halogen chemical species.
[0050] In one embodiment, the process gas used in step ST2 includes a fluorine-containing gas and a boron-containing gas. The process gas may further include a phosphorus-containing gas. The process gas may further include a halogen-containing gas. The halogen-containing gas may contain, for example, chlorine (Cl2) gas. The process gas may further include a carbon-containing gas. The process gas may further include an inert gas. The inert gas may contain, for example, a noble gas. The process gas may further include an oxygen-containing gas. The oxygen-containing gas may contain, for example, O2.
[0051] Fluorine-containing gases include hydrofluorocarbons (C s H t F u ) gas, fluorocarbon (C v F w ) gas, hydrogen fluoride (HF) gas, nitrogen trifluoride (NF3) gas, and sulfur hexafluoride (SF6) gas. Here, each of s, t, u, v, and w is a natural number. The hydrofluorocarbon is, for example, at least one of CH2F2, CHF3, CH3F, C2HF5, C3H2F4, etc. The hydrofluorocarbon may be a hydrofluorocarbon containing two or more carbon atoms. The fluorocarbon is, for example, at least one of CF4, C2F6, C3F6, C3F8, C4F6, C4F8, C5F8, etc. Fluorocarbons and hydrofluorocarbons contain carbon atoms and play a role in protecting the mask.
[0052] The phosphorus-containing gas may be a gas containing phosphorus atoms and halogen atoms, or may be a gas containing phosphorus atoms and fluorine atoms. Examples of gas containing phosphorus atoms and halogen atoms include phosphorus trifluoride (PF3), phosphorus pentafluoride (PF5), phosphorus trichloride (PCl3), phosphorus pentachloride (PCl5) and phosphoryl chloride (POCl3). Examples of gas containing phosphorus atoms and fluorine atoms include phosphorus trifluoride (PF3) and phosphorus pentafluoride (PF5). In a state where phosphorus chemical species generated from the phosphorus-containing gas are present on the surface of the substrate W, the adsorption of the etchant to the substrate W is promoted. That is, in a state where phosphorus chemical species generated from the phosphorus-containing gas are present on the surface of the substrate W, the supply of the etchant to the bottom of the opening (recess) is promoted, and the etching rate of the silicon-containing film SF is increased.
[0053] Carbon-containing gases are hydrocarbons (C x H y ) gas. Here, x and y are each a natural number. The hydrocarbon is, for example, at least one of CH4, C3H6, etc. When a carbon-containing gas containing two or more carbon atoms is used, the protective effect of the sidewall surfaces defining the openings in the mask MK and the silicon-containing film SF can be increased.
[0054] The boron-containing gas may include boron trichloride (BCl3) gas. The ratio of the flow rate of the boron-containing gas to the flow rate of the processing gas is greater than 0%, and may be 0.5% or more, or 1% or more. The ratio may be 6% or less, 3% or less, or 2% or less. By reducing the ratio of the flow rate of the boron-containing gas, the etching rate of the silicon oxide film can be increased and the amount of the mask MK etched by the boron-containing gas can be suppressed.
[0055] To perform step ST2, the control unit 80 controls the gas supply unit to supply a process gas into the chamber 10. The control unit 80 controls the exhaust device 50 to set the gas pressure in the chamber 10 to a designated pressure. The control unit 80 controls the chiller unit to set the temperature of the substrate support 14 to a designated temperature. The control unit 80 controls the plasma generation unit to generate plasma from the process gas.
[0056] In one embodiment, the temperature of the substrate support 14 in step ST2 may be set to a temperature less than 0° C., less than −20° C., less than −30° C., or not more than −40° C., or may be set to a temperature not less than −170° C. When the temperature of the substrate W is set to less than −30° C., the etching rate of the silicon-containing film SF in step ST2 increases.
[0057] According to the above-mentioned method MT, in the plasma etching of the silicon-containing film SF, it is possible to suppress the shape defect (twist or twist) of the opening OP formed in the silicon-containing film SF. The mechanism by which the shape defect of the opening OP is suppressed is considered to be as follows, but is not limited thereto.
