Lithium manganese iron phosphate positive electrode material, preparation method thereof and lithium ion battery

By using nitride surface modification on lithium manganese iron phosphate material to form a core-shell structure, the water absorption and manganese dissolution problems of the material are solved, and the cycle stability and high-temperature performance of lithium-ion batteries are significantly improved.

CN118919700APending Publication Date: 2024-11-08DONGFENG MOTOR GRP
View PDF 0 Cites 8 Cited by

Patent Information

Application Number
CN202411277753.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Due to the introduction of manganese, lithium manganese ferroferric phosphate material has reduced ion/electronic conductivity, poor material rate performance, and nano-removal treatment increases water absorption and manganese dissolution problems, resulting in reduced cyclic stability and lithium storage sites.

Method used

The surface modification is used for nitride to form a core-shell structure, including the core of lithium manganese iron phosphate and a nitride coating, which inhibits the dissolution of manganese ions and the side reaction of water, and improves circulation stability.

Benefits of technology

It effectively isolates the side reaction of water, inhibits the dissolution of manganese ions, improves the cycle stability and high-temperature performance of the battery, reduces the gas production rate, and improves the discharge capacity and conductivity of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919700A_ABST
    Figure CN118919700A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium iron manganese phosphate positive electrode material, a preparation method thereof and a lithium ion battery, and relates to the technical field of battery materials, the lithium iron manganese phosphate positive electrode material is of a core-shell structure, and comprises a lithium iron manganese phosphate core and a nitride coating layer, the particle size of the lithium iron manganese phosphate positive electrode material is 0.2-5 microns, and the nitride coating layer is a silicon nitride coating layer. The chemical formula of the lithium manganese iron phosphate inner core is LiMn < x > Fe < 1-x > PO4, and x ranges from 0.1 to 0.9. Nitride is adopted for surface modification, so that side reaction with water is isolated, and dissolution of manganese ions is inhibited; meanwhile, due to the characteristic of high temperature resistance of the nitride, the problem of air expansion of the lithium manganese iron phosphate battery core can be effectively inhibited, and the cycling stability is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a lithium manganese iron phosphate positive electrode material, a preparation method thereof and a lithium ion battery. Background Art

[0002] Since lithium iron manganese phosphate material has a higher discharge platform and energy density than lithium iron phosphate material, lithium iron manganese phosphate material is considered to be an upgraded version of lithium iron phosphate material. However, due to the introduction of manganese, the ion / electronic conductivity of the material is greatly reduced, so the material rate performance is poor. At present, major electrode material manufacturers improve the electrochemical performance of lithium iron manganese phosphate materials through nano-sizing, ion doping and carbon coating.

[0003] Nano-processing of materials has greatly increased the specific surface area of ​​the materials, but it also makes the materials easier to absorb water, which intensifies the side reactions of the materials. In order to reduce the water absorption of the materials, strict preservation and preparation schemes need to be established, which undoubtedly increases the production, preservation and transportation costs. In addition, during the cycle, due to the high activity of nano-materials, the manganese dissolution problem is aggravated, resulting in a reduction in lithium storage sites and a loss of positive electrode active materials. At high temperatures, the side reactions of the electrolyte are intensified, and the production of HF will react with the manganese in the material and produce a large amount of gas. At the same time, the dissolved manganese ions are deposited on the surface of the negative electrode to destroy the SEI film, resulting in poor cycle stability. Therefore, it is urgent to develop suitable strategies to reduce the side reactions of lithium iron manganese phosphate with water, especially to improve its high-temperature gas production problem. Summary of the invention

[0004] The main purpose of the present invention is to provide a lithium iron manganese phosphate positive electrode material, a preparation method thereof and a lithium ion battery, aiming to use nitride for surface modification, thereby suppressing the flatulence problem of the lithium iron manganese phosphate battery cell and improving the cycle stability.

[0005] To achieve the above object, the lithium iron manganese phosphate positive electrode material proposed in the present invention is a core-shell structure, including a lithium iron manganese phosphate core and a nitride coating layer, the particle size of the lithium iron manganese phosphate positive electrode material is 0.2-5 μm, and the chemical formula of the lithium iron manganese phosphate core is LiMn x Fe 1-x PO4, wherein x is 0.1-0.9.

