Process for producing terephthalic acid-based polyesters with integrated depolymerization process
The integrated depolymerization and polymerization method for recycled PET addresses the challenge of opaque PET recycling by producing high-quality polyesters with optimized material flow, reducing energy and raw material consumption.
Patent Information
- Application Number
- JP2021544500
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-01
- Filing Date
- 2020-01-27
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-01-27
AI Technical Summary
The recycling of opaque PET is challenging due to its high pigment content, which adversely affects the mechanical properties of recycled PET and is difficult to remove through filtration, leading to inefficiencies in current chemical recycling methods.
A method integrating depolymerization and polymerization steps to produce terephthalic polyesters from recycled PET, involving glycolysis, separation, purification, and mixing processes to optimize material flow and reduce energy consumption, allowing for the production of high-quality polyesters with properties similar to virgin PET.
The method enables the production of high-quality polyesters from recycled PET without impairing their mechanical and physicochemical properties, reducing energy consumption and raw material use by optimizing the integration of material streams and minimizing intermediate processing steps.
Smart Images

Figure 00000030_0000
Abstract
Description
[Technical field]
[0001] The present invention is a process for producing polyester, particularly polyethylene terephthalate (PET), which incorporates a process for depolymerization of a feedstock of polyester, particularly including opaque polyester, to be recycled. [Background technology]
[0002] The chemical recycling of polyesters, especially polyethylene terephthalate (PET), has been the subject of numerous research studies aimed at breaking down polyesters recovered in waste form into monomers that can be reused as feedstock for polymerization processes.
[0003] Many polyesters come from material collection and sorting cycles. In particular, polyester, especially PET, can come from the collection of bottles, containers, films, resins, and / or fibers made of polyester (e.g. textile fibers, tire fibers). Polyesters coming from the collection and sorting industry are known as polyesters to be recycled.
[0004] PET to be recycled can be divided into four main categories: - Clear PET. Colorless clear PET (generally at least 60% by weight) and sky blue colored clear PET are predominant. They do not contain pigments and can be fed into mechanical recycling processes; - dark or colored (green, red, etc.) PET, which may generally contain up to 0.1% by weight of dye or pigment but still remain transparent or translucent; - Opaque PET, which contains a significant amount of pigment to make the polymer opaque. The content typically varies from 0.25% to 5.0% by weight. For example, opaque PET is increasingly used in the manufacture of food containers such as milk bottles, as well as in the composition of bottles of cosmetics, plant protection agents or dyes; - multi-layered PET, which contains layers of other polymers than PET or layers of recycled PET between layers of virgin PET (i.e. PET that has not been recycled), or a film of e.g. aluminium, which is used after thermoforming to produce packaging such as containers.
[0005] The collection industries that allow the supply to the recycling industry are structured differently in different countries. They evolve to maximize the amount of plastic recycled from waste, depending on the nature and volume of the waste streams, as well as their sorting technologies. The waste stream recycling industry generally consists of a first stage of conditioning in flake form. In this stage, bales of raw packaging are washed, refined, sorted, crushed, and then refined and sorted again. This results in a flake stream that generally contains less than 1% by weight of "visible to the naked eye" impurities (glass, metals, other plastics, wood, paper, cardboard, inorganic elements) and preferentially less than 0.2% and even more preferentially less than 0.05% of "visible to the naked eye".
[0006] The clear PET flakes can then be subjected to a process of extrusion-filtration, which makes it possible to produce an extrudate that can then be reused as a mixture with virgin PET to produce new products (bottles, fibers, films). To be used for food applications, a process of solid-state polymerization under vacuum (known under the acronym SSP) is necessary. This type of regeneration process is known as mechanical recycling.
[0007] Dark (or pigmented) PET flakes can also be subjected to mechanical recycling. However, their use is limited by the color of the extrudates formed from the pigmented stream: dark PET is typically used to make packaging strips and packaging fibers. Thus, its outlets are more limited compared to those of clear PET.
[0008] The presence of opaque PET with a high content of pigments in the PET to be recycled poses a problem for recyclers, as this opaque PET has a negative effect on the mechanical properties of the recycled PET. Opaque PET is currently collected together with colored PET and is found in the colored PET stream. The content of opaque PET in the colored PET stream to be recycled is currently 5-20% by weight, but is likely to increase further, taking into account the development of applications for opaque PET. In a period of a few years, the content of opaque PET in the colored PET stream could reach more than 20-30% by weight. In fact, it has been shown that when the proportion of opaque PET in the coloured PET stream exceeds 10-15%, the mechanical properties of the recycled PET are adversely affected (see Impact du developpement du PET opaque blanc sur le recyclage des emballages en PET (Impact of the increase in white opaque PET on the recycling of PET packaging), COTREP preliminary report, published 5 December 2013) and that in these cases the mechanical properties of the recycled PET prevent its recycling in fibre form, which is the main industrial exit point for coloured PET.
[0009] Dyes are natural or synthetic substances that are soluble in polyester materials and are introduced into the materials to color them. Commonly used dyes have different properties and often contain O- and N-type heteroatoms and conjugated unsaturation, for example quinone, methine or azo functional groups or molecules such as pyrazolones and quinophthalones. Pigments are finely divided substances that are insoluble in polyester materials and are introduced into the materials to color and / or opacify them. The main pigments used to color and / or opacify polyesters, especially PET, are metal oxides such as TiO2, CoAl2O4 or Fe2O3, silicates, polysulfides, as well as carbon black. Pigments are particles that generally have a size of 0.1-10 μm, predominantly 0.4-0.8 μm. Complete removal of these pigments by filtration is necessary to envisage the regeneration of opaque PET, but is technically difficult due to the extremely high clogging tendency of the pigments.
[0010] Recycling of colored and opaque PET thus poses extremely difficult problems.
[0011] Several methods have been proposed in the literature for the chemical recycling of polyesters, especially PET, but all of them are not intended to obtain the same end product that can then be used to produce terephthalate polymers again.
[0012] In particular, US Pat. No. 5,999,633 discloses the production of high quality polyester. It comprises a process for depolymerizing PET flakes by glycolysis at atmospheric pressure in the presence of ethylene glycol in a bis(2-hydroxyethyl) terephthalate (BHET) base. The intermediate product obtained at the end of the depolymerization stage is filtered through a sintering system, which retains particles of at least 25 μm before being introduced into the polymerization reactor, resulting in high quality polyester. In Patent Document 2, after depolymerization of the polyalkylene terephthalate resin by hydrolysis or methanolysis, the carboxylic acid monomers in crystalline form and the polyol monomers in liquid form are recovered and then recombined to reform the polyester. US Patent No. 5,399,933 itself describes a process for preparing recycled copolyesters with high monomer content, which comprises the steps of depolymerization by methanolysis, separation of the released dimethyl terephthalate, followed by polymerization of the latter with at least one polyol.
[0013] US Patent No. 4,399,633 discloses a method for depolymerization by glycolysis of colored PET, especially from the recovery of green colored PET bottles. The BHET stream obtained at the end of the glycolysis step is passed through activated carbon to separate certain dyes, such as blue dyes, and then purified by extraction of the remaining dyes, such as yellow dyes, with alcohol or water. The BHET is separated with the aim of being crystallized from the extraction solvent and then usable in the PET polymerization process. In US Pat. No. 5,233,993, post-consumption PET, including a mixture of variously colored PETs such as clear, blue, green, and / or amber, is depolymerized by glycolysis in the presence of an amine catalyst and an alcohol, and the resulting diester monomers can be purified by filtration, ion exchange, and / or passage through activated carbon, and then crystallized and recovered by filtration, thus polymerizing to reform the polyester.
[0014] Patent document 6 discloses a method for preparing glycol modified polyethylene terephthalate (r-PETG) which comprises a step of depolymerization of PET in the presence of a mixture of monoethylene glycol (MEG) and neopentyl glycol, followed immediately by a step of polymerization of the reaction effluent.
[0015] US Pat. No. 5,399,633 describes a method for the depolymerization of a polyester feedstock containing, inter alia, 0.1-10% by weight of pigment. The depolymerization is carried out by glycolysis in the presence of ethylene glycol. The effluent of bis(2-hydroxyethyl) terephthalate (BHET) monomer, obtained after specific separation and purification steps, can be fed, without any specified conditions, to a step of polymerization aimed at producing PET. In the document, the method for depolymerization of polyesters, the nature of which is not specified, involves the steps of depolymerization in the presence of a diol, evaporation of the diol, dissolution of the mixture in a hot solvent, filtration, and precipitation of the filtered solution, which can then be used in the fresh preparation of the polymer.
[0016] US Pat. No. 5,399,633 describes the production of purified BHET from PET, which can be used as a raw material in the production process of plastic products. Depolymerization is followed by steps of preliminary purification by cooling, filtration, adsorption and treatment with ion exchange resins (presented as being of great importance), followed by evaporation of the glycol and purification of the BHET. Prepurification makes it possible to prevent repolymerization of the BHET in the subsequent purification steps. However, carrying out the steps of filtration and ion exchange resins can be very difficult when the feedstock contains a large amount of very small solid particles, such as pigments. This is the case when the treated feedstock contains a significant proportion of opaque PET, especially (more than 10% by weight of opaque PET). Similarly, US Pat. No. 5,399,633 discloses the possible use of high-purity bis(2-hydroxyethyl) terephthalate as a raw material for regenerating high-quality polyesters. For this purpose, EP 1 120 394 B1 describes a process for depolymerizing polyesters, which comprises a step of glycolysis in the presence of ethylene glycol, and a process for purifying the solution of bis(2-hydroxyethyl) terephthalate using cation- and anion-exchange resins. [Prior art documents] [Patent documents]
[0017] [Patent Document 1] Mexican Patent Application Publication No. 2007 / 004429 [Patent Document 2] U.S. Pat. No. 4,578,502 [Patent Document 3] International Publication No. 2013 / 025186 Brochure [Patent Document 4] US Patent Application Publication No. 2006 / 0074136 [Patent Document 5] US Patent Application Publication No. 2015 / 0105532 [Patent Document 6] International Publication No. 2017 / 006217 Brochure [Patent Document 7] French Patent Application Publication No. 3053691 [Patent Document 8] European Patent No. 0865464 [Patent Document 9] Japanese Patent No. 3715812 [Patent Document 10] European Patent No. 1120394 Summary of the Invention [Problem to be solved by the invention]
[0018] None of the documents proposes a direct link between the depolymerization step, including dark and / or opaque PET, in particular of the PET to be recycled, and the polymerization step of the resulting intermediate products, in particular with optimal integration of the material streams, especially the diol streams, which would allow a considerable reduction in raw material and energy consumption.
