Positive electrode slurry, positive electrode, secondary battery, and method for producing positive electrode

By using a compound with a polyether group and an acidic group in the positive electrode slurry, the coating process is simplified, reducing stringiness and manufacturing costs, and improving productivity and reliability of positive electrodes.

JP7565539B2Active Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020562971
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-28
Filing Date
2019-11-29
Publication Date
2024-10-11
Estimated Expiration
2039-11-29

AI Technical Summary

Technical Problem

Existing positive electrode coating devices require a separate vibration generator, complicating operations and increasing manufacturing costs, especially when scaling up or increasing coating speed.

Method used

Incorporating a compound with a polyether group and an acidic group in the positive electrode slurry to suppress stringiness at the coating end, eliminating the need for a vibration generator and simplifying the coating process.

Benefits of technology

This approach reduces stringiness, enhances productivity, and lowers manufacturing costs while maintaining electrode reliability, allowing for easier scaling and increased coating speeds without additional equipment complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565539000002
    Figure 0007565539000002
  • Figure 0007565539000003
    Figure 0007565539000003
  • Figure 0007565539000004
    Figure 0007565539000004
Patent Text Reader

Abstract

The positive electrode slurry includes a positive electrode mixture and a dispersion medium for dispersing the positive electrode mixture. The positive electrode mixture includes a positive electrode active material, a conductive agent, a binder, and an additive. The additive includes a compound having a polyether group and an acidic group in the molecule.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a positive electrode slurry, a positive electrode, a secondary battery, and a method for producing a positive electrode. [Background technology]

[0002] A secondary battery, such as a lithium-ion secondary battery, includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode usually includes a current collector sheet and a positive electrode mixture layer supported on the current collector sheet. The positive electrode mixture layer is formed by applying a positive electrode slurry to the surface of the current collector sheet and drying it. The positive electrode slurry includes a positive electrode mixture including a positive electrode active material and the like, and a dispersion medium for dispersing the positive electrode mixture.

[0003] Incidentally, Patent Document 1 discloses a coating device in which a vibration generator is attached to the lip tip of a coating head. The vibration generator transmits vibration to the lip tip, thereby improving the drainage of the coating liquid discharged from the lip tip to the workpiece, and suppressing stringiness at the end of the coating on the workpiece. The coating device described in Patent Document 1 can be used to coat a positive electrode slurry on a current collecting sheet. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-176824 A Summary of the Invention

[0005] However, the applicator described in Patent Document 1 requires a separate vibration generator to be attached, which complicates the applicator. The operation of the applicator also becomes complicated. For example, operations such as turning on and off the vibration generation, adjusting the vibration magnitude, and adjusting the timing of vibration generation are required. Therefore, it is difficult to improve the productivity of the positive electrode and reduce the manufacturing cost. In particular, when the applicator is enlarged or the application speed is increased, a special vibration generator must be used, which tends to increase the manufacturing cost of the positive electrode.

[0006] Therefore, an object of the present disclosure is to provide a positive electrode slurry that can suppress stringing at the coating end portion compared to conventional positive electrode slurries.

[0007] In view of the above, a first aspect of the present disclosure relates to a positive electrode slurry including a positive electrode mixture and a dispersion medium for dispersing the positive electrode mixture, the positive electrode mixture including a positive electrode active material, a conductive agent, a binder, and an additive, and the additive including a compound having a polyether group and an acidic group in the molecule.

[0008] A second aspect of the present disclosure relates to a positive electrode comprising: a current collecting sheet; and a positive electrode mixture layer supported on the current collecting sheet, the positive electrode mixture layer being formed using the positive electrode slurry of the first aspect of the present disclosure.

[0009] A third aspect of the present disclosure relates to a secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, the positive electrode being the positive electrode of the second aspect of the present disclosure.

[0010] A fourth aspect of the present disclosure relates to a method for producing a positive electrode, the method including: a first step of preparing the positive electrode slurry of the first aspect of the present disclosure; and a second step of applying the positive electrode slurry to a surface of the current collecting sheet, followed by drying to form a positive electrode mixture layer.