[0006] In one embodiment, the material of the nitride coating layer includes one of carbon nitride, boron nitride, phosphorus nitride, silicon nitride, magnesium nitride, aluminum nitride, titanium nitride, zirconium nitride and tantalum nitride; and / or,

[0007] The thickness of the nitride coating layer is 0.5-10 nm.

[0008] In one embodiment, a carbon layer is further included between the lithium manganese iron phosphate core and the nitride coating layer; and the nitride coating layer is located on the outer surface of the carbon layer.

[0009] The present invention also provides a method for preparing the lithium iron manganese phosphate positive electrode material, comprising the following steps:

[0010] S10, mixing a manganese source, an iron source and a precipitant to obtain a precursor;

[0011] S20, wet-milling the precursor, a lithium source, a carbon source and a phosphate and drying the mixture to obtain a mixed intermediate;

[0012] S30, calcining the mixed intermediate to obtain a lithium manganese iron phosphate material coated with a carbon layer;

[0013] S40, mixing the carbon layer-coated lithium iron manganese phosphate material with a nitride precursor to prepare the lithium iron manganese phosphate positive electrode material;

[0014] Wherein, the outermost layer of the lithium manganese iron phosphate positive electrode material is a nitride coating layer.

[0015] In one embodiment, the precipitant in step S10 comprises oxalic acid; and / or,

[0016] The manganese source comprises at least one of manganese sulfate, manganese acetate and manganese chloride; and / or,

[0017] The iron source comprises at least one of ferrous sulfate, ferrous acetate and ferrous chloride; and / or,

[0018] The molar ratio of the manganese source to the iron source is (1-9): (1-9); and / or,

[0019] The molar ratio of the precipitant to the manganese source and the iron source is (1.5-4):1;

[0020] The total concentration of the manganese source and the iron source is 0.1 mol L -1 -0.4mol L -1 .

[0021] In one embodiment, the lithium source in step S20 includes at least one of lithium carbonate and lithium hydroxide; and / or,

[0022] The phosphate includes at least one of diammonium phosphate and diammonium hydrogen phosphate; and / or,

[0023] The molar ratio of the lithium source, phosphate and precursor is (1.0-1.2): (1.0-1.05): 1; and / or,

[0024] The carbon source comprises at least one of glucose, sucrose and starch; and / or,

[0025] The amount of the carbon source added is 3-15wt% of the total mass of the lithium source, phosphate and precursor.

[0026] In one embodiment, step S30 includes:

[0027] The mixed intermediate is heated from room temperature to 300-400°C for 2-6 hours, and then heated to 600-800°C for 5-10 hours;

[0028] Wherein, the rate of the primary heating is 1-2°C / min; and / or,

[0029] The secondary heating rate is 5-10°C / min.

[0030] In one embodiment, the nitride precursor in step S40 includes one of melamine, urea, boride, silicate and metal salt; and / or,

[0031] After mixing, a lithium manganese iron phosphate positive electrode material is obtained by one of a solid phase pyrolysis method, a magnetron sputtering method and a chemical vapor deposition method;

[0032] When chemical vapor deposition is used, the atmosphere used is one of ammonia and nitrogen.

[0033] In one embodiment, when solid phase pyrolysis is used, the specific operation is:

[0034] The carbon layer-coated lithium manganese iron phosphate material is mixed with a nitride precursor by wet ball milling for 0.5-12 hours, and then vacuum dried at 40-80°C for 2-12 hours; then, in an inert atmosphere, the temperature is raised from 25°C to 300°C, kept for 2 hours, and then raised to 900-1500°C, and kept for 2-5 hours.

[0035] The present invention also provides a lithium-ion battery, comprising the lithium iron manganese phosphate positive electrode material or the lithium iron manganese phosphate positive electrode material prepared by the preparation method of the lithium iron manganese phosphate positive electrode material.

[0036] The lithium iron manganese phosphate positive electrode material proposed in the present invention is a core-shell structure, including a lithium iron manganese phosphate core and a nitride coating layer. The particle size of the lithium iron manganese phosphate positive electrode material is 0.2-5 μm, and the chemical formula of the lithium iron manganese phosphate core is LiMn x Fe 1-xPO4, where x is 0.1-0.9. The use of nitrides for surface modification not only isolates the side reaction with water and inhibits the dissolution of manganese ions, but also effectively inhibits the flatulence problem of lithium manganese iron phosphate batteries and improves cycle stability due to the high temperature resistance of nitrides. The use of nitrides for surface modification does not require major changes to the current production process, and is highly feasible to implement. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0038] Figure 1 A synthetic route map of the lithium iron manganese phosphate positive electrode material provided by the present invention;

[0039] Figure 2 This is a schematic diagram of the structure of the lithium iron manganese phosphate positive electrode material provided by the present invention.