[0019] The subject of the present invention is a process for the manufacture of terephthalic acid-based polyesters from at least one feedstock of polyester to be recycled, comprising at least the following steps: a) a depolymerization step of the feedstock of polyester to be recycled, comprising at least one reaction section to which the feedstock of polyester to be recycled and a glycol feedstock are fed, said reaction section being operated at a temperature between 150°C and 400°C, preferably between 180°C and 300°C, more preferably between 200°C and 280°C, at a pressure of at least 0.1 MPa, preferentially at least 0.4 MPa, with a residence time per reactor of 0.05 to 10 hours, thereby obtaining a depolymerization reaction effluent; b) a separation step comprising at least one separation section to which the depolymerization reaction effluent obtained at the end of the depolymerization step a) is fed, thereby obtaining at least one glycol effluent and one diester effluent; c) a purification step of the diester effluent obtained at the end of step b), comprising at least one separation section to which the diester effluent obtained at the end of step b) is fed and which is operated at a temperature of not more than 250°C, a pressure of not more than 0.001 MPa and a liquid residence time per section of not more than 10 minutes, followed by a decolorization section in the presence of an adsorbent and operated at a temperature between 100°C and 250°C and a pressure between 0.1 and 1.0 MPa, thereby obtaining a purified liquid diester effluent, d) a process for preparing a polymerization feedstock, comprising at least one mixing section to which is fed at least one terephthalic acid feedstock and, in liquid form, at least one fraction of the purified diester effluent obtained in step c), wherein the amount of at least the terephthalic acid feedstock and the fraction of the purified diester effluent introduced into the mixing section is determined by the formula -[C (n+1) H (2n+2)a preparation step in which the ratio of the total number of moles of diol units of the formula -[CO-(CH)-CO]- (wherein n is an integer equal to or greater than 1) to the total number of moles of terephthalic acid units of the formula -[CO-(CH)-CO]- introduced into said mixing section is adjusted to be 1.0-2.0, and said mixing section is operated at a temperature of 25°C-250°C and a pressure of 0.1 MPa or more; e) a condensation step of the polymerization feedstock from step d) to produce at least one condensation reaction effluent, one diol effluent, and one aqueous or one methanol effluent, said condensation step comprising at least one reaction section operated at a temperature between 150°C and 400°C, a pressure between 0.05 and 1 MPa, and a residence time between 1 and 10 hours, and at least one separation section; f) a polycondensation step of the condensation reaction effluent obtained in step e) to obtain at least the terephthalic polyester and a diol effluent, the polycondensation step comprising at least one reaction section, the reaction section comprising at least one reactor in which polycondensation takes place, operated at a temperature between 200°C and 400°C, a pressure between 0.0001 and 0.1 MPa and a residence time between 0.1 and 5 hours, the reaction section also comprising at least one withdrawal of the diol effluent; g) a diol treatment step comprising at least a recovery section to which all or part of the glycol effluent from step b) and all or part of the diol effluent from step f) are fed in order to obtain a diol stream to be treated, and a purification section of said diol stream to be treated in order to obtain a purified diol stream; The manufacturing method includes:
[0020] Preferably, the present invention relates to a process for producing terephthalic acid-based polyesters from at least one polyester feedstock to be recycled, comprising the above steps a), b), c), d), e), f) and g). Effect of the Invention
[0021] The main advantage of the present invention is the production of polyesters, at least in part, from compounds originating from the polyesters to be recycled, without compromising the quality of the polyesters produced, which are in significant quantities, in particular of opaque polyesters, in amounts consistent with those encountered in polyester materials originating from the collection and sorting industry. In particular, the present invention makes it possible to produce polyesters, at least in part, from the polyesters to be recycled, which have properties, in particular physicochemical and mechanical properties, similar to those of virgin polyesters of the same type.
[0022] The present invention relates to a particular method that involves linking a process for depolymerization, in particular by glycolysis, of polyester material to be recycled with a process for polymerization of polyester, which allows the integration of the material streams. It more particularly allows an optimal integration of the streams of diols introduced and recovered between the depolymerization and polymerization stages, in particular by a particular recycling system. The present invention also allows the production of purified liquid diester intermediates that meet the specifications of the polymerization process and therefore can be fed directly to the polymerization process. This production is carried out without intermediate steps of purification and / or conditioning (such as, for example, crystallization of said intermediates and then transfer of said crystalline diester intermediates to the liquid phase), which makes it possible to avoid additional processing operations and high energy consumption. At the same time, the incorporation of the purified diester intermediates, obtained in liquid form at the end of the depolymerization step, into the polymerization process, in particular into the mixture of monomers, makes it possible to reduce the amount of diol monomer feedstock fed to the polymerization process, while retaining good operability, in particular of the step of preparing the monomer mixture of the polymerization process. Since the amount of diol introduced into the mixture is reduced, the amount of diol to be recycled in the subsequent operation of the polymerization process is reduced, and thus the energy consumption of the overall process for producing polyester, at least in part, from the polyester material to be recycled is reduced.
[0023] Another advantage of the present invention is the sharing of operations for recovering and purifying the diol effluents from the depolymerization and polymerization processes, which in particular leads to reduced overall process energy consumption and reduced capital costs. [Brief description of the drawings]
[0024] [Figure 1] 1 illustrates one particular configuration of a process for producing polyethylene terephthalate (PET) according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The present invention relates to a process for producing polyester, in particular a process for integrating the depolymerization process of polyester feedstock to be recycled, including opaque polyester.
[0026] In accordance with the present invention, the terms "polyester", "terephthalic acid-based polyester", and "polyalkylene terephthalate" are interchangeable and refer to a polymer having a basic repeat unit, such as a terephthalic acid unit, -[CO-(CH)-CO]-, where -(CH)- represents an aromatic ring, which is in turn linked to a diol unit, -[OC (n+1) H (2n+2)-O]- (where n is an integer greater than or equal to 1, preferably between 1 and 5, preferentially between 1 and 3), denotes a polymer (i.e. a molecule of high molecular weight consisting of monomers covalently bonded to each other). Very generally, polyalkylene terephthalates are the result of polycondensation of diol (or glycol) monomers with terephthalic acid (or dimethyl terephthalate) monomers. According to the invention, the terephthalic acid-based polyester or polyalkylene terephthalate is in particular polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT) or any other polymer whose main chain repeating units contain ester functional groups and aromatic rings derived from terephthalic acid (or from one of its esters, in particular dimethyl terephthalate). According to the invention, the preferred terephthalic acid-based polyester is polyethylene terephthalate, or poly(ethylene terephthalate), also known simply as PET. The basic repeat unit has the formula:
[0027] [ka]
[0028] Traditionally, PET is obtained by polycondensation of terephthalic acid (PTA) or dimethyl terephthalate (DMT) with ethylene glycol.
[0029] According to the present invention, the expression "to be recycled" describes any material, including, inter alia, polyester, originating from the plastic waste collection and sorting industry. In contrast, virgin polyester originates exclusively from the polymerization of a monomer feedstock comprising at least one dicarboxylic acid (e.g., terephthalic acid, PTA) or one dicarboxylic acid ester (e.g., dimethyl terephthalate, DMT) and at least one compound of the diol or glycol classes (e.g., ethylene glycol).
[0030] According to the present invention, the term "diester monomer" refers to a diester monomer having the formula HOC (m+1) H (2m+2) -CO2-(C6H4)-CO2-C (n+1) H (2n+2) In this chemical formula, -(C6H4)- represents an aromatic ring, and n and m are the same or different integers, preferably the same integer (i.e., n=m), and are 1 or more, preferably 1 to 5, and more preferably 1 to 3. A molecule of the diester monomer corresponds to a compound resulting from the esterification of one molecule of terephthalic acid HOOC-(C6H4)-COOH (wherein -(C6H4)- represents an aromatic ring) with two molecules of at least one diol (or glycol). More specifically, the two molecules are represented by the chemical formula HO-C (n+1) H (2n+2) One molecule of diol with the formula HO-C (m+1) H (2m+2) One molecule of the diol with -OH. The preferred diester monomer is bis(2-hydroxyethyl) terephthalate (BHET).
[0031] The term oligomer typically refers to a polymer of small size, generally consisting of 2 to 20 basic repeating units.
[0032] According to the present invention, the term "ester oligomer" means a terephthalic acid ester oligomer, which has the formula -[O-CO-(CH)-CO-O- C (n+1) H (2n+2) The copolymer contains 2 to 20, preferably 2 to 5, basic repeating units of the formula: --(C6H4)-- (wherein --(C6H4)-- is an aromatic ring, and n is an integer of 1 or more, preferably 1 to 5, more preferably 1 to 3).
[0033] The term "dye" is understood to mean a substance that is soluble in the polyester material and is used to color the polyester material. The dyes can be of natural or synthetic origin.
[0034] The term "pigment", more particularly colouring pigments and / or opacifying pigments, is understood to mean finely divided substances insoluble in the polyester material. The pigments are in the form of particles having a size generally between 0.1 and 10 μm, predominantly between 0.4 and 0.8 μm. Pigments are often of inorganic nature. Commonly used pigments, especially opacifying pigments, are metal oxides such as TiO2, CoAl2O4 or Fe2O3, silicates, polysulfides and carbon black.
[0035] According to the present invention, the expression "... to..." means that the two stated ranges include the two limiting values at both ends of the separation. If this is not the case, and the stated range does not include the limiting value, this is expressly stated by the present invention.
[0036] feedstock According to the invention, the process is provided with at least one feedstock of polyester to be recycled.
[0037] Advantageously, the feedstock of polyester to be recycled originates from an industry that collects and separates waste, in particular plastic waste. The feedstock of polyester to be recycled may for example originate from the collection of bottles, containers, films, resins and / or fibres made of polyethylene terephthalate.
[0038] The polyester feedstock to be recycled may be in the form of flakes, completely or partially. The flakes are in the form of particles with a maximum length of less than 10 cm, preferentially between 5 and 25 mm, or in the form of ultrafinely divided solids, i.e. preferably with a size between 10 microns and 1 mm. The polyester feedstock to be recycled preferably contains less than 2% by weight, preferentially less than 1% by weight, of "visible to the naked eye" impurities (glass, metal, plastics other than terephthalic polyesters, wood, paper, cardboard, or inorganic elements, etc.). The polyester feedstock to be recycled may also be in the form of fibers, such as textile fibers, optionally pretreated to remove cotton, polyamide fibers, or any other textile fibers other than polyester fibers, or tire fibers, in particular, optionally pretreated to remove polyamide fibers, rubber, or polybutadiene residues. The polyester feedstock to be recycled may further comprise polyester originating from production scrap from the polymerization and / or conversion processes of polyester materials.
[0039] Advantageously, said feedstock of polyester to be recycled contains more than 50% by weight of polyalkylene terephthalate, preferably more than 70% by weight, more preferably more than 90% by weight of polyalkylene terephthalate.
[0040] Preferably, the polyester feedstock to be recycled is a polyethylene terephthalate feedstock to be recycled (or a PET feedstock to be recycled) and comprises more than 50% by weight of polyethylene terephthalate (PET), preferably more than 70% by weight of polyethylene terephthalate (PET), more preferably more than 90% by weight of polyethylene terephthalate (PET). The PET feedstock to be recycled advantageously comprises opaque PET, dark (or colored) PET, multi-layer PET, clear (i.e. water-free and / or sky-blue colored transparent) PET, and mixtures thereof, preferably at least opaque PET. Preferably, it comprises at least 10% by weight of opaque PET, very preferably at least 15% by weight of opaque PET.
[0041] The polyester feedstock to be reclaimed may contain up to 10 wt.% pigment, in particular 0.1 wt.% to 10 wt.% pigment, especially 0.1 wt.% to 5 wt.% pigment, and / or up to 1 wt.% dye, in particular 0.05 wt.% to 1 wt.% dye, especially 0.05 wt.% to 0.2 wt.% dye.
[0042] The feedstock of polyester to be reclaimed may also contain elements used as polymerization catalysts and / or stabilizers in the polyester production process, such as antimony, titanium, or tin.
[0043] According to the invention, the depolymerization step a) is further provided with a glycol feedstock, which comprises at least one, preferably one, glycol (or diol) compound, of the same or different type as the diols corresponding to the diol units of the basic polyalkylene terephthalate units of the feedstock of the polyester to be regenerated. Advantageously, the weight content of the glycol compounds in the glycol feedstock is greater than or equal to 80% by weight, preferentially greater than or equal to 90% by weight, preferably greater than or equal to 95% by weight, relative to the total weight of the glycol feedstock.