[0058] When the temperature of the substrate support 14 is low (e.g., below 0° C.), by-products generated by etching (e.g., ammonium silicofluoride ((NH4)2SiF6) are less likely to volatilize. Alternatively, when the process gas contains a phosphorus-containing gas, the generation of by-products generated by etching (e.g., ammonium silicofluoride ((NH4)2SiF6) is promoted. As a result, the by-products accumulate on the sidewalls or bottom of the opening during etching, and the etching does not proceed linearly in the depth direction. This causes the sidewalls of the opening to bend, which can cause defects in the shape of the opening. However, when the process gas contains a boron-containing gas, the generation of by-products is suppressed and the decomposition of the by-products is promoted. Therefore, defects in the shape of the opening caused by the by-products are suppressed.
[0059] The mechanism by which the boron-containing gas suppresses the generation of by-products is believed to be as follows, but is not limited to this. The boron-containing gas has the function of scavenging fluorine atoms. As a result, the reaction for generating the by-product ammonium silicofluoride does not proceed, and the generation of the by-products is suppressed.
[0060] The mechanism by which the boron-containing gas promotes the decomposition of the by-products is believed to be as follows, but is not limited to this: The boron-containing gas lowers the activation energy of the decomposition reaction of the by-products, thereby promoting the decomposition of the by-products.
[0061] The mechanism by which the phosphorus-containing gas promotes the generation of by-products is believed to be, but is not limited to, the following: The reaction between SiN and the phosphorus-containing gas leaves excess NH3 on the sidewall or bottom of the opening, which then reacts with the fluorine-containing gas to generate ammonium silicofluoride.
[0062] Although various exemplary embodiments have been described above, the present invention is not limited to the above-described exemplary embodiments, and various additions, omissions, substitutions, and modifications may be made. In addition, elements in different embodiments can be combined to form other embodiments.
[0063] For example, the plasma processing apparatus used in the method MT may be a capacitively coupled plasma processing apparatus other than the plasma processing apparatus 1. Alternatively, the plasma processing apparatus used in the method MT may be a type of plasma processing apparatus other than the capacitively coupled type. Such a plasma processing apparatus may be an inductively coupled plasma processing apparatus, an ECR (electron cyclotron resonance) plasma processing apparatus, or a plasma processing apparatus that generates plasma using surface waves such as microwaves.
[0064] In addition to the bias power supply 64 that supplies high frequency power LF to the lower electrode 18, the plasma processing apparatus may also include another bias power supply configured to apply pulses of negative polarity DC voltage intermittently or periodically to the lower electrode 18.
[0065] Various experiments performed to evaluate Method MT will be described below, but the experiments described below are not intended to limit the present disclosure.
[0066] (Experiments 1 to 4)
[0067] Fig. 5 is a partially enlarged cross-sectional view of an example of a substrate for evaluating the degree of shape defects of an opening. An opening (recess) OP is formed in the silicon-containing film SF of the substrate W shown in Fig. 5. A center reference line CL of the opening OP passes through a midpoint MP of the width of the opening OP at the upper end of the opening OP. By measuring the deviation of the midpoint MP from the center reference line CL along the depth direction of the opening OP, the degree of shape defects (twist or twist) of the opening OP can be evaluated.
[0068] In the first to fourth experiments, a plurality of sample substrates having the same structure as the substrate W shown in FIG. 2 were prepared. Each of the plurality of sample substrates had a silicon-containing film and a mask provided on the silicon-containing film. The silicon-containing film was a multilayer film having a plurality of silicon oxide films and a plurality of silicon nitride films alternately stacked. The thickness of each of the silicon nitride films and each of the silicon oxide films was about several tens of nm. The mask was a mask formed from an amorphous carbon film. In each of the first to fourth experiments, a plasma processing apparatus having the same structure as the plasma processing apparatus 1 of FIG. 3 was used to generate plasma from a processing gas to etch the silicon-containing film of the sample substrate.