[0040] Description of Figure Numbers:

[0041] 1. Lithium manganese iron phosphate core; 2. Nitride coating layer; 3. Carbon layer.

[0042] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] It should be noted that if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if "and / or" or "and / or" appears in the full text, its meaning includes three parallel schemes. Taking "A and / or B" as an example, it includes scheme A, or scheme B, or a scheme that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0045] During the cycle, due to the high activity of nanomaterials, the manganese dissolution problem is aggravated, resulting in a reduction in lithium storage sites and loss of positive electrode active materials. At high temperatures, the side reactions of the electrolyte are intensified, and the generation of HF will react with the manganese in the material and produce a large amount of gas. At the same time, the dissolved manganese ions are deposited on the surface of the negative electrode to destroy the SEI film, resulting in poor cycle stability.

[0046] The present invention proposes a lithium iron manganese phosphate positive electrode material with a core-shell structure, comprising a lithium iron manganese phosphate core 1 and a nitride coating layer 2, wherein the particle size of the lithium iron manganese phosphate positive electrode material is 0.2-5 μm, and the chemical formula of the lithium iron manganese phosphate core 1 is LiMn x Fe 1-x PO4, where x is 0.1-0.9. The use of nitride for surface modification not only isolates the side reaction with water and inhibits the dissolution of manganese ions, but also effectively inhibits the flatulence problem of lithium manganese iron phosphate batteries and improves cycle stability due to the high temperature resistance of nitride.

[0047] See also Figure 1 In one embodiment of the present invention, the material of the nitride coating layer 2 includes one of carbon nitride, boron nitride, phosphorus nitride, silicon nitride, magnesium nitride, aluminum nitride, titanium nitride, zirconium nitride and tantalum nitride. Carbon nitride (CN) has good electrical conductivity and chemical stability; boron nitride (BN) and silicon nitride (SiN) both have high hardness and good thermal stability; phosphorus nitride (PN) has excellent oxidation stability and electrocatalytic activity, and can be selected according to specific application requirements.

[0048] In one embodiment of the present invention, the thickness of the nitride coating layer 2 is 0.5-10 nm. When controlled within this range, the electrochemical performance of the lithium manganese iron phosphate positive electrode material can be effectively optimized. This thin layer structure helps to improve the transmission efficiency of electrons while maintaining the structural stability of the material as a whole. The appropriate thickness can ensure that the nitride layer is evenly covered on the surface of the lithium manganese iron phosphate positive electrode material, thereby improving the cycle stability and discharge capacity of the battery.

[0049] Preferably, the thickness of the nitride coating layer 2 is 3-8 nm.

[0050] In one embodiment of the present invention, a carbon layer 3 is further included between the lithium iron manganese phosphate core 1 and the nitride coating layer 2; the nitride coating layer 2 is located on the outer surface of the carbon layer 3. The carbon layer 3 in the middle effectively inhibits the agglomeration of the lithium iron manganese phosphate core 1 during the calcination process, while giving the material excellent conductivity; the nitride coating layer 2 in the outermost layer is conducive to direct isolation from the contact with the electrolyte, avoiding corrosion by water and HF.

[0051] The present invention also provides a method for preparing the lithium manganese iron phosphate positive electrode material. Since the preparation method adopts all the technical solutions of all the above embodiments, it at least has all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here. The preparation method includes the following steps:

[0052] S10, mixing a manganese source, an iron source and a precipitant to obtain a precursor;

[0053] S20, wet-milling the precursor, a lithium source, a carbon source and a phosphate and drying the mixture to obtain a mixed intermediate;

[0054] S30, calcining the mixed intermediate to obtain a lithium manganese iron phosphate material coated with a carbon layer 3;

[0055] S40, mixing the lithium iron manganese phosphate material coated with the carbon layer 3 with a nitride precursor to prepare the lithium iron manganese phosphate positive electrode material;

[0056] The outermost layer of the lithium manganese iron phosphate positive electrode material is a nitride coating layer 2 .