[0044] Preferably, the glycol feedstock of the process, fed to the depolymerization step a), comprises ethylene glycol, also known as monoethylene glycol (MEG), the weight content of which is advantageously greater than or equal to 80% by weight, preferentially greater than or equal to 90% by weight and preferably greater than or equal to 95% by weight, relative to the total weight of said glycol feedstock, in which case the glycol feedstock is referred to as ethylene glycol feedstock.
[0045] The ethylene glycol may be advantageously produced by the hydrolysis of ethylene oxide, the selective hydrogenation of glycolaldehyde, the depolymerization of polyesters, or any other process capable of obtaining an ethylene glycol feedstock meeting the specifications required by the polymerization process. The ethylene glycol may be derived from fossil hydrocarbon sources or from biomass.
[0046] Said glycol feedstock supplied to the depolymerization step a) of the process according to the invention advantageously comprises, and preferably consists exclusively of, at least one fraction of said purified diol stream obtained at the end of step g) of the process according to the invention for the preparation of terephthalic acid-based polyesters.
[0047] According to the invention, the process also comprises, in step d) of preparing the polymerization feedstock, being provided with at least one terephthalic acid feedstock. According to the invention, the terephthalic acid feedstock is a terephthalic acid feedstock comprising terephthalic acid as a compound having terephthalic acid units, or a dimethyl terephthalate feedstock comprising dimethyl terephthalate as a compound having terephthalic acid units.
[0048] Said terephthalic acid feedstock comprises terephthalic acid (PTA) or dimethyl terephthalate (DMT) in a weight content of at least 95% by weight, preferentially at least 98% by weight, preferably at least 99% by weight, relative to the total weight of said terephthalic acid.
[0049] In one preferred embodiment, the feedstock is a terephthalic acid feedstock comprising terephthalic acid (PTA). The terephthalic acid of the terephthalic acid feedstock can advantageously be produced by the oxidation of paraxylene, the depolymerization of polyesters, or any other process that makes it possible to obtain a terephthalic acid feedstock that meets the specifications required by the polymerization process. The terephthalic acid can be derived from fossil hydrocarbon sources or biomass.
[0050] The terephthalic acid feedstock is advantageously in the form of a powder, i.e. in the form of solid terephthalic acid particles. The terephthalic acid particles preferably incorporated in the mixture of monomers have an average diameter of preferably 1 to 1000 μm, in particular 30 to 500 μm, especially 80 to 200 μm. The average diameter of the terephthalic acid particles can be determined by any method of particle size analysis known to the skilled person, for example by laser diffraction or sieving, preferably by sieving through a column of suitable sieves by techniques known to the skilled person.
[0051] Depolymerization step a) According to the invention, the process for producing terephthalic acid-based polyesters comprises a step a) of depolymerization of a feedstock of polyester to be recycled, thereby obtaining a depolymerization reaction effluent, said depolymerization step a) comprising at least one reaction section, to which said feedstock of polyester to be recycled and a glycol feedstock are fed.
[0052] Advantageously, the supply of the glycol feedstock is adjusted so that the amount of glycol compound contained in the glycol feedstock corresponds at the inlet of the reaction section to 1 to 20 moles, preferably 3 to 10 moles, of glycol compound per mole of polyester basic repeat unit contained in the feedstock of polyester to be recycled.
[0053] Advantageously, said glycol feedstock advantageously comprises, and preferably consists exclusively of, at least a fraction of said purified diol stream obtained at the end of step g) of the process for the manufacture of terephthalic acid-based polyesters according to the invention.
[0054] Advantageously, the depolymerization step a) employs, in particular in the reaction section, a glycolysis reaction of the polyalkylene terephthalates of the feedstock of the polyester to be regenerated in the presence of glycol compound(s) of the glycol feedstock.
[0055] Said reaction section of the depolymerization step a) is preferably operated in one or more reactors at a temperature between 150°C and 400°C, preferably between 180°C and 300°C, more preferably between 200°C and 280°C, at a pressure of at least 0.1 MPa, preferentially at least 0.4 MPa, and with a residence time per reactor of 0.05 to 10 hours, preferentially between 0.1 and 6 hours, preferably between 0.5 and 4 hours. The residence time in the reactors of said reaction section of step a) is defined as the ratio of the volume of reaction liquid in the reactor of said reaction section to the volumetric flow rate of the stream fed to said reactor of said reaction section.
[0056] Any type of reactor known to the skilled artisan that makes it possible to carry out the depolymerization or transesterification reaction may be used in the reaction section of step a). Preferably, the reactor(s) in the reaction section of step a) are stirred by a mechanical stirring system, a recirculation loop and / or fluidization. Said reactor(s) may comprise a conical base that makes it possible to withdraw impurities. Advantageously, said reaction section of step a) may comprise one or more tubular reactors, in series or in parallel, or a combination of one or more stirred reactors and one or more tubular reactors.
[0057] In one particular embodiment of the invention, the depolymerization step a) comprises at least one reaction section to which a feedstock of PET to be recycled and an ethylene glycol feedstock are fed, the amount of ethylene glycol contained in the ethylene glycol feedstock being such that it corresponds to 1-20 moles, preferably 3-10 moles, of ethylene glycol of the ethylene glycol feedstock per mole of basic repeating unit, i.e. terephthalic acid unit, in the feedstock of PET to be recycled, the reaction section being operated in one or more reactors at a temperature of 150°C to 400°C, preferably 180°C to 300°C, more preferably 200°C to 280°C, at an operating pressure of at least 0.1 MPa, preferentially at least 0.4 MPa, with a residence time per reactor of 0.05 to 10 hours, preferably 0.1 to 6 hours, more preferably 0.5 to 4 hours, the residence time per reactor being defined as the ratio of the liquid volume of the reactor to the volumetric flow rate of the stream fed to the reactor.
[0058] The depolymerization reaction of step a) of the process according to the invention may be carried out with or without the addition of a catalyst. If the depolymerization reaction is carried out after the addition of a catalyst, the catalyst may be homogeneous or heterogeneous and is selected from esterification catalysts known to those skilled in the art, such as complexes, oxides and salts of antimony, tin or titanium, alkoxides of metals from groups (I) and (IV) of the periodic table of the elements, organic peroxides or acidic / basic metal oxides. Preferably, the depolymerization reaction is carried out without the addition of a catalyst.
[0059] The depolymerization reaction may also advantageously be carried out in the presence of a solid adsorbent in powder or shaped form, the role of which is to capture at least a portion of the impurities, in particular the coloring impurities, and thus to ease the burden on the purification stage of step b). Said solid adsorbent is in particular activated carbon.
[0060] The depolymerization effluent obtained at the end of the depolymerization step a) is a diester monomer (i.e., (m+1) H (2m+2)-CO2-(C6H4)-CO2-C (n+1) H (2n+2) OH (wherein -(C6H4)- represents an aromatic ring; n and m are the same or different integers, preferably the same integers, and are 1 or more, preferably 1 to 5, more preferably 1 to 3)) and a compound of the formula -[O-CO-(C6H4)-CO-OC (n+1) H (2n+2) The depolymerization reaction effluent comprises a mixture of oligomers containing 1 to 5, preferably 1 to 3, basic units of 1-5-1,1-2,1-diol compounds, impurities optionally present in said feedstock of polyester to be regenerated, and compounds optionally resulting at the end of side reactions, such as etherification or decomposition reactions. The diol compounds optionally present in the depolymerization reaction effluent are advantageously unreacted ones originating from the diol monomers and comonomers incorporated in the composition of the feedstock of polyester to be recycled and discharged at the end of the depolymerization reaction, and from the glycol stream fed to the depolymerization step a). The depolymerization reaction effluent may contain unconverted polyester and other polymers.
[0061] Separation step b) According to the invention, the process for producing terephthalic polyesters comprises a separation step b) which comprises at least one separation section to which the depolymerization reaction effluent obtained at the end of the depolymerization step a) is fed, thereby obtaining at least one glycol effluent and one diester effluent.
[0062] Said separation step b) advantageously makes it possible to recover the diol compounds of the glycol feedstock of step a) that have not reacted and the diol compounds possibly released during the depolymerization reaction. The glycol effluent obtained at the end of said step b) preferably comprises at least 50% by weight, preferentially at least 70% by weight and preferably more than 90% by weight of diol compounds.
[0063] Advantageously, said separation section comprises one or more separation operations, which allow the recovery of an effluent rich in diol (called glycol effluent) and, optionally, an effluent rich in light impurities and an effluent rich in heavy impurities. In particular, the separation section may comprise one or more separation (distillation, stripping, rectification) columns, which allow the obtaining of at least one effluent rich in diol (i.e. glycol effluent) and, optionally, an effluent rich in light impurities and an effluent rich in heavy impurities. Preferably, said separation section comprises a series of gas / liquid separations, preferably 1 to 5 gas / liquid separations, preferentially 3 to 5 gas / liquid separations, carried out at a temperature between 100°C and 250°C, preferably between 110°C and 220°C, more preferably between 120°C and 210°C, and at a pressure between 0.00001 and 0.2 MPa, preferably between 0.00004 and 0.15 MPa, more preferably between 0.00004 and 0.1 MPa. Said gas / liquid separations are advantageously stirred by any method known to the skilled person. Under such pressure and temperature conditions, at least a part of the diol in the reaction effluent, in liquid form, is evaporated in each of the gas / liquid separations and separated from the liquid stream comprising the diester monomer, so that crystallization and polymerization of the diester monomer are prevented. Advantageously, the temperature and pressure of the subsequent gas / liquid separation is lower than that of the preceding gas / liquid separation, so that at least a portion of the glycol effluent from the preceding separation can reboil, upon condensation, a portion of the liquid effluent of the subsequent separation. In this configuration, the input of heat for glycol recovery is minimized.
[0064] Advantageously, in a separation step b) an operation of separating the various diols and, optionally, dyes, light alcohols or water in the glycol recovered by an optional series of gas / liquid separations can be carried out. The glycol effluent obtained at the end of step b) thus contains a content of at least 50% by weight, preferentially at least 70% by weight and preferably at least 90% by weight of diol compounds corresponding to the diol units of the polyalkylene terephthalate feedstock of the polyester to be regenerated. Preferably, this optional separation operation is carried out in a distillation, stripping or rectification column, advantageously at a temperature between 50°C and 250°C, preferably between 60°C and 210°C, more preferably between 70°C and 180°C, and at a pressure between 0.00001 and 0.2 MPa, preferably between 0.00004 and 0.15 MPa and more preferably between 0.00004 and 0.1 MPa.
[0065] Preferably, all or part of said glycol effluent obtained at the end of step b) is advantageously sent to process step g) of the process according to the invention.
[0066] All or part of the glycol effluent recovered at the end of step b) may be pre-purified in a section for pre-purification of diols included in step b), which removes part of the impurities accompanying the glycol effluent, such as dyes, pigments or other solid particles. The pre-purification section to which all or part of the glycol effluent is fed may comprise, by way of non-limiting example, adsorption on solids (e.g. activated carbon) and filtration systems. At least part of the pre-purified glycol effluent may be directly recycled to the depolymerization step a) and / or to the step c) of preparing the esterification feedstock.
[0067] The diester effluent obtained at the end of the separation step b), advantageously in liquid form, advantageously comprises more than 10% by weight, preferably more than 25% by weight and more preferably more than 50% by weight of diester monomers and ester oligomers.
[0068] The separation section of step b) may optionally advantageously comprise one or more falling film or thin film evaporation systems, in series or in parallel, carried out at a temperature below 200°C, preferably below 180°C, and at a pressure below 0.001 MPa, preferably below 0.0005 MPa, to further reduce the amount of diol optionally remaining in the diester effluent while minimizing polymerization of diester monomers in said diester effluent.