[0011] According to the present disclosure, it is possible to provide a positive electrode slurry that can suppress stringiness at the coating end portion. [Brief description of the drawings]

[0012] [Figure 1] FIG. 4 is a schematic diagram showing a main part of an example of a step of applying a positive electrode slurry. [Diagram 2] FIG. 4 is a schematic diagram showing a state in which a positive electrode slurry is applied to a surface of a current collecting sheet. [Diagram 3] FIG. 1 is a schematic perspective view of a secondary battery according to an embodiment of the present disclosure, with a portion cut away. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [Positive electrode slurry] The positive electrode slurry according to the embodiment of the present disclosure includes a positive electrode mixture and a dispersion medium for dispersing the positive electrode mixture, and the positive electrode mixture includes a positive electrode active material, a conductive agent, a binder, and an additive. The additive includes a compound having a polyether group and an acidic group in the molecule (hereinafter referred to as compound A).

[0014] Here, Fig. 1 is a schematic diagram of a main part showing an example of a positive electrode slurry coating process. Fig. 1 shows a main part of an intermittent coating process using a positive electrode slurry 14. Fig. 2 is a schematic diagram showing a state in which the positive electrode slurry is coated on the surface of a current collector sheet. Arrow X in Figs. 1 and 2 indicates the conveyance direction of current collector sheet 12.

[0015] While the roll 11 is rotated to transport the strip-shaped current collecting sheet 12 in the X direction, the positive electrode slurry 14 is intermittently discharged from the coating head 13 of the coating device onto the current collecting sheet 12. Discharge of the positive electrode slurry 14 from the coating head 13 is started at the coating start end P1, and discharge of the positive electrode slurry 14 from the coating head 13 is stopped at the coating end P2. In this manner, the positive electrode slurry 14 is intermittently applied onto the current collecting sheet 12. As a result, as shown in FIG. 2, a coating film 15 is intermittently formed on the current collecting sheet 12, and the current collecting sheet 12 has a plurality of coated regions 16 and uncoated regions 17 that are alternately formed. The coated region 16 refers to the region from the coating start end P1 to the coating end end P2. The uncoated region 17 is later used for welding the positive electrode lead and / or cutting each positive electrode for one battery.

[0016] Normally, even when the discharge of the positive electrode slurry 14 from the coating head 13 stops, the surface tension of the positive electrode slurry 14 causes the coating film 15 to extend from the coating head 13, so that the positive electrode slurry 14 extends from the coating end portion P2 toward the uncoated region 17 adjacent to P2 along the conveying direction X, and stringy marks 18 are likely to occur. If the length L of the stringy marks 18 is large, poor welding of the positive electrode lead in the uncoated region may occur, and the reliability of the positive electrode may decrease.

[0017] In contrast, in the present disclosure, the positive electrode slurry contains compound A. This makes it possible to suppress stringiness at the coating end. That is, the length L of the stringiness mark 18 shown in FIG. 2 can be reduced, or the stringiness mark 18 can be eliminated. By suppressing stringiness, a highly reliable positive electrode can be obtained.

[0018] In addition, the addition of compound A to the positive electrode slurry suppresses the above-mentioned stringiness, so there is no need to attach a vibration generator to the coating device, and the coating device and its operation can be avoided from becoming complicated, improving the productivity of the positive electrode and reducing the manufacturing cost. It is also possible to easily accommodate larger coating devices and faster coating speeds at low cost.

[0019] (Compound A) Compound A has a polyether group and an acidic group in the molecule. The acidic group includes a carboxyl group, a sulfonic acid group, a phosphoric acid group, a phosphoric acid ester group, and the like. The polyether group includes a polyalkylene oxide group, and the like. The polyalkylene oxide group includes polyethylene oxide (PEO), polypropylene oxide (PPO), a copolymer of ethylene oxide (EO) and propylene oxide (PO), and the like. The above copolymer may be a block copolymer or a random copolymer. Compound A may have a linking group between the polyether group and the acidic group. Specifically, compound A includes polyether acid, and the like.