[0057] By modifying the nitride coating 2 on the outer surface of the lithium iron manganese phosphate core 1, the material is isolated from direct contact with water and electrolyte at the beginning of the cycle, avoiding corrosion by inorganic acid and water. In addition, the nitride coating 2 has the characteristics of high temperature resistance, which effectively improves the dissolution and gas production of manganese during the cycle and improves the high temperature cycle performance of the battery. Due to the poor conductivity of the lithium iron manganese phosphate core 1, a carbon source is introduced into the precursor, uniformly mixed, and carbonized at high temperature, so that the surface of the lithium iron manganese phosphate core 1 is coated with a layer of carbon (i.e., carbon layer 3) with a thickness of 2-10nm.

[0058] In one embodiment of the present invention, the precipitant in step S10 includes oxalic acid. Manganese ions and iron ions react with oxalate ions to form oxalate precipitates.

[0059] In one embodiment of the present invention, the manganese source in step S10 includes at least one of manganese sulfate, manganese acetate and manganese chloride. Manganese sulfate, manganese acetate and manganese chloride are all soluble manganese salts.

[0060] In one embodiment of the present invention, the iron source in step S10 includes at least one of ferrous sulfate, ferrous acetate and ferrous chloride. Ferrous sulfate, ferrous acetate and ferrous chloride are all soluble iron salts.

[0061] In one embodiment of the present invention, the molar ratio of the manganese source to the iron source in step S10 is (1-9): (1-9). Under this ratio, on the one hand, the energy density of the lithium iron phosphate-based material as a positive electrode can be improved, and on the other hand, the problem of poor electronic / ionic conductivity of lithium manganese phosphate can be synergistically improved.

[0062] In one embodiment of the present invention, the sum of the concentrations of the manganese source and the iron source in step S10 is 0.1 mol L -1 -0.4molL -1 At this concentration, it is conducive to the full reaction of the manganese source and the iron source with the precipitant, and the reaction time is shortened and the consistency is improved.

[0063] In one embodiment of the present invention, the lithium source in step S20 includes at least one of lithium carbonate and lithium hydroxide. Both lithium carbonate and lithium hydroxide are soluble.

[0064] In one embodiment of the present invention, the phosphate in step S20 includes at least one of diammonium phosphate and diammonium hydrogen phosphate. The use of these two phosphates has a relatively low cost, and the ammonium ions are vaporized and overflowed during the high temperature process, thereby avoiding the introduction of other metal cation impurities.

[0065] In one embodiment of the present invention, the carbon source in step S20 includes at least one of glucose, sucrose and starch. The advantages of selecting the above carbon sources are that such materials are cheap, relevant carbonization technologies have been widely used, and the residual carbon content in the material, the degree of graphitization of carbon, etc. can be accurately controlled.

[0066] In one embodiment of the present invention, the molar ratio of the lithium source, phosphate and precursor in step S20 is (1.0-1.2): (1.0-1.05): 1. Under the above ratio, the lithium source and phosphorus source are slightly excessive, which not only makes up for the loss of lithium source and phosphoric acid during the high temperature process, but also ensures the full lithiation and phosphation of the material. In addition, the slightly excessive lithium source and phosphoric acid avoid the problem of excessive impurity content in the product.

[0067] In one embodiment of the present invention, step S30 includes:

[0068] The mixed intermediate is heated from room temperature to 300-400°C for 2-6 hours, and then heated to 600-800°C for 5-10 hours;

[0069] The rate of the first heating is 1-2°C / min, and the rate of the second heating is 5-10°C / min. Gradient heating is used, and the first heating rate is relatively low, which effectively avoids insufficient material reaction and agglomeration caused by over-rapid heating.

[0070] In one embodiment of the present invention, the nitride precursor in step S40 includes one of melamine, urea, boride, silicate and metal salt; and / or,

[0071] After mixing, a lithium manganese iron phosphate positive electrode material is obtained by one of a solid phase pyrolysis method, a magnetron sputtering method and a chemical vapor deposition method;

[0072] When chemical vapor deposition is used, the atmosphere used is one of ammonia and nitrogen.