[0069] Purification process c) According to the invention, the diester effluent obtained at the end of separation step b) is then fed to a purification step c), which comprises at least one separation section followed by one decolorization section.
[0070] Advantageously, a step for purifying the diester effluent obtained at the end of the separation step b) makes it possible to separate at least one purified diester effluent from all or some of the following compounds originating from the depolymerization step a), while minimizing losses of diester monomers: ester oligomers, possibly unconverted polyester, impurities possibly present in the feedstock of the polyester to be regenerated (other polymers, pigments, dyes, polymerization catalysts or any other inorganic compounds constituting said feedstock of the polyester to be regenerated or formed during the depolymerization step a), and, if necessary, diol compounds not yet separated, etc.
[0071] Said purification step therefore makes it possible to recover a purified diester effluent, in which the yield of diester monomer in said purified diester effluent is at least 50% by weight, preferably at least 70% by weight, more preferably at least 80% by weight. The expression "yield of diester monomer in said diester effluent" means the amount of diester monomer in said diester effluent relative to the total amount of diester monomer introduced into the purification section of step b).
[0072] Preferably, the purification step involves one or more purification procedures such as filtration, evaporation, distillation, adsorption onto a trapping mass, etc.
[0073] According to the invention, purification step c) comprises one or more sections for separating the diester effluent obtained at the end of step b), which are intended to separate the vaporized diester monomer from heavy impurities, in particular oligomers and possibly polyesters not converted in step a), which remain liquid and therefore capture solid impurities (in particular pigments, unconverted polymer, other polymers possibly present and the polymerization catalysts), while minimizing losses of diester monomers, in particular by repolymerization. Some ester oligomers may be entrained together with the diester monomers.
[0074] Said separation section(s) of step c) are advantageously fed with said diester effluent obtained at the end of step b) and are operated at a temperature below 250°C, preferably below 230°C, very preferably below 200°C, at a pressure below 0.001 MPa, preferably below 0.0001 MPa, more preferably below 0.00005 MPa, and with a liquid residence time per section below 10 minutes, preferably below 5 minutes, more preferably below 1 minute. According to the invention, the liquid residence time per section is defined by the ratio of the liquid volume of said section to the volumetric flow rate of the hottest stream leaving said section. At the end of said separation section(s) of purification step c) at least one liquid effluent enriched in heavy impurities and one pre-purified diester effluent are obtained (preferably lean in impurities).
[0075] The separation of the prepurified diester effluent and the liquid effluent enriched in heavy impurities is advantageously carried out in a falling film or thin film evaporation system by falling film or thin film short stage distillation or a series of several falling film or thin film short stage distillations and / or evaporations at temperatures below 250° C., preferably below 230° C., very preferably below 200° C., and at pressures below 0.001 MPa, preferably below 0.0001 MPa, preferably below 0.00005 MPa. To carry out the separation at temperatures below 250° C., preferably below 230° C., while still allowing the vaporization of the diester monomer, very low operating pressures are required.
[0076] A polymerization inhibitor may advantageously be mixed with the diester effluent obtained at the end of step b) before being fed to said purification step c). Advantageously, a flux may also be mixed with the diester effluent from step b) before being fed to said step c), which facilitates the removal of heavy impurities, especially pigments, at the bottom of the short-path distillation or evaporation system. If a flux is introduced, it must have a much higher boiling point than the diester monomers of the diester effluent under the operating conditions of step c). It may be, for example, polyethylene glycol, or PET oligomers.
[0077] The liquid effluent concentrated in heavy impurities advantageously concentrates oligomers, unconverted PET, and heavy impurities, in particular pigments, other polymers possibly present, and the polymerization catalyst. The operating conditions of the separation in the separation section(s) of said step c) are adjusted so that losses of diester monomers by repolymerization are minimized. Some oligomers may be entrained with the diester monomers in the prepurified diester effluent, in particular in gaseous form.
[0078] At least one fraction of said liquid effluent enriched in heavy impurities may advantageously be recycled to the depolymerization step a), thereby increasing the yield of diester monomers of the depolymerization process. Prior to any recycling operation, said liquid effluent enriched in heavy impurities is advantageously subjected to at least one purification step, preferably a filtration step, which reduces the amount of pigment and / or other solid impurities possibly present. All or part of said liquid effluent enriched in heavy impurities may also advantageously be withdrawn from the process and sent to an incineration system or to a pigment recovery system.
[0079] The liquid effluent enriched in heavy impurities may advantageously be mixed with at least one fraction of the glycol effluent obtained at the end of separation step b) and / or with at least one fraction of the purified diol stream obtained at the end of step g) of the process according to the invention, thereby reducing the viscosity of said liquid effluent enriched in heavy impurities and facilitating its transport to the depolymerization step a) and, optionally, its treatment in the filtration step.
[0080] Optionally, the pre-purified diester effluent may advantageously be mixed with at least one fraction of the glycol effluent resulting from separation step b) and / or with at least one fraction of the purified diol stream resulting from step g).
[0081] According to the invention, purification step c) comprises a section for decolorization of the prepurified diester effluent, advantageously operated at a temperature between 100°C and 250°C, preferably between 110°C and 200°C, more preferably between 120°C and 180°C, and at a pressure between 0.1 and 1.0 MPa, preferably between 0.2 and 0.8 MPa, more preferably between 0.3 and 0.5 MPa, in the presence of an adsorbent, thereby resulting in a purified diester effluent. The said adsorbent may be any adsorbent known to the person skilled in the art capable of capturing dyes, preferably activated carbon, such as activated carbon or clay.
[0082] The purified diester effluent obtained at the end of step c) comprises at least one diester monomer. It may optionally comprise at least one diol (or glycol) corresponding to the diol unit contained in said diester monomer of said purified diester effluent. Advantageously, the purified diester effluent obtained at the end of step c) comprises at least 10% by weight, preferably at least 20% by weight of diester monomer. It preferably contains less than 1% by weight, preferably less than 0.1% by weight of pigments introduced into the process together with the feedstock of polyester to be recycled, and less than 10% by weight, preferably less than 1% by weight of dyes introduced into the process together with the feedstock of polyester to be recycled. Preferably, the purified diester effluent obtained at the end of step c) comprises less than 10% by weight, preferentially less than 1% by weight, preferably less than 0.1% by weight of impurities heavier than said diester monomer, other than possibly oligomers of said diester. Very advantageously, the purified diester effluent obtained at the end of step c) is free of colored or inorganic impurities such as pigments, dyes, depolymerization catalysts and ions. Preferably, the purified diester monomer comprises diester monomer and optionally oligomeric molecules of said diester with a degree of polymerization between 2 and 5. According to the invention, the term "free" means that the content of the compound of interest in the purified diester effluent is below the limit of determination of the analytical method used to determine said content.
[0083] Advantageously, a purified diester effluent is obtained at the end of step c) in liquid form. At least one fraction of said purified diester effluent obtained at the end of step c) in liquid form is fed to step d) of the process according to the invention. At least one fraction of said purified diester effluent may also be recycled to step a) of the process according to the invention for the manufacture of terephthalic polyesters.
[0084] Step d) of preparation of polymerization feedstock According to the invention, the process for producing terephthalic acid-based polyesters comprises a step d) of preparation of a polymerization feedstock, said step d) comprising at least one mixing section to which is fed at least one terephthalic acid feedstock and at least one fraction of the purified diester effluent obtained at the end of step c), in liquid form. Advantageously, said terephthalic acid feedstock is a terephthalic acid feedstock comprising terephthalic acid as the compound comprising terephthalic acid units, or a dimethyl terephthalate feedstock comprising dimethyl terephthalate as the compound comprising terephthalic acid units.
[0085] In one particular embodiment, where the terephthalic acid feedstock is a terephthalic acid feedstock comprising terephthalic acid, the polymerization feedstock obtained at the end of step d) is a homogeneous two-phase mixture comprising at least terephthalic acid, diester monomer and optionally diol (or glycol). The term "two-phase" is advantageously understood to mean a state in which a solid phase is suspended in a liquid or pasty phase. The term "homogeneous" should be understood to mean that the solid phase suspended in the liquid or pasty phase is homogeneously distributed throughout the liquid or pasty phase. More specifically, the polymerization feedstock in this embodiment is a mixture of solid terephthalic acid particles, typically with a diameter of 1 to 1000 μm, in particular 80 to 300 μm, homogeneously distributed in a liquid or pasty phase comprising the diester monomer.
[0086] In another particular embodiment, where the terephthalic acid feedstock is a dimethyl terephthalate feedstock comprising dimethyl terephthalate, the polymerization feedstock comprising at least dimethyl terephthalate, diester monomer, and optionally a diol (or glycol) feedstock is advantageously a single-phase mixture.
[0087] Advantageously, the amounts of terephthalic acid feedstock and purified diester effluent introduced into said mixing section are such that the amount of terephthalic acid feedstock and purified diester effluent introduced into said mixing section is greater than or equal to 100% by weight of the diester of formula -[C (n+1) H (2n+2)The ratio of the total number of moles of diol units of the formula -[CO-(C6H4)-CO]- (wherein n is an integer equal to or greater than 1, preferably between 1 and 5, preferentially between 1 and 3) to the total number of moles of terephthalic acid units of the formula -[CO-(C6H4)-CO]- introduced into said mixing section is adjusted to be between 1.0 and 2.0, preferably between 1.0 and 1.5, preferentially between 1.0 and 1.3.
[0088] According to one embodiment of the present invention, the mixing section of step d) of the method according to the present invention preferably contains a cyclohexane having the formula HO-C (n+1) H (2n+2) A diol monomer feedstock is further provided, comprising a diol monomer of the formula -OH, where n is an integer of 1 or more, preferably 1 to 5, more preferably 1 to 3. Preferably, the diol monomer feedstock comprises at least 90 mol %, preferentially at least 95 mol %, very preferably 98 mol % of the diol monomer to be incorporated into the composition of the individual units of the desired terephthalic acid-based polyester. Preferably, the diol monomer feedstock comprises ethylene glycol in a content of 90 mol % or more, at least 95 mol %, preferentially at least 98 mol %. The diol of the diol monomer feedstock may have a different or the same chemical structure, preferably the same chemical structure, as the diol monomer to be incorporated into the composition of the feedstock of the polyester to be regenerated in the depolymerization step a). Preferably, said diol monomer feedstock may at least in part be a fraction of the purified diol stream obtained in step g) of the process according to the invention and / or may be at least a partial fraction of the glycol effluent obtained at the end of step b) of the process according to the invention.
[0089] If a diol monomer feed is incorporated into the mixing section of step d), the amount of said diol feed introduced into the mixing section of step d) is adjusted so that the ratio of the number of diol units to the number of terephthalic acid units in the mixture of step d), as defined above, is between 1.0 and 2.0, preferably between 1.0 and 1.5, preferentially between 1.0 and 1.3.
[0090] Advantageously, the molecular weight of the diester monomers of the purified diester effluent introduced into the mixing section of step d) represents at least 5% by weight, preferably at least 15% by weight, relative to the weight of terephthalic acid (PTA) or dimethyl terephthalate (DMT).
[0091] To the extent that a diester monomer molecule contains two diol units and one terephthalic acid unit, a terephthalic acid or dimethyl terephthalate molecule contains one terephthalic acid unit, and a diol molecule contains one diol unit, it is possible to replace a portion of the terephthalic acid feedstock and all or some of the diol feedstock by incorporating one mole of a diester monomer, e.g., one mole of bis(2-hydroxyethyl) terephthalate (BHET), in a mixture with a terephthalic acid or dimethyl terephthalate monomer feedstock and a diol monomer feedstock, such as ethylene glycol.