[0020] From the viewpoint of suppressing the stringiness, the content of compound A in the positive electrode slurry is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.6 parts by mass or more per 100 parts by mass of the positive electrode active material. Also, from the viewpoint of ensuring the positive electrode capacity (amount of positive electrode active material), the content of compound A in the positive electrode slurry is, for example, 5.0 parts by mass or less per 100 parts by mass of the positive electrode active material.

[0021] (Positive electrode mixture) The positive electrode mixture contains a positive electrode active material capable of electrochemically absorbing and releasing lithium ions, a conductive agent, a binder, and the above-mentioned compound A.

[0022] As the positive electrode active material, for example, a lithium-containing composite oxide containing transition metal elements such as Ni, Co, and Mn can be used. Examples of the lithium-containing composite oxide include Li a CoO2, Li a NiO2, Li a MnO2, Li a Co b Ni 1-b O2, Li a Co b M 1-b O c 、Li a Ni 1-b M b O c 、Li a Mn2O4, Li a Mn 2-b M b O 4、 LiMPO 4、 Li2MPO4F and the like. Here, M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, and 0 < a ≤ 1.2, 0 < b ≤ 0.9, 0 ≤ c ≤ 2.3. The a value indicating the molar ratio of lithium increases or decreases during charge and discharge.

[0023] Examples of the conductive agent include carbons such as acetylene black, carbon black, and carbon nanotubes; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and organic conductive materials such as phenylene derivatives. In the case of the positive electrode mixture, graphites such as natural graphite and artificial graphite can be further exemplified as the conductive agent. The conductive agent may be used alone or in combination of two or more.

[0024] Examples of the binder include resin materials, such as fluororesins such as polytetrafluoroethylene and polyvinylidene fluoride, polyolefin resins such as polyethylene and polypropylene, polyamide resins such as aramid resin, polyimide and polyamideimide resins, acrylic resins such as polyacrylic acid, polymethyl acrylate and ethylene-acrylic acid copolymer, vinyl resins such as polyacrylonitrile and polyvinyl acetate, and rubber-like materials such as styrene-butadiene copolymer rubber (SBR). One type of binder may be used alone, or two or more types may be used in combination.

[0025] (dispersion medium) The dispersion medium is not particularly limited, but examples thereof include water, alcohols such as ethanol, ethers such as tetrahydrofuran, amides such as dimethylformamide, and N-methyl-2-pyrrolidone (NMP).

[0026] [Cathode manufacturing method] The manufacturing method of the positive electrode according to the embodiment of the present disclosure includes a first step of preparing a positive electrode slurry, and a second step of applying the positive electrode slurry to a surface of a current collector sheet, drying the same, and forming a positive electrode mixture layer. The positive electrode mixture layer may be formed on one surface or both surfaces of the current collector sheet. The manufacturing method may further include a step of rolling the positive electrode mixture layer.

[0027] (1st step) In the first step, the materials for the positive electrode mixture are added to the dispersion medium, and then the mixture of the positive electrode mixture and the dispersion medium is stirred, which makes it possible to easily include compound A in the positive electrode slurry.

[0028] (2nd process) The second step includes a step 2A of applying a positive electrode slurry to the surface of the current collector sheet, and a step 2B of drying the coating film attached to the surface of the current collector sheet to form a positive electrode mixture layer.

[0029] (2nd A process) In step 2A, the positive electrode slurry may be intermittently applied to the surface of the strip-shaped current collecting sheet while the current collecting sheet is being transported. In the intermittent application, many coating end portions are repeatedly formed on the surface of the current collecting sheet, and therefore the use of the positive electrode slurry can significantly suppress stringiness of the coating end portions.

[0030] A roll or the like may be used to transport the current collecting sheet, and the transport speed of the current collecting sheet may be adjusted by the number of rotations of the roll or the like. The transport speed of the current collecting sheet is, for example, 10 m / min or more and 100 m / min or less. Examples of the coating device include a die coater.