[0073] In one embodiment of the present invention, when the solid phase pyrolysis method is adopted, the specific operation is as follows:

[0074] The carbon layer-coated lithium manganese iron phosphate material is mixed with a nitride precursor by wet ball milling for 0.5-12 hours, and then vacuum dried at 40-80°C for 2-12 hours; then, in an inert atmosphere, the temperature is raised from 25°C to 300°C, kept for 2 hours, and then raised to 900-1500°C, and kept for 2-5 hours.

[0075] The present invention also provides a lithium ion battery, comprising the lithium iron manganese phosphate positive electrode material or the lithium iron manganese phosphate positive electrode material prepared by the preparation method of the lithium iron manganese phosphate positive electrode material. Since the lithium ion battery adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.

[0076] Example 1

[0077] This embodiment provides a method for preparing a lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0078] S10, prepare 1.0L, 0.6mol / L oxalic acid aqueous solution, then quickly pour 100mL, 0.24mol / L manganese acetate solution and 100mL, 0.16mol / L ferrous sulfate solution into the oxalic acid aqueous solution, stir at room temperature for 4h, then filter, wash and dry to obtain a precursor powder;

[0079] S20, mixing the precursor powder with lithium carbonate and ammonium dihydrogen phosphate in a molar ratio of 1:1.1:1.05 to obtain a mixture, adding glucose (8 wt% of the mixture), wet ball milling for 12 h, using ethanol as the solvent, and drying to obtain a mixed intermediate;

[0080] S30, calcining the mixed intermediate in stages, first heating from room temperature to 350°C, with a heating rate of 2°C / min, pre-calcining for 4 hours; then heating to 700°C, with a heating rate of 5°C / min, calcining for 7 hours. Calcining to obtain a lithium manganese iron phosphate material coated with a carbon layer 3, grinding after cooling in the furnace;

[0081] S40, the lithium manganese iron phosphate material coated with the carbon layer 3 and boron oxide are mixed by wet ball milling at a mass ratio of 19:1, the solvent used in the wet method is ethanol, the ball milling is carried out for 4 hours, and then vacuum dried at 60° C. for 6 hours. Then, in an ammonia atmosphere, the temperature is increased from 25° C. to 300° C., and the temperature is kept for 2 hours, and then the temperature is increased to 1000° C. and the temperature is kept for 5 hours.

[0082] The thickness of the nitride coating layer 2 of the prepared lithium manganese iron phosphate positive electrode material is 5 nm.

[0083] Example 2

[0084] This embodiment provides a method for preparing a lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0085] S10, prepare 1.0L, 0.8mol / L oxalic acid aqueous solution, then quickly pour 100mL, 0.24mol / L manganese acetate solution and 100mL, 0.16mol / L ferrous sulfate solution into the aqueous oxalic acid solution, stir at room temperature for 4h, then filter, wash and dry to obtain a precursor powder;

[0086] S20, mixing the precursor powder with lithium carbonate and ammonium dihydrogen phosphate in a molar ratio of 1:1.1:1.05 to obtain a mixture, adding glucose (10 wt% of the mixture), wet ball milling for 12 h, using ethanol as the solvent, and drying to obtain a mixed intermediate;

[0087] S30, calcining the mixed intermediate in stages, first heating from room temperature to 350°C at a heating rate of 2°C / min, pre-calcining for 4 hours; then heating to 700°C at a heating rate of 5°C / min, calcining for 7 hours. The carbon layer 3-coated lithium manganese iron phosphate material is calcined to obtain the material, which is ground after cooling in the furnace;

[0088] S40, the lithium manganese iron phosphate material coated with the carbon layer 3 and nano silicon are mixed by wet ball milling at a mass ratio of 19:1, the solvent used in the wet method is ethanol, the ball milling is carried out for 6 hours, and then vacuum dried at 80° C. for 4 hours. Then, in an ammonia atmosphere, the temperature is increased from 25° C. to 300° C., and the temperature is kept for 2 hours, and then the temperature is increased to 1500° C. and the temperature is kept for 4 hours.

[0089] The thickness of the nitride coating layer 2 of the prepared lithium manganese iron phosphate positive electrode material is 5 nm.