[0092] Advantageously, the mixing of the terephthalic acid feedstock, at least one fraction of the purified diester effluent and optionally the diol monomer feedstock is carried out in any equipment known to the skilled artisan that allows effective mixing. In a particular embodiment in which the polymerization feedstock comprises terephthalic acid, step d) makes it possible to obtain a homogeneous distribution of suspended solids in a liquid mixture or paste. Preferably, the mixing of step d) of the process according to the invention is carried out in a mixer with mechanical stirring or it is stirred by recirculation of the liquid or of the mixture, for example by means of a pump that circulates the mixture in a loop.
[0093] The terephthalic acid feedstock, the purified diester effluent fraction, and optionally the diol monomer feedstock are introduced together or separately into a mixer.
[0094] Advantageously, said mixing section in step d) of the process according to the invention is operated at a temperature between 25° C. and 250° C., preferably between 60° C. and 200° C., preferably between 100° C. and 150° C., and at a pressure greater than or equal to 0.1 MPa. Very advantageously, the pressure in said mixing section is less than or equal to 5 MPa.
[0095] In addition, one or more polymerization catalysts may be incorporated into the mixture of step d) of the process according to the invention.
[0096] Other monomeric (or comonomer) compounds may advantageously be introduced into the mixture or may be found in the esterification feedstock. As non-limiting examples, said other monomeric compounds may be dicarboxylic acids, such as isophthalic acid, and diols, such as 1,4-dihydroxymethylcyclohexane and diethylene glycol.
[0097] According to one particular embodiment of the present invention, in which a terephthalic acid feedstock is used, the incorporation of a diester monomer, for example a BHET monomer, into the polymerization feedstock allows the replacement of part of the terephthalic acid, a compound in the form of a powder of solid particles, in the two-phase mixture of monomers for the production of polyesters. This replacement of part of the terephthalic acid and all or some of the diols with diester monomers in the process according to the present invention allows a significant reduction in the amount of diol, for example ethylene glycol, introduced into the mixture in excess, when compared to that of a conventional polyester production process, when the solid content of the two-phase mixture is the same, which leads not only to a reduction in costs, especially raw material costs, but also to a significant reduction in the energy consumption of the polyester production process. This is due to the reduction in the amount of diol recovered during polymerization that must be treated and recycled.
[0098] Condensation step e) According to the invention, the process for producing terephthalic acid-based polyesters comprises a step e) of condensation of the polymerization feedstock obtained at the end of step d), resulting in at least one condensation reaction effluent, one diol effluent and one aqueous or one methanol effluent. Said condensation step e) comprises at least one reaction section and at least one separation section.
[0099] In a particular embodiment, in which the terephthalic acid-based feedstock is a terephthalic acid feedstock, the reaction carried out in step e) advantageously comprises an esterification reaction consisting of a condensation reaction of at least hydroxyl groups (-OH) of the diester monomers of the purified diester effluent fraction resulting in step c) and at least partially incorporated in the polymerization feedstock in step d) and of the diol monomers optionally present in the polymerization feedstock with at least carboxyl groups (-COOH) of the terephthalic acid of the terephthalic acid feedstock incorporated in the polymerization feedstock in step d). This esterification reaction gives rise to molecules of diester monomers, for example bis(2-hydroxyethyl) terephthalate (BHET), and molecules of diester oligomers advantageously comprising 2 to 5 terephthalic acid units. The esterification reaction also liberates water. The reaction carried out in step e) of the process according to the invention also advantageously comprises a transesterification reaction consisting of a condensation reaction between molecules of diester monomers, thereby liberating diol molecules.
[0100] In another particular embodiment, where the terephthalic acid-based feedstock is a dimethyl terephthalate feedstock, the reaction carried out in step e) advantageously comprises a transesterification reaction consisting of a condensation reaction of at least hydroxyl groups (-OH) of the diester monomers of the purified diester effluent fraction resulting in step c) and at least partially incorporated in the polymerization feedstock in step d) and of the diol monomers optionally present in the polymerization feedstock with at least carboxylate (-COO-) groups of the dimethyl terephthalate of the dimethyl terephthalate feedstock incorporated in the polymerization feedstock in step d). This transesterification reaction gives rise to molecules of diester monomers, for example bis(2-hydroxyethyl) terephthalate (BHET), and molecules of diester oligomers advantageously comprising 2 to 5 terephthalic acid units. It also releases methanol. The reaction carried out in step e) of the process according to the invention also advantageously comprises a transesterification reaction consisting of a condensation reaction between molecules of diester monomers, thus releasing diol molecules.
[0101] Advantageously, the reaction section is operated in one or more reactors in series or parallel at a temperature between 150° C. and 400° C., preferably between 200° C. and 300° C., a pressure between 0.05 and 1 MPa, preferably between 0.1 and 0.3 MPa, and a residence time between 0.5 and 10 hours, preferably between 1 and 5 hours. According to the invention, the residence time in the esterification step d) is defined as the ratio of the reaction volume of the reactor of the reaction section to the volumetric flow rate of the liquid stream leaving said reactor.
[0102] Advantageously, in particular in the case of esterification reactions starting from a polymerization feedstock, polymerization catalysts known to those skilled in the art may be optionally introduced into the reaction section of the condensation step e), optionally in admixture with the diol stream. By way of non-limiting examples, polymerization catalysts are catalysts based on antimony, tin, germanium or aluminum, zinc acetate, calcium or manganese. In a particular embodiment in which the polymerization feedstock comprises a dimethyl terephthalate feedstock, transesterification catalysts known to those skilled in the art are optionally added to the reaction section of step e), advantageously in admixture with the diol stream.
[0103] The condensation reaction is advantageously carried out in one or more stirred reactors, one or more tubular reactors, or a combination of stirred and tubular reactors.
[0104] Advantageously, the reaction section also comprises the withdrawal of at least one withdrawn effluent rich in water or methanol and diol. The water or methanol and diol in said withdrawn effluent are separated in the separation section of step e), which is fed with said withdrawn effluent rich in water or methanol and diol, advantageously giving an aqueous or methanol effluent and a diol effluent. Advantageously, the water or methanol is separated by difference in volatility, for example by distillation or by adsorption starting from said withdrawn effluent which contains at least in part the released diol and water or methanol present in the reaction medium.
[0105] Advantageously, at least one fraction of said diol effluent obtained in step e) of the process according to the invention may be optionally sent to step g) for processing the diol or alternatively sent directly back to the reaction section of said step e).Preferably, said diol effluent obtained at the end of the separation section of step e) is sent directly back to the reaction section of said step e).
[0106] The condensation reaction effluent obtained at the end of step e), in particular at the outlet of the reactor section of step e), comprises diester monomers and ester oligomers. Preferably, the diester monomers in the condensation reaction effluent are of the same type as the diester monomers of the purified liquid diester effluent obtained in step c) and at least partially incorporated in the mixture of step d). Preferably, the ester oligomers in the condensation reaction effluent consist of basic units which advantageously correspond to the basic repeating units of the terephthalic polyesters targeted by the process according to the invention.
[0107] The incorporation of at least one fraction of the purified diester effluent into the monomer feed of the polymerization makes it possible to replace at least a portion of the terephthalic acid feed and all or a portion of the diol feed, thereby making it possible to reduce the amount of water or methanol discharged and therefore to limit the amount of aqueous or methanol effluent withdrawn from the reaction medium to be treated, which advantageously reduces energy consumption.
[0108] Polycondensation step f) According to the invention, the process for the preparation of terephthalic acid-based polyesters comprises a step f) of polycondensation of the condensation reaction effluent obtained in step e) to obtain at least said terephthalic acid-based polyesters and a diol effluent, which is at least partially fed to the mixing section of step d) of the process according to the invention by the addition of a diester monomer of the formula -[C (n+1) H (2n+2) O2]-, where n is an integer greater than or equal to 1, preferably between 1 and 5, and preferentially between 1 and 3.
[0109] The polycondensation step f) consists in carrying out a condensation reaction between the diester monomers and ester oligomers of the condensation reaction effluent obtained in step e), thereby obtaining a polyester having a given degree of polymerization and desired physicochemical properties (e.g. viscosity index, crystallinity, color, mechanical properties, etc.) Said condensation reaction releases diol compounds, optionally water or methanol, and by-products, which are recommended to be removed.
[0110] The polycondensation step f) comprises at least one reaction section comprising at least one reactor in which the polycondensation reaction takes place and at least one withdrawal of a diol effluent, the diol effluent comprising at least one diol monomer, advantageously the diol monomer being represented by the formula -[C (n+1) H (2n+2) O2]- (wherein n is an integer of 1 or more, preferably 1 to 5, and preferentially 1 to 3).
[0111] Advantageously, said reaction section of step f) is operated in one or more reactors, working in series or in parallel, at temperatures between 200°C and 400°C, preferably between 250°C and 300°C, at pressures between 0.0001 and 0.1 MPa, preferably between 0.0004 and 0.01 MPa, and with residence times between 0.1 and 5 hours, preferably between 0.5 and 3 hours. According to the invention, the residence time in said polycondensation step f) is defined as the ratio of the reaction volume of the reactor of said reaction section to the volumetric flow rate of the liquid stream leaving said reactor. The polycondensation reaction of step f) may be carried out in two successive reaction steps: a melt phase condensation step followed by a solid phase post-condensation step.
[0112] Advantageously, polymerization additives and polymerization catalysts can be introduced in the polycondensation step f). By way of non-limiting example, additives can include, for example, inhibitors of etherification side reactions, such as amines (n-butylamine, diisopropylamine or triethylamine), sodium hydroxide, organic hydroxides, lithium carbonate, stabilizers, such as phosphites or phosphates, and polyamide type compounds to reduce the amount of decomposition products, such as acetaldehyde. Commonly used polymerization catalysts are, for example, catalysts based on antimony, titanium, germanium or aluminum, zinc acetate, calcium or manganese, etc.
[0113] Advantageously, the withdrawal of said diol effluent is carried out using one or more withdrawal systems, advantageously connected to the reactor(s) of the reaction section of said stage f), which make it possible to separate the diol monomers released during the polycondensation reaction, the optional water or methanol and other by-products optionally released during the condensation reaction. Preferably, the diol effluent withdrawn from the reactor(s) of stage f) is withdrawn in gaseous form and is then cooled and condensed, advantageously to a temperature between 0 and 100° C., thereby obtaining a liquid diol effluent.
[0114] Preferably, at least one fraction of the liquid diol effluent is sent to step g) of the process according to the invention. At least one fraction of said liquid diol effluent may also be recycled directly to step d) of the preparation of the polymerization feedstock. In a very particular embodiment, said liquid diol effluent may be recycled completely or partially directly to the condensation step e).
[0115] Diol treatment process g) According to the invention, the process for the manufacture of terephthalic polyesters comprises a step g) of treating a diol comprising at least a recovery section to which all or part of the glycol effluent from step b) and all or part of the diol effluent from step f) are fed to obtain a diol stream to be treated, and a purification section of said diol stream to be treated to obtain a purified diol stream.
[0116] Said recovery section of step g) may further optionally be fed with at least one fraction of the diol effluent resulting from the condensation step e) and / or with externally supplemented diol.
[0117] Advantageously, the recovery section may include one or more filtration operations.
[0118] The diol stream to be treated obtained at the end of the recovery section of step g) is sent to the purification section of step g), thereby obtaining a purified diol stream.