[0031] (2nd B process) In the 2B step, the dispersion medium is removed from the coating film by drying. After the coating film is dried and rolled using a rolling roller, the thickness of the positive electrode mixture layer is, for example, 10 μm or more and 100 μm or less. When the positive electrode slurry is intermittently applied in the 2A step, the positive electrode mixture layer is intermittently formed on the surface of the current collector sheet in the 2B step. That is, the current collector sheet has a plurality of positive electrode mixture layer formation regions and positive electrode mixture layer non-formation regions that are alternately formed.

[0032] The above manufacturing method may further include a step of cutting the electrode plate including the current collector sheet obtained in the second step and the positive electrode mixture layer formed on the surface of the current collector sheet at a predetermined interval. This makes it possible to obtain a plurality of positive electrodes including the current collector sheet and the positive electrode mixture layer supported on the current collector sheet. When the positive electrode slurry is intermittently applied in the 2A step, the current collector sheet may be cut together with the positive electrode mixture layer in the region where the positive electrode mixture layer is formed on the current collector sheet, or the current collector sheet may be cut in the region where the positive electrode mixture layer is not formed on the current collector sheet.

[0033] (current collecting sheet) As the current collecting sheet, a non-porous conductive substrate (such as metal foil) or a porous conductive substrate (such as a mesh, net, or punched sheet) is used.

[0034] Examples of the material of the positive electrode current collector sheet include stainless steel, aluminum, aluminum alloy, titanium, etc. The thickness of the positive electrode current collector sheet is, for example, 10 μm or more and 15 μm or less.

[0035] [Positive electrode] The electrode according to the embodiment of the present disclosure includes a current collector sheet and a positive electrode mixture layer supported on the current collector sheet, and the positive electrode mixture layer is formed using the above-mentioned positive electrode slurry. The positive electrode mixture layer is usually formed by applying the positive electrode slurry to the surface of the current collector sheet and drying it. That is, the positive electrode is obtained by the above-mentioned manufacturing method.

[0036] [Secondary battery] The secondary battery according to the embodiment of the present disclosure includes a positive electrode, a negative electrode, and an electrolyte, and the positive electrode is obtained using the above-mentioned positive electrode slurry. Compound A in the positive electrode mixture layer may remain in a small amount in the positive electrode mixture layer in the battery.

[0037] The secondary battery according to the embodiment of the present disclosure will be described in detail below.

[0038] (positive electrode) The positive electrode includes, for example, a positive electrode current collector (current collector sheet) and a positive electrode mixture layer formed on the surface of the positive electrode current collector. The positive electrode mixture layer can be formed by applying the above-mentioned positive electrode slurry to the surface of the positive electrode current collector and drying it. The positive electrode mixture layer includes a positive electrode active material, a binder, a conductive agent, and compound A. The positive electrode mixture layer may be formed on one surface or both surfaces of the positive electrode current collector.

[0039] (Negative electrode) The negative electrode includes, for example, a negative electrode current collector (current collector sheet) and a negative electrode mixture layer formed on the surface of the negative electrode current collector. The negative electrode mixture layer can be formed by applying a negative electrode slurry in which the negative electrode mixture is dispersed in a dispersion medium to the surface of the negative electrode current collector and drying it. As the dispersion medium, those exemplified in the positive electrode slurry can be used. After drying the coating, the thickness of the negative electrode mixture layer after rolling with a rolling roller is, for example, 10 μm or more and 100 μm or less. The negative electrode mixture layer may be formed on one surface of the negative electrode current collector or on both surfaces. The negative electrode mixture layer includes, for example, a negative electrode active material, a binder, and a thickener.

[0040] Examples of the negative electrode active material include carbon materials, silicon, silicon compounds such as silicon oxide, and lithium alloys containing at least one selected from the group consisting of tin, aluminum, zinc, and magnesium. Examples of the carbon material include graphite (natural graphite, artificial graphite, etc.), amorphous carbon, etc.