[0090] Example 3

[0091] This embodiment provides a method for preparing a lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0092] S10, prepare 1.0L, 0.8mol / L oxalic acid aqueous solution, then quickly pour 100mL, 0.24mol / L manganese acetate solution and 100mL, 0.16mol / L ferrous sulfate solution into the aqueous oxalic acid solution, stir at room temperature for 4h, then filter, wash and dry to obtain a precursor powder;

[0093] S20, mixing the precursor powder with lithium carbonate and ammonium dihydrogen phosphate in a molar ratio of 1:1.1:1.05 to obtain a mixture, adding glucose (8 wt% of the mixture), wet ball milling for 12 h, using ethanol as the solvent, and drying to obtain a mixed intermediate;

[0094] S30, calcining the mixed intermediate in stages, first heating from room temperature to 350°C at a heating rate of 2°C / min, pre-calcining for 4 hours; then heating to 700°C at a heating rate of 5°C / min, calcining for 7 hours. The lithium manganese iron phosphate core 1 is calcined to obtain the core, which is ground after cooling in the furnace;

[0095] S40, in an atmosphere of boron trichloride and ammonia, using chemical vapor deposition at a temperature of 1000° C., modifying the surface of the lithium manganese iron phosphate material coated with the carbon layer 3 with boron nitride, thereby obtaining a lithium manganese iron phosphate positive electrode material in which the nitride coating layer 2 is deposited on the surface of the carbon layer 3.

[0096] The thickness of the nitride coating layer 2 of the prepared lithium manganese iron phosphate positive electrode material is 3 nm.

[0097] Example 4

[0098] This embodiment provides a method for preparing a lithium iron manganese phosphate positive electrode material. Compared with Example 3, the difference is that step S40 is: in a titanium tetrachloride gas and nitrogen atmosphere with hydrogen as a carrier, titanium nitride is modified on the surface of the lithium iron manganese phosphate powder by chemical vapor deposition at a temperature of 800°C.

[0099] The thickness of the nitride coating layer 2 of the prepared lithium manganese iron phosphate positive electrode material is 8 nm.

[0100] Example 5

[0101] This embodiment provides a method for preparing a lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0102] S10, prepare 1.0L, 0.6mol / L oxalic acid aqueous solution, then quickly pour 100mL, 0.24mol / L manganese acetate solution and 100mL, 0.16mol / L ferrous sulfate solution into the aqueous oxalic acid solution, stir at room temperature for 4h, then filter, wash and dry to obtain a precursor powder;

[0103] S20, mixing the precursor powder with lithium carbonate and ammonium dihydrogen phosphate in a molar ratio of 1:1.1:1.05 to obtain a mixture, adding glucose (10 wt% of the mixture), wet ball milling for 12 h, using ethanol as the solvent, and drying to obtain a mixed intermediate;

[0104] S30, calcining the mixed intermediate in stages, first heating from room temperature to 350°C at a heating rate of 2°C / min, pre-calcining for 4 hours; then heating to 700°C at a heating rate of 5°C / min, calcining for 7 hours. The carbon layer 3-coated lithium manganese iron phosphate material is calcined to obtain the material, which is ground after cooling in the furnace;

[0105] S40, the lithium manganese iron phosphate material coated with the carbon layer 3 and boron oxide are mixed in a mass ratio of 50:1 by wet ball milling, the solvent used in the wet method is ethanol, the ball milling is carried out for 6 hours, and then vacuum dried at 80° C. for 6 hours. Then, in an ammonia atmosphere, the temperature is increased from 25° C. to 300° C., and the temperature is kept for 2 hours, and then the temperature is increased to 1000° C. and the temperature is kept for 5 hours.

[0106] The thickness of the nitride coating layer 2 of the prepared lithium manganese iron phosphate positive electrode material is 0.5 nm.

[0107] Example 6

[0108] This embodiment provides a method for preparing a lithium manganese iron phosphate positive electrode material, comprising the following steps:

[0109] S10, prepare 1.0L, 0.6mol / L oxalic acid aqueous solution, then quickly pour 100mL, 0.24mol / L manganese acetate solution and 100mL, 0.16mol / L ferrous sulfate solution into the aqueous oxalic acid solution, stir at room temperature for 4h, then filter, wash and dry to obtain a precursor powder;

[0110] S20, mixing the precursor powder with lithium carbonate and ammonium dihydrogen phosphate in a molar ratio of 1:1.1:1.05 to obtain a mixture, adding glucose (8 wt% of the mixture), wet ball milling for 12 h, using ethanol as the solvent, and drying to obtain a mixed intermediate;