[0119] The purification section comprises at least one separation system performing any of the physical, physicochemical or chemical separation methods known to the skilled person, such as, for example, gas / liquid separation, distillation or adsorption. Preferably, the purification of the diol effluent to be treated employs at least one distillation column, preferably a series of distillation columns, operated at a temperature between 50°C and 250°C, preferably between 70°C and 220°C, and at a pressure between 0.001 and 0.2 MPa, preferably between 0.01 and 0.1 MPa. Preferably, the purification section comprises a stage of separation of impurities lighter than the diol monomer in the diol stream to be treated and a stage of separation of impurities heavier than the diol monomer in the diol stream to be treated, preferably in a series of distillation columns.
[0120] Advantageously, said step g) may also comprise a section for removing volatile organic compounds by thermal or catalytic combustion of said compounds in order to prevent their emission into the environment. As a non-limiting example, said section for the treatment of impurities comprises filtration, if present, of solid particles, and catalytic or non-catalytic combustion systems.
[0121] Said purified diol stream obtained at the end of step g) of the process according to the invention may then be passed completely or partly to at least steps a) and d) of the process according to the invention.
[0122] The process according to the invention therefore makes it possible to obtain terephthalic acid-based polyesters, advantageously with the targeted degree of polymerization and the desired physicochemical properties, from polyester materials to be recycled, originating from the collection and sorting industry, while limiting the consumption of "fresh" raw materials and the overall energy consumption. A reduction in energy consumption is made possible, in particular thanks to an optimized recycle system of the diol(s), in particular the diols released during the polymerization and the unconverted diols possibly introduced into the mixture of monomers for the polymerization (i.e. the polymerization feedstock).
[0123] The process of the invention makes it possible, at the end of steps a), b) and c), to produce, very advantageously, a high purity intermediate stream, which contains a terephthalic acid diester (such as BHET) and meets the specifications required by the polymerization process for obtaining terephthalic acid-based polyesters. The liquid diester intermediate stream can be directly injected into the so-called polymerization process, in particular directly incorporated into the mixture of monomer feedstocks fed to the polymerization section, preferably replacing at least a portion of the monomer feedstock. The direct injection of the diester intermediate stream makes it possible to have a lower energy consumption than the combined depolymerization and polymerization processes. Preferably, the terephthalic acid diester is bis(2-hydroxyethyl) terephthalate (BHET), derived from the glycolysis of PET with ethylene glycol.
[0124] The method of the present invention makes it possible to recycle plastics that have been difficult to recycle up to now, such as opaque PET, thereby making it possible to meet environmental protection demands.
[0125] The following figures and examples are provided to illustrate the invention but are not intended to limit the scope of the invention.
[0126] Figure 1 shows one particular configuration of the process for producing polyethylene terephthalate (PET) according to the present invention, which integrates a scheme for depolymerizing, preferably by glycolysis, the PET feedstock to be recycled, and a scheme for polymerizing the intermediate purified BHET stream obtained by the depolymerization process, a mixture comprising terephthalic acid and monoethylene glycol diol (or ethylene glycol, MEG).
[0127] The glycolysis process of FIG. 1 comprises, in sequence, a depolymerization step a), followed by a separation step b), followed by a purification step c).
[0128] The depolymerization step a) is fed with at least the PET feedstock to be recycled (1) and the MEG feedstock (3c). Advantageously, the PET feedstock to be recycled is preheated and pressurized under the operating conditions of step a). Advantageously, at least 80% by weight, very advantageously at least 90% by weight and preferentially at least 95% by weight of the feedstock is introduced into step a) in liquid form. The temperature of the PET feedstock to be recycled is advantageously between 225°C and 275°C. The time required for introduction and the associated temperature are adjusted so that thermal degradation of the polyester is minimized.
[0129] Advantageously, said step a) comprises a screw conveying section, called extrusion section, to which the PET feedstock to be recycled is fed. The residence time in said extrusion section, defined as the volume of said section divided by the volumetric flow rate of the feedstock, is advantageously less than 15 minutes, preferably less than 10 minutes, more preferably less than 2 minutes. The extrusion section is advantageously connected to a vacuum extraction system, which removes impurities such as dissolved gases, light organic compounds and / or moisture present in the PET feedstock to be recycled. The extrusion section may also advantageously comprise a filtration system, which removes solid particles such as sand particles having a size of more than 40 μm, preferably between 3 and 40 μm.
[0130] The PET feedstock to be recycled is advantageously contacted with at least one fraction of the MEG effluent (3c) from step b) in said extrusion section, also called reactive extrusion section. The MEG stream (3c) may advantageously be superheated before being fed to step a), thereby facilitating the heating of the PET feedstock to be recycled. The number of moles of MEG from step b) per mole of diester in said PET feedstock to be recycled is advantageously less than or equal to 1.0, preferably less than or equal to 0.5.
[0131] Said step a) may also be advantageously fed with a fraction of effluent (5) coming from step c), comprising a mixture of unconverted oligomers and polyesters, preferentially purified in a filtration step.
[0132] The depolymerization step a) comprises a reaction section operated in one or more reactors at a temperature between 150°C and 400°C, preferably between 180°C and 300°C, more preferably between 200°C and 280°C, in liquid phase, with 1 to 20 moles of MEG per mole of diester in the feedstock of PET to be recycled, preferably between 3 to 15 moles per mole, more preferably between 5 to 10 moles per mole, with a residence time of 0.1 to 6 hours, preferably between 0.5 and 4 hours, and at an operating pressure of at least 0.1 MPa, preferentially at least 0.4 MPa. Preferably, the depolymerization step is carried out without the addition of a catalyst.
[0133] The glycolysis reaction allows the conversion of the PET feedstock to be recycled to give bis(2-hydroxyethyl) terephthalate (BHET) monomers and BHET oligomers. In the depolymerization step, the conversion of the PET feedstock to be recycled is greater than 50%, preferably greater than 70%, more preferably greater than 85%. The molar yield of BHET is greater than 50%, preferably greater than 70%, more preferably greater than 85%. The molar yield of BHET corresponds to the molar flow rate of BHET at the outlet of step a) relative to the molar flow rate of diester units in the PET feedstock to be recycled (1).
[0134] An internal recirculation loop is advantageously also used in step a), which comprises the withdrawal of a fraction of the reaction system (i.e. all the components and phases present in said reaction section), filtering this fraction and reinjecting said fraction into said step a). This internal recirculation loop advantageously makes it possible to remove solid impurities possibly present in the reaction liquid.
[0135] The reaction effluent (2) coming from the depolymerization step a) is fed to a step b) of separation of MEG, which is operated at a pressure lower than that of step a) in order to vaporize a fraction of the reaction effluent (2) giving at least one gaseous MEG effluent containing more than 50% by weight, preferably more than 70% by weight, more preferably more than 90% by weight of MEG, and a liquid effluent enriched in the BHET monomer (4).
[0136] Step b) advantageously comprises a series of gas / liquid separations, advantageously from 1 to 5, very advantageously from 3 to 5 successive gas / liquid separations, which are carried out at temperatures between 100° C. and 250° C., preferably between 110° C. and 220° C., more preferably between 120° C. and 210° C. The liquid effluent from the preceding separator is fed to the subsequent separator. The liquid effluent from the final gas / liquid separation constitutes the liquid effluent (4) enriched in BHET monomer. At least one fraction of the gaseous MEG effluent recovered is condensed to give a liquid MEG effluent.
[0137] The temperature and pressure of the subsequent separator are lower than those of the preceding separator, such that at least a portion of the gaseous MEG effluent from the preceding separation can, upon condensation, reboil a portion of the liquid effluent from the subsequent separation. In this configuration, the heat input for MEG recovery is minimized.
[0138] Step b) is carried out in such a way that the temperature of the liquid effluent is maintained above the precipitation temperature of the BHET monomer and below a high value above which, depending on the diol / monomer molar ratio, the BHET monomer repolymerizes to a significant extent. The temperature in the gas / liquid separation section of step b) is between 100°C and 250°C, preferably between 110°C and 220°C, more preferably between 120°C and 210°C. The pressure in the gas / liquid separator of step b) is adjusted to allow evaporation of the MEG and of impurities possibly present in the reaction effluent (2) at a temperature which minimizes repolymerization and allows optimal energy integration. It is generally between 0.00001 and 0.2 MPa, preferably between 0.00004 and 0.15 MPa, preferably between 0.00004 and 0.1 MPa.
[0139] The gaseous and liquid MEG effluents resulting from the gas / liquid separation may contain other compounds such as dyes, light alcohols, water, diethylene glycol, etc. Step b) advantageously comprises one or more sections for fractionating all or part of the gaseous and liquid MEG effluents, thereby giving at least a light impurity-rich effluent (3a), a heavy impurity-rich effluent impurities (3b) and a MEG effluent (3c). The above sections are operated at temperatures between 50°C and 250°C, preferably between 60°C and 210°C, more preferably between 70°C and 180°C, and at pressures between 0.00001 and 0.2 MPa, preferably between 0.00004 and 0.15 MPa, more preferably between 0.00004 and 0.1 MPa. Preferably, the fractionation of the gaseous and liquid MEG effluents is carried out in a distillation column, a stripping column or a rectification column. Advantageously, all or part of the MEG effluent may be treated in a pre-purification step, upstream or downstream of the fractionation section, to remove dyes, for example via adsorption onto a solid (e.g. activated carbon).
[0140] The MEG effluent (3c) advantageously contains more than 99% by weight of MEG, preferably more than 99.5% by weight of MEG. All or part of the MEG effluent (3c) is advantageously recycled to step a), in admixture with at least one fraction of the purified MEG effluent originating from recovery step g) of the polymerization process.
[0141] The effluent enriched in light impurities (3a) and the effluent enriched in heavy impurities (3b) are advantageously sent to a recovery step g) of the polymerization process.
[0142] The liquid effluent (4) rich in BHET monomer is fed to a purification step c), which comprises one or more sections for the separation of the liquid effluent (4) rich in BHET monomer, thereby giving a liquid effluent (5) rich in heavy impurities and a pre-purified BHET effluent, which section is operated at a temperature below 250°C, preferably below 230°C, very preferably below 200°C, at a pressure below 0.001 MPa, preferably below 0.0001 MPa, preferably below 0.00005 MPa and with a residence time below 10 minutes, preferably below 5 minutes, more preferably below 1 minute.
[0143] The liquid effluent (5) enriched in heavy impurities is advantageously enriched in oligomers, unconverted PET, and heavy impurities, in particular pigments, other polymers possibly present, and the polymerization catalyst. The operating conditions for the separation in said step c) are adjusted so as to minimize the loss of BHET monomer by repolymerization. Some oligomers may be entrained together with the monomer in the prepurified gaseous BHET effluent.
[0144] The separation of said pre-purified BHET effluent is advantageously carried out in a falling film or thin film evaporation system or by short-stage distillation of a falling film or thin film or by short-stage distillation and / or evaporation of several falling films in a series. Very low operating pressures are necessary to make it possible to carry out said separation at temperatures below 250° C., preferably below 230° C., whilst still allowing the evaporation of the monomers.
[0145] The fraction of said effluent enriched in heavy impurities (5) may advantageously be recycled to the depolymerization step a) in order to improve the BHET yield of the depolymerization process.
[0146] Said heavy impurities effluent (5) is advantageously subjected to at least one purification step, preferably a filtration step, before it is recycled, which reduces the amount of pigments and / or other solid impurities. All or part of said heavy impurities effluent (5) may advantageously be withdrawn from the process or sent to an incineration system or a pigment recovery system.
[0147] A fraction of the MEG effluent (3c), a fraction of the purified MEG effluent (15) coming from step g), or a mixture of the fractions of said two effluents may advantageously be mixed with the effluent (5) enriched in heavy impurities coming from step c), thereby reducing the viscosity of said heavy impurity effluent and facilitating its transport to step a) and its optional treatment in an optional filtration step.