[0069] The process gas used in the first experiment was 38% H2 gas, 11% halogen-containing gas, and 20% C v F w The process gas used in the second experiment was 35% H2 gas, 10% halogen-containing gas, 18% C v F wThe processing gas contained 10% H2 gas, 29% O2 gas, and 8% PF3 gas. Each percentage indicates the ratio of the flow rate (unit: sccm) of each gas to the flow rate (unit: sccm) of the processing gas. In the first and second experiments, the temperature of the substrate support 14 was -40°C. The processing gas used in the third experiment was the same as the processing gas used in the first experiment. The processing gas used in the fourth experiment was the same as the processing gas used in the second experiment. In the third and fourth experiments, the temperature of the substrate support 14 was -70°C. Other conditions for each of the first to fourth experiments are shown below. <Other conditions for each of the first to fourth experiments> Gas pressure in chamber 10: 20 mTorr (2.7 Pa)
[0070] In each of the first to fourth experiments, after etching the silicon-containing film, the deviation of the midpoint MP of the width of the opening OP from the central reference line CL was obtained as shown in FIG. 5. The results are shown in FIG. 6 and FIG. 7. FIG. 6 is a graph showing the results of the first and second experiments. FIG. 7 is a graph showing the results of the third and fourth experiments. As shown in FIG. 6, the maximum deviation (22 nm) of the profile E2 showing the deviation of the midpoint MP in the second experiment was larger than the maximum deviation (14 nm) of the profile E1 showing the deviation of the midpoint MP in the first experiment. Therefore, it was found that the degree of shape defect of the opening OP may worsen when the processing gas contains a phosphorus-containing gas.
[0071] 6 and 7, the maximum deviation (58 nm) of the profile E3 showing the deviation of the midpoint MP in the third experiment was larger than the maximum deviation (14 nm) of the profile E1 showing the deviation of the midpoint MP in the first experiment. The maximum deviation (50 nm) of the profile E4 showing the deviation of the midpoint MP in the fourth experiment was larger than the maximum deviation (22 nm) of the profile E2 showing the deviation of the midpoint MP in the second experiment. Therefore, it was found that the degree of the shape defect of the opening OP worsens when the temperature of the substrate support 14 decreases.
[0072] (Experiments 5 to 13)
[0073] In the fifth to thirteenth experiments, the same sample substrate as the sample substrate prepared in the first to fourth experiments was prepared. In each of the fifth to thirteenth experiments, plasma was generated from the processing gas using the plasma processing apparatus 1 to etch the silicon-containing film of the sample substrate. The processing gas used in the fifth experiment contained 96% fluorine-containing gas, 1% C4F8, and 3% PF3 gas. The processing gas used in the sixth experiment contained 91% fluorine-containing gas, 1% C4F8, 2% PF3 gas, and 6% BCl3. The processing gas used in the seventh experiment contained 92% fluorine-containing gas, 1% C4F8, 2% PF3 gas, and 5% SiCl4. The processing gas used in the eighth experiment contained 88% fluorine-containing gas, 1% C4F8, 2% PF3 gas, and 9% Cl2. The process gas used in the ninth experiment contained 90% fluorine-containing gas, 2% C4F8, 2% PF3 gas, and 6% BCl3. The process gas used in the tenth experiment contained 92% fluorine-containing gas, 1% C4F8, 2% PF3 gas, and 5% BCl3. The process gas used in the eleventh experiment contained 94% fluorine-containing gas, 1% C4F8, 2% PF3 gas, and 3% BCl3. The process gas used in the twelfth experiment contained 95% fluorine-containing gas, 1% C4F8, 2% PF3 gas, and 2% BCl3. The process gas used in the thirteenth experiment contained 96% fluorine-containing gas, 1% C4F8, 2% PF3 gas, and 1% BCl3. Other conditions for each of the fifth to thirteenth experiments are shown below. <Other conditions for each of the 5th to 13th experiments> Gas pressure in chamber 10: 27 mTorr (3.6 Pa) Temperature of the substrate support 14: -70°C
[0074] In each of the fifth to thirteenth experiments, after etching the silicon-containing film, the deviation of the midpoint MP of the width of the opening OP from the center reference line CL was obtained as shown in FIG. 5. The results are shown in FIG. 8 and FIG. 9. FIG. 8 is a graph showing the results of the fifth to eighth experiments. As shown in FIG. 8, the maximum deviation (18 nm) of the profile E6 showing the deviation of the midpoint MP in the sixth experiment was smaller than the maximum deviation (38 nm) of the profile E5 showing the deviation of the midpoint MP in the fifth experiment. Therefore, it was found that the degree of the shape defect of the opening OP was improved by adding BCl3 to the processing gas. On the other hand, the maximum deviation (51 nm) of the profile E7 showing the deviation of the midpoint MP in the seventh experiment was larger than the maximum deviation (18 nm) of the profile E6 showing the deviation of the midpoint MP in the sixth experiment. The maximum deviation (26 nm) of the profile E8 showing the deviation of the midpoint MP in the eighth experiment was larger than the maximum deviation (18 nm) of the profile E6 showing the deviation of the midpoint MP in the sixth experiment. The deviation width (18 nm) of the profile E6 showing the deviation of the midpoint MP in the sixth experiment was smaller than the deviation width (about 40 nm) of the profile E8 showing the deviation of the midpoint MP in the eighth experiment. The deviation width corresponds to the range in which the deviation of each profile E6, E8 changes. Therefore, it was found that adding BCl3 to the process gas improves the degree of shape defects of the opening OP compared to adding SiCl4 or Cl2 to the process gas.