[0111] S30, calcining the mixed intermediate in stages, first heating from room temperature to 350°C at a heating rate of 2°C / min, pre-calcining for 4 hours; then heating to 700°C at a heating rate of 5°C / min, calcining for 7 hours. The carbon layer 3-coated lithium manganese iron phosphate material is calcined to obtain the material, which is ground after cooling in the furnace;

[0112] S40, the lithium manganese iron phosphate material coated with the carbon layer 3 and boron oxide are mixed by wet ball milling at a mass ratio of 10:1, the solvent used in the wet method is methanol, the ball milling is carried out for 6 hours, and then vacuum dried at 60° C. for 8 hours. Then, in an ammonia atmosphere, the temperature is increased from 25° C. to 300° C., and the temperature is kept for 2 hours, and then the temperature is increased to 1000° C. and the temperature is kept for 5 hours.

[0113] The thickness of the nitride coating layer 2 of the prepared lithium manganese iron phosphate positive electrode material is 10.0 nm.

[0114] Example 7

[0115] This embodiment provides a method for preparing a lithium iron manganese phosphate positive electrode material. Compared with Example 3, the difference is that step S40 is: using magnetron sputtering, placing the lithium iron manganese phosphate core in an operating chamber, the target material is a high-purity silicon target, the working gas is high-purity nitrogen, the coating power is 100 W, the temperature is 350°C, and the operation time is 0.5 h.

[0116] The thickness of the nitride coating layer 2 of the prepared lithium manganese iron phosphate positive electrode material is 5 nm.

[0117] Comparative Example 1

[0118] Compared with Example 3, this comparative example does not perform step S40, does not perform nitride coating, and only obtains the lithium manganese iron phosphate core 1.

[0119] Table 1 Comparison of structures and performances of Examples 1-7 and Comparative Example 1

[0120]

[0121]

[0122] From the specific surface area data in Table 1, it can be seen that compared with Comparative Example 1, the nitride coating layer 2 prepared in Examples 1-7 will not have a significant impact on the specific surface area of ​​the lithium iron manganese phosphate positive electrode material, thereby avoiding the incremental addition of the electrolyte and reducing the side reaction; from the first coulomb efficiency data in Table 1, it can be seen that compared with Comparative Example 1, the presence of the nitride coating layer 2 in Examples 1-7 significantly improves the first coulomb efficiency of the battery, indicating that the side reaction with the electrolyte is isolated at the beginning of the cycle, thereby improving the reversibility of the charge and discharge cycle; from the first discharge capacity data in Table 1, it can be seen that compared with Comparative Example 1, due to the reduction of side reactions and the improvement of reversibility, the loss of active lithium in Examples 1-7 is significantly reduced, thereby improving its first discharge capacity; from the 1C discharge capacity in Table 1, it can be seen that due to the nitride coating layer The presence of 2 not only inhibits the side reaction with the electrolyte, but also significantly improves the conductivity of the material, so that it maintains a higher specific capacity under high current; from the expansion rate data of the soft-pack battery after 100 cycles at 45°C in Table 1, it can be seen that compared with Comparative Example 1, Examples 1-7 have a significantly reduced gas production rate at high temperature due to the presence of the nitride coating 2. Compared with Comparative Example 1, the expansion rate of Examples 1-7 is directly reduced by an order of magnitude, further illustrating that the material after nitride modification is more resistant to high temperatures; from the data of the capacity retention rate at 1C, 200 cycles in Table 1, it can be seen that compared with Comparative Example 1, Examples 1-7 have a significantly improved cycle stability due to the presence of the nitride coating 2, and at the same time, it is illustrated that the manganese dissolution phenomenon is effectively suppressed.

[0123] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A lithium manganese iron phosphate positive electrode material, characterized in that: The lithium iron manganese phosphate positive electrode material is a core-shell structure, including a lithium iron manganese phosphate core and a nitride coating layer. The particle size of the lithium iron manganese phosphate positive electrode material is 0.2-5 μm, and the chemical formula of the lithium iron manganese phosphate core is LiMn x Fe 1-x PO4, wherein x is 0.1-0.

9.

2. The lithium iron manganese phosphate positive electrode material according to claim 1, characterized in that The material of the nitride coating layer includes one of carbon nitride, boron nitride, phosphorus nitride, silicon nitride, magnesium nitride, aluminum nitride, titanium nitride, zirconium nitride and tantalum nitride; and / or, The thickness of the nitride coating layer is 0.5-10 nm.