[0148] Step c) comprises one or more sections for decolorization of the pre-purified BHET effluent, which are operated at a temperature between 100°C and 250°C, preferably between 110°C and 200°C, more preferably between 120°C and 180°C, and at a pressure between 0.1 and 1.0 MPa, preferably between 0.2 and 0.8 MPa, more preferably between 0.3 and 0.5 MPa, in the presence of an adsorbent to give a purified BHET effluent (6). The adsorbent may be any adsorbent known to the person skilled in the art capable of capturing dyes, for example activated carbon or clay, advantageously activated carbon.
[0149] The pre-purified BHET effluent is advantageously mixed with a fraction of the MEG effluent (3c) resulting from step b) or alternatively with a fraction of the purified MEG effluent resulting from step g).
[0150] The purified BHET effluent (6) obtained at the end of step c) of the depolymerization process advantageously contains more than 50 mol %, preferably more than 60 mol %, more preferably more than 70 mol % of MEG.
[0151] The purified BHET effluent (6) is advantageously fed to a feed preparation step d) in which it is mixed with at least one terephthalic acid feedstock (7), optionally with a portion of the MEG effluent (15) originating from step g) and optionally with a comonomer (8).
[0152] The feedstock preparation step d) is preferably carried out at a temperature above 80°C, more preferably above 110°C.
[0153] If the depolymerization unit is attached to a pre-existing polymerization unit, the amount of BHET monomer originating from the purified BHET effluent (6) may advantageously represent less than 30 mol %, preferably less than 25 mol %, preferably less than 20 mol % of the total amount of aromatic monomers, including terephthalic acid, BHET, in the mixture prepared in step d) of the polymerization process, which makes it possible to ensure optimal integration by minimizing the investments in the depolymerization unit and the improvements made to the polymerization unit.
[0154] The polymerization process also comprises at least an esterification step e), a polycondensation step f) and a step g) for recovery and purification of the MEG effluent.
[0155] The polymerization process is preferably a process that is already in operation, i.e. already in operation with PTA and MEG monomers and optional comonomers feedstocks prior to the integration of the process for depolymerization of the PET to be recycled. In said particular configuration of the process according to the invention, the integration of the depolymerization process allows the incorporation of the PET to be recycled into virgin PET without any effect on the properties of the final PET produced. This is made possible by the optimal integration of the depolymerization process with steps d), e) and g) of the polymerization process, as well as by the performance and reduced energy consumption of the depolymerization process, with minimal impact on the configuration of the polymerization process and energy consumption.
[0156] The esterification step e) is fed with the mixture (9) from step d). The esterification reaction comprises a reaction section in one or more reactors operated at a temperature between 150° C. and 400° C., preferably between 200° C. and 300° C., at a pressure between 0.05 and 1 MPa, preferably between 0.1 and 0.3 MPa, and with a residence time between 1 and 10 hours, preferably between 1.5 and 5 hours.
[0157] The water produced by the esterification reaction is advantageously separated by at least one water separation system in step e), preferably by distillation, thereby generating an aqueous stream (10).
[0158] The reaction effluent (11) is then fed to a polycondensation step f) advantageously fed with a polymerization catalyst and an additive (14), preferably in admixture with a fraction of the purified MEG effluent (15) coming from step g).
[0159] The polycondensation step f) comprises at least one reaction section for generating a polyester stream (12) and at least one withdrawal making it possible to separate at least one effluent (13) containing MEG, water and other by-products released during the condensation reaction, said effluent (13) being advantageously sent to step g) for recovery and purification of the MEG effluent.
[0160] The reaction section of the polycondensation step f) comprises one or more reactors and is operated at a temperature between 200°C and 400°C, preferably between 250°C and 300°C, at a pressure between 0.0001 and 0.1 MPa, preferably between 0.0004 and 0.01 MPa, with a residence time between 0.1 and 5 hours, preferably between 0.5 and 3 hours.
[0161] Step g) for recovery and purification of the MEG effluents advantageously recovers the effluent (13) coming from step f) of the polymerization process and the effluents (3a) and (3b) coming from step b) of the depolymerization process.
[0162] Said step g) comprises one or more separation sections, preferably one section for the separation of impurities lighter than MEG and one section for the separation of impurities heavier than MEG.Preferably, the purification of the MEG effluent is performed by a series of two distillation columns operated at a temperature between 50°C and 250°C, preferably between 70°C and 220°C, and at a pressure between 0.001 and 0.2 MPa, preferably between 0.01 and 0.1 MPa.
[0163] The light impurity-rich effluent (3a) is advantageously mixed with the effluent (13) and then sent to a first distillation column, which makes it possible to separate the light impurities (16), in particular water, from the MEG effluent, which is then advantageously sent in admixture with the heavy impurity-rich effluent (3b) to a second distillation column, which recovers a purified MEG effluent (15) and an effluent of heavy impurities (17).
[0164] By carrying out a depolymerization process which minimizes the formation of light and heavy impurities, and advantageously carrying out a prior fractionation in step b) of said depolymerization process, it is possible to feed the separation column of step g) of the polymerization process with minimal impact on the initial composition of the polymerization process.
[0165] Working Example
[0166] Example 1 - Comparative Example Production of virgin PET in the PET polymerization process 5.5 t / h of terephthalic acid (PTA) were introduced into a mixing vessel equipped with mechanical stirring and mixed with a stream of 2.5 t / h of monoethylene glycol (MEG) at 110° C. This stream contained 2.13 t / h of MEG coming from a storage tank and 0.37 t / h of recycled MEG coming from a section for the purification of MEG.
[0167] The amounts of PTA and MEG introduced corresponded to a PTA / MEG molar ratio of 1.23.
[0168] The solids by volume, defined as the ratio of solid volume to the total volume of the paste (solids + liquids) at 110° C., was 60.7% by volume. The resulting mixture formed a viscous paste.
[0169] The resulting mixture was then transferred using a suitable pump to a first esterification reactor operated at 260° C., 5 bar (ie, 0.5 MPa) with a residence time of 1.25 hours.
[0170] 1.4 t / h of a vapor effluent containing 71% by weight of water and 29% by weight of MEG was withdrawn and sent to a reflux tower, which separated the water and MEG produced by the esterification reaction. The MEG was then returned to the reactor. The conversion of PTA obtained in the first reactor was 85%.
[0171] The liquid effluent from the first reactor was then sent to a second esterification reactor operated at 260° C., 2 bar (i.e., 0.2 MPa) with a residence time of 1.25 hours. A vapor effluent of 140 kg / h containing 40 wt. % water and 60 wt. % MEG was withdrawn from the second reactor and sent to a reflux tower. The conversion of PTA at the outlet of the second reactor reached 92%.
[0172] The liquid effluent from the second esterification reactor was sent to a third reactor operated at 275 ° C, 33 mbar (i.e. 0.033 MPa) and a residence time of 0.5 hours. This made it possible to start the polycondensation with a PTA conversion of 95.8%. At the inlet of the third reactor, antimony trioxide was added as a polymerization catalyst in a proportion of 220 ppm by weight. A vapor effluent containing 70% by weight of MEG, 16.5% by weight of water, 5.5% by weight of acetaldehyde, 2.5% by weight of diethylene glycol and 5.5% by weight of oligomers was withdrawn from the third reactor, partially condensed and then sent to a section for the purification of MEG.
[0173] The liquid effluent from the third reactor was sent to a fourth reactor (polycondensation reactor) operated at 275° C., 66 mbar (i.e., 0.0066 MPa) with a residence time of 0.5. A vapor effluent with a composition of 60% by weight MEG, 25% by weight water, 6% by weight acetaldehyde, 3% by weight diethylene glycol, and 6% by weight oligomers was withdrawn from the fourth reactor, partially condensed, and then sent to a section for purification of MEG.
[0174] The liquid effluent from the fourth reactor was sent to the final reactor (polycondensation reactor) operated at 280° C., 1.3 mbar (i.e. 0.000013 MPa) with a residence time of 1 hour. The vapor effluent, with a composition of 57% by weight MEG and 43% by weight water, was withdrawn, partially condensed and then sent to a section for purification of MEG.
[0175] The section for the purification of MEG included a first distillation column with 25 plates, operated at 145° C. and 200 mbar (i.e. 0.02 MPa) at the top. This made it possible to separate diethylene glycol. The bottom product from the first distillation column was sent to a second distillation column with 17 plates, operated at 100° C. and 1 bar (i.e. 0.1 MPa) at the top. This made it possible to separate light components (water, acetaldehyde, etc.). The MEG recovered at the end of these two distillations had a purity of more than 99.8%. This MEG was then recycled to the mixing vessel.
[0176] 6.25t / hour of PET was produced. The total primary energy consumption for PET production was 5.8MMkcal / hour.
[0177] Preparation of decolorized and depigmented solid BHET and incorporation of at least one fraction in a PET polymerization process
[0178] 4 t / h of flakes from a ground and washed PET feedstock to be recycled, consisting of 50 wt.% opaque PET and 50 wt.% colored PET, were melted in an extruder at 250°C and mixed with 11.4 t / h of ethylene glycol (MEG). The resulting mixture was injected into a stirred reactor and maintained at 220°C and a pressure of 4 bar (i.e., 0.4 MPa) for a residence time of 4 hours. At the reactor outlet, the reaction effluent contained 66 wt.% MEG, 27.4 wt.% BHET, 1.7 wt.% diethylene glycol (DEG), 0.2 wt.% water, 4.7 wt.% oligomers, pigments, and other heavy compounds.
[0179] The ethylene glycol present in the reaction effluent was separated by evaporation in a series of five vessels at temperatures ranging from 200° C. to 124° C. and pressures ranging from 0.1 MPa to 0.00025 MPa. At the end of this evaporation process, a MEG stream of 10.95 t / h and a BHET-rich liquid stream of 5.17 t / h were recovered, consisting of 97 wt. % MEG, 2.5 wt. % DEG, 0.2 wt. % water, and 0.2 wt. % BHET. The MEG stream was sent to a first distillation column with 25 plates and operated at 145°C and 200 mbar (i.e., 0.02 Mpa) at the top, which separated the DEG and heavy products, and then to a second distillation column with 17 plates and operated at 100°C and 1 bar (i.e., 0.1 MPa) at the top, which separated the water and recovered the purified MEG effluent. This MEG effluent was then recycled to the depolymerization reactor as a mixture with supplemented fresh MEG. The BHET-rich liquid stream contained 87.1 wt% BHET, 0.2 wt% MEG, 0.1 wt% DEG, 12.6 wt% oligomers, pigments, and other heavy compounds.
[0180] The BHET-rich liquid stream was then injected into the short-stage distillation at a temperature of 205° C. and a pressure of 0.2 mbar (i.e., 0.00002 MPa). The pre-purified liquid BHET effluent with a flow rate of 4.46 t / h was recovered by cooling the vapors to 115° C. in the short-stage distillation. It contained 99.8 wt. % BHET, 0.1 wt. % MEG, and 0.1 wt. % DEG. A heavy residue containing 93 wt. % oligomers, pigments, and other heavy compounds and 7 wt. % BHET was also recovered at the outlet of the short-stage distillation with a flow rate of 0.7 t / h.
[0181] The liquid stream of pre-purified BHET was compressed to 0.5 MPa, heated to 150°C, and then fed to a fixed bed of activated carbon with an adsorption capacity equal to 5% of its weight. At the end of this process, the liquid stream of decolorized and depigmented BHET was recovered. It was then cooled and solidified at 40°C.