[0075] FIG. 9 is a graph showing the results of the fifth to sixth and ninth to thirteenth experiments. As shown in FIG. 9, the maximum deviation (8.2 nm) of the profile E9 showing the deviation of the midpoint MP in the ninth experiment was smaller than the maximum deviation (18 nm) of the profile E6 showing the deviation of the midpoint MP in the sixth experiment. C4F8 was added to adjust the shape defect of the opening OP. Even if BCl3 is added after adjusting the shape defect by adding C4F8, the degree of the shape defect of the opening OP can be improved. In addition, the maximum deviation (5.2 nm) of the profile E10 showing the deviation of the midpoint MP in the tenth experiment was smaller than the maximum deviation (18 nm) of the profile E6 showing the deviation of the midpoint MP in the sixth experiment. Therefore, it was found that the degree of the shape defect of the opening OP can be improved even if the ratio of the flow rate of BCl3 to the flow rate of the processing gas is as small as, for example, 1%.
[0076] (Experiment No. 14)
[0077] In the fourteenth experiment, a plurality of sample substrates were prepared. Each sample substrate had a silicon oxide film. In the fourteenth experiment, plasma was generated from a processing gas containing BCl3 using the plasma processing apparatus 1 to etch the silicon oxide film of the sample substrate. In the fourteenth experiment, the ratio of the flow rate of BCl3 to the flow rate of the processing gas was set to 0%, 1%, 2%, 6% or 13%, and the silicon oxide film of each sample substrate was etched. The temperature of the substrate support 14 was -70°C.
[0078] In the 14th experiment, the etching rate of the silicon oxide film was obtained after etching the silicon oxide film. The results are shown in Figure 10. Figure 10 is a graph showing the results of the 14th experiment. As shown in Figure 10, it was found that the etching rate of the silicon oxide film increases as the ratio of the BCl3 flow rate decreases.
[0079] (15th experiment)
[0080] In the fifteenth experiment, a plurality of sample substrates were prepared. Each sample substrate had a silicon nitride film. In the fifteenth experiment, plasma was generated from a processing gas containing BCl3 using the plasma processing apparatus 1 to etch the silicon nitride film of the sample substrate. In the fifteenth experiment, the ratio of the flow rate of BCl3 to the flow rate of the processing gas was set to 0%, 1%, 2%, 6% or 13%, and the silicon nitride film of each sample substrate was etched. The temperature of the substrate support 14 was -70°C.
[0081] In the fifteenth experiment, the etching rate of the silicon nitride film was obtained after etching the silicon nitride film. The results are shown in FIG. 11. FIG. 11 is a graph showing the results of the fifteenth experiment. As shown in FIG. 11, it was found that the etching rate of the silicon nitride film hardly changed even if the ratio of the BCl3 flow rate was reduced.
[0082] (Experiments 16 to 18)
[0083] In the 16th to 18th experiments, a plurality of sample substrates were prepared, which were the same as the plurality of sample substrates prepared in the 1st to 4th experiments. In each of the 16th to 18th experiments, plasma was generated from a processing gas using the plasma processing apparatus 1 to etch the silicon-containing film of the sample substrate. The processing gas used in the 16th experiment contained 8% Cl2, 4% C4F8, and 88% other gases, and did not contain BCl3. The processing gas used in the 17th experiment contained 8% Cl2, 4% C4F8, 5% BCl3, and 83% other gases. The processing gas used in the 18th experiment contained 5% BCl3, 5% C4F8, and 90% other gases, and did not contain Cl2. In the 16th to 18th experiments, the temperature of the substrate support 14 was −40° C.