3. The lithium iron manganese phosphate positive electrode material according to claim 1, characterized in that A carbon layer is further included between the lithium manganese iron phosphate core and the nitride coating layer; the nitride coating layer is located on the outer surface of the carbon layer.

4. A method for preparing the lithium manganese iron phosphate positive electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S10, mixing a manganese source, an iron source and a precipitant to obtain a precursor; S20, wet-milling the precursor, a lithium source, a carbon source and a phosphate and drying the mixture to obtain a mixed intermediate; S30, calcining the mixed intermediate to obtain a lithium manganese iron phosphate material coated with a carbon layer; S40, mixing the carbon layer-coated lithium iron manganese phosphate material with a nitride precursor to prepare the lithium iron manganese phosphate positive electrode material; Wherein, the outermost layer of the lithium manganese iron phosphate positive electrode material is a nitride coating layer.

5. The method for preparing the lithium manganese iron phosphate positive electrode material according to claim 4, characterized in that: The precipitant in step S10 includes oxalic acid; and / or, The manganese source comprises at least one of manganese sulfate, manganese acetate and manganese chloride; and / or, The iron source comprises at least one of ferrous sulfate, ferrous acetate and ferrous chloride; and / or, The molar ratio of the manganese source to the iron source is (1-9): (1-9); and / or, The ratio of the amount of the precipitant to the amount of the manganese source and the iron source is (1.5-4):1; The total concentration of the manganese source and the iron source is 0.1 mol L -1 -0.4mol L -1 .

6. The method for preparing the lithium iron manganese phosphate positive electrode material according to claim 4, characterized in that: The lithium source in step S20 includes at least one of lithium carbonate and lithium hydroxide; and / or, The phosphate includes at least one of diammonium phosphate and diammonium hydrogen phosphate; and / or, The molar ratio of the lithium source, phosphate and precursor is (1.0-1.2): (1.0-1.05): 1; and / or, The carbon source comprises at least one of glucose, sucrose and starch; and / or, The amount of the carbon source added is 3-15wt% of the total mass of the lithium source, phosphate and precursor.

7. The method for preparing the lithium iron manganese phosphate positive electrode material according to claim 4, characterized in that: Step S30 includes: The mixed intermediate is heated from room temperature to 300-400°C for 2-6 hours, and then heated to 600-800°C for 5-10 hours; Wherein, the rate of the primary heating is 1-2°C / min; and / or, The secondary heating rate is 5-10°C / min.

8. The method for preparing the lithium iron manganese phosphate positive electrode material according to claim 4, characterized in that: The nitride precursor in step S40 includes one of melamine, urea, boride, silicate and metal salt; and / or, After mixing, a lithium manganese iron phosphate positive electrode material is obtained by one of a solid phase pyrolysis method, a magnetron sputtering method and a chemical vapor deposition method; When chemical vapor deposition is used, the atmosphere used is one of ammonia and nitrogen.

9. The method for preparing the lithium iron manganese phosphate positive electrode material according to claim 8, characterized in that: When the solid phase pyrolysis method is used, the specific operation is: The carbon layer-coated lithium manganese iron phosphate material is mixed with a nitride precursor by wet ball milling for 0.5-12 hours, and then vacuum dried at 40-80°C for 2-12 hours; in an inert atmosphere, the temperature is increased from 25°C to 300°C, kept for 2 hours, and then increased to 900-1500°C, and kept for 2-5 hours.

10. A lithium ion battery, characterized in that: The invention comprises the lithium iron manganese phosphate positive electrode material as claimed in claims 1 to 3 or the lithium iron manganese phosphate positive electrode material prepared by the preparation method of the lithium iron manganese phosphate positive electrode material as claimed in claims 4 to 9.

Citation Information

Cited By

  • High-performance lithium manganese iron phosphate composite material as well as preparation method and application thereof

    CN117936736A

  • A high-performance lithium iron manganese phosphate composite material, a preparation method thereof and application thereof

    CN117936736B

  • Composite positive electrode material and preparation method and application thereof

    CN119447251A

  • Composite positive electrode material and preparation method and application thereof

    CN119447251B

  • Composite positive electrode material and preparation method thereof, positive plate and secondary battery

    CN119833596A