[0182] The total primary energy consumption for depolymerization was 1.25 MMkcal per ton of BHET.
[0183] The decolorized and depigmented fraction of solid BHET was reinjected into a process for preparing a mixture of monomers for a PET polymerization process similar to the polymerization process described above, with the aim of producing a total of 6.25 t / h of PET. The PET polymerization process was identical to the polymerization process described above. The depolymerization and polymerization steps are completely separate and not integrated.
[0184] In the following Table 1, the amounts of PTA and MEG monomers, the amount of solid BHET monomer incorporated, the solids content in the feed mixture obtained at 110 °C, the ratio of the number of diol units to the number of terephthalic acid units, and the total primary energy consumption are reported for two ratios of diol units to terephthalic acid units (1.23 and 1.1) for the production of 6.25 t / h of PET, taking into account the incorporation of BHET resulting from the depolymerization method described above. The results shown in the table are calculated results for different MEG incorporation amounts, where 1 mole of BHET is considered to replace 1 mole of PTA and 2 moles of MEG in the mixture, and are based on a process simulation integrating solubility data and thermodynamic data set at experimental points.
[0185] [Table 1]
[0186] Example 2 - In accordance with the present invention
[0187] Integrating the depolymerization and polymerization processes to produce PET that incorporates the PET to be recycled
[0188] 1.56 t / h of flakes from a ground and washed feedstock of PET to be recycled, consisting of 50 wt.% opaque PET and 50 wt.% colored PET, were melted in an extruder at 250°C and mixed with 4.68 t / h of ethylene glycol (MEG). The mixture was then injected into a stirred reactor at 220°C and a pressure of 4 bar (i.e. 0.4 MPa). The residence time was set to 4 hours. At the reactor outlet, the reaction effluent contained 66 wt.% MEG, 27.4 wt.% BHET, 1.7 wt.% DEG, 0.2 wt.% water, 4.7 wt.% oligomers, pigments, and other heavy compounds.
[0189] The ethylene glycol present in the reaction effluent was separated by evaporation in a series of five vessels at temperatures ranging from 200°C to 124°C and pressures ranging from 0.1 Mpa to 0.00025 Mpa, then sent to a stripping column and a rectification column.
[0190] At the end of this separation step, a MEG-rich stream (containing 97% by weight of MEG) and a BHET-rich liquid stream of 1.76 t / h were recovered. The MEG-rich stream was fractionated: one part was directly recycled to the depolymerization and monomer preparation steps upstream of the esterification step, and another part was sent to the section for purification of MEG (described below). The BHET-rich liquid stream contained 87.1% by weight of BHET, 0.2% by weight of MEG, 0.1% by weight of DEG, 12.6% by weight of oligomers, pigments, and other heavy compounds.
[0191] The BHET-rich liquid stream was then injected into the short-stage distillation at a temperature of 205° C. and a pressure of 0.2 mbar (i.e. 0.00002 MPa). A pre-purified BHET liquid effluent with a flow rate of 1.74 t / h was recovered by cooling the vapors to 115° C. in the short-stage distillation. It contained 99.8 wt. % BHET, 0.1 wt. % MEG, and 0.1 wt. % DEG. A heavy residue with a flow rate of 0.27 t / h was also recovered at the outlet of the short-stage distillation: it contained 93 wt. % oligomers, pigments, other heavy compounds, and 7 wt. % BHET.
[0192] The pre-purified BHET liquid stream was compressed to 0.5 MPa, heated to 150° C., and then fed to a fixed bed of activated carbon with an adsorption capacity equal to 5% of its weight. At the end of this step, a decolorized and depigmented BHET liquid stream was obtained at a temperature of about 150° C. This decolorized and depigmented BHET liquid stream was sent directly to the monomer preparation step of the polymerization process.
[0193] The decolorized and depigmented BHET liquid stream was mixed in a mixing vessel equipped with mechanical stirring at 110° C. with the following: - 4.36 t / h of terephthalic acid (PTA) and 1.65 t / h of monoethylene glycol (MEG) (Example 2a), or - 4.36 t / h of terephthalic acid (PTA) and 1.39 t / h of monoethylene glycol (MEG) (example 2b).
[0194] The mixture obtained in the form of a paste was then sent to the esterification and polycondensation steps as described in Example 1.
[0195] The MEG-rich condensate from the polycondensation section was sent to the MEG purification section, which was similar to that described in Example 1. The MEG recovered at the end of the MEG purification section had a purity of more than 99.8%.
[0196] Table 2 reports the amounts of PTA and fresh MEG monomer, the amount of PET monomer to be recycled, the solids obtained at the end of the step of preparing the monomer feedstock, the ratio of the number of diol units to the number of terephthalic acid units in said step, as well as the total primary energy consumption for the integrated process, for the production of 6.25 t / h of PET. The results shown in the table are calculated results, where 1 mole of BHET is considered to replace 1 mole of PTA and 2 moles of MEG in the mixture, and are based on a process simulation integrating solubility data and thermodynamic data set at experimental points.
[0197] [Table 2]
[0198] It seems clear that the overall process integrating the depolymerization and polymerization steps reduces the energy consumption compared to the total energy consumption of the non-integrated depolymerization and polymerization processes, assuming a comparable ratio of the number of diol units to the number of terephthalic acid units introduced in the process of preparing the polymerization feedstock (monomer preparation process): - When the diol units / terephthalic acid units ratio is 1.23: 0.48 MMkcal / hour (i.e., about 6%) reduction; - Diol units / terephthalic acid units = 1.1: 0.51 MMkcal / hr (i.e., approximately 7%) reduction.
Claims
1. 1. A process for producing terephthalic acid-based polyester from at least one feedstock of polyester to be recycled, the feedstock comprising at least 10% by weight of opaque PET, the process comprising at least the following steps: a) a depolymerization step of said feedstock of polyester to be recycled, said depolymerization step comprising at least one reaction section to which said feedstock of polyester to be recycled and a glycol feedstock are fed, said glycol feedstock comprising at least a fraction of a purified diol stream, said reaction section being operated at a temperature of from 150° C. to 400° C., a pressure of at least 0.1 MPa and a residence time per reactor of from 0.05 to 10 hours, thereby obtaining a depolymerization reaction effluent; b) a separation step comprising at least one separation section to which the depolymerization reaction effluent obtained at the end of the depolymerization step a) is fed, whereby at least one glycol effluent and one diester effluent are obtained; c) a purification step of the diester effluent obtained at the end of step b), comprising at least one separation section to which the diester effluent obtained at the end of step b) is fed and which is operated at a temperature of at most 250° C., at a pressure of at most 0.001 MPa and with a liquid residence time per section of at most 10 minutes, followed by a decolorization section in the presence of an adsorbent and operated at a temperature between 100° C. and 250° C. and at a pressure between 0.1 and 1.0 MPa, thereby obtaining a purified liquid diester effluent comprising at least bis(2-hydroxyethyl) terephthalate (BHET); d) a process for preparing a polymerization feedstock, comprising at least one mixing section to which is fed at least one terephthalic acid feedstock comprising terephthalic acid or dimethyl terephthalate, at least one fraction of the purified liquid diester effluent obtained in step c) and a diol monomer feedstock, the fraction of which is at least in part a purified diol stream, wherein the amount of at least the terephthalic acid feedstock and the fraction of the purified liquid diester effluent introduced into the mixing section is a diol monomer feedstock having a molecular weight of at least 1000, preferably at least 1000, more ... (n+1) H (2n+2) O 2 ]- (wherein n is an integer equal to or greater than 1) is introduced into the mixing section. 6 H 4 a ratio of moles of terephthalic acid units of 1.0 to 2.0, said mixing section being operated at a temperature of 100° C. to 150° C. and a pressure of 0.1 MPa or more; e) a condensation step of said polymerization feedstock from step d) to produce at least one condensation reaction effluent, one diol effluent, and one aqueous or one methanol effluent, said condensation step comprising at least one reaction section operated at a temperature of 150° C. to 400° C., a pressure of 0.05 to 1 MPa, and a residence time of 0.5 to 10 hours, and at least one separation section; f) a polycondensation step of the condensation reaction effluent obtained in step e) to obtain at least the terephthalic acid-based polyester and a diol effluent, the polycondensation step comprising at least one reaction section, the reaction section comprising at least one reactor in which polycondensation takes place, operated at a temperature between 200° C. and 400° C., a pressure between 0.0001 and 0.1 MPa and a residence time between 0.1 and 5 hours, the reaction section also comprising at least one withdrawal of the diol effluent; g) a diol treatment step comprising at least a recovery section to which all or part of the glycol effluent from step b) and all or part of the diol effluent from step f) are fed in order to obtain a diol stream to be treated, and a purification section of said diol stream to be treated in order to obtain a purified diol stream which is sent completely or partially to at least step a) or d), A manufacturing method comprising:
2. 10. The process of claim 1, wherein the feedstock of polyester to be recycled comprises at least 15% by weight of opaque PET.
3. 3. The process according to claim 1 or 2, wherein the feedstock of polyester to be recycled contains from 0.1% to 10% by weight of pigment.
4. 4. The process according to claim 1, wherein the reaction section of step a) is supplied with the feedstock of polyester to be recycled and the glycol feedstock, and the amount of glycol compound contained in the glycol feedstock is such that at the inlet of the reaction section, the amount of glycol compound corresponds to 1 to 20 moles of glycol compound per mole of polyester basic repeat unit contained in the feedstock of polyester to be recycled.
5. A method as described in claim 4, wherein the amount of glycol compound contained in the glycol feedstock at the inlet of the reaction section corresponds to 3 to 10 moles of glycol compound per mole of basic repeating unit of polyester contained in the feedstock of the polyester to be recycled.
6. A process described in any one of claims 1 to 5, wherein the reaction section of step a) is operated at a temperature of 200°C to 280°C.
7. A method for producing a product described in any one of claims 1 to 6, wherein the reaction section of step a) is operated at a pressure of at least 0.4 MPa.
8. The process according to any one of claims 1 to 7, wherein the separation section of step b) comprises a series of 1 to 5 gas-liquid separations carried out at a temperature between 100°C and 250°C and a pressure between 0.00001 and 0.2 MPa.
9. 9. The process according to claim 1 , wherein the separation section of purification step c) uses a falling film or thin film evaporation system by short falling film or thin film distillation or a series of several falling film or thin film short distillations and / or evaporations at a temperature of not more than 250° C. and a pressure of not more than 0.001 MPa.
10. A manufacturing method described in any one of claims 1 to 9, wherein the system of the separation section in the purification step c) is at a temperature of not more than 200°C and a pressure of not more than 0.0001 MPa.
11. The process according to any one of claims 1 to 10, wherein the adsorbent in the decolorization section of step c) is activated carbon.
12. A method for producing a polyester resin according to any one of claims 1 to 11, wherein the ratio of the total number of moles of diol units introduced into the mixing section to the total number of moles of terephthalic acid units introduced into the mixing section is 1.0 to 1.
5.
13. A method for producing a polyester resin described in any one of claims 1 to 12, wherein the ratio of the total number of moles of diol units introduced into the mixing section to the total number of moles of terephthalic acid units introduced into the mixing section is 1.0 to 1.3.
Citation Information
Patent Citations
Process including glycolysis and subsequent purification for recycling polyester materials
EP0865464A1
METHODS FOR THE PREPARATION OR PURIFICATION OF BIS-$g(b)-HYDROXYETHYL TEREPHTHALATE
EP1120394A1
Process for the depolymerization of a polyester comprising opaque polyethylene terephthalate
FR3053691A1
Production of polyester resin
JP1999217429A
Chemical recycling methods for polyethylene terephthalate waste
JP3715812B2