[0041] As the binder, those exemplified in the positive electrode mixture can be used. As the thickener, carboxymethyl cellulose (CMC) and its modified form (including salts such as Na salt) can be exemplified.

[0042] As the current collector sheet, a non-porous conductive substrate (metal foil, etc.) or a porous conductive substrate (mesh, net, punched sheet, etc.) is used. Examples of the material of the current collector sheet for the negative electrode include stainless steel, nickel, nickel alloy, copper, copper alloy, etc. The thickness of the current collector sheet for the negative electrode is, for example, 3 μm or more and 50 μm or less.

[0043] (electrolyte) The electrolyte may be a liquid electrolyte in which a solute such as a lithium salt is dissolved in a solvent. As the solvent, a non-aqueous solvent may be used, and water may also be used. The electrolyte may also be a solid electrolyte.

[0044] The electrolyte includes, for example, a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. The concentration of the lithium salt in the electrolyte is preferably, for example, 0.5 mol / L or more and 2 mol / L or less. When the concentration of the lithium salt is within the above range, an electrolyte having excellent ion conductivity and appropriate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.

[0045] Examples of the non-aqueous solvent include cyclic carbonates, chain carbonates, cyclic carboxylates, and chain carboxylates. Examples of the cyclic carbonates include propylene carbonate (PC) and ethylene carbonate (EC). Examples of the chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of the cyclic carboxylates include γ-butyrolactone (GBL) and γ-valerolactone (GVL). Examples of the chain carboxylates include methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, and propyl propionate. The non-aqueous solvent may be used alone or in combination of two or more.

[0046] Examples of lithium salts include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1 <x<6、nは1または2)、LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylates, borates, imide salts, etc. Borates include Li2B4O7, Li(B(C2O4)F2), etc. Imide salts include LiN(SO2CF3)2, LiN(C l F 2l+1 SO2)(C m F 2m+1SO2) {l and m are integers of 0 or more}. The lithium salt may be used alone or in combination of two or more.

[0047] (Separator) Generally, it is desirable to interpose a separator between the positive electrode and the negative electrode. The separator has high ion permeability and has appropriate mechanical strength and insulation. As the separator, a microporous thin film, a woven fabric, a nonwoven fabric, etc. can be used. As the material of the separator, a polyolefin such as polypropylene or polyethylene is preferable. A heat-resistant layer containing an aramid resin or ceramics may be formed on the surface of the separator.

[0048] An example of the structure of the secondary battery is a structure in which an electrode group formed by winding a positive electrode and a negative electrode with a separator interposed therebetween and an electrolyte are housed in an exterior body. Alternatively, instead of a wound type electrode group, other types of electrode groups may be applied, such as a stacked type electrode group formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween. The secondary battery may be in any form, such as a cylindrical type, a square type, a coin type, a button type, a laminate type, or the like.

[0049] Hereinafter, the structure of a prismatic secondary battery according to an embodiment of the present disclosure will be described with reference to Fig. 3. Fig. 3 is a schematic perspective view of a secondary battery according to an embodiment of the present disclosure, with a portion cut away.

[0050] The battery includes a bottomed rectangular battery case 4, and an electrode group 1 and an electrolyte (not shown) housed in the battery case 4. The electrode group 1 includes a long strip-shaped negative electrode, a long strip-shaped positive electrode, and a separator interposed between them to prevent the negative electrode and the positive electrode from coming into direct contact with each other. The electrode group 1 is formed by winding the negative electrode, the positive electrode, and the separator around a flat winding core and removing the winding core. The positive electrode is produced by a method for producing a positive electrode according to an embodiment of the present disclosure.