[0084] In each of the 16th to 18th experiments, the top surface of the circular opening OP formed in the silicon-containing film SF by etching was observed. The results are shown in FIG. 12. (a) to (c) of FIG. 12 are diagrams showing the results of the 16th to 18th experiments, respectively. As shown in FIG. 12, the circularity of the opening OP in the 17th experiment was improved compared to the circularity of the opening OP in the 16th experiment. The circularity of the opening OP in the 18th experiment was improved compared to the circularity of the opening OP in the 17th experiment. Therefore, it was found that the circularity was improved by adding BCl3 to the processing gas. It was also found that the circularity was further improved when the processing gas did not contain Cl2.
[0085] From the foregoing, it will be understood that various embodiments of the present disclosure have been described herein for purposes of illustration, and that various modifications may be made without departing from the scope and spirit of the present disclosure. Accordingly, the various embodiments disclosed herein are not intended to be limiting, with the true scope and spirit being indicated by the appended claims. [Explanation of symbols]
[0086] 10: chamber; 14: substrate support; W: substrate; SF: silicon-containing film.
Claims
1. (a) providing a substrate having a silicon-containing film, the silicon-containing film comprising a silicon nitride film, in a chamber; (b) generating a plasma from a process gas in the chamber to etch the silicon-containing film, the process gas including a phosphorus-containing gas, a fluorine-containing gas, and a boron-containing gas; An etching method comprising:
2. 2. The etching method according to claim 1, wherein in (b), a temperature of a substrate support that supports the substrate is set to a temperature lower than 0°C.
3. 3. The etching method according to claim 1, wherein the fluorine-containing gas includes at least one of a fluorocarbon gas, a hydrofluorocarbon gas, hydrogen fluoride, nitrogen trifluoride gas, and sulfur hexafluoride gas.
4. 4. The etching method according to claim 1, wherein a ratio of a flow rate of the boron-containing gas to a flow rate of the processing gas is 6% or less.
5. The etching method according to claim 1 , wherein the silicon-containing film further comprises a silicon oxide film.
6. 6. The etching method according to claim 1, wherein the phosphorus-containing gas is a gas containing phosphorus atoms and halogen atoms.
7. The phosphorus-containing gas is PF 3 Gas, PF 5 Gas, PCl 3 Gas and POCl 3 7. The etching method according to claim 1, further comprising at least one selected from the group consisting of gases.
8. The phosphorus-containing gas is PF 3 Gas, PCl 3 Gas and POCl 3 7. The etching method according to claim 1, further comprising at least one selected from the group consisting of gases.
9. 9. The etching method according to claim 1, wherein the fluorine-containing gas includes hydrogen fluoride gas.
10. The boron-containing gas is BCl 3 The etching method according to any one of claims 1 to 9, further comprising a gas.
11. The etching method according to any one of claims 1 to 10, wherein the process gas further comprises a carbon-containing gas.
12. The etching method according to any one of claims 1 to 11, wherein the process gas further contains an oxygen-containing gas.
13. the substrate has a mask on the silicon-containing film; the mask is made of a carbon-containing material, a silicon-containing material, or a metal-containing material; The etching method according to any one of claims 1 to 12.
14. the substrate having a metal-containing mask on the silicon-containing film; The etching method according to any one of the preceding claims, wherein the metal-containing mask is made of titanium nitride, tungsten or tungsten carbide.
15. A plasma processing apparatus comprising: A chamber; a substrate support for supporting a substrate in the chamber, the substrate having a silicon-containing film including a silicon nitride film; a gas supply configured to supply a process gas into the chamber, the process gas including a phosphorus-containing gas, a fluorine-containing gas, and a boron-containing gas; a plasma generating unit configured to generate a plasma from the process gas in the chamber; A control unit; Equipped with The control unit is configured to control the plasma processing apparatus to perform an etching method, the etching method including: (b) generating the plasma from the process gas in the chamber to etch the silicon-containing film.
Citation Information
Patent Citations
Plasma processing method and plasma processing apparatus
JP2014017406A
Method for etching multilayered film
JP2016039309A
Etching processing method and etching processing apparatus
JP2020115538A
Methods of forming high aspect ratio openings, methods of forming high aspect ratio features, and related semiconductor devices
US20190206723A1
Plasma etching chemistries of high aspect ratio features in dielectrics
WO2019178030A1