[0051] One end of the negative electrode lead 3 is attached to the negative electrode current collector of the negative electrode by welding or the like. The other end of the negative electrode lead 3 is electrically connected to a negative electrode terminal 6 provided on the sealing plate 5 via a resin insulating plate (not shown). The negative electrode terminal 6 is insulated from the sealing plate 5 by a resin gasket 7. One end of the positive electrode lead 2 is attached to the positive electrode current collector of the positive electrode by welding or the like. The other end of the positive electrode lead 2 is connected to the back surface of the sealing plate 5 via an insulating plate. That is, the positive electrode lead 2 is electrically connected to the battery case 4 which also serves as the positive electrode terminal. The insulating plate separates the electrode group 1 and the sealing plate 5, and separates the negative electrode lead 3 and the battery case 4. The periphery of the sealing plate 5 is fitted into the open end of the battery case 4, and the fitting portion is laser welded. In this way, the opening of the battery case 4 is sealed with the sealing plate 5. The electrolyte injection hole provided in sealing plate 5 is closed with a sealing plug 8 . EXAMPLES

[0052] Hereinafter, the present disclosure will be specifically described based on examples and comparative examples, but the present disclosure is not limited to the following examples.

[0053] Example 1 (1) Preparation of positive electrode slurry A dispersion medium was added to the positive electrode active material, binder, conductive agent, and additives (that is, the positive electrode mixture), and the mixture was stirred using a mixer (TK Hivismix, manufactured by Primix Corporation) to prepare a positive electrode slurry.

[0054] A powdered lithium-containing composite oxide (average particle size 10 μm) was used as the positive electrode active material. A powdered polyvinylidene fluoride was used as the binder. A powdered acetylene black was used as the conductive agent. A polyether acid (HIPLAAD ED420, manufactured by Kusumoto Chemicals Co., Ltd.) was used as the additive compound A. N-methyl-2-pyrrolidone was used as the dispersion medium. The compounding ratio (mass ratio) of the positive electrode active material, the conductive agent, and the binder was 95:2.5:2.5. The content of the polyether acid in the positive electrode slurry was 0.6 parts by mass per 100 parts by mass of the positive electrode active material.

[0055] (2) Formation of positive electrode mixture layer The positive electrode slurry obtained above was used to carry out intermittent coating in the same manner as in Fig. 1. That is, while a roll was rotated to transport a strip-shaped current collector sheet, the positive electrode slurry obtained above was intermittently coated on the surface of the current collector sheet using a coating device. The coating film was then heated and dried at 100°C to form a positive electrode mixture layer.

[0056] An aluminum foil (thickness 15 μm) was used as the current collecting sheet. The rotation speed of the roll was adjusted so that the conveying speed of the current collecting sheet was 20 m / min. A slit-type die coater was used as the coating device. The gap between the die head and the roll was 200 μm. Intermittent coating was performed so that the length of the coated area (length in the conveying direction) of the current collecting sheet was 200 mm and the length of the uncoated area (length in the conveying direction) was 50 mm.

[0057] [evaluation] For the positive electrode mixture layer (coating film after drying) intermittently formed above, the length L of the stringy trace at the coating end was determined. Specifically, three coating end portions were randomly selected from the multiple coating end portions formed intermittently, the lengths of the stringy traces at the three selected coating end portions were measured, and the average value was calculated to be the length L.

[0058] The length of the stringy trace at each coating end was determined as follows. When the number N of stringy traces present at one coating end was 1, the length of one stringy trace was measured and defined as the length of the stringy trace at that coating end. When the number N of stringy traces present at one coating end was 2 to 20, the lengths of the N stringy traces were measured, their average value was calculated, and defined as the length of the stringy trace at that coating end. When the number N of stringy traces present at one coating end was 21 or more, 20 stringy traces were selected in order from the center of the coating film, the lengths of the selected 20 stringy traces were measured, and their average value was calculated, and defined as the length of the stringy trace at that coating end. The length of the stringy trace here refers to the length in the coating direction (the conveyance direction of the current collecting sheet) at the stringy trace portion at the coating end, and indicates the length from the root to the tip of the stringy trace.

[0059] Comparative Example 1 A positive electrode mixture layer was formed and evaluated in the same manner as in Example 1, except that a polycarboxylic acid (manufactured by Kusumoto Chemicals, Ltd., HIPLAAD ED111) was used instead of the polyether acid.

[0060] Comparative Example 2 A positive electrode mixture layer was formed and evaluated in the same manner as in Example 1, except that an amine mixture (HIPLAAD ED120, manufactured by Kusumoto Chemicals Co., Ltd.) was used instead of the polyether acid.

[0061] Comparative Example 3 A positive electrode mixture layer was formed and evaluated in the same manner as in Example 1, except that the positive electrode slurry did not contain polyether acid.

[0062] The evaluation results of Example 1 and Comparative Examples 1 to 3 are shown in Table 1. The length L of the stringy trace in Table 1 is expressed as a relative value, with the length L of the stringy trace in Comparative Example 3 taken as 100.

[0063] [Table 1]

[0064] In Example 1 in which polyether acid was contained in the positive electrode slurry, the length L of the stringy trace was smaller than in Comparative Examples 1 to 3. [Industrial Applicability]

[0065] The positive electrode slurry according to the present disclosure is suitably used for producing positive electrodes that require high reliability. [Explanation of symbols]

[0066] 1 electrode group 2 Positive Lead 3 Negative lead 4 Battery case 5 Sealing plate 6 Negative terminal 7 Gasket 8. Sealing 11 Rolls 12 Current collector sheet 13 Coating head 14 Positive electrode slurry 15 Coating 16 Application area 17 Uncoated area 18 Thread marks P1 Coating start point P2 Coating end

Claims

1. A positive electrode mixture and a dispersion medium (excluding aqueous solvents) for dispersing the positive electrode mixture, The positive electrode mixture includes a positive electrode active material, a conductive agent, a binder, and an additive, The additive includes a compound having a polyether group and an acidic group in the molecule (excluding the compound chemically bonded to the binder), The content of the compound is 0.1 parts by mass or more per 100 parts by mass of the positive electrode active material, The positive electrode slurry, wherein the acidic group includes at least one selected from the group consisting of a carboxyl group and a sulfonic acid group.

2. The cathode slurry of claim 1 , wherein the polyether group comprises a polyalkylene oxide group.

3. A positive electrode mixture comprising: a dispersion medium for dispersing the positive electrode mixture; The positive electrode mixture includes a positive electrode active material, a conductive agent, a binder, and an additive, The additive includes a compound having a polyether group and an acidic group in the molecule (excluding the compound chemically bonded to the binder), The content of the compound is 0.1 parts by mass or more per 100 parts by mass of the positive electrode active material, the acidic group includes at least one selected from the group consisting of a carboxyl group and a sulfonic acid group, The polyether group comprises a polyalkylene oxide group.

4. A current collecting sheet; and a positive electrode mixture layer supported on the current collecting sheet, The positive electrode mixture layer is formed using the positive electrode slurry according to any one of claims 1 to 3.

5. The battery includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode of claim 4 .

6. A first step of preparing a positive electrode slurry according to any one of claims 1 to 3; a second step of applying the positive electrode slurry to a surface of a current collecting sheet and drying the positive electrode slurry to form a positive electrode mixture layer.

7. The method for producing a positive electrode according to claim 6 , wherein in the second step, the positive electrode slurry is intermittently applied to a surface of the current collector sheet while the strip-shaped current collector sheet is being transported.

8. The method for producing a positive electrode according to claim 6 or 7, wherein in the first step, the binder and the additive are separately added to the dispersion medium.

Citation Information

Patent Citations

  • Dispersion method for nanometer silicon

    CN105118996A

  • Non-aqueous secondary battery and manufacture thereof

    JP1995029605A

  • Intermittent coating device and method and manufacture of cell electrode and nonaqueous electrolyte solution cell

    JP1996229481A

  • Negative electrode and battery, and manufacturing method of these

    JP2004146253A

  • A composite binder polymer for electrodes with a dispersant chemically bonded to it.

    JP2006